Liquid crystal polyester resin composition and molded article composed of the same

The liquid crystal polyester resin composition with controlled milled fibers and specific structural units addresses burr and anisotropy issues, enabling high-quality thin-walled part production.

JP2024168936AInactive Publication Date: 2024-12-05TORAY INDUSTRIES INC

Patent Information

Application Number
JP2023086009
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing liquid crystal polyester resin compositions face issues with molding defects such as burrs and anisotropy when molding thin-walled parts, particularly at elevated temperatures, leading to reduced productivity and poor surface quality.

Method used

A liquid crystal polyester resin composition containing milled fibers with specific average fiber lengths and structural units, controlled through a narrow range of cumulative fiber length ratios, is developed to enhance burr resistance and reduce anisotropy.

Benefits of technology

The composition allows for the production of thin-walled parts with minimal burrs and low anisotropy, improving productivity and surface quality, especially in small electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168936000009
    Figure 2024168936000009
  • Figure 2024168936000001
    Figure 2024168936000001
  • Figure 2024168936000002
    Figure 2024168936000002
Patent Text Reader

Abstract

To provide a liquid crystal polyester resin composition which enables molding of a thin molding component to generate little burrs, and can obtain a molding component having low anisotropy, and a molded article composed of the same.SOLUTION: A liquid crystal polyester resin composition contains a liquid crystal polyester resin (A), and 1 to 100 pts.wt. of a milled fiber (B) with respect to 100 pts.wt. of the liquid crystal polyester resin (A), wherein the liquid crystal polyester resin (A) contains the following structural units (I) to (VI), the liquid crystal polyester resin composition satisfies the following formulae (a) to (e), and an average fiber length of the milled fiber (B) in the liquid crystal polyester resin composition is 1 to 100 μm, (a) 1≤[I]≤20, (c) 2≤[II]+[III]≤35, (b) 25≤[IV]≤75, (d) 2≤[V]≤35, and (e) 0.01≤[VI]≤10. ([I] to [VI] represent contents (mol%) of the following respective structural units (I) to (VI) with respect to 100 mol% of the total structural units of the liquid crystal polyester resin (A).)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid crystal polyester resin composition and a molded article made of the same. More specifically, the present invention relates to a liquid crystal polyester resin composition and a molded article obtained by using the same. [Background technology]

[0002] Liquid crystal polyester resins are used in electrical and electronic components that require these properties because they have excellent heat resistance, fluidity, and dimensional stability. In recent years, such electrical and electronic components have become thinner and more complex in shape as devices become smaller and lighter. In particular, thin and complex molded parts require high rigidity, and liquid crystal polyester resin compositions containing a wide variety of fillers have been proposed. However, general fibrous fillers cause the smoothness of the molded product surface to deteriorate and molding shrinkage occurs due to the orientation of the filler. Therefore, in order to improve molding shrinkage and the smoothness of the molded product surface, liquid crystal polyester resin compositions containing inorganic fillers and having a specified bending modulus (for example, Patent Document 1), liquid crystal polyester resin compositions containing fibrous fillers with a specified weight average fiber length (for example, Patent Document 2), and liquid crystal polyester resin compositions containing fibrous fillers and having a specified bending modulus (for example, Patent Document 3) have been disclosed. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-104527 A [Patent Document 2] JP 2018-104506 A [Patent Document 3] Special Publication No. 2016-523291 Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the inventions shown in Patent Documents 1 to 3, when injection molding is performed at a temperature higher than the recommended conditions for each resin to mold thin-walled molded parts such as precision connectors, the phenomenon of resin overflowing from gaps in the mating surfaces of the mold or gaps in ejector pins, etc., so-called burrs are generated, which causes defective products and reduces productivity. In addition, liquid crystal polyester resin has a molecular structure that is rigid and difficult to bend, and since there is little entanglement of the molecules, they are oriented in the MD direction (flow direction) by a slight shear stress, and a strength difference occurs in the MD / TD (flow direction / transverse direction), which causes a problem of large anisotropy. An object of the present invention is to provide a liquid crystal polyester resin composition which can be molded into thin molded parts with little burrs and has low anisotropy, and a molded article made from the same. [Means for solving the problem]

[0005] As a result of intensive research to solve the above problems, the present inventors have found that the above problems can be solved by a liquid crystal polyester resin composition containing a milled fiber having a specific average fiber length for a liquid crystal polyester resin having a specific structural unit, and have arrived at the present invention. That is, the present invention has the following configuration. (1) A liquid crystal polyester resin composition comprising a liquid crystal polyester resin (A) and 1 to 100 parts by weight of milled fibers (B) per 100 parts by weight of the liquid crystal polyester resin (A), wherein the liquid crystal polyester resin (A) is a liquid crystal polyester resin comprising the following structural units (I) to (VI), and satisfies the following formulae (a) to (e), and the milled fibers (B) have an average fiber length of 1 to 100 μm in the liquid crystal polyester resin composition. 1≦[I]≦20 (a) 2≦[II]+[III]≦35 (c) 25≦[IV]≦75 (b) 2≦[V]≦35 (d) 0.01≦[VI]≦10 (e) ([I] to [VI] indicate the contents (mol %) of the following structural units (I) to (VI) relative to 100 mol % of all structural units in the liquid crystal polyester resin (A).)

[0006] [ka]

[0007] (2) The liquid crystal polyester resin composition according to (1), wherein the [V] and [VI] satisfy the following formula (f): 0.003≦([VI] / [V])≦0.15···(f) (3) The liquid crystal polyester resin composition according to (1) or (2), characterized in that the ratio (D85 / D15) of the 85% cumulative fiber length (D85) to the 15% cumulative fiber length (D15) obtained from the cumulative fiber length distribution curve of the milled fiber (B) is 2.0 to 4.0. (4) A molded article comprising the liquid crystal polyester resin composition according to any one of (1) to (3). (5) The molded article according to (4), which is any one selected from the group consisting of a connector, a coil bobbin, a lens holding part of a camera module, and an actuator part of a camera module. Effect of the Invention

[0008] The liquid crystal polyester resin composition of the present invention can be molded into thin molded parts with little flash and can obtain molded parts with low anisotropy. In particular, it can be suitably used when molding small electric and electronic parts. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a diagram showing an example of a cumulative fiber length distribution curve of milled fiber (B). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below.

[0011] <Liquid crystal polyester resin (A)> The liquid crystal polyester resin is a polyester that forms an anisotropic molten phase. Examples of such polyester resins include polyesters composed of structural units selected from oxycarbonyl units, dioxy units, dicarbonyl units, etc., which will be described later, so as to form an anisotropic molten phase. Next, the structural units constituting the liquid crystal polyester resin will be described.

[0012] The liquid crystal polyester resin (A) used in the present invention is characterized in that it contains, as an oxycarbonyl unit, the following structural unit (I) derived from 6-hydroxy-2-naphthoic acid, in an amount of 1 to 20 mol% relative to 100 mol% of all structural units of the liquid crystal polyester resin (A). The structural unit (I) has a naphthalene ring structure, and has a slightly longer molecular chain length and a slightly curved structure compared to monomers having a benzene ring, such as p-hydroxybenzoic acid, terephthalic acid, and hydroquinone, which will be described later. This makes it possible to suppress the molecular chain of the liquid crystal polyester resin from being tightly packed while maintaining liquid crystallinity. In addition, since the packing property can be reduced while maintaining liquid crystallinity, even thin-walled molded parts are improved in burr prevention, productivity is improved, and low anisotropy is achieved. In addition, as described above, the structural unit (I) bends the molecular chain, so that the molecular chains of the liquid crystal polyester resin can be moderately entangled with each other during melt kneading, and the apparent viscosity increases, so that it becomes easy to control the average fiber length of the milled fiber (B) within a specific range and to control the ratio (D85 / D15) of the 85% cumulative fiber length (D85) to the 15% cumulative fiber length (D15) obtained from the cumulative fiber length distribution curve of the milled fiber within a preferred range. The structural unit (I) is preferably 2 mol% or more, more preferably 3 mol% or more, based on 100 mol% of all structural units of the liquid crystal polyester resin (A). The structural unit (I) is preferably 15 mol% or less, more preferably 10 mol% or less.

[0013] [ka]

[0014] From the viewpoint of improving flash prevention and anisotropy even in a thin molded part, the liquid crystal polyester resin (A) of the present invention contains, as an oxycarbonyl unit, 25 to 75 mol % of the structural unit (IV) derived from p-hydroxybenzoic acid relative to 100 mol % of all structural units of the liquid crystal polyester resin (A). It is preferably 30 mol % or more, more preferably 40 mol % or more, and even more preferably 45 mol % or more. On the other hand, it is preferably 65 mol % or less, more preferably 50 mol % or less, and even more preferably 55 mol % or less.

[0015] [ka]

[0016] In order to improve flash resistance and anisotropy even in thin molded parts, the liquid crystal polyester resin (A) of the present invention contains, as dioxy units, the following structural unit (II) derived from hydroquinone and the structural unit (III) derived from 4,4'-dihydroxybiphenyl in a total amount of 2 to 35 mol% relative to 100 mol% of all structural units of the liquid crystal polyester resin (A). The total amount of the structural units (II) and (III) is preferably 3 mol% or more, more preferably 8 mol% or more, and even more preferably 13 mol% or more. The total amount of the structural units (II) and (III) is preferably 20 mol% or less, more preferably 17 mol% or less, and even more preferably 15 mol% or less.

[0017] [ka]

[0018] The structural unit (II) is preferably 2 mol% or more, more preferably 5 mol% or more, and even more preferably 8 mol% or more, based on 100 mol% of all structural units in the liquid crystal polyester resin (A). The structural unit (II) is preferably 20 mol% or less, more preferably 17 mol% or less, and even more preferably 15 mol% or less.

[0019] Furthermore, from the viewpoint of improving flash prevention and anisotropy even in a thin molded part, the aromatic diol preferably contains 1 to 25 mol % of structural units (III) derived from 4,4'-dihydroxybiphenyl relative to 100 mol % of all structural units of the liquid crystal polyester resin (A). More preferably, it is 3 mol % or more, and even more preferably, it is 5 mol % or more. On the other hand, it is more preferably 20 mol % or less, and even more preferably, it is 15 mol % or less.

[0020] In order to improve flash prevention and anisotropy even in a thin molded part, the liquid crystal polyester resin (A) of the present invention contains, as dicarbonyl units, 2 to 35 mol % of structural units (V) derived from terephthalic acid relative to 100 mol % of all structural units of the liquid crystal polyester resin (A). It is preferably 5 mol % or more, more preferably 10 mol % or more, and even more preferably 15 mol % or more. On the other hand, it is preferably 30 mol % or less, more preferably 25 mol % or less.

[0021] [ka]

[0022] The liquid crystal polyester resin (A) of the present invention contains 0.01 to 10 mol % of structural units (VI) derived from isophthalic acid relative to 100 mol % of all structural units of the liquid crystal polyester resin (A) in order to improve flash resistance and anisotropy even in thin molded parts. Isophthalic acid has carboxyl groups at the 1st and 3rd positions of the benzene ring, and has a significantly curved structure compared to other monomers with high linearity. This makes it possible to suppress the molecular chains of the liquid crystal polyester resin from packing tightly, thereby improving flash resistance and low anisotropy even in thin molded parts. 0.05 mol % or more is preferable, and 0.1 mol % or more is more preferable. On the other hand, 8 mol % or less is preferable, 6 mol % or less is more preferable, and 4 mol % or more is even more preferable.

[0023] [ka]

[0024] From the viewpoint of improving flash prevention and anisotropy even in thin-walled molded parts, the liquid crystal polyester resin (A) of the present invention preferably satisfies the following formula (f). 0.003≦([VI] / [V])≦0.15···(f) From the viewpoint of improving flash resistance and anisotropy even in thin-walled molded parts, [VI] / [V] is more preferably 0.02 or more, and even more preferably 0.03 or more. On the other hand, from the viewpoint of improving flash resistance and anisotropy even in thin-walled molded parts, [VI] / [V] is more preferably 0.12 or less, and even more preferably 0.10 or less.

[0025] In addition to the above structural units, structural units derived from ethylene glycol, p-aminobenzoic acid, p-aminophenol, etc. may be contained within the range that does not impair the liquid crystallinity or other characteristics.

[0026] The monomers serving as raw materials for forming each of the structural units described above are not particularly limited as long as they have a structure capable of forming each of the structural units. In addition, acylation products of the hydroxyl groups of such monomers, esterification products of the carboxyl groups, acid halides, acid anhydrides and other carboxylic acid derivatives may be used.

[0027] The method for calculating the content of each structural unit in the liquid crystal polyester resin (A) is shown below. The content of each structural unit is determined by 1H-nuclear magnetic resonance spectrum (1H-NMR) measurement. 5 mg of the ground component (A) is weighed and dissolved in 800 μL of a solvent (pentafluorophenol / 1,1,2,2-tetrachloroethane-d2 = 65 / 35 (weight ratio) mixed solvent), and 1H-NMR measurement is performed at an observation frequency of 500 MHz and a temperature of 80 ° C. using a UNITY INOVA500 NMR device (manufactured by Varian Inc.), and the composition is analyzed from the peak area ratio derived from each structural unit observed around 7 to 9.5 ppm.

[0028] The melting point (Tm) of the liquid crystal polyester resin (A) is preferably 280°C or higher, more preferably 300°C or higher, and even more preferably 320°C or higher. On the other hand, the melting point (Tm) of the liquid crystal polyester resin (A) is preferably 370°C or lower, more preferably 360°C or lower, and even more preferably 350°C or lower. The melting point (Tm) is measured by differential scanning calorimetry. Specifically, first, the liquid crystal polyester resin (A) is heated from room temperature at a temperature rise rate of 20°C / min to observe the endothermic peak temperature (Tm1). After observing the endothermic peak temperature (Tm1), the polymer is held at a temperature of endothermic peak temperature (Tm1) + 20°C for 5 minutes. Then, the polymer is cooled to room temperature at a temperature drop rate of 20°C / min. Then, the polymer is heated at a temperature rise rate of 20°C / min to observe the endothermic peak temperature (Tm2). The melting point (Tm) refers to the endothermic peak temperature (Tm2).

[0029] The melt viscosity of the liquid crystal polyester resin is preferably 3 Pa·s or more, more preferably 5 Pa·s or more, and even more preferably 10 Pa·s or more, from the viewpoint of easily controlling the viscosity within a preferred range during production of a liquid crystal polyester resin composition described later. On the other hand, from the viewpoint of easily controlling the viscosity within a preferred range during production of a liquid crystal polyester resin composition described later and improving the fluidity, the melt viscosity of the liquid crystal polyester resin is preferably 50 Pa·s or less, preferably 40 Pa·s or less, and even more preferably 30 Pa·s or less.

[0030] The melt viscosity is a value measured by a Koka type flow tester at a temperature of the melting point (Tm) of the liquid crystal polyester resin + 20° C. under the condition of a shear rate of 1000 / sec.

[0031] <Method for producing liquid crystal polyester resin (A)> The method for producing the liquid crystal polyester resin (A) used in the present invention is not particularly limited, and can be produced in accordance with a known polyester polycondensation method. Examples of known polyester polycondensation methods include the following, for example, liquid crystal polyester resin (A) consisting of a structural unit derived from p-hydroxybenzoic acid, a structural unit derived from 6-hydroxy-2-naphthoic acid, a structural unit derived from 4,4'-dihydroxybiphenyl, a structural unit derived from hydroquinone, and a structural unit derived from terephthalic acid and isophthalic acid.

[0032] (1) A method for producing a liquid crystal polyester resin (A) from p-acetoxybenzoic acid, 6-acetoxy-2-naphthoic acid, 4,4'-diacetoxybiphenyl, diacetoxybenzene, terephthalic acid, and isophthalic acid by a deacetic acid condensation polymerization reaction.

[0033] (2) A method for producing a liquid crystal polyester resin (A) by reacting p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 4,4'-dihydroxybiphenyl, hydroquinone, terephthalic acid, and isophthalic acid with acetic anhydride to acetylate the phenolic hydroxyl groups, followed by deacetylation polymerization.

[0034] (3) A method for producing a liquid crystal polyester resin (A) by a dephenolation polycondensation reaction of phenyl p-hydroxybenzoate, phenyl 6-hydroxy-2-naphthoate, 4,4'-dihydroxybiphenyl, hydroquinone, diphenyl terephthalate, and diphenyl isophthalate.

[0035] (4) A method in which a predetermined amount of diphenyl carbonate is reacted with aromatic carboxylic acids, such as p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, terephthalic acid, and isophthalic acid, to form the phenyl esters, respectively, and then an aromatic dihydroxy compound, such as 4,4'-dihydroxybiphenyl or hydroquinone, is added to carry out a dephenolation polycondensation reaction to produce a liquid crystal polyester resin (A).

[0036] Among these, the method (2) of reacting p-hydroxybenzoic acid, 4,4'-dihydroxybiphenyl, hydroquinone, terephthalic acid, and isophthalic acid with acetic anhydride to acetylate the phenolic hydroxyl groups, followed by a deacetylase polycondensation reaction to produce the liquid crystal polyester resin (A) is preferably used because it is industrially excellent in controlling the terminal structure and the degree of polymerization of the liquid crystal polyester resin (A).

[0037] As a method for producing the liquid crystal polyester resin (A) used in the present invention, it is also possible to complete the polycondensation reaction by a solid-phase polymerization method. Examples of the treatment by the solid-phase polymerization method include the following method. First, the polymer or oligomer of the liquid crystal polyester resin (A) is pulverized by a pulverizer. The pulverized polymer or oligomer is heated under a nitrogen stream or reduced pressure to polycondense to a desired degree of polymerization, thereby completing the reaction. The heating can be performed for 1 to 50 hours at a temperature in the range of the melting point of the liquid crystal polyester resin (A) -50°C to the melting point -5°C (for example, 200 to 300°C).

[0038] <Milled Fiber (B)> The liquid crystal polyester resin composition of the present invention is characterized in that it contains 1 to 100 parts by weight of milled fiber (B) per 100 parts by weight of liquid crystal polyester resin (A). From the viewpoint of improving flash and anisotropy even in thin molded parts, it is preferably 5 parts by weight or more, more preferably 10 parts by weight or more, and even more preferably 15 parts by weight or more. From the viewpoint of heat resistance and low anisotropy while improving flash even in thin molded parts, it is preferably 80 parts by weight or less, more preferably 60 parts by weight or less, and even more preferably 50 parts by weight or less.

[0039] The milled fiber (B) in the present invention has an average fiber length in the liquid crystal polyester resin composition of 1 to 100 μm. From the viewpoint of improving burr prevention and low anisotropy even in thin molded parts, the average fiber length is preferably 5 μm or more, more preferably 15 μm or more. On the other hand, from the viewpoint of improving burr prevention and anisotropy even in thin molded parts, the average fiber length is preferably 80 μm or less, more preferably 60 μm or less.

[0040] Furthermore, from the viewpoint of improving flash resistance and anisotropy even in thin-walled molded parts, it is preferable that the milled fiber (B) has a distribution with little variation in fiber length. Specifically, the ratio (D85 / D15) of the 85% cumulative fiber length (D85) to the 15% cumulative fiber length (D15) obtained from the cumulative fiber length distribution curve is more preferably in the range of 2.0 to 4.0, and even more preferably 2.5 to 3.5.

[0041] The average fiber length, 85% cumulative fiber length (D85) and 15% cumulative fiber length (D15) of the milled fiber (B) can be determined by the following method. 50 g of the liquid crystal polyester resin composition is heated in air at 550°C for 3 hours to remove the resin component, and the residue remaining as a non-combustible material is used as the milled fiber. 1000 remaining milled fibers are randomly selected using an optical microscope, and the fiber length is measured at a magnification of 120 times (manufactured by Inotec, "Quick Grain Standard"), and a cumulative fiber length distribution curve is calculated. The cumulative fiber length of 50% cumulative fiber length (D50) obtained from the cumulative fiber length distribution curve is used as the average fiber length of the milled fiber (B). The cumulative fiber length of 85% cumulative fiber length obtained from the cumulative fiber length distribution curve is used as D85, and the cumulative fiber length of 15% cumulative fiber length is used as D15.

[0042] FIG. 1 shows a schematic diagram of the cumulative fiber length distribution curve of the milled fiber (B). The horizontal axis shows the fiber length (μm) expressed in common logarithm, and the vertical axis shows the cumulative frequency (%) of the milled fiber corresponding to each fiber length. In FIG. 1, the average fiber length is point 3, the cumulative fiber length of 85% (D85) is point 2, and the cumulative fiber length of 15% (D15) is point 4. When the fiber length distribution is measured for a composition containing milled fiber in a known liquid crystal polyester resin as a general liquid crystal polyester resin composition, for example, the ratio (D85 / D15) of the cumulative fiber length of 85% (D85) to the cumulative fiber length of 15% (D15) exceeds 4.0. This result is considered to be due to the fact that in the case of a known liquid crystal polyester resin composition, the distribution width of the fiber length becomes wider due to breakage of the milled fiber caused by melt kneading, and the large fiber length side, which is the fiber length before melt kneading of the milled fiber, remains to a certain extent, and the distribution of the large fiber length side becomes wider.

[0043] The milled fiber used as component (B) in the present invention is preferably E glass, which has a low content of alkaline components, from the viewpoint of improving dispersibility in the resin of the liquid crystalline polyester resin composition of the present invention, but C glass, which contains alkaline components, can also be used.

[0044] The milled fiber used in the present invention may be surface-treated with a coupling agent. Specifically, the fiber may be coupled with a silane coupling agent such as γ-(2-aminoethyl)aminopropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, methyltrimethoxysilane, γ-anilinopropyltrimethoxysilane, hydroxypropyltrimethoxysilane, γ-ureidopropyltriethoxysilane, or vinylacetoxysilane; a titanium coupling agent such as isopropyltrisisostearoyltitanate, isopropyltris(dioctylpyrophosphate)titanate, tetraoctylbis(ditridecylphosphite)titanate, bis(dioctylpyrophosphate)ethylenetitanate, isopropyltridecylbenzenesulfonyltitanate, or isopropyltri(dioctylphosphate)titanate; or an aluminum coupling agent such as acetoalkoxyaluminumdiisopropylate.

[0045] During injection molding of the liquid crystal polyester resin composition, the milled fiber (B) is oriented in the longitudinal direction along the flow direction of the liquid crystal polyester resin (A). At this time, while controlling the milled fiber to the specific blending amount described above, in particular by controlling the ratio (D85 / D15) of the cumulative fiber length distribution curve of the milled fiber to the cumulative fiber length distribution curve of the 85% cumulative fiber length (D85) and the cumulative fiber length (D15) of the 15% cumulative fiber length, the liquid crystal polyester resin (A) can be oriented not only in the longitudinal direction but also in the transverse direction. As a result, the flow direction of the liquid crystal polyester resin in the molding die is diverse, and even a thin molded part can be molded at low pressure. In particular, by combining with the liquid crystal polyester resin (A) containing all of the structural units (I) to (VI), the low anisotropy is improved while improving the flash property specifically.

[0046] The ratio (D85 / D15) of the 85% cumulative fiber length (D85) to the 15% cumulative fiber length (D15), obtained from the cumulative fiber length distribution curve of the milled fiber (B) of the present invention, can be adjusted to the aforementioned range by suppressing breakage of the filler and preventing the range from expanding in the fiber length distribution. Examples of such a method include using a liquid crystal polyester resin having low shear rate dependency and consisting of the structural units (I) to (VI) described above, adjusting the average fiber length of the milled fiber to the above specific range so that the fiber length range does not expand even if the fiber breaks, and using a preferred method in the production of a liquid crystal polyester resin composition described below.

[0047] <Other additives> The liquid crystal polyester resin composition of the present invention contains the liquid crystal polyester resin (A) and the milled fiber (B) described above, but may contain other fillers to impart other properties. The fillers used in the present invention are not particularly limited, and examples thereof include fibrous, whisker-like, plate-like, powdery, and granular fillers. Specifically, examples of fibrous and whisker-like fillers include chopped glass fiber, long fiber glass fiber, PAN-based or pitch-based carbon fiber, stainless steel fiber, metal fibers such as aluminum fiber and brass fiber, organic fibers such as aromatic polyamide fiber, gypsum fiber, ceramic fiber, asbestos fiber, zirconia fiber, alumina fiber, silica fiber, titanium oxide fiber, silicon carbide fiber, rock wool, potassium titanate whisker, barium titanate whisker, aluminum borate whisker, silicon nitride whisker, and needle-shaped titanium oxide. Examples of plate-like fillers include mica, talc, kaolin, glass flakes, clay, molybdenum disulfide, and wollastonite. Examples of powdery or granular fillers include silica, glass beads, titanium oxide, zinc oxide, calcium polyphosphate, and graphite. The above fillers used in the present invention may have their surfaces treated with a known coupling agent (e.g., a silane coupling agent, a titanate coupling agent, etc.) or other surface treatment agent. In addition, two or more of the above fillers used in the present invention may be used in combination.

[0048] On the other hand, in the liquid crystal polyester resin composition of the present invention, if the content of the filler is too high, the fluidity may deteriorate, which may cause deterioration of anisotropy. The content of the filler is preferably 5 parts by weight or less, more preferably 3 parts by weight or less, based on 100 parts by weight of the liquid crystal polyester resin.

[0049] The liquid crystal polyester resin composition of the present invention may further contain conventional additives selected from antioxidants, heat stabilizers (e.g., hindered phenols, phosphites, thioethers, and their substitutes), ultraviolet absorbers (e.g., resorcinol, salicylate), color inhibitors such as phosphites and hypophosphites, lubricants and mold release agents (montanic acid and its metal salts, its esters, its half esters, stearyl alcohol, stearamide, and polyethylene wax), colorants including dyes or pigments, conductive agents or colorants such as carbon black, crystal nucleating agents, plasticizers, flame retardants (bromine-based flame retardants, phosphorus-based flame retardants, red phosphorus, silicone-based flame retardants, and the like), flame retardant assistants, and antistatic agents, within the scope of the present invention.

[0050] <Method of producing liquid crystal polyester resin composition> Examples of methods for blending milled fiber (B) and other additives with liquid crystal polyester resin (A) to prepare a liquid crystal polyester resin composition include a dry blend method in which milled fiber (B) and other solid additives are blended with liquid crystal polyester resin (A), a solution blending method in which milled fiber (B) and other liquid additives are blended with liquid crystal polyester resin (A), a method in which milled fiber (B) and other additives are added during polymerization of liquid crystal polyester resin (A), and a method in which milled fiber (B) and other additives are melt-kneaded with liquid crystal polyester resin (A), and among these, the melt-kneading method is preferred.

[0051] The melt kneading can be carried out by a known method, such as a Banbury mixer, a rubber roll machine, a kneader, a single-screw or twin-screw extruder, etc. Among them, a twin-screw extruder is preferable.

[0052] A manufacturing method for controlling the average fiber length of the milled fiber (B) of the present invention within a specific range and controlling the ratio (D85 / D15) of the 85% cumulative fiber length (D85) to the 15% cumulative fiber length (D15), obtained from the cumulative fiber length distribution curve of the milled fiber, within the above-mentioned preferred range will be described below.

[0053] From the viewpoint of controlling the average fiber length of the milled fiber (B) to a specific range and controlling the ratio (D85 / D15) of the cumulative fiber length at 85% (D85) to the cumulative fiber length at 15% (D15) obtained from the cumulative fiber length distribution curve of the milled fiber to the above-mentioned preferred range, the method of melt kneading using a twin-screw extruder is preferred as a method of producing the liquid crystal polyester resin of the present invention. Among them, a method of melt kneading using a twin-screw extruder with L / D>30, where L is the screw length and D is the screw diameter, is particularly preferred. The screw length here refers to the length from the position where the raw material is supplied at the base of the screw to the tip of the screw. The upper limit of L / D of the twin-screw extruder is 150, and preferably, an extruder with L / D exceeding 30 and not exceeding 100 can be used.

[0054] From the viewpoint of controlling the ratio (D85 / D15) of the 85% cumulative fiber length (D85) to the 15% cumulative fiber length (D15) obtained from the cumulative fiber length distribution curve of the milled fiber (B) within the above-mentioned preferred range, the set temperature of the cylinder of the extruder during melt kneading is preferably set in the range of the melting point of the liquid crystal polyester resin (A) +15 to +30° C. The lower the set temperature, the higher the shear heat generated in the extruder, causing excessive breakage of the milled fiber, widening the fiber length distribution width, and leaving a certain amount of the large fiber length side indicating the fiber length of the milled fiber before melt kneading, thereby increasing the ratio (D85 / D15) of the 85% cumulative fiber length (D85) to the 15% cumulative fiber length (D15) obtained from the cumulative fiber length distribution curve of the milled fiber.

[0055] It is also preferable to melt-knead at a temperature at which the liquid crystal polyester resin composition has a melt viscosity of 3 to 50 Pa s, measured under conditions of a shear rate of 1000 / sec. Melt-kneading at a temperature at which such a melt viscosity is obtained makes it easy to control the average fiber length of the milled fiber (B) within a specific range and to control the ratio (D85 / D15) of the 85% cumulative fiber length (D85) to the 15% cumulative fiber length (D15), obtained from the cumulative fiber length distribution curve of the milled fiber, within the above-mentioned preferred range.

[0056] <Molded products> The liquid crystal polyester resin composition of the present invention can be processed into a molded product having excellent surface appearance (color tone), mechanical properties, and heat resistance by a molding method such as ordinary injection molding, extrusion molding, press molding, solution cast film formation, and spinning. The molded product here includes injection molded products, extrusion molded products, press molded products, sheets, pipes, various films such as unstretched films, uniaxially stretched films, and biaxially stretched films, and various fibers such as unstretched yarns and ultrastretched yarns. In particular, injection molding is preferable from the viewpoint of processability. When melt molding, it is preferable to melt mold at 370 ° C or less, and more preferably 360 ° C or less, from the viewpoint of suppressing deterioration of the liquid crystal polyester resin composition and improving mechanical strength.

[0057] The molded article obtained by molding the liquid crystal polyester resin composition of the present invention can be preferably used as an electric / electronic part. Examples of electric / electronic parts include flexible printed circuit boards, laminated circuit boards, printed wiring boards, and three-dimensional circuit boards used in antennas of mobile communication / electronic devices such as personal computers, GPS-equipped devices, mobile phones, and millimeter wave and quasi-millimeter wave radars such as collision prevention radars, tablets, and smartphones; lamp reflectors and lamp sockets such as LEDs, communication base station small cells and microcell members of mobile communication terminals, antenna covers, housings, sensors, lens holding parts of camera modules, actuator parts of camera modules, connectors, relay cases and bases, switches, coil bobbins, and capacitors. Among them, when thin-walled molded parts are injection molded under the recommended temperature conditions for each resin, the resin is filled with fluidity and low molding pressure, and the anisotropy does not deteriorate, and even when injection molded at a temperature higher than the recommended conditions for each resin, the burr property can be improved, so that it is useful for connectors, coil bobbins, lens holding parts of camera modules, and actuator parts of camera modules having thin-walled shapes. EXAMPLES

[0058] The present invention will be described below using examples, but the present invention is not limited to these examples. The composition and characteristics of the liquid crystal polyester resin (A) shown in the production examples in Table 1 were measured by the following methods.

[0059] (1) Composition analysis of liquid crystal polyester resin (A) The composition of the liquid crystal polyester resin (A) was analyzed by 1H-nuclear magnetic resonance spectroscopy (1H-NMR). 5 mg of the ground component (A) was weighed and dissolved in 800 μL of a solvent (pentafluorophenol / 1,1,2,2-tetrachloroethane-d2 = 65 / 35 (weight ratio) mixed solvent), and 1H-NMR measurement was performed at an observation frequency of 500 MHz and a temperature of 80 ° C. using a UNITY INOVA500 NMR device (manufactured by Varian Inc.). The composition was analyzed from the peak area ratio derived from each structural unit observed around 7 to 9.5 ppm.

[0060] (2) Melting point (Tm) measurement of liquid crystal polyester resin (A) Using a differential scanning calorimeter DSC-7 (PerkinElmer), the liquid crystal polyester resin (A) was heated from room temperature at a temperature increase rate of 20°C / min to observe the endothermic peak temperature (Tm1), and then held at a temperature of Tm1+20°C for 5 minutes. The resin was then cooled to room temperature at a temperature decrease rate of 20°C / min, and the endothermic peak temperature observed when the resin was heated again at a temperature increase rate of 20°C / min was determined as the melting point (Tm).

[0061] (3) Melt viscosity of liquid crystal polyester resin The melt viscosity of the liquid crystal polyester resin was measured at Tm+20° C. and a shear rate of 1000 / sec using a high-performance flow tester CFT-500D (orifice 0.5φ×10 mm) (manufactured by Shimadzu Corporation).

[0062] The production examples of the liquid crystal polyester resin (A) or other liquid crystal polyester resin (a) used in the examples and comparative examples will be described below.

[0063] [Production Example 1] In a 5L reaction vessel equipped with an agitator and a distillation tube, 808 parts by weight of p-hydroxybenzoic acid (HBA), 88 parts by weight of 6-hydroxy-2-naphthoic acid (HNA), 229 parts by weight of 4,4'-dihydroxybiphenyl (DHB), 161 parts by weight of hydroquinone (HQ), 428 parts by weight of terephthalic acid (TPA), 19 parts by weight of isophthalic acid (IPA) and 1278 parts by weight of acetic anhydride (1.07 equivalents of phenolic hydroxyl groups in total) were charged as monomers, and reacted at 145°C for 120 minutes while stirring under a nitrogen gas atmosphere, and then the temperature was raised from 145°C to 360°C over 4 hours. Thereafter, the polymerization temperature was maintained at 360°C, the pressure was reduced to 1.0 mmHg (133 Pa) over 1.0 hour, and the reaction was continued until the polymerization was completed when a predetermined stirring torque was reached. Next, the polymer was extruded in a strand shape through a die having one circular extrusion orifice with a diameter of 6 mm, and pelletized with a cutter to obtain a liquid crystal polyester resin (A-1). When the composition of this liquid crystal polyester resin (A-1) was analyzed, the ratio of structural units derived from p-hydroxybenzoic acid was 50.0 mol%, the ratio of structural units derived from 6-hydroxy-2-naphthoic acid was 4.0 mol%, the ratio of structural units derived from 4,4'-dihydroxybiphenyl was 10.5 mol%, the ratio of structural units derived from hydroquinone was 12.5 mol%, the ratio of structural units derived from terephthalic acid was 22.0 mol%, and the ratio of structural units derived from isophthalic acid was 1.00 mol%. The total of the structural units derived from 4,4'-dihydroxybiphenyl and the structural units derived from hydroquinone was 23.0 mol% relative to the total structural units of the polyester (100 mol%). In addition, the ratio of structural units derived from terephthalic acid to structural units derived from isophthalic acid was 0.045. Furthermore, the Tm was 332°C and the melt viscosity was 22 Pa·sec.

[0064] [Production Example 2] A liquid crystal polyester resin (A-2) was obtained in the same manner as in Example 1, except that the monomer charge was changed to HBA 905 parts by weight, HNA 88 parts by weight, DHB 109 parts by weight, HQ 193 parts by weight, TPA 321 parts by weight, and IPA 68 parts by weight. When the composition of this liquid crystal polyester resin (A-2) was analyzed, the ratio of structural units derived from p-hydroxybenzoic acid was 56.0 mol%, the ratio of structural units derived from 6-hydroxy-2-naphthoic acid was 4.0 mol%, the ratio of structural units derived from 4,4'-dihydroxybiphenyl was 5.0 mol%, the ratio of structural units derived from hydroquinone was 15.0 mol%, the ratio of structural units derived from terephthalic acid was 16.5 mol%, and the ratio of structural units derived from isophthalic acid was 3.50 mol%. The total of the structural units derived from 4,4'-dihydroxybiphenyl and the structural units derived from hydroquinone was 20.0 mol% relative to 100 mol% of the total structural units of the polyester. The ratio of structural units derived from terephthalic acid to structural units derived from isophthalic acid was 0.212, and the Tm and melt viscosity were 335°C and 22 Pa·sec, respectively.

[0065] [Production Example 3] A liquid crystal polyester resin (a-3) was obtained in the same manner as in Example 1, except that the monomer charge was changed to HBA 870 parts by weight, DHB 352 parts by weight, HQ 89 parts by weight, TPA 292 parts by weight, and IPA 157 parts by weight. When the composition analysis was performed on this liquid crystal polyester resin (a-3), the ratio of structural units derived from p-hydroxybenzoic acid was 53.8 mol%, the ratio of structural units derived from 4,4'-dihydroxybiphenyl was 16.9 mol%, the ratio of structural units derived from hydroquinone was 6.2 mol%, the ratio of structural units derived from terephthalic acid was 15.0 mol%, and the ratio of structural units derived from isophthalic acid was 8.08 mol%. The total of structural units derived from 4,4'-dihydroxybiphenyl and structural units derived from hydroquinone was 23.1 mol% relative to the total structural units of polyester (100 mol%). In addition, the ratio of structural units derived from terephthalic acid to structural units derived from isophthalic acid was 0.538. Furthermore, the Tm was 310°C and the melt viscosity was 24 Pa·sec.

[0066] [Production Example 4] A liquid crystal polyester resin (a-4) was obtained in the same manner as in Example 1, except that the monomer charge was changed to HBA 970 parts by weight, DHB 436 parts by weight, TPA 292 parts by weight, and IPA 97 parts by weight. When the composition analysis was performed on this liquid crystal polyester resin (a-4), the ratio of structural units derived from p-hydroxybenzoic acid was 60.0 mol%, the ratio of structural units derived from 4,4'-dihydroxybiphenyl was 20.0 mol%, the ratio of structural units derived from terephthalic acid was 15.0 mol%, and the ratio of structural units derived from isophthalic acid was 5.00 mol%. The ratio of structural units derived from terephthalic acid to structural units derived from isophthalic acid was 0.333. Furthermore, Tm was 339°C, and the melt viscosity was 23 Pa·sec.

[0067] [Production Example 5] A liquid crystal polyester resin (a-5) was obtained in the same manner as in Example 1, except that the monomer charge was changed to HBA 970 parts by weight, DHB 261 parts by weight, HQ 203 parts by weight, TPA 292 parts by weight, and IPA 97 parts by weight. When the composition analysis was performed on this liquid crystal polyester resin (a-5), the ratio of the structural unit derived from p-hydroxybenzoic acid was 60.0 mol, the ratio of the structural unit derived from 4,4'-dihydroxybiphenyl was 12.0 mol%, the ratio of the structural unit derived from hydroquinone was 8.0 mol%, the ratio of the structural unit derived from terephthalic acid was 15.0 mol%, and the ratio of the structural unit derived from isophthalic acid was 5.00 mol%. The total of the structural unit derived from 4,4'-dihydroxybiphenyl and the structural unit derived from hydroquinone was 20.0 mol% relative to the total structural units of the polyester, 100 mol%. In addition, the ratio of the structural unit derived from terephthalic acid to the structural unit derived from isophthalic acid was 0.333. Furthermore, the Tm was 327°C and the melt viscosity was 22 Pa·sec.

[0068] Milled fiber (B) or other milled fiber (b) (B-1) Milled fiber 1: EFH50-01 (manufactured by Central Glass Fiber Co., Ltd., average fiber length 50 μm) was used. (B-2) Milled fiber 2: EFH75-01 (manufactured by Central Glass Fiber Co., Ltd., average fiber length 75 μm) was used. (b-3) Milled fiber 3: EFH150-01 (manufactured by Central Glass Fiber Co., Ltd., average fiber length 150 μm) was used.

[0069] [Examples 1 to 5, Comparative Examples 1 to 4] The liquid crystal polyester resin (A) or other liquid crystal polyester resin (a) obtained in each production example and the milled fiber (B) or other milled fiber (b) were introduced into the twin-screw extruder (TEX-30α, manufactured by Japan Steel Works, Ltd.) with a screw diameter of 30 mm and L / D of 35 in the same direction and equipped with a vent, in the amounts shown in Table 2. The liquid crystal polyester resin (A) was added from the bottom of the twin-screw extruder, and the milled fiber (B) or other milled fiber (b) was added by installing a side feeder between the bottom of the twin-screw extruder and the vent. The cylinder temperature was set to the melting point of the liquid crystal polyester resin (A) or other liquid crystal polyester resin (a) + 25°C, and melt mixing was performed, discharged in the form of a strand, solidified through a cooling bath, and pelletized by a strand cutter.

[0070] [Example 6] Pellets were obtained in the same manner as in Example 1, except that the cylinder temperature was set to the melting point of the liquid crystal polyester resin (A) or the other liquid crystal polyester resin (a) + 5°C. The pellets obtained by each of the above-mentioned methods were used to carry out the following evaluations (4) to (7), and the results are shown in Table 1.

[0071] (4) Average fiber length of milled fiber (B) 50 g of the liquid crystal polyester resin composition was heated in air at 550°C for 3 hours to remove the resin components, and the residue remaining as a non-combustible material was used as milled fiber. 1000 of the remaining milled fibers were randomly selected using an optical microscope, and the fiber length was measured at 120 times magnification (manufactured by Inotec, "Quick Grain Standard"), and a cumulative fiber length distribution curve was calculated. The cumulative degree of 50% fiber length (D50) obtained from the cumulative fiber length distribution curve was evaluated as the average fiber length of the milled fiber (B).

[0072] (5) (D85 / D15) value of milled fiber (B) In the cumulative fiber length distribution curve obtained in the above evaluation (4), the 85% cumulative fiber length was defined as D85, and the 15% cumulative fiber length was defined as D15, and the evaluation was performed as the (D85 / D15) value.

[0073] (6) Burr evaluation The liquid crystal polyester resin composition was dried at 150°C for 12 hours using a hot air dryer, and then subjected to an SE50EV-C160 injection molding machine (manufactured by Sumitomo Heavy Industries, Ltd.). On the circumference of a disk with the gate position at the center, (p) width 5 mm × length 20 mm × thickness 1000 μm, (q) width 5 mm × length 20 mm × thickness 700 μm, (r) width 5 mm × length 20 mm × thickness 500 μm, (s) width 5 mm × length 20 mm × thickness 300 μm, (t) width 5 mm × length 20 mm × thickness 100 μm, (u) width 5 mm A disk-shaped mold having eight projections, (v) 20 mm in diameter and 20 mm in length and 50 μm in thickness, (v) 5 mm in width and 20 mm in length and 20 μm in thickness, and (w) 5 mm in width and 20 mm in length and 10 μm in thickness, was used, and the cylinder temperature was set to the melting point of the liquid crystal polyester resin + 25°C. 50 pieces were injection molded at a mold temperature of 90°C. The filling length of the projections (w) when the projections (q) were filled to the tip was measured using an optical microscope, and the average value was evaluated as the burr length. The shorter the burr length, the better the burr resistance.

[0074] (7) Evaluation of low anisotropy The liquid crystal polyester resin composition was dried with hot air at 150°C for 12 hours using a hot air dryer, and then fed to a FANUC α30C injection molding machine (manufactured by FANUC), and a cylinder temperature was set to the melting point of the liquid crystal polyester resin + 10°C, and a mold temperature was set to 90°C to mold a rectangular molded product of 50mm x 50mm x 1mm thickness. The molded rectangular plate was cut out to a length of 50mm x width of 10mm x 1mm thickness in the resin flow direction (MD) to prepare a rod-shaped test piece. In addition, the rectangular plate was cut out to a length of 50mm x width of 10mm x 1mm thickness in the resin flow perpendicular direction (TD) to prepare a rod-shaped test piece. For each rod-shaped test piece, a bending test was performed on 10 pieces using a bending tester UTA-1T (manufactured by Orientec) according to ASTM D790, and the average value of the obtained bending strength was taken as the bending strength in the TD and MD directions. From that value, the bending strength in MD / bending strength in TD was calculated as anisotropy. The closer the ratio is to 1, the better the low anisotropy.

[0075] [Table 1]

[0076] The results in Table 1 show that only by blending a milled fiber whose average fiber length is controlled within a specific range with a liquid crystal polyester resin (A) having a specific structural unit can it be possible to achieve both high levels of burr resistance and low anisotropy. [Explanation of symbols]

[0077] 1. Cumulative fiber length distribution curve 2. D85 value of cumulative fiber length distribution curve 3. D50 value of cumulative fiber length distribution curve 4. D15 value of cumulative fiber length distribution curve 5 Cumulative frequency (%) axis 6 Fiber length (μm) axis (common logarithm): The arrow points to the long fiber side [Industrial Applicability]

[0078] The liquid crystal polyester resin composition of the present invention has low burr properties and low anisotropy, and is therefore suitable for use in electrical and electronic parts such as connectors, coil bobbins, lens holding parts for camera modules, and actuator parts for camera modules.

Claims

1. A liquid crystal polyester resin composition comprising a liquid crystal polyester resin (A) and 1 to 100 parts by weight of milled fiber (B) per 100 parts by weight of the liquid crystal polyester resin (A), wherein the liquid crystal polyester resin (A) is a liquid crystal polyester resin comprising the following structural units (I) to (VI), and satisfies the following formulae (a) to (e), and the milled fiber (B) has an average fiber length of 1 to 100 μm in the liquid crystal polyester resin composition. 1≦[I]≦20...(a) 2≦[II]+[III]≦35...(c) 25≦[IV]≦75...(b) 2≦[V]≦35...(d) 0.01≦[VI]≦10...(e) ([I] to [VI] indicate the content (mol %) of each of the following structural units (I) to (VI) relative to 100 mol % of all structural units in the liquid crystal polyester resin (A).) 【Chemistry 1】

2. The liquid crystal polyester resin composition according to claim 1, wherein the [V] and [VI] satisfy the following formula (f): 0.003≦([VI] / [V])≦0.15...(f)

3. The liquid crystal polyester resin composition according to claim 1, characterized in that the ratio (D85 / D15) of the 85% cumulative fiber length (D85) to the 15% cumulative fiber length (D15) obtained from the cumulative fiber length distribution curve of the milled fiber (B) is 2.0 to 4.

0.

4. A molded article comprising the liquid crystal polyester resin composition according to any one of claims 1 to 3.

5. 5. The molded article according to claim 4, which is any one selected from the group consisting of a connector, a coil bobbin, a lens holding part of a camera module, and an actuator part of a camera module.

Citation Information

Patent Citations

  • High strength thermotropic liquid crystal polymer

    JP2016523291A

  • Liquid crystalline resin composition for surface mount relay and surface mount relay using the same

    JP2018104506A

  • Liquid crystal polyester resin composition and molded article made of the same

    JP2018104527A