Acoustic wave device

By using a piezoelectric member layer with alternately stacked rotated Y-cut lithium tantalate and lithium niobate layers, the elastic wave device achieves adjustable fractional bands and improved frequency-temperature characteristics, addressing the limitations of conventional devices in filter applications.

JP2024162642AInactive Publication Date: 2024-11-21MURATA MFG CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023078365
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-21
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional elastic wave devices face difficulties in achieving a sufficiently wide fractional band adjustment to suit different communication bands, making it challenging to optimize their performance in filter devices.

Method used

The elastic wave device incorporates a piezoelectric member layer composed of alternately stacked rotated Y-cut lithium tantalate and lithium niobate layers, with a total of three or more layers, allowing for easy adjustment of the fractional band.

Benefits of technology

This configuration enables easy and wide adjustment of the fractional band, suppresses unnecessary Rayleigh mode waves, and improves frequency-temperature characteristics, enhancing the device's performance in filter applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024162642000001_ABST
    Figure 2024162642000001_ABST
Patent Text Reader

Abstract

To provide an acoustic wave device that can easily adjust a specific band.SOLUTION: An acoustic wave device 1 according to the present invention includes a support substrate 2, a piezoelectric material layer 6 provided directly or indirectly on the support substrate 2, and an IDT electrode 12 provided on the piezoelectric material layer 6. The piezoelectric material layer 6 includes at least one rotated Y-cut lithium tantalate layer 7 and at least one rotated Y-cut lithium niobate layer 8. The lithium tantalate layers 7 and the lithium niobate layers 8 are alternately laminated. The total number of layers of the lithium tantalate layers 7 and the lithium niobate layers 8 is three or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an acoustic wave device. [Background technology]

[0002] Conventionally, acoustic wave devices have been widely used in filters for mobile phones and the like. Patent Document 1 listed below discloses an example of an acoustic wave device. In this acoustic wave device, a laminate is provided on a support substrate. An IDT (Interdigital Transducer) electrode is provided on the laminate. The laminate includes one lithium tantalate piezoelectric layer and one lithium niobate piezoelectric layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2021 / 177341 Summary of the Invention [Problem to be solved by the invention]

[0004] When an elastic wave device is used in a filter device, the optimal bandwidth ratio of the elastic wave device varies depending on the communication band of the filter device. However, in the elastic wave device described in Patent Document 1, it is difficult to sufficiently widen the bandwidth ratio. Therefore, it may be difficult to adjust the bandwidth ratio of the elastic wave device to a value suitable for the filter device.

[0005] An object of the present invention is to provide an acoustic wave device that allows easy adjustment of the bandwidth ratio. [Means for solving the problem]

[0006] An elastic wave device according to the present invention comprises a support substrate, a piezoelectric material layer provided directly or indirectly on the support substrate, and an IDT electrode provided on the piezoelectric material layer, wherein the piezoelectric material layer includes at least one rotated Y-cut lithium tantalate layer and at least one rotated Y-cut lithium niobate layer, the lithium tantalate layers and the lithium niobate layers are alternately stacked, and the total number of the lithium tantalate layers and the lithium niobate layers is three or more. Effect of the Invention

[0007] Advantageous Effects of Invention According to the present invention, it is possible to provide an acoustic wave device in which the bandwidth ratio can be easily adjusted. [Brief description of the drawings]

[0008] [Figure 1] 1 is a schematic front cross-sectional view illustrating a portion of an elastic wave device according to a first preferred embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic front cross-sectional view showing an enlarged portion of FIG. [Diagram 3] FIG. 1 is a schematic plan view of an elastic wave device according to a first preferred embodiment of the present invention. [Figure 4] FIG. 4 is a diagram showing impedance frequency characteristics in the first embodiment of the present invention, the first comparative example, and the second comparative example. [Diagram 5] FIG. 13 is a diagram showing the relationship between the number of lithium tantalate layers and the number of lithium niobate layers and the band width ratio. [Figure 6] FIG. 13 is a diagram showing impedance frequency characteristics of a third comparative example. [Figure 7] FIG. 4 is a diagram showing impedance frequency characteristics in the vicinity of a frequency at which a Rayleigh mode occurs in the first embodiment of the present invention. [Figure 8] 6 is a schematic enlarged front cross-sectional view showing a portion of a piezoelectric material layer in a second embodiment of the present invention. FIG. [Figure 9]FIG. 4 is a diagram showing impedance frequency characteristics in the vicinity of a frequency at which a Rayleigh mode occurs in the first and second embodiments of the present invention. [Figure 10] 13 is a schematic cross-sectional front view illustrating the vicinity of a pair of electrode fingers in an acoustic wave device according to a first modified example of a second embodiment of the present invention. FIG. [Figure 11] 13 is a schematic cross-sectional front view illustrating the vicinity of a pair of electrode fingers in an elastic wave device according to a second modified example of the second embodiment of the present invention. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be clarified below by describing specific embodiments of the present invention with reference to the drawings.

[0010] It should be noted that each embodiment described in this specification is merely an example, and partial substitution or combination of configurations is possible between different embodiments.

[0011] Fig. 1 is a schematic front cross-sectional view showing a part of an elastic wave device according to a first preferred embodiment of the present invention. Fig. 2 is a schematic front cross-sectional view showing an enlarged part of Fig. 1. Fig. 3 is a schematic plan view of the elastic wave device according to the first preferred embodiment. Fig. 1 is a schematic cross-sectional view taken along line II in Fig. 3.

[0012] As shown in Fig. 1, the elastic wave device 1 has a support substrate 2, an intermediate layer 3, and a piezoelectric material layer 6. The intermediate layer 3 is provided on the support substrate 2. The piezoelectric material layer 6 is provided on the intermediate layer 3. The piezoelectric material layer 6 is a layer made of a material having piezoelectric properties. Therefore, the piezoelectric material layer 6 has piezoelectric properties.

[0013] 1 and 2, the piezoelectric material layer 6 is a laminate of a plurality of piezoelectric layers. Specifically, the plurality of piezoelectric layers includes a plurality of lithium tantalate layers 7 and a plurality of lithium niobate layers 8. In the piezoelectric material layer 6, the lithium tantalate layers 7 and the lithium niobate layers 8 are alternately laminated.

[0014] More specifically, each of the lithium tantalate layers 7 is a rotated Y-cut lithium tantalate layer. In this embodiment, each lithium tantalate layer 7 is a LiTaO3 layer. The cut angle of each lithium tantalate layer 7 is 35°Y, and the Euler angles are (0°, 125°, 0°). However, the cut angle of the lithium tantalate layer 7 is not limited to the above.

[0015] On the other hand, each of the lithium niobate layers 8 is a rotated Y-cut lithium niobate layer. In this embodiment, each lithium niobate layer 8 is a LiNbO3 layer. The cut angle of each lithium niobate layer 8 is 45°Y, and the Euler angles are (0°, 135°, 0°). However, the cut angle of the lithium niobate layer 8 is not limited to the above.

[0016] The piezoelectric material layer 6 may have three or more piezoelectric layers. The piezoelectric layers may include at least one rotated Y-cut lithium tantalate layer 7 and at least one rotated Y-cut lithium niobate layer 8. When the number of the piezoelectric layers is three, the number of rotated Y-cut lithium tantalate layers 7 may be two, and the number of rotated Y-cut lithium niobate layers 8 may be two.

[0017] 1, in this embodiment, a piezoelectric material layer 6 is indirectly provided on a support substrate 2 via an intermediate layer 3. The intermediate layer 3 is not necessarily provided. The piezoelectric material layer 6 may be provided directly on the support substrate 2.

[0018] Intermediate layer 3 is a single dielectric layer. Silicon oxide is used as the material for intermediate layer 3. This reduces the absolute value of the temperature coefficient of frequency (TCF) of acoustic wave device 1, thereby improving the frequency-temperature characteristics of acoustic wave device 1. However, the material for intermediate layer 3 is not limited to the above. For example, silicon nitride, polysilicon, or the like may be used as the material for intermediate layer 3.

[0019] Specifically, the support substrate 2 is a silicon substrate. The surface orientation of the support substrate 2 is (111). More specifically, the surface orientation of the surface of the support substrate 2 facing the piezoelectric material layer 6 is (111). In this embodiment, the Euler angles of the support substrate 2 are (-45°, -54.7°, 73°). However, the Euler angles and surface orientation of the support substrate 2 are not limited to those described above. The material of the support substrate 2 is also not limited to silicon. For example, ceramics such as aluminum oxide can be used as the material of the support substrate 2.

[0020] An IDT electrode 12 is provided on the piezoelectric material layer 6. As shown in FIG. 3, the IDT electrode 12 has a pair of bus bars and a plurality of electrode fingers. The pair of bus bars is specifically a first bus bar 16 and a second bus bar 17. The first bus bar 16 and the second bus bar 17 face each other. The plurality of electrode fingers is specifically a plurality of first electrode fingers 18 and a plurality of second electrode fingers 19. One ends of the plurality of first electrode fingers 18 are connected to the first bus bar 16, respectively. One ends of the plurality of second electrode fingers 19 are connected to the second bus bar 17, respectively. The plurality of first electrode fingers 18 and the plurality of second electrode fingers 19 are interdigitated with each other. The first electrode fingers 18 and the second electrode fingers 19 are connected to different potentials.

[0021] An AC voltage is applied to the IDT electrode 12 to excite an acoustic wave. The direction in which the first electrode fingers 18 and the second electrode fingers 19 extend is perpendicular to the acoustic wave propagation direction. A pair of reflectors 13A and 13B are provided on the piezoelectric material layer 6. More specifically, the reflectors 13A and 13B are provided facing each other in the acoustic wave propagation direction with the IDT electrode 12 in between. The acoustic wave device 1 is a surface acoustic wave resonator. In this embodiment, the SH mode is excited as the main mode. In this case, the Rayleigh mode becomes an unwanted wave.

[0022] In this embodiment, the IDT electrode 12 and each reflector are made of a laminated metal film. More specifically, the layer configuration of the IDT electrode 12 and each reflector is a configuration in which a Ti layer, an AlCu layer, and a Ti layer are laminated in this order from the piezoelectric material layer 6 side. However, the materials of the IDT electrode 12 and each reflector are not limited to those mentioned above. Alternatively, the IDT electrode 12 and each reflector may be made of a single-layer metal film.

[0023] In the following, λ denotes a wavelength defined by the electrode finger pitch of IDT electrode 12. The electrode finger pitch is the center-to-center distance in the acoustic wave propagation direction between adjacent first electrode fingers 18 and second electrode fingers 19. For example, when the electrode finger pitch is p, λ=2p.

[0024] 1, in piezoelectric material layer 6, the piezoelectric layer located closest to IDT electrode 12 is lithium niobate layer 8. The piezoelectric layer located closest to IDT electrode 12 may be lithium tantalate layer 7. On the other hand, the piezoelectric layer located closest to support substrate 2 is lithium tantalate layer 7. The piezoelectric layer located closest to support substrate 2 may be lithium niobate layer 8.

[0025] The present embodiment is characterized by the following configuration: 1) In the piezoelectric material layer 6, rotated Y-cut lithium tantalate layers 7 and rotated Y-cut lithium niobate layers 8 are alternately laminated. 2) The total number of rotated Y-cut lithium tantalate layers 7 and rotated Y-cut lithium niobate layers 8 is three or more. This allows the band width to be easily adjusted. The band width can be expressed by (|fa-fr| / fr)×100[%], where fr is the resonant frequency and fa is the anti-resonant frequency. The above effects will be described in detail below.

[0026] The impedance frequency characteristics were compared between the elastic wave device 1 having the configuration of the first embodiment and the elastic wave devices of the first and second comparative examples. The first comparative example differs from the first embodiment in that the piezoelectric material layer is made of a single layer of rotated Y-cut lithium tantalate. The second comparative example differs from the first embodiment in that the piezoelectric material layer is made of a single layer of rotated Y-cut lithium niobate. The impedance frequency characteristics of the elastic wave devices of the first embodiment, the first and second comparative examples were derived by simulation. The design parameters of the elastic wave device 1 having the configuration of the first embodiment are as follows:

[0027] Support substrate: Material: Si, surface orientation: (111), Euler angles: (-45°, -54.7°, 73°) Intermediate layer: Material: SiO2, thickness: 300 nm Piezoelectric material layer: Total number of lithium tantalate layers and lithium niobate layers: 20 layers; Total thickness of lithium tantalate layers and lithium niobate layers: 400 nm Lithium tantalate layer: Material: Rotated Y-cut X-propagation LiTaO3, Cut angle: 35°Y, Euler angles: (0°, 125°, 0°), Thickness: 20nm, Number of layers: 10 layers Lithium niobate layer: Material: Rotated Y-cut X-propagation LiNbO3, Cut angle: 45°Y, Euler angles: (0°, 135°, 0°), Thickness: 20nm, Number of layers: 10 layers IDT electrode: Layer structure: Ti layer / AlCu layer / Ti layer from the piezoelectric material layer side, thickness: 12 nm / 10 nm / 4 nm Wavelength…1.346μm Duty ratio: 0.45

[0028] The lithium tantalate layer in the first comparative example has a cut angle of 35°Y, and the lithium niobate layer in the second comparative example has a cut angle of 45°Y.

[0029] Fig. 4 is a diagram showing impedance frequency characteristics in the first embodiment, the first comparative example, and the second comparative example. In Fig. 4, the resonant frequencies in the first embodiment, the first comparative example, and the second comparative example are shown as being the same. Therefore, in the first embodiment, the first comparative example, and the second comparative example, the higher the anti-resonant frequency is, the larger the value of the fractional bandwidth is.

[0030] As shown in Fig. 4, the bandwidth fraction in the first embodiment is an intermediate value between the bandwidth fraction in the first comparative example and the bandwidth fraction in the second comparative example. Specifically, the bandwidth fraction in the first embodiment is 7.8%, the bandwidth fraction in the first comparative example is 4.8%, and the bandwidth fraction in the second comparative example is 12.8%.

[0031] When an elastic wave device is used as an elastic wave resonator in a high frequency filter, the optimal bandwidth ratio of the elastic wave device varies depending on the communication band of the filter device. For example, the optimal bandwidth ratio of the elastic wave device may be approximately 8%. In such a case, it is difficult to bring the bandwidth ratio of the elastic wave device close to the optimal value in conventional elastic wave devices such as the first and second comparative examples. In contrast, the first embodiment makes it easy to adjust the bandwidth ratio, which is difficult in conventional elastic wave devices.

[0032] Furthermore, the bandwidth ratio was calculated by simulation for each number of lithium tantalate layers and lithium niobate layers in the piezoelectric material layer. More specifically, the bandwidth ratio was calculated when the piezoelectric layer closest to the IDT electrode was a lithium tantalate layer. The bandwidth ratio was also calculated when the piezoelectric layer closest to the IDT electrode was a lithium niobate layer.

[0033] FIG. 5 is a diagram showing the relationship between the number of lithium tantalate layers and lithium niobate layers and the relative bandwidth. The horizontal axis in FIG. 5 indicates the total number of lithium tantalate layers and lithium niobate layers. The triangular plots show the results when the piezoelectric layer located closest to the IDT electrode side is a lithium tantalate layer. Thus, the results of the triangular plots when the horizontal axis is 1 correspond to the results of the first comparative example. The circular plots show the results when the piezoelectric layer located closest to the IDT electrode side is a lithium niobate layer. Thus, the results of the circular plots when the horizontal axis is 1 correspond to the results of the second comparative example.

[0034] As shown in Fig. 5, when the number of lithium tantalate layers and the number of lithium niobate layers are different, the band width ratio is different. More specifically, the more the number of lithium tantalate layers is, the larger the band width ratio is. On the other hand, the more the number of lithium niobate layers is, the smaller the band width ratio is.

[0035] These results show that the fractional bandwidth can be adjusted by adjusting the number of lithium tantalate layers 7 and lithium niobate layers 8 shown in Fig. 1. Moreover, by making the total number of lithium tantalate layers 7 and lithium niobate layers 8 three or more as in the first embodiment, the fractional bandwidth can be easily and widely adjusted.

[0036] The total number of lithium tantalate layers 7 and lithium niobate layers 8 in the piezoelectric material layer 6 is preferably 10 or more, and more preferably 30 or more. This makes it possible to suppress variation in the relative bandwidth of the elastic wave device 1. On the other hand, the total number of lithium tantalate layers 7 and lithium niobate layers 8 in the piezoelectric material layer 6 is preferably 100 or less. In this case, the relative bandwidth of the elastic wave device 1 can be suitably adjusted and a decrease in productivity can be suppressed.

[0037] In the first embodiment, the use of the rotated Y-cut lithium tantalate layer 7 and the rotated Y-cut lithium niobate layer 8 makes it possible to easily adjust the bandwidth ratio. Furthermore, it is also possible to suppress the Rayleigh mode as an unwanted wave. This will be shown by referring to the third comparative example.

[0038] The third comparative example differs from the first embodiment in that both the lithium tantalate layer and the lithium niobate layer are (001) oriented. The lithium tantalate layer and the lithium niobate layer in the third comparative example are alternately stacked. The total number of the lithium tantalate layer and the lithium niobate layer is 20.

[0039] FIG. 6 is a diagram showing impedance frequency characteristics of the third comparative example.

[0040] As shown in FIG. 6, the value of the bandwidth ratio is very small in the third comparative example. Specifically, the bandwidth ratio in the third comparative example is 0.8%. Therefore, when used in a filter device, it is not possible to configure a suitable passband. Furthermore, as shown by the arrow R in FIG. 6, a large unwanted wave is generated. This unwanted wave is a Rayleigh mode.

[0041] FIG. 7 is a diagram showing impedance frequency characteristics in the vicinity of a frequency at which a Rayleigh mode occurs in the first embodiment.

[0042] As shown in Fig. 7, in the first embodiment, Rayleigh waves as unwanted waves are suppressed more than in the third comparative example shown in Fig. 6. Furthermore, as shown in Fig. 5, in the first embodiment, the relative bandwidth can be easily adjusted, for example, within a range of about 4%. This is because the rotated Y-cut lithium tantalate layer 7 and the rotated Y-cut lithium niobate layer 8 are used in the first embodiment, as described above.

[0043] The results shown in FIG. 5 are obtained when the lithium tantalate layer 7 and the lithium niobate layer 8 have the same thickness. However, in the present invention, the lithium tantalate layer 7 and the lithium niobate layer 8 may be made different in thickness. Alternatively, the lithium tantalate layers 7 may be made different in thickness. The lithium niobate layers 8 may be made different in thickness. In other words, the specific bandwidth can be adjusted by adjusting the number and thickness of the lithium tantalate layers 7 and the number and thickness of the lithium niobate layers 8.

[0044] A second embodiment is described below, which differs from the first embodiment in the configuration of the piezoelectric material layer. However, in the second embodiment, the configuration other than the piezoelectric material layer is the same as in the first embodiment. Therefore, the drawings and symbols used in the description of the first embodiment may be used in the description of the second embodiment.

[0045] FIG. 8 is a schematic enlarged front cross-sectional view showing a portion of a piezoelectric member layer in the second embodiment.

[0046] This embodiment differs from the first embodiment in that the lithium tantalate layer 7 and the lithium niobate layer 8 have the same cut angle. Except for the above, the elastic wave device of this embodiment has the same configuration as the elastic wave device 1 of the first embodiment.

[0047] 8, the polarization direction of the lithium tantalate layer 7 is indicated by an arrow P1, and the polarization direction of the lithium niobate layer 8 is indicated by an arrow P2. The polarization direction of the lithium tantalate layer 7 and the polarization direction of the lithium niobate layer 8 are the same direction.

[0048] In the present embodiment, similarly to the first embodiment, rotated Y-cut lithium tantalate layers 7 and rotated Y-cut lithium niobate layers 8 are alternately laminated in piezoelectric material layer 26. The total number of rotated Y-cut lithium tantalate layers 7 and rotated Y-cut lithium niobate layers 8 is three or more. This makes it possible to easily adjust the relative bandwidth of the acoustic wave device.

[0049] In addition, in this embodiment, the Rayleigh mode as an unwanted wave can be further suppressed, as will be shown below.

[0050] As an elastic wave device having the configuration of the second embodiment, an elastic wave device in which the cut angle of each lithium tantalate layer 7 and each lithium niobate layer 8 is 45°Y was prepared. As another elastic wave device having the configuration of the second embodiment, an elastic wave device in which the cut angle of each lithium tantalate layer 7 and each lithium niobate layer 8 is 35°Y was prepared. Note that the design parameters of these elastic wave devices are similar to those of the elastic wave device 1 of the first embodiment having the impedance frequency characteristics shown in FIG. 4, except for the cut angles of each lithium tantalate layer 7 and each lithium niobate layer 8.

[0051] The impedance frequency characteristics of each of the elastic wave devices having the configuration of the second preferred embodiment were derived by simulation, and the results of the first preferred embodiment are also shown.

[0052] Fig. 9 is a diagram showing impedance frequency characteristics in the vicinity of a frequency at which the Rayleigh mode occurs in the first and second embodiments. In Fig. 9, the lithium tantalate layer is denoted as LT, and the lithium niobate layer is denoted as LN.

[0053] As shown in Fig. 9, in the first embodiment, the Rayleigh mode as an unwanted wave is sufficiently suppressed. On the other hand, in the second embodiment, the Rayleigh mode is further suppressed. More specifically, in both cases where the cut angle of each of the lithium tantalate layers 7 and each of the lithium niobate layers 8 is 35°Y and where the cut angle is 45°Y, the Rayleigh mode is further suppressed.

[0054] It is preferable that the absolute value of the difference in cut angle between the lithium tantalate layer 7 and the lithium niobate layer 8 adjacent to each other in the thickness direction of the piezoelectric material layer 6 is 0.5° or less. In this case, in the present invention, it can be said that the cut angles of the adjacent lithium tantalate layer 7 and the lithium niobate layer 8 are substantially the same. Therefore, when the absolute value of the difference in cut angle between the two layers is 0.5° or less, the Rayleigh mode as an unwanted wave can be further suppressed. It is more preferable that the absolute value of the difference between the maximum and minimum values ​​of the cut angle of the lithium tantalate layer 7 and the lithium niobate layer 8 in the piezoelectric material layer 26 is 0.5° or less. In this case, the Rayleigh mode as an unwanted wave can be more reliably and further suppressed.

[0055] Additionally, in the second embodiment, the frequency-temperature characteristics of the elastic wave device can be effectively improved. Note that, in the first embodiment, the frequency-temperature characteristics of the elastic wave device 1 can also be improved. This will be shown below by comparing with a first comparative example, a second comparative example, and a fourth comparative example.

[0056] As described above, in the first comparative example, the piezoelectric member layer is a single layer of lithium tantalate. In the second comparative example, the piezoelectric member layer is a single layer of lithium niobate. On the other hand, in the fourth comparative example, the piezoelectric member layer is a laminate of one layer of lithium tantalate and one layer of lithium niobate.

[0057] Here, the TCF at the resonant frequency of the elastic wave device is TCFr [ppm / °C], the TCF at the anti-resonant frequency is TCFa [ppm / °C], and the difference between TCFr and TCFa is ΔTCF [ppm / °C]. Specifically, ΔTCF=TCFa-TCFr. Table 1 shows ΔTCF in the first embodiment, the second embodiment, the first comparative example, the second comparative example, and the fourth comparative example. In Table 1, the lithium tantalate layer is abbreviated as LT, and the lithium niobate layer is abbreviated as LN.

[0058] [Table 1]

[0059] As shown in Table 1, in the first embodiment, it is seen that the absolute value of ΔTCF is smaller than that of each of the comparative examples. Specifically, in the first embodiment, ΔTCF is 9 ppm / ° C., and ΔTCF can be made in the single digits. This is because the piezoelectric material layer 6 shown in FIG. 1 is a laminate of the lithium tantalate layer 7 and the lithium niobate layer 8, and has a multi-layer structure. In the second embodiment, it is seen that the absolute value of ΔTCF is even smaller. This is because the orientations of the lithium tantalate layer 7 and the lithium niobate layer 8 adjacent to each other in the thickness direction of the piezoelectric material layer 26 are aligned as shown in FIG. 8.

[0060] Note that, similarly to the second embodiment, the absolute value of ΔTCF can be further reduced even when the absolute value of the difference in cut angle between the lithium tantalate layer 7 and the lithium niobate layer 8 adjacent to each other in the thickness direction of the piezoelectric material layer 6 is 0.5° or less. The absolute value of ΔTCF can be further reduced even when the absolute value of the difference between the maximum and minimum cut angles of the lithium tantalate layer 7 and the lithium niobate layer 8 in the piezoelectric material layer 26 is 0.5° or less.

[0061] As shown with reference to FIG. 1, in the second embodiment, the intermediate layer 3 is a single dielectric layer. However, in the present invention, the intermediate layer 3 may be a laminate. For example, in a first modified example of the second embodiment shown in FIG. 10, the intermediate layer 23 has a high acoustic velocity film 24 and a low acoustic velocity film 25. Specifically, the high acoustic velocity film 24 is provided on the support substrate 2. The low acoustic velocity film 25 is provided on the high acoustic velocity film 24. A piezoelectric member layer 26 is provided on the low acoustic velocity film 25.

[0062] The high acoustic velocity film 24 is a film with a relatively high acoustic velocity. More specifically, the acoustic velocity of the bulk wave propagating through the high acoustic velocity film 24 is higher than the acoustic velocity of the elastic wave propagating through each piezoelectric layer in the piezoelectric member layer 26. Examples of the material of the high acoustic velocity film 24 include piezoelectric materials such as aluminum nitride, lithium tantalate, lithium niobate, and quartz; ceramics such as alumina, sapphire, magnesia, silicon nitride, silicon carbide, zirconia, cordierite, mullite, steatite, forsterite, spinel, and sialon; dielectric materials such as aluminum oxide, silicon oxynitride, DLC (diamond-like carbon), and diamond; semiconductors such as silicon; and materials containing the above materials as main components. The spinel includes an aluminum compound containing one or more elements selected from Mg, Fe, Zn, Mn, and the like, and oxygen. Examples of the spinel include MgAl2O4, FeAl2O4, ZnAl2O4, and MnAl2O4.

[0063] In this specification, the term "main component" refers to a component that accounts for more than 50% by weight. The main component material may be in any one of single crystal, polycrystalline, and amorphous states, or a mixture of these states.

[0064] The low acoustic velocity film 25 is a film with a relatively low acoustic velocity. More specifically, the acoustic velocity of the bulk wave propagating through the low acoustic velocity film 25 is lower than the acoustic velocity of the bulk wave propagating through each piezoelectric layer in the piezoelectric material layer 26. The low acoustic velocity film 25 can be made of a material such as glass, silicon oxide, silicon oxynitride, lithium oxide, tantalum oxide, or a dielectric material such as a compound in which fluorine, carbon, or boron is added to silicon oxide, or a material containing the above-mentioned material as a main component.

[0065] In the acoustic wave device, high acoustic velocity film 24, low acoustic velocity film 25, and piezoelectric material layer 26 are laminated in this order, so that the energy of the acoustic waves can be effectively confined on the side of piezoelectric material layer 26. In addition, in this modification as well, the fractional bandwidth of the acoustic wave device can be easily adjusted, as in the second embodiment.

[0066] In the second embodiment, silicon is used as the material of the support substrate 2. However, in the present invention, the material given as an example of the material of the high acoustic velocity film 24 may be used as the material of the support substrate 2.

[0067] When intermediate layer 23 is a laminate, intermediate layer 23 does not necessarily have to include high acoustic velocity film 24 and low acoustic velocity film 25. However, intermediate layer 23 preferably includes a layer made of silicon oxide, which can improve the frequency-temperature characteristics of the acoustic wave device.

[0068] Incidentally, a dielectric film may be provided on piezoelectric material layer 26. For example, in a second modification of the second embodiment shown in FIG. 11, a dielectric film 29 is provided on piezoelectric material layer 26 so as to cover IDT electrode 12. This protects IDT electrode 12 from damage by dielectric film 29. In addition, in this modification, as in the second embodiment, the relative bandwidth of the acoustic wave device can be easily adjusted. Examples of materials that can be used for dielectric film 29 include silicon oxide, silicon nitride, and silicon oxynitride.

[0069] Examples of configurations of the elastic wave device according to the present invention will be described below.

[0070] <1> An elastic wave device comprising: a support substrate; a piezoelectric material layer provided directly or indirectly on the support substrate; and an IDT electrode provided on the piezoelectric material layer, wherein the piezoelectric material layer includes at least one rotated Y-cut lithium tantalate layer and at least one rotated Y-cut lithium niobate layer, the lithium tantalate layers and the lithium niobate layers are alternately stacked, and the total number of the lithium tantalate layers and the lithium niobate layers is three or more.

[0071] <2> an absolute value of a difference in cut angle between the lithium tantalate layer and the lithium niobate layer adjacent to each other in a thickness direction of the piezoelectric material layer is 0.5° or less; <1> The acoustic wave device according to claim 1 .

[0072] <3> the total number of the lithium tantalate layers and the lithium niobate layers in the piezoelectric material layer is 10 or more and 100 or less; <1> or <2> The acoustic wave device according to claim 1 .

[0073] <4> the total number of the lithium tantalate layers and the lithium niobate layers in the piezoelectric material layer is 30 or more and 100 or less; <3> The acoustic wave device according to claim 1 .

[0074] <5> The piezoelectric element further includes an intermediate layer provided between the support substrate and the piezoelectric member layer, the intermediate layer including a layer made of silicon oxide. <1> ~ <4> 13. The acoustic wave device according to claim 12,

[0075] <6> Silicon is used as the material of the support substrate. <1> ~ <5> 13. The acoustic wave device according to claim 12,

[0076] <7> a dielectric film provided on the piezoelectric material layer so as to cover the IDT electrodes; <1> ~ <6> 13. The acoustic wave device according to claim 12, [Explanation of symbols]

[0077] 1. Elastic wave device 2…Support substrate 3. Middle class 6...Piezoelectric material layer 7...Lithium tantalate layer 8...Lithium niobate layer 12...IDT electrode 13A,13B…Reflector 16,17…1st and 2nd bus bars 18, 19...First and second electrode fingers 23. Middle class 24...High sonic membrane 25…Low sound velocity membrane 26...Piezoelectric member layer 29...Dielectric film

Claims

1. A support substrate; a piezoelectric member layer provided directly or indirectly on the support substrate; an IDT electrode provided on the piezoelectric material layer; Equipped with an elastic wave device, wherein the piezoelectric material layer includes at least one rotated Y-cut lithium tantalate layer and at least one rotated Y-cut lithium niobate layer, the lithium tantalate layers and the lithium niobate layers are alternately stacked, and the total number of the lithium tantalate layers and the lithium niobate layers is three or more.

2. The acoustic wave device according to claim 1 , wherein an absolute value of a difference in cut angle between the lithium tantalate layer and the lithium niobate layer adjacent to each other in a thickness direction of the piezoelectric material layer is 0.5° or less.

3. The acoustic wave device according to claim 1 , wherein a total number of the lithium tantalate layers and the lithium niobate layers in the piezoelectric material layer is 10 to 100.

4. The acoustic wave device according to claim 3 , wherein a total number of the lithium tantalate layers and the lithium niobate layers in the piezoelectric material layer is equal to or greater than 30 and equal to or less than 100.

5. The acoustic wave device according to claim 1 , further comprising an intermediate layer provided between the support substrate and the piezoelectric material layer, the intermediate layer including a layer made of silicon oxide.

6. The acoustic wave device according to claim 1 , wherein the supporting substrate is made of silicon.

7. The acoustic wave device according to claim 1 , further comprising a dielectric film provided on the piezoelectric material layer so as to cover the IDT electrodes.

Citation Information