Superabsorbent resin film and absorbent product comprising the same
A super absorbent resin film with specific thickness and absorption capacity is integrated into absorbent articles to address the issue of dampness, improving comfort by absorbing moisture and maintaining breathability.
Patent Information
- Application Number
- JP2024135679
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-03-18
- Filing Date
- 2024-08-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-03-21
AI Technical Summary
Existing absorbent articles suffer from a damp feeling on the outside due to moisture permeability of the liquid-impermeable backsheet, which reduces wearing comfort.
Incorporation of a super absorbent resin film with a thickness of 500 μm or less and moisture absorption capacity of 10-100 g/m², interposed between the liquid-impermeable backsheet and breathable waterproof film, or between the breathable waterproof film and the absorbent body, to absorb moisture and maintain a dry feeling.
The super absorbent resin film effectively reduces the damp feeling on the outside of the absorbent article while maintaining breathability, enhancing user comfort and usability.
Smart Images

Figure 2024167248000001_ABST
Abstract
Description
[Technical field]
[0001] Cross-reference to related applications This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0039666 filed on March 26, 2021, and Korean Patent Application No. 10-2022-0034232 filed on March 18, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to a superabsorbent polymer film having excellent moisture absorption ability, and to a water-absorbing article which contains the superabsorbent polymer film and thus has an improved feeling of dampness on the outside and is therefore excellent in feel when used. [Background technology]
[0003] Absorbent articles such as disposable diapers, sanitary napkins, and incontinence pads generally comprise a liquid-impermeable backsheet, an absorbent body, and a liquid-permeable topsheet that comes into contact with the wearer's skin. If necessary, they may further comprise a breathable waterproof film for improving breathability, a decorative sheet for improving the appearance, leg elastics for improving comfort and preventing side leakage, etc.
[0004] In such absorbent articles, the liquid-permeable top sheet is made of a material such as a synthetic polymer nonwoven fabric that allows bodily fluids to quickly pass through to the absorbent body. The absorbent body is made of a highly absorbent resin, pulp, tissue, or nonwoven fabric, and functions to rapidly absorb and retain bodily fluids that have permeated the liquid-permeable top sheet. The liquid-impermeable back sheet is used to prevent bodily fluids absorbed in the absorbent body from leaking out, and is made of a woven or nonwoven fabric made of natural or synthetic fibers.
[0005] The liquid-impermeable backsheet is designed to have a waterproof performance for that purpose, but if the waterproof performance is too high, there is a problem that water vapor and air cannot pass through, resulting in a poor wearing comfort. Therefore, liquid-impermeable backsheets generally use moisture-permeable waterproof woven or nonwoven fabrics that have pores large enough to allow water particles to pass through but small water vapor particles to pass through. However, due to the moisture permeability of the backsheet, moisture released from the absorbent body is transmitted to the outside of the backsheet, resulting in a damp feeling even on the outside of the absorbent article when worn for a long time, resulting in a poor wearing comfort. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made to solve the above problems, and aims to provide a superabsorbent polymer film that is thin and has excellent moisture absorption capacity, and an absorbent article that includes the superabsorbent polymer film and improves the damp feeling on the outside. [Means for solving the problem]
[0007] According to one embodiment of the present invention, the thickness is less than or equal to 500 μm, and the moisture absorption capacity measured according to the KS F 2611 standard is 10 to 100 g / m 2 The present invention provides a highly water-absorbent polymer film,
[0008] The highly water-absorbent resin film may have a thickness of 10 to 200 μm.
[0009] The highly water-absorbent resin film may have a moisture content of 1 to 15% and a tensile strength of 5 to 50 MPa.
[0010] According to another embodiment of the present invention, there is provided an absorbent article comprising a liquid-impermeable backsheet; a breathable waterproof film; an absorbent body comprising superabsorbent polymer powder and pulp; and a liquid-permeable topsheet, the superabsorbent polymer film being between the liquid-impermeable backsheet and the breathable waterproof film and / or between the breathable waterproof film and the absorbent body, the superabsorbent polymer film having a thickness of 500 μm or less and a moisture absorption capacity of 10 to 100 g / m as measured according to the KS F 2611 standard. 2 The present invention provides a water-absorbent article,
[0011] The highly water-absorbent resin film may have a thickness of 10 to 200 μm.
[0012] The highly water-absorbent resin film may be laminated to one side of the liquid-impermeable backsheet; and / or to one or both sides of the breathable waterproof film.
[0013] In one example, the superabsorbent resin film is laminated to one side of the breathable waterproof film, and the laminated superabsorbent resin film and breathable waterproof film have an air permeability of 3000 to 5000 g / m 2 May be 24hr.
[0014] The liquid-impermeable backsheet may be a nonwoven fabric having a pore size of 20 to 1000 μm.
[0015] The breathable waterproof film has a breathability of 2000 to 5000 g / m 2 May be 24hr.
[0016] The absorbent body may contain 10 to 90% by weight of highly water-absorbent resin powder.
[0017] The liquid-permeable top sheet has a basis weight of 15 to 30 g / m 2 may be also possible. Effect of the Invention
[0018] The superabsorbent polymer film of the present invention has excellent moisture absorption ability despite its very thin thickness, and can be suitably used for articles that require moisture absorption function. In addition, the water-absorbing article of the present invention includes the superabsorbent polymer film in addition to the absorbent body, so that the damp feeling felt from the outside is significantly reduced, and therefore, skin rashes and other irritations that occur when heated by the wearer's body can be reduced, providing excellent usability. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a cross-sectional view showing the configuration of an existing water-absorbent article. [Diagram 2] 1 is a cross-sectional view showing a configuration of a water-absorbent article according to one embodiment of the present invention. [Diagram 3] 1 is a cross-sectional view showing a configuration of a water-absorbent article according to one embodiment of the present invention. [Figure 4] 1 is a cross-sectional view showing a configuration of a water-absorbent article according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In this specification, the terms "include", "comprise", "have" and the like are intended to specify the presence of an implemented feature, step, component, or combination thereof, and should be understood not to preclude the presence or additional possibility of one or more other features, steps, components, or combinations thereof.
[0021] Since the present invention can be modified in various ways and has various forms, a specific embodiment will be exemplified and described in detail below, but it should be understood that this is not intended to limit the invention to the specific disclosed form, but rather to include all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.
[0022] Similarly, the drawings attached to this specification for explaining the present invention are one embodiment of the present invention, and the present invention can be realized in various different forms, and is not limited to this specification. At this time, in the drawings, parts unnecessary for the explanation are omitted in order to clearly explain the present invention, and similar drawing symbols are used for similar parts throughout the specification. In addition, the size and relative size of the components shown in the drawings are not related to the actual scale, and may be reduced or exaggerated for clarity of explanation.
[0023] The highly absorbent resin film of the present invention and the water-absorbent article containing the same will be described in detail below.
[0024] Highly absorbent resin film The superabsorbent resin film according to one embodiment of the present invention has a thickness of 500 μm or less and a moisture absorption capacity of 10 to 100 g / m2 as measured according to the KS F 2611 standard. 2 Satisfy.
[0025] The superabsorbent polymer film is an acrylic acid-based polymer in the form of a thin film, which is different from existing particulate superabsorbent polymers, and has a water content of 15% or less, is colorless and transparent, and has excellent elasticity and flexibility. The superabsorbent polymer film is not likely to be scattered or leaked from absorbent articles during handling, and can be used without auxiliary agents such as pulp.
[0026] In addition, the superabsorbent resin film has a thin thickness and excellent moisture absorbing ability, and can be used as a moisture absorbent in various articles without increasing the volume or damaging the shape of the article.
[0027] Specifically, the moisture absorption capacity of the highly water-absorbent resin film is 10 g / m 2 More than 13g / m 2 More than 15g / m 2 or more than 20g / m 2 More than 100g / m 2 or less than 90g / m 2The moisture absorption capacity can be measured according to the KS F 2611 standard, and a specific measurement method will be described later in the Examples.
[0028] The thicker the superabsorbent polymer film, the greater the moisture absorption capacity, but if the film is too thick (exceeding 500 μm), it may affect the shape of the article to which it is applied, and conversely, if the film is too thin, it may not be able to obtain sufficient moisture absorption effect.
[0029] In addition, if the thickness of the superabsorbent resin film exceeds 500 μm, the breathability may decrease, but in the case of a thin-film type superabsorbent resin film of 500 μm or less, the flexibility of the film increases significantly when moisture is absorbed, and the capacity between the polymer chains increases, so that the film can exhibit moisture absorption performance while maintaining breathability. Therefore, it can be used more preferably in articles that require both moisture absorption ability and breathability, such as the water-absorbing articles described below.
[0030] From this viewpoint, the thickness (h) of the superabsorbent resin film is preferably 5 μm or more, 10 μm or more, or 15 μm or more, and may be 400 μm or less, 300 μm or less, 200 μm or less, or 150 μm or less.
[0031] On the other hand, the moisture content of the superabsorbent resin film may be 15% by weight or less, or 12% by weight or less, or 11% by weight or less, or 10% by weight or less, but 1% by weight or more, or 2% by weight or more, or 4% by weight or more, or 6% by weight or more.
[0032] The "moisture content" is the amount of moisture contained in the sample relative to the weight of the sample before drying, expressed as a percentage. That is, the moisture content can be calculated by subtracting the weight of the sample after drying from the weight of the sample before drying, dividing the result by the weight of the sample before drying, and multiplying the result by 100. At this time, the drying conditions are to increase the temperature from room temperature to about 150°C and then maintain it at 150°C, and the total drying time is set to 20 minutes, including 5 minutes for the temperature increase step.
[0033] The superabsorbent resin film has a thickness of 500 μm or less, and in this thickness range, the total light transmittance for visible light is 89.5%, showing high transparency. The total light transmittance of the superabsorbent resin film according to one embodiment of the present invention may be 90% or more, 90.3% or more, 91% or more, 91.5% or more, or 92% or more. The total light transmittance may be theoretically 100%, and may be 99% or less, for example.
[0034] Furthermore, the superabsorbent resin film of the present invention may have a yellow index according to the ASTM D1925 standard of 2.6 or less, 2.5 or less, 2.4 or less, 2.3 or less, 1.9 or less, 1.5 or less, or 1.3 or less in a thickness range of 1 to 500 μm.
[0035] Meanwhile, the superabsorbent resin film may have a moisture content of 1% to 15% and a tensile strength of 5 MPa or more. Preferably, when the moisture content is 5 to 15%, the tensile strength of the superabsorbent resin film may be 10 MPa or more, 13 MPa or more, 14 MPa or more, 19 MPa or more, or 22 MPa or more, and may be 50 MPa or less, 47 MPa or less, 45 MPa or less, 40 MPa or less, or 35 MPa or less. A superabsorbent resin film satisfying the above tensile strength range is less likely to be damaged, and when applied to absorbent articles such as diapers, it is not easily damaged by the movement of the wearer and can exhibit excellent moisture absorption ability.
[0036] Meanwhile, in order to further improve the breathability of the superabsorbent resin film, a pattern including a hole structure may be formed in the superabsorbent resin film. The shape of the pattern is not particularly limited, and the shape, maximum diameter, average diameter, hole interval, arrangement, etc. of the holes may be adjusted to produce a superabsorbent resin film having appropriate breathability and moisture absorption ability.
[0037] Alternatively, when the superabsorbent resin film is produced, a foaming agent such as calcium carbonate may be used to form a porous structure, thereby further improving the breathability of the superabsorbent resin film.
[0038] The superabsorbent resin film can be produced by a production method including the steps of: preparing a monomer composition by mixing an acrylic acid-based monomer having acidic groups, at least a portion of which has been neutralized, a cellulose-based thickener, a moisturizing agent, an internal crosslinking agent, a polymerization initiator, and a solvent; casting the monomer composition on a substrate to form a monomer composition film; stretching the monomer composition film while irradiating it with heat and / or light to form a hydrous gel polymer film; and drying the hydrous gel polymer film.
[0039] According to the above-mentioned preparation method, a monomer composition film is prepared from a viscosity-controlled monomer composition solution by a solution casting method, and the monomer composition film is polymerized and dried to prepare a film-type superabsorbent resin. In particular, the tensile strength of the superabsorbent resin film can be adjusted by applying tension to the monomer composition film during the polymerization step to stretch it.
[0040] The method for producing the highly water-absorbent resin film will now be described in detail.
[0041] The monomer composition includes an acrylic acid monomer having an acidic group, at least a portion of which has been neutralized, a cellulose-based thickener, a moisturizer, a polymerization initiator, and a solvent.
[0042] First, the acrylic acid monomer is a compound represented by the following Chemical Formula 1:
[0043] [Chemical formula 1] R 1 -COOM 1
[0044] In the above chemical formula 1, R 1 is an alkyl group having 2 to 5 carbon atoms and containing an unsaturated bond, M 1 is a hydrogen atom, a monovalent or divalent metal, an ammonium group, or an organic amine salt.
[0045] Preferably, the acrylic acid-based monomer includes at least one selected from the group consisting of acrylic acid, methacrylic acid, and their monovalent metal salts, divalent metal salts, ammonium salts, and organic amine salts.
[0046] Here, the acrylic acid monomer may have an acidic group and at least a part of the acidic group may be neutralized. Preferably, the monomer may be partially neutralized with an alkaline substance such as sodium hydroxide, potassium hydroxide, or ammonium hydroxide. In this case, the neutralization degree of the acrylic acid monomer may be 40 to 95 mol%, or 40 to 80 mol%, or 45 to 75 mol%. The range of the neutralization degree may be adjusted according to the final physical properties. If the neutralization degree is too high, the neutralized monomer may precipitate, making it difficult to smoothly carry out polymerization, and conversely, if the neutralization degree is too low, the absorbency of the polymer may be significantly reduced.
[0047] In a preferred embodiment, the alkaline substance may be sodium hydroxide (NaOH), potassium hydroxide (KOH), or a combination thereof. In particular, when the alkaline substance contains potassium hydroxide, a superabsorbent resin film having better flexibility and dimensional stability can be produced.
[0048] The concentration of the acrylic acid monomer may be about 20 to about 60% by weight, preferably about 40 to about 50% by weight, based on the monomer composition containing the raw material of the superabsorbent resin and the solvent, and may be an appropriate concentration taking into consideration the polymerization time and reaction conditions, etc. However, if the concentration of the monomer is too low, the yield of the superabsorbent resin may be low, causing problems in terms of economy, while if the concentration is too high, problems may occur in the process, such as partial precipitation of the monomer, and the physical properties of the superabsorbent resin may be deteriorated.
[0049] Meanwhile, in the present invention, the monomer composition contains a thickener and a humectant so that the monomer composition can be applied in the form of a film by a solution casting method.
[0050] By simultaneously containing a thickener and a humectant in this manner, the monomer composition of the present invention exhibits a viscosity suitable for casting into a film form, and can maintain an appropriate water content during the polymerization process after film casting, allowing the produced superabsorbent resin film to exhibit high flexibility.
[0051] In the present invention, a cellulose-based thickener is used as the thickener, and specifically, one or more selected from the group consisting of nanocellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxyethyl methyl cellulose, and hydroxypropyl methyl cellulose can be used. Preferably, nanocellulose, hydroxyethyl cellulose, or a combination thereof can be used.
[0052] The cellulose-based thickener may be contained in an amount of 0.01 parts by weight or more, 0.1 parts by weight or more, 0.2 parts by weight or more, or 0.35 parts by weight or more, but 5 parts by weight or less, 3 parts by weight or less, 1 part by weight or less, or 0.9 parts by weight or less, relative to 100 parts by weight of the solid content in the monomer composition.
[0053] In this case, the solid content in the monomer composition means all components of the composition excluding the solvent, that is, the solid content means the total content of the acrylic acid monomer, the alkaline substance for neutralizing the acrylic acid monomer, the cellulose thickener, the moisturizing agent, the crosslinking agent, the thermal polymerization initiator, the photopolymerization initiator, the internal crosslinking agent, and other additives.
[0054] If the content of the cellulose-based thickener is less than 0.01 parts by weight based on 100 parts by weight of the solid content in the monomer composition, it may be difficult to produce a monomer composition film because a sufficient thickening effect cannot be secured. Conversely, if it exceeds 5 parts by weight, the viscosity of the monomer composition becomes excessively high, the thickness of the film becomes thick, and it may be difficult to control the film thickness uniformly.
[0055] The moisturizing agent can be any substance that is generally used as a moisturizing component in pharmaceuticals, cosmetics, chemical products, etc. Examples of such moisturizing agents include one or more selected from the group consisting of polyhydric alcohols containing two or more hydroxyl groups in the molecule, citric acid, and citrate salts.
[0056] Specifically, the polyhydric alcohol may be a polyhydric alcohol having 3 to 30 carbon atoms and containing 3 to 12 hydroxy groups in the molecule. As an example, the polyhydric alcohol may be one or more selected from the group consisting of glycerin, diglycerin, propylene glycol, butylene glycol, sorbitol, polyethylene glycol, polyglycerin-3, polyglycerin-6, polyglycerin-10, and polyglyceryl-10 distearate and its derivatives (having 3 to 18 carbon atoms); among these, one or more selected from the group consisting of glycerin, diglycerin, ethylene glycol, and sorbitol can be preferably used.
[0057] Citric acid and / or citrates can also be used as moisturizing agents. Examples of citrates include triethyl citrate, methyl citrate, sodium citrate, trisodium 2-methyl citrate, etc.
[0058] It is preferred that the humectant be used in an amount of 5 parts by weight or more, 10 parts by weight or more, 20 parts by weight or more, or 30 parts by weight or more, but 70 parts by weight or less, 60 parts by weight or less, or 50 parts by weight or less, based on 100 parts by weight of the acrylic acid-based monomer.
[0059] If the content of the humectant is less than 5 parts by weight per 100 parts by weight of the acrylic acid monomer, the moisture content of the monomer composition film is insufficient, and the film may dry out or crumble during the subsequent polymerization and drying process, and the flexibility of the produced superabsorbent resin film may not be ensured. Conversely, if the content of the polyhydric alcohol exceeds 70 parts by weight per 100 parts by weight of the acrylic acid monomer, the absorption capacity of the superabsorbent resin film may be reduced. Therefore, it is preferable that the content of the humectant satisfies the above range.
[0060] The monomer composition includes an internal crosslinking agent for crosslinking the polymer. The internal crosslinking agent may be one that is generally used in the manufacture of superabsorbent resins. More specifically, the internal crosslinking agent may be a crosslinking agent having one or more functional groups capable of reacting with the water-soluble substituent of the acrylic acid monomer and one or more ethylenically unsaturated groups; or a crosslinking agent having two or more functional groups capable of reacting with the water-soluble substituent of the monomer and / or the water-soluble substituent formed by hydrolysis of the monomer.
[0061] Specific examples of the internal crosslinking agent include bisacrylamide, bismethacrylamide, poly(meth)acrylate of polyol having 2 to 10 carbon atoms, or poly(meth)allyl ether of polyol having 2 to 10 carbon atoms, and more specifically, one or more selected from the group consisting of N,N'-methylenebis(meth)acrylate, ethyleneoxy(meth)acrylate, polyethyleneoxy(meth)acrylate, propyleneoxy(meth)acrylate, glycerin diacrylate, glycerin triacrylate, trimethylol triacrylate, polyethylene glycol diacrylate, triallylamine, triaryl cyanurate, triallyl isocyanate, polyethylene glycol, diethylene glycol, and propylene glycol may be used. In one embodiment, polyethylene glycol diacrylate may be used as the internal crosslinking agent.
[0062] The internal crosslinking agent is included in a concentration of 5000 ppm or less based on the monomer composition to crosslink the polymerized polymer. In one embodiment, the internal crosslinking agent may be included in an amount of 100 ppm or more, 250 ppm or more, or 500 ppm or more, and 5000 ppm or less, 4500 ppm or less, or 4000 ppm or less. The content of the internal crosslinking agent may be adjusted to an appropriate content depending on the thickness of the superabsorbent resin film to be manufactured and the desired range of tensile strength.
[0063] In the method for producing a superabsorbent resin film of the present invention, the polymerization initiator used during polymerization is not particularly limited as long as it is one that is generally used in the production of superabsorbent resins.
[0064] Specifically, the polymerization initiator may be a thermal polymerization initiator or a photopolymerization initiator using UV irradiation, depending on the polymerization method. However, even in the photopolymerization method, a certain amount of heat is generated by irradiation such as UV irradiation, and a certain amount of heat is generated by the progress of the polymerization reaction, which is an exothermic reaction, so a thermal polymerization initiator may also be included. According to a preferred embodiment, a photopolymerization initiator and a thermal polymerization initiator may be used simultaneously as the polymerization initiator.
[0065] The photopolymerization initiator can be used without any limitation on its constitution as long as it is a compound capable of forming radicals by light such as ultraviolet light.
[0066] The photopolymerization initiator may be, for example, one or more selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyl alkylketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone. Specific examples of acylphosphine include commercially available lucirin TPO (2,4,6-trimethylbenzoyldiphenylphosphine oxide) and Irgacure 819 (phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide). More detailed information on various photopolymerization initiators is provided in Reinhold Schwalm's book "UV Coatings: Basics, Recent Developments and New Application (Elsevier, 2007)" p. 115, and is not limited to the above examples.
[0067] The photopolymerization initiator may be included in the monomer composition at 10 ppm or more, 20 ppm or more, or 40 ppm or more, but 2000 ppm or less, 1000 ppm or less, 500 ppm or less, or 100 ppm or less. If the concentration of the photopolymerization initiator is too low, the polymerization rate may be slow, and if the concentration of the photopolymerization initiator is too high, the molecular weight of the superabsorbent resin may be small, resulting in non-uniform physical properties.
[0068] The thermal polymerization initiator may be at least one selected from the group consisting of persulfate initiators, azo initiators, hydrogen peroxide, and ascorbic acid. Specifically, examples of persulfate initiators include sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), and ammonium persulfate ((NH4)2S2O8). Examples of azo initiators include 2,2-azobis(2-amidinopropane) dihydrochloride, 2,2-azobis-(N,N-dimethylene)isobutyramidine dihydrochloride, and the like. dihydrochloride, 2-(carbamoylazo)isobutylonitrile, 2,2-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 4,4-azobis-(4-cyanovaleric acid), etc. A wide variety of thermal polymerization initiators are well described in Odian's book 'Principle of Polymerization' (Wiley, 1981), p. 203, and are not limited to the above examples.
[0069] The thermal polymerization initiator may be included in the monomer composition at 10 ppm or more, 100 ppm or more, or 500 ppm or more, but not more than 2000 ppm, not more than 1500 ppm, or not more than 1000 ppm. If the concentration of the thermal polymerization initiator is too low, additional thermal polymerization hardly occurs, and the effect of adding the thermal polymerization initiator may be small, whereas if the concentration of the thermal polymerization initiator is too high, the molecular weight of the superabsorbent resin may be small, resulting in non-uniform physical properties.
[0070] The monomer composition may further contain additives such as a plasticizer, a storage stabilizer, and an antioxidant, if necessary.
[0071] Alternatively, the monomer composition may further include a foaming agent as an additive. The superabsorbent resin film produced from such a monomer composition has a porous structure having a large number of pores, thereby exhibiting higher breathability.
[0072] The foaming agent is foamed during polymerization and / or drying, and may be at least one selected from the group consisting of heat-expandable microspheres, expanded microspheres, azo compounds, and inorganic foaming agents. These foaming agents form a large number of pores in the superabsorbent resin film, thereby significantly improving the initial absorption capacity of the superabsorbent resin film.
[0073] The heat-expandable microspheres may have a structure including a core containing a hydrocarbon and a thermoplastic resin shell surrounding the core.
[0074] The hydrocarbon constituting the core of the thermally expandable microspheres may be one or more selected from the group consisting of n-propane, n-butane, iso-butane, cyclobutane, n-pentane, iso-pentane, cyclopentane, n-hexane, iso-hexane, cyclohexane, n-heptane, iso-heptane, cycloheptane, n-octane, iso-octane, and cyclooctane. Among these, hydrocarbons having 3 to 5 carbon atoms (n-propane, n-butane, iso-butane, cyclobutane, n-pentane, iso-pentane, and cyclopentane) are suitable.
[0075] The thermoplastic resin constituting the shell of the heat-expandable microspheres may be a polymer formed from one or more monomers selected from the group consisting of (meth)acrylate, (meth)acrylonitrile, aromatic vinyl, vinyl acetate, vinyl halide and vinylidene halide. Among these, a copolymer of (meth)acrylate and (meth)acrylonitrile or a (meth)acrylate homopolymer is most suitable for achieving the initial absorption capacity in the above-mentioned range.
[0076] The heat-expandable microspheres are a foaming agent that expands when heat is supplied, and can form pores in the superabsorbent resin film by expanding under high temperature conditions during the polymerization and / or drying step of the monomer. The expansion characteristics of the heat-expandable microspheres vary depending on the components constituting the core and shell, the weight of each component, and the average particle size. By adjusting these, the microspheres can expand to a desired size, and therefore the pore structure of the superabsorbent resin film can be controlled.
[0077] The average particle size (D50) of the heat-expandable microspheres before expansion may be 2 μm or more, 5 μm or more, 7 μm or more, or 10 μm or more, and may be 50 μm or less, 40 μm or less, or 35 μm or less. When the heat-expandable microspheres have such an average particle size, they can be determined to be suitable for achieving an appropriate porosity.
[0078] Here, the average particle size (D50) of the thermally expandable microspheres can be measured by dispersing the powder to be measured in a dispersion medium, introducing the dispersion into a commercially available laser diffraction particle size analyzer (e.g., Mastersizer 3000), and measuring the difference in diffraction pattern according to the particle size when the particles pass through a laser beam to calculate the particle size distribution.
[0079] Whether the heat-expandable microspheres can form pores of appropriate size in the superabsorbent resin film can be confirmed by foaming the capsules in air and checking the expansion ratio and size.
[0080] The superabsorbent resin film produced by the present invention has a thickness of 0.8 mm or less, preferably in the range of 0.001 to 0.8 mm, and therefore the appropriate pore size is about 10 to 500 μm. Therefore, in order to form pores of an appropriate size in the superabsorbent resin film, it is necessary to understand the expansion characteristics of the heat-expandable microspheres.
[0081] Specifically, the heat-expandable microspheres are applied to a glass Petri dish, and then heated in air for 10 minutes to expand the heat-expandable microspheres. If the heat-expandable microspheres show a maximum expansion ratio in air of 3 to 15 times, 2 to 12 times, or 1 to 7 times, it is suitable for producing a superabsorbent resin film having pores of an appropriate size.
[0082] When the heat-expandable microspheres have a maximum expansion size in air of 150 μm or less, pores of an appropriate size can be formed. Specifically, when the heat-expandable microspheres have a maximum expansion size in air of 10 to 500 μm, 50 to 300 μm, 70 to 150 μm, or 75 to 150 μm, they are suitable for producing a superabsorbent resin film having pores of an appropriate size.
[0083] The heat-expandable microspheres may start to expand at a temperature of 60 to 200°C, 70 to 170°C, or 80 to 165°C, and may reach maximum expansion at a temperature of 100 to 240°C, 120 to 200°C, or 130 to 190°C.
[0084] Examples of such thermally expandable microspheres include Nouryon's Expancel DU series, such as Expancel 461 DU 40, Expancel 461 DU 20, Expancel 031 DU 40, Expancel 053 DU 40, and Expancel 551 DU 40; and / or Matsunomo's Microsphere F series, such as Microsphere F-AC170D, Microsphere F-36, Microsphere F-36LV, Microsphere F-48, Microsphere F-80GS, and Microsphere F-50. Preferably, Expancel 031 DU 40, which includes a hydrocarbon core and a shell of an acrylate and acrylonitrile copolymer, and / or Microsphere F-AC170D, which includes a hydrocarbon core and a shell of an acrylate copolymer, can be used, but are not limited thereto.
[0085] The expanded microspheres are foaming agents that are already expanded before use, and may be hollow thermoplastic resin particles coated with inorganic substances such as talc and / or calcium carbonate.
[0086] The thermoplastic resin may be a polymer formed from one or more monomers selected from the group consisting of (meth)acrylate, (meth)acrylonitrile, aromatic vinyl, vinyl acetate, vinyl halide, and vinylidene halide.
[0087] Preferably, the expanded microspheres may be (meth)acrylate and / or (meth)acrylonitrile copolymer hollow particles having a surface coated with calcium carbonate.
[0088] The expanded thermoplastic resin hollow particles of the microspheres do not expand any further and shrink when heated, but the inorganic material on the surface exhibits foaming properties, and thus pores of a size similar to the particle size of the expanded microspheres are formed, so that the size of the pores formed in the superabsorbent resin film can be controlled by appropriately selecting the particle size of the expanded microspheres.
[0089] Therefore, the average particle size (D50) of the expanded microspheres is in the range of 10 μm or more, 20 μm or more, or 30 μm or more, and 150 μm or less, 130 μm or less, or 120 μm or less, which is suitable for producing a superabsorbent resin film having pores of an appropriate size as described above. In this case, the average particle size can be measured by the particle size measurement method for heat-expandable microspheres described above.
[0090] Meanwhile, the foaming temperature of the expanded microspheres is 130°C or more, 140°C or more, or 150°C or more, and may be 200°C or less, 180°C or more.
[0091] Examples of the expanded capsules include Matsunomo's Microsphere MFL series, such as MFL-110CAL, MFL-100MCA, MFA HD60CA, MFL HD30CA, and MFL-SEVEN. Preferably, MFL-110CAL, which is a hollow particle of an acrylate and acrylonitrile copolymer coated with calcium carbonate powder, can be used, but is not limited thereto.
[0092] As the azo compound, an azoamidine compound such as 2,2'-azobis(2-methylpropionamidine) dihydrochloride and 2,2-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate can be used, and preferably, 2,2'-azobis(2-methylpropionamidine) dihydrochloride can be used.
[0093] The inorganic foaming agent may be one or more selected from calcium carbonate (CaCO3), sodium bicarbonate (NaHCO3), ammonium bicarbonate (NH4HCO3), ammonium carbonate ((NH4)2CO3), ammonium nitrite (NH4NO2), sodium borohydride (NaBH4) and sodium carbonate (Na2CO3), and preferably calcium carbonate.
[0094] As the inorganic foaming agent, micro- or nano-sized particles having a particle size ranging from 1 nm to 100 μm can be used, and an appropriate type can be selected depending on the physical properties of the target superabsorbent resin sheet. At this time, the particle size of the inorganic foaming agent can be measured by the above-mentioned laser diffraction method or by a scanning electron microscope (SEM).
[0095] In the present invention, the heat-expandable microspheres, expanded microspheres, azo-based compounds, and inorganic foaming agents can be used individually as foaming agents, or one or more of the foaming agents can be used in combination.
[0096] Meanwhile, when one or more of the thermally expandable microspheres and expanded microspheres are used as the first foaming agent and one or more of the azo compound and inorganic foaming agent are used as the second foaming agent, the weight ratio of the first foaming agent to the second foaming agent may be in the range of 1:0.3 to 1:3, or in the range of 1:0.5 to 1:2. When such a weight ratio is satisfied, the improved initial absorption speed can be exhibited as described above.
[0097] On the other hand, the foaming agent is contained in an amount of 0.1 to 10 parts by weight, more preferably 0.5 to 7 parts by weight, or 1 to 5 parts by weight, based on 100 parts by weight of the monomer composition.
[0098] If the content of the foaming agent is less than 0.1 parts by weight per 100 parts by weight of the monomer composition, the porous structure of the superabsorbent resin film due to foaming cannot be secured, and therefore the effect of improving the initial absorption rate cannot be obtained.
[0099] In addition, if the content of the blowing agent exceeds 10 parts by weight based on 100 parts by weight of the monomer composition, the degree of crosslinking of the polymer during polymerization may be reduced by the blowing agent.In addition, since the thermally expandable microspheres and the expanded microsphere blowing agent have low solubility in a solvent (e.g., water) and low density, if the content exceeds 10 parts by weight based on 100 parts by weight of the monomer composition, the blowing agent may separate out from the monomer composition, which may result in poor foaming.
[0100] Most of the foaming agents are actively foamed at temperatures of 80° C. or higher, or 100° C. or higher. Therefore, foaming of the foaming agent mainly occurs during the drying stage of the hydrogel polymer film.
[0101] The raw materials, such as the acrylic unsaturated monomer, the cellulose thickener, the humectant, the internal crosslinking agent, the polymerization initiator, and the additives, are prepared in the form of a monomer composition solution dissolved in a solvent.
[0102] The solvent that can be used is not limited in composition as long as it can dissolve the above-mentioned components, and for example, one or more selected from water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, and N,N-dimethylacetamide can be used in combination. As an example, water can be used as the solvent.
[0103] In the present invention, the monomer composition exhibits a viscosity suitable for a solution casting method by including a cellulose-based thickener and a humectant. Specifically, the viscosity of the monomer composition at 25°C may be 100 mPa·s or more, 140 mPa·s or more, or 200 mPa·s or more, and may be 5000 mPa·s or less, 2300 mPa·s or less, 2000 mPa·s or less, 1500 mPa·s or less, or 1400 mPa·s or less. The viscosity of the monomer composition can be measured using a viscometer (e.g., TOKI TV-22) under the conditions of spindle #1 and a rotation speed of 1 rpm.
[0104] If the viscosity of the monomer composition is less than 100 mPa·s, it may be difficult to cast a monomer composition film with a uniform thickness and polymerize it while stretching it.On the other hand, if the viscosity of the monomer composition exceeds 5000 mPa·s, it is difficult to produce a uniform monomer composition, the flowability of the monomer composition is low, processability decreases, and degassing is difficult, which is undesirable.
[0105] After preparing the monomer composition, the monomer composition is cast on a substrate to prepare a monomer composition film, which is stretched and polymerized at the same time to form a hydrogel polymer film. The processes of casting the monomer composition and polymerizing the monomer composition can be carried out continuously through a roll-to-roll process.
[0106] First, a monomer composition is applied onto a substrate to produce a monomer composition film.
[0107] Specifically, the substrate may be a polyethylene terephthalate (PET) film, which is generally used as a release film and has at least one surface hydrophobically treated with silicone or fluorine. As an example, the substrate may be a PET film surface-treated with a siloxane-based polymer or polytetrafluoroethylene (Teflon (registered trademark)). However, the material of the substrate is not limited thereto, and a suitable substrate may be selected depending on the composition and properties of the monomer composition.
[0108] For example, the PET film with the hydrophobic surface may have a contact angle with respect to water of 105° to 110° and a surface energy of 20 to 25 mN / m. Such a hydrophobic PET film not only allows easy application of a monomer composition film, but also allows easy peeling of a hydrogel polymer film produced after polymerization, thereby improving the convenience of the manufacturing process. In particular, when the monomer composition contains the polyether-modified siloxane surfactant, the affinity with the hydrophobic PET film having the above contact angle and surface energy characteristics is even higher, so that casting with a uniform thickness is possible, and a uniform and thin film can be formed even in a roll-to-roll continuous process, thereby further improving productivity.
[0109] Unlike a typical polymer solution casting method in which the solvent is removed after casting the polymer solution, in the present invention, the monomer composition is coated on the substrate and then immediately stretched and polymerized to prevent a decrease in water content.
[0110] If the moisture content of the monomer composition film is excessively low, the components constituting the monomer composition before polymerization may precipitate, and the film may break after polymerization. Therefore, the moisture content of the monomer composition film is preferably in the range of 30% by weight to 60% by weight, more preferably in the range of 30% by weight to 50% by weight, or even more preferably in the range of 30% by weight to 45% by weight.
[0111] The thickness of the monomer composition film can be appropriately adjusted depending on the desired thickness of the superabsorbent resin film. The thickness of the monomer composition film hardly changes during the polymerization stage, but the thickness may decrease by about 10 to 40% or 15 to 35% as the moisture content decreases during the drying process of the hydrogel polymer film after polymerization. Taking this into consideration, the monomer composition film is manufactured to an appropriate thickness.
[0112] For example, the thickness of the monomer composition film may be 800 μm or less, 600 μm or less, or 500 μm or less, and may be 1 μm or more, 5 μm or more, or 10 μm or more, but is not limited thereto, and may be appropriately adjusted depending on the composition of the monomer composition, specific conditions in the polymerization and drying stages, and the desired thickness of the superabsorbent resin film.
[0113] Next, the monomer composition film is stretched in the machine direction (MD) while being irradiated with heat and / or light to carry out a polymerization reaction to form a hydrogel polymer film. By stretching the film during polymerization in this manner, the physical properties such as tensile strength of the superabsorbent resin film produced can be adjusted.
[0114] In this case, the tension applied to the monomer composition film may be 40N / m or more, or 45N / m or more, or 50N / m or more, or 60N / m or more, but may be 100N / m or less, or 90N / m or less, or 70N / m or less. If an excessively large tension is applied to stretch the monomer composition film, problems may occur in that the film is cut or the thickness becomes excessively thin, and if the tension is too small, physical properties such as the tensile strength of the film may not be ensured.
[0115] The polymerization temperature can be appropriately adjusted depending on the composition of the monomer composition, and is preferably 40° C. or 50° C. or higher for smooth reaction. If the temperature is too high, the solvent may evaporate and the components constituting the monomer composition may precipitate, so the polymerization temperature is preferably 90° C. or lower or 80° C. or lower.
[0116] The water content of the hydrogel polymer film produced through the polymerization step is about 20% by weight or more, preferably 25% by weight or more, but may be 40% by weight or less, or 35% by weight or less, and then the hydrogel polymer film is dried to produce the final superabsorbent resin film.
[0117] The temperature of the drying step is preferably in the range of 80 to 150° C. or 90 to 100° C. By drying within the above temperature range for about 5 to 30 minutes, it is possible to obtain a superabsorbent resin film having a moisture content of 15% by weight or less, 12% by weight or less, 10% by weight or less, or 9% by weight or less, but 1% by weight or more, 2% by weight or more, 4% by weight or more, or 6% by weight or more.
[0118] water absorbent articles The water-absorbent article according to one embodiment of the present invention includes the above-mentioned superabsorbent resin film between the liquid-impermeable backsheet and the absorbent body, thereby improving the damp feeling felt from the outside due to moisture released from the absorbent body after absorbing liquid, and providing an excellent feeling of use.
[0119] 1 is a cross-sectional view showing the structure of an existing water-absorbent article 1. The existing water-absorbent article 1 includes a liquid-impermeable backsheet 11, a breathable waterproof film 12, an absorbent body 13, and a liquid-permeable topsheet .
[0120] In contrast, as shown in Figures 2 to 4, the water-absorbent articles 2, 3, and 4 of the present invention include a superabsorbent polymer film 20 between a liquid-impermeable backsheet 11 and a breathable waterproof film 12, and / or between the breathable waterproof film 12 and an absorbent body 13. The superabsorbent polymer film has a thickness (h) of 500 µm or less and a moisture absorption capacity of 10 to 100 g / m2 measured according to the KS F 2611 standard. 2 To absorb moisture discharged from an absorbent body to the outside, thereby maintaining a dry feeling of use of the water-absorbent article.
[0121] On the other hand, when a superabsorbent resin film is interposed between the liquid-impermeable back sheet 11 and the breathable waterproof film 12, and between the breathable waterproof film 12 and the absorbent body 13, as shown in Figure 4, the thickness (h) and / or physical properties of each superabsorbent resin film may be the same as or different from each other.
[0122] Hereinafter, the absorbent article of the present invention will be described in detail with respect to each component.
[0123] Highly absorbent resin film In the water-absorbent article of the present invention, the superabsorbent polymer film as described above is interposed between the liquid-impermeable backsheet and the breathable waterproof film and / or between the breathable waterproof film and the absorbent body.
[0124] The superabsorbent resin film has excellent moisture absorption ability as described above, and can absorb moisture released from the absorbent body to significantly improve the damp feeling felt from the outside of the backsheet. In addition, since the superabsorbent resin film is thin, having a thickness of 500 μm or less, it can exhibit the moisture absorption performance described above and significantly improve the feeling of use of the absorbent article without significantly increasing the thickness of the absorbent article.
[0125] Liquid-impermeable back sheet The liquid-impermeable back sheet of the absorbent article may be a nonwoven fabric produced by spinning an olefin resin such as polyethylene, polypropylene, etc. The method for producing the nonwoven fabric is not particularly limited, and nonwoven fabrics produced by processing methods such as airlaid, thermal bond, spunlace, spunbond, meltblown, stitch bond, etc. may be used without limitation.
[0126] The nonwoven fabric used for the liquid-impermeable backsheet may have a pore size in the range of 20 to 1000 μm, 50 to 700 μm, or 10 to 300 μm. When the pores of the woven or nonwoven fabric satisfy the above range, the permeation of liquid is blocked, while water vapor and air can permeate, providing an excellent wearing comfort.
[0127] The basis weight of the liquid-impermeable back sheet is not particularly limited, but is preferably about 10 to 25 g / m 2 , preferably about 12 to 20 g / m 2 In this case, the feel can be further improved while preventing the body waste absorbed in the absorbent core from leaking out.
[0128] The liquid-impermeable back sheet and the superabsorbent resin film can be bonded together by a method such as heat bonding before the production of the absorbent article. Specifically, the superabsorbent resin film can be bonded to one side of the liquid-impermeable back sheet, and the breathable waterproof film, absorbent body, and liquid-permeable top sheet can be laminated on the superabsorbent resin film side of the bonded body to produce the absorbent article.
[0129] Breathable waterproof film On the other hand, the water-absorbent article of the present invention includes a breathable waterproof film on a liquid-impermeable backsheet, which has waterproof properties while allowing air to flow more smoothly.
[0130] The breathable waterproof film can be manufactured by blending a thermoplastic polymer with an additive to prepare a resin composition, and molding the composition using casting, expanding film extrusion, or other suitable film-forming techniques. The resin composition can have a composition of, for example, 40-60% thermoplastic polymer and 40-60% additive. The additive can be various components such as antioxidants, filler particles, dyes, etc., depending on the desired properties.
[0131] As an example, a film can be produced by casting a resin composition that is a blend of a thermoplastic polymer and an additive, and then stretching the film uniaxially or biaxially through three steps: a preheating step, a stretching step, and a heat setting step, to produce a waterproof film with breathability.
[0132] The thermoplastic polymers include, but are not limited to, very low density polyethylene (VLDPE), low density polyethylene (LDPE), high density polyethylene (HDPE), polypropylene, copolymers of ethylene with C3-C12 alpha-olefins, copolymers of propylene with ethylene and / or C4-C12 alpha-olefins, and propylene-based polymers containing both atactic and isotactic propylene units in the polypropylene backbone; elastomers such as polyurethanes, copolyetheresters, polyamide polyether block copolymers, ethylene vinyl acetate copolymers, copoly(styrene / ethylene-butylene), block copolymers such as styrene-poly(ethylene-propylene)-styrene, styrene-poly(ethylene-butylene)-styrene, polystyrene / poly(ethylene-butylene) / polystyrene, poly(styrene / ethylene-butylene / styrene), and the like.
[0133] The additive may be a filler such as calcium carbonate (CaCO3). Calcium carbonate is a white solid material formed by the reaction of carbonate ions and calcium ions, and can form a number of holes in the film by being bound by a polymer resin. In the present invention, when manufacturing a breathable waterproof film, the content of the calcium carbonate is adjusted to a range of 40 to 45 wt% based on the total weight of the breathable waterproof film-forming composition, and the stretch ratio of the film is adjusted to a range of 2.5 to 3.5 times in the mechanical direction in consideration of the tensile strength and moisture permeability, thereby adjusting the size of the holes formed in the film, so that the excrement absorbed in the absorbent is not leaked to the outside, and air and water vapor can be more smoothly passed through the back sheet.
[0134] Specifically, when the calcium carbonate content and the film stretch ratio are adjusted to the above ranges, holes with a size (diameter) of about 10 to 90 μm, preferably about 40 to 60 μm, can be formed in the film. The size of such holes is smaller than the size of water particles, which is 100 μm or more, and larger than the size of steam, which is about 0.001 to 0.01 μm. Therefore, the excrement absorbed in the absorbent body is prevented from leaking out by the breathable waterproof film, while the hot air and water vapor inside the diaper can be easily discharged to the outside through the breathable waterproof film.
[0135] The breathable waterproof film has an air permeability of 2000 to 5000 g / m 2 24hr, preferably 3500~4500g / m 2 If the breathability range is satisfied, side effects on the skin caused by moist air can be more effectively prevented.
[0136] The weight of the breathable waterproof film is not particularly limited, but is preferably about 15 to 22 g / m 2 In this case, the strength of the film is further improved, and the air permeability of the film is about 3500 to 4500 g / m 2 Adjustable within a 24-hour range, it blocks the excrement absorbed in the absorbent core from leaking out, while allowing air and water vapor to pass through the backsheet smoothly, further improving the comfort of the wearer.
[0137] The above-mentioned breathable waterproof film and superabsorbent resin film can be bonded together by a method such as heat bonding before the production of a water-absorbent article. As an example, the superabsorbent resin film is bonded to one side of the breathable waterproof film, and the air permeability of the bonded superabsorbent resin film and breathable waterproof film is 3000g / m 2 24hr or more, or 3200g / m 2 - 5000g / m2 for 24hr or more 2 ·24hr or less, 4500g / m 2 24hr or less, or 4200g / m2 The superabsorbent resin film has excellent moisture absorption capacity and high air permeability as described above, and therefore can impart moisture absorption performance to the absorbent article without reducing the air permeability.
[0138] Absorber The absorbent material used in the water-absorbent article of the present invention contains a highly absorbent resin powder, which is an aggregate of highly absorbent resin particles, and pulp.
[0139] The superabsorbent resin powder can be any material that is generally used to impart absorbency to absorbent articles without any restrictions. The superabsorbent resin can be, for example, one or more selected from the group consisting of acrylate polymer crosslinked product, vinyl alcohol-acrylate copolymer crosslinked product, maleic anhydride graft polyvinyl alcohol crosslinked product, acrylate-methacrylate copolymer crosslinked product, methyl acrylate-vinyl acetate copolymer saponification crosslinked product, starch-acrylate graft copolymer crosslinked product, starch-acrylonitrile graft copolymer saponification crosslinked product, carboxymethylcellulose crosslinked product, isobutylene-maleic anhydride copolymer crosslinked product, and methylene oxide polymer crosslinked product, and preferably acrylate polymer crosslinked product.
[0140] The size of the superabsorbent resin particles constituting the superabsorbent resin powder may be 100 to 1,000 μm, 150 to 800 μm, or 300 to 600 μm. If the size of the superabsorbent resin particles is less than 100 μm, the superabsorbent resin gel that has absorbed body fluid and swelled may be discharged to the outside of the absorbent article or may cause a gel blocking phenomenon, impairing the physical properties. If the particle size exceeds 1,000 μm, there is a problem that it is difficult to slim down the absorbent article.
[0141] The highly absorbent resin powder may be included in an amount of 10 to 90% by weight of the total weight of the absorbent, and may be included in an amount of 20% by weight or more, 30% by weight or more, or 40% by weight or more, but may be included in an amount of 80% by weight or less, or 60% by weight or less.
[0142] The pulp used in the absorbent may be cellulose fluff pulp formed by grinding wood pulp, which can rapidly absorb liquid and separate superabsorbent polymer particles from each other, reducing gel stickiness.
[0143] To ensure such effects, the pulp may be included in an amount of 10 to 90% by weight of the total weight of the absorbent, and preferably 20% by weight or more, or 40% by weight or more, but may be included in an amount of 80% by weight or less, 70% by weight or less, or 50% by weight or less.
[0144] Specifically, the superabsorbent polymer may be present in an amount of about 10 to 90% by weight, preferably about 30 to 60% by weight, based on the total weight of the absorbent core, and the pulp content may be about 10 to 90% by weight, preferably about 40 to 70% by weight, based on the total weight of the absorbent.
[0145] In addition to the superabsorbent resin powder and pulp, the absorbent may further include synthetic fibers such as polyethylene fibers, polypropylene fibers, polyester fibers, polyamide fibers, rayon fibers, polyurethane fibers, etc., in which case the binding strength between the superabsorbent resin powder and the pulp can be further improved. Such synthetic fibers may be used in an amount of 20% by weight or less, or 10% by weight or less, of the total weight of the absorbent.
[0146] The method for producing the absorbent body is not particularly limited, and for example, the absorbent body can be produced by uniformly mixing a highly water-absorbent resin powder with pulp and, optionally, synthetic fibers, squeezing the mixture to form a shape, and then packaging the squeezed product in a packaging material such as tissue.
[0147] Liquid permeable top sheet The liquid-permeable upper sheet can be preferably made of a material that is hydrophilic so that liquid can quickly permeate through it, and is soft to the touch and does not irritate the skin of the user.
[0148] The liquid-permeable upper sheet may be, for example, a hydrophilic nonwoven fabric, an apertured film such as an apertured polyethylene film, or a foamed film such as a urethane foam, and one or more of these may be laminated for use.
[0149] Preferably, the liquid-permeable top sheet may be a hydrophilic nonwoven fabric made of synthetic or natural fibers such as polypropylene, polyethylene, polyester, polyethylene terephthalate, rayon, cotton, etc. The method of manufacturing the nonwoven fabric is not particularly limited, and nonwoven fabrics manufactured by processing methods such as airlaid, thermal bond, spunlace, spunbond, meltblown, stitch bond, etc. may be used without limitation.
[0150] The fiber fineness of the liquid-permeable nonwoven fabric is not particularly limited, but when the fiber fineness is in the range of about 1.5 to 6 denier (d), preferably about 1.5 to 2 denier (d), skin irritation can be minimized when wearing an absorbent article, thereby minimizing the occurrence of side effects on the skin and improving the instantaneous absorption function.
[0151] In addition, the length of the fibers is not particularly limited, but when the length is about 36 to 39 mm, the workability of the carding process during the manufacture of the nonwoven fabric can be improved, and the surface uniformity of the nonwoven fabric can be improved, thereby minimizing friction on the wearer's skin.
[0152] The basis weight of the nonwoven fabric formed from such fibers is not particularly limited, but is about 15 to 30 g / m 2 , preferably about 15 to 20 g / m 2 In this case, the surface feel can be made softer while improving the absorbency, thereby minimizing the occurrence of side effects on the skin.
[0153] Method for manufacturing water-absorbent articles The method for manufacturing the water-absorbent article of the present invention is not particularly limited, and the water-absorbent article may be manufactured by laminating each component, i.e., the liquid-impermeable back sheet, the highly absorbent resin film, the breathable waterproof film, the absorbent body, and the liquid-permeable top sheet, in an appropriate order and then fixing them using embossing, or by fixing each component between each other using an adhesive such as a hot melt adhesive.
[0154] For example, when a superabsorbent polymer film is interposed between a breathable waterproof film and an absorbent body, a liquid-impermeable back sheet, a breathable waterproof film, a superabsorbent polymer film, an absorbent body, and a liquid-permeable top sheet can be laminated in that order, and then fixed with an adhesive or embossing to produce an absorbent article.
[0155] Alternatively, the absorbent article can be manufactured by first heat-bonding the highly absorbent polymer film to a liquid-impermeable back sheet or a breathable waterproof film, and then laminating and fixing the resulting film to other components.
[0156] On the other hand, when the superabsorbent resin film is interposed between a liquid-impermeable back sheet and a breathable waterproof film, the superabsorbent resin film is first bonded to one side of the liquid-impermeable back sheet, and then a breathable film is laminated on the upper side of the superabsorbent resin film (the side not in contact with the liquid-impermeable back sheet), and the absorbent body and the liquid-permeable upper sheet are laminated and then fixed together to produce an absorbent article.
[0157] Alternatively, a highly absorbent resin film can first be bonded to one or both sides of a breathable waterproof film, and then this can be placed on a liquid-impermeable back sheet, after which an absorbent body and a liquid-permeable upper sheet can be laminated and fixed to produce an absorbent article.
[0158] The bonding of the superabsorbent resin film and the liquid-impermeable backsheet, and the bonding of the superabsorbent resin film and the breathable waterproof film can be performed by thermal bonding, and the temperature and pressure during thermal bonding can be appropriately adjusted depending on the properties of the liquid-impermeable backsheet, the breathable waterproof film, and the superabsorbent resin film used.
[0159] The absorbent article may be a disposable diaper, a sanitary napkin, or an incontinence pad.
[0160] Hereinafter, preferred examples will be presented for the understanding of the present invention. However, the following examples are merely illustrative of the present invention, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope and technical spirit of the present invention. Naturally, such changes and modifications fall within the scope of the appended claims. EXAMPLES
[0161] [Example] <Production of superabsorbent resin film> Example 1-1 55 g of acrylic acid, 66.6 g of a 45 wt % solution of potassium hydroxide (KOH), and 55 g of water were mixed together to prepare a neutralized solution in which 70 mol % of the acrylic acid was neutralized.
[0162] Hydroxyethyl cellulose (HEC, Ashland Natrosol 250HR), glycerin, sodium persulfate as a thermal polymerization initiator, and Irgacure 819 as a photopolymerization initiator were added to the neutralization solution to prepare a monomer composition having a total solid content (TSC) of 54 wt %.
[0163] At this time, 0.45 parts by weight of HEC was added per 100 parts by weight of the solid content of the monomer composition, 40 parts by weight of glycerin was added per 100 parts by weight of acrylic acid, and 1000 ppm of the thermal polymerization initiator and 80 ppm of the photopolymerization initiator were added per total weight of the monomer composition.
[0164] The viscosity of the prepared monomer composition at 25° C. was measured using a TOKI TV-22 viscometer at a spindle #1 and a rotation speed of 1 rpm, and the viscosity of the monomer composition was confirmed to be 201 mPa·s.
[0165] Next, the monomer composition was coated on one side of a polyethylene terephthalate (PET) film to form a monomer composition film (water content 30%) having a thickness of 20 μm. A comma coater was used for the coating, and the moving speed of the applicator roll was 0.5 m / min.
[0166] Thereafter, the monomer composition film was irradiated with 370 mJ / cm 2 The polymerization was carried out by irradiating ultraviolet rays of 1000 nm to form a hydrogel polymer film. At this time, the monomer composition film was stretched by applying a tension of 60 N / m in the MD direction to carry out the polymerization reaction. The thickness of the produced hydrogel polymer film was 20 μm, which was confirmed to be no significant change compared to the monomer composition, and the water content was 15 wt%.
[0167] Then, the prepared hydrogel polymer film was dried at 80° C. for 5 minutes to prepare a super absorbent resin film (SAP film) having a water content of 10 wt % and a thickness of 17 μm.
[0168] The moisture content was calculated from the pre-drying weight (a) and post-drying weight (b) of the superabsorbent resin film according to the following formula: In this case, the superabsorbent resin film was dried by increasing the temperature from room temperature (25°C) to 150°C over 5 minutes and then maintaining it at 150°C for 15 minutes.
[0169] Moisture content (%)=(ab) / a×100
[0170] Example 1-2 A superabsorbent resin film having a moisture content of 10% by weight and a thickness of 45 μm was produced in the same manner as in Example 1-1, except that the thickness of the monomer composition film was 50 μm, the drying temperature of the hydrous gel polymer was 80° C., and the drying time was 10 minutes.
[0171] Examples 1-3 A superabsorbent resin film having a moisture content of 10% by weight and a thickness of 149 μm was produced in the same manner as in Example 1-1, except that the thickness of the monomer composition film was 160 μm, the drying temperature of the hydrous gel polymer was 90° C., and the drying time was 10 minutes.
[0172] Examples 1-4 55 g of acrylic acid, 66.6 g of a 45 wt % solution of potassium hydroxide (KOH), and 55 g of water were mixed together to prepare a neutralized solution in which 70 mol % of the acrylic acid was neutralized.
[0173] To the neutralization solution, an internal crosslinker (polyethylene glycol diacrylate (PEGDA), MW=400, Aldrich), expanded microspheres MFL110CAL (Matsumoto Yushi-Seiyaku, average particle size 90-120 μm, foaming temperature 160-170° C.) as a foaming agent, hydroxyethyl cellulose (HEC, Ashland Natrosol 250HR), glycerin, sodium persulfate as a thermal polymerization initiator, and Irgacure 819 as a photopolymerization initiator were added to prepare a monomer composition having a total solid content (TSC) of 40 wt %.
[0174] In this case, the foaming agent was added at 1 part by weight per 100 parts by weight of the monomer composition, HEC was added at 0.45 parts by weight per 100 parts by weight of the solid content of the monomer composition, and glycerin was added at 40 parts by weight per 100 parts by weight of acrylic acid. The thermal polymerization initiator was added at 1000 ppm and the photopolymerization initiator was added at 80 ppm, per the total weight of the monomer composition.
[0175] The viscosity of the prepared monomer composition at 25° C. was measured using a TOKI TV-22 viscometer with a spindle #1 and a rotation speed of 1 rpm, and the viscosity of the monomer composition was confirmed to be 211 mPa·s.
[0176] Next, the monomer composition was coated on one side of a polyethylene terephthalate (PET) film to form a monomer composition film (water content 30%) having a thickness of 160 μm. A comma coater was used for the coating, and the moving speed of the applicator roll was 0.5 m / min.
[0177] Thereafter, the monomer composition film was irradiated with 370 mJ / cm 2 The polymerization was carried out by applying ultraviolet light of 60 N / m to the monomer composition film in the MD direction to stretch it, thereby forming a hydrogel polymer film.
[0178] Next, the prepared hydrogel polymer was dried at 90° C. for 10 minutes to prepare a super absorbent resin film (SAP film) having a water content of 10 wt % and a thickness of 153 μm.
[0179] <Production of water-absorbent articles> Comparative Example 1 (1) Manufacturing of liquid-impermeable backsheets Polypropylene is spun at high temperature to form a web in which polypropylene fibers are laminated, and then the web is bonded through a calendar roll with embossed protrusions of a certain pattern to form a liquid-impermeable back sheet (nonwoven fabric, pore size of about 40 to 60 μm, basis weight of 12 g / m) with a certain pattern embossed on the surface. 2 ) was manufactured.
[0180] (2) Manufacturing of breathable waterproof films A waterproof film-forming composition was obtained by mixing 50-55% by weight of polyethylene, 40-45% by weight of calcium carbonate, 1-1.5% by weight of a dispersant, 1-1.5% by weight of an antioxidant, and 2-3% by weight of a toning agent.
[0181] The waterproof film-forming composition was fed to an extruder through a feed hopper and melted. The molten composition was kneaded in the extruder, extruded through a T-die into a film shape, cooled, and then heated to a temperature at which the film can be stretched, stretching the film to a stretch ratio of 2.5 to 3.5 times in the mechanical direction. The film was gradually cooled and then cut to a certain width and length, and then cut into pieces of 17 g / m 2 Breathable waterproof film with a basis weight of 4400g / m 2 24hr).
[0182] (3) Manufacture of absorbent bodies A deodorant composition was prepared by mixing 8% by weight of salicylic acid, 61% by weight of polyethylene glycol, and 31% by weight of cetyl alcohol. The deodorant composition was then coated on a sheet of paper with a basis weight of 30 g / m2 using a gravure coating device. 2 The deodorizing composition was applied to the surface of a breathable bonded nonwoven fabric sheet made of cotton spunlace. The breathable bonded nonwoven fabric sheet coated with the deodorizing composition was then passed through a hot air drying chamber to evaporate the water, thereby producing a core wrap sheet surface-treated with the deodorizing composition.
[0183] Basis weight 50g / m 2 40% by weight of fluff pulp was mixed with 60% by weight of polyacrylate-based superabsorbent resin powder (average particle size 400 μm, CRC: 34 g / g, 0.3 psi AUP: 28 g / g) having a particle size of 250 to 600 μm, and the mixture was surrounded by the core wrap sheet produced above to produce an absorbent body having a thickness of 3.0 mm.
[0184] (4) Manufacturing of liquid-permeable top sheet For the liquid-permeable top sheet, 15 g / m 2 A spunbond nonwoven fabric with a thickness of 0.1 mm was used. The liquid-permeable upper sheet was manufactured in a shape that could completely cover the body-facing surface of the upper absorbent body so that liquids such as urine could be diffused into the upper absorbent body without leakage.
[0185] (5) Manufacture of absorbent products A breathable waterproof film was attached to one side of the prepared liquid-impermeable back sheet, and then the absorbent and the liquid-permeable top sheet were laminated on the breathable waterproof film in order, and then bonded together to prepare an absorbent article (disposable diaper).
[0186] Example 2-1 An absorbent article was manufactured in the same manner as in Comparative Example 1, except that the superabsorbent resin film prepared in Example 1-1 was additionally laminated between the liquid impermeable backsheet and the breathable waterproof film.
[0187] Example 2-2 An absorbent article was manufactured in the same manner as in Comparative Example 1, except that the superabsorbent resin film prepared in Example 1-2 was additionally laminated between the liquid impermeable backsheet and the breathable waterproof film.
[0188] Example 2-3 An absorbent article was manufactured in the same manner as in Comparative Example 1, except that the superabsorbent resin film prepared in Example 1-3 was additionally laminated between the liquid impermeable backsheet and the breathable waterproof film.
[0189] Examples 2-4 An absorbent article was manufactured in the same manner as in Comparative Example 1, except that the superabsorbent resin film prepared in Example 1-4 was additionally laminated between the breathable waterproof film and the absorbent body.
[0190] Examples 2-5 An absorbent article was manufactured in the same manner as in Comparative Example 1, except that the superabsorbent resin film prepared in Example 1-1 was additionally laminated between the breathable waterproof film and the absorbent body.
[0191] Examples 2-6 An absorbent article was manufactured in the same manner as in Comparative Example 1, except that the superabsorbent resin film prepared in Example 1-2 was additionally laminated between the breathable waterproof film and the absorbent body.
[0192] Examples 2-7 An absorbent article was manufactured in the same manner as in Comparative Example 1, except that the superabsorbent resin film prepared in Example 1-3 was additionally laminated between the breathable waterproof film and the absorbent body.
[0193] Comparative Example 2 An absorbent article was manufactured in the same manner as in Example 2, except that a 52 μm thick superabsorbent fiber (SAP fiber, Luquafleece (registered trademark) SAF-52, Basf) was laminated between the liquid-impermeable backsheet and the breathable waterproof film instead of the superabsorbent resin film.
[0194] Comparative Example 3 An absorbent article was manufactured in the same manner as in Example 2, except that a 112 μm thick superabsorbent fiber (SAP fiber, Luquafleece (registered trademark) SAF-112, Basf) was laminated between the liquid-impermeable backsheet and the breathable waterproof film instead of the superabsorbent resin film.
[0195] Comparative Example 4 An absorbent article was manufactured in the same manner as in Example 2, except that a 1.0 mm thick absorbent body (40% by weight fluff pulp, 60% by weight superabsorbent resin) was laminated between the liquid-impermeable back sheet and the breathable waterproof film instead of the superabsorbent resin film.
[0196] <Experimental Example 1: Evaluation of the physical properties of superabsorbent resin film> (1) Moisture absorption The superabsorbent resin film was cut to a size of 15cm x 24cm, and aluminum tape was attached to one side of the film to prevent moisture from entering the film, to prepare a specimen for analyzing moisture absorption performance. The moisture absorption amount of the superabsorbent resin was measured using the specimen according to the following method in accordance with the KS F 2611:2019 standard.
[0197] 1) The inside of the thermo-hygrostat is maintained at 25°C and relative humidity 50%, and the sample is cured for 12 hours, after which the initial mass (W1) is measured. 2) The inside of the thermo-hygrostat is maintained at 25°C and a relative humidity of 75%, and the sample is allowed to absorb moisture for 12 hours, after which the mass (W2) is measured. 3) Calculate the amount of moisture absorption using the following formula. Moisture absorption (g / m 2 )=(W2-W1) / 0.036
[0198] (2) Tensile strength The superabsorbent resin film was cut into a rectangular shape measuring 20 mm x 60 mm so that the cut surface was smooth, and the specimen was prepared. The specimen was attached to a tensile strength measuring device (TAXTplus, Stable Micro Systems) with an initial grip distance of 20 mm. The specimen was pulled at a speed of 0.5 mm per second, and the force (N) at the time when the specimen broke was measured. This value was expressed as the cross-sectional area (mm 2 ) to obtain the tensile strength (MPa).
[0199] <Experimental Example 2: Evaluation of the physical properties of absorbent articles> (1) Evaluation of external dampness In a chamber with a humidity of 50% and a temperature of 38.7°C, the absorbent articles manufactured in each of the Examples and Comparative Examples were placed on a glass plate, and 350 ml of physiological saline (0.9% NaCl aqueous solution) at 37°C was poured onto the liquid-permeable upper sheet of the absorbent article.
[0200] After 30 minutes, it was checked whether steam had accumulated on the glass plate. If steam had accumulated, it was rated as having a damp feeling outside (O), and if steam had not accumulated, it was rated as not having a damp feeling outside (X).
[0201] (2) Water vapor barrier permeability 1000 ml of distilled water was poured into the absorbent articles having an area of 25 cm x 10 cm produced in each of the Examples and Comparative Examples and absorbed. The absorbent articles having absorbed the distilled water were then placed in a thermo-hygrostat (humidity: 50%, temperature: 38.7°C) for 12 hours. Thereafter, the water vapor barrier permeability (g / m2) was measured based on the weight increase relative to the area of the absorbent article. 2 12hr) was calculated using the following formula:
[0202] Water vapor barrier permeability (g / m 2 12hr)=(W2-W1) / T
[0203] (In the above calculation formula, W1 is the weight per area (g / m2) of the absorbent article that absorbed distilled water before the constant temperature and humidity treatment. 2 ) and W2 is the weight per area of the absorbent article after constant temperature and humidity treatment (g / m 2 ) and T is the constant temperature and humidity treatment time, which is 12 hours.
[0204] (3) Breathability The test piece for measuring the air permeability was a breathable waterproof film (17 g / m 2 , breathability 4400g / m 2 In each example and comparative example, a superabsorbent resin film, SAP fiber, or absorbent was applied between the liquid-impermeable back sheet and the breathable waterproof film, or between the breathable waterproof film and the absorbent, to one side of the sheet (24 hr, thickness 25 μm) by heat bonding at 130°C and 20 kgf / cm.
[0205] A test piece of 150 mm (MD) x 150 mm (CD) was taken and measured using a Frazier Type Air Permeability Tester in accordance with JIS L 1096. The average value of n=5 was taken as the measured value.
[0206] [Table 1]
[0207] As a result of the experiment, it was confirmed that Examples 1-1 to 1-4 exhibited excellent moisture absorption capacity and tensile strength. Also, it was confirmed that the water-absorbent articles of Examples 2-1 to 2-7 had significantly improved external dampness compared to Comparative Example 1 while not impairing breathability due to the superabsorbent resin film interposed between the liquid-impermeable backsheet and the breathable waterproof film, or between the breathable waterproof film and the absorbent body.
[0208] In addition, to evaluate the feel of the diapers when actually used, a simulated wearing test was conducted (37°C saline was poured onto the liquid-permeable upper sheet of the diaper, and the diaper was left at 36.5°C for 5 minutes, after which the feel of the back sheet was checked). As a result, the diapers of Examples 2-1 to 2-7 exhibited an even warmer and drier feel than the diaper of Comparative Example 1.
[0209] However, when superabsorbent fibers were used instead of the superabsorbent resin film, the breathability was excellent but the moisture permeability was inferior, and the effect of improving the dampness outside could not be secured. Also, when an absorbent was used instead of the superabsorbent resin film, the dampness outside was improved, but the breathability was significantly reduced. [Explanation of symbols]
[0210] 1, 2, 3, 4: Water absorbent articles 11: Liquid-impermeable back sheet 12: Breathable waterproof film 13: Absorbent 14: Liquid-permeable top sheet 20: Highly absorbent resin film
Claims
1. The thickness is 500 μm or less, Moisture absorption capacity measured according to the KS F 2611 standard is 10 to 100 g / m 2 A highly absorbent resin film.
2. 2. The highly water-absorbent resin film according to claim 1, having a thickness of 10 to 200 μm.
3. 3. The highly water-absorbent resin film according to claim 1, wherein the film has a moisture content of 1 to 15% and a tensile strength of 5 to 50 MPa.
4. 1. An absorbent article comprising: a liquid-impermeable backsheet; a breathable waterproof film; an absorbent body comprising a superabsorbent polymer powder and pulp; and a liquid-permeable topsheet, A water-absorbent article comprising the superabsorbent polymer film according to any one of claims 1 to 3 between the liquid-impermeable backsheet and the breathable waterproof film, and / or between the breathable waterproof film and an absorbent body.
5. 5. The water-absorbent article according to claim 4, wherein the highly water-absorbent resin film is attached to one side of the liquid-impermeable backsheet and / or to one or both sides of the breathable waterproof film.
6. The highly water-absorbent resin film is attached to one side of the breathable waterproof film, The air permeability of the laminated highly water-absorbent resin film and breathable waterproof film is 3000 to 5000 g / m 2 The absorbent article according to claim 4, wherein the retention time is 24 hours.
7. The water-absorbent article according to any one of claims 4 to 6, wherein the liquid-impermeable backsheet is a nonwoven fabric having a pore size of 20 to 1000 µm.
8. The breathable waterproof film has an air permeability of 2000 to 5000 g / m 2 The absorbent article according to any one of claims 4 to 7, wherein the retention time is 24 hours.
9. The water-absorbent article according to any one of claims 4 to 8, wherein the absorbent body contains 10 to 90% by weight of highly water-absorbent resin powder.
10. The liquid-permeable top sheet has a basis weight of 15 to 30 g / m 2 The absorbent article according to any one of claims 4 to 9,
Citation Information
Patent Citations
Absorbent articles
JP1995132126A
Production of film and sheet
JP1998279712A
Hygroscopic / water absorbing structure and superabsorbent compound material
JP2004001461A
Water-absorbent film and packaging material using it
JP2006027204A
Disposable absorbent article
JP2015058034A