Two-component phosphate ester cavity filling semi rigid foam

A two-component epoxy phosphate ester-based foam system addresses the limitations of polyurethane foams by offering rapid curing and foaming at reduced temperatures, ensuring stable mixing ratios and improved adhesion, and enhancing safety and performance.

JP2024167408AActive Publication Date: 2024-12-03ZEPHYROS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024154379
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-11-15
Filing Date
2024-09-07
Publication Date
2024-12-03
Estimated Expiration
2039-05-06

AI Technical Summary

Technical Problem

Existing foam materials, particularly polyurethane-based foams, face challenges such as isocyanate content, limited adhesion, poor hydrolysis resistance, sensitivity to temperature changes, and health and safety risks, making them unsuitable for certain applications. Phosphoric acid alternatives like phosphoric acid esters offer improvements but still require slower reaction times and stable mixing ratios.

Method used

A two-component system comprising an A side with epoxy material and a B side with phosphate ester and phosphoric acid, which reacts at reduced temperatures (below 50°C) to provide fast curing and foaming, allowing for adhesion to various substrates without additional curing agents and achieving volumetric expansion of at least 200%.

Benefits of technology

The system enables rapid curing and foaming at ambient temperatures, ensuring stable mixing ratios and improved adhesion, while minimizing health and safety risks, and providing desirable flammability and toxicity properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167408000001
    Figure 2024167408000001
  • Figure 2024167408000002
    Figure 2024167408000002
  • Figure 2024167408000003
    Figure 2024167408000003
Patent Text Reader

Abstract

To provide a method and composition related to two component epoxy phosphate ester based foam materials.SOLUTION: There is provided a method comprising: providing a two-component system, the two-component system including an A side and a B side, the A side including epoxy material and the B side including phosphate ester and phosphoric acid; mixing the A side and the B side to form a resulting reaction product; wherein the resulting reaction product of the A side and the B side cures at a temperature of less than 50°C. There is also provided a composition comprising: a) a first component including epoxy; b) a second component including phosphate ester and phosphoric acid; wherein a resulting reaction product of the first component and second component cures at a temperature of less than 50°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present teachings relate generally to two-component epoxy phosphate-based foam materials. [Background technology]

[0002] Foam materials are frequently employed in the transportation and construction industries for various applications. For example, foam materials can provide one or more of structural support, sealing, and sound attenuation. When room temperature activation (e.g., expansion) is desired, polyurethane-based foams are most often used. Polyurethane foams have many drawbacks, some of which include the inclusion of isocyanates, limited adhesion capabilities to certain substrates, poor hydrolysis resistance in wet or humid environments, unsuitability for use in slow-reacting systems, high sensitivity to temperature changes during dispensing and foaming, and the requirement for high specificity of mix ratios during compounding.

[0003] Phosphoric acid has been utilized for in-situ foaming reactions in polymeric materials as an alternative to polyurethane-based foams. However, phosphoric acid introduces additional concerns. As one example, the reaction time with phosphoric acid is very fast and is not ideal for assembly processes that require time to place the polymeric material on a surface prior to the foaming step. Thus, a somewhat slower reaction time is preferred. In some situations, the nature of phosphoric acid may have negative health and safety risks due to its low pH and splash hazard. Therefore, alternative materials with reduced health and safety risks would be preferred. There is also a significant difference in viscosity between phosphoric acid and the oligomeric or polymeric materials with which it reacts. This poses challenges both in the manufacture (e.g., mixing) of the material and in the storage of the material. Phosphoric acid also has a much lower molecular weight than many oligomeric and polymeric materials, and thus a much lower molecular weight per functional reactive group, which leads to undesirable mix ratios. A relatively equivalent mix ratio of 1:1 or 2:1 would be preferred. Finally, the reactive nature of phosphoric acid makes it difficult to formulate adhesive and sealant materials since many chemical components can become unstable when utilized with phosphoric acid. The ability to include a variety of different moieties that may be advantageous for adhesion, physical or chemical compatibility, or other reasons would be desirable.

[0004] WO 2016 / 149700, incorporated herein by reference for all purposes, discloses the use of phosphoric acid esters as a replacement for phosphoric acid. However, adding some amount of phosphoric acid in addition to the ester may provide significant benefits for one or more of the rate of reactivity and additional functionality. For example, if reactivity at low temperatures is desired, adding an amount of phosphoric acid in combination with the phosphoric acid ester could increase the rate of reaction compared to using the phosphoric acid ester alone. As another example, the addition of phosphoric acid could impart multi-functionality to the foam material to prevent foam collapse. Such collapse may occur due to the reaction of the phosphoric acid ester with the metal carbonate (which reduces the average functionality of the material). The addition of phosphoric acid effectively compensates for the reaction between the metal carbonate and the phosphoric acid ester, thereby minimizing foam collapse.

[0005] Notwithstanding the above teachings, there remains a need for improved foam materials. There is a need for foam materials that provide room temperature cure. There is a need for foam materials that provide expansion and crosslinking at reduced temperatures compared to known foam materials. There is a need for foam materials that provide adhesion to a wide variety of substrates. There is a need for foam materials that utilize components that allow for both curing and foaming without the need for additional components. There is a need for foam materials that provide desired properties of fire, smoke, and toxicity (FST) while eliminating the use of undesirable agents in imparting those properties. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2016 / 149700 Summary of the Invention [Problem to be solved by the invention]

[0007] The present teachings provide one or more of the benefits discussed above. The foam materials of the present teachings can be utilized for one or more of the following: cavity filling, sealing, reinforcement, or cushioning. [Means for solving the problem]

[0008] The present teachings provide a method comprising providing a two-component system, the two-component system including an A-side and a B-side, where the A-side includes an epoxy material and the B-side includes a phosphate ester and phosphoric acid, and mixing the A-side and the B-side to form a resultant reaction product, wherein the resultant reaction product of the A-side and the B-side cures at a temperature less than 50 degrees.

[0009] The B side may include one or more phosphate esters. The A side, the B side, or both may include one or more fillers and / or one or more reinforcing materials. The A side may include one or more metal carbonates.

[0010] The foaming and curing reactions can occur at temperatures from about 10° C. to about 35° C. The foaming and curing reactions can occur at higher or lower temperatures. The degree of foaming can vary depending on the temperature at which foaming and curing occurs. The foaming and curing reactions can occur at temperatures from about 15° C. to about 25° C.

[0011] The cure time of the resulting reaction product may be less than 15 minutes. The cure time of the resulting reaction product may be about 5 to about 10 minutes. The cure time may be 30 minutes or less. The cure time may be 60 minutes or less. The foaming time may be 10 minutes or less, 5 minutes or less, or even 1 minute or less. The foaming time may be less than the time to complete the cure. The method may be free of any additional curing agent. The resulting reaction product may have a volume expansion of at least 200%.

[0012] The phosphoric acid may be added after preparation of the phosphate ester. The A-side and B-side may be mixed in a volumetric mix ratio of about 1:4 to about 4:1 (A-side:B-side). The A-side and B-side may be mixed in a volumetric mix ratio of about 2:1 (A-side:B-side). The reaction product may be fully expanded in less than 10 minutes, less than 5 minutes, or even less than 2 minutes. The method may include adding a second amount of phosphoric acid. The viscosity of the A-side at 23° C. may be about 20,000 cP to about 50,000 cP. The viscosity of the A-side at 23° C. may be about 35,000 cP to about 45,000 cP. The A-side may be formulated with increasing functionality to create an infinite network by using a functionality higher than 2.

[0013] The present disclosure further provides a composition comprising: a) a first component comprising an epoxy material; b) a second component comprising a phosphate ester and phosphoric acid. The resulting reaction product of the first component and the second component cures at a temperature below 50° C.

[0014] The second component may include at least one phosphate ester. The second component may include at least two different phosphate esters. The first component, the second component, or both may include one or more fillers and / or one or more reinforcing materials. The first component may include calcium carbonate.

[0015] The curing temperature (eg, the temperature at which the material begins to cure or the temperature at which the material completes curing) may be from about 10° C. to about 35° C. The curing temperature may be from about 15° C. to about 25° C.

[0016] The resulting reaction product may have a cure time of less than 15 minutes. The resulting reaction product may have a cure time of about 5 minutes to about 10 minutes. The resulting reaction product may have a volume expansion of at least 200%.

[0017] The A-side and B-side may be in a volumetric mix ratio of about 1:4 to about 4:1 (A-side:B-side). The A-side and B-side may be in a volumetric mix ratio of about 2:1 (A-side:B-side). The reaction product may be fully expanded in less than 10 minutes, less than 5 minutes, or even less than 2 minutes. The composition may include a second amount of phosphoric acid. The viscosity of the A-side at 23° C. may be about 20,000 cP to about 50,000 cP. The viscosity of the A-side at 23° C. may be about 35,000 cP to about 45,000 cP. The A-side may be formulated with increasing functionality to create an infinite network by using a functionality higher than 2.

[0018] The present teachings further provide a composition comprising: a) a first component comprising one or more of: i) a liquid epoxy resin; ii) a flexible epoxy resin; iii) an epoxy phenol novolac resin; iv) an aliphatic multifunctional epoxy resin; v) calcium carbonate; vi) wollastonite; and vii) a hydrophobic silica; and b) a second component comprising one or more of: i) a first phosphate ester; ii) a second phosphate ester; iii) a hydrophobic silica; and iv) a phosphoric acid, wherein a resulting reaction product of the first component and the second component cures at a temperature less than 50° C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present teachings satisfy one or more of the above needs through improved devices and methods described herein. The explanations and illustrations provided herein are intended to familiarize one of ordinary skill in the art with the present teachings, their principles, and their practical application. One of ordinary skill in the art can adapt and apply the present teachings in numerous forms that may be most appropriate to the requirements of a particular use. Thus, the specific embodiments of the present teachings shown are not intended to be exhaustive or to limit the present teachings. The scope of the present teachings should therefore be determined not with reference to the above description, but instead with reference to the appended claims and the full scope of equivalents to which such claims are entitled. The disclosures of all articles and references, including patent applications and patent publications, are incorporated by reference for all purposes. Moreover, other combinations that may be gleaned from the appended claims are possible, and such combinations are also hereby incorporated by reference into this written description.

[0020] This application claims the benefit of the filing date of U.S. Provisional Patent Application No. 62 / 767,543, filed November 15, 2018, the contents of which are incorporated herein by reference for all purposes.

[0021] The present teachings provide a method comprising providing a two-component system including an A-side and a B-side. The A-side includes an epoxy and the B-side includes a phosphate ester and optionally a phosphoric acid. The A-side and the B-side can be mixed to form a resultant reaction product. The resultant reaction product of the A-side and the B-side cures at a temperature less than 50° C.

[0022] At least one component of the two-component system may include a phosphate ester. The phosphate ester may be produced by reaction of phosphoric acid with various epoxide-functional monomers, although other preparation methods are feasible. The phosphate ester may be produced by reaction of epoxidized cashew nut liquid (CNSL) polymer to produce epichlorohydrin phosphate. The phosphate ester may be used to produce 1,2-propanediol, 3-[(2-ethylhexyl)oxyl]-phosphate.

[0023] At least one component of the two-component system may include one or more phosphate esters. At least one component of the two-component system may include exactly two different phosphate esters. For example, the second component or side B may include a first phosphate ester and a second phosphate ester. The first phosphate ester may be a reaction product of an epoxidized cashew nut liquid (CNSL) polymer to produce a phosphate ester. The second phosphate ester may be a reaction product of 2-propanediol, 3-[(2-ethylhexyl)oxyl]-phosphate.

[0024] The first phosphate ester may be present in an amount of about 55% to about 75% by weight of the second component or B side. The first phosphate ester may be present in an amount of about 60% to about 70% by weight of the second component or B side. The first phosphate ester may be present in an amount of about 60% by weight of the second component or B side. The first phosphate ester may be present in an amount of about 65% by weight of the second component or B side. The second phosphate ester may be present in an amount of about 15% to about 35% by weight of the second component or B side. The second phosphate ester may be present in an amount of about 20% to about 30% by weight of the second component or B side. The second phosphate ester may be present in an amount of about 25% by weight of the second component or B side. The second phosphate ester may be present in an amount of about 28% by weight of the second component or B side.

[0025] At least one component of the two-component system may include phosphoric acid. It is preferred that the component that includes one or more phosphoric acid esters further includes phosphoric acid. For example, the second component or B-side may include one or more phosphoric acid esters and phosphoric acid. The addition of phosphoric acid to the B-side could result in increased expansion (e.g., foaming) of the resulting reaction product and / or decreased reaction time. The reaction time can be adjusted by the use of concentrations of phosphoric acid. The addition of phosphoric acid to the B-side can increase the reactivity of the system to help maintain a desired level of expansion and hardening when the temperature is below 23°C.

[0026] The phosphoric acid may be orthophosphoric acid. The phosphoric acid may be polyphosphoric acid. The phosphoric acid may be an 85% solution in water. The phosphoric acid may be present in an amount of about 1% to about 10% by weight of the second component or side B. The phosphoric acid may be present in an amount of about 5% to about 8% by weight of the second component or side B.

[0027] Curing and / or foaming may occur at a temperature of less than 40° C. Curing and / or foaming may occur at a temperature of less than 30° C. Curing and / or foaming may occur at a temperature of less than 20° C. Curing and / or foaming may occur at a temperature of about 10° C. to about 35° C. Curing and / or foaming may occur at room temperature (e.g., a temperature of about 15° C. to about 25° C.). Curing and / or foaming may occur at a temperature of about 23° C. Curing and / or foaming may occur at a temperature of about 10° C.

[0028] The present disclosure achieves relatively fast cure and / or foaming times that occur without the addition of a stimulus (e.g., at ambient or room temperature) compared to other curing agent / curing systems. For example, the cure time of the resulting reaction product may be less than 75 minutes. The cure time of the resulting reaction product may be less than 50 minutes. The cure time of the resulting reaction product may be less than 30 minutes, or even less than about 20 minutes. The cure time of the resulting reaction product may be from about 5 minutes to about 20 minutes. The cure time of the resulting reaction product may be about 10 minutes. The cure time of the resulting reaction product may be about 7 minutes. The cure time of the resulting reaction product may be about 5 minutes.

[0029] Foaming will begin prior to full cure of the resulting reaction product. The foaming time of the resulting reaction product may be less than 30 minutes, or even less than about 20 minutes. The foaming time of the resulting reaction product may be from about 30 seconds to about 10 minutes. The foaming time of the resulting reaction product may be about 5 minutes. The foaming time of the resulting reaction product may be about 7 minutes.

[0030] The foam material described herein may further include an epoxy-based material containing one or more epoxy resins. Epoxy resin is used herein to mean any of the conventional dimeric, oligomeric, or polymeric epoxy materials containing at least one epoxy functional group. The term epoxy resin may also be used to describe one or some combination of epoxy resins. The epoxy may be aliphatic, cycloaliphatic, aromatic, etc. The epoxy may be provided as a solid (e.g., as pellets, chunks, strips, etc.) or as a liquid (e.g., as a liquid epoxy resin). As used herein, unless otherwise stated, a resin is a solid resin if it is solid at a temperature of 23° C. and a liquid resin if it is liquid at a temperature of 23° C. At least a portion of the epoxy resin may be a liquid epoxy resin. To use a solid epoxy, it will typically be necessary to dissolve it in a liquid resin.

[0031] The foam material described herein may include a liquid epoxy resin. The liquid epoxy resin may be present as a first component or part of the A-side of the two-component system of the present teachings. The liquid epoxy resin may be a liquid reaction product of epichlorohydrin and bisphenol A. The liquid epoxy resin may have an epoxide equivalent weight (g / eq) of about 82 to about 192 as measured according to ASTM D-1652. The liquid epoxy resin may have an epoxide percentage of about 20 to about 25. The liquid epoxy resin may have a viscosity of 11,000 to 14,000 mPa·s at 25° C. as measured according to ASTM D-445. One suitable liquid epoxy resin is sold under the trade name DER™ 331.

[0032] The liquid epoxy resin may be present in an amount of about 10% to about 30% by weight of the first component or side A. The liquid epoxy resin may be present in an amount of about 15% to about 25% by weight of the first component or side A. The liquid epoxy resin may be present in an amount of about 20% by weight of the first component or side A.

[0033] The foam material described herein may include a flexible epoxy resin. The inclusion of a flexible component may reduce the modulus or increase the strain to failure. The flexible epoxy resin may improve the gas entrapment capabilities of the foam by acting as a viscosity modifier. The flexible epoxy resin may be present in the first component or A-side of the two-component system of the present teachings. The flexible epoxy resin may be a difunctional glycidyl ether epoxy resin. The flexible epoxy resin may be a difunctional epoxy derived from cardanol obtained from cashew nut shell liquid (CNSL). The flexible epoxy resin may have an epoxide equivalent weight (EEW) of about 350 to about 500 according to ASTM D-1652-97. The flexible epoxy resin may have a viscosity of 10,000 to 35,000 cP at 25° C. as measured according to ASTM D2196. One exemplary flexible epoxy resin is sold under the trade name Cardolite NC-514, commercially available from Cardolite Corporation, Monmouth Junction, New Jersey.

[0034] The flexible epoxy resin, when present, may be present in an amount of about 5% to about 25% by weight of the first component or A-side. The flexible epoxy resin may be present in an amount of about 10% to about 20% by weight of the first component or A-side. The flexible epoxy resin may be present in an amount of about 15% by weight of the first component or A-side. The flexible epoxy resin may be present in an amount of at least about 5%, at least about 10%, or even at least about 15% by weight of the first component or A-side. The flexible epoxy resin may be present in an amount less than about 50%, less than about 30%, or even less than about 25% by weight of the first component or A-side.

[0035] The foam material described herein may further include an epoxy phenol novolac resin. The epoxy phenol novolac resin may be present as part of a first component or A-side of a two-component system of the present teachings. The first component or A-side may include a first epoxy phenol novolac resin and a second epoxy phenol novolac resin. The epoxy phenol novolac resin may have an epoxide equivalent weight (g / eq) of about 165 to about 178 as measured according to ASTM D-1652. The epoxy phenol novolac resin may have an epoxide equivalent weight (g / eq) of about 171 to about 183 as measured according to ASTM D-1652. The epoxy phenol novolac resin may have an average epoxy functionality of about 2.6 to about 3.6. For example, the first epoxy phenol novolac resin may have an epoxy functionality of about 2.6 and the second epoxy phenol novolac resin may have an epoxy functionality of about 3.6. The epoxy phenolic novolac resin may have a viscosity of 18,000 to 28,000 cP at 25° C. The epoxy phenolic novolac resin may have a viscosity of 20,000 to 30,000 cP at 52° C. Suitable flexible epoxy resins are sold under the trade names Epalloy 8250 and Epalloy 8330, commercially available from CVC Thermoset Specialties, Inc., Morestown, New Jersey.

[0036] The epoxy phenol novolac resin may be present in an amount of about 1% to about 45% by weight of the first component or A side. The epoxy phenol novolac resin may be present in an amount of about 5% to about 35% by weight of the first component or A side. The epoxy phenol novolac resin may be present in an amount of about 10% to about 20% by weight of the first component or A side. The epoxy phenol novolac resin may be present in an amount of about 15% by weight of the first component or A side. The epoxy phenol novolac resin may be present in an amount of about 35% to about 40% by weight of the first component or A side. The epoxy phenol novolac resin may be present in an amount of at least about 5%, at least about 10%, or even at least about 30% by weight of the first component or A side. The epoxy phenol novolac resin may be present in an amount of less than about 70%, less than about 50%, or even less than about 30% by weight of the first component or A side.

[0037] The foam material may include an aliphatic multifunctional epoxy resin. The aliphatic multifunctional epoxy resin may be present as a first component or part of the A-side of the two-component system of the present teachings. The aliphatic multifunctional epoxy resin may be an epoxidized sorbitol. The aliphatic multifunctional epoxy resin may have an epoxide equivalent weight (g / eq) of about 160 to about 195 as measured according to ASTM D-1652. The aliphatic multifunctional epoxy resin may have a viscosity of 8000-18000 cP at 25° C. One suitable aliphatic multifunctional epoxy resin is sold under the trade name Erisys GE-60, commercially available from CVC Thermoset Specialties, Inc., Morestown, New Jersey.

[0038] The aliphatic multifunctional epoxy resin may be present in an amount of about 15% to about 35% by weight of the first component or side A. The aliphatic multifunctional epoxy resin may be present in an amount of about 20% to about 30% by weight of the first component or side A. The aliphatic multifunctional epoxy resin may be present in an amount of about 20% to about 25% by weight of the first component or side A.

[0039] It is possible that one or more of the A-side components described herein impart additional functionality to the A-side. The B-side may be formed, at least in part, as a salt utilizing at least some of the phosphoric acids and acid esters of the B-side. This essentially reduces the reactive functionality of the B-side. In an effort to compensate for this reduced functionality, the A-side may be formulated with increased functionality by using a functionality higher than 2 to create an infinite network.

[0040] The foam material may include a metal carbonate. The foam material may include calcium carbonate. The calcium carbonate may be present as one or more calcium carbonate fillers and may be derived from a mineral filler having a low metal carbonate concentration. The one or more calcium carbonate fillers may have a median particle size of about 3 microns to about 25 microns. The calcium carbonate may be medium fine ground. For example, the calcium carbonate may have a median particle size of about 22 microns. An example of a suitable medium ground calcium carbonate is Hubercarb® Q200, commercially available from Huber Engineered Material, Atlanta, Georgia. The calcium carbonate may be fine particle size. For example, the calcium carbonate may have a median particle size of 4 microns. An example of a suitable fine particle size calcium carbonate is Hubercarb® Q4, commercially available from Huber Engineered Material, Atlanta, Georgia.

[0041] Calcium carbonate may be present as part of the first component or A side of the two-component system of the present teachings. Calcium carbonate may be present in an amount less than 40% by weight of the first component or A side, between about 10% and about 30% by weight of the first component or A side, or even between about 15% and about 25% by weight of the first component or A side. Calcium carbonate may be present in an amount of about 20% by weight of the first component or A side. Calcium carbonate may be present in an amount of at least about 5% by weight of the first component or A side, at least about 10% by weight of the first component or A side, or even at least about 15% by weight of the first component or A side. Calcium carbonate may be present in an amount less than about 60% by weight of the first component or A side, less than about 45% by weight of the first component or A side, or even less than about 30% by weight of the first component or A side.

[0042] The first component or A-side may comprise about 10% to about 20% by weight medium ground calcium carbonate. The first component or A-side may comprise about 15% by weight medium ground calcium carbonate. The first component or A-side may comprise about 2% to about 9% by weight fine size calcium carbonate. The first component or A-side may comprise about 5% to about 7% by weight fine size calcium carbonate. The first component or A-side may comprise about 15% by weight medium ground calcium carbonate and about 5% by weight fine size calcium carbonate. For example, the ratio of medium ground calcium carbonate to fine size calcium carbonate in the first component or A-side may be about 3:1.

[0043] The calcium carbonate may include a coating or be selected to a particular size (e.g., larger size) in an effort to retard or slow the expansion of the material. The coating may be any material that decomposes during the activation / expansion process. The coating may be a wax, a fatty acid, or a combination thereof.

[0044] The foam material may include one or more minerals. The characteristic external shape of the individual crystals or crystal groups of the mineral may be needle-like or needle-like. The median particle size of the mineral may be about 10 μm to about 20 μm.

[0045] The foam material may include a reinforcing material such as wollastonite or calcium silicate. The wollastonite may be relatively pure CaSiO3. The wollastonite may contain one or more of iron, magnesium, manganese, aluminum, potassium, sodium, or strontium that substitute for calcium in the mineral structure. The wollastonite may have a median particle size of about 18 μm. The wollastonite may have a median particle size of about 12 μm. Suitable wollastonites are sold under the trade names NYGLOS® 12 and NYGLOS® 8, commercially available from NYCO Minerals Inc. of Willsboro, New York.

[0046] Wollastonite may be present as part of the first component or A-side of the two-component system of the present teachings. Wollastonite may be present in an amount of about 1% to about 10% by weight of the first component or A-side. Wollastonite may be present in an amount of about 3% to about 7% by weight of the first component or A-side. Wollastonite may be present in an amount of about 5% by weight of the first component or A-side.

[0047] As yet another means for slowing or retarding the expansion process, inorganic complexes containing metal carbonate concentrations, but not solely comprised of metal carbonate, may be included.

[0048] The foam material may include hydrophobic silica. The hydrophobic silica may be fumed. The fumed silica may be surface treated with polydimethylsiloxane. The hydrophobic silica may be present as part of a first component or A-side of a two-component system of the present teachings. The hydrophobic silica may be present as part of a second component or B-side of a two-component system of the present teachings. The hydrophobic silica may be present as part of both the first component or A-side and the second component or B-side of a two-component system of the present teachings. A suitable hydrophobic silica is sold under the trade name AEROSIL® R202, commercially available from Evonik Corporation, Parsipani, New Jersey.

[0049] The hydrophobic silica may be present in an amount of about 0.25% to about 2% by weight of the first component or A side. The hydrophobic silica may be present in an amount of about 0.5% to about 1.5% by weight of the first component or A side. The hydrophobic silica may be present in an amount of about 1% by weight of the first component or A side. The hydrophobic silica may be present in an amount of about 1% to about 10% by weight of the second component or B side. The hydrophobic silica may be present in an amount of about 1% to about 8% by weight of the second component or B side. The hydrophobic silica may be present in an amount of about 6% by weight of the second component or B side. For example, the ratio of hydrophobic silica in the first component or A side to the second component or B side may be about 1:10 to about 10:1. The ratio of hydrophobic silica in the first component or A side to the second component or B side may be 1:6.

[0050] The foam material may include calcined kaolin clay. Contaminating the clay with metal carbonates may also stimulate the foaming (e.g., expansion) process. Calcined kaolin clay may be present as part of the first component or A-side of the two-component system of the present teachings. Calcined kaolin clay may be present in an amount of about 0.25% to about 5% by weight of the first component or A-side. Calcined kaolin clay may be present in an amount of about 1% by weight of the first component or A-side. Calcined kaolin clay may have an average particle size (average Stokes equivalent diameter) of 1.3 μm. Calcined kaolin clay may have an average particle size (median Malvern laser) of 3.2 μm. A suitable calcined kaolin clay is sold under the trade name KaMin® 70C, commercially available from KaMin® LLC, Macon, Georgia.

[0051] The B-side may include one or more phosphate esters. The B-side may include phosphoric acid. The B-side may include a material to modify viscosity. The material to modify viscosity may be a silica-based material. The one or more phosphate esters may be selected from mono-esters, di-esters, or tri-esters, as shown below. [ka]

[0052] The one or more esters may be combined with the A-side components alone or mixed with the phosphoric acid before being combined with additional components. The resulting reaction of one or more epoxide-functional materials with phosphoric acid is depicted below. [ka] [ka] [ka]

[0053] The viscosity of the A-side at 23° C. may be from about 20,000 cP to about 50,000 cP, or even from about 35,000 cP to 45,000 cP. The viscosity of the A-side at 10° C. may be from about 280,000 cP to about 350,000 cP, or even from about 300,000 cP to about 325,000 cP. The viscosity of the B-side at 23° C. may be from about 20,000 cP to about 50,000 cP, or even from about 35,000 cP to about 45,000 cP. The viscosity of the B-side at 10° C. may be from about 130,00 cP to about 220,000 cP, or even from about 175,000 cP to 195,000 cP.

[0054] In one non-limiting embodiment of the present teachings, the foam material may include in the first component or A-side one or more of the following: liquid epoxy resin, flexible epoxy resin, epoxy phenol novolac resin, aliphatic multifunctional epoxy resin, calcium carbonate, wollastonite, and hydrophobic silica. The foam material may include in the second component or B-side one or more of the following: phosphate ester, hydrophobic silica, and phosphoric acid. In one non-limiting embodiment, the present teachings provide a composition comprising: a) a first component comprising: i) a liquid epoxy resin; ii) a flexible epoxy resin, iii) an epoxy phenolic novolac resin; iv) an aliphatic multifunctional epoxy resin; v) calcium carbonate; vi) wollastonite; and vii) a hydrophobic silica; and b) a second component comprising: i) a first phosphate ester; ii) a second phosphate ester; iii) a hydrophobic silica; and iv) a phosphoric acid, wherein a resulting reaction product of the first component and the second component cures at a temperature less than 50° C.

[0055] The foam material may include one or more additives (e.g., functional additives) to improve one or more various properties of the composition. By way of example, the additives may include antioxidants, antiozonants, UV absorbers, antistatic agents, colorants, coupling agents, curing agents, flame retardants, foaming agents, heat stabilizers, impact modifiers, lubricants, plasticizers, preservatives, processing aids, and stabilizers, as well as combinations thereof.

[0056] Certain non-limiting example formulations according to the present teachings are provided in Table 1 below.

[0057] [Table 1]

[0058] Table 2 provides technical data for formulations according to the present teachings at cure temperatures of 23°C and 10°C.

[0059] [Table 2]

[0060] Additional examples of formulations according to the present teachings are provided in Table 3 below.

[0061] [Table 3]

[0062] As depicted in Table 3, the addition of 85% phosphoric acid to the B side results in increased expansion and helps maintain the desired expansion level when the temperature is below 23°C.

[0063] The two-component systems of the present teachings may be provided as side-by-side cartridges, pails, and drums. The resulting reaction product of the two components cures at temperatures below 50° C., providing excellent adhesion to many substrates as well as fast cure times.

[0064] Use of the teachings herein may result in materials that exhibit sufficient flame retardancy to meet one or more of the requirements for demonstrating flame retardancy (e.g., meet vertical burn and / or smoke density requirements (or any other requirements)) set forth in 14 C.FR 25.853 and 14 C.FR 25.856 (U.S. Department of Transportation Code of Federal Regulations for Passenger Cabin Interiors, including but not limited to 14 C.FR 25.853(a) and reference Appendix F and the procedures referenced therein), all of which are incorporated herein by reference for all purposes.

[0065] As used herein, unless otherwise stated, the teachings contemplate that any member of a genus (list) may be excluded from the genus and / or any member of a Markush grouping may be excluded from the grouping.

[0066] Unless otherwise stated, any numerical value described herein includes all values ​​from the lower value to the upper value in increments of one unit, provided that there is a separation of at least two units between any lower value and any upper value. As an example, if an amount of an ingredient, a property, or a value of a process variable, such as temperature, pressure, time, etc., is stated to be, for example, 1 to 90, preferably 20 to 80, more preferably 30 to 70, the intermediate range values ​​(e.g., 15 to 85, 22 to 68, 43 to 51, 30 to 32, etc.) are intended to be within the scope of the teachings herein. Similarly, each intermediate value is also within the scope of the teachings. For values ​​less than one, one unit is considered to be 0.0001, 0.001, 0.01, or 0.1 accordingly. These are merely examples of what is specifically intended, and all possible combinations of numerical values ​​between the lowest and highest values ​​listed are considered to be expressly stated in the same manner within the present application. As can be seen, teachings of amounts expressed as "parts by weight" herein also contemplate the same ranges being expressed in terms of weight percent. Thus, a range expression such as "at least 'x' parts by weight of the resulting composition" also contemplates teachings of a range in weight percent of the resulting composition for the same recited amount "x."

[0067] Unless otherwise stated, all ranges include both endpoints and all numbers between the endpoints. The use of "about" or "approximately" in connection with a range applies to both ends of the range. Thus, "about 20 to 30" is intended to cover "about 20 to about 30," including at least the specified endpoint. Unless otherwise stated, teachings using the term "about" or "approximately" in combination with a numerical quantity encompass teachings of the recited amount as well as approximations of the recited amount. As an example, a teaching of "about 100" encompasses the teaching of "100."

[0068] The disclosures of all articles and references, including patent applications and patent publications, are incorporated by reference for all purposes. The term "consisting essentially of" to describe a combination is intended to include the identified elements, ingredients, components, or steps, as well as such other elements, ingredients, components, or steps that do not materially affect the basic and novel characteristics of the combination. The use of the terms "comprising" or "including" to describe a combination of elements, ingredients, components, or steps herein also contemplates embodiments that consist of or consist essentially of the elements, ingredients, components, or steps in question.

[0069] A plurality of elements, ingredients, components, or steps may be provided by a single integrated element, ingredient, component, or step. Alternatively, a single integrated element, ingredient, component, or step may be divided into separate elements, ingredients, components, or steps. The disclosure of "a" or "one" to describe an element, ingredient, component, or step is not intended to exclude additional elements, ingredients, components, or steps.

[0070] For example, embodiments of the present invention are as follows. [Embodiment 1] providing a two-component system, the two-component system comprising an A side and a B side, the A side comprising an epoxy and the B side comprising a phosphate ester and phosphoric acid; mixing said A-side and said B-side to form a resultant reaction product; A method comprising: a method wherein the resulting reaction product of said A-side and said B-side cures at a temperature less than 50°C.

[0071] [Embodiment 2] 2. The method of embodiment 1, wherein said side B comprises two different phosphate esters. [Embodiment 3] 3. The method of claim 1 or claim 2, wherein the A-side, the B-side, or both, comprise a filler. [Embodiment 4] 4. The method of any one of the preceding claims, wherein the A-side comprises calcium carbonate. [Embodiment 5] 5. The method of any one of the preceding claims, wherein curing occurs at a temperature of about 10° C. to about 35° C.

[0072] [Embodiment 6] 6. The method of any one of the preceding claims, wherein curing occurs at a temperature of about 15°C to about 25°C. [Embodiment 7] 7. The method of any one of the preceding claims, wherein the resulting reaction product has a cure time of less than 15 minutes. [Embodiment 8] 8. The method of any one of the preceding claims, wherein the curing time of the resulting reaction product is from about 5 minutes to about 10 minutes.

[0073] [Embodiment 9] 9. The method of any one of the preceding claims, wherein the method does not include a curing agent. [Embodiment 10] 10. The method of any one of the preceding claims, wherein the resulting reaction product has a volume expansion of at least 200%. [Embodiment 11] 11. The method of any one of the preceding claims, wherein the phosphoric acid is added after preparation of the phosphate ester.

[0074] [Embodiment 12] 12. The method of any one of the preceding claims, wherein the A-side and the B-side are mixed in a volumetric mix ratio of about 1:4 to about 4:1 (A-side:B-side). [Embodiment 13] 13. The method of any one of the preceding claims, wherein the A-side and the B-side are mixed in a volumetric mix ratio of about 2:1 (A-side:B-side). [Embodiment 14] 14. The method of any one of the preceding claims, wherein the reaction product is fully expanded in less than 10 minutes, less than 5 minutes, or even less than 2 minutes.

[0075] [Embodiment 15] 15. The method of any one of the preceding claims, wherein the method further comprises adding a second amount of phosphoric acid. [Embodiment 16] 16. The method of any one of the preceding claims, wherein the viscosity of the A-side at 23°C is from about 20,000 cP to about 50,000 cP. [Embodiment 17] 17. The method of any one of the preceding claims, wherein the viscosity of the A-side at 23°C is from about 35,000 cP to about 45,000 cP.

[0076] [Embodiment 18] 18. The method of any one of the preceding claims, wherein the A-side is formulated with increasing functionality to create an infinite network by using a functionality higher than 2. [Embodiment 19] 1. A composition comprising: a) a first component comprising an epoxy; b) a second component comprising a phosphate ester and phosphoric acid; A composition, wherein the resulting reaction product of said first component and said second component cures at a temperature less than 50°C.

[0077] [Embodiment 20] 20. The composition of embodiment 19, wherein the second component comprises at least two different phosphate esters. [Embodiment 21] 21. The composition of embodiment 19 or embodiment 20, wherein the first component, the second component, or both, comprise a filler. [Embodiment 22]

[0036] Embodiment 22. The composition of any one of embodiments 19 to 21, wherein the first component comprises calcium carbonate.

[0078] [Embodiment 23] 23. The composition of any one of embodiments 19 to 22, wherein the curing temperature is from about 10° C. to about 35° C. [Embodiment 24] 24. The composition of any one of embodiments 19 to 23, wherein the curing temperature is from about 15° C. to about 25° C. [Embodiment 25] 25. The composition of any one of claims 19 to 24, wherein the resulting reaction product has a cure time of less than 15 minutes.

[0079] [Embodiment 26] 26. The composition of any one of embodiments 19 to 25, wherein the cure time of the resulting reaction product is about 5 minutes to about 10 minutes. [Embodiment 27]

[0041] Embodiment 27. The composition of any one of embodiments 19 to 26, wherein the resulting reaction product has a volume expansion of at least 200%. [Embodiment 28] 28. The composition of any one of embodiments 19 to 27, wherein the A side and the B side are in a volumetric mix ratio of about 1:4 to about 4:1 (A side:B side).

[0080] [Embodiment 29] 29. The composition of any one of embodiments 19 to 28, wherein the A-side and the B-side are in a volumetric mix ratio of about 2:1 (A-side:B-side). [Embodiment 30] 30. The composition of any one of embodiments 19 to 29, wherein the reaction product is fully expanded in less than 10 minutes, less than 5 minutes, or even less than 2 minutes. [Embodiment 31] The composition of any one of embodiments 19 to 30, comprising a second amount of phosphoric acid.

[0081] [Embodiment 32] Embodiment 32. The composition of any one of embodiments 19 to 31, wherein the viscosity of the A-side at 23° C. is from about 20,000 cP to about 50,000 cP. [Embodiment 33] Embodiment 33. The composition of any one of embodiments 19 to 32, wherein the viscosity of the A-side at 23° C. is about 35,000 cP to about 45,000 cP. [Embodiment 34]

[0036] Embodiment 34. The composition of any one of embodiments 19 to 33, wherein the A-side is formulated with increasing functionality to create an infinite network by using a functionality higher than 2.

[0082] [Embodiment 35] A composition comprising: a) a first component, i) liquid epoxy resin, ii) a flexible epoxy resin; iii) epoxy phenol novolac resins; iv) Aliphatic multifunctional epoxy resins v) calcium carbonate, vi) Wollastonite vii) a first component comprising a hydrophobic silica; b) a second component, i) a first phosphate ester, ii) a second phosphate ester; iii) Hydrophobic Silica iv) a second component comprising phosphoric acid; A composition, wherein the resulting reaction product of said first component and said second component cures at a temperature less than 50°C.

[0083] It is understood that the above description is illustrative and not intended to be limiting. Many embodiments other than the examples provided, as well as many applications, will become apparent to those skilled in the art upon reading the above description. Therefore, the scope of the present invention should not be determined with reference to the above description, but instead with reference to the appended claims and the full scope of equivalents to which such claims are entitled. The disclosures of all articles and references, including patent applications and patent publications, are incorporated by reference for all purposes. The omission of any aspect of the subject matter disclosed herein in the appended claims should not be construed as a disclaimer of such subject matter, nor as a failure by the inventors to acknowledge such subject matter as part of the subject matter of the disclosed invention.

Claims

1. providing a two-component system, the two-component system comprising an A-side and a B-side, the A-side comprising an epoxy, the B-side comprising a phosphate ester, and phosphoric acid, the A-side and the B-side being free of a blowing agent; mixing said A-side and said B-side to form a resultant reaction product; It is equipped with wherein the resulting reaction product of the A-side and the B-side cures at a temperature less than 50° C. and has a volume expansion of at least 200%, the B side comprises two different phosphate esters, a first phosphate ester and a second phosphate ester; the B side comprises about 55% to about 75% by weight of the first phosphate ester, about 15% to about 35% by weight of the second phosphate ester, and about 1% to about 10% by weight of the phosphoric acid.

2. The method of claim 1 , wherein the A-side, the B-side, or both, include a filler material.

3. 3. The method of claim 1 or claim 2, wherein the A-side comprises calcium carbonate.

4. 3. The method of claim 1 or claim 2, wherein curing occurs at a temperature of from about 10° C. to about 35° C.

5. 3. The method of claim 1 or claim 2, wherein curing occurs at a temperature of about 15°C to about 25°C.

6. 3. The method of claim 1 or claim 2, wherein the resulting reaction product has a cure time of less than 15 minutes.

7. 3. The method of claim 1 or claim 2, wherein the cure time of the resulting reaction product is from about 5 minutes to about 10 minutes.

8. The method of claim 1 or claim 2, wherein the method does not include a curing agent.

9. 3. The method of claim 1 or claim 2, wherein the A-side and the B-side are mixed in a volumetric mix ratio of about 1:4 to about 4:1 (A-side:B-side).

10. 3. The method of claim 1 or claim 2, wherein the A-side and the B-side are mixed in a volumetric mix ratio of about 2:1 (A-side:B-side).

11. 3. The method of claim 1 or claim 2, wherein the reaction product is fully expanded in less than 10 minutes, less than 5 minutes, or even less than 2 minutes.

12. 3. The method of claim 1 or claim 2, wherein the viscosity of the A-side at 23° C. is from about 20,000 cP to about 50,000 cP.

13. 3. The method of claim 1 or claim 2, wherein the viscosity of the A-side at 23° C. is from about 35,000 cP to about 45,000 cP.

14. 3. The method of claim 1 or claim 2, wherein the A-side is formulated with increasing functionality to create an infinite network by using a functionality higher than 2.

Citation Information

Patent Citations

  • Epoxy resin foam and its production

    JP1997227709A

  • Production of epoxy resin foam

    JP1998101836A

  • Preparatio of epoxy resin foam

    JP2001081223A

  • Esterified acids for use in polymeric materials

    US20180037695A1

  • Esterified acids for use in polymeric materials

    WO2016149700A1