Manufacturing method of anode mixture containing graphite particles and a sulfide solid electrolyte
By optimizing the blending and mixing of graphite and LPS particles with controlled sizes and shapes, the method enhances the mixing properties and reduces porosity, resulting in an all-solid-state battery with improved discharge capacity and retention.
Patent Information
- Application Number
- JP2024140941
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-10-28
AI Technical Summary
The challenge in manufacturing all-solid-state lithium ion batteries is the difficulty in uniformly mixing graphite particles and sulfide-based solid electrolytes (LPS) due to poor fluidity of LPS particles, leading to insufficient mixing properties and increased porosity, which hinders the full utilization of LPS as a conduction path for Li ions, thereby limiting discharge capacity.
A method involving specific blending ratios and mixing times of graphite particles and LPS particles with controlled particle sizes and shapes, including fine and large-diameter LPS particles, to minimize porosity and enhance contact area, using a dry mixing technique to maintain ionic conductivity and adhesiveness.
The method results in an all-solid-state battery with high initial charge/discharge capacity and improved capacity retention during cycling, achieved by reducing porosity to 3% or less in the negative electrode composite layer.
Smart Images

Figure 2024161053000002 
Figure 2024161053000003 
Figure 2024161053000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a negative electrode mixture containing graphite particles and a sulfide solid electrolyte. [Background technology]
[0002] In recent years, electronic devices such as mobile phones, tablet terminals, and notebook computers have become increasingly high-performance and highly functional, and as a result, there is a growing demand for secondary batteries to be smaller, lighter, and have higher capacities. Under these circumstances, non-aqueous electrolyte (liquid) secondary batteries, such as lithium secondary batteries, have a higher battery voltage and can also have a higher energy density than nickel-cadmium batteries and nickel-metal hydride batteries, and are therefore rapidly becoming popular in the field of the above-mentioned electronic devices.
[0003] In addition, non-aqueous electrolyte secondary batteries are also becoming mainstream in the use of motor drive power sources for electric vehicles and hybrid vehicles against the backdrop of recent environmental problems. However, non-aqueous electrolyte secondary batteries generally contain flammable organic solvents, and therefore have safety problems such as ignition when abnormalities such as thermal runaway occur in the secondary battery, and immediate improvement is desired. As one of the techniques for improving such safety problems, research and development of all-solid-state lithium secondary batteries that use solid electrolytes instead of electrolytes using organic solvents is being actively carried out.
[0004] The main components of the all-solid-state lithium secondary battery are a positive electrode mixture (layer) containing a positive electrode active material and a solid electrolyte, a negative electrode mixture (layer) containing a negative electrode material using In metal, Li-In alloy, or carbon and a solid electrolyte, and a solid electrolyte (layer) provided between the positive electrode mixture and the negative electrode mixture. The solid electrolytes contained in the above-mentioned constituent materials can be broadly divided into oxide-based and sulfide-based types, and a representative example of the former oxide type is Li7La3Zr2O 12 or Li5La3Nb2O 12 The following can be mentioned.
[0005] However, oxide-based solid electrolytes have poor crushability, and therefore may not be able to obtain a dense structure in the powder compaction process in which powdered raw materials are compressed and molded during the manufacture of all-solid-state lithium secondary batteries. In addition, oxide-based solid electrolytes have problems such as the need for sintering under high temperature conditions to develop high ionic conductivity. In contrast, sulfide-based solid electrolytes do not have the problems of oxide-based solid electrolytes, and in particular, representative sulfide-based solid electrolytes having Li7PS6 phase, Li4P2S6 phase, or Li3PS4 phase as disclosed in Patent Document 1 (hereinafter also referred to as LPS) have flexibility and adhesion specific to sulfides, so they can be easily deformed during the above-mentioned powder compaction. Furthermore, sulfide-based solid electrolytes have the advantage that high ionic conductivity can be obtained without heat treatment depending on the composition, and are therefore expected to be more promising materials than oxide-based solid electrolytes.
[0006] The above-mentioned LPS is a compound synthesized using diphosphorus pentasulfide and lithium sulfide as raw materials, and the synthesis method generally used is a method of synthesizing the LPS by reaction with heat caused by impact of balls over a long period of time using a planetary ball mill (mechanical milling device) filled with inert gas, or a method of precipitating a crystalline phase (metastable phase) by further heat treatment as necessary. In addition, Patent Document 2 discloses a technique of blending graphite particles, which are cost-effective and can insert and remove ions by electrochemical action, as an active material when preparing a negative electrode composite material using the LPS synthesized by the above-mentioned method. This technique mechanically mixes graphite particles and LPS particles, and the resulting mixed powder is compacted and used as a negative electrode composite material layer. The LPS contained in the negative electrode composite material layer plays the role of a conductive path for Li ions. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2013-155087 A [Patent Document 2] JP 2014-203545 A Summary of the Invention [Problem to be solved by the invention]
[0008] In the above-mentioned all-solid-state lithium ion battery (hereinafter also referred to as all-solid-state battery), it is considered preferable to increase the content of graphite particles in the negative electrode mixture from the viewpoint of increasing the capacity. The reason is that if the content of graphite particles is high, the negative electrode can accept more Li ions that have migrated from the positive electrode. However, when the negative electrode mixture is prepared so as to contain a large amount of graphite particles, it may be difficult to uniformly mix the graphite particles and the LPS particles depending on the type of graphite particles.
[0009] In particular, when preparing a negative electrode composite by a dry method, the mixture of graphite particles and LPS particles is likely to be insufficient, and the quality of the mixture can affect the superiority or inferiority of the battery characteristics. Therefore, unless the above-mentioned mixture is improved, simply increasing the content of graphite particles cannot fully exert the role of LPS as a conductive path, and the desired discharge capacity cannot be obtained. The present invention has been made in consideration of the above problems, and aims to provide a method for producing a negative electrode composite for an all-solid-state battery that can achieve a high discharge capacity. [Means for solving the problem]
[0010] In order to achieve the above object, a method for producing a negative electrode composite for an all-solid-state battery according to the present invention includes the steps of: weighing out a sulfide all-solid-state electrolyte having a form of secondary aggregates made of an ion-conductive compound constituted by lithium, sulfur, and phosphorus, and graphite particles so as to obtain a predetermined blending ratio; dry-mixing the total amount of the weighed graphite particles with an amount of the weighed sulfide all-solid-state electrolyte in a range of 20% by mass or more and 40% by mass or less for a mixing time of 5 minutes or more; and adding the remainder of the weighed sulfide all-solid-state electrolyte in an amount in a range of 20% by mass or more and 40% by mass or less to the dry-mixed mixture, and dry-mixing each amount for a mixing time of 1 minute or less. Effect of the Invention
[0011] According to the present invention, it is possible to provide an all-solid-state battery having a high initial charge / discharge capacity and an excellent capacity retention rate in a cycle test. [Brief description of the drawings]
[0012] [Figure 1] 1 is a photograph of a battery evaluation cell used in an example of the present invention. [Diagram 2] 2 is a perspective view of the battery evaluation cell of FIG. 1 with the housing removed. FIG. [Diagram 3] FIG. 2 is a schematic vertical cross-sectional view of a battery evaluation cell with the housing removed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] 1.Negative electrode composite material for all-solid-state batteries Hereinafter, a negative electrode composite for an all-solid-state battery according to an embodiment of the present invention will be described. This negative electrode composite contains graphite particles and a sulfide solid electrolyte having ion conductivity, and the porosity of the negative electrode composite layer obtained by powder compacting of this negative electrode composite is 3% or less. Here, the porosity of the negative electrode composite layer can be obtained by the following method. That is, the cross section of the powder compacted negative electrode composite layer is processed using a CP (Cross Section Polisher) device, and five fields of view arbitrarily selected from the cross section thus mirror-finished are imaged by SEM. The SEM images of each obtained field are binarized to separate the voids from the other parts, and the ratio of the area occupied by the voids to the total area of the SEM image of each field is obtained, and the obtained area ratio is averaged over the five fields of view. This allows the porosity to be obtained.
[0014] As described above, by suppressing the porosity in the negative electrode mixture to 3% or less, it is possible to increase the initial charge / discharge capacity of an all-solid-state battery having the negative electrode mixture layer, and also to increase the capacity retention rate in a cycle test. That is, during charging and discharging of an all-solid-state battery, Li ions are inserted into or removed from the crystalline layer of the graphite particles by moving through the LPS, which plays the role of an ion conduction path in the negative electrode mixture. Therefore, when the contact between the graphite particles and the surrounding LPS particles is reduced, the ratio of voids present at their interface (sometimes expressed as the graphite particle / LPS interface) increases, and when the porosity in the negative electrode mixture layer exceeds 3%, the contact area between the graphite particles and the LPS particles becomes too small, preventing good movement of Li ions, and making it difficult for Li ions to be inserted and removed from the graphite particles. That is, graphite particles that do not contribute to charging and discharging are excessively present in the negative electrode mixture layer, and the charge / discharge capacity is significantly reduced.
[0015] As mentioned above, the reason for the formation of voids at the graphite particle / LPS interface is believed to be that the graphite particles are not sufficiently mixed with the LPS particles when preparing the negative electrode composite, so that the LPS particles are not sufficiently packed around the graphite particles during powder compaction. In other words, since LPS particles generally have very poor fluidity, it is difficult to obtain a uniform mixture when mixing graphite particles with LPS particles to prepare the negative electrode composite.
[0016] Under the above circumstances, we conducted intensive research to suppress the porosity in the negative electrode composite layer to 3% or less by minimizing the generation of voids at the graphite particle / LPS interface, and found that by using a mixture of at least two types of LPS particles, namely fine particles and particles with a diameter larger than the fine particles, the mixability of the graphite particles and the LPS particles can be improved and the porosity can be suppressed. Specifically, the porosity can be suppressed by mixing the LPS particles constituting the negative electrode composite so that the ratio of fine particles with an average particle diameter of 2μ to 5μm is 20% by mass to 40% by mass, and the ratio of large particles with an average particle diameter of 40μm to 60μm is 20% by mass to 40% by mass, of the total amount of LPS particles.
[0017] As described above, by using LPS particles containing at least 2-5 μm fine particles and 40-60 μm large particles, the contact state between the graphite particles and the LPS particles is good when compacted, and voids are unlikely to occur at the graphite particle / LPS interface, so that the void ratio in the negative electrode mixture layer can be reduced to 3% or less. As a result, the contact area of the interface between the graphite particles and the solid electrolyte particles constituting the negative electrode mixture layer is sufficiently secured, so that countless ion conduction paths are formed in the negative electrode mixture layer, and the utilization rate of the graphite particles can be increased. As a result, the charge / discharge capacity of the all-solid-state battery can be increased, and the discharge capacity retention rate during cycle testing can also be improved.
[0018] In the negative electrode mixture according to the embodiment of the present invention, the graphite particles constituting the negative electrode mixture further have an average flatness of 0 or more and less than 0.3, a particle size distribution D50 of 8 μm or more and 13 μm or less, and a BET value of 1 m 2 / g or more 3m 2 By using graphite particles that satisfy these requirements, the contact state between the graphite particles and the LPS particles can be further improved when the graphite particles are compacted.
[0019] If the average flattening ratio, which is a characteristic related to the shape of the graphite particles, is 0.3 or more, many irregularly shaped graphite particles will be included, which will hinder the smooth flow of the LPS particles when forming the negative electrode composite layer by powder compaction, making it easier for voids to form around the graphite particles where the LPS particles are not filled in. Conversely, as the average flattening ratio of the graphite particles approaches zero, the shape will change from irregular to spherical, improving the packing of the LPS particles around the graphite particles even if the flowability of the LPS particles is poor.
[0020] The average flattening of graphite particles can be calculated by the following formula 1. Here, f is the average flattening, a is the major axis of a single particle, and b is the minor axis of a single particle. These radii were calculated by taking images of five arbitrarily selected fields of the cross section or surface of a group of graphite particles using an SEM, measuring the major and minor radii of five arbitrarily selected graphite particles from each SEM image, and averaging the results. [Formula 1] f=1-b / a
[0021] If the particle size distribution D50, which is a characteristic related to the average particle size of graphite particles, is less than 8 μm, the graphite particles are too fine and therefore less dispersible when mixed with LPS particles, which makes it easier for voids to form around the graphite particles. In other words, if the graphite particles are too fine, they tend to aggregate with each other, resulting in an increase in LPS particles that do not conduct ions due to insufficient contact area with LPS particles and graphite particles that do not insert or release Li ions. Conversely, if the particle size distribution D50 exceeds 13 μm, the number of graphite particles per unit thickness of the negative electrode mixture layer decreases, resulting in a decrease in charge / discharge capacity. The particle size distribution D50 of the graphite particles was determined using a laser diffraction method in which a laser was irradiated onto graphite particles dispersed in a liquid to obtain refracted and scattered light.
[0022] The BET value, which is a characteristic related to the specific surface area of graphite particles, is 1m 2 If the BET value is less than 3m / g, the graphite particles have less chance to come into contact with the LPS particles during mixing to prepare the negative electrode composite, resulting in poor mixing and making it difficult for the LPS particles to adhere to the graphite particle surfaces, which makes it easier for voids to form at the graphite particle / LPS interface during powder compaction. 2 If the BET value exceeds 1 / g, gas components and moisture are excessively adsorbed onto the surface of the graphite particles, which can cause the battery characteristics to become unstable and can make it difficult to obtain a high capacity. The BET value is obtained using the BET equation based on the gas adsorption method (nitrogen adsorption method).
[0023] Although it is possible to achieve a porosity of 5% or less in the negative electrode mixture layer by simply specifying the above-mentioned graphite particle properties, namely, the average flatness, particle size distribution D50, and BET value, in order to further improve the properties of all-solid-state batteries, it is desirable to have a porosity of 3% or less, and it has been difficult to achieve a porosity of 3% or less by simply specifying the above-mentioned graphite particle properties. Although reducing the porosity from 5% to 3% is a small amount in terms of numbers, the voids in the negative electrode mixture layer are mainly voids that occur at the graphite particle / LPS interface, and the size of the voids is often about 5 to 10 μm, so it has generally been extremely difficult to reduce the porosity from 5% to 3%.
[0024] For example, even when spherical graphite particles are used, small voids may remain at the interface, and so we conducted extensive research, thinking that there must be some other reason for the poor mixability of graphite and LPS particles in addition to the poor fluidity of the LPS particles mentioned above. As a result, we focused on the fact that when graphite particles and LPS particles are mixed to produce a negative electrode composite, LPS does not always adhere to the surface of the graphite particles. In other words, after mixing the graphite particles and LPS particles, the particles may separate at a microscopic level, and we thought that this was the cause of preventing a reduction in the porosity.
[0025] Therefore, the inventors further studied not only the properties of graphite particles but also LPS, which is likely to adhere to the surface of graphite particles, and found that when LPS particles are synthesized by the mechanical milling method described below, they are generated in the form of secondary aggregates with a particle size of about 60 to 100 μm, which is the cause of insufficient adhesion to the surface of graphite particles and insufficient mixing with graphite particles. In this case, it is thought that the mixability can be improved by crushing the LPS particles in the form of secondary aggregates, but the secondary aggregates of LPS are easily deteriorated when mechanically mixed or crushed to obtain single particles, and for example, the ionic conductivity can be significantly reduced when the mixing time is extended.
[0026] Therefore, two types of LPS particles with different particle sizes, which were produced by changing the crushing time, were prepared, and these were mixed with graphite particles to produce a negative electrode composite. As a result, it became possible to reduce the porosity in the negative electrode composite layer to 3% or less. In other words, since the voids generated at the graphite particle / LPS interface are only a small amount in volume, the LPS particles that enter the gaps do not need to be the entire amount of LPS particles mixed into the negative electrode composite. In addition, in order to adhere to the surface of graphite particles, if the LPS particles adhere along the uneven surface formed on the surface of the graphite particles, it is preferable that the LPS particles are fine powders, but in this case, it is sufficient to have an amount that covers one layer of the surface area of the graphite particles.
[0027] Therefore, for example, by gradually adding LPS particles to graphite particles during crushing in at least two separate batches, it is possible to mix finer LPS particles obtained by mixing for a long period of time with larger LPS particles that are less likely to deteriorate obtained by mixing for a short period of time with the graphite particles. This makes it possible to produce a negative electrode mixture layer that has a low porosity at the graphite particle / LPS interface while keeping the content of LPS particles damaged by mixing to a minimum.
[0028] Specifically, it is preferable that the total amount of LPS particles used as the negative electrode mixture contains 20% by mass to 40% by mass of fine particles with an average particle diameter of 2 μm to 5 μm, which are more finely pulverized, and 20% by mass to 40% by mass of large particles with an average particle diameter of 40 μm to 60 μm, which are less damaged by mixing. By using a negative electrode mixture in which LPS particles containing fine particles and large particles each having a predetermined particle size range at a predetermined content rate are mixed with graphite particles, the porosity of the negative electrode mixture layer after powder compaction can be suppressed to 3% or less, and an all-solid-state battery cell with excellent battery characteristics such as initial charge / discharge capacity can be manufactured.
[0029] 1. Method for manufacturing negative electrode mixture layer Next, an embodiment of a method for producing a negative electrode mixture layer according to the present invention will be described taking as an example a case in which lithium sulfide and diphosphorus pentasulfide are used as raw materials for the LPS particles.
[0030] 1.1 Graphite particles Natural graphite or artificial graphite can be used for the graphite particles constituting the negative electrode composite material. However, artificial graphite is preferable because it easily satisfies the above-mentioned average flatness, particle size distribution D50, and BET value characteristics, and MCMB (Meso-Carbon MicroBeads: spherical carbon particles) are particularly preferable. On the other hand, natural graphite is generally inferior in flatness because it is not spherical in shape, has a wide particle size distribution D50, and has a high BET value, so that the mixability with LPS particles is often not improved. In addition, amorphous carbon may be provided on the surface of the graphite particles to increase the insertion and removal of Li ions during charging and discharging. This makes it easier for the LPS particles to adhere to the surface of the graphite particles when the negative electrode composite material is mixed, making it possible to obtain a higher charge and discharge capacity.
[0031] 1.2LPS particles (1) Lithium sulfide (LiS) There is no particular restriction on lithium sulfide (Li2S), which is one of the raw materials of the LPS particles constituting the negative electrode composite material, but it is preferable to use an industrially produced commercially available product, and it is particularly preferable to use one with a purity of 99% or more. Lithium sulfide can be produced, for example, by the method described in Japanese Patent No. 3528866. This production method is a method in which hydrogen sulfide is blown into a charge liquid consisting of lithium hydroxide and an aprotic organic solvent placed in a reaction vessel, the lithium hydroxide and the hydrogen sulfide are reacted to produce lithium hydrosulfide, and the resulting reaction liquid containing lithium hydrosulfide is then subjected to a dehydrosulfidation treatment to produce lithium sulfide.
[0032] (2) Diphosphorus pentasulfide (P2S5) There are no particular restrictions on the phosphorus sulfide, which is the other raw material for the LPS particles that make up the negative electrode mixture, but it is preferable to use commercially available industrially produced diphosphorus pentasulfide (P2S5), which preferably has a purity of 99% or more.
[0033] (3) Mixture ratio When a general highly ion-conductive sulfide is produced, it is preferable to adjust the blending ratio of lithium sulfide to the total of the lithium sulfide and diphosphorus pentasulfide used as the starting materials so that it is within the range of 30 to 95 mol%. The specific blending ratio is appropriately determined depending on the application. For example, as in the 70Li2S-30P2S5 solid electrolyte produced using starting materials in which the blending ratio of lithium sulfide and diphosphorus pentasulfide is 70:30 on a molar basis, when the blending ratio of lithium sulfide is 70 mol% or less, the highly ion-conductive sulfide becomes glassy, and it becomes necessary to perform heat treatment when producing the highly ion-conductive sulfide. In addition, since it is unstable in the air atmosphere, it becomes difficult to handle during synthesis, storage, etc. Therefore, the blending ratio of lithium sulfide in the starting material of LPS, which is the highly ion-conductive sulfide, is preferably within the range of 75 to 80 mol%.
[0034] (4) LPS synthesis LPS can be obtained by synthesizing the starting materials lithium sulfide and diphosphorus pentasulfide mixed in the above-mentioned ratio. This synthesis is preferably performed by using a mechanical milling method. The mechanical milling method is a processing method in which a powder to be treated is loaded into a milling container of a mixing device together with a number of metal or ceramic balls, which are media that physically act on the powder, and the media move with the rotation and vibration of the milling container, thereby applying physical forces such as mixing, stirring, and impact to the powder.
[0035] The mixing device used in this mechanical milling method is not particularly limited as long as it can charge and mix the above-mentioned media, which perform the action of uniformly mixing, stirring, etc. on the powder to be treated, into a milling container, and general powder mixing devices such as planetary ball mills, rotary ball mills, and attritors can be used, but among these, planetary ball mills are particularly preferred. In planetary ball mills, the random movement of balls due to planetary motion promotes uniform mixing of the powder to be treated and gives large reaction energy to the powder, so that a driving force that promotes the synthesis reaction can be applied very efficiently.
[0036] Thus, unlike two-step processing in which multiple starting material powders are first mixed and then the resulting mixed powder is heat-treated, mechanical milling generates heat by the impact of rapidly moving balls, which makes it possible to simultaneously mix multiple starting material powders uniformly and to cause rapid localized chemical reactions, making it suitable for producing special high ionic conductors.
[0037] In the mechanical milling method, it is preferable to control the atmosphere in the milling container. For example, when the starting material is filled in a milling container made of SUS with the inner surface covered with ZrO2, it is preferable to make the milling container an inert gas atmosphere. For this reason, it is preferable to perform the filling operation in the milling container in a glove box filled with an inert gas such as Ar gas, N2 gas, or He gas. However, since it is usually not possible to put the mechanical milling device body in the glove box, after filling, the milling container is taken out of the glove box and milling such as mixing is performed in an environment exposed to the outside air atmosphere. For this reason, it is preferable that the cover of the milling container is structured so that the inside of the milling container can be airtightly sealed by a packing made of silicone.
[0038] The reason why it is preferable to seal the inside of the milling container airtight as described above is that sulfides start to deteriorate immediately when exposed to the air, and are particularly vulnerable to moisture, and if the gas in the milling container contains even a small amount of moisture, decomposition occurs and H2S gas is generated. Therefore, it is preferable that the inert gas filling the milling container is sealed in the milling container in a dry state and hermetically sealed with a packing as described above so that it does not leak to the outside. The state in which the gas leaks to the outside can also be said to be a state in which the air containing moisture from the outside air enters the milling container. In order to seal the dry inert gas in the milling container as described above, it is preferable to control the dew point in the glove box in which the above filling work is performed to be preferably -70°C dp or less, more preferably -80°C dp (moisture content 0.5 ppm) or less.
[0039] 1.3 Powder compaction The negative electrode composite layer for an all-solid-state battery can be produced by compacting the negative electrode composite obtained by mixing the graphite particles and the LPS particles. In the compaction of the negative electrode composite, it is preferable to laminate the positive electrode composite, the solid electrolyte, and the negative electrode composite in this order into three layers, and pressurize them in the lamination direction to simultaneously form a three-layered compact. It is desirable for the compaction of the negative electrode composite to have good moldability, but since the negative electrode composite of the embodiment of the present invention does not contain a resin binder, the moldability depends on the adhesiveness of the LPS particles.
[0040] In order to fully utilize the adhesive properties of the LPS particles, it is preferable to mix the graphite particles with the LPS particles in a ratio of 50 to 70 parts by mass per 100 parts by mass of the graphite particles and the LPS particles combined, which makes it possible to form a green compact with excellent shape retention and no defects or cracks when the graphite particles and the LPS particles are compressed together.
[0041] On the other hand, if the graphite particles are mixed in an amount of more than 70 parts by mass relative to 100 parts by mass of the graphite particles and LPS particles, the shape retention may decrease and cracks may occur. If cracks occur in the compact in this way, it may cause an increase in resistance, which may decrease the charge / discharge capacity. On the other hand, if the graphite particles are mixed in an amount of less than 50 parts by mass relative to 100 parts by mass of the graphite particles and LPS particles, the content of carbon derived from the graphite particles in the negative electrode composite layer obtained after compaction is too small, so that the Li ions sent from the positive electrode active material cannot be sufficiently accepted, and in this case, the charge / discharge capacity may also decrease. As a countermeasure in this case, it is possible to compensate for the amount of carbon by increasing the thickness of the negative electrode composite layer, but increasing the thickness of the negative electrode composite layer increases the resistance by that amount, so this is not a preferable countermeasure.
[0042] As described above, the LPS particles immediately after synthesis by mechanical milling preferably have the form of secondary aggregates (secondary particles) with an average particle size of 60 to 100 μm, which are formed by aggregation of primary particles with an average particle size of 0.5 to 2 μm. It is preferable to adopt a dry mixing method for mixing the LPS particles consisting of the secondary aggregates with the graphite particles. The reason is that in the wet mixing method, the solvent used for mixing and the LPS may react violently and change in quality, whereas in the dry mixing method, such a problem does not occur. Note that the LPS particles after synthesis are weak against friction and impact generated during mixing, and MCMB may also be crushed or distorted when force is applied, which may cause a decrease in battery characteristics, so a mixing method that does not damage the LPS particles and graphite particles as much as possible is preferable. For this reason, hand mixing using a mortar described later is preferable, but when mixing by mechanical milling such as a planetary ball mill as in the case of producing the LPS particles, it is desirable to mix at the minimum rotation speed for as short a time as possible.
[0043] A more preferable mixing method in terms of not causing the above damage is the mixing method using a mortar, and by appropriately adjusting the force applied to the powder during mixing and the mixing time, mixing can be performed with almost no damage. However, when the LPS particles and graphite particles, each weighed out in the above desired mixing ratio, are added to a mortar and mixed with a pestle for 10 minutes or more, the LPS particles are easily crushed and finely pulverized, but are damaged by this crushing. When the LPS particles are damaged in this way, the adhesiveness inherent to the sulfide that LPS has decreases, and it becomes difficult to function as a binder, so that there is a risk of many voids being generated at the interface between the graphite particles and the LPS particles when the negative electrode mixture layer is molded. In addition, the ionic conductivity of the LPS itself decreases, so that the resistance of the negative electrode mixture layer made using it increases, and the battery capacity may decrease. Furthermore, since the activity of the LPS particles increases when they are finely pulverized, they deteriorate due to trace amounts of moisture and oxygen in the environment, so their shelf life decreases and they cannot be prepared in advance.
[0044] Therefore, in an embodiment of the present invention, LPS particles and graphite particles are mixed using a mortar in the following manner. That is, first, LPS particles and graphite particles are weighed out so as to obtain the desired blending ratio. Next, the total amount of the weighed graphite particles and 20% by mass to 40% by mass of the total amount of the weighed LPS particles are charged into a mortar, and a first mixing is performed using a pestle at a speed of about 30 to 120 revolutions per minute so as to mix uniformly throughout, while being careful not to press them. Secondary aggregates of LPS particles are easily broken down by mixing with a pestle for about 5 minutes, and primary particles and secondary aggregates (secondary particles) having a particle size of about 2 μm to 5 μm are obtained, so this first mixing is performed for 5 minutes.
[0045] This makes it easier for the LPS particles to adhere to the surface of the graphite particles, so that the surface can be covered with LPS particles. Note that the LPS particles will be somewhat damaged during the first mixing process, but this disadvantage is outweighed by the benefit of the reduced porosity at the graphite particle / LPS interface, which has a greater effect on increasing capacity. However, by making the ratio of fine particles to the total amount of LPS particles weighed out above as small as possible, the adverse effects of the damage described above are limited to only those that fill the voids.
[0046] After the first mixing, all the remaining LPS particles are added to the mixture in the mortar after the first mixing in an amount ranging from 20% to 40% by mass. Then, for each addition, mixing is performed for 1 minute with a pestle in the same manner as above. In this way, the LPS particles added during the second and subsequent mixing are less likely to be damaged because of the short mixing time, and therefore the LPS particles added during the second and subsequent mixing hardly have a negative effect on the characteristics of the negative electrode mixture layer. However, because the mixing time is short, the disintegration cannot be sufficiently carried out, and as a result, the particle size of the LPS particles is about 40 μm to 60 μm, which is the extent to which the secondary aggregates are slightly disintegrated.
[0047] That is, in the manufacturing method of the negative electrode composite material according to the embodiment of the present invention, fine LPS particles having a particle diameter of 2 μm to 5 μm are formed by a first mixing for 5 minutes, and the surface of the graphite particles is covered with these fine LPS particles, and by mixing for 1 minute each from the second time onwards, relatively large LPS particles having a particle diameter of 40 μm to 60 μm, which are less damaged, are mixed with the graphite particles whose surfaces are covered with the fine LPS particles. This makes it possible to suppress the porosity in the negative electrode composite material layer formed by the powder compaction to 3% or less due to the synergistic effect of the improvement in the filling of the voids at the graphite particle / LPS interface by the fine LPS particles and the densification during powder compaction by the relatively large LPS particles that maintain their adhesiveness, and as a result, a high-capacity all-solid-state battery can be manufactured.
[0048] The average particle size of the secondary aggregates of LPS particles (also called the average aggregate size) was calculated by taking images of five randomly selected fields of view using an SEM, measuring the outer diameters of five randomly selected secondary aggregates from each SEM image, and averaging them. This is because the laser diffraction method, which uses a general laser to irradiate the sample and obtain refracted and scattered light, cannot be used because most of the water or organic solvents used react chemically with LPS and change their properties. It is also possible to calculate the particle size from the BET value, but this has problems such as the deterioration of LPS during handling.
[0049] When evaluating the charge / discharge capacity of an all-solid-state battery prepared by laminating the above-mentioned negative electrode composite with a solid electrolyte made of LPS particles used in the negative electrode composite and a separately prepared positive electrode composite, samples of the negative electrode composite, positive electrode composite, and solid electrolyte for evaluation are compressed into a green compact and measured. The thickness of the green compact compressed from each sample is preferably about 100 to 200 μm for the positive electrode composite layer and the negative electrode composite layer, and about 300 to 500 μm for the solid electrolyte layer, taking into consideration the balance between the shape retention during the green compact (no breaks or cracks during compaction) and the resistance during the green compact.
[0050] When forming a negative electrode composite layer from the negative electrode composite, for example, the negative electrode composite is filled in a mold having an inner diameter of 10 mm, and a pressure of about 2 to 4 kN is applied in the thickness direction to perform temporary powder compaction, and then high pressure powder compaction is performed. During this high pressure powder compaction, the positive electrode composite, the solid electrolyte, and the negative electrode composite are stacked in this order from the bottom, and a pressure of 40 kN is applied in this stacking direction to simultaneously compact the three layers. This allows a three-layer integral compact to be obtained. The three-layer integral compact thus formed is placed in a commercially available battery cell case (sealed type: not exposed to air) and incorporated to produce an all-solid-state battery. Next, the present invention will be described in more detail based on the following examples and comparative examples, but the present invention is not limited to these examples. EXAMPLES
[0051] [Example 1] (LPS synthesis) A total of 80 g of ZrO2 balls (ball diameter 4 mm) were placed in a milling container (volume 45 ml: inner wall made of ZrO2) attached to a mechanical milling device (PL-7) manufactured by Fritsch, and dried in vacuum at 100° C. This dried milling container was placed in a glove box (−80° C. dp) in an Ar atmosphere, and further dried overnight.
[0052] In the milling container in the glove box, 0.3828 g of lithium sulfide (Li2S) manufactured by Junsei Chemical Co., Ltd. and 0.6172 g of diphosphorus pentasulfide (P2S5) manufactured by Sigma-Aldrich were charged and sealed. In this case, the molar ratio of lithium sulfide and diphosphorus pentasulfide was Li2S:P2S5=75:25. After the sealing, the milling container was removed from the glove box and placed in the mechanical milling device (PL-7) manufactured by Fritsch Co., Ltd. installed in a dry room (ambient temperature 22°C:-45°Cdp), and mechanical milling was performed at 510 rpm for 20 hours. After the mechanical milling was completed, the milling container was returned to the glove box, the lid of the milling container was opened, and the LPS in the form of powder produced by synthesis was taken out and passed through a 100 mesh sieve.
[0053] The obtained undersieve LPS particles were analyzed by a non-exposed-air Raman spectrometer (Horiba, Ltd.) (microscopic laser Raman spectrometer LabRAM HR-800, light source: Ar laser (514 nm excitation), excitation power: 0.2 mW, measurement range: 100–4000 cm -1 ), it was confirmed that the LPS particles contained a Li3PS4 phase. In order to confirm the degree of disintegration when the LPS particles synthesized by the mechanical milling method were mixed in a mortar, 120 mg of the LPS particles that fell through the sieve were sampled and divided into six samples, and five of these samples were separately placed in a mortar and disintegrated in the mortar for 1 minute, 3 minutes, 5 minutes, 10 minutes, and 20 minutes, respectively. After that, the average value of five aggregate sizes (secondary particle sizes) in the SEM images was calculated for each of the six samples, including these five samples and one undisintegrated sample.
[0054] As a result, the uncrushed sample in the synthesized state had an average particle size of 89 μm, the sample with a 1 minute crushing time had an average particle size of 53 μm, the sample with a 3 minute crushing time had an average particle size of 19 μm, and the sample with a 5 minute crushing time had an average particle size of 3 μm. On the other hand, the sample with a 10 minute crushing time had re-aggregated fine powder, reaching an average particle size of 21 μm. The sample with a 20 minute crushing time had re-aggregated in the same way as the 10 minute crushing time sample, and had an average particle size of 26 μm.
[0055] (Preparation of negative electrode mixture) In a mortar in a glove box (-80℃ dp) with an Ar atmosphere, the average flatness of the particles was 0.03, the particle size distribution D50 was 10.2μm, and the BET value was 1.2m. 280 mg of graphite particles (PG11A) manufactured by Rongtan Electronic Materials Co., Ltd., with a particle size of 1 / g, was added, and 20 mg of the LPS particles that fell under the sieve were added. The first mixing was performed for 5 minutes at a rotation speed of 60 revolutions per minute using a pestle, while being careful not to press the particles. Next, 20 mg of the LPS particles that fell under the sieve were added to the mixture in the mortar after the first mixing, and the second mixing was performed for 1 minute using the same mixing method using a mortar. The addition of 20 mg of LPS particles and mixing for 1 minute were repeated two more times to perform the third and fourth mixing. As a result, a powder-like negative electrode mixture was produced as an intermediate product in which graphite particles and LPS particles were mixed at a ratio of 50:50 by mass.
[0056] (Preparation of positive electrode mixture) A lithium nickel composite oxide powder prepared in advance by a known technique was used as the positive electrode active material. That is, nickel oxide powder containing Ni as the main component and lithium hydroxide were mixed and fired to obtain Li 1.090 Ni 0.76 Co 0.14 Al 0.10 A powder of lithium nickel composite oxide (hereinafter referred to as NCA particles) was prepared as the positive electrode active material represented by 1002. The average particle size of the obtained NCA particles was measured by a laser diffraction method and found to be 10.6 μm. The specific surface area was measured by the BET method and found to be 0.16 m. 2 120 mg of the NCA particles and 80 mg of the LPS particles that fell under the sieve were placed in a mortar in a glove box (-80°C dp) with an Ar atmosphere, and gently mixed with a pestle at a rotation speed of 60 revolutions per minute for 10 minutes, taking care not to press the particles.
[0057] (Preparation of powder compacts) In a glove box (-80°C dp) in an Ar atmosphere, 60 mg of the above-mentioned undersized LPS powder was charged into a cylindrical mold with an inner diameter of 10 mm, and the solid electrolyte layer was prepared by preforming at 2 kN. 15 mg of the powder-like negative electrode composite prepared above was stacked on this solid electrolyte layer, and preforming was performed again at 2 kN. The obtained two-layered compact was turned over, and 20 mg of the powder of the positive electrode composite prepared above was deposited on the opposite side of the both sides of the solid electrolyte layer from the side of the preformed negative electrode composite layer, and then it was molded at 40 kN. As a result, a three-layered compact consisting of a positive electrode composite layer / solid electrolyte layer (SE layer) / negative electrode composite layer was prepared. This compact was placed in a sealed battery evaluation cell (KP-solidCell) manufactured by Hosen Co., Ltd. as shown in Figures 1 and 2, and the evaluation cell was assembled by restraining it with a torque of 7 Nm. As shown in FIG. 3, this evaluation cell has an integrally structured green compact 10 consisting of a negative electrode composite layer 11, a solid electrolyte layer (SE layer) 12, and a positive electrode composite layer 13, which can be pressed in the stacking direction with a predetermined restraining force by an upper electrode 21 and a lower electrode 22 within a cylindrical insulating tube 20.
[0058] (Evaluation of battery characteristics and measurement of porosity of negative electrode mixture layer) The terminals of the obtained evaluation cell were connected to a charge / discharge device (HJ-SD8) manufactured by Hokuto Denko Corporation, and the initial discharge capacity was determined at a voltage range of 2.37 to 4.17 V_CC (0.1 C = 19 mAh / g), which was 124 mAh / g. In addition, as the discharge capacity retention rate in a cycle test, charge / discharge was repeated 20 times under the same conditions as the initial charge / discharge, and the change in capacity between the initial discharge and the 20th repetition was examined, which was 92%. After evaluating the battery characteristics, the porosity of the negative electrode composite layer was determined as an average of SEM images of five fields of view as described above, which was 2.4%.
[0059] [Example 2] A negative electrode composite material was prepared as an intermediate product in which graphite particles and LPS particles were mixed at a ratio of 50:50 by mass in the same manner as in Example 1, except that 30 mg of LPS particles were charged instead of 20 mg in the first and third mixings, and the fourth mixing was not performed. This was used to prepare a three-layer integral compact consisting of a positive electrode composite layer / solid electrolyte layer (SE layer) / negative electrode composite layer in the same manner as in Example 1. Furthermore, this compact was placed in a sealed battery cell in the same manner as in Example 1 to assemble an evaluation cell, and then the battery characteristics were evaluated and the porosity of the negative electrode composite layer was measured in the same manner as in Example 1. As a result, the initial discharge capacity was 123 mAh / g, the discharge capacity retention rate was 91%, and the porosity of the negative electrode composite layer was 2.6%.
[0060] [Example 3] Average flatness is 0.24, particle size distribution D50 is 8.7μm, BET value is 1.2m 2 A negative electrode composite material was prepared as an intermediate product in which the graphite particles and the LPS particles were mixed at a ratio of 50:50 by mass in the same manner as in Example 1, except that graphite particles (PW8A) manufactured by Rongtan Electronic Materials Co., Ltd., which has a particle size of 1.0 μm / g, were used, and a three-layer integral structure compact consisting of a positive electrode composite layer / solid electrolyte layer (SE layer) / negative electrode composite layer was prepared using this in the same manner as in Example 1. Furthermore, this compact was placed in a sealed battery cell in the same manner as in Example 1 to assemble an evaluation cell, and then the battery characteristics were evaluated and the porosity of the negative electrode composite layer was measured in the same manner as in Example 1. As a result, the initial discharge capacity was 120 mAh / g, the discharge capacity retention rate was 90%, and the porosity of the negative electrode composite layer was 2.9%.
[0061] [Comparative Example 1] Average flatness is 0.42, particle size distribution D50 is 5.3μm, BET value is 2.4m 2A negative electrode composite material was produced as an intermediate product in which the graphite particles and the LPS particles were mixed at a ratio of 50:50 by mass in the same manner as in Example 1, except that 80 mg of graphite particles (AC1) manufactured by Rongtan Electronic Materials Co., Ltd., having a particle size of 100 μm / g and 80 mg of the undersized LPS particles used in Example 1 were charged into a mortar and mixed once for 10 minutes using a similar mixing method using a pestle. Using this, a three-layer integral compact consisting of a positive electrode composite layer / solid electrolyte layer (SE layer) / negative electrode composite layer was produced in the same manner as in Example 1. Furthermore, this compact was placed in a sealed battery cell in the same manner as in Example 1 to assemble an evaluation cell, and then the battery characteristics were evaluated and the porosity of the negative electrode composite layer was measured in the same manner as in Example 1. As a result, the initial discharge capacity was 104 mAh / g, the discharge capacity retention rate was 79%, and the porosity of the negative electrode composite layer was 6.7%.
[0062] [Comparative Example 2] Graphite particles (AC1) with an average flatness of 0.37, particle size distribution D50 of 11.8 μm, and BET value of 4.4 m 2 A negative electrode composite material was prepared as an intermediate product in which graphite particles and LPS particles were mixed at a ratio of 50:50 by mass in the same manner as in Comparative Example 1, except that graphite particles (OMAC-R) manufactured by Osaka Gas Chemicals, which has a particle size of 1000 nm / g, were used. Using this, a three-layer integral structure compact consisting of a positive electrode composite layer / solid electrolyte layer (SE layer) / negative electrode composite layer was prepared in the same manner as in Example 1. Furthermore, this compact was placed in a sealed battery cell in the same manner as in Example 1 to assemble an evaluation cell, and then the battery characteristics were evaluated and the porosity of the negative electrode composite layer was measured in the same manner as in Example 1. As a result, the initial discharge capacity was 105 mAh / g, the discharge capacity retention rate was 80%, and the porosity of the negative electrode composite layer was 5.3%. The measurement results of the above-mentioned Examples 1 to 3 and Comparative Examples 1 to 2 are summarized in Table 1 below.
[0063] [Table 1] [Explanation of symbols]
[0064] 10 Powder Compacts 11 Negative electrode composite layer 12 Solid electrolyte layer (SE layer) 13 Positive electrode mixture layer 20 Insulating tube 21 Upper electrode 22 Lower electrode
Claims
[Claim 1] A method for producing a negative electrode composite material, comprising the steps of: weighing out a sulfide all-solid-state electrolyte having a form of secondary aggregates made of an ion-conductive compound constituted by lithium, sulfur, and phosphorus; and graphite particles so as to obtain a predetermined blending ratio; dry-mixing the total amount of the weighed graphite particles with an amount of the weighed sulfide all-solid-state electrolyte in a range of 20% by mass or more and 40% by mass or less for a mixing time of 5 minutes or more; and adding the remainder of the weighed sulfide all-solid-state electrolyte in an amount in a range of 20% by mass or more and 40% by mass or less to the dry-mixed mixture, and dry-mixing each of the weighed amounts for a mixing time of 1 minute or less.
Citation Information
Patent Citations
Method of manufacturing composite active material
JP2015220196A
Negative electrode for all-solid battery
JP2017054720A
All-solid-state battery
WO2014016907A1
Solid electrolyte glass and lithium ion battery using the same
JP2013155087A
Negative electrode mixture
JP2014203545A