Tennis ball
A tennis ball core using microfibrillated fibers, particularly cellulose nanofibers, addresses density issues in high-reinforcement fillers by maintaining mass compliance and enhancing rebound and control performance.
Patent Information
- Application Number
- JP2023085920
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
AI Technical Summary
Existing tennis balls with high amounts of inorganic fillers for reinforcement face issues with density, violating International Tennis Federation mass standards.
A tennis ball core composed of a rubber composition incorporating microfibrillated fibers, particularly cellulose nanofibers, which provides reinforcement without excessive mass, using a manufacturing process that includes mixing microfibrillated fibers with rubber latex, forming a masterbatch, and bonding half shells to create a core with embedded fibers.
The core achieves sufficient reinforcement while maintaining compliance with mass standards, offering improved rebound performance, grip, and control due to the unique properties of microfibrillated fibers, ensuring long-term durability and energy efficiency.
Smart Images

Figure 2024168888000001_ABST
Abstract
Description
[Technical field]
[0001] This specification discloses a tennis ball. In particular, this specification relates to an improvement in the core of the tennis ball. [Background technology]
[0002] The tennis ball has a core and a skin covering the core. The core is hollow. The core is formed by crosslinking a rubber composition. The core can contribute to the resilience performance of the tennis ball. An example of a rubber composition for the core is disclosed in JP 2019-17996 A. The rubber composition contains an inorganic filler. The inorganic filler can reinforce the rubber. The inorganic filler can contribute to the resilience performance of the tennis ball. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP2019-17996A Summary of the Invention [Problem to be solved by the invention]
[0004] In the tennis ball disclosed in JP 2019-17996 A, the reinforcing effect of the inorganic filler is insufficient. If the core contains a large amount of filler, the core can contribute to the resilience performance of the tennis ball. However, the inclusion of a large amount of filler leads to a high density of the core. A high density core can prevent the tennis ball from complying with the International Tennis Federation's mass standard.
[0005] It is Applicant's intent to provide a tennis ball having a core that is of suitable mass and adequately reinforced. [Means for solving the problem]
[0006] The tennis ball disclosed herein has a core and a cover. The core is formed from a rubber composition that includes a base rubber and microfibrillated fibers. Effect of the Invention
[0007] In this tennis ball, the core is sufficiently reinforced by the microfibrillated fibers, a small amount of reinforcing material and filler is sufficient in this core, and the weight of a tennis ball having this core is not excessive. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a front view showing a tennis ball according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, preferred embodiments will be described in detail with reference to the drawings as appropriate.
[0010] [Tennis ball] 1 shows a tennis ball 2. This tennis ball 2 has a core 4, two sheets of felt 6, and a seam 8. These felt 6 and seam 8 form an outer shell 10. This outer shell 10 covers the core 4. The outer diameter of the tennis ball 2 is preferably 6.54 cm or greater and 6.86 cm or less. The mass of the tennis ball 2 is preferably 56.0 g or greater and 59.4 g or less.
[0011] [core] The core 4 has a spherical shape. The core 4 is hollow. The thickness of the core 4 is generally 3.0 mm to 4.0 mm. The core 4 may be filled with compressed gas. The internal pressure of the core 4 may be the same as atmospheric pressure. The material of the core 4 will be described in detail later.
[0012] [felt] Each felt 6 has a shape similar to a dumbbell. The felt 6 is attached to the core 4. The attachment is achieved by means of an adhesive (latex). The appearance of the tennis ball 2 depends mainly on the appearance of the felt 6. In this embodiment, the color of the felt 6 is yellow. The felt 6 achieves a color of the tennis ball 2 that complies with the standards of the International Tennis Federation. The color of the felt 6 may be white. For tennis balls 2 that do not need to comply with this standard, felt 6 of various colors may be employed. The outer shell 10 may be formed from a sheet other than the felt 6.
[0013] [Seam] The seam 8 is located between one felt 6 and the other felt 6. The seam 8 can be obtained by crosslinking a rubber composition. The width of the seam 8 is 2.0 mm or more and 8.0 mm or less.
[0014] [Core material] The core 4 is formed by crosslinking a rubber composition.
[0015] [Base rubber] The rubber composition of the core 4 contains a base rubber. An example of a rubber suitable for the base rubber is an isoprene-based rubber. The isoprene-based rubber can contribute to the resilience performance of the tennis ball 2. The isoprene-based rubber includes natural rubber, epoxidized natural rubber, highly purified natural rubber, deproteinized natural rubber, and polyisoprene. The rubber composition may contain two or more types of isoprene-based rubber.
[0016] Rubbers other than isoprene-based rubber may be used as the base rubber. Examples of rubbers other than isoprene-based rubber include polybutadiene, styrene-butadiene copolymers, acrylonitrile-butadiene copolymers, polychloroprene, ethylene-propylene copolymers, ethylene-propylene-diene copolymers, and acrylic rubbers.
[0017] The rubber composition may contain an isoprene-based rubber and a rubber other than the isoprene-based rubber. From the viewpoint of resilience performance, it is preferable that the main component of the base rubber is an isoprene-based rubber. The ratio of the isoprene-based rubber to the total base rubber is preferably 30% by mass or more, more preferably 50% by mass or more, and particularly preferably 60% by mass or more. This ratio is ideally 100% by mass.
[0018] From the viewpoint of resilience performance, the base rubber is particularly preferably natural rubber. The rubber composition may contain natural rubber and other rubbers. From the viewpoint of resilience performance, the base rubber is preferably mainly composed of natural rubber. The ratio of natural rubber to the total base rubber is preferably 30% by mass or more, more preferably 50% by mass or more, and particularly preferably 60% by mass or more. This ratio may be 100% by mass.
[0019] [Microfibrillated fiber] The rubber composition contains microfibrillated fibers. The microfibrillated fibers can be obtained by unraveling raw material fibers. Examples of raw material fibers include cellulose fibers and aramid fibers. The microfibrillated fibers have a small fiber diameter. Therefore, the specific surface area of the microfibrillated fibers is large. The reinforcing effect of the microfibrillated fibers is large. Even if the content of the microfibrillated fibers in the core 4 is small, the core 4 can sufficiently contribute to the resilience performance of the tennis ball 2.
[0020] From the viewpoint of reinforcing effect, the number average fiber diameter of the microfibrillated fibers is preferably 1000 nm or less, more preferably 500 nm or less, and particularly preferably 100 nm or less. From the viewpoint of the strength of each fiber, the number average fiber diameter is preferably 3 nm or more, more preferably 5 nm or more, and particularly preferably 10 nm or more.
[0021] The amount of microfibrillated fibers is preferably 5.0 parts by mass or more per 100 parts by mass of the base rubber. A rubber composition having this amount of 5.0 parts by mass can provide the core 4 that contributes to the resilience performance of the tennis ball 2. From this viewpoint, the amount is more preferably 7.5 parts by mass or more, and particularly preferably 10.0 parts by mass or more. From the viewpoint of the appropriate mass of the tennis ball 2, the amount is preferably 30.0 parts by mass or less, more preferably 25.0 parts by mass or less, and particularly preferably 22.5 parts by mass or more.
[0022] [Cellulose nanofiber] From the viewpoint of conformity with the spirit of the Sustainable Development Goals (SDGs), plant-derived microfibrillated fibers are preferred. A particularly preferred microfibrillated fiber is cellulose nanofiber. Since the specific surface area of cellulose nanofiber is large, the reinforcing effect of this cellulose nanofiber is large. The cellulose nanofiber can contribute to the resilience performance of the tennis ball 2. The cellulose nanofiber is also highly versatile.
[0023] The density of cellulose nanofibers is low. Therefore, even if the content of cellulose nanofibers in the rubber composition is small, a sufficient reinforcing effect can be obtained. The mass of cellulose nanofibers in the mass of this tennis ball 2 can be small. This tennis ball 2 allows a high degree of freedom in adding other additives. Even if the content of cellulose nanofibers is high, the effect on the mass of tennis ball 2 is small, so that this tennis ball 2 can satisfy the mass range set by the International Tennis Federation standards even when cellulose nanofibers are used in combination with other additives.
[0024] In the core 4, the adhesion between the cellulose nanofibers and the rubber matrix is not excessive. Therefore, when the tennis ball 2 is hit with a racket, a moderate energy loss occurs. Because the contact time of the tennis ball 2 with the racket during the hit is long, the player feels that the tennis ball 2 has good grip. In other words, the tennis ball 2 has excellent controllability.
[0025] The gas permeability coefficient of a rubber molded product containing cellulose nanofibers is small. The internal pressure is easily maintained in the core 4 containing cellulose nanofibers. The tennis ball 2 having this core 4 can withstand long-term use.
[0026] Cellulose nanofibers can be obtained by disintegrating cellulose fibers, which are raw materials. Cellulose fibers are abundant on earth. Cellulose fibers can be obtained from wood, bamboo, hemp, jute, kenaf, straw, rice husks, thatch, seaweed, etc. Cellulose fibers can also be obtained from agricultural residues such as vegetable waste, tea leaves, and tangerine peel. Cellulose nanofibers may be obtained from regenerated cellulose fibers (viscose, cupra, tencel, etc.) or cellulose derivative fibers.
[0027] The cellulose nanofibers may be obtained from cellulose fibers that are inorganic esters. Examples of inorganic esters include nitrates, sulfates, phosphates, and silicates. The cellulose nanofibers may be obtained from cellulose fibers that are etherified. Examples of etherified products include methyl ether, hydroxyethyl ether, hydroxypropyl ether, hydroxybutyl ether, carboxymethyl ether, and cyanoethyl ether. The cellulose nanofibers may be obtained from TEMPO-oxidized pulp.
[0028] The cellulose fibers can be loosened by mechanical processing. Examples of the processing include grinding and beating. Examples of machines suitable for processing include a refiner, a twin-screw kneader, a twin-screw extruder, a twin-screw kneading extruder, a high-pressure homogenizer, a media stirring mill, a stone mill, a grinder, a vibration mill, and a sand grinder.
[0029] The shape of the cellulose nanofiber may be a single nanofiber consisting of a crystalline portion, a quasi-crystalline portion, and an amorphous portion. The cellulose nanofiber may have a shape in which the cellulose fiber is locally decomposed into a plurality of single nanofibers. The cellulose nanofiber may have a shape in which a plurality of single nanofibers are entangled. The cellulose nanofiber may have a shape in which a plurality of single nanofibers are assembled in a mesh-like shape. The amorphous portion may be hydrolyzed.
[0030] From the viewpoint of reinforcing effect, the number average fiber diameter of the single nanofiber is preferably 100 nm or less, more preferably 80 nm or less, and particularly preferably 70 nm or less. From the viewpoint of the strength of each single nanofiber, the number average fiber diameter is preferably 3 nm or more, more preferably 5 nm or more, and particularly preferably 10 nm or more. From the viewpoint of reinforcing effect, the number average aspect ratio of the single nanofiber is preferably 10 or more, preferably 20 or more, and particularly preferably 25 or more. The length of the single nanofiber is preferably 100 μm or less.
[0031] Specific examples of cellulose nanofibers include Oji Holdings' product names "AUROVISCO" and "AUROVEIL," Daio Paper's product name "ELLEX," Daiichi Kogyo Seiyaku's product name "RHEOCRYSTA," Nippon Paper Group's product name "cellenpia," and Daicel Miraize's product name "Celish."
[0032] [Vulcanizing agent] The rubber composition may include a vulcanizing agent, such as sulfur, such as powdered sulfur, insoluble sulfur, precipitated sulfur, and colloidal sulfur; and sulfur compounds, such as morpholine disulfide and alkylphenol disulfide.
[0033] In light of the resilience performance of the tennis ball 2, the amount of the vulcanizing agent per 100 parts by mass of the base rubber is preferably at least 0.5 parts by mass, more preferably at least 1.5 parts by mass, and particularly preferably at least 2.0 parts by mass. This amount is preferably at most 6.0 parts by mass, more preferably at most 5.0 parts by mass, and particularly preferably at most 4.5 parts by mass.
[0034] [Vulcanization accelerator] The rubber composition may contain a vulcanization accelerator. Preferred vulcanization accelerators include guanidine-based vulcanization accelerators such as 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, and 1-o-tolylbiguanide; thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, 2-mercaptobenzothiazole cyclohexylamine salt, 2-(N,N-diethylthiocarbamoylthio)benzothiazole, and 2-(4'-morpholinodithio)benzothiazole; N-cyclohexyl-2-benzothiazolyl sulfenamide, N Examples of the vulcanization accelerator include sulfenamide vulcanization accelerators such as N-tert-butyl-2-benzothiazolylsulfenamide, N-oxydiethylene-2-benzothiazolylsulfenamide, and N,N'-dicyclohexyl-2-benzothiazolylsulfenamide; thiuram vulcanization accelerators such as tetraethylthiuram disulfide and tetramethylthiuram monosulfide; and dithiocarbamate vulcanization accelerators such as zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibenzyldithiocarbamate, and tellurium diethyldithiocarbamate. The rubber composition may contain two or more types of vulcanization accelerators.
[0035] In light of the resilience performance of the tennis ball 2, the amount of the vulcanization accelerator per 100 parts by mass of the base rubber is preferably at least 0.5 parts by mass, more preferably at least 1.5 parts by mass, and particularly preferably at least 2.0 parts by mass. This amount is preferably at most 6.0 parts by mass, more preferably at most 5.0 parts by mass, and particularly preferably at most 4.5 parts by mass.
[0036] [Vulcanization aid] The rubber composition may contain a vulcanization accelerator. Preferred vulcanization accelerators include fatty acids such as stearic acid, metal oxides such as zinc oxide, and fatty acid metal salts such as zinc stearate.
[0037] [Reinforcement material] The rubber composition may contain a reinforcing material. An example of the reinforcing material is carbon black. From the viewpoint of the resilience performance of the tennis ball 2, the amount of carbon black per 100 parts by mass of the base rubber is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and particularly preferably 3 parts by mass or more. This amount is preferably 20 parts by mass or less, more preferably 17 parts by mass or less, and particularly preferably 15 parts by mass or less.
[0038] [Filler] The rubber composition may contain a filler. Preferred examples of the filler include silica, calcium carbonate, magnesium carbonate, barium sulfate, talc, kaolin clay, graphite, graphene, bentonite, halloysite, montmorillonite, mica, beidellite, saponite, hectorite, nontronite, vermiculite, illite, and allophane.
[0039] From the standpoint of the physical properties and mass of the tennis ball 2, the amount of the filler per 100 parts by mass of the base rubber is preferably 10 parts by mass or more and 120 parts by mass or less. This amount is more preferably 20 parts by mass or more and particularly preferably 25 parts by mass or more. This amount is more preferably 110 parts by mass or less and particularly preferably 100 parts by mass or less.
[0040] [Other additives] The rubber composition may contain other additives, examples of which include an antiaging agent, an antioxidant, a light stabilizer, a softener, a processing aid, and a colorant.
[0041] [Core properties] From the viewpoint of the balance of the resilience performance, shot feeling, and controllability of the tennis ball 2, the complex modulus E * is preferably 12.0 MPa or more and 18.0 MPa or less. * The complex elastic modulus E is more preferably 13.0 MPa or more, and particularly preferably 13.5 MPa or more. * It is more preferably 17.0 MPa or less, and particularly preferably 16.5 MPa or less.
[0042] From the viewpoint of a balance between the resilience performance, shot feeling, and controllability of the tennis ball 2, the loss tangent tan δ of the rubber composition of the core 4 is preferably 0.050 or more and 0.085 or less. The loss tangent tan δ is more preferably 0.060 or more and particularly preferably 0.065 or more. The loss tangent tan δ is more preferably 0.075 or less and particularly preferably 0.070 or less.
[0043] Complex modulus E * The loss tangent tan δ is measured in accordance with the provisions of JIS K 6394. The measurement conditions are as follows: Initial distortion: 10% Amplitude: 0.05% Frequency: 10Hz Deformation mode: tension Temperature range: -50℃ to +50℃ Heating rate: 4℃ / min Step temperature: 2℃ An example of an apparatus suitable for this measurement is a viscoelasticity spectrometer (product name: "E4000") manufactured by UBM. For the measurement, a test piece obtained from a rubber composition having the same composition as the rubber composition of the core 4 is used. The vulcanization temperature for this test piece is 160°C, and the vulcanization time is 2 minutes. This test piece has a thickness of 2 mm, a width of 4 mm, and a length of 20 mm. The measurement is performed by temperature dispersion, and the complex modulus E at 10°C is* and the loss tangent tan δ is extracted.
[0044] [Manufacturing method] An example of a method for manufacturing the tennis ball 2 will be described below. In this manufacturing method, microfibrillated fibers are added to the latex of the base rubber to obtain a mixed liquid. The mixed liquid is solidified to obtain a master batch. Additives are added to the master batch to obtain a rubber composition. The rubber composition is pressurized and heated in a mold to obtain a half shell. The half shell has a hemispherical shape. The two half shells are bonded together to obtain a spherical core 4. Prior to bonding, a gas generating source may be introduced into the core 4. An example of the gas generating source is a combination of an ammonium salt and a nitrite. Nitrogen gas generated by a chemical reaction between the ammonium salt and the nitrite applies internal pressure to the core 4. Meanwhile, seam glue is applied to the back surface of the dumbbell-shaped felt 6. Two felts 6 are attached to the surface of the core 4 by the adhesive force of the seam glue. The core 4 and felt 6 are introduced into a mold and pressurized and heated to obtain a tennis ball 2. In the core 4 of this tennis ball 2, microfibrillated fibers are uniformly dispersed in the rubber matrix. EXAMPLES
[0045] The effects of the tennis balls according to the examples will be explained below, but the scope of the disclosure in this specification should not be construed as being limited based on the description of these examples.
[0046] [Example 1] The solid content concentration of natural rubber latex (Muhibaratex Co., Ltd.) was adjusted to 30% (w / v). 12.5 g of a 10% aqueous solution of sodium polyoxyethylene lauryl ether sulfate (Kao Corporation's product name "EMAL E-27C") as a surfactant was added to 500 g of this latex. This latex was mixed with a predetermined amount of a 1% aqueous solution of cellulose nanofiber (CNF) to obtain a mixed solution. This mixed solution was put into a cylindrical homogenizer (Primix Corporation's product name "Automixer 20 type") and stirred at a speed of 8000 rpm for 1 hour. 3 g of an antioxidant dispersion was added to this mixed solution and further stirred. While continuing this stirring, a coagulant was gradually added to this mixed solution until the pH reached 4.0, and a coagulant was obtained. This coagulant was squeezed with a water squeeze roll to obtain a sheet. This sheet was kept at a temperature of 70°C for 10 hours to obtain a master batch. The solid content of the cellulose nanofiber was 7.5 parts by mass per 100 parts by mass of natural rubber.
[0047] 100 parts by mass of the masterbatch, calculated as natural rubber, 0.51 parts by mass of stearic acid (NOF Corp. trade name "Tsubaki"), 12 parts by mass of zinc oxide (Seido Chemical Co., Ltd. trade name "Zinc Oxide Type 2"), 5.0 parts by mass of silica (Tosoh Silica Corp. trade name "Nipsil VN3"), 51 parts by mass of kaolin clay, and 15 parts by mass of carbon black (Cabot Japan Corp. trade name "Show Black N330") were charged into a Banbury mixer and kneaded for 5 minutes at a temperature of 90°C to obtain a kneaded product. To this kneaded product, 3.6 parts by mass of sulfur (Sanshin Chemical's product name "Sunfer EX", containing 20% oil), 1.0 part by mass of vulcanization accelerator DPG (Sanshin Chemical's product name "Suncerer D"), 1.0 mass of vulcanization accelerator CZ (Ouchi Shinko Chemical's product name "Noccela CZ"), and 1.88 parts by mass of vulcanization accelerator DM (Ouchi Shinko Chemical's product name "Noccela DM") were added to obtain a rubber composition. Details of the vulcanization accelerators were as follows. DPG: 1,3-diphenylguanidine CZ: N-cyclohexyl-2-benzothiazolyl sulfenamide DM: Di-2-benzothiazolyl disulfide
[0048] This rubber composition was placed in a mold and pressed at 150°C for 4 minutes to obtain a half shell. 0.2g of an ammonium chloride tablet, 0.3g of a sodium nitrite tablet, and 1.5g of water were placed in this half shell. Another half shell was attached to this half shell, which was then placed in a mold and pressed at 150°C for 4 minutes to obtain a core. Two sheets of felt were attached to this core using core glue and felt back glue. This core and felt were placed in a mold and pressed at 135°C for 14 minutes to obtain the tennis ball of Example 1.
[0049] [Examples 2 and 3 and Comparative Example 1] Tennis balls of Examples 2 and 3 and Comparative Example 1 were obtained in the same manner as in Example 1, except that the amounts of cellulose nanofibers (CNF) and carbon black were as shown in Table 1 below.
[0050] [Comparative Example 2] A tennis ball of Comparative Example 2 was obtained in the same manner as in Example 1, except that the rubber composition of the core was as shown in Table 1 below.
[0051] [Core Viscoelasticity] Using the method described above, the complex elastic modulus of the core E * and the loss tangent tan δ were measured, the results of which are shown in Table 1 below.
[0052] [Rate of change of pressure] Tennis balls were stored in a container with a pressure of P1. The container was opened and the tennis balls were kept under the following environment: Pressure: Atmospheric pressure Temperature: 23.4℃ Humidity: 55% The internal pressure P2 of the tennis ball was measured after 28 days. The pressure change rate Pp was calculated based on the following formula: Pp = (P1 - P2) / P1 * 100 The results are shown in Table 1 below.
[0053] [Gas permeability] A rubber composition having the same composition as the rubber composition of the core was prepared. This rubber composition was poured into a mold and vulcanized to obtain a sheet having a thickness of 2 mm. The vulcanization conditions were as follows: Temperature: 160℃ Time: 2 minutes This sheet was subjected to a test based on the differential pressure method specified in "JIS K 7126-1" to measure the gas permeability coefficient (cm 3 cm / cm 2 / sec / cmHg) was measured under the following measurement conditions. Testing machine: GTR Tech's gas permeation testing machine (product name "GTR-30ANI") Sample temperature: 40℃ Measurement cell cross-sectional area: 15.2 cm 2 Differential pressure: 0.2MPa Measurement environment: Room temperature The results are shown in Table 1 below.
[0054] [Return deformation (RD) rate of change] The tennis ball was deformed by 2.54 cm using a Stephens compression tester. The tennis ball was then restored to its original shape until the load reached 80.07 N, and the return deformation D1 was measured. The tennis ball was repeatedly impacted against a metal plate at a speed of 25 m / s. After 500 impacts, the return deformation D2 was measured in the same manner. The rate of change Pd of the return deformation was calculated based on the following formula: Pd = (D2 - D1) / D1 * 100 The results are shown in Table 1 below.
[0055] [Table 1]
[0056] As is clear from Table 1, the tennis balls of the examples are excellent in various performances. The superiority of this tennis ball is clear from these evaluation results.
[0057] [Disclosure items] Each of the following sections discloses a preferred embodiment.
[0058] [Item 1] It has a core and a skin, the core is formed from a rubber composition, The tennis ball, wherein the rubber composition comprises a base rubber and microfibrillated fibers.
[0059] [Item 2] Item 2. The tennis ball of item 1, wherein the microfibrillated fibers are of plant origin.
[0060] [Item 3] 3. The tennis ball according to item 2, wherein the microfibrillated fibers are cellulose nanofibers.
[0061] [Item 4] 4. The tennis ball according to any one of items 1 to 3, wherein the rubber composition comprises 100 parts by mass of a base rubber and 5.0 parts by mass or more and 30.0 parts by mass or less of microfibrillated fibers.
[0062] [Item 5] 5. The tennis ball according to any one of items 1 to 4, wherein the main component of the base rubber is an isoprene-based rubber.
[0063] [Item 6] Item 6. The tennis ball according to item 5, wherein the isoprene-based rubber contains natural rubber, and the proportion of this natural rubber in the total base rubber is 30% by mass or more.
[0064] [Item 7] 7. The tennis ball according to any one of items 1 to 6, wherein the rubber composition has a complex modulus (10 Hz) at 10° C. of 13.5 MPa or greater and 16.5 MPa or less.
[0065] [Item 8] 8. The tennis ball according to any one of items 1 to 7, wherein the rubber composition has a loss tangent (10 Hz) at 10° C. of 0.065 or greater and 0.070 or less.
[0066] [Item 9] (1) A step of adding microfibrillated fibers to rubber latex to obtain a mixed liquid; (2) A step of solidifying the mixture to obtain a master batch. (3) adding additives to the masterbatch to obtain a rubber composition; (4) pressurizing and heating the rubber composition to obtain half shells; (5) bonding the two half shells together to obtain a core; and (6) A process of attaching felt to the surface of the core. The method for manufacturing a tennis ball comprises: [Industrial Applicability]
[0067] The microfibrillated fibers described above are also suitable for pressureless tennis balls. [Explanation of symbols]
[0068] 2. Tennis ball 4. Core 6. Felt 8. Seam 10...hull
Claims
1. It has a core and a skin, the core is formed from a rubber composition, The tennis ball, wherein the rubber composition comprises a base rubber and microfibrillated fibers.
2. 2. The tennis ball of claim 1, wherein the microfibrillated fibers are of plant origin.
3. 3. The tennis ball of claim 2, wherein the microfibrillated fibers are cellulose nanofibers.
4. 4. The tennis ball according to claim 1, wherein the rubber composition comprises 100 parts by weight of a base rubber and at least 5.0 parts by weight but not more than 30.0 parts by weight of the microfibrillated fibers.
5. 4. The tennis ball according to claim 1, wherein the base rubber is primarily made of an isoprene-based rubber.
6. 6. The tennis ball according to claim 5, wherein the isoprene-based rubber contains natural rubber, and the proportion of the natural rubber in the total base rubber is 30% by mass or more.
7. 4. The tennis ball according to claim 1, wherein the rubber composition has a complex modulus at 10° C. (10 Hz) of 13.5 MPa or greater and 16.5 MPa or less.
8. 4. The tennis ball according to claim 1, wherein the rubber composition has a loss tangent (10 Hz) at 10° C. of 0.065 or greater and 0.070 or less.
9. (1) A step of adding microfibrillated fibers to rubber latex to obtain a mixed liquid; (2) A step of solidifying the mixed liquid to obtain a master batch; (3) adding additives to the master batch to obtain a rubber composition; (4) A step of pressurizing and heating the rubber composition to obtain half shells; (5) A step of bonding two half shells together to obtain a core; and (6) A step of attaching felt to the surface of the core The method for manufacturing a tennis ball comprises:
Citation Information
Patent Citations
Rubber composition for tennis balls, and tennis ball
JP2019017996A