Quantum dot-containing composition, wavelength conversion member, and method for producing quantum dot-containing composition
A quantum dot composition with a core-shell structure and siloxane-bonded surface coating, combined with a polymerizable polymer, addresses stability issues in quantum dots, maintaining quantum yield and preventing aggregation, suitable for thin liquid crystal displays and color filters.
Patent Information
- Application Number
- JP2023086483
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2043-05-25
AI Technical Summary
Existing quantum dot-containing wavelength conversion materials face stability issues due to moisture and oxygen, leading to decreased quantum yield, and the use of barrier films increases cost and thickness, which is impractical for thinner liquid crystal displays and color filters.
A quantum dot-containing composition with a core-shell structure and a surface coating layer having siloxane bonds, combined with a polymerizable polymer, enhances stability and dispersibility by forming a siloxane bond with a ZnS outermost shell and incorporating reactive substituents like vinyl, acrylic, or epoxy groups.
The composition maintains quantum dot characteristics while improving stability, reducing aggregation, and ensuring high quantum yield, even in high humidity environments without the need for barrier films.
Smart Images

Figure 2024169209000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a quantum dot-containing composition, a wavelength conversion member, and a method for producing a quantum dot-containing composition. [Background technology]
[0002] In single crystal semiconductor nanoparticles, when the size of the crystal is equal to or smaller than the Bohr radius of the exciton, a strong quantum confinement effect occurs, and the energy levels become discrete. The energy levels depend on the size of the crystal, and the optical absorption wavelength and emission wavelength can be adjusted by the crystal size.
[0003] In addition, the quantum confinement effect makes the light emitted by exciton recombination in single crystal semiconductor nanoparticles highly efficient, and because this light emission is essentially an emission line, if a uniform particle size distribution can be achieved, it will be possible to emit light with high brightness and narrow bandwidth, which has attracted attention. The phenomenon caused by the strong quantum confinement effect in such nanoparticles is called the quantum size effect, and semiconductor nanocrystals that utilize this property are being studied for wide-ranging application development as quantum dots (QDs).
[0004] One application of quantum dots is being considered for use as phosphor materials for displays. If narrow-band, highly efficient light emission can be achieved, it will be possible to express colors that could not be reproduced with existing technology, and so quantum dots are attracting attention as a next-generation display material.
[0005] One display in which quantum dots are currently being used is the quantum dot liquid crystal display, which is already being commercialized. Attempts are being made to convert the color of light irradiated from a white or blue LED backlight into green or red by passing it through a wavelength conversion material containing quantum dots.
[0006] The surface of quantum dots is active, and the quantum yield gradually decreases due to moisture and oxygen in the air, so improving the stability of quantum dot-containing wavelength conversion materials is an essential item that needs to be considered.
[0007] Various studies have been conducted on the stabilization of wavelength conversion materials containing quantum dots. One example is gas barrier sealing. Stability is improved by forming an inner layer in which quantum dots are dispersed in an amphiphilic polymer or a compatible polymer, and then dispersing them in another resin layer with low gas permeability.
[0008] Patent document 1 discloses a method in which polymer beads are formed by dispersing QDs in a hydrophobic resin layer, and the polymer beads are surface-modified so that they can be dispersed in a hydrophilic polymer.
[0009] Hydrophilic polymers tend to have better gas barrier properties than hydrophobic polymers, so QDs are dispersed in such bilayer or multilayer structures. However, the gas barrier properties are insufficient for use in applications where high temperature and humidity may occur, such as those used in liquid crystal display units, so the QD film is sandwiched between gas barrier films to eliminate the effects of oxygen and water vapor.
[0010] Various studies have been conducted on the method of producing polymer beads. Patent Document 2 discloses a method in which QD-containing polymer beads are produced from polysiloxane having an amino group and a polymerizable functional group, and then a polymer having another polymerizable functional group is mixed, emulsified, and further cured.
[0011] In this method, the adhesion to the QDs is increased by introducing a ligand that coordinates to the QD surface into the polymer bead, which increases the concentration of QDs contained in the polymer bead, improving stability. However, the stability is still insufficient with this method, so the QDs are mounted by sandwiching them between barrier films. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] U.S. Pat. No. 9,708,532 [Patent Document 2] JP 2016-111292 A [Patent Document 3] Special Publication No. 2019-536653 [Patent Document 4] US Patent Application Publication No. 2019 / 0322926 Summary of the Invention [Problem to be solved by the invention]
[0013] However, using a barrier film not only increases costs, but also inevitably increases thickness. Currently, there is a demand for thinner LCDs, and it is necessary to reduce the thickness of the wavelength conversion material, so there is a demand for improved stability without the barrier film. In addition, when considering color filter applications, patterning is required, and it is not realistic to provide a protective layer such as a barrier film, so the stability of the quantum dots themselves is necessary.
[0014] Patent Document 3 has been published as a study on improving heat resistance and moisture resistance without using a barrier film. In this method, a silazane coating process is further performed on the multilayer resin composition using the polymer bead structure of Patent Document 1, and stability is improved. However, this method has a problem in that the quantum yield decreases when the silazane coating is photocured by irradiation with short ultraviolet light (170 nm).
[0015] Another attempt is disclosed in Patent Document 4. In this method, a ligand is coordinated to the quantum dot, reactive substituents such as vinyl groups and methacryl groups are introduced into the ligand, and then a silicone resin containing Si-H is mixed with a curing agent, and the mixture is spin-coated as is and cured by heating to produce a film with improved heat resistance and moisture resistance.
[0016] However, the Si-H-containing silicone resin and quantum dots used have low compatibility, and aggregation occurs when attempting to disperse them at high concentrations. Therefore, compatibility must be improved by ligand treatment, but if the balance between hydrophobic and hydrophilic groups changes when coordinating the ligand, aggregation is likely to occur, resulting in a decrease in quantum yield.
[0017] In addition, when applying to color filters, it is important to form a quantum dot surface state suitable for the patterning method. Currently, color filters are made by applying a photosensitive resin composition containing a pigment onto a glass substrate, drying the solvent, exposing the substrate to UV light through a mask, and removing the uncured parts by alkaline development to form color patterns. This process is repeated to form blue, red, and green patterns using photolithography.
[0018] Photolithography has many problems, such as the uncured parts being wasted, resulting in a large loss of raw materials, complicated processes, and the use of expensive equipment. For this reason, the inkjet method has also been considered in recent years.
[0019] The inkjet method is cost-competitive because there is no loss of raw materials and it is possible to produce larger sizes and areas without introducing expensive equipment. However, the technology to make fine nozzles is difficult, and as the nozzles get smaller, there are problems such as clogging and unstable ejection, so both photolithography, which has a proven track record in miniaturization, and inkjet, which is cost-competitive, are being considered for miniaturization.
[0020] On the other hand, in both photolithography and inkjet printing, it is difficult to prepare a resin composition containing quantum dots at a high concentration and high dispersion. When quantum dots are dispersed at a high concentration, there are problems such as the properties of the resin after curing being altered, for example, the curing is slowed down by the amount of the quantum dots contained.
[0021] The present invention has been made to solve the above problems, and aims to provide a quantum dot-containing composition and a wavelength conversion member that can improve stability while maintaining the properties of quantum dots. Another object of the present invention is to provide a method for producing a quantum dot-containing composition that can improve the stability while maintaining the properties of the quantum dots. [Means for solving the problem]
[0022] The present invention has been made to achieve the above-mentioned object, and provides a quantum dot-containing composition that contains quantum dots that emit fluorescence when excited by excitation light, the quantum dot-containing composition being a mixture of quantum dots and a polymerizable polymer composition, the quantum dots having a core-shell structure with an outermost shell being ZnS, the quantum dot surfaces containing a surface coating layer having a siloxane bond, and the quantum dots have a wavelength of 1000 to 1200 cm by Fourier transform infrared spectroscopy. -1 The peak intensity in the range of 2800 to 3000 cm -1 The present invention provides a quantum dot-containing composition, which is characterized in that the peak intensity is greater than that present in
[0023] Such a quantum dot-containing composition can improve the stability while maintaining the properties of the quantum dots.
[0024] In this case, the surface coating layer may have at least one reactive substituent selected from the group consisting of a vinyl group, an acrylic group, a methacrylic group, a hydroxyl group, a phenolic hydroxyl group, and an epoxy group.
[0025] This makes it possible to introduce a substituent group capable of polymerizing with the polymerizable polymer into the surface coating layer, thereby improving the stability while maintaining the properties of the quantum dots.
[0026] In this case, the polymer contained in the polymerizable polymer composition may contain, as a substituent polymerizable with the reactive substituent, one or more of a vinyl group, an acrylic group, a methacrylic group, a hydroxyl group, a phenolic hydroxyl group, and an epoxy group.
[0027] This allows the reactive substituent to be polymerized with the polymer, and not only can it suppress poor curing during polymerization of the polymer but also improve dispersibility.
[0028] The present invention also provides a wavelength conversion member which is a cured product of the quantum dot-containing composition described above.
[0029] Such a wavelength conversion material is a cured product of a quantum dot-containing composition that can improve stability while maintaining the properties of the quantum dots, and therefore the wavelength conversion material can also improve stability while maintaining the properties of the quantum dots.
[0030] Furthermore, the present invention provides a method for producing a quantum dot-containing composition containing quantum dots that emit fluorescence when excited by excitation light, comprising: a surface treatment step of heating and mixing a solution in which quantum dots having ZnS formed on the outermost shell are dispersed, a ligand having a substituent capable of forming a siloxane bond and a thiol group, and a solution containing a zinc precursor and a sulfur precursor, to form additional ZnS on the outermost surface of the quantum dots while coordinating the ligand; a surface coating layer formation step of reacting the substituent capable of forming a siloxane bond with a compound having a reactive substituent capable of forming a siloxane bond to form a surface coating layer having a siloxane bond after the surface coating layer formation step; and a mixing step of adding and mixing a polymerizable polymer composition containing the reactive substituent and a polymerizable substituent after the surface coating layer formation step.
[0031] According to this manufacturing method, by reacting a ligand containing a substituent capable of forming a siloxane bond while forming a ZnS shell, it is possible to form a surface coating layer to inactivate the quantum dots while suppressing the decrease in the luminous efficiency of the quantum dots due to surface treatment, thereby improving the stability. Furthermore, by arranging a polymerizable substituent in the polymerizable polymer composition, it is possible to not only suppress poor curing during polymerization of the polymer, but also improve dispersibility. Effect of the Invention
[0032] As described above, the quantum dot-containing composition and wavelength conversion member of the present invention can improve stability while maintaining the properties of the quantum dots. Furthermore, according to the method for producing a quantum dot-containing composition of the present invention, it is possible to improve the stability while maintaining the properties of the quantum dots. [Brief description of the drawings]
[0033] [Figure 1] 1 shows a Fourier transform infrared spectroscopy (FT-IR) spectrum of the quantum dots of Example 1. [Diagram 2] 1 shows the FT-IR spectrum of the quantum dots of Comparative Example 1. [Diagram 3] 1 shows a flow diagram of a method for producing a quantum dot-containing composition of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] The present invention will be described in detail below, but the present invention is not limited thereto.
[0035] As described above, there has been a demand for a quantum dot-containing composition that can improve the stability while maintaining the properties of the quantum dots.
[0036] As a result of intensive research into the above-mentioned problems, the present inventors have discovered a quantum dot-containing composition that contains quantum dots that emit fluorescence when excited by excitation light, the quantum dot-containing composition being a mixture of quantum dots and a polymerizable polymer composition, the quantum dots having a core-shell structure with an outermost shell being made of ZnS, the surfaces of the quantum dots containing a surface coating layer having a siloxane bond, and the quantum dots having a wavelength of 1000 to 1200 cm as determined by Fourier transform infrared spectroscopy. -1 The peak intensity in the range of 2800 to 3000 cm -1 The present inventors have found that a quantum dot-containing composition characterized in that the peak intensity is greater than that present in the quantum dot-containing composition can improve the stability while maintaining the properties of the quantum dots, and have completed the present invention.
[0037] As described above, there has been a demand for a wavelength conversion member that can improve stability while maintaining the properties of quantum dots.
[0038] As a result of extensive research into the above-mentioned problems, the inventors have discovered that a wavelength conversion member that is a cured product of the quantum dot-containing composition described above can improve stability while maintaining the properties of the quantum dots, and have completed the present invention.
[0039] Furthermore, as described above, there has been a need for a method for producing a quantum dot-containing composition that can improve the stability while maintaining the properties of the quantum dots.
[0040] As a result of intensive research into the above-mentioned problems, the present inventors have found that a method for producing a quantum dot-containing composition containing quantum dots that emit fluorescence when excited by excitation light, comprising: a surface treatment step of heating and mixing a solution in which quantum dots having ZnS formed in the outermost shell are dispersed, a ligand having a substituent capable of forming a siloxane bond and a thiol group, and a solution containing a zinc precursor and a sulfur precursor, and coordinating the ligand while forming additional ZnS on the outermost surface of the quantum dots; a surface coating layer formation step of reacting the substituent capable of forming a siloxane bond with a compound having a reactive substituent capable of forming a siloxane bond to form a surface coating layer having a siloxane bond after the surface coating layer formation step; and a mixing step of adding and mixing a polymerizable polymer composition containing the reactive substituent and a polymerizable substituent after the surface coating layer formation step, can improve the stability while maintaining the properties of the quantum dots, and have completed the present invention.
[0041] The present invention will be described in detail below, but the present invention is not limited thereto. The quantum dot-containing composition of the present invention is a composition containing quantum dots that emit fluorescence when excited by excitation light and have a surface coating layer containing siloxane bonds formed on the surface. More specifically, the quantum dot-containing composition is a mixture of quantum dots and a polymerizable polymer composition. In addition, the quantum dot-containing composition may be a composite particle in which a substituent capable of condensation polymerization with the polymerizable polymer composition is introduced into the surface coating layer, and a mixture thereof.
[0042] (Quantum dots) The shape of the quantum dots in the present invention is not particularly limited, and any shape can be used. Quantum dots are mainly nanoparticles with a particle diameter of 10 nm or less, but they may also be nanowires, nanorods, nanotubes, nanocubes, etc., and any shape can be used.
[0043] The quantum dots used in the present invention can be made of any suitable material that emits fluorescence when excited by excitation light. For example, the semiconductor material can be selected from the group consisting of II-VI group, III-V group, IV group, IV-VI group, I-III-VI group, II-IV-V group, mixed crystals or alloys thereof, or compounds having a perovskite structure.
[0044] Specific examples of compounds include, but are not limited to, ZnS, ZnSe, ZnTe, CdS, CdSe, CdTe, AlN, AlP, AlAs, AlSb, GaN, GaP, GaAs, GaSb, InN, InP, InAs, InSb, Si, Ge, Sn, Pb, PbS, PbSe, PbTe, SnS, SnSe, SnTe, AgGaS2, AgInS2, AgGaSe2, AgInSe2, CuGaS2, CuGaSe2, CuInS2, ZnSiP2, ZnGeP2, CdSiP2, CdGeP2, CsPbCl3, CsPbBr3, CsPbI3, CsSnCl3, CsSnBr3, and CsSnI3.
[0045] The quantum dots used in the present invention have a core-shell structure. The shell material capable of forming the core-shell structure is not particularly limited as long as the outermost shell is ZnS, but it is preferable that the shell material has a large band gap and low lattice mismatch with respect to the core material, and is also preferable that the band gap is smaller than that of the outermost shell, ZnS, and it is possible to arbitrarily combine the core material and the outermost shell material according to the material.
[0046] Specific shell materials include ZnO, ZnS, ZnSe, ZnTe, CdS, CdSe, CdTe, AlN, AlP, AlAs, AlSb, GaN, GaP, GaAs, GaSb, InN, InP, InAs, InSb, BeS, BeSe, BeTe, MgS, MgSe, MgTe, PbS, PbSe, PbTe, SnS, SnSe, SnTe, CuF, CuCl, CuBr, and CuI. The above materials may be selected as a single or multiple mixed crystals, but are not limited thereto.
[0047] There are various methods for producing quantum dots, such as a liquid phase method or a gas phase method, and the present invention is not particularly limited thereto. However, from the viewpoint of exhibiting high fluorescence emission efficiency, it is preferable to use semiconductor nanoparticles obtained by a hot soap method or a hot injection method, in which a precursor species is reacted at high temperature in a nonpolar solvent with a high boiling point, and it is desirable that an organic ligand is coordinated to the surface in order to impart dispersibility in the nonpolar solvent and reduce surface defects.
[0048] From the viewpoint of dispersibility, the ligand preferably contains an aliphatic hydrocarbon. Examples of such ligands include oleic acid, stearic acid, palmitic acid, myristic acid, lauric acid, decanoic acid, octanoic acid, oleylamine, stearyl (octadecyl)amine, dodecyl (lauryl)amine, decylamine, octylamine, octadecanethiol, hexadecanethiol, tetradecanethiol, dodecanethiol, decanethiol, octanethiol, trioctylphosphine, trioctylphosphine oxide, triphenylphosphine, triphenylphosphine oxide, tributylphosphine, and tributylphosphine oxide, and the like, and these may be used alone or in combination.
[0049] (Ligands with thiol groups) In addition to the above-mentioned ligand, the quantum dot of the present invention preferably has a ligand having a substituent capable of forming a siloxane bond. The ligand having a substituent capable of forming a siloxane bond preferably has a substituent that interacts with or is adsorbed to the surface of the quantum dot.
[0050] Substituents that interact or react with the quantum dot surface include amino groups, carboxy groups, mercapto groups, phosphine groups, phosphine oxide groups, sulfonyl groups, and quaternary ammonium salts. The outermost shell is made of ZnS, and among these, thiol groups are preferred from the viewpoint of coordination ability and reactivity.
[0051] In addition, the quantum dot-containing composition of the present invention contains a surface coating layer having a siloxane bond. For example, the quantum dot surface is coated with a polymer using polysiloxane. Therefore, it is desirable that the ligand having a substituent capable of coordinating to the quantum dot surface has a substituent capable of forming a siloxane bond.
[0052] Examples of the ligand having a substituent capable of forming a siloxane bond include compounds containing alkoxysilanes such as trimethoxysilyl, triethoxysilyl, dimethoxymethylsilyl, diethoxymethylsilyl, dimethylmethoxysilyl, and ethoxydimethylsilyl groups, compounds having a silazane bond, compounds having a Si-OH bond, compounds having a Si-X (X: halogen) bond, and carboxylic acids. However, it is preferable to use a ligand containing alkoxysilane, silazane, or Si-OH, since the reaction can proceed under mild conditions in which no acid is generated as a by-product of the reaction.
[0053] (Surface coating layer) The surface coating layer of the quantum dot-containing composition of the present invention has a siloxane bond. More specifically, it is desirable that the quantum dot surface is coated with a polymer by polysiloxane. Therefore, it is desirable to form a quantum dot surface polymer coating layer containing polysiloxane by reacting a substituent capable of forming a siloxane bond contained in a ligand having a thiol group capable of coordinating with the quantum dot with a compound having a reactive substituent capable of forming a siloxane bond.
[0054] In addition, the surface coating layer of the present invention preferably has at least one reactive substituent polymerizable with a polymer contained in a polymerizable polymer composition described below. The substituent polymerizable with a polymer is preferably contained in the surface coating layer by forming a covalent bond.
[0055] By forming a covalent bond, the substituent that can polymerize with the polymer is less likely to be removed during subsequent purification operations, compared to when the substituent forms an association with the surface-coated quantum dots or when the substituent is contained so as to be coordinated to the surface of the quantum dots or the surface coating layer.
[0056] Examples of reactive substituents that can polymerize with a polymer include vinyl groups, acrylic groups, methacrylic groups, hydroxyl groups, phenolic hydroxyl groups, epoxy groups, sulfonyl groups, carboxyl groups, and thiol groups. However, if the acidity is not too strong and the coordination with the quantum dots is not too easy, aggregation can be reliably suppressed, and thus it is preferable. Specifically, vinyl groups, acrylic groups, methacrylic groups, hydroxyl groups, phenolic hydroxyl groups, and epoxy groups are preferred.
[0057] (FT-IR spectrum) As shown in Figure 1, the surface-coated quantum dots were measured by FT-IR with a wavelength of 1000 to 1200 cm -1 The peak intensity in the range of 2800 to 3000 cm -1 The intensity of the peak is greater than that present in the
[0058] As shown in Figure 2, 1000-1200 cm -1 The peak intensity in the range of 2800 to 3000 cm -1 If the intensity is lower than the peak intensity present in the graph, the properties of the quantum dots, such as the internal quantum efficiency, may decrease, and the stability may become poor.
[0059] (Polymerizable polymer composition) The quantum dot-containing composition of the present invention is a mixture of quantum dots and a polymerizable polymer composition. The polymerizable polymer composition comprises, for example, a polymer that is a base polymer and a polymerization initiator, and may further contain an organic solvent, a polymerizable crosslinking agent, a photoacid generator, an antioxidant, a light scattering agent, and the like.
[0060] Suitable polymers that can be used include polymers derived from acrylic acid, methacrylic acid, acrylic acid esters, and methacrylic acid esters, copolymers combining multiple polymers, polymers having glycidyl (meth)acrylate as a repeating unit, and polymers containing a siloxane skeleton, a urethane skeleton, a silphenylene skeleton, a norbornene skeleton, a fluorene skeleton, or an isocyanurate skeleton. The polymer to be used may be selected appropriately depending on the application.
[0061] Examples of the resin include acrylic resins, alkyd resins, melamine resins, epoxy resins, silicone resins, polyvinyl alcohol, polyvinylpyrrolidone, polyamides, polyamide-imides, polyimide precursors such as polyimides, and esterification products thereof, and reaction products of tetracarboxylic dianhydrides and diamines.
[0062] In addition, it is preferable that a polymerizable substituent capable of polymerizing with the reactive substituent is introduced into these polymers, and curing is possible by using them in combination with a polymerization initiator. The radically polymerizable substituents include vinyl groups, acrylic groups, methacrylic groups, thiol groups, etc., and any of them can be suitably used. The cationic polymerizable substituents include those containing at least one of hydroxyl groups, phenolic hydroxyl groups, and epoxy groups. In addition, glycidyl groups, oxetanyl groups, isocyanate groups, etc., and any of them can be suitably used. In addition, a carboxyl group may be introduced to impart alkaline developability.
[0063] It is also preferable that the quantum dot-containing composition of the present invention contains a polymerization initiator. The polymerization initiator may be a thermal or photopolymerization initiator, and either may be suitably used according to the base polymer. As the photoradical polymerization initiator, in the Irgacure (registered trademark) series commercially available from BASF, for example, Irgacure 290, Irgacure 651, Irgacure 754, Irgacure 184, Irgacure 2959, Irgacure 907, Irgacure 369, Irgacure 379, Irgacure 819, Irgacure 1173, etc. may be mentioned. In addition, in the Darocure (registered trademark) series, for example, TPO, Darocure 1173, etc. may be mentioned. In addition, the composition may contain a known thermal radical polymerization initiator or a photocation polymerization initiator.
[0064] The content of the polymerization initiator is preferably 0.1 to 10 parts by mass, and more preferably 0.2 to 5 parts by mass, based on 100 parts by mass of the polymer to be added.
[0065] The quantum dot-containing composition of the present invention may contain a solvent to improve its applicability. As the solvent, an organic solvent is preferable from the viewpoint of compatibility with the quantum dots, for example, ketone, alkylene glycol ether, alcohol, and aromatic compound. From the group of ketones, acetone, methyl ethyl ketone, cyclohexanone, etc., from the group of alkylene glycol ethers, methyl cellosolve (ethylene glycol monomethyl ether), butyl cellosolve (ethylene glycol monobutyl ether), methyl cellosolve acetate, cellosolve acetate, butyl cellosolve acetate, ethylene glycol monopropyl ether, ethylene glycol monohexyl ether, ethylene glycol dimethyl ether, diethylene glycol ethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, diethylene glycol ... and the like; from the group of alcohols, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-butyl alcohol, 3-methyl-3-methoxybutanol, and the like; and from the group of aromatic solvents, benzene, toluene, and xylene can be suitably used.
[0066] Furthermore, the quantum dot-containing composition of the present invention may further contain a polymerizable crosslinking agent, a photoacid generator, an antioxidant, a light scattering agent, etc., and there are no particular limitations on these as long as they do not affect the coatability of the quantum dot-containing composition.
[0067] (Method for producing a quantum dot-containing composition) The quantum dot-containing composition of the present invention can be produced by the following method illustrated in FIG. First, quantum dots that emit fluorescence when excited by excitation light and have ZnS formed in the outermost shell are manufactured, or if they have already been manufactured, prepared quantum dots are dispersed in a solution (S0 in Fig. 3). Examples of the manufacturing method of quantum dots include the liquid phase method and gas phase method already mentioned.
[0068] Next, the solution in which the quantum dots are dispersed, a ligand having a substituent capable of forming a siloxane bond and a thiol group, and a solution containing a zinc precursor and a sulfur precursor are heated and mixed, and the ligand is coordinated while forming additional ZnS on the outermost surface of the quantum dots (S1 in Figure 3, surface treatment process).
[0069] The reason why the ligand is coordinated while forming ZnS in this way is as follows. When coordinating a ligand having a thiol group with a substituent capable of forming a siloxane bond, quantum dots with a ligand containing a long-chain hydrocarbon coordinated thereto are generally dispersed in a hydrophobic solvent, and then mixed with a ligand having a thiol group capable of coordinating with a substituent capable of forming a siloxane bond and the surface of the quantum dot to perform ligand exchange. The conditions of the ligand exchange reaction, such as the amount of ligand added, heating temperature, time, and light irradiation, are appropriately changed depending on the type of ligand. However, it has been found that this method causes a certain amount of decrease in quantum yield.
[0070] Therefore, by mixing a ligand into the zinc precursor and sulfur precursor solutions when forming the ZnS shell, it is possible to introduce the ligand without decreasing the quantum yield, and it is also possible to introduce more ligands than by ligand exchange.
[0071] Next, after the surface treatment step, a substituent capable of forming a siloxane bond is reacted with a compound having a reactive substituent capable of forming a siloxane bond to form a surface coating layer having a siloxane bond (S2 in FIG. 3, surface coating layer formation step).
[0072] Specifically, a reaction is carried out between the quantum dots coordinated with thiols having substituents capable of forming siloxane bonds, which were introduced in the surface coating layer formation process, and polysiloxane to form a surface coating layer containing siloxane bonds.
[0073] The sol-gel method is a common method for forming polysiloxane bonds. However, since quantum dots are vulnerable to acidic conditions and moisture, a sol-gel method under basic conditions or a sol-gel method using a Lewis acid catalyst is preferred. More preferred are non-hydrolytic sol-gel methods using diphenylsilanediol, tetramethyldisiloxanediol, or the like, or Lewis Acid Promoted Sol-Gel Reaction (LANHSG) using alkoxysilanes having reactive substituents under Lewis acid catalyst.
[0074] In addition, the surface coating layer of the present invention preferably has at least one or more substituents polymerizable with the polymer contained in the polymerizable polymer composition or a skeletal structure of a similar structure. The substituents polymerizable with the polymer or the compound having a similar skeletal structure are preferably contained in the surface coating layer by forming a covalent bond. There is no particular limitation on the method of forming the covalent bond, but for example, a method of introducing a substituent capable of forming a siloxane bond into a substituent polymerizable with the polymer or a compound having a similar skeletal structure, and adding it during the above-mentioned non-hydrolytic sol-gel reaction to contain it in a state in which a covalent bond is formed in the surface coating layer, or a method of introducing a substituent polymerizable with the polymer contained in the polymerizable polymer composition during the above-mentioned non-hydrolytic sol-gel reaction, and then reacting the polymer or monomer to introduce it into the surface coating layer can be suitably used.
[0075] After the surface coating layer formation step, a polymerizable polymer composition containing a reactive substituent and a polymerizable substituent is added and mixed to obtain a quantum dot-containing composition (S3 in FIG. 3, mixing step). Specifically, after forming the surface coating layer, unreacted substances are removed by purification, and the resultant mixture is mixed with a polymerizable polymer composition to produce a quantum dot-containing composition. By forming the surface coating layer, compatibility with the polymerizable polymer composition is improved, and a quantum dot-containing composition in which the quantum dots are uniformly dispersed without aggregation can be produced.
[0076] (Wavelength conversion member having quantum dot-containing composition) The wavelength conversion member of the present invention is a resin composition that is a cured product of the quantum dot-containing composition produced by the above method. The form of the wavelength conversion member in the present invention is not particularly limited, but examples thereof include a wavelength conversion film in which quantum dots are dispersed in a polymerizable polymer composition by processing into a sheet shape and then curing, and a wavelength conversion color filter patterned by inkjet or as a resist material.
[0077] The method for producing (manufacturing) the wavelength conversion member is not particularly limited; for example, the quantum dot-containing composition can be applied to a transparent film or substrate material such as PET or polyimide, cured, and laminated to obtain the wavelength conversion member.
[0078] To apply the material to transparent film, spraying methods such as spray or inkjet, spin coating or bar coater can be used.
[0079] The quantum dot-containing composition can be cured, for example, by heating a film coated with the quantum dot-containing composition at 60° C. for 2 hours and then at 150° C. for 4 hours. The quantum dot-containing composition may also be cured using a photopolymerization reaction, for example, by using a UV LED irradiation device with a wavelength of 365 nm and an output of 4000 mW / cm. 2 The composition can be cured by irradiating the composition with light for 20 seconds. Although not particularly limited, the composition can be appropriately changed depending on the application.
[0080] Here, it is preferable that a substituent capable of polymerizing with the polymer in the quantum dot-containing composition is introduced into the surface coating layer, since this makes it possible to produce a wavelength conversion member that is highly reliable after curing and is free of aggregation or curing inhibition. EXAMPLES
[0081] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these. In these examples, InP / ZnSe / ZnS core-shell quantum dots were used as the quantum dot material.
[0082] ~Example 1~ (Quantum dot core synthesis process) 0.23 g (0.9 mmol) of palmitic acid, 0.088 g (0.3 mmol) of indium acetate, and 10 mL of 1-octadecene were added to a flask, and the mixture was heated to 100° C. under reduced pressure and stirred, followed by degassing for 1 hour while dissolving the raw materials.
[0083] Thereafter, nitrogen was purged into the flask, and 0.75 mL (0.15 mmol) of a solution prepared by mixing tristrimethylsilylphosphine with trioctylphosphine to adjust the concentration to 0.2 M was added and heated to 300°C. It was confirmed that the solution turned from yellow to red and that core particles had been formed.
[0084] (Quantum dot shell layer synthesis process) Next, 2.85 g (4.5 mmol) of zinc stearate and 15 mL of 1-octadecene were added to a separate flask, and the mixture was heated to 100°C under reduced pressure and stirred. While dissolving, the mixture was degassed for 1 hour to prepare a 0.3 M zinc stearate octadecene solution. 3.0 mL (0.9 mmol) of the solution was added to the reaction solution after the core synthesis, and the solution was cooled to 200°C.
[0085] Next, 0.474 g (6 mmol) of selenium and 4 mL of trioctylphosphine were added to another flask and dissolved by heating to 150°C to prepare a 1.5 M selenium trioctylphosphine solution. The reaction solution after the core synthesis step, which had been cooled to 200°C, was heated to 320°C over 30 minutes, while the selenium trioctylphosphine solution was added in 0.1 mL increments to a total of 0.6 mL (0.9 mmol), and the mixture was kept at 320°C for 10 minutes and then cooled to room temperature. 0.44 g (2.2 mmol) of zinc acetate was added, and the mixture was dissolved by heating to 100°C under reduced pressure and stirring.
[0086] The flask was purged again with nitrogen and heated to 230° C., and 0.98 mL (4 mmol) of 1-dodecanethiol was added and held for 1 hour. The resulting solution was cooled to room temperature to prepare a solution containing core-shell quantum dots.
[0087] (Surface treatment process) (3-mercaptopropyl)triethoxysilane (Tokyo Chemical Industry Co., Ltd.) was used as a ligand having a substituent capable of forming a siloxane bond and a substituent capable of coordinating to the quantum dot surface. 0.45 g (2 mmol) of zinc bromide was dissolved in 2.4 mL of trioctylphosphine to prepare a zinc precursor solution.
[0088] Next, 0.064 g (2 mmol) of sulfur was dissolved in a mixed solution of 1.1 mL of 1-dodecanethiol and 1.1 mL of (3-mercaptopropyl)triethoxysilane to prepare a sulfur precursor solution. The core-shell type quantum dot-containing solution obtained in the quantum dot shell layer synthesis process was heated to 210°C, and 1.25 mL of the zinc precursor solution and 1.3 mL of the sulfur precursor solution were added.
[0089] After the reaction was completed, ethanol was added to precipitate the reactants, which were then centrifuged to remove the supernatant. The same purification process was repeated, and the reactants were dispersed in toluene to produce a solution in which quantum dots coordinated with ligands having substituents capable of forming siloxane bonds were dispersed.
[0090] (Surface coating layer formation process) Triethoxyvinylsilane (4.0 mmol), diphenylsilanediol (6 mmol), barium hydroxide monohydrate (0.15 mmol), and the toluene solution containing the quantum dots dispersed after the surface treatment process were added to a flask that had been purged with nitrogen, and the mixture was heated and stirred at 65°C for 24 hours. After the reaction was completed, the mixture was cooled to room temperature, ethanol was added to precipitate the reactants, the mixture was centrifuged, the supernatant was removed, and the mixture was dispersed in toluene.
[0091] (Fourier transform infrared spectroscopy) FT-IR measurements are performed by dropping a dispersion liquid containing semiconductor nanoparticles (quantum dots) directly onto a detection section using a diamond ATR (Attenuated Total Reflection), drying thoroughly, and then measuring the wavelength of the dispersion liquid from 400 to 4000 cm. -1 The measurement range was 1000 to 1200 cm, which is derived from the Si-O bond. -1 The intensity of peak A in the range of 2800 to 3000 cm -1 It was confirmed that the intensity of peak B derived from the C-H bond present in
[0092] (Quantum dot-containing composition mixing process) The solution after the surface coating layer formation process dispersed in toluene and methacrylic modified silicone oil X-32-3817-3 (Shin-Etsu Chemical Co., Ltd.) were weighed and mixed so that the quantum dots were contained at 20 wt% in terms of non-volatile content. After mixing, the solvent was removed using an evaporator to obtain a quantum dot-containing composition.
[0093] (Fabrication process of wavelength conversion material) The quantum dot-containing composition thus obtained was used to produce a wavelength conversion member. The quantum dot-containing composition was degassed using a stirring degassing machine, poured onto a PET film, and formed into a thin film using a bar coater. The formed thin film was then irradiated with a UV LED irradiation device in a nitrogen atmosphere at a wavelength of 365 nm and an output of 4000 mW / cm. 2 The quantum dot-containing resin layer was photocured by irradiating it with light for 20 seconds to prepare a wavelength conversion member having a thickness of 50 μm.
[0094] (Emission wavelength, emission half-width, emission efficiency measurement) In the examples and comparative examples, the fluorescence emission characteristics of the quantum dots were evaluated by measuring the emission wavelength, fluorescence emission half-width, and fluorescence emission efficiency (internal quantum efficiency) of the quantum dots at an excitation wavelength of 450 nm using a quantum efficiency measurement system (QE-2100) manufactured by Otsuka Electronics Co., Ltd.
[0095] (Reliability test) The obtained wavelength conversion member was treated under conditions of 85° C. and 85% RH (relative humidity) for 250 hours, and the fluorescence emission efficiency of the wavelength conversion member after the treatment was measured to evaluate its reliability.
[0096] ~Comparative Example 1~ The steps up to the quantum dot shell layer synthesis were carried out in the same manner as in Example 1, to obtain a solution in which quantum dots were dispersed.
[0097] (Surface treatment process) As a ligand having a substituent capable of forming a siloxane bond and a substituent capable of coordinating to the surface of the quantum dots, (3-mercaptopropyl)triethoxysilane (Tokyo Chemical Industry Co., Ltd.) (3.0 mmol) was added to the solution in which the quantum dots were dispersed, and the solution was stirred for 24 hours. After the reaction was completed, ethanol was added to precipitate the quantum dots in the same manner as in Example 1, and the quantum dots were purified, and then dispersed in toluene. That is, unlike Example 1, no additional ZnS was formed in the surface treatment step.
[0098] (Surface coating layer formation process) Triethoxyvinylsilane (4.0 mmol), diphenylsilanediol (6 mmol), barium hydroxide monohydrate (0.15 mmol), and the toluene solution containing the quantum dots dispersed after the surface treatment process were added to a flask that had been purged with nitrogen, and the mixture was heated and stirred at 65°C for 24 hours. After the reaction was completed, the mixture was cooled to room temperature, ethanol was added to precipitate the reactants, the mixture was centrifuged, the supernatant was removed, and the mixture was dispersed in toluene.
[0099] (Fourier transform infrared spectroscopy) FT-IR measurements are performed by dropping a dispersion liquid containing semiconductor nanoparticles (quantum dots) directly onto a detection section using a diamond ATR (Attenuated Total Reflection), drying thoroughly, and then measuring the wavelength of the dispersion liquid from 400 to 4000 cm. -1 The measurement range was 1000 to 1200 cm, which is derived from the Si-O bond. -1 The intensity of peak A in the range of 2800 to 3000 cm -1 The intensity of peak B originating from the C-H bond present in the fluorine-containing ...
[0100] (Quantum dot-containing composition mixing process) The solution after the surface coating layer formation process dispersed in toluene and methacrylic modified silicone oil X-32-3817-3 (Shin-Etsu Chemical Co., Ltd.) were weighed and mixed so that the quantum dots were contained at 20 wt% in terms of non-volatile content. After mixing, the solvent was removed using an evaporator to obtain a quantum dot-containing composition.
[0101] (Fabrication process of wavelength conversion material) The quantum dot-containing composition thus obtained was used to produce a wavelength conversion member. The quantum dot-containing composition was degassed using a stirring degassing machine, poured onto a PET film, and formed into a thin film using a bar coater. The formed thin film was then irradiated with a UV LED irradiation device in a nitrogen atmosphere at a wavelength of 365 nm and an output of 4000 mW / cm. 2 The quantum dot-containing resin layer was photocured by irradiating it with light of 1000 nm for 20 seconds to prepare a wavelength conversion member having a thickness of 50 μm. Compared to Example 1, aggregates were found in some places, and the quantum yield was lower than that of Example 1.
[0102] ~Example 2~ A toluene solution in which quantum dots were dispersed was prepared in the same manner as in Example 1 up to the surface treatment step.
[0103] (Surface coating layer formation process) [(3-triethoxysilyl)propyl]succinic anhydride (Tokyo Chemical Industry Co., Ltd.) (4.0 mmol), diphenylsilanediol (6 mmol), barium hydroxide monohydrate (0.15 mmol), and the toluene solution in which the quantum dots were dispersed after the surface treatment process were added to a flask that had been purged with nitrogen, and the mixture was heated and stirred at 65°C for 24 hours. After the reaction was completed, the mixture was cooled to room temperature, ethanol was added to precipitate the reactants, the mixture was centrifuged, the supernatant was removed, and the mixture was dispersed in toluene.
[0104] (Quantum dot-containing composition mixing process) The solution after the surface coating layer formation process dispersed in toluene and acrylic resin RA-4101 (Negami Sangyo Co., Ltd.) were weighed so that the quantum dots were contained at 20 wt% in terms of non-volatile content ratio, and 5 parts by mass of photoradical generator Irgacure 1173 was added to 100 parts by mass of the acrylic resin non-volatile content and mixed. After mixing, the toluene solvent was removed by distillation under reduced pressure to obtain a quantum dot-containing composition.
[0105] (Method of manufacturing wavelength conversion member) The obtained quantum dot-containing composition was used to produce a wavelength conversion member. The quantum dot-containing composition was vacuum degassed, and the quantum dot-containing composition with a solid content of 20% was poured into a PTFE-coated mold measuring 20 cm x 10 cm square and 500 μm thick, and heated on a hot plate at 120°C for 1 hour to evaporate the solvent and produce a quantum dot-containing resin layer. A part of the layer was cut out and developed with a PGMEA solution to confirm that there was no remaining film.
[0106] After that, the remaining quantum dot-containing resin layer was irradiated with a UV LED irradiator in a nitrogen atmosphere at a wavelength of 365 nm and an output of 4000 mW / cm 2 The film was photocured by irradiating it with light for 20 seconds to prepare a wavelength conversion member having a thickness of 100 μm.
[0107] ~Comparative Example 2~ A toluene solution in which quantum dots were dispersed was prepared in the same manner as in Comparative Example 1 up to the surface treatment step, and a wavelength conversion member was prepared in the same manner as in Example 2 except for that.
[0108] ~Example 3~ Up to the surface treatment step, a toluene solution in which quantum dots were dispersed was prepared in the same manner as in Examples 1 and 2.
[0109] (Surface coating layer formation process) Tris[3-(trimethoxysilyl)propyl]isocyanurate (1.0 mmol), diphenylsilanediol (6 mmol), barium hydroxide monohydrate (0.15 mmol), and the toluene solution containing the quantum dots dispersed after the surface treatment process were added to a flask that had been purged with nitrogen, and the mixture was heated and stirred at 65°C for 24 hours. After the reaction was completed, the mixture was cooled to room temperature, ethanol was added to precipitate the reactants, the mixture was centrifuged, the supernatant was removed, and the mixture was dispersed in toluene.
[0110] (Quantum dot-containing composition mixing process) The solution after the surface coating layer formation process in which an epoxy-containing silicone resin (manufactured by Shin-Etsu Chemical, CAS No. 2253674-54-1) was dispersed in toluene was weighed and mixed so that the quantum dots were contained at 20 wt% in terms of non-volatile content ratio. 2 parts by mass of photoacid generator CPI-310FG (manufactured by San-Apro) and 20 parts by mass of crosslinker THI-DE were weighed and mixed for 100 parts by mass of silicone resin non-volatile content. After mixing, the toluene solvent was removed by distillation under reduced pressure to obtain a quantum dot-containing composition.
[0111] (Method of manufacturing wavelength conversion member) The obtained quantum dot-containing composition was used to produce a wavelength conversion member. The quantum dot-containing composition was vacuum degassed, and the quantum dot-containing composition with a solid content of 20% was poured into a PTFE-coated mold measuring 20 cm x 10 cm square and 500 μm thick, and heated on a hot plate at 120°C for 1 hour to evaporate the solvent and produce a quantum dot-containing resin layer. A part of the layer was cut out and developed with a PGMEA solution to confirm that there was no remaining film.
[0112] After that, the remaining quantum dot-containing resin layer was irradiated with a UV LED irradiator in a nitrogen atmosphere at a wavelength of 365 nm and an output of 4000 mW / cm 2The film was photocured by irradiating it with light for 20 seconds to prepare a wavelength conversion member having a thickness of 100 μm.
[0113] ~Comparative Example 3~ A toluene solution in which quantum dots were dispersed was prepared in the same manner as in Comparative Example 1 up to the surface treatment step, and a wavelength conversion member was prepared in the same manner as in Example 3 except for that.
[0114] ~Example 4~ A toluene solution in which quantum dots were dispersed was prepared in the same manner as in Examples 1, 2, and 3 up to the surface treatment step.
[0115] (Surface coating layer formation process) Triethoxysilylpropyl methacrylate (4.0 mmol), diphenylsilanediol (6 mmol), barium hydroxide monohydrate (0.15 mmol), and the toluene solution in which the quantum dots after the surface treatment process were dispersed were added to a flask that had been purged with nitrogen, and the mixture was heated and stirred at 65°C for 24 hours. After the reaction was completed, the mixture was cooled to room temperature, ethanol was added to precipitate the reactants, the mixture was centrifuged, the supernatant was removed, and the mixture was dispersed in toluene.
[0116] (Quantum dot-containing composition mixing process) The solution after the surface coating layer formation process, in which a phenol-crosslinkable silicone resin (manufactured by Shin-Etsu Chemical, CAS No. 916059-41-1) was dispersed in toluene, was weighed and mixed so that the quantum dots were contained at 20 wt% in terms of non-volatile content ratio. 2 parts by mass of photoacid generator CPI-310FG (manufactured by San-Apro) and 20 parts by mass of crosslinker THI-DE were weighed and mixed with respect to 100 parts by mass of silicone resin non-volatile content. After mixing, the toluene solvent was removed by distillation under reduced pressure to obtain a quantum dot-containing composition.
[0117] (Method of manufacturing wavelength conversion member) The obtained quantum dot-containing composition was used to produce a wavelength conversion member. The quantum dot-containing composition was vacuum degassed, and the quantum dot-containing composition with a solid content of 20% was poured into a PTFE-coated mold measuring 20 cm x 10 cm square and 500 μm thick, and heated on a hot plate at 120°C for 1 hour to evaporate the solvent and produce a quantum dot-containing resin layer. A part of the layer was cut out and developed with a PGMEA solution to confirm that there was no remaining film.
[0118] After that, the remaining quantum dot-containing resin layer was irradiated with a UV LED irradiator in a nitrogen atmosphere at a wavelength of 365 nm and an output of 4000 mW / cm 2 The film was photocured by irradiating it with light for 20 seconds to prepare a wavelength conversion member having a thickness of 100 μm.
[0119] ~Comparative Example 4~ A toluene solution in which quantum dots were dispersed was prepared in the same manner as in Comparative Example 1 up to the surface treatment step, and a wavelength conversion member was prepared in the same manner as in Example 4 except for the above.
[0120] Table 1 shows the results of comparing Examples 1 to 4 with Comparative Examples 1 to 4.
[0121] [Table 1]
[0122] The emission wavelength, fluorescence half-width and internal quantum efficiency after quantum dot synthesis, after the surface treatment process, after the formation of the surface coating layer, after the mixing process (quantum dot-containing composition), and after hardening of the quantum dot-containing composition (wavelength conversion member), the rate of decrease in internal quantum efficiency during reliability testing, and the presence or absence of aggregates in the wavelength conversion member are shown in Table 1. Table 1 also shows the results of FT-IR after the formation of the surface coating layer.
[0123] As can be seen from the results in Table 1, in all of the Examples, peak A in the FT-IR after the formation of the surface coating layer was larger than peak B, whereas in the Comparative Examples, peak B was larger than peak A, and the internal quantum efficiency was also inferior after the surface treatment process, after the formation of the surface coating layer, and after the preparation of the quantum dot-containing composition.
[0124] Furthermore, it is found that the internal quantum efficiency after the wavelength conversion member is produced in the comparative example is lower than that in the examples, and the emission wavelength is also significantly shifted to longer wavelengths. This is probably because the comparative example has insufficient dispersion stability and aggregates are formed.
[0125] In addition, when the results of the reliability test (treated at 85°C and 85% RH for 250 hours) of the Example and Comparative Example were compared, the stability was about the same due to the formation of the surface coating layer, but the Comparative Example showed greater deterioration than the Example.
[0126] Thus, in the examples, in a reliability test at 85°C and 85% RH without a barrier film, it was found that the rate of decrease in internal quantum efficiency during 250 hours of treatment (the rate of decrease in internal quantum efficiency after treatment) was suppressed to within 10%, making stabilization possible.
[0127] As described above, it has been confirmed that the quantum dot-containing composition of the present invention exhibits high internal quantum efficiency and stability, has good film quality after curing, and can be applied to quantum dot-containing resists and quantum dot-containing inkjet inks.
[0128] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.
Claims
1. A quantum dot-containing composition containing quantum dots that emit fluorescence when exposed to excitation light, The quantum dot-containing composition is a mixture of quantum dots and a polymerizable polymer composition, the quantum dots have a core-shell structure with an outermost shell being ZnS, and the quantum dot surfaces contain a surface coating layer having a siloxane bond; The quantum dots are characterized by Fourier transform infrared spectroscopy at 1000 to 1200 cm -1 The peak intensity present in the range of 2800 to 3000 cm -1 The quantum dot-containing composition is characterized in that the peak intensity is greater than that present in the
2. The quantum dot-containing composition according to claim 1, characterized in that the surface coating layer has one or more reactive substituents selected from the group consisting of a vinyl group, an acrylic group, a methacrylic group, a hydroxyl group, a phenolic hydroxyl group, and an epoxy group.
3. The polymer contained in the polymerizable polymer composition contains one or more of a vinyl group, an acrylic group, a methacrylic group, a hydroxyl group, a phenolic hydroxyl group, and an epoxy group as a substituent polymerizable with the reactive substituent. The quantum dot-containing composition according to claim 2, characterized in that the polymer contains one or more of a vinyl group, an acrylic group, a methacrylic group, a hydroxyl group, a phenolic hydroxyl group, and an epoxy group as a substituent polymerizable with the reactive substituent.
4. A wavelength conversion member comprising a cured product of the quantum dot-containing composition according to any one of claims 1 to 3.
5. A method for producing a quantum dot-containing composition containing quantum dots that emit fluorescence when exposed to excitation light, comprising: a surface treatment step of heating and mixing a solution in which quantum dots having ZnS formed on the outermost shell are dispersed, a ligand having a substituent capable of forming a siloxane bond and a thiol group, and a solution containing a zinc precursor and a sulfur precursor, thereby forming additional ZnS on the outermost surface of the quantum dots while coordinating the ligand; a surface coating layer forming step of forming a surface coating layer having a siloxane bond by reacting the substituent capable of forming a siloxane bond with a compound having a reactive substituent capable of forming a siloxane bond after the surface treatment step; A method for producing a quantum dot-containing composition, comprising: a mixing step of adding and mixing a polymerizable polymer composition containing the reactive substituent and a polymerizable substituent after the surface coating layer forming step.
Citation Information
Patent Citations
Photosensitive resin composition, photosensitive resin coating, photosensitive dry film, pattern forming method, and light emitting element
JP2021089347A
Display device
JP2022027519A
Coated semiconductor nanoparticles and manufacturing method therefor
WO2021235152A1
Wavelength conversion member, backlight unit, liquid crystal display device, and method for manufacturing wavelength conversion member
JP2016111292A
Gas barrier coatings for semiconductor nanoparticles
JP2019536653A
Cited By
High-light-transmittance weather-proof coated glass for photovoltaic module and preparation method of high-light-transmittance weather-proof coated glass
CN121406235A