Method for inspecting lithium-ion storage device and method for manufacturing group of devices
By analyzing the distribution of Li or P in the SEI coating on negative electrode plates, the method addresses the issue of localized performance unevenness in lithium ion power storage devices, enabling accurate prediction and manufacturing of devices with slower deterioration.
Patent Information
- Application Number
- JP2023086209
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2043-05-25
AI Technical Summary
Existing methods for evaluating lithium ion power storage devices, such as secondary batteries, fail to accurately predict localized performance unevenness in the electrode body, leading to inconsistent deterioration rates due to variations in the thickness of the SEI film on negative electrode active material particles.
A method involving disassembly, cleaning, and analysis of the Li or LiP-containing SEI coating on negative electrode plates to determine the distribution of Li or P, using techniques like ICP-MS, ICP-OES, XPS, or EDS, to assess the uniformity of the SEI film and predict deterioration progression.
Enables precise prediction of deterioration rates by identifying local unevenness in the SEI film, allowing for the selection and manufacturing of devices with slower deterioration progression.
Smart Images

Figure 2024169035000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for inspecting a lithium ion electricity storage device and a method for manufacturing a group of devices using the same. [Background technology]
[0002] When manufacturing an electricity storage device such as a lithium ion secondary battery, it is preferable to be able to predict deterioration. Patent Document 1 discloses a battery deterioration prediction system that can improve the accuracy of prediction of deterioration of a secondary battery through which a large current flows. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2022-007946 A Summary of the Invention [Problem to be solved by the invention]
[0004] As adopted in Patent Document 1, secondary batteries are evaluated based on the magnitude of battery capacity and battery resistance. However, it has been found that even if a battery has good values for battery capacity and battery resistance, some batteries will deteriorate significantly with subsequent use (repeated charging and discharging) compared to the deterioration state of other batteries. The reason for this is that in batteries with localized performance unevenness in the electrode body, deterioration progresses locally with use compared to batteries with almost no localized performance unevenness in the electrode body, and it was thought that deterioration also progresses when viewed as a whole battery. However, localized performance unevenness in the electrode body cannot be found by measuring the average characteristics of the whole battery, such as battery capacity and battery resistance.
[0005] Therefore, the present inventors conducted an investigation to obtain a new method for evaluating batteries, and found that one of the causes of localized performance unevenness in an electrode body is that the amount (thickness) of the SEI coating formed on the negative electrode active material particles differs depending on the portion of the negative electrode active material layer of the negative electrode plate used in the electrode body. Specifically, it has been found that if there are portions in the negative electrode active material layer where the amount of SEI coating is locally greater (thicker) or less (thinner) than the portion where the amount of SEI coating is average, then with subsequent use of the battery, degradation will progress in the portions where the amount of SEI coating is greater and less than the portion where the amount of SEI coating is average, and degradation will also progress when viewed from the perspective of the entire battery.
[0006] The present invention has been made in consideration of such findings, and provides an inspection method for lithium ion storage devices that makes it possible to predict the degree of deterioration, and a manufacturing method for a group of devices that are less likely to deteriorate using this inspection method. [Means for solving the problem]
[0007] (1) One aspect of the present invention for solving the above problems is an inspection method for a lithium ion storage device including an electrolyte, a positive electrode plate having a positive electrode active material layer, a negative electrode plate having a coated negative electrode active material layer on which a Li-containing SEI coating containing lithium is formed, and a separator interposed between the positive electrode active material layer and the coated negative electrode active material layer, an electrode body permeated with the electrolyte, and a case accommodating the electrode body and the electrolyte, the inspection method for a lithium ion storage device including a negative electrode plate removal step of disassembling the lithium ion storage device and removing the negative electrode plate, a removal step of washing and removing the electrolyte adhering to the removed negative electrode plate, and a Li amount distribution acquisition step of examining the distribution of the Li amount contained in the Li-containing SEI coating of the coated negative electrode active material layer.
[0008] In the method for inspecting this lithium ion storage device (hereinafter, simply referred to as the device), the device is disassembled to remove the negative plate, the negative plate is washed to remove any adhering electrolyte, and the distribution of the amount of Li contained in the Li-containing SEI coating formed on the coated negative active material layer is investigated. From the distribution of the amount of Li, it is possible to know the distribution of the amount of the SEI coating formed on the negative active material particles of the coated negative active material layer in the negative plate of the electrode body of the device. Thus, from the presence or absence and the degree of localized uneven distribution of the SEI coating, it is possible to predict the degree of deterioration, such as whether the deterioration will progress quickly or slowly if the device is used.
[0009] The lithium ion storage device may be a lithium ion secondary battery or a capacitor such as a lithium ion capacitor. The electrode body housed in the device may be a laminated electrode body or a wound electrode body. The wound electrode body may be a cylindrical wound type or a flat wound type.
[0010] The electrolyte may be a non-aqueous electrolyte obtained by dissolving a supporting salt in an organic solvent. Examples of the organic solvent used in the electrolyte include cyclic carbonates such as propylene carbonate and ethylene carbonate (EC), and chain carbonates such as dimethyl carbonate (DMC), diethyl carbonate, and ethyl methyl carbonate (EMC).
[0011] Examples of supporting salts to be dissolved in the electrolytic solution include lithium salts that serve as electrolytes, such as LiBF4, LiAsF6, LiPF6, LiCF3SO3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), etc. These salts may be used alone or in mixtures of two or more kinds, but are not limited thereto.
[0012] In the Li amount distribution acquisition process, methods for investigating the Li amount distribution include ICP-MS, ICP-OES, XPS, AES, EDS, etc.
[0013] The distribution data of the Li amount to be obtained may be distribution data of the Li amount in a predetermined range to be investigated, and examples of such data include linear distribution data obtained in a linear range extending in a desired direction such as the width direction or length direction of the negative electrode active material layer, and planar distribution data in a desired circular or rectangular range.
[0014] (2) The method for inspecting a lithium ion storage device according to the above-mentioned (1), wherein the electrolyte is a P-containing electrolyte containing a supporting salt containing phosphorus, and the coated negative electrode active material layer of the negative electrode plate has a LiP-containing SEI coating that also contains phosphorus, the Li-containing SEI coating being formed on the negative electrode active material layer that does not contain phosphorus, and the method for inspecting a lithium ion storage device may further include a P amount distribution acquisition step, which is performed instead of the Li amount distribution acquisition step or is performed together with the Li amount distribution acquisition step, of examining a distribution of P contained in the LiP-containing SEI coating of the coated negative electrode active material layer.
[0015] In this device inspection method, the electrolyte of the device is a P-containing electrolyte, and the coated negative electrode active material layer has a LiP-containing SEI coating that does not contain phosphorus in the negative electrode active material layer but contains phosphorus in addition to lithium. In addition, a P amount distribution acquisition step is provided, which is performed instead of the Li amount distribution acquisition step or together with the Li amount distribution acquisition step. Therefore, from the distribution of the P amount or the distribution of the P amount and the Li amount, it is possible to know the distribution of the amount of the SEI coating formed on the negative electrode active material particles of the coated negative electrode active material layer in the negative electrode plate of the electrode body of the device. Even in this way, the degree of progression of deterioration when the device is used can be predicted from the presence or absence and the degree of local uneven distribution of the SEI coating. In addition, by measuring the distribution of the Li amount and the distribution of the P amount in the same region, it is possible to more reliably detect the presence or absence and the degree of local uneven distribution of the SEI film and predict the progress of degradation of the device.
[0016] An example of a phosphorus-containing supporting salt is LiPF6. Methods for investigating the distribution of P content include ICP-MS, ICP-OES, XPS, AES, and EDS.
[0017] The distribution data of the P amount to be obtained may be the distribution data of the P amount in a predetermined range to be investigated, and may be, for example, linear distribution data obtained in a range extending linearly in a desired direction such as the width direction or length direction of the negative electrode active material layer, or surface distribution data in a desired circular or rectangular range. When the distribution of the Li amount is obtained in addition to the distribution of the P amount, it is preferable to obtain the P amount and the Li amount at the same position. This is because it is easy to compare the distributions of the two types of elements.
[0018] (3) Another aspect is a method for producing a device group consisting of a plurality of lithium ion electricity storage devices, the device group including: an electrolyte; a positive electrode plate having a positive electrode active material layer; a negative electrode plate having a coated negative electrode active material layer in which a Li-containing SEI coating containing lithium is formed on negative electrode active material particles; and a separator interposed between the positive electrode active material layer and the coated negative electrode active material layer, the electrode body being permeated with the electrolyte; and a case accommodating the electrode body and the electrolyte, the method including the steps of: selecting a sample device from an undetermined device group consisting of a plurality of the lithium ion electricity storage devices; the Li-containing SEI coating of the coated negative electrode active material layer of the device group is determined based on the Li amount distribution obtained by ...
[0019] In this method for manufacturing a group of devices, a sample device is selected from the group of devices, and a degradation test is performed. The sample device is then disassembled to take out the negative plate, and the negative plate is washed to remove the electrolyte adhering thereto, and the distribution of the amount of Li contained in the Li-containing SEI coating formed on the coated negative active material layer is investigated. From the distribution of the amount of Li, it is possible to know the distribution of the amount of the SEI coating formed on the negative active material particles of the coated negative active material layer in the negative plate of the electrode body of the sample device. In addition, it is possible to predict and select the degree of degradation progression when using the undetermined device group from which the sample device was obtained, based on the presence or absence and the degree of localized uneven distribution of the SEI coating of the sample device. Thus, it is possible to manufacture a good group of devices having the characteristic of slow progression of degradation.
[0020] The selection method of the sample device from the device group in the selection step includes a method of randomly selecting one or more sample devices from the multiple devices that make up the device group. In addition, the first device manufactured, the last device manufactured, or a device manufactured in the middle of the device group that makes up the production lot can also be selected. In addition, the sample device can be selected by focusing on the characteristics of the device, such as selecting a sample device with a previously inspected characteristic, such as a battery capacity, that has the average size of the device group.
[0021] (4) The method for producing a device group of (3), further comprising the steps of: (a) providing a phosphorus-containing electrolyte solution containing a supporting salt containing phosphorus; (b) providing a LiP-containing SEI coating, the Li-containing SEI coating also containing phosphorus, on a phosphorus-free negative electrode active material layer; and (c) providing a P amount distribution acquisition step for examining a distribution of P contained in the LiP-containing SEI coating of the coated negative electrode active material layer, which is performed instead of or together with the Li amount distribution acquisition step. The method for producing a device group of (3), further comprising the steps of: (a) providing a P amount distribution solution containing a phosphorus-containing supporting salt; and (b) determining whether or not the sample devices of the undetermined device group from which the sample devices have been obtained, using the P amount distribution instead of or together with the Li amount distribution.
[0022] In this method for producing a group of devices, the electrolyte of each device is a P-containing electrolyte, and the coated negative electrode active material layer has a LiP-containing SEI coating that does not contain phosphorus in the negative electrode active material layer, but contains phosphorus in addition to lithium. In addition, a P amount distribution acquisition step is provided for the sample device, which is performed instead of the Li amount distribution acquisition step or is performed together with the Li amount distribution acquisition step. Therefore, the distribution of the amount of the SEI coating formed on the negative electrode active material particles of the coated negative electrode active material layer in the negative electrode plate of the electrode body of the device can be known from the distribution of the P amount or the distribution of the P amount and the Li amount. Even in this way, the degree of deterioration progression when the undetermined device group from which the sample device was obtained is used can be predicted and selected from the presence or absence and degree of localized uneven distribution of the SEI coating, and a good device group having the characteristic of slow deterioration progression can be produced.
[0023] (5) In the method for manufacturing a device group according to (3), the judgment step may be a method for manufacturing a device group in which a pass / fail judgment is made for the unjudged device group using a minimum Li amount value and a maximum Li amount value in the obtained distribution of Li amounts.
[0024] In this method of manufacturing a group of devices, the minimum and maximum values of the Li amount are used in the judgment step, so that the pass / fail judgment of the group of unjudged devices can be easily performed.
[0025] In the method for manufacturing a device group according to (6) or (4), the judgment step may be a method for manufacturing a device group in which pass / fail judgment is performed on the undetermined device group using a minimum and a maximum P amount in the obtained P distribution, or using the minimum and maximum P amount, and the minimum and maximum Li amount in the obtained Li distribution.
[0026] In this method of manufacturing a device group, the pass / fail judgment of an undetermined device group can be performed easily by using the minimum and maximum P amounts in the judgment process, or more reliably by using the minimum and maximum P amounts, and the minimum and maximum Li amounts.
[0027] (7) Furthermore, in the method for manufacturing a device group described in any one of (3) to (6), the degradation process may be a process for reducing the capacity of the sample device until a capacity retention rate becomes smaller than a predetermined value.
[0028] In this method for manufacturing a group of devices, the capacity of the sample devices is reduced in the degradation step until the capacity maintenance rate becomes smaller than a predetermined value, and this makes it possible to appropriately judge the quality of the sample devices and, in turn, the quality of the unjudged device group using the distribution of Li amount obtained in the Li amount distribution acquisition step or the distribution of P amount obtained in the P amount distribution acquisition step.
[0029] As a forced degradation test for reducing the capacity of the sample device, a charge-discharge cycle test in which charging and discharging are repeated over a predetermined SOC range is preferably performed. In the sample device, the amount of the SEI coating formed on the negative electrode active material particles in the coating-coated negative electrode active material layer can be increased early, and the quality of the device group can be determined early. [Brief description of the drawings]
[0030] [Figure 1] FIG. 2 is a partially cutaway perspective view of a battery according to the embodiment and first and second modified embodiments. [Diagram 2] FIG. 2 is a perspective view of a flat wound electrode body according to the embodiment and modified embodiments 1 and 2. [Diagram 3] FIG. 2 is an explanatory diagram showing the positive electrode plate, the negative electrode, and the separator in a developed flat wound electrode body according to the embodiment and the first and second modified embodiments. [Figure 4] FIG. 4 is an explanatory diagram showing a state in which a negative electrode SEI coating is formed on a negative electrode active material particle of a coating-coated negative electrode active material layer in the embodiment and first and second modified embodiments. [Diagram 5] 4 is a flowchart showing a manufacturing process of a battery pack according to the embodiment. [Figure 6] 1 is a graph showing an example of distribution of Li amounts contained in band-shaped coated negative electrode active material layers obtained from degraded good batteries from a good lot and from degraded defective batteries from a defective lot. [Figure 7] 1 is a graph showing the relationship between the capacity maintenance rate of degraded good batteries from a good lot and defective batteries from a defective lot and the Li fluctuation rate obtained from the distribution of the Li amount. [Figure 8] 10 is a flowchart showing a manufacturing process of a battery pack according to the first modified embodiment. [Figure 9] 1 is a graph showing an example of the distribution of P amounts contained in band-shaped coated negative electrode active material layers obtained from degraded good batteries from a good product lot and from degraded defective batteries from a defective product lot. [Figure 10] 1 is a graph showing the relationship between the capacity maintenance rate of degraded good batteries from a good lot and defective batteries from a defective lot and the P variation rate obtained from the distribution of the P amount. [Figure 11] 10 is a flowchart showing a manufacturing process of a battery pack according to a second modified embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] (Embodiment) Hereinafter, according to an embodiment of the present invention, a battery group GB (an example of a device group) including a plurality of batteries 1 (an example of a lithium ion power storage device) that are lithium ion secondary batteries, and the manufacture thereof will be described with reference to Figures 1 to 7. Each of the plurality of batteries 1 belonging to this battery group GB is a rectangular, sealed lithium ion secondary battery, and is mounted in vehicles such as hybrid cars, plug-in hybrid cars, and electric cars, as well as in various devices.
[0032] The battery 1 of this embodiment includes a rectangular parallelepiped case 7, and an electrode assembly 2 and an electrolyte 6 housed inside the case 7. The rectangular parallelepiped box-shaped case 7 is made of metal (aluminum in this embodiment) and includes a bottomed rectangular cylindrical case body 7H and a lid 7L located at the upper BH1 in the height direction BH. A positive electrode terminal 8P and a negative electrode terminal 8N are fixed to the lid 7L via an insulating member 9. A liquid injection hole 7LH for injecting the electrolyte 6 is perforated in the lid 7L, and is sealed by a liquid injection plug 7LP after the liquid is injected. The electrode assembly 2 is covered in a bag-shaped insulating film (not shown) inside the case 7. A part of the electrolyte 6 housed in the case 7 is impregnated in the electrode assembly 2, and the remaining part is collected at the bottom of the case 7.
[0033] The electrode body 2 (see Figs. 2 and 3) is a so-called flat wound type electrode body, in which a strip-shaped positive electrode plate 3 and a strip-shaped negative electrode plate 4 are wound with a pair of strip-shaped separators 5 between them, pressed in the thickness direction CH to be flattened, and housed in the case 7. This electrode body 2 is housed in the case 7 in a horizontal position with the winding axis AX coinciding with the width direction AH (the left-right direction in Fig. 1).
[0034] In the flat wound electrode body 2, a positive current collecting part 2P is provided on one side XH1 of the axial direction XH along the winding axis AX (in this embodiment, this corresponds to one side AH1 of the width direction AH of the battery 1; upper side in FIG. 2) around which the current collecting part 3S of the positive plate 3 is wound. Conversely, a negative current collecting part 2N is provided on the other side XH2 of the axial direction XH (in this embodiment, this corresponds to the other side AH2 of the width direction AH of the battery 1; lower side in FIG. 2) around which the current collecting part 4S of the negative plate 4 is wound. The part between the positive current collecting part 2P and the negative current collecting part 2N is a main body part 2H in which the positive plate 3 and the negative plate 4 are wound with a separator 5 interposed therebetween.
[0035] The positive electrode terminal 8P is made of an aluminum plate bent into a predetermined shape. An inner connection part 8PI forming one end of the positive electrode terminal 8P is connected to a positive electrode current collector 2P arranged on one side AH1 in the width direction AH of the electrode body 2. On the other hand, the other end of the positive electrode terminal 8P is drawn out of the case 7 (specifically, onto the lid body 7L) to form an external terminal part 8PO. In addition, the negative electrode terminal 8N is made of a copper plate bent into a predetermined shape. An inner connection part 8NI forming one end of this negative electrode terminal 8N is connected to a negative electrode current collector 2N arranged on the other side AH2 in the width direction AH of the electrode body 2. On the other hand, the other end of the negative electrode terminal 8N is drawn out of the case 7 (specifically, onto the lid body 7L) to form an external terminal part 8NO.
[0036] The electrolyte 6 is a non-aqueous electrolyte containing an organic solvent 6V and a supporting salt 6S. In this embodiment, the organic solvent 6V is an organic solvent in which ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) are mixed in a weight ratio of 3:4:3. LiPF6 is used as the supporting salt 6S containing P. The concentration of LiPF6 in the electrolyte 6 is 1.1 mol / L.
[0037] As shown in FIG. 3, the belt-shaped positive electrode plate 3 of the electrode body 2 includes a positive electrode foil 3F made of aluminum foil and a positive electrode active material layer 3A laminated on both surfaces of the positive electrode foil 3F. The positive electrode active material layer 3A is made of positive electrode active material particles, conductive particles, and a binder (not shown). In this embodiment, lithium transition metal composite oxide particles, specifically, for example, lithium nickel cobalt manganese composite oxide particles, are used as the positive electrode active material particles. For example, acetylene black (AB) is used as the conductive particles. Also, for example, polyvinylidene fluoride (PVDF) is used as the binder. At the end of one side WH1 (upper side in FIG. 3) of the belt-shaped positive electrode plate 3 in the width direction WH, the positive electrode active material layer 3A does not exist on the positive electrode foil 3F, and the positive electrode foil 3F is exposed as a current collecting portion 3S. On the other hand, the remaining part of the positive electrode plate 3 is a positive electrode portion 3P in which the positive electrode active material layer 3A is laminated on both surfaces of the positive electrode foil 3F. As can be seen from FIGS. 2 and 3, the width direction WH (the vertical direction in FIG. 3) of the positive electrode plate 3 etc. coincides with the axial direction XH, and one side WH1 coincides with one side XH1.
[0038] On the other hand, the strip-shaped negative electrode plate 4 of the electrode body 2 includes a negative electrode foil 4F made of copper foil and a coated negative electrode active material layer 4A laminated on both surfaces of the negative electrode foil 4F. The coated negative electrode active material layer 4A includes a negative electrode active material layer 4AB made of negative electrode active material particles 4AP and a binder (not shown) that does not contain P, and a negative electrode SEI coating 4AC formed in a coating state around the negative electrode active material particles 4AP in an initial charging process described later. In this embodiment, graphite particles are used as the negative electrode active material particles 4AP. In addition, for example, carboxymethyl cellulose (CMC) is used as the binder. Note that, at the end of the other side WH2 (lower in FIG. 3) in the width direction WH of the strip-shaped negative electrode plate 4, the coated negative electrode active material layer 4A does not exist on the negative electrode foil 4F, and the negative electrode foil 4F is exposed as a current collector 4S. On the other hand, the remaining portion of the negative electrode plate 4 is a negative electrode portion 4N in which a negative electrode active material layer 4A with a coating is laminated on both surfaces of a negative electrode foil 4F.
[0039] In addition, the pair of strip-shaped separators 5 of the electrode body 2 are made of a porous resin. As shown in FIG. 3, the separator 5 is stacked between the negative electrode plate 4 and the positive electrode plate 3 in a wound state. The negative electrode plate 4 and the negative electrode portion 4N are slightly wider in the width direction WH than the positive electrode plate 3 and the positive electrode portion 3P. Moreover, the negative electrode portion 4N is arranged so as to cover the entire positive electrode portion 3P in the width direction WH, that is, so that the coated negative electrode active material layer 4A facing the positive electrode active material layer 3A exists at any part of the positive electrode active material layer 3A. In addition, the separator 5 is slightly wider in the width direction WH than the negative electrode portion 4N and the positive electrode portion 3P. Moreover, the separator 5 is arranged so as to cover the entire negative electrode portion 4N and the positive electrode portion 3P in the width direction WH, i.e., so that the separator 5 covering the positive electrode active material layer 3A and the coated negative electrode active material layer 4A is present in every portion of the positive electrode active material layer 3A and the coated negative electrode active material layer 4A.
[0040] By initially charging the battery 1 after permeating the electrode body 2 with the electrolyte solution 6, a negative electrode SEI coating 4AC containing Li and P is formed around the negative electrode active material particles 4AP constituting the coated negative electrode active material layer 4A formed on the negative electrode foil 4F of the negative electrode plate 4, as shown in Fig. 4. The formation of this negative electrode SEI coating 4AC enables the battery 1 to be charged and discharged stably with low resistance, compared to a case in which the negative electrode SEI coating 4AC is not formed or is insufficiently formed.
[0041] In manufacturing the battery 1, the electrode body 2 is connected to the positive electrode terminal 8P and the negative electrode terminal 8N and housed in the case 7. When the electrolyte 6 is poured into the case 7, the electrolyte 6 permeates from the outside XHO to the inside XHI in the axial direction XH of the electrode body 2, that is, from one side XH1 and the other side XH2 toward the inside of the electrode body 2. Specifically, the electrolyte 6 permeates along the positive electrode plate 3, the negative electrode plate 4, and the separator 5 from one side WH1 and the other side WH2 (upper and lower in FIG. 3 ) in the width direction WH that coincides with the axial direction XH, respectively, toward the center line ML of the width direction WH of the negative electrode active material layer 4AB, that is, toward the inside WHI of the width direction WH.
[0042] After a predetermined waiting time TT has elapsed since the start of the liquid injection, a power source (not shown) is connected to the positive electrode terminal 8P and the negative electrode terminal 8N, and a voltage is applied to the electrode body 2 of the battery 1 through the positive electrode terminal 8P and the negative electrode terminal 8N to perform initial charging. That is, a voltage is applied between the positive electrode plate 3 and the negative electrode plate 4 of the electrode body 2 in a predetermined initial charging pattern, and a negative electrode SEI coating 4AC is formed by the electrolyte 6 on the negative electrode active material particles 4AP of the negative electrode active material layer 4AB of the negative electrode plate 4 to form a coated negative electrode active material layer 4A (see FIG. 4). In this embodiment, initial charging is performed with an initial charging pattern of 0.5C-CCCV charging (SOC 85%). Thereafter, the liquid injection hole 7LH is sealed with the liquid injection plug 7LP.
[0043] Next, the sealed batteries 1 are subjected to high-temperature aging by being left in an environment of 60° C. for 25 hours. Furthermore, various inspections are performed on the batteries 1 to complete the batteries 1. By such an unjudged battery group manufacturing process S1, an unjudged battery group GBB is manufactured, which is made up of a large number of batteries 1 and is managed by a single manufacturing lot number or the like, and whose deterioration prediction, which will be described later, has not yet been judged (see FIG. 5).
[0044] However, depending on the battery 1, the negative electrode SEI coating 4AC formed on the negative electrode active material layer 4AB by the electrolyte 6 during initial charging may not be formed uniformly over the entire coated negative electrode active material layer 4A, and there may be location-specific variations (unevenness) in the amount and composition of the formed negative electrode SEI coating 4AC.
[0045] Thus, even in a battery 1 in which unevenness occurs in the negative electrode SEI coating 4AC formed on the coating-coated negative electrode active material layer 4A, the characteristics such as the battery capacity and battery resistance are good at the initial stage of use. However, it has been found that a battery 1 in which unevenness occurs in the negative electrode SEI coating 4AC deteriorates significantly as it is repeatedly charged and discharged with subsequent use, compared to the deterioration state of a battery 1 in which unevenness does not occur in the negative electrode SEI coating 4AC. It was thought that in a battery 1 in which unevenness occurs in the negative electrode SEI coating 4AC and localized performance unevenness exists in the electrode body 2, deterioration progresses locally as the battery 1 is used, and therefore deterioration is likely to progress even when viewed as a whole battery 1.
[0046] (Li distribution survey) Therefore, a defective battery 1N, which had been used in the same manner but had significantly deteriorated in characteristics, and a good battery 1G, which had relatively slow deterioration and maintained good characteristics, were prepared. Each battery 1G, 1N was discharged to SOC 0%, and disassembled in a glove box under an inert atmosphere, and the electrode body 2 was removed. The electrode body 2 was then unwound (see FIG. 3) to remove the strip-shaped negative electrode plate 4. A negative electrode sample (not shown) including a region for measuring the Li amount distribution was obtained from this negative electrode plate 4. For example, the flattened portion of the negative electrode plate 4 was cut in the width direction WH (the vertical direction in FIG. 3) to obtain a tape-shaped negative electrode sample extending in the width direction WH.
[0047] The negative electrode sample is then washed with EMC to remove the electrolyte 6. This removes Li, LiPF6, and the like contained in the electrolyte 6. Next, an ICP-MS is used to obtain the distribution of the amount of Li contained in the negative electrode SEI coating 4AC formed on the coating-attached negative electrode active material layer 4A in a desired measurement region of the negative electrode sample. Specifically, the Li amount AL is measured at each width direction position WP of the linear measurement region extending in the width direction WH using ICP-MS.
[0048] The results of measuring the distribution of the Li amount AL for the good battery 1G and the defective battery 1N are shown in Fig. 6. The horizontal axis of the graph in Fig. 6 is the widthwise position WP, which is shown in the dimension (mm) measured from the edge 4AE1 on one side WH1 in the width direction WH to the other side WH2 in the width direction WH, of the negative electrode plate 4 shown in Fig. 3. Meanwhile, the vertical axis of the graph in Fig. 6 is a relative value indicating the relative magnitude of the Li amount AL.
[0049] 6, the distribution of the Li amount AL of the good battery 1G shown by the solid line was almost constant regardless of the width direction position WP. That is, it is found that the variation (unevenness) of the Li amount AL in the width direction WH is very small in the coated negative electrode active material layer 4A. From this result, it is found that the amount (thickness) of the negative electrode SEI coating 4AC formed in the coated negative electrode active material layer 4A in the good battery 1G is also almost constant regardless of the width direction position WP, and the variation (unevenness) is small.
[0050] On the other hand, in the distribution of the Li amount AL of the defective battery 1N shown by the dashed line in FIG. 6, there were some parts, specifically, near the width direction position WP of 28 to 37 mm and 42 to 49 mm, where the Li amount AL was significantly larger than other parts. That is, it can be seen that in the defective battery 1N, the Li amount AL contained in the negative electrode SEI coating 4AC has a large variation (unevenness) at the width direction position WP. From this, it can be seen that in the defective battery 1N, the amount (thickness) of the negative electrode SEI coating 4AC formed on the coated negative electrode active material layer 4A also has a locally large part, and has a large variation (unevenness) at the width direction position WP. And, in the part where the amount of the negative electrode SEI coating 4AC is abnormally large, there is a local abnormal deterioration of the battery characteristics, specifically, a local decrease in the battery capacity and a local increase in the battery resistance, and it is considered that for this reason, the battery characteristics of the entire defective battery 1N have also been greatly deteriorated compared to the battery characteristics of the non-defective battery 1G. It is presumed that the above-mentioned local abnormal increase in the amount (thickness) of the negative electrode SEI coating 4AC gradually accumulated with the use of the battery.
[0051] (Li fluctuation ratio investigation) Therefore, a plurality of unused good batteries 1G from the same lot (good lot) as the good battery 1G used in the investigation shown in Fig. 6, and a plurality of unused defective batteries 1N from the same lot (defective lot) as the defective battery 1N used in the investigation shown in Fig. 6 are prepared. A predetermined charge-discharge cycle test is performed on each of the plurality of good batteries 1G and the plurality of defective batteries 1N, specifically, a forced deterioration test is performed by a charge-discharge cycle test in which 1C CCCV charging and 1C CCCV discharging are repeated in the range of SOC 20 to 80%, thickening the negative electrode SEI coating 4AC over time and causing deterioration in each battery 1G, 1N.
[0052] In this embodiment, a forced degradation test was performed on a plurality of good batteries 1G and defective batteries 1N, including a case where the forced degradation test was not performed (test time 0 hours), to achieve seven stages of capacity retention rates. That is, the forced degradation test was performed until the time when the good batteries 1G or defective batteries 1N were estimated to achieve a predetermined capacity retention rate, and the battery capacities of the removed good batteries 1G and defective batteries 1N were measured, and the capacity retention rates CC of the batteries 1G and 1N were calculated from the pre-test battery capacities obtained before the forced degradation test. Note that the number of cycles and test time of the charge-discharge cycle tests performed on the good batteries 1G and defective batteries 1N that had approximately the same capacity retention rates CC were different from each other.
[0053] Thereafter, in the same manner as in the above-mentioned distribution investigation of the Li amount AL, the good battery 1G and the bad battery 1N are disassembled, and the distribution of the Li amount AL similar to that shown in FIG. 6 is obtained using the negative electrode sample of the negative electrode plate 4. Next, as shown in FIG. 6, the minimum Li amount LI and the maximum Li amount LX are obtained from the distribution of the Li amount AL, and the Li fluctuation ratio RL is calculated by RL=LX / LI. Specifically, the minimum Li amount GLI and the maximum Li amount GLX are obtained from the distribution of the Li amount AL of the good battery 1G. Furthermore, the Li fluctuation ratio RL of the good battery 1G is calculated by RL=GLX / GLI. Similarly, the minimum Li amount NLI and the maximum Li amount NLX are obtained from the distribution of the Li amount AL of the bad battery 1N, and the Li fluctuation ratio RL of the bad battery 1N is calculated by RL=NLX / NLI.
[0054] Figure 7 shows the changes in the capacity retention rate CC and the Li fluctuation ratio RL obtained from multiple good batteries 1G and multiple bad batteries 1N. Figure 7 shows that in the good batteries 1G shown by the solid line, the Li fluctuation ratio RL is maintained at approximately the same value even though the capacity retention rate CC gradually decreases as the above-mentioned forced deterioration test is performed over a long period of time. That is, in the good batteries 1G, the amount (thickness) of the negative electrode SEI coating 4AC is maintained approximately uniform in the width direction WH even as the batteries deteriorate, and no unevenness occurs.
[0055] In contrast, in the defective battery 1N, the Li fluctuation ratio RL was approximately the same as that of the good battery 1G at the beginning of the forced degradation test, that is, until the capacity retention rate CC reached about 97%. However, unlike the good battery 1G, when the forced degradation test time was extended and the capacity retention rate CC dropped beyond 97%, the Li fluctuation ratio RL increased as the capacity retention rate CC dropped. By performing the forced degradation test, the negative electrode SEI coating 4AC was abnormally generated at a specific portion of the coated negative electrode active material layer 4A, and the abnormally generated portion expanded to the surroundings. In addition, at the abnormally generated portion, the abnormally generated negative electrode SEI coating 4AC made it difficult for the battery reaction to occur, the local battery capacity decreased, and the battery resistance increased, so that it is considered that the electrode body 2 of the defective battery 1N as a whole also experienced a decrease in battery capacity, etc.
[0056] According to these results, for a certain battery 1, before the aforementioned forced deterioration test is conducted, or after a short period of forced deterioration test is conducted to cause slight deterioration, when the capacity retention rate CC is maintained at approximately 97% or more, even if the battery 1 is disassembled and the aforementioned Li amount distribution investigation is conducted to obtain the distribution of Li amount AL (see Figure 6), it is not possible to properly determine whether the battery 1 is a good battery 1G or a defective battery 1N.
[0057] However, if the Li amount distribution investigation is performed after the forced deterioration test is performed until the capacity maintenance rate CC becomes 95% or less, it is possible to determine whether the battery 1 is a good battery 1G or a bad battery 1N. Specifically, for example, as shown by the dashed line in Fig. 7, a threshold value RLT (RLT = 2.0 in Fig. 7) is set for the Li fluctuation ratio RL, and if the obtained Li fluctuation ratio RL is smaller than the threshold value RLT, it is determined to be a good battery 1G, and if it is larger than the threshold value RLT, it is determined to be a bad battery 1N. This makes it possible to determine whether the undetermined battery group GBB to which the battery 1 belongs is a good battery group GBG consisting of good batteries 1G, or a bad battery group GBN consisting of bad batteries 1N (see Fig. 5).
[0058] (Battery pack manufacturing) In this embodiment, therefore, a battery group GB that includes a large number of batteries 1 and constitutes a single production lot is manufactured as follows. First, in an undetermined battery group manufacturing process S1, an undetermined battery group GBB that includes a large number of batteries 1 (see FIG. 1, for example) and constitutes a single production lot is manufactured using a known method. Note that each battery 1 is assumed to have already been subjected to high-temperature aging and initial charging.
[0059] Next, in a selection step S2, one or a small number of sample batteries 1S are selected from the many batteries 1 belonging to the undetermined battery group GBB. In the subsequent deterioration step S3, the selected sample battery 1S is subjected to the above-mentioned forced deterioration test. Specifically, the above-mentioned forced deterioration test is performed to reduce the capacity of the sample battery 1S until the capacity maintenance rate CC of the sample battery 1S falls to a predetermined value of 95% or less, specifically, about 95 to 93%. By performing this forced deterioration test (charge / discharge cycle test), the amount of the negative electrode SEI coating 4AC formed on the negative electrode active material particles 4AP of the coated negative electrode active material layer 4A in the sample battery 1S can be increased early, and the pass / fail judgment of the undetermined battery group GBB can be performed early.
[0060] After the forced deterioration test is completed, in the negative electrode plate removal process S4, the sample battery 1S is discharged to SOC 0% and disassembled in a glove box under an inert atmosphere to remove the electrode body 2. The electrode body 2 is then unwound to remove the strip-shaped negative electrode plate 4. A negative electrode sample (not shown) including a region for measuring the Li amount distribution is obtained from this negative electrode plate 4. For example, the flattened portion of the negative electrode plate 4 is cut in the width direction WH (the vertical direction in FIG. 3) to obtain a tape-shaped negative electrode sample extending in the width direction WH.
[0061] In the removal process S5, the removed negative electrode sample of the negative electrode plate 4 is washed with EMC to remove the attached electrolyte 6. As a result, Li, LiPF6, and the like contained in the electrolyte 6 are removed from the negative electrode sample of the negative electrode plate 4.
[0062] In the Li amount distribution acquisition step S6, for the negative electrode sample, in the same manner as described above, using IPC-MS, for a desired measurement region, the distribution of the Li amount AL contained in the negative electrode SEI film 4AC formed on the coated negative electrode active material layer 4A is obtained (see FIG. 6).
[0063] After that, in the determination step S7, based on the obtained distribution of the Li amount AL, the quality of the undetermined battery group GBB from which the sample battery 1S is obtained is determined. Specifically, for example, as described above, the minimum Li amount LI and the maximum Li amount LX are obtained from the distribution of the Li amount AL, and the Li variation ratio RL is calculated. The obtained Li variation ratio RL is compared with a predetermined threshold value RLT. When the Li variation ratio RL is greater than the threshold value RLT (RL>RLT), it is determined that the sample battery 1S is a defective battery 1N. At the same time, the undetermined battery group GBB to which the sample battery 1S belongs is determined to be a defective battery group GBN (NG in the determination step S7). Thereafter, processing such as disposal is performed.
[0064] Conversely, for example, when the Li variation ratio RL is smaller than the threshold value RLT (RL<RLT), it is determined that the sample battery 1S is a non-defective battery 1G (GOOD in the determination step S7). At the same time, the undetermined battery group GBB to which the sample battery 1S belongs is determined to be a non-defective battery group GBG. Thus, a good battery group GB (non-defective battery group GBG) having characteristics with slow progress of deterioration can be manufactured.
[0065] As described above, in this embodiment, in the determination step S7, since the minimum Li amount LI and the maximum Li amount LX are used, the quality of the undetermined battery group GBB can be easily determined.
[0066] (Modification 1) In the above-described embodiment, in manufacturing the battery group GB, the distribution of the Li amount AL was obtained from the negative electrode sample of the negative electrode plate 4 of the sample battery 1S, and the quality of the sample battery 1S and the undetermined battery group GBB to which this sample battery 1S belongs was determined using this Li amount distribution (see FIG. 5). However, the electrolyte 6 of the battery 1 described above is a phosphorus-containing supporting salt 6S, specifically, a P-containing electrolyte containing LiPF6. Therefore, during initial charging, the negative electrode SEI coating 4AC formed on the negative electrode active material particles 4AP contains P in addition to Li.
[0067] (Distribution survey of P content) Therefore, in this modified embodiment 1, instead of obtaining the Li amount distribution (see FIG. 6), the distribution of the P amount AP in the negative electrode sample obtained from the negative electrode plate 4 is obtained. That is, similarly to the embodiment, the distribution of the P amount AP contained in the negative electrode SEI coating 4AC formed in the coating-coated negative electrode active material layer 4A is obtained for a desired measurement region in the negative electrode sample obtained for the above-mentioned good battery 1G and the defective battery 1N by using ICP-MS (see FIG. 9). The horizontal axis of the graph in FIG. 9 also indicates the width direction position WP indicated by the dimension (mm) measured from the edge 4AE1 on one side WH1 in the width direction WH to the other side WH2 in the width direction WH in the negative electrode plate 4 shown in FIG. 3. On the other hand, the vertical axis of the graph in FIG. 9 indicates a relative value indicating the relative magnitude of the P amount AP.
[0068] As can be easily understood by comparing Fig. 9 with Fig. 6, in the good battery 1G shown by the solid line in Fig. 9, the distribution of the P amount AP is almost constant regardless of the width direction position WP, just like the distribution of the Li amount AL. That is, it can be seen that the variation (unevenness) in the width direction WH of the P amount AP contained in the negative electrode SEI coating 4AC formed in the coated negative electrode active material layer 4A of the good battery 1G is also very small, just like the variation in the Li amount AL. From this result, it can also be seen that in the good battery 1G, the amount (thickness) of the negative electrode SEI coating 4AC formed in the coated negative electrode active material layer 4A is also almost constant regardless of the width direction position WP, and the variation (unevenness) is small.
[0069] On the other hand, the distribution of the P amount AP of the defective battery 1N shown by the dashed line in FIG. 9 is almost the same as the distribution of the Li amount AL of the defective battery 1N shown by the dashed line in FIG. 6, and there are parts where the P amount AP is significantly larger than other parts locally, specifically, near the width direction position WP of 28 to 37 mm and 42 to 49 mm. That is, it can be seen that in the defective battery 1N, the P amount AP contained in the negative electrode SEI coating 4AC also varies (unevenly) significantly at the width direction position WP. From the distribution of the P amount AP, it can be seen that in the defective battery 1N, the amount (thickness) of the negative electrode SEI coating 4AC formed on the coating-coated negative electrode active material layer 4A also varies (unevenly) significantly locally, and there are parts where the amount (thickness) is significantly larger, and there is a large variation (unevenness) at the width direction position WP. For this reason, it is considered that the battery characteristics of the entire defective battery 1N are also significantly deteriorated compared to the battery characteristics of the non-defective battery 1G.
[0070] (Investigation of P fluctuation ratio) In this modified embodiment 1, the negative electrode samples of the negative plate 4 of the plurality of good batteries 1G and the plurality of defective batteries 1N used in the investigation of the Li fluctuation ratio RL in the embodiment (see FIG. 7) were used to investigate the P fluctuation ratio RP (see FIG. 10) in the same manner as in the embodiment. As shown in FIG. 9, the minimum P amount PI and the maximum P amount PX are obtained from the value of the P amount AP, and the P fluctuation ratio RP is calculated by RP=PX / PI. Specifically, the minimum P amount GPI and the maximum P amount GPX are obtained from the distribution of the P amount AP of the good battery 1G. Furthermore, the P fluctuation ratio RP of the good battery 1G is calculated by RP=GPX / GPI. Similarly, the minimum P amount NPI and the maximum P amount NPX are obtained from the distribution of the P amount AP of the defective battery 1N, and the P fluctuation ratio RP of the defective battery 1N is calculated by RL=NLX / NLI.
[0071] Fig. 10 shows the transitions of the capacity retention rate CC and the P fluctuation ratio RP of the good battery 1G and the bad battery 1N. As in the embodiment (see Fig. 7), in Fig. 10, in the good battery 1G, even if the capacity retention rate CC decreases due to the above-mentioned forced deterioration test, the P fluctuation ratio RP is maintained at approximately the same value. That is, from the transition of the P fluctuation ratio RP in Fig. 10, it can be seen that in the good battery 1G, even if it deteriorates, the amount (thickness) of the negative electrode SEI coating 4AC is maintained in an approximately uniform state in the width direction WH, and no unevenness occurs.
[0072] In contrast, as in the embodiment (see FIG. 7), the defective battery 1N has a P fluctuation ratio RP that is generally similar to that of the non-defective battery 1G until the capacity retention ratio CC reaches about 97%. However, when the capacity retention ratio CC falls below 97%, the P fluctuation ratio RP increases as the capacity retention ratio CC falls. By performing the forced deterioration test, the negative electrode SEI coating 4AC is abnormally formed in a specific portion of the coated negative electrode active material layer 4A. In this abnormal formation portion, the abnormally formed negative electrode SEI coating 4AC makes it difficult for a battery reaction to occur, and it is believed that the electrode body 2 of the defective battery 1N as a whole also experienced a noticeable decrease in battery capacity, etc.
[0073] From this result, as in the embodiment, if the forced deterioration test described above is performed until the capacity maintenance rate CC becomes 95% or less, and then a distribution survey of the P amount AP is performed, it is possible to determine whether the battery 1 is a good battery 1G or a defective battery 1N. Specifically, for example, as shown by the dashed line in Fig. 10, a threshold value RPT (RPT = 2.0 in Fig. 10) is set for the P fluctuation ratio RP, and if the obtained P fluctuation ratio RP is smaller than the threshold value RPT, it is determined that the battery 1 is a good battery 1G. Furthermore, it is also possible to determine whether the undetermined battery group GBB to which the battery 1 belongs is a good battery group GBG consisting of good batteries 1G, or a defective battery group GBN consisting of defective batteries 1N (see Fig. 8).
[0074] (Battery pack manufacturing) Therefore, in this modified embodiment 1, a battery group GB is manufactured that constitutes a single production lot and includes a large number of batteries 1. Specifically, in the manufacturing method of the battery group GB shown in Fig. 8, the undetermined battery group manufacturing step S1 to the removal step S5 are the same as the manufacturing method of the battery group GB shown in the embodiment (see Fig. 5).
[0075] However, in a P amount distribution acquisition step S16 of this modified embodiment 1, instead of the Li amount distribution acquisition step S6 of the embodiment, a distribution of the P amount AP contained in the negative electrode SEI coating 4AC formed on the coated negative electrode active material layer 4A is obtained for a desired measurement region of the negative electrode sample using ICP-MS (see FIG. 9).
[0076] Thereafter, different from the determination step S7 of the embodiment, in the determination step S17, from the obtained distribution of the P amount AP, the quality of the undetermined battery group GBB from which the sample battery 1S was obtained is determined. Specifically, for example, as described above, the minimum P amount PI and the maximum P amount PX are obtained from the distribution of the P amount AP, and the P variation ratio RP is calculated. Then, the obtained P variation ratio RP is compared with a predetermined threshold value RPT. When the P variation ratio RP is greater than the threshold value RPT (RP > RPT), it is determined that the sample battery 1S is a defective battery 1N, and the undetermined battery group GBB to which the sample battery 1S belongs is determined to be a defective battery group GBN (NG in the determination step S17).
[0077] Conversely, for example, when the P variation ratio RP is smaller than the threshold value RPT (RP < RPT), it is determined that the sample battery 1S is a non-defective battery 1G (GOOD in the determination step S17), and the undetermined battery group GBB to which the sample battery 1S belongs is determined to be a non-defective battery group GBG. Thus, also in this modified form 1, a good battery group GB (non-defective battery group GBG) having a characteristic of slow progress of deterioration can be manufactured.
[0078] Note that in this way, in this modified form 1, since the minimum P amount PI and the maximum P amount PX are used in the determination step S17, the quality of the undetermined battery group GBB can be easily determined.
[0079] (Modified Form 2) In the above-described embodiment and modified form 1, in manufacturing the battery group GB, the Li amount distribution or the P amount distribution is obtained from the negative electrode sample of the negative electrode plate 4 of the sample battery 1S, and only one of the obtained Li amount distribution or P amount distribution is used to determine the quality of the sample battery 1S and the undetermined battery group GBB to which this sample battery 1S belongs (see FIGS. 5 and 8).
[0080] In contrast, in this modified form 2, both the Li amount distribution (see FIG. 6) and the P amount distribution (see FIG. 9) are obtained from the negative electrode sample of the negative electrode plate 4 of the sample battery 1S, and the quality of the sample battery 1S and the undetermined battery group GBB to which this sample battery 1S belongs is determined using both the obtained Li amount distribution and P amount distribution.
[0081] (Battery pack manufacturing) That is, in this modified embodiment 2, a battery group GB is manufactured that constitutes a single production lot and includes a large number of batteries 1. Specifically, in the manufacturing method of the battery group GB shown in Fig. 11, the undetermined battery group manufacturing step S1 to the removal step S5 are the same as the manufacturing method of the battery group GB in the embodiment and modified embodiment 1 shown in Figs.
[0082] However, in the LiP amount distribution acquisition step S26 of the present modified embodiment 2, the distribution of the Li amount AL and the distribution of the P amount AP contained in the negative electrode SEI coating 4AC formed in the coating-coated negative electrode active material layer 4A are obtained for a desired measurement region of the negative electrode sample using ICP-MS (see FIGS. 6 and 9). That is, the LiP amount distribution acquisition step S26 is a step that combines the Li amount distribution acquisition step S6 in the embodiment and the P amount distribution acquisition step S16 in the modified embodiment.
[0083] Thereafter, in the judgment step S27 of the present modified embodiment 2, the quality of the undetermined battery group GBB from which the sample battery 1S was obtained is judged based on the obtained distribution of the Li amount AL and the distribution of the P amount AP. Specifically, for example, as described above, the Li amount minimum value LI and the Li amount maximum value LX are obtained from the distribution of the Li amount AL to calculate the Li fluctuation ratio RL. Also, the P amount minimum value PI and the P amount maximum value PX are obtained from the distribution of the P amount to calculate the P fluctuation ratio RP. The obtained Li fluctuation ratio RL is compared with a predetermined threshold value RLT, and the P fluctuation ratio RP is compared with a predetermined threshold value RPT, and if at least one of the Li fluctuation ratio RL is greater than the threshold value RLT (RL>RLT) and the P fluctuation ratio RP is greater than the threshold value RPT (RP>RPT), the sample battery 1S is judged to be a defective battery 1N. At the same time, the undetermined battery group GBB to which the sample battery 1S belongs is judged to be a defective battery group GBN (NG in the judgment step S27).
[0084] Conversely, for example, when the Li variation ratio RL is smaller than the threshold value RLT (RL < RLT) and the P variation ratio RP is smaller than the threshold value RPT (RP < RPT), the sample battery 1S is determined to be a good battery 1G (GOOD in the determination step S27). At the same time, the undetermined battery group GBB to which the sample battery 1S belongs is determined to be a good battery group GBG. Thus, also in this second modified form, a good battery group GB (good battery group GBG) having a characteristic of slow progress of deterioration can be manufactured.
[0085] Note that as described above, in this second modified form, in the determination step S27, in addition to the minimum Li value LI and the maximum Li value LX, the minimum P value PI and the maximum P value PX are also used for determination, so that the determination of the quality of the undetermined battery group GBB can be performed more reliably.
[0086] As described above, the present invention has been described in accordance with the embodiments and the first and second modified forms. However, it goes without saying that the present invention is not limited to the embodiments and the like, and can be appropriately modified and applied without departing from the gist thereof. For example, in the embodiments and the first and second modified forms, in the defective battery 1N in which deterioration has occurred, an example is shown in which in the Li amount distribution and the P amount distribution, a portion where the Li amount AL and the P amount AP are larger than other portions locally exists (see FIGS. 6 and 9). However, conversely, there may be a defective battery 1N in which a portion where the Li amount AL and the P amount AP are smaller than other portions locally exists. In this case as well, the quality determination of the undetermined battery group GBB can be performed by obtaining the minimum Li value LI and the maximum Li value LX from the Li amount distribution and calculating the Li variation ratio RL, or by obtaining the minimum P value PI and the maximum P value PX from the P amount distribution and calculating the P variation ratio RP.
Explanation of Reference Numerals
[0087] 1 Battery (Lithium Ion Storage Device) 1G Good Battery 1N Defective Battery 1S Sample Battery (Sample Device) GB Battery Group (Device Group) GBB Undetermined Battery Group (Undetermined Device Group) GBG Good Battery Group GBN Defective Battery Group 2 Electrode Body 3 Positive Electrode Plate 3A Positive Electrode Active Material Layer 4 Negative Electrode Plate 4A Negative Electrode Active Material Layer (Coated Negative Electrode Active Material Layer) 4AB Negative Electrode Active Material Layer ML Center Line WP Width Direction Position of (Negative Electrode Active Material Layer) 4AE1 Edge (on One Side in Width Direction) 4AP Negative Electrode Active Material Particles 4AC Negative Electrode SEI Film (Li-Containing SEI Film, LiP-Containing SEI Film) AL Li Content AP P Content LX, GLX, NLX Maximum Value of Li Content LI, GLI, NLI Minimum Value of Li Content PX, GPX, NPX Maximum Value of P Content LI, GPI, NPI Minimum Value of P Content RL Li Variation Ratio RLT Threshold Value RP P Variation Ratio RPT Threshold Value 6 Electrolyte 6V Organic Solvent 6S Supporting Salt (Supporting Salt Containing P) 7 Case XH Axial Direction XHI Inside XHO Outside WH Width Direction S1 Manufacturing Process of Undetermined Battery Group S2 Selection Process S3 Deterioration Process S4 Negative Electrode Plate Extraction Process S5 Removal Process S6 Li Content Distribution Acquisition Process S16 P Content Distribution Acquisition Process S26 LiP Content Distribution Acquisition Process (Li Content Distribution Acquisition Process, P Content Distribution Acquisition Process) S7 Li Content Distribution Judgment Process S17 P Content Distribution Judgment Process S27 LiP quantity distribution determination project
Claims
1. An electrolyte; an electrode body including a positive electrode plate having a positive electrode active material layer, a negative electrode plate having a coating-attached negative electrode active material layer on which a Li-containing SEI coating containing lithium is formed, and a separator interposed between the positive electrode active material layer and the coating-attached negative electrode active material layer, and permeated with the electrolyte; and a case that accommodates the electrode body and the electrolyte. A method for inspecting a lithium ion storage device, comprising: a negative electrode plate removal step of dismantling the lithium ion storage device and removing the negative electrode plate; a removing step of washing and removing the electrolyte adhering to the removed negative electrode plate; and a Li amount distribution acquisition step of examining the distribution of the Li amount contained in the Li-containing SEI coating of the coating-attached negative electrode active material layer. A method for inspecting a lithium-ion storage device.
2. A method for inspecting the lithium ion storage device according to claim 1, the electrolyte is a P-containing electrolyte containing a supporting salt containing phosphorus, The coating-attached negative electrode active material layer of the negative electrode plate is the Li-containing SEI coating, which is a LiP-containing SEI coating that also contains phosphorus, is formed on a negative electrode active material layer that does not contain phosphorus, A P amount distribution acquisition step is provided for examining the distribution of the P amount contained in the LiP-containing SEI coating of the coating-coated negative electrode active material layer, which is performed instead of or together with the Li amount distribution acquisition step. A method for inspecting a lithium-ion storage device.
3. An electrolyte; an electrode body including a positive electrode plate having a positive electrode active material layer, a negative electrode plate having a coating-attached negative electrode active material layer on which a Li-containing SEI coating containing lithium is formed, and a separator interposed between the positive electrode active material layer and the coating-attached negative electrode active material layer, and permeated with the electrolyte; and a case that accommodates the electrode body and the electrolyte. A method for manufacturing a group of lithium ion storage devices, comprising: A selection step of selecting a sample device from an undetermined device group including a plurality of the lithium ion power storage devices; a degradation step of subjecting the sample device to a degradation test in which the Li-containing SEI coating of the coating-coated negative electrode active material layer of the sample device is thickened; a negative electrode plate removal step of dismantling the deteriorated sample device and removing the negative electrode plate; a removing step of washing and removing the electrolyte adhering to the removed negative electrode plate; a Li amount distribution acquisition step of examining the distribution of the Li amount contained in the Li-containing SEI coating of the coating-coated negative electrode active material layer; and a determining step of determining whether the undetermined device group is defective or defective by selecting the sample device from the obtained distribution of the Li amount. A method for manufacturing a group of devices.
4. A method for producing a group of devices according to claim 3, comprising the steps of: the electrolyte is a P-containing electrolyte containing a supporting salt containing phosphorus, The coating-attached negative electrode active material layer of the negative electrode plate is the Li-containing SEI coating, which is a LiP-containing SEI coating that also contains phosphorus, is formed on a negative electrode active material layer that does not contain phosphorus, a P amount distribution acquisition step of examining a distribution of the P amount contained in the LiP-containing SEI coating of the coating-coated negative electrode active material layer, which is performed instead of the Li amount distribution acquisition step or together with the Li amount distribution acquisition step; The determination step includes: The pass / fail judgment of the unjudged device group from which the sample device was obtained is performed using the P content distribution instead of or in addition to the Li content distribution. A method for manufacturing a group of devices.
5. A method for producing a group of devices according to claim 3, comprising the steps of: The determination step includes: The minimum and maximum values of the Li amount in the obtained distribution of the Li amount are used to determine the pass / fail quality of the undetermined devices. A method for manufacturing a group of devices.
6. A method for producing a group of devices according to claim 4, comprising the steps of: The determination step includes: Using the minimum and maximum values of the P content in the obtained P content distribution, or Using the minimum value of the P amount and the maximum value of the P amount, and the minimum value of the Li amount and the maximum value of the Li amount in the obtained distribution of the Li amount, The pass / fail judgment of the unjudged devices is performed. A method for manufacturing a group of devices.
7. A method for producing a device group according to any one of claims 3 to 6, comprising the steps of: The deterioration step includes: decreasing the capacity of the sample device until the capacity retention is less than a predetermined value. A method for manufacturing a group of devices.
Citation Information
Patent Citations
Lithium ion secondary battery
JP2013246992A
Nonaqueous electrolyte secondary battery and method for manufacturing nonaqueous electrolyte secondary battery
JP2022154251A
Non-aqueous electrolyte solution secondary battery and manufacturing method therefor
JP2022162876A
Non-aqueous electrolyte solution secondary battery and manufacturing method therefor
JP2022162877A
Lithium-ion secondary battery manufacturing method