Rubber composition containing cellulose nanofibers

The use of a modified rubber coupling agent with cellulose nanofibers in rubber compositions addresses the dispersion and viscoelastic challenges, resulting in cured rubber products with enhanced mechanical and viscoelastic properties suitable for tires and shoe outsoles.

JP2024165318APending Publication Date: 2024-11-28ASAHI KASEI KOGYO KABUSHIKI KAISHA

Patent Information

Application Number
JP2023081424
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing rubber compositions containing cellulose nanofibers face challenges in achieving a broad control of viscoelastic properties while maintaining excellent mechanical properties, as they tend to be hydrophilic and difficult to disperse uniformly in hydrophobic rubber, affecting the performance of cured rubber products.

Method used

A method involving the use of a modified rubber coupling agent, such as maleic anhydride modified isoprene rubber, with a specific molecular weight and content, is employed to produce a masterbatch with cellulose nanofibers and rubber, enhancing their interaction and dispersion, thereby controlling viscoelastic properties and mechanical properties.

Benefits of technology

The method results in cured rubber products with excellent mechanical properties and desired viscoelastic properties, particularly low loss tangent, enabling applications in tires and shoe outsoles with improved performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165318000001
    Figure 2024165318000001
  • Figure 2024165318000002
    Figure 2024165318000002
  • Figure 2024165318000003
    Figure 2024165318000003
Patent Text Reader

Abstract

To provide a rubber cured product that has excellent mechanical properties and exhibits desired viscoelastic properties (in particular, a low loss tangent), as well as a masterbatch and a rubber composition useful for producing the rubber cured product.SOLUTION: There is provided a method for producing a masterbatch comprising cellulose nanofibers and a rubber. The method comprises a step of kneading a masterbatch component containing the cellulose nanofibers, a first rubber and a modified rubber-based coupling agent to produce a masterbatch. A modified group of the modified rubber-based coupling agent is a modified maleic anhydride group. The content of the modified group in the modified rubber-based coupling agent is 1.5 mass% to 20 mass%. The modified rubber-based coupling agent is a liquid rubber, and the number-average molecular weight of the modified rubber-based coupling agent is 10,000 to 100,000.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] One aspect of the present disclosure relates to a rubber composition containing cellulose nanofibers. [Background technology]

[0002] Conventionally, rubber molded bodies are required to have a high level of balance among various properties such as mechanical strength, flexibility, abrasion resistance, and processability. For example, in order to improve elastic modulus, hardness, abrasion resistance, and the like, fillers are generally incorporated into rubber molded bodies. In order for such rubber molded bodies containing fillers to exhibit the desired properties, it is important that the fillers are well dispersed in the rubber. In recent years, due to the increasing awareness of environmental issues, various attempts have been made to use cellulose, which is a low specific gravity and renewable material, as a filler to be incorporated into rubber molded bodies. Among these, cellulose nanofibers are extremely promising as a filler for polymer molded bodies because of the good reinforcing effect per amount of use given to the polymer molded body when it is combined with various polymers to form the polymer molded body. If cellulose nanofibers can be used in rubber molded bodies, it is possible to provide rubber molded bodies that have low specific gravity, excellent physical properties, can be used for a variety of applications, and are advantageous in terms of transportation costs and disposal costs. However, cellulose nanofibers are essentially hydrophilic due to the contribution of hydroxyl groups in cellulose, and therefore it is generally difficult to mix them with rubber, which is a highly hydrophobic material. Therefore, various attempts have been made to improve the compatibility between cellulose nanofibers and rubber.

[0003] For example, Patent Document 1 describes a rubber composition for tires that includes a rubber component, microfibrillated plant fibers, which may be cellulose fibers, and a modifier capable of covalently bonding to the microfibrillated plant fibers. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-41076 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when the formulation of a rubber composition containing cellulose nanofibers is changed to improve the mechanical properties of the cured product of the rubber composition, for example, the viscoelastic properties of the cured product also change, making it difficult to produce a cured rubber product that has excellent mechanical properties and desired viscoelastic properties. The technology described in Patent Document 1 aims to provide a rubber composition for tires that has excellent dispersibility of microfibrillated plant fibers and can improve tensile properties and fuel efficiency, but does not provide a rubber composition that can achieve high mechanical properties of the cured rubber while widely controlling the viscoelastic properties within a desired range.

[0006] An object of one aspect of the present invention is to solve the above-mentioned problems and to provide a cured rubber product that has excellent mechanical properties and desired viscoelastic properties (particularly a low loss tangent), as well as a masterbatch and a rubber composition that are useful for producing the cured rubber product. [Means for solving the problem]

[0007] This disclosure encompasses the following items. [Item 1] A method for producing a masterbatch containing cellulose nanofibers and rubber, comprising the steps of: The method includes a step of kneading a masterbatch component including cellulose nanofibers, a first rubber, and a modified rubber-based coupling agent to produce a masterbatch, the modified group of the modified rubber coupling agent is a maleic anhydride modified group, The modified rubber coupling agent has a modifying group content of 1.5% by mass to 20% by mass, the modified rubber coupling agent is a liquid rubber, The modified rubber coupling agent has a number average molecular weight of 10,000 to 100,000. [Item 2] 2. The method according to item 1, wherein in the master batch component, an amount of the cellulose nanofibers relative to 100 parts by mass of the first rubber is 10 parts by mass to 100 parts by mass. [Item 3] 3. The method according to item 1 or 2, wherein the content of the modified rubber-based coupling agent in the master batch component is 5 parts by mass to 100 parts by mass based on 100 parts by mass of the first rubber. [Item 4] 4. The method according to any one of items 1 to 3, wherein in the master batch component, the amount of the modified rubber coupling agent relative to 100 parts by mass of the cellulose nanofibers is 30 parts by mass to 500 parts by mass. [Item 5] 5. The method according to any one of items 1 to 4, wherein the modified rubber coupling agent is maleic anhydride modified isoprene rubber. [Item 6] 6. The method according to any one of items 1 to 5, wherein the masterbatch components further comprise an unmodified liquid rubber. [Item 7] 7. The method according to any one of items 1 to 6, wherein the first rubber is one or more selected from the group consisting of styrene-butadiene rubber, natural rubber, and isoprene rubber. [Item 8] 8. The method according to any one of items 1 to 7, wherein the cellulose nanofibers are mechanically defibrated. [Item 9] A method for producing a rubber composition containing cellulose nanofibers and rubber, comprising the steps of: A step of producing a masterbatch by the method according to any one of items 1 to 8; and A step of kneading the master batch and a rubber composition component including a second rubber to produce a rubber composition; A method comprising: [Item 10] A method for producing a rubber composition containing cellulose nanofibers and rubber, comprising the steps of: A step of producing a masterbatch containing cellulose nanofibers and a first rubber; and A step of kneading a rubber composition component including the master batch, a second rubber, and a modified rubber-based coupling agent to produce a rubber composition; Including, the modified group of the modified rubber coupling agent is a maleic anhydride modified group, The modified rubber coupling agent has a modifying group content of 1.5% by mass to 20% by mass, the modified rubber coupling agent is a liquid rubber, The method for producing a rubber composition, wherein the modified rubber coupling agent has a number average molecular weight of 10,000 to 100,000. [Item 11] Item 11. The method according to item 9 or 10, wherein in the rubber composition component, an amount of the cellulose nanofibers per 100 parts by mass of the total of the first rubber and the second rubber is 0.5 parts by mass to 30 parts by mass. [Item 12] 12. The method according to any one of items 9 to 11, wherein in the rubber composition component, a content of the modified rubber-based coupling agent relative to a total of 100 parts by mass of the first rubber and the second rubber is 1 part by mass to 15 parts by mass. [Item 13] 13. The method according to any one of items 9 to 12, wherein in the rubber composition component, the amount of the modified rubber coupling agent is 80 parts by mass to 300 parts by mass per 100 parts by mass of the cellulose nanofibers. [Item 14] 14. The method according to any one of items 9 to 13, wherein the modified rubber coupling agent is maleic anhydride modified isoprene rubber. [Item 15] 15. The method according to any one of items 9 to 14, wherein the rubber composition component further comprises an unmodified liquid rubber. [Item 16] 16. The method according to any one of items 9 to 15, wherein the first rubber and / or the second rubber is one or more selected from the group consisting of styrene-butadiene rubber, natural rubber, and isoprene rubber. [Item 17] 17. The method according to any one of items 9 to 16, wherein the cellulose nanofibers are mechanically defibrated. [Item 18] A step of producing a rubber composition by the method according to any one of items 9 to 17; and curing the rubber composition to produce a rubber cured product; The method for producing a cured rubber product comprising the steps of: [Item 19] A masterbatch comprising cellulose nanofibers and rubber, The masterbatch is a mixture of masterbatch components including cellulose nanofibers, a first rubber, and a modified rubber-based coupling agent, the modified group of the modified rubber coupling agent is a maleic anhydride modified group, The modified rubber coupling agent has a modifying group content of 1.5% by mass to 20% by mass, the modified rubber coupling agent is a liquid rubber, The modified rubber coupling agent has a number average molecular weight of 10,000 to 100,000. [Item 20] Item 20. The masterbatch according to item 19, wherein in the masterbatch components, an amount of the cellulose nanofibers relative to 100 parts by mass of the first rubber is 10 parts by mass to 100 parts by mass. [Item 21] 21. The masterbatch according to item 19 or 20, wherein the content of the modified rubber coupling agent in the masterbatch components is 5 parts by mass to 100 parts by mass relative to 100 parts by mass of the first rubber. [Item 22] 22. The masterbatch according to any one of items 19 to 21, wherein the amount of the modified rubber coupling agent in the masterbatch components is 30 parts by mass to 500 parts by mass per 100 parts by mass of the cellulose nanofibers. [Item 23] 23. The masterbatch according to any one of items 19 to 22, wherein the modified rubber coupling agent is maleic anhydride modified isoprene rubber. [Item 24] 24. The masterbatch according to any one of items 19 to 23, wherein the masterbatch components further comprise an unmodified liquid rubber. [Item 25] 25. The masterbatch according to any one of items 19 to 24, wherein the first rubber is one or more selected from the group consisting of styrene-butadiene rubber, natural rubber, and isoprene rubber. [Item 26] 26. The masterbatch according to any one of items 19 to 25, wherein the cellulose nanofibers are mechanically defibrated cellulose nanofibers. [Item 27] A rubber composition comprising cellulose nanofibers and rubber, the rubber composition is a mixture of rubber composition components including cellulose nanofibers, a first rubber, a second rubber, and a modified rubber-based coupling agent; the modified group of the modified rubber coupling agent is a maleic anhydride modified group, The modified rubber coupling agent has a modifying group content of 1.5% by mass to 20% by mass, the modified rubber coupling agent is a liquid rubber, The rubber composition, wherein the modified rubber coupling agent has a number average molecular weight of 10,000 to 100,000. [Item 28] Item 28. The rubber composition according to item 27, wherein in the rubber composition component, an amount of the cellulose nanofibers per 100 parts by mass of the total of the first rubber and the second rubber is 0.5 parts by mass to 30 parts by mass. [Item 29] Item 29. The rubber composition according to item 27 or 28, wherein the content of the modified rubber coupling agent in the rubber composition component is 1 part by mass to 15 parts by mass relative to a total of 100 parts by mass of the first rubber and the second rubber. [Item 30] 30. The rubber composition according to any one of items 27 to 29, wherein in the rubber composition components, the amount of the modified rubber coupling agent per 100 parts by mass of the cellulose nanofibers is 80 parts by mass to 300 parts by mass. [Item 31] Item 31. The rubber composition according to any one of Items 27 to 30, wherein the modified rubber coupling agent is a maleic anhydride modified isoprene rubber. [Item 32] 32. The rubber composition according to any one of items 27 to 31, wherein the rubber composition components further contain an unmodified liquid rubber. [Item 33] Item 33. The rubber composition according to any one of Items 27 to 32, wherein the first rubber and / or the second rubber is one or more selected from the group consisting of styrene-butadiene rubber, natural rubber, and isoprene rubber. [Item 34] Item 34. The rubber composition according to any one of Items 27 to 33, wherein the cellulose nanofibers are mechanically defibrated. [Item 35] 35. A cured rubber product, which is a cured product of the rubber composition according to any one of items 27 to 34. [Item 36] 36. A tire comprising the rubber vulcanizate according to item 35. [Item 37] Item 36. An anti-vibration rubber comprising the rubber cured product according to item 35. [Item 38] 36. A shoe outsole comprising the rubber vulcanized product according to item 35. Effect of the Invention

[0008] According to one aspect of the present invention, it is possible to provide a cured rubber product that exhibits excellent mechanical properties and desired viscoelastic properties (particularly low loss tangent), as well as a masterbatch and a rubber composition that are useful for producing the cured rubber product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, exemplary embodiments of the present invention (hereinafter, abbreviated as "present embodiments") will be described, but the present invention is not limited to these embodiments. Note that, unless otherwise specified, the characteristic values ​​of the present disclosure are values ​​measured by the method described in the [Examples] section of the present disclosure or a method that is understood to be equivalent to the above by a person skilled in the art.

[0010] One aspect of the present invention provides a masterbatch containing cellulose nanofibers and rubber and a method for producing the same. Another aspect of the present invention provides a rubber composition containing cellulose nanofibers and rubber and a method for producing the same. Another aspect of the present invention provides a cured rubber product, which is a cured product of a rubber composition containing cellulose nanofibers and rubber, and a method for producing the same. Another aspect of the present invention provides various molded articles containing the cured rubber product. In one aspect, the masterbatch components for producing the masterbatch include cellulose nanofibers, a modified rubber-based coupling agent, and a first rubber, and the rubber composition components for producing the rubber composition include cellulose nanofibers, a modified rubber-based coupling agent, and a second rubber.

[0011] Cellulose nanofibers are essentially hydrophilic due to their hydroxyl groups, while rubber is essentially hydrophobic, and it is usually difficult to uniformly disperse cellulose nanofibers in rubber. For example, the use of a dispersant can improve dispersibility to a certain extent, but in order to obtain a cured rubber product that is useful for a wide range of applications, it is important to develop a method for producing a cured rubber product that exhibits good mechanical properties while allowing the viscoelastic properties (particularly the loss tangent) to be adjusted according to the desired application. The present inventors have found that a masterbatch or rubber composition obtained by using a modified rubber coupling agent is useful for producing a cured rubber product that has good mechanical properties and exhibits the desired viscoelastic properties according to the application.

[0012] In one embodiment, at least a portion of the modified rubber-based coupling agent may be present in the masterbatch or rubber composition in a state of being bonded to or interacting with the cellulose nanofibers. In a typical embodiment, at least a portion of the modified rubber-based coupling agent is bonded to or interacts with the cellulose nanofibers, while another rubber (first rubber, second rubber, etc.) that the masterbatch or rubber composition may contain, and optionally a portion of the modified rubber-based coupling agent, are not bonded to or interacting with the cellulose nanofibers. In one embodiment, when the masterbatch or rubber composition is treated with a rubber-dissolving solvent (hexane or cyclohexane in one embodiment), the rubber portion bonded to the cellulose nanofibers forms a residue together with the cellulose nanofibers, and the rubber portion not bonded to the cellulose nanofibers is dissolved in the solvent. In one embodiment, the modified rubber-based coupling agent is a rubber having a specific range of modifying group content and molecular weight, and thus is easily bonded to or interacts with the cellulose nanofibers and with the rubber, and has an extremely excellent coupling effect between the cellulose nanofibers and the rubber. The masterbatch or rubber composition of this embodiment is advantageous in providing a cured rubber product that has excellent mechanical properties and desired viscoelastic properties due to the contribution of the modified rubber-based coupling agent.

[0013] Hereinafter, preferred examples of the masterbatch, rubber composition, cured rubber product, and their applications will be described. The amount of each component described as a value in the masterbatch component or the rubber composition component may be regarded as the amount of each component in the masterbatch or the rubber composition of this embodiment.

[0014] <Master batch> In one embodiment, the masterbatch includes cellulose nanofibers and a rubber. In one embodiment, the masterbatch can be produced by a method including a step of kneading masterbatch components including cellulose nanofibers, a first rubber, and a modified rubber-based coupling agent to produce a masterbatch.

[0015] <Cellulose nanofiber> As raw materials for cellulose nanofibers, natural cellulose and regenerated cellulose can be used. As natural cellulose, wood pulp obtained from wood species (broadleaf or coniferous trees), non-wood pulp obtained from non-wood species (cotton, bamboo, hemp, bagasse, kenaf, cotton linters, sisal, straw, etc.), and cellulose aggregates produced by animals (e.g., ascidians), algae, and microorganisms (e.g., acetic acid bacteria) can be used. As regenerated cellulose, regenerated cellulose fibers (viscose, cupra, tencel, etc.), cellulose derivative fibers, and ultrafine threads of regenerated cellulose or cellulose derivatives obtained by electrospinning can be used.

[0016] In one embodiment, the cellulose nanofiber is a fine cellulose fiber obtained by treating pulp or the like with hot water of 100°C or higher, hydrolyzing and weakening hemicellulose, and then mechanically defibrating the cellulose nanofiber by a pulverizing method such as a high-pressure homogenizer, a microfluidizer, a ball mill, a disk mill, or a mixer (e.g., a homomixer). In one embodiment, the cellulose nanofiber has a number average fiber diameter of 1 nm or more and 1000 nm or less. The cellulose nanofiber may be chemically modified as described below, but in terms of the reinforcing effect as a filler, it is preferable to use a non-chemically modified cellulose nanofiber. For example, cellulose nanofibers defibrated by chemical oxidation treatment such as 2,2,6,6-tetramethylpiperidine-1-oxyl (TEMPO) phosphate ester tend to have low heat resistance due to the ionic group (e.g., carboxyl group) introduced into the cellulose nanofiber, and also tend to have a small fiber diameter after defibration. In terms of the reinforcing effect as a filler, cellulose nanofibers that are only mechanically defibrated (i.e., not chemically defibrated such as oxidation) are more advantageous. Therefore, in a preferred embodiment, the cellulose nanofibers are mechanically defibrated, and in a preferred embodiment, the cellulose nanofibers do not have ionic groups. In this disclosure, the cellulose nanofibers having no ionic groups means that the amount of ionic groups measured by conductometric titration is 0.1 mmol / g or less.

[0017] The slurry can be prepared by dispersing the cellulose fibers in a liquid medium, and the dispersion may be carried out using a high-pressure homogenizer, a microfluidizer, a ball mill, a disk mill, a mixer (e.g., a homomixer), etc., and the product of the defibration may be obtained as the product of the slurry preparation process of the present disclosure. The liquid medium in the slurry may further contain, in addition to water, other liquid media (e.g., organic solvents) either alone or in combination of two or more. Examples of the organic solvent include commonly used water-miscible organic solvents, such as alcohols having a boiling point of 50° C. to 170° C. (e.g., methanol, ethanol, n-propanol, i-propanol, n-butanol, i-butanol, s-butanol, t-butanol, etc.); ethers (e.g., propylene glycol monomethyl ether, 1,2-dimethoxyethane, diisopropyl ether, tetrahydrofuran, 1,4-dioxane, etc.); carboxylic acids (e.g., formic acid, acetic acid, lactic acid, etc.); esters (e.g., ethyl acetate, vinyl acetate, etc.); ketones (e.g., acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, etc.); and nitrogen-containing solvents (dimethylformamide, dimethylacetamide, acetonitrile, etc.). In a typical embodiment, the liquid medium in the slurry is substantially water alone.

[0018] Since the cellulose raw material contains alkali soluble matter and sulfuric acid insoluble matter (lignin, etc.), the alkali soluble matter and sulfuric acid insoluble matter may be reduced through a purification process such as delignification by cooking and a bleaching process. On the other hand, the purification process such as delignification by cooking and the bleaching process cut the molecular chains of cellulose, changing the weight average molecular weight and number average molecular weight, so it is desirable to control the purification process and bleaching process of the cellulose raw material so that the weight average molecular weight of the cellulose nanofiber and the ratio of the weight average molecular weight to the number average molecular weight are within an appropriate range.

[0019] In addition, since the refining process such as delignification by cooking and the bleaching process reduce the molecular weight of cellulose molecules, there is concern that these processes will result in a lower molecular weight of cellulose nanofibers and alter the cellulose raw material, increasing the proportion of alkali-soluble matter. Since alkali-soluble matter has poor heat resistance, it is desirable to control the refining process and bleaching process of the cellulose raw material so that the amount of alkali-soluble matter contained in the cellulose raw material is within a certain range or less.

[0020] In one aspect, the number average fiber diameter of the cellulose nanofibers is preferably 2 to 1000 nm from the viewpoint of obtaining a good effect of improving physical properties by the cellulose nanofibers. The number average fiber diameter of the cellulose nanofibers is more preferably 4 nm or more, or 5 nm or more, or 10 nm or more, or 15 nm or more, or 20 nm or more, and more preferably 500 nm or less, or 450 nm or less, or 400 nm or less, or 350 nm or less, or 300 nm or less, or 250 nm or less.

[0021] From the viewpoint of satisfactorily improving the mechanical properties of a rubber composition containing cellulose nanofibers with a small amount of cellulose nanofibers, the average fiber length (L) / fiber diameter (D) ratio of the cellulose nanofibers is preferably 30 or more, or 50 or more, or 80 or more, or 100 or more, or 120 or more, or 150 or more. There is no particular upper limit, but from the viewpoint of handleability, it is preferably 5,000 or less.

[0022] In the present disclosure, the fiber length, fiber diameter, and L / D ratio of the cellulose nanofibers are determined by dispersing an aqueous dispersion of cellulose nanofibers using a high-shear homogenizer (e.g., Nippon Seiki Co., Ltd., product name "Excel Auto Homogenizer ED-7") under processing conditions: rotation speed 15,000 rpm × 5 minutes, diluting the aqueous dispersion with pure water to 0.1 to 0.5 mass%, casting it on mica, and air-drying it to obtain a measurement sample, and measuring it with a scanning electron microscope (SEM) or atomic force microscope (AFM). Specifically, the length (L) and diameter (D) of 100 randomly selected cellulose nanofibers are measured in an observation field where the magnification is adjusted so that at least 100 cellulose nanofibers are observed, and the ratio (L / D) is calculated. The number average value of the fiber length (L), the number average value of the fiber diameter (D), and the number average value of the ratio (L / D) are calculated for the cellulose nanofibers.

[0023] Alternatively, the fiber length, fiber diameter, and L / D ratio of the cellulose nanofibers contained in the powder, master batch, rubber composition, cured rubber, etc. can be confirmed by measuring these as measurement samples using the above-mentioned measurement methods.

[0024] Alternatively, the fiber length, fiber diameter, and L / D ratio of cellulose nanofibers contained in powders, masterbatches, rubber compositions, cured rubber products, etc. can be confirmed by dissolving the polymer components contained therein in an organic or inorganic solvent capable of dissolving the polymer components, isolating the cellulose nanofibers, thoroughly washing with the solvent, and then replacing the solvent with pure water to prepare an aqueous dispersion, diluting the cellulose nanofiber concentration with pure water to 0.1 to 0.5% by mass, casting on mica, and air-drying the resulting sample to be measured using the above-mentioned measurement method. At this time, the measurement is performed on 100 or more randomly selected cellulose nanofibers.

[0025] The crystallinity of the cellulose nanofiber is preferably 55% or more. When the crystallinity is in this range, the mechanical properties (strength, dimensional stability) of the cellulose itself are high, so that when the cellulose nanofiber is dispersed in rubber, the strength and dimensional stability of the rubber composite tend to be high. A more preferable lower limit of the crystallinity is 60%, even more preferably 70%, and most preferably 80%. There is no particular upper limit for the crystallinity of the cellulose nanofiber, and the higher the better, but from the viewpoint of production, a preferable upper limit is 99%.

[0026] Alkali-soluble polysaccharides such as hemicellulose and acid-insoluble components such as lignin are present between the microfibrils and between the microfibril bundles of plant-derived cellulose nanofibers. Hemicellulose is a polysaccharide composed of sugars such as mannan and xylan, and plays a role in binding the microfibrils together by hydrogen bonding with cellulose. Lignin is a compound having an aromatic ring, and is known to be covalently bonded to hemicellulose in the cell walls of plants. If there is a large amount of impurities such as lignin remaining in the cellulose nanofibers, discoloration may occur due to heat during processing. Therefore, from the viewpoint of suppressing discoloration of the rubber composite during extrusion processing and molding processing, it is desirable to set the crystallinity of the cellulose nanofibers within the above-mentioned range.

[0027] The degree of crystallinity here, when the cellulose is cellulose type I crystal (derived from natural cellulose), is calculated from the diffraction pattern (2θ / deg. is 10 to 30) obtained by measuring a sample by wide-angle X-ray diffraction, using the Segal method and the following formula: Crystallinity (%) = ([diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] - [diffraction intensity due to amorphous matter at 2θ / deg. = 18]) / [diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] × 100

[0028] When the cellulose is cellulose II type crystal (derived from regenerated cellulose), the degree of crystallinity can be calculated from the absolute peak intensity h0 at 2θ=12.6° assigned to the (110) plane peak of cellulose II type crystal in wide-angle X-ray diffraction and the peak intensity h1 from the baseline at this interplanar spacing, according to the following formula: Crystallinity (%) =h1 / h0 ×100

[0029] Known cellulose crystal forms include type I, type II, type III, and type IV, of which types I and II are particularly widely used, and types III and IV have been obtained on a laboratory scale but are not widely used on an industrial scale. The cellulose nanofibers of the present disclosure are preferably cellulose nanofibers containing cellulose type I crystals or cellulose type II crystals, since they have relatively high structural mobility and, by dispersing the cellulose nanofibers in rubber, can provide molded articles with a lower linear expansion coefficient and superior strength and elongation during tensile and bending deformation, and more preferably cellulose nanofibers containing cellulose type I crystals and having a crystallinity of 55% or more.

[0030] In addition, the degree of polymerization of the cellulose nanofiber is preferably 100 or more, more preferably 150 or more, more preferably 200 or more, more preferably 300 or more, more preferably 400 or more, more preferably 450 or more, and preferably 3500 or less, more preferably 3300 or less, more preferably 3200 or less, more preferably 3100 or less, and more preferably 3000 or less.

[0031] From the viewpoint of processability and mechanical property expression, it is desirable that the degree of polymerization of the cellulose nanofiber is within the above-mentioned range. From the viewpoint of processability, it is preferable that the degree of polymerization is not too high, and from the viewpoint of mechanical property expression, it is desirable that the degree of polymerization is not too low.

[0032] The degree of polymerization of cellulose nanofibers refers to the average degree of polymerization measured according to the reduced specific viscosity method using a copper ethylenediamine solution described in the Verification Test (3) of the "15th Revised Japanese Pharmacopoeia Commentary (published by Hirokawa Publishing)."

[0033] In one embodiment, the weight average molecular weight (Mw) of the cellulose nanofiber is 100,000 or more, more preferably 200,000 or more. The ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) is 6 or less, preferably 5.4 or less. The larger the weight average molecular weight, the fewer the number of terminal groups of the cellulose molecule. In addition, since the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight represents the width of the molecular weight distribution, the smaller the Mw / Mn, the fewer the number of terminals of the cellulose molecule. Since the terminals of the cellulose molecules are the starting points of thermal decomposition, when the cellulose molecules of the cellulose nanofibers not only have a large weight average molecular weight but also have a narrow molecular weight distribution, a cellulose nanofiber with particularly high heat resistance and a rubber composition containing the cellulose nanofiber and rubber can be obtained. The weight average molecular weight (Mw) of the cellulose nanofiber may be, for example, 600,000 or less, or 500,000 or less, from the viewpoint of the availability of the cellulose raw material. From the viewpoint of ease of production of cellulose nanofibers, the ratio (Mw / Mn) of weight average molecular weight to number average molecular weight (Mn) may be, for example, 1.5 or more, or 2 or more. Mw can be controlled to the above range by selecting a cellulose raw material having an Mw appropriate for the purpose, by appropriately performing physical and / or chemical treatment on the cellulose raw material within an appropriate range, etc. Mw / Mn can also be controlled to the above range by selecting a cellulose raw material having an Mw / Mn appropriate for the purpose, by appropriately performing physical and / or chemical treatment on the cellulose raw material within an appropriate range, etc. Each of the Mw and Mw / Mn of the cellulose raw material may be within the above range in one embodiment. In both the control of Mw and the control of Mw / Mn, examples of the physical treatment include dry or wet grinding using a microfluidizer, ball mill, disk mill, or the like, and physical treatments that apply mechanical forces such as impact, shear, friction, and the like using a crusher, homomixer, high-pressure homogenizer, ultrasonic device, or the like, and examples of the chemical treatment include digestion, bleaching, acid treatment, and conversion to regenerated cellulose.

[0034] The weight average molecular weight and number average molecular weight of the cellulose nanofiber referred to here are values ​​obtained by dissolving the cellulose nanofiber in N,N-dimethylacetamide containing added lithium chloride and then performing gel permeation chromatography using N,N-dimethylacetamide as a solvent.

[0035] Methods for controlling the degree of polymerization (i.e., average degree of polymerization) or molecular weight of cellulose nanofibers include hydrolysis. Hydrolysis promotes depolymerization of amorphous cellulose inside the cellulose nanofibers, decreasing the average degree of polymerization. At the same time, hydrolysis removes impurities such as hemicellulose and lignin in addition to the above-mentioned amorphous cellulose, making the inside of the fiber more porous.

[0036] The hydrolysis method is not particularly limited, and examples thereof include acid hydrolysis, alkali hydrolysis, hydrothermal decomposition, steam explosion, and microwave decomposition. These methods may be used alone or in combination of two or more. In the acid hydrolysis method, for example, α-cellulose obtained as pulp from a fibrous plant is used as a cellulose raw material, and this is dispersed in an aqueous medium, and an appropriate amount of a protonic acid, a carboxylic acid, a Lewis acid, a heteropoly acid, etc. is added, and the mixture is heated while stirring, so that the average degree of polymerization can be easily controlled. The reaction conditions such as temperature, pressure, and time at this time vary depending on the cellulose type, cellulose concentration, acid type, acid concentration, etc., but are appropriately adjusted so that the desired average degree of polymerization is achieved. For example, a condition in which a mineral acid aqueous solution of 2% by mass or less is used and cellulose nanofibers are treated at 100°C or higher under pressure for 10 minutes or more can be mentioned. Under these conditions, the catalyst component such as acid penetrates into the inside of the cellulose nanofibers, promoting hydrolysis, reducing the amount of catalyst component used, and making subsequent purification easier. The dispersion of the cellulose raw material during hydrolysis may contain, in addition to water, a small amount of an organic solvent within a range that does not impair the effects of the present invention.

[0037] Alkali-soluble polysaccharides that may be contained in cellulose nanofibers include hemicellulose, β-cellulose, and γ-cellulose. Alkali-soluble polysaccharides are understood by those skilled in the art as components obtained as the alkali-soluble portion of holocellulose obtained by solvent extraction and chlorine treatment of plants (e.g., wood) (i.e., components obtained by removing α-cellulose from holocellulose). Alkali-soluble polysaccharides are polysaccharides containing hydroxyl groups and have poor heat resistance, and may cause inconveniences such as decomposition when exposed to heat, yellowing during thermal aging, and a decrease in strength of cellulose nanofibers. Therefore, it is preferable that the content of alkali-soluble polysaccharides in cellulose nanofibers is low.

[0038] In one aspect, the average content of alkali-soluble polysaccharides in the cellulose nanofibers is preferably 20% by mass or less, 18% by mass or less, 15% by mass or less, or 12% by mass or less, relative to 100% by mass of the cellulose nanofibers, from the viewpoint of obtaining good dispersibility of the cellulose nanofibers. From the viewpoint of ease of production of the cellulose nanofibers, the above content may be 1% by mass or more, 2% by mass or more, or 3% by mass or more.

[0039] The average alkali-soluble polysaccharide content can be determined by the method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000), by subtracting the α-cellulose content from the holocellulose content (Wise method). This method is understood in the industry as a method for measuring the amount of hemicellulose. The alkali-soluble polysaccharide content is calculated three times for each sample, and the number average of the calculated alkali-soluble polysaccharide contents is taken as the average alkali-soluble polysaccharide content.

[0040] In one aspect, the average content of acid-insoluble components in the cellulose nanofibers is preferably 10% by mass or less, 5% by mass or less, or 3% by mass or less, relative to 100% by mass of the cellulose nanofibers, from the viewpoint of avoiding a decrease in heat resistance of the cellulose nanofibers and the associated discoloration. From the viewpoint of ease of production of the cellulose nanofibers, the above content may be 0.1% by mass or more, 0.2% by mass or more, or 0.3% by mass or more.

[0041] The average acid-insoluble content is determined as a quantitative determination of the acid-insoluble content using the Clason method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000). This method is understood in the industry as a method for measuring the amount of lignin. The sample is stirred in a sulfuric acid solution to dissolve cellulose, hemicellulose, etc., and then filtered through a glass fiber filter paper, and the resulting residue corresponds to the acid-insoluble content. The acid-insoluble content is calculated from the weight of the acid-insoluble content, and the number average of the acid-insoluble content calculated for the three samples is taken as the average acid-insoluble content.

[0042] The thermal decomposition temperature of cellulose nanofiber (T D ) is 270° C. or higher in one embodiment, from the viewpoint of being able to exhibit the heat resistance and mechanical strength desired for in-vehicle applications and the like, preferably 275° C. or higher, more preferably 280° C. or higher, and even more preferably 285° C. or higher. The higher the thermal decomposition onset temperature, the more preferable it is, but from the viewpoint of ease of production of cellulose nanofibers, it may be, for example, 320° C. or lower, or 300° C. or lower.

[0043] In this disclosure, T D is a value obtained from a graph in which the horizontal axis is temperature and the vertical axis is the weight residual rate % in thermogravimetry (TG) analysis. Starting from the weight of cellulose nanofiber at 150°C (a state in which most of the moisture has been removed) (weight loss of 0 wt%), the temperature is continued to be increased until the temperature at which the weight loss reaches 1 wt% (T 1% ) and the temperature at which the weight loss reaches 2 wt% (T 2%The temperature at the point where this line intersects with the horizontal line (baseline) that passes through the starting point of the weight loss of 0 wt% is called T D It is defined as:

[0044] 1% weight loss temperature (T 1% ) is the above T D This is the temperature at which the weight loss reaches 1% by weight, starting from the weight at 150°C, when the temperature is continued to be increased using the method described above.

[0045] Weight loss rate of cellulose nanofiber at 250°C (T 250℃ ) is the weight loss rate when cellulose nanofibers were kept at 250°C under nitrogen flow for 2 hours in TG analysis.

[0046] (chemical modification) The cellulose nanofibers may be chemically modified cellulose nanofibers. The cellulose nanofibers may be chemically modified in advance, for example, at the stage of raw pulp or linters, during or after the defibration treatment, or during or after the slurry preparation process, or during or after the drying (granulation) process.

[0047] As a modifying agent for cellulose nanofibers, a compound that reacts with the hydroxyl groups of cellulose can be used, and examples of such agents include esterifying agents, etherifying agents, and silylation agents. On the other hand, modifying agents having polar groups, such as carboxylic acids and phosphoric esters, tend to reduce the heat resistance of cellulose nanofibers by introducing ionic groups (e.g., carboxyl groups) into the cellulose nanofibers, and also tend to reduce the fiber diameter after defibration, so it is preferable not to use them from the viewpoint of the reinforcing effect as a filler. In a preferred embodiment, the chemical modification is acylation using an esterifying agent, and acetylation is particularly preferred. As the esterifying agent, acid halides, acid anhydrides, vinyl carboxylates, and carboxylic acids are preferred.

[0048] The acid halide may be at least one selected from the group consisting of compounds represented by the following formula: R 1-C(=O)-X (In the formula, R 1 represents an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 24 carbon atoms, or an aryl group having 6 to 24 carbon atoms, and X is Cl, Br, or I. Specific examples of acid halides include, but are not limited to, acetyl chloride, acetyl bromide, acetyl iodide, propionyl chloride, propionyl bromide, propionyl iodide, butyryl chloride, butyryl bromide, butyryl iodide, benzoyl chloride, benzoyl bromide, and benzoyl iodide. Among them, acid chlorides can be preferably used in terms of reactivity and handling. In addition, in the reaction of acid halides, one or more alkaline compounds may be added to act as a catalyst and neutralize the by-product acidic substances. Specific examples of alkaline compounds include, but are not limited to, tertiary amine compounds such as triethylamine and trimethylamine; and nitrogen-containing aromatic compounds such as pyridine and dimethylaminopyridine.

[0049] As the acid anhydride, any suitable acid anhydride can be used. For example, Anhydrides of saturated aliphatic monocarboxylic acids such as acetic acid, propionic acid, (iso)butyric acid, valeric acid, etc.; anhydrides of unsaturated aliphatic monocarboxylic acids such as (meth)acrylic acid, oleic acid, etc.; Anhydrides of alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid and tetrahydrobenzoic acid; Anhydrides of aromatic monocarboxylic acids such as benzoic acid, 4-methylbenzoic acid, etc.; Examples of dibasic carboxylic acid anhydrides include anhydrides of saturated aliphatic dicarboxylic acids such as succinic acid and adipic acid; unsaturated aliphatic dicarboxylic acid anhydrides such as maleic anhydride and itaconic anhydride; alicyclic dicarboxylic acid anhydrides such as 1-cyclohexene-1,2-dicarboxylic acid anhydride, hexahydrophthalic anhydride, and methyltetrahydrophthalic anhydride; and aromatic dicarboxylic acid anhydrides such as phthalic anhydride and naphthalic anhydride. Examples of polybasic carboxylic acid anhydrides having three or more bases include polycarboxylic acids (anhydrides) such as trimellitic anhydride and pyromellitic anhydride. In addition, in the reaction of an acid anhydride, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.

[0050] The vinyl carboxylate may be represented by the following formula: R-COO-CH=CH2 {wherein R is any one of an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, and an aryl group having 6 to 24 carbon atoms.} is preferred. The vinyl carboxylate is more preferably at least one selected from the group consisting of vinyl acetate, vinyl propionate, vinyl butyrate, vinyl caproate, vinyl cyclohexanecarboxylate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl myristate, vinyl palmitate, vinyl stearate, vinyl pivalate, vinyl octylate, divinyl adipate, vinyl methacrylate, vinyl crotonate, vinyl octylate, vinyl benzoate, and vinyl cinnamate. In the esterification reaction with a vinyl carboxylate, one or more catalysts selected from the group consisting of alkali metal hydroxides, alkaline earth metal hydroxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal hydrogencarbonates, primary to tertiary amines, quaternary ammonium salts, imidazole and derivatives thereof, pyridine and derivatives thereof, and alkoxides may be added.

[0051] Examples of the alkali metal hydroxides and alkaline earth metal hydroxides include sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, barium hydroxide, etc. Examples of the alkali metal carbonates, alkaline earth metal carbonates, and alkali metal hydrogen carbonates include lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate, magnesium carbonate, calcium carbonate, barium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, cesium hydrogen carbonate, etc.

[0052] The primary, secondary and tertiary amines refer to primary, secondary and tertiary amines, and specific examples thereof include ethylenediamine, diethylamine, proline, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,3-propanediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, tris(3-dimethylaminopropyl)amine, N,N-dimethylcyclohexylamine and triethylamine.

[0053] Examples of imidazole and its derivatives include 1-methylimidazole, 3-aminopropylimidazole, and carbonyldiimidazole.

[0054] Examples of pyridine and its derivatives include N,N-dimethyl-4-aminopyridine and picoline.

[0055] Examples of the alkoxide include sodium methoxide, sodium ethoxide, and potassium t-butoxide.

[0056] The carboxylic acid may be at least one selected from the group consisting of compounds represented by the following formulas: R-COOH (In the formula, R represents an alkyl group having 1 to 16 carbon atoms, an alkenyl group having 2 to 16 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, or an aryl group having 6 to 16 carbon atoms.)

[0057] Specific examples of carboxylic acids include at least one selected from the group consisting of acetic acid, propionic acid, butyric acid, caproic acid, cyclohexane carboxylic acid, caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, pivalic acid, methacrylic acid, crotonic acid, octylic acid, benzoic acid, and cinnamic acid.

[0058] Among these carboxylic acids, at least one selected from the group consisting of acetic acid, propionic acid, and butyric acid, and particularly acetic acid, is preferred from the viewpoint of reaction efficiency. In addition, in the reaction of carboxylic acid, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.

[0059] Among these esterification reactants, at least one selected from the group consisting of acetic anhydride, propionic anhydride, butyric anhydride, vinyl acetate, vinyl propionate, vinyl butyrate, and acetic acid, and among these, acetic anhydride and vinyl acetate are preferred from the viewpoint of reaction efficiency.

[0060] When cellulose nanofibers are chemically modified (e.g., by hydrophobization such as acylation), the cellulose nanofibers tend to have good dispersibility in rubber, but the cellulose nanofibers of the present disclosure can exhibit good dispersibility in rubber even if they are unsubstituted or have a low degree of substitution.

[0061] In one embodiment, the degree of substitution of the cellulose nanofibers is 0 (i.e., unsubstituted). Alternatively, in one embodiment, from the viewpoint of obtaining chemically modified cellulose nanofibers with a high thermal decomposition onset temperature, the degree of acyl substitution (DS) of the cellulose nanofibers may be greater than 0, or 0.1 or more, or 0.2 or more, or 0.25 or more, or 0.3 or more, or 0.5 or more. In addition, since an unmodified cellulose skeleton remains in the esterified cellulose nanofibers, it is possible to obtain esterified cellulose nanofibers that combine high tensile strength and dimensional stability derived from cellulose with a high thermal decomposition onset temperature derived from chemical modification, the degree of acyl substitution (DS) of the cellulose nanofibers may be 1.2 or less, or 1.0 or less, or 0.8 or less, or 0.7 or less, or 0.6 or less, or 0.5 or less.

[0062] When the modification group of the chemically modified cellulose nanofiber is an acyl group, the degree of acyl substitution (DS) can be calculated based on the peak intensity ratio of the peak derived from the acyl group to the peak derived from the cellulose skeleton from the attenuated total reflectance (ATR) infrared absorption spectrum of the esterified cellulose nanofiber. The peak of the absorption band of C=O based on the acyl group is at 1730 cm -1 The absorption band of CO based on the cellulose backbone appears at 1030 cm -1 The DS of esterified cellulose nanofibers was calculated by plotting a correlation graph between the DS obtained from solid-state NMR measurements of esterified cellulose nanofibers (described below) and the modification ratio (IR index 1030), which is defined as the ratio of the peak intensity of the absorption band of C=O based on acyl groups to the peak intensity of the absorption band of CO in the cellulose backbone chain, and then calculating the calibration curve from the correlation graph. Degree of substitution DS = 4.13 × IR index (1030) It can be found by using

[0063] The content of cellulose nanofibers in the masterbatch components is preferably 0.5% by mass or more, or 1% by mass or more, or 3% by mass or more from the viewpoint of obtaining a good reinforcing effect of the cellulose nanofibers, and is preferably 80% by mass or less, or 60% by mass or less, or 33% by mass or less, or 30% by mass or less, or 20% by mass or less, or 10% by mass or less from the viewpoint of obtaining a rubber molded body having good rubber elasticity.

[0064] In the masterbatch components, the amount of cellulose nanofibers per 100 parts by mass of the first rubber is preferably 10 parts by mass or more, or 25 parts by mass or more, or 50 parts by mass or more, and preferably 100 parts by mass or less, or 70 parts by mass or less, or 50 parts by mass or less.

[0065] <First Rubber> The first rubber may be a natural rubber, a conjugated diene polymer, a non-conjugated diene polymer, or a hydrogenated product thereof, or may be a modified rubber. The above polymer or its hydrogenated product may be an oligomer. The first rubber may also be a thermoplastic elastomer. In one aspect, the first rubber is a rubber that is not the modified rubber coupling agent of the present embodiment. In this disclosure, the rubber that is not the modified rubber coupling agent of the present embodiment means a rubber that is different from the modified rubber coupling agent of the present embodiment in the content of modified groups and / or the number average molecular weight. In this disclosure, the molecular weight and molecular weight distribution of the rubber are values ​​obtained by measuring a chromatogram using gel permeation chromatography using three columns connected together, each of which is filled with a polystyrene gel, and calculating the results using a calibration curve using standard polystyrene. Tetrahydrofuran is used as the solvent.

[0066] [Natural rubber] The natural rubber is not particularly limited, but examples thereof include, from the viewpoint of containing a large amount of high molecular weight components and having excellent breaking strength, smoke-dried types such as RSS (Ribbed Smoked Sheet) No. 3 to 5; mechanically dried TSR (Technically Specified Rubber) such as SIR (Standard Indonesian Rubber) (made in Indonesia), STR (Standard Thai Rubber) (made in Thailand), and SMR (Standard Malaysian Rubber) (made in Malaysia); and epoxidized natural rubber.

[0067] [Conjugated diene polymer] The conjugated diene polymer may be a homopolymer, a copolymer of two or more conjugated diene monomers, or a copolymer of a conjugated diene monomer and another monomer. The copolymer may be either random or block.

[0068] Conjugated diene monomers include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 3-methyl-1,3-pentadiene, 1,3-heptadiene, and 1,3-hexadiene, which may be used alone or in combination of two or more.

[0069] In one embodiment, the conjugated diene polymer is a copolymer of the above-mentioned conjugated diene monomer and an aromatic vinyl monomer. The aromatic vinyl monomer is not particularly limited as long as it is a monomer copolymerizable with the conjugated diene monomer, and examples thereof include styrene, m- or p-methylstyrene, α-methylstyrene, ethylstyrene, p-tert-butylstyrene, vinylethylbenzene, vinylxylene, vinylnaphthalene, diphenylethylene, and divinylbenzene, which may be used alone or in combination of two or more. From the viewpoints of the molding processability of the rubber composite and the impact resistance of the molded article, styrene is preferred.

[0070] Examples of random copolymers include butadiene-isoprene random copolymers, butadiene-styrene random copolymers, isoprene-styrene random copolymers, and butadiene-isoprene-styrene random copolymers. The composition distribution of each monomer in the copolymer chain includes a completely random copolymer that is close to a statistically random composition, and a tapered (gradient) random copolymer that has a gradient in composition distribution. The bond type of the conjugated diene polymer, i.e., the composition of 1,4-bonds, 1,2-bonds, etc., may be uniform or different between molecules.

[0071] The block copolymer may be a copolymer consisting of two or more blocks. For example, the block copolymer may be a block copolymer in which a block A of an aromatic vinyl monomer and a block B of a conjugated diene monomer and / or a copolymer of an aromatic vinyl monomer and a conjugated diene monomer constitute a structure such as AB, ABA, or ABAB. The boundaries of the blocks do not necessarily need to be clearly distinguished. For example, when the block B is a copolymer of an aromatic vinyl monomer and a conjugated diene monomer, the aromatic vinyl monomer in the block B may be distributed uniformly or in a tapered shape. In addition, the block B may have a plurality of parts in which the aromatic vinyl monomer is distributed uniformly and / or a plurality of parts in which the aromatic vinyl monomer is distributed in a tapered shape. Furthermore, the block B may have a plurality of segments with different aromatic vinyl monomer contents. When the copolymer has a plurality of blocks A and B, the molecular weights and compositions of the blocks A and B may be the same or different.

[0072] The block copolymer may be a mixture of two or more types differing from each other in one or more of the bond type, molecular weight, aromatic vinyl compound type, conjugated diene compound type, 1,2-vinyl content or the total amount of 1,2-vinyl content and 3,4-vinyl content, aromatic vinyl compound component content, hydrogenation rate, etc.

[0073] The amount of vinyl bonds (for example, 1,2- or 3,4-bonds of butadiene) in the conjugated diene bond units in the conjugated diene polymer is preferably 10 mol % or more and 75 mol % or less, or 13 mol % or more and 65 mol % or less. The amount of vinyl bonds in the conjugated diene bond units (for example, the amount of 1,2-bonds in butadiene) is 13 It can be determined by C-NMR (quantitative mode). 13 By integrating the peak areas appearing in the following C-NMR, a value proportional to the carbon amount of each structural unit can be obtained, which can then be converted into mass % of each structural unit. Styrene 145~147ppm Vinyl 110~116ppm Diene(cis) 24~28ppm Diene (trans) 29~33ppm

[0074] In the copolymer of a conjugated diene monomer and an aromatic vinyl monomer, the amount of the aromatic vinyl monomer bonded to the conjugated diene monomer (also referred to as the aromatic vinyl bond amount in the present disclosure) may be preferably 5.0% by mass or more and 70% by mass or less, or 10% by mass or more and 50% by mass or less, based on the total mass of the conjugated diene polymer. The aromatic vinyl bond amount can be determined by the ultraviolet absorbance of the phenyl group, and the conjugated diene bond amount can also be determined based on this.

[0075] The hydrogenated product of the conjugated diene polymer may be the hydrogenated products of the conjugated diene polymers exemplified above, for example, a hydrogenated product of a butadiene homopolymer, an isoprene homopolymer, a styrene-butadiene copolymer, or an acrylonitrile-butadiene copolymer.

[0076] [Non-conjugated diene polymer] The non-conjugated diene polymer may be a homopolymer, a copolymer of two or more non-conjugated diene monomers, or a copolymer of a non-conjugated diene monomer and another monomer. The copolymer may be either random or block. Examples of the non-conjugated diene polymer include: Olefin polymers such as ethylene-propylene rubber, ethylene-propylene-diene rubber, ethylene-butene-diene rubber, and ethylene-α-olefin copolymers; Examples of the rubber include butyl rubber, brominated butyl rubber, acrylic rubber, fluororubber, silicone rubber, chlorinated polyethylene rubber, epichlorohydrin rubber, α,β-unsaturated nitrile-acrylate-conjugated diene copolymer rubber, urethane rubber, and polysulfide rubber.

[0077] In ethylene-α-olefin copolymers, monomers that can be copolymerized with ethylene units include: aliphatic substituted vinyl monomers such as propylene, butene-1, pentene-1, 4-methylpentene-1, hexene-1, heptene-1, octene-1, nonene-1, decene-1, undecene-1, dodecene-1, tridecene-1, tetradecene-1, pentadecene-1, hexadecene-1, heptadecene-1, octadecene-1, nonadecene-1, eicosene-1, and isobutylene; styrene, substituted vinyl monomers, and the like. aromatic vinyl monomers such as substituted styrene; ester vinyl monomers such as vinyl acetate, acrylic esters, methacrylic esters, glycidyl acrylic esters, glycidyl methacrylic esters, and hydroxyethyl methacrylic esters; nitrogen-containing vinyl monomers such as acrylamide, allylamine, vinyl-p-aminobenzene, and acrylonitrile; and dienes such as butadiene, cyclopentadiene, 1,4-hexadiene, and isoprene.

[0078] Preferably, it is a copolymer of ethylene and one or more α-olefins having 3 to 20 carbon atoms, more preferably a copolymer of ethylene and one or more α-olefins having 3 to 16 carbon atoms, and most preferably a copolymer of ethylene and one or more α-olefins having 3 to 12 carbon atoms. From the viewpoint of impact resistance, the number average molecular weight of the ethylene-α-olefin copolymer is preferably 10,000 or more, more preferably 10,000 to 100,000, more preferably 10,000 to 80,000, and even more preferably 20,000 to 60,000. In one embodiment, the number average molecular weight is less than 29,000. From the viewpoint of achieving both fluidity and impact resistance, the molecular weight distribution (weight average molecular weight / number average molecular weight: Mw / Mn) is preferably 3 or less, and more preferably 1.8 to 2.7.

[0079] Moreover, the preferred content of ethylene units in the ethylene-α-olefin copolymer is 30 to 95% by mass based on the total amount of the ethylene-α-olefin copolymer, from the viewpoint of ease of handling during processing.

[0080] These preferred ethylene-α-olefin copolymers can be produced, for example, by the production methods described in JP-B-4-12283, JP-A-60-35006, JP-A-60-35007, JP-A-60-35008, JP-A-5-155930, JP-A-3-163088, and U.S. Pat. No. 5,272,236.

[0081] The conjugated diene polymer may be partially or completely hydrogenated. The hydrogenation rate of the hydrogenated product is preferably 50% or more, 80% or more, or 98% or more from the viewpoint of suppressing thermal degradation during processing, and is preferably 50% or less, 20% or less, or 0% (i.e., non-hydrogenated product) from the viewpoint of low temperature toughness.

[0082] In the conjugated diene polymer, the amount of vinyl bonds (e.g., 1,2- or 3,4-bonds of butadiene) in the conjugated diene bond units is, from the viewpoint of suppressing crystallization of the soft segment, preferably 5 mol % or more, or 10 mol % or more, or 13 mol % or more, or 15 mol % or more, and preferably 80 mol % or less, or 75 mol % or less, or 65 mol % or less, or 50 mol % or less, or 40 mol % or less.

[0083] [Modified rubber] The first rubber may be a modified rubber, and for example, in the conjugated diene polymer or non-conjugated diene polymer exemplified above, a modified group such as an epoxy group, an acid anhydride group, a carboxy group, an aldehyde group, a hydroxyl group, an alkoxy group, an amino group, an amide group, an imide group, a nitro group, an isocyanate group, or a mercapto group may be introduced. Examples of modified rubbers include epoxy modified natural rubber, epoxy modified butadiene rubber, epoxy modified styrene butadiene rubber, carboxy modified natural rubber, carboxy modified butadiene rubber, carboxy modified styrene butadiene rubber, acid anhydride modified natural rubber, acid anhydride modified butadiene rubber, and acid anhydride modified styrene butadiene rubber.

[0084] The amount of the modifying group relative to 100 mol% of all monomer units is preferably 0.1 mol% or more, or 0.2 mol% or more, or 0.3 mol% or more, and preferably 5 mol% or less, or 3 mol% or less, from the viewpoint of affinity between the cellulose nanofiber and the first rubber. The amount of the modifying group can be confirmed by infrared absorption spectroscopy, solid-state NMR (nuclear magnetic resonance), solution NMR, or a method of calculating the molar ratio of the modifying group by combining a previously specified monomer composition with the quantification by elemental analysis of elements not contained in the unmodified rubber.

[0085] In one embodiment, the modified group content of the first rubber is less than 1.5% by mass or more than 20% by mass. The method for measuring the modified group content will be described later in the section on <Modified rubber-based coupling agent>.

[0086] [Thermoplastic elastomer] In one embodiment, the first rubber may include or be a thermoplastic elastomer. In the present disclosure, an elastomer is, in one embodiment, a substance (specifically, a natural or synthetic polymer substance) that is elastic at room temperature (23°C). In addition, being elastic in one embodiment means that the storage modulus at 23°C and 10 Hz measured by dynamic viscoelasticity measurement is 1 MPa or more and 100 MPa or less. The thermoplastic elastomer may be a conjugated diene polymer or a non-conjugated diene polymer, and in one embodiment, is a crosslinked product. The suitable monomer composition of the thermoplastic elastomer may be the same as that described above in the above sections (conjugated diene polymer) and (non-conjugated diene polymer).

[0087] The number average molecular weight (Mn) of the thermoplastic elastomer is preferably from 10,000 to 500,000, or from 40,000 to 250,000, from the viewpoint of achieving both impact strength and fluidity.

[0088] The thermoplastic elastomer may have a core-shell structure. Examples of elastomers having a core-shell structure include core-shell type elastomers having a core that is a particulate rubber and a shell that is a glassy graft layer formed on the outside of the core. The core is preferably a butadiene rubber, an acrylic rubber, a silicone-acrylic composite rubber, or the like. The shell is preferably a glassy polymer such as a styrene resin, an acrylonitrile-styrene copolymer, or an acrylic resin.

[0089] From the viewpoint of excellent compatibility with modified rubber coupling agents and the like, the thermoplastic elastomer is preferably at least one selected from the group consisting of styrene-butadiene block copolymers, styrene-ethylene-butadiene block copolymers, styrene-ethylene-butylene block copolymers, styrene-butadiene-butylene block copolymers, styrene-isoprene block copolymers, styrene-ethylene-propylene block copolymers, styrene-isobutylene block copolymers, hydrogenated styrene-butadiene block copolymers, hydrogenated styrene-ethylene-butadiene block copolymers, hydrogenated styrene-butadiene-butylene block copolymers, hydrogenated styrene-isoprene block copolymers, and homopolymers of styrene (polystyrene), and more preferably at least one selected from the group consisting of styrene-butadiene block copolymers, hydrogenated styrene-butadiene block copolymers, and polystyrene.

[0090] In one embodiment, at least a part of the thermoplastic elastomer may have an acidic functional group. In the present disclosure, when the thermoplastic elastomer has an acidic functional group, it means that the acidic functional group is added to the molecular skeleton of the elastomer via a chemical bond. In the present disclosure, the acidic functional group means a functional group capable of reacting with a basic functional group, etc., and specific examples thereof include a hydroxyl group, a carboxyl group, a carboxylate group, a sulfo group, and an acid anhydride group.

[0091] From the viewpoint of affinity with modified rubber coupling agents, etc., the amount of acidic functional groups added in the elastomer is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.2% by mass or more, and preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 2% by mass or less, and even more preferably less than 1.5% by mass, based on 100% by mass of the elastomer. The number of acidic functional groups is a value obtained by measuring a calibration curve sample in which an acidic substance is mixed in advance with an infrared absorption spectrometer, and measuring the sample based on a calibration curve that has been prepared using the characteristic absorption band of the acid.

[0092] Examples of elastomers having an acidic functional group include elastomers having a core-shell structure having a shell layer formed using acrylic acid or the like as a copolymerization component, and elastomers which are modified products obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof to an ethylene-α-olefin copolymer, polyolefin, aromatic compound-conjugated diene copolymer, or a hydrogenated aromatic compound-conjugated diene copolymer containing acrylic acid or the like as a monomer, in the presence or absence of a peroxide.

[0093] In a preferred embodiment, the elastomer is an anhydride modified elastomer.

[0094] Among these, modified products obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof onto a polyolefin, an aromatic compound-conjugated diene copolymer, or a hydrogenated aromatic compound-conjugated diene copolymer in the presence or absence of a peroxide are more preferred, and among these, modified products obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof onto an ethylene-α-olefin copolymer, or a hydrogenated aromatic compound-conjugated diene block copolymer in the presence or absence of a peroxide are particularly preferred.

[0095] Specific examples of the α,β-unsaturated dicarboxylic acid and its derivatives include maleic acid, fumaric acid, maleic anhydride, and fumaric anhydride, with maleic anhydride being particularly preferred.

[0096] In one embodiment, the elastomer may be a mixture of an elastomer having an acidic functional group and an elastomer not having an acidic functional group. When the total of the elastomer having an acidic functional group and the elastomer not having an acidic functional group is 100% by mass, the mixing ratio of the elastomer having an acidic functional group is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and most preferably 40% by mass or more, from the viewpoint of maintaining high toughness and physical property stability of the rubber composite. There is no particular upper limit, and substantially all of the elastomer may be an elastomer having an acidic functional group, but from the viewpoint of not causing problems in flowability, it is desirable to have 80% by mass or less.

[0097] The content of the thermoplastic elastomer in the masterbatch components is preferably 20% by mass or more, or 30% by mass or more, and preferably 90% by mass or less, or 85% by mass or less, or 80% by mass or less.

[0098] From the viewpoint of compatibility with the modified rubber coupling agent, the first rubber is preferably at least one type selected from the group consisting of styrene-butadiene rubber, natural rubber, and isoprene rubber.

[0099] The number average molecular weight (Mn) of the first rubber is preferably more than 100,000, or 150,000 or more, or 200,000 or more from the viewpoint of obtaining a cured rubber product with excellent storage modulus, etc., and is preferably 800,000 or less, or 750,000 or less, or 700,000 or less, or 600,000 or less from the viewpoint of ease of dispersion of cellulose nanofibers in the first rubber and the first rubber not becoming too hard after curing and having good rubber elasticity.

[0100] In the masterbatch components, the content of the first rubber is preferably 20% by mass or more, or 30% by mass or more, or 40% by mass or more, and preferably 90% by mass or less, or 85% by mass or less, or 80% by mass or less.

[0101] <Modified rubber coupling agent> The modified rubber coupling agent has a modifying group and a rubber molecular chain. In one embodiment, the modifying group can bond or interact with the cellulose nanofiber, and the rubber molecular chain can bond or interact with the rubber. The rubber molecular chain may bond to the rubber directly or via another component (a vulcanizing agent in one embodiment). The cellulose nanofiber and the rubber are held together via the modified rubber coupling agent, so that the master batch, the rubber composition, or the cured rubber can exhibit good mechanical properties. In particular, the modified rubber coupling agent is rubber-based, so that it can exhibit good coupling effect even if the first and / or second rubber is unmodified. In one embodiment, the modifying group of the modified rubber coupling agent is an acid anhydride group, or a carboxylic acid anhydride group, or one or more selected from the group consisting of a maleic anhydride group and a succinic anhydride group, or a maleic anhydride group.

[0102] The modified rubber coupling agent may be a modified product of a conjugated diene polymer or a non-conjugated diene polymer, or a hydrogenated product thereof. The above polymer or the hydrogenated product thereof may be an oligomer. Examples of the rubber molecular chain in the modified rubber coupling agent include those having the same constituent monomers as those described above for the first rubber, farnesene polymers, and copolymers of farnesene polymers and conjugated diene polymers.

[0103] From the viewpoint of miscibility with the first rubber, the modified rubber coupling agent is preferably a modified isoprene rubber or a maleic anhydride modified isoprene rubber.

[0104] The present inventors have found that increasing the content of the modified group in the modified rubber coupling agent improves the mechanical properties, particularly the tensile properties, of the cured rubber, and in particular suppresses the slowdown in stress increase associated with an increase in the elongation percentage when the cured rubber is tensile. Such behavior when tensile can be evaluated, for example, by using a high ratio of the 300% modulus to the 100% modulus (M300 / M100) as an indicator. In one aspect, the cured rubber of this embodiment tends to have a high M300 / M100 due to the contribution of the modified rubber coupling agent, and therefore has excellent shape stability when tensile. Such excellent shape stability is advantageous in that it can reduce deterioration behavior such as the generation of voids at the origin of cellulose nanofibers when an external force is applied to the cured rubber.

[0105] In one embodiment, the modified group of the modified rubber coupling agent may form a covalent bond with the cellulose nanofiber and / or rubber during the production of the masterbatch, rubber composition, or cured rubber, particularly during heating and mixing. In one embodiment, a covalent bond between the modified rubber coupling agent and the cellulose nanofiber may be formed during the production of the masterbatch, and a covalent bond between the modified rubber coupling agent and the first and / or second rubber may be formed directly or via another component (vulcanizing agent in one embodiment) during the production of the cured rubber (i.e., during curing). In one embodiment, it can be confirmed by the following method that the masterbatch, rubber composition, or cured rubber is produced using the modified rubber coupling agent. In one embodiment, the residue obtained by removing the uncured rubber with a solvent is analyzed by nuclear magnetic resonance (NMR) or infrared absorption spectroscopy in the masterbatch or rubber composition. In one embodiment, the cured rubber is analyzed by an electron microscope or atomic force microscope (AFM). The presence of the site derived from the modified rubber coupling agent is confirmed as a phase present in the vicinity of the cellulose nanofibers (in the cured rubber, as a phase present in the vicinity of the cellulose nanofibers and different from the cured products of the first and second rubbers) by analysis using NMR, infrared absorption spectrum, or Nano-IR in one embodiment. Note that, when the modified rubber coupling agent remains in the master batch, rubber composition, or cured rubber, the modified rubber coupling agent itself can be extracted with a solvent and detected by NMR in one embodiment.

[0106] The modified rubber coupling agent has a modifying group content of 1.5% by mass or more, or 3.0% by mass or more, or 4.5% by mass or more from the viewpoint of obtaining a cured rubber product having excellent mechanical properties by increasing the number of sites contributing to bonding or interaction with the cellulose nanofibers, and from the viewpoint of improving the handleability during the production of the masterbatch or rubber composition and the dispersibility of the cellulose nanofibers by preventing the masterbatch component or rubber composition component from becoming excessively viscous, the modified group content is 20% by mass or less, or 15% by mass or less, or 10% by mass or less in one embodiment. The modified group content can be confirmed by NMR in one embodiment.

[0107] In one embodiment, the modified rubber coupling agent is a liquid rubber. In the present disclosure, the liquid rubber means a rubber having fluidity at 23°C. In one embodiment, the liquid rubber is a substance that forms a rubber elastomer by crosslinking (more specifically, vulcanization) and / or chain extension. That is, in one embodiment, the liquid rubber is an uncured product. In addition, the fluidity means that, in one embodiment, the liquid rubber dissolved in cyclohexane is placed in a vial having a body diameter of 21 mm and a total length of 50 mm at 23°C, and then dried, the liquid rubber is filled in the vial to a height of 1 mm, sealed, and the vial is left standing for 24 hours in an upside-down state, and a movement of the substance of 0.1 mm or more in the vertical direction can be confirmed. The liquid rubber may have a monomer composition of a general rubber. In one embodiment, the liquid rubber has a number average molecular weight (Mn) of 100,000 or less, thereby exhibiting a liquid form.

[0108] When the number average molecular weight of the modified rubber coupling agent is increased, the modified rubber coupling agent and the molecular chain of the cellulose nanofiber or rubber tend to be easily entangled, and the loss tangent of the cured rubber tends to be lowered. The number average molecular weight (Mn) of the modified rubber coupling agent is 10,000 or more, or 15,000 or more, or 20,000 or more, or 25,000 or more, or 29,000 or more, or 31,000 or more, or 52,000 or more in one aspect from the viewpoint of lowering the loss tangent of the cured rubber and obtaining good performance according to the desired application (for example, good fuel efficiency performance in tire applications, etc.), and in one aspect, is 100,000 or less, or 80,000 or less, or 600,000 or less in one aspect from the viewpoint of improving the handleability and dispersibility of the cellulose nanofiber during the production of the master batch or rubber composition by preventing the master batch component or rubber composition component from becoming excessively viscous.

[0109] From the viewpoint of improving the mechanical properties of the cured rubber, the modified rubber coupling agent may be bonded to the rubber (specifically, the first and / or second rubber) via the vulcanizing agent during curing of the rubber composition.

[0110] It is advantageous for uniformly dispersing cellulose nanofibers in rubber that the viscosity of the modified rubber coupling agent at 80° C. is a predetermined value or less. From the viewpoint of favorably dispersing cellulose nanofibers in rubber, the viscosity of the modified rubber coupling agent at 80° C. is preferably 1,000,000 mPa·s or less, or 500,000 mPa·s or less, or 250,000 mPa·s or less, or 100,000 mPa·s or less, and from the viewpoint of obtaining a rubber composition having excellent physical properties (particularly storage modulus), the viscosity is preferably 50 mPa·s or more, or 100 mPa·s or more, or 300 mPa·s or more.

[0111] The viscosity of the modified rubber coupling agent at 38°C is preferably 1,000,000 mPa·s or less, or 500,000 mPa·s or less, or 200,000 mPa·s or less from the viewpoint of dispersing the cellulose nanofibers well in the rubber, and is preferably 100 mPa·s or more, or 300 mPa·s or more, or 500 mPa·s or more from the viewpoint of obtaining a rubber composition having excellent physical properties (particularly storage modulus).

[0112] It is advantageous when dispersing cellulose nanofibers in rubber that the viscosity of the modified rubber coupling agent at 0° C. is a predetermined value or less. From the viewpoint of favorably dispersing cellulose nanofibers in rubber, the viscosity of the modified rubber coupling agent at 0° C. is preferably 2,000,000 mPa·s or less, or 1,000,000 mPa·s or less, or 400,000 mPa·s or less, and from the viewpoint of obtaining a rubber composition having excellent physical properties (particularly storage modulus), the viscosity is preferably 200 mPa·s or more, or 600 mPa·s or more, or 1,000 mPa·s or more.

[0113] The small temperature dependency of the viscosity of the modified rubber coupling agent is preferable because it allows the cellulose nanofibers to be well dispersed in the rubber over a wide range of mixing temperatures. From this viewpoint, it is particularly preferable that the viscosity of the modified rubber coupling agent at all of 80°C, 38°C, and 0°C is within the above range. In this disclosure, the viscosity is a value measured using a Brookfield viscometer at a rotation speed of 10 rpm.

[0114] The means for producing the modified rubber-based coupling agent is not particularly limited, but for example, the method described in JP 2016-172859 A can be used.

[0115] The content of the modified rubber-based coupling agent in the master batch components is preferably 1 mass % or more, or 5 mass % or more, or 10 mass % or more from the viewpoint of obtaining the above-mentioned advantages of the modified rubber-based coupling agent, and is preferably 33 mass % or less, or 30 mass % or less, or 25 mass % or less from the viewpoint of containing an appropriate amount of other components (such as cellulose nanofibers) and obtaining the advantages of these components.

[0116] In the masterbatch components, the content of the modified rubber-based coupling agent per 100 parts by mass of the first rubber is preferably 5 parts by mass or more, or 10 parts by mass or more, or 20 parts by mass or more, from the viewpoint of obtaining the above-mentioned advantages of the modified rubber-based coupling agent well, and is preferably 100 parts by mass or less, or 80 parts by mass or less, or 60 parts by mass or less, from the viewpoint of avoiding a decrease in the physical properties of the cured rubber product due to the presence of an excessively large amount of modified rubber-based coupling agent.

[0117] In the masterbatch components, the amount of modified rubber-based coupling agent per 100 parts by mass of cellulose nanofiber is preferably 30 parts by mass or more, or 50 parts by mass or more, or 80 parts by mass or more from the viewpoint of obtaining a good coupling effect, and is preferably 500 parts by mass or less, or 300 parts by mass or less, or 200 parts by mass or less from the viewpoint of avoiding a decrease in the physical properties of the cured rubber product due to the presence of an excessively large amount of modified rubber-based coupling agent.

[0118] <Additional components of master batch> The masterbatch component may further contain additional components. Examples of the additional components include additional polymers, dispersants (e.g., liquid rubber, surfactants, etc.), organic or inorganic fillers, heat stabilizers, antioxidants, antistatic agents, colorants, etc. The content ratio of any additional component in the masterbatch component is appropriately selected within a range that does not impair the desired effects of the present invention, and may be, for example, 0.01 to 50 mass %, or 0.1 to 30 mass %.

[0119] [Liquid rubber] In one embodiment, the master batch component includes a liquid rubber. The liquid rubber may be an unmodified rubber or a modified rubber, but in one embodiment, the liquid rubber is a rubber that is not the modified rubber-based coupling agent of the present embodiment, and is typically an unmodified liquid rubber. The liquid rubber can function as a dispersant for cellulose nanofibers. Examples of monomers constituting the rubber molecular chain in the liquid rubber include those similar to those described above for the first rubber.

[0120] When the liquid rubber is a modified rubber, it may have reactive groups (e.g., one or more selected from the group consisting of hydroxyl groups, carboxyl groups, isocyanato groups, thio groups, amino groups, and halo groups) at both ends and therefore may be bifunctional. These reactive groups contribute to crosslinking and / or chain extension of the liquid rubber, thereby further improving the mechanical properties of the cured rubber.

[0121] The number average molecular weight (Mn) of the liquid rubber is preferably 1,000 or more, or 1,500 or more, or 2,000 or more from the viewpoint of obtaining a master batch having excellent storage modulus and dispersibility in rubber composition components, and is preferably 80,000 or less, or 50,000 or less, or 40,000 or less, or 30,000 or less, or less than 29,000, or less than 10,000 in terms of having high fluidity suitable for dispersing cellulose nanofibers well in rubber, and in terms of the liquid rubber not becoming too hard in the cured rubber and having good rubber elasticity.

[0122] The weight average molecular weight (Mw) of the liquid rubber is preferably 1,000 or more, or 2,000 or more, or 4,000 or more from the viewpoint of obtaining a master batch having excellent storage modulus and dispersibility in rubber composition components, and is preferably 240,000 or less, or 150,000 or less, or 30,000 or less from the viewpoint of having high fluidity suitable for dispersing cellulose nanofibers well in rubber, and of having good rubber elasticity without the liquid rubber becoming too hard in the cured rubber.

[0123] The ratio (Mw / Mn) of the number average molecular weight (Mn) to the weight average molecular weight (Mw) of the liquid rubber is preferably 1.5 or more, or 1.8 or more, or 2.0 or more, in order to achieve a high degree of compatibility between multiple properties of the cured rubber material (in one embodiment, a high degree of compatibility between the storage modulus and rubber elasticity of the cured rubber material) due to a certain degree of variation in molecular weight, and is preferably 10 or less, or 8 or less, or 5 or less, in order to achieve stably desired physical properties of the cured rubber material without excessively large variation in molecular weight.

[0124] It is advantageous for uniformly dispersing cellulose nanofibers in rubber that the viscosity of the liquid rubber at 80° C. is a predetermined value or less. From the viewpoint of favorable dispersion of cellulose nanofibers in rubber, the viscosity of the liquid rubber at 80° C. is preferably 1,000,000 mPa·s or less, or 500,000 mPa·s or less, or 250,000 mPa·s or less, or 100,000 mPa·s or less, and from the viewpoint of obtaining a rubber composition having excellent physical properties (particularly storage modulus), the viscosity is preferably 50 mPa·s or more, or 100 mPa·s or more, or 300 mPa·s or more.

[0125] The viscosity of the liquid rubber at 25°C is preferably 1,000,000 mPa·s or less, or 500,000 mPa·s or less, or 200,000 mPa·s or less, from the viewpoint of dispersing the cellulose nanofibers well in the rubber, and is preferably 100 mPa·s or more, or 300 mPa·s or more, or 500 mPa·s or more, from the viewpoint of obtaining a rubber composition having excellent physical properties (particularly storage modulus).

[0126] It is advantageous when dispersing cellulose nanofibers in rubber that the viscosity of the liquid rubber at 0° C. is a predetermined value or less. From the viewpoint of favorably dispersing cellulose nanofibers in rubber, the viscosity of the liquid rubber at 0° C. is preferably 2,000,000 mPa·s or less, or 1,000,000 mPa·s or less, or 400,000 mPa·s or less, and from the viewpoint of obtaining a rubber composition having excellent physical properties (particularly storage modulus), the viscosity is preferably 200 mPa·s or more, or 600 mPa·s or more, or 1,000 mPa·s or more.

[0127] It is preferable that the viscosity of the liquid rubber has a small temperature dependency, since this allows the cellulose nanofibers to be well dispersed in the rubber over a wide range of mixing temperatures. From this viewpoint, it is particularly preferable that the viscosity of the liquid rubber at all of 80°C, 25°C, and 0°C is within the above range.

[0128] The amount of liquid rubber in the masterbatch components, per 100 parts by mass of cellulose nanofiber, is preferably 10 parts by mass or more, or 15 parts by mass or more, or 20 parts by mass or more, and preferably 200 parts by mass or less, or 150 parts by mass or less, or 100 parts by mass or less, or 90 parts by mass or less, or 80 parts by mass or less, or 70 parts by mass or less, or 60 parts by mass or less, or 50 parts by mass or less, or 45 parts by mass or less, or 40 parts by mass or less.

[0129] [Surfactants] In one embodiment, the master batch component includes a surfactant. In one embodiment, a dried body containing cellulose nanofibers and a surfactant may be used as the master batch component. In one embodiment, the surfactant is a nonionic surfactant, a cationic surfactant, or a combination thereof. As the surfactant, a nonionic surfactant is preferable from the viewpoint of heat resistance. The nonionic surfactant and the cationic surfactant can enter the voids of the cellulose nanofiber aggregate to make the aggregate porous. For example, when the wet aggregate is impregnated with a nonionic surfactant and / or a cationic surfactant and then dried to form a dried body, shrinkage during drying can be reduced compared to a dried body obtained by drying the aggregate without using the nonionic surfactant and the cationic surfactant, so that the cellulose nanofibers are well dispersed when the dried body is mixed with other master batch components.

[0130] The nonionic surfactant is preferably a compound having a hydrophilic group selected from the group consisting of a hydroxyl group, a carboxyl group, a sulfonic acid group, and an amino group, and a hydrocarbon group.

[0131] In one embodiment, the nonionic surfactant has an aliphatic group having 6 to 30 carbon atoms as the hydrophobic portion. The cellulose nanofibers of this embodiment typically form loose aggregates, and the nonionic surfactant has good affinity with rubber due to the contribution of the carbon chain of the hydrophobic portion, and since the carbon chain of the hydrophobic portion is not too long, it can easily enter the voids of the cellulose nanofiber aggregate to make the aggregate porous. For example, when the nonionic surfactant is impregnated into the wet aggregate and then dried to form a dried body, shrinkage during drying can be reduced compared to a dried body obtained by drying the aggregate without using the nonionic surfactant, and the cellulose nanofibers are well dispersed when the dried body is mixed with other master batch components.

[0132] The aliphatic group may be linear or alicyclic, or a combination thereof. From the viewpoint of obtaining good dispersibility of the cellulose nanofiber in the rubber, the number of carbon atoms of the aliphatic group is, in one embodiment, 6 or more, or 8 or more, or 10 or more, and from the viewpoint of penetrating into the voids of the cellulose nanofiber aggregate, in one embodiment, 30 or less, or 25 or less, or 20 or less.

[0133] The nonionic surfactant preferably has one or more structures selected from the group consisting of oxyethylene, glycerol, and sorbitan (specifically, a repeating structure having one or more of these as repeating units) as the hydrophilic portion. These structures are preferred in that they exhibit high hydrophilicity and can easily produce various nonionic surfactants in combination with various hydrophobic portions. In the nonionic surfactant having the hydrophilic portion, the carbon number n of the hydrophobic portion and the number of repeating units m of the hydrophilic portion preferably satisfy the following formula: n>m, from the viewpoint of obtaining good dispersibility of the cellulose nanofibers in the rubber. The repeating number m of the hydrophilic portion is preferably 1 or more, or 2 or more, or 3 or more, or 5 or more, from the viewpoint of good penetration of the nonionic surfactant into the voids of the cellulose nanofiber aggregate, and is preferably 30 or less, or 25 or less, or 20 or less, or 18 or less, from the viewpoint of obtaining good dispersibility of the cellulose nanofibers in the rubber.

[0134] The nonionic surfactant is preferably The following general formula (1): R-(OCH2CH2) m -OH (1) [wherein R represents a monovalent aliphatic group having 6 to 30 carbon atoms, and m is a natural number smaller than the number of carbon atoms in R], and The following general formula (2): R1OCH2-(CHOH)4-CH2OR2(2) [wherein R1 and R2 each independently represent a hydrogen atom, an aliphatic group having 1 to 30 carbon atoms, -COR3 {wherein R3 represents an aliphatic group having 1 to 30 carbon atoms}, or -(CH2CH2O) y-R4 {wherein R4 represents a hydrogen atom or an aliphatic group having 1 to 30 carbon atoms, and y represents an integer of 1 to 30.}, The compound is one or more selected from the group consisting of:

[0135] In general formula (1), R corresponds to the hydrophobic portion described above, and (OCH2CH2) (i.e., oxyethylene unit) corresponds to the hydrophilic portion described above. The carbon number of R and the repeat number m of (OCH2CH2) are preferably in the same range as the carbon number n of the hydrophobic portion and the repeat number m of the hydrophilic portion described above, respectively.

[0136] In general formula (2), for each of R1, R2, R3, and R4, the number of carbon atoms in the aliphatic group having 1 to 30 carbon atoms is preferably 6 or more, or 8 or more, or 10 or more, and preferably 24 or less, or 20 or less, or 18 or less. Furthermore, y is 1 or more, preferably 2 or more, or 4 or more, and preferably 30 or less, or 25 or less, or 20 or less.

[0137] Examples of cationic surfactants include benzalkonium chloride, alkyltrimethylammonium chloride, stearyldimethylammonium chloride, stearyltrimethylammonium chloride, lanolin fatty acid aminopropylethyldimethylammonium ethyl sulfate, stearyldimethylbenzylammonium chloride, stearylamine acetate, and coconutamine acetate.

[0138] The amount of surfactant in the masterbatch components, relative to 100 parts by mass of cellulose nanofiber, is preferably 10 parts by mass or more, or 15 parts by mass or more, or 20 parts by mass or more, and preferably 200 parts by mass or less, or 150 parts by mass or less, or 100 parts by mass or less, or 90 parts by mass or less, or 80 parts by mass or less, or 70 parts by mass or less, or 60 parts by mass or less, or 50 parts by mass or less, or 45 parts by mass or less, or 40 parts by mass or less.

[0139] <Masterbatch manufacturing> The master batch can be produced by a method including a step of kneading master batch components including cellulose nanofibers, a first rubber, and a modified rubber-based coupling agent to produce a master batch. The kneading conditions are not particularly limited, but for example, a kneader used in general rubber kneading such as a Banbury mixer or an open roll can be used. Conditions favorable for forming bonds between the cellulose nanofibers and the modified rubber-based coupling agent include a kneading temperature of 80°C or higher.

[0140] The cellulose nanofibers contained in the master batch components may be in the form of a cellulose composition mixed with a dispersant (in one embodiment, liquid rubber and / or surfactant) and optionally other components. The mixing in this case may be performed by stirring means such as a rotation-revolution mixer, a planetary mixer, a homogenizer, a propeller type stirrer, a rotary stirrer, an electromagnetic stirrer, an open roll, a Banbury mixer, a single screw extruder, or a twin screw extruder. In addition, the mixture may be stirred under heating in order to efficiently perform shearing. A mixing method using a homogenizer is preferred because it can promote dispersion by applying high shearing force and pressure. The order of addition of the components during mixing is not limited, but for example, (1) A method of simultaneously adding and mixing cellulose nanofibers, a dispersant, and optionally other components to obtain a cellulose composition; (2) A method in which components other than the dispersant are mixed in advance to obtain a premixture, and then the premixture and the dispersant are mixed to obtain a cellulose composition; etc. As the above method (2), for example, The cellulose nanofibers are mixed with a surfactant to allow the surfactant to penetrate into the voids in the cellulose nanofiber aggregates, Next, liquid rubber is added and mixed to allow the liquid rubber to penetrate into the voids. In this case, after obtaining the premixture, the premixture may be dried before mixing with the liquid rubber. The cellulose composition may be a dry product, or in one embodiment, a powder. The drying conditions may be appropriately designed as desired.

[0141] [Powder manufacturing] An example of a method for producing a powder includes a slurry preparation step of preparing a slurry containing cellulose nanofibers and a liquid medium, and a drying step of drying the slurry to form a powder.

[0142] (Slurry preparation process) In this step, a slurry is prepared. As the liquid medium, a water-miscible organic solvent, for example: alcohols having a boiling point of 50°C to 170°C (e.g., methanol, ethanol, n-propanol, i-propanol, n-butanol, i-butanol, s-butanol, t-butanol, etc.); ethers (e.g., propylene glycol monomethyl ether, 1,2-dimethoxyethane, diisopropyl ether, tetrahydrofuran, 1,4-dioxane, etc.); carboxylic acids (e.g., formic acid, acetic acid, lactic acid, etc.); esters (e.g., ethyl acetate, vinyl acetate, etc.); ketones (e.g., acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, etc.); nitrogen-containing solvents (dimethylformamide, dimethylacetamide, acetonitrile, etc.), etc., can be used. In a typical embodiment, the liquid medium in the slurry is substantially only water. The slurry may be composed of cellulose nanofibers and a liquid medium, or may contain a dispersant and any additional components.

[0143] The concentration of cellulose nanofibers in the slurry is preferably 5% by mass or more, or 10% by mass or more, or 15% by mass or more, or 20% by mass or more, or 25% by mass or more from the viewpoint of process efficiency in the subsequent drying step, and is preferably 60% by mass or less, or 55% by mass or less, or 50% by mass or less, or 45% by mass or less from the viewpoint of maintaining good handleability by avoiding an excessive increase in the viscosity of the slurry and solidification due to aggregation. For example, cellulose nanofibers are often produced in a dilute dispersion, and the cellulose nanofiber concentration in the slurry may be adjusted to the above-mentioned preferred range by concentrating such a dilute dispersion. For concentration, methods such as suction filtration, pressure filtration, centrifugal deliquation, and heating can be used.

[0144] (drying process) In this step, the slurry is dried under controlled drying conditions to form a powder. Components other than cellulose nanofibers may be added before, during, and / or after drying of the slurry. Drying can be performed using drying devices such as a spray dryer or an extruder. The drying device may be a commercially available product, and examples of the drying device include a micromist spray dryer (manufactured by Fujisaki Electric), a spray dryer (manufactured by Okawara Kakoki), and a twin-screw extruder (manufactured by Japan Steel Works). Among the drying conditions, appropriately controlling the drying speed, drying temperature, and / or pressure (degree of reduced pressure), especially the drying speed, can be advantageous in achieving the desired shape of the powder.

[0145] The drying speed, which is the amount (parts by mass) of liquid medium desorbed per minute per 100 parts by mass of slurry, may be, for example, 10% / min or more, or 50% / min or more, or 100% / min or more, from the viewpoint of forming a powder of the desired particle size by rapidly drying the slurry, and may be, for example, 10,000% / min or less, or 1,000% / min or less, or 500% / min or less, from the viewpoint of suppressing aggregation of the cellulose nanofibers and obtaining good handleability by avoiding excessive pulverization of the cellulose nanofibers. The drying speed is calculated by the following formula: Drying rate (% / min) = (slurry moisture content at start of drying (mass%) - powder moisture content at end of drying (mass%)) / time required from start of drying to end of drying (min) (i.e., the average value throughout the drying process). Here, the start of drying refers to the time when the process of supplying the slurry or cake to be dried to the device and drying at the intended drying temperature, degree of vacuum, and shear rate begins, and the time for premixing under conditions where the drying temperature, degree of vacuum, and shear rate are different from those in the drying process is not included in the drying time. The end point of drying refers to the point at which the moisture content first becomes 7% by mass or less when sampling is performed at intervals of at most 10 minutes from the start of drying. In the case of a continuous drying device, the time required from the start of drying to the end of drying can be interpreted as the residence time. In the case of a spray dryer, the residence time can be calculated from the heating air volume and the volume of the drying chamber. In addition, when an extruder is used as a drying device, the residence time can be calculated from the screw rotation speed and the total pitch number of the screw.

[0146] The drying temperature may be, for example, 20°C or more, or 30°C or more, or 40°C or more, or 50°C or more from the viewpoints of drying efficiency and of appropriately agglomerating the cellulose nanofibers to form a powder of the desired particle size, and may be, for example, 200°C or less, or 150°C or less, or 140°C or less, or 130°C or less, or 100°C or less from the viewpoints of preventing thermal degradation of the cellulose nanofibers and additional components and avoiding excessive pulverization of the cellulose nanofibers. The drying temperature is the temperature of the heat source in contact with the slurry, and is defined, for example, as the surface temperature of the temperature-regulating jacket of the drying device, the surface temperature of the heating cylinder, or the temperature of the hot air.

[0147] The degree of reduced pressure may be -1 kPa or less, or -10 kPa or less, or -20 kPa or less, or -30 kPa or less, or -40 kPa or less, or -50 kPa or less from the viewpoints of drying efficiency and moderately agglomerating the cellulose nanofibers to form a powder of the desired particle size, and may be -100 kPa or more, or -95 kPa or more, or -90 kPa or more from the viewpoint of avoiding excessive pulverization of the cellulose nanofibers.

[0148] In the drying step, the residence time of the slurry at a temperature of 20° C. to 200° C. may be set to preferably 0.01 to 10 minutes, or 0.05 to 5 minutes, or 0.1 to 2 minutes. Drying under such conditions rapidly dries the cellulose nanofibers, and a powder of the desired particle size is successfully produced.

[0149] For example, when a spray dryer is used, the slurry is sprayed and introduced into a drying chamber in which hot gas is circulated using a spray mechanism (rotating disk, pressure nozzle, etc.) and dried. The size of the slurry droplets when sprayed may be, for example, 0.01 μm to 500 μm, or 0.1 μm to 100 μm, or 0.5 μm to 10 μm. The hot gas may be an inert gas such as nitrogen or argon, or air, etc. The hot gas temperature may be, for example, 50° C. to 300° C., or 80° C. to 250° C., or 100° C. to 200° C. The contact between the slurry droplets and the hot gas in the drying chamber may be a parallel flow, a counter flow, or a parallel counter flow. The particulate powder generated by drying the droplets is collected by a cyclone, a drum, or the like.

[0150] Also, for example, when an extruder is used, the slurry is fed from a hopper into a kneading section equipped with a screw, and the slurry is continuously transported by the screw in the kneading section under reduced pressure and / or heating to dry the slurry. As for the screw mode, a conveying screw, a counterclockwise screw, and a kneading disk may be combined in any order. The drying temperature may be, for example, 50°C to 300°C, or 80°C to 250°C, or 100°C to 200°C.

[0151] <Rubber composition> One aspect of the present disclosure provides a rubber composition comprising a cellulose nanofiber and a rubber. In one aspect, the rubber composition is a mixture of rubber composition components comprising the cellulose nanofiber of the present embodiment, the modified rubber coupling agent of the present embodiment, and the second rubber of the present embodiment.

[0152] <Second Rubber> The second rubber may be one or more selected from the group consisting of uncured rubber and thermoplastic elastomer. In one embodiment, the rubber composition is a mixture of rubber composition components including the master batch of this embodiment and the second rubber. In one embodiment, the second rubber is a rubber that is not the modified rubber-based coupling agent of this embodiment. Specific preferred embodiments of the second rubber may be the same as those described above for the first rubber. The first and second rubbers may be different (dissimilar) from each other in one or more of the constituent monomer component type, the constituent monomer component ratio, and the molecular weight.

[0153] In the rubber composition components, the mass ratio of the masterbatch to the second rubber (masterbatch / second rubber) may be, in one embodiment, 1 / 99 to 99 / 1, or 5 / 95 to 95 / 5, or 10 / 90 to 90 / 10, or 20 / 80 to 80 / 20, or 30 / 70 to 70 / 30, or 40 / 60 to 60 / 40.

[0154] For example, when the cellulose nanofibers are supplied as the above-mentioned powder to the production of a rubber composition, the mass ratio of the powder to the second rubber in the rubber composition components (powder / second rubber) may be, in one embodiment, 1 / 99 to 99 / 1, or 5 / 95 to 95 / 5, or 10 / 90 to 90 / 10, or 20 / 80 to 80 / 20, or 30 / 70 to 70 / 30, or 40 / 60 to 60 / 40.

[0155] <Additional Components of Rubber Composition Component> The rubber composition component may contain, as an additional component, one or more of the exemplified additional components of the master batch component. The content of the additional component in the rubber composition component is appropriately selected within a range that does not impair the desired effects of the present invention, and may be, for example, 0.01 to 50 mass %, or 0.1 to 30 mass %.

[0156] [Vulcanizing agents, vulcanization accelerators] When the rubber composition component contains uncured rubber, the rubber composition component typically contains a vulcanizing agent and may optionally contain a vulcanization accelerator. The vulcanizing agent and vulcanization accelerator may be appropriately selected from conventionally known ones according to the type of uncured rubber in the rubber composition component. As the vulcanizing agent, organic peroxides, azo compounds, oxime compounds, nitroso compounds, polyamine compounds, sulfur, sulfur compounds, etc. can be used. As the sulfur compound, sulfur monochloride, sulfur dichloride, disulfide compounds, polymeric polysulfur compounds, etc. can be used.

[0157] The amount of the vulcanizing agent in the rubber composition components is preferably 0.01 to 20 parts by mass, or 0.1 to 15 parts by mass, per 100 parts by mass of the uncured rubber in the rubber composition components.

[0158] Examples of the vulcanization accelerator include sulfenamide-based, guanidine-based, thiuram-based, aldehyde-amine-based, aldehyde-ammonia-based, thiazole-based, thiourea-based, and dithiocarbamate-based vulcanization accelerators. Zinc oxide, stearic acid, and the like may be used as a vulcanization aid. The amount of the vulcanization accelerator is preferably 0.01 to 20 parts by mass, or 0.1 to 15 parts by mass, based on 100 parts by mass of the uncured rubber in the rubber composition components.

[0159] [Rubber additives] The rubber composition component may contain various conventionally known rubber additives (stabilizers, softeners, antioxidants, etc.). As the rubber stabilizer, one or more antioxidants such as 2,6-di-tert-butyl-4-hydroxytoluene (BHT), n-octadecyl-3-(4'-hydroxy-3',5'-di-tert-butylphenyl)propionate, and 2-methyl-4,6-bis[(octylthio)methyl]phenol may be used. As the rubber softener, one or more process oils, extender oils, etc. may be used. However, the rubber composition of the present embodiment can form a flexible molded body in one embodiment, and therefore the rubber composition component may not contain a rubber softener in one embodiment.

[0160] The vulcanizing agent, vulcanization accelerator, and rubber additives are typically added during the production of the rubber composition, but may be contained in the master batch components during the production of the master batch.

[0161] The amount of cellulose nanofiber in the rubber composition component is preferably 0.5 parts by mass or more, or 1 part by mass or more, or 3 parts by mass or more, per 100 parts by mass of the total of the first rubber and the second rubber, and preferably 30 parts by mass or less, or 20 parts by mass or less, or 10 parts by mass or less.

[0162] The mass ratio of [cellulose nanofiber] / [total of first rubber and second rubber] in the rubber composition components is preferably 1 / 99 to 50 / 50, or 2 / 98 to 40 / 60, or 3 / 97 to 30 / 70.

[0163] In the rubber composition components, the total content of the first and second rubbers is preferably 50 mass% or more, or 60 mass% or more, or 70 mass% or more, and preferably 99 mass% or less, or 95 mass% or less, or 90 mass% or less.

[0164] In the rubber composition component, the content of the modified rubber-based coupling agent per 100 parts by mass of the total of the first rubber and the second rubber is preferably 1 part by mass or more, or 2 parts by mass or more, or 3 parts by mass or more, and preferably 15 parts by mass or less, or 14 parts by mass or less, or 13 parts by mass or less.

[0165] In the rubber composition component, the amount of modified rubber-based coupling agent per 100 parts by mass of cellulose nanofiber is preferably 80 parts by mass or more, or 100 parts by mass or more, from the viewpoint of obtaining a good coupling effect, and is preferably 300 parts by mass or less, or 200 parts by mass or less, or 150 parts by mass or less, from the viewpoint of avoiding a decrease in the physical properties of the cured rubber due to the presence of an excessively large amount of modified rubber-based coupling agent.

[0166] In the rubber composition components, the amount of each of the liquid rubber and the surfactant relative to a total of 100 parts by mass of the first rubber and the second rubber may be 1 part by mass to 50 parts by mass, or 2 parts by mass to 40 parts by mass, or 3 parts by mass to 30 parts by mass, respectively.

[0167] The content of the liquid rubber in the rubber composition components may be, in one embodiment, 0.1% by mass or more, or 0.5% by mass or more, or 1% by mass or more, and in one embodiment, 10% by mass or less, or 5% by mass or less, or 1% by mass or less.

[0168] The content of the surfactant in the rubber composition components may be, in one embodiment, 0.1 mass% or more, or 0.5 mass% or more, or 1 mass% or more, and in one embodiment, 10 mass% or less, or 5 mass% or less, or 1 mass% or less.

[0169] In the rubber composition, the mass ratio (masterbatch / additional component) of the masterbatch to the additional component (in one embodiment, the second rubber) is preferably 1 / 99 to 99 / 1, or 5 / 95 to 95 / 5, or 10 / 90 to 90 / 10, or 20 / 80 to 80 / 20, or 30 / 70 to 70 / 30, or 40 / 60 to 60 / 40.

[0170] <Production of Rubber Composition> A method for producing a rubber composition containing cellulose nanofibers and rubber includes the following steps: (1) A method including a step of producing the masterbatch of the present embodiment, and a step of kneading the masterbatch and a rubber composition component including a second rubber to produce a rubber composition; (2) A method including a step of producing a master batch containing cellulose nanofibers and a first rubber, and a step of kneading the master batch, a second rubber, and a rubber composition component containing a modified rubber coupling agent to produce a rubber composition; The master batch in the above method (2) may further contain the modified rubber coupling agent of this embodiment. The kneading conditions are not particularly limited, but for example, a kneader used in general rubber kneading such as a Banbury mixer or an open roll can be used. The method of incorporating the modified rubber coupling agent in the master batch components in advance can be advantageous from the viewpoint of improving the physical properties of the rubber composition and the rubber cured product due to the bond or interaction between the first rubber and the modified rubber coupling agent.

[0171] <Rubber cured product and molded product> One aspect of the present disclosure provides a cured rubber product, which is a cured product of the rubber composition of the present embodiment. In one aspect, the cured rubber product can be produced by a method including a step of obtaining a rubber composition by the method of producing a rubber composition of the present disclosure, and a step of curing the rubber composition to obtain a cured rubber product. In one aspect, the cured rubber product can be obtained by a vulcanization press conforming to JIS K6299.

[0172] In one embodiment, the masterbatch may be mixed with a second rubber and, optionally, additional components to form a rubber composition, which may then be molded into a desired shape, either alone or together with other components, to produce a desired molded article including a cured rubber product. The method of combining the ingredients and the molding method are not particularly limited and may be selected depending on the desired molded article. Molding methods include, but are not limited to, (1) A method for obtaining a molded article containing a cured rubber by curing a rubber composition containing an uncured rubber before, during and / or after molding the rubber composition alone or together with an additional component, (2) A method in which the rubber composition contains uncured rubber, the uncured rubber in the rubber composition is cured to form a cured rubber product, and then the cured rubber product is molded together with additional components to obtain a molded product; (3) A method in which the rubber in the rubber composition is a thermoplastic elastomer, and the rubber composition is melt-molded alone or together with additional components to obtain a molded article. The molding may be carried out by injection molding, extrusion molding, extrusion profile molding, blow molding, compression molding, or the like.

[0173] In the above method (2), the mass ratio of the cured rubber / additional component in the molded product may be, for example, 1 / 99 to 99 / 1, or 5 / 95 to 95 / 5, or 10 / 90 to 90 / 10, or 20 / 80 to 80 / 20, or 30 / 70 to 70 / 30, or 40 / 60 to 60 / 40.

[0174] The tensile stress (modulus) at 100% elongation (M100) of the cured rubber may be, in one embodiment, 2.0 MPa or more, or 3.0 MPa or more, or 4.0 MPa or more, and in one embodiment, 10.0 MPa or less, or 9.0 MPa or less, or 8.0 MPa or less.

[0175] The tensile stress at 300% elongation (M300) of the cured rubber may be, in one embodiment, 3.0 MPa or more, or 5.0 MPa or more, or 6.0 MPa or more, and in one embodiment, 20.0 MPa or less, or 15.0 MPa or less, or 13.0 MPa or less.

[0176] The ratio (M300 / M100) of the tensile stress at 300% elongation (M300) to the tensile stress at 100% elongation (M100) of the cured rubber may be, in one embodiment, 1.3 or more, or 1.4 or more, or 1.5 or more, and in one embodiment, 2.0 or less, or 1.8 or less.

[0177] The storage modulus of the rubber cured product may be, in one embodiment, 2.0 MPa or more, or 2.5 MPa or more, and in one embodiment, 4.0 MPa or less, or 3.5 MPa or less, or 3.0 MPa or less.

[0178] It is advantageous for the cured rubber to have a loss tangent of a predetermined value or less in terms of, for example, fuel efficiency and low heat generation in tire applications. From this viewpoint, the loss tangent may be, in one embodiment, 0.18 or less, or 0.15 or less, or 0.10 or less. On the other hand, it is advantageous for the cured rubber to have a loss tangent of a predetermined value or more in terms of, for example, vibration-proof performance in vibration-proof rubber applications. From this viewpoint, the loss tangent may be, in one embodiment, 0.02 or more, or 0.03 or more, or 0.04 or more. The storage modulus and loss tangent are values ​​measured using a rheometer in a torsional manner at 50° C. and 10 Hz.

[0179] The cured rubber may be formed into molded articles of various shapes. The molded articles can be used in a wide range of applications, such as industrial machine parts, general machine parts, automobile, railway, vehicle, ship, and aerospace-related parts, electronic and electrical parts, building and civil engineering materials, daily necessities, sports and leisure goods, wind power generation housing parts, containers and packaging parts, etc. Examples of applications include automobile parts (for example, exterior parts such as tires, bumpers, fenders, door panels, various moldings, emblems, engine hoods, wheel caps, roofs, spoilers, and various aero parts, and interior parts such as instrument panels, console boxes, and trims), battery parts (automotive secondary battery parts, lithium ion secondary battery parts, fuel cases for solid methanol batteries, piping for fuel cells, etc.), electronic and electrical equipment parts (for example, various computers and their peripherals, junction boxes, various connectors, various office automation equipment, televisions, videos, disc players, chassis, refrigerators, air conditioners, parts for liquid crystal projectors, etc.), and daily necessities (shoe outsoles, etc.). One aspect of the present disclosure provides a tire, anti-vibration rubber, or shoe outsole comprising the rubber vulcanized product of the present disclosure. EXAMPLES

[0180] The following examples further illustrate exemplary embodiments of the present invention, but the present invention is not limited to these examples.

[0181] Evaluation method <Rubber> [Modifying group content] The content (mass%) of the modified group in the modified rubber coupling agent was determined by solution NMR. That is, the sum of the integral values ​​of two peaks (165 ppm to 175 ppm) derived from the carbonyl carbon of the maleic anhydride group in the side chain of the polymer molecule (C1), the sum of the integral values ​​of multiple peaks (120 ppm to 140 ppm) derived from the C=C in the main chain of the rubber (C2), and the sum of the integral values ​​of two peaks (145 ppm to 150 ppm and 110 to 115 ppm) derived from other rubber isomers (C3) were used to determine the maleic anhydride group addition rate (C4) as mol % by 100×C1 / (C2+C3), and converted to mass % of maleic acid group by the following formula. Mass% of maleic anhydride groups = 100 x (99 x C4) / (68 x (100-C4) + 166 x C4) Equipment: AVANCE NEO 600 (BRUKER) Observation kernel: 13 C Observation frequency: 150.91 MHz Pulse width: 30° Pulse program: zgig30 (quantitative mode) Waiting time: 10.0 sec Measurement temperature: 25℃ Accumulation count: 10,000 times Chemical shift reference: 0 ppm (TMS) Solvent: CDCl3 Sample tube: 5 mmΦ

[0182] [Viscosity at 38℃] The viscosity of the liquid rubber was measured using a Brookfield viscometer at a rotation speed of 10 rpm.

[0183] [Number average molecular weight (Mn)] The chromatogram was measured using GPC (gel permeation chromatography), and the molecular weight (Mn) was calculated from a calibration curve using standard polystyrene. Tetrahydrofuran was used as the solvent.

[0184] <Master batch> The master batch was evaluated as follows. [Dispersibility of cellulose nanofibers] For the master batch, 10 randomly selected cross-sectional images of a cube with sides of 2 mm were observed using X-ray CT. 2 The number of CNF aggregates of the above sizes was counted, the average number of aggregates per cross section was calculated, and the CNF dispersion state was ranked according to the following criteria. A: 3 or less B: 4~6 pieces C: 7 or more The measurement conditions for the X-ray CT are as follows. Equipment: Bruker X-CT Skyscan1272 Tube voltage: 40kV, tube current: 100μA Number of pixels: 2452 x 1640, pixel resolution: 1.2 μm, number of integrations: 8 Scan: 0.2 degree interval, 180 degree scan

[0185] <Cured rubber> The cured rubber products were evaluated as follows. (1) Tensile stress (modulus) The tensile stress at 100% elongation (100% modulus, M100) and the tensile stress at 300% elongation (300% modulus, M300) were measured according to the tensile test method of JIS K-6251. (2) Storage modulus and loss tangent (tan δ) The storage modulus and loss tangent (tan δ) were evaluated at 50° C., a frequency of 10 Hz, and a strain of 3% using a viscoelasticity tester ARES-G2 manufactured by TA Instruments by torsion method. (3) Dispersibility of cellulose nanofibers For the cured rubber, 10 randomly selected cross-sectional images from a cube with sides of 2 mm were observed using X-ray CT, and the dispersibility of cellulose nanofibers was evaluated using the same procedure as described above for the masterbatch.

[0186] ≪Materials used≫ <Modified rubber coupling agents and comparative rubbers> The liquid rubbers obtained in the following Production Examples 1 to 3 and Comparative Production Examples 1 to 4 were used.

[0187] [Production Example 1] After drying the pressure-resistant reactor, it was replaced with nitrogen, and 600 g of hexane and 13.1 g of n-butyllithium (17% by mass in hexane solution) were charged and heated to 50°C. While thoroughly stirring, 600 g of isoprene was added successively at 50°C, and polymerization was carried out for 1 hour. Then, methanol was added to terminate the polymerization reaction, and a polymer solution was obtained. The polymer solution was washed with water, and after removing the water, the polymer solution was vacuum-dried at 70°C for 24 hours to obtain unmodified liquid polyisoprene. 100 parts by mass of the obtained unmodified liquid polyisoprene was placed in a nitrogen-substituted reactor, and 10 parts by mass of maleic anhydride and 0.1 parts by mass of BHT (2,6-di-t-butyl-4-methylphenol) (available from Honshu Chemical Industry Co., Ltd., the same applies below) were added, and the mixture was reacted at 160°C for 20 hours to obtain maleic anhydride-modified liquid polyisoprene.

[0188] [Production Example 2] After drying the pressure-resistant reactor, it was replaced with nitrogen, and 600 g of hexane and 6.3 g of n-butyllithium (17% by mass in hexane solution) were charged and heated to 50°C. While thoroughly stirring, 600 g of isoprene was added successively at 50°C, and polymerization was carried out for 1 hour. Then, methanol was added to terminate the polymerization reaction, and a polymer solution was obtained. The polymer solution was washed with water, and after removing the water, the polymer solution was vacuum-dried at 70°C for 24 hours to obtain unmodified liquid polyisoprene. 100 parts by mass of the obtained unmodified liquid polyisoprene was placed in a nitrogen-substituted reactor, and 5 parts by mass of maleic anhydride and 0.1 parts by mass of BHT (2,6-di-t-butyl-4-methylphenol) were added, and the mixture was reacted at 160°C for 20 hours to obtain maleic anhydride-modified liquid polyisoprene.

[0189] [Production Example 3] After drying the pressure-resistant reactor, it was replaced with nitrogen, and 600 g of hexane and 16.0 g of n-butyllithium (17% by mass in hexane solution) were charged and heated to 50°C. While thoroughly stirring, 600 g of butadiene was added successively at 50°C, and polymerization was carried out for 1 hour. Then, methanol was added to terminate the polymerization reaction, and a polymer solution was obtained. The polymer solution was washed with water, and after removing the water, the polymer solution was vacuum-dried at 70°C for 24 hours to obtain unmodified liquid polyisoprene. 100 parts by mass of the obtained unmodified liquid butadiene was placed in a nitrogen-substituted reactor, and 7 parts by mass of maleic anhydride and 0.1 parts by mass of BHT (2,6-di-t-butyl-4-methylphenol) were added, and the mixture was reacted at 160°C for 20 hours to obtain maleic anhydride-modified liquid butadiene.

[0190] [Comparative Manufacturing Example 1] Commercially available maleic anhydride modified liquid polyisoprene (Kuraray Co., Ltd., LIR-403) was obtained and dried at 70° C. for 24 hours.

[0191] [Comparative Manufacturing Example 2] After drying the pressure-resistant reactor, it was replaced with nitrogen, and 600g of cyclohexane and 212g of n-butyllithium (10.5% by mass cyclohexane solution) were charged and heated to 70°C. While thoroughly stirring, 2050g of isoprene was added successively at 70°C, and polymerization was carried out for 1 hour. Then, methanol was added to terminate the polymerization reaction, and a polymer solution was obtained. The polymer solution was washed with water, and after removing the water, the polymer solution was vacuum-dried at 70°C for 24 hours to obtain unmodified liquid polyisoprene. 100 parts by mass of the obtained unmodified liquid polyisoprene was placed in a nitrogen-substituted reactor, and 5 parts by mass of maleic anhydride and 0.1 parts by mass of BHT (2,6-di-t-butyl-4-methylphenol) were added, and the mixture was reacted at 160°C for 20 hours to obtain maleic anhydride-modified liquid polyisoprene.

[0192] [Comparative Manufacturing Example 3] Commercially available maleic anhydride modified liquid polybutadiene (Cryvalle, RICON 130MA13) was obtained and dried at 70° C. for 24 hours.

[0193] [Comparative Manufacturing Example 4] Commercially available unmodified liquid polyisoprene (Kuraray Co., Ltd., LIR-30) was obtained and dried at 70° C. for 24 hours.

[0194] The viscosity, molecular weight, and amount of modified groups of each liquid rubber were evaluated by the methods described above.

[0195] <Unmodified liquid rubber> Butadiene-styrene random copolymer (RICON 184, available from Cray Valley), viscosity at 25°C 40,000 cP, number average molecular weight (Mn) 3,200, weight average molecular weight (Mw) 14,000, Mw / Mn 4.3, vinyl content 19 mol%, aromatic styrene content 8 mol%

[0196] <Cellulose nanofiber (CNF): Microfibrous cellulose> 3 parts by mass of cotton linter pulp was immersed in 27 parts by mass of water and dispersed with a pulper. 30 parts by mass of the pulper-treated cotton linter pulp slurry (including 3 parts by mass of cotton linter pulp) was added to 170 parts by mass of water to disperse the mixture in water (solid content rate: 1.5% by mass), and the aqueous dispersion was beaten for 30 minutes using a SDR14 lab refiner (pressure type DISK type) manufactured by Aikawa Iron Works Co., Ltd. as a disc refiner device with a clearance between discs of 1 mm. Subsequently, thorough beating was performed under conditions in which the clearance was reduced to a level close to zero, to obtain a beaten aqueous dispersion (solid content concentration: 1.5% by mass). The obtained beaten aqueous dispersion was directly subjected to a high-pressure homogenizer (NSO15H manufactured by Niro Soavi Co., Ltd. (Italy)) for 10 times of refinement under an operating pressure of 100 MPa to obtain a fine cellulose fiber slurry (solid content concentration: 1.5% by mass). The mixture was then concentrated using a dehydrator to a solid content of 10% by mass to obtain a concentrated cake of CNF.

[0197] <Surfactant> Nonionic surfactant: Polyoxyethylene (2) monolauryl ether (Emulgen 102KG, available from Kao Corporation) (The number in parentheses indicates the number of repeats of the oxyethylene chain.)

[0198] <Vulcanization aid> Zinc oxide: available from Fujifilm Wako Pure Chemical Industries, Ltd. Stearic acid: available from Fujifilm Wako Pure Chemical Industries, Ltd.

[0199] <Wax> Sunnock: Selected Special Wax (available from Ouchi Shinko Chemical Co., Ltd.)

[0200] <Anti-aging agent> Nocrac 6C: N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (available from Ouchi Shinko Chemical Co., Ltd.)

[0201] <Vulcanization accelerator> Noccela CZ: N-cyclohexyl-2-benzothiazolyl sulfenamide (available from Ouchi Shinko Chemical Co., Ltd.) Noccelaer D: 1,3-diphenylguanidine (available from Ouchi Shinko Chemical Co., Ltd.)

[0202] <Production of dried CNF> Purified water was added to the concentrated cake of CNF obtained above (aqueous dispersion of cellulose fibers) to obtain an aqueous dispersion with a final cellulose nanofiber content of 5% by mass. Unmodified liquid rubber and surfactant were added to this to prepare an aqueous dispersion with a final composition of 90% by mass of water, 5% by mass of cellulose nanofiber, 2.86% by mass of liquid rubber, and 2.14% by mass of surfactant. The aqueous dispersion was mixed for 5 minutes using a planetary centrifugal mixer ARE-310 manufactured by Thinky Corporation to obtain a dispersion of a cellulose nanofiber composition. The obtained dispersion was dried at 80°C using an SPH-201 manufactured by Espec Corporation, and then pulverized for 30 seconds using a mini speed mill MS-05 manufactured by LabNect Co., Ltd. to obtain a dried CNF body.

[0203] <Masterbatch manufacturing> <Examples 1 to 5 and Comparative Examples 1 to 4> A Toyo Seiki Laboplastomill was heated to 70°C, and 100 parts by mass of natural rubber (first rubber) was kneaded for 0.5 minutes. The dried CNF and modified rubber coupling agent or comparative rubber were added according to the composition shown in Table 2, and kneaded for 5.5 minutes. The amounts of the dried CNF, modified rubber coupling agent, or comparative rubber added were as shown in Table 2. The obtained rubber master batch was collected and molded into a sheet by passing through a roll. A portion was cut out from the sheet, and the cellulose nanofiber dispersibility was evaluated by X-ray CT. The results are shown in Table 2.

[0204] <Production of rubber composition and cured rubber> <Examples 6 to 10 and Comparative Examples 5 to 8> A Labo Plastomill manufactured by Toyo Seiki Co., Ltd. was heated to 70°C, natural rubber (second rubber) was added and kneaded for 0.5 minutes, and then a master batch, a vulcanization aid (2.5 parts by mass of zinc oxide and 2 parts by mass of stearic acid), 1.5 parts by mass of wax, and 2 parts by mass of antioxidant were added according to the composition shown in Table 3 and kneaded for 5.5 minutes to perform the first stage kneading. Next, the obtained first stage kneaded composition was added to the Labo Plastomill heated to 70°C and kneaded for 0.5 minutes, and sulfur and vulcanization accelerators (Noxeler CZ and Noxeler D) were added according to the composition shown in Table 3 and kneaded for 2 minutes. The obtained second stage kneaded composition (rubber composition) was vulcanized at 160°C for 20 minutes in a vulcanization press to obtain a rubber cured product. Various evaluations were performed on the obtained rubber cured product. The results are shown in Table 3.

[0205] [Table 1]

[0206] [Table 2]

[0207] [Table 3] [Industrial Applicability]

[0208] The masterbatch and rubber composition according to the present disclosure can form a cured rubber product with good physical properties, and therefore can be suitably used in a wide range of applications, such as industrial machine parts, general machine parts, automobile, railway, vehicle, ship, and aerospace related parts, electronic and electrical parts, building and civil engineering materials, daily necessities, sports and leisure goods, housing parts for wind power generation, containers and packaging parts, etc.

Claims

1. A method for producing a masterbatch containing cellulose nanofibers and rubber, comprising the steps of: The method includes a step of kneading a masterbatch component including cellulose nanofibers, a first rubber, and a modified rubber-based coupling agent to produce a masterbatch, the modified group of the modified rubber coupling agent is a maleic anhydride modified group, The modified rubber coupling agent has a modifying group content of 1.5% by mass to 20% by mass, the modified rubber coupling agent is a liquid rubber, The modified rubber coupling agent has a number average molecular weight of 10,000 to 100,000.

2. The method according to claim 1, wherein in the master batch component, the amount of the cellulose nanofiber relative to 100 parts by mass of the first rubber is 10 parts by mass to 100 parts by mass.

3. The method according to claim 1, wherein the content of the modified rubber coupling agent in the master batch component is 5 parts by mass to 100 parts by mass based on 100 parts by mass of the first rubber.

4. The method according to claim 1, wherein in the master batch component, the amount of the modified rubber coupling agent relative to 100 parts by mass of the cellulose nanofibers is 30 parts by mass to 500 parts by mass.

5. The method of claim 1 , wherein the modified rubber coupling agent is a maleic anhydride modified isoprene rubber.

6. The method of claim 1 , wherein the masterbatch components further comprise an unmodified liquid rubber.

7. 2. The method of claim 1, wherein the first rubber is one or more selected from the group consisting of styrene butadiene rubber, natural rubber, and isoprene rubber.

8. The method according to claim 1 , wherein the cellulose nanofibers are mechanically defibrated.

9. A method for producing a rubber composition containing cellulose nanofibers and rubber, comprising the steps of: forming a masterbatch according to the method of claim 1; and A step of kneading a rubber composition component including the master batch and a second rubber to produce a rubber composition; A method comprising:

10. A method for producing a rubber composition containing cellulose nanofibers and rubber, comprising the steps of: A step of producing a masterbatch containing cellulose nanofibers and a first rubber; and A step of kneading a rubber composition component including the master batch, a second rubber, and a modified rubber-based coupling agent to produce a rubber composition; Including, the modified group of the modified rubber coupling agent is a maleic anhydride modified group, The modified rubber coupling agent has a modifying group content of 1.5% by mass to 20% by mass, the modified rubber coupling agent is a liquid rubber, The modified rubber coupling agent has a number average molecular weight of 10,000 to 100,000.

11. The method according to claim 9 or 10, wherein in the rubber composition component, the amount of the cellulose nanofiber per 100 parts by mass of the total of the first rubber and the second rubber is 0.5 parts by mass to 30 parts by mass.

12. The method according to claim 9 or 10, wherein the content of the modified rubber coupling agent in the rubber composition component is 1 part by mass to 15 parts by mass relative to a total of 100 parts by mass of the first rubber and the second rubber.

13. The method according to claim 9 or 10, wherein in the rubber composition component, the amount of the modified rubber coupling agent per 100 parts by mass of the cellulose nanofiber is 80 parts by mass to 300 parts by mass.

14. 11. The method according to claim 9 or 10, wherein the modified rubber coupling agent is a maleic anhydride modified isoprene rubber.

15. The method of claim 9 or 10, wherein the rubber composition component further comprises an unmodified liquid rubber.

16. The method according to claim 9 or 10, wherein the first rubber and / or the second rubber is at least one selected from the group consisting of styrene butadiene rubber, natural rubber and isoprene rubber.

17. The method according to claim 9 or 10, wherein the cellulose nanofibers are mechanically defibrated.

18. Producing a rubber composition according to the method of claim 9 or 10; and curing the rubber composition to produce a rubber cured product; The method for producing a cured rubber product comprising the steps of:

19. A masterbatch comprising cellulose nanofibers and rubber, The masterbatch is a mixture of masterbatch components including cellulose nanofibers, a first rubber, and a modified rubber-based coupling agent, the modified group of the modified rubber coupling agent is a maleic anhydride modified group, The modified rubber coupling agent has a modifying group content of 1.5% by mass to 20% by mass, the modified rubber coupling agent is a liquid rubber, The modified rubber coupling agent has a number average molecular weight of 10,000 to 100,000.

20. The masterbatch according to claim 19, wherein the amount of the cellulose nanofiber per 100 parts by mass of the first rubber in the masterbatch components is 10 parts by mass to 100 parts by mass.

21. The master batch according to claim 19, wherein the content of the modified rubber coupling agent in the master batch components is 5 parts by mass to 100 parts by mass relative to 100 parts by mass of the first rubber.

22. The master batch according to claim 19, wherein the amount of the modified rubber coupling agent per 100 parts by mass of the cellulose nanofiber in the master batch components is 30 parts by mass to 500 parts by mass.

23. 20. The masterbatch of claim 19, wherein the modified rubber coupling agent is a maleic anhydride modified isoprene rubber.

24. 20. The masterbatch of claim 19, wherein the masterbatch components further comprise an unmodified liquid rubber.

25. 20. The masterbatch of claim 19, wherein the first rubber is at least one selected from the group consisting of styrene butadiene rubber, natural rubber, and isoprene rubber.

26. The masterbatch according to claim 19, wherein the cellulose nanofibers are mechanically defibrated.

27. A rubber composition comprising cellulose nanofibers and rubber, the rubber composition is a kneaded mixture of rubber composition components including cellulose nanofibers, a first rubber, a second rubber, and a modified rubber-based coupling agent; the modified group of the modified rubber coupling agent is a maleic anhydride modified group, The modified rubber coupling agent has a modifying group content of 1.5% by mass to 20% by mass, the modified rubber coupling agent is a liquid rubber, The modified rubber coupling agent has a number average molecular weight of 10,000 to 100,000.

28. The rubber composition according to claim 27, wherein the amount of the cellulose nanofiber per 100 parts by mass of the total of the first rubber and the second rubber is 0.5 parts by mass to 30 parts by mass.

29. The rubber composition according to claim 27, wherein the content of the modified rubber coupling agent relative to a total of 100 parts by mass of the first rubber and the second rubber in the rubber composition component is 1 part by mass to 15 parts by mass.

30. The rubber composition according to claim 27, wherein the amount of the modified rubber coupling agent per 100 parts by mass of the cellulose nanofiber in the rubber composition component is 80 parts by mass to 300 parts by mass.

31. 28. The rubber composition of claim 27, wherein the modified rubber coupling agent is a maleic anhydride modified isoprene rubber.

32. 30. The rubber composition of claim 27, wherein said rubber composition component further comprises an unmodified liquid rubber.

33. The rubber composition according to claim 27, wherein the first rubber and / or the second rubber is at least one selected from the group consisting of styrene-butadiene rubber, natural rubber, and isoprene rubber.

34. The rubber composition according to claim 27 , wherein the cellulose nanofibers are mechanically defibrated.

35. A rubber cured product, which is a cured product of the rubber composition according to any one of claims 27 to 34.

36. A tire comprising the rubber vulcanized product of claim 35.

37. A rubber vibration isolator comprising the cured rubber product according to claim 35.

38. 36. A shoe outsole comprising the rubber vulcanized product of claim 35.

Citation Information

Patent Citations

  • Tire rubber composition and tire