Extrusion molded product for tube container and tube container
The extruded tube container, using recycled low-density polyethylene resin with a multilayer structure, addresses appearance and strength issues in laminated tubes, offering superior sealing and smoothness with environmental advantages.
Patent Information
- Application Number
- JP2023079429
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
AI Technical Summary
Laminated tubes face issues with appearance discrepancies due to overlapping ends, permeation of contents through exposed end faces, and difficulty in increasing thickness and maintaining strength, especially in large diameters.
An extruded tube container made from recycled low-density polyethylene resin with specific molecular weight and endothermic peak characteristics, combined with a multilayer structure, including adhesive and gas barrier layers, to enhance sealing strength and surface smoothness.
The solution provides tubes with excellent sealing strength and surface smoothness, allowing for seamless construction and increased thickness without deformation, while utilizing recycled materials for environmental benefit.
Smart Images

Figure 2024163641000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an extrusion molded product for a tubular container and a tubular container. [Background technology]
[0002] Conventionally, resin scraps generated during the manufacture of resin products have been crushed and reused, and resin products that have been discarded as used have also been reused.
[0003] On the other hand, laminated tubes are known as tube containers for storing toothpaste, cosmetics, etc. Laminated tubes are manufactured using a laminated sheet made by laminating polyethylene resin, special paper, aluminum foil, etc., as a raw material. Generally, laminated tubes are manufactured by rolling a laminated sheet into a cylindrical shape, overlapping both ends of the sheet, welding the overlapped parts, and joining a cap fitting part to the obtained container body.
[0004] Such laminate tubes have the following problems, for example. Since laminate tubes are manufactured by overlapping both ends, a step occurs at the overlapped portion, which causes problems in appearance. Since the end faces of the laminate sheet are exposed at the overlapped portion, the contents contained therein permeate into the laminate from the end faces, which deteriorates the physical properties of the laminate sheet. In addition, since laminate tubes include a process of rolling into a cylindrical shape and it is desired to make the above-mentioned step less noticeable, it is difficult to make the tube thicker, and it is difficult to maintain sufficient strength in a tube with a large diameter.
[0005] In order to solve the above problems of laminated tubes, it has been proposed to manufacture the container body of a tube container by extrusion molding (Patent Documents 1 and 2). A tube container manufactured by extrusion molding is called an extrusion molded tube. An extrusion molded tube is manufactured by continuously extruding molten resin into a tube shape using an extruder, then cutting it to an appropriate length, and joining a cap fitting portion to the resulting container body. In the case of a multi-layer extrusion molded tube, it is manufactured by extruding multiple types of molten resin into a single mold using separate extruders, and forming a multi-layered tube shape within the mold. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 11-309406 [Patent Document 2] Japanese Patent Application Publication No. 11-309785 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a technique for an extrusion molded tube that contains recycled low-density polyethylene resin and has excellent sealing strength and surface smoothness. [Means for solving the problem]
[0008] According to one aspect, there is provided an extrusion-molded product for a tubular container, which has an overall tubular shape and contains recycled low-density polyethylene resin, the recycled low-density polyethylene resin having an average molecular weight of 30,000 or more, and which has an endothermic peak obtained by differential scanning calorimetry only in the range of 100 to 140°C.
[0009] According to another aspect, there is provided an extrusion molded article according to the above aspect, having a multi-layer structure including at least an innermost layer and an outermost layer.
[0010] According to yet another aspect, there is provided the extrusion-molded article according to the above aspect, wherein the outermost layer comprises the recycled low-density polyethylene resin.
[0011] According to yet another aspect, there is provided the extrusion molded article according to any of the above aspects, wherein the innermost layer comprises the recycled low density polyethylene resin.
[0012] According to yet another aspect, there is provided the extrusion-molded product according to any of the above aspects, wherein the innermost layer comprises a plant-derived low-density polyethylene resin and a plant-derived linear low-density polyethylene resin.
[0013] According to yet another aspect, there is provided an extrusion-molded product relating to any of the above aspects, wherein the multilayer structure is a five-layer structure in which the innermost layer, a first adhesive layer, an intermediate layer, a second adhesive layer, and the outermost layer are laminated in this order from the inside to the outside.
[0014] According to still another aspect, there is provided the extrusion molded product according to the above aspect, wherein the intermediate layer contains a resin having gas barrier properties.
[0015] According to yet another aspect, there is provided an article for a tube container, comprising an extrusion molded article according to any of the above aspects and one or more layers disposed on the extrusion molded article.
[0016] According to yet another aspect, there is provided a tube container comprising a container body including an extrusion molded product having one sealed end and relating to any of the above-mentioned sides or a molded product having one sealed end and relating to any of the above-mentioned sides, and a cap fitting portion joined to the other end of the extrusion molded product having one sealed end or the molded product having one sealed end.
[0017] According to yet another aspect, there is provided a containerized article comprising a container body including an extrusion molded product relating to any of the above-mentioned sides having one end sealed or a molded product relating to the above-mentioned sides having one end sealed, a cap fitting portion joined to the other end of the extrusion molded product having one end sealed or the molded product having one end sealed, and contents filled in the container body. Effect of the Invention
[0018] According to the present invention, a technique can be provided for an extrusion molded tube that contains recycled low-density polyethylene resin and has excellent sealing strength and surface smoothness. [Brief description of the drawings]
[0019] [Figure 1] FIG. 2 is a cross-sectional view showing a five-layer structure of an extrusion molded product according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a plan view showing a configuration of a tube container according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, embodiments of the present invention will be described. The embodiments described below are more specific embodiments of any of the above aspects. The following items can be incorporated into each of the above aspects alone or in combination.
[0021] 1. Recycled low-density polyethylene resin First, the recycled low-density polyethylene resin used in the present invention will be described. In the technical field, the term "recycled resin" refers to a material that is obtained by collecting used resin products or waste from the manufacturing process of resin products and processing it so that it can be used as a material or raw material for new products. Therefore, the recycled low-density polyethylene resin may be derived from used resin products or waste from the manufacturing process of resin products. The recycled low-density polyethylene resin is preferably derived from used resin products.
[0022] The recycled low-density polyethylene resin used in the present invention meets the following two requirements: (i) having an average molecular weight of 30,000 or more; and (ii) The endothermic peak obtained by differential scanning calorimetry is present only within the range of 100 to 140°C. Meet the following.
[0023] Requirement (i) means that the recycled low-density polyethylene resin used in the present invention is a recycled resin, and is therefore repeatedly subjected to a melt-solidification process for recycling, and although the molecular weight may decrease due to the thermal history, the level of decrease in molecular weight is low. Requirement (ii) means that the recycled low-density polyethylene resin used in the present invention is a recycled resin, and therefore may contain impurities, but the impurities are contained in small amounts that are not detectable by differential scanning calorimetry, or are not contained at all.
[0024] Thus, the recycled low-density polyethylene resin used in the present invention is a recycled resin, but the deterioration of the physical properties of the resin is within an acceptable range, and it is of relatively high quality. Such recycled low-density polyethylene resin is, for example, a recycled low-density polyethylene resin derived from used medical resin products.
[0025] Requirements (i) and (ii) are explained below. Requirement(i) The average molecular weight of the recycled low-density polyethylene resin is 30,000 or more, and preferably 35,000 or more. The upper limit of the average molecular weight of the recycled low-density polyethylene resin is, for example, 100,000. That is, the average molecular weight of the recycled low-density polyethylene resin is, for example, in the range of 30,000 to 100,000, and preferably in the range of 35,000 to 100,000.
[0026] Recycled resins are repeatedly subjected to melt-solidification processes for recycling, and the longer the thermal history, the lower the molecular weight tends to be. When the molecular weight of recycled resins is lowered, the mechanical properties and melt viscosity also decrease, making extrusion molding difficult. In contrast, recycled low-density polyethylene resins having the above-mentioned average molecular weight can be extruded without problems associated with a decrease in melt viscosity.
[0027] The average molecular weight of recycled low-density polyethylene resin refers to the number average molecular weight (Mn) measured using gel permeation chromatography. Measurement of the number average molecular weight using gel permeation chromatography can be performed using a high-temperature gel permeation chromatograph (high-temperature GPC) device and a styrene-divinylbenzene-based packed column for high-temperature GPC. For example, measurement of the number average molecular weight using gel permeation chromatography can be performed under the following conditions. The number average molecular weight (Mn) can be obtained by creating a calibration curve using monodisperse polystyrene as a standard substance and calculating the molecular weight from the retention time.
[0028] High-temperature GPC equipment: Tosoh HLC-8321GPC / HT high-temperature gel permeation chromatograph Columns: 2 x Tosoh TSKgel GMH6-HT, 2 x Tosoh TSKgel GMH6-HTL Solvent: o-dichlorobenzene (containing 0.025% by mass BHT) Flow rate: 1.0 mL / min Temperature: 140℃ Measured concentration: 20 mg / 20mL Injection volume: 0.4 mL
[0029] Requirement (ii) The recycled low-density polyethylene resin has an endothermic peak obtained by differential scanning calorimetry only in the range of 100 to 140° C. That is, the recycled low-density polyethylene resin has no endothermic peak obtained by differential scanning calorimetry outside the range of 100 to 140° C. Preferably, the recycled low-density polyethylene resin has an endothermic peak obtained by differential scanning calorimetry as one peak in the range of 100 to 140° C. In this specification, "endothermic peak" refers to the peak top of the endothermic peak, and "temperature of the endothermic peak" refers to the temperature of the peak top of the endothermic peak.
[0030] In general, recycled resins may contain various impurities (e.g., colorants, additives, other resin components, etc.), which can cause a decrease in mechanical properties. In contrast, even if the recycled low-density polyethylene resin exhibits the above-mentioned endothermic peak contains impurities, the content is so small that it cannot be detected by differential scanning calorimetry, and therefore extrusion molded products manufactured using such recycled resins have excellent seal strength and surface smoothness.
[0031] Impurities that may be contained in recycled low-density polyethylene resin include, for example, ethylene-vinyl alcohol copolymer resin, polypropylene, polyamide, etc.
[0032] When the endothermic peak of the recycled low-density polyethylene resin is outside the range of 100 to 140°C, the endothermic peak is observed, for example, within the range of 160 to 185°C (164°C in one example), and this endothermic peak is derived from the ethylene-vinyl alcohol copolymer resin. When the endothermic peak of the recycled low-density polyethylene resin is outside the range of 100 to 140°C, the endothermic peak is, for example, 165°C, and this endothermic peak is derived from polypropylene. When the endothermic peak of the recycled low-density polyethylene resin is outside the range of 100 to 140°C, the endothermic peak is observed, for example, within the range of 170 to 270°C, and this endothermic peak is derived from polyamide.
[0033] The endothermic peak temperature of the recycled low-density polyethylene resin can be obtained by performing differential scanning calorimetry (DSC) to obtain a differential scanning calorimetry curve (DSC curve). Differential scanning calorimetry can be performed using a differential scanning calorimeter. For example, differential scanning calorimetry can be performed using a differential scanning calorimeter: TA Instrument Q200, as follows. Specifically, about 5 mg is cut out from the sample tube and sealed in an aluminum pan for measurement. Thereafter, the temperature is raised from room temperature (e.g., 20°C) to 200°C at a rate of 10°C / min, then lowered to room temperature at 10°C / min, and again raised from room temperature to 200°C at 10°C / min, and the melting endothermic peak temperature of the sample is measured. When differential scanning calorimetry is performed in such a temperature range, the endothermic peak obtained by differential scanning calorimetry of the recycled low-density polyethylene resin does not exist in the range of room temperature (e.g., 20°C) or more and less than 100°C, and in the range of more than 140°C and less than 200°C.
[0034] The density of recycled low-density polyethylene resin is 0.91 g / cm 3 ~0.93g / cm 3 and preferably in the range of 0.915 g / cm 3 ~0.93g / cm 3 It is more preferable that the density of the resin described in this specification is a measured value obtained by a method in accordance with JIS K7112:1999.
[0035] The melt flow rate (MFR) of the recycled low density polyethylene resin is preferably within the range of 0.1 g / 10 min to 10 g / 10 min, more preferably within the range of 1 g / 10 min to 5 g / 10 min. The melt flow rate (MFR) of the resin described in this specification is a measured value obtained by a method conforming to JIS K7210:1999. Specifically, the melt flow rate is a measured value of the weight of the resin discharged in 10 minutes when a load of 21.18 N is applied to the resin at 190°C.
[0036] 2. Extrusion moldings for tube containers The extrusion molding for tube containers has a tubular shape as a whole and contains the recycled low-density polyethylene resin described in the above section "1. Recycled low-density polyethylene resin." That is, the extrusion molding for tube containers meets the following two requirements: (i) having an average molecular weight of 30,000 or more; and (ii) The endothermic peak obtained by differential scanning calorimetry is present only within the range of 100 to 140°C. Contains recycled low-density polyethylene resin that meets the following requirements.
[0037] In this specification, the term "extrusion molded product" refers to a product formed into a tube shape by extrusion molding. In other words, the term "extrusion molded product" refers to a product that has a tube shape immediately after extrusion molding. Therefore, the term "extrusion molded product" does not include a product that is extruded into a sheet shape and then rolled into a tube shape. Therefore, an extrusion molded product can achieve a seamless appearance without overlapping parts (i.e., seams) as seen in the body part of a laminated tube. In addition, an extrusion molded product can be easily thickened compared to the body part of a laminated tube, and can maintain sufficient strength even in a tube container with a large diameter.
[0038] In the following description, the extrusion molded product for tubular containers is also simply referred to as the “extrusion molded product.” The layer structure and resin composition of the extrusion molded product will be described below.
[0039] 2-1. Layer structure The layer structure of the extrusion molded product is not particularly limited, and the extrusion molded product may have a single layer structure or a multilayer structure. Preferably, the extrusion molded product has a multilayer structure including at least an innermost layer and an outermost layer. For example, the extrusion molded product may have a two-layer structure consisting of an innermost layer and an outermost layer, a three-layer structure consisting of an innermost layer, an intermediate layer, and an outermost layer, or a five-layer structure consisting of an innermost layer, a first adhesive layer, an intermediate layer, a second adhesive layer, and an outermost layer. More preferably, the extrusion molded product has a five-layer structure in which the innermost layer, the first adhesive layer, the intermediate layer, the second adhesive layer, and the outermost layer are laminated in this order from the inside to the outside.
[0040] Fig. 1 is a cross-sectional view showing a five-layer structure of an extrusion molded product according to one embodiment of the present invention. As shown in Fig. 1, the extrusion molded product 1 has a five-layer structure in which an innermost layer 1a, a first adhesive layer 1b, an intermediate layer 1c, a second adhesive layer 1d, and an outermost layer 1e are laminated in this order from the inside to the outside. When the extrusion molded product 1 shown in Fig. 1 is used as a container body of a tube container, the surface on the innermost layer 1a side is adjacent to the internal space of the tube container, and the surface on the outermost layer 1e side is adjacent to the external space of the tube container.
[0041] The extrusion molded product 1 may be in a cylindrical shape or an elliptical cylindrical shape. The extrusion molded product 1 has a circumferential length of, for example, 30 to 190 mm. The extrusion molded product 1 preferably has a circumferential length of 40 to 160 mm. The circumferential length refers to the outer periphery of the tubular extrusion molded product 1.
[0042] The extrusion molded product 1 has a thickness of, for example, 190 to 550 μm, preferably 240 to 500 μm. The thickness refers to the thickness of the wall of the tubular extrusion molded product 1, and is the average value of thicknesses measured at three points set at approximately equal intervals along the longitudinal direction of the extrusion molded product 1.
[0043] The innermost layer 1a has a thickness of, for example, 120 to 250 μm, preferably 140 to 240 μm. The first adhesive layer 1b has a thickness of, for example, 1 to 30 μm, preferably 5 to 20 μm. The intermediate layer 1c has a thickness of, for example, 10 to 100 μm, preferably 20 to 80 μm. The second adhesive layer 1d has a thickness of, for example, 1 to 30 μm, preferably 5 to 20 μm. The outermost layer 1e has a thickness of, for example, 60 to 200 μm, preferably 80 to 180 μm.
[0044] The extrusion molded product 1 can have any length, and may be longer than the container body of the tube container, or may be the same length as the container body of the tube container. In the former case, the extrusion molded product 1 is cut to the length of the container body of the tube container, and then used as the container body of the tube container.
[0045] 2-2. Resin composition The resin composition of the extrusion molding is not particularly limited as long as the extrusion molding contains the above-mentioned recycled low-density polyethylene resin. When the extrusion molding has a multi-layer structure including at least an innermost layer and an outermost layer, it is preferable that the outermost layer contains the above-mentioned recycled low-density polyethylene resin.
[0046] (First embodiment) The extrusion molded product according to the first embodiment has a multilayer structure including at least an innermost layer and an outermost layer, the outermost layer including the above-mentioned recycled low-density polyethylene resin, and the innermost layer including the above-mentioned recycled low-density polyethylene resin. In this case, the ratio of the recycled low-density polyethylene resin included in the extrusion molded product (specifically, the ratio of the mass of the recycled low-density polyethylene resin to the total mass of all the resins constituting the extrusion molded product) can be increased. Therefore, the extrusion molded product according to the first embodiment is excellent in that it has a high effect of reducing environmental load.
[0047] The extrusion molded product according to the first embodiment preferably has a five-layer structure as shown in Fig. 1, that is, a five-layer structure in which an innermost layer 1a, a first adhesive layer 1b, an intermediate layer 1c, a second adhesive layer 1d, and an outermost layer 1e are laminated in this order from the inside to the outside. Hereinafter, the innermost layer 1a, the first adhesive layer 1b, the intermediate layer 1c, the second adhesive layer 1d, and the outermost layer 1e will be described in order.
[0048] (Innermost layer 1a) The innermost layer 1a contains the recycled low-density polyethylene resin described above in the section "1. Recycled low-density polyethylene resin." The proportion of the recycled low-density polyethylene resin in the innermost layer 1a is, for example, 50% by mass or more, preferably 70% by mass or more. Thus, the innermost layer 1a is mainly composed of recycled low-density polyethylene resin, but may contain known additives as necessary in addition to the recycled low-density polyethylene resin. The additives will be described later.
[0049] (1st adhesive layer 1b) The first adhesive layer 1b serves to bond the innermost layer 1a to the intermediate layer 1c. The first adhesive layer 1b contains a petroleum-derived adhesive polyethylene resin (adhesive PE), for example, a petroleum-derived maleic anhydride-modified polyethylene resin (MA-modified PE).
[0050] Examples of the "petroleum-derived maleic anhydride modified low-density polyethylene resin (MA modified LDPE)" that can be used include a resin sold by Mitsubishi Chemical Corporation under the trade name "MODIC" (registered trademark) and a resin sold by Mitsui Chemicals, Inc. under the trade name "ADMER" (registered trademark).
[0051] The intermediate layer 1c preferably contains a resin having gas barrier properties. The resin constituting the intermediate layer 1c may be a resin known as a resin having gas barrier properties. The resin constituting the intermediate layer 1c may be, for example, an ethylene-vinyl alcohol copolymer resin (EVOH), nylon (NY), polyvinyl alcohol (PVA), polyacrylonitrile (PAN), or polyvinylidene chloride (PVDC). The resin constituting the intermediate layer 1c is preferably an ethylene-vinyl alcohol copolymer resin (EVOH).
[0052] Examples of the ethylene-vinyl alcohol copolymer resin (EVOH) that can be used include a resin sold by Mitsubishi Chemical Corporation under the trade name "Soarnol" (registered trademark) and a resin sold by Kuraray Co., Ltd. under the trade name "Eval" (registered trademark).
[0053] (2nd adhesive layer 1d) The second adhesive layer 1d serves to bond the outermost layer 1e to the intermediate layer 1c. The second adhesive layer 1d contains a petroleum-derived adhesive polyethylene resin (adhesive PE), for example, a petroleum-derived maleic anhydride-modified polyethylene resin (MA-modified PE). The second adhesive layer 1d may have the same resin composition as the first adhesive layer 1b, or may have a different resin composition from the first adhesive layer 1b.
[0054] (outermost layer 1e) The outermost layer 1e contains the recycled low-density polyethylene resin described in the above section "1. Recycled low-density polyethylene resin". The proportion of the recycled low-density polyethylene resin in the outermost layer 1e is, for example, 50% by mass or more, preferably 70% by mass or more. In this way, the outermost layer 1e is mainly composed of recycled low-density polyethylene resin, but may contain known additives in addition to the recycled low-density polyethylene resin as necessary. The additives will be described later. The outermost layer 1e may have the same resin composition as the innermost layer 1a, or may have a resin composition different from that of the innermost layer 1a.
[0055] (Additives) The innermost layer 1a, the first adhesive layer 1b, the intermediate layer 1c, the second adhesive layer 1d, and the outermost layer 1e are mainly composed of resin, but may contain known additives in addition to the resin as necessary. As the additives, various additives known as resin additives can be used. Examples of the additives include antioxidants, ultraviolet absorbers, weathering agents, antistatic agents, fillers, crystal nucleating agents, color pigments, matting agents, coloring inhibitors, anti-fogging agents, flame retardants, anti-blocking agents, lubricants (including slip agents and release agents), and CO2 absorbers. The total content of the additives can be, for example, 0.01 to 10 parts by mass with respect to 100 parts by mass of the resin of each layer.
[0056] Second embodiment The extrusion molded product according to the second embodiment has a multilayer structure including at least an innermost layer and an outermost layer, the outermost layer including the above-mentioned recycled low-density polyethylene resin, and the innermost layer including a plant-derived low-density polyethylene resin and a plant-derived linear low-density polyethylene resin. In this case, since the innermost layer includes virgin resin rather than recycled resin, a tube container that takes hygiene into consideration can be manufactured. In addition, since the innermost layer includes a plant-derived polyethylene resin rather than a petroleum-derived polyethylene resin, the extrusion molded product according to the second embodiment is excellent in that it has a high effect of reducing environmental load.
[0057] The extrusion molded product according to the second embodiment preferably has a five-layer structure as shown in FIG. 1, i.e., a five-layer structure in which an innermost layer 1a, a first adhesive layer 1b, an intermediate layer 1c, a second adhesive layer 1d, and an outermost layer 1e are laminated in this order from the inside to the outside.
[0058] The extrusion molded product according to the second embodiment differs from the extrusion molded product according to the first embodiment only in the resin composition of the innermost layer 1a. That is, in the extrusion molded product according to the second embodiment, the layers other than the innermost layer 1a (i.e., the first adhesive layer 1b, the intermediate layer 1c, the second adhesive layer 1d, and the outermost layer 1e) can have the same resin composition as each layer of the extrusion molded product according to the first embodiment. Therefore, for the extrusion molded product according to the second embodiment, the description of the layers other than the innermost layer 1a is omitted, and only the resin composition of the innermost layer 1a will be described below.
[0059] In the extrusion molded product according to the second embodiment, the innermost layer 1a contains a plant-derived low-density polyethylene resin (biomass LDPE) and a plant-derived linear low-density polyethylene resin (biomass L-LDPE). The innermost layer 1a contains the plant-derived low-density polyethylene resin (biomass LDPE) and the plant-derived linear low-density polyethylene resin (biomass L-LDPE) in a mass ratio of, for example, 9:1 to 4:6.
[0060] The proportion of the plant-derived polyethylene resin in the innermost layer 1a is, for example, 50% by mass or more, and preferably 70% by mass or more. In this way, the outermost layer 1e is composed mainly of the plant-derived polyethylene resin, but may contain known additives in addition to the plant-derived polyethylene resin as necessary.
[0061] Below, we will explain the structural differences between "low-density polyethylene resin (LDPE)" and "linear low-density polyethylene resin (L-LDPE)", and then provide a specific explanation of "plant-derived low-density polyethylene resin (biomass LDPE)" and "plant-derived linear low-density polyethylene resin (biomass L-LDPE)".
[0062] Low-density polyethylene resin (LDPE) and linear low-density polyethylene resin (L-LDPE) are structurally different due to differences in the manufacturing methods. That is, low-density polyethylene resin (LDPE) is a polymer of ethylene, and has a structure in which ethylene is randomly branched and bonded. For this reason, low-density polyethylene resin (LDPE) has side chains with various carbon numbers bonded to the main chain, and the side chains include short-chain branches (e.g., short-chain branches with about 20 carbon atoms or less) and long-chain branches (e.g., long-chain branches with more than about 20 carbon atoms). On the other hand, linear low-density polyethylene resin (L-LDPE) is a copolymer of ethylene and α-olefin. For this reason, linear low-density polyethylene resin (L-LDPE) does not have long-chain branches (e.g., long-chain branches with more than about 20 carbon atoms) bonded to the main chain, but only short-chain branches (e.g., short-chain branches with about 20 carbon atoms or less) bonded.
[0063] "Plant-derived low-density polyethylene resin (biomass LDPE)" "Plant-derived low-density polyethylene resin (biomass LDPE)" is an ethylene polymer produced using plants as a raw material, and has a structure in which ethylene is randomly branched and bonded. "Plant-derived low-density polyethylene resin (biomass LDPE)" is, for example, a low-density polyethylene resin derived from sugarcane. Sugarcane-derived low-density polyethylene resin is an ethylene polymer produced using sugarcane as a raw material, and has a structure in which ethylene is randomly branched and bonded.
[0064] The density of "plant-derived low-density polyethylene resin (biomass LDPE)" is 0.91 g / cm 3 ~0.93g / cm 3 and preferably in the range of 0.915 g / cm 3 ~0.93g / cm 3 In addition, the melt flow rate (MFR) of the "plant-derived low-density polyethylene resin (biomass LDPE)" is preferably in the range of 0.1 g / 10 min to 10 g / 10 min, and more preferably in the range of 1 g / 10 min to 5 g / 10 min.
[0065] As the "plant-derived low-density polyethylene resin (biomass LDPE)", for example, plant-derived low-density polyethylene sold by Braskem can be used, and examples of such resins include those sold under the trade names SEB853, SBC818, SBF0323HC, STN7006, and SPB618.
[0066] "Plant-derived linear low-density polyethylene resin (biomass L-LDPE)" "Plant-derived linear low-density polyethylene resin (biomass L-LDPE)" is a copolymer of ethylene and α-olefin produced using plants as a raw material. "Plant-derived linear low-density polyethylene resin (biomass L-LDPE)" is, for example, a linear low-density polyethylene resin derived from sugarcane. Sugarcane-derived linear low-density polyethylene resin is a copolymer of ethylene and α-olefin produced using sugarcane as a raw material.
[0067] The "α-olefin" is at least one compound selected from the group consisting of α-olefins having 3 to 20 carbon atoms, and examples thereof include 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene.
[0068] The density of "plant-derived linear low-density polyethylene resin (biomass L-LDPE)" is 0.91 g / cm 3 ~0.93g / cm 3 and preferably in the range of 0.915 g / cm 3 ~0.93g / cm 3 In addition, the melt flow rate (MFR) of the "plant-derived linear low-density polyethylene resin (biomass L-LDPE)" is preferably in the range of 0.1 g / 10 min to 10 g / 10 min, and more preferably in the range of 1 g / 10 min to 5 g / 10 min.
[0069] As the "plant-derived linear low-density polyethylene resin (biomass L-LDPE)", for example, plant-derived linear low-density polyethylene sold by Braskem can be used, and examples thereof include resins sold under the trade names SLL118, SLL118 / 21, SLL218, SLL218 / 21, SLL318, SLH118, SLH218, and SLH0820 / 30AF.
[0070] 2-3. Manufacturing method The extrusion molded product 1 can be manufactured according to a known extrusion molding method. When the extrusion molded product 1 has a multi-layer structure, the extrusion molded product 1 can be manufactured according to a known co-extrusion molding method. Specifically, when the extrusion molded product 1 has a five-layer structure, the resin constituting the innermost layer 1a, the resin constituting the first adhesive layer 1b, the resin constituting the intermediate layer 1c, the resin constituting the second adhesive layer 1d, and the resin constituting the outermost layer 1e can be extruded into one die by separate extruders to form a tube shape having a five-layer structure in the die.
[0071] 3. Molded products for tube containers The extrusion molded product 1 may have one or more additional layers on the extrusion molded product 1. That is, according to another aspect, a molded product for a tube container is provided, which includes an extrusion molded product and one or more layers provided on the extrusion molded product. In the following description, this molded product for a tube container is simply referred to as a "molded product."
[0072] The additional layer can be formed on the extrusion molded product according to known decoration techniques, for example, by printing (e.g., offset printing, screen printing), painting (e.g., clear coating for protecting the surface of the printed layer, UV coating), labeling, hot stamping, shrink film application, vapor deposition, or film transfer. The additional layer can be one layer or multiple layers, for example, 1 to 5 layers.
[0073] 4. Tube containers The tube container is a container body including the above-mentioned extrusion molded product with one end sealed; a cap fitting portion joined to the other end of the extrusion molded product whose one end is sealed; It is equipped with:
[0074] Alternatively, the tube container may include: A container body including the above-mentioned molded article (i.e., a molded article for a tube container) with one end sealed; a cap fitting portion joined to the other end of the molded article whose one end is sealed; It is equipped with:
[0075] A tube container according to one embodiment of the present invention will be described below with reference to Fig. 2. Fig. 2 is a plan view showing the configuration of a tube container according to one embodiment of the present invention.
[0076] As shown in FIG. 2, the tube container 10 includes a container body 11 and a cap fitting portion 12 joined to the container body 11. The tube container 10 is used by filling the container body 11 with contents and fitting a cap to the cap fitting portion 12. Here, the contents may be a high-viscosity liquid or a semi-solid. Examples of the contents include cosmetics, toothpaste, hand cream, and other daily necessities, and foods such as jam and butter. Specific examples of cosmetics include moisturizing cream, face wash, cleansing agent, sunscreen, shaving agent, hair styling agent, hair care agent, and foundation.
[0077] The container body 11 is obtained by sealing one end of the extrusion molded product 1 described above. The sealing can be performed by a method known as an end sealing process for tube containers, for example, a heat sealing method, an ultrasonic sealing method, or a hot air sealing method. As described above, the extrusion molded product 1 may be provided with one or more additional layers on the outer surface before sealing one end. That is, the container body 11 may further include one or more additional layers formed according to a known decoration technique, for example, by printing (e.g., offset printing, screen printing), painting (e.g., clear coating for protecting the surface of the printed layer, UV coating), labeling, hot stamping, shrink film application, vapor deposition, or film transfer.
[0078] As shown in FIG. 2, the container body 11 includes a body portion 21 and a seal portion 22 provided at one end of the body portion 21.
[0079] The body portion 21 is an unsealed portion of the extrusion molded product 1 or a molded product. The end portion of the body portion 21 where the seal portion 22 is not provided has a circular or elliptical cylindrical shape when viewed from the opening.
[0080] The sealed portion 22 is a portion formed by thermally welding one end of the extrusion molded product 1 or a molded product. The sealed portion 22 has a flat shape, and the opposing inner surfaces are sealed. The sealed portion 22 closes one end of the container body 11.
[0081] The cap fitting portion 12 is provided at the end of the body portion 21 opposite to the end where the seal portion 22 is provided. The cap fitting portion 12 has a shoulder portion 31 that is integrally continuous with the end of the body portion 21 where the seal portion 22 is not provided, and a cylindrical mouth portion 32 provided at the center of the shoulder portion 31. The cap fitting portion 12 is manufactured by injection molding or compression molding separately from the body portion 21, and is joined to the body portion 21. In the case of injection molding, the formation of the cap fitting portion 12 and the joining of the cap fitting portion 12 to the container body 11 may be performed simultaneously by insert molding, or the cap fitting portion 12 may be injection molded as a separate part and then joined to the container body 11 by ultrasonic welding.
[0082] The shoulder 31 has an outer surface facing the exterior space of the tube container 10 and an inner surface facing the interior space of the tube container 10, each of which has a truncated cone shape tapering from the interior space to the exterior space. The outer peripheral edge of the shoulder 31 is continuous with the body 21. The mouth 32 is provided at the center of the shoulder 31 so as to protrude outward.
[0083] 5. Containerized items The above-mentioned tube container 10 may have a content filled in the container body 11. The content may be any of the above-mentioned examples. In this specification, a tube container filled with a content is referred to as a "container-filled item."
[0084] That is, the containerized goods are a container body including the above-mentioned extrusion molded product with one end sealed; a cap fitting portion joined to the other end of the extrusion molded product whose one end is sealed; The contents filled in the container body; It is equipped with:
[0085] Alternatively, the packaged goods are A container body including the above-mentioned molded article (i.e., a molded article for a tube container) with one end sealed; a cap fitting portion joined to the other end of the molded article whose one end is sealed; The contents filled in the container body; It is equipped with:
[0086] The packaged article is used by fitting a cap to the cap fitting portion. For example, the packaged article can be manufactured by preparing a tube container (intermediate product) including a container body containing the above-mentioned extrusion molding (or the above-mentioned molded product) with one end not sealed and a cap fitting portion joined to the other end of the extrusion molding (or molded product), filling the container body of the tube container with contents, and sealing the unsealed end (i.e., the end on the side where the cap fitting portion is not joined).
[0087] 6.Effects As described above, in the present invention, recycled low-density polyethylene resin that meets certain requirements is used as the material for the extrusion tube. This allows the present invention to stably produce a tube-shaped extrusion product. In addition, the extrusion tube of the present invention can achieve excellent seal strength and excellent surface smoothness. The present invention uses recycled resin as the material for the extrusion tube, which can contribute to reducing the environmental load. EXAMPLES
[0088] [1] Manufacturing of extrusion molded products <Comparative Example 1> An extrusion molded product having the following five-layer structure was manufactured. In this example, virgin resin was used as the resin for the innermost and outermost layers.
[0089] Innermost layer: Petroleum-derived low-density polyethylene resin (density: 0.92 g / cm 3 , MFR: 1.9 g / 10 min (190℃, 21.18 N load), number average molecular weight: 60621, endothermic peak temperature: 109℃) First adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Middle layer: Ethylene-vinyl alcohol copolymer (density: 1.14 g / cm 3, MFR: 12.0 g / 10 min (210°C, 21.18 N load) Second adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Outermost layer: Petroleum-derived low-density polyethylene resin (density: 0.92 g / cm 3 , MFR: 1.9 g / 10 min (190℃, 21.18 N load), number average molecular weight: 60621, endothermic peak temperature: 109℃)
[0090] The resin material (pellets) for each layer was fed into five hoppers of a single-screw tube extruder. The extruder and die temperatures were set to 170-200°C, and a tube with a five-layer structure of innermost layer / first adhesive layer / middle layer / second adhesive layer / outermost layer was molded under molding conditions of a production speed of 60 tubes / min and a take-up speed of 9.1 m / min.
[0091] The resulting tube (i.e., extrusion molded product) had a circumference of 108 mm, a length of 150 mm, and an average wall thickness of 0.46 mm. The thicknesses of the innermost layer, first adhesive layer, intermediate layer, second adhesive layer, and outermost layer were 225 μm, 10 μm, 40 μm, 10 μm, and 175 μm, respectively.
[0092] <Example 1> An extrusion molded product having the following five-layer structure was manufactured. In this example, recycled low-density polyethylene resin was used as the resin for the innermost and outermost layers. The recycled low-density polyethylene resin used met the following two requirements: (i) having an average molecular weight of 30,000 or more; and (ii) The endothermic peak obtained by differential scanning calorimetry is present only within the range of 100 to 140°C. It met the following criteria.
[0093] Innermost layer: Recycled low-density polyethylene resin derived from medical resin products (density: 0.92 g / cm 3, MFR: 1.0 g / 10 min (190℃, 21.18 N load), number average molecular weight: 37300, endothermic peak temperature: 109℃) First adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Middle layer: Ethylene-vinyl alcohol copolymer (density: 1.14 g / cm 3 , MFR: 12.0 g / 10 min (210°C, 21.18 N load) Second adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Outermost layer: Recycled low-density polyethylene resin derived from medical resin products (density: 0.92 g / cm 3 , MFR: 1.0 g / 10 min (190℃, 21.18 N load), number average molecular weight: 37300, endothermic peak temperature: 109℃)
[0094] Except for changing the resin material of each layer to the above resin material, a tube was molded in the same manner as in Comparative Example 1. The circumference, length, and average wall thickness of the obtained tube (i.e., extrusion molded product), as well as the thickness of each layer, were all the same as those in Comparative Example 1.
[0095] <Example 2> An extrusion molded product having the following five-layer structure was manufactured. In this example, virgin resin was used as the resin for the innermost layer, and the recycled low-density polyethylene resin used in Example 1 was used as the resin for the outermost layer.
[0096] Innermost layer: Petroleum-derived low-density polyethylene resin (density: 0.92 g / cm 3 , MFR: 1.9 g / 10 min (190℃, 21.18 N load), number average molecular weight: 60621, endothermic peak temperature: 109℃) First adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3, MFR: 1.0 g / 10 min (190°C, 21.18 N load) Middle layer: Ethylene-vinyl alcohol copolymer (density: 1.14 g / cm 3 , MFR: 12.0 g / 10 min (210°C, 21.18 N load) Second adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Outermost layer: Recycled low-density polyethylene resin derived from medical resin products (density: 0.92 g / cm 3 , MFR: 1.0 g / 10 min (190℃, 21.18 N load), number average molecular weight: 37300, endothermic peak temperature: 109℃)
[0097] Except for changing the resin material of each layer to the above resin material, a tube was molded in the same manner as in Comparative Example 1. The circumference, length, and average wall thickness of the obtained tube (i.e., extrusion molded product), as well as the thickness of each layer, were all the same as those in Comparative Example 1.
[0098] <Example 3> An extrusion molded product having the following five-layer structure was manufactured. In this example, the recycled low-density polyethylene resin used in Example 1 was used as the resin for the innermost and outermost layers, but the thickness of the tube (extrusion molded product) was made thinner than that of Example 1.
[0099] Innermost layer: Recycled low-density polyethylene resin derived from medical resin products (density: 0.92 g / cm 3 , MFR: 1.0 g / 10 min (190℃, 21.18 N load), number average molecular weight: 37300, endothermic peak temperature: 109℃) First adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Middle layer: Ethylene-vinyl alcohol copolymer (density: 1.14 g / cm 3, MFR: 12.0 g / 10 min (210°C, 21.18 N load) Second adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Outermost layer: Recycled low-density polyethylene resin derived from medical resin products (density: 0.92 g / cm 3 , MFR: 1.0 g / 10 min (190℃, 21.18 N load), number average molecular weight: 37300, endothermic peak temperature: 109℃)
[0100] Except for changing the resin material of each layer to the above resin material, a tube was molded in the same manner as in Comparative Example 1. The resulting tube (i.e., extrusion molded product) had a circumference of 108 mm, a length of 150 mm, and an average thickness of 0.29 mm. The thicknesses of the innermost layer, first adhesive layer, intermediate layer, second adhesive layer, and outermost layer were 145 μm, 10 μm, 40 μm, 10 μm, and 85 μm, respectively.
[0101] <Example 4> An extrusion molded product having the following five-layer structure was manufactured. In this example, a plant-derived resin was used as the resin for the innermost layer, and the recycled low-density polyethylene resin used in Example 1 was used as the resin for the outermost layer.
[0102] Innermost layer: Plant-derived low-density polyethylene resin (density: 0.923 g / cm 3 , MFR: 2.7 g / 10 min (190°C, 21.18 N load)) and plant-derived linear low-density polyethylene resin (density: 0.916 g / cm 3 , MFR: 2.3 g / 10 min (190°C, 21.18 N load)) in a mass ratio of 50:50 (number average molecular weight: 30029, endothermic peak temperature: 109°C) First adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Middle layer: Ethylene-vinyl alcohol copolymer (density: 1.14 g / cm 3 , MFR: 12.0 g / 10 min (210°C, 21.18 N load) Second adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Outermost layer: Recycled low-density polyethylene resin derived from medical resin products (density: 0.92 g / cm 3 , MFR: 1.0 g / 10 min (190℃, 21.18 N load), number average molecular weight: 37300, endothermic peak temperature: 109℃)
[0103] Except for changing the resin material of each layer to the above resin material, a tube was molded in the same manner as in Comparative Example 1. The circumference, length, and average wall thickness of the obtained tube (i.e., extrusion molded product), as well as the thickness of each layer, were all the same as those in Comparative Example 1.
[0104] <Comparative Example 2> We manufactured an extrusion molded product with the following five-layer structure. In this example, recycled low-density polyethylene resin derived from waste from our own factory was used as the resin for the innermost and outermost layers. The recycled low-density polyethylene resin used contains low-density polyethylene resin as its main component, but is colored due to the presence of ethylene-vinyl alcohol copolymer and printing, etc. The recycled low-density polyethylene resin used meets the following two requirements: (i) having an average molecular weight of 30,000 or more; and (ii) The endothermic peak obtained by differential scanning calorimetry is present only within the range of 100 to 140°C. None of the above were met.
[0105] Innermost layer: Recycled low-density polyethylene resin (density: 0.93 g / cm3) made from waste from our own factory 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load), number average molecular weight: 29400, endothermic peak temperatures: 109°C, 122°C, 164°C) First adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Middle layer: Ethylene-vinyl alcohol copolymer (density: 1.14 g / cm 3 , MFR: 12.0 g / 10 min (210°C, 21.18 N load) Second adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Outermost layer: Recycled low-density polyethylene resin (density: 0.93 g / cm3) made from waste from our own factory 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load), number average molecular weight: 29400, endothermic peak temperatures: 109°C, 122°C, 164°C)
[0106] Except for changing the resin material of each layer to the above resin material, a tube was molded in the same manner as in Comparative Example 1. The circumference, length, and average wall thickness of the obtained tube (i.e., extrusion molded product), as well as the thickness of each layer, were all the same as those in Comparative Example 1.
[0107] <Comparative Example 3> An extrusion molded product having the following five-layer structure was manufactured. In this example, the same recycled resin as used in Comparative Example 2 was used as the resin for the innermost and outermost layers, but the thickness of the tube (extrusion molded product) was made thinner than that of Comparative Example 2.
[0108] Innermost layer: Recycled low-density polyethylene resin (density: 0.93 g / cm3) made from waste from our own factories 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load), number average molecular weight: 29400, endothermic peak temperatures: 109°C, 122°C, 164°C) First adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Middle layer: Ethylene-vinyl alcohol copolymer (density: 1.14 g / cm 3 , MFR: 12.0 g / 10 min (210°C, 21.18 N load) Second adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Outermost layer: Recycled low-density polyethylene resin (density: 0.93 g / cm3) made from waste from our own factories 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load), number average molecular weight: 29400, endothermic peak temperatures: 109°C, 122°C, 164°C)
[0109] Except for changing the resin material of each layer to the above resin material, a tube was molded in the same manner as in Comparative Example 1. The resulting tube (i.e., extrusion molded product) had a circumference of 108 mm, a length of 150 mm, and an average thickness of 0.29 mm. The thicknesses of the innermost layer, first adhesive layer, intermediate layer, second adhesive layer, and outermost layer were 145 μm, 10 μm, 40 μm, 10 μm, and 85 μm, respectively.
[0110] <Comparative Example 4> An extrusion molded product having the following five-layer structure was manufactured. In this example, recycled low-density polyethylene resin provided by a recycled material manufacturer was used as the resin for the innermost and outermost layers. The recycled low-density polyethylene resin used did not meet requirement (i): "average molecular weight of 30,000 or more", but met requirement (ii): "endothermic peaks obtained by differential scanning calorimetry are present only within the range of 100 to 140°C".
[0111] Innermost layer: Recycled low-density polyethylene resin (density: 0.92 g / cm3) provided by a recycled material manufacturer 3 , MFR: 4.0 g / 10 min (190°C, 21.18 N load), number average molecular weight: 21800, endothermic peak temperatures: 105°C, 122°C, 126°C) First adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Middle layer: Ethylene-vinyl alcohol copolymer (density: 1.14 g / cm 3 , MFR: 12.0 g / 10 min (210°C, 21.18 N load) Second adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Outermost layer: Recycled low-density polyethylene resin (density: 0.92 g / cm3) provided by a recycled material manufacturer 3 , MFR: 4.0 g / 10 min (190°C, 21.18 N load), number average molecular weight: 21800, endothermic peak temperatures: 105°C, 122°C, 126°C)
[0112] Except for changing the resin material of each layer to the above resin material, a tube was molded in the same manner as in Comparative Example 1. The circumference, length, and average wall thickness of the obtained tube (i.e., extrusion molded product), as well as the thickness of each layer, were all the same as those in Comparative Example 1.
[0113] <Comparative Example 5> An extrusion molded product with the following five-layer structure was manufactured. In this example, a mixture of virgin resin and ethylene-vinyl alcohol copolymer as an impurity (pseudo recycled material) was used as the resin for the innermost and outermost layers. The resin (pseudo recycled material) used contained low-density polyethylene resin as the main component and was not colored. The resin (pseudo recycled material) used met requirement (i): "average molecular weight is 30,000 or more", but did not meet requirement (ii): "endothermic peak obtained by differential scanning calorimetry is present only within the range of 100 to 140°C".
[0114] Innermost layer: Petroleum-derived low-density polyethylene resin (density: 0.92 g / cm 3, MFR: 1.9 g / 10 min (190 °C, 21.18 N load)) and ethylene-vinyl alcohol copolymer (density: 1.14 g / cm 3 , MFR: 12.0 g / 10 min (210°C, 21.18 N load)) in a mass ratio of 100:10 (number average molecular weight: 52200, endothermic peak temperatures: 109°C, 164°C) First adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Middle layer: Ethylene-vinyl alcohol copolymer (density: 1.14 g / cm 3 , MFR: 12.0 g / 10 min (210°C, 21.18 N load) Second adhesive layer: petroleum-derived maleic anhydride modified low-density polyethylene resin (density: 0.93 g / cm 3 , MFR: 1.0 g / 10 min (190°C, 21.18 N load) Outermost layer: Petroleum-derived low-density polyethylene resin (density: 0.92 g / cm 3 , MFR: 1.9 g / 10 min (190 °C, 21.18 N load)) and ethylene-vinyl alcohol copolymer (density: 1.14 g / cm 3 , MFR: 12.0 g / 10 min (210°C, 21.18 N load)) in a mass ratio of 100:10 (number average molecular weight: 52200, endothermic peak temperatures: 109°C, 164°C)
[0115] Except for changing the resin material of each layer to the above resin material, a tube was molded in the same manner as in Comparative Example 1. The circumference, length, and average wall thickness of the obtained tube (i.e., extrusion molded product), as well as the thickness of each layer, were all the same as those in Comparative Example 1.
[0116] [2] Evaluation method The properties of the tubes of Examples 1 to 4 and Comparative Examples 1 to 5 were evaluated by the following methods.
[0117] <Number average molecular weight> The number average molecular weight of the resin was determined by gel permeation chromatography according to the method described in the detailed description of the present application. That is, the measurement of the number average molecular weight using gel permeation chromatography was performed under the following conditions. High-temperature GPC equipment: Tosoh HLC-8321GPC / HT high-temperature gel permeation chromatograph Columns: 2 x Tosoh TSKgel GMH6-HT, 2 x Tosoh TSKgel GMH6-HTL Solvent: o-dichlorobenzene (containing 0.025% by mass BHT) Flow rate: 1.0 mL / min Temperature: 140℃ Measured concentration: 20 mg / 20mL Injection volume: 0.4 mL
[0118] <Endothermic peak temperature> The endothermic peak temperature of the resin (which indicates the melting point) was determined by differential scanning calorimetry according to the method described in the detailed description of the present application. That is, the differential scanning calorimetry was performed as follows using a differential scanning calorimeter: TA Instrument Q200. Specifically, about 5 mg was cut out from the sample tube and sealed in an aluminum pan for measurement. Thereafter, the temperature was raised from room temperature (20°C) to 200°C at a rate of 10°C / min, then lowered to room temperature (20°C) at 10°C / min, and again raised from room temperature (20°C) to 200°C at 10°C / min, and the melting endothermic peak temperature of the sample was measured.
[0119] <Possibility of molding> The feasibility of extrusion molding was evaluated as follows. Evaluation criteria ○: Molding was possible ×: Unable to mold
[0120] <Ultrasonic seal strength> Using an ultrasonic sealer (TS-2 manufactured by Branson, Power Supply 2000X), the sample was sealed under the sealing conditions of 90% amplitude and 200 msec welding time, and then evaluated by the method described below. The sealed sample was cut into 15 mm wide strips to prepare test pieces. The sealed portion of the test piece was opened 180° and attached to the grip of a tensile tester (manufactured by Shimadzu Corporation, product name AUTOGRAPH AGS-X). A T-type tensile test was performed at a tensile speed of 50 mm / min, and the stable value was taken as the ultrasonic seal strength [kgf]. Evaluation criteria 〇: 4.0 kgf or more △: 3.0 kgf or more, less than 4.0 kgf × : Less than 3.0 kgf
[0121] <Surface roughness> The surface roughness of the resulting tube was visually inspected. Evaluation criteria 〇: No roughness △: Slightly rough ×: Significant roughness
[0122] [3] Evaluation results The evaluation results are shown in Tables 1 and 2.
[0123] [Table 1]
[0124] [Table 2]
[0125] In Examples 1 to 4 and Comparative Examples 1, 2, and 5, tubular extrusion molded products could be produced by extrusion molding, but in Comparative Examples 3 and 4, the tubes were deformed or torn, making it impossible to produce tubular extrusion molded products. For this reason, in Comparative Examples 3 and 4, evaluation of ultrasonic seal strength and surface roughness were not performed.
[0126] The tubes (extrusion molded products) of Examples 1 to 4 showed good results in the evaluation of ultrasonic seal strength and surface roughness. The tube (extrusion molded product) of Comparative Example 1 showed good results in the evaluation of ultrasonic seal strength and surface roughness, but did not contain recycled resin. The tube (extrusion molded product) of Comparative Example 2 had insufficient ultrasonic seal strength and noticeable roughness was confirmed on the surface. Moreover, the tube (extrusion molded product) of Comparative Example 5 had insufficient ultrasonic seal strength and noticeable roughness was confirmed on the surface. [Explanation of symbols]
[0127] 1...extrusion molded product, 1a...innermost layer, 1b...first adhesive layer, 1c...middle layer, 1d...second adhesive layer, 1e...outermost layer, 10...tube container, 11...container body, 12...cap fitting portion, 21...body portion, 22...seal portion, 31...shoulder portion, 32...mouth portion.
Claims
1. An extrusion molded product for tube containers, which has an overall tubular shape and contains recycled low-density polyethylene resin, the recycled low-density polyethylene resin having an average molecular weight of 30,000 or more, and which has an endothermic peak obtained by differential scanning calorimetry only within the range of 100 to 140°C.
2. 2. The extrusion molded article according to claim 1, which has a multi-layer structure including at least an innermost layer and an outermost layer.
3. The extrusion molded product according to claim 2 , wherein the outermost layer comprises the recycled low density polyethylene resin.
4. 4. The extrusion molded article of claim 3, wherein the innermost layer comprises the recycled low density polyethylene resin.
5. 4. The extrusion molded product according to claim 3, wherein the innermost layer comprises a plant-derived low-density polyethylene resin and a plant-derived linear low-density polyethylene resin.
6. 3. The extrusion molded product according to claim 2, wherein the multilayer structure is a five-layer structure in which the innermost layer, the first adhesive layer, the intermediate layer, the second adhesive layer, and the outermost layer are laminated in this order from the inside to the outside.
7. The extrusion molded product according to claim 6 , wherein the intermediate layer contains a resin having gas barrier properties.
8. The extrusion molded product according to any one of claims 1 to 7, one or more layers disposed on the extrusion; A molded article for a tube container comprising:
9. A container body including the extrusion molded article according to any one of claims 1 to 7, one end of which is sealed, or the molded article according to claim 8, one end of which is sealed; a cap fitting portion joined to the other end of the extrusion molded product having one end sealed or the molded product having one end sealed; A tube container comprising:
10. A container body including the extrusion molded article according to any one of claims 1 to 7, one end of which is sealed, or the molded article according to claim 8, one end of which is sealed; a cap fitting portion joined to the other end of the extrusion molded product or the molded product having one end sealed; The contents filled in the container body; A container-packed article comprising:
Citation Information
Patent Citations
Manufacturing device for plastic tube containers
JP1999309406A
Method and apparatus for producing plastic tube container
JP1999309785A
Cited By
Robot, control method of robot, and computer program product
CN121696930A