Polylactic acid-based resin composition

A polylactic acid resin composition with layered silicate filler and acrylic thermoplastic elastomer enhances fluidity and molding cycleability, addressing slow crystallization and melt fluidity issues in PLA, achieving efficient and stable injection molding.

JP2024167547AInactive Publication Date: 2024-12-04NAGASE & CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023083697
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polylactic acid (PLA) resins exhibit slow crystallization speed during injection molding, leading to insufficient crystallization, instability in rigidity and thermal deformation temperature, and lack of melt fluidity, resulting in issues like short shots in thin-walled products and poor molding cycleability.

Method used

A polylactic acid resin composition comprising polylactic acid resin, layered silicate filler, acrylic thermoplastic elastomer, and optionally aliphatic or aliphatic aromatic polyester elastomer, with specific ratios and additives for improved fluidity and molding cycleability, using melt-kneading to achieve high filler concentration.

Benefits of technology

The composition achieves excellent fluidity, fast crystallization, good mold releasability, and balanced mechanical and thermal properties, enabling short molding cycles and continuous production with improved rigidity, heat resistance, and impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167547000001
    Figure 2024167547000001
  • Figure 2024167547000002
    Figure 2024167547000002
  • Figure 2024167547000003
    Figure 2024167547000003
Patent Text Reader

Abstract

To provide a resin composition which is excellent in fluidity and molding cyclability and uses a polylactic acid-based resin as a base resin.SOLUTION: The polylactic acid-based resin composition of the present invention contains: 15-87 mass% of a polylactic acid-based resin (A); 10-55 mass% of a layered silicate-based filler (B); 3-15 mass% of an acrylic thermoplastic elastomer (C); and 0-40 mass% of at least one polyester elastomer (D) selected from aliphatic polyester elastomers and aliphatic-aromatic polyester elastomers. The contents (mass%) are based on the total amount of the composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polylactic acid resin composition. [Background technology]

[0002] Polylactic acid (PLA) is a plant-derived aliphatic polyester made from starch, and has been attracting attention as a biodegradable plastic made from non-petroleum-based raw materials. For example, Patent Document 1 describes a biodegradable resin composition containing a biodegradable resin, an inorganic filler, and a flowability modifier having a high acid value. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 7228110 Summary of the Invention [Problem to be solved by the invention]

[0004] However, because PLA has a slow crystallization rate, especially when trying to obtain products by injection molding, the molten resin does not crystallize sufficiently in a short time inside the mold, and molded products with insufficient crystallization have problems such as unstable rigidity and heat distortion temperature. In addition, PLA often has a problem with insufficient melt fluidity during injection molding, which causes short shots (incomplete filling of a part of a molded product) in thin-walled molded products. For this reason, there is a demand for resin materials based on polylactic acid (PLA) resins with improved "fluidity" and "molding cycle performance" to facilitate injection molding. In addition, it is also desired that the resin material be able to obtain molded products with excellent rigidity, heat resistance, impact resistance, and dimensional stability, and it is also desired that not only the moldability of the resin material but also the ease of controlling the balance of physical properties of the resulting molded product (high degree of design freedom) be achieved.

[0005] As described above, Patent Document 1 discloses a resin composition containing a biodegradable resin, an inorganic filler, and a flowability modifier having a high acid value. However, the document only describes the improvement of flowability and makes no mention of molding cycle properties.

[0006] Resin materials for injection molding are desired to have "fluidity" and "high cycle performance." "Fluidity" is necessary to obtain molded products with complex shapes and thin walls. "High cycle performance" refers to a short unit time from the start of injection molding to the end of removing the molded product from the mold, which leads to improved productivity.

[0007] An object of the present invention is to provide a resin composition having excellent flowability and molding cycle properties, the resin composition containing a polylactic acid resin as a base resin. [Means for solving the problem]

[0008] In the present invention, by combining a polylactic acid-based resin as a base resin with a layered silicate-based filler and an acrylic thermoplastic elastomer, and, as necessary, an aliphatic polyester elastomer and / or an aliphatic aromatic polyester elastomer, we have discovered a polylactic acid-based resin composition that has high fluidity and excellent molding cycle properties (high cycle properties) in injection molding, and whose rigidity, heat resistance, impact resistance, etc. can be widely designed depending on the application and purpose.

[0009] Furthermore, as an effective means for producing the polylactic acid-based resin composition of the present invention, the layered silicate-based filler is first made into a specific powder granule, and then this powder granule is melt-kneaded with a polylactic acid-based resin, thereby making it possible to melt-knead and compound the polylactic acid-based resin composition of the present invention having a high filler concentration at a high production speed.

[0010] Thus, an embodiment of the present invention is as follows. (1) 15% by mass to 87% by mass of a polylactic acid-based resin (A), 10% by mass to 55% by mass of a layered silicate-based filler (B); 3% by mass to 15% by mass of an acrylic thermoplastic elastomer (C), and 0% to 40% by mass of at least one polyester elastomer (D) selected from aliphatic polyester elastomers and aliphatic aromatic polyester elastomers The content (mass %) is based on the total amount of the composition. (2) The polylactic acid resin composition according to (1), wherein the polylactic acid resin (A) has a weight average molecular weight of 100,000 to 150,000. (3) The polylactic acid resin composition according to (1) or (2), wherein the layered silicate filler (B) is at least one selected from the group consisting of talc and mica. (4) The polylactic acid resin composition according to any one of (1) to (3), wherein the acrylic thermoplastic elastomer (C) is a polymethyl methacrylate (PMMA)-butyl acrylate (BA) block copolymer. (5) The polylactic acid resin composition according to any one of (1) to (4), wherein the amount of the PMMA block component of the polymethyl methacrylate (PMMA)-butyl acrylate (BA) block copolymer is 20% by mass to 30% by mass. (6) The polylactic acid resin composition according to any one of (1) to (5), wherein the polyester elastomer (D) is a polybutylene adipate terephthalate (PBAT) resin. (7) The polylactic acid resin composition according to any one of (1) to (6), further comprising 0.1% by mass to 5% by mass of a filler dispersing agent (E). (8) The polylactic acid resin composition according to any one of (1) to (7), further comprising 0.1% by mass to 5% by mass of a polymer for dispersing fillers (F). (9) A method for producing the polylactic acid resin composition according to any one of (1) to (8), comprising the steps of: The polylactic acid-based resin composition contains 0.1% by mass to 5% by mass of a filler dispersant (E) and / or 0.1% by mass to 5% by mass of a filler dispersing polymer (F), The method includes a step of melt-kneading a polylactic acid-based resin (A), a filler granule containing a layered silicate-based filler (B), and an acrylic thermoplastic elastomer (C), The filler granules contain a layered silicate-based filler (B), a filler dispersant (E), and a filler dispersion polymer (F), The production method, wherein the content of the layered silicate-based filler (B) in the filler granules is 80 parts by mass to 99.9 parts by mass per 100 parts by mass of the total amount of all solids in the filler granules. (10) A molded product obtained by using the polylactic acid resin composition according to any one of (1) to (8). Effect of the Invention

[0011] According to the present invention, there can be provided a resin composition having a polylactic acid-based resin as a base resin, which has excellent flowability and molding cycle properties. The resin composition of the present invention is particularly useful as an injection molding material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] A. Polylactic acid resin composition A-1. Overview of polylactic acid resin composition The polylactic acid resin composition of the present invention contains a polylactic acid resin (A), a layered silicate filler (B), an acrylic thermoplastic elastomer (C), and, as necessary, at least one polyester elastomer (D) selected from an aliphatic polyester elastomer and an aliphatic aromatic polyester elastomer.

[0013] The polylactic acid resin composition may further contain a filler dispersing agent (E) and / or a filler dispersing polymer (F).

[0014] The polylactic acid-based resin composition of the present invention is a polylactic acid-based resin composition comprising 15% by mass to 87% by mass of a polylactic acid-based resin (A), 10% by mass to 55% by mass of a layered silicate-based filler (B), 3% by mass to 15% by mass of an acrylic thermoplastic elastomer (C), and 0% by mass to 40% by mass of at least one polyester elastomer (D) selected from an aliphatic polyester elastomer and an aliphatic aromatic polyester elastomer, the contents (% by mass) being based on the total amount of the composition.

[0015] The polylactic acid resin composition of the present invention has high fluidity and excellent molding cycle properties, even though it is mainly composed of polylactic acid resin. Furthermore, a molded article (product) obtained by using the polylactic acid resin composition of the present invention can have high levels of well-balanced mechanical and thermal properties such as rigidity, heat resistance (heat distortion temperature resistance), impact resistance, and dimensional stability (low molding shrinkage, low linear expansion coefficient, and low warpage).

[0016] In particular, when the molded product is an injection molded product, it is necessary to solidify the resin in the mold within a short period of time, and therefore crystallizing the polylactic acid within a short period of time is an important issue in shortening the molding cycle.

[0017] Furthermore, if the molded product sticks to the molding die when it is removed and has poor releasability, this will result in an increase in the molding cycle, so good "mold release" or, in other words, good "releasability" is also important.

[0018] The polylactic acid resin composition of the present invention exhibits the effects of "good fluidity," "fast crystallization rate," and "good releasability from a mold," and can shorten the molding cycle.

[0019] In one embodiment, the polylactic acid resin composition of the present invention can achieve a molding cycle in which, as an index for judging its molding cycle property in injection molding, when a dumbbell-shaped test piece for bending test (Type 1A multipurpose test piece) conforming to ISO 178 is injection molded, the cooling time required to remove the molded piece from the mold at a mold temperature of 90°C is 120 seconds or less, based on the number of seconds of cooling time required to remove the molded piece and the releasability of the molded article from the mold, and the composition can achieve a molding cycle that enables continuous molding.

[0020] Furthermore, by the above evaluation method, the cooling time can be reduced to 90 seconds or less, and a molding cycle that allows continuous molding can be achieved.

[0021] Furthermore, by the above evaluation method, the cooling time can be taken out within 60 seconds, and a molding cycle that allows continuous molding can be achieved.

[0022] Moreover, the polylactic acid resin composition is excellent in appearance and colorability (ability to be colored in bright colors).

[0023] The polylactic acid resin composition of the present invention can be preferably obtained, for example, by producing a filler granule containing a layered silicate filler (B) and at least one selected from a filler dispersant (E) and a filler dispersion polymer (F), and then mixing the filler granule with a polylactic acid resin (A) and an acrylic thermoplastic elastomer (C) (for example, by melt kneading). By adopting such a production method, the workability of adding the filler and the filler dispersibility are significantly improved, and it becomes possible to incorporate a high content of the filler.

[0024] A-2. Polylactic acid resin (component A) The polylactic acid resin composition of the present invention contains a polylactic acid resin (A).

[0025] The polylactic acid resin (A) is not particularly limited, and any polylactic acid resin can be used as long as it is a polymer containing a structural unit derived from lactic acid. Polylactic acid resins can have the same stability as synthetic resins under normal use conditions (normal temperature and normal humidity), but when placed in an environment with moderate moisture and temperature, such as in compost or soil after use, hydrolysis is promoted, and then decomposition (biodegradation) by microorganisms progresses, and finally decomposition into carbon dioxide and water.

[0026] The polylactic acid resin (A) may be a polylactic acid (homopolymer) or a copolymer containing a structural unit derived from lactic acid. In one embodiment, the polylactic acid resin (A) may be a copolymer of lactic acid and a hydroxycarboxylic acid. Examples of the hydroxycarboxylic acid include glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 4-hydroxyvaleric acid, 5-hydroxyvaleric acid, and 6-hydroxycaproic acid. From the viewpoint of a high melting point, a polylactic acid resin having a high L-lactic acid ratio is preferably used as the polylactic acid resin (A). The L-lactic acid ratio of the polylactic acid resin is preferably 96% or more, more preferably 98% or more, and even more preferably 98.6% or more. The polylactic acid resin (A) may be used alone or in combination of two or more.

[0027] The weight average molecular weight of the polylactic acid resin (A) varies depending on the molding method, shape and application of the target molded article, but in the case of injection molding, from the viewpoint of melt fluidity, the weight average molecular weight is preferably 80,000 to 200,000, more preferably 100,000 to 180,000, even more preferably 100,000 to 150,000, and most preferably 120,000 to 150,000.

[0028] The content of the polylactic acid resin (A) is 15% by mass to 87% by mass based on the total amount of the composition in the polylactic acid resin composition. By making the content of the polylactic acid resin (A) 15% by mass or more, an effective amount as a base resin can be contained in the composition. By making the content of the polylactic acid resin (A) 87% by mass or less, the component amounts with other components such as the layered silicate filler (B) and the acrylic thermoplastic elastomer (C) can be balanced, and a resin composition having desired properties can be obtained. The content of the polylactic acid resin (A) is preferably 20% by mass to 80% by mass, and more preferably 25% by mass to 70% by mass.

[0029] A-3. Layered silicate filler (ingredient B) The polylactic acid resin composition of the present invention contains a layered silicate filler (B).

[0030] The layered silicate filler (B), also called phyllosilicate, is a mineral having the property of easily peeling off in parallel thin pieces (wall cleavage). The layered silicate filler (B) used in the present invention is not particularly limited, but examples thereof include kaolinite, halloysite, talc, pyrophyllite, smectite, vermiculite, mica, and chlorite. Among these, talc and / or mica are particularly preferably used. The layered silicate filler (B) may be used alone or in combination of two or more types. The layered silicate filler (B) can function as a crystallization nucleating agent that promotes the crystallization of the polylactic acid resin (A), and can also improve the rigidity and heat distortion temperature of the molded article obtained from the resin composition, thereby shortening the molding cycle. The layered silicate filler (B) can also function as a release agent that easily releases the molded article from the mold.

[0031] The content of the layered silicate filler (B) is 10% by mass to 55% by mass based on the total amount of the polylactic acid resin composition (100% by mass). By making the content of the layered silicate filler (B) 10% by mass or more, the molding cycle property of the polylactic acid resin composition can be effectively improved. In addition, by making the content of the layered silicate filler (B) 55% by mass or less, excessive decrease in the fluidity of the polylactic acid resin composition can be avoided. Preferably, by blending talc and / or mica at a high concentration of 10% by mass to 55% by mass, it is advantageous in that the crystallization rate and crystallization degree of the polylactic acid resin can be increased. The content of the layered silicate filler (B) is preferably 15% by mass to 52% by mass, preferably 20% by mass to 50% by mass. Within such a range, the effects of excellent rigidity, dimensional stability, heat resistance, and excellent molding cycle are preferably remarkable.

[0032] The average particle size of the layered silicate filler (B) may be any suitable particle size. The average particle size of the layered silicate filler (B) is preferably 0.1 μm to 40 μm, more preferably 0.5 μm to 10 μm, and even more preferably 1 μm to 8 μm. When the layered silicate filler (B) functions as a crystallization nucleating agent, the smaller the particle size of the filler, the greater the contact area with the resin per blend amount, and the more preferable it is for bringing out the effect of the crystallization nucleating agent. The average particle size of the layered silicate filler can be determined, for example, by a laser diffraction method. The average particle size of the layered silicate filler may be the particle size (d50) at 50% cumulative in the cumulative particle size distribution on a volume basis.

[0033] A-4. Acrylic thermoplastic elastomer (component C) The polylactic acid resin composition of the present invention contains an acrylic thermoplastic elastomer (C).

[0034] The acrylic thermoplastic elastomer (C) refers to a polymer having elastomeric properties and constituted from at least one (meth)acrylic monomer.

[0035] The acrylic thermoplastic elastomer (C) can function as a flowability modifier. The use of the acrylic thermoplastic elastomer (C) can improve the flowability while maintaining the effect of improving the crystallization rate of the polylactic acid resin by the layered silicate filler (B) at a high level, compared to the use of other flowability modifiers, and therefore can be particularly advantageous for achieving high cycle performance.

[0036] The content of the acrylic thermoplastic elastomer (C) is 3% by mass to 15% by mass based on the total amount of the polylactic acid resin composition (100% by mass). By making the content of the acrylic thermoplastic elastomer (C) 3% by mass or more, the flowability improving effect can be exhibited well. In addition, by making the content of the acrylic thermoplastic elastomer (C) 15% by mass or less, it is possible to obtain a resin composition that can express desired properties in a well-balanced manner by adjusting the component amounts of other components such as the polylactic acid resin (A) and the layered silicate filler (B). The content of the acrylic thermoplastic elastomer (C) is preferably 4% by mass to 12% by mass, and more preferably 5% by mass to 10% by mass.

[0037] The acrylic thermoplastic elastomer (C) is preferably a block copolymer having a hard segment having a glass transition temperature of room temperature (23° C.) or higher and a soft segment having flexibility.

[0038] In the block copolymer of the acrylic thermoplastic elastomer (C), the glass transition temperature based on the hard segment is preferably 25°C or higher, preferably 30°C or higher, preferably 40°C or higher, preferably 50°C or higher, and on the other hand, preferably 200°C or lower, more preferably 180°C or lower, and even more preferably 150°C or lower. The above-mentioned range of glass transition temperature is preferable from the viewpoint of heat resistance, moldability, etc. The glass transition temperature of the acrylic thermoplastic elastomer (C) is the peak temperature of the loss tangent (tan δ) observed when a test piece is heated by a dynamic viscoelasticity measuring device under the conditions of a temperature range of -100 to 280°C, a heating rate of 5°C / min, and a frequency of 10Hz. In a thermoplastic elastomer having multiple blocks, multiple loss tangent peaks are usually observed, but in this case, the peak on the low temperature side is derived from the soft segment, and the peak on the high temperature side is derived from the hard segment.

[0039] The hard segment of the acrylic thermoplastic elastomer (C) is preferably a polymer block obtained from at least one of the following (meth)acrylic monomers. Examples of the (meth)acrylic monomers used in the hard segment include methyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, phenyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, glycidyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and phenoxyethyl (meth)acrylate. Among these, methyl methacrylate, ethyl methacrylate, and butyl methacrylate are preferred, and methyl methacrylate is particularly preferred. The hard segment is particularly preferably a polymer block of methyl methacrylate.

[0040] The soft segment of the acrylic thermoplastic elastomer (C) is preferably a polymer block obtained from at least one of the following (meth)acrylic monomers. Examples of the (meth)acrylic monomers used in the soft segment include n-propyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, n-hexyl (meth)acrylate, ethylhexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, and phenylethyl (meth)acrylate. Among these, n-propyl acrylate, n-butyl acrylate, sec-butyl acrylate, n-hexyl acrylate, ethylhexyl acrylate, n-heptyl acrylate, n-octyl acrylate, and phenylethyl acrylate are preferred, and n-butyl acrylate is particularly preferred. The soft segment is particularly preferably a polymer block of n-butyl acrylate.

[0041] The mass ratio of the hard segment to the soft segment in the acrylic thermoplastic elastomer (C) ([mass of hard segment] / [mass of soft segment]) is preferably from 10 / 90 to 70 / 30, and more preferably from 15 / 85 to 60 / 40.

[0042] The weight average molecular weight (Mw) of the acrylic thermoplastic elastomer (C) is preferably 10,000 or more, more preferably 20,000 or more, more preferably 30,000 or more, and even more preferably 40,000 or more, while it is preferably 600,000 or less, more preferably 400,000 or less, and even more preferably 200,000 or less. The ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the acrylic thermoplastic elastomer (C), i.e., the molecular weight distribution (Mw / Mn), is usually 1.1 to 5.0, and preferably 1.1 to 3.0.

[0043] Here, the weight average molecular weight (Mw) and the number average molecular weight (Mn) can be measured by gel permeation chromatography (GPC) under the following conditions. Equipment: Tosoh HLC-8120 Column: Inertsil WF300 Solvent: Tetrahydrofuran Calibration: Polystyrene

[0044] The acrylic thermoplastic elastomer (C) is commercially available, and may be selected from, for example, the "Clarity (registered trademark)" series manufactured by Kuraray Co., Ltd. and the "Nanostrength (registered trademark)" manufactured by Arkema.

[0045] The acrylic thermoplastic elastomer (C) may be used alone or in combination of two or more kinds. For example, the acrylic thermoplastic elastomer (C) may be used in combination of two or more kinds having different compositions, physical properties, etc. of the hard segment or soft segment.

[0046] In one embodiment, as the acrylic thermoplastic elastomer (C), a block copolymer (hereinafter sometimes referred to as "PMMA-BA block copolymer") having two or more polymerized blocks (glass transition temperature 100°C to 120°C) mainly made of polymethyl methacrylate (PMMA) as hard segments in its structure, and a polymerized block (glass transition temperature -40°C to -50°C) mainly made of n-butyl acrylate (BA) as a soft segment between the hard segments (hereinafter sometimes referred to as "PMMA-BA block copolymer") can be preferably used. In one embodiment, a block copolymer (hereinafter sometimes referred to as "PMMA-BA block copolymer") having two or more polymerized blocks (glass transition temperature 100°C to 120°C) mainly made of polymethyl methacrylate (PMMA) obtained by living anionic polymerization method as hard segments in its structure, and a polymerized block (glass transition temperature -40°C to -50°C) mainly made of n-butyl acrylate (BA) as a soft segment between the hard segments (hereinafter sometimes referred to as "PMMA-BA block copolymer").

[0047] The hard segment exhibits high compatibility with polylactic acid resin, and therefore can improve the melt flowability of the polylactic acid resin, and can also disperse well in the PLA phase, improving impact resistance. The hard segment has a high glass transition temperature, and therefore can suppress the decrease in heat distortion temperature of the polylactic acid resin composition. This allows the heat distortion temperature to be maintained at a high temperature while improving the flowability of the polylactic acid resin composition. Such an effect is favorable for improving the releasability of the molded product from the mold.

[0048] The weight average molecular weight (Mw) of the PMMA-BA block copolymer is preferably 10,000 to 200,000, more preferably 20,000 to 150,000, further preferably 30,000 to 120,000, and particularly preferably 50,000 to 100,000. Within this range, the effects of the present invention can be effectively exhibited.

[0049] The ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn), ie, the molecular weight distribution (Mw / Mn) is usually 1.1 to 1.3, and preferably 1.1 to 1.2.

[0050] Here, the weight average molecular weight (Mw) and (Mw / Mn) can be measured by the above-mentioned gel permeation chromatography method (GPC method).

[0051] The content of the hard segment mainly composed of PMMA is preferably 15% by mass to 40% by mass, more preferably 18% by mass to 35% by mass, and even more preferably 20% by mass to 30% by mass, as the total amount of two or more hard segment blocks. If it is within this range, it is easy to effectively increase impact resistance, melt fluidity, and high cycle property while maintaining rigidity and heat resistance.

[0052] The proportion of PMMA blocks in the block copolymer can be determined by proton-NMR (proton nuclear magnetic resonance) measurement. Equipment: JEOL nuclear magnetic resonance equipment "JNM-LA400" Heavy solvent: Deuterated chloroform

[0053] The PMMA-BA block copolymer is available as "CLARITY (registered trademark)" manufactured and sold by Kuraray Co., Ltd.

[0054] A-5. Aliphatic polyester elastomer and / or aliphatic aromatic polyester elastomer (component D) The polylactic acid resin composition of the present invention may contain at least one polyester elastomer (D) selected from an aliphatic polyester elastomer and an aliphatic aromatic polyester elastomer.

[0055] In the present invention, an aliphatic polyester elastomer and / or an aliphatic aromatic polyester elastomer can be used to compensate for the brittleness, embrittlement, notch sensitivity and crack propagation of polylactic acid-based resins and improve impact strength.

[0056] The aliphatic polyester elastomer is an aliphatic polyester having elastomeric properties, excluding polylactic acid resins, and the aliphatic aromatic polyester elastomer is an aliphatic aromatic polyester having elastomeric properties.

[0057] Examples of the aliphatic polyester elastomer include aliphatic polyesters obtained by polycondensation reaction of aliphatic diols and aliphatic dicarboxylic acids. Examples of the aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanediol, and 1,4-cyclohexanedimethanol. The aliphatic diols may be used alone or in combination of two or more. Among these, it is preferable to use 1,4-butanediol. Examples of the aliphatic dicarboxylic acids include oxalic acid, succinic acid, glutaric acid, adipic acid, sebacic acid, suberic acid, and dodecanedioic acid, and acid anhydrides that are derivatives of these may be used. The aliphatic dicarboxylic acids may be used alone or in combination of two or more. Among these, it is preferable to use succinic acid, succinic anhydride, or adipic acid.

[0058] Examples of the aliphatic aromatic polyester resin include copolymers containing an aliphatic dicarboxylic acid unit, an aromatic dicarboxylic acid unit, and a chain aliphatic and / or alicyclic diol unit. The diol component that gives the diol unit usually has 2 to 10 carbon atoms, such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, and 1,4-cyclohexanedimethanol. Among these, diols having 2 to 4 carbon atoms are preferred, and ethylene glycol and 1,4-butanediol are more preferred, with 1,4-butanediol being even more preferred. The dicarboxylic acid component that gives the dicarboxylic acid unit usually has 2 to 10 carbon atoms, such as succinic acid, adipic acid, suberic acid, sebacic acid, and dodecanedioic acid. Among these, succinic acid or adipic acid is preferred. Examples of aromatic dicarboxylic acid components that give aromatic dicarboxylic acid units include terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid. Among these, terephthalic acid and isophthalic acid are preferred, and terephthalic acid is more preferred. Specifically, polybutylene adipate terephthalate (PBAT), which is a copolymer of 1,4-butanediol, adipic acid, and terephthalic acid, can be mentioned.

[0059] In one embodiment, the polyester elastomer (D) is preferably a polybutylene adipate terephthalate (PBAT) resin or a polyhydroxyalkanoate (preferably an amorphous PHA), etc. These may be used alone or in combination of two or more.

[0060] Among them, polybutylene adipate terephthalate (PBAT) resin is particularly preferably used because of its excellent impact resistance improving effect and thermal stability.

[0061] The content of the polyester elastomer (D) is 0% by mass to 40% by mass, preferably 5% by mass to 35% by mass, preferably 10% by mass to 30% by mass, and preferably 15% by mass to 25% by mass, based on the total amount of the polylactic acid resin composition (100% by mass).

[0062] A-6. Filler dispersant (ingredient E) The polylactic acid resin composition of the present invention may contain a filler dispersing agent (E).

[0063] In the present invention, for the purpose of increasing the dispersibility of the layered silicate-based filler (B) that is blended in a high concentration (10 mass % or more) in the polylactic acid-based resin composition, a filler dispersant (E) and / or a filler-dispersed polymer (F) can be preferably used.

[0064] In one embodiment, the filler dispersant (E) is a compound composed of a hydrophobic group and a hydrophilic group. The hydrophilic / hydrophobic balance can be controlled by adjusting the degree of esterification of the compound to be the filler dispersant, the type of fatty acid (presence or absence of a hydroxyl group, saturated or unsaturated fatty acid, alkyl chain length), and the degree of polymerization.

[0065] Examples of the filler dispersant (E) include fatty acids, fatty acid metal salts, fatty acid sulfonates, fatty acid amides, acrylamides, polyhydric alcohol fatty acid esters, polyglycerin fatty acid esters, etc. The filler dispersant (E) may be used alone or in combination of two or more.

[0066] The preferred filler dispersing agent (E) is at least one selected from the group consisting of polyhydric alcohol fatty acid esters, fatty acid amides, polyglycerin fatty acid esters, condensed hydroxy fatty acids, and alcohol esters of condensed hydroxy fatty acids.

[0067] The polyhydric alcohol fatty acid ester is an ester compound composed of a polyhydric alcohol and a fatty acid. Examples of the polyhydric alcohol fatty acid ester include esters of polyhydric alcohols such as pentaerythritol and glycerin and fatty acids having 8 or more carbon atoms (preferably 8 to 24 carbon atoms, more preferably 10 to 22 carbon atoms).

[0068] The fatty acid amide is a compound having a structure in which a fatty acid and ammonia or a primary or secondary amine are dehydrated and condensed. Examples of the fatty acid amide include saturated fatty acid monoamides such as lauric acid amide, palmitic acid amide, stearic acid amide, and behenic acid amide.

[0069] The polyglycerol fatty acid ester is an ester compound composed of polyglycerol and a fatty acid. Examples of the polyglycerol fatty acid ester include diglycerol palmitate, diglycerol stearate, diglycerol oleate, decaglycerol palmitate, decaglycerol stearate, and decaglycerol oleate.

[0070] Among the above-mentioned filler dispersing agents (E), at least one selected from the group consisting of polyhydric alcohol fatty acid esters, polyglycerin fatty acid esters, condensed hydroxy fatty acids, and alcohol esters of condensed hydroxy fatty acids is particularly preferred, as these are excellent in compatibility with polylactic acid resins (PLA) and are unlikely to cause hydrolysis of PLA.

[0071] The polyglycerin fatty acid ester, condensed hydroxy fatty acid, and alcohol ester of condensed hydroxy fatty acid may be a commercially available product. Examples of commercially available products include "Chirabazol P-4", "Chirabazol VR-01", "Chirabazol VR-08" (polyglycerin fatty acid ester), and "Chirabazol H-818" (alcohol ester of condensed hydroxy fatty acid), all manufactured by Taiyo Kagaku Co., Ltd. These may be used alone or in combination of two or more.

[0072] The content of the filler dispersant (E) is, for example, 0% by mass to 5% by mass, preferably 0.1% by mass to 5% by mass, preferably 0.3% by mass to 3% by mass, and preferably 0.5% by mass to 2% by mass, based on the total amount of the polylactic acid resin composition (100% by mass).

[0073] A-7. Filler dispersion polymer (component F) The polylactic acid resin composition of the present invention may contain a filler-dispersing polymer (F).

[0074] The polylactic acid resin composition of the present invention may contain a filler dispersion polymer (F) for the purpose of improving the dispersibility of the filler. The filler dispersion polymer (F) may also have the effect of improving the interfacial adhesion between the filler and the polylactic acid resin, or the effect of suppressing hydrolysis of the polylactic acid resin by the filler.

[0075] The filler dispersion polymer is not particularly limited, and may be, for example, at least one selected from the group consisting of polyolefin-based resins, polystyrene-based resins, polyvinyl alcohol-based resins, polyalkylene glycol-based resins, polyvinylpyrrolidone-based resins, polyester-based resins, polyamide-based resins, acrylic-based resins, urethane-based resins, epoxy-based resins, and water-soluble polysaccharides.

[0076] Among the above listed resins, polyolefin resins and polystyrene resins are preferred because they have the effect of effectively inhibiting hydrolysis of polylactic acid resins by component B.

[0077] Among the above-listed resins, at least one selected from the group consisting of polyvinyl alcohol resins, polyalkylene glycol resins, polyvinylpyrrolidone resins, and water-soluble polysaccharides is preferred. These resins are not only excellent in compatibility with polylactic acid resins and in filler dispersion function, but also have the characteristic of being biodegradable themselves, and therefore can be used preferably.

[0078] Specific examples of the polyvinyl alcohol resin used as the filler dispersion polymer include ethylene-vinyl alcohol copolymer (EVOH; EVAL (registered trademark) manufactured by Kuraray Co., Ltd.), butenediol-vinyl alcohol copolymer (BVOH; Nichigo G-Polymer (registered trademark) manufactured by Mitsubishi Chemical Corporation), and the like.

[0079] The water-soluble polysaccharides refer to water-soluble compounds formed by long chains of monosaccharides such as glucose, mannose, pullulan, and mannan. In one embodiment, the water-soluble polysaccharides are water-soluble carbohydrates formed by binding 10 or more monosaccharides. In one embodiment, the water-soluble polysaccharides may be naturally derived polymeric substances. For example, water-soluble polysaccharides derived from plants (seeds, sap, fruits, etc.), seaweed, and microorganisms may be used. Specific examples of the water-soluble polysaccharides include pullulan, dextrin, chitosan, tamarind seed gum, guar gum, locust bean gum, gum arabic, karaya gum, pectin, cellulose, konjac mannan, soybean polysaccharides, carrageenan, agar, tragacanth gum, alginic acid, xanthan gum, gellan gum, Agrobacterium succinoglycan, carboxymethylcellulose, and cationized guar gum. Among them, pullulan or dextrin is preferable, and pullulan is more preferable.

[0080] The content of the filler-dispersing polymer (F) is, for example, 0% by mass to 5% by mass, preferably 0.1% by mass to 5% by mass, preferably 0.3% by mass to 3% by mass, and preferably 0.5% by mass to 2% by mass, based on the total amount of the polylactic acid resin composition (100% by mass).

[0081] A-8. Hydrolysis inhibitor (ingredient G) The polylactic acid resin composition of the present invention may contain a hydrolysis inhibitor (G).

[0082] The hydrolysis inhibitor can be blended for the purpose of improving the processing stability, long-term heat resistance, and long-term wet heat resistance of the polylactic acid resin composition. The hydrolysis inhibitor has the function of suppressing the decrease in the molecular weight of the polylactic acid resin and stabilizing it by capturing the carboxylic acid generated by the hydrolysis of the polylactic acid resin.

[0083] In one embodiment, the hydrolysis inhibitor is a compound having at least one functional group selected from the group consisting of a carbodiimide group, an oxazoline group, and an epoxy group. The compound may be a polymer.

[0084] Examples of the compound containing a carbodiimide group include dicyclohexylcarbodiimide, diisopropylcarbodiimide, dimethylcarbodiimide, diisobutylcarbodiimide, dioctylcarbodiimide, t-butylisopropylcarbodiimide, diphenylcarbodiimide, di-t-butylcarbodiimide, di-β-naphthylcarbodiimide, N,N'-di-2,6-diisopropylphenylcarbodiimide, 2,6,2',6'-tetraisopropyldiphenylcarbodiimide, as well as cyclic carbodiimides and polycarbodiimides such as Carbodilite (registered trademark: manufactured by Nisshinbo Chemical Inc.) and Stavaxol (registered trademark: manufactured by Rhein Chemie).

[0085] Examples of commercially available products of the compound having the epoxy group include "Celloxide 2021P" manufactured by Daicel Corporation, "Denacol" manufactured by Nagase ChemteX Corporation, and "Epofriend" manufactured by Daicel Corporation.

[0086] An example of a commercially available product of the compound having an oxazoline group is "Epocross" manufactured by Nippon Shokubai Co., Ltd.

[0087] The content of the hydrolysis inhibitor (G) is, for example, 0% by mass to 5% by mass, preferably 0.1% by mass to 5% by mass, preferably 0.3% by mass to 4% by mass, and preferably 0.5% by mass to 3% by mass, based on the total amount of the polylactic acid resin composition (100% by mass).

[0088] A-9. Other ingredients The polylactic acid resin composition may further contain any other appropriate components (additives) as necessary. Examples of additives include antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, antiblocking agents, antibacterial agents, compatibilizers, plasticizers, tackifiers, processing aids, lubricants, coupling agents, flame retardants, oxygen scavengers, foaming agents, and colorants. The additives may be added at any appropriate timing in the production process of the polylactic acid resin composition, for example, in the form of liquid, powder, pellets, granules, or master batch. The additives may be used alone or in combination of two or more. The content of other components (additives) is, for example, 0% by mass to 5% by mass, preferably 0.1% by mass to 5% by mass, preferably 0.2% by mass to 4% by mass, preferably 0.3% by mass to 3% by mass, preferably 0.4% by mass to 2% by mass, and preferably 0.5% by mass to 1% by mass, based on the total amount of the polylactic acid resin composition (100% by mass).

[0089] B. Method for producing polylactic acid-based resin composition The polylactic acid resin composition of the present invention can be obtained by melt-kneading at least a polylactic acid resin (A), a layered silicate filler (B), and an acrylic thermoplastic elastomer (C). The polylactic acid resin composition of the present invention can be obtained by melt-kneading a state in which, in addition to the above components (A) to (C), at least one selected from a polyester elastomer (D), a filler dispersant (E), a filler dispersion polymer (F), and a hydrolysis inhibitor (G) is contained as necessary. That is, the polylactic acid resin composition can be obtained as a melt-kneaded product. The polylactic acid resin composition can be in the form of a solid, and the shape can be, for example, a pellet, a rod, or a powder.

[0090] The polylactic acid resin composition of the present invention can be produced by any known production method, such as a method of uniformly mixing the components in advance using a high-speed or low-speed stirrer, and then melt-kneading the components at a temperature above the melting point of the resin using a single-screw or multi-screw extruder having sufficient kneading capacity, or a method of mixing and kneading the components when melted.

[0091] Any suitable method can be adopted as the melt-kneading method. For example, a kneader, a Banbury mixer, a roll, a single-screw extruder or a multi-screw extruder having two or more screws can be used. A twin-screw extruder is preferably used. The melt-kneaded composition can be pelletized. In one embodiment, the melt-kneading is performed in a temperature range of 80°C to 170°C, preferably 100°C to 160°C.

[0092] In one embodiment, the layered silicate-based filler (B) is supplied to a melt-kneading device as a "filler granule" described below, and melt-kneaded.

[0093] According to this method, the layered silicate-based filler (B) can be blended at a high concentration (10 to 55 mass%) necessary to achieve the effects of the present invention, while the feeding speed and feeding stability into an apparatus such as an extruder are remarkably excellent, so that the productivity of the resin composition (compound processing speed per hour) can be dramatically improved.

[0094] That is, one embodiment of the method for producing a polylactic acid-based resin composition according to the present invention includes a step of melt-kneading a polylactic acid-based resin (A), a filler granule containing a layered silicate-based filler (B), and an acrylic thermoplastic elastomer (C), wherein the filler granule contains the layered silicate-based filler (B), a filler dispersant (E) and a filler dispersion polymer (F), and the content of the layered silicate-based filler (B) in the filler granule is 80 parts by mass to 99.9 parts by mass relative to 100 parts by mass of the total solid content of the filler granule.

[0095] (Filler granules) The "filler granule" refers to a granule having a filler content of preferably 80 to 99.9 parts by mass relative to 100 parts by mass of the total solid content of the filler granule, and can be produced by any appropriate method. The filler granule can be obtained, for example, by subjecting a mixture containing a layered silicate-based filler (B), a filler dispersant (E) and / or a filler dispersion polymer (F) (which can be a binder for the filler in the filler granule) to a semi-wet granulation method.

[0096] Specifically, the filler dispersant (E) and / or the filler dispersing polymer (F) are preferably in a uniformly dispersed state in the step of mixing with the layered silicate-based filler (B).

[0097] Furthermore, in the granulation process of the granulation precursor obtained by the semi-wet granulation process by adding an appropriate amount of water, or in the heating process of removing moisture from the granulation precursor, at least a portion of the filler dispersion polymer is thermally melted, thereby increasing the adhesion between the fillers and resulting in a powder granulation product with a stable shape.

[0098] In one embodiment, the method for producing the powder granulated material includes a mixing step of mixing the layered silicate-based filler (B), the filler dispersing agent (E) and / or the filler dispersion polymer (F) with water, a granulation step of granulating the mixture obtained through the mixing step to obtain a granulated material precursor, and a heating step of heating the granulated material precursor. In the mixing step, a binder other than the filler dispersion polymer may be further added. The granulated material precursor can be dried by heating in the heating step. Furthermore, the binding of the layered silicate-based filler (B) is promoted through the heating step.

[0099] In one embodiment, in the above mixing step, the layered silicate-based filler (B) is mixed with the filler dispersant (E) and / or the filler dispersion polymer (F) to prepare a mixture, and water is added while stirring the mixture. In this way, water can be uniformly dispersed throughout the mixture at an appropriate blending ratio, which is advantageous in obtaining a granulated product having stable granulation and excellent shape and granulated product hardness in the granulated product after heat drying in the next semi-wet granulation step. Water can be gradually added, for example, in the form of a spray, a shower, or a drip using a nozzle. The spray means that a liquid pressurized by a gas such as compressed air is suddenly ejected from a fine hole of a nozzle to form fine particles of the liquid. The shower means that a fluid under the same pressure is dispersed and ejected from a shower head (a jig with multiple holes of the same size). The water to be added is not particularly limited, and for example, tap water, distilled water, ion-exchanged water, hard water, soft water, etc. can be used. If necessary, water may be used in combination with other components such as alcohol to improve wettability to the powder raw material. When other components (e.g., solid components) are added, the components may be mixed with the above mixture. The filler granules may contain other components (additives) described in "A-9. Other Components".

[0100] As described above, the content of the layered silicate-based filler (B) in the filler granules is, relative to 100 parts by mass of the total amount of all solids in the filler granules, preferably 80 parts by mass to 99.9 parts by mass, more preferably 82 parts by mass to 99 parts by mass, even more preferably 85 parts by mass to 98 parts by mass, particularly preferably 87 parts by mass to 97 parts by mass, and most preferably 90 parts by mass to 96 parts by mass.

[0101] The content of the filler dispersant (E) and the filler dispersion polymer (F) is preferably 0.1 to 20 parts by mass, more preferably 1 to 18 parts by mass, even more preferably 2 to 15 parts by mass, particularly preferably 3 to 13 parts by mass, and most preferably 4 to 10 parts by mass, in total relative to 100 parts by mass of the total solid content of the filler granules.

[0102] The blending ratio (E:F) of the filler dispersing agent (E) and the filler dispersing polymer (F) is arbitrary, but usually (E:F) is in the range of 0:100 to 80:20, preferably 1:99 to 70:30, more preferably 5:95 to 60:40, and even more preferably 10:90 to 50:50.

[0103] In the mixing step, it is preferable to mix uniformly using any appropriate mixer. Examples of the mixer include a Henschel mixer, a powder kneader (KDH, KDA, CKD, CPM) (Dalton), a Nauta mixer, a Spartan mixer (SPM) (Dalton), and an SP granulator (SPG) (Dalton). In order to obtain a preferable mixture with excellent granulation properties, it is preferable that the stirring blades of the mixing and stirring device are appropriate. For example, when using a Henschel mixer type mixer, it is preferable that the mixer blades are a combination of upper and lower blades, and the upper blade is a Y1 blade (trade name, manufactured by Nippon Coke Co., Ltd.) and the lower blade is an S0 blade (trade name, manufactured by Nippon Coke Co., Ltd.). It is also preferable to install a deflector in the stirring tank and mix. That is, by making it possible to uniformly disperse each component throughout the mixture in the mixing step, it is advantageous to increase the productivity and quality stability in the subsequent semi-wet granulation step and obtain granules with excellent shape and granule hardness.

[0104] The amount of water is, for example, 5 to 100 parts by mass, preferably 8 to 70 parts by mass, more preferably 10 to 50 parts by mass, and even more preferably 15 to 30 parts by mass, based on 100 parts by mass of the total solid content of the layered silicate filler (B), the filler dispersant (E) and / or the filler dispersion polymer (F). If the amount is within this range, a powder mixture with excellent granulation properties can be obtained in the granulation step by the semi-wet method. If such a mixture is used, a powder granulation precursor in which the layered silicate filler (B) is preferably bound can be stably obtained.

[0105] It is preferable to add water to the powder mixture while uniformly dispersing the powder mixture over a period of usually 1 to 60 minutes, preferably 3 to 30 minutes, and more preferably 5 to 20 minutes, so that the powder mixture is saturated with water.

[0106] The mixing time in the mixing step can be any appropriate mixing time depending on the type of components, the type of mixer, the component blending ratio, etc. Preferably, the mixing time is set so that all the raw material components are uniformly dispersed and mixed. With a high-speed mixer such as a Henschel mixer or a Spartan mixer, the processing time can be 1 to 10 minutes. On the other hand, with a powder kneader, a processing time of several minutes to 60 minutes may be required.

[0107] In one embodiment, the filler-dispersing polymer (F) may be subjected to mixing in the form of a polymer liquid (polymer solution or polymer dispersion) containing the filler-dispersing polymer.

[0108] In the case of mixing the polymer liquid containing the filler dispersion polymer, it is also preferable to gradually add and mix the liquid in the form of a spray atomization, shower, or dropwise addition using a nozzle.

[0109] In the granulation step, a compression granulation method is preferably used. In addition, in the granulation step, a semi-wet granulation method can be preferably used. Examples of the compression granulation method / semi-wet granulation method include a disk pelleter method, a tableting method, and a briquetting method. From the viewpoint of the balance between productivity and the quality of the obtained filler granules, the disk pelleter method is preferably used.

[0110] The basic structure of a disk pelletizer has one or two disks with many holes of 2 mm to 30 mm, and a roller for pressure-feeding the raw material into the holes of the disk. The raw material supplied between the disk and the roller, or between two disks, is pressed into the holes of the disk as the roller rotates, and a cylindrical extrudate is formed. The filler mixture forced into the disk hole is given a compressive stress from the outer periphery of the die hole in the process of passing through the hole, and the extruded granule precursor is cut by a cutter or the like on the back side of the disk to form a pellet-shaped granule. The length of the granule precursor (resulting in a filler granule) can be adjusted by the distance between the back side of the disk and the cutter and the number of rotations of the roller.

[0111] More specifically, the disc pelleter type includes a roller disc die type, a roller ring die type, a double die type, a flat die type, etc. An example of a commercially available disc pelleter type granulator is the Disc Pelletter F Series manufactured by Dalton.

[0112] Any suitable drying method can be used in the drying step. After the drying step, a filler granule from which fine powder has been removed can be obtained by a vibrating sieve or the like. Any suitable drying equipment can be used in the drying step. For example, a vibrating fluidized dryer is preferred because it can perform drying efficiently in a short time, and examples of such equipment include the VDF series vibrating fluidized dryers manufactured by Dalton.

[0113] The polylactic acid resin composition of the present invention can be molded by various methods such as injection molding and extrusion molding. In particular, since it has excellent flowability and a short molding cycle time, it can be a suitable material for injection molding. EXAMPLES

[0114] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In addition, parts and % are based on mass unless otherwise specified.

[0115] [Production example] Production of filler powder granules 94 parts by mass of talc powder (Asada Flour Milling Co., Ltd., product name "JM-300"; bulk density: 0.17), 3 parts by mass of a filler dispersant (polyglycerol fatty acid ester powder, Taiyo Kagaku Co., Ltd., product name "Chirabazol VR-08"), and 3 parts by mass of a filler dispersion polymer (water-soluble vinyl alcohol resin powder (BVOH), Mitsubishi Chemical Corporation, product name "Nichigo G-polymer AZF8035Q"; saponification degree 98.0 mol% or more; melting point: 172°C) were added to an FM mixer (Nippon Coke and Engineering Co., Ltd., product name "5FM5C / I"; processing volume: 5 L), and the mixture was stirred for 10 minutes at 2,000 rpm to obtain a powder mixture.

[0116] The FM mixer had a combination of upper and lower blades, with the upper blade being a Y1 blade (product name, manufactured by Nippon Coke Co., Ltd.) and the lower blade being an S0 blade (product name, manufactured by Nippon Coke Co., Ltd.). A baffle plate (also called a deflector) was installed in the mixing vessel.

[0117] While rotating the stirring blade at a rotation speed of 2,000 rpm, 15 parts by mass of clean water (tap water) was continuously sprayed into the powder mixture in a spray form for 10 minutes to obtain a water-containing powder mixture.

[0118] This water-containing powder mixture was charged into a disc pelleter (manufactured by Dalton, product name "Disc Pelleter F-5 / 11-175") to obtain a pellet-shaped granulated material precursor.

[0119] In this case, the die hole diameter was 3 mmφ, the die plate thickness was 15 mm, the effective length of the die hole (the length of the zone receiving compressive stress from the die wall surface) was 10 mm, and the rotation speed of the disc pelletizer roller was 108 rpm.

[0120] The obtained granule precursor was dried at 140° C. for 4 hours using a hot air circulation type dryer to obtain a “filler powder granule”.

[0121] <Evaluation> The "filler powder granules" obtained in the production examples were subjected to the following evaluations. The results are shown in Table 1.

[0122] (1) Bulk density After drying, the "filler powder granules" were allowed to fall naturally into a 1-liter measure, filled to the brim, and weighed to exactly 1 liter in volume. The mass was then measured to calculate the bulk density of the granules (unit: kg / L).

[0123] (2) Pellet size 20 particles of the filler powder granules were taken out, and the average length and diameter (unit: mm) of the particles were measured using a vernier caliper.

[0124] (3) Moisture content The amount of moisture (unit: mass%) remaining in the filler powder granules was measured using an infrared moisture meter (FD-660 manufactured by Kett Electric Laboratory).

[0125] (4) Breaking strength The breaking strength (load required to break) (unit: kg) of the dried filler powder granules was measured using a Kiya hardness tester (manufactured by Shiro Sangyo Co., Ltd., product name "WPF1600-B"). The measurement was performed by applying stress to the side of the filler powder granules using a cylindrical jig with a diameter of 3 mm. The measured value was the average value of 25 granules.

[0126] (5) Filler concentration in the "filler powder granules" 1 to 3 g of the "filler powder granules" were sampled, placed in a crucible, and held in an electric furnace at 600°C for 3 hours, and the concentration (mass%) of the filler (talc) in the granules was calculated from the ash weight.

[0127] [Table 1]

[0128] [Example 1] 55 parts by mass of the "filler powder granules" obtained in the manufacturing example, 22.5 parts by mass of polylactic acid (PLA; Total Corbion, product name "Luminy L130"; weight average molecular weight 130,000, melting point 175°C), 10 parts by mass of an acrylic thermoplastic elastomer (PMMA-BA block copolymer; Kuraray, product name "Clarity LA2250"; PMMA content 30% by mass), and polybutylene adipate terephthalate (PBAT) resin (BASF, product name "Ecoflex F Blend 22.5 parts by mass of a polymer having a carbodiimide group as a hydrolysis inhibitor (manufactured by Nisshinbo Chemical Co., Ltd., trade name "Carbodilite HMV-5CA-LC") and 1 part by mass of a polymer having a carbodiimide group as a hydrolysis inhibitor (manufactured by Toshiba Machine Co., Ltd., trade name "TEM37SS", L / D=48) were quantitatively charged into a twin-screw extruder (manufactured by Toshiba Machine Co., Ltd., trade name "TEM37SS", L / D=48) through a hopper provided at the most upstream position of the extruder using a weight feeder, and continuously melt-kneaded (discharge: 20 kg / Hr) to obtain pellets of the resin composition. The cylinder temperature of the extruder was set to 200°C from the middle stage of the extruder onwards. The rotation speed of the main screw of the twin-screw extruder was set to 100 rpm. The melt-kneaded resin composition was extruded into a strand shape, cooled in a water-cooled bath, and made into pellets with a length of about 3 mm.

[0129] In Example 1, the "filler powder granules" contain 3 mass% of filler dispersion polymer and 3 mass% of filler dispersant, so the final resin composition contains 46.6 mass parts of talc, 1.5 mass parts of filler dispersion polymer (BVOH), and 1.5 mass parts of filler dispersant (Chirabazole VR-08) per 100 mass parts of resin composition.

[0130] <Evaluation> The polylactic acid resin compositions obtained in the Examples and Comparative Examples were subjected to the following evaluations. The results are shown in Table 2.

[0131] (1) Evaluation of molding cycle performance of injection molded specimens (dumbbell test specimens) When injection molding a dumbbell test piece for bending tests (Type 1A multipurpose test piece) conforming to ISO178, the mold temperature was set to 90°C, and the molding cycle properties were evaluated based on the number of seconds of cooling time required to remove the molded piece and the releasability of the molded product from the mold, according to the following criteria. A: It can be removed in less than 60 seconds of cooling, allowing for continuous molding. B: The part can be removed in less than 90 seconds, allowing for continuous molding. C: The part can be removed in less than 120 seconds of cooling, allowing for continuous molding. D: The molded product does not solidify even after 120 seconds of cooling, and cannot be removed from the mold, or the product has poor releasability from the mold (due to sticking, etc.), making continuous molding impossible. (Molding cycle performance ranking: A>B>C>D (left is good))

[0132] (2) MFR measurement (unit: g / 10 min) The melt mass flow rate (MFR) was measured and the fluidity was evaluated using a "Melt Indexer" manufactured by Toyo Seiki Seisakusho Co., Ltd. in accordance with JIS K7210. The measurement was performed at a temperature of 210°C and a load of 5 kg.

[0133] (3) Fluidity (spiral flow) of resin composition (unit: cm) Using a flow length measurement mold in an injection molding machine (Japan Steel Works "JD110AD-110H", mold clamping 100 ton) with a spiral groove cavity of 2 mm depth and 10 mm width in cross section perpendicular to the flow direction, the fluidity of the resin composition was evaluated under the following conditions: cylinder setting temperature 200°C, mold temperature 120°C (both fixed side and moving side), cooling time 90 seconds, injection pressure 80 MPa (and 120 MPa), no pressure holding, injection speed 40 mm / sec, and back pressure 10 MPa.

[0134] (4) Ash content measurement (unit: mass %) 1 to 3 g of pellets of the polylactic acid-based resin composition were collected and kept in a crucible in an electric furnace at 600° C. for 3 hours, and the ash mass was calculated.

[0135] (5) Dispersibility of fillers Pellets of the polylactic acid resin composition were rolled by a hot press to form a sheet having a thickness of about 0.5 mm. The remaining filler aggregates were visually observed through the sheet and evaluated according to the following criteria. AA: Good dispersion state with almost no filler agglomerates observed A: A state in which a small amount of relatively small filler aggregates remain BB: A state in which a considerable number of relatively small filler aggregates remain. B: Large filler aggregates (Distribution order: AA>A>BB>B (left good))

[0136] (6) Bending measurement (unit: MPa) A bending test was carried out in accordance with ISO 178 to measure the bending strength and bending modulus. The test pieces for the measurements were dumbbell test pieces (1A type multipurpose test pieces) cut out from pellets of the polylactic acid resin composition using an injection molding machine ("SI-80W" manufactured by Toyo Machinery & Metals Co., Ltd., mold clamping 100 tons) with a cylinder setting temperature of 200°C, a mold temperature of 110°C (both fixed side and moving side), and a cooling time of 60 seconds.

[0137] (7) Temperature of deflection under load (DTUL) measurement (unit: °C) The deflection temperature under load (DTUL) was measured under a load of 0.45 MPa in accordance with ISO 75. The test specimens used for the measurement were dumbbell test specimens cut out from the above bending measurement.

[0138] (8) Charpy impact strength measurement (unit: KJ / m 2 ) The Charpy impact strength of a notched test piece formed from a polylactic acid-based resin composition was measured in accordance with ISO 179. The test piece for measurement was cut out from the dumbbell test piece obtained in the bending measurement described above.

[0139] (9) Mold shrinkage rate (unit: %) Using an injection molding machine (Toyo Machinery & Metals "SI-80W", mold clamping 100 tons), a flat molded product of 100 mm x 100 mm x 2 mm (thickness) was molded using pellets of the polylactic acid resin composition under the conditions of a cylinder setting temperature of 200°C, a mold temperature of 110°C (both fixed side and moving side), and a cooling time of 60 seconds. At this time, the resin gate in the mold was a film gate.

[0140] After molding, the sample was left in an environment of 23°C and 50% relative humidity for 24 hours, and then the dimensions in the flow direction (MD) were measured to determine the molding shrinkage rate.

[0141] [Examples 2 to 5 and Comparative Examples 1 to 7] Resin compositions were produced using a twin-screw extruder under the same conditions as in Example 1, except that the blending ratios were changed to those shown in Table 2, and various evaluations were carried out using the same methods as described in Example 1. The results are shown in Table 2.

[0142] In addition, the "filler powder granules" used in Example 1 are used in the production of the resin compositions in Examples 2 to 5 and Comparative Examples 1, 2, and 7. Table 2 shows the final composition.

[0143] [Table 2-1]

[0144] [Table 2-2]

[0145] Comparison of Example 1 and Comparative Example 1 (containing about 50% by mass of component (B)) shows that the polylactic acid-based resin composition containing component (C) obtained by the present invention has improved fluidity (MFR and spiral flow) and excellent molding cycle properties. The incorporation of component (C) (acrylic thermoplastic elastomer) does not decrease the molding cycle properties.

[0146] Similarly, a comparison of Examples 2 and 3 with Comparative Example 2 (containing about 50% by mass of component (B) and not containing component (D)) shows that the polylactic acid resin composition obtained by the present invention has improved fluidity (MFR and spiral flow) and is also excellent in molding cycle properties. It is shown that even when component (C) is added, there is no or only a small decrease in fluidity.

[0147] Examples 4 and 5 also show excellent fluidity and molding cycle properties.

[0148] Comparative Examples 3 to 6 are examples lacking component (B), but in all cases, at a mold temperature of 90° C., the molded pieces did not crystallize within 120 seconds, and the molded articles could not be removed.

[0149] Comparative Example 7 shows the result of blending 10 mass% of Chirabazole VR-08 (polyglycerol fatty acid ester) as a flowability modifier instead of component (C) (acrylic thermoplastic elastomer) used in Example 4. Although the flowability (MFR) was improved, the molded product had poor releasability and stuck to the mold, making it difficult to eject the molded product using an ejector pin, and thus failing to achieve the effect of shortening the molding cycle.

[0150] As shown in Table 2, it is confirmed that the polylactic acid resin composition of the present invention has excellent melt fluidity and molding cycle properties. In addition, since the molded article of the polylactic acid resin composition of the present invention can be easily removed from a mold, it is clear that the composition is a resin composition having high productivity in injection molding. Furthermore, the polylactic acid resin composition of the present invention can exhibit a wide range of well-balanced mechanical and thermal properties such as rigidity, heat resistance (heat distortion temperature resistance), impact resistance, and dimensional stability (low molding shrinkage, low linear expansion coefficient, and low warpage) in the molded article.

Claims

1. 15% by mass to 87% by mass of a polylactic acid-based resin (A), 10% by mass to 55% by mass of a layered silicate-based filler (B); 3% to 15% by weight of an acrylic thermoplastic elastomer (C), and 0% to 40% by weight of at least one polyester elastomer (D) selected from aliphatic polyester elastomers and aliphatic-aromatic polyester elastomers; The content (mass%) is based on the total amount of the composition.

2. 2. The polylactic acid resin composition according to claim 1, wherein the weight average molecular weight of the polylactic acid resin (A) is 100,000 to 150,000.

3. 2. The polylactic acid resin composition according to claim 1, wherein the layered silicate filler (B) is at least one selected from the group consisting of talc and mica.

4. 2. The polylactic acid resin composition according to claim 1, wherein the acrylic thermoplastic elastomer (C) is a polymethyl methacrylate (PMMA)-butyl acrylate (BA) block copolymer.

5. 5. The polylactic acid resin composition according to claim 4, wherein the amount of the PMMA block component of the polymethyl methacrylate (PMMA)-butyl acrylate (BA) block copolymer is 20% by mass to 30% by mass.

6. 2. The polylactic acid resin composition according to claim 1, wherein the polyester elastomer (D) is a polybutylene adipate terephthalate (PBAT) resin.

7. The polylactic acid resin composition according to claim 1, further comprising 0.1% by mass to 5% by mass of a filler dispersant (E).

8. The polylactic acid resin composition according to claim 1, further comprising 0.1% by mass to 5% by mass of a polymer (F) for dispersing fillers.

9. A method for producing the polylactic acid resin composition according to any one of claims 1 to 8, comprising the steps of: The polylactic acid-based resin composition contains 0.1% by mass to 5% by mass of a filler dispersant (E) and / or 0.1% by mass to 5% by mass of a filler dispersion polymer (F), The method includes a step of melt-kneading a polylactic acid-based resin (A), a filler granule containing a layered silicate-based filler (B), and an acrylic thermoplastic elastomer (C), The filler granules contain a layered silicate-based filler (B), and a filler dispersant (E) and / or a filler dispersion polymer (F), The content of the layered silicate-based filler (B) in the filler granules is 80 parts by mass to 99.9 parts by mass per 100 parts by mass of the total amount of all solids in the filler granules.

10. A molded article obtained by using the polylactic acid resin composition according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Biodegradable resin composition and molded article made from said composition

    JP7228110B2