Phosphor element, wavelength converter, illumination device, and projector
The phosphor element with a balanced oxide layer and AlN matrix phase enhances thermal conductivity and fluorescence extraction, addressing efficiency issues in conventional ceramic composites for projectors.
Patent Information
- Application Number
- JP2023085215
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional ceramic composites used in wavelength conversion members for projectors face challenges in improving fluorescence extraction efficiency due to insufficient thermal conductivity and fluorescence emission efficiency.
A phosphor element composed of a phosphor phase with a garnet structure containing Ce, a matrix phase of AlN with higher refractive index, and an oxide layer of MgAl2O4 between the phases, optimized with a volume ratio of 0.1-0.9% to balance grain growth, enhancing thermal conductivity and fluorescence extraction.
The solution results in a phosphor element with improved thermal conductivity and fluorescence extraction efficiency, enabling brighter and more efficient fluorescence generation, suitable for use in projectors.
Smart Images

Figure 2024168492000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a phosphor element, a wavelength conversion device, an illumination device, and a projector. [Background technology]
[0002] Conventionally, ceramic composites have been used as wavelength conversion members for use in light sources for projectors. The following Patent Document 1 discloses a ceramic composite made of inorganic materials having a matrix phase made of translucent ceramics such as Al2O3, MgAl2O4, and MgO, and a phosphor phase made of YAG containing Ce. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-062459 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the ceramic composite disclosed in Patent Document 1, although the thermal conductivity is improved by mixing and sintering a highly thermally conductive filler, it is difficult to sufficiently improve the fluorescence extraction efficiency. [Means for solving the problem]
[0005] In order to solve the above problems, according to one aspect of the present invention, a garnet-structured A3B5O 12A phosphor element is provided, which has a phosphor body including a phosphor phase composed of A and Ce, a matrix phase having a refractive index higher than that of the phosphor phase, and an oxide layer provided between the phosphor phase and the matrix phase, the oxide layer being made of a composite oxide of a metal contained in the phosphor phase and a metal contained in a sintering aid, and the content of the oxide layer is 0.1 vol% or more and 0.9 vol% or less in terms of volume ratio to the phosphor body, where A is at least one selected from the group consisting of Lu, Gd, Tb, Ga and Y, and B is Al.
[0006] According to another aspect of the present invention, there is provided a wavelength conversion device comprising: a substrate; a phosphor element of the above aspect that is provided on the substrate and converts incident excitation light into fluorescence; and a reflective layer that is provided on the opposite side to the light incident side of the phosphor element and reflects the excitation light and the fluorescence.
[0007] According to another aspect of the present invention, there is provided a wavelength conversion device comprising: a substrate; a phosphor element of the above aspect that is provided on the substrate and converts incident excitation light into fluorescence; and an optical layer that is provided on the light incident side of the phosphor element and transmits the excitation light and reflects the fluorescence.
[0008] According to another aspect of the present invention, there is provided an illumination device including a light source that emits excitation light, and the wavelength conversion device of the above aspect onto which the excitation light is incident.
[0009] According to another aspect of the present invention, there is provided a projector comprising an illumination device according to the above aspect, an optical modulator that modulates light emitted from the illumination device, and a projection optical device that projects the light modulated by the optical modulator. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic configuration diagram showing a projector according to a first embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing a configuration of a lighting device. [Diagram 3]FIG. 1 is a cross-sectional view showing a configuration of a wavelength conversion device. [Figure 4] This is an SEM image of a phosphor element. [Diagram 5] FIG. 11 is a schematic configuration diagram showing an illumination device according to a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Note that the drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand, and the dimensional ratios of each component may not necessarily be the same as in reality.
[0012] (First embodiment) Hereinafter, one embodiment of the present invention will be described. FIG. 1 is a schematic configuration diagram showing a projector according to a first embodiment. 1, the projector 1 of this embodiment is a projection type image display device that displays an image on a screen SCR. The projector 1 includes an illumination device 2, a color separation optical system 3, a light modulation device 4R, a light modulation device 4G, a light modulation device 4B, a synthesis optical system 5, and a projection optical device 6.
[0013] The illumination device 2 emits white illumination light WL toward the color separation optical system 3. The configuration of the illumination device 2 will be described in detail later.
[0014] The color separation optical system 3 separates the illumination light WL emitted from the illumination device 2 into red light LR, green light LG, and blue light LB. The color separation optical system 3 includes a first dichroic mirror 7a, a second dichroic mirror 7b, a first reflecting mirror 8a, a second reflecting mirror 8b, a third reflecting mirror 8c, a first relay lens 9a, and a second relay lens 9b.
[0015] The first dichroic mirror 7a separates the illumination light WL from the illumination device 2 into red light LR and light containing green light LG and blue light LB. The first dichroic mirror 7a transmits the red light LR and reflects the light containing green light LG and blue light LB. On the other hand, the second dichroic mirror 7b reflects the green light LG and transmits the blue light LB. In this way, the second dichroic mirror 7b separates the light containing green light LG and blue light LB into green light LG and blue light LB.
[0016] The first reflecting mirror 8a is disposed in the optical path of the red light LR and reflects the red light LR transmitted through the first dichroic mirror 7a toward the optical modulation device 4R. On the other hand, the second reflecting mirror 8b and the third reflecting mirror 8c are disposed in the optical path of the blue light LB and guide the blue light LB transmitted through the second dichroic mirror 7b to the optical modulation device 4B. The green light LG is reflected from the second dichroic mirror 7b toward the optical modulation device 4G.
[0017] The first relay lens 9a is disposed between the second dichroic mirror 7b and the second reflecting mirror 8b in the optical path of the blue light LB. The second relay lens 9b is disposed between the second reflecting mirror 8b and the third reflecting mirror 8c in the optical path of the blue light LB. The first relay lens 9a and the second relay lens 9b compensate for the optical loss of the blue light LB caused by the optical path length of the blue light LB being longer than the optical path lengths of the red light LR and the green light LG.
[0018] The light modulation device 4R modulates the red light LR according to image information to form image light corresponding to the red light LR. The light modulation device 4G modulates the green light LG according to image information to form image light corresponding to the green light LG. The light modulation device 4B modulates the blue light LB according to image information to form image light corresponding to the blue light LB.
[0019] For example, a transmissive liquid crystal panel is used for each of the light modulation device 4R, the light modulation device 4G, and the light modulation device 4B. Furthermore, a polarizing plate (not shown) is disposed on each of the incident side and the exit side of the liquid crystal panel.
[0020] A field lens 10R is disposed on the incident side of the optical modulation device 4R. The field lens 10R collimates the red light LR incident on the optical modulation device 4R. A field lens 10G is disposed on the incident side of the optical modulation device 4G. The field lens 10G collimates the green light LG incident on the optical modulation device 4G. A field lens 10B is disposed on the incident side of the optical modulation device 4B. The field lens 10B collimates the blue light LB incident on the optical modulation device 4B.
[0021] The image light emitted from the light modulation device 4R, the light modulation device 4G, and the light modulation device 4B is incident on the combining optical system 5. The combining optical system 5 combines the image light corresponding to the red light LR, the green light LG, and the blue light LB, respectively, and emits the combined image light toward the projection optical device 6. The combining optical system 5 uses, for example, a cross dichroic prism.
[0022] The projection optical device 6 has a plurality of projection lenses. The projection optical device 6 enlarges and projects the image light combined by the combining optical system 5 onto the screen SCR. As a result, an enlarged image is displayed on the screen SCR.
[0023] The configuration of the lighting device 2 will be described below. FIG. 2 is a schematic diagram showing the configuration of an illumination device 2 according to the present embodiment. As shown in FIG. 2, the illumination device 2 includes a first light source 40, a collimating optical system 41, a dichroic mirror 42, a first focusing optical system 43, a wavelength conversion device 50, a second light source 44, a second focusing optical system 45, a diffusion plate 46, and a collimating optical system 47.
[0024] The first light source 40 is composed of a plurality of semiconductor lasers 40a that emit blue excitation light E made of laser light. The emission intensity of the excitation light E has a peak of, for example, 445 nm. The plurality of semiconductor lasers 40a are arranged in an array in a plane perpendicular to the optical axis ax of the first light source 40. Note that the semiconductor lasers 40a may be semiconductor lasers that emit blue light of a wavelength other than 445 nm, for example, 455 nm or 460 nm. The optical axis ax of the first light source 40 is perpendicular to the illumination optical axis 100ax of the illumination device 2. The first light source 40 of the present embodiment corresponds to the "light source" in the claims.
[0025] The collimating optical system 41 includes a first lens 41a and a second lens 41b. The collimating optical system 41 approximately collimates the light emitted from the first light source 40. Each of the first lens 41a and the second lens 41b is formed of a convex lens.
[0026] The dichroic mirror 42 is disposed in the optical path from the collimating optical system 41 to the first collecting optical system 43 in a direction intersecting at an angle of 45° with respect to both the optical axis ax of the first light source 40 and the illumination optical axis 100ax. The dichroic mirror 42 reflects the blue light component and transmits the red light component and the green light component. Thus, the dichroic mirror 42 reflects the excitation light E and the blue light B and transmits the yellow fluorescence Y.
[0027] The first focusing optical system 43 focuses the excitation light E transmitted through the dichroic mirror 42 and makes it incident on the wavelength conversion device 50, while approximately collimating the fluorescence Y emitted from the wavelength conversion device 50. The first focusing optical system 43 includes a first lens 43a and a second lens 43b. Each of the first lens 43a and the second lens 43b is formed by a convex lens.
[0028] The second light source 44 is composed of a semiconductor laser having the same wavelength band as the first light source 40. The second light source 44 may be composed of one semiconductor laser, or may be composed of multiple semiconductor lasers. The second light source 44 may also be composed of a semiconductor laser having a different wavelength band from the semiconductor laser of the first light source 40.
[0029] The second light collecting optical system 45 includes a first lens 45a and a second lens 45b. The second light collecting optical system 45 collects the blue light B emitted from the second light source 44 on or near the diffusion surface of the diffusion plate 46. Each of the first lens 45a and the second lens 45b is formed of a convex lens.
[0030] The diffusion plate 46 diffuses the blue light B emitted from the second light source 44, and generates blue light B having a light distribution close to the light distribution of the fluorescence Y emitted from the wavelength conversion device 50. As the diffusion plate 46, for example, ground glass made of optical glass can be used.
[0031] The collimating optical system 47 includes a first lens 47a and a second lens 47b. The collimating optical system 47 approximately collimates the light emitted from the diffusion plate 46. Each of the first lens 47a and the second lens 47b is formed of a convex lens.
[0032] The blue light B emitted from the second light source 44 is reflected by the dichroic mirror 42, emitted from the wavelength conversion device 50, and combined with the fluorescence Y transmitted through the dichroic mirror 42 to generate white illumination light WL. The illumination light WL is incident on the uniform illumination optical system 80.
[0033] The uniform illumination optical system 80 includes a first lens array 81, a second lens array 82, a polarization conversion element 83, and a superimposing lens 84.
[0034] The first lens array 81 has a plurality of first lenses 81a for splitting the illumination light WL from the illumination device 2 into a plurality of partial light beams. The plurality of first lenses 81a are arranged in a matrix in a plane perpendicular to the illumination optical axis 100ax.
[0035] The second lens array 82 has a plurality of second lenses 82a corresponding to the plurality of first lenses 81a of the first lens array 81. The plurality of second lenses 82a are arranged in a matrix in a plane perpendicular to the illumination optical axis 100ax.
[0036] The second lens array 82, together with the superimposing lens 84, forms images of the first lenses 81a of the first lens array 81 near the image forming areas of the light modulation device 4R, the light modulation device 4G, and the light modulation device 4B, respectively.
[0037] The polarization conversion element 83 converts the light emitted from the second lens array 82 into one type of linearly polarized light. The polarization conversion element 83 includes, for example, a polarization separation film and a phase difference plate (not shown).
[0038] The superimposing lens 84 collects the partial light beams emitted from the polarization conversion element 83 and superimposes them near the image forming areas of the light modulation device 4R, the light modulation device 4G, and the light modulation device 4B.
[0039] Next, the configuration of the wavelength converter 50 will be described. Fig. 3 is a cross-sectional view showing the configuration of the wavelength conversion device 50. Fig. 3 corresponds to a cross-sectional view of the wavelength conversion device 50 cut along a plane including the illumination optical axis 100ax in Fig. 2.
[0040] 3, the wavelength converter 50 includes a substrate 51, a phosphor element 52, a bonding layer 53, and a reflective layer 54. The wavelength converter 50 of the present embodiment is configured as a fixed-type wavelength converter in which the incident position of the excitation light E with respect to the phosphor element 52 does not change over time.
[0041] The substrate 51 supports the reflective layer 54 and the phosphor elements 52 via a bonding layer 53. The substrate 51 is made of a metal material having high thermal conductivity, such as aluminum or copper. The bonding layer 53 is made of a bonding material having high thermal conductivity, such as nano silver paste. The bonding layer 53 bonds a first surface 51a, which is the surface of the substrate 51, to the phosphor elements 52.
[0042] The phosphor element 52 has a back surface 52a facing the substrate 51 and a front surface 52b opposite to the back surface 52a. The phosphor element 52 emits fluorescence Y from the front surface 52b, which is wavelength-converted excitation light E incident from the front surface 52b.
[0043] The reflective layer 54 is provided facing the back surface 52a of the phosphor element 52 with the bonding layer 53 interposed therebetween. That is, the reflective layer 54 is provided between the substrate 51 and the back surface 52a of the phosphor element 52. The reflective layer 54 is made of a metal film such as silver having high light reflectance, a dielectric multilayer film, or a combination of these films. The reflective layer 54 reflects the fluorescence Y traveling toward the side opposite to the light incident side (back surface 52a side) in the phosphor element 52 toward the light incident side (surface 52b side). The reflective layer 54 may reflect a part of the excitation light E toward the light incident side (surface 52b side), and the excitation light E reflected by the reflective layer 54 is used to excite the fluorescence Y. The wavelength converter 50 of this embodiment functions as a reflection-type wavelength converter that emits fluorescence Y from the surface 52b of the phosphor element 52 on which the excitation light E is incident.
[0044] It is generally known that the luminous efficiency of fluorescent light decreases as the temperature of a phosphor element increases, and improving the heat dissipation is an effective way to increase the fluorescent light conversion efficiency of the phosphor element. The inventors focused on increasing the thermal conductivity of phosphor elements by mixing and sintering a YAG:Ce phosphor, which is widely used as a phosphor element, with a highly thermally conductive filler material made of AlN. Generally, a sintered body of a phosphor element containing a phosphor phase made of YAG:Ce and a matrix phase made of AlN is formed by mixing and sintering the raw material powders Al2O3 (alumina), Y2O3 (yttria), and CeO2 (cerium oxide) with AlN powder as a binder material.
[0045] However, if YAG:Ce and AlN are simply sintered, the grain growth of AlN during sintering is faster than that of YAG:Ce, so the YAG:Ce particles cannot grow to a size that can emit a sufficient amount of light, and the fluorescence emission efficiency decreases, resulting in a small amount of extracted fluorescent light. In other words, if YAG:Ce and AlN are simply sintered, there is a problem that the internal quantum yield decreases and the amount of extracted fluorescent light decreases. Note that the internal quantum yield means the value (unit: %) obtained by dividing the amount of fluorescent light emitted by the phosphor element by the amount of excitation light absorbed by the phosphor element.
[0046] As a result of intensive research, the inventors have found that by using a specific sintering aid when producing a fluorescent light-emitting element made of a sintered body containing a crystal phase made of YAG:Ce and a matrix phase made of AlN, a specific amount of oxide layer is produced at the boundary between the phosphor phase and the matrix phase, thereby making it possible to produce a phosphor element with improved thermal conductivity and internal quantum yield (extraction amount) of fluorescence.The inventors have then completed the configuration of the phosphor element 52 of this embodiment.
[0047] Specifically, the phosphor element 52 of this embodiment has a phosphor body 520 including a phosphor phase 521 , a matrix phase 522 , and an oxide layer 523 . In the phosphor element 52, the phosphor phase 521 is ABO having a garnet structure. 12The phosphor phase 521 of this embodiment contains phosphor particles composed of Y (yttrium) and B (aluminum). That is, the phosphor phase 521 of this embodiment contains yttrium aluminum garnet (YAG(Y3Al5O4)) to which cerium (Ce) is added as an activator. 12 ):Ce) phosphor particles.
[0048] The matrix phase 522 is a translucent ceramic that functions as a binder that binds together the multiple phosphor particles that constitute the phosphor phase 521 and transmits the fluorescence emitted by the phosphor phase 521. The matrix phase 522 in this embodiment is made of AlN (aluminum nitride). The matrix phase 522 has a refractive index (2.2) higher than the refractive index (1.8) of YAG:Ce that constitutes the phosphor phase 521.
[0049] The thermal conductivity of AlN constituting the matrix phase 522 is approximately 285 W / m·K, and the thermal conductivity of YAG:Ce constituting the phosphor phase 521 is approximately 9 W / m·K. In other words, the matrix phase 522 has a thermal conductivity that is sufficiently higher than that of the phosphor phase 521.
[0050] Moreover, the thermal conductivity of the matrix phase 522 of this embodiment is sufficiently higher than the thermal conductivity (approximately 30 W / m K) of Al2O3 (alumina) that is generally used as the matrix phase of ceramic phosphors. Therefore, the phosphor element 52 of this embodiment has superior thermal conductivity compared to conventional phosphor elements that use Al2O3 as the matrix phase, and therefore has excellent heat dissipation properties.
[0051] The phosphor element 52 of this embodiment is manufactured by adding a predetermined sintering aid when sintering YAG:Ce and AlN, and mixing and sintering the YAG raw material powders Al2O3, Y2O3, and CeO2 with AlN powder. Examples of the predetermined sintering aid include MgO (magnesium oxide) and CaO (calcium oxide), and in the phosphor element 52 of this embodiment, MgO is used as the sintering aid.
[0052] In the manufacturing process of the phosphor element 52 of this embodiment, MgO is added as a sintering aid. MgO added as a sintering aid can suppress the grain growth rate of AlN constituting the matrix phase 522, thereby relatively increasing the grain growth rate of YAG:Ce constituting the phosphor phase 521. In other words, by adjusting MgO to optimize the grain growth rate difference between the matrix phase 522 and the phosphor phase 521, the YAG:Ce particles constituting the phosphor phase 521 can be grown to a grain size that allows sufficient fluorescent emission. Therefore, the phosphor element 52 of this embodiment has excellent thermal conductivity and can increase the efficiency of extracting the fluorescent Y (internal quantum yield).
[0053] MgO added as a sintering aid during sintering of the phosphor element 52 of this embodiment generates an oxide layer 523 between the phosphor phase 521 and the matrix phase 522. More specifically, the oxide layer 523 of this embodiment is provided at the boundary between the phosphor phase 521 and the matrix phase 522. The oxide layer 523 is made of a composite oxide of a metal contained in the phosphor phase 521 and a metal contained in the sintering aid. In other words, the oxide layer 523 is a by-product generated from the sintering aid. Specifically, the oxide layer 523 of this embodiment is made of MgAl2O4. Note that in FIG. 3, the oxide layer 523 is generated at all the boundaries between the phosphor phase 521 and the matrix phase 522, but it is sufficient that the oxide layer 523 is generated at at least some of the boundaries.
[0054] The content of the oxide layer 523 is 0.1 vol% or more and 0.9 vol% or less in terms of volume ratio to the phosphor body 520. According to the phosphor element 52 having the content of the oxide layer 523 of 0.1 vol% or more and 0.9 vol% or less, a suitable amount of MgO that enables the grain growth rate difference between the matrix phase 522 and the phosphor phase 521 to be appropriately adjusted is added, thereby achieving high thermal conductivity and internal quantum yield.
[0055] The phosphor element 52 of this embodiment includes the oxide layer 523, and thus can scatter light at the interface between the oxide layer 523 and the phosphor phase 521, or at the interface between the oxide layer 523 and the matrix phase 522. Therefore, the phosphor element 52 can scatter light well inside the element, and can increase the extraction efficiency (internal quantum yield) of the fluorescence Y.
[0056] Fig. 4 is a diagram showing a configuration of a main part of the phosphor element 52 of this embodiment. Fig. 4 is an image of the phosphor element 52 captured using a SEM (scanning electron microscope). As shown in FIG. 4, the phosphor body 520 of the phosphor element 52 of this embodiment has a phosphor phase 521 and a matrix phase 522 that are evenly distributed. In other words, it can be confirmed from the image of FIG. 4 that the phosphor element 52 of this embodiment is a ceramic sintered body having a dense crystal structure. Note that the oxide layer 523 generated at the boundary between the phosphor phase 521 and the matrix phase 522 is not shown in the image of FIG. 4, so the oxide layer 523 is shown virtually in FIG. 4. For this reason, the oxide layer 523 shown in FIG. 4 is different from the actual state. Note that the presence or absence of the oxide layer 523 can be determined by using, for example, X-ray diffraction (XRD).
[0057] As described above, the phosphor element 52 of the present embodiment is a YAG (YAlO 12 The phosphor body 520 includes a phosphor phase 521 made of Ce, a matrix phase 522 made of AlN having a refractive index higher than that of the phosphor phase 521, and an oxide layer 523 provided between the phosphor phase 521 and the matrix phase 522. The oxide layer 523 is made of a composite oxide of a metal contained in the phosphor phase 521 and a metal contained in MgO, which is a sintering aid. The content of the oxide layer 523 is 0.1 vol% or more and 0.9 vol% or less in terms of volume ratio to the phosphor body 520.
[0058] According to the phosphor element 52 of this embodiment, the content of the oxide layer 523 contained in the phosphor body 520 is 0.1 vol% or more and 0.9 vol% or less, so that the phosphor element 52 is sintered with an appropriate amount of MgO added as a sintering aid. Therefore, by adjusting the difference in grain growth rate between the matrix phase 522 and the phosphor phase 521, the phases can grow in a well-balanced manner. Therefore, the YAG:Ce particles constituting the phosphor phase 521 grow to a grain size that allows sufficient fluorescent emission, so that the phosphor element 52 of this embodiment has excellent thermal conductivity and can improve the extraction efficiency (internal quantum yield) of the fluorescent Y.
[0059] The phosphor element 52 of this embodiment has a matrix phase 522 made of AlN with high thermal conductivity, and therefore can efficiently release heat accompanying fluorescent emission, thereby suppressing a decrease in fluorescence conversion efficiency accompanying a rise in temperature. As a result, the excitation light E is efficiently absorbed by the phosphor phase 521, increasing the luminous efficiency of the fluorescence Y, and a bright fluorescence Y can be generated.
[0060] According to the phosphor element 52 of this embodiment, by increasing the internal quantum yield of the fluorescence Y to 85% or more, it is possible to emit fluorescence Y from the phosphor element 52 with a brightness that does not cause any problems in practical use as illumination light for a projector.
[0061] The wavelength conversion device 50 of this embodiment comprises a substrate 51, a phosphor element 52 provided on the substrate 51 for converting incident excitation light E into fluorescence, and a reflective layer 54 provided on the side opposite the light incident side of the phosphor element 52. According to the wavelength converter 50 of the present embodiment, a reflective wavelength converter that efficiently extracts bright fluorescence Y can be provided.
[0062] The illumination device 2 of this embodiment includes a first light source 40 that emits excitation light E, and a wavelength conversion device 50 into which the excitation light E is incident. According to the lighting device 2 of the present embodiment, it is possible to provide a lighting device that has excellent wavelength conversion efficiency and emits bright illumination light WL.
[0063] The projector 1 of this embodiment includes an illumination device 2, light modulation devices 4R, 4G, and 4B that modulate the light emitted from the illumination device 2, and a projection optical device 6 that projects the light modulated by the light modulation devices 4R, 4G, and 4B.
[0064] According to the projector 1 of the present embodiment, it is possible to provide a highly efficient projector with excellent display quality.
[0065] Second embodiment The projector according to the second embodiment will be described below. The basic configuration of the projector of the second embodiment is similar to that of the first embodiment, but the configuration of the illumination device is different from that of the first embodiment, so the configuration of the illumination device will be described below.
[0066] FIG. 5 is a schematic configuration diagram showing an illumination device 2A according to the second embodiment. In FIG. 5, components common to those in the above embodiment are denoted by the same reference numerals, and description thereof will be omitted.
[0067] As shown in FIG. 5, the illumination device 2A includes an excitation light source unit 10, an afocal optical system 11, a homogenizer optical system 12, a focusing optical system 13, a wavelength conversion device 250, a pickup optical system 30, and a uniform illumination optical system 80.
[0068] The excitation light source unit 10 is composed of a plurality of semiconductor lasers 10a that emit blue excitation light E composed of laser light, and a plurality of collimator lenses 10b. The plurality of semiconductor lasers 10a are arranged in an array in a plane perpendicular to the illumination optical axis 100ax. The collimator lenses 10b are arranged in an array in a plane perpendicular to the illumination optical axis 100ax so as to correspond to each semiconductor laser 10a. The collimator lenses 10b convert the excitation light E emitted from the semiconductor lasers 10a corresponding to the collimator lenses 10b into parallel light. The excitation light source unit 10 of this embodiment corresponds to the "light source" in the claims.
[0069] The afocal optical system 11 includes, for example, a convex lens 11a and a concave lens 11b. The afocal optical system 11 reduces the beam diameter of the excitation light E emitted from the excitation light source unit 10 and consisting of a parallel beam.
[0070] The homogenizer optical system 12 includes, for example, a first multi-lens array 12a and a second multi-lens array 12b. The homogenizer optical system 12 makes the light intensity distribution of the excitation light uniform on the phosphor element 52 of the wavelength conversion device 250, that is, a so-called top hat distribution. The homogenizer optical system 12, together with the focusing optical system 13, superimposes a plurality of small light beams emitted from a plurality of lenses of the first multi-lens array 12a and the second multi-lens array 12b on the phosphor element 52 of the wavelength conversion device 250. This makes the light intensity distribution of the excitation light E irradiated on the phosphor element 52 uniform.
[0071] The focusing optical system 13 includes, for example, a first lens 13a and a second lens 13b. In this embodiment, the first lens 13a and the second lens 13b are each formed of a convex lens. The focusing optical system 13 is disposed in the optical path from the homogenizer optical system 12 to the wavelength conversion device 250, and focuses the excitation light E to make it incident on the phosphor element 52 of the wavelength conversion device 250.
[0072] The wavelength converter 250 of this embodiment includes a substrate 251, a phosphor element 52, a bonding layer 253, and an optical layer 254. The wavelength converter 250 of this embodiment is configured as a fixed type wavelength converter in which the incident position of the excitation light E with respect to the phosphor element 52 does not change over time.
[0073] The substrate 251 supports the optical layer 254 and the phosphor elements 52 via a bonding layer 253. The substrate 251 is made of a light-transmitting material such as glass or plastic. The bonding layer 253 in this embodiment is made of a light-transmitting material such as epoxy. The bonding layer 253 bonds a first surface 251a, which is the surface of the substrate 251, to the phosphor elements 52.
[0074] In the phosphor element 52 of this embodiment, excitation light E is incident on the back surface 52a facing the substrate 251, and fluorescence Y is emitted from the front surface 52b. In the wavelength conversion device 250 of this embodiment, the phosphor element 52 transmits and emits not only the fluorescence Y, but also a portion of the excitation light E1 that has not been wavelength-converted. This causes white illumination light WL1 to be emitted from the phosphor element 52.
[0075] The optical layer 254 is provided on a rear surface 52a, which is the light incident side, of the phosphor element 52. The optical layer 254 is composed of a dichroic mirror that transmits the excitation light E and reflects the fluorescence Y.
[0076] The wavelength converter 250 of this embodiment functions as a transmissive wavelength converter that emits illumination light WL1 containing fluorescence Y from a front surface 52b opposite to a back surface 52a of the phosphor element 52 on which excitation light E is incident.
[0077] The pickup optical system 30 includes, for example, a first collimating lens 31 and a second collimating lens 32. The pickup optical system 30 is a collimating optical system that approximately collimates the light emitted from the phosphor element 52 of the wavelength conversion device 250. The first collimating lens 31 and the second collimating lens 32 are each composed of a convex lens. The light collimated by the pickup optical system 30 enters the uniform illumination optical system 80.
[0078] (Effects of the second embodiment) According to this embodiment, by using the phosphor element 52 capable of increasing the amount of extracted fluorescence Y, it is possible to realize a transmissive wavelength conversion device 250 that generates bright fluorescence Y. Also, by providing the illumination device 2A of this embodiment with the transmissive wavelength conversion device 250, it is possible to obtain the same effect as in the first embodiment, that is, excellent wavelength conversion efficiency and the ability to emit bright illumination light WL1.
[0079] The technical scope of the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the spirit of the present invention. The specific descriptions of the shape, number, arrangement, material, manufacturing method, etc. of each component of the phosphor element, wavelength conversion device, lighting device, and projector shown in the above embodiments are not limited to the above embodiments and can be modified as appropriate.
[0080] In the above embodiment, YAG containing Ce is used as the phosphor phase 521. 12 , Tb3Al5O 12 , Ga3Al5O 12 , Gd3Al5O 12 The present invention is also applicable to the case where a phosphor phase containing Ce in at least one of the following structures is used. 12 In addition to Y (yttrium), A in Ce) can also be replaced with Lu (lutetium), Gd (gadolinium), Tb (terbium), or Ga (gallium), which has the same luminescence characteristics as Y, and therefore the present invention is also applicable when A is replaced with any of these.
[0081] In the above embodiment, AlN is used as the matrix phase 522, but SiC or BN may also be used.
[0082] In the above embodiment, MgO is used as the sintering aid, but CaO may be used as the sintering aid instead of MgO. When CaO is used as the sintering aid, the oxide layer made of a composite oxide of a metal contained in the phosphor phase and a metal contained in the sintering aid is made of CaAl2O4.
[0083] The following is a summary of this disclosure. (Appendix 1) A3B5O with garnet structure 12 A phosphor phase composed of Ce; a matrix phase having a refractive index higher than that of the phosphor phase; an oxide layer provided between the phosphor phase and the matrix phase; the oxide layer is made of a composite oxide of a metal contained in the phosphor phase and a metal contained in a sintering aid, The content of the oxide layer is 0.1 vol% or more and 0.9 vol% or less in terms of volume ratio to the phosphor body. A phosphor element characterized by: Here, A is at least one selected from the group consisting of Lu, Gd, Tb, Ga and Y, and B is Al.
[0084] According to the phosphor element of this configuration, the content of the oxide layer in the phosphor body is 0.1 vol% or more and 0.9 vol% or less, so that the phosphor element is sintered with an appropriate amount of sintering aid added. Therefore, the difference in grain growth rate between the matrix phase and the phosphor phase is adjusted, and each phase can grow in a well-balanced manner. In addition, the phosphor phase grows to a grain size that allows sufficient fluorescent emission, so that the phosphor element has excellent thermal conductivity and can improve the efficiency of extracting the fluorescent light. Therefore, a phosphor element having this configuration can efficiently generate bright fluorescent light.
[0085] (Appendix 2) A is Y, 2. A phosphor element according to claim 1.
[0086] According to this configuration, YAG (Y3Al5O 12 ): A phosphor element that efficiently generates bright fluorescence containing a phosphor phase composed of Ce can be realized.
[0087] (Appendix 3) The matrix phase is AlN. 3. The phosphor element according to claim 1 or 2,
[0088] According to this configuration, since the matrix phase is made of AlN, which has high thermal conductivity, the heat generated by the fluorescent light emission can be efficiently released, thereby suppressing the decrease in the fluorescent light conversion efficiency caused by the temperature rise.
[0089] (Appendix 4) The oxide layer is MgAl2O4. 4. The phosphor element according to claim 1, wherein the phosphor element is a fluorine-containing compound.
[0090] According to this configuration, since the phosphor body contains a predetermined amount of MgAl2O4 as the oxide layer, when MgO is used as a sintering aid, a fluorescent light emitting device that efficiently generates bright fluorescent light can be realized.
[0091] (Appendix 5) The oxide layer is CaAl2O4. 4. The phosphor element according to claim 1, wherein the phosphor element is a fluorine-containing compound.
[0092] According to this configuration, since the phosphor body contains a predetermined amount of CaAl2O4 as the oxide layer, when CaO is used as a sintering aid, a fluorescent light emitting device that efficiently generates bright fluorescent light can be realized.
[0093] (Appendix 6) A substrate; A phosphor element according to any one of claims 1 to 5, which is provided on the substrate and converts incident excitation light into fluorescent light; A reflective layer is provided on the opposite side to the light incident side of the phosphor element. A wavelength conversion device characterized by:
[0094] According to the wavelength converter having this configuration, a reflective wavelength converter that efficiently extracts bright fluorescent light Y can be provided.
[0095] (Appendix 7) A substrate; A phosphor element according to any one of claims 1 to 5, which is provided on the substrate and converts incident excitation light into fluorescent light; an optical layer provided on the light incident side of the phosphor element, the optical layer transmitting the excitation light and reflecting the fluorescence; A wavelength conversion device characterized by:
[0096] According to the wavelength converter having this configuration, it is possible to provide a transmission type wavelength converter that efficiently extracts bright fluorescent light.
[0097] (Appendix 8) A light source that emits the excitation light; and a wavelength conversion device according to claim 6 or 7, into which the excitation light is incident. A lighting device characterized by:
[0098] According to the illumination device having this configuration, it is possible to provide an illumination device that has excellent wavelength conversion efficiency and emits bright illumination light.
[0099] (Appendix 9) A lighting device according to claim 8; a light modulation device that modulates the light emitted from the illumination device; a projection optical device that projects the light modulated by the light modulation device. A projector characterized by:
[0100] According to a projector having this configuration, a highly efficient projector with excellent display quality can be provided. EXAMPLES
[0101] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0102] Example 1 In Example 1, a phosphor element was fabricated by sintering YAG:Ce and AlN together with 0.25 wt % MgO as a sintering aid, and the oxide layer had a MgAl2O4 content of 0.10%.
[0103] Example 2 In Example 2, a phosphor element was produced by sintering YAG:Ce and AlN together, containing 0.50 wt % MgO as a sintering aid, and setting the content of MgAl2O4, which is the oxide layer, to 0.10%.
[0104] Example 3 In Example 3, a phosphor element was produced in which 0.75 wt % of MgO was contained as a sintering aid, and YAG:Ce and AlN were sintered to produce an oxide layer having an MgAl2O4 content of 0.15%.
[0105] Example 4 In Example 4, a phosphor element was fabricated by sintering YAG:Ce and AlN together with 1.00 wt % MgO as a sintering aid, with the oxide layer having an MgAl2O4 content of 0.40%.
[0106] Example 5 In Example 5, a phosphor element was produced by sintering YAG:Ce and AlN together, containing 1.50 wt % MgO as a sintering aid, and setting the content of MgAl2O4, which is the oxide layer, to 0.90%.
[0107] Comparative Example 1 Comparative Example 1 was a phosphor element produced by sintering YAG:Ce and AlN without containing MgO (content 0 wt %) as a sintering aid.
[0108] Comparative Example 2 Comparative Example 2 was a phosphor element produced by sintering YAG:Ce and AlN together with 0.10 wt % MgO as a sintering aid, with the oxide layer having an MgAl2O4 content of 0.05%.
[0109] Comparative Example 3 Comparative Example 3 was a phosphor element produced by sintering YAG:Ce and AlN together, containing 2.00 wt % MgO as a sintering aid, and having an oxide layer with an MgAl2O4 content of 1.30%.
[0110] Comparative Example 4 Comparative Example 4 was a phosphor element produced by sintering YAG:Ce and AlN together with 5.00 wt % MgO as a sintering aid, with the oxide layer having an MgAl2O4 content of 3.005%.
[0111] (Evaluation of each Example and Comparative Example) For each of the above-mentioned examples and comparative examples, the thermal conductivity (unit: W / m K) and internal quantum yield (unit: %) were confirmed, and phosphor elements with high internal quantum yield and thermal conductivity were determined to have high light utilization efficiency. The results are shown in Table 1. The content of MgAl2O4, which is the oxide layer, was measured by X-ray diffraction (XRD). The thermal conductivity is a value based on the measurement results at room temperature.
[0112] In Table 1, samples with a thermal conductivity of 20% or more were rated A (passable), and samples with a thermal conductivity of less than 20% were rated B (unacceptable). Also, in Table 1, samples with an internal quantum yield of 85% or more were rated A (passable), and samples with an internal quantum yield of less than 85% were rated B (unacceptable). In the overall evaluation, samples that achieved an A in both the thermal conductivity and internal quantum yield evaluation items were rated as A (passable), and samples that achieved a B in at least one of the thermal conductivity and internal quantum yield evaluation items were rated as B (unacceptable).
[0113] [Table 1]
[0114] As shown in Table 1, in the case of Comparative Example 1 (MgAl2O4 content 0 vol%), YAG:Ce particles are more difficult to grow than AlN particles, so the amount of YAG:Ce particles contributing to light emission is small. In contrast, AlN grows more easily than YAG:Ce, so there are more defects at the interface between AlN and YAG:Ce, resulting in low values for thermal conductivity 14.3 and internal quantum yield 66.6%. In the case of Comparative Example 2 (MgAl2O4 content 0.05 vol%), the thermal conductivity of 29.4 is improved compared to Comparative Example 1 by suppressing defects at the interface between AlN and YAG:Ce, but the amount of YAG:Ce particles is insufficient, resulting in a low internal quantum yield of 72.6%.
[0115] In contrast, in the cases of Example 1 (MgAl2O4 content 0.10 vol%), Example 2 (MgAl2O4 content 0.10 vol%), Example 3 (MgAl2O4 content 0.15 vol%), Example 4 (MgAl2O4 content 0.40 vol%), and Example 5 (MgAl2O4 content 0.90 vol%), it was confirmed that the thermal conductivities of 35.1, 40.7, 41.4, 46.1, and 42.8, and the internal quantum yields of 87.2%, 87.4%, 89.1%, 86.5%, and 86.1% were all high values. That is, it was confirmed that when the content of MgAl2O4, which is the oxide layer, is 0.1 vol% or more and 0.9 vol% or less as in Examples 1 to 5, a fluorescent light emitting device with a thermal conductivity of 20 or more and an internal quantum yield of 55% or more can be obtained.
[0116] On the other hand, in the case of Comparative Example 3 (MgAl2O4 content 1.30 vol%), a sufficient thermal conductivity of 40.1 was obtained, but the growth balance of AlN and YAG:Ce was lost, resulting in a low internal quantum yield of 83.6%. In the case of Comparative Example 4 (MgAl2O4 content 3.00 vol%) in which the MgO content was increased more than in Comparative Example 3, the amount of MgAl2O4 generated increased too much, further disrupting the growth balance of AlN and YAG:Ce, and increasing the light loss inside the phosphor element, resulting in low thermal conductivity of 19.7 and internal quantum yield of 70.4%. That is, it was confirmed that when the MgAl2O4 content was higher than 0.9 vol %, as in Comparative Examples 3 and 4, both the thermal conductivity and the fluorescent luminous efficiency decreased.
[0117] From the above results, it was confirmed that, according to the phosphor elements of Examples 1 to 5, by setting the MgAl2O4 content to be 0.1 vol% or more and 0.9 vol% or less, the thermal conductivity and quantum yield can be increased in a balanced manner, thereby increasing the luminous efficiency of the fluorescence and generating bright fluorescence. [Explanation of symbols]
[0118] 1...projector, 2, 2A...illumination device, 4B, 4G, 4R...light modulation device, 6...projection optical device, 50, 250...wavelength conversion device, 51, 251...substrate, 52...phosphor element, 54...reflective layer, 254...optical layer, 520...phosphor body, 521...phosphor phase, 522...matrix phase, 523...oxide layer, E, E1...excitation light, Y...fluorescence.
Claims
1. A having a garnet structure 3 B 5 O 12 A phosphor phase composed of Ce; a matrix phase having a refractive index higher than that of the phosphor phase; an oxide layer provided between the phosphor phase and the matrix phase; the oxide layer is made of a composite oxide of a metal contained in the phosphor phase and a metal contained in a sintering aid, The content of the oxide layer is 0.1 vol% or more and 0.9 vol% or less in terms of volume ratio with respect to the phosphor body. A phosphor element characterized by: Here, A is at least one selected from the group consisting of Lu, Gd, Tb, Ga and Y, and B is Al.
2. A is Y, 2. The phosphor element according to claim 1 .
3. The matrix phase is AlN.
3. The phosphor element according to claim 1 or 2.
4. The oxide layer is made of MgAl 2 O 4 That is, 3. The phosphor element according to claim 1 or 2.
5. The oxide layer is CaAl 2 O 4 That is, 3. The phosphor element according to claim 1 or 2.
6. A substrate; The phosphor element according to claim 1 , which is provided on the substrate and converts incident excitation light into fluorescent light; A reflective layer is provided on the opposite side to the light incident side of the phosphor element. A wavelength conversion device characterized by:
7. A substrate; The phosphor element according to claim 1 , which is provided on the substrate and converts incident excitation light into fluorescent light; an optical layer provided on the light incident side of the phosphor element, the optical layer transmitting the excitation light and reflecting the fluorescence; A wavelength conversion device characterized by:
8. A light source that emits the excitation light; The wavelength conversion device according to claim 6 or 7, into which the excitation light is incident. A lighting device characterized by:
9. A lighting device according to claim 8 ; a light modulation device that modulates the light emitted from the illumination device; a projection optical device that projects the light modulated by the light modulation device. A projector characterized by:
Citation Information
Patent Citations
Ceramic composite
JP2012062459A