Method for manufacturing laminated optical film

By using a boron-containing compound and controlled water content in the adhesive composition, the method enhances adhesion and allows for faster production of laminated optical films with improved adhesiveness.

JP2024162277APending Publication Date: 2024-11-21NITTO DENKO CORP

Patent Information

Application Number
JP2023077628
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing methods for producing laminated optical films face challenges in increasing line speed while maintaining excellent adhesiveness between optical films, particularly due to issues with water content and polymerization initiator migration in adhesive compositions.

Method used

A method involving the application of an adhesive composition with a specific boron-containing compound and controlled water content, followed by immediate curing with active energy rays, without a drying step, to enhance adhesion between first and second optical films.

Benefits of technology

This approach allows for increased production line speed with improved adhesion and water-resistant bonding between optical films, ensuring high-quality laminated optical films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162277000001
    Figure 2024162277000001
  • Figure 2024162277000002
    Figure 2024162277000002
  • Figure 2024162277000003
    Figure 2024162277000003
Patent Text Reader

Abstract

To provide a method for manufacturing a laminated optical film excellent in adhesiveness between first and second optical films while increasing the line speed of a manufacturing line for the laminated optical film.SOLUTION: A method for manufacturing a laminated optical film having at least first and second optical films laminated through an adhesive layer comprises: a first application step of applying an easy adhesive composition including at least a specific boron-containing compound and water to the lamination surface of the first optical film; a second application step of applying an adhesive composition including at least a curable component and a polymerization initiator to the lamination surface of the second optical film; a lamination step of laminating the first optical film to the second optical film; and a bonding step of bonding the first optical film to the second optical film. The content of water in the easy adhesive composition is 40 mass% or less; and when setting the film thickness of the easy adhesive composition after the first application step to α and the film thickness of the easy adhesive composition after the second application step to β, β>α is satisfied.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer. The laminated optical film can form an image display device such as a liquid crystal display (LCD), an organic electroluminescence display device, a CRT, or a PDP. [Background technology]

[0002] Liquid crystal display devices are rapidly expanding into the market for watches, mobile phones, PDAs, notebook computers, PC monitors, DVD players, TVs, etc. Liquid crystal display devices visualize the polarization state by switching liquid crystals, and polarizers are used due to their display principle. In particular, for applications such as TVs, higher brightness, higher contrast, and wider viewing angles are required, and polarizing films are also required to have higher transmittance, higher polarization degree, and better color reproducibility.

[0003] As a polarizer, since it has high transmittance and high polarization degree, for example, an iodine-based polarizer having a structure in which iodine is adsorbed to polyvinyl alcohol (hereinafter also simply referred to as "PVA") and stretched is most commonly used. In general, a polarizing film is used in which transparent protective films are bonded to both sides of a polarizer using a so-called water-based adhesive in which a polyvinyl alcohol-based material is dissolved in water (Patent Document 1 below). As the transparent protective film, triacetyl cellulose, which has high moisture permeability, is used. When the water-based adhesive is used (so-called wet lamination), a drying process is required after bonding the polarizer and the transparent protective film.

[0004] On the other hand, instead of the water-based adhesive, an active energy ray curable adhesive has been proposed. When a polarizing film is produced using an active energy ray curable adhesive, a drying process is not required, so the productivity of the polarizing film can be improved. For example, a radical polymerization type active energy ray curable adhesive using an N-substituted amide monomer as a curable component has been proposed (Patent Document 2 below).

[0005] Patent Document 3 listed below discloses a method for producing a polarizing film in which a transparent protective film is provided on at least one surface of a polarizer via an adhesive layer, and the method includes a first coating step in which a solvent-containing easy-adhesion composition is applied to the bonding surface of the polarizer while transporting the polarizer to form a wet first coating film, a second coating step in which an adhesive composition is applied to the bonding surface of the transparent protective film while transporting the transparent protective film to form a second coating film, a first thickness measurement step in which the thickness of the wet first coating film is measured in-line, a drying step in which, after the first thickness measurement step, the solvent in the wet first coating film is removed using a dryer to form a dry first coating film, and a drying step in which, after the drying step, the thickness of the dry first coating film is measured in-line. The method for producing a polarizing film is described, including a second thickness measurement step of measuring the thickness in-line, a dryness adjustment step of adjusting the dryness of the newly formed dry first coating film by adjusting the temperature and / or air volume of a dryer so that the ratio of the thickness of the wet first coating film obtained by the in-line measurement to the thickness of the dry first coating film satisfies a specific formula, a lamination step of laminating the dry first coating film formed on the lamination surface of a polarizer with the second coating film formed on the lamination surface of a transparent protective film to form an uncured adhesive layer, and an adhesion step of adhering the polarizer and the transparent protective film via the adhesive layer obtained by curing the uncured adhesive layer. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2001-296427 A [Patent Document 2] JP 2012-052000 A [Patent Document 3] JP 2020-160391 A Summary of the Invention [Problem to be solved by the invention]

[0007] In the above Patent Document 3, a dryness adjustment step is performed, but in recent years, it has become necessary to increase the line speed of the laminated optical film production line, particularly from the viewpoint of improving productivity. For this reason, it has been found that there is room for further improvement in both the materials, such as the adhesive composition and the easy-adhesion composition constituting the adhesive layer, and the process.

[0008] The present invention has been developed to solve the above-mentioned problems, and aims to provide a method for producing a laminated optical film having excellent adhesion between a first optical film and a second optical film while increasing the line speed of the laminated optical film production line. [Means for solving the problem]

[0009] The above-mentioned problems can be solved by the following configuration: That is, the present invention is a method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, the method comprising the steps of: applying a compound represented by the following general formula (1): to a bonding surface of the first optical film while conveying the first optical film: [ka] (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent; R 1 and R 2each independently represents a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group which may have a substituent) and water; a second coating step of coating an adhesive composition containing at least a curable component and a polymerization initiator on the bonding surface of the second optical film while transporting the second optical film; a laminating step of laminating the first optical film and the second optical film; and an adhesion step of bonding the first optical film and the second optical film via the adhesive layer formed by irradiating the first optical film side or the second optical film side with active energy rays to cure at least the adhesive composition, wherein the content of the water in the easy-adhesion composition is 40 mass% or less, and when the film thickness of the easy-adhesion composition after the first coating step is α and the film thickness of the adhesive composition after the second coating step is β, β>α.

[0010] In the above-mentioned method (1) for producing a laminated optical film, a method (2) for producing a laminated optical film is preferable in which a drying step is not provided between the first coating step and the laminating step.

[0011] In the above-mentioned method (1) or (2) for producing a laminated optical film, the method (3) for producing a laminated optical film is preferable, in which the time required from the end of the first coating step to the start of the laminating step is 5 seconds or less.

[0012] In any one of the above-mentioned methods (1) to (3) for producing a laminated optical film, the method (4) for producing a laminated optical film is preferable, in which the first optical film is a polarizer.

[0013] In any one of the above-mentioned methods (1) to (4) for producing a laminated optical film, the method (5) for producing a laminated optical film is preferred, in which the second optical film is a transparent protective film.

[0014] In any one of the methods (1) to (5) for producing a laminated optical film, the adhesive composition contains, as a polymerizable component, a polymerizable compound represented by the following general formula (2): [ka] Compounds represented by the formula (wherein R 4 is a hydrogen atom or a methyl group, and R 5 and R 6 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or a cyclic ether group, and R 5 and R 6 (may form a cyclic heterocycle) is preferably used.

[0015] In any one of the above-mentioned methods (1) to (6) for producing a laminated optical film, the method (7) for producing a laminated optical film is preferred, in which the easy-adhesion composition contains a compound represented by the above-mentioned general formula (2). Effect of the Invention

[0016] In the method for producing a laminated optical film according to the present invention, an easy-adhesion composition is applied to the bonding surface of a first optical film (first coating step), an adhesive composition is applied to the bonding surface of a second optical film (second coating step), and the first optical film and the second optical film are bonded together so that their bonding surfaces overlap (bonding step). Here, in the method for producing a laminated optical film according to the present invention, the following innovations are implemented in terms of materials. (i) At least a specific boron-containing compound (a compound represented by general formula (1)) and water are blended into the easy-adhesion composition, and the water content in the easy-adhesion composition is designed to be 40 mass% or less. (ii) At least a curable component and a polymerization initiator are blended into the adhesive composition. In addition, in the method for producing the laminated optical film according to the present invention, the following improvements are made in the process. (iii) When the film thickness of the adhesive composition after the first coating step is α and the film thickness of the adhesive composition after the second coating step is β, the relationship is designed to be β>α. By providing all of the above configurations (i), (ii), and (iii), the method for producing a laminated optical film according to the present invention can produce a laminated optical film having excellent adhesion between the first optical film and the second optical film while increasing the line speed of the laminated optical film production line. The reason for this effect can be presumed to be as follows.

[0017] The specific boron-containing compound blended in the adhesive composition contributes greatly to improving the adhesion between the first optical film and the adhesive layer, particularly to improving the adhesion under humid conditions. However, when the line speed of the laminated optical film production line is increased, the water in the adhesive composition is hardly removed, and the moisture content in the adhesive composition increases, which reduces the relative concentration of the polymerization initiator migrating from the adhesive composition. As a result, the boron-containing compound cannot sufficiently react with the curable component blended in the adhesive composition, and it is expected that the adhesion between the first optical film and the adhesive layer will deteriorate. However, in the method for producing a laminated optical film according to the present invention, the water content in the easy-adhesion composition is designed to be 40% by mass or less, that is, the water content is less than that of a conventional easy-adhesion composition (above (i)), and when the film thickness of the easy-adhesion composition after the first coating step is α and the film thickness of the adhesive composition after the second coating step is β, it is designed to be β>α (above (iii)). This makes it easier for the polymerization initiator blended in the adhesive composition to migrate into the easy-adhesion composition, that is, by increasing the relative concentration of the polymerization initiator migrating from the adhesive composition, the reaction rate between the curable component blended in the adhesive composition and the boron-containing compound is increased (above (ii)). As a result of these, for example, by not providing a drying step between the first coating step and the lamination step, or by designing the time required from the end of the first coating step to the start of the lamination step to be short, it is presumed that a laminated optical film having excellent adhesion between the first optical film and the second optical film, particularly excellent water-resistant adhesion, can be produced even when the line speed of the laminated optical film production line is increased. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The method for producing a laminated optical film according to the present invention is a method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, and the method comprises the steps of: applying a compound represented by the following general formula (1): to a bonding surface of the first optical film while transporting the first optical film: [ka] (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent; R 1 and R 2 each independently represents a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group which may have a substituent) and water, a second coating step of coating an adhesive composition containing at least a curable component and a polymerization initiator on the bonding surface of the second optical film while conveying the second optical film, a bonding step of bonding the first optical film and the second optical film together, and a bonding step of bonding the first optical film and the second optical film together via an adhesive layer formed by irradiating the first optical film side or the second optical film side with active energy rays to cure at least the adhesive composition, wherein the content of water in the easy-adhesion composition is 40 mass% or less, and when the film thickness of the easy-adhesion composition after the first coating step is α and the film thickness of the adhesive composition after the second coating step is β, β>α. First, each material used in the method for producing a laminated optical film according to the present invention will be described.

[0019] (Easy adhesive composition) The easily adhesive composition comprises at least one compound represented by the following general formula (1): [ka] (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent; R 1 and R 2each independently represents a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group which may have a substituent) and water.

[0020] In the compound represented by the general formula (1), the aliphatic hydrocarbon group includes a linear or branched alkyl group having 1 to 20 carbon atoms which may have a substituent, a cyclic alkyl group having 3 to 20 carbon atoms which may have a substituent, and an alkenyl group having 2 to 20 carbon atoms. The aryl group includes a phenyl group having 6 to 20 carbon atoms which may have a substituent, and a naphthyl group having 10 to 20 carbon atoms which may have a substituent, and the heterocyclic group includes, for example, a 5- or 6-membered ring group containing at least one hetero atom which may have a substituent. These may be linked together to form a ring. In the general formula (1), R 1 and R 2 is preferably a hydrogen atom or a linear or branched alkyl group having 1 to 3 carbon atoms, and is most preferably a hydrogen atom.

[0021] X in the compound represented by general formula (1) is a reactive group, which is a functional group that can react with a curable component that constitutes the adhesive layer, and examples of such a functional group include a hydroxyl group, an amino group, an aldehyde group, a carboxyl group, a vinyl group, a (meth)acrylic group, a styryl group, a (meth)acrylamide group, a vinyl ether group, an epoxy group, an oxetane group, an α,β-unsaturated carbonyl group, a mercapto group, and a halogen group. When the curable adhesive composition constituting the adhesive layer is active energy ray curable, the reactive group X is preferably at least one reactive group selected from the group consisting of vinyl group, (meth)acrylic group, styryl group, (meth)acrylamide group, vinyl ether group, epoxy group, oxetane group and mercapto group, and when the curable adhesive composition constituting the adhesive layer is radical polymerizable, the reactive group X is preferably at least one reactive group selected from the group consisting of (meth)acrylic group, styryl group and (meth)acrylamide group, and when the compound represented by general formula (1) has a (meth)acrylamide group, it is more preferable because it has high reactivity and increases the copolymerization rate with the curable component in the adhesive layer. In addition, it is also preferable from the viewpoint that the effect of the present invention can be efficiently obtained because the polarity of the (meth)acrylamide group is high and the adhesiveness is excellent. When the curable adhesive composition constituting the adhesive layer is cationic polymerizable, the reactive group X preferably has at least one functional group selected from a hydroxyl group, an amino group, an aldehyde, a carboxyl group, a vinyl ether group, an epoxy group, an oxetane group, and a mercapto group. In particular, when the reactive group X has an epoxy group, this is preferred because the resulting adhesive layer has excellent adhesion to the adherend, and when the reactive group X has a vinyl ether group, this is preferred because the curability of the curable adhesive composition is excellent.

[0022] Preferable specific examples of the compound represented by the general formula (1) include the following compounds (1a) to (1d). 3 is a hydrogen atom or a methyl group. [ka]

[0023] In addition to the compounds exemplified above, examples of the compound represented by general formula (1) include esters of (meth)acrylates and boric acid, such as esters of hydroxyethylacrylamide and boric acid, esters of methylol acrylamide and boric acid, esters of hydroxyethyl acrylate and boric acid, and esters of hydroxybutyl acrylate and boric acid.

[0024] In order to increase the copolymerization rate with the curable component constituting the adhesive layer and improve the adhesion between the first optical film and the adhesive layer, the amount of the compound represented by general formula (1) in the adhesion-promoting composition is preferably 0.5 to 15 mass %, and more preferably 1 to 10 mass %.

[0025] The adhesive composition used in the present invention contains water in addition to the compound represented by general formula (1). However, in the method for producing a laminated optical film according to the present invention, since it is necessary to increase the line speed of the laminated optical film production line, the water in the adhesive composition is hardly removed. For this reason, the content of water in the adhesive composition is preferably 40% by mass or less, more preferably 30% by mass or less.

[0026] In the present invention, the easy-adhesion composition may contain a solvent other than water. The solvent that may be contained in the easy-adhesion composition is preferably one that can stabilize and dissolve or disperse the compound represented by the general formula (1). Such a solvent is selected from, for example, esters such as ethyl acetate, butyl acetate, and 2-hydroxyethyl acetate; ketones such as methyl ethyl ketone, acetone, cyclohexanone, methyl isobutyl ketone, diethyl ketone, methyl-n-propyl ketone, and acetylacetone; cyclic ethers such as tetrahydrofuran (THF) and dioxane; aliphatic or alicyclic hydrocarbons such as n-hexane and cyclohexane; aromatic hydrocarbons such as toluene and xylene; aliphatic or alicyclic alcohols such as methanol, ethanol, n-propanol, isopropanol, and cyclohexanol; glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, and diethylene glycol monoethyl ether; glycol ether acetates such as diethylene glycol monomethyl ether acetate and diethylene glycol monoethyl ether acetate; and the like.

[0027] Furthermore, in the present invention, other additives, such as tackifiers, ultraviolet absorbers, antioxidants, and stabilizers such as heat stabilizers, may be blended into the easily adhesive composition.

[0028] In the present invention, a curable component may be blended in the easy-adhesion composition, and preferably, a compound represented by general formula (2), which is preferably blended in an adhesive composition, may be blended as the curable component. The compound represented by general formula (2) will be described later. When a curable component, preferably a compound represented by general formula (2), is blended in the easy-adhesion composition, the blending amount is preferably 20 to 80 mass%, more preferably 40 to 70 mass%.

[0029] In the present invention, it is preferable not to blend a polymerization initiator into the easily adhesive composition used in the first coating step, and even if a polymerization initiator is blended, the amount is preferably 3% by mass or less, more preferably 1% by mass or less, and it is particularly preferable not to blend a polymerization initiator.

[0030] (Adhesive Composition) The adhesive composition contains at least a curable component and a polymerization initiator. The adhesive composition used in the present invention is preferably an active energy ray curable adhesive composition. The active energy ray curable adhesive composition can be classified into a radical polymerization curable adhesive composition and a cationic polymerization curable adhesive composition. In the present invention, active energy rays in the wavelength range of 10 nm to less than 380 nm are referred to as ultraviolet rays, and active energy rays in the wavelength range of 380 nm to 800 nm are referred to as visible rays.

[0031] The curable component to be incorporated in the radical polymerization curable adhesive composition may be, for example, a compound represented by the following general formula (2): [ka] Compounds represented by the formula (wherein R 4 is a hydrogen atom or a methyl group, and R 5 and R 6 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or a cyclic ether group, and R 5 and R 6 may form a cyclic heterocycle). The number of carbon atoms in the alkyl portion of the alkyl group, hydroxyalkyl group, and / or alkoxyalkyl group is not particularly limited, but examples include those having 1 to 4 carbon atoms. 5 and R 6 Examples of the cyclic heterocycle that may be formed include N-acryloylmorpholine.

[0032] Specific examples of the compound represented by general formula (2) include N-alkyl group-containing (meth)acrylamide derivatives such as N-methyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, and N-hexyl(meth)acrylamide; N-hydroxyalkyl group-containing (meth)acrylamide derivatives such as N-methylol(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, and N-methylol-N-propane(meth)acrylamide; and N-alkoxy group-containing (meth)acrylamide derivatives such as N-methoxymethylacrylamide and N-ethoxymethylacrylamide. Examples of the cyclic ether group-containing (meth)acrylamide derivative include heterocycle-containing (meth)acrylamide derivatives in which the nitrogen atom of the (meth)acrylamide group forms a heterocycle, such as N-acryloylmorpholine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylpyrrolidine, etc. Among these, N-hydroxyethylacrylamide and N-acryloylmorpholine can be preferably used because of their excellent reactivity, ability to obtain a cured product with a high elastic modulus, and excellent adhesion to polarizers.

[0033] From the viewpoint of improving the adhesion between the first optical film and the adhesive layer, and further between the first optical film and the second optical film, the content of the compound represented by general formula (2) in the curable adhesive composition is preferably 20 to 80 mass %, and more preferably 30 to 60 mass %.

[0034] The curable adhesive composition used in the present invention may contain, as a curable component, other monofunctional radical polymerizable compounds in addition to the compound represented by formula (2). Examples of the monofunctional radical polymerizable compounds include various (meth)acrylic acid derivatives having a (meth)acryloyloxy group. Specific examples of the acrylate include (meth)acrylic acid (carbon number: 1 to 20) alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, t-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, cetyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and n-octadecyl (meth)acrylate.

[0035] Examples of the (meth)acrylic acid derivatives include cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate and cyclopentyl (meth)acrylate; aralkyl (meth)acrylates such as benzyl (meth)acrylate; 2-isobornyl (meth)acrylate, 2-norbornylmethyl (meth)acrylate, 5-norbornen-2-yl-methyl (meth)acrylate, 3-methyl-2-norbornylmethyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxy. Examples of the methacrylate include polycyclic (meth)acrylates such as ethyl (meth)acrylate and dicyclopentanyl (meth)acrylate; alkoxy group- or phenoxy group-containing (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, and alkylphenoxypolyethylene glycol (meth)acrylate; etc. Among these, dicyclopentenyloxyethyl acrylate and phenoxyethyl acrylate are preferred because of their excellent adhesion to various protective films.

[0036] In addition, examples of the (meth)acrylic acid derivatives include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate. hydroxyl group-containing (meth)acrylates such as [4-(hydroxymethyl)cyclohexyl]methyl acrylate, cyclohexanedimethanol mono(meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate; epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate glycidyl ether; 2,2,2-trifluoroethyl (meth)acrylate, 2,2,2-trifluoroethylethyl (meth)acrylate, Halogen-containing (meth)acrylates such as acrylates, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate; alkylaminoalkyl (meth)acrylates such as dimethylaminoethyl (meth)acrylate; 3-oxetanylmethyl (meth)acrylate, 3-methyl-oxetanylmethyl (meth)acrylate; acrylate, 3-ethyl-oxetanylmethyl (meth)acrylate, 3-butyl-oxetanylmethyl (meth)acrylate, 3-hexyl-oxetanylmethyl (meth)acrylate, and other oxetane group-containing (meth)acrylates; tetrahydrofurfuryl (meth)acrylate, butyrolactone (meth)acrylate, and other (meth)acrylates having a heterocycle; hydroxypivalic acid neopentyl glycol (meth)acrylic acid adduct; p-phenylphenol (meth)acrylate, and other. Among these, 2-hydroxy-3-phenoxypropyl acrylate is preferred because of its excellent adhesion to various protective films.

[0037] Furthermore, examples of the monofunctional radically polymerizable compound include carboxyl group-containing monomers such as (meth)acrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.

[0038] Examples of the monofunctional radically polymerizable compound include lactam-based vinyl monomers such as N-vinylpyrrolidone, N-vinyl-ε-caprolactam, and methylvinylpyrrolidone; and vinyl monomers having a nitrogen-containing heterocycle such as vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, and vinylmorpholine.

[0039] In addition, as the monofunctional radical polymerizable compound, a radical polymerizable compound having an active methylene group can be used. The radical polymerizable compound having an active methylene group is a compound having an active double bond group such as a (meth)acrylic group at the end or in the molecule, and having an active methylene group. Examples of the active methylene group include an acetoacetyl group, an alkoxymalonyl group, and a cyanoacetyl group. It is preferable that the active methylene group is an acetoacetyl group. Specific examples of radical polymerizable compounds having an active methylene group include acetoacetoxyalkyl (meth)acrylates such as 2-acetoacetoxyethyl (meth)acrylate, 2-acetoacetoxypropyl (meth)acrylate, and 2-acetoacetoxy-1-methylethyl (meth)acrylate; 2-ethoxymalonyloxyethyl (meth)acrylate, 2-cyanoacetoxyethyl (meth)acrylate, N-(2-cyanoacetoxyethyl)acrylamide, N-(2-propionylacetoxybutyl)acrylamide, N-(4-acetoacetoxymethylbenzyl)acrylamide, and N-(2-acetoacetylaminoethyl)acrylamide. The radical polymerizable compound having an active methylene group is preferably an acetoacetoxyalkyl (meth)acrylate.

[0040] A bifunctional or higher polyfunctional radical polymerizable compound can be blended as a curable component constituting the radical polymerization curable adhesive composition. Examples of the polyfunctional radical polymerizable compound include polyfunctional (meth)acrylamide derivatives such as N,N'-methylenebis(meth)acrylamide, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol diacrylate, 2-ethyl-2-butylpropanediol di(meth)acrylate, bisphenol A di(meth)acrylate, bisphenol A ethylene oxide adduct di(meth)acrylate, bisphenol A propylene oxide adduct di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, and the like. esters of (meth)acrylic acid and polyhydric alcohols such as ethyl acrylate, neopentyl glycol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, dioxane glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and EO-modified diglycerin tetra(meth)acrylate; and 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene. Specific examples include Aronix M-220 (manufactured by Toagosei Co., Ltd.), Light Acrylate 1,9ND-A (manufactured by Kyoeisha Chemical Co., Ltd.), Light Acrylate DGE-4A (manufactured by Kyoeisha Chemical Co., Ltd.), Light Acrylate DCP-A (manufactured by Kyoeisha Chemical Co., Ltd.), SR-531 (manufactured by Sartomer Co., Ltd.), CD-536 (manufactured by Sartomer Co., Ltd.), etc. In addition, various epoxy (meth)acrylates, urethane (meth)acrylates, polyester (meth)acrylates, various (meth)acrylate monomers, etc. may be mentioned as necessary.It is preferable to include a polyfunctional (meth)acrylamide derivative in the adhesive composition, since the polyfunctional (meth)acrylamide derivative has a high polymerization rate and excellent productivity, and also has excellent crosslinking properties when the adhesive composition is cured.

[0041] From the viewpoint of achieving both adhesion to the first and second optical films and optical durability under harsh environments, it is preferable to use a monofunctional radically polymerizable compound and a polyfunctional radically polymerizable compound in combination. The amount of the monofunctional radically polymerizable compound in the adhesive composition is preferably 30 to 90 mass%, more preferably 50 to 80 mass%. The amount of the polyfunctional radically polymerizable compound in the adhesive composition is preferably 10 to 70 mass%, more preferably 20 to 50 mass%.

[0042] From the viewpoint of improving the adhesion between the first optical film and the adhesive layer, and further between the first optical film and the second optical film, the adhesive composition used in the present invention may contain a compound represented by the general formula (1) as a curable component. The content of the compound represented by the general formula (1) in the curable adhesive composition is preferably 0.1 to 7 mass%, more preferably 1 to 5 mass%.

[0043] <Embodiments of Radical Polymerization Curable Adhesive Composition> The adhesive composition used in the present invention can be used as an active energy ray-curable adhesive composition when the curable component is an active energy ray-curable component. When ultraviolet light or visible light is used as the active energy ray, it is preferable to contain a photopolymerization initiator as the polymerization initiator.

[0044] The photopolymerization initiator is appropriately selected depending on the active energy ray. When curing is performed by ultraviolet or visible light, a photopolymerization initiator that is cleaved by ultraviolet or visible light is used. Examples of the photopolymerization initiator include benzophenone-based compounds such as benzil, benzophenone, benzoylbenzoic acid, and 3,3'-dimethyl-4-methoxybenzophenone; aromatic ketone compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, and α-hydroxycyclohexylphenylketone; acetophenone-based compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin methyl ether. Examples of the benzoin ether compounds include benzoin butyl ether and anisoin methyl ether; aromatic ketal compounds include benzil dimethyl ketal; aromatic sulfonyl chloride compounds include 2-naphthalenesulfonyl chloride; photoactive oxime compounds include 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; thioxanthone compounds include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone; camphorquinone; halogenated ketones; acylphosphinoxides; and acylphosphonates.

[0045] From the viewpoint of improving the adhesion between the first optical film and the adhesive layer, and further between the first optical film and the second optical film, when a photopolymerization initiator is blended in the adhesive composition in the present invention, the amount is preferably 0.5 to 10 mass %, and more preferably 1 to 5 mass %.

[0046] When the active energy ray-curable adhesive composition is used as a visible light-curable type, it is preferable to use a photopolymerization initiator that is highly sensitive to light of 380 nm or more. Photopolymerization initiators that are highly sensitive to light of 380 nm or more will be described later.

[0047] The photopolymerization initiator may be a compound represented by the following general formula (3): [ka] (In the formula, R 7 and R 8 represents -H, -CH2CH3, -iPr or Cl, R 7 and R 8 It is preferable to use a compound represented by general formula (3) alone (which may be the same or different), or to use a compound represented by general formula (3) in combination with a photopolymerization initiator having high sensitivity to light of 380 nm or more, which will be described later. When a compound represented by general formula (3) is used, the adhesiveness is superior to the case where a photopolymerization initiator having high sensitivity to light of 380 nm or more is used alone. Among the compounds represented by general formula (3), R 7 and R 8 Diethylthioxanthone, in which is -CH2CH3, is particularly preferred. The amount of the compound represented by general formula (3) in the active energy ray-curable adhesive composition is preferably 0.1 to 10 mass %, and more preferably 1 to 5 mass %.

[0048] It is also preferable to add a polymerization initiator aid as necessary. Examples of the polymerization initiator aid include triethylamine, diethylamine, N-methyldiethanolamine, ethanolamine, 4-dimethylaminobenzoic acid, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, and isoamyl 4-dimethylaminobenzoate, with ethyl 4-dimethylaminobenzoate being particularly preferable. When using a polymerization initiator aid, the amount added is preferably 0.1 to 10% by mass, more preferably 1 to 5% by mass.

[0049] If necessary, a known photopolymerization initiator can be used in combination. Since the optical functional layer and the base film having UV absorbing ability do not transmit light of 380 nm or less, it is preferable to use a photopolymerization initiator that is highly sensitive to light of 380 nm or more. Specifically, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(η5-2,4-cyclopentadiene-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, and the like can be mentioned.

[0050] The adhesive composition used in the present invention may contain an acrylic oligomer obtained by polymerizing a (meth)acrylic monomer. By containing the acrylic oligomer in the adhesive composition, it is possible to reduce the cure shrinkage when the composition is irradiated with active energy rays and cured, and to reduce the interfacial stress between the adhesive layer and the first and second optical films, thereby suppressing a decrease in adhesion.

[0051] Considering the workability and uniformity during application, it is preferable that the active energy ray curable adhesive composition has a low viscosity, and therefore it is preferable that the acrylic oligomer obtained by polymerizing the (meth)acrylic monomer also has a low viscosity. As an acrylic oligomer having a low viscosity and capable of preventing the curing shrinkage of the adhesive layer, it is preferable that the weight average molecular weight (Mw) is 15000 or less, more preferably 10000 or less, and particularly preferably 5000 or less. On the other hand, in order to sufficiently suppress the curing shrinkage of the cured product layer (adhesive layer), the weight average molecular weight (Mw) of the acrylic oligomer is preferably 500 or more, more preferably 1000 or more, and particularly preferably 1500 or more. Specific examples of the (meth)acrylic monomer constituting the acrylic oligomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, S-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, t-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,Examples of the methacrylic acid (1 to 20 carbon atoms) alkyl esters include 2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, cetyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and N-octadecyl (meth)acrylate. Examples of the methacrylic acid (1 to 20 carbon atoms) alkyl esters include cycloalkyl (meth)acrylates (e.g., cyclohexyl (meth)acrylate, cyclopentyl (meth)acrylate, and the like), aralkyl (meth)acrylates (e.g., benzyl (meth)acrylate, and the like), polycyclic (meth)acrylates (e.g., 2-isobornyl (meth)acrylate, 2-norbornylmethyl (meth)acrylate, 5-norbornen-2-yl-methyl (meth)acrylate, 3-methyl-2-norbornylmethyl (meth)acrylate, and the like). (meth)acrylate, etc.), hydroxyl group-containing (meth)acrylic acid esters (e.g., hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2,3-dihydroxypropylmethyl-butyl (meth)methacrylate, etc.), alkoxy group- or phenoxy group-containing (meth)acrylic acid esters (2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, etc.), epoxy group-containing (meth)acrylic acid esters (e.g., glycidyl (meth)acrylate, etc.), halogen-containing (meth)acrylic acid esters (e.g., 2,2,2-trifluoroethyl (meth)acrylate, 2,2,Examples of the acrylic oligomer (E) include 2-trifluoroethylethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, etc., and alkylaminoalkyl (meth)acrylates (e.g., dimethylaminoethyl (meth)acrylate, etc.). These (meth)acrylates can be used alone or in combination of two or more. Specific examples of the acrylic oligomer (E) include "ARUFON" manufactured by Toagosei Co., Ltd., "Actflow" manufactured by Soken Chemical & Engineering Co., Ltd., and "JONCRYL" manufactured by BASF Japan Ltd.

[0052] The content of the acrylic oligomer in the adhesive composition is preferably 3 to 40% by mass, and more preferably 5 to 20% by mass.

[0053] The adhesive composition used in the present invention may contain a silane coupling agent.Specific examples of the silane coupling agent include vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane, as active energy ray curable compounds.

[0054] Preferred are 2-(3,4 epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane.

[0055] Specific examples of silane coupling agents other than those mentioned above that are not active energy ray-curable include 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatepropyltriethoxysilane, and imidazole silane.

[0056] The adhesive composition used in the present invention may be a cationic polymerization curable adhesive composition. The cationic polymerizable compound used in the cationic polymerization curable adhesive composition is classified into a monofunctional cationic polymerizable compound having one cationic polymerizable functional group in the molecule and a polyfunctional cationic polymerizable compound having two or more cationic polymerizable functional groups in the molecule. Since the liquid viscosity of the monofunctional cationic polymerizable compound is relatively low, the liquid viscosity can be reduced by including it in the cationic polymerization curable adhesive composition. In addition, the monofunctional cationic polymerizable compound often has a functional group that exhibits various functions, and by including it in the cationic polymerization curable adhesive composition, various functions can be exhibited in the cationic polymerization curable adhesive composition and / or the cured product of the cationic polymerization curable adhesive composition. The polyfunctional cationic polymerizable compound can three-dimensionally crosslink the cured product of the cationic polymerization curable adhesive composition, so it is preferable to include it in the cationic polymerization curable adhesive composition. The ratio of the monofunctional cationic polymerizable compound to the polyfunctional cationic polymerizable compound is preferably in the range of 10 to 1000 parts by mass of the polyfunctional cationic polymerizable compound to 100 parts by mass of the monofunctional cationic polymerizable compound. Examples of the cationic polymerizable functional group include an epoxy group, an oxetanyl group, and a vinyl ether group. Examples of the compound having an epoxy group include an aliphatic epoxy compound, an alicyclic epoxy compound, and an aromatic epoxy compound. It is particularly preferable that the cationic polymerizable adhesive composition of the present invention contains an alicyclic epoxy compound because of its excellent curability and adhesiveness. Examples of alicyclic epoxy compounds include 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, caprolactone-modified 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, trimethylcaprolactone-modified 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, and valerolactone-modified 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate. Specific examples include Celloxide 2021, Celloxide 2021A, Celloxide 2021P, Celloxide 2081, Celloxide 2083, Celloxide 2085 (all manufactured by Daicel Chemical Industries, Ltd.), Cyracure UVR-6105, Cyracure UVR-6107, Cyracure 30, and R-6110 (all manufactured by Dow Chemical Japan, Ltd.).Compounds having an oxetanyl group are preferably contained because they improve the curing property of the cationic polymerizable adhesive composition and reduce the liquid viscosity of the composition. Examples of compounds having an oxetanyl group include 3-ethyl-3-hydroxymethyloxetane, 1,4-bis[(3-ethyl-3-oxetanyl)methoxymethyl]benzene, 3-ethyl-3-(phenoxymethyl)oxetane, di[(3-ethyl-3-oxetanyl)methyl]ether, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, and phenol novolac oxetane, and ARON OXETANE OXT-101, ARON OXETANE OXT-121, ARON OXETANE OXT-211, ARON OXETANE OXT-221, and ARON OXETANE OXT-212 (all manufactured by Toagosei Co., Ltd.) are commercially available. The compound having a vinyl ether group is preferably contained since it has the effect of improving the curing property of the cationic polymerizable adhesive composition and reducing the liquid viscosity of the composition. Examples of the compound having a vinyl ether group include 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, triethylene glycol divinyl ether, cyclohexane dimethanol divinyl ether, cyclohexane dimethanol monovinyl ether, tricyclodecane vinyl ether, cyclohexyl vinyl ether, methoxyethyl vinyl ether, ethoxyethyl vinyl ether, and pentaerythritol tetravinyl ether.

[0057] The cationic polymerization curable adhesive composition contains at least one compound selected from the compounds having an epoxy group, the compounds having an oxetanyl group, and the compounds having a vinyl ether group described above as a curable component, and since all of these are cured by cationic polymerization, a photocationic polymerization initiator is blended. This photocationic polymerization initiator generates cationic species or Lewis acid by irradiation with active energy rays such as visible light, ultraviolet light, X-rays, and electron beams, and initiates the polymerization reaction of the epoxy group or the oxetanyl group. As the photocationic polymerization initiator, a photoacid generator described later is preferably used. In addition, when the cationic polymerizable adhesive composition is used as a visible light curable composition, it is preferable to use a photocationic polymerization initiator that is highly sensitive to light of 380 nm or more, but since photocationic polymerization initiators are generally compounds that show maximum absorption in the vicinity of 300 nm or shorter wavelength range, by blending a photosensitizer that shows maximum absorption in light of a longer wavelength range, specifically, a wavelength longer than 380 nm, it is possible to promote the generation of cationic species or acid from the photocationic polymerization initiator by responding to light of a wavelength in this vicinity. Examples of photosensitizers include anthracene compounds, pyrene compounds, carbonyl compounds, organic sulfur compounds, persulfides, redox compounds, azo and diazo compounds, halogen compounds, photoreducible dyes, etc., and these may be used in combination of two or more. In particular, anthracene compounds are preferred because they have excellent photosensitizing effects, and specific examples include Anthracure UVS-1331 and Anthracure UVS-1221 (manufactured by Kawasaki Chemical Industries, Ltd.). The content of the photosensitizer is preferably 0.1% by mass to 5% by mass, more preferably 0.5% by mass to 3% by mass.

[0058] In the present invention, the active energy ray curable adhesive composition may contain a photoacid generator. When the active energy ray curable adhesive composition contains a photoacid generator, the water resistance and durability of the adhesive layer can be dramatically improved compared to when the adhesive composition does not contain a photoacid generator. The photoacid generator can be represented by the following general formula (3).

[0059] General formula (4) [ka] (However, L + represents any onium cation. - PF66 - , SbF6 - , AsF6 - , SbCl6 - , BiCl5 - , SnCl6 - , ClO4 - , a dithiocarbamate anion, and a counter anion selected from the group consisting of SCN-.

[0060] Next, the counter anion X in the general formula (4) - This article explains:

[0061] Counter anion X in general formula (4) - is not particularly limited in principle, but is preferably a non-nucleophilic anion. - When PF6 is a non-nucleophilic anion, nucleophilic reactions are unlikely to occur with the cations coexisting in the molecule or with various materials used in combination, and as a result, it is possible to improve the stability over time of the photoacid generator represented by general formula (4) itself and compositions using it. The term "non-nucleophilic anion" as used here refers to an anion that has a low ability to cause a nucleophilic reaction. Examples of such anions include PF6 - , SbF6 - , AsF6 - , SbCl6 - , BiCl5 - , SnCl6 - , ClO4 - , B(C6H5)4 - , dithiocarbamate anion, SCN - etc.

[0062] Specifically, these include "Cyracure UVI-6992", "Cyracure UVI-6974" (both manufactured by Dow Chemical Japan Co., Ltd.), "ADEKA OPTOMER SP150", "ADEKA OPTOMER SP152", "ADEKA OPTOMER SP170", "ADEKA OPTOMER SP172" (all manufactured by ADEKA Corporation), "Omnicat250" (manufactured by IGM Resins BV), "CI-5102", "CI-2855" (all manufactured by Nippon Soda Co., Ltd.), "SAN-AID SI-60L", "SAN-AID SI-80L", "SAN-AID SI-100L", "SAN-AID SI-110L", "SAN-AID SI-180L" (all manufactured by Sanshin Chemical Co., Ltd.), "IK-1", "CPI-100P", "CPI-101A", "CPI-110P", "CPI-200K", "CPI-210S", "CPI- Specific preferred examples of the photoacid generator of the present invention include "310B", "CPI-410B", and "CPI-410S" (all manufactured by San-Apro Ltd.), "WPI-069", "WPI-113", "WPI-116", "WPI-041", "WPI-044", "WPI-054", "WPI-055", "WPAG-281", "WPAG-567", and "WPAG-596" (all manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.).

[0063] (First optical film) The first optical film used in the present invention may be a polarizer, a transparent protective film, a retardation film, or the like. In particular, when a polarizer is used as the first optical film, it is preferable because of excellent adhesion between the polarizer and the adhesive layer.

[0064] In the present invention, the polarizer is not particularly limited, and various polarizers can be used. Examples of the polarizer include a hydrophilic polymer film, such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or an ethylene-vinyl acetate copolymer partially saponified film, which is uniaxially stretched after iodine is adsorbed thereon. The thickness of the polarizer is, for example, 3 to 20 μm.

[0065] However, in the present invention, from the viewpoint of improving humidification reliability in a harsh environment of high temperature and high humidity, it is preferable to use a thin polarizer having a thickness of 3 μm or more and 15 μm or less as the polarizer. In particular, it is preferable that the thickness is 12 μm or less, and furthermore, it is preferable that the thickness is 10 μm or less, and particularly, it is preferable that the thickness is 8 μm or less. Such a thin polarizer has little thickness unevenness, excellent visibility, and also has excellent durability against thermal shock due to little dimensional change.

[0066] A polarizer obtained by dyeing a polyvinyl alcohol-based film with iodine and stretching it uniaxially can be produced, for example, by dyeing the polyvinyl alcohol by immersing it in an aqueous solution of iodine and stretching it to 3 to 7 times its original length. If necessary, the polyvinyl alcohol-based film may contain boric acid, zinc sulfate, zinc chloride, or the like, or may be immersed in an aqueous solution of potassium iodide or the like. Furthermore, if necessary, the polyvinyl alcohol-based film may be immersed in water and washed before dyeing. Washing the polyvinyl alcohol-based film with water can wash off dirt and blocking inhibitors on the surface of the polyvinyl alcohol-based film, and also has the effect of preventing unevenness such as uneven dyeing by swelling the polyvinyl alcohol-based film. Stretching may be performed after dyeing with iodine, or may be stretched while dyeing, or may be dyed with iodine after stretching. Stretching can be performed in an aqueous solution of boric acid, potassium iodide, or the like, or in a water bath.

[0067] The polarizer preferably contains boric acid from the viewpoints of stretching stability and humidification reliability. The content of boric acid in the polarizer is preferably 22% by mass or less, more preferably 20% by mass or less, based on the total amount of the polarizer, from the viewpoints of suppressing the occurrence of through cracks. From the viewpoints of stretching stability and humidification reliability, the content of boric acid in the polarizer is preferably 10% by mass or more, more preferably 12% by mass or more, based on the total amount of the polarizer.

[0068] Representative examples of thin polarizers include: Patent No. 4751486 specification, Patent No. 4751481 specification, Patent No. 4815544 specification, Patent No. 5048120 specification, International Publication No. 2014 / 077599, International Publication No. 2014 / 077636, or thin polarizers obtained by the manufacturing methods described therein.

[0069] Among the thin polarizers including the steps of stretching and dyeing the laminate, those obtained by the steps including the steps of stretching in an aqueous boric acid solution as described in Japanese Patent Nos. 4751486, 4751481, and 4815544 are preferred because they can be stretched at a high ratio and have improved polarization performance, and those obtained by the steps including the steps of supplementary air stretching before stretching in an aqueous boric acid solution as described in Japanese Patent Nos. 4751481 and 4815544 are particularly preferred. These thin polarizers can be obtained by the steps including the steps of stretching a polyvinyl alcohol resin (hereinafter also referred to as PVA resin) layer and a resin substrate for stretching in a laminate and the steps of dyeing. With this method, even if the PVA resin layer is thin, it can be stretched without problems such as breakage due to stretching because it is supported by the resin substrate for stretching.

[0070] (Second optical film) The second optical film used in the present invention may be a polarizer, a transparent protective film, a retardation film, or the like. In particular, when a polarizer is used as the first optical film, it is preferable to use a transparent protective film as the second optical film.

[0071] As a material for forming the transparent protective film, for example, a thermoplastic resin excellent in transparency, mechanical strength, thermal stability, moisture blocking property, isotropy, etc. is used. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose-based resin films, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The transparent protective film may contain one or more types of any appropriate additives. Examples of the additives include ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, coloring inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants. The content of the thermoplastic resin in the transparent protective film is preferably 50 to 100% by weight, more preferably 50 to 99% by weight, even more preferably 60 to 98% by weight, and particularly preferably 70 to 97% by weight. If the content of the thermoplastic resin in the transparent protective film is 50% by weight or less, the inherent properties of the thermoplastic resin, such as high transparency, may not be fully exhibited.

[0072] The material for forming the transparent protective film is preferably one having excellent transparency, mechanical strength, thermal stability, moisture barrier properties, isotropy, etc., and in particular, a moisture permeability of 150 g / m 2 / 24h or less is more preferable, and 140g / m 2 / 24h or less is particularly preferred, and 120g / m 2 / 24h or less is even more preferable.

[0073] A functional layer such as a hard coat layer, an anti-reflection layer, an anti-sticking layer, a diffusion layer, an anti-glare layer, etc. may be provided on the surface of the transparent protective film to which the polarizer is not adhered. The functional layer such as the hard coat layer, the anti-reflection layer, the anti-sticking layer, the diffusion layer, the anti-glare layer, etc. may be provided on the transparent protective film itself, or may be provided separately from the transparent protective film.

[0074] The thickness of the transparent protective film can be appropriately determined, but is generally about 1 to 500 μm, preferably 1 to 300 μm, more preferably 5 to 200 μm, further preferably 10 to 200 μm, and more preferably 20 to 80 μm, from the viewpoints of workability such as strength and handleability, thinness, etc.

[0075] As the transparent protective film, a retardation film having a front retardation of 40 nm or more and / or a thickness direction retardation of 80 nm or more can be used. The front retardation is usually controlled to be in the range of 40 to 200 nm, and the thickness direction retardation is usually controlled to be in the range of 80 to 300 nm. When a retardation film is used as the transparent protective film, the retardation film also functions as the transparent protective film, so that a thinner film can be achieved.

[0076] Examples of the retardation film include a birefringent film obtained by uniaxially or biaxially stretching a polymer material, an oriented film of a liquid crystal polymer, and an oriented layer of a liquid crystal polymer supported by a film, etc. The thickness of the retardation film is not particularly limited, but is generally about 20 to 150 μm.

[0077] The retardation film may be one represented by the following formulas (1) to (3): 0.70 <Re

[0450] / Re

[0550] <0.97···(1) 1.5×10 -3 <Δn<6×10 -3 (2) 1.13 <NZ<1.50···(3) (wherein Re

[0450] and Re

[0550] are in-plane retardation values ​​of the retardation film measured at 23° C. with light of wavelengths of 450 nm and 550 nm, respectively, Δn is in-plane birefringence, which is nx-ny, when the refractive indices in the slow axis direction and the fast axis direction of the retardation film are nx and ny, respectively, and NZ is the ratio of thickness direction birefringence, nx-nz, to in-plane birefringence, nx-ny, when nz is the refractive index in the thickness direction of the retardation film) may be used.

[0078] The method for producing a laminated optical film according to the present invention is a method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, and includes a first coating step of coating an easy-adhesion composition containing at least a compound represented by general formula (1) and water on the bonding surface of the first optical film while transporting the first optical film, a second coating step of coating an adhesive composition containing at least a curable component and a polymerization initiator on the bonding surface of the second optical film while transporting the second optical film, a bonding step of bonding the first optical film and the second optical film together, and a bonding step of bonding the first optical film and the second optical film together via an adhesive layer formed by irradiating the first optical film side or the second optical film side with active energy rays to cure at least the adhesive composition. Each step will be described below.

[0079] (Coating process) The method for producing a laminated optical film according to the present invention includes a first coating step of coating an easy-adhesion composition containing at least a compound represented by general formula (1) and water on the lamination surface of the first optical film while conveying the first optical film, and a second coating step of coating an adhesive composition containing at least a curable component and a polymerization initiator on the lamination surface of the second optical film while conveying the second optical film. In the present invention, when the thickness of the easy-adhesion composition after the first coating step is α and the thickness of the adhesive composition after the second coating step is β, β is designed to be greater than α. In order to produce a laminated optical film having excellent adhesion between the first optical film and the second optical film while increasing the line speed of the laminated optical film production line, β is preferably greater than 1.0×α, and more preferably greater than 1.1×α. The thickness α of the easy-adhesion composition after the first coating step is preferably 200 to 2000 nm, and more preferably 300 to 1500 nm. Furthermore, the film thickness β of the adhesive composition after the second coating step is preferably 200 to 2000 nm, and more preferably 300 to 1500 nm.

[0080] The method of applying the adhesive composition and the adhesive composition is appropriately selected depending on the viscosity of the composition and the desired thickness, and examples thereof include a reverse coater, a gravure coater (direct, reverse or offset), a bar reverse coater, a roll coater, a die coater, a bar coater, and a rod coater. The viscosity of the adhesive composition and the adhesive composition is preferably 0.1 to 200 mPa·s, more preferably 1 to 100 mPa·s, and most preferably 5 to 50 mPa·s. If the viscosity of the composition is high, the surface smoothness after application is poor, which is not preferable, and a defective appearance occurs. For this reason, each composition can be heated or cooled to adjust the viscosity to a preferred range and then applied.

[0081] The first optical film and / or the second optical film may be subjected to a surface modification treatment before the coating step. In particular, when a polarizer is used as the first optical film, it is preferable to perform the surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, and itro treatment, and corona treatment is particularly preferable. By performing corona treatment, reactive functional groups such as carbonyl groups and amino groups are generated on the polarizer surface, improving the adhesion with the adhesive layer. In addition, the ashing effect removes foreign matter on the surface and reduces surface unevenness, making it possible to produce a laminated optical film with excellent appearance characteristics.

[0082] (Lamination process) The first optical film and the second optical film are bonded together using a roll laminator or the like via the adhesive composition and the adhesive composition applied as described above.

[0083] In the method for producing a laminated optical film according to the present invention, in order to increase the line speed of the production line, it is preferable not to provide a drying step for removing water contained in the easy-adhesion composition between the first coating step and the lamination step. In addition, in order to increase the line speed of the production line, the time required from the end of the first coating step to the start of the lamination step is preferably within 10 seconds, more preferably within 5 seconds.

[0084] In the present invention, the thickness α of the easy-adhesion composition after the first coating step, the thickness α' of the easy-adhesion composition when the first optical film and the second optical film are bonded together, and the thickness β of the adhesive composition after the second coating step can be measured by in-line measurement while transporting the first optical film and the second optical film. As the thickness meter used for in-line measurement, it is preferable to use an optical (non-contact) thickness meter. The optical (non-contact) thickness meter is not particularly limited, and examples thereof include a spectral interference thickness meter, a reflection spectral thickness meter, and a confocal thickness meter. In particular, a spectral interference thickness meter capable of measuring the thickness of the coating film over the entire width is preferable.

[0085] (Adhesion process) The first optical film and the second optical film are bonded via an adhesive layer formed by curing at least the adhesive composition by irradiating the first optical film side or the second optical film side with active energy rays. The irradiation direction of the active energy rays (electron beams, ultraviolet rays, visible light, etc.) can be any appropriate direction.

[0086] When irradiating with electron beams, any suitable irradiation conditions can be adopted as long as the conditions are such that at least the adhesive composition can be cured. For example, the acceleration voltage of the electron beam irradiation is preferably 5 kV to 300 kV, more preferably 10 kV to 250 kV. If the acceleration voltage is less than 5 kV, the electron beam may not reach the adhesive, resulting in insufficient curing, and if the acceleration voltage is more than 300 kV, the penetration force through the sample is too strong, resulting in damage to the first optical film and the second optical film. The irradiation dose is 5 to 100 kGy, more preferably 10 to 75 kGy. If the irradiation dose is less than 5 kGy, the adhesive may not be cured sufficiently, and if it exceeds 100 kGy, the first optical film and the second optical film may be damaged, resulting in a decrease in mechanical strength and yellowing, and the desired optical properties may not be obtained.

[0087] Electron beam irradiation is usually performed in an inert gas, but may be performed in air or with a small amount of oxygen introduced if necessary. Although it depends on the materials of the first and second optical films, by appropriately introducing oxygen, oxygen inhibition is intentionally generated on the first and second optical film surfaces that are first hit by the electron beam, which makes it possible to prevent damage to the first and second optical films and to efficiently irradiate only the adhesive with the electron beam.

[0088] When manufacturing the laminated optical film according to the present invention, it is preferable to use active energy rays including visible light in the wavelength range of 380nm to 450nm, particularly active energy rays having the largest amount of visible light in the wavelength range of 380nm to 450nm. When using ultraviolet rays and visible light, if a second optical film having ultraviolet absorbing ability is used, such as an ultraviolet non-transmitting transparent protective film, light with a wavelength shorter than about 380nm is absorbed, so that light with a wavelength shorter than 380nm does not reach the adhesive composition and does not contribute to the polymerization reaction. Furthermore, light with a wavelength shorter than 380nm absorbed by the first optical film and the second optical film is converted into heat, and the first optical film and the second optical film themselves generate heat, causing defects such as curling and wrinkling of the laminated optical film. Therefore, when ultraviolet rays and visible light are employed in the present invention, it is preferable to use a device that does not emit light with a wavelength shorter than 380 nm as an active energy ray generator, and more specifically, the ratio of the integrated illuminance in the wavelength range of 380 to 440 nm to the integrated illuminance in the wavelength range of 250 to 370 nm is preferably 100:0 to 100:50, more preferably 100:0 to 100:40. When producing the laminated optical film according to the present invention, the active energy ray is preferably a gallium-encapsulated metal halide lamp or an LED light source that emits light in the wavelength range of 380 to 440 nm. Alternatively, a light source containing ultraviolet rays and visible light such as a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, an incandescent lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a metal halide lamp, a fluorescent lamp, a tungsten lamp, a gallium lamp, an excimer laser, or sunlight can be used, and a bandpass filter can be used to block ultraviolet rays with a wavelength shorter than 380 nm. In order to prevent curling of the laminated optical film while improving the adhesive performance of the adhesive layer between the first optical film and the second optical film, it is preferable to use active energy rays obtained by using a gallium-encapsulated metal halide lamp and passing through a bandpass filter capable of blocking light with wavelengths shorter than 380 nm, or active energy rays with a wavelength of 405 nm obtained by using an LED light source.

[0089] When the laminated optical film according to the present invention is produced on a continuous line, the line speed depends on the curing time of the adhesive composition, but is preferably 1 to 500 m / min, more preferably 5 to 300 m / min, and even more preferably 10 to 100 m / min. If the line speed is too slow, the productivity is poor, or the damage to the first optical film or the second optical film is too great, and a laminated optical film that can withstand a durability test or the like cannot be produced. If the line speed is too high, the adhesive composition is insufficiently cured, and the desired adhesiveness may not be obtained.

[0090] (Laminated optical film) The laminated optical film is formed by laminating at least a first optical film and a second optical film via an adhesive layer, and may also have a pressure-sensitive adhesive layer for bonding to other members such as a liquid crystal cell. The pressure-sensitive adhesive forming the pressure-sensitive adhesive layer is not particularly limited, and may be appropriately selected and used, for example, from a base polymer such as an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyether, a fluorine-based polymer, or a rubber-based polymer. In particular, a pressure-sensitive adhesive that is excellent in optical transparency, exhibits appropriate adhesive properties such as wettability, cohesiveness, and adhesiveness, and is excellent in weather resistance, heat resistance, etc., such as an acrylic pressure-sensitive adhesive, may be preferably used.

[0091] The adhesive layer can be provided on one or both sides of the polarizing film or optical film as a superimposed layer of different compositions or types. When provided on both sides, the adhesive layers on the front and back of the polarizing film or optical film can be different in composition, type, thickness, etc. The thickness of the adhesive layer can be appropriately determined depending on the purpose of use, adhesive strength, etc., and is generally 1 to 500 μm, preferably 1 to 200 μm, and particularly preferably 1 to 100 μm.

[0092] The exposed surface of the adhesive layer is covered with a separator temporarily attached to prevent contamination until it is put into practical use. This prevents contact with the adhesive layer during normal handling. As the separator, apart from the above thickness conditions, any suitable thin material such as a plastic film, a rubber sheet, paper, cloth, nonwoven fabric, net, foam sheet, metal foil, or a laminate thereof, which is coated with a suitable release agent such as a silicone-based, long-chain alkyl-based, fluorine-based, or molybdenum sulfide-based material as necessary, may be used in accordance with conventional methods.

[0093] The laminated optical film can be preferably used for forming various devices such as liquid crystal display devices. The formation of the liquid crystal display device can be carried out in accordance with the conventional method. That is, a liquid crystal display device is generally formed by appropriately assembling components such as a liquid crystal cell, a polarizing film or an optical film, and an optional lighting system, and incorporating a driving circuit, but in the present invention, there is no particular limitation except that the polarizing film or optical film according to the present invention is used, and the method can be carried out in accordance with the conventional method. As for the liquid crystal cell, any type such as TN type, STN type, or π type can be used.

[0094] It is possible to form a suitable liquid crystal display device, such as a liquid crystal display device in which an optical laminate is arranged on one or both sides of a liquid crystal cell, or a display device using a backlight or a reflector in the illumination system. In this case, the optical laminate according to the present invention can be installed on one or both sides of a liquid crystal cell. When optical laminates are provided on both sides, they may be the same or different. Furthermore, when forming a liquid crystal display device, suitable components such as a diffusion plate, an anti-glare layer, an anti-reflection film, a protective plate, a prism array, a lens array sheet, a light diffusion plate, a backlight, etc. can be arranged in one or more layers at suitable positions. EXAMPLES

[0095] Examples of the present invention are described below, but the embodiments of the present invention are not limited thereto.

[0096] <First optical film (polarizer)> A laminate in which a 9 μm-thick PVA layer was formed on an amorphous PET substrate was subjected to air-assisted stretching at a stretching temperature of 130° C. to produce a stretched laminate, and then the stretched laminate was dyed to produce a colored laminate, and the colored laminate was further stretched in boric acid water at a stretching temperature of 65° C. to produce an optical film laminate including a 5 μm-thick PVA layer, which was stretched together with the amorphous PET substrate to a total stretch ratio of 5.94 times. By such two-stage stretching, the PVA molecules of the PVA layer formed on the amorphous PET substrate were highly oriented, and an optical film laminate including a 5.5 μm-thick PVA layer was obtained, which constitutes a thin polarizer in which iodine adsorbed by dyeing was highly oriented in one direction as a polyiodine ion complex. The thin polarizer obtained here was used as the first optical film.

[0097] <Second optical film (transparent protective film)> Transparent protective film: Triacetyl cellulose resin film (product name "TJ25", manufactured by Fujifilm) The above transparent protective film was used as the second optical film.

[0098] <Active energy rays> Visible light (gallium-filled metal halide lamp) as active energy rays Irradiation device: Light HAMMER10 manufactured by Fusion UV Systems, Inc. Bulb: V bulb Peak illuminance: 1600mW / cm 2 , cumulative dose 1000 / mJ / cm 2 The illuminance of visible light was measured using a Sola-Check system manufactured by Solatell.

[0099] Example 1 (Preparation of Easy-Adhesion Composition) An easily adhesive composition was prepared using 65 mass% N-acryloylmorpholine (a compound represented by general formula (2) (trade name "ACMO", manufactured by Kojinsha)), 7 mass% 3-methacrylamidophenylboronic acid (a compound represented by general formula (1) (trade name "MAPBA", manufactured by Junsei Chemical Industry Co., Ltd.)), 27.8 mass% pure water, and 0.2 mass% surface conditioner (trade name "EXP.4200", manufactured by Nissin Chemical Industry Co., Ltd.).

[0100] (Adjustment of Adhesive Composition) An adhesive composition was prepared using 40.2% by mass of N-acryloylmorpholine (a compound represented by general formula (2) (trade name "ACMO", manufactured by Kohjin Co., Ltd.)), 2.9% by mass of 3-methacrylamidophenylboronic acid (a compound represented by general formula (1) (trade name "MAPBA", manufactured by Junsei Chemical Co., Ltd.)), 52.6% by mass of tripropylene glycol diacrylate (TPGDA) (trade name "Aronix M-220", manufactured by Toagosei Co., Ltd.), 1.9% by mass of 2-methyl-4'-methylthio-2-morpholinopropiophenone (a photopolymerization initiator (trade name "Omnirad 907", manufactured by IGM Resins BV)), 1.9% by mass of diethylthioxanthone (a photopolymerization initiator (trade name "KAYACURE DETX-S", manufactured by Nippon Kayaku Co., Ltd.)), and 0.5% by mass of a surface conditioner (trade name "EXP.4200", manufactured by Nissin Chemical Industry Co., Ltd.).

[0101] (Manufacture of laminated optical films (polarizing films)) The adhesive composition was applied to the bonding surface of the first optical film (thin polarizer) using an MCD coater (manufactured by Fuji Machine Co., Ltd.) (cell shape: honeycomb, gravure roll line number: 1000 / inch, rotation speed 200% / to line speed) (first coating step). The thickness α of the adhesive composition after the first coating step was 550 nm. The adhesive composition was applied to the bonding surface of the second optical film (transparent protective film) using an MCD coater (manufactured by Fuji Machine Co., Ltd.) (cell shape: honeycomb, gravure roll line number: 1000 / inch, rotation speed 160% / to line speed) (second coating step). The thickness β of the adhesive composition after the second coating step was 600 nm. The film thicknesses α and β were measured by in-line measurement using a spectroscopic interference film thickness meter (Ocean Optics: spectrometer "USB2000+", light source "HL-2000", fiber "OCF-103995").

[0102] Next, the transparent protective film and the optical film laminate including the thin polarizer were laminated from the coated side by a roller (lamination process). No drying process was provided between the first coating process and the lamination process, and the time required from the first coating process to the lamination process was designed to be 3 seconds.

[0103] Thereafter, the above-mentioned visible light was irradiated from the laminated transparent protective film side by an active energy ray irradiation device to cure the easy-adhesion composition and the adhesive composition, thereby bonding the thin polarizer and the transparent protective film via the adhesive layer obtained. Next, the amorphous PET substrate of the optical film laminate was peeled off to produce a laminated optical film (polarizing film).

[0104] Examples 2-3 and Comparative Examples 1-2 A laminated optical film (polarized film) was produced in the same manner as in Example 1, except that the film thickness α (nm) of the easy-adhesion composition after the first coating step and the film thickness β (nm) of the adhesive composition after the second coating step were changed to those shown in Table 1.

[0105] Example 4 (Preparation of Easy-Adhesion Composition) An easily adhesive composition was prepared using 77.8 mass% N-acryloylmorpholine (a compound represented by general formula (2) (trade name "ACMO", manufactured by Kojinsha)), 7 mass% 3-methacrylamidophenylboronic acid (a compound represented by general formula (1) (trade name "MAPBA", manufactured by Junsei Chemical Industry Co., Ltd.)), 15 mass% pure water, and 0.2 mass% surface conditioner (trade name "EXP.4200", manufactured by Nissin Chemical Industry Co., Ltd.).

[0106] A laminated optical film (polarized film) was produced in the same manner as in Example 1, except that the film thickness α (nm) of the easy-adhesion composition after the first coating step and the film thickness β (nm) of the adhesive composition after the second coating step were changed to those shown in Table 1.

[0107] <Evaluation of water-resistant peel strength (water-resistant adhesion)> A double-sided tape (No. 500, manufactured by Nitto Denko Corporation) was attached to the PET release surface of the polarizing film. In addition, a piece was cut into a size of 200 mm parallel to the stretching direction of the thin polarizer and 15 mm in the perpendicular direction, and a cut was made between the thin polarizer and the transparent protective film with a cutter knife, after which the release film of the double-sided tape was peeled off and the adhesive surface was attached to a glass plate. Next, the obtained polarizing film attached to the glass plate was exposed to an environment of 20°C and 98% RH for 240 hours, and then removed. After removing excess moisture, the thin polarizer and the transparent protective film were peeled off in the 90° direction at a peeling speed of 1000 mm / min using an angle-free type adhesive / film peeling analyzer (VPA-2, manufactured by Kyowa Interface Science Co., Ltd.), and the peel strength (N / 15 mm) was measured. ○: >1.5N or more, △: 1.0N or more but less than 1.5N, ×: less than 1.0N

[0108] [Table 1]

Claims

1. A method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, comprising the steps of: While transporting the first optical film, a compound having at least the following general formula (1): 【Chemistry 1】 (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent; R 1 and R 2 each independently represents a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group which may have a substituent) and water; a second coating step of coating an adhesive composition containing at least a curable component and a polymerization initiator onto a bonding surface of the second optical film while transporting the second optical film; a bonding step of bonding the first optical film and the second optical film; and a bonding step of bonding the first optical film and the second optical film via the adhesive layer formed by irradiating the first optical film surface side or the second optical film surface side with active energy rays to cure at least the adhesive composition, The content of the water in the easily adhesive composition is 40% by mass or less, A method for producing a laminated optical film, characterized in that, when the film thickness of the easy-adhesion composition after the first coating step is α and the film thickness of the adhesive composition after the second coating step is β, β>α.

2. The method for producing a laminated optical film according to claim 1 , wherein a drying step is not provided between the first coating step and the laminating step.

3. The method for producing a laminated optical film according to claim 1 , wherein the time required from the end of the first coating step to the start of the laminating step is within 5 seconds.

4. The method for producing a laminated optical film according to claim 1 , wherein the first optical film is a polarizer.

5. The method for producing a laminated optical film according to claim 1 , wherein the second optical film is a transparent protective film.

6. The adhesive composition contains, as a polymerizable component, a polymerizable compound represented by the following general formula (2): 【Chemistry 2】 A compound represented by the formula (wherein R 4 is a hydrogen atom or a methyl group, R 5 and R 6 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or a cyclic ether group, and R 5 and R 6 The method for producing a laminated optical film according to claim 1 , further comprising the step of:

7. The method for producing a laminated optical film according to claim 1 , wherein the adhesive composition contains a compound represented by the general formula (2).

Citation Information

Patent Citations

  • Method for manufacturing polarizing plate and liquid crystal display device

    JP2001296427A

  • Active energy ray-curable resin composition, adhesive layer, polarizing plate, optical film, and image display device

    JP2012052000A

  • Method for manufacturing polarization film

    JP2020160391A

Cited By

  • Polarizing film

    WO2026115773A1

  • Method for producing polarizing film

    WO2026115774A1