Phosphor element, wavelength converter, illumination device, and projector
The phosphor element with a YAG:Ce phosphor phase, AlN matrix, and YAlO3 crystalline phase addresses the thermal conductivity issue in ceramic composites, enhancing fluorescence extraction efficiency and emission brightness.
Patent Information
- Application Number
- JP2023085216
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional ceramic composites used in wavelength conversion members for projectors face challenges in improving fluorescence extraction efficiency due to insufficient thermal conductivity, leading to decreased fluorescence emission efficiency.
A phosphor element composed of a YAG:Ce phosphor phase with a garnet structure, a matrix phase of AlN, and a crystalline phase of YAlO3, where the crystalline phase content is between 0 vol% and 7.0 vol%, enhancing thermal conductivity and fluorescence extraction efficiency.
The phosphor element achieves improved thermal conductivity, increased external quantum yield, and enhanced fluorescence emission efficiency, allowing for brighter and more efficient fluorescence generation.
Smart Images

Figure 2024168493000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a phosphor element, a wavelength conversion device, an illumination device, and a projector. [Background technology]
[0002] Conventionally, ceramic composites have been used as wavelength conversion members for use in light sources for projectors. The following Patent Document 1 discloses a ceramic composite made of inorganic materials having a matrix phase made of translucent ceramics such as Al2O3, MgAl2O4, and MgO, and a phosphor phase made of YAG containing Ce. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-062459 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the ceramic composite disclosed in Patent Document 1, although the thermal conductivity is improved by mixing and sintering a highly thermally conductive filler, it is difficult to sufficiently improve the fluorescence extraction efficiency. [Means for solving the problem]
[0005] In order to solve the above problems, according to one aspect of the present invention, a garnet structure A3B5O 12A phosphor element is provided, which has a phosphor body including a phosphor phase constituted by Lu, Gd, Tb, Ga and Y, a matrix phase having a refractive index higher than that of the phosphor phase, and a crystalline phase constituted by YAlO3 having a perovskite structure, wherein the content of the crystalline phase is greater than 0 vol% and not more than 7.0 vol% in terms of volume ratio to the phosphor body, where A is at least one selected from the group consisting of Lu, Gd, Tb, Ga and Y, and B is Al.
[0006] According to another aspect of the present invention, there is provided a wavelength conversion device comprising: a substrate; a phosphor element of the above aspect that is provided on the substrate and converts incident excitation light into fluorescence; and a reflective layer that is provided on the opposite side to the light incident side of the phosphor element and reflects the excitation light and the fluorescence.
[0007] According to another aspect of the present invention, there is provided a wavelength conversion device comprising: a substrate; a phosphor element of the above aspect that is provided on the substrate and converts incident excitation light into fluorescence; and an optical layer that is provided on the light incident side of the phosphor element and transmits the excitation light and reflects the fluorescence.
[0008] According to another aspect of the present invention, there is provided an illumination device including a light source that emits excitation light, and the wavelength conversion device of the above aspect onto which the excitation light is incident.
[0009] According to another aspect of the present invention, there is provided a projector comprising an illumination device according to the above aspect, an optical modulator that modulates light emitted from the illumination device, and a projection optical device that projects the light modulated by the optical modulator. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic configuration diagram showing a projector according to a first embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing a configuration of a lighting device. [Diagram 3] FIG. 1 is a cross-sectional view showing a configuration of a wavelength conversion device. [Figure 4]FIG. 2 is a diagram showing an emission spectrum of a phosphor element. [Diagram 5] This is an SEM image of a phosphor element. [Figure 6] FIG. 11 is a schematic configuration diagram showing an illumination device according to a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Note that the drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand, and the dimensional ratios of each component may not necessarily be the same as in reality.
[0012] (First embodiment) Hereinafter, one embodiment of the present invention will be described. FIG. 1 is a schematic configuration diagram showing a projector according to a first embodiment. 1, the projector 1 of this embodiment is a projection type image display device that displays an image on a screen SCR. The projector 1 includes an illumination device 2, a color separation optical system 3, a light modulation device 4R, a light modulation device 4G, a light modulation device 4B, a synthesis optical system 5, and a projection optical device 6.
[0013] The illumination device 2 emits white illumination light WL toward the color separation optical system 3. The configuration of the illumination device 2 will be described in detail later.
[0014] The color separation optical system 3 separates the illumination light WL emitted from the illumination device 2 into red light LR, green light LG, and blue light LB. The color separation optical system 3 includes a first dichroic mirror 7a, a second dichroic mirror 7b, a first reflecting mirror 8a, a second reflecting mirror 8b, a third reflecting mirror 8c, a first relay lens 9a, and a second relay lens 9b.
[0015] The first dichroic mirror 7a separates the illumination light WL from the illumination device 2 into red light LR and light containing green light LG and blue light LB. The first dichroic mirror 7a transmits the red light LR and reflects the light containing green light LG and blue light LB. On the other hand, the second dichroic mirror 7b reflects the green light LG and transmits the blue light LB. In this way, the second dichroic mirror 7b separates the light containing green light LG and blue light LB into green light LG and blue light LB.
[0016] The first reflecting mirror 8a is disposed in the optical path of the red light LR and reflects the red light LR transmitted through the first dichroic mirror 7a toward the optical modulation device 4R. On the other hand, the second reflecting mirror 8b and the third reflecting mirror 8c are disposed in the optical path of the blue light LB and guide the blue light LB transmitted through the second dichroic mirror 7b to the optical modulation device 4B. The green light LG is reflected from the second dichroic mirror 7b toward the optical modulation device 4G.
[0017] The first relay lens 9a is disposed between the second dichroic mirror 7b and the second reflecting mirror 8b in the optical path of the blue light LB. The second relay lens 9b is disposed between the second reflecting mirror 8b and the third reflecting mirror 8c in the optical path of the blue light LB. The first relay lens 9a and the second relay lens 9b compensate for the optical loss of the blue light LB caused by the optical path length of the blue light LB being longer than the optical path lengths of the red light LR and the green light LG.
[0018] The light modulation device 4R modulates the red light LR according to image information to form image light corresponding to the red light LR. The light modulation device 4G modulates the green light LG according to image information to form image light corresponding to the green light LG. The light modulation device 4B modulates the blue light LB according to image information to form image light corresponding to the blue light LB.
[0019] For example, a transmissive liquid crystal panel is used for each of the light modulation device 4R, the light modulation device 4G, and the light modulation device 4B. Furthermore, a polarizing plate (not shown) is disposed on each of the incident side and the exit side of the liquid crystal panel.
[0020] A field lens 10R is disposed on the incident side of the optical modulation device 4R. The field lens 10R collimates the red light LR incident on the optical modulation device 4R. A field lens 10G is disposed on the incident side of the optical modulation device 4G. The field lens 10G collimates the green light LG incident on the optical modulation device 4G. A field lens 10B is disposed on the incident side of the optical modulation device 4B. The field lens 10B collimates the blue light LB incident on the optical modulation device 4B.
[0021] The image light emitted from the light modulation device 4R, the light modulation device 4G, and the light modulation device 4B is incident on the combining optical system 5. The combining optical system 5 combines the image light corresponding to the red light LR, the green light LG, and the blue light LB, respectively, and emits the combined image light toward the projection optical device 6. The combining optical system 5 uses, for example, a cross dichroic prism.
[0022] The projection optical device 6 has a plurality of projection lenses. The projection optical device 6 enlarges and projects the image light combined by the combining optical system 5 onto the screen SCR. As a result, an enlarged image is displayed on the screen SCR.
[0023] The configuration of the lighting device 2 will be described below. FIG. 2 is a schematic diagram showing the configuration of an illumination device 2 according to the present embodiment. As shown in FIG. 2, the illumination device 2 includes a first light source 40, a collimating optical system 41, a dichroic mirror 42, a first focusing optical system 43, a wavelength conversion device 50, a second light source 44, a second focusing optical system 45, a diffusion plate 46, and a collimating optical system 47.
[0024] The first light source 40 is composed of a plurality of semiconductor lasers 40a that emit blue excitation light E made of laser light. The emission intensity of the excitation light E has a peak of, for example, 445 nm. The plurality of semiconductor lasers 40a are arranged in an array in a plane perpendicular to the optical axis ax of the first light source 40. Note that the semiconductor lasers 40a may be semiconductor lasers that emit blue light of a wavelength other than 445 nm, for example, 455 nm or 460 nm. The optical axis ax of the first light source 40 is perpendicular to the illumination optical axis 100ax of the illumination device 2. The first light source 40 of the present embodiment corresponds to the "light source" in the claims.
[0025] The collimating optical system 41 includes a first lens 41a and a second lens 41b. The collimating optical system 41 approximately collimates the light emitted from the first light source 40. Each of the first lens 41a and the second lens 41b is formed of a convex lens.
[0026] The dichroic mirror 42 is disposed in the optical path from the collimating optical system 41 to the first collecting optical system 43 in a direction intersecting at an angle of 45° with respect to both the optical axis ax of the first light source 40 and the illumination optical axis 100ax. The dichroic mirror 42 reflects the blue light component and transmits the red light component and the green light component. Thus, the dichroic mirror 42 reflects the excitation light E and the blue light B and transmits the yellow fluorescence Y.
[0027] The first focusing optical system 43 focuses the excitation light E transmitted through the dichroic mirror 42 and makes it incident on the wavelength conversion device 50, while approximately collimating the fluorescence Y emitted from the wavelength conversion device 50. The first focusing optical system 43 includes a first lens 43a and a second lens 43b. Each of the first lens 43a and the second lens 43b is formed by a convex lens.
[0028] The second light source 44 is composed of a semiconductor laser having the same wavelength band as the first light source 40. The second light source 44 may be composed of one semiconductor laser, or may be composed of multiple semiconductor lasers. The second light source 44 may also be composed of a semiconductor laser having a different wavelength band from the semiconductor laser of the first light source 40.
[0029] The second light collecting optical system 45 includes a first lens 45a and a second lens 45b. The second light collecting optical system 45 collects the blue light B emitted from the second light source 44 on or near the diffusion surface of the diffusion plate 46. Each of the first lens 45a and the second lens 45b is formed of a convex lens.
[0030] The diffusion plate 46 diffuses the blue light B emitted from the second light source 44, and generates blue light B having a light distribution close to the light distribution of the fluorescence Y emitted from the wavelength conversion device 50. As the diffusion plate 46, for example, ground glass made of optical glass can be used.
[0031] The collimating optical system 47 includes a first lens 47a and a second lens 47b. The collimating optical system 47 approximately collimates the light emitted from the diffusion plate 46. Each of the first lens 47a and the second lens 47b is formed of a convex lens.
[0032] The blue light B emitted from the second light source 44 is reflected by the dichroic mirror 42, emitted from the wavelength conversion device 50, and combined with the fluorescence Y transmitted through the dichroic mirror 42 to generate white illumination light WL. The illumination light WL is incident on the uniform illumination optical system 80.
[0033] The uniform illumination optical system 80 includes a first lens array 81, a second lens array 82, a polarization conversion element 83, and a superimposing lens 84.
[0034] The first lens array 81 has a plurality of first lenses 81a for splitting the illumination light WL from the illumination device 2 into a plurality of partial light beams. The plurality of first lenses 81a are arranged in a matrix in a plane perpendicular to the illumination optical axis 100ax.
[0035] The second lens array 82 has a plurality of second lenses 82a corresponding to the plurality of first lenses 81a of the first lens array 81. The plurality of second lenses 82a are arranged in a matrix in a plane perpendicular to the illumination optical axis 100ax.
[0036] The second lens array 82, together with the superimposing lens 84, forms images of the first lenses 81a of the first lens array 81 near the image forming areas of the light modulation device 4R, the light modulation device 4G, and the light modulation device 4B, respectively.
[0037] The polarization conversion element 83 converts the light emitted from the second lens array 82 into one type of linearly polarized light. The polarization conversion element 83 includes, for example, a polarization separation film and a phase difference plate (not shown).
[0038] The superimposing lens 84 collects the partial light beams emitted from the polarization conversion element 83 and superimposes them near the image forming areas of the light modulation device 4R, the light modulation device 4G, and the light modulation device 4B.
[0039] Next, the configuration of the wavelength converter 50 will be described. Fig. 3 is a cross-sectional view showing the configuration of the wavelength conversion device 50. Fig. 3 corresponds to a cross-sectional view of the wavelength conversion device 50 cut along a plane including the illumination optical axis 100ax in Fig. 2.
[0040] 3, the wavelength converter 50 includes a substrate 51, a phosphor element 52, a bonding layer 53, and a reflective layer 54. The wavelength converter 50 of the present embodiment is configured as a fixed-type wavelength converter in which the incident position of the excitation light E with respect to the phosphor element 52 does not change over time.
[0041] The substrate 51 supports the reflective layer 54 and the phosphor elements 52 via a bonding layer 53. The substrate 51 is made of a metal material having high thermal conductivity, such as aluminum or copper. The bonding layer 53 is made of a bonding material having high thermal conductivity, such as nano silver paste. The bonding layer 53 bonds a first surface 51a, which is the surface of the substrate 51, to the phosphor elements 52.
[0042] The phosphor element 52 has a back surface 52a facing the substrate 51 and a front surface 52b opposite to the back surface 52a. The phosphor element 52 emits fluorescence Y from the front surface 52b, which is wavelength-converted excitation light E incident from the front surface 52b.
[0043] The reflective layer 54 is provided facing the back surface 52a of the phosphor element 52 with the bonding layer 53 interposed therebetween. That is, the reflective layer 54 is provided between the substrate 51 and the back surface 52a of the phosphor element 52. The reflective layer 54 is made of a metal film such as silver having high light reflectance, a dielectric multilayer film, or a combination of these films. The reflective layer 54 reflects the fluorescence Y traveling toward the side opposite to the light incident side (back surface 52a side) in the phosphor element 52 toward the light incident side (surface 52b side). The reflective layer 54 may reflect a part of the excitation light E toward the light incident side (surface 52b side), and the excitation light E reflected by the reflective layer 54 is used to excite the fluorescence Y. The wavelength converter 50 of this embodiment functions as a reflection-type wavelength converter that emits fluorescence Y from the surface 52b of the phosphor element 52 on which the excitation light E is incident.
[0044] It is generally known that the luminous efficiency of fluorescent light decreases as the temperature of a phosphor element increases, and improving the heat dissipation is an effective way to increase the fluorescent light conversion efficiency of the phosphor element. The inventors focused on increasing the thermal conductivity of phosphor elements by mixing and sintering a YAG:Ce phosphor, which is widely used as a phosphor element, with a highly thermally conductive filler material made of AlN. Generally, a sintered body of a phosphor element containing a phosphor phase made of YAG:Ce and a matrix phase made of AlN is formed by mixing and sintering the raw material powders Al2O3 (alumina), Y2O3 (yttria), and CeO2 (cerium oxide) with AlN powder as a binder material. However, simply sintering YAG:Ce and AlN creates crystal defects in AlN and impurities of oxynitrides such as AlON, making it difficult to sufficiently improve the thermal conductivity of the phosphor element, and the fluorescent light emission efficiency decreases, resulting in a small amount of extracted fluorescent light. In other words, simply sintering YAG:Ce and AlN reduces the external quantum yield and reduces the amount of extracted fluorescent light. The external quantum yield is the value (unit: %) obtained by dividing the total amount of fluorescent light emitted by the total amount of excitation light.
[0045] As a result of intensive research, the present inventors have found that when producing a fluorescent light-emitting element made of a sintered body containing a crystalline phase made of YAG:Ce and a matrix phase made of AlN, by adjusting the composition of the raw material powder of YAG:Ce so as to express a predetermined amount of crystalline phase in the phosphor phase, the thermal conductivity of the phosphor element can be increased and the external quantum yield (extraction amount) of fluorescence can be increased. Then, the present inventors have completed the configuration of the phosphor element 52 of this embodiment.
[0046] Specifically, the phosphor element 52 of this embodiment has a phosphor body 520 including a phosphor phase 521 , a matrix phase 522 , a crystal phase 523 , and another phosphor phase 524 . In the phosphor element 52, the phosphor phase 521 is ABO having a garnet structure. 12 The phosphor phase 521 of this embodiment contains phosphor particles composed of Y (yttrium) and B (aluminum). That is, the phosphor phase 521 of this embodiment contains yttrium aluminum garnet (YAG(Y3Al5O4)) to which cerium (Ce) is added as an activator. 12):Ce) phosphor particles.
[0047] The matrix phase 522 is a translucent ceramic that functions as a binder that binds together the multiple phosphor particles that constitute the phosphor phase 521 and transmits the fluorescence emitted by the phosphor phase 521. The matrix phase 522 in this embodiment is made of AlN (aluminum nitride). The matrix phase 522 has a refractive index (2.2) higher than the refractive index (1.8) of YAG:Ce that constitutes the phosphor phase 521.
[0048] The thermal conductivity of AlN constituting the matrix phase 522 is approximately 285 W / m·K, and the thermal conductivity of YAG:Ce constituting the phosphor phase 521 is approximately 9 W / m·K. In other words, the matrix phase 522 has a thermal conductivity that is sufficiently higher than that of the phosphor phase 521.
[0049] Moreover, the thermal conductivity of the matrix phase 522 of this embodiment is sufficiently higher than the thermal conductivity (approximately 30 W / m K) of Al2O3 (alumina) that is generally used as the matrix phase of ceramic phosphors. Therefore, the phosphor element 52 of this embodiment has superior thermal conductivity compared to conventional phosphor elements that use Al2O3 as the matrix phase, and therefore has excellent heat dissipation properties.
[0050] In the phosphor element 52 of the present embodiment, the crystalline phase 523 is included in the phosphor phase 521. It is difficult to determine based on an image or the like whether the phosphor phase 521 includes the crystalline phase 523, but it can be determined by using, for example, X-ray diffraction (XRD).
[0051] The crystal phase 523 is composed of YAlO3 (hereinafter, YAP) having a perovskite structure. In the phosphor element 52 of this embodiment, the content of the crystal phase 523 in terms of volume ratio to the phosphor body 520 is greater than 0 vol % and equal to or less than 7.0 vol %.
[0052] The other phosphor phase 524 includes phosphor particles composed of AlN:Ce. The other phosphor phase 524 is generated when the phosphor phase 521 and the matrix phase 522 are sintered.
[0053] Here, the emission spectrum of the phosphor element 52 of this embodiment will be described. The thick solid line in Fig. 4 indicates the emission spectrum of phosphor element 52 of the present embodiment, and the thin solid line in Fig. 4 indicates the emission spectrum of the phosphor element of the comparative example. The difference between the phosphor element of the comparative example and phosphor element 52 of the present embodiment is the presence or absence of another phosphor phase 524 composed of AlN:Ce. In Fig. 4, the horizontal axis indicates wavelength, and the vertical axis indicates relative emission intensity.
[0054] 4, the emission peak wavelength P1 of the spectrum in the phosphor element 52 of the present embodiment is higher than the emission peak wavelength P2 of the spectrum in the phosphor element of the comparative example. In other words, according to the phosphor element 52 of the present embodiment, the emission peak wavelength can be shifted to the longer wavelength side by including another phosphor phase 524 composed of AlN:Ce. Therefore, according to the phosphor element 52 of this embodiment, the peak wavelength is shifted to the long wavelength side, so that the color rendering of the emitted fluorescence Y can be further improved.
[0055] The phosphor element 52 of this embodiment is manufactured by, for example, mixing and sintering YAG raw material powder Al2O3, Y2O3, and CeO2 in a ratio of 56% by mass or more of Y2O3 and 0.5% by mass or more of CeO2 when sintering YAG:Ce and AlN. In this way, the manufacturing process of the phosphor element 52 of this embodiment adds an excess of Y2O3, so that a predetermined amount of YAP can be expressed in the phosphor phase 521 of the phosphor element 52. In the case of the phosphor element 52 of this embodiment, since Y2O3 functions as a sintering aid when sintering the phosphor body 520, the phosphor body 520 constituting the phosphor element 52 is made of a ceramic composite made of a sintered body with a dense crystal structure. Therefore, the phosphor element 52 of this embodiment has excellent thermal conductivity and can also increase the external quantum yield of the fluorescence Y.
[0056] The phosphor element 52 of this embodiment includes a phosphor phase 521, a matrix phase 522, a crystal phase 523, and a by-product different from another phosphor phase 524. The by-product of this embodiment is AlON, which is an oxynitride-based impurity generated when the materials of the phosphor element 52 are mixed and sintered.
[0057] In the phosphor element 52 of this embodiment, the state in which YAP is expressed in the phosphor phase 521 as described above means that the sintering of the phosphor body 520 proceeds smoothly while suppressing the generation of by-products that become impurities.
[0058] For this reason, in the phosphor element 52 of this embodiment, the content of the by-product (AlON) is less than 1.0 vol% in terms of volume ratio to the phosphor body 520. As described above, according to the phosphor element 52 of this embodiment, the amount of by-products is small, and therefore, the absorption of the fluorescence Y by the by-products and the heat generation associated with the absorption of the fluorescence Y are suppressed, thereby increasing the fluorescence conversion efficiency and generating bright fluorescence Y.
[0059] Here, when the content of the by-product (AlON) that becomes an impurity is low, the sintering of the phosphor body 520 proceeds well, and the occurrence of crystal defects in the AlN that constitutes the matrix phase 522 is also suppressed. Therefore, the content of impurities caused by AlN crystal defects in the phosphor body 520 is also very low, similar to the case of the by-product. It is known that the emission peak wavelength of a phosphor light-emitting element containing AlN with a high crystal defect rate is 610 nm.
[0060] In contrast, the phosphor element 52 of the present embodiment contains a small amount of by-products and impurities caused by crystal defects in AlN as described above. Therefore, the emission peak wavelength of the phosphor body 520 in the phosphor element 52 of the present embodiment is less than 610 nm.
[0061] Fig. 5 is a diagram showing the main configuration of a phosphor element 52 of this embodiment. Fig. 5 is an image of the phosphor element 52 captured using a SEM (scanning electron microscope). The image capture range of the image shown in Fig. 5 is 400 μm 2 It is.
[0062] The phosphor element 52 of this embodiment has a small number of voids (air gaps) contained in the phosphor body 520. Specifically, as shown in FIG. 2 The number of voids (air gaps) 525 of 1.0 μm or more contained in the imaging area is 9 or less. The size of the voids 525 is, for example, 400 μm or less by a microscope. 2 The definition was based on the length of the void 525 in the major axis direction in the image obtained in the cross-sectional observation. The phosphor element 52 of the present embodiment has a small number of voids 525 contained in the phosphor body 520, and therefore the strength and thermal conductivity of the phosphor body 520 can be further increased. Thus, the reliability of the phosphor element 52 can be further increased.
[0063] As described above, the phosphor element 52 of the present embodiment is a YAG (YAlO 12 ): The phosphor body 520 includes a phosphor phase 521 made of Ce, a matrix phase 522 made of AlN having a refractive index higher than that of the phosphor phase 521, and a crystal phase 523 made of YAlO3 having a perovskite structure. The content of the crystal phase 523 is greater than 0 vol% and equal to or less than 7.0 vol% in terms of volume ratio to the phosphor body 520. Hereinafter, in this specification, the content of the crystal phase 523 is referred to as the "YAP content."
[0064] According to the phosphor element 52 of this embodiment, the amount of YAP contained in the phosphor body 520 is greater than 0 vol% and equal to or less than 7.0 vol%, so that the phosphor element 52 is sintered in a state in which Y2O3 functioning as a sintering aid is added in excess. The phosphor element 52 is sintered in a state in which it contains a large amount of Y2O3 functioning as a sintering aid, so that the phosphor element 52 has a phosphor body 520 made of a ceramic composite having a dense crystal structure.
[0065] The phosphor element 52 of this embodiment has a matrix phase 522 made of AlN with high thermal conductivity, and therefore can efficiently release heat accompanying fluorescent emission, thereby suppressing a decrease in fluorescence conversion efficiency accompanying a rise in temperature. As a result, the excitation light E is efficiently absorbed by the phosphor phase 521, increasing the luminous efficiency of the fluorescence Y, and a bright fluorescence Y can be generated.
[0066] According to the phosphor element 52 of this embodiment, by increasing the external quantum yield of the fluorescence Y to 55% or more, it is possible to emit fluorescence Y from the phosphor element 52 with a brightness that does not cause any problems in practical use as illumination light for a projector.
[0067] The wavelength conversion device 50 of this embodiment comprises a substrate 51, a phosphor element 52 provided on the substrate 51 for converting incident excitation light E into fluorescence, and a reflective layer 54 provided on the side opposite the light incident side of the phosphor element 52. According to the wavelength converter 50 of the present embodiment, a reflective wavelength converter that efficiently extracts bright fluorescence Y can be provided.
[0068] The illumination device 2 of this embodiment includes a first light source 40 that emits excitation light E, and a wavelength conversion device 50 into which the excitation light E is incident. According to the lighting device 2 of the present embodiment, it is possible to provide a lighting device that has excellent wavelength conversion efficiency and emits bright illumination light WL.
[0069] The projector 1 of this embodiment includes an illumination device 2, light modulation devices 4R, 4G, and 4B that modulate the light emitted from the illumination device 2, and a projection optical device 6 that projects the light modulated by the light modulation devices 4R, 4G, and 4B.
[0070] According to the projector 1 of the present embodiment, it is possible to provide a highly efficient projector with excellent display quality.
[0071] Second embodiment The projector according to the second embodiment will be described below. The basic configuration of the projector of the second embodiment is similar to that of the first embodiment, but the configuration of the illumination device is different from that of the first embodiment, so the configuration of the illumination device will be described below.
[0072] FIG. 6 is a schematic configuration diagram showing an illumination device 2A according to the second embodiment. In FIG. 6, components common to those in the drawings used in the above embodiment are given the same reference numerals, and description thereof will be omitted.
[0073] As shown in FIG. 6, the illumination device 2A includes an excitation light source unit 10, an afocal optical system 11, a homogenizer optical system 12, a focusing optical system 13, a wavelength conversion device 250, a pickup optical system 30, and a uniform illumination optical system 80.
[0074] The excitation light source unit 10 is composed of a plurality of semiconductor lasers 10a that emit blue excitation light E composed of laser light, and a plurality of collimator lenses 10b. The plurality of semiconductor lasers 10a are arranged in an array in a plane perpendicular to the illumination optical axis 100ax. The collimator lenses 10b are arranged in an array in a plane perpendicular to the illumination optical axis 100ax so as to correspond to each semiconductor laser 10a. The collimator lenses 10b convert the excitation light E emitted from the semiconductor lasers 10a corresponding to the collimator lenses 10b into parallel light. The excitation light source unit 10 of this embodiment corresponds to the "light source" in the claims.
[0075] The afocal optical system 11 includes, for example, a convex lens 11a and a concave lens 11b. The afocal optical system 11 reduces the beam diameter of the excitation light E emitted from the excitation light source unit 10 and consisting of a parallel beam.
[0076] The homogenizer optical system 12 includes, for example, a first multi-lens array 12a and a second multi-lens array 12b. The homogenizer optical system 12 makes the light intensity distribution of the excitation light uniform on the phosphor element 52 of the wavelength conversion device 250, that is, a so-called top hat distribution. The homogenizer optical system 12, together with the focusing optical system 13, superimposes a plurality of small light beams emitted from a plurality of lenses of the first multi-lens array 12a and the second multi-lens array 12b on the phosphor element 52 of the wavelength conversion device 250. This makes the light intensity distribution of the excitation light E irradiated on the phosphor element 52 uniform.
[0077] The focusing optical system 13 includes, for example, a first lens 13a and a second lens 13b. In this embodiment, the first lens 13a and the second lens 13b are each formed of a convex lens. The focusing optical system 13 is disposed in the optical path from the homogenizer optical system 12 to the wavelength conversion device 250, and focuses the excitation light E to make it incident on the phosphor element 52 of the wavelength conversion device 250.
[0078] The wavelength converter 250 of this embodiment includes a substrate 251, a phosphor element 52, a bonding layer 253, and an optical layer 254. The wavelength converter 250 of this embodiment is configured as a fixed type wavelength converter in which the incident position of the excitation light E with respect to the phosphor element 52 does not change over time.
[0079] The substrate 251 supports the optical layer 254 and the phosphor elements 52 via a bonding layer 253. The substrate 251 is made of a light-transmitting material such as glass or plastic. The bonding layer 253 in this embodiment is made of a light-transmitting material such as epoxy. The bonding layer 253 bonds a first surface 251a, which is the surface of the substrate 251, to the phosphor elements 52.
[0080] In the phosphor element 52 of this embodiment, excitation light E is incident on the back surface 52a facing the substrate 251, and fluorescence Y is emitted from the front surface 52b. In the wavelength conversion device 250 of this embodiment, the phosphor element 52 transmits and emits not only the fluorescence Y, but also a portion of the excitation light E1 that has not been wavelength-converted. This causes white illumination light WL1 to be emitted from the phosphor element 52.
[0081] The optical layer 254 is provided on a rear surface 52a which is the light incident side of the phosphor element 52. The optical layer 254 is composed of a dichroic mirror which transmits the excitation light E and reflects the fluorescence Y.
[0082] The wavelength converter 250 of this embodiment functions as a transmissive wavelength converter that emits illumination light WL1 containing fluorescence Y from a front surface 52b opposite to a back surface 52a of the phosphor element 52 on which excitation light E is incident.
[0083] The pickup optical system 30 includes, for example, a first collimating lens 31 and a second collimating lens 32. The pickup optical system 30 is a collimating optical system that approximately collimates the light emitted from the phosphor element 52 of the wavelength conversion device 250. The first collimating lens 31 and the second collimating lens 32 are each composed of a convex lens. The light collimated by the pickup optical system 30 enters the uniform illumination optical system 80.
[0084] (Effects of the second embodiment) According to this embodiment, by using the phosphor element 52 capable of increasing the amount of extracted fluorescence Y, it is possible to realize a transmissive wavelength conversion device 250 that generates bright fluorescence Y. Also, by providing the illumination device 2A of this embodiment with the transmissive wavelength conversion device 250, it is possible to obtain the same effect as in the first embodiment, that is, excellent wavelength conversion efficiency and the ability to emit bright illumination light WL1.
[0085] The technical scope of the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the spirit of the present invention. The specific descriptions of the shape, number, arrangement, material, manufacturing method, etc. of each component of the phosphor element, wavelength conversion device, lighting device, and projector shown in the above embodiments are not limited to the above embodiments and can be modified as appropriate.
[0086] In the above embodiment, YAG containing Ce is used as the phosphor phase 521. 12 , Tb3Al5O 12 , Ga3Al5O 12 , Gd3Al5O 12 The present invention is also applicable to the case where a phosphor phase containing Ce in at least one of the following structures is used. 12 In addition to Y (yttrium), A in Ce) can also be replaced with Lu (lutetium), Gd (gadolinium), Tb (terbium), or Ga (gallium), which has the same luminescence characteristics as Y, and therefore the present invention is also applicable when A is replaced with any of these.
[0087] The following is a summary of this disclosure. (Appendix 1) A3B5O with garnet structure 12 A phosphor phase composed of Ce; a matrix phase having a refractive index higher than that of the phosphor phase; A phosphor body including a crystalline phase constituted by YAlO3 having a perovskite structure, The content of the crystalline phase is, in terms of volume ratio with respect to the phosphor body, greater than 0 vol% and less than 7.0 vol%; A phosphor element characterized by: Here, A is at least one selected from the group consisting of Lu, Gd, Tb, Ga and Y, and B is Al.
[0088] The phosphor element of this configuration includes a phosphor body that is sintered in a state where a large amount of sintering aid is included so that the crystalline phase is more than 0 vol% and not more than 7.0 vol%. The phosphor element of this configuration is composed of a ceramic composite made of a sintered body with a dense crystal structure, so that it has excellent thermal conductivity and can also increase the external quantum yield of fluorescence. In addition, the excellent thermal conductivity allows the heat associated with fluorescent light emission to be efficiently released, thereby suppressing the decrease in fluorescence conversion efficiency associated with temperature rise. Therefore, a phosphor element having this configuration can efficiently generate bright fluorescent light.
[0089] (Appendix 2) A is Y, 2. A phosphor element according to claim 1.
[0090] According to this configuration, YAG (Y3Al5O 12 ): A phosphor element that efficiently generates bright fluorescence containing a phosphor phase composed of Ce can be realized.
[0091] (Appendix 3) The matrix phase is AlN. 3. The phosphor element according to claim 1 or 2,
[0092] According to this configuration, since the matrix phase is made of AlN, which has high thermal conductivity, the heat generated by the fluorescent light emission can be efficiently released, thereby suppressing the decrease in the fluorescent light conversion efficiency caused by the temperature rise.
[0093] (Appendix 4) The phosphor body further includes another phosphor phase composed of AlN:Ce. 4. The phosphor element according to claim 3.
[0094] According to this configuration, the inclusion of another phosphor phase made of AlN:Ce makes it possible to shift the emission peak wavelength of the phosphor body to the longer wavelength side, thereby further improving the color rendering of the emitted fluorescence.
[0095] (Appendix 5) In the cross-sectional view of the phosphor body, 2 The number of voids of 1.0 μm or more contained in the area is 9 or less. 5. The phosphor element according to claim 1,
[0096] According to this configuration, the phosphor body contains fewer voids, so that the strength and thermal conductivity of the phosphor body can be further increased.
[0097] (Appendix 6) the phosphor body contains by-products different from the phosphor phase, the matrix phase, and the crystalline phase; The content of the by-product is less than 1.0 vol% in terms of volume ratio to the phosphor body; 6. A phosphor element according to any one of claims 1 to 5,
[0098] According to this configuration, by suppressing the content of by-products in the phosphor body to less than 1.0 vol %, a phosphor element having high thermal conductivity and excellent fluorescence extraction efficiency can be provided.
[0099] (Appendix 7) The emission peak wavelength of the phosphor body is less than 610 nm; 7. The phosphor element according to claim 1,
[0100] According to this configuration, the emission peak wavelength of the phosphor body is less than 610 nm, so that a phosphor element can be provided that contains a small amount of by-products and impurities caused by crystal defects.
[0101] (Appendix 8) A substrate; A phosphor element according to any one of claims 1 to 7, which is provided on the substrate and converts incident excitation light into fluorescent light; A reflective layer is provided on the opposite side to the light incident side of the phosphor element. A wavelength conversion device characterized by:
[0102] According to the wavelength converter having this configuration, a reflective wavelength converter that efficiently extracts bright fluorescent light Y can be provided.
[0103] (Appendix 9) A substrate; A phosphor element according to any one of claims 1 to 7, which is provided on the substrate and converts incident excitation light into fluorescent light; an optical layer provided on the light incident side of the phosphor element, the optical layer transmitting the excitation light and reflecting the fluorescence; A wavelength conversion device characterized by:
[0104] According to the wavelength converter having this configuration, it is possible to provide a transmission type wavelength converter that efficiently extracts bright fluorescent light.
[0105] (Appendix 10) A light source that emits the excitation light; and a wavelength conversion device according to claim 8 or 9, into which the excitation light is incident. A lighting device characterized by:
[0106] According to the illumination device having this configuration, it is possible to provide an illumination device that has excellent wavelength conversion efficiency and emits bright illumination light.
[0107] (Appendix 11) A lighting device according to claim 10; a light modulation device that modulates the light emitted from the illumination device; a projection optical device that projects the light modulated by the light modulation device. A projector characterized by:
[0108] According to a projector having this configuration, a highly efficient projector with excellent display quality can be provided. EXAMPLES
[0109] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0110] Example 1 First, the amounts of Al2O3, Y2O3, and CeO2 in the YAG raw material powder were adjusted so that the YAP content was 0.1 vol %, and the phosphor element of Example 1 was produced by sintering YAG:Ce and AlN.
[0111] Example 2 The phosphor element of Example 2 was manufactured by carrying out the same steps as in Example 1, except that the amounts of Al2O3, Y2O3, and CeO2 in the YAG raw material powder were adjusted so that the YAP content was 0.3 vol %.
[0112] Example 3 A phosphor element of Example 3 was manufactured by carrying out the same steps as in Example 1, except that the amounts of Al2O3, Y2O3, and CeO2 in the YAG raw material powder were adjusted so that the YAP content was 0.7 vol %.
[0113] Example 4 The phosphor element of Example 4 was manufactured by carrying out the same steps as in Example 1, except that the amounts of Al2O3, Y2O3, and CeO2 in the YAG raw material powder were adjusted so that the YAP content was 1.1 vol %.
[0114] Example 5 The phosphor element of Example 5 was manufactured by carrying out the same steps as in Example 1, except that the amounts of Al2O3, Y2O3, and CeO2 in the YAG raw material powder were adjusted so that the YAP content was 1.9 vol %.
[0115] Example 6 The phosphor element of Example 6 was manufactured by carrying out the same steps as in Example 1, except that the amounts of Al2O3, Y2O3, and CeO2 in the YAG raw material powder were adjusted so that the YAP content was 4.6 vol %.
[0116] Example 7 The phosphor element of Example 7 was manufactured by carrying out the same steps as in Example 1, except that the amounts of Al2O3, Y2O3, and CeO2 in the YAG raw material powder were adjusted so that the YAP content was 7.0 vol %.
[0117] Comparative Example 1 A phosphor element of Comparative Example 1 was manufactured by carrying out the same steps as in Example 1, except that the YAG raw material powder was adjusted so that the YAP content was 0 vol %.
[0118] Comparative Example 2 A phosphor element of Comparative Example 2 was manufactured by carrying out the same steps as in Example 1, except that the YAG raw material powder was adjusted so that the YAP content was 7.2 vol %.
[0119] Comparative Example 3 A phosphor element of Comparative Example 3 was manufactured by carrying out the same steps as in Example 1, except that the YAG raw material powder was adjusted so that the YAP content was 8.0 vol %.
[0120] Comparative Example 4 A phosphor element of Comparative Example 4 was manufactured by carrying out the same steps as in Example 1, except that the YAG raw material powder was adjusted so that the YAP content was 9.1 vol %.
[0121] Comparative Example 5 A phosphor element of Comparative Example 5 was manufactured by carrying out the same steps as in Example 1, except that the YAG raw material powder was adjusted so that the YAP content was 10.0 vol %.
[0122] (Evaluation of each Example and Comparative Example) For each of the above-mentioned examples and comparative examples, the number of voids (unit: voids), thermal conductivity (unit: W / m K), and external quantum yield (unit: %) were confirmed, and phosphor elements with high external quantum yield and thermal conductivity were determined to have high light utilization efficiency. The results are shown in Table 1. The number and size of voids were measured, for example, by a microscope using a 400 μm 2The thermal conductivity is defined based on the length in the long axis direction of the image obtained in the cross-sectional observation of the specimen. The thermal conductivity is a value based on the measurement results at room temperature.
[0123] In Table 1, samples with a thermal conductivity of 20% or more were rated A (passable), and samples with a thermal conductivity of less than 20% were rated B (unacceptable). Also, in Table 1, samples with an external quantum yield of 55% or more were rated A (passable), and samples with an external quantum yield of less than 55% were rated B (unacceptable). As an overall evaluation, samples that achieved an A in both the evaluation items of thermal conductivity and external quantum yield were rated as A (passable), and samples that achieved a B in at least one of the evaluation items of thermal conductivity and external quantum yield were rated as B (unacceptable). In Table 1, the YAG amount was defined as the content (vol%) of YAP in the entire phosphor element.
[0124] [Table 1]
[0125] As shown in Table 1, in the case of Comparative Example 1 (YAP content 0 vol%), YAG phosphor and AlN are simply mixed and sintered, which causes crystal defects in AlN and impurities of oxynitrides such as AlON, resulting in a low thermal conductivity of 14.3 and a low external quantum yield of 46.8%. In addition, the number of voids contained in the phosphor element is high at 16.
[0126] In contrast, in the case of Example 1 (YAP content: 0.1 vol%), Example 2 (YAP content: 0.3 vol%), Example 3 (YAP content: 0.7 vol%), Example 4 (YAP content: 1.1 vol%), Example 5 (YAP content: 1.9 vol%), Example 6 (YAP content: 4.6 vol%), and Example 7 (YAP content: 7.0 vol%), it was confirmed that the number of voids was 9 or less in all cases, and the thermal conductivities were 40.9, 40.7, 46.1, 41.4, 59.2, 43.0, and 40.1, and the external quantum yields were 65.6%, 64.9%, 64.8%, 65.4%, 62.3%, 57.3%, and 55.0%, all of which were high. That is, it was confirmed that when the YAP amount was greater than 0 vol % and not more than 7.0 vol % as in Examples 1 to 7, the thermal conductivity was 20 or more and the external quantum yield was 55% or more.
[0127] On the other hand, in the case of Comparative Example 2 (YAP content: 7.2 vol%), Comparative Example 3 (YAP content: 8.0 vol%), Comparative Example 4 (YAP content: 9.1 vol%), and Comparative Example 5 (YAP content: 10.0 vol%), the number of voids was all 9 or less, and sufficient values of thermal conductivity were obtained, 36.7, 38.0, 31.6, and 30.8, respectively, but the external quantum yields were 49.5%, 46.7%, 42.4%, and 38.7%, respectively, which were not sufficient in terms of fluorescence conversion efficiency. That is, it was confirmed that when the YAP amount was higher than 7.0 vol %, as in Comparative Examples 2 to 5, the external quantum yield was reduced to less than 55%, and the fluorescence luminous efficiency was reduced.
[0128] From the above results, it was confirmed that, according to the phosphor elements of Examples 1 to 7, by setting the YAP amount to be greater than 0 vol% and equal to or less than 7.0 vol%, the thermal conductivity and quantum yield can be increased in a balanced manner, thereby increasing the luminous efficiency of the fluorescence and generating bright fluorescence. [Explanation of symbols]
[0129] 1...projector, 2, 2A...illumination device, 4B, 4G, 4R...light modulation device, 6...projection optical device, 50, 250...wavelength conversion device, 51, 251...substrate, 52...phosphor element, 54...reflective layer, 254...optical layer, 520...phosphor body, 521...phosphor phase, 522...matrix phase, 523...crystalline phase, 524...other phosphor phase, 525...void (air gap), E, E1...excitation light, Y...fluorescence.
Claims
1. A having a garnet structure 3 B 5 O 12 A phosphor phase composed of Ce; a matrix phase having a refractive index higher than that of the phosphor phase; YAlO having a perovskite structure 3 and a crystalline phase constituted by The content of the crystalline phase is, in terms of volume ratio with respect to the phosphor body, greater than 0 vol% and less than 7.0 vol%; A phosphor element characterized by: Here, A is at least one selected from the group consisting of Lu, Gd, Tb, Ga and Y, and B is Al.
2. A is Y, 2. The phosphor element according to claim 1 .
3. The matrix phase is AlN.
3. The phosphor element according to claim 1 or 2.
4. The phosphor body further includes another phosphor phase composed of AlN:Ce.
4. The phosphor element according to claim 3.
5. In a cross-sectional view of the phosphor body, 2 The number of voids of 1.0 μm or more contained in the region is 9 or less.
3. The phosphor element according to claim 1 or 2.
6. the phosphor body contains by-products different from the phosphor phase, the matrix phase, and the crystalline phase; The content of the by-product is less than 1.0 vol% in terms of volume ratio to the phosphor body; 3. The phosphor element according to claim 1 or 2.
7. The emission peak wavelength of the phosphor body is less than 610 nm; 3. The phosphor element according to claim 1 or 2.
8. A substrate; The phosphor element according to claim 1 , which is provided on the substrate and converts incident excitation light into fluorescent light; A reflective layer is provided on the opposite side to the light incident side of the phosphor element. A wavelength conversion device characterized by:
9. A substrate; The phosphor element according to claim 1 , which is provided on the substrate and converts incident excitation light into fluorescent light; an optical layer provided on the light incident side of the phosphor element, the optical layer transmitting the excitation light and reflecting the fluorescence; A wavelength conversion device characterized by:
10. A light source that emits the excitation light; The wavelength conversion device according to claim 8 or 9, into which the excitation light is incident. A lighting device characterized by:
11. A lighting device according to claim 10; a light modulation device that modulates the light emitted from the illumination device; a projection optical device that projects the light modulated by the light modulation device. A projector characterized by:
Citation Information
Patent Citations
Ceramic composite
JP2012062459A