Manufacturing method of cellulose fine fiber dispersion concentrate and manufacturing method of resin composition
A continuous deliquifying process for cellulose fine fiber concentrates addresses inefficiencies and environmental concerns, achieving uniform dispersion and enhanced resin composite properties through controlled fiber content and chemical modification.
Patent Information
- Application Number
- JP2023084601
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Existing methods for producing cellulose fine fiber dispersion concentrates face challenges such as inefficiency, batch-to-batch variability, and environmental impact, particularly in large-scale production, due to aggregation and uneven distribution of cellulose fine fibers, which affect the quality and uniformity of resin composites.
A continuous deliquifying process is employed to produce cellulose fine fiber dispersion concentrates with controlled fiber content and diameter, using a concentration device that includes a tank, slit, filtration substrate, suction section, and press roll to achieve uniformity and redispersibility, with chemical modification to enhance fiber-resin affinity.
The method enables the production of cellulose fine fiber concentrates with minimal variation in fiber content and low environmental impact, ensuring uniform dispersion and improved mechanical properties in resin composites.
Smart Images

Figure 2024168161000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a concentrate of a cellulose fine fiber dispersion, and a method for producing a resin composition. [Background technology]
[0002] Thermoplastic resins are light and have excellent processing properties, and therefore are widely used in many fields such as automobile parts, electrical and electronic parts, office equipment housings, and precision parts. However, resins alone often have insufficient mechanical properties and dimensional stability, so composites of resins and various fillers are generally used. In recent years, the use of organic fibers such as cellulose fibers as such fillers has been considered. Cellulose is a promising filler for environmentally friendly resin compositions because it is a material that places little strain on the environment, has a low specific gravity, and can have an excellent effect of improving the physical properties of resin compositions. In particular, cellulose fine fibers can exhibit an excellent reinforcing effect on resin compositions even in small amounts due to their fine structure, so their use as fillers for resin compositions has been considered in recent years. As a method for producing cellulose fine fibers, a method in which a dilute dispersion with a low solid content is treated with a refiner, a high-pressure homogenizer, or the like is generally used. A dilute dispersion needs to be concentrated because it is difficult to mix it into a resin as a filler as it is. However, cellulose fine fibers are extremely susceptible to aggregation due to hydrogen bonds between cellulose molecules, and excessive concentration reduces redispersibility, making it difficult to uniformly disperse the cellulose fine fibers in the resin. Therefore, in order to realize a state in which the cellulose fine fibers are well dispersed in the resin while exhibiting an excellent reinforcing effect, various techniques for concentrating the cellulose fine fibers have been proposed.
[0003] For example, Patent Document 1 describes a method in which a resin emulsion is added to a dispersion of cellulose fine fibers to obtain a molded body as a mixture of cellulose fine fibers and resin, and the molded body is pulverized and melt-kneaded with a base resin.
[0004] Patent Document 2 describes a method of dewatering an aqueous dispersion of chemically modified pulp by squeezing it under treatment conditions of 2 to 10 MPa. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2013 / 137449 [Patent Document 2] JP 2017-95813 A Summary of the Invention [Problem to be solved by the invention]
[0006] When kneading cellulose fine fibers with a resin, it is necessary to remove the dispersion medium from the cellulose fine fiber dispersion. However, since the dispersion is generally dilute, in an industrial process using a large amount of cellulose fine fibers, the amount of dispersion medium to be removed is also enormous, and the efficiency of a batch-type process is very poor. In addition, there was a problem that the cellulose fine fiber content in the obtained concentrate differed from batch to batch, and even in the same batch, the cellulose fine fibers were locally concentrated to a high content in some parts, resulting in an uneven state. Due to such variation in the cellulose fine fiber content, defects are likely to occur when used as a filler for filler-reinforced resin, and the conventional method was not suitable for mass production. In addition, for example, the papermaking process widely used in the papermaking industry includes a heat drying step, so the dried product obtained by this process has poor redispersibility when kneaded with a resin, and is difficult to exhibit performance as a filler for filler-reinforced resin.
[0007] Patent Document 1 describes a manufacturing method in which a resin emulsion is added to a dispersion of cellulose fine fibers, and the mixture of cellulose fine fibers and resin is made into paper, thereby obtaining a concentrated cellulose fine fiber composition as an intermediate. However, depending on the properties of the resin emulsion and the coarseness of the papermaking machine, it is considered that the added resin emulsion is not 100% utilized and is discharged in wastewater, resulting in large energy consumption when disposing of it as industrial waste. Therefore, the above technology cannot be said to be suitable as an industrial process from the viewpoints of cost and environmental load.
[0008] On the other hand, Patent Document 2 describes a method for dehydrating a dispersion of chemically modified pulp by applying pressure, but the pressure method is difficult to make into a continuous process. Cellulose fine fiber compositions are more likely to clog filters than pulp, and the cake layer formed at the beginning of the process is compressed tightly in the pressure method. As a result, the above technology is prone to problems such as products with different cellulose fine fiber contents being mixed together within a batch.
[0009] The present invention aims to solve the above problems and provide a method for producing a cellulose fine fiber dispersion concentrate, which can produce a concentrate with little variation in cellulose fine fiber content with low environmental impact even when a dilute cellulose fine fiber dispersion is used, and a method for producing a resin composition using the concentrate. [Means for solving the problem]
[0010] The present disclosure includes the following aspects. [Item 1] 1. A method for producing a cellulose fine fiber dispersion concentrate, comprising the steps of: The method includes a concentration step of deliquifying the cellulose fine fiber dispersion to obtain the concentrate, The average fiber diameter of the cellulose fine fibers in the cellulose fine fiber dispersion is 50 nm or more and 1000 nm or less, In the concentrating step, the cellulose fine fiber dispersion is continuously deliquified at a treatment speed of 50 kg / h or more and less than 10,000 kg / h, The mass content of the cellulose fine fibers in the cellulose fine fiber dispersion is 0.3 mass% or more and 5.0 mass% or less, the ratio of the mass content of cellulose fine fibers in the concentrate to the mass content of cellulose fine fibers in the cellulose fine fiber dispersion is 4 or more and 100 or less; method. [Item 2] 2. The method according to Item 1, wherein in the concentrating step, the cellulose fine fiber dispersion is deliquified by suction to produce an intermediate concentrate, and the intermediate concentrate is deliquified by pressing to produce a concentrate. [Item 3] The concentrating step comprises: a tank for storing a cellulose fine fiber dispersion; a dispersion liquid temporary storage section having a slit and connected to the tank; a filtering substrate that carries thereon a cellulose fine fiber dispersion received from the dispersion temporary storage section via the slit and that travels; a suction section for sucking and deliquifying the cellulose fine fiber dispersion on the filtration substrate through the filtration substrate to produce the intermediate concentrate; A press roll and a press belt which sandwich the intermediate concentrate and press-deliquify it to produce the concentrate; The method according to Item 2, wherein the method is carried out using a concentrating device comprising: [Item 4] 4. The method according to claim 3, wherein the treatment speed is controlled by adjusting the slit width of the slit and the running speed of the filtration substrate. [Item 5] 5. The method according to item 3 or 4, wherein the suction section has two or more reduced pressure sections with different reduced pressure levels adjusted to increase in the running direction of the filtration substrate. [Item 6] 6. The method according to any one of items 3 to 5, wherein the filtration substrate runs on the suction part at an ascending gradient of 10° or more and 45° or less. [Item 7] The method according to any one of Items 3 to 6, wherein the cellulose fine fiber dispersion overflowing from the dispersion temporary storage section is returned to the tank, thereby circulating the cellulose fine fiber dispersion between the tank and the dispersion temporary storage section. [Item 8] 8. The method according to claim 7, wherein the tank is a tank without a stirring mechanism. [Item 9] 9. The method according to any one of items 3 to 8, wherein the press roll presses and deliquors the intermediate concentrate together with the press belt in a roll angle range of 30° or more and 270° or less. [Item 10] The filtration substrate is an endless substrate having no support, 10. The method according to any one of items 3 to 9, wherein in the concentrating step, a cleaning treatment is performed in which at least the dispersion-mounting surface of the filtration substrate is cleaned by liquid washing and / or physical scraping operation. [Item 11] 11. The method according to any one of items 3 to 10, wherein the mass content of cellulose fine fibers in the intermediate concentrate is 3 to 7 mass%. [Item 12] The mass content of the cellulose fine fibers in the intermediate concentrate is 2% by mass to 20% by mass, 12. The method according to any one of items 3 to 11, wherein the mass content of the cellulose fine fibers in the concentrate is 5% by mass to 30% by mass. [Item 13] 13. The method according to any one of items 1 to 12, wherein, in the concentrating step, when the mass content of the cellulose fine fibers in the concentrate is measured by sampling 10 points, the number average value of the mass content is 5% by mass or more and 30% by mass or less, and the CV value (standard deviation / number average value) of the mass content is 0.001 or more and 0.300 or less. [Item 14] 14. The method according to any one of items 1 to 13, wherein the concentrating step is carried out at 80° C. or lower. [Item 15] 15. The method according to any one of items 1 to 14, wherein the cellulose fine fibers in the cellulose fine fiber dispersion contain 70% or more, by number, of fibers having a fiber length of less than 0.1 mm. [Item 16] 16. The method according to any one of items 1 to 15, wherein the cellulose fine fibers in the cellulose fine fiber dispersion are chemically modified with a hydrophobic substituent. [Item 17] 17. The method according to any one of items 1 to 16, wherein the cellulose fine fibers in the cellulose fine fiber dispersion are chemically modified with an acetyl group. [Item 18] 18. The method according to any one of items 1 to 17, wherein the cellulose fine fibers in the cellulose fine fiber dispersion are made from cotton linters. [Item 19] A step of producing a concentrate of a cellulose fine fiber dispersion by the method according to any one of items 1 to 18; drying the concentrate to produce a dried cellulose fine fiber body; The method for producing a dried cellulose fine fiber material comprises the steps of: [Item 20] A step of producing a concentrate of a cellulose fine fiber dispersion by the method according to any one of items 1 to 18, or producing a dried cellulose fine fiber body by the method according to item 19; mixing the concentrate of the cellulose fine fiber dispersion or the dried cellulose fine fiber with a thermoplastic resin to produce a resin composition; A method for producing a resin composition comprising the steps of: Effect of the Invention
[0011] According to one aspect of the present invention, there can be provided a method for producing a cellulose fine fiber dispersion concentrate, which can produce a concentrate with little variation in cellulose fine fiber content with low environmental impact even when a dilute cellulose fine fiber dispersion is used, and a method for producing a resin composition using the concentrate. [Brief description of the drawings]
[0012] [Figure 1]FIG. 2 is a diagram illustrating an example of the arrangement of blades and grooves of a disc refiner. [Diagram 2] FIG. 2 is a diagram illustrating the blade width, groove width, and blade distance of a disc refiner. [Diagram 3] FIG. 2 is a diagram illustrating a configuration example of a continuous concentrating device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, exemplary embodiments of the present invention (hereinafter, abbreviated as "present embodiments") will be described, but the present invention is not limited to these embodiments. Note that, unless otherwise specified, the characteristic values of the present disclosure are values measured by the method described in the [Examples] section of the present disclosure or a method that is understood to be equivalent to the above by a person skilled in the art.
[0014] <Method for producing concentrated cellulose fine fiber dispersion> One aspect of the present invention provides a method for producing a concentrate of a cellulose fine fiber dispersion (also simply referred to as a concentrate in the present disclosure). In one aspect, the method includes a concentration step of deliquifying a cellulose fine fiber dispersion (also simply referred to as a dispersion in the present disclosure) to obtain a concentrate. In one aspect, in the concentration step, the cellulose fine fiber dispersion is continuously deliquified in a concentration device at a processing speed of 50 kg / h or more and less than 10,000 kg / h. In one aspect, the mass content of cellulose fine fibers in the cellulose fine fiber dispersion is 0.3 mass% to 5.0 mass%. In one aspect, the ratio of the mass content of cellulose fine fibers in the concentrate to the mass content of cellulose fine fibers in the cellulose fine fiber dispersion is 4 to 100. In one aspect, the average fiber diameter of the cellulose fine fibers in the cellulose fine fiber dispersion is 50 to 1,000 nm. In one aspect, the method may include a defibration step of beating and / or defibrating a cellulose raw material (e.g., pulp) in the dispersion to produce a cellulose fine fiber dispersion.
[0015] Cellulose microfibers are a material made mainly from cellulose naturally produced by plants, and their use is expected to provide sustainable industrial products with low environmental impact. One example is their use as a filler that is mixed with resin to enhance physical properties, but in order to mix with resin, it is necessary to remove water from the cellulose microfiber dispersion, which is produced as a dilute dispersion. Furthermore, while cellulose microfibers maintain a stable dispersion state in a dilute dispersion, when the dispersion medium is removed, the microfibers approach each other and are strongly bound by hydrogen bonds, making redispersion difficult, which can lead to defects in physical properties and non-uniform quality.
[0016] The present inventors have found that, in a specific embodiment, when a dispersion of cellulose fine fibers having a predetermined average fiber diameter is concentrated to a predetermined cellulose fine fiber content in a continuous deliquing device, the dispersion is easy to handle, and when used as a filler for filler-reinforced resin, good physical properties and uniform quality can be achieved with a low environmental load (i.e., without the need for wastewater treatment or the like, which has a high environmental load). If the ratio of the mass content of cellulose fine fibers in the concentrate to the mass content of cellulose fine fibers in the cellulose fine fiber dispersion (hereinafter also referred to as the concentration rate) is lower than an appropriate range, the cellulose fine fibers are likely to adhere to the deliquing device due to insufficient concentration, resulting in a decrease in the yield of the concentrate and the inclusion of solid foreign matter that has solidified while adhering to the device and is no longer redispersible in the concentrate. In addition, if the concentration rate is low, the fluidity of the dispersion during the concentration process is too high, which can result in a decrease in yield due to liquid flow, etc. On the other hand, if the concentration rate is higher than the appropriate range, the cellulose fine fiber content in the concentrate becomes too high, resulting in a decrease in redispersibility, or the concentration is so rapid that the cellulose fine fiber content in the concentrate varies from one part to another. In addition, if the concentration proceeds to a state close to dryness, the variation in the cellulose fine fiber content of the concentrate decreases, but the redispersibility decreases significantly. For example, in a batch-type deliquor device or a device that repeats batch operations, local unevenness in the cellulose fine fiber content occurs within the batch, which tends to cause problems such as a decrease in the physical properties of the filler-reinforced resin when the product is used as a filler, and a decrease in yield due to the elimination of non-standard products from the product in order to suppress the variation in the cellulose fine fiber content between batches. On the other hand, according to the method of this embodiment, it is possible to mass-produce a concentrate that maintains redispersibility and has little variation in the cellulose fine fiber content.
[0017] The method for producing a concentrate of a cellulose fine fiber dispersion according to the present embodiment includes a concentration step, typically including a defibration step and a concentration step. Each step will be described below.
[0018] <Defibration process> In this process, a cellulose raw material (e.g., cellulose-containing pulp) is beaten and / or defibrated in a dilute dispersion to obtain cellulose fine fibers. As the cellulose raw material, wood pulp obtained from wood species (broadleaf or coniferous trees), non-wood pulp obtained from non-wood species (bamboo, hemp-based fiber, bagasse, kenaf, linter, etc.), and refined pulp thereof (refined linter, etc.) can be used. As the non-wood pulp, cotton-derived pulp including cotton linter pulp, hemp-derived pulp, bagasse-derived pulp, kenaf-derived pulp, bamboo-derived pulp, straw-derived pulp, etc. can be used. The cotton-derived pulp, hemp-derived pulp, bagasse-derived pulp, kenaf-derived pulp, bamboo-derived pulp, and straw-derived pulp may each be a refined pulp obtained from raw materials such as cotton lint, cotton linters, hemp-based abaca (e.g., from Ecuador or the Philippines), sisal, bagasse, kenaf, bamboo, straw, etc., through a refining step such as delignification by cooking treatment, a bleaching step, etc. The cellulose raw material is preferably derived from cotton linters (e.g., pulp derived from cotton linters) in that it has a high degree of crystallinity and can produce cellulose fine fibers with excellent mechanical properties when used as a filler for filler-reinforced resin.
[0019] The cellulose fine fibers (in one embodiment, the cellulose fine fibers in the cellulose fine fiber dispersion) may be chemically modified. The chemical modification may be performed on the cellulose raw material (e.g., pulp) and / or on the cellulose fine fibers, but in a preferred embodiment, it is performed on the pulp. The chemical modification may be performed by introducing a hydrophilic substituent or a hydrophobic substituent, and may be appropriately selected depending on the application. Methods for introducing a hydrophilic substituent include TEMPO oxidation, carboxymethylation, phosphate esterification, and sulfate esterification. Methods for introducing a hydrophobic substituent include esterification (acylation), etherification, and silylation.
[0020] When the cellulose fine fibers are used as a filler for filler-reinforced resins, chemical modification to introduce a hydrophobic substituent into the cellulose is preferred, esterification is more preferred because it does not destroy the I-type crystal structure of natural cellulose and has good reactivity, and acetylation is particularly preferred from the viewpoint of ease of reaction and cost. Therefore, the hydrophobic substituent is preferably one or more selected from the group consisting of an acyl group, an ether group, and a silyl group, more preferably an acyl group, and particularly preferably an acetyl group. When the affinity between the cellulose fine fibers and the dispersion medium (particularly water) is reduced by chemical modification, particularly by the introduction of a hydrophobic substituent, the cellulose fine fibers are easily separated from the dispersion medium, but the concentrate obtained by the method of this embodiment, which has little variation in the cellulose fine fiber content, can exhibit a good effect of improving the physical properties and quality stability of the resin composition by chemical modification.
[0021] The esterification reaction may be carried out in a solvent in the presence of an esterifying agent. The solvent used in the esterification (also referred to as the esterification solvent in the present disclosure) may be an aprotic solvent, such as an alkyl sulfoxide, an alkyl amide, a pyrrolidone, or the like, which may be used alone or in combination of two or more.
[0022] Examples of alkyl sulfoxides include di-C alkyl sulfoxides such as dimethyl sulfoxide (DMSO), methyl ethyl sulfoxide, and diethyl sulfoxide. 1-4 Alkyl sulfoxides and the like.
[0023] Examples of alkylamides include N,N-diC alkylamides such as N,N-dimethylformamide (DMF) and N,N-diethylformamide. 1-4 Alkylformamides; N,N-diC such as N,N-dimethylacetamide (DMAc) and N,N-diethylacetamide 1-4 Alkylacetamides and the like.
[0024] Examples of pyrrolidones include pyrrolidones such as 2-pyrrolidone and 3-pyrrolidone; NC such as N-methyl-2-pyrrolidone (NMP); 1-4Alkylpyrrolidone and the like.
[0025] As the esterification solvent, dimethyl sulfoxide (DMSO) is particularly preferred from the viewpoint of obtaining good esterification efficiency.
[0026] As the esterification agent, acid halides, acid anhydrides, and vinyl carboxylates are preferred, and from the viewpoint of esterification efficiency, vinyl carboxylates are particularly preferred.
[0027] The acid halide may be at least one selected from the group consisting of compounds represented by the following formula: R 1 -C(=O)-X (In the formula, R 1 represents an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 24 carbon atoms, or an aryl group having 6 to 24 carbon atoms, and X is Cl, Br, or I.
[0028] Specific examples of acid halides include, but are not limited to, acetyl chloride, acetyl bromide, acetyl iodide, propionyl chloride, propionyl bromide, propionyl iodide, butyryl chloride, butyryl bromide, butyryl iodide, benzoyl chloride, benzoyl bromide, and benzoyl iodide. Among them, acid chlorides can be preferably used in terms of reactivity and handling. In addition, in the reaction of acid halides, one or more alkaline compounds may be added to act as a catalyst and neutralize the by-product acidic substances. Specific examples of alkaline compounds include, but are not limited to, tertiary amine compounds such as triethylamine and trimethylamine; and nitrogen-containing aromatic compounds such as pyridine and dimethylaminopyridine.
[0029] As the acid anhydride, any suitable acid anhydride can be used. For example, Anhydrides of saturated aliphatic monocarboxylic acids such as acetic acid, propionic acid, (iso)butyric acid, valeric acid, etc.; anhydrides of unsaturated aliphatic monocarboxylic acids such as (meth)acrylic acid, oleic acid, etc.; Anhydrides of alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid and tetrahydrobenzoic acid; Anhydrides of aromatic monocarboxylic acids such as benzoic acid, 4-methylbenzoic acid, etc.; Examples of dibasic carboxylic acid anhydrides include saturated aliphatic dicarboxylic acid anhydrides such as succinic anhydride and adipic acid, unsaturated aliphatic dicarboxylic acid anhydrides such as maleic anhydride and itaconic anhydride, alicyclic dicarboxylic acid anhydrides such as 1-cyclohexene-1,2-dicarboxylic acid anhydride, hexahydrophthalic anhydride and methyltetrahydrophthalic anhydride, and aromatic dicarboxylic acid anhydrides such as phthalic anhydride and naphthalic anhydride; Examples of polybasic carboxylic acid anhydrides having three or more bases include polycarboxylic acids (anhydrides) such as trimellitic anhydride and pyromellitic anhydride.
[0030] In addition, in the reaction of an acid anhydride, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.
[0031] The vinyl carboxylate may be represented by the following formula: R-COO-CH=CH2 Preferred is a vinyl carboxylate represented by the formula: {wherein R is any one of an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, and an aryl group having 6 to 24 carbon atoms.} The vinyl carboxylate is more preferably at least one selected from the group consisting of vinyl acetate, vinyl propionate, vinyl butyrate, vinyl caproate, vinyl cyclohexanecarboxylate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl myristate, vinyl palmitate, vinyl stearate, vinyl pivalate, vinyl octylate, divinyl adipate, vinyl methacrylate, vinyl crotonate, vinyl pivalate, vinyl octylate, vinyl benzoate, and vinyl cinnamate. In the esterification reaction with a vinyl carboxylate, one or more catalysts selected from the group consisting of alkali metal hydroxides, alkaline earth metal hydroxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal hydrogencarbonates, primary to tertiary amines, quaternary ammonium salts, imidazole and derivatives thereof, pyridine and derivatives thereof, and alkoxides may be added.
[0032] Examples of the alkali metal hydroxides and alkaline earth metal hydroxides include sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, barium hydroxide, etc. Examples of the alkali metal carbonates, alkaline earth metal carbonates, and alkali metal hydrogen carbonates include lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate, magnesium carbonate, calcium carbonate, barium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, cesium hydrogen carbonate, etc.
[0033] The primary, secondary and tertiary amines refer to primary, secondary and tertiary amines, and specific examples thereof include ethylenediamine, diethylamine, proline, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,3-propanediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, tris(3-dimethylaminopropyl)amine, N,N-dimethylcyclohexylamine, triethylamine and diazabicycloundecene.
[0034] Examples of imidazole and its derivatives include 1-methylimidazole, 3-aminopropylimidazole, and carbonyldiimidazole.
[0035] Examples of pyridine and its derivatives include N,N-dimethyl-4-aminopyridine and picoline.
[0036] Examples of the alkoxide include sodium methoxide, sodium ethoxide, and potassium t-butoxide.
[0037] The carboxylic acid may be at least one selected from the group consisting of compounds represented by the following formulas: R-COOH (In the formula, R represents an alkyl group having 1 to 16 carbon atoms, an alkenyl group having 2 to 16 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, or an aryl group having 6 to 16 carbon atoms.)
[0038] Specific examples of carboxylic acids include at least one selected from the group consisting of acetic acid, propionic acid, butyric acid, caproic acid, cyclohexane carboxylic acid, caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, pivalic acid, methacrylic acid, crotonic acid, pivalic acid, octylic acid, benzoic acid, and cinnamic acid.
[0039] Among these carboxylic acids, at least one selected from the group consisting of acetic acid, propionic acid, and butyric acid, and particularly acetic acid, is preferred from the viewpoint of reaction efficiency.
[0040] In addition, in the reaction of carboxylic acid, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.
[0041] Among these esterifying agents, at least one selected from the group consisting of acetic anhydride, propionic anhydride, butyric anhydride, vinyl acetate, vinyl propionate, vinyl butyrate, and acetic acid, and among these, acetic anhydride and vinyl acetate are preferred from the viewpoint of reaction efficiency.
[0042] The degree of substitution (DS) of the chemically modified cellulose raw material (e.g., pulp) or the chemically modified cellulose fine fibers, for example the degree of esterification of the esterified product, is in one aspect more than 0.5, or 0.6 or more, or 0.7 or more, from the viewpoint of obtaining chemically modified (e.g., esterified) cellulose fine fibers having excellent dispersibility in resins, heat resistance, etc., and in one aspect, is 2.0 or less, or 1.9 or less, or 1.8 or less, from the viewpoint of obtaining chemically modified (e.g., esterified) cellulose fine fibers having good mechanical properties inherent to cellulose upon defibration.
[0043] For example, the degree of esterification, which is the degree of substitution (DS) of the esterified product, can be calculated based on the peak intensity ratio between the peak derived from the acyl group and the peak derived from the cellulose skeleton from the reflection infrared absorption spectrum of the esterified cellulose raw material (e.g., pulp) or the esterified cellulose fine fiber (hereinafter, these are also collectively referred to as esterified cellulose). The peak of the absorption band of C=O based on the acyl group is at 1730 cm -1 The absorption band of CO based on the cellulose backbone appears at 1030 cm-1 The DS of esterified cellulose is calculated by plotting a correlation graph between the DS obtained from solid-state NMR measurement (described later) and the modification ratio (IR index 1030), which is defined as the ratio of the peak intensity of the absorption band of C=O based on the acyl group to the peak intensity of the absorption band of CO in the cellulose backbone chain, and then calculating the calibration curve from the correlation graph. Degree of substitution DS = 4.13 × IR index (1030) It can be found by using
[0044] In addition, when it is difficult to perform an appropriate measurement using the reflection infrared absorption spectrum, solid-state NMR is used. The DS calculation method using solid-state NMR is as follows for frozen and crushed esterified cellulose: 13 C solid-state NMR measurement was performed, and the intensity can be calculated using the area intensity (Inf) of a signal assigned to one carbon atom derived from the modifying group relative to the total area intensity (Inp) of signals assigned to carbons C1-C6 derived from the pyranose ring of cellulose, which appear in the range from 50 ppm to 110 ppm, using the following formula. DS = (Inf) x 6 / (Inp) For example, when the modifying group is an acetyl group, the signal at 23 ppm assigned to -CH3 may be used.
[0045] Use 13 The conditions for the C solid-state NMR measurement are, for example, as follows: Equipment:Bruker Biospin Avance500WB Frequency: 125.77MHz Measurement method: DD / MAS method Waiting time: 75sec NMR sample tube: 4mmφ Accumulation times: 640 times (approx. 14 hours) MAS: 14,500Hz Chemical shift reference: glycine (external reference: 176.03 ppm)
[0046] Known crystal forms of cellulose raw materials or cellulose fine fibers include type I, type II, type III, type IV, etc. Types I and II are widely used, while types III and IV are not widely used on an industrial scale. The crystal form of cellulose raw materials or cellulose fine fibers is preferably type I or type II, more preferably type I, in terms of high structural mobility, low linear expansion coefficient, and high tensile strength, bending strength, and bending elongation.
[0047] The crystallinity of the cellulose raw material or cellulose fine fibers may, in one embodiment, be 50% or more, or 60% or more, or 70% or more, or 73% or more, or 75% or more, and in one embodiment, be 95% or less, or 90% or less, or 85% or less. In one embodiment, the above crystallinity is that of cellulose type I.
[0048] In the present disclosure, when the cellulose is cellulose type I crystal (derived from natural cellulose), the degree of crystallinity is determined by the following formula using the Segal method from the diffraction pattern (2θ / deg. is 10 to 30) obtained by measuring a sample by wide-angle X-ray diffraction. Crystallinity (%)=[I(200)-I(amorphous)] / I(200)×100 I(200): Diffraction peak intensity due to the 200 plane (2θ=22.5°) in cellulose I crystals I (amorphous): The halo peak intensity due to amorphous in cellulose type I crystals, which is the peak intensity at an angle 4.5° lower than the diffraction angle of the 200 plane (2θ = 18.0°).
[0049] When the cellulose is cellulose II type crystal (derived from regenerated cellulose), the degree of crystallinity can be calculated from the absolute peak intensity h0 at 2θ=12.6° assigned to the (110) plane peak of cellulose II type crystal in wide-angle X-ray diffraction and the peak intensity h1 from the baseline at this interplanar spacing, according to the following formula: Crystallinity (%) =h1 / h0 ×100
[0050] In this step, cellulose raw material (e.g., pulp) is beaten and / or defibrated to produce cellulose fine fibers. In one embodiment, beating and / or defibration is performed in a solvent (also referred to as a defibration solvent in the present disclosure). For example, the cellulose raw material (e.g., pulp) is treated in a defibration solvent, typically in the form of a slurry, using a single disc refiner, double disc refiner, conical refiner, Niagara beater, PFI mill, or the like as a beating device, and a high-pressure homogenizer, microfluidizer, ball mill, bead mill, disc mill, wet type micronizer, or the like as a defibration device, to obtain cellulose fine fibers. These treatments may be used alone or in combination.
[0051] Examples of the defibration solvent include water, DMSO (dimethyl sulfoxide), DMF (dimethylformamide), DMAc (dimethylacetamide), NMP (N-methylpyrrolidone), acetic acid, etc. Two or more of these solvents may be mixed and used.
[0052] In addition, it is preferable to homogenously disperse the raw material in a defibration solvent using a pulper or homomixer before the beating and / or defibration treatment and then perform the micronization treatment. In particular, when the cellulose raw material is first chemically modified and then micronized, since the hydrophilicity of the cellulose raw material is reduced, it is preferable to perform the dispersion treatment using a mixer such as a homomixer having a peripheral speed of preferably 10 m / s or more, more preferably 20 m / s or more, more preferably 25 m / s or more, preferably 90 m / s or less, more preferably 80 m / s or less, and more preferably 50 m / s or less. By reducing lumps and the like as a pretreatment, homogenous cellulose fine fibers can be obtained by homogenous micronization treatment. When water is used as a solvent in this case, it may be effective to use highly pure water such as distilled water or ion-exchanged water.
[0053] When multiple beating and / or defibration processes are used in combination to produce cellulose fine fibers, it is effective to combine two or more processes with different fineness mechanisms or shear rates. As the above-mentioned multi-stage fineness method, it is preferable to use disc refiners with different disc configurations for multi-stage fineness, or to fineness using a disc refiner followed by fineness using a high-pressure homogenizer. Here, the disc refiner may be a single disc refiner, a double disc refiner, or a conical refiner, but in order to highly control the fineness, a single disc refiner with high clearance accuracy between the fixed blade and the rotary blade is preferred.
[0054] (Refining by disc refiner) When the fiber is refined using a disc refiner, for example, pulp or cotton-like refined cellulose fibers are dispersed and stored in a tank in a defibrating solvent to a solids concentration of 0.5% by mass to 6% by mass, preferably 0.8% by mass to 3.5% by mass, and more preferably 1% by mass to 3% by mass, and then the fiber is refined using the disc refiner. When water is used as the solvent in this case, it may be effective to use highly pure water such as distilled water or ion-exchanged water.
[0055] In operating the disc refiner, the defibration process may be performed in a continuous circulation process in which the slurry stored in a tank is returned to the original tank via the disc refiner. However, it is preferable to prepare two tanks (Tank A and Tank B) connected by piping via the disc refiner, and first transfer the slurry from Tank A to Tank B via the disc refiner and store it there. When the processing of the slurry in Tank A is completed, the process is switched to continuously transfer the slurry from Tank B to Tank A via the disc refiner and store it there. Thereafter, if the defibration process is performed in a continuous processing process in which these steps are repeated alternately, the slurry will be reliably passed through the disc refiner every time it is processed, and a uniform number of passes can be applied to the total amount of slurry, which is more preferable from the standpoint of the uniformity of the degree of defibration, i.e., the quality stability of the cellulose fine fibers.
[0056] Fig. 1 is a diagram for explaining an example of the arrangement of the blades and grooves of a disc refiner, and Fig. 2 is a diagram for explaining the blade width, groove width, and blade distance of a disc refiner. When multiple disc refiners are used for multi-stage refinement, it is preferable to use refiners having at least two different types of blades. With reference to Figs. 1 and 2, a specific blade configuration is as follows: in a disc refiner having blades 11 and grooves 12 as shown in Fig. 1, the blade width W B , groove width W G , and blade width W B The groove width W G It is important to appropriately adjust the value obtained by dividing the diameter of the fiber by the groove ratio (hereinafter referred to as the groove ratio). It is particularly preferable to carry out the refining process (hereinafter referred to as the front stage) using a refiner equipped with a blade having a blade width of 1.5 mm or more and 5 mm or less and a groove ratio of 0.1 to 1.0, and then carry out the refining process (hereinafter referred to as the rear stage) using a refiner equipped with a blade having a blade width of 0.1 mm or more and 1.0 mm or less and a groove ratio of 0.5 to 1.0. By defibrating the fiber using a disc refiner having such a configuration, the number of long and large fibers that cause aggregation in the resin is reduced, and cellulose fibers with a low fibrillation rate can be obtained. In this case, another refining process may be added between the front stage and the rear stage.
[0057] In addition, when a disk refiner is used in one stage using one type of blade, it is particularly preferable to carry out the fine processing with a refiner having a blade with a blade width of 0.1 mm or more and 1.0 mm or less and a blade groove ratio of 0.5 or more and 1.0 or less. In this case, the fiber length of the raw material used is preferably 500 μm or more, more preferably 700 μm or more, and even more preferably 900 μm or more, and preferably 3000 μm or less, more preferably 2000 μm or less, more preferably 1500 μm or less, and even more preferably 1300 μm or less, as the length-weighted average fiber length measured by an automatic fiber shape analyzer (specifically, Morfi Neo manufactured by Techpap). By using a raw material within this range, it is possible to efficiently reduce long and large fibers that cause aggregation in the resin in one stage and obtain cellulose fine fibers with a low fibril ratio.
[0058] (Blade distance in disc refiner processing) In addition, referring to FIG. 2, in the case of refinement using a disc refiner, the blade distance W between two blades (specifically, the rotary blade 21 and the fixed blade 22 in FIG. 2) is L It is important to control the clearance (hereinafter simply referred to as the blade distance). By controlling the blade distance, it is possible to control the fiber length and the degree of beating of the cellulose fibers. In the case of multi-stage processing, it is preferable that the blade distance is 0.05 mm or more and 0.5 mm or less in the first stage processing, and 0.05 mm or more and 0.3 mm or less in the second stage processing. In addition, in the case of processing in one stage, it is preferable that the blade distance is 0.05 mm or more and 0.3 mm or less. In addition, when adjusting the blade distance, it is preferable to gradually narrow the blade distance from a wide blade distance while suppressing the current value of the device below a certain value. By controlling in this way, clogging and overloading of the device can be prevented, and highly homogeneous cellulose fibers can be obtained.
[0059] In this way, in the cellulose refining treatment using a disc refiner, highly controlling the blade distance between the fixed blade and the rotary blade is advantageous in producing homogeneous cellulose fine fibers having good mechanical properties as a filler. For example, the blade distance adjustment of a conventionally used single disc refiner uses a screw-type screw jack or the like, and therefore there is play in the runner part that fixes the rotary blade. Therefore, if the runner part is pulled strongly in the thrust direction, it moves about 0.3 mm. Therefore, in order to obtain cellulose fine fibers with good accuracy and reproducibility, it is preferable that the movement amount (play) is small. In one embodiment, the movement amount (play) is preferably 0.10 mm or less, more preferably 0.08 mm or less, and even more preferably 0.05 mm or less. In addition, it is preferable that the precision of narrowing the blade gap is 5 μm or less, more preferably 3 μm or less, and most preferably 1 μm or less. In one embodiment, by using a ball screw type jack as the blade distance adjustment mechanism, a single disc refiner with the above-mentioned movement amount in the thrust direction of 0.03 mm can be used. Furthermore, a speed reducer can be attached to the ball screw jack to adjust the blade distance in 1 μm increments. In addition, any mechanism can be used, such as a combination of a ball screw jack and a servo motor, as long as it can obtain the amount of movement of the runner and the precision of narrowing the blade distance.
[0060] The use of a single disc refiner in this way enables highly accurate adjustment of the blade distance. It also makes it possible to maintain a constant blade distance without blade vibration during the refinement process, and prevents the fixed blade from coming into contact with the rotary blade when the blade distance is reduced. This prevents the fiber length of the cellulose fine fibers from becoming too short and reduces the number of coarse fibers that are insufficiently defibrated. As a result, cellulose fine fibers with a highly uniform shape distribution can be produced with good reproducibility, and the cellulose fine fibers become a filler that exhibits excellent mechanical properties when compounded with resin.
[0061] (Number of passes in disc refiner processing) The refining process can also be controlled by the number of times the cellulose fibers pass between the rotary blade and the fixed blade (hereinafter referred to as the number of passes). By increasing the number of passes, cellulose fibers with a uniform fiber diameter and fiber length distribution can be obtained. Here, the number of passes refers to the number of times the refining process is performed (passing between the rotary blade and the fixed blade) after the blade distance is reduced to the desired blade distance.
[0062] The number of passes through the disc refiner is preferably 5 or more, more preferably 20 or more, and even more preferably 40 or more. As the number of passes is increased, the distribution of fiber shapes gradually converges to a constant value, so the more passes the better, but taking productivity into consideration, the upper limit of the number of passes may be 300 or less.
[0063] (Method of determining refinement conditions using a disc refiner) The shape of the cellulose fine fibers obtained by the disc refiner treatment is controlled by the combined effects of the type of disc refiner blade, the blade distance, the number of passes, the concentration, and the like. In order to obtain a preferred shape of cellulose fibers when used in fiber-reinforced resins, it is preferable to increase the number of passes under viscous beating conditions. Viscous beating is a beating method that has a strong tendency to fluff and refine the fibers, while a beating method that has a strong tendency to cut the fibers is called free beating. As for the configuration of the disc refiner blades, the more the number of blades, the longer the blade length, the larger the ratio of the blade width to the groove width (blade groove ratio), and the larger the contact angle, the more the number of intersections between the rotating blade and the fixed blade increases, so that the force applied to the fiber at one intersection is dispersed, and the number of impacts on the fiber increases, which tends to result in viscous beating, and the opposite tendency to result in free beating. The blade distance of the disc refiner is preferably widened when a blade showing a tendency to beating in a free state is used, and is preferably narrowed when a blade showing a tendency to beating in a viscous state is used, but if the blade distance is too narrow, clogging occurs, the fibers are shortened due to cutting of the fiber length, and the fibers are too fine, resulting in a decrease in performance as a filler, so the blade distance is preferably 0.05 mm or more. The fiber shape, such as the average fiber diameter and fiber length distribution, can be controlled within a preferred range by adjusting the blade distance and / or the number of passes described above depending on the shape (fiber length and fiber diameter) of the cellulose raw material (e.g., pulp), the treatment concentration, and the blade used.
[0064] (Multi-stage refinement process using a combination of a disc refiner and a high-pressure homogenizer) It is also a preferred embodiment to subject the cellulose fibers refined by the disc refiner to further refinement treatment by a high-pressure homogenizer. The high-pressure homogenizer has a greater effect of thinning the fibers than the disc refiner. The high-pressure homogenizer treatment is preferably carried out at a pressure of 30 MPa or more, more preferably 50 MPa or more, and more preferably 80 MPa or more. The upper limit may be 300 MPa or less, 250 MPa or less, or 150 MPa or less, depending on the characteristics of the device.
[0065] Examples of high-pressure homogenizers include the NS-type high-pressure homogenizer from Nilo Soavi (Italy), the Lanier-type (R model) pressure homogenizer from SMT Co., Ltd., and the high-pressure homogenizer from Sanwa Machine Co., Ltd., and examples of ultra-high-pressure homogenizers include high-pressure collision type micronization machines such as the Microfluidizer from Mizuho Kogyo Co., Ltd., the Nanomizer from Yoshida Kikai Kogyo Co., Ltd., and the Ultimizer from Sugino Machine Co., Ltd., but other devices may also be used as long as they perform micronization using a mechanism similar to that of these devices.
[0066] In the high-pressure homogenizer treatment, as in the disc refiner treatment, the defibration treatment can be performed using a continuous circulation process in which the slurry stored in a tank is returned to the original tank via the high-pressure homogenizer. However, it is preferable to prepare two tanks connected by piping via a high-pressure homogenizer (Tank A and Tank B), and first transfer the slurry from Tank A to Tank B via the high-pressure homogenizer and store it there. When the processing of the slurry in Tank A is completed, the slurry is continuously transferred from Tank B to Tank A via the high-pressure homogenizer and stored there. If the defibration treatment is performed using a continuous processing process in which these steps are repeated alternately, the slurry will be reliably passed through the high-pressure homogenizer every time it is treated, and a uniform number of passes can be applied to the total amount of slurry, which is more preferable from the viewpoint of the uniformity of the degree of defibration, i.e., the quality stability of the cellulose fine fibers.
[0067] <Concentration process> In this step, for example, the dispersion of cellulose fine fibers defibrated in the defibration step is drained to obtain a concentrate. In a preferred embodiment, in the concentration step, the cellulose fine fiber dispersion is suction deliquified to produce an intermediate concentrate, and the intermediate concentrate is press deliquified to produce a concentrate. In this way, after suction deliquifying is performed under relatively mild conditions to produce an intermediate concentrate having a relatively low cellulose fine fiber content, the intermediate concentrate can be further concentrated by press deliquifying to produce a concentrate having a desired cellulose fine fiber content. When suction deliquifying is performed under mild conditions, the cellulose fine fibers are likely to be entangled with each other, and a cake layer that is not easily disintegrated (i.e., strong) can be formed. Such a strong cake layer contributes to improving the yield of the concentrate and the process efficiency of the concentration step because it is difficult to penetrate the filter substrate described below, is not easily deformed during press deliquifying, and is not easily escaped from the press roll described below (i.e., liquid pools are not easily formed on the side of the roll). The combination of suction deliquifying and press deliquifying is also advantageous in terms of reducing the size of the entire concentration device.
[0068] As the cellulose fine fiber dispersion, the cellulose fine fiber slurry obtained in the defibration step can be used as it is or after dilution. As the dilution solvent, the same solvents as those exemplified above as the defibration solvent can be exemplified, and more preferably water or a mixed solvent of water and one or more of the organic solvents exemplified as the defibration solvent.
[0069] The mass content of the cellulose fine fibers in the cellulose fine fiber dispersion supplied to the concentration step is, in one embodiment, 0.3% by mass or more, or 0.5% by mass or more, or 0.7% by mass or more, or 1.0% by mass or more, or 1.5% by mass or more, and in one embodiment, 5.0% by mass or less, or 4.0% by mass or less, or 3.0% by mass or less, or 2.5% by mass or less. When the mass content of the cellulose fine fibers in the dispersion is equal to or more than the above lower limit, the membrane does not become too thin during the process of concentrating the liquid membrane of the dispersion to form a concentrate, so that pinholes are unlikely to occur, and the concentration proceeds while maintaining a uniform state. In addition, when the dispersion is concentrated on a filtration member described later, if the mass content of the cellulose fine fibers is equal to or more than the above lower limit, the cellulose fine fibers are likely to be entangled with each other and therefore are unlikely to pass through the filtration substrate, so that a cake layer that is difficult to flow can be formed, which is advantageous for improving the yield of the concentrate and the process efficiency of the concentration step. On the other hand, when the mass content of the cellulose fine fibers is equal to or less than the upper limit, the thixotropy or viscosity of the dispersion does not become too high, so that the liquid thickness of the dispersion tends to be uniform and the mass content of the cellulose fine fibers in the concentrate is less likely to vary.
[0070] A concentrating device (more specifically, a deliquing device) for concentrating a cellulose fine fiber dispersion is advantageously a continuous type from the viewpoint of reducing the variation in the mass content of cellulose fine fibers in the concentrate of the cellulose fine fiber dispersion. The concentrating device is provided with a concentrating mechanism for receiving and deliquifying the cellulose fine fiber dispersion. An example of the concentrating mechanism is a combination of a filter substrate on which the cellulose fine fiber dispersion is held, and a suction section that deliquifies the cellulose fine fiber dispersion on the filter substrate by reducing the pressure from the filter substrate side. Other examples of the concentrating mechanism include a method of deliquifying the cellulose fine fiber dispersion on the filter substrate by gravity, a method of squeezing the cellulose fine fibers between two filter substrates, a method of squeezing the cellulose fine fibers between a press roll and a press belt to press deliquify, and a method of deliquifying by squeezing and shearing with a cylindrical screen and a screw inside the cylinder. The concentrating mechanism, which is a combination of the filter substrate and the suction section, is preferable in that it is less likely to leak from the end of the filter substrate and that even a dilute dispersion with high fluidity can be concentrated. The concentrating mechanism, which is a combination of the press roll and the press belt, is preferable in that the degree of concentration can be easily adjusted and a concentrate with little variation in the cellulose fine fiber content can be produced. The procedure of the method of this embodiment will be described below using a continuous concentrating device equipped with these concentrating mechanisms as an example.
[0071] In a preferred embodiment, the concentration step comprises: a tank for storing a cellulose fine fiber dispersion; A dispersion liquid temporary storage section having a slit and connected to the tank; a filtration substrate that carries and travels with a cellulose fine fiber dispersion received from a dispersion temporary storage section through a slit; a suction section for sucking and deliquifying the cellulose fine fiber dispersion on the filtration substrate via the filtration substrate to produce an intermediate concentrate; A press roll and a press belt which sandwich the intermediate concentrate and press-deliquify it to produce a concentrate; In one embodiment, the concentrator is a continuous concentrator. 3 is a diagram illustrating a configuration example of a continuous concentrating apparatus. In one embodiment, the continuous concentrating apparatus 300 includes a tank 301 for storing a cellulose fine fiber dispersion D, a pump 302, a dispersion temporary storage section 303, a suction section 304, a filtration substrate 305, feed mechanisms 306a, 306b, 306c, and 306d, a press section including a press roll 307 and a press belt 308, a scraper 310, and a collection container 311.
[0072] The pump 302 supplies the cellulose fine fiber dispersion from the tank 301 to the dispersion temporary storage section 303 via the feed line L1. Examples of the pump 302 include a piston pump, a diaphragm pump, a plunger pump, a mono pump, a hose pump, a rotary pump, etc. A mono pump, which is non-pulsating and has excellent constant volume liquid delivery, is preferably used.
[0073] The temporary dispersion storage section 303 temporarily stores the cellulose fine fiber dispersion D in order to supply the dispersion D in a controlled amount onto the filtration substrate 305. The slit S is an outlet for the cellulose fine fiber dispersion onto the filtration substrate 305. The slit S may be a blade with a gap adjusted according to the desired thickness of the dispersion. The gap may be adjusted so that the thickness of the dispersion is, in one embodiment, 0.5 mm or more, or 1.0 mm or more, or 1.5 mm or more, and in one embodiment, 20.0 mm or less, or 19.0 mm or less, or 18.0 mm or less.
[0074] The volume of the temporary dispersion liquid storage section 303 can be designed appropriately depending on the purpose, but in one embodiment, it may be 50 L or more, or 60 L or more, or 70 L or more, and in another embodiment, it may be 150 L or less, or 140 L or less, or 130 L or less.
[0075] The filtration substrate 305 has a cellulose fine fiber dispersion placed thereon, and is run over the suction section 304 by means of feed mechanisms 306a, 306b, 306c, and 306d that continuously feed and / or circulate the filtration substrate 305. The cellulose fine fiber dispersion is deliquified under reduced pressure on the suction section 304 to produce an intermediate concentrate IC. While held on the filtration substrate 305, the intermediate concentrate IC is press-deliquified by a press roll 307 and a press belt 308 to produce a concentrate C. After being separated from the press roll 307 by a scraper 310, the concentrate C peels off from the filtration substrate 305 and is collected in a collection container 311.
[0076] Compared with the procedure of directly supplying the cellulose fine fiber dispersion to the filtration substrate 305 via the pump 302, the procedure of supplying the cellulose fine fiber dispersion via the slit S of the dispersion temporary storage section 303 allows the cellulose fine fiber dispersion to be supplied onto the filtration substrate 305 in a state of lower fluidity (high cellulose fine fiber content in one embodiment) and / or at a higher supply speed. In other words, the use of the dispersion temporary storage section 303 is advantageous in setting the mass content of cellulose fine fibers in the cellulose fine fiber dispersion relatively high (for example, 0.3 mass % or more, or 0.5 mass % or more, or 1.0 mass % or more).
[0077] From the viewpoint of uniformity of the concentrate, it is preferable to supply the cellulose fine fiber dispersion liquid stirred at a peripheral speed of 0.01 m / sec or more and 6.00 m / sec or less to the concentration step. For example, the tank 301 is preferably equipped with a stirring device 312 that stirs the dispersion liquid to keep the concentration uniform. The stirring device 312 may have a configuration in which a stirring blade 312b is attached to a stirrer 312a. The stirring speed when stirring the dispersion liquid is preferably a peripheral speed of 0.01 m / sec or more, or 0.05 m / sec or more, or 0.10 m / sec or more, or 0.25 m / sec or more, or 0.50 m / sec or more, or 0.70 m / sec or more, or 1.00 m / sec or more, or 1.50 m / sec or more, and preferably 6.00 m / sec or less, or 5.00 m / sec or less, or 4.00 m / sec or less, or 3.00 m / sec or less. When the peripheral speed is equal to or higher than the lower limit, concentration distribution due to flocculation or settling of cellulose fine fibers inside the tank is unlikely to occur, and concentration is uniform.When the peripheral speed is equal to or lower than the upper limit, problems such as foam generation due to stirring, splashing of the dispersion liquid and adhesion to a position above the liquid level in the tank, and solid matter that has dried and lost redispersibility falling off and becoming mixed in, resulting in non-uniform concentration, are unlikely to occur.
[0078] On the other hand, in a preferred embodiment, the tank 301 may not have a stirring mechanism. For example, the cellulose fine fiber dispersion overflowing from the dispersion temporary storage section 303 may be returned to the tank 301 through the return line L2, thereby circulating the cellulose fine fiber dispersion between the tank 301 and the dispersion temporary storage section 303. This makes it possible to maintain the cellulose fine fiber dispersion in the tank 301 in a stirred state even if the tank 301 does not have a stirring mechanism. The cellulose fine fiber dispersion from the return line L2 may be allowed to flow into the tank 301 from any position that can provide stirring to the dispersion in the tank 301.
[0079] The ratio of the flow rate (kg / hr) of the return line L2 to the flow rate (kg / hr) of the feed line L1 may be, in one embodiment, 10% or more, or 11% or more, or 12% or more, and in one embodiment, 30% or less, or 29% or less, or 28% or less.
[0080] [Suction dehydration] In the suction deliquation, the cellulose fine fiber dispersion D on the filtration substrate 305 is suction-deliquated by the suction part 304 via the filtration substrate 305, thereby causing solid-liquid separation and obtaining an intermediate concentrate IC.
[0081] The filtering substrate 305 may be any substrate that is permeable to the solvent but can retain the cellulose fine fibers, and may be a wire (net), or a porous material such as a woven or nonwoven fabric. The wire may be made of metal or plastic. The porous material may be made of unmodified cellulose, modified cellulose, regenerated cellulose, polyester, polypropylene, polyethylene, polyamide, glass fiber, or a combination of a plurality of materials, such as a mixed sheet. These filtering substrates may be used alone, or two or more substrates may be laminated. Examples of filtering substrates include TETEXMONODLW07-8435-SK010 (made of PET (polyethylene terephthalate)) manufactured by SEFAR (Switzerland), LTT-9FE (made of polyester) manufactured by Nippon Filcon, NT20 (PET / nylon blend) and TT30 (made of PET) manufactured by Shikishima Canvas, and ultra-strong Japanese paper manufactured by Nakamura Seishisho, but are not limited thereto.
[0082] The filtering substrate 305 may be held on a support (not shown) such as a wire, or when two or more filtering substrates are used in a laminated form, a filtering substrate different from the filtering substrate 305 may be used as the support. However, in a typical embodiment, the filtering substrate 305 is used without a support. In a preferred embodiment, the filtering substrate 305 is an endless substrate without a support. The filtering substrate 305, which is an endless substrate, may be continuously circulated by the feed mechanisms 306a, 306b, 306c, 306d, for example by roll drive.
[0083] When the filtration substrate is an endless substrate, it is preferable to carry out a cleaning treatment in which at least the dispersion-mounted surface of the filtration substrate is cleaned by liquid cleaning and / or physical scraping. The cleaning treatment can suppress clogging of the filtration substrate. The liquid used for cleaning may be water or the like. In one embodiment, a cleaning mechanism 313 may be provided in the middle of the circulation path of the endless substrate. When the cleaning mechanism 313 is a liquid cleaning mechanism, the cleaning waste liquid may be discharged outside the system via a waste liquid tank (not shown). Instead of or in combination with the liquid cleaning mechanism, a cleaning mechanism (e.g., a brush, spatula, etc.) that performs a physical scraping operation may be provided.
[0084] By continuously concentrating a cellulose fine fiber dispersion using a continuous (i.e., non-batch) concentrating device equipped with the above-mentioned feed mechanism, it is possible to reduce fluctuations in the mass content of cellulose fine fibers in the dispersion immediately after the start of concentration and immediately before the end of concentration, as well as variations in the mass content of cellulose fine fibers in the concentrate, thereby improving the uniformity of the concentrate.
[0085] The suction section 304 deliquifies (desolvents) the cellulose fine fiber dispersion on the filtration substrate 305 by reducing the pressure, thereby concentrating it. The suction section 304 may have two or more sections with different degrees of reduced pressure. In a typical embodiment, the suction section 304 has two or more reduced pressure sections with different degrees of reduced pressure that are adjusted to increase in the running direction of the filtration substrate 305. Such two or more sections are preferable in that they allow the cellulose fine fiber dispersion to be concentrated with high accuracy so as to produce a concentrate with less variation in the cellulose fine fiber content. The pressure reduction in the suction section may be performed by a pressure reduction mechanism 304a.
[0086] In the suction deliquation, in the early stage when the mass content of the cellulose fine fibers in the dispersion is low, it is advantageous to set the degree of decompression relatively low from the viewpoint of suppressing the passage of the cellulose fine fibers through the filter substrate to achieve a good yield and promoting entanglement between the cellulose fine fibers to reduce the fluidity of the dispersion. On the other hand, in the later stage when the mass content of the cellulose fine fibers is high, it is advantageous to set the degree of decompression relatively high from the viewpoint of efficiently increasing the mass content of the cellulose fine fibers to produce an intermediate concentrate with low fluidity. By reducing the pressure in such a plurality of compartments, an intermediate concentrate that is a strong cake layer can be formed. When the intermediate concentrate has low fluidity, the intermediate concentrate is unlikely to flow to the side of the press roll to form a liquid pool when pressed by the press roll, and therefore the concentrate can be obtained in high yield.
[0087] The number of sections with different decompression degrees is preferably 2 or more, or 3 or more, from the viewpoint of the concentrate yield and reduction in fluidity of the intermediate concentrate, and is preferably 5 or less, or 4 or less, from the viewpoint of process efficiency.
[0088] In a preferred embodiment, the filtration substrate 305 runs on the suction portion 304 at an upward gradient of 10° to 45°. Such an upward gradient is preferred from the viewpoint of maintaining a uniform liquid thickness of the dispersion liquid on the filtration substrate 305. The angle of the upward gradient is preferably 10° or more, or 15° or more, or 20° or more, and preferably 45° or less, or 40° or less, or 35° or less, or 30° or less.
[0089] In the concentration step, the treatment speed for concentrating the cellulose fine fiber dispersion is, in one embodiment, 50 kg / h or more, or 100 kg / h or more, or 150 kg / h or more, or 200 kg / h or more, and in one embodiment, less than 10,000 kg / h, or 8,000 kg / h or less, or 5,000 kg / h or less, from the viewpoints of productivity and reducing the variation in the mass content of the cellulose fine fibers in the concentrate. The treatment speed may be determined from the weight of the concentrate produced per unit time. Specifically, the mass content of the cellulose fine fibers in the concentrate collected from the collection container 311 is measured and calculated using an infrared (IR) moisture meter. However, when the dispersion medium contains an organic solvent, the cellulose fine fiber content is calculated from the weight of the solid matter dried in a vacuum dryer from the viewpoint of safety. By performing concentration at a treatment speed within the above range, the fiber size distribution of the cellulose fine fibers (for example, the fiber size distribution of the cellulose fine fibers in the thickness direction of the intermediate concentrate produced on the filtration substrate) becomes uniform. When the treatment speed is equal to or higher than the lower limit, the cellulose fine fibers having a large fiber diameter and / or fiber length are less likely to settle, resulting in uniform deliquation (particularly suction deliquation in the suction section), which is preferable.When the treatment speed is equal to or lower than the upper limit, deliquation is performed well, which reduces adhesion of the concentrate to the device, increases the recovery rate, and reduces variation in the cellulose fine fiber content of the concentrate.
[0090] The above-mentioned processing speed can be controlled within a predetermined range by adjusting, for example, the width of the filtration substrate 305 (i.e., the dimension in the direction perpendicular to the traveling direction), the temperature, the degree of reduced pressure applied by the suction unit 304, the supply speed of the dispersion liquid, the traveling speed of the filtration substrate 305, etc. At this time, continuing the stirring state in the tank 301 in order to maintain the uniformity of the dispersion liquid throughout the concentration process is useful in terms of reliably controlling the processing speed within a desired range. In a preferred embodiment, the above-mentioned processing speed may be controlled by a combination of adjusting the slit width of the slit S in the dispersion liquid temporary storage unit 303 (hence the liquid thickness of the dispersion liquid) to adjust the dispersion liquid supply speed and adjusting the traveling speed of the filtration substrate 305.
[0091] The ratio of the mass content of cellulose fine fibers in the intermediate concentrate to the mass content of cellulose fine fibers in the cellulose fine fiber dispersion is preferably 3 or more, or 3.5 or more, from the viewpoint of forming the intermediate concentrate as a strong cake layer to improve concentrate yield and process efficiency, and is preferably 5 or less, or 4.5 or less, from the viewpoint of obtaining an intermediate concentrate with little variation in cellulose fine fiber content by performing suction deliquescence under relatively mild conditions.
[0092] The mass content of cellulose fine fibers in the intermediate concentrate is preferably 2 mass% or more, or 3 mass% or more, or 5 mass% or more, from the viewpoint of forming the intermediate concentrate as a strong cake layer to improve concentrate yield and process efficiency, and is preferably 20 mass% or less, or 18 mass% or less, or 15 mass% or less, or 12 mass% or less, or 10 mass% or less, or 7 mass% or less, or 5 mass% or less, from the viewpoint of obtaining an intermediate concentrate with less variation in cellulose fine fiber content by performing suction deliquescence under relatively mild conditions.
[0093] [Press deliquification] In the press deliquification, the intermediate concentrate IC deposited on the filtration substrate 305 is press-deliquified to obtain a concentrate C. In one embodiment, the intermediate concentrate is sandwiched between a press roll 307 and a press belt 308 and press-deliquified to produce a concentrate C. The concentrate C may be collected by a method such as providing a scraper 310 in the running direction of the filtration substrate 305 to scrape off the concentrate. Alternatively, the concentrate C may be collected by directly scraping it off from the filtration substrate 305.
[0094] In a preferred embodiment, the press roll 307 presses and deliquifies the intermediate concentrate IC together with the press belt 308 in a region where the roll angle θ is 30° to 180°. The roll angle θ can be adjusted by changing the arrangement of the press belt 308 along the press roll 307 as desired by the arrangement of the belt drive units 309a, 309b, and 309c. The roll angle involved in the press deliquification is preferably 30° or more, or 60° or more, or 90° or more, or 120° or more, or 150° or more, or 180° or more from the viewpoint of easily obtaining a concentrate having a desired or higher cellulose fiber content by smoothly progressing the deliquification, and is preferably 270° or less, or 250° or less, or 240° or less, or 230° or less from the viewpoint of obtaining a concentrate having excellent redispersibility by preventing the cellulose fiber content of the concentrate from becoming excessively high.
[0095] The pressing pressure applied to the intermediate concentrate IC may be controlled by adjusting the gap width between the press roll 307 and the press belt 308. In addition, the positions of the feed mechanisms 306b and 306c may be adjusted to make them function as tension rolls, so that the intermediate concentrate IC before and after the press deliquification is pressed against the press roll 307 by the filtration substrate 305. This allows additional squeezing of the intermediate concentrate IC before and after the press deliquification. For example, the degree of additional squeezing may be adjusted by changing the length of the filtration substrate from the end of the region where the press roll 307 and the press belt 308 face each other to the tension roll as desired.
[0096] The diameter of the press roll 307 can be appropriately selected according to the purpose in combination with the setting of the roll angle θ so as to achieve the desired degree of press deliquation. From the viewpoint of obtaining a good effect of press deliquation, in one embodiment, the diameter may be 100 to 600 mm.
[0097] The ratio of the mass content of cellulose fines in the concentrate to the mass content of cellulose fines in the cellulose fine fiber dispersion is, in one aspect, 4 or more, or 5 or more, or 8 or more, or 10 or more, from the viewpoint of preventing the cellulose fine fiber content of the concentrate from becoming excessively low, thereby preventing the cellulose fines that have solidified while adhering to the equipment from being mixed into the concentrate as solid foreign matter, and in one aspect, is 100 or less, or 90 or less, or 80 or less, or 70 or less, or 60 or less, or 50 or less, or 40 or less, or 30 or less, from the viewpoint of obtaining good redispersibility of the cellulose fines by preventing the cellulose fine fiber content of the concentrate from becoming excessively high.
[0098] The mass content of cellulose fine fibers in the concentrate is preferably 5% by mass or more, or 8% by mass or more, or 10% by mass or more, or 15% by mass or more, from the viewpoint of suppressing a decrease in the yield of the concentrate due to adhesion of the cellulose fine fibers to the deliquor device, and from the viewpoint of reducing the inclusion of solid foreign matter that has solidified while adhering to the device into the concentrate; and is preferably 30% by mass or less, or 25% by mass or less, or 20% by mass or less, from the viewpoint of obtaining good redispersibility of the cellulose fine fibers and preventing excessive adhesion between the concentrate and the filtration substrate, thereby facilitating recovery.
[0099] In one embodiment, the CV value (coefficient of variation) of the mass content of the cellulose fine fibers in the concentrate is 0.001 or more, or 0.005 or more, or 0.010 or more, or 0.020 or more, or 0.050 or more, or 0.070 or more, or 0.090 or more, and preferably 0.300 or less, or 0.250 or less, or 0.200 or less, or 0.150 or less, or 0.100 or less. When the CV value is within the above range, the concentrate is excellent in quantitativeness even though it still contains a large amount of dispersion medium. Therefore, when the concentrate is used as a raw material for producing a filler for resin reinforcement, and when the filler is used to produce a filler-reinforced resin, the amount of cellulose fine fibers can be accurately controlled, so that the quality of the filler-reinforced resin can be stabilized when mass-producing the filler-reinforced resin, and defective products can be reduced. If the cellulose fine fibers are dried, i.e., if the amount of dispersing medium such as water is very small, the variation in the cellulose fine fiber content will decrease, making it possible to reduce the CV value. However, in terms of the redispersibility of the cellulose fine fibers in subsequent processes, it is advantageous to handle them in a concentrated form.
[0100] In the present disclosure, the mass content of cellulose fine fibers in a concentrate or intermediate concentrate is a number average value obtained by sampling 10 samples of the concentrate or intermediate concentrate at any timing during the continuous concentration process and measuring the mass content of cellulose fine fibers in each sample with an IR moisture meter (however, when the dispersion medium contains an organic solvent, a vacuum dryer is used). The CV value is calculated according to the following formula by determining the number average value and standard deviation of the mass content based on the above measurement. CV value = standard deviation / number average value In one embodiment, sampling is performed at 15-minute intervals. However, when the continuous operation time is shorter than 150 minutes, sampling is performed at 1 / 10 of the continuous operation time. For example, when the continuous operation time is 100 minutes, sampling is performed at 10-minute intervals.
[0101] The concentration step is preferably performed at 80°C or less, more preferably at 70°C or less, even more preferably at 60°C or less, and particularly preferably at 50°C or less. When the temperature of the concentration step is maintained at or below the upper limit, drying from the surface of the concentrate of the cellulose fine fiber dispersion can be suppressed, and the variation in the cellulose fine fiber content can be reduced. In this case, the aggregation of the cellulose fine fibers due to excessive drying of the concentrate can be prevented, and the redispersibility can be maintained well. The lower limit of the temperature of the concentration step is preferably 5°C or more, more preferably 10°C or more, and even more preferably 20°C or more. When the temperature of the concentration step is maintained at or above the lower limit, the refrigerant temperature can be suppressed from falling below the set temperature in order to lower the temperature of the entire system, so that the dispersion medium such as water that is locally cooled too much is unlikely to freeze. If the dispersion medium freezes, aggregation of the cellulose fine fibers occurs during thawing, and the redispersibility decreases, so it is preferable to avoid freezing of the dispersion medium. In addition, when the temperature of the concentration step is adjusted by a heating mechanism such as hot air, infrared rays, or microwaves, the temperature during heating is measured. When the temperature is not adjusted by a heating mechanism, the temperature is evaluated as the temperature of the cellulose fine fiber dispersion in the tank and the temperature of the concentrate of the cellulose fine fiber dispersion immediately after deliquification.
[0102] <Method for producing dried cellulose fine fiber body> One aspect of the present invention provides a method for producing a dried cellulose fine fiber body, the method comprising the steps of producing a concentrate of a cellulose fine fiber dispersion by the method of the present disclosure, and drying the concentrate to produce a dried cellulose fine fiber body. Such a dried body is preferable because it can be easily mixed with a resin in the production of a resin composition containing cellulose fine fibers and a resin.
[0103] For drying the concentrate, drying devices such as kneaders, planetary mixers, Henschel mixers, high-speed mixers, propeller mixers, ribbon mixers, single- or twin-screw extruders, Banbury mixers, freeze dryers, shelf dryers, spray dryers, and fluidized bed dryers can be used. For example, when a dried body containing an additional component (e.g., a dispersant exemplified in the present disclosure) is added to the concentrate and then dried, dynamic dryers such as extruders, mixers, spray dryers, and fluidized bed dryers are preferred from the viewpoint of uniformly dispersing the additional component in the dried body, and extruders and mixers that can easily stir and knead even high-viscosity materials are preferred from the viewpoint of productivity. Granulation may also be performed during drying to form a particle shape of the desired size.
[0104] The drying temperature may be, for example, 20° C. or more, or 30° C. or more, or 40° C. or more, or 50° C. or more from the viewpoint of obtaining a dried body having excellent drying efficiency and dispersibility in resin, and may be, for example, 160° C. or less, or 150° C. or less, or 140° C. or less, or 130° C. or less, or 100° C. or less from the viewpoint of preventing thermal deterioration of the cellulose fine fibers and additional components. The drying temperature is the temperature of the heat source in contact with the concentrate, and is defined, for example, by the surface temperature of the temperature-control jacket of the drying device, the surface temperature of the heating cylinder, the temperature of the hot air, etc.
[0105] The pressure during drying may be atmospheric pressure or reduced pressure, but from the viewpoint of obtaining a dried body having excellent drying efficiency and dispersibility in resin, it may be -1 kPa or less, or -10 kPa or less, or -20 kPa or less, or -30 kPa or less, or -40 kPa or less, or -50 kPa or less, and from the viewpoint of avoiding excessive pulverization of the dried body due to rapid drying of the concentrate, it may be -100 kPa or more, or -95 kPa or more, or -90 kPa or more. The pressure may be adjusted by a method of fully operating a reduced pressure pump having an appropriate exhaust capacity, a method of intentionally introducing air and / or an inert gas using a vacuum regulator, a leak valve, or the like, or the like.
[0106] In one aspect, the residence time of the concentrate in the drying process at a temperature of 40°C to 100°C may be, for example, 30 minutes to 600 minutes, or 45 minutes to 300 minutes, or 60 minutes to 200 minutes.
[0107] In one aspect, the dried cellulose microfiber may be in the form of particles. In this case, the average particle size is preferably 1 μm or more, or 10 μm or more, or 50 μm or more, or 100 μm or more, or 200 μm or more, or 500 μm or more, and preferably 5000 μm or less, or 4000 μm or less, or 3000 μm or less, or 2000 μm or less. The above average particle size is a value measured by the laser diffraction / scattering method.
[0108] <BET specific surface area> In one aspect, from the viewpoint of the dispersibility of the dried cellulose microfiber in the resin composition, the BET specific surface area of the dried cellulose microfiber is preferably 1 m 2 / g or more, or 3 m 2 / g or more, or 5 m 2 / g or more, or 8 m 2 / g or more, or 10 m 2 / g or more, or 12 m 2 / g or more, and from the viewpoint of the ease of manufacturing the dried product, it is preferably 50 m 2 / g or less, or 40 m 2 / g or less, or 30 m 2 / g or less, or 25 m 2 / g or less, or 20 m 2 / g or less. The specific surface area is measured by a specific surface area and pore size distribution measuring device (for example, Nova-4200e, manufactured by Quantachrome Instruments). After drying about 0.2 g of the dried product under vacuum at 120°C for 5 hours, the nitrogen gas adsorption amount at the boiling point of liquid nitrogen is measured at 5 points in the range of relative vapor pressure (P / P0) of 0.05 or more and 0.2 or less (multi-point method), and then the BET specific surface area (m 2 / g) is obtained by calculating with the device program.
[0109] ≪Properties of Cellulose Raw Material and Cellulose Microfiber≫ Hereinafter, exemplary aspects of the characteristics of the cellulose raw material and cellulose fine fibers of the present disclosure will be described. Unless otherwise specified, the following characteristics may be characteristics related to the cellulose fine fibers in the cellulose fine fiber dispersion of the present disclosure (sometimes referred to as the cellulose fine fibers before concentration in the present disclosure), the cellulose fine fibers in the intermediate concentrate of the present disclosure (sometimes referred to as the cellulose fine fibers after intermediate concentration in the present disclosure), the cellulose fine fibers in the concentrate of the present disclosure (sometimes referred to as the cellulose fine fibers after concentration in the present disclosure), or the cellulose fine fibers in the dry body of the present disclosure.
[0110] In one embodiment, the average fiber diameter of the cellulose fine fibers is 50 to 1000 nm, preferably 55 nm or more, or 60 nm or more, or 65 nm or more, or 70 nm or more, or 75 nm or more, and preferably 900 nm or less, or 800 nm or less, or 700 nm or less, or 600 nm or less, or 500 nm or less. When the average fiber diameter of the cellulose fine fibers is within the above range, not only unmodified cellulose fine fibers but also cellulose fine fibers whose surface hydrophobicity has been increased by chemical modification can be concentrated with less variation in the cellulose fine fiber content. When the average fiber diameter is equal to or greater than the above lower limit, the water retention is not too high, making it easy to remove the cellulose fine fiber from the cellulose fine fiber dispersion, and clogging of the concentrating device and a decrease in the recovery rate are unlikely to occur. On the other hand, when the average fiber diameter is equal to or less than the above upper limit, the cellulose fine fibers are unlikely to settle in the dispersion, so that concentration unevenness due to settling is unlikely to occur.
[0111] In one embodiment, the number average fiber diameter (D) of the cellulose fine fibers is a value measured by the following procedure using a scanning electron microscope (SEM). The cellulose fine fibers before or after concentration are diluted with tert-butanol to 0.1 to 0.5% by mass, and the sheet is prepared by suction filtration and dried in an oven at 150°C for 5 minutes to obtain a measurement sample. The number average fiber diameter (D) is determined by measuring an image at 10,000 times magnification observed with a high-resolution scanning electron microscope (SEM). Specifically, three straight lines passing through the center point of the observed image are arbitrarily drawn, and the widths of the fibers intersecting with these straight lines are determined for at least 100 fibers, to calculate the number average value.
[0112] The crystallinity of the cellulose raw material or cellulose fine fibers is preferably 55% or more, or 60% or more, or 70% or more, or 73% or more, or 75% or more, from the viewpoint of obtaining a resin composition excellent in heat resistance, mechanical strength and dimensional stability. When the crystallinity is within this range, the mechanical properties (heat resistance, strength, dimensional stability) of the cellulose itself are high, so that when the cellulose is dispersed in a resin, the heat resistance, strength and dimensional stability of the resin composition tend to be high. Although a high crystallinity is preferable, the upper limit is preferably 99% from the viewpoint of production.
[0113] From the viewpoint of mechanical property expression, the degree of polymerization of the cellulose raw material or cellulose fine fibers is preferably 100 or more, or 150 or more, or 200 or more, or 300 or more, or 400 or more, and from the viewpoint of processability, it is preferably 3500 or less, or 3300 or less, or 3200 or less, or 3100 or less, or 3000 or less.
[0114] The degree of polymerization of cellulose means the average degree of polymerization measured according to the reduced specific viscosity method using a copper ethylenediamine solution described in the Verification Test (3) of the "Japanese Pharmacopoeia Commentary, 15th Edition (published by Hirokawa Shoten)."
[0115] In one embodiment, the weight average molecular weight (Mw) of the cellulose raw material or cellulose fine fiber is 100,000 or more, more preferably 200,000 or more. The ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) is 6 or less, preferably 5.4 or less. The larger the weight average molecular weight, the fewer the number of terminal groups of the cellulose molecule. In addition, since the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight represents the width of the molecular weight distribution, the smaller the Mw / Mn, the fewer the number of terminals of the cellulose molecule. Since the terminals of the cellulose molecule are the starting points of thermal decomposition, when the weight average molecular weight of the cellulose molecule is not only large but also has a narrow molecular weight distribution width, a particularly high heat resistant cellulose and a resin composition containing cellulose and a resin can be obtained. The weight average molecular weight (Mw) of the cellulose fine fiber may be, for example, 600,000 or less, or 500,000 or less, from the viewpoint of the availability of the cellulose raw material. From the viewpoint of ease of production of cellulose fine fibers, the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) may be, for example, 1.5 or more, or 2 or more. Mw can be controlled within the above range by selecting a cellulose raw material having an Mw appropriate for the purpose, performing a physical treatment and / or a chemical treatment on the cellulose raw material appropriately within a moderate range, and the like. Mw / Mn can also be controlled within the above range by selecting a cellulose raw material having an Mw / Mn appropriate for the purpose, performing a physical treatment and / or a chemical treatment on the cellulose raw material appropriately within a moderate range, and the like. In both the control of Mw and the control of Mw / Mn, examples of the physical treatment include dry or wet grinding using a microfluidizer, ball mill, disk mill, etc., physical treatment that applies mechanical forces such as impact, shear, shear, and friction using a crusher, homomixer, high-pressure homogenizer, ultrasonic device, etc., and examples of the chemical treatment include digestion, bleaching, acid treatment, and conversion to regenerated cellulose.
[0116] The weight average molecular weight and number average molecular weight referred to here are values obtained by dissolving the cellulose raw material or cellulose fine fibers in N,N-dimethylacetamide containing lithium chloride and then performing gel permeation chromatography using N,N-dimethylacetamide as a solvent.
[0117] Methods for controlling the degree of polymerization (i.e., average degree of polymerization) or molecular weight of cellulose fine fibers include hydrolysis treatment after the fiberization process. The hydrolysis process advances the depolymerization of amorphous cellulose inside the cellulose, decreasing the average degree of polymerization. At the same time, the hydrolysis process removes impurities such as hemicellulose and lignin in addition to amorphous cellulose, making the inside of the fiber porous. This makes the cellulose more susceptible to mechanical treatment in a process of applying mechanical shear force to the cellulose, such as the kneading process described below, and makes the cellulose more easily finely dispersed.
[0118] Since cellulose fine fibers can have a high aspect ratio shape with a long fiber length relative to the fiber diameter and can be in a curved state, it is difficult to quantitatively measure the fiber length, but the fineness ratio reflecting the fiber length distribution can be calculated using an automatic fiber shape analyzer (e.g., Morfi Neo manufactured by Techpap). In this disclosure, the fineness ratio is defined and calculated as the content of fibers with a length-weighted fiber length of less than 0.1 mm.
[0119] (Automatic fiber shape analyzer) The measurement procedure using the automatic fiber shape analyzer (Morfi Neo manufactured by Techpap) is described below. The fiber parameters during measurement are defined as a fiber length of 0.1 mm as a threshold, and cellulose fine fibers with a length equal to or greater than the threshold are defined as normal fibers, and fibers with a length less than the threshold are defined as fine fibers.
[0120] Cellulose fine fibers are dispersed in pure water to prepare 1 L of an aqueous dispersion with a solid content of 0.003 to 0.005% by mass. When the aqueous dispersion contains 2% by mass or less of cellulose fine fibers before dilution, it is sufficient to simply mix with a spatula or the like. However, when the aqueous dispersion contains 2% by mass or more of cellulose fine fibers, or the cellulose fine fibers are in the form of a wet cake or powder, a high-shear homogenizer (manufactured by IKA, product name "Ultra Turrax T18") is used to perform dispersion treatment under the following treatment conditions: rotation speed 25,000 rpm x 5 minutes. When dispersed in a medium other than water, a high shear homogenizer (e.g., IKA, trade name "Ultra Turrax T18") is used to perform dispersion processing in a sufficient amount of pure water under processing conditions: rotation speed 25,000 rpm x 5 minutes, and then the medium is removed by means of suction filtration or the like, and a high shear homogenizer (e.g., IKA, trade name "Ultra Turrax T18") is used again to perform dispersion processing in pure water under processing conditions: rotation speed 25,000 rpm x 5 minutes to a solid content concentration of 0.003 to 0.005 mass%, thereby replacing the medium with water. The aqueous dispersion prepared as above is subjected to measurement using an autosampler, and each shape parameter is extracted or calculated from the results. In addition, since the data interval can be set arbitrarily in the measurement of the fiber length distribution in the device, any setting may be used as long as the distribution of fibers having the above-mentioned fiber length can be confirmed. Each shape parameter will be described in detail below.
[0121] (length-weighted average fiber length) The length-weighted average fiber length was measured using an automatic fiber shape analyzer according to the method defined in ISO / FDIS 16065-2:2006, and the average was calculated for fibers with a fiber length of 0.1 mm or more. For bent fibers, the average fiber length is the average fiber length that corresponds to the actual fiber length taking into account the bent shape.
[0122] (Fine Rate) The ratio of the number of fine fibers (fibers with a fiber length of less than 0.1 mm) to the total number of cellulose fine fibers observed by a fiber shape automatic analyzer. In one embodiment, the fine ratio is preferably 70% or more, or 80% or more, or 90% or more, and preferably 99% or less, or 98% or less, or 97% or less. By controlling the fine ratio within the above range, a good reinforcing effect can be obtained when the cellulose fine fibers are used as a filler for filler-reinforced resin. When the fine ratio is equal to or more than the above lower limit, the cellulose fine fibers tend to be well defibrated, and the cellulose fine fibers are unlikely to settle in the dispersion liquid, which is preferable because concentration unevenness due to sedimentation is unlikely to occur. In this case, the reinforcing effect as a filler for filler-reinforced resin is also good. On the other hand, when the fine ratio is equal to or less than the above upper limit, the cellulose fine fibers tend not to be excessively defibrated, and the cellulose fine fibers are unlikely to pass through the filtration substrate or clog the filtration substrate in the concentration process, which is preferable. In this case, the heat resistance of the cellulose fine fibers is unlikely to decrease due to excessive defibration, so that the filler for filler-reinforced resin is unlikely to suffer from severe coloration or deterioration in physical properties due to thermal deterioration.
[0123] (fine fiber area ratio) The fine fiber area ratio is the ratio of the total area of the observation images of fine fibers with a fiber length of less than 0.1 mm to the total area of the observation images of all cellulose fine fibers (area of normal fibers + area of fine fibers). The fine fiber area ratio is preferably 90% or less, or 80% or less, or 70% or less, or 60% or less, and preferably 5% or more, or 10% or more, or 20% or more, or 25% or more, or 30% or more. When the fine fiber area ratio is in the preferred range, concentration with less variation in the cellulose fine fiber content in the concentration step is facilitated.
[0124] (Fibrillation rate) The fibrillation rate means the total length of n branched side chains L(Sub) relative to the main chain length L(Main) of the largest diameter part in a fiber having at least a partially branched structure, and is defined by the following formula:
number
[0125] The fibrillation rate of the cellulose fine fibers is preferably 0.5% or more, or 0.7% or more, or 0.8% or more, or 0.9% or more, or 1.0% or more, or 1.2% or more, or 1.5% or more, and is preferably 3.5% or less, or 3.0% or less, or 2.5% or less, or 2.0% or less. When the fibrillation rate is within this range, the area of the interface between the cellulose fine fibers and the resin in the resin composition when the cellulose fine fibers are used as a filler for a filler-reinforced resin is in an appropriate range, and the number of starting points of fracture is reduced, resulting in a large fracture strain.
[0126] In one embodiment, the cellulose fine fibers may contain alkali-soluble polysaccharides. Alkali-soluble polysaccharides include hemicellulose, β-cellulose, and γ-cellulose. Those skilled in the art will understand alkali-soluble polysaccharides as components obtained as the alkali-soluble portion of holocellulose obtained by solvent extraction and chlorine treatment of plants (e.g., wood) (i.e., components obtained by removing α-cellulose from holocellulose). Alkali-soluble polysaccharides are polysaccharides containing hydroxyl groups, and may cause a decrease in heat resistance, physical properties, discoloration, and dispersibility in resins of the cellulose fine fibers. Therefore, it is preferable that the content of alkali-soluble polysaccharides in the cellulose fine fibers is low.
[0127] In one embodiment, the average content of alkali-soluble polysaccharides in the cellulose fine fibers is preferably 20% by mass or less, or 18% by mass or less, or 15% by mass or less, or 12% by mass or less, or 11% by mass or less, or 8% by mass or less, based on 100% by mass of the cellulose fine fibers, from the viewpoint of maintaining good function of the cellulose fine fibers. The above content may be 1% by mass or more, or 2% by mass or more, or 3% by mass or more, or 6% by mass or more, from the viewpoint of ease of production of the cellulose fine fibers. In one embodiment, the average content of alkali-soluble polysaccharides in the cellulose raw material may be 13% by mass or less, or 12% by mass or less, or 11% by mass or less, or 8% by mass or less, and is most preferably 0% by mass, but may be, for example, 3% by mass or more, or 6% by mass or more, from the viewpoint of ease of availability of the cellulose raw material.
[0128] The average alkali-soluble polysaccharide content can be determined by the method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000), by subtracting the α-cellulose content from the holocellulose content (Wise method). This method is understood in the industry as a method for measuring the amount of hemicellulose. The alkali-soluble polysaccharide content is calculated three times for each sample, and the number average of the calculated alkali-soluble polysaccharide contents is taken as the average alkali-soluble polysaccharide content.
[0129] In one embodiment, the average content of acid-insoluble components in the cellulose fine fibers is preferably 10% by mass or less, 5% by mass or less, or 3% by mass or less, based on 100% by mass of the cellulose fine fibers, from the viewpoint of avoiding a decrease in heat resistance of cellulose and the associated discoloration. From the viewpoint of ease of production of the cellulose fine fibers, the content may be 0.1% by mass or more, 0.2% by mass or more, or 0.3% by mass or more.
[0130] The average acid-insoluble content is determined as a quantitative determination of the acid-insoluble content using the Clason method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000). This method is understood in the industry as a method for measuring the amount of lignin. The sample is stirred in a sulfuric acid solution to dissolve cellulose, hemicellulose, etc., and then filtered through a glass fiber filter paper, and the resulting residue corresponds to the acid-insoluble content. The acid-insoluble content is calculated from the weight of the acid-insoluble content, and the number average of the acid-insoluble content calculated for the three samples is taken as the average acid-insoluble content.
[0131] <Method for producing resin composition> Another aspect of the present invention provides a method for producing a resin composition containing cellulose fine fibers and a thermoplastic resin. In one aspect, the method includes the steps of producing a cellulose fine fiber dispersion concentrate by the method for producing a cellulose fine fiber dispersion concentrate of the present disclosure or producing a dried cellulose fine fiber body by the method for producing a dried cellulose fine fiber body of the present disclosure, and mixing (typically melt-kneading) the cellulose fine fiber dispersion concentrate or the dried cellulose fine fiber body with a thermoplastic resin to produce a resin composition.
[0132] For melt kneading, an extruder such as a single screw extruder or a twin screw extruder can be used, but a twin screw extruder is preferred in terms of controlling the dispersibility of the cellulose fine fibers. The L / D obtained by dividing the cylinder length (L) of the extruder by the screw diameter (D) is preferably 30 or more, and particularly preferably 40 or more. The screw rotation speed during kneading is preferably in the range of 50 to 800 rpm, and more preferably in the range of 100 to 600 rpm. Each screw in the cylinder of the extruder is optimized by combining a conveying screw with an elliptical two-blade screw shape, a kneading element called a kneading disk, and the like.
[0133] <Thermoplastic resin> The thermoplastic resin is appropriately selected depending on the intended use of the resin composition, and may be, for example, a crystalline thermoplastic resin having a melting point within the range of 100° C. to 350° C., or an amorphous thermoplastic resin having a glass transition temperature within the range of 100° C. to 250° C. Examples of the resin include polyolefin-based resins, polyamide-based resins, polyester-based resins, polyacetal-based resins, polyphenylene ether-based resins, polyphenylene sulfide-based resins, and mixtures of two or more of these. From the viewpoint of handling and cost, preferred are polyolefin-based resins, polyamide-based resins, polyester-based resins, polyacetal-based resins, etc., more preferred are polyamide-based resins, polyolefin-based resins, and polyacetal-based resins, and particularly preferred are polyamide-based resins and polyacetal-based resins. From the viewpoint of enhancing the heat resistance of the resin composition, the melting point of the thermoplastic resin (particularly the crystalline resin) is preferably 140°C or more, or 150°C or more, or 160°C or more, or 170°C or more, or 180°C or more, or 190°C or more, or 200°C or more, or 210°C or more, or 220°C or more, or 230°C or more, or 240°C or more, or 245°C or more, or 250°C or more.
[0134] The melting point of the thermoplastic resin can be, for example, 150°C to 190°C or 160°C to 180°C for a resin with a relatively low melting point (such as a polyolefin-based resin), and 220°C to 350°C or 230°C to 320°C for a resin with a relatively high melting point (such as a polyamide-based resin).
[0135] In this disclosure, the melting point of a resin refers to the peak top temperature of an endothermic peak that appears when the temperature is increased from 23°C at a heating rate of 10°C / min using a differential scanning calorimeter (DSC), and when two or more endothermic peaks appear, it refers to the peak top temperature of the endothermic peak with the highest temperature.
[0136] In this disclosure, the glass transition temperature of a resin refers to the peak top temperature at which the storage modulus is significantly reduced and the loss modulus is maximized when measured using a dynamic viscoelasticity measuring device while increasing the temperature from 23° C. at a rate of 2° C. / min and applying a frequency of 10 Hz. When two or more peaks of the loss modulus appear, the glass transition temperature refers to the peak top temperature of the peak on the highest temperature side.
[0137] The polyolefin resin preferred as the thermoplastic resin is a polymer obtained by polymerizing olefins (e.g., α-olefins) or alkenes as monomer units.Specific examples of the polyolefin resin include ethylene (co)polymers such as low-density polyethylene (e.g., linear low-density polyethylene), high-density polyethylene, ultra-low-density polyethylene, and ultra-high-molecular-weight polyethylene, polypropylene (co)polymers such as polypropylene, ethylene-propylene copolymer, and ethylene-propylene-diene copolymer, and copolymers of α-olefins such as ethylene, typified by ethylene-acrylic acid copolymer, ethylene-methyl methacrylate copolymer, and ethylene-glycidyl methacrylate copolymer.
[0138] The most preferred polyolefin resin here is polypropylene. In particular, polypropylene having a melt mass flow rate (MFR) of 3 g / 10 min or more and 30 g / 10 min or less, measured at 230 ° C. and a load of 21.2 N according to ISO1133, is preferred. The lower limit of MFR is more preferably 5 g / 10 min, even more preferably 6 g / 10 min, and most preferably 8 g / 10 min. The upper limit is more preferably 25 g / 10 min, even more preferably 20 g / 10 min, and most preferably 18 g / 10 min. It is desirable that MFR does not exceed the upper limit from the viewpoint of improving the toughness of the composition, and it is desirable that MFR does not fall below the lower limit from the viewpoint of the fluidity of the composition.
[0139] In addition, in order to increase the affinity with cellulose fine fibers, an acid-modified polyolefin resin can also be suitably used. As the acid used for the acid modification, a mono- or polycarboxylic acid can be used, and examples thereof include maleic acid, fumaric acid, succinic acid, phthalic acid and their anhydrides, and citric acid. Maleic acid or its anhydride is particularly preferred because it is easy to increase the modification rate. There is no particular restriction on the modification method, but a method in which a polyolefin resin is heated to a melting point or higher in the presence or absence of a peroxide and melt-kneaded is generally used. As the polyolefin resin to be acid-modified, all of the above-mentioned polyolefin resins can be used, but polypropylene is particularly suitable. The acid-modified polypropylene resin may be used alone, but it is more preferable to use it in combination with an unmodified polypropylene resin in order to adjust the modification rate of the resin as a whole. In this case, the ratio of the acid-modified polypropylene resin to all polypropylene resins is preferably 0.5% by mass to 50% by mass. A more preferred lower limit is 1 mass%, or 2 mass%, or 3 mass%, or 4 mass%, or 5 mass%. A more preferred upper limit is 45 mass%, or 40 mass%, or 35 mass%, or 30 mass%, or 20 mass%. In order to maintain the interfacial strength between the resin and the cellulose fine fibers, a content equal to or greater than the lower limit is preferred, and in order to maintain the ductility of the resin, a content equal to or less than the upper limit is preferred.
[0140] The melt mass flow rate (MFR) of the acid-modified polypropylene measured at 230°C and a load of 21.2N according to ISO1133 is preferably 50g / 10min or more in order to enhance affinity with the cellulose interface. A more preferred lower limit is 100g / 10min, even more preferably 150g / 10min, and most preferably 200g / 10min. There is no particular upper limit, but it is 500g / 10min in order to maintain mechanical strength. By setting the MFR within this range, when acid-modified polypropylene and unmodified polypropylene are used in combination, the acid-modified polypropylene can be advantageously easily present at the interface between cellulose and resin.
[0141] Examples of polyamide-based resins that are preferable as the thermoplastic resin include polyamides obtained by polycondensation reaction of lactams (e.g., polyamide 6, polyamide 11, polyamide 12, etc.); diamines (e.g., 1,6-hexanediamine, 2-methyl-1,5-pentanediamine, 1,7-heptanediamine, 2-methyl-1-6-hexanediamine, 1,8-octanediamine, 2-methyl-1,7-heptanediamine, 1,9-nonanediamine, 2-methyl-1,8-octanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, m-xylylenediamine, etc.) and dicarboxylic acids (e.g., butanedioic acid, pentanedioic acid, hexanedioic acid, , heptanedioic acid, octanedioic acid, nonanedioic acid, decanedioic acid, benzene-1,2-dicarboxylic acid, benzene-1,3-dicarboxylic acid, benzene-1,4-dicarboxylic acid, cyclohexane-1,3-dicarboxylic acid, cyclohexane-1,4-dicarboxylic acid, etc.) (for example, polyamide 6,6, polyamide 6,10, polyamide 6,11, polyamide 6,12, polyamide 6,T, polyamide 6,I, polyamide 9,T, polyamide 10,T, polyamide 2M5,T, polyamide MXD,6, polyamide 6,C, polyamide 2M5,C, etc.); and copolymers in which these are copolymerized (for example, polyamide 6,T / 6,I, etc.).
[0142] Among these polyamide resins, aliphatic polyamides such as polyamide 6, polyamide 11, polyamide 12, polyamide 6,6, polyamide 6,10, polyamide 6,11, and polyamide 6,12, and alicyclic polyamides such as polyamide 6,C and polyamide 2M5,C are more preferred.
[0143] The terminal carboxyl group concentration of the polyamide resin is not particularly limited, but may be preferably 20 μmol / g or more, or 25 μmol / g or more, and may be preferably 150 μmol / g or less, or 100 μmol / g or less.
[0144] The terminal amino group concentration of the polyamide resin may be preferably 20 μmol / g or more, or 30 μmol / g or more, and may be preferably 150 μmol / g or less, or 100 μmol / g or less.
[0145] The total concentration of terminal amino groups and terminal carboxyl groups in the polyamide resin is not particularly limited, but may be preferably 10 μmol / g or more, or 50 μmol / g or more, or 100 μmol / g or more, or 135 μmol / g or more, and from the viewpoint of preventing a decrease in viscosity due to the resin having an excessively low molecular weight and suppressing the occurrence of burrs and the like during molding, may be preferably 500 μmol / g or less, or 300 μmol / g or less, or 135 μmol / g or less, or 100 μmol / g or less.
[0146] The amino end group ratio ([NH2] / [COOH]) of the polyamide resin to the carboxyl end group is preferably more than 1.00, or 1.01 or more, or 1.05 or more, or 1.10 or more. There is no particular upper limit to the amino end group ratio, but from the viewpoint of maintaining a good color tone of the resin composition, it may be preferably 10,000 or less, 1,000 or less, 100 or less, or 10 or less.
[0147] The terminal group concentration of the polyamide resin can be adjusted by a known method, such as adding a terminal regulator (e.g., a diamine compound, a monoamine compound, a dicarboxylic acid compound, a monocarboxylic acid compound, an acid anhydride, a monoisocyanate, a monoacid halide, a monoester, a monoalcohol, etc.) that reacts with the terminal group during polymerization of the polyamide to the polymerization liquid so as to obtain a predetermined terminal group concentration.
[0148] The concentration of amino end groups and carboxyl end groups of the polyamide resin is 1 It can be determined from the integral value of the characteristic signal corresponding to each terminal group by H-NMR. This method is preferable in terms of accuracy and simplicity. More specifically, it is recommended to use the method described in JP-A-7-228775, use deuterated trifluoroacetic acid as the measurement solvent, and set the number of integration scans to 300 or more.
[0149] The intrinsic viscosity [η] of the polyamide resin measured under the condition of 30°C in concentrated sulfuric acid is preferably 0.6 to 2.0 dL / g, or 0.7 to 1.4 dL / g, or 0.7 to 1.2 dL / g, or 0.7 to 1.0 dL / g, from the viewpoint that the fluidity in the mold is good and the appearance of the molded piece is good when the resin composition is injection molded. In the present disclosure, the "intrinsic viscosity" is synonymous with the viscosity generally called the limiting viscosity. The intrinsic viscosity is obtained by measuring the ηsp / c of several measurement solvents having different concentrations under the temperature condition of 30°C in 96% concentrated sulfuric acid, deriving the relational equation between each of the ηsp / c and the concentration (c), and extrapolating the concentration to zero. The value extrapolated to zero is the intrinsic viscosity. Details of the above method are described, for example, in Polymer Process Engineering (Prentice-Hall, Inc. 1994), pages 291 to 294, etc. From the viewpoint of accuracy, it is desirable to set at least four concentrations in the above-mentioned measurement solvents having different concentrations (for example, 0.05 g / dL, 0.1 g / dL, 0.2 g / dL, and 0.4 g / dL).
[0150] The polyester resin may be one or more selected from polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), polyhydroxyalkanoic acid (PHA), polylactic acid (PLA), polyarylate (PAR), polycarbonate (PC), etc. More preferred examples of the polyester resin include PET, PBS, PBSA, PBT, and PEN, and even more preferred examples include PBS, PBSA, and PBT.
[0151] In addition, the polyester resin can freely change the terminal group depending on the monomer ratio during polymerization and the presence or absence and amount of addition of a terminal stabilizer, but the carboxyl terminal group ratio ([COOH] / [total terminal groups]) to the total terminal groups of the polyester resin is more preferably 0.30 to 0.95. The lower limit of the carboxyl terminal group ratio is more preferably 0.35, even more preferably 0.40, and most preferably 0.45. The upper limit of the carboxyl terminal group ratio is more preferably 0.90, even more preferably 0.85, and most preferably 0.80. The carboxyl terminal group ratio is preferably 0.30 or more from the viewpoint of dispersibility of cellulose in the composition, and is preferably 0.95 or less from the viewpoint of the color tone of the obtained composition.
[0152] As polyacetal resins, homopolyacetals made from formaldehyde and copolyacetals containing trioxane as a main monomer and 1,3-dioxolane as a comonomer component are common. Both can be used, but copolyacetals are preferred from the viewpoint of thermal stability during processing. In particular, the amount of the structure derived from the comonomer component (e.g., 1,3-dioxolane) is more preferably within the range of 0.01 to 4 mol%. The preferred lower limit of the amount of the structure derived from the comonomer component is 0.05 mol%, more preferably 0.1 mol%, and even more preferably 0.2 mol%. The preferred upper limit is 3.5 mol%, more preferably 3.0 mol%, even more preferably 2.5 mol%, and most preferably 2.3 mol%.
[0153] From the viewpoint of thermal stability during extrusion and molding, the lower limit is desirably within the above-mentioned range, and from the viewpoint of mechanical strength, the upper limit is desirably within the above-mentioned range.
[0154] From the viewpoint of affinity with cellulose, the resin is particularly preferably a resin having a hydrophilic group (e.g., one or more selected from a hydroxyl group, an ether group, an ester group, an amino group, and a carboxy group). Suitable examples of the resin having a hydrophilic group are one or more selected from the group consisting of an acid-modified polyolefin resin, a polyacetal resin, a polycarbonate resin, a polyamide resin, a polyester resin, a polyphenylene ether resin, and an acrylic resin. Among them, polyamide resins and maleated polypropylene are preferred.
[0155] <Additional Ingredients> The resin composition of the present embodiment may further contain additional components as necessary to improve its performance. Examples of the additional components include dispersants, filler components other than cellulose, compatibilizers, plasticizers, polysaccharides such as starches and alginic acid, natural proteins such as gelatin, glue, and casein, inorganic compounds such as zeolite, ceramics, talc, silica, metal oxides, and metal powders, colorants, fragrances, pigments, flow regulators, leveling agents, conductive agents, antioxidants, antistatic agents, ultraviolet absorbers, ultraviolet dispersants, and deodorants. The content ratio of any additional component in the resin composition is appropriately selected within a range in which the desired effects of the present invention are not impaired, and may be, for example, 0.01 to 50% by mass, or 0.1 to 30% by mass.
[0156] The dispersant used can be one that suppresses aggregation and solidification of cellulose when mixed with the concentrated cellulose fine fibers to form a dried cellulose fine fiber body, and improves the dispersion stability of the cellulose fine fibers in the resin composition obtained by kneading the resin and the dried cellulose fine fiber body, and may be hydrophilic or hydrophobic. Suitable examples of the dispersant include one or more selected from the group consisting of cellulose derivatives, polyalkylene oxides, amides, and amines, but are not limited thereto. Among them, cellulose derivatives are preferred because they have a high affinity with cellulose fine fibers because they are cellulose-based substances, while they are also thermoplastic resins, and therefore have a high effect of improving the dispersion stability of cellulose fine fibers in the resin composition. The dispersant is preferably one that has a boiling point higher than that of water. Note that a boiling point higher than that of water refers to a boiling point higher than the boiling point at each pressure in the vapor pressure curve of water (for example, 100°C under 1 atmosphere). The boiling point of the dispersant is more preferably higher than the resin temperature during kneading, and the higher the better. The boiling point of the dispersant may be, for example, 130°C or higher, or 140°C or higher, or 150°C or higher, or 160°C or higher, or 170°C or higher, or 180°C or higher, and a dispersant having a boiling point higher than the expected kneading temperature may be selected. Alternatively, the dispersant may be one that does not have a boiling point and is thermally decomposed. In this case, the thermal decomposition temperature of the dispersant is preferably higher than the resin temperature during kneading, and in one embodiment, the dispersant may have a thermal decomposition temperature similar to the above-mentioned preferred boiling point.
[0157] The amount of cellulose fine fibers relative to 100% by mass of the entire resin composition is preferably 0.1% by mass or more, or 0.5% by mass or more, or 1% by mass or more, or 3% by mass or more from the viewpoint of obtaining a good reinforcing effect by the cellulose fine fibers, and is preferably 30% by mass or less, or 25% by mass or less, or 20% by mass or less, or 15% by mass or less from the viewpoint of maintaining the inherent properties of the resin well. It is preferable that the content of the cellulose fine fibers is not biased throughout the entire molded product of the resin composition. If there are locally low or high content of the cellulose fine fibers in parts, the reinforcing effect of the molded product may be reduced or may cause destruction due to those parts. In particular, when small molded products are manufactured, there is a risk of an increase in defective products.
[0158] The amount of resin relative to 100% by mass of the entire resin composition is, from the viewpoint of maintaining the inherent properties of the resin well, preferably 20% by mass or more, or 30% by mass or more, or 40% by mass or more, or 50% by mass or more, or 60% by mass or more, or 70% by mass or more, or 75% by mass or more, or 80% by mass or more, or 85% by mass or more, and from the viewpoint of obtaining the effects of other components well, preferably 99.9% by mass or less, or 99.5% by mass or less, or 99% by mass or less, or 97% by mass or less, or 95% by mass or less, or 90% by mass or less.
[0159] In the resin composition, the amount of dispersant per 100 parts by mass of cellulose fine fibers is, from the viewpoint of good dispersion of cellulose and network formation, preferably 1 part by mass or more, or 5 parts by mass or more, or 10 parts by mass or more, or 20 parts by mass or more, or 30 parts by mass or more, and from the viewpoint of reducing variation in performance of the resin composition, preferably 500 parts by mass or less, or 300 parts by mass or less, or 200 parts by mass or less, or 100 parts by mass or less.
[0160] The resin composition of the present embodiment can be used as various resin molded products. There is no particular limitation on the method for producing the resin molded product, and injection molding, extrusion molding, blow molding, inflation molding, foam molding, etc. can be used. Among these, injection molding is particularly preferred from the viewpoints of design and cost.
[0161] <Applications of resin composition> The resin composition obtained by the method of this embodiment is useful as a substitute for steel plates, fiber-reinforced plastics (e.g., carbon fiber-reinforced plastics, glass fiber-reinforced plastics, etc.), resin composites containing inorganic fillers, etc. Suitable applications of the resin composition include industrial machine parts, general machine parts, automobile / railroad / vehicle / ship / aerospace-related parts, electronic / electrical parts, building / civil engineering materials, daily necessities, sports / leisure goods, housing parts for wind power generation, containers / packaging parts, etc. EXAMPLES
[0162] The following examples further illustrate exemplary aspects of the present invention, but the present invention is not limited to these examples.
[0163] Evaluation method <Evaluation of fine ratio, fine fiber area ratio and fibrillation ratio using an automatic fiber shape analyzer> The measurement procedure using the automatic fiber shape analyzer (Morfi Neo manufactured by Techpap) is explained below. The fiber parameters during the measurement are defined as a fiber length of 0.1 mm, with cellulose fine fibers above the threshold being defined as normal fibers, and fibers below the threshold being defined as fine fibers. The following shape parameters were extracted or calculated from the measurement results using the automatic fiber shape analyzer. Fine ratio: The ratio of fine fibers (fibers with a fiber length of less than 0.1 mm) to the total number of cellulose microfibers. Fine fiber area ratio: Fine content,% in area[%] Fibrillation rate: MacroFibrillation index [%]
[0164] The cellulose fine fiber dispersion was diluted with pure water to prepare 1 L of an aqueous dispersion with a solid content concentration of 0.003 to 0.005% by mass. This aqueous dispersion was subjected to dispersion treatment using a high-shear homogenizer (manufactured by IKA, product name "Ultra Turrax T18") under treatment conditions: rotation speed 25,000 rpm x 5 minutes. The aqueous dispersion prepared as above was subjected to measurement using an autosampler, and the fine ratio was calculated from the results.
[0165] <Preparation of porous sheets of pulp and cellulose fine fibers> Pulp (solid content 0.5 g equivalent) described later or cellulose fine fiber dispersion liquid obtained in the manufacturing example described later (solid content 0.5 g equivalent) was collected and filtered by suction, and the filtered residue was added to tert-butanol, and further dispersed in a mixer until no aggregates were present. The concentration was adjusted to 0.5 mass% per 0.5 g of cellulose solid content. 100 g of the obtained tert-butanol dispersion liquid was filtered on filter paper, dried at 150°C, and the filter paper was peeled off to obtain a porous sheet.
[0166] <Average fiber diameter (D) of cellulose fine fibers> The number average fiber diameter (D) of the cellulose fine fibers was measured using a scanning electron microscope (SEM) according to the following procedure. A porous sheet was prepared by the above method as a measurement sample, and the diameter was determined by measuring images observed at 10,000x or 50,000x with a high-resolution scanning electron microscope (SEM). Specifically, three straight lines were drawn at random through the center point of the observed image, and the widths of the fibers intersecting with these straight lines were determined for at least 100 fibers, and the number average value was calculated.
[0167] <Crystallization degree of cellulose fine fibers> The porous sheet produced by the above method was measured by wide-angle X-ray diffraction, and the diffraction pattern (2θ / deg. 10 to 30) was used to determine the following formula using the Segal method. Crystallinity (%)=[I(200)-I(amorphous)] / I(200)×100 I(200): Diffraction peak intensity due to the 200 plane (2θ=22.5°) in cellulose I crystals I (amorphous): The halo peak intensity due to amorphous in cellulose type I crystals, which is the peak intensity at an angle 4.5° lower than the diffraction angle of the 200 plane (2θ = 18.0°).
[0168] (X-ray diffraction measurement conditions) Equipment: MiniFlex (manufactured by Rigaku Corporation) Operation axis 2θ / θ Source CuKα Measurement method: Continuous Voltage 40kV Current 15mA Starting angle 2θ=5° End angle 2θ=30° Sampling width 0.020° Scan speed: 2.0° / min Sample: A porous sheet is attached onto the sample holder.
[0169] <Degree of substitution (DS) of acetylated pulp and acetylated cellulose fine fibers> The degree of substitution (DS) of the acetylated pulp and acetylated cellulose fine fibers was calculated based on the peak intensity ratio between the peak derived from the acetyl group and the peak derived from the cellulose skeleton from the reflection infrared absorption spectrum of each of the porous sheets prepared by the above-mentioned method. The peak of the absorption band of C=O based on the acetyl group was at 1730 cm -1 The absorption band of CO based on the cellulose backbone appears at 1030 cm -1 The DS of acetylated cellulose is calculated by plotting a correlation graph between the DS obtained from solid-state NMR measurement of acetylated cellulose (described later) and the modification ratio (IR index 1030), which is defined as the ratio of the peak intensity of the absorption band of C=O based on the acetyl group to the peak intensity of the absorption band of CO in the cellulose backbone chain, and calculating the calibration curve substitution degree from the correlation graph. DS = 4.13 × IR index (1030) It was found by using
[0170] (Reflection type infrared spectrum measurement conditions) Equipment: Fourier transform infrared spectrophotometer (Nicolet Summit Pro, ThermoFisher Scientific) Number of times: 16 Wavenumber resolution: 4cm -1 ATR Crystal: Diamond Incident angle: 45°
[0171] The method for calculating the DS of acetylated cellulose by solid-state NMR was as follows for freeze-ground acetylated pulp and acetylated cellulose microfibers. 13 C solid-state NMR measurements were performed, and the intensity was calculated using the area intensity (Inf) of a signal assigned to one carbon atom derived from the modifying group relative to the total area intensity (Inp) of signals assigned to carbons C1-C6 derived from the pyranose ring of cellulose, which appear in the range from 50 ppm to 110 ppm, using the following formula. DS = (Inf) x 6 / (Inp) For the acetyl group, the signal at 23 ppm assigned to -CH3 was used.
[0172] Used 13 The conditions for C solid-state NMR measurement are as follows. Equipment:Bruker Biospin Avance500WB Frequency: 125.77MHz Measurement method: DD / MAS method Waiting time: 75sec NMR sample tube: 4mmφ Accumulation times: 640 times (approx. 14 hours) MAS: 14,500Hz Chemical shift reference: glycine (external reference: 176.03 ppm)
[0173] <Number of moles of substituent> For the acetylated cellulose fine fibers, the number of moles of acetyl groups per unit mass of the acetylated cellulose fine fibers was calculated using the following formula based on the above-mentioned DS measurement results. {1 / [(162-DS)+(molecular weight of acetyl group × DS)]} × DS
[0174] <Processing speed> Starting from the point when the supply of the cellulose fine fiber dispersion to the continuous concentrator was started, the weight of the cellulose fine fiber concentrate recovered in the recovery container after 30 minutes of operation was measured and converted into the processing speed per hour.
[0175] <Mass content of cellulose fine fibers in concentrate or intermediate concentrate> 5 g of the concentrate or intermediate concentrate was taken and dried at 150°C using an IR moisture meter (MX-50, manufactured by A&D) to determine the solid content, which was regarded as the mass content of cellulose fine fibers. For each example, 10 samples were taken every 15 minutes during the concentration process, and the number average and CV values (standard deviation / number average) of the 10 samples were determined. In Reference Example 1, the intermediate concentrate and the concentrate dripped, so the cellulose fine fiber content of the collected samples could not be accurately measured. For these samples, the above CV values were obtained as reference values.
[0176] <Yield> [Fiber loss during suction deliquency] The removal of cellulose fine fibers from the filter substrate during suction deliquescence was evaluated. Specifically, the turbidity of the filtrate at the suction section was measured using a turbidity meter TR-55 manufactured by Kasahara Chemical Co., Ltd., and evaluated according to the following criteria. ×: The turbidity of the filtrate at the suction section was 250 or more. △: The turbidity of the filtrate at the suction section was 150 or more and less than 250. ○: The turbidity of the filtrate at the suction section was less than 150.
[0177] [Liquid flow when passing through press roll] The flow of the intermediate concentrate in the direction perpendicular to the running direction (i.e., width direction) was evaluated according to the following criteria. ×: The intermediate concentrate that had been retained in front of the press roll fell off from the filtration substrate within 10 minutes, or the intermediate concentrate fell off between the press roll and the press belt during squeezing. △: The intermediate concentrate that had been retained in front of the press roll did not fall off the filter substrate even after 10 minutes had passed, and the intermediate concentrate did not fall off from between the press roll and the press belt during squeezing. However, the width of the concentrate (sheet-like material) after squeezing was enlarged by more than 2 cm compared to the width of the intermediate concentrate before squeezing. ◯: The intermediate concentrate retained in front of the press roll did not fall off from the filtration substrate even after 10 minutes had passed, and the intermediate concentrate did not fall off from between the press roll and the press belt during squeezing, and the increase in width of the concentrate (sheet-like material) after squeezing compared with the width of the intermediate concentrate before squeezing was within 2 cm.
[0178] [comprehensive evaluation] The yield was evaluated according to the following criteria. ×: One or more of fiber loss and liquid flow is ×. △: No × for fiber loss or liquid flow, and 1 or more is △. ◯: Both fiber loss and liquid flow are ◯.
[0179] <Handling> The handling properties in the concentration process were evaluated according to the following criteria. ×: One or more of the following defects (1) to (4) occurs. ○: None of the following defects (1) to (4) occurred. (1) Continuous concentration was impossible due to clogging of the cellulose fine fiber filter substrate. (2) Because separation of the concentrate from the filtration substrate was difficult, the residue remained attached to the filtration substrate, resulting in low recovery rates or in the impossibility of recovery. (3) The recovered cellulose fine fibers were not permeated by the dispersant and molten resin due to aggregation. (4) Compression was not possible due to dropout or retention in front of the press rolls.
[0180] <Tensile yield strength and tensile elongation at break of resin composition> The resin composition pellets were molded using an injection molding machine under conditions in accordance with JIS K6920-2 to mold multipurpose test pieces in accordance with ISO294-3. The molding temperature for injection molding was 260°C.
[0181] <Content of Cellulose Fine Fibers in Resin Composition> Five pieces were cut from the pellets of the resin composition for each resin composition, and the following treatment was performed on each. 1 g of the sample was weighed on a precision balance, 30 mL of hexafluoroisopropanol at room temperature, which is a solvent that dissolves the resin and dispersant but does not dissolve the cellulose fine fibers, was added, and ultrasonic waves were applied in an ultrasonic cleaner to dissolve the resin. The sample was filtered under pressure with a PTFE membrane filter, and the residue was washed by pressure filtration twice with the above solvent, twice with ethanol, and twice with water. The residue was dried in an oven at 110 ° C. for 1 hour, and the weight was measured with a precision balance to calculate the content of cellulose fine fibers in the resin composition. Five samples were weighed for each resin composition. The maximum and minimum values obtained are shown in Table 3.
[0182] ≪Materials used≫ <Resin> Polyamide 6 (UBE NYLON 1013B, manufactured by Ube Industries, Ltd.), melting point 225°C
[0183] <Dispersant> Polyethylene oxide-polypropylene oxide copolymer (Sanyo Chemical: GL-3000)
[0184] <Pulp> Cotton linter pulp Cotton linter pulp sheets obtained from Japan Pulp and Paper Co., Ltd. were used.
[0185] <Production of acetylated pulp> Dimethyl sulfoxide (30 kg) was added to a 40 L jacketed reactor, and the catalyst sodium hydrogen carbonate (0.48 kg) and pulp (1.5 kg) were added and stirred. Warm water was run through the jacket to heat the liquid to 60°C. The inside of the reactor was replaced with nitrogen, and vinyl acetate (1.4 kg) was added. The reaction was carried out for 2 hours, and then pure water (10 kg) was added to stop the reaction. A filter cloth (PP9B, available from Nakao Filter Kogyo Co., Ltd.) was set in a 100 L Nutsche filter, and pure water (50 kg) and the reaction liquid were added and pressure filtration was carried out (first filtration). Furthermore, pressure filtration with pure water (50 kg) was repeated five times at room temperature (second to sixth filtrations), and a total of six pressure filtrations were carried out to obtain acetylated pulp in a water-containing state with a solid content of 15% by mass, which was used in the next process without drying. At this time, the DS of the pulp surface determined from reflection infrared spectroscopy was 1.50.
[0186] <Production of Dispersion> <Production Example 1> (Production of Dispersion of Cellulose Fine Fibers) Defibration was performed using a defibration device equipped with two tanks (tank A and tank B) connected by piping via a disc refiner. The cotton linter pulp sheet was immersed in water to a solid content concentration of 1.5% by mass, and a total of 20 kg of the cotton linter pulp sheet was dispersed using a lab pulper (manufactured by Aikawa Iron Works). The dispersion was then sent to tank A and processed using a single disc refiner (manufactured by Aikawa Iron Works, SDR14 type lab refiner, pressurized disc type). First, the slurry was sent from tank A, into which the slurry was charged, via the disc refiner to tank B, where it was stored. When the processing of the slurry in tank A was completed, the slurry was continuously sent from tank B to tank A via the disc refiner, where it was stored, thereby controlling the number of times the slurry passed through the disc refiner (number of passes). The blade distance adjustment mechanism of the disc refiner was equipped with a ball screw jack and a reducer, and the deviation of the blade distance during the beating process after the target blade distance was reached was 0.005 mm or less as measured by a displacement sensor. The disc refiner blade had a blade width of 4.0 mm and a blade groove ratio of 0.89, and was passed 30 times at a blade distance of 0.25 mm, after which a blade width of 0.8 mm and a blade groove ratio of 0.53 was used and passed 30 times at a blade distance of 0.25 mm.
[0187] The obtained slurry was treated with a high-pressure homogenizer (NS3015H, manufactured by Niro Soavi) at 80 MPa for 10 passes. The high-pressure homogenizer treatment was also performed in two tanks, similar to the above-mentioned disc refiner treatment, by controlling the number of passes through the high-pressure homogenizer treatment, to obtain a dispersion of cellulose fine fibers with an average fiber diameter of 95 nm.
[0188] <Production Example 2> (Production of Dispersion of Acetylated Cellulose Fine Fibers) The raw material was 40 kg of acetylated pulp produced by repeating the above method multiple times. The disc refiner treatment was performed in the same manner as in Production Example 1, except that a blade with a blade width of 0.8 mm and a blade groove ratio of 0.53 was used, the blade distance was 0.25 mm, and one stage was performed with 30 passes. The number of passes in the high-pressure homogenizer treatment was 3 passes. A dispersion of acetylated cellulose fine fibers with a DS of 0.78 and an average fiber diameter of 150 nm was obtained.
[0189] <Production Example 3> (Production of Dispersion of Cellulose Fine Fibers) The same procedure as in Production Example 2 was carried out except that 75 kg of unmodified cotton linter pulp was used, to obtain a dispersion of cellulose fine fibers having an average fiber diameter of 178 nm.
[0190] <Production Example 4> (Production of acetylated cellulose fine fiber dispersion) The raw material was 10 kg of acetylated pulp produced by repeating the above method multiple times, and the disc refiner treatment was carried out in the same manner as in Production Example 1, except that a blade with a blade width of 4.0 mm, a blade groove ratio of 0.89, and a blade distance of 0.30 mm were used in one stage of 20 passes. A dispersion of acetylated cellulose fine fibers with a DS of 0.88 and an average fiber diameter of 660 nm was obtained without performing high-pressure homogenizer treatment.
[0191] The properties of the cellulose fine fibers in the resulting dispersion are summarized in Table 1.
[0192] <Production of concentrate> <Example 1> The cellulose fine fiber dispersion obtained in Production Example 2 was dehydrated and concentrated using the continuous concentrator shown in Fig. 3. The above dispersion was diluted with pure water to a solid content (mass content of cellulose fine fibers) of 1.5 mass %, and then concentrated using a 1.5 m 3 The dispersion was poured into a tank and stirred continuously at a peripheral speed of 0.7 m / sec to maintain a uniform state of the dispersion. A 36 cm wide filter substrate (a blended nonwoven fabric of cellulose and polyester) was layered on a circulating papermaking wire and sent out at a speed of 1.5 m / min. The dispersion was pumped at a speed of 17 L / min with a mono pump to a volume of 0.1 m. 3The cellulose fine fibers were concentrated in a layer by passing through a slit in the temporary storage section and then deliquored in a suction section with a decompression section length of 50 cm to obtain an intermediate concentrate. This intermediate concentrate was pressed and deliquored by being sandwiched between a press roll and a press belt while still on the filter substrate to produce a concentrate. The concentrate was scraped off and collected with a scraper on the press roll. Throughout the process, the processing speed was maintained at 78 kg / hr and the temperature at 23°C. The temperature was the temperature of the dispersion in the tank (the same applies to the following examples).
[0193] <Examples 2 to 11, Comparative Examples 1 and 2, Reference Example 1> Dehydration and concentration were performed in the same manner as in Example 1, except that the conditions were changed as shown in Table 2. In Table 2, the slit width "∞" means that no slit was provided in the temporary storage section, and the dispersion in the temporary storage section was allowed to flow out as it was. In Comparative Examples 1 and 2, the press belt 308 was moved away from the press roll 307 to transport the intermediate concentrate without press deliquification, the feed mechanism 306c was moved close to the press roll 307 to transfer the intermediate concentrate to the press roll, and the transferred intermediate concentrate was scraped off with a scraper on the press roll and collected as a concentrate. The results are shown in Table 2.
[0194] <Production of resin composition> <Examples 12 to 16, Comparative Examples 3 and 4> [Production of dried cellulose fine fibers] A dispersant was added to the concentrate obtained above in an amount of 43 parts by mass per 100 parts by mass of the cellulose fine fiber solid content, and the mixture was thoroughly stirred in a commercial mixer (Kenmix Aiko Chef PRO) manufactured by Aikosha Seisakusho Co., Ltd. to obtain a concentrated cake containing the dispersant. These were fed into a drying device as raw materials and dried under the following conditions. The moisture content was measured using an infrared heating moisture meter (MX-50 (manufactured by A&D)), and the time when the moisture content reached 7% by mass or less (93% by mass or more of solid content) was set as the end point of drying, to obtain a dried cellulose fine fiber body. Equipment: FM mixer (model: FM20) manufactured by Nippon Coke & Engineering Co., Ltd. Conditions: Jacket temperature 80°C, stirring with a stirring blade (500 rpm), pressure reduced to -70 kPa with a vacuum pump. Reduced pressure drying was carried out until the product temperature reached 70°C.
[0195] [Melting and kneading] The dried cellulose fine fibers and the thermoplastic resin were fed into a twin-screw extruder so as to obtain the mass ratio shown in Table 3, melt-kneaded at a rotation speed of 250 rpm, extruded into a strand shape, water-cooled and cut to obtain a resin composition as pellets.
[0196] (Extruder Configuration) The cylinder temperature of the twin-screw extruder (OMEGA30H, manufactured by STEER, L / D=60) having 13 cylinder blocks was set to 250°C. As for the screw configuration, cylinders 1 to 3 were used as a conveying zone consisting of only a conveying screw, and two clockwise kneading discs (feed type kneading discs: hereinafter sometimes simply referred to as RKD) and two neutral kneading discs (non-conveying type kneading discs: hereinafter sometimes simply referred to as NKD) were arranged in order from the upstream side in cylinder 4. Cylinder 5 was used as a conveying zone, one RKD and two subsequent NKDs were arranged in cylinder 6, cylinders 7 and 8 were used as conveying zones, and two NKDs were arranged in cylinder 9. The following cylinder 10 was used as a conveying zone, and two NKDs and one subsequent counterclockwise screw were arranged in cylinder 11, and cylinders 12 and 13 were used as conveying zones. In addition, the cellulose fine fiber dried body and the thermoplastic resin pellets were supplied to cylinder 1. A vent port was installed at the top of cylinder 12 to enable reduced pressure suction, and vacuum suction was performed.
[0197] [Table 1]
[0198] [Table 2]
[0199] [Table 3]
[0200] As shown in Tables 1 to 3, in each Example, a concentrate having a desired cellulose fine fiber content and little variation in the content could be produced with good yield and handleability, and by using the concentrate as a filler, a filler-reinforced resin composition having excellent physical property improvement effects and fiber content stability could be produced. [Industrial Applicability]
[0201] The concentrate of the cellulose fine fiber dispersion produced by the method of the present disclosure has a small variation in the cellulose fine fiber content, and therefore can be mass-produced while maintaining the desired quality when used in applications requiring redispersion of cellulose fine fibers or uniform mixing with other materials. Therefore, the concentrate and its dried form can be suitably applied to a wide range of applications that utilize resin compositions reinforced with cellulose fine fibers, such as industrial machine parts, general machine parts, automobile / railroad / vehicle / ship / aerospace-related parts, electronic / electrical parts, building / civil engineering materials, daily necessities, sports / leisure goods, housing parts for wind power generation, containers / packaging parts, etc. [Explanation of symbols]
[0202] 11 Blades 12 grooves 21 Rotary Blade 22 Fixed blade 300 Continuous Concentrator 301 Tank 302 Pump 303 Dispersion liquid temporary storage section 304 Suction section 304a Pressure reducing mechanism 305 Filtration base material 306a, 306b, 306c, 306d Feed mechanism 307 Press Roll 308 Press Belt 309a, 309b, 309c Belt drive unit 310 Scraper 311 Collection container 312 Mixing device 312a Mixer 312b Mixing blade 313 Purification Mechanism L1 Feed Line L2 Return Line S slit θ Roll angle
Claims
1. 1. A method for producing a cellulose fine fiber dispersion concentrate, comprising the steps of: The method includes a concentration step of deliquifying the cellulose fine fiber dispersion to obtain the concentrate, the average fiber diameter of the cellulose fine fibers in the cellulose fine fiber dispersion is 50 nm or more and 1000 nm or less; In the concentrating step, the cellulose fine fiber dispersion is continuously deliquified at a treatment speed of 50 kg / h or more and less than 10,000 kg / h, The mass content of the cellulose fine fibers in the cellulose fine fiber dispersion is 0.3 mass% or more and 5.0 mass% or less, the ratio of the mass content of cellulose fine fibers in the concentrate to the mass content of cellulose fine fibers in the cellulose fine fiber dispersion is 4 or more and 100 or less; method.
2. The method according to claim 1 , wherein in the concentrating step, the cellulose fine fiber dispersion is deliquified by suction to produce an intermediate concentrate, and the intermediate concentrate is deliquified by pressing to produce a concentrate.
3. The concentrating step comprises: a tank for storing a cellulose fine fiber dispersion; a dispersion liquid temporary storage section having a slit and connected to the tank; a filtration substrate that carries and travels on the cellulose fine fiber dispersion received from the dispersion temporary storage section via the slit; a suction section for sucking and deliquifying the cellulose fine fiber dispersion on the filtration substrate through the filtration substrate to produce the intermediate concentrate; A press roll and a press belt which sandwich the intermediate concentrate and press-deliquify it to produce the concentrate; The method of claim 2 , carried out using a concentrator comprising:
4. The method of claim 3, wherein the treatment speed is controlled by adjusting a slit width of the slit and a running speed of the filtration substrate.
5. 4. The method of claim 3, wherein the suction section has two or more reduced pressure sections with different reduced pressure levels adjusted to increase in the direction of travel of the filtration substrate.
6. The method according to claim 3, wherein the filtering substrate runs on the suction section at an ascending gradient of 10° to 45°.
7. The method according to claim 3, wherein the cellulose fine fiber dispersion liquid overflowing from the dispersion liquid temporary storage section is returned to the tank, thereby circulating the cellulose fine fiber dispersion liquid between the tank and the dispersion liquid temporary storage section.
8. The method of claim 7 , wherein the tank is a tank without a stirring mechanism.
9. The method according to claim 3 , wherein the press roll presses and deliquores the intermediate concentrate together with the press belt at a roll angle in the range of 30° to 270°.
10. The filtration substrate is an endless substrate having no support, The method according to claim 3 , wherein in the concentrating step, a cleaning treatment is performed in which at least the dispersion-mounting surface of the filtration substrate is cleaned by liquid washing and / or physical scraping operation.
11. The method according to claim 3, wherein the mass content of cellulose fine fibers in the intermediate concentrate is 3 to 7 mass%.
12. The mass content of cellulose fine fibers in the intermediate concentrate is 2% by mass to 20% by mass, The method according to claim 3, wherein the mass content of cellulose fines in the concentrate is from 5% to 30% by mass.
13. The method according to claim 1, wherein, in the concentration process, when the mass content of the cellulose fine fibers in the concentrate is measured by sampling 10 points, the number average value of the mass content is 5 mass% or more and 30 mass% or less, and the CV value (standard deviation / number average value) of the mass content is 0.001 or more and 0.300 or less.
14. 2. The method of claim 1, wherein the concentrating step is carried out at 80° C. or below.
15. The method according to claim 1 , wherein the cellulose fine fibers in the cellulose fine fiber dispersion contain 70% or more, by number, of fibers having a fiber length of less than 0.1 mm.
16. 10. The method of claim 1, wherein the cellulose fibrils in the cellulose fibrils dispersion are chemically modified with hydrophobic substituents.
17. 2. The method of claim 1, wherein the cellulose fibrils in the cellulose fibrils dispersion are chemically modified with acetyl groups.
18. 10. The method of claim 1, wherein the cellulose fines in the cellulose fine dispersion are derived from cotton linters.
19. Producing a concentrate of cellulose fines dispersion by the method of any one of claims 1 to 18; drying the concentrate to produce a dried cellulose fine fiber body; The method for producing a dried cellulose fine fiber material comprises the steps of:
20. A process for producing a concentrate of a cellulose fine fiber dispersion by the method according to any one of claims 1 to 18, or a process for producing a dried cellulose fine fiber body by the method according to claim 19; mixing the concentrate of the cellulose fine fiber dispersion or the dried cellulose fine fiber with a thermoplastic resin to produce a resin composition; A method for producing a resin composition comprising the steps of:
Citation Information
Patent Citations
Dewatering process of chemically modified pulp
JP2017095813A
Method for producing plant fiber-containing resin composition, method for producing ground product of molded article, and plant fiber-containing resin composition