Polymer, compact, monomer, and producing method thereof

Polymers with anthracene and siloxane structures are developed for reversible polymerization and depolymerization, facilitating recyclability and adaptable physical properties, addressing the limitations of existing polymers.

JP2024161730AInactive Publication Date: 2024-11-20NAT UNIV CORP KUMAMOTO UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023076706
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-20
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polymers lack the ability to be polymerized by photopolymerization, recovered as monomers, and reused, limiting their recyclability and adaptability to different applications.

Method used

Development of polymers and monomers with anthracene and siloxane structures that can be polymerized by light irradiation, depolymerized by heat or light, and modified through equilibration reactions, allowing for reversible polymerization and monomer recovery.

Benefits of technology

The developed polymers can be efficiently polymerized and depolymerized, enabling resource recycling and adaptable physical properties through controlled chain length adjustments, suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024161730000001_ABST
    Figure 2024161730000001_ABST
Patent Text Reader

Abstract

To provide a polymer capable of forming a compact using a novel monomer and a producing method thereof.SOLUTION: A method for producing a polymer having a repeating structure between a siloxane structure derived from a siloxane-based compound and a dimeric structure of anthracene comprising a polymerization step in which the monomer having anthracene structures at a plurality of ends of a structure of a siloxane-based compound is irradiated with light for polymerizing monomers to dimerize the anthracene structures between the monomers. A method for producing a polymer having an equilibration reaction step for causing the equilibration reaction by mixing a raw material polymer having a repeating structure between a structure of the siloxane-based compound and a dimer structure of anthracene, an improving siloxane-based compound, and a catalyst.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a monomer having a siloxane compound structure and an anthracene group. The present invention also relates to a polymer using this monomer. The present invention also relates to a molded article containing this polymer. The present invention also relates to a method for producing them. [Background technology]

[0002] Various polymers and other materials have been developed and put to practical use. Polymers also exhibit a variety of physical properties depending on their specific structures, and their manufacturing methods and recyclability also vary. There is a daily demand for the development of new polymers and other materials in response to demand for various applications and changes in social conditions.

[0003] The present inventors have developed, for example, a necklace-type polymer in which bifunctional cage-type silsesquioxanes (POSS) are alternately linked by dimethylsiloxane chains. Patent Document 1 discloses a polysiloxane composite comprising a substance selected from inorganic substances and organic substances, and a polysiloxane containing a cage-type silsesquioxane repeating unit represented by a specific formula and a chain-type siloxane repeating unit represented by a specific formula, which is bonded to the surface of the substance, and the polysiloxane is bonded to the surface of the substance via the chain-type siloxane represented by the specific formula.

[0004] These polysiloxane composites, also known as necklace-type polymers, are being developed into practical applications that take advantage of their heat resistance and adhesive properties. Necklace-type polymers are made by alternating bulky rigid units and soft siloxane chains. This gives them an amorphous structure that realizes homogeneous dispersion of functional nanounits, and allows systematic control of the polymer's physical properties (glass transition temperature and flexibility) by adjusting the length of the siloxane chains that connect the hard units.

[0005] As a study on the reactivity of compounds and materials, Non-Patent Document 1 relates to a study using anthracene dimerization for crosslinking silicone polymers. This involves introducing anthracene into the side chain of polysiloxane to realize a reversible crosslinking system that utilizes the photodimerization and thermal monomerization of anthracene. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent Publication No. 2021-178892 [Non-patent literature]

[0007] [Non-Patent Document 1] Light- and heat-triggered reversible luminescent materials based on polysiloxanes with anthracene groups, D. Han, et. al., RSC Adv.,2017, 7, 56489. Summary of the Invention [Problem to be solved by the invention]

[0008] The present inventors have studied how to provide a material with different physical properties from the conventional necklace-shaped polymers and the like described in Patent Document 1 and the like. Through this study, they have discovered new polymers and monomers and the like. The present application aims to provide a polymer that can be polymerized by photopolymerization or the like, can be recovered as a monomer, and is suitable for reuse, and a molded product and the like that uses this polymer. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the following invention meets the above object, thereby completing the present invention.

[0010] <1> A method for producing a polymer having a repeating structure of a siloxane structure derived from a siloxane compound and an anthracene dimer structure, the method comprising: a polymerization step of irradiating a monomer having an anthracene structure at multiple ends of a siloxane compound structure with light for polymerizing the monomer, thereby dimerizing the anthracene structures between the monomers. <2> A method for producing a polymer, comprising an equilibration reaction step of mixing a raw material polymer having a repeating structure of a siloxane compound structure and an anthracene dimer structure, a modifying siloxane compound, and a catalyst to carry out an equilibration reaction. <3> The above <1> or <2> 2. A method for producing a molded article, comprising the step of molding a molded article containing a polymer produced by the method for producing a polymer according to claim 1. <4> A polymer having a repeating structure of a siloxane structure derived from a siloxane compound and an anthracene dimer structure. <5> A method for producing a monomer, comprising: a depolymerization step of heating and / or irradiating a polymer having a repeating structure of a siloxane-based compound structure and a plurality of anthracene dimer structures to dissociate the anthracene dimer structures of the polymer, thereby depolymerizing the polymer and obtaining a monomer of the polymer. <6> A reaction step of mixing a reactive anthracene compound with a siloxane compound having a plurality of reactive terminals and reacting the reactive terminals of the siloxane compound with the reactive groups of the reactive anthracene compound is included. A method for producing a monomer having an anthracene structure derived from the anthracene compound at a plurality of ends of a siloxane structure derived from the siloxane compound. <7> The reactive anthracene compound is vinylanthracene, the siloxane compound is polydimethylsiloxane, and the reaction step is carried out in the presence of a catalyst. <6> The manufacturing method described in <8> A method for producing a monomer, comprising an equilibration reaction step of mixing a raw material monomer having an anthracene structure derived from an anthracene compound at multiple ends of a siloxane structure derived from a siloxane compound, a modifying siloxane compound, and a catalyst to carry out an equilibration reaction. <9> A monomer having an anthracene structure at multiple ends of a siloxane compound structure. Effect of the Invention

[0011] The polymer of the present invention can be polymerized by photopolymerization or the like, and can be recovered as a monomer or the like, making it suitable for reuse. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a flow diagram of a manufacturing method of the present invention. [Diagram 2] FIG. 1 is a schematic diagram of a reaction for producing a necklace-shaped polymer according to the present invention using a monomer according to the present invention. [Diagram 3] FIG. 1 is a schematic diagram illustrating adjustment of polymer chain length by polymerization / depolymerization and ring-opening polymerization according to the present invention. [Figure 4] 1 is a graph showing the reaction time and molecular weight evaluation results in the polymerization examples of the examples. [Diagram 5] 1 is an image of a film-like molded product of the polymer, etc., produced in the examples. [Figure 6] 2 is a graph showing the evaluation results of monomers and polymers produced in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The following is a detailed description of the embodiments of the present invention, but the following description of the constituent elements is one example (representative example) of the embodiment of the present invention, and the present invention is not limited to the following content as long as the gist of the present invention is not changed. Note that in this specification, when the expression "~" is used, it is used as an expression including the numerical values ​​before and after it.

[0014] [Monomer of the present invention] The monomer of the present invention is a monomer having anthracene structures at multiple ends of the structure of a siloxane compound.

[0015] [First method for producing the monomer of the present invention] A first production method for a monomer of the present invention is a production method for a monomer having anthracene structures derived from the anthracene compound at multiple ends of a siloxane structure derived from the siloxane compound, the method comprising a reaction step of mixing a reactive anthracene compound with a siloxane compound having multiple reactive ends and reacting the reactive ends of the siloxane compound with reactive groups of the reactive anthracene compound.

[0016] [Second method for producing the monomer of the present invention] The second method for producing a monomer of the present invention is a method for producing a monomer, which includes an equilibration reaction step of mixing a raw material monomer having anthracene structures derived from an anthracene compound at multiple ends of a siloxane structure derived from a siloxane compound, a modifying siloxane compound, and a catalyst to carry out an equilibration reaction.

[0017] The monomer of the present invention can be used to produce the polymer of the present invention. In addition, the second method for producing the monomer of the present invention can change the siloxane structure by using the monomer of the present invention produced by the first method for producing the monomer of the present invention or the like as a raw material monomer, and can produce a monomer of the present invention having a new structure.

[0018] [Polymer of the present invention] The polymer of the present invention is a polymer having a repeating structure of a siloxane structure derived from a siloxane compound and an anthracene dimer structure.

[0019] [First method for producing the polymer of the present invention] A first method for producing a polymer of the present invention is a method for producing a polymer having a repeating structure of a siloxane structure derived from a siloxane-based compound and an anthracene dimer structure, the method comprising a polymerization step of irradiating a monomer having an anthracene structure at multiple ends of a siloxane-based compound structure with light for polymerizing the monomer, thereby dimerizing the anthracene structures between the monomers.

[0020] [Second method for producing the polymer of the present invention] The second method for producing a polymer of the present invention is a method for producing a polymer, which includes an equilibration reaction step of mixing a raw material polymer having a repeating structure of a siloxane compound structure and an anthracene dimer structure, a modifying siloxane compound, and a catalyst to carry out an equilibration reaction.

[0021] [Third method for producing the monomer of the present invention] The third method for producing a monomer of the present invention is a method for producing a monomer, comprising a depolymerization step of heating and / or irradiating a polymer having a siloxane compound structure and a plurality of anthracene dimer structures to dissociate the anthracene dimers in the polymer, thereby depolymerizing the polymer and obtaining a monomer of the polymer.

[0022] The polymer of the present invention can be polymerized by photopolymerization or the like using the monomer of the present invention. The polymer of the present invention can also be depolymerized to recover the monomer of the present invention. These polymerization and depolymerization are reversible, and the polymer of the present invention and the monomer of the present invention are suitable for recycling resources.

[0023] In addition, the second method for producing the polymer of the present invention can modify the structure of the polymer, such as the average siloxane chain length between anthracene dimer sites, by utilizing an equilibration reaction process of polysiloxane. The polymerization, depolymerization, and modification of the polymer of the present invention are reversible, and the polymer and monomer of the present invention are also suitable for recycling resources.

[0024] In the present application, the monomer of the present invention can be produced by the first production method for the monomer of the present invention, the second production method for the monomer of the present invention, or the third production method for the monomer of the present invention, and the polymer of the present invention can be produced by the first production method for the polymer of the present invention or the second production method for the polymer of the present invention. Furthermore, the monomer of the present invention can be used for the polymer of the present invention, and the second production method for the monomer of the present invention can be applied to the polymer of the present invention. In the present application, the configurations corresponding to each of these inventions can be mutually used.

[0025] The present inventors have investigated new materials and developed a necklace-shaped polymer in which anthracene dimer moieties and polysiloxane moieties are alternately linked by photopolymerization using polysiloxane having multiple anthracene moieties as a monomer. This necklace-shaped polymer can change the hardness of the polymer by controlling the average chain length of the siloxane chains through an equilibrium reaction. They have also found that polymerization and monomerization can be performed reversibly by photopolymerization and heating. The present invention relates to monomers and polymers based on this finding.

[0026] FIG. 1 is a flow diagram of the production method of the present invention. Fig. 1(a) shows a flow for producing a monomer using a compound as a raw material. Step S11 is a step for mixing the raw materials. Step S12 is a step for reacting the raw materials to obtain a monomer. Step S13 is a step for recovering the monomer. Fig. 1(b) shows a flow of producing a polymer using a monomer. Step S21 is a step of feeding the monomer. Step S22 is a step of polymerizing the monomer to obtain a polymer. Step S23 is a step of recovering the polymer. Fig. 1(c) shows a flow of producing a monomer using a polymer as a raw material. Step S31 is a step of feeding a polymer. Step S32 is a step of depolymerizing the polymer to obtain a monomer. Step S33 is a step of recovering the monomer. Each step of each manufacturing method and specific examples of raw materials will be described in more detail below.

[0027] [Production of Monomer (First Production Method)] The first method for producing the monomer of the present invention is carried out using a reactive anthracene compound and a siloxane compound having multiple reactive terminals. The following formula (1) is a generalized reaction diagram showing an example of the production of this monomer.

[0028] A reactive anthracene compound and a siloxane compound having multiple reactive ends are mixed in a predetermined ratio. Then, the reactive ends of the siloxane compound (Y1, Y2 in the following formula (1)) are reacted with the reactive groups of the reactive anthracene compound (X in the following formula (1)). This results in a monomer having an anthracene structure at multiple ends of the structure derived from the siloxane compound.

[0029] [ka]

[0030] [Reactive anthracene compounds] The monomers and the like of the present invention use reactive anthracene compounds as raw materials. The following formula (2) is an example of a general formula for reactive anthracene compounds. The reactive anthracene compounds are anthracenes having reactive groups. The reactive groups here are structures that react when a monomer is formed using an appropriate catalyst depending on the combination of raw materials. In the following formula (2), X is a reactive group. Examples of reactive groups include vinyl groups, carboxy groups (carboxylic acids), carbonyl chloride groups, chloro groups, bromo groups, chloromethyl groups, bromomethyl groups, amino groups, alkyl ester groups, alkyl amide groups, alkyl ether groups, and alkyl groups.

[0031] R10 can be an alkyl group, an aryl group, or the above reactive group. p1 is an integer of 0 to 9, and may be 0 to 5 or 0 to 3. When p1 is 2 or more, each R10 may be the same or different. The anthracene compound may have multiple reactive groups. For example, the anthracene compound may have a reactive group at one or more positions selected from the group consisting of 1-position, 2-position, 5-position, 9-position, and 10-position, and the number of reactive groups is preferably 1 or 2.

[0032] [ka]

[0033] The following formula (2-1) is an example of a general formula for an anthracene compound having a reactive group at position 9. Although this formula shows the 9-position as an example, the reactive group may be present at other positions in the anthracene.

[0034] [ka]

[0035] As a specific anthracene compound, for example, vinylanthracene can be used. Representative examples include 9-vinylanthracene, 1-vinylanthracene, and 2-vinylanthracene as shown in the following formula (2-2). In addition, 9,10-divinylanthracene and 1,5-(1,1'-)divinylanthracene can be used.

[0036] [ka]

[0037] [Siloxane-based compounds with multiple reactive ends] The monomers and the like of the present invention use a siloxane-based compound having multiple reactive ends as a raw material. The following formula (3) is an example of a general formula for a siloxane-based compound having multiple reactive ends.

[0038] In the following formula (3), Y1 and Y2 are reactive terminals that react with the reactive group of the reactive anthracene compound. This reactive terminal reacts by condensation reaction or the like in the presence of a catalyst or the like, depending on the reactivity of the combination with the anthracene compound. Y1 and Y2 can be, for example, independently of each other, H, OH, CH3, or the like.

[0039] The siloxane compound used in the present invention has a plurality of reactive terminals. The number of reactive terminals is 2 or more. This number may be 2 or 3 or more. By having at least two reactive terminals, these terminals are bonded to an anthracene structure derived from a reactive anthracene compound to become the monomer of the present invention. This monomer of the present invention has a plurality of anthracene structures, and can be polymerized to form an anthracene dimer to become the polymer of the present invention.

[0040] The siloxane compound may be linear or branched, but linear polysiloxane in which both ends of the main chain are reactive ends is preferred. The following formula (3) is an example of a linear one. In the following formula (3), R1 to R4 are linear end groups of the siloxane compound, and can be, for example, alkyl groups such as methyl and ethyl groups, aryl groups such as phenyl groups, or H. R1 to R4 can also be of various structures used as introduction inducer groups for the side chain of polysiloxane such as modified silicone oil, and reactive silicone or non-reactive silicone structures can be used appropriately. n is a real number of 2 or more. R1 to R4 can be the same or different, and when n is 3 or more, R3 and R4 can be the same or different.

[0041] [ka]

[0042] For example, reactive silicones include monoamine-modified, diamine-modified, special amino-modified, epoxy-modified, alicyclic epoxy-modified, carbinol-modified, mercapto-modified, carboxyl-modified, amino-polyether-modified, epoxy-polyether-modified, and epoxy-aralkyl-modified silicones.

[0043] Further, for example, non-reactive silicones include polyether-modified, aralkyl-modified, fluoroalkyl-modified, long-chain alkyl-modified, higher fatty acid ester-modified, higher fatty acid amide-modified, polyether-long-chain alkyl-aralkyl-modified, and long-chain alkyl-aralkyl-modified silicones.

[0044] Examples of linear siloxane compounds include polydialkylsiloxanes, polyalkylarylsiloxanes, polydiarylsiloxanes, polydimethylsiloxanes, polymethylphenylsiloxanes, and polydiphenylsiloxanes. Among these, dimethylsiloxane, methylphenylsiloxane, diphenylsiloxane, and copolymers thereof can be used.

[0045] The monomer of the present invention can be produced by mixing a reactive anthracene compound with a siloxane compound having a plurality of reactive ends, and carrying out a reaction step between the reactive ends of the siloxane compound and the reactive groups of the reactive anthracene compound.

[0046] [Manufacturing conditions] The reactive anthracene compound and the siloxane compound are monomers obtained by reacting a reactive group of the anthracene compound with a reactive end of the siloxane compound under conditions according to their reactivity.

[0047] [mixture] The reactive anthracene compound and the siloxane compound, which are raw materials for the monomer, are mixed together. The mixing may be performed at a temperature or the like that matches the reaction conditions, or the mixing may be performed at about room temperature, and then the reaction conditions may be changed.

[0048] The reactive anthracene compound and the siloxane compound may be in a liquid state during mixing or reaction, and substantially only the reactive anthracene compound, the siloxane compound, and the catalyst may be mixed. Alternatively, a solvent or the like may be appropriately mixed in consideration of mixability, purification after synthesis, and the like.

[0049] The mixing ratio of the reactive anthracene compound and the siloxane compound can be set based on the number of moles, etc., in accordance with the number of reactive terminals of the siloxane compound, taking into consideration the number of reactive terminals of the siloxane compound.

[0050] For example, when the purpose is to provide an anthracene structure at both ends of a linear dimethylsiloxane, since the siloxane compound has two reactive ends, the reactive anthracene compound can be mixed with 1 mol of the siloxane compound, for example, 1.8 to 5 mol, 2 to 3 mol, or 2.1 to 2.5 mol. The unreacted raw material may be separated from the monomer, or may remain in the monomer composition since it is unlikely to contribute to polymer polymerization. For this reason, one raw material may be mixed in excess of the other raw material.

[0051] The reaction step may be carried out in the presence of a catalyst. The catalyst is synthesized according to the combination of the reactive anthracene compound and the siloxane compound. The main reaction is a hydrosilylation reaction, and a metal catalyst such as a platinum catalyst can be used as the catalyst. The necessity and amount of the catalyst can be determined according to the combination of raw materials used in the reaction, the reaction conditions, the target monomer structure, the catalyst type, etc.

[0052] The synthesis of the monomer can be appropriately set depending on the combination of raw materials. Examples of main conditions for synthesizing the monomer include the following. The temperature at which the synthesis is performed may be room temperature since the reaction can be performed at about room temperature. The time may be several hours to several days, with appropriate stirring. The synthesis is usually performed in a liquid or slurry state and is not easily affected by the atmosphere, but the atmosphere may be replaced with nitrogen so that side reactions due to the influence of oxygen, etc. are less likely to occur. The reaction may be stopped when the raw materials based on the amount of charge, etc. are used up, or the reaction may be stopped by removing the catalyst, etc.

[0053] The monomer after the reaction is 1 It can be confirmed by H-NMR structural analysis that a monomer has been obtained. After the reaction, the monomer may be recovered by removing unreacted materials and media such as a solvent through purification or volatilization, or may be converted into a solution or dispersion state by replacing the monomer with a medium that can be used in polymerizing a polymer.

[0054] After the synthesis of the monomer, it may be purified appropriately to remove the medium such as the solvent and by-products, etc. Purification can be carried out, for example, by recovering the monomer from a fraction fractionated by gel chromatography or the like.

[0055] [Production of Monomer (Second Production Method)] The monomer of the present invention can also be prepared by mixing a raw material monomer, a siloxane compound for modification, and a catalyst, and carrying out an equilibration reaction. This allows at least a part of the structure of the siloxane compound of the raw material monomer to be partially replaced with a structure derived from the siloxane compound for modification, thereby obtaining a monomer having a siloxane chain length or structure different from that of the raw material monomer.

[0056] The raw material monomer may be one produced by the first method for producing the monomer of the present invention, etc. The modifying siloxane compound may be one exemplified by cyclic siloxane or the first method for producing the monomer of the present invention, etc.

[0057] The monomer of the present invention can be modified, for example, by adjusting the chain length of the siloxane compound structure through an equilibration reaction, if necessary. In addition, the raw material monomer can be modified to have a dimethyl silicone structure, with a portion of the dimethyl silicone being converted to methylphenyl silicone.

[0058] The equilibration reaction is carried out in the presence of a catalyst. As the catalyst, various acid catalysts and basic catalysts used for the equilibration of silicone resins and the like can be used. As the acid catalyst, for example, a sulfuric acid catalyst can be used. As the basic catalyst, for example, tetramethylammonium hydroxide and an alkali metal catalyst can be used.

[0059] The equilibrium reaction can be stopped by removing the catalyst, which is an acid or alkali catalyst and can be removed by washing with water, etc.

[0060] [monomer] The monomer of the present invention is a monomer having an anthracene structure at multiple ends of the structure of a siloxane compound. The following formula (4) is an example of a general formula of the monomer of the present invention. This monomer can be produced using the above-mentioned reactive anthracene compound and a siloxane compound having multiple reactive ends. Therefore, the structure of the following formula (4) is similar to that described above. This monomer has an anthracene structure at both ends of the siloxane compound as shown at both ends of the following formula (4). That is, it has an anthracene structure at two ends. It also has a linear siloxane structure. In the following formula, X1 is a structure derived from either or both of the monomer raw materials. For example, it can be an alkylene group, an amide group, an ester group, an ether group, etc. In particular, an alkylene group is preferable, and as the alkylene group, for example, a methylene group, an ethylene group, a propylene group, a butylene group, a heptylene group, a hexylene group, etc. are preferable.

[0061] In the following formula (4), n can be 2 to 2,000, 3 to 1,000, 4 to 500, etc. The upper limit of n may be 200 or less, 100 or less, 50 or less, or 20 or less. Depending on the application, if n is too small, the brittleness of molded products such as films may become a problem, so n may be 13 or more, 16 or more, etc.

[0062] [ka]

[0063] The following formula (4-1) is a general example of a monomer having a 9-anthryl group according to the present invention, where R1 to R4 and n are as defined above, and X' is the same as X1.

[0064] [ka]

[0065] The following formula (4-2) is a typical example of the monomer of the present invention. This monomer is made from dimethylpolysiloxane and 9-vinylanthracene as raw materials, and has an anthracene structure bonded to both ends of the dimethylpolysiloxane.

[0066] [ka]

[0067] [Production of polymer (first production method of polymer)] The production of the polymer of the present invention involves a process in which a monomer that becomes a polymer raw material having an anthracene structure at multiple ends of a siloxane-based compound structure is irradiated with light for polymerizing the polymer raw material, thereby dimerizing the anthracene structures of the multiple polymer raw materials and polymerizing the monomer that becomes the polymer raw material.

[0068] The following formula (5) is a reaction formula showing a typical example of producing the polymer of the present invention using the monomer of the present invention. By polymerizing the monomer of the present invention, the anthracene structure of the monomer of the present invention forms an anthracene dimer, and by repeating this, the polymer of the present invention can be polymerized.

[0069] [ka]

[0070] [Anthracene dimer] The polymer of the present invention has a structure in which an anthracene structure derived from the monomer of the present invention forms an anthracene dimer. In general, dimerization is unlikely to occur even in various structures. However, it has been found that an anthracene structure such as the monomer of the present invention relatively easily forms a dimer by photopolymerization or the like. By utilizing this, a siloxane structure having multiple anthracene structures can be used to polymerize the polymer.

[0071] FIG. 2 is a schematic diagram of a reaction for producing a necklace-shaped polymer according to the present invention using the monomer of the present invention. By polymerizing a linear monomer having an anthracene structure at both ends of a linear siloxane structure, an anthracene dimer structure can be formed to produce a necklace-shaped polymer. In addition, as described below, this necklace-shaped polymer can also be depolymerized to obtain a linear monomer that was the raw material for the polymer. Note that the ends of the polymer in FIG. 2 can be bonded to each other to form a closed ring, so it is described as a necklace-shaped polymer, but the ends do not necessarily have to be closed, and the ends may be linear and separated from each other.

[0072] Necklace-shaped polymers containing anthracene dimer moieties can be made into a wide range of shapes, from hard molded bodies to flexible films, by changing the chain length of the siloxane structure or the degree of polymerization of the monomer.

[0073] Furthermore, in the monomer and polymer states, the siloxane chain length between the hard units can be changed by an equilibration reaction, thereby adjusting the basic physical properties of the polymer.

[0074] [polymer] The polymer of the present invention has a repeating structure of a siloxane structure derived from a siloxane compound and an anthracene dimer structure.

[0075] The polymer of the present invention is preferably a linear or cyclic polymer, and can be, for example, the following polymer: A linear or cyclic polymer having a siloxane compound structure and an anthracene dimer structure alternately, the siloxane compound structure being represented by the following formula (Z) and the anthracene dimer structure being represented by one or more of the following formulas (A1) to (A4): A linear or cyclic polymer having a siloxane compound structure and an anthracene dimer structure alternately, the siloxane compound structure being represented by the following formula (Z) and the anthracene dimer structure being represented by one or more of the following formulas (B1) to (B4): A linear or cyclic polymer having a siloxane compound structure and an anthracene dimer structure alternately, the siloxane compound structure being represented by the following formula (Z) and the anthracene dimer structure being represented by one or more of the following formulas (C1) to (C4):

[0076] [ka]

[0077] R23 and R24 in the above formula (Z) are the same as R3 and R4 above, and each is independently preferably an alkyl group or an aryl group, and n is as defined above.

[0078] [ka]

[0079] [ka]

[0080] [ka]

[0081] R11 to R20 in the above-mentioned (A1) to (A4), (B1) to (B4), and (C1) to (C4) can each independently be H, an alkyl group, an aryl group, or the like.

[0082] An example of such a polymer of the present invention is a polymer containing one or more of the following structures (a1) to (a4). Such a polymer has a structure in which 9-anthryl groups are dimerized.

[0083] [ka]

[0084] The polymer of the present invention may be a polymer containing one or more of the following (b1) to (b4): Such a polymer has a structure in which 1-anthryl groups are dimerized.

[0085] [ka]

[0086] The polymer of the present invention may be a polymer containing one or more of the following (c1) to (c4): Such a polymer has a structure in which 2-anthryl groups are dimerized.

[0087] [ka]

[0088] R11 to R20 in the above (a1) to (a4), (b1) to (b4), and (c1) to (c4) can each independently be H, an alkyl group, an aryl group, or the like. Z1 is a structure represented by the following formula (6). R21 to R24 in the following formula (6) are the same as R1 to R4 described above, and each independently is preferably an alkyl group or an aryl group. W is the same as X1 and X' described above. n is as described above. m1 to m4 are 0 or more, and m, which is the sum of m1+m2+m3+m4, can be equivalent to n described above.

[0089] [ka]

[0090] The following formula (7) is an example of a structure having a siloxane compound structure derived from polydimethylsiloxane and a repeating anthracene dimer, where n and m are as described above.

[0091] [ka]

[0092] The number average molecular weight and weight average molecular weight of the polymer of the present invention are appropriately set according to the structure and use of the polymer. In particular, they are appropriately set within a range that allows the polymer to show a solid form at room temperature for use as a molded article. The number average molecular weight of the polymer can be, for example, approximately 1,000 to 500,000, approximately 2,000 to 400,000, or approximately 3,000 to 300,000. The weight average molecular weight of the polymer can be, for example, approximately 3,000 to 1,000,000, approximately 5,000 to 800,000, or approximately 10,000 to 500,000.

[0093] The present invention utilizes the knowledge that the siloxane chain length can be freely changed by equilibration reaction in both polysiloxane monomers having anthracene moieties and necklace-shaped siloxane polymers having anthracene dimer moieties photopolymerized from the monomers, which means that the thermal and mechanical properties of the plastics can be adjusted.

[0094] [Photopolymerization] The polymer of the present invention can be produced, for example, by systematically synthesizing siloxane having anthracene groups at both ends of the siloxane chain, and then photopolymerizing this with ultraviolet light to synthesize a polymer having an anthracene dimer moiety.

[0095] The wavelength for photopolymerization may be about UV-A (315 nm to 400 nm). For example, the polymer can be polymerized by irradiating the monomer of the present invention with light having a wavelength of about 365 nm (hν (365 nm)). This is because even light equivalent to that in sunlight can provide an illuminance that contributes to polymerization, and therefore the polymer of the present invention can also be produced by irradiating the monomer with sunlight.

[0096] [Solvents, etc.] In producing the polymer of the present invention, the monomer of the present invention can be placed in a container for forming a molded product, and polymerization conditions can be set such that the monomer is directly irradiated with light. In addition, in consideration of reactivity and handleability of the polymer molded product, the polymerization may be carried out under conditions including a solvent, etc. In particular, since it is considered that the flowability of the monomer decreases with the polymerization, making it difficult to form a dimer, it is considered preferable to produce the polymer by polymerization under conditions including a solvent from the viewpoint of yield.

[0097] As the solvent, a solvent that disperses the monomer sufficiently and does not inhibit the polymerization reaction can be used. For example, tetrahydrofuran (THF), toluene, etc. can be used. The reaction rate tends to be faster when the monomer is polymerized substantially alone without using a solvent. On the other hand, in a state where the monomer concentration is high, such as when only the monomer is used, the movement of the monomer is restricted and unused monomer is likely to be generated. On the other hand, the reaction rate tends to be slower when the monomer is dissolved and dispersed in a solvent and then polymerized, but the utilization rate of the monomer is improved.

[0098] When a solvent is used, the composition can be appropriately set depending on the molecular weight of the monomer, the type of solvent, the reaction time, the reaction conditions, etc. When a solvent is used, the composition of the solution can be determined mainly with the monomer concentration as an indicator, and can be, for example, approximately 10 mmol / L to 10 mol / L, 50 mmol / L to 1 mol / L, or 100 mmol / L to 500 mmol / L.

[0099] The polymerization time can be appropriately set depending on the conditions, the degree of polymerization, and the like. The production of the polymer of the present invention utilizes the formation of a dimer that proceeds with the movement of monomers, and therefore, depending on the conditions, it is considered that the reaction will proceed relatively slowly. For this reason, the polymerization time can be set to 10 minutes or more, 30 minutes or more, or 1 hour or more. On the other hand, when the dimer is sufficiently formed to form a polymer such as a linear, necklace, or three-dimensional crosslinked polymer, the movement of the molecules is also restricted, so that there is no need to set an excessive reaction time. Therefore, the upper limit of the polymerization time may be set to within 100 hours, within 50 hours, or within 30 hours.

[0100] [Production of polymer (second production method of polymer)] The method for producing a polymer of the present invention can include an equilibration reaction step in which a raw material polymer having a repeating structure of a siloxane compound structure and an anthracene dimer structure, a modifying siloxane compound, and a catalyst are mixed together to carry out an equilibration reaction.

[0101] [Raw polymer] The raw polymer may be one produced by the first method for producing a polymer of the present invention or the third method for producing a polymer of the present invention, etc. The modifying siloxane compound may be a cyclic siloxane or one exemplified in the first method for producing a monomer of the present invention.

[0102] In the polymer of the present invention, the structure of the siloxane compound can be modified, for example, to adjust the chain length by subjecting the structure of the siloxane compound to a partial substitution reaction through an equilibration reaction, as necessary.

[0103] The equilibrium reaction is carried out in the presence of a catalyst. The catalyst may be an acid catalyst or a base catalyst used in the ring-opening equilibrium reaction of cyclic silicone. For example, sulfuric acid may be used as the acid catalyst. For example, an alkali metal catalyst may be used as the base catalyst.

[0104] The equilibration reaction can be stopped by removing the catalyst. This catalyst is an acid catalyst or an alkali catalyst, and can be removed by washing with water or the like, thereby stopping the equilibration reaction. Alternatively, the reaction can be stopped by mixing a reaction stopper such as an anion inhibitor. Kyoward (registered trademark), for example, can be used as such a reaction stopper.

[0105] The polymer of the present invention can be used as a substitute for general plastics and thermoplastic materials, etc. In addition, since it can be polymerized by sunlight and its thermal decomposition into monomers is an exothermic reaction, it can also be considered as a means of storing natural energy.

[0106] The physical properties of the polymer of the present invention can also be adjusted by the number of repetitions (n) of the siloxane structure of the raw material monomer and the ratio of the degree of polymerization (m) in the polymer.

[0107] [Molded body] The present invention can relate to a molded article containing the polymer of the present invention. The polymer of the present invention has properties similar to plastics by being made to have a structure of a linear siloxane compound or the like. This has properties equivalent to thermoplastic resins, and while it has fluidity during processing suitable for molding in a state mixed with a solvent or in a heated state, after molding, it has properties equivalent to a solid or solid state that can maintain a certain shape. The shape of the molded article of the present invention is not particularly limited, and can be a shape according to each application, such as a film, a plate, a block, or various components. The content of the polymer of the present invention in the molded article containing the polymer of the present invention is not particularly limited, and it can be mixed with other materials and molded appropriately according to its shape and application.

[0108] The molded article of the present invention can be produced by a molded article production method having a molding step of a molded article containing the polymer of the present invention produced by the production method of the present invention. The molding step can be a method suitable for the shape of the molded article. For example, the molded article can be formed into a film by casting, or filled into a mold and solidified, deformed, or cut.

[0109] [Depolymerization (heating) (third method for producing monomer)] The method for producing a monomer of the present invention can be a production method having a depolymerization step of heating and / or irradiating a polymer having a repeating structure of a siloxane compound structure and a plurality of anthracene dimer structures to dissociate the anthracene dimer structures of the polymer, thereby depolymerizing the polymer and obtaining a monomer of the polymer. This production method utilizes so-called depolymerization of the polymer to recover the monomer.

[0110] The following formula (8) is a typical example of a general reaction scheme for depolymerizing a polymer to obtain a monomer.

[0111] [ka]

[0112] The polymer of the present invention can be depolymerized and returned to the monomer by irradiation with deep ultraviolet light having a wavelength of about UV-C (100 nm to 280 nm) (hν (245 nm) in the formula is an example) or by heating at high temperature (Δ in the formula). The polymer can be reversibly decomposed to the monomer at a heating temperature of, for example, 140°C or higher or 150°C or higher. The heating temperature may be appropriately set to an upper limit of 250°C or lower or 200°C or lower. This physical property also makes it possible to directly convert the polymer to a monomer.

[0113] The present invention not only provides a novel molding material, but also contributes to a green and eco-friendly sustainable plastic material recycling system. Furthermore, the physical properties can be adjusted. Figure 4 is a schematic diagram explaining the adjustment of the polymer chain length by polymerization / depolymerization and ring-opening polymerization according to the present invention.

[0114] It is possible to completely convert polymers to monomers using heat. Since polymerization is possible using sunlight and the decomposition into monomers is an exothermic reaction, it can be used in an extremely eco-friendly system. In addition, polymerization is possible using the wavelength of sunlight, which also contributes to the storage of solar energy. In addition, it is possible to change the chemical structure of the polymer to suit the application. EXAMPLES

[0115] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples unless the gist of the present invention is changed.

[0116] [Example 1] Production of Monomer [Example 1-1] Synthesis of fixed chain length monomer (Ant-Si6) A hydrosilylation reaction was carried out to synthesize the fixed chain length monomer "Ant-Si6" using the siloxane compound DMHS and the anthracene compound 9-VAn as raw materials.

[0117] [Monomer raw materials, etc.] "DMHS" 1,1,3,3,5,5,7,7,9,9,11,11-dodecamethylhexasiloxane, Tokyo Chemical Industry Co., Ltd. "OMTS" 1,1,3,3,5,5,7,7-Octamethyltetrasiloxane, Tokyo Chemical Industry Co., Ltd. "TDMHS" 1,1,3,3,5,5,7,7,9,9,11,11,13,13-Tetradecamethylheptasiloxane, Tokyo Chemical Industry Co., Ltd. "9-VAn" 9-Vinylanthracene, Tokyo Chemical Industry Co., Ltd. "Karstedt's catalyst" Platinum(0)1,3-Divinyltetramethyldisiloxane Complex, Tokyo Chemical Industry Co., Ltd. "Toluene, Super Dehydrated," Wako Pure Chemical Industries, Ltd.

[0118] [Purified Reagents] Sea sand (30~50mesh), Wako Pure Chemical Industries, Ltd. "Silica gel" Sillca gel60, Fuji Silysia Chemical Co., Ltd. Hexane, Nacalai Tesque, Inc. Ethyl acetate, Wako Pure Chemical Industries, Ltd.

[0119] The synthesis of Ant-Si6 was carried out under a nitrogen atmosphere. DMHS is linear and the stoichiometric ratio based on the terminal of DMHS and the vinyl group of 9-VAn is DMHS:9-VAn=1:2 mol / mol. Here, DMHS:9-VAn=1:2.5 mol / mol was used, and the synthesis was carried out in a state where 9-VAn was abundant. Ant-Si6 was synthesized by hydrosilylation reaction (see reaction formula (9) below).

[0120] [ka]

[0121] [Synthesis] 1) First, 22.0 mL of ultra-dehydrated toluene, 1.0860 g (2.52 mmol) of DMHS, and 7.6 μL of Karstedt's catalyst (1.0 mol% DMHS ratio) were added to a brown sample bottle containing 1.2292 g (6.02 mmol) of 9-VAn, and the mixture was stirred at room temperature for 50 hours in the container. 2) The reaction solution was then distilled under reduced pressure to remove the solvent, and the crude product was obtained as a brown viscous liquid. 3) The crude product was purified by silica gel chromatography using a mixed solvent of hexane and ethyl acetate (hexane / ethyl acetate = 60 / 1 (vol / vol)) as the mobile phase to obtain a monomer (Ant-Si6) as a yellow viscous liquid. This monomer is called "Ant-Si6" because it is made from anthracene (Ant) and siloxane (Si), and the Si chain length of the siloxane raw material is 6.

[0122] [analysis( 1 H-NMR and TLC)] A portion of the crude product was sampled. 1 Analysis was carried out by 1 H-NMR and TLC. 1 The H-NMR sample was a deuterated chloroform solution, and the TLC sample was a hexane solution of the Ant-Si6 crude product. The stationary phase was a silica gel plate (Silica gel 60 F254), and the mobile phase was a mixed solvent of hexane and ethyl acetate (hexane / ethyl acetate = 60 / 1 (vol / vol)). Crude product 1 All peaks in the H-NMR spectrum were assigned. The crude product contained excess 9-VAn, the solvent toluene, and a monosubstituted siloxane in which only one end of the siloxane was modified with anthracene. 1 This was confirmed by the H-NMR chart.

[0123] [purification] In the purification by column chromatography, methanol-washed sea sand was placed in a column chromatography tube equipped with a glass filter, and silica gel slurried with hexane was packed in. When the silica gel became clogged, more methanol-washed sea sand was placed on top and the inside of the column was replaced with the mobile phase solvent.

[0124] The obtained fraction was distilled under reduced pressure to obtain 1.80 g of Ant-Si6 (yield 85.1%). 1 Only H-NMR analysis was performed. 1 All peaks observed in H-NMR measurements could be assigned, and the integral values ​​were almost consistent with the theoretical values.

[0125] The top spot that did not develop was recovered by pouring acetone over it, but it was not possible to recover it completely. In addition, because acetone is a highly polar solvent, the recovered fraction may not be a single compound. The resulting fraction was also subjected to reduced pressure distillation to remove the developing solvent, yielding compounds. While Ant-Si6 was a yellow viscous liquid, the compound in the top spot was obtained as a brown viscous liquid.

[0126] 1 The analysis was carried out by H-NMR and FT-IR. 1 From H-NMR, the anthryl group peaks became more complex, suggesting that some kind of anthryl group modification occurred. In addition, the Si-Me peaks became broader, suggesting that the intermolecular interactions became stronger. However, the phenyl group peaks (6.7-7.0 ppm) derived from the anthracene dimer were not observed.

[0127] FT-IR shows 1700cm -1 A peak derived from carbonyl (C=O) was observed near the peak, suggesting oxidation of the aromatic ring (quinone formation). The brown discoloration is also thought to be due to this quinone formation.

[0128] [Example 1-2] Ant-Si7 A monomer was synthesized using "TDMHS" instead of DMHS as a raw material in accordance with the manufacturing example of Example 1-1 described above. This monomer is called "Ant-Si7" because it is made from anthracene (Ant) and siloxane (Si) and the Si chain length of the siloxane raw material is 7.

[0129] [Example 1-3] Ant-Si4 A monomer was synthesized using "OMTS" instead of DMHS as a raw material in accordance with the manufacturing example of Example 1-1 described above. This monomer is called "Ant-Si4" because it is made from anthracene (Ant) and siloxane (Si) and the Si chain length of the siloxane raw material is 4.

[0130] [Example 2] Synthesis of chain-extended monomers by ring-opening equilibration reaction The siloxane chain length between the anthracenes of the monomers was adjusted by ring-opening equilibration reaction.

[0131] [Example 2-1] Production of cyclic monomer (Ant-rSi13.3)

[0132] "Ant-Si6" Example 1 Sample "D4" Octamethylcyclotetrasiloxane, Tokyo Chemical Industry Co., Ltd. "Toluene" Wako Pure Chemical Industries, Ltd. "MsOH" Methanesulfonic acid, Wako Pure Chemical Industries, Ltd. "Kyoward (registered trademark)" Kyoward (registered trademark) 500SN, Kyowa Chemical Industry Co., Ltd.

[0133] The siloxane chain length between anthracenes was randomized and extended by ring-opening equilibration reaction. Ant-Si6 was used as the terminal modifier and D4 was used as the cyclic monomer. Methanesulfonic acid (MsOH) was used as the acid catalyst. The reaction formula for siloxane chain extension by ring-opening equilibration reaction is as follows.

[0134] [ka]

[0135] 1) 0.4212g (0.476mmol) of Ant-Si6, 0.8937g (2.859mmol) of D4, and 1.5mL of toluene were placed in a sample bottle and stirred at 70°C for 36 hours until a homogeneous solution was obtained. Then, 8.43μL of MsOH was added and stirred for another 36 hours. 2) After that, 0.1 g of Kyoward was added to the reaction vessel and stirred again at room temperature for 30 minutes to stop the reaction. Kyoward was removed by filtration, and the reaction solution was distilled under reduced pressure to obtain the target product as a brown viscous liquid.

[0136] [Structural analysis] The purified Ant-rSi13.3 was 1 The structure was analyzed by H-NMR and SEC. 1 From the H-NMR analysis, the average number of Si atoms between anthracenes was calculated to be 13.3 using the integral value of Si-Me. This monomer is called "Ant-rSi13.3" because the average number of Si atoms is 13.3 when anthracene (Ant) and cyclosiloxane (cSi) are used. rSi refers to the siloxane chain with chain length distribution introduced by the equilibration reaction, and the subsequent numbers indicate the average degree of polymerization. The same applies below.

[0137] Furthermore, after the equilibration reaction, the Si-Me peaks broadened and the number of peaks increased compared to before the equilibration reaction. Furthermore, the peak intensity of the internal Si-Me of the silicone became stronger on the low magnetic field side. SEC analysis showed that the peaks broadened, the number average molecular weight Mn was 575, and the polydispersity Mw / Mn was 1.83. The peaks only broadened, and the peak tops hardly shifted to the higher molecular weight side, appearing in roughly the same position as the monomer.

[0138] [Example 2-2] Preparation of cyclic monomer (Ant-rSi11.6) A monomer was synthesized by changing the amounts of Ant-Si6, D4, methanesulfonic acid, and toluene in accordance with the manufacturing example of Example 2-1 described above. This monomer is called "Ant-rSi11.6" because the average number of Si atoms is 11.6.

[0139] [Example 2-3] Preparation of cyclic monomer (Ant-rSi16) According to the manufacturing example of Example 2-1 described above, 0.357 mmol of Ant-Si6, 2.71 mmol of D4, 9.46 μL of methanesulfonic acid, and 3.0 mL of toluene were reacted at 70° C. for 17 hours to synthesize a monomer. This monomer is called “Ant-rSi16.4” because the average number of Si atoms is 16.4.

[0140] [Example 3] Polymerization Polymerization experiments were carried out using monomers under various conditions.

[0141] [Example 3-1] Solvent-free photopolymerization was investigated using Ant-rSi11.6.

[0142] "Ant-rSi11.6" Sample from Example 2-2. Number average molecular weight 1252.4, amount charged 5.2 mg

[0143] 5.2 mg of Ant-rSi11.6 was placed on a cover glass and irradiated with ultraviolet light (365 nm) from a distance of about 4 cm while observing the change in appearance. After irradiation, it was not possible to extract the sample as a polymer film. 1 The reaction rate was calculated from H-NMR.

[0144] A shrinkage in volume was evident after about 10 seconds of light exposure. The surface also appeared to solidify after 30 seconds of light exposure. After 1 minute, it was clearly solidified, indicating that this was an extremely fast reaction. The volume continued to shrink, with almost no change observed after 3 minutes of light exposure. The volume shrinkage is due to the formation of new covalent bonds.

[0145] 1 The H-NMR results showed that the reaction rate was 62.6%. The reaction rate of the sample irradiated for 2 hours in the same manner was also around 60%.

[0146] The reaction rate was calculated using the following formula: Reaction rate (%) = integral value (polymer origin) / (integral value (monomer origin) + integral value (polymer origin)) * 100

[0147] The reason why the reaction rate is about 60% even after irradiation with ultraviolet light (365 nm) for a certain period of time or more is due to the fact that the viscosity of the sample increases as the polymerization proceeds, restricting the movement of the terminal anthracene. Note that, since a polymer is obtained in this example as well, it can be purified and molded to form a polymer molded product, and the unreacted monomer may be used as it is as the monomer, or only the monomer may be recovered and used.

[0148] [Example 3-2] Photopolymerization in THF (synthesis of poly Ant-Si6) We used Ant-Si6 as a monomer raw material and investigated the synthesis of its polymer, Poly(Ant-Si6). We also investigated photopolymerization using ultraviolet light (UV light).

[0149] "Ant-Si6" Example 1-1 Sample "THF" Tetrahydrofuran, HPLC grade, Nacalai Tesque, Inc.

[0150] 0.239g of Ant-Si6 and 0.95mL of THF were placed in a sample bottle, and ultraviolet light was irradiated from the bottom of the sample bottle. Sampling was done at regular intervals of irradiation, and the reaction was evaluated by measuring the absorption spectrum and molecular weight. The ultraviolet light irradiation was continued for 6 hours. 1 H-NMR measurements were performed.

[0151] The appearance of the reaction solution was observed, but no particular change was observed. The viscosity of the solution increased slightly. A 1.4 μL sample was taken from the reaction solution and dissolved in 3 mL of THF, and absorbance measurement and size exclusion chromatography (SEC measurement) were performed.

[0152] [Conditions for absorbance measurement] Measurement wavelength: 200-500 nm, Scanning speed: 20 nm / min, Data interval: 0.2 nm, Band width: 1.0 nm

[0153] [SEC measurement conditions] Flow rate: 1.0 mL / min, column oven temperature: 45.0°C, detector: UV, detection wavelength: 254 nm, mobile phase solvent: THF (Stabilizer Free), sample volume: 20 μL

[0154] [Evaluation Results] The peak appearing at a retention time of about 11 minutes is the solvent peak, and the peak appearing at about 10.5 minutes is the monomer peak. It was confirmed that the molecular weight increases by irradiating light. Ultimately, a polymer with Mn: 8,000 and Mw: 10,000 was obtained.

[0155] It is possible to know that Poly(Ant-Si6) has been synthesized. 1 The H-NMR spectrum of Poly(Ant-Si6) was obtained. 1 The H-NMR analysis results are shown below.

[0156] [Table 1]

[0157] 1 All the signals observed in the H-NMR measurement could be assigned, and the integral values ​​were reasonable except for the Si-Me signal. The Si-Me signal was broadened, making it difficult to obtain an ideal integral value.

[0158] After polymerization 1 Trends seen in the H-NMR chart include the disappearance of the anthryl signal, the shift of the methylene proton chemical shift, the appearance of methine and phenyl signals, and the broadening of the Si-Me peak. The shift of the methylene protons to the upfield side is due to the receding aromatic ring, and the broadening of the Si-Me peak is due to polymerization.

[0159] Finally, 0.4766 g of polymer was obtained (yield 199.4%). The larger yield was due to incomplete drying of the sample. The obtained polymer was cast into a Teflon (registered trademark) petri dish to prepare a polymer film.

[0160] After drying, the polymer became like small pieces that easily broke and did not become a self-supporting film. It was thought that the reason for this was that the polymer had a high low molecular weight, so a reprecipitation operation was performed. The good solvent for the reprecipitation operation was chloroform, and the poor solvent was hexane.

[0161] After reprecipitation, the sample was dried by heating to produce a polymer film. The polymer could be extracted as a film, and was brittle and transparent.

[0162] [Example 3-3] Synthesis of poly(Ant-rSi13.3) Poly(Ant-rSi13.3) was synthesized using 0.3820 g of Ant-rSi13.3 as the raw monomer. This synthesis was carried out by mixing 0.3820 g of Ant-rSi13.3 with 1 mL of THF, using THF as the solvent, and irradiating with UV light for 24 hours under a nitrogen atmosphere. Photopolymerization was carried out under a nitrogen atmosphere to prevent the anthryl group from becoming quinone. When photopolymerization was carried out in the presence of sufficient air, crystals with poor solubility were sometimes obtained.

[0163] "Ant-rSi13.3" Example 2-1 sample "THF" Tetrahydrofuran HPLC grade, Nacalai Tesque, Inc.

[0164] By photopolymerizing for 24 hours under a nitrogen atmosphere, a stronger film was obtained. A slight transparency was also obtained. The yield was 0.4265g, which was 111.6%.

[0165] The number average molecular weight of this poly(Ant-rSi13.3) was 4.9k and the weight average molecular weight was 18k as determined by SEC.

[0166] [Example 3-4] Photopolymerization with sunlight Two reaction conditions were prepared: under N2 gas atmosphere and under air atmosphere. Ant-Si7 and THF were added to a sample bottle and the bottle was placed on a windowsill exposed to sunlight.

[0167] "Ant-Si7" Example 1-2 sample "THF" Tetrahydrofuran HPLC grade, Nacalai Tesque, Inc.

[0168] Based on the weather information during the solar polymerization (Kumamoto City, Kumamoto Prefecture, Japan), the weather was bad and the sunshine hours could not be secured, so the experiment took a long time. Also, the net sunlight exposure time is thought to be about 17 hours.

[0169] The solution viscosity of the sample in nitrogen increased, while the viscosity of the sample in air did not increase. In addition to the solution viscosity, the two samples also differed in color. Only the sample in air changed color slightly, becoming slightly brown.

[0170] This control experiment suggested that photo-oxidation occurred in air due to ultraviolet light and oxygen in the air. 1 The following explanation will be given while comparing the results of the H-NMR chart, SEC chart, and IR chart.

[0171] The color change observed in the reaction solution was related to the color change of the product. Since the color of the polymer comes from unreacted anthracene, it is thought that polymerization proceeded without the anthracene moiety being destroyed under nitrogen conditions. Conversely, it is thought that there was a change in the anthracene moiety under air conditions.

[0172] 1 The final conversion was determined from the H-NMR spectrum. The conversion was 79.5% for the air sample and 90.3% for the nitrogen sample. The conversion was lower in air and the spectrum attributable to the aromatic ring was slightly more complex.

[0173] The FT-IR chart shows peaks attributable to carbonyl bonds (1680 and 1700 cm) in the air-conditioned sample. -1 ) was detected. However, no such peak was detected in the sample under nitrogen conditions, and no differences were observed in the other peaks.

[0174] From the SEC measurement results, a small amount of residual monomer could be observed as a peak in the sample polymerized in a nitrogen atmosphere. Furthermore, it was confirmed that the peak rise was faster, indicating that a polymer with a higher molecular weight was produced. In this way, it was confirmed that polymers can be obtained by irradiating with sunlight.

[0175] [Examples 3-5] Photopolymerization of Ant-Si4 (poly Ant-Si4) Based on the results of the above-mentioned Examples, additional tests were carried out. Figure 4 is a graph showing the evaluation results of the reaction time and molecular weight in the polymerization examples of the Examples.

[0176] Under conditions similar to those of Example 3-2, a sample of Ant-Si4 (Example 2-3) was used, and THF was used as a solvent to evaluate the relationship between the UV irradiation time and the number average molecular weight. The image in FIG. 4 shows the test state. It was confirmed that the number average molecular weight increased significantly after the irradiation time exceeded 1.0 hour, and a polymer with a number average molecular weight of about 16k or more was produced.

[0177] [Image of molded product] Figure 5 is an image of a film-shaped molded product of the polymer produced in the example. The left side of Figure 5 is an image of a film molded by Poly AntSi6 produced in Example 3-2. The right side of Figure 5 is an image of a film of poly Ant-rSi16 produced using Ant-rSi16.4 according to poly Ant-rSi13.3 produced in Example 3-3.

[0178] [Example 4] Thermal depolymerization The depolymerization of poly Ant-Si6 and poly Ant-rSi13.3 was investigated.

[0179] "Poly Ant-Si6" Sample of Example 3-2. "poly Ant-rSi13.3" Sample of Example 3-3.

[0180] [Example 4-1] Depolymerization of polyAnt-Si6 A solid sample polymerized in the above-mentioned embodiment was used. PolyAnt-Si6 was placed in a sample bottle, the atmosphere in the sample bottle was replaced with nitrogen (N2), and the bottle was placed in an oil bath at 160°C. After 30 minutes of oil bath treatment, the polyAnt-Si6 in the sample bottle was depolymerized and became liquid. The composition of this liquid was confirmed to be an Ant-Si6 monomer with an average chain length of 6.0.

[0181] [Example 4-2] Depolymerization of polyAnt-rSi13.3 Instead of polyAnt-Si6 in Example 4-1, polyAnt-rSi13.3 was used to carry out depolymerization by heating. After 30 minutes of oil bath treatment, polyAnt-rSi13.3 in the sample bottle was depolymerized and became liquid. As a result of checking the composition of this liquid, it was confirmed that the average chain length was 12.3 as a measured value, and it was a monomer equivalent to Ant-rSi13.3 used as a polymer raw material.

[0182] The following reaction scheme (11) corresponds to these examples and shows the polymerization and depolymerization of Ant-Sin.

[0183] [ka]

[0184] [Summary of evaluation results] FIG. 6 includes graphs showing the evaluation results of the monomers and polymers produced in the examples. The top part of Figure 6 shows the evaluation results of the monomer, Ant-Si6, and a typical image of the same. The middle part of Figure 6 shows the evaluation results and typical images of the photopolymerized polymer, polyAnt-Si6. The lower part of Figure 6 shows the evaluation results and a typical image of Ant-Si6, a recycled monomer obtained by thermal depolymerization. [Industrial Applicability]

[0185] INDUSTRIAL APPLICABILITY The present invention can be utilized for the production of new polymers and monomers, as well as for recycling systems thereof, and is therefore industrially useful.

Claims

1. A method for producing a polymer having a repeating structure of a siloxane structure derived from a siloxane compound and an anthracene dimer structure, the method comprising: a polymerization step of irradiating a monomer having an anthracene structure at multiple ends of a siloxane compound structure with light for polymerizing the monomer, thereby dimerizing the anthracene structures between the monomers.

2. A method for producing a polymer, comprising an equilibration reaction step of mixing a raw material polymer having a repeating structure of a siloxane compound structure and an anthracene dimer structure, a modifying siloxane compound, and a catalyst to carry out an equilibration reaction.

3. A method for producing a molded article, comprising a molding step of producing a molded article containing a polymer produced by the method for producing a polymer according to claim 1 or 2.

4. A polymer having a repeating structure of a siloxane structure derived from a siloxane compound and an anthracene dimer structure.

5. A method for producing a monomer, comprising: a depolymerization step of heating and / or irradiating a polymer having a repeating structure of a siloxane-based compound structure and a plurality of anthracene dimer structures to dissociate the anthracene dimer structures of the polymer, thereby depolymerizing the polymer and obtaining a monomer of the polymer.

6. A reaction step of mixing a reactive anthracene compound with a siloxane compound having a plurality of reactive terminals and reacting the reactive terminals of the siloxane compound with the reactive groups of the reactive anthracene compound is included. A method for producing a monomer having an anthracene structure derived from the anthracene compound at a plurality of ends of a siloxane structure derived from the siloxane compound.

7. 7. The method according to claim 6, wherein the reactive anthracene compound is vinylanthracene, the siloxane compound is polydimethylsiloxane, and the reacting step is carried out in the presence of a catalyst.

8. A method for producing a monomer, comprising an equilibration reaction step of mixing a raw material monomer having an anthracene structure derived from an anthracene compound at multiple ends of a siloxane structure derived from a siloxane compound, a modifying siloxane compound, and a catalyst to carry out an equilibration reaction.

9. A monomer having an anthracene structure at multiple ends of a siloxane compound structure.

Citation Information

Patent Citations

  • Polysiloxane composite

    JP2021178892A