Method for recovering boron nitride powder from silicone rubber cured product, and boron nitride

A method using organic sulfonic acid and solvent to dissolve and recover boron nitride from cured silicone rubber addresses recyclability and toxicity issues, achieving efficient separation and purification for reuse.

JP2024162164AActive Publication Date: 2024-11-21SHIN ETSU CHEMICAL CO LTD

Patent Information

Application Number
JP2023077457
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-21
Estimated Expiration
2043-05-09

AI Technical Summary

Technical Problem

The recycling of thermally conductive cured silicone rubber products containing boron nitride is challenging due to the high cost and limited recyclability, and existing dissolution methods using toxic chemicals pose health and environmental risks.

Method used

A method involving organic sulfonic acid, water, and a specific organic solvent is used to dissolve silicone rubber, followed by filtration, washing, and drying to recover boron nitride powder efficiently.

Benefits of technology

The method effectively separates and purifies boron nitride powder, enabling its reuse with minimal environmental impact and maintaining high thermal conductivity properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162164000001
    Figure 2024162164000001
Patent Text Reader

Abstract

To provide a method for recovering boron nitride powder from a silicone rubber cured product, which contains the boron nitride powder, and also to provide boron nitride.SOLUTION: The present invention provides a method for recovering boron nitride powder from a silicone rubber cured product, which contains organopolysiloxane as well as the boron nitride powder. This method includes the step for immersing the silicone rubber cured product in a silicone rubber solution in a temperature range that is equal to or higher than 20°C, and equal to or lower than the boiling point of component (C), wherein the silicone rubber solution includes (A) an organic sulfonic acid: 0.1-50 mass%, (B) water: 0.01-6 mass%, and (C) an organic solvent: 44-99.89 mass%, the organic solvent having a boiling point of 60°C or higher and 200°C or lower at an atmospheric pressure of 1013 hPa.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recovering boron nitride powder from a cured silicone rubber, and to boron nitride. [Background technology]

[0002] In recent years, heat-conducting layers that transfer heat from heat-generating components to heat-dissipating components in integrated circuits, electrical devices, electronic devices, light-emitting devices, and the like, are required to have high thermal conductivity and insulation, and heat-dissipating materials in which fillers are dispersed in resin or rubber are widely used to meet such requirements. In order to increase the thermal conductivity of heat-dissipating materials, there are methods of using heat-conducting fillers with high thermal conductivity such as aluminum nitride and boron nitride, and methods of increasing the filling rate of heat-conducting fillers.

[0003] However, fillers with high thermal conductivity, especially boron nitride, are expensive and in tight supply.

[0004] Furthermore, in recent years, the importance of recycling has increased in various fields due to environmental issues, and the recyclability of parts used in electrical and electronic equipment has become an important issue. Thermally conductive cured products made of silicone rubber, etc. are crosslinked rubber cured products, and even if they are recycled, they cannot be melt-molded and reused again, which poses a major problem in terms of recyclability. In response to this, methods of dissolving silicone rubber to recover thermally conductive fillers have been studied.

[0005] As a method for dissolving silicone rubber, a silicone dissolving liquid containing phosphonitrilic chloride and a linear polysiloxane with a degree of polymerization of 10 to 50 has been disclosed (Patent Document 1). This method is capable of selectively dissolving silicone rubber without causing swelling of other plastic members, but requires the use of phosphonitrilic chloride, which is highly toxic, and there are concerns about the health hazards and environmental burden on the surrounding area.

[0006] As another method for dissolving silicone rubber, a silicone rubber solubilizer in which tetraalkylammonium fluoride and an inorganic base capable of bonding with hydrogen ions are dissolved in an organic solvent has been disclosed (Patent Document 2). This method makes it possible to dissolve silicone rubber without corroding metal pieces, but it is necessary to dissolve an inorganic base capable of bonding with hydrogen ions in an organic solvent, which limits the organic solvents that can be used. In addition, this document only specifically discloses the dissolution rate of the silicone resin and its corrosiveness to metal pieces, and the effects on other substrates are unclear. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Special Publication No. 2014-524941 [Patent Document 2] Special Publication No. 2015-505886 Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made in consideration of the above circumstances, and has an object to provide a method for recovering boron nitride powder from a cured silicone rubber product containing boron nitride powder, and a recovered boron nitride product. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention provides a method for recovering boron nitride powder from a silicone rubber cured product containing an organopolysiloxane and boron nitride powder, the method comprising the steps of: (A) organic sulfonic acid: 0.1 to 50 mass%, (B) water: 0.01 to 6% by mass, and (C) an organic solvent having a boiling point of 60°C or more and 200°C or less at an atmospheric pressure of 1013 hPa: 44 to 99.89% by mass, The present invention provides a method for recovering boron nitride powder from a cured silicone rubber product, the method comprising the step of immersing the cured silicone rubber product in a silicone rubber dissolving liquid containing the above component (C) at a temperature in the range of 20° C. or higher and the boiling point of the component (C).

[0010] Such a method for recovering boron nitride powder from cured silicone rubber makes it possible to efficiently recover boron nitride from cured silicone rubber, and to reuse the recovered boron nitride.

[0011] In the present invention, the immersion time in the immersion step is preferably 1 hour to 24 hours.

[0012] Such an immersion time makes it possible to more efficiently recover boron nitride from the cured silicone rubber, and to reuse the recovered boron nitride.

[0013] In the present invention, it is preferable to use, as the organic sulfonic acid of the component (A), at least one selected from dodecylbenzenesulfonic acid, p-toluenesulfonic acid, and benzenesulfonic acid.

[0014] As the component (A), such materials can be suitably used.

[0015] In the present invention, it is preferable to use an organic solvent having a relative dielectric constant of 8.0 or less as the component (C).

[0016] Such component (C) is preferred because it allows the silicone rubber to swell sufficiently, has good compatibility with component (A), and prevents separation of components (A) and (C).

[0017] In the present invention, it is preferable to include a filtration step after the immersion step.

[0018] By including the filtration step, the filler can be filtered out from the mixture of the silicone rubber solution and the boron nitride-containing filler obtained through the immersion step.

[0019] In this case, it is preferable to include a washing step with an organic solvent after the filtration step.

[0020] By including the washing step, the filler containing boron nitride recovered in the filtration step can be washed with an organic solvent.

[0021] In this case, it is preferable to include a drying step after the washing step.

[0022] By including the drying step, the organic solvent and the like used in the washing step can be removed from the boron nitride recovered in the washing step.

[0023] The present invention also provides boron nitride, which is recovered from a cured silicone rubber product, and which has a weight loss rate of 4% or less from 50 to 500°C as measured by TG, a graphitization index (G1 value) of less than 5 as measured by powder X-ray diffraction method, and a residual boron oxide amount of 0.2% or less.

[0024] Such recovered boron nitride can be reused. Effect of the Invention

[0025] According to the present invention, by immersing a cured silicone rubber in a silicone rubber solution containing an organic sulfonic acid, water, and an organic solvent, it is possible to separate boron nitride from silicone rubber and recover and purify the boron nitride powder, thereby contributing to solving environmental and cost problems. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] As described above, there has been a need for a method for recovering boron nitride powder from cured silicone rubber containing boron nitride powder, and for the development of recovered boron nitride.

[0027] In order to achieve the above-mentioned object, the inventors conducted extensive research and discovered that by using organic sulfonic acid and water, silicone rubber can be decomposed highly efficiently in an organic solvent, and that by filtering, washing and drying the decomposition product, boron nitride powder can be recovered and purified, thereby arriving at the present invention.

[0028] That is, the present invention provides a method for recovering boron nitride powder from a silicone rubber cured product containing an organopolysiloxane and boron nitride powder, comprising the steps of: (A) organic sulfonic acid: 0.1 to 50 mass%, (B) water: 0.01 to 6% by mass, and (C) an organic solvent having a boiling point of 60°C or more and 200°C or less under an atmospheric pressure of 1013 hPa: 44 to 99.89% by mass, The method for recovering boron nitride powder from a cured silicone rubber product includes the step of immersing the cured silicone rubber product in a silicone rubber dissolving liquid containing the above component (C) at a temperature in the range of 20°C or higher and the boiling point of the above component (C).

[0029] The present invention also relates to boron nitride, which is recovered from a cured silicone rubber product, and which has a weight loss rate of 4% or less from 50 to 500°C as measured by TG, a graphitization index (G1 value) of less than 5 as measured by powder X-ray diffraction method, and a residual boron oxide amount of 0.2% or less.

[0030] The present invention will be described in detail below, but the present invention is not limited thereto.

[0031] [Boron nitride] The present invention relates to boron nitride, which is a material recovered from a cured silicone rubber, and which has a weight loss rate of 4% or less from 50 to 500°C as measured by TG, a graphitization index (G1 value) of less than 5 as measured by powder X-ray diffraction method, and a residual boron oxide amount of 0.2% or less.

[0032] Such boron nitride (recovered boron nitride) can be obtained by the method of recovering boron nitride powder from a cured silicone rubber according to the present invention described below. Furthermore, such boron nitride can be reused as a filler for the cured silicone rubber.

[0033] <Cured silicone rubber> The silicone rubber cured product used in the present invention is applicable to silicone rubber cured products containing organopolysiloxane and boron nitride powder, that is, all silicone rubber cured products containing siloxane bonds and boron nitride powder. For example, addition curing type silicone rubber that cures by addition reaction of vinyl group and hydrosilyl group with platinum catalyst, radical curing type silicone rubber that cures with radicals generated by decomposition of organic peroxide, condensation curing type silicone rubber that cures by condensation such as dehydration, dealcoholization, acetone removal, and oxime removal, and ultraviolet curing type silicone rubber that cures by irradiating ultraviolet light to a mixture of silicone polymer having an acrylic group and a photoinitiator, etc.

[0034] <Filling agent> The silicone rubber cured product used in the present invention contains boron nitride as a filler. In addition, it may contain hydrophobic silica, hydrophilic silica, iron oxide, ultramarine, silicone resin, carbon black, glass beads, resin balloons, diatomaceous earth, metal oxide powder, metal powder, and metal hydroxide powder. In addition, it may contain additives such as reaction regulators, antioxidants, adhesion aids, adhesion promoters, plasticizers, and flame retardants.

[0035] [Method for recovering boron nitride powder from cured silicone rubber] The present invention relates to a method for recovering boron nitride powder from a silicone rubber cured product containing an organopolysiloxane and boron nitride powder, the method comprising the steps of: (A) organic sulfonic acid: 0.1 to 50 mass%, (B) water: 0.01 to 6% by mass, and (C) an organic solvent having a boiling point of 60°C or more and 200°C or less at an atmospheric pressure of 1013 hPa: 44 to 99.89% by mass, The method for recovering boron nitride powder from a cured silicone rubber product includes the step of immersing the cured silicone rubber product in a silicone rubber dissolving liquid containing the above component (C) at a temperature in the range of 20°C or higher and the boiling point of the above component (C).

[0036] <Silicone rubber solution> The components of the silicone rubber solution used in the method of the present invention for recovering boron nitride powder from a cured silicone rubber will now be described in detail.

[0037] [Component (A)] Component (A) is an organic sulfonic acid that acts as a decomposition catalyst for siloxane bonds (-O-Si-O-).

[0038] The organic sulfonic acid of component (A) is preferably a sulfonic acid having a long-chain alkyl group-containing aromatic hydrocarbon group having 12 or more carbon atoms, more preferably at least one selected from dodecylbenzenesulfonic acid, p-toluenesulfonic acid, and benzenesulfonic acid, and particularly preferably dodecylbenzenesulfonic acid.

[0039] The amount of organic sulfonic acid (A) blended is 0.1% to 50% by mass, preferably 1% to 40% by mass, and more preferably 2% to 30% by mass, based on the total amount of water (B) and organic solvent (C). If the blending amount is less than 0.1% by mass, the silicone rubber may not be sufficiently decomposed, whereas if it is more than 50% by mass, the viscosity of the silicone rubber solution may increase, which may lead to poor workability and complicated post-treatment of the waste acid.

[0040] The component (A) may be used alone or in combination of two or more kinds.

[0041] [(B) Component] Component (B) is water, which contributes to improving the decomposition efficiency of silicone rubber.

[0042] The blending amount of component (B) is 0.01% by mass to 6% by mass, preferably 0.1% by mass to 2% by mass, based on the total amount of the organic sulfonic acid (component (A)) and the organic solvent (component (C)). If the blending amount is less than 0.01% by mass, the efficiency of decomposing the silicone rubber will not improve, and if it is more than 6% by mass, it may not be mixed uniformly with the organic solvent.

[0043] [(C) component] Component (C) is an organic solvent that acts as a swelling agent for the silicone rubber and as a solvent for component (A).

[0044] The boiling point of the organic solvent of component (C) is from 60° C. to 200° C. at an atmospheric pressure of 1013 hPa, preferably from 70° C. to 180° C., and more preferably from 80° C. to 160° C. If the boiling point is less than 60° C., the organic solvent will be highly volatile, which may increase the environmental load and deteriorate the working environment, while if the boiling point exceeds 200° C., it may be difficult to recover and recycle the organic solvent by distillation or the like from the silicone rubber solution after the immersion step is completed.

[0045] It is preferable to use an organic solvent for component (C) that has a relative dielectric constant of 8.0 or less. If the relative dielectric constant is 8.0 or less, the silicone rubber swells sufficiently and has good compatibility with component (A), so that components (A) and (C) do not separate.

[0046] Examples of the organic solvent of component (C) include linear or branched saturated aliphatic hydrocarbons such as hexane, heptane, octane, isooctane (2,2,4-trimethylpentane), nonane, decane, undecane, isododecane (2,2,4,6,6-pentamethylheptane), etc., and aromatic hydrocarbons such as benzene, toluene, dimethylbenzene, trimethylbenzene, ethylbenzene, diethylbenzene, propylbenzene, isopropylbenzene, etc. Among these, octane, decane, toluene, and xylene are particularly preferred organic solvents.

[0047] The blending amount of component (C) is 44% by mass to 99.89% by mass, preferably 80% by mass to 99.89% by mass, based on the total amount of the organic sulfonic acid (component (A)) and water (component (B)). A blending amount lower than 44% by mass is undesirable because the swelling of the silicone rubber becomes insufficient, while a blending amount greater than 99.89% by mass is undesirable because the amounts of components (A) and (B) are too small, reducing the efficiency of decomposing the silicone rubber.

[0048] The component (C) may be used alone or in combination of two or more kinds.

[0049] Each step of the method of the present invention for recovering boron nitride powder from a cured silicone rubber will now be described in detail.

[0050] <Soaking process> The method of recovering boron nitride powder from the silicone rubber cured product of the present invention requires an immersion step in which the silicone rubber cured product is immersed in the prepared silicone rubber dissolving solution. At this time, dissolution proceeds sufficiently just by immersing the silicone rubber cured product in the silicone rubber dissolving solution, but stirring with a dynamic mixer using a stirring blade, stirring with a magnetic stirrer, shaking with a shaker, ultrasonic treatment, etc. are effective for improving the dissolution rate, and stirring with a dynamic mixer or a magnetic stirrer is particularly preferred. In addition, when dissolving a large amount of silicone rubber cured product, a reactor with a stirring blade used in normal chemical reactions may be used, or it may simply be immersed in a treatment bath. In addition, it is preferable that the silicone rubber cured product is cut into a size that is easy to stir.

[0051] There are no particular limitations on the weight ratio between the silicone rubber solution and the silicone rubber cured product, but it is preferable to use an amount of silicone rubber solution that completely immerses the silicone rubber cured product.

[0052] The immersion temperature is not particularly limited as long as it is within the range of 20° C. or higher and the boiling point of the organic solvent used or lower, but is preferably 20° C. to 100° C., more preferably 30° C. to 90° C., and even more preferably 40° C. to 80° C. If the temperature is lower than 20° C., the dissolution rate of the silicone resin may become extremely slow, and if the temperature exceeds the boiling point of the organic solvent used, polymerization of the siloxane monomer may proceed.

[0053] The immersion time is not particularly limited, but varies depending on the weight ratio of the silicone rubber cured product to the silicone rubber solution, stirring conditions, and temperature conditions, and it is preferable to select an appropriate time. In general, the immersion time is preferably 1 hour to 24 hours, more preferably 2 hours to 12 hours, and even more preferably 4 hours to 8 hours.

[0054] <Filtration process> The method for recovering boron nitride powder from the silicone rubber cured product of the present invention preferably includes a filtration step after the immersion step. The filtration step is a step of filtering the filler from the mixture of the silicone rubber solution and the filler containing boron nitride obtained through the immersion step. Specifically, the mixture is passed through a filter material such as cellulose, glass fiber, wire mesh, or membrane filter to filter out the solution and the filler containing boron nitride. Examples of the filtration method include natural filtration, reduced pressure filtration, and pressure filtration. Among them, pressure filtration using an inert gas such as nitrogen is preferred, taking into account the filtration time and the handling of flammable organic solvents.

[0055] <Cleaning process> The method for recovering boron nitride powder from the silicone rubber cured product of the present invention preferably includes a washing step after the filtration step. This washing step is a step of washing the filler containing boron nitride recovered in the filtration step with an organic solvent. Specifically, washing is performed using 50 to 200 parts by mass of an organic solvent per 100 parts by mass of the filler containing boron nitride. The organic solvent for washing is not particularly limited as long as it is an organic solvent exemplified in the component (C), but it is preferable to perform washing using the same organic solvent as that used in the component (C). This makes it easy to recycle the organic solvent. As a washing method, after the filtration step, the organic solvent may be poured onto the filler remaining on the filter medium, or the filler after filtration may be taken out, mixed with an organic solvent, and filtered again for washing. This washing step may be performed once or may be repeated two or more times.

[0056] <Drying process> The method of recovering boron nitride powder from a silicone rubber cured product of the present invention preferably includes a drying step after the washing step. This drying step is a step of removing the organic solvent and the like used in the washing step from the boron nitride recovered in the washing step. Specifically, drying is performed at a drying temperature of 20 to 100°C for a drying time of 4 to 24 hours. Drying may be performed under normal pressure or reduced pressure, but reduced pressure drying using a vacuum dryer or the like is preferred.

[0057] <Evaluation of the recovered boron nitride powder> The boron nitride powder recovered according to the present invention is evaluated by TG measurement, powder X-ray diffraction method, and the amount of remaining boron oxide.

[0058] [TG measurement] The weight loss rate of reusable boron nitride powder at 50 to 500°C in TG measurement is 4% or less, preferably 2% or less, and more preferably 1% or less. If it exceeds 4%, the powder contains a lot of polymer components and the physical properties will deteriorate when reused. TG measurement can be performed, for example, using a high-sensitivity differential thermobalance STA2500Regulus manufactured by NETZSCH in the range of 50 to 500°C at a heating rate of 5°C / min.

[0059] [Powder X-ray diffraction method] Furthermore, reusable boron nitride powder has a graphitization index (G1 value) calculated from the peak areas of three diffraction peaks (100), (101), and (102) observed in XRD analysis, a powder X-ray diffraction method, using the following formula (1): G1 value is less than 5, preferably not more than 3, and more preferably not more than 2. If the G1 value exceeds 5, the crystallinity of the boron nitride is low, and good physical properties cannot be obtained when reused. G1 = peak area [(100) + (101)] / peak area (102) (1)

[0060] XRD analysis can be performed, for example, using a benchtop powder X-ray diffractometer, D2 PHASER 2nd Generation, manufactured by BRUKER JAPAN, with a scan range of 20-90°, a step time of 0.03 sec, and a sample rotation speed of 10 rpm.

[0061] [Residual boron oxide content] The amount of remaining boron oxide is calculated from the measured boron concentration by ICP measurement. The amount of remaining boron oxide in reusable boron nitride powder is 0.2% or less. If the amount of remaining boron oxide exceeds 0.2%, foaming will occur during reuse. The amount of remaining boron oxide can be measured, for example, using the SPS3520UV-DD manufactured by Hitachi High-Tech Science Corporation. EXAMPLES

[0062] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these.

[0063] <Examples and Comparative Examples> (CH3)2SiO 2 / 2 Unit: 99.85 mol%, (CH3)2(CH2=CH)SiO 1 / 2 Unit 0.025mol% and (CH2=CH)SiO 2 / 2100 parts by mass of a dimethylpolysiloxane having vinyl groups at both ends, consisting of 0.125 mol%, and 340 parts by mass of toluene were placed in a mixer and stirred and mixed. 190 parts by mass of boron nitride powder was added to the obtained mixture and stirred and mixed. Next, 3 parts by mass of a peroxide crosslinking agent (Perhexa 25B, manufactured by NOF Corporation) and 70 parts by mass of toluene were added and stirred and mixed to obtain a composition. The obtained composition was coated to a thickness of 0.3 mm on both sides of a glass cloth having a thickness of 0.05 mm using a bar coater, dried at 80 ° C for 10 minutes, and then pressed at a pressure of 100 kg / cm 2 2 , and pre-cured at 170 ° C for 10 minutes to obtain a cured product. 100 g of the obtained cured product was weighed into a 1 L separable flask. Then, each solvent was added at the blending ratio shown in Table 1, and stirred at 80 ° C for 4 hours using a magnetic stirrer. Then, it was filtered using a 150-mesh wire mesh to remove the glass cloth, and subsequently filtered using a filter paper having a retention particle size of 4 μm to recover boron nitride. After washing 100 parts by mass of the obtained boron nitride with 100 parts by mass of toluene, it was finally dried in a vacuum dryer at 50 ° C for 12 hours to obtain boron nitride powder. TG measurement, XRD measurement, and composition analysis were performed on the obtained powder.

[0064] <TG measurement method> The weight change rate of the boron nitride powder was measured under the following apparatus and conditions. Apparatus: High-sensitivity differential scanning calorimeter STA2500Regulus manufactured by NETZSCH Measurement range: 50 to 500 ° C Temperature rising rate: 5 ° C / min

[0065] <XRD measurement method> The XRD of the boron nitride powder was measured under the following apparatus and conditions. Apparatus: Desktop powder X-ray diffractometer manufactured by BRUKER JAPAN D2 PHASER 2nd Generation Scan range: 20 - 90 ° Step time: 0.03 sec Sample rotation: 10 rpm Measurements were performed using XRD, and for the item "Confirmation of the shape of boron nitride," a G1 value of 5 or more was evaluated as "X," and a value of less than 5 was evaluated as "O." The results are shown in Table 1.

[0066] <Composition analysis method> The composition of the boron nitride powder was analyzed using the following equipment and conditions. Equipment: Hitachi High-Tech Science SPS3520UV-DD A composition analysis was performed, and the results of the evaluation of the "residual B2O3 content" item are shown in Table 1. The content was evaluated as "×" when it was more than 0.2%, and as "○" when it was 0.2% or less.

[0067] [Table 1]

[0068] In the method of recovering boron nitride powder from a cured silicone rubber product of the present invention, a silicone rubber dissolving solution containing components (A) to (C) in specific ratios was used. In Examples 1 to 4, the silicone components were efficiently decomposed and removed without affecting the boron nitride. The recovered boron nitride powder can be reused in the same product. On the other hand, in Comparative Example 1, which used a dissolving solution not containing component (B), the boron nitride powder was not affected, but the silicone components remained, and the same physical properties were not obtained when reused.

[0069] The present specification includes the following aspects. [1]: A method for recovering boron nitride powder from a cured silicone rubber product containing an organopolysiloxane and boron nitride powder, comprising: (A) organic sulfonic acid: 0.1 to 50 mass%, (B) water: 0.01 to 6% by mass, and (C) an organic solvent having a boiling point of 60°C or more and 200°C or less at an atmospheric pressure of 1013 hPa: 44 to 99.89% by mass, 1. A method for recovering boron nitride powder from a cured silicone rubber product, comprising the step of: immersing the cured silicone rubber product in a silicone rubber dissolving liquid containing the above component (C) at a temperature in the range of 20°C or higher and the boiling point of the above component (C). [2]: The method for recovering boron nitride powder from a cured silicone rubber product according to the above [1], characterized in that in the immersion step, the immersion time is from 1 hour to 24 hours. [3]: A method for recovering boron nitride powder from a cured silicone rubber product according to the above [1] or [2], characterized in that the organic sulfonic acid of component (A) is one or more selected from the group consisting of dodecylbenzenesulfonic acid, p-toluenesulfonic acid, and benzenesulfonic acid. [4]: A method for recovering boron nitride powder from a silicone rubber cured product according to any one of [1] to [3] above, characterized in that the organic solvent for component (C) has a dielectric constant of 8.0 or less. [5]: A method for recovering boron nitride powder from a silicone rubber cured product according to any one of [1] to [4] above, comprising a filtration step after the immersion step. [6]: A method for recovering boron nitride powder from a cured silicone rubber product according to [5] above, characterized in that the method comprises a step of washing with an organic solvent after the filtering step. [7]: A method for recovering boron nitride powder from a cured silicone rubber product according to [6] above, characterized in that it comprises a drying step after the washing step. [8]: Boron nitride, which is recovered from a cured silicone rubber product, and which has a weight loss rate of 4% or less from 50 to 500°C in TG measurement, a graphitization index (G1 value) of less than 5 in powder X-ray diffraction method, and a residual boron oxide amount of 0.2% or less.

[0070] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.

Claims

1. A method for recovering boron nitride powder from a cured silicone rubber product containing organopolysiloxane and boron nitride powder, comprising the steps of: (A) organic sulfonic acid: 0.1 to 50% by mass, (B) water: 0.01 to 6% by mass, and (C) an organic solvent having a boiling point of 60° C. or higher and 200° C. or lower at an atmospheric pressure of 1013 hPa: 44 to 99.89% by mass, immersing the cured silicone rubber in a silicone rubber dissolving solution containing the component (C) at a temperature in the range of 20°C or higher and the boiling point of the component (C) or lower.

2. 2. The method for recovering boron nitride powder from a cured silicone rubber product according to claim 1, wherein the immersion time in the immersion step is from 1 hour to 24 hours.

3. 2. The method for recovering boron nitride powder from a cured silicone rubber product according to claim 1, wherein the organic sulfonic acid of component (A) is at least one selected from the group consisting of dodecylbenzenesulfonic acid, p-toluenesulfonic acid, and benzenesulfonic acid.

4. 2. The method for recovering boron nitride powder from a cured silicone rubber product according to claim 1, wherein the organic solvent of component (C) has a relative dielectric constant of 8.0 or less.

5. 5. The method for recovering boron nitride powder from a cured silicone rubber product according to claim 1, further comprising a filtering step after the immersion step.

6. 6. The method for recovering boron nitride powder from a cured silicone rubber product according to claim 5, further comprising a step of washing with an organic solvent after the filtering step.

7. 7. The method for recovering boron nitride powder from a cured silicone rubber product according to claim 6, further comprising a drying step after the washing step.

8. 1. A boron nitride which is a material recovered from a cured silicone rubber, and which has a weight loss rate of 4% or less from 50 to 500°C as measured by TG, a graphitization index (G1 value) of less than 5 as measured by powder X-ray diffraction method, and a residual boron oxide amount of 0.2% or less.

Citation Information

Patent Citations

  • Separation of high pressure boron nitride

    JP1977156799A

  • Method for removing boron nitride film

    JP1995292485A

  • Processing method for reuse of waste silicone hardened matter

    JP2002348407A

  • Contains silica-reinforced rubber that releases less volatile organic compounds (VOC)

    JP2008537740A

  • Silicone solubilizer

    JP2015505886A

Cited By

  • Information leakage possibility assessment device, information leakage possibility assessment method, and program