Bonding method and bonding system
The method and system address the inaccuracy and destructiveness of traditional bonding strength measurement by monitoring bonding speed and warpage, providing precise and waste-free estimation of bonding strength for polymerized substrates.
Patent Information
- Application Number
- JP2023084846
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Existing methods for measuring the bonding strength of polymerized substrates are inaccurate and destructive, leading to waste and limited accuracy, as they require separate measurement wafers and cannot reliably assess the actual bonding strength of product wafers.
A method and system that measures the bonding strength by monitoring the bonding speed and warpage of substrates during the bonding process, using sensors to track the progression of bonding waves and measuring the amount of warpage, allowing for non-destructive estimation of bonding strength.
Enables accurate and non-destructive estimation of bonding strength, reducing waste and improving measurement precision, while allowing the use of product wafers for bonding strength assessment.
Smart Images

Figure 2024168298000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a bonding method and a bonding system. [Background technology]
[0002] Patent Document 1 discloses a bonding device for bonding wafers together. The bonding device has an upper chuck that suction-holds an upper wafer, and a lower chuck that is provided below the upper chuck and suction-holds a lower wafer. The bonding device bonds two wafers arranged opposite each other above and below to form an overlapped wafer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-073455 A Summary of the Invention [Problem to be solved by the invention]
[0004] The technology according to the present disclosure provides a simple estimation of the bonding strength of a laminated substrate in which substrates are bonded together. [Means for solving the problem]
[0005] One aspect of the present disclosure is a method for bonding substrates together, comprising the steps of: abutting a center of a first substrate and a center of a second substrate, and sequentially bonding the first substrate and the second substrate from the center to the outer periphery to form a laminated substrate; measuring a bonding speed for bonding from the center to the outer periphery; and estimating a bonding strength of the bonded laminated substrate from the relationship between the bonding speed and the bonding strength based on the measured bonding speed. Effect of the Invention
[0006] According to the present disclosure, it is possible to easily estimate the bonding strength of a laminated substrate in which substrates are bonded together. [Brief description of the drawings]
[0007] [Figure 1] 1 is a plan view showing an outline of a configuration of a joining system according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a side view showing an outline of the configuration of an upper wafer and a lower wafer. [Diagram 3] 1 is a cross-sectional view showing an outline of the configuration of a surface modification device. [Figure 4] FIG. 2 is a cross-sectional view showing an outline of the configuration of a joining device. [Diagram 5] FIG. 2 is a cross-sectional view showing an outline of the configuration of an upper chuck and a lower chuck. [Figure 6] 1A to 1C are explanatory views showing main steps of wafer processing. [Figure 7] 1A to 1C are explanatory views showing main steps of a wafer bonding process. [Figure 8] FIG. 11 is an explanatory diagram showing how a joining speed is measured. [Figure 9] FIG. 2 is an explanatory diagram showing the arrangement of sensors. [Figure 10] FIG. 4 is an explanatory diagram showing the relationship between joining speed and joining strength. [Figure 11] FIG. 13 is an explanatory diagram showing a state in which the overlapped wafer is warped. [Figure 12] FIG. 1 is an explanatory diagram showing the reason why a laminated wafer is warped. [Figure 13] FIG. 11 is an explanatory diagram showing the relationship between the amount of warping and the bonding strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] In 3D integration technology, which stacks semiconductor devices in three dimensions, two semiconductor wafers (hereinafter referred to as "wafers") are bonded together. In the bonding process, the wafers are bonded together by, for example, van der Waals forces and hydrogen bonds (intermolecular forces).
[0009] In the bonding device disclosed in Patent Document 1, first, the center of the upper wafer, which is held by suction on the upper chuck, is pressed down by a pressing pin to bring it into contact with the center of the lower wafer, which is held by suction on the lower chuck. Then, the bonding due to the intermolecular force described above starts between the center of the surface of the pressed upper wafer and the center of the surface of the lower wafer. Next, the vacuum drawing of the upper wafer is stopped from the center to the outer periphery of the upper wafer, and the upper wafer is gradually dropped onto the lower wafer and brought into contact with it, and the bonding due to the intermolecular force between the surfaces described above gradually spreads. In this way, the surfaces of the upper wafer and the lower wafer are brought into contact with each other over their entire surfaces, and the upper wafer and the lower wafer are bonded together.
[0010] The bonding strength between the upper and lower wafers in the overlapped wafer affects the quality of the overlapped wafer. Conventionally, it is known to use the so-called blade insertion method to measure the bonding strength of the overlapped wafer. In the blade insertion method, a measurement wafer having no pattern formed on its surface, which is separate from the product wafer, is used. After bonding the measurement wafer, a blade is inserted into the bonding interface from the edge of the measurement overlapped wafer. Then, an image of a crack when the edge of the measurement overlapped wafer opens is taken to measure the radial length of the crack, and the bonding energy is calculated from the radial length of the crack using a known formula.
[0011] However, when the blade insertion method is used, the measurement wafer is damaged by the blade insertion, and the measurement wafer is discarded and cannot be reused, resulting in waste. In addition, since the wafer used is damaged in the blade insertion method, product wafers and expensive wafers with patterns cannot be used, and simple measurement wafers without patterns are used. In this case, it is difficult to measure the actual bonding strength, and there is room for improvement in the measurement accuracy.
[0012] The technology disclosed herein provides a simple method for estimating the bonding strength of a laminated substrate formed by bonding substrates together. Hereinafter, a bonding system and a bonding method according to the present embodiment will be described with reference to the drawings. In this specification and the drawings, elements having substantially the same functional configurations are denoted by the same reference numerals, and redundant description will be omitted.
[0013] <Configuration of the joining system> First, the configuration of the bonding system according to the present embodiment will be described. Fig. 1 is a plan view showing an outline of the configuration of the bonding system 1. In the following description, in order to clarify the positional relationship, the X-axis direction, the Y-axis direction, and the Z-axis direction which are orthogonal to each other are defined, and the positive direction of the Z-axis is defined as the vertically upward direction.
[0014] In the bonding system 1, a wafer W as a substrate shown in FIG. U , W L Hereinafter, the wafer placed on the upper side in the bonding device 41 described later is referred to as the “upper wafer W” as the first substrate. U The wafer placed on the lower side is called the "lower wafer W" as the second substrate. L " Also, the upper wafer W U In the lower wafer W L The surface to be joined is called "surface W U1 " and the opposite side is called "Back W U2 Similarly, the lower wafer W L In the upper wafer W U The surface to be joined is called "surface W L1 " and the opposite side is called "Back W L2 In the following description, the upper wafer W U and lower wafer W L The upper wafer W is also called the "wafer W". U Surface of W U1 and lower wafer W L Surface of W L1 are collectively referred to as "front surface W1", and the upper wafer W U Back of W U2 and the lower wafer W L Back of W L2 In the bonding system 1, the upper wafer W U and the lower wafer W L The laminated wafer W is bonded to the laminated substrate. T Form.
[0015] As shown in FIG. 2, the bonding system 1 has a configuration in which a loading / unloading station 2 and a processing station 3 are integrally connected. In the loading / unloading station 2, for example, a plurality of upper wafers W are transferred between the loading / unloading station 2 and the outside. U , lower wafer W L , laminated wafer W T Cassette C can accommodate U , C L , C T The processing station 3 carries in and out the upper wafer W U , lower wafer W L , laminated wafer W T The system is equipped with various processing devices that perform desired processing on the substrate.
[0016] The loading / unloading station 2 is provided with a cassette placement table 10. The cassette placement table 10 is provided with a plurality of, for example, four, cassette placement plates 11. The cassette placement plates 11 are arranged in a line in the Y-axis direction. The cassette placement plates 11 are provided with a cassette C U , C L , C T When loading and unloading the cassette C U , C L , C T The number of cassette placement plates 11 is not limited to that in this embodiment, and can be set arbitrarily.
[0017] In the loading / unloading station 2, a wafer transport section 20 is provided adjacent to the cassette mounting table 10 on the positive side of the X-axis of the cassette mounting table 10. The wafer transport section 20 is provided with a wafer transport device 22 that is movable on a transport path 21 extending in the Y-axis direction. The wafer transport device 22 transports the cassettes C on each cassette mounting plate 11. U , C L , C T The upper wafer W is transferred between the transition devices 50 and 51 and the warpage measuring device 52, which will be described later. U , lower wafer W L , laminated wafer W T can be transported.
[0018] Processing station 3 is provided with a plurality of processing blocks, for example, three processing blocks G1, G2, G3, each equipped with various devices. For example, a first processing block G1 is provided on the negative Y-axis side of processing station 3, and a second processing block G2 is provided on the positive Y-axis side of processing station 3. Furthermore, a third processing block G3 is provided on the negative X-axis side of processing station 3.
[0019] The first processing block G1 is provided with a surface modification device 30 for modifying the surface W1 of the wafer W. The second processing block G2 is provided with a surface hydrophilization device 40 for hydrophilizing the surface W1 of the wafer W and cleaning the surface W1, and a surface hydrophilization device 50 for cleaning the upper wafer W. U and the lower wafer W L The third processing block G3 includes a bonding device 41 for bonding the upper wafer W to the lower wafer W. U , lower wafer W L , laminated wafer W T The transition devices 50 and 51 temporarily hold the overlapped wafer W. T A warpage measuring device 52 is disposed in a layered manner as a warpage measuring section for measuring the amount of warpage of the substrate.
[0020] In the surface hydrophilization device 40, pure water is supplied onto the surface W1 of the wafer W while rotating the wafer W held by, for example, a spin chuck. The supplied pure water then spreads over the surface W1 of the wafer W, making the surface W1 hydrophilic. Note that the above configuration is merely an example, and the surface hydrophilization device 40 may have any configuration as long as it can make the surface W1 of the wafer W hydrophilic. The configurations of the surface modification device 30 and the bonding device 41 will be described later.
[0021] The transition devices 50 and 51 are U , lower wafer W L , laminated wafer W T In order to transfer the upper wafer W between the wafer transfer device 22 of the wafer transfer section 20 and the wafer transfer device 62 of the wafer transfer section 60 described later, U , lower wafer W L , laminated wafer W TThe warpage measuring device 52 temporarily holds the bonded overlapped wafer W. T The warpage of the overlapped wafer W is measured using a displacement meter. T The amount of warping is measured.
[0022] A wafer transfer section 60 is provided in an area surrounded by the first processing block G1 to the third processing block G3. The wafer transfer section 60 is provided with a wafer transfer device 62 that is movable on a transfer path 61 extending in the X-axis direction. The wafer transfer device 62 transfers the upper wafer W between the surface modification device 30, the surface hydrophilization device 40, the bonding device 41, the transition devices 50 and 51, and the warpage measurement device 52. U , lower wafer W L , laminated wafer W T can be transported.
[0023] The bonding system 1 described above is provided with a control device 70. The control device 70 is, for example, a computer equipped with a CPU, a memory, and the like, and has a program storage unit (not shown). A program for controlling wafer processing in the bonding system 1 is stored in the program storage unit. The program may be recorded in a computer-readable storage medium H and installed from the storage medium H to the control device 70. The storage medium H may be temporary or non-temporary.
[0024] <Configuration of surface modification equipment> In the above-described surface modification apparatus 30, for example, in a reduced pressure atmosphere, oxygen gas or nitrogen gas serving as a processing gas is excited to be turned into plasma and ionized. The oxygen ions or nitrogen ions are irradiated onto the surface W1 of the wafer W, so that the surface W1 is subjected to the plasma processing and modified.
[0025] As shown in FIG. 3, the surface modification apparatus 30 includes a processing vessel 100 , a processing gas supply unit 110 , a plasma generation unit 120 , an ion attraction unit 130 , and an exhaust unit 140 .
[0026] The processing vessel 100 is configured so that the inside can be sealed. The processing vessel 100 is formed with a loading / unloading port for the wafer W (not shown), and the loading / unloading port is provided with a gate valve (not shown). A stage 101 is disposed on the bottom side of the processing vessel 100, and the stage 101 holds the back surface W2 of the wafer W by suction so that the front surface W1 of the wafer W faces upward. At least a portion of the stage 101 is made of, for example, an insulating material.
[0027] The process gas supply unit 110 supplies a process gas into the process vessel 100. The process gas supply unit 110 includes a gas supply line 111 for introducing the process gas into the process vessel 100, at least one gas supply source 112, and at least one flow rate controller 113. The gas supply line 111 introduces the process gas supplied from the gas supply source 112 into the process vessel 100. The flow rate controller 113 may include, for example, a mass flow controller, a pressure control type, or a flow rate modulation device. Note that the process gas supplied from the gas supply source 112 is not limited to oxygen gas or nitrogen gas, and may be, for example, argon gas or helium gas.
[0028] The plasma generating unit 120 generates plasma of the processing gas inside the processing vessel 100. In the illustrated example, the plasma generating unit 120 includes a surface wave plasma (SWP) type plasma generating device, but the configuration of the plasma generating unit 120 is not particularly limited. The plasma generating unit 120 may be configured with any plasma generating device such as a capacitively coupled plasma (CCP), an inductively coupled plasma (ICP), an electron-cyclotron-resonance plasma (ECR plasma), or a helicon wave plasma (HWP). In addition, various types of plasma generating units may be used, including an alternating current (AC) plasma generating unit and a direct current (DC) plasma generating unit.
[0029] The ion drawing unit 130 draws ions distributed inside the plasma generated in the processing vessel 100 to the surface W1 of the wafer W on the stage 101. In one example, the ion drawing unit 130 has at least one electrode 131, a high frequency power supply 132, and a capacitor 133. Note that the high frequency power supply 132 may be used to generate plasma inside the processing vessel 100, in addition to drawing ions to the surface W1 of the wafer W. Therefore, the high frequency power supply 132 supplies at least one of source power and bias power to the electrode 131.
[0030] The exhaust unit 140 is connected to, for example, a gas exhaust port 100e provided at the bottom of the processing vessel 100. The exhaust unit 140 may include a pressure regulating valve and a vacuum pump. The internal pressure of the processing vessel 100 is adjusted by the pressure regulating valve. The vacuum pump may include a turbo molecular pump, a dry pump, or a combination thereof.
[0031] The above is a configuration of the surface modification apparatus 30. Note that the above configuration is just an example, and the surface modification apparatus 30 may have any configuration as long as it can modify the surface W1 of the wafer W.
[0032] <Configuration of the joining device> In the above-mentioned bonding apparatus 41, the upper wafer W U and the lower wafer W L and surface W, which has been subjected to surface modification treatment and surface hydrophilization treatment in sequence. U1 , surface W L1 Join with.
[0033] As shown in FIG. 4, the bonding apparatus 41 includes a processing vessel 200 , an upper chuck 210 , and a lower chuck 220 .
[0034] The processing vessel 200 is configured so that the inside can be sealed. The processing vessel 200 is formed with a loading / unloading port for the wafer W (not shown), and the loading / unloading port is provided with a gate valve (not shown). The upper chuck 210 is provided on the top side of the processing vessel 200, and the lower chuck 220 is provided on the bottom side of the processing vessel 200.
[0035] The upper chuck 210 supports the upper wafer WU Back of W U2 The upper chuck 210 is supported by an upper chuck stage 211 provided above the upper chuck 210. The upper chuck stage 211 supports the lower wafer W held by the lower chuck 220. L Surface of W L1 An upper imaging section 212 is provided to capture an image of the upper portion of the substrate 210. The upper imaging section 212 may be, for example, a CCD camera.
[0036] The upper chuck stage 211 is supported by a rotating part 214 provided on the ceiling surface of the processing vessel 200 via a plurality of support members 213 above the upper chuck stage 211. The rotating part 214 rotates the upper chuck stage 211 and the upper chuck 210 around a vertical axis (θ-axis). The rotating part 214 may be provided with a measuring part (e.g., a linear scale) (not shown) for measuring the position of the upper chuck 210 in the θ-axis direction.
[0037] The lower chuck 220 holds the lower wafer W L Back of W L2 The lower chuck 220 is provided below the upper chuck 210 and is configured to be able to be arranged opposite the upper chuck 210. That is, the upper wafer W held by the upper chuck 210 is attracted to the lower chuck 220. U and the lower wafer W held by the lower chuck 220. L The lower chuck 220 is supported by a lower chuck stage 221 provided below the lower chuck 220. The lower chuck stage 221 supports the upper wafer W held by the upper chuck 210. U Surface of W U1 The lower imaging section 222 is provided to capture an image of the lower portion of the substrate 210. The lower imaging section 222 may be, for example, a CCD camera.
[0038] The lower chuck 220 is provided with a moving unit 223. The moving unit 223 moves the lower chuck stage 221 and the lower chuck 220 in the horizontal direction. The moving unit 223 also moves the lower chuck 220 in the vertical direction. The moving unit 223 may be provided with a measurement unit (e.g., a laser interferometer) (not shown) for measuring the horizontal and vertical positions of the lower chuck 220.
[0039] Next, the detailed configurations of the upper chuck 210 and the lower chuck 220 will be described together with the peripheral members.
[0040] 5, a pin chuck system is adopted for the upper chuck 210. The upper chuck 210 holds the upper wafer W in a plan view. U The main body 230 has a diameter equal to or larger than the diameter of the upper wafer W. U Back of W U2 The main body 230 has a plurality of pins 231 on the outer periphery of the lower surface thereof, which have the same height as the pins 231 and contact the upper wafer W. U Back of W U2 An outer rib 232 is provided to support the outer periphery of the pins 231. The outer rib 232 is provided in an annular shape on the outside of the pins 231.
[0041] In addition, on the lower surface of the main body 230, inside the outer rib 232, there is a pin 231 having the same height as the upper wafer W. U Back of W U2 An inner rib 233 is provided to support the inner rib 232. The inner rib 233 is provided in an annular shape concentric with the outer rib 232. An inner region 234 of the outer rib 232 (hereinafter, sometimes referred to as the suction region 234) is divided into a first suction region 234a on the inner side of the inner rib 233 and a second suction region 234b on the outer side of the inner rib 233.
[0042] The lower surface of the main body 230 is provided with a first suction region 234a, on which the upper wafer W UA first suction port 235a is formed in the first suction region 234a to draw a vacuum. The first suction port 235a is formed at a plurality of locations in the first suction region 234a, for example. A first suction pipe 236a provided inside the main body 230 is connected to the first suction port 235a. Furthermore, a vacuum pump (not shown) is connected to the first suction pipe 236a.
[0043] In addition, the lower surface of the main body 230 is provided with a second suction region 234b, which is provided with the upper wafer W. U A second suction port 235b is formed in the second suction region 234b to draw a vacuum. The second suction port 235b is formed at a plurality of locations in the second suction region 234b, for example. A second suction pipe 236b provided inside the main body 230 is connected to the second suction port 235b. Furthermore, a vacuum pump (not shown) is connected to the second suction pipe 236b.
[0044] Upper wafer W U The suction regions 234a and 234b formed by the main body 230 and the outer rib 232 are evacuated through the suction ports 235a and 235b, respectively, to reduce the pressure in the suction regions 234a and 234b. The upper chuck 210 suctions the upper wafer W for each of the first suction region 234a and the second suction region 234b. U The substrate is configured to be capable of being adsorbed and held thereon.
[0045] A through hole 237 is formed in the center of the main body 230 of the upper chuck 210 and the center of the upper chuck stage 211, penetrating the main body 230 and the upper chuck stage 211 in the thickness direction. The center of the main body 230 is a hole for holding the upper wafer W held by the upper chuck 210. U The through hole 237 is adapted to receive an actuator portion 241 of a pushing portion 240, which will be described later.
[0046] Two transmission windows 238a, 238b are formed on the outer periphery of the main body 230 of the upper chuck 210 and the outer periphery of the upper chuck stage 211, penetrating the main body 230 and the upper chuck stage 211 in the thickness direction. The first transmission window 238a and the second transmission window 238b are arranged in this order from the inside to the outside in the radial direction. The transmission windows 238a, 238b are made of, for example, quartz, and transmit LED light irradiated from sensors 250a, 250b, which will be described later.
[0047] The upper chuck stage 211 has an upper wafer W at its center. U The center of the back W U2 The pressing portion 240 has an actuator portion 241 and a cylinder portion 242.
[0048] The actuator portion 241 is capable of being raised and lowered in the vertical direction through the through hole 237 by air from, for example, an electropneumatic regulator. U and the upper wafer W U The pressure load applied to the center of the material can be controlled.
[0049] The actuator portion 241 is supported by a cylinder portion 242. The cylinder portion 242 can move the actuator portion 241 in the vertical direction by a drive portion having a built-in motor, for example.
[0050] As described above, the pressing unit 240 controls the pressing load by the actuator unit 241, and controls the movement of the actuator unit 241 by the cylinder unit 242. The pressing unit 240 presses the wafer W, which will be described later, against the wafer W. U , W L When bonding the upper wafer W U The center of the lower wafer W L The center of the plate can be brought into contact with the plate and pressed against it.
[0051] A plurality of sensors, for example, two sensors 250a and 250b, are provided on the outer periphery of the upper chuck stage 211. The first sensor 250a and the second sensor 250b are arranged in this order from the inside to the outside in the radial direction. The first sensor 250a is arranged corresponding to the first transmission window 238a, and the second sensor 250b is arranged corresponding to the second transmission window 238b.
[0052] The sensors 250a and 250b are connected to the upper wafer W U Back of W U2 The measurement results of the sensors 250a and 250b are output to the control device 70, which then controls the height position of the upper wafer W as described below. U Back of W U2 The bonding speed (bonding wave propagation speed) is calculated based on the height position of the bonding wave. That is, the sensors 250a and 250b correspond to the speed measurement unit in this disclosure.
[0053] The lower chuck 220 employs a pin chuck system similar to the upper chuck 210. The lower chuck 220 supports the lower wafer W in a plan view. L The main body 260 has a diameter equal to or larger than the diameter of the lower wafer W. L Back of W L2 The main body 260 is provided with a plurality of pins 261 on the outer periphery of the upper surface thereof, which have the same height as the pins 261 and are in contact with the lower wafer W. L Back of W L2 An outer rib 262 is provided to support the outer periphery of the pins 261. The outer rib 262 is provided in an annular shape on the outside of the pins 261.
[0054] In addition, on the upper surface of the main body 260, inside the outer rib 262, there is a pin 261 having the same height as the lower wafer W. L Back of W L2An inner rib 263 is provided to support the inner rib 263. The inner rib 263 is provided in an annular shape concentric with the outer rib 262. An inner region 264 of the outer rib 262 (hereinafter sometimes referred to as the suction region 264) is divided into a first suction region 264a on the inner side of the inner rib 263 and a second suction region 264b on the outer side of the inner rib 263.
[0055] The upper surface of the main body 260 is provided with a first suction region 264a, on which the lower wafer W L A first suction port 265a is formed in the first suction region 264a to draw a vacuum. The first suction port 265a is formed at one location in the first suction region 264a, for example. A first suction pipe 266a provided inside the main body 260 is connected to the first suction port 265a. Furthermore, a vacuum pump (not shown) is connected to the first suction pipe 266a.
[0056] In addition, on the upper surface of the main body 260, the lower wafer W is L A second suction port 265b is formed in the second suction region 264b to draw a vacuum. The second suction port 265b is formed at a plurality of locations in the second suction region 264b, for example. A second suction pipe 266b provided inside the main body 260 is connected to the second suction port 265b. Furthermore, a vacuum pump (not shown) is connected to the second suction pipe 266b.
[0057] Lower wafer W L The suction regions 264a and 264b formed by the main body 260 and the outer rib 262 are evacuated through the suction ports 265a and 265b, respectively, to reduce the pressure in the suction regions 264a and 264b. The lower chuck 220 holds the lower wafer W in each of the first suction region 264a and the second suction region 264b. L The substrate is configured to be capable of being adsorbed and held thereon.
[0058] In the lower chuck 220, near the center of the main body 260, through holes (not shown) are formed in, for example, three places, penetrating the main body 260 in the thickness direction. Lifting pins provided below the moving part 223 are inserted into the through holes.
[0059] The wafer W is mounted on the outer periphery of the main body 260. U , W L , laminated wafer W T A guide member (not shown) is provided to prevent the lower chuck 220 from jumping out or sliding off from the lower chuck 220. The guide members are provided at multiple locations, for example, four locations, at equal intervals on the outer periphery of the main body 260.
[0060] In addition, the bonding device 41 includes an upper wafer W that is transported to the bonding device 41 and is attracted and held by the upper chuck 210. U A reversing device (not shown) may be provided to reverse the front and back sides of the upper wafer W. U is a surface W that has been subjected to surface modification and surface hydrophilization treatment. U1 The reverse side W is conveyed facing up, but the reverse side is reversed by this reversing device, so that the reverse side W is properly conveyed. U2 can be held by the upper chuck 210. However, the location of the inversion device is not limited to this. Instead of inside the bonding device 41, the upper wafer W may be placed at any position in the processing station 3 of the bonding system 1. U A reversing device (not shown) for reversing the front and back sides may be provided separately.
[0061] The bonding apparatus 41 is configured as described above. Note that the above configuration is an example. U Surface of W U1 and the lower wafer W L Surface of W L1 Any configuration can be adopted as long as the above can be joined.
[0062] <Joining method> Next, the bonding of the upper wafer W is performed using the bonding system 1 configured as above. U and the lower wafer W L 6 is an explanatory diagram showing main steps of wafer processing in the bonding system 1. As shown in FIG.
[0063] First, a plurality of upper wafers W U Cassette C containingU , multiple lower wafers W L Cassette C containing L , and an empty cassette C T The cassette C is placed on the cassette placement plate 11 of the loading / unloading station 2. Then, the cassette C is U Upper wafer W U is removed and transported to the transition device 50 of processing station 3.
[0064] Next, the upper wafer W U The upper wafer W is transported to the surface modification device 30 by the wafer transport device 62. In the surface modification device 30, the processing gas, oxygen gas or nitrogen gas, is excited to be turned into plasma and ionized in a desired reduced pressure atmosphere. The oxygen ions or nitrogen ions are then ionized into the upper wafer W. U Surface of W U1 is irradiated onto the surface W U1 The upper wafer W is then subjected to plasma processing. U Surface of W U1 is modified (step SU1 in FIG. 6).
[0065] Next, the upper wafer W U The upper wafer W held by the spin chuck is transferred to the surface hydrophilization device 40 by the wafer transfer device 62. U While rotating the upper wafer W U The pure water is then supplied to the upper wafer W. U Surface of W U1 The upper wafer W is then diffused and modified in the surface modification device 30. U Surface of W U1 Hydroxyl groups (silanol groups) are attached to the surface W U1 The upper wafer W is made hydrophilic by the pure water. U Surface of W U1 is washed (step SU2 in FIG. 6).
[0066] Next, the upper wafer W U The upper wafer W is transferred to the bonding device 41 by the wafer transfer device 62. UThe upper wafer W is then turned over by a turning device (not shown). U The horizontal direction of the back surface W is adjusted by a position adjustment mechanism (not shown). U2 Specifically, the upper wafer W is attracted and held in the suction regions 234a and 234b through the suction ports 235a and 235b. U The upper wafer W is vacuumed. U is attracted and held by the upper chuck 210.
[0067] Upper wafer W U While the above-mentioned various processes are being performed on the upper wafer W U Next, the lower wafer W L First, the wafer transfer device 22 transfers the wafer to the cassette C. L Lower wafer W L is removed and transported to the transition device 50 of processing station 3.
[0068] Next, the lower wafer W L The lower wafer W is transferred to the surface modification device 30 by the wafer transfer device 62. L Surface of W L1 The lower wafer W in step SL1 is modified (step SL1 in FIG. 6). L Surface of W L1 The modification is the same as in the above-mentioned step SU1.
[0069] Next, the lower wafer W L The lower wafer W is transferred to the surface hydrophilization device 40 by the wafer transfer device 62. L Surface of W L1 is hydrophilized and the surface W L1 The lower wafer W is cleaned (step SL2 in FIG. 6). L Surface of W L1 The hydrophilization and washing are similar to those in the above-mentioned step SU2.
[0070] Next, the lower wafer W L The lower wafer W is transferred to the bonding device 41 by the wafer transfer device 62. LAfter the horizontal direction is adjusted by a position adjustment mechanism (not shown), the back surface W is attached to the lower chuck 220. L2 Specifically, the lower wafer W is attracted and held in the suction regions 264a and 264b through the suction ports 265a and 265b. L The lower wafer W is vacuumed. L is sucked and held by the lower chuck 220.
[0071] Next, the upper wafer W held by the upper chuck 210 U and the lower wafer W held by the lower chuck 220. L Specifically, the upper imaging unit 212 adjusts the horizontal position of the lower wafer W held by the lower chuck 220. L Surface of W L1 The upper wafer W held by the upper chuck 210 is imaged by the lower imaging unit 222 in sequence. U Surface of W U1 The control device 70 sequentially captures images of predetermined reference points on the upper wafer W based on the images captured by the upper imaging unit 212 and the images captured by the lower imaging unit 222. U The reference point and the lower wafer W L The upper chuck 210 (upper wafer W) is rotated by the rotating part 214 so that the reference points of the upper chuck 210 and the upper wafer W are aligned with each other. U ) is rotated, and the lower chuck 220 (lower wafer W) is moved by the moving part 223. L In this way, the upper wafer W U and the lower wafer W L The position of the upper wafer W is adjusted. U and the lower wafer W L are disposed opposite each other at a desired position.
[0072] Next, the upper wafer W held by the upper chuck 210 U and the lower wafer W held by the lower chuck 220. L Specifically, the lower chuck 220 is moved vertically upward by the moving part 223 to adjust the vertical position of the upper wafer W. U and the lower wafer W LThen, as shown in FIG. 7(a), the vertical position of the upper wafer W U and the lower wafer W L are disposed opposite each other at a desired position.
[0073] Next, the upper wafer W U and the lower wafer W L The bonding process is then performed (step S3 in FIG. 6). Specifically, first, as shown in FIG. 7(b), the actuator part 241 is lowered by the cylinder part 242, and the actuator part 241 is brought into contact with the upper wafer W. U Back of W U2 The center of the plate is abutted against the plate.
[0074] Next, as shown in FIG. 7(c), the actuator part 241 continues to move downward to the upper wafer W U The upper wafer W is lowered by pressing the center of the U The center of the lower wafer W L At this time, the upper wafer W is pressed against the first suction port 235a in the first suction region 234a. U The vacuum pumping of the upper wafer W is stopped, and the second suction region 234b is vacuum pumped through the second suction port 235b. U Hold the outer periphery.
[0075] Upper wafer W U The center of the lower wafer W L When the centers of the upper wafer W and the lower wafer W are pressed against each other, U and the lower wafer W L The bonding of the upper wafer W starts (thick line in FIG. 7(c)). U Surface of W U1 and the lower wafer W L Surface of W L1 Since the surfaces are modified in steps SU1 and SL1, respectively, the surface W U1 , W L1 Van der Waals forces (intermolecular forces) occur between the surfaces W U1 , W L1 The upper wafer W U Surface of W U1 and the lower wafer WL Surface of W L1 Since the surfaces are hydrophilized in steps SU2 and SL2, respectively, the surface W U1 , W L1 Hydrophilic groups between the surfaces form hydrogen bonds (intermolecular forces), U1 , W L1 As shown in FIG. 7(d), the above-mentioned surface W U1 , surface W L1 The bonding between the particles due to van der Waals forces and hydrogen bonds diffuses from the center to the periphery, generating a bonding wave.
[0076] After that, the upper wafer W is pushed by the pushing part 240 as shown in FIG. U The center of the lower wafer W L In a state where the center of the upper wafer W is pressed, the upper wafer W is sucked from the second suction port 235b in the second suction region 234b. U The vacuum pumping of the upper wafer W is then stopped. U The outer periphery of the lower wafer W L Then, as shown in FIG. 7(f), the upper wafer W U Surface of W U1 and the lower wafer W L Surface of W L1 The upper wafer W U and the lower wafer W L are joined.
[0077] Upper wafer W U and the lower wafer W L The laminated wafer W T The overlapped wafer W is transported to the warpage measuring device 52 by the wafer transport device 62. T The amount of warping is then measured. T The cassette C is transferred to the wafer transfer device 22 of the transfer station 2. T In this way, a series of upper wafers W U and the lower wafer W L The wafer processing (bonding processing) is then completed.
[0078] In this way, the upper wafer W U and the lower wafer WL The laminated wafer W formed by bonding T The upper wafer W is then subjected to a heating (annealing) process in a heating device provided outside the bonding system 1 (step S4 in FIG. 6). Although this heating process may be performed outside the bonding system 1 in this way, a heating device (not shown) may be provided in the processing station 3 of the bonding system 1 to heat the upper wafer W in the bonding device 41. U and the lower wafer W L Alternatively, the above-mentioned step may be performed after the joining.
[0079] In addition, the heat-treated laminated wafer W T Then, the back surface W is ground by a grinding device provided outside the bonding system 1. U2 Then, the back surface W is removed in an etching device provided outside the bonding system 1. U2 Then, the overlapped wafer W T is thinned.
[0080] <Method of estimating bond strength> Next, the laminated wafer W bonded as described above is T The method for estimating the bonding strength of the overlapped wafer W will be described in two embodiments. T The bonding strength of the laminated wafer W after heat treatment is T The bond strength is estimated.
[0081] (First embodiment) In the first embodiment, the overlapped wafer W is determined based on the bonding speed (the propagation speed of the bonding wave). T The bond strength is estimated.
[0082] In the bonding device 41, as described above, a bonding wave is generated that spreads from the center to the outer periphery of the upper wafer W. U and the lower wafer W L At this time, the upper wafer W U Back of W U2 Since the height of the bonding wave changes, the bonding speed, which is the propagation speed of the bonding wave, is measured based on this height position.
[0083] As shown in FIG. 8, the sensors 250a and 250b are U Back of W U2 Specifically, the sensors 250a and 250b measure the height position of the upper wafer W through the transmission windows 238a and 238b. U Back of W U2 The LED light is irradiated onto the back surface W U2 The light reflected from the back W U2 The height position of the upper wafer W is measured. The measurement results of the sensors 250a and 250b are output to the control device 70. Note that the transmission windows 238a and 238b may be omitted, and a through hole (not shown) may be formed penetrating the main body 230 of the upper chuck 210 and the upper chuck stage 211. In such a case, the LED light from the sensors 250a and 250b passes through the through hole and is incident on the upper wafer W. U Back of W U2 is irradiated.
[0084] In the control device 70, the upper wafer W U Back of W U2 Specifically, the controller 70 calculates the bonding speed based on the height position of the upper wafer W. U Back of W U2 The bonding wave is detected from the height position of the upper wafer W. U Back of W U2 The height position of the upper wafer W U and the lower wafer W L The arrival of the bonding wave is detected when the bonding wave reaches the position where the first sensor 250a and the second sensor 250b were joined. Then, the time from when the bonding wave reaches the position of the first sensor 250a to when the bonding wave reaches the position of the second sensor 250b is calculated, and the joining speed is calculated from the distance between the sensors 250a and 250b, which is known in advance.
[0085] The bonding wave advances concentrically from the center to the outer periphery. Therefore, if the bonding speed between at least two sensors 250a and 250b arranged in the radial direction is measured, the measured bonding speed represents the bonding speed of the bonding wave.
[0086] As shown in FIG. 9, the upper surface of the upper chuck stage 211 may be provided with three or more sensors 250a to 250g.
[0087] For example, the sensor 250c is disposed at the center. In this case, the bonding speed between the sensors 250c, 250a, and 250b can be measured in the radial direction D1. When comparing the bonding speed between the sensors 250c and 250a with the bonding speed between the sensors 250a and 250b, it is preferable to measure the bonding speed between the sensors 250a and 250b on the outer periphery side. U The center of the lower wafer W L Since the center of the sensor 250c is pressed, the bonding wave between the sensors 250a and 250b is affected by the pressing of the center. For this reason, it is preferable to measure the bonding speed between the sensors 250a and 250b, which are located away from the actuator part 241. In addition, the inner rib 233 is located between the sensors 250c and 250a, and the measurement of the bonding speed may be affected by the individual difference between the vacuum pump communicating with the first suction port 235a on the inner side of the inner rib 233 and the vacuum pump communicating with the second suction port 235b on the outer side of the inner rib 233. In this regard, there is no inner rib between the sensors 250a and 250b, that is, the sensors 250a and 250b are provided in the same second suction region 234b, so that the bonding speed can be measured without being affected by the individual difference between the vacuum pumps.
[0088] For example, the sensors 250d and 250e are arranged in this order in the radial direction D2. The sensor 250d is arranged on the same circumference as the sensor 250a, and the sensor 250e is arranged on the same circumference as the sensor 250b. In this case, the bonding speed between the sensors 250d and 250e can be measured in the radial direction D2. Note that in the radial directions D1 and D2, the bonding speed of the upper wafer W UThe crystal orientation may be different between the cross and the diagonal. When the crystal orientation is different in this way, the joining speed may be different in the radial directions D1 and D2. Therefore, for example, the average value of the joining speed in the radial direction D1 and the joining speed in the radial direction D2 may be calculated, and the average value may be used as the joining speed of the bonding wave. In such a case, the joining speed can be measured more accurately.
[0089] For example, the sensors 250f and 250g are arranged on opposite sides of the center in the radial direction D3. The sensor 250f is arranged on the same circumference as the sensor 250a, and the sensor 250g is arranged on the same circumference as the sensor 250b. In this case, the welding speed between the sensors 250f and 250g can be measured in the radial direction D3. By measuring the welding speed in a plurality of radial directions D1, D2, and D3 in this manner, the number of measurements of the welding speed increases, and the welding speed can be measured more accurately.
[0090] Here, the inventors have intensively studied and found that the bonding speed, which is the propagation speed of the bonding wave, and the overlapped wafer W after the heat treatment T It was found that there is a correlation between the bonding speed (horizontal axis) and the bonding strength (vertical axis) of the overlapped wafers W. T The bonding speed and bonding strength were investigated and plotted in Figure 10. Referring to Figure 10, there is a correlation shown by the dotted line.
[0091] Therefore, the overlapping wafer W T Before the wafer processing, the first correlation between the bonding speed and the bonding strength is obtained and stored in a database. T The first correlation is, for example, the bonding strength of the upper wafer W U Surface of W U1 and the lower wafer W L Surface of W L1 The first correlation is obtained for each of the characteristics of the upper wafer W. U and the lower wafer W LBased on the measured bonding speed, the bonding speed of the overlapped wafer W after bonding is calculated from the first correlation in the bonding speed database. T The joining speed can be estimated.
[0092] Second embodiment In the second embodiment, the bonded overlapped wafer W T Based on the amount of warping, the laminated wafer W T The bond strength is estimated.
[0093] In the bonding device 41, as described above, a bonding wave is generated that spreads from the center to the outer periphery of the upper wafer W. U and the lower wafer W L At this time, the upper wafer W is bonded by the pushing part 240. U The center of the lower wafer W L As shown in FIG. 11, the upper wafer W U Specifically, during bonding, the upper wafer W U and the lower wafer W L The air between the lower wafer W and the lower wafer W is pushed out from the center to the outer periphery. L The upper wafer W is fixed by suction to the lower chuck 220. U Since the upper wafer W is not fixed to the upper chuck 210, the upper wafer W is moved by the viscosity of air. U In this case, the upper wafer W U and the lower wafer W L Even if the centers of the upper wafer W and the lower wafer W are aligned, the outer periphery of the upper wafer W may be misaligned in the horizontal direction. This phenomenon is called scaling. U The bonded laminated wafer W T bends downward convexly.
[0094] In the warpage measuring device 52, the bonded laminated wafer W T As shown in Figure 12, the amount of warpage R of the upper wafer W U Back of W U2 is the difference between the height position of the center and the height position of the outer periphery.
[0095] Here, the inventors have intensively studied and found that this laminated wafer W T The amount of warping of the laminated wafer W after heat treatment T FIG. 13 is an explanatory diagram showing the relationship between the amount of warpage (horizontal axis) and the bonding strength (vertical axis). T The warpage and bonding strength were investigated and plotted in Fig. 13. Referring to Fig. 13, there is a correlation shown by the dotted line.
[0096] Therefore, the overlapping wafer W T Before the wafer processing, the second correlation between the amount of warpage and the bonding strength is obtained and stored in a database. T The second correlation is, for example, the bonding strength of the upper wafer W U Surface of W U1 and the lower wafer W L Surface of W L1 The second correlation is obtained for each of the plasma processing conditions in the surface modification device 30. T Based on the measured amount of warping, the bonded overlapped wafer W is calculated from the second correlation in the database. T The joining speed can be estimated.
[0097] The lower chuck 220 may be, for example, a flat chuck with a flat surface or a deformed chuck with a deformed surface that is convex upward. L is deformed convexly, the above-mentioned scaling is corrected, and the bonded overlapped wafer W T On the other hand, when a flat chuck is used, the warping of the lower wafer W is suppressed. L Since the wafer is kept flat, scaling occurs and the overlapped wafer W after bonding T For this reason, the second embodiment is useful when a flat chuck is used as the lower chuck 220.
[0098] As described above, according to the first embodiment, the bonding speed during bonding and the overlapped wafer W T Based on the first correlation with the bonding strength of the laminated wafer W T According to the second embodiment, the bonding strength of the overlapped wafer W after bonding can be estimated. T Warpage of the laminated wafer W T Based on the second correlation with the bonding strength of the laminated wafer W T In any of the embodiments, the bonding strength of the overlapped wafer W can be estimated without using the conventional blade insertion method. T As a result, it is not necessary to prepare a wafer for measurement as in the past, and it is possible to non-destructively estimate the bonding strength of the product-grade overlapped wafer W. T This allows the bonding strength of the wire to be estimated, thus reducing waste that would occur if the conventional blade insertion method were used.
[0099] In addition, in the conventional blade insertion method, a simple measurement wafer without a pattern is used, but according to the above embodiment, a product overlapped wafer W T Therefore, the accuracy of measuring the actual bonding strength can be improved.
[0100] In addition, the first and second embodiments may be combined. That is, the bonding speed during bonding and the overlapped wafer W after bonding may be changed. T The combination of the warpage of the laminated wafer W T The third correlation between the bonding strength of the upper wafer W and the bonding strength of the lower wafer W is obtained and stored in a database. U and the lower wafer W L The bonding speed when bonding the overlapped wafer W is measured, and the warp measuring device 52 measures the warp of the overlapped wafer W. T Based on the measured bonding speed and the amount of warping, the bonded laminated wafer W is calculated from the third correlation in the database. T In this case, the welding speed can be estimated with higher accuracy.
[0101] In the above embodiment, the overlapped wafer W after bondingT The amount of warpage of the overlapped wafer W was measured by the warpage measuring device 52. The bonding device 41 was provided with a warpage measuring section, and the amount of warpage of the overlapped wafer W was measured by the warpage measuring section. T Alternatively, the amount of warping of the overlapped wafer W may be measured. T The amount of warpage may be measured by a warpage measuring device provided outside the bonding system 1.
[0102] In the above embodiments, the first correlation, the second correlation, and the third correlation are based on the heat treatment of the laminated wafer W T The bonding strength of the laminated wafer W before the heat treatment was measured. T In this case, the bonding strength of the overlapped wafer W after bonding but before the heat treatment may be measured. T The bond strength can be estimated.
[0103] <How to use estimated bond strength> Next, the overlapped wafer W estimated as above T This section explains how to utilize the bonding strength.
[0104] (1st usage method) Estimated overlapping wafer W T Based on the bonding strength of the laminated wafer W T For example, the bonding strength may be compared with a predetermined threshold value, and if the bonding strength is equal to or greater than the threshold value, the overlapped wafer W may be determined. T is judged to be normal, and if the bonding strength is less than the threshold value, the overlapped wafer W T is determined to be abnormal.
[0105] Overlapped Wafer W T If it is determined that the overlapped wafer W is abnormal, a warning may be output and the subsequent wafer processing may be stopped. T The normal laminated wafer W is flagged as abnormal. T The overlapped wafer W may be distinguished from the overlapped wafer W and the subsequent wafer processing may be continued. TIf it is determined that the bonding process is abnormal, a pre-processing inspection may be performed. As the pre-processing inspection, for example, the plasma processing conditions in the surface modification device 30 of the bonding system 1 may be inspected. Alternatively, the conditions when a film formation process is performed on the front surface W1 of the wafer W outside the bonding system 1, or the conditions when the front surface W1 is polished may be inspected.
[0106] (Second usage method) Estimated overlapping wafer W T The processing conditions for each process may be feedback-controlled based on the bonding strength.
[0107] For example, a laminated wafer W T Based on the bonding strength of the upper wafer W on the upper chuck 210, the bonding conditions when the bonding process of the step S3 is performed by the bonding device 41 are feedback-controlled. U The chucking pressure of the lower wafer W on the lower chuck 220 L The chucking pressure of the actuator 241 of the pushing part 240, the stroke (movement distance) of the actuator 241 of the pushing part 240, U , W L The pressure when pressing the center of the wafer W after adjusting the vertical position U , W L The distance between them, etc.
[0108] For example, a laminated wafer W T Based on the bonding strength, the plasma processing conditions (modification conditions) for performing the surface modification processing of steps SU1 and SU2 in the surface modification apparatus 30 are feedback-controlled. Examples of the plasma processing conditions that are feedback-controlled include the source power of the high-frequency power supply 132, the pressure inside the processing vessel 100, the processing time of the plasma processing, and the flow rate of the processing gas supplied from the processing gas supply unit 110.
[0109] (Third usage method) The control device 70 determines the estimated overlapped wafer W T The information on the bonding strength may be output to a device that performs a post-process of the bonding process.
[0110] The post-processing device may be any device, such as a peeling device. T Insert the blade into the bonding interface of the upper wafer W U and the lower wafer W L Then, the upper wafer W is separated by a pad. U By holding and moving the lower wafer W L At this time, the peeling conditions are feed-forward controlled based on the output bonding strength. Examples of the peeling conditions that are feed-forward controlled include the blade insertion speed, the pad movement speed (peeling speed), and the pad movement position.
[0111] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. For example, the components of the above-described embodiments may be arbitrarily combined. From such an arbitrary combination, the actions and effects of each of the components in the combination can be obtained as a matter of course, and other actions and effects that are obvious to a person skilled in the art from the description of this specification can be obtained.
[0112] In addition, the effects described in this specification are merely explanatory or exemplary and are not limiting. In other words, the technology according to the present disclosure may achieve other effects that are apparent to a person skilled in the art from the description of this specification in addition to or in place of the above effects.
[0113] Note that the following configuration examples also fall within the technical scope of the present disclosure. (1) A method for bonding substrates, comprising the steps of: a step of forming a laminated substrate by sequentially bonding the first substrate and the second substrate from the center toward the outer periphery while the center of the first substrate and the center of the second substrate are in contact with each other; measuring a welding speed in the welding from the center portion toward the outer periphery; and estimating a bonding strength of the joined laminated substrates from a relationship between the bonding speed and the bonding strength based on the measured bonding speed. (2) The joining method according to (1) above, wherein in the step of measuring the joining speed, the joining speed between two points in a radial direction between the central portion and the outer circumferential portion is measured. (3) The joining method according to (2) above, wherein in the step of measuring the joining speed, a joining speed between at least two points on the outer periphery side not including the center portion is measured. (4) The bonding method according to (3) above, wherein the two points in the step of measuring the bonding speed are provided in the same suction region that evacuates the first substrate. (5) The bonding method according to any one of (2) to (4), wherein in the step of measuring the bonding speed, a bonding speed between two points in a plurality of radial directions corresponding to different crystal orientations in the first substrate is measured. (6) measuring the amount of warping of the bonded laminated substrates; and estimating a bonding strength of the joined laminated substrates from a relationship between the combination of the joining speed and the amount of warping and the bonding strength based on the measured joining speed and the amount of warping. (7) A method for bonding substrates, comprising the steps of: a step of forming a laminated substrate by sequentially bonding the first substrate and the second substrate from the center toward the outer periphery while the center of the first substrate and the center of the second substrate are in contact with each other; measuring the amount of warping of the bonded laminated substrate; and estimating a bonding strength of the bonded laminated substrates from a relationship between the amount of warping and bonding strength based on the measured amount of warping. (8) The bonding method according to any one of (1) to (7), further comprising the step of determining a bonding state of the laminated substrate based on the estimated bonding strength of the laminated substrate. (9) The bonding method according to any one of (1) to (8), further comprising controlling bonding conditions for bonding the first substrate and the second substrate based on the estimated bonding strength of the laminated substrate. (10) before the step of bonding the first substrate and the second substrate, a step of modifying at least one of a surface of the first substrate and a surface of the second substrate by plasma of a processing gas; The bonding method according to any one of (1) to (9), further comprising controlling modification conditions for modifying at least one of the surfaces of the first substrate and the second substrate based on the estimated bonding strength of the laminated substrates. (11) The bonding method according to any one of (1) to (10), further comprising outputting information on the estimated bonding strength of the laminated substrate to a processing device that processes the bonded laminated substrate. (12) A bonding system for bonding substrates, comprising: a bonding device that bonds the first substrate and the second substrate in sequence from the center toward the outer periphery while the centers of the first substrate and the second substrate are in contact with each other to form a laminated substrate; a speed measuring unit for measuring a welding speed in the welding from the center portion to the outer periphery; and a control device that estimates a bonding strength of the bonded laminated substrates from a relationship between the bonding speed and the bonding strength based on the measured bonding speed. (13) The joining system according to (12), wherein the speed measuring unit measures the joining speed between two points in a radial direction between the center portion and the outer periphery. (14) The joining system according to (13), wherein the speed measuring unit measures the joining speed between at least two points on the outer periphery side not including the center portion. (15) A warpage measuring unit for measuring the amount of warpage of the bonded laminated substrates, The bonding system according to any one of (12) to (14), wherein the control device estimates a bonding strength of the bonded laminated substrates from a relationship between a combination of the bonding speed and the amount of warping and the bonding strength based on the measured bonding speed and amount of warping. (16) A bonding system for bonding substrates, comprising: a bonding device that bonds the first substrate and the second substrate in sequence from the center toward the outer periphery while the centers of the first substrate and the second substrate are in contact with each other to form a laminated substrate; a warpage measuring unit for measuring the amount of warpage of the bonded laminated substrate; and a control device that estimates a bonding strength of the bonded laminated substrates from a relationship between the amount of warping and bonding strength based on the measured amount of warping. (17) The bonding system according to any one of (12) to (16), wherein the control device determines a bonding state of the laminated substrate based on the estimated bonding strength of the laminated substrate. (18) The bonding system according to any one of (12) to (17), wherein the control device controls bonding conditions for bonding the first substrate and the second substrate based on the estimated bonding strength of the laminated substrate. (19) A modification device is provided for modifying at least one of a surface of the first substrate and a surface of the second substrate by plasma of a processing gas before the first substrate and the second substrate are bonded in the bonding device, The bonding system according to any one of (12) to (18), wherein the control device controls modification conditions for modifying at least one of the surface of the first substrate and the surface of the second substrate based on the estimated bonding strength of the laminated substrates. (20) The bonding system according to any one of (12) to (19), wherein the control device outputs information on the estimated bonding strength of the laminated substrates to a processing device that processes the bonded laminated substrates. [Explanation of symbols]
[0114] 1 Joining System 250a, 250b Sensor 41 Joining equipment 52 Warpage measuring device 70 Control device W U Upper wafer W L Lower wafer W T Polymerized Wafer
Claims
1. A method for bonding substrates, comprising the steps of: a step of forming a laminated substrate by sequentially bonding the first substrate and the second substrate from the center toward the outer periphery while the center of the first substrate and the center of the second substrate are in contact with each other; measuring a welding speed in the welding from the center portion toward the outer periphery; and estimating a bonding strength of the joined laminated substrates from a relationship between the bonding speed and the bonding strength based on the measured bonding speed.
2. The welding method according to claim 1 , wherein in the step of measuring the welding speed, the welding speed between two points in a radial direction between the central portion and the outer circumferential portion is measured.
3. The joining method according to claim 2 , wherein in the step of measuring the joining speed, the joining speed between at least two points on the outer circumferential portion side not including the central portion is measured.
4. The bonding method according to claim 3 , wherein the two points in the step of measuring the bonding speed are provided in a same suction region where the first substrate is evacuated.
5. The bonding method according to claim 2 , wherein in the step of measuring the bonding speed, the bonding speed is measured between two points in a plurality of radial directions corresponding to different crystal orientations in the first substrate.
6. measuring the amount of warping of the bonded laminated substrate; The bonding method according to claim 1 , further comprising a step of estimating a bonding strength of the bonded laminated substrates from a relationship between a combination of the bonding speed and the amount of warping and the bonding strength based on the measured bonding speed and amount of warping.
7. A method for bonding substrates, comprising the steps of: a step of forming a laminated substrate by sequentially bonding the first substrate and the second substrate from the center toward the outer periphery while the center of the first substrate and the center of the second substrate are in contact with each other; measuring the amount of warping of the bonded laminated substrate; and estimating a bonding strength of the bonded laminated substrates from a relationship between the amount of warping and bonding strength based on the measured amount of warping.
8. The bonding method according to any one of claims 1 to 7, further comprising the step of determining a bonding state of the laminated substrate based on the estimated bonding strength of the laminated substrate.
9. The bonding method according to any one of claims 1 to 7, further comprising controlling bonding conditions for bonding the first substrate and the second substrate together based on the estimated bonding strength of the laminated substrate.
10. a step of modifying at least one of a surface of the first substrate and a surface of the second substrate by plasma of a processing gas before the step of bonding the first substrate and the second substrate; The bonding method according to any one of claims 1 to 7, further comprising controlling modification conditions for modifying at least one of the surface of the first substrate and the surface of the second substrate based on the estimated bonding strength of the laminated substrate.
11. The bonding method according to any one of claims 1 to 7, further comprising the step of outputting information on the estimated bonding strength of the laminated substrate to a processing device that processes the bonded laminated substrate.
12. 1. A bonding system for bonding substrates together, comprising: a bonding device that bonds the first substrate and the second substrate in sequence from the center toward the outer periphery while the centers of the first substrate and the second substrate are in contact with each other to form a laminated substrate; a speed measuring unit for measuring a welding speed in the welding from the center portion to the outer periphery; and a control device that estimates a bonding strength of the bonded laminated substrates from a relationship between the bonding speed and the bonding strength based on the measured bonding speed.
13. The joining system according to claim 12 , wherein the speed measuring unit measures the joining speed between two points in a radial direction between the central portion and the outer circumferential portion.
14. The joining system according to claim 13 , wherein the speed measuring unit measures the joining speed between at least two points on the outer periphery side not including the center portion.
15. A warpage measuring unit is provided for measuring the amount of warpage of the bonded laminated substrate, The bonding system according to claim 12 , wherein the control device estimates a bonding strength of the bonded laminated substrates from a relationship between a combination of the bonding speed and the amount of warping and the bonding strength, based on the measured bonding speed and the amount of warping.
16. 1. A bonding system for bonding substrates together, comprising: a bonding device that bonds the first substrate and the second substrate in sequence from the center toward the outer periphery while the centers of the first substrate and the second substrate are in contact with each other to form a laminated substrate; a warpage measuring unit for measuring the amount of warpage of the bonded laminated substrate; and a control device that estimates a bonding strength of the bonded laminated substrates from a relationship between the amount of warping and bonding strength based on the measured amount of warping.
17. The bonding system according to any one of claims 12 to 16, wherein the control device determines a bonding state of the laminated substrate based on the estimated bonding strength of the laminated substrate.
18. The bonding system according to any one of claims 12 to 16, wherein the control device controls bonding conditions for bonding the first substrate and the second substrate based on the estimated bonding strength of the laminated substrate.
19. a modifying device for modifying at least one of a surface of the first substrate and a surface of the second substrate by plasma of a processing gas before the first substrate and the second substrate are bonded in the bonding device; The bonding system according to any one of claims 12 to 16, wherein the control device controls modification conditions when modifying at least one of the surface of the first substrate and the surface of the second substrate, based on the estimated bonding strength of the laminated substrate.
20. The bonding system according to any one of claims 12 to 16, wherein the control device outputs information on the estimated bonding strength of the laminated substrates to a processing device that processes the bonded laminated substrates.
Citation Information
Patent Citations
Joint system
JP2017073455A