Optical laminate and image display unit

The optical laminate with coaxially laminated polarizers and a retardation layer addresses the visual distinction issue in image display devices, ensuring seamless appearance from various viewing angles.

JP2024162454APending Publication Date: 2024-11-21NITTO DENKO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023077967
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Image display devices with colored areas around the display screen exhibit noticeable differences in appearance between the display and non-display areas when the screen is off, which affects design harmony.

Method used

An optical laminate is constructed with two polarizers coaxially laminated and a retardation layer with specific optical properties between them, along with a printed layer, to minimize the visual distinction between the display and non-display areas when viewed from different angles.

Benefits of technology

The configuration effectively reduces the visibility of the boundary between the display and non-display areas, enhancing design cohesion by making the difference difficult to recognize from both front and oblique directions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162454000001_ABST
    Figure 2024162454000001_ABST
Patent Text Reader

Abstract

To provide an image display device that is provided with a colored part forming a display area and a non-display area on a display screen and that hardly has differences in appearance between the display area and non-display area recognized at nondisplay time.SOLUTION: An optical laminate includes a first polarizing plate including a first polarizer, a phase difference layer having a thickness-directional phase difference, a printing layer, and a second polarizing plate including a second polarizer in this order, where the phase difference layer includes a phase difference film having birefringence in a thickness direction, and the absorption axis direction of the first polarizer and the absorption axis direction of the second polarizer are substantially parallel.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical laminate and an image display device. [Background technology]

[0002] In recent years, automobiles are equipped with displays for various purposes such as various instrument displays, car navigation, rear monitors, audiovisuals, etc. In such in-vehicle displays, a colored portion is generally provided along the periphery of the display screen for the purpose of harmonizing the appearance with the frame member of the display itself and peripheral members such as the instrument panel and console, and for the purpose of shielding wiring, terminals, etc., thereby forming a display area and a non-display area. In addition, in tablet terminals for general or commercial use, a colored portion is often provided along the periphery of the display screen.

[0003] In image display devices in which a colored portion is provided along the outer periphery of the display screen, the difference in appearance between the display area (black screen) and the non-display area (colored portion) may be noticeable when no display is in progress (when the power is off), and improvements are required from the standpoint of design.

[0004] In relation to the above demand, Patent Document 1 proposes a display device in which the color difference between the display area and the non-display area during non-display is reduced, but there is a demand for further improvement. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-192708 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made to solve the above problems, and its main object is to provide an image display device having colored sections that form display areas and non-display areas on a display screen, in which the difference in appearance between the display area and the non-display area when not in use is difficult to perceive. [Means for solving the problem]

[0007] In order to solve the above problem, the inventors have intensively studied and found that, in an image display device, by laminating two polarizers coaxially on the viewing side of a display element and providing a printed layer (colored portion) between them, it is possible to make it difficult to recognize the difference in appearance between the display area and the non-display area when not displaying. On the other hand, with such a configuration, the difference in appearance tends to be more noticeable when observed from an oblique direction than when observed from the front direction. Therefore, the inventors have further studied and found that by laminating two polarizers coaxially on the viewing side of a display element and providing a retardation layer having a predetermined optical property and a printed layer between them in this order toward the viewing side, the difference in appearance becomes difficult to recognize in both the front direction and the oblique direction, and have completed the present invention. That is, according to an embodiment of the present invention, the following optical laminate and image display device are provided.

[0008] [1] An optical laminate according to an embodiment of the present invention includes, in this order, a first polarizing plate including a first polarizer, a retardation layer having a retardation in a thickness direction, a printed layer, and a second polarizing plate including a second polarizer, wherein the retardation layer includes a retardation film having birefringence in the thickness direction, and the absorption axis direction of the first polarizer and the absorption axis direction of the second polarizer are substantially parallel to each other. [2] In the optical laminate described in [1] above, the absolute value of the thickness direction retardation value Rth(550) of the retardation layer (more specifically, the absolute value of the sum of Rth(550) of all retardation films having birefringence in the thickness direction included in the first retardation layer) may be 100 nm or more. [3] In the optical laminate described in [1] or [2] above, the retardation film having birefringence in the thickness direction may include a retardation film having a refractive index characteristic of nx>ny>nz, nx>nz>ny, or nz>nx=ny, where "nx" is the refractive index in the slow axis direction, "ny" is the refractive index in the fast axis direction, and "nz" is the refractive index in the thickness direction. [4] In the optical laminate described in either [1] or [3] above, the retardation film having birefringence in the thickness direction may have an in-plane retardation, and the slow axis direction thereof may be substantially parallel to the slow axis directions of the first polarizer and the second polarizer. [5] In the optical laminate according to either [1] or [4] above, the printed layer may have a thickness of 3 μm to 30 μm. [6] The optical laminate according to either [1] or [5] above may further include a surface substrate layer on the side of the second polarizing plate opposite to the side on which the retardation layer is disposed. [7] An image display device according to an embodiment of the present invention comprises a display element and an optical laminate described in either [1] or [6] above, in that order toward a viewing side, and the optical laminate is arranged so that the second polarizing plate is on the viewing side relative to the first polarizing plate. [8] In the image display device according to [7] above, the display element may include a liquid crystal cell, an organic electronic element, or an inorganic electronic element. [9] The image display device according to [7] or [8] above may further include a touch panel.

[10] In the image display device described in any one of [7] to [9] above, the display element may be a liquid crystal cell, and may include, in this order toward the viewing side, a third polarizing plate including a third polarizer, the liquid crystal cell, and the optical laminate. Effect of the Invention

[0009] The optical laminate according to the embodiment of the present invention includes a first polarizing plate including a first polarizer, a retardation layer having a predetermined optical property, a printed layer, and a second polarizing plate including a second polarizer, in this order, and the absorption axis direction of the first polarizer and the absorption axis direction of the second polarizer are substantially parallel. By disposing the optical laminate having such a configuration on the viewing side of a display element, it is possible to make it difficult to recognize the difference in appearance between the display area and the non-display area when the image display device obtained is observed from the front direction and from an oblique direction. [Brief description of the drawings]

[0010] [Figure 1A] FIG. 1A is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention, and FIG. 1B is a schematic top view of the optical laminate shown in FIG. [Figure 1B] 1 is a schematic cross-sectional view of an optical laminate according to one embodiment of the present invention. [Figure 2A] 1 is a schematic cross-sectional view of an image display device according to one embodiment of the present invention. [Figure 2B] 1 is a schematic cross-sectional view of an image display device according to one embodiment of the present invention. [Figure 2C] 1 is a schematic cross-sectional view of an image display device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, preferred embodiments of the present invention will be described, but the present invention is not limited to these embodiments. In this specification, the term "to" indicating a range of values ​​includes the upper and lower limits.

[0012] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re. (5)Angle When an angle is mentioned in this specification, the angle includes both clockwise and counterclockwise with respect to a reference direction unless otherwise specified. Thus, for example, "45°" means 45° clockwise or counterclockwise. In addition, in this specification, "substantially parallel" and "approximately parallel" include cases within the range of 0°±10°, preferably within the range of 0°±5°, more preferably within the range of 0°±3°, and even more preferably within the range of 0°±1°, and "substantially perpendicular" and "approximately perpendicular" include cases within the range of 90°±10°, preferably within the range of 90°±5°, more preferably within the range of 90°±3°, and even more preferably within the range of 90°±1°. (6) The terms "layer," "plate," "sheet," and "film" are not to be distinguished from one another solely on the basis of differences in name. For example, the term "layer" is a concept that includes members that may be called "plate," "sheet," and "film."

[0013] A. Optical laminate The optical laminate according to the embodiment of the present invention includes a first polarizing plate including a first polarizer, a retardation layer having a retardation in the thickness direction (hereinafter also referred to as "first retardation layer"), a print layer, and a second polarizing plate including a second polarizer, in this order, and the first retardation layer includes a retardation film having birefringence in the thickness direction, and the absorption axis direction of the first polarizer and the absorption axis direction of the second polarizer are substantially parallel. The optical laminate is preferably used in an image display device, and in this case, the optical laminate is disposed on the viewing side of a display element such as an organic electroluminescence (EL) element, an inorganic EL element, or a liquid crystal cell, such that the second polarizing plate is closer to the viewing side than the first polarizing plate. According to this configuration, it is possible to make it difficult to recognize the difference in appearance between the display area and the non-display area when the image display device is not displayed when observed from the front direction and from an oblique direction. In this specification, making it difficult to recognize (making it less noticeable) the difference in appearance between the display area and the non-display area may be referred to as "seamlessness between the display area and the non-display area".

[0014] A-1. Overall configuration of optical laminate FIG. 1A is a schematic cross-sectional view (a) and a schematic top view (b) of an optical laminate according to one embodiment of the present invention. In the optical laminate 100A shown in FIG. 1A, a first polarizing plate 10 including a first polarizer 12, a first retardation layer 20 having a retardation in the thickness direction, and a second polarizing plate 30 including a second polarizer 32 are arranged in this order, and a printed layer 40 is provided on a part of the main surface of the second polarizing plate 30 on the side where the first retardation layer 20 is arranged. In the optical laminate 100A, the absorption axis direction of the first polarizer 12 and the absorption axis direction of the second polarizer 32 are substantially parallel. The first retardation layer 20 having a retardation in the thickness direction includes a retardation film having birefringence in the thickness direction. In FIG. 1A, the printed layer 40 is provided with a predetermined width along the outer edge of the main surface of the second polarizing plate 30 on the first retardation layer 20 side. When an image display device is constructed by placing the optical laminate 100A on the viewing side of a display element, part A of the display screen where the printing layer 40 is not provided becomes the display area, and part B where the printing layer 40 is provided becomes the non-display area, thereby making it possible to conceal components such as wiring and terminals arranged around the display element.

[0015] In the optical laminate 100A, a surface substrate layer 50 is disposed on the viewing side (the side opposite to the side on which the first retardation layer 20 is disposed) of the second polarizing plate 30. The surface substrate layer 50 can function as a front plate of the image display device. The surface substrate layer 50 may be omitted depending on the purpose.

[0016] FIG. 1B is a schematic cross-sectional view of an optical laminate according to another embodiment of the present invention. The optical laminate 100B shown in FIG. 1B is different from the optical laminate 100A in that a second retardation layer 60 is provided on the side opposite to the side on which the first retardation layer 20 of the first polarizing plate 10 is arranged. The second retardation layer 60 functions as a circular polarizing plate together with the first polarizing plate 10, for example. When applied to an organic EL display device, the optical laminate 100B can suitably achieve anti-reflection function and seamlessness.

[0017] Each member constituting the optical laminate may be bonded via any suitable adhesive layer (adhesive layer, adhesive layer, etc.), or may simply be laminated without an adhesive layer. In the illustrated example, the first retardation layer 20 and the second polarizing plate 30 are bonded via an adhesive layer 70. The optical laminates 100A and 100B may further include an adhesive layer for bonding adjacent members such as a display element on the outside of the first polarizing plate 10 and the second retardation layer 60, respectively. In this case, the adhesive layer is typically protected by a release liner until it is used. Also, unlike the illustrated example, the printing layer 40 may be provided on the surface of the first retardation layer 20 on the second polarizing plate 30 side.

[0018] The total light transmittance of the display region of the optical laminate exceeds 35.0%, for example, and is preferably 39.0% to 42.5%, and more preferably 42.5% to 45%.

[0019] The thickness of the optical laminate is, for example, 100 μm to 4000 μm, and preferably 200 μm to 2000 μm.

[0020] A-2. First polarizing plate and second polarizing plate Each of the first polarizing plate 10 and the second polarizing plate 30 includes a polarizer, and typically includes a protective layer provided on one or both sides of the polarizer. The first polarizing plate and the second polarizing plate may have the same configuration or different configurations. Unless otherwise specified, the following description applies to the polarizer and protective layer that the first polarizing plate and the second polarizing plate may include.

[0021] A-2-1. Polarizer The polarizer is typically made of a polyvinyl alcohol-based resin film containing a dichroic material (e.g., iodine). The polarizer may be made of a single-layer resin film or may be made of a laminate of two or more layers.

[0022] Specific examples of polarizers made of a single-layer resin film include hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films that have been dyed with iodine or a dichroic substance such as a dichroic dye and stretched, and polyene-based oriented films such as dehydrated PVA films and dehydrochlorinated polyvinyl chloride films. A polarizer obtained by dyeing a PVA film with iodine and uniaxially stretching it is preferably used because of its excellent optical properties.

[0023] The dyeing with iodine is carried out, for example, by immersing the PVA-based film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be carried out after the dyeing treatment, or may be carried out while dyeing. Alternatively, the film may be stretched and then dyed. If necessary, the PVA-based film may be subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like. For example, by immersing the PVA-based film in water and washing it with water before dyeing, it is possible to wash off dirt and antiblocking agents on the surface of the PVA-based film, and also to swell the PVA-based film and prevent uneven dyeing, etc.

[0024] Specific examples of polarizers obtained using laminates include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer coated on the resin substrate can be produced by, for example, applying a PVA-based resin solution to the resin substrate and drying the resin substrate to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; stretching and dyeing the laminate to make the PVA-based resin layer a polarizer. In this embodiment, stretching typically includes immersing the laminate in an aqueous solution of boric acid to stretch it. Furthermore, stretching may further include, as necessary, stretching the laminate in air at a high temperature (for example, 95°C or higher) before stretching in the aqueous solution of boric acid. The obtained laminate of resin substrate / polarizer may be used as it is (i.e., the resin substrate may be used as a protective layer for the polarizer), or the resin substrate may be peeled off from the laminate of resin substrate / polarizer, and any suitable protective layer may be laminated on the peeled surface depending on the purpose. Details of such a method for producing a polarizer are described in, for example, JP2012-73580A. The entire disclosure of this publication is incorporated herein by reference.

[0025] The thickness of the polarizer is, for example, 30 μm or less, preferably 15 μm or less, more preferably 1 μm to 12 μm, further preferably 2 μm to 10 μm, and further more preferably 2 μm to 8 μm.

[0026] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer is, for example, 41.0% or more, preferably 43.0% to 46.0%, and more preferably 44.5% to 46.0%. The degree of polarization of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more.

[0027] A-2-2.Protective layer The protective layer is composed of any suitable film that can be used as a protective layer for a polarizer. Specific examples of materials that are the main components of the film include cellulose-based resins such as triacetyl cellulose (TAC), polyester-based resins, polyvinyl alcohol-based resins, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, polyethersulfone-based resins, polysulfone-based resins, polystyrene-based resins, polynorbornene-based resins, polyolefin-based resins, (meth)acrylic resins, acetate-based resins, and other transparent resins. In addition, examples include thermosetting resins or ultraviolet-curing resins such as (meth)acrylic, urethane, (meth)acrylic urethane, epoxy, and silicone. In addition, examples include glassy polymers such as siloxane-based polymers. In addition, polymer films described in JP-A-2001-343529 (WO01 / 37007) can also be used. The material for this film may be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain, and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. The polymer film may be, for example, an extrusion molded product of the above resin composition.

[0028] The thickness of the protective layer is typically 300 μm or less, preferably 100 μm or less, more preferably 5 μm to 80 μm, and further preferably 10 μm to 60 μm. When a surface treatment is applied, the thickness of the protective layer includes the thickness of the surface treatment layer.

[0029] A-3. First retardation layer The first retardation layer 20 has a retardation in the thickness direction. The first retardation layer 20 includes a retardation film having birefringence in the thickness direction. The first retardation layer may include only one retardation film having birefringence in the thickness direction, or may include two or more. By disposing such a retardation layer between the first polarizing plate, the printing layer, and the second polarizing plate, when the optical laminate is disposed on the viewing side of the display element, light leakage in the oblique direction can be suppressed, and as a result, the seamlessness in the oblique direction can be improved. In the present specification, the "retardation film having birefringence in the thickness direction" means a retardation film in which ny / nz is less than 1 or greater than 1, and preferably has an Nz coefficient of 0.9 or less or 1.1 or more. The "retardation film having birefringence in the thickness direction" typically does not include a retardation film (positive A plate) having refractive index characteristics of nx>ny=nz and an isotropic film. Here, "ny=nz" includes not only the case where ny and nz are exactly equal, but also the case where they are substantially equal. Therefore, the positive A plate may have an Nz coefficient exceeding 0.9 and less than 1.1, for example. The isotropic film means a film satisfying the relationship of Re(550)<10 nm and -10 nm<Rth(550)<10 nm.

[0030] The absolute value of the retardation value Rth(550) in the thickness direction of the first retardation layer is preferably 100 nm or more, and may be, for example, 250 nm or more, 400 nm or more, or 550 nm or more. The upper limit of the absolute value of Rth(550) of the first retardation layer is not particularly limited, but may be, for example, 1000 nm or less. When Rth(550) of the first retardation layer is in such a range, the effects of the present invention can be preferably obtained. When the first retardation layer includes two or more retardation films, Rth(550) of the first retardation layer is obtained as the sum of Rth(550) of all the retardation films having birefringence in the thickness direction included in the first retardation layer.

[0031] As the retardation film having birefringence in the thickness direction, any appropriate retardation film can be used as long as the effect of the present invention can be obtained. For example, a retardation film having a refractive index characteristic of nz>nx=ny, nx=ny>nz, nx>ny>nz, nx>nz>ny, or nz>nx>ny can be preferably exemplified, and among them, a retardation film having a refractive index characteristic of nz>nx=ny, nx>ny>nz, or nx>nz>ny is preferable. Note that, when a retardation film having birefringence in the thickness direction has an in-plane phase difference (for example, when it has Re(550) of 10 nm or more or 20 nm or more, for example, 200 nm or less), the retardation film is preferably arranged so that its slow axis direction is substantially parallel to the absorption axis direction of the first polarizer and the second polarizer.

[0032] The retardation film having birefringence in the thickness direction can be used alone or in combination with the same or different retardation films (for example, retardation films having different retardation values, refractive index characteristics, forming materials, etc.) so that the retardation value (for example, Rth(550)) in the thickness direction of the first retardation layer is in a desired range. The number of retardation films to be combined is not limited as long as the effects of the present invention can be obtained. When a plurality of retardation films are used in combination, each retardation film can be integrated via an adhesive layer.

[0033] The retardation value in the thickness direction of the retardation film (positive C plate) having the refractive index characteristic of nz>nx=ny can be appropriately set according to the retardation value desired for the first retardation layer, the presence or absence of a retardation film to be used in combination or its retardation value, manufacturability, etc., and can be, for example, -50 nm or less, -200 nm or less, or -400 nm or less. In one embodiment, the positive C plate has an Rth(550) of -50 nm to -300 nm, preferably -70 nm to -250 nm, more preferably -90 nm to -200 nm. The Re(550) of the positive C plate can be less than 10 nm.

[0034] The positive C plate may be formed of any appropriate material. The positive C plate is preferably made of a film containing a liquid crystal material fixed in homeotropic alignment. The liquid crystal material (liquid crystal compound) that can be homeotropically aligned may be a liquid crystal monomer or a liquid crystal polymer. Specific examples of the liquid crystal compound and the method for forming the positive C plate include the liquid crystal compound and the method for forming the retardation film described in

[0020] to

[0028] of JP-A-2002-333642. In this case, the thickness of the positive C plate is preferably 0.5 μm to 10 μm, more preferably 0.5 μm to 8 μm, and even more preferably 0.5 μm to 5 μm.

[0035] The retardation value in the thickness direction of the retardation film (negative B plate) having a refractive index characteristic of nx>ny>nz can be appropriately set depending on the retardation value desired for the first retardation layer, the presence or absence of a retardation film to be used in combination or its retardation value, manufacturability, etc. In one embodiment, the negative B plate has an Rth(550) of, for example, 50 nm to 400 nm, preferably 70 nm to 350 nm, and more preferably 90 nm to 300 nm. The Nz coefficient of the negative B plate is, for example, 1.1 or more, preferably 3 or more, and more preferably 5 or more.

[0036] The negative B plate is formed, for example, from a resin film formed of any suitable resin that can realize the above-mentioned characteristics. Examples of the resin that forms this resin film include polycarbonate-based resin, cyclic olefin-based resin, cellulose-based resin, polyester-based resin, polyvinyl alcohol-based resin, polyamide-based resin, polyimide-based resin, polyether-based resin, polystyrene-based resin, acrylic resin, and polyester carbonate resin. Among these, cyclic olefin-based resin or polycarbonate-based resin can be preferably used.

[0037] Cyclic olefin resin is a general term for resins polymerized with cyclic olefins as polymerization units, and examples of such resins include those described in JP-A-1-240517, JP-A-3-14882, and JP-A-3-122137. Specific examples include ring-opening (co)polymers of cyclic olefins, addition polymers of cyclic olefins, copolymers (typically random copolymers) of cyclic olefins with α-olefins such as ethylene and propylene, and graft modified products obtained by modifying these with unsaturated carboxylic acids and their derivatives, as well as hydrogenated products thereof. Specific examples of cyclic olefins include norbornene monomers. Examples of norbornene monomers include monomers described in JP-A-2015-210459 and the like. Various products of the above cyclic olefin resins are commercially available. Specific examples include Zeon Corporation's product names "ZEONEX" and "ZEONOR", JSR Corporation's product name "Arton", TICONA Corporation's product name "TOPUS", and Mitsui Chemicals' product name "APEL".

[0038] As the polycarbonate-based resin, any suitable polycarbonate-based resin can be used as long as the effects of the present invention can be obtained. Preferably, the polycarbonate-based resin contains a structural unit derived from an isosorbide-based dihydroxy compound, and a structural unit derived from at least one dihydroxy compound selected from the group consisting of an alicyclic diol, an alicyclic dimethanol, a di-, tri- or polyethylene glycol, and an alkylene glycol or a spiroglycol. More preferably, the polycarbonate-based resin contains a structural unit derived from an isosorbide-based dihydroxy compound, and a structural unit derived from an alicyclic dimethanol and / or a structural unit derived from a di-, tri- or polyethylene glycol. The polycarbonate-based resin may contain a structural unit derived from another dihydroxy compound as necessary. Details of the polycarbonate-based resin and the method for producing the retardation film that can be suitably used in the present invention are described, for example, in International Publication No. 2011 / 062239, and the description is incorporated herein by reference.

[0039] The negative B plate is produced by stretching the resin film. The stretching temperature and stretching ratio are appropriately set according to the retardation value and thickness in the thickness direction desired for the negative B plate, the type of resin used, Tg, etc.

[0040] The thickness of the negative B plate is, for example, 10 μm to 150 μm, preferably 10 μm to 100 μm, and more preferably 10 μm to 30 μm.

[0041] The thickness direction retardation value of the retardation film (Z plate) having the refractive index characteristic of nx>nz>ny can be appropriately set according to the retardation value desired for the first retardation layer, the presence or absence of a retardation film to be used in combination or its retardation value, manufacturability, etc. In one embodiment, the Z plate has an Rth(550) of, for example, 50 nm to 300 nm, preferably 70 nm to 250 nm, and more preferably 90 nm to 200 nm. The Nz coefficient of the Z plate is, for example, 0.1 to 0.5, preferably 0.15 to 0.45, and more preferably 0.2 to 0.4.

[0042] Z-plate is typically formed from a resin film formed of any suitable resin that can realize the above-mentioned characteristics.The resin that forms this resin film can be, for example, polycarbonate-based resin, cyclic olefin-based resin, cellulose-based resin, polyester-based resin, polyvinyl alcohol-based resin, polyamide-based resin, polyimide-based resin, polyether-based resin, polystyrene-based resin, acrylic resin, polyester carbonate resin.Among these, cyclic olefin-based resin or polycarbonate-based resin is preferably used, and the cyclic olefin-based resin or polycarbonate-based resin that can form Z-plate can be preferably exemplified.

[0043] The Z plate can be formed, for example, by applying a coating liquid in which the above-mentioned resin is dissolved or dispersed in any suitable solvent to a shrinkable film to form a coating film, and then shrinking the coating film. Typically, the coating film is shrunk by heating a laminate of the shrinkable film and the coating film to shrink the shrinkable film, and the coating film is shrunk by the shrinkage of the shrinkable film. The shrinkage rate of the coating film is preferably 0.50 to 0.99, more preferably 0.60 to 0.98, and even more preferably 0.70 to 0.95. The heating temperature is preferably 130°C to 170°C, and more preferably 150°C to 160°C. In one embodiment, when shrinking the coating film, the laminate may be stretched in a direction perpendicular to the shrinkage direction. In this case, the stretching ratio of the laminate is preferably 1.01 times to 3.0 times, more preferably 1.05 times to 2.0 times, and even more preferably 1.10 times to 1.50 times. Specific examples of materials constituting the shrinkable film include polyolefin resins, polyester resins, acrylic resins, polyamide resins, polycarbonate resins, norbornene resins, polystyrene resins, polyvinyl chloride resins, polyvinylidene chloride resins, cellulose resins, polyethersulfone resins, polysulfone resins, polyimide resins, acetate resins, polyarylate resins, polyvinyl alcohol resins, and liquid crystal polymers. These may be used alone or in combination. The shrinkable film is preferably a stretched film formed from these materials.

[0044] The thickness of the Z plate is, for example, 10 μm to 150 μm, preferably 10 μm to 100 μm, and more preferably 10 μm to 30 μm.

[0045] The thickness (total thickness) of the first retardation layer is, for example, 1 μm to 500 μm, and preferably 1 μm to 300 μm.

[0046] A-4.Printing layer The printing layer 40 is a colored layer that is colored by printing according to the application and the desired design. The printing layer may be a design layer with a predetermined design, or may be a solid colored layer. The printing layer is preferably a solid colored layer, more preferably a colored layer of a deep dark color such as black, blue, navy blue, purple, brown, etc. (for example, L* in the L*a*b* color space of the SCI system is 50 or less, a* value is +10 to -10, and b* value is +10 to -10), and even more preferably a colored layer of black (for example, L* in the L*a*b* color space of the SCI system is 20 or less, a* value is +5 to -5, and b* value is +5 to -5). By making the printing layer a black colored layer, wiring, terminals, backlights, and other components can be suitably concealed in the non-display area.

[0047] The printing layer may be formed in any suitable pattern according to the purpose. Typically, the printing layer may be formed in a frame shape along the outer periphery of the main surface of the polarizing plate, for example, at a position corresponding to the bezel. With this configuration, the non-display area can be concealed without using a bezel.

[0048] The print layer can be formed by any suitable printing method using the print layer-forming composition. Specific examples of the printing method include gravure printing, offset printing, silk screen printing, and transfer printing from a transfer sheet.

[0049] The composition for forming a print layer typically contains a colorant, a solvent and / or a binder, and any suitable additives that may be used as necessary. Examples of binders include chlorinated polyolefins (e.g., chlorinated polyethylene, chlorinated polypropylene), polyester resins, urethane resins, acrylic resins, vinyl acetate resins, vinyl chloride-vinyl acetate copolymers, and cellulose resins. The binder resins may be used alone or in combination of two or more. In one embodiment, the binder resin is a thermally polymerizable resin. Since the thermally polymerizable resin requires less use than the photopolymerizable resin, the amount of colorant used (colorant content in the colored layer) can be increased. As a result, particularly when forming a black colored layer, a colored layer having a very small total light transmittance and excellent concealing properties can be formed. In one embodiment, the binder resin is a (meth)acrylic resin, and is preferably a (meth)acrylic resin containing a polyfunctional monomer (e.g., pentaerythritol tri(meth)acrylate) as a copolymerization component. By using a (meth)acrylic resin containing a polyfunctional monomer as a copolymerization component, a printing layer having an appropriate elastic modulus can be formed. In addition, a step is formed due to the thickness of the printing layer, and the step can effectively function to prevent blocking.

[0050] As the coloring material, any suitable coloring material can be used depending on the purpose and the desired color. The coloring material may be a pigment or a dye, and is preferably a pigment. Specific examples of the coloring material include inorganic pigments such as titanium white, zinc white, carbon black, iron black, red iron oxide, chrome vermilion, ultramarine blue, cobalt blue, yellow lead, and titanium yellow; organic pigments or dyes such as phthalocyanine blue, indanthrene blue, isoindolinone yellow, benzidine yellow, quinacridone red, polyazo red, perylene red, and aniline black; metal pigments made of scaly foil such as aluminum and brass; and pearlescent pigments (pearl pigments) made of scaly foil such as titanium dioxide-coated mica and basic lead carbonate. When forming a black colored layer, carbon black, iron black, and aniline black are preferably used. In this case, it is preferable to use the coloring material in combination. This is because it is possible to form a colored layer that is colorless (i.e., jet black) by absorbing visible light widely and evenly. For example, in addition to the above coloring materials, azo compounds and / or quinone compounds can be used. In one embodiment, the coloring material contains carbon black as a main component and other coloring materials (for example, an azo compound and / or a quinone compound). With this configuration, a colored layer that is not colored and has excellent stability over time can be formed. When forming a black colored layer, the coloring material can be used in a ratio of preferably 50 parts by weight to 200 parts by weight with respect to 100 parts by weight of the binder resin. In this case, the content ratio of carbon black in the coloring material is preferably 80% to 100%. By using the coloring material (particularly carbon black) in such a ratio, a colored layer that has a very small total light transmittance and excellent stability over time can be formed.

[0051] The total light transmittance of the printed layer is preferably 0.01% or less, and more preferably 0.008% or less. If the total light transmittance is in this range, the non-display area of ​​the image display device can be concealed satisfactorily.

[0052] The thickness of the printed layer is, for example, 3 μm to 30 μm, preferably 5 μm to 20 μm, and more preferably 10 μm to 15 μm. If the thickness of the printed layer is within this range, a seamless effect between the display area and the non-display area can be suitably obtained.

[0053] A-5.Surface base material layer The surface substrate layer 50 can function as a front panel of an image display device. Therefore, the surface substrate layer is preferably disposed at a position that becomes the outermost surface when the optical laminate is disposed on the viewing side of a display element. The surface substrate layer includes a substrate film, and may further include a functional layer such as an anti-reflection layer, an antifouling layer, or a hard coat layer, as necessary. The surface substrate layer preferably includes an anti-reflection layer. Examples of the anti-reflection layer include a thin layer type that prevents reflection by utilizing the cancellation effect of reflected light due to the interference of light as disclosed in JP-A-2005-248173, and a surface structure type that develops low reflectance by imparting a fine structure to the surface as disclosed in JP-A-2011-2759. The functional layer can be used in combination of one type or two or more types. The functional layer may be laminated on the substrate film via an adhesive layer (e.g., a pressure-sensitive adhesive layer, an adhesive layer) in a state where it is formed on a support film as necessary, or may be formed directly on the substrate film without an adhesive layer.

[0054] As the substrate film, a glass film (inorganic glass film) or a resin film can be used.

[0055] Glass constituting the glass film can be classified according to composition, for example, soda-lime glass, borate glass, aluminosilicate glass, and quartz glass. Also, can be classified according to alkali component, for example, alkali-free glass and low-alkali glass. The thickness of the glass film is preferably 100 μm to 2000 μm, and more preferably 200 μm to 1000 μm.

[0056] Examples of the resin constituting the resin film include polyethylene terephthalate resins, polyethylene naphthalate resins, acetate resins, polyethersulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyamideimide resins, polyolefin resins, (meth)acrylic resins, polyvinyl chloride resins, polyvinylidene chloride resins, polystyrene resins, polyvinyl alcohol resins, polyarylate resins, and polyphenylene sulfide resins. Among these, polyamide resins, polyimide resins, polyamideimide resins, polyethylene naphthalate resins, and polycarbonate resins are preferred, and polyimide resins are more preferred. These resins may be used alone or in combination of two or more. The thickness of the resin film is preferably 100 μm to 2000 μm, and more preferably 200 μm to 1000 μm.

[0057] A-6.Adhesive layer As the adhesive layer, any suitable pressure-sensitive adhesive layer or adhesive layer applicable to optical applications may be used. The total light transmittance of the adhesive layer is preferably 85% or more, more preferably 88% or more. The haze of the adhesive layer is preferably 1.0% or less, more preferably 0.8% or less. In one embodiment, the first retardation layer 20 and the second polarizing plate 30 are bonded together via a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer can suitably fill the step at the end of the printing layer 40 provided between the first retardation layer 20 and the second polarizing plate 30.

[0058] Any suitable adhesive composition may be used as the adhesive composition constituting the adhesive layer. For example, rubber-based, acrylic-based, silicone-based, urethane-based, vinyl alkyl ether-based, polyvinyl alcohol-based, polyvinyl pyrrolidone-based, polyacrylamide-based, cellulose-based, and other adhesive compositions may be used. Among them, acrylic adhesive compositions are preferably used because of their excellent optical transparency, adhesion properties, weather resistance, heat resistance, and the like.

[0059] The thickness of the adhesive layer used to bond the first retardation layer 20 and the second polarizing plate 30 (thickness in the display region) is, for example, 50 μm to 1000 μm, preferably 200 μm to 750 μm, and more preferably 250 μm to 500 μm. The thickness of the adhesive layer used to bond any other component member can be, for example, 1 μm to 300 μm, preferably 5 μm to 100 μm, and more preferably 10 μm to 50 μm.

[0060] Any suitable adhesive composition may be used as the adhesive composition constituting the adhesive layer. For example, water-based adhesives, solvent-based adhesives, emulsion-based adhesives, solventless adhesives, active energy ray curable adhesives, and heat-curable adhesives may be used. Examples of active energy ray curable adhesives include electron beam curable adhesives, ultraviolet ray curable adhesives, and visible light curable adhesives. Preferably, a heat-curable adhesive or an ultraviolet ray curable adhesive is used.

[0061] The thickness of the adhesive layer is preferably 0.01 μm to 3.0 μm, more preferably 0.1 μm to 2.5 μm, and further preferably 0.5 μm to 1.5 μm.

[0062] A-7. Second retardation layer The second retardation layer 60 functions, for example, as a circular polarizing plate together with the first polarizing plate. The second retardation layer preferably includes a retardation film (hereinafter simply referred to as a "λ / 4 plate") that functions as a λ / 4 plate. The λ / 4 plate has a Re(550) of, for example, 120 nm to 160 nm, preferably 135 nm to 155 nm. The λ / 4 plate may have a refractive index characteristic of, for example, nx>ny≧nz. The Nz coefficient of the λ / 4 plate is preferably 0.9 to 1.5, more preferably 0.9 to 1.3. The λ / 4 plate may be disposed such that its slow axis direction forms an angle of, for example, 45°±10°, preferably 45°±5°, more preferably 45° with the absorption axis direction of the first polarizer. The λ / 4 plate preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. Re(450) / Re(550) at λ / 4 is, for example, 0.75 or more and less than 1, and may be 0.8 or more and 0.95 or less.

[0063] The second retardation layer may include a retardation film (hereinafter simply referred to as "lambda / 2 plate") that functions as a lambda / 2 plate in addition to the lambda / 4 plate. The lambda / 2 plate has a Re(550) of, for example, 210 nm to 280 nm, preferably 230 nm to 240 nm. The lambda / 2 plate may have a refractive index characteristic of, for example, nx>ny≧nz. The Nz coefficient of the lambda / 2 plate is preferably 0.9 to 1.5, more preferably 0.9 to 1.3. The lambda / 2 plate may be disposed between the first polarizing plate and the lambda / 4 plate. The angle between the absorption axis of the first polarizer and the slow axis of the lambda / 4 plate is preferably 65° to 85°, more preferably 72° to 78°, and even more preferably about 75°. The angle between the absorption axis of the first polarizer and the slow axis of the λ / 2 plate is preferably from 10° to 20°, more preferably from 13° to 17°, and further preferably about 15°.

[0064] When the optical laminate including the second retardation layer is used in combination with an organic EL element, it can exhibit excellent anti-reflection function in addition to seamlessness. The λ / 4 plate and the λ / 2 plate can be composed of, for example, a stretched film of a resin film or an oriented solidified layer of a liquid crystal compound. Such λ / 4 plate and λ / 2 plate are well known to those skilled in the art, so detailed description thereof will be omitted.

[0065] B. Image display device An image display device according to an embodiment of the present invention includes a display element and the optical laminate described in section A, in this order toward the viewing side, and the optical laminate is arranged so that the second polarizing plate is closer to the viewing side than the first polarizing plate. An image display device having such a configuration has excellent seamlessness when observed from the front and oblique directions, and therefore has excellent design properties.

[0066] In the SCI system L*a*b* color space of the display area when not displayed, for example, L* is preferably 15 or less, more preferably 10 or less, a* is preferably -10 to +10, more preferably -5 to +5, and b* is preferably -10 to +10, more preferably -5 to +5. In the SCE system L*a*b* color space of the display area when not displayed, L* is preferably 10 or less, more preferably 5 or less, a* is preferably -10 to +10, more preferably -5 to +5, and b* is preferably -10 to +10, more preferably -5 to +5.

[0067] The L*a*b* color difference (CIE 1976) ΔE*ab of the SCI method between the display area and the non-display area when not displayed is preferably less than 20, more preferably 15 or less, and even more preferably 10 or less. The L*a*b* color difference (CIE 1976) ΔE*ab of the SCE method is preferably less than 5, more preferably 3 or less, and even more preferably 1 or less. The L*a*b* color difference (CIE 1976) ΔE*ab when measured (received light) at a polar angle of 45° is preferably less than 5, more preferably 3 or less, and even more preferably 1 or less. If ΔE*ab is within the above range, the difference in appearance between the display area and the non-display area when not displayed is difficult to recognize. The L*a*b* color difference (CIE 1976) ΔE*ab is a value calculated by the following formula (wherein L* represents lightness, a* represents chromaticity a*, and b* represents chromaticity b*). ΔE*ab=〔(ΔL*) 2 +(Δa*) 2 +(Δb*) 2 〕 1 / 2

[0068] The reflectance of the SCI system in the display area when not displayed is preferably less than 5%, more preferably 3% or less, and even more preferably 1% or less. The reflectance in the non-display area is preferably 3% or less, more preferably 2% or less, and even more preferably 1% or less. The difference in reflectance between the two areas is preferably 3% or less, and more preferably 1% or less.

[0069] The reflectance of the SCE system in the display area when not displayed is preferably 3% or less, more preferably 2% or less, and even more preferably 1% or less. The reflectance in the non-display area is preferably 3% or less, more preferably 2% or less, and even more preferably 1% or less. The difference in reflectance between the two areas is preferably 3% or less, and more preferably 1% or less.

[0070] The reflectance when measured (light received) at a polar angle of 45° in the display area in the non-display state is preferably 5% or less, more preferably 3% or less, and even more preferably 1% or less. The reflectance in the non-display area is preferably 3% or less, more preferably 2% or less, and even more preferably 1% or less. The difference in reflectance between the two areas is preferably 3% or less, and more preferably 1% or less.

[0071] Examples of the display element include a liquid crystal cell, an organic EL element, an inorganic EL element, etc. The display element may further include a touch panel. These display elements are well known to those skilled in the art, so detailed description thereof will be omitted.

[0072] 2A is a schematic cross-sectional view of an image display device (liquid crystal display device) including a liquid crystal cell as a display element. The image display device 200A includes a backlight unit 110, a third polarizing plate 120 including a third polarizer, a liquid crystal cell 130, and an optical laminate 100A, in this order toward the viewing side. Preferably, the optical laminate 100A has an adhesive layer (not shown) on the outer side of the first polarizing plate 10, and is bonded to the liquid crystal cell 130 via the adhesive layer. In addition, the optical laminate 100A is typically arranged so that the absorption axis direction of the first polarizing plate 10 (first polarizer 12) and the absorption axis direction of the third polarizing plate 120 (third polarizer) are substantially perpendicular to each other, and the first polarizing plate 10, the liquid crystal cell 130, and the third polarizing plate 120 constitute a liquid crystal panel.

[0073] 2B is a schematic cross-sectional view of an image display device (organic EL display device) including an organic EL element as a display element. The image display device 200B includes an organic EL element 140 and an optical laminate 100B in this order toward the viewing side. The optical laminate 100B is bonded to the organic EL element 140 via, for example, a pressure-sensitive adhesive layer (not shown) provided on the outer side of the second retardation layer 60.

[0074] 2C is a schematic cross-sectional view of an image display device (organic EL display device) including a touch panel and an organic EL element as a display element. Image display device 200C includes organic EL element 140, touch panel 150, and optical laminate 100B in this order toward the viewing side. These members are preferably bonded together via an adhesive layer (not shown). In the illustrated example, the touch panel is an out-cell type disposed on the viewing side of the display element, but the touch panel may be incorporated into the display element by an on-cell type or an in-cell type. EXAMPLES

[0075] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties are as follows. (1) Thickness Measurements were made using a digital gauge (manufactured by Ozaki Manufacturing Co., Ltd., product name "PEACOCK"). (2) Single transmittance and polarization degree of polarizer The polarizing plate (protective layer / polarizer / protective layer) was measured using an ultraviolet-visible-near infrared spectrophotometer (V-7100 manufactured by JASCO Corporation) to obtain the single transmittance Ts, parallel transmittance Tp, and crossed transmittance Tc, which were taken as Ts, Tp, and Tc, respectively, of the polarizer. These Ts, Tp, and Tc are Y values ​​measured using a 2-degree visual field (C light source) according to JIS Z8701 and corrected for visibility. The degree of polarization was calculated from the obtained Tp and Tc using the following formula. Degree of polarization (%)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100 (3) Refractive index (nx, ny, nz), Re(λ), and Rth(λ) Measurements were performed using an Axoscan manufactured by Axometrics, Inc. The measurement wavelength was 550 nm and the measurement temperature was 23°C.

[0076] [Production Example 1A: Retardation film A (negative B plate) having a refractive index characteristic of nx>ny>nz] As the retardation film A having a refractive index characteristic of nx>ny>nz, a commercially available retardation film (a stretched film of a cyclic olefin resin film, Zeon Corporation, “ZeonorFilm (R) The retardation film A had a Re(550) of 55 nm and a Rth(550) of 275 nm.

[0077] [Production Example 1B: Retardation film B (positive C plate) having refractive index characteristics of nz>nx=ny] A liquid crystal coating solution was prepared by dissolving 20 parts by weight of a side-chain liquid crystal polymer represented by the following chemical formula (1) (the numbers 65 and 35 in the formula indicate the mole percent of the monomer unit, and are conveniently represented as a block polymer: weight average molecular weight 5000), 80 parts by weight of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: trade name Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (manufactured by Ciba Specialty Chemicals: trade name Irgacure 907) in 200 parts by weight of cyclopentanone. The coating solution was then applied to a PET substrate that had been subjected to a vertical alignment treatment using a bar coater, and the liquid crystal was aligned by heating and drying at 80°C for 4 minutes. The liquid crystal layer was irradiated with ultraviolet light to harden the liquid crystal layer, thereby forming a liquid crystal alignment solidified layer (thickness 3 μm) on the substrate. This liquid crystal alignment solidified layer had a refractive index characteristic of nz>nx=ny, Re(550) was 0 nm, and Rth(550) was -135 nm. [ka]

[0078] [Production Example 1C: Retardation film C (Z plate) having refractive index characteristics of nx>nz>ny] A 60 μm thick shrinkable film (Toray Industries, Inc., product name "Torayfan BO2873") was laminated on both sides of a commercially available cyclic olefin resin film (manufactured by JSR Corporation, product name "Arton (R5000)", thickness: 130 μm, Tg: 137 ° C.) via an acrylic adhesive layer (thickness 15 μm), and subjected to free end uniaxial stretching to obtain a retardation film C having a refractive index characteristic of nx>nz>ny. The stretching temperature was 146 ° C., and the stretching ratio was 1.38 times. The Re (550) of the obtained retardation film C was 270 nm, and the Rth (550) was 135 nm.

[0079] [Production Example 1D: Retardation film D (positive A plate) having a refractive index characteristic of nx>ny=nz] A commercially available retardation film (Kaneka Corporation, "UTZ-Film #270", thickness: 33 μm) was prepared as the retardation film D having a refractive index characteristic of nx>ny=nz. The Re(550) and Rth(550) of the retardation film D were 270 nm and 270 nm, respectively.

[0080] [Production Example 2: Polarizing Plate A] 1. Preparation of Polarizer A polyvinyl alcohol film having an average polymerization degree of 2,400, a saponification degree of 99.9 mol%, and a thickness of 45 μm was prepared. The polyvinyl alcohol film was stretched 2.2 times in the conveying direction while swelling by immersing in a swelling bath (water bath) at 20 ° C. between rolls with different peripheral speed ratios (swelling step), and then stretched 3.3 times in the conveying direction based on the original polyvinyl alcohol film (polyvinyl alcohol film not stretched at all in the conveying direction) while dyeing by immersing in a dyeing bath (aqueous solution with an iodine concentration of 0.1 wt % and a potassium iodide concentration of 0.9 wt %) at 30 ° C. (dyeing step). Next, the dyed polyvinyl alcohol film was immersed in a crosslinking bath (aqueous solution with a boric acid concentration of 3.0 wt % and a potassium iodide concentration of 3.0 wt %) at 40 ° C. for 28 seconds to stretch 3.6 times in the conveying direction based on the original polyvinyl alcohol film (crosslinking step). The obtained polyvinyl alcohol film was then immersed in a 61°C stretching bath (aqueous solution with a boric acid concentration of 4.0% by weight and a potassium iodide concentration of 5.0% by weight) for 60 seconds to stretch the film to 6.0 times the original polyvinyl alcohol film in the conveying direction (stretching step), and then immersed in a 20°C washing bath (aqueous solution with a potassium iodide concentration of 2.0% by weight) for 10 seconds (washing step). The washed polyvinyl alcohol film was dried at 40°C for 30 seconds to produce a polarizer. The polarizer had a thickness of 18 μm.

[0081] 2. Preparation of Polarizing Plate A As the adhesive, an aqueous solution containing a polyvinyl alcohol resin containing an acetoacetyl group (average polymerization degree 1,200, saponification degree 98.5 mol%, acetoacetylation degree 5 mol%) and methylolmelamine in a weight ratio of 3:1 was used. Using this adhesive, a 30 μm-thick transparent protective film (manufactured by Nippon Shokubai Co., Ltd.) made of a (meth)acrylic resin (modified acrylic polymer having a lactone ring structure) was laminated as a protective layer on one side (display element side) of the polarizer obtained above, and a 49 μm-thick transparent protective film made of a triacetyl cellulose film (manufactured by Fuji Film Co., Ltd., product name "TJ40UL") with HC was laminated as a protective layer on the other side (viewing side) using a roll laminator, and then heated and dried in an oven (temperature 90°C, time 10 minutes) to produce a polarizing plate A in which the transparent protective film was laminated on both sides of the polarizer. The single transmittance of the obtained polarizer was 41.7%, and the polarization degree was 99.9%.

[0082] [Manufacture example 3: Printing layer forming composition A] A coloring material (black pigment), "HF GV3 RX01" manufactured by Seiko Advance Corporation, was impregnated into the solvent at a concentration of 10% by weight to obtain a black print layer forming composition A.

[0083] [Production example 4: Adhesive layer A] A monomer mixture consisting of 60 parts by weight of butyl acrylate (BA), 6 parts by weight of cyclohexyl acrylate (CHA), 26 parts by weight of 4-hydroxybutyl acrylate (4HBA), and 8 parts by weight of hydroxyethyl acrylate (HEA) was added to a four-neck flask with 0.09 parts by weight of 2,2-dimethoxy-1,2-diphenyl-1-one (trade name "Irgacure 651", manufactured by BASF Japan) and 0.09 parts by weight of 1-hydroxy-cyclohexyl-phenyl-ketone (trade name "Irgacure 184", manufactured by BASF Japan), and the mixture was exposed to ultraviolet light under a nitrogen atmosphere to cause partial photopolymerization, thereby obtaining a partially polymerized product (monomer syrup) with a polymerization rate of about 10%. To 100 parts by weight of this partial polymer, 0.12 parts by weight of dipentaerythritol hexaacrylate ("KAYARAD DPHA" manufactured by Nippon Kayaku Co., Ltd.) as a multifunctional polymerizable compound and 0.3 parts by weight of 3-glycidoxypropyltrimethoxysilane ("KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd.) as a silane coupling agent were added and mixed uniformly to prepare an adhesive (adhesive composition). Thus, adhesive composition A was obtained.

[0084] The adhesive composition A obtained above was applied to a 38 μm thick release liner R1 (Mitsubishi Plastics, Inc., MRF#38) having a release surface on one side of a polyester film, and then covered with a 38 μm thick release liner R2 (Mitsubishi Plastics, Inc., MRE#38) having a release surface on one side of a polyester film to block out air. The adhesive composition A was then cured by irradiating with ultraviolet light to form an adhesive layer A (thickness 250 μm, total light transmittance 92.0%, haze 0.3%).

[0085] [Manufacturing example 5: Surface base material layer A] An anti-reflective film (manufactured by Nitto Denko Corporation, product name "T-60LA28HCAR6N", thickness 85 μm) having a structure of anti-reflective layer / TAC film was attached to one side of a 1 mm thick glass film (manufactured by Matsunami Glass Industry Co., Ltd., product name "Soda Lime Glass") via an adhesive layer A, to obtain a surface substrate layer A having a structure of [glass film / TAC film / anti-reflective layer].

[0086] [Example 1] The polarizing plate A was cut into a rectangular shape to form a second polarizing plate. The printed layer forming composition A was applied by silk screen printing along the outer periphery of the (meth)acrylic resin film side surface of the second polarizing plate in a frame shape with a width of 1.5 mm in plan view, and naturally dried to form a black printed layer with a thickness of 5 μm. Next, the printed layer was similarly applied again by silk screen printing to the printed layer, and dried at 50 ° C. for 1 hour to form a black printed layer with a thickness of 5 μm (final printed layer thickness: 10 μm). Next, the adhesive layer A was transferred from the release liner to the side of the second polarizing plate on which the printed layer was formed, and the retardation film A was further laminated thereon so that the absorption axis direction of the second polarizing plate and the slow axis direction of the retardation film A were parallel to each other. At this time, the step portion at the boundary between the printed layer and the second polarizing plate was completely filled with the adhesive layer A, and no voids were generated. Next, a surface base material layer was attached to the surface of the obtained laminate on the second polarizing plate side via an acrylic adhesive (thickness: 250 μm), thereby obtaining a laminate 1 having a structure of [surface base material layer A / second polarizing plate / printed layer A / adhesive layer A / retardation film A].

[0087] The polarizing plate A was cut into a rectangular shape to obtain a first polarizing plate. A reverse dispersion retardation film (a stretched film of a polycarbonate-based resin film, Re(550)=147 nm) capable of functioning as a λ / 4 plate was attached to the first polarizing plate via an adhesive layer so that the slow axis direction of the film was at an angle of 45° with the absorption axis direction of the first polarizing plate, to obtain a circular polarizing plate 1.

[0088] A glass plate was attached to the surface of the laminate 1 obtained above opposite to the surface base material layer A via an acrylic adhesive (thickness: 23 μm) to obtain a laminate 1 with a glass plate attached. A laminate 1 with a glass plate was attached to the first polarizing plate side of the circular polarizing plate 1 via an acrylic adhesive (thickness 23 μm), and another glass plate was attached to the λ / 4 plate side via an acrylic adhesive (thickness 23 μm). At this time, the surface base layer A of the laminate 1 with a glass plate was arranged to be the outermost layer, and the absorption axis directions of the first polarizing plate and the second polarizing plate were arranged parallel to each other. This resulted in an optical laminate 1 having a configuration of [surface base layer A / second polarizing plate / printed layer A / adhesive layer A / retardation film A / glass plate / first polarizing plate / λ / 4 plate / glass plate]. In the optical laminate 1, the glass plate was provided from the viewpoint of ease of handling during characteristic evaluation.

[0089] [Example 2] A laminate 2 having a structure of [surface base material layer A / second polarizing plate / printed layer A / adhesive layer A / retardation film A / retardation film B] was obtained in the same manner as in Example 1, except that the retardation film A and the retardation film B were laminated in this order on the adhesive layer A. The lamination (transfer) of the retardation film B was performed by attaching the retardation film B to the retardation film A via an adhesive, and then peeling off the base material. An optical laminate 2 was obtained in the same manner as in Example 1, except that the laminate 2 was used instead of the laminate 1.

[0090] [Example 3] A laminate 3 having a structure of [surface base material layer A / second polarizing plate / printed layer A / adhesive layer A / retardation film A / retardation film A] was obtained in the same manner as in Example 1, except that two retardation films A were laminated on the adhesive layer A via an acrylic adhesive (thickness 23 μm). The two retardation films A were arranged so that the slow axis directions were both parallel to the absorption axis direction of the second polarizing plate. An optical laminate 3 was obtained in the same manner as in Example 1, except that the laminate 3 was used instead of the laminate 1.

[0091] [Example 4] A laminate 4 having a structure of [surface base material layer A / second polarizing plate / printed layer A / adhesive layer A / retardation film C] was obtained in the same manner as in Example 1, except that a retardation film C was laminated on the adhesive layer A. The retardation film C and the second polarizing plate were arranged so that their slow axis directions were parallel to each other. An optical laminate 4 was obtained in the same manner as in Example 1, except that the laminate 4 was used instead of the laminate 1.

[0092] [Example 5] A laminate 5 having a structure of [surface base material layer A / second polarizing plate / printed layer A / adhesive layer A / retardation film C / retardation film C] was obtained in the same manner as in Example 1, except that two retardation films C were laminated on the adhesive layer A via an acrylic adhesive (thickness 23 μm). The two retardation films C were arranged so that the slow axis directions were both parallel to the absorption axis direction of the second polarizing plate. An optical laminate 5 was obtained in the same manner as in Example 1, except that the laminate 5 was used instead of the laminate 1.

[0093] [Example 6] A laminate 6 having a structure of [surface base material layer A / second polarizing plate / printed layer A / adhesive layer A / retardation film B] was obtained in the same manner as in Example 1, except that a retardation film B was laminated (transferred) onto the adhesive layer A. An optical laminate 6 was obtained in the same manner as in Example 1, except that the laminate 6 was used instead of the laminate 1.

[0094] [Example 7] A laminate 7 having a structure of [surface substrate layer A / second polarizing plate / printed layer A / adhesive layer A / retardation film B / retardation film B] was obtained in the same manner as in Example 1, except that two sheets of retardation film B were laminated (transferred) onto the adhesive layer A via an acrylic adhesive layer (thickness 23 μm). Optical laminate 7 was obtained in the same manner as in Example 1, except that laminate 7 was used instead of laminate 1.

[0095] [Example 8] A laminate 8 having a structure of [surface base material layer A / second polarizing plate / printed layer A / adhesive layer A / retardation film B / retardation film B / retardation film B] was obtained in the same manner as in Example 1, except that three sheets of retardation film B were laminated (transferred) onto the adhesive layer A via an acrylic adhesive layer (thickness 23 μm). An optical laminate 8 was obtained in the same manner as in Example 1, except that the laminate 8 was used instead of the laminate 1.

[0096] [Example 9] A laminate 9 having a structure of [surface base material layer A / second polarizing plate / printed layer A / adhesive layer A / retardation film B / retardation film B / retardation film B / retardation film B] was obtained in the same manner as in Example 1, except that four sheets of retardation film B were laminated (transferred) onto the adhesive layer A via an acrylic adhesive layer (thickness 23 μm). An optical laminate 9 was obtained in the same manner as in Example 1, except that the laminate 9 was used instead of the laminate 1.

[0097] [Comparative Example 1] A laminate C1 having a structure of [surface substrate layer A / second polarizing plate / printed layer A / adhesive layer A] was obtained in the same manner as in Example 1, except that no retardation film was laminated on top of the adhesive layer A. An optical laminate C1 was obtained in the same manner as in Example 1, except that the laminate C1 was used instead of the laminate 1.

[0098] [Comparative Example 2] A laminate C2 having a structure of [surface base material layer A / second polarizing plate / printed layer A / adhesive layer A / retardation film D] was obtained in the same manner as in Example 1, except that a retardation film D was laminated on the adhesive layer A. The retardation film D and the second polarizing plate were arranged so that their slow axis directions were parallel to each other. An optical laminate C2 was obtained in the same manner as in Example 1, except that the laminate C2 was used instead of the laminate 1.

[0099] [Comparative Example 3] A laminate C3 having the structure of [surface base material layer A / second polarizing plate / printing layer A / adhesive layer A / retardation film D / retardation film D] was obtained in the same manner as in Example 1 except that two retardation films D were laminated on the adhesive layer A via an acrylic adhesive (thickness: 23 μm). Note that the slow axis directions of the two retardation films D were arranged to be parallel to the absorption axis direction of the second polarizing plate. An optical laminate C3 was obtained in the same manner as in Example 1 except that the laminate C3 was used instead of the laminate 1.

[0100] Table 1 and Table 2 show the structures (excluding the glass plate), various measurement results, and the evaluation results of the seamless property of the optical laminates 1 to 9 and C1 to C3 obtained above. Note that the display area and the non-display area are the areas where the printing layer is not formed and the area where it is formed, respectively, in plan view. <L*a*b* color space, color difference ΔE*ab, and reflectance> An acrylic adhesive was used to bond the optical laminate onto a reflector (manufactured by Toray Film Co., Ltd., trade name "DMS-X42") to prepare a measurement sample. At this time, it was bonded so that the surface on the glass plate side faced the reflector. For the said measurement sample, the spectral reflectance was measured under the following measurement conditions, and L*a*b* was obtained. Note that for the reflectance in the oblique direction (polar angle 45°), the maximum value of the measured values measured omnidirectionally was adopted. (Measurement conditions) Front direction: Using a spectrocolorimeter (manufactured by Konica Minolta, "CM-2600d"), the measurement sample was illuminated by the diffuse illumination method, and light was received by the SCI (including specularly reflected light) method or the SCE (excluding specularly reflected light) method. Oblique direction: Using a display measurement system (manufactured by Konica Minolta, "DMS505"), the measurement sample was illuminated from the normal direction of the main surface, and light was received at an angle of 45° with respect to the normal. Measurement wavelength range: 360 nm - 740 nm Light source: D65 Measurement diameter MAV: φ8 mm Also, the color difference (ΔE*ab) was calculated by the following formula. ΔE*ab = 〔(ΔL*) 2 +(Δa*)2 +(Δb*) 2 〕 1 / 2 <Brightness> The backlight was removed from the liquid crystal display device. The optical laminate was placed on the backlight so that the glass plate side surface faced the backlight, and the luminance when the backlight was turned on was measured using a "Conoscope" manufactured by AUTRONIC MELCHERS. The measurements were performed in two directions, the front direction and the oblique direction (polar angle 45°), and the minimum value measured in all directions in the oblique direction was used. <Seamlessness> A reflector (manufactured by Toray Films, product name "DMS-X42") was attached to the glass plate side of the optical laminates 1 to 9 and C1 to C3 via an acrylic adhesive layer (thickness 23 μm) to prepare an evaluation sample. With the fluorescent lamp turned on, the optical laminate was visually observed from the surface base layer side at a polar angle of 45° from all directions, and the boundary visibility between the display area and the non-display area was evaluated. The evaluation criteria were as follows. [Evaluation Criteria] ×: No change compared to ref 〇: Slight improvement compared to ref ◎: Significant improvement compared to the reference [Table 1] [Table 2]

[0101] As shown in Table 1, in the optical laminate of the Example, the color difference of the reflected light in the oblique direction between the display area and the non-display area is smaller than that of the optical laminate of Comparative Example 1, and the seamlessness evaluation result is also excellent. From this, when the optical laminate of the Example is applied to an image display device, the seamlessness when observed from an oblique direction can be improved compared to the case of applying the optical laminate of Comparative Example 1. On the other hand, in Comparative Examples 2 and 3 in which the first retardation layer does not include a retardation film having birefringence in the thickness direction, the retardation value in the thickness direction of the first retardation layer as a whole was equivalent to that of the first retardation layer of the Example, but the seamlessness improvement effect was not obtained. In addition, in the front direction, both the optical laminates of the Example and the Comparative Example showed good seamlessness. [Industrial Applicability]

[0102] The optical layered body of the present invention can be suitably used in an image display device. [Explanation of symbols]

[0103] 10 First polarizing plate 20 First retardation layer 30 Second polarizing plate 40 printing layer 50 Surface base material layer 60 Second retardation layer 100 Optical laminate 110 Backlight unit 120 Third polarizing plate 130 Liquid crystal cell 140 Organic EL element 150 Touch Panel 200 Image display device

Claims

1. A first polarizing plate including a first polarizer, a retardation layer having a retardation in a thickness direction, a printing layer, and a second polarizing plate including a second polarizer, in this order; The retardation layer includes a retardation film having birefringence in a thickness direction, an absorption axis direction of the first polarizer and an absorption axis direction of the second polarizer are substantially parallel to each other; Optical laminate.

2. 2. The optical laminate according to claim 1, wherein an absolute value of a retardation value Rth(550) in a thickness direction of the retardation layer is 100 nm or more.

3. The retardation film having birefringence in the thickness direction includes a retardation film having a refractive index characteristic of nx>ny>nz, nx>nz>ny, or nz>nx=ny, where nx is a refractive index in the slow axis direction, ny is a refractive index in the fast axis direction, and nz is a refractive index in the thickness direction. The optical laminate according to claim 1,

4. The retardation film having birefringence in the thickness direction has an in-plane retardation, The optical laminate according to claim 1 , wherein the slow axis direction is substantially parallel to the slow axis directions of the first polarizer and the second polarizer.

5. The optical laminate according to claim 1, wherein the printed layer has a thickness of 3 μm to 30 μm.

6. The optical laminate according to claim 1 , further comprising a surface base material layer on the side of the second polarizing plate opposite to the side on which the retardation layer is disposed.

7. A display element and the optical laminate according to any one of claims 1 to 6 are provided in this order toward a viewing side, The optical laminate is disposed so that the second polarizing plate is closer to the viewing side than the first polarizing plate. Image display device.

8. The image display device according to claim 7 , wherein the display element comprises a liquid crystal cell, an organic electronic element, or an inorganic electronic element.

9. The image display device according to claim 7 , further comprising a touch panel.

10. the display element is a liquid crystal cell, The image display device according to claim 8 , comprising, in this order toward a viewing side, a third polarizing plate including a third polarizer, the liquid crystal cell, and the optical laminate.

Citation Information

Patent Citations

  • Black protecgulum, black touch -sensitive screen and LCD module

    CN207133546U

  • Optical film and picture display device

    JP2004004642A

  • Image display device

    JP2021131570A

  • Display device

    US20180157078A1

  • Circularly polarizing plate and display device

    WO2019093501A1