Method for producing steel slag hydrated matrix

The method addresses fluidity and strength issues in producing hydrated solidified steel slag by optimizing the mixing of steelmaking slag, binder, and water ratios, enabling efficient production and use in roadbed materials with improved expansion stability.

JP2024169318AActive Publication Date: 2024-12-05JFE STEEL CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024068927
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2024-04-22
Publication Date
2024-12-05
Estimated Expiration
2044-04-22

AI Technical Summary

Technical Problem

Existing methods for producing hydrated solidified steel slag face issues with poor fluidity, requiring specialized equipment and complex operations, and result in low workability due to the fine particle size and low fluidity of powdered steelmaking slag.

Method used

A method involving mixing steelmaking slag, a binder, and water, with specific ratios and particle sizes, to achieve appropriate fluidity and strength, using CaO/SiO2 mass ratio of 1.4 or more and P2O5 content of 0.3% or less, with a water-to-binder ratio of 0.60 to 0.90, and a maximum particle size of 15 mm or less.

Benefits of technology

Ensures proper fluidity and strength of the mixture, allowing for easier production and use in roadbed materials without the need for specialized equipment, with early road opening and improved expansion stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169318000001
    Figure 2024169318000001
  • Figure 2024169318000002
    Figure 2024169318000002
  • Figure 2024169318000003
    Figure 2024169318000003
Patent Text Reader

Abstract

To provide a method for producing steel slag hydrated matrix that can ensure appropriate fluidity of a mixture of water and a material that contains powdery steel slag.SOLUTION: A method for producing steel slag hydrated matrix includes: a mixing step in which a mixture is produced by mixing water with a material that contains steel slag containing CaO, SiO2, and P2O5, and a binder that contains fine powders of blast furnace slag; and a hardening step in which the mixture is hardened. The steel slag has a mass ratio of CaO / SiO2 of 1.4 or more and a P2O5 content of 0.3 mass% or less. In the mixing step, the water, the blast furnace slag, and the binder are added so as to satisfy the following relation. Volume of water / (Volume of binder+volume of steel slag)=0.60-0.90.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a steel slag hydrated body produced by hardening a mixture of a material containing steelmaking slag and water. [Background technology]

[0002] Some steelmaking slags generated during reduction refining, such as secondary refining slags and smelting reduction slags, contain less P2O5 than other steelmaking slags. Steelmaking slags with high basicity, as indicated by CaO / SiO2, contain dicalcium silicate as the main mineral phase. In steelmaking slags with low P2O5 content, the dicalcium silicate undergoes a phase transformation from α' to γ ​​during the solidification process.

[0003] Steelmaking slag having a basicity of 1.4 or more and a P2O5 content of 0.3 mass% or less tends to be pulverized due to the phase transformation. Slag that satisfies the above conditions of basicity and P2O5 mass% is hereinafter referred to as pulverized steelmaking slag.

[0004] Powdered steel slag is not suitable as an aggregate for hydrated solidified bodies because of its fine particle size. Attempts have been made to use such powdered steel slag as a hydrated solidified body. For example, Patent Document 1 describes a method for producing a hardened slag body by adding water to a mixture containing powdered steel slag and a SiO2-containing substance with latent hydraulic properties, mixing the mixture, and then molding the mixture under a specified pressure.

[0005] Meanwhile, steelmaking slag is also used as a material for roadbeds. For example, Patent Document 2 describes that a steelmaking slag-containing composition obtained by compacting a composition containing steelmaking slag, ground granulated blast furnace slag, and water is used as a pavement slab. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2001-114547 A [Patent Document 2] JP 2015-196631 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, when the manufacturing method described in Patent Document 1 is used, there is a problem that the fluidity of the powdered steel slag is poor, which deteriorates workability. For this reason, in the manufacturing method of Patent Document 1, molding is performed at a predetermined pressure. Therefore, it is necessary to newly install dedicated equipment for this molding, and improvements are required in terms of introduction costs. In addition, the operation of the equipment is complicated, and improvements are required in terms of work efficiency.

[0008] Furthermore, when a steel slag-containing composition is produced using powdered steel slag as described in Patent Document 2, the fluidity of the mixture containing the powdered steel slag and water is extremely low, which makes it difficult to produce the steel slag-containing composition.

[0009] The present invention has been made in consideration of the above circumstances, and aims to provide a method for producing a steel slag hydrated body that can easily ensure appropriate fluidity of a mixture of a material containing powdered steelmaking slag and water. [Means for solving the problem]

[0010] In order to solve the above problems, the present invention has the following features. [1] CaO, SiO 2、 A mixing step of mixing a material including a steelmaking slag containing P2O5 and a binder including ground granulated blast furnace slag with water to generate a mixture; and a curing step of curing the mixture, The steelmaking slag has a CaO / SiO2 mass ratio of 1.4 or more and a P2O5 content of 0.3 mass% or less, A method for producing a steel slag hydrated body, wherein in the mixing step, the water, the steelmaking slag, and the binder are added so as to satisfy the following relationship: Volume of water / (volume of binder + volume of steelmaking slag) = 0.60~0.90 [2] The content of the steel slag in the mixture is 1 m 3 The method for producing a steel slag hydrated body according to [1], wherein the amount of the hydrated body is 370 kg or less per unit time. [3] The method for producing a steel slag hydrated body according to [1] or [2], wherein the steelmaking slag has a maximum particle size of 15 mm or less. Effect of the Invention

[0011] According to the method for producing a steel slag hydrated solid of the present invention, in the mixing step in which the material and water are mixed to produce a mixture, each component is added in an amount that satisfies the above-mentioned relationship, thereby ensuring appropriate fluidity of the mixture. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention relates to a method for producing a hydrated iron and steel slag product, and more particularly to a method for producing a hydrated iron and steel slag product comprising the steps of: mixing steel slag, a material containing a binder, and water to produce a mixture; and hardening the mixture.

[0013] The steelmaking slag is not particularly limited, but may contain CaO, SiO 2、 It contains P2O5. Steelmaking slag has a CaO / SiO2 mass ratio of 1.4 or more and a P2O5 content of 0.3 mass% or less. Here, a P2O5 content of 0.3 mass% or less may be a content below the detection limit of a device for detecting P2O5. In other words, it is sufficient that P2O5 may be contained in steelmaking slag, and the content may be so small that it cannot actually be detected by a detection device. Note that general steelmaking slag contains P2O5, and the probability that the content exceeds 0.3 mass% is very high.

[0014] As such steelmaking slag, slag with a CaO / SiO2 ratio of 2.0 or more is preferable because it has a large amount of dicalcium silicate precipitation. For example, secondary refining slag generated during secondary refining of molten steel in a vacuum degassing device, or smelting reduction refining slag generated when molten mother metal is directly melted with Cr ore before the production of stainless steel, may be used.

[0015] In steelmaking slag with this composition, the dicalcium silicate phase precipitates when cooled. In addition, because the steelmaking slag contains a small amount of P2O5, the dicalcium silicate transforms into the γ phase, causing the steelmaking slag to pulverize. Therefore, hereafter, steelmaking slag with this composition is also referred to as powdered steelmaking slag.

[0016] The maximum particle size of the powdered steel slag is preferably 15 mm or less, more preferably 10 mm or less, and even more preferably 5 mm or less. By making the maximum particle size of the powdered steel slag 15 mm or less, it is possible to reduce the expansion due to hydration of the steel slag hydrated body obtained by hardening a mixture of the material and water. In other words, it is possible to increase the expansion stability of the steel slag hydrated body.

[0017] The maximum particle size of the pulverized steel slag is the particle size represented by the smallest mesh size of a sieve through which all of the pulverized steel slag passes. The mesh size used in the sieve analysis is not particularly limited, but for example, the mesh size specified in JIS Z 8801 can be used. Specifically, when the maximum particle size of the pulverized steel slag is to be 15 mm or less, a sieve with a nominal size of 15 mm has a mesh size of 16 mm, so it is preferable to use pulverized steel slag that passes entirely through a sieve with a mesh size of 16 mm.

[0018] The material may also include steel slag that does not meet the requirements for pulverized steel slag described above.

[0019] The binder includes ground granulated blast furnace slag. For example, ground granulated blast furnace slag can be used. For example, ground granulated blast furnace slag used in JIS R 5211 2009 "Blast furnace cement" or ground granulated blast furnace slag conforming to JIS A 6206 2013 "Blast furnace slag for concrete" can be used.

[0020] The specific surface area of ​​ground granulated blast furnace slag produced by the Blaine method is approximately 3000 cm 2 / g or more. In addition, the specific surface area of ​​ground granulated blast furnace slag by the Blaine method is preferably 4000 cm 2 / g or more, the activity index, which is an index of hydraulic property, is high, which is more preferable.

[0021] The binder is not particularly limited, and may be an alkaline stimulant or a silica-containing substance having pozzolanic reactivity. Examples of the alkaline stimulant include hydrated lime and ordinary Portland cement as specified in JIS R 5210 2019. Examples of the silica-containing substance having pozzolanic reactivity include fly ash and silica fume.

[0022] Examples of such silica-containing substances include those conforming to JIS R 5210 2009 "Portland cement", JIS R 5211 2009 "Blast-furnace cement", and JIS A 6201 2015 "Fly ash for concrete".

[0023] The material may contain a water reducing agent. By containing a water reducing agent in the material, the amount of water added to the mixture can be reduced and the dispersibility of the material can be increased. By reducing the amount of water added to the mixture, the strength of the steel slag hydrated body can be increased.

[0024] As the water reducing agent, for example, a polycarboxylic acid type water reducing agent can be used. The amount of the water reducing agent used is preferably 0.3 to 0.5 mass% of the unit amount of binder. The unit amount of binder is 1 m of the mixture.3 is the mass of binder contained in

[0025] In the mixing step, materials including water, pulverized steel slag, and a binder are added so as to satisfy the following relationship: Volume of water / (volume of binder + volume of powdered steel slag) = 0.60~0.90 The volume ratio is preferably 0.65 to 0.85, more preferably 0.65 to 0.80, and even more preferably 0.70 to 0.75.

[0026] By setting the ratio of the volume of water to the volume of powdered steel slag and binder (hereinafter also referred to as the main material) to 0.60 or more, it is possible to impart appropriate fluidity to the mixture of the materials and water.

[0027] In addition, as the ratio of the volume of water to the volume of the main material increases, i.e., as the volume of water in the mixture increases, the strength of the steel slag hydrate tends to decrease. In addition, as the volume of the main material becomes smaller than the volume of water, the amount of powdered steel slag added decreases, and the amount of powdered steel slag used decreases. For this reason, it is recommended that the ratio of the volume of water to the volume of the main material in the mixture be 0.90 or less.

[0028] The unit powdered steel slag content of the steel slag hydrated body is 370 kg / m 3 In other words, the content of pulverized steel slag in the mixture should be less than 1 m 3 The weight is preferably 370 kg or less, more preferably 70 to 370 kg, even more preferably 80 to 350 kg, and even more preferably 90 to 350 kg.

[0029] The powdered steel slag content of the mixture is 3 By keeping the amount of free CaO and free MgO in the mixture at 370 kg or less per unit area, the amount of free CaO and free MgO in the mixture is suppressed, and as a result, sufficient expansion stability can be ensured when the mixture is made into a steel slag hydrated solidified body.

[0030] In addition, the powdered steel slag content of the mixture is 1m 3 If the amount of powdered steel slag exceeds 370 kg / m, the fluidity of the mixture tends to decrease. 3 The content of powdered steel slag in the mixture is preferably 1 m 3 A concentration of 70 kg or more per unit area is preferable because it increases the amount of powdered steel slag added, promoting its utilization.

[0031] The mixing in the mixing step is not particularly limited, but for example, mixing can be performed using a concrete mixer under room temperature conditions.

[0032] In the hardening step for hardening the mixture, a hardening method used in the fields of cement and concrete can be adopted. For example, the mixture can be hardened by curing in water at 20°C. The processing time of the hardening step can be adjusted appropriately depending on the temperature, humidity, etc. EXAMPLES

[0033] (Test Example 1: Fluidity Evaluation) A mixture was produced by mixing powdered steel slag, a material containing a binder, and water. By changing the blending amounts of the materials when producing the steel slag hydrated body, Examples 1 to 6 and Comparative Examples 1 and 2 were produced, and the fluidity of each mixture was evaluated.

[0034] (material) The materials used for the mixture were powdered steelmaking slag, steelmaking slag (hereinafter also referred to as slag A), a binder, and a water-reducing agent.

[0035] As the powdered steelmaking slag, two types of secondary refining slag with the compositions shown in Table 1 were used. The detection limit of the detection device used to detect P2O5 was 0.05 mass%. In Table 1, the P2O5 content of powdered steelmaking slag 2 is expressed as <0.05 mass% because, although there is a possibility that P2O5 is contained, the content is below the detection limit of the detection device. The units of the values ​​shown in Table 1 are mass% except for the item "CaO / SiO2".

[0036] [Table 1]

[0037] Slag A is an aggregate. Slag A is not limited to slag, and crushed stone can also be used. In this embodiment, steel slag with a maximum particle size of 40 mm or less is used as slag A. When steel slag is used as slag A, it is preferable that the PO content is higher than 0.3 mass % and that the slag is not powdered.

[0038] The binders used were ground granulated blast furnace slag and ordinary Portland cement as specified in JIS R 5210 2019. The densities of ground granulated blast furnace slag, ordinary Portland cement, and powdered steel slag are shown in Table 2. In the following test examples, the cases where ground granulated blast furnace slag, ordinary Portland cement, and powdered steel slag were used as the main materials will be described.

[0039] [Table 2]

[0040] As the water reducing agent, a polycarboxylic acid-based high performance water reducing agent (Tupol manufactured by Takemoto Oil Co., Ltd.) was used.

[0041] The mixtures of Examples 1 to 6 and Comparative Examples 1 and 2 were prepared according to the formulations shown in Table 3.

[0042] (fluidity and strength evaluation) The materials were mixed with water to prepare a mixture, which was then poured into concrete. The mixture was allowed to harden at room temperature, and the form was removed the next day. The hardened mixture was then cured underwater at 20°C for up to 7 days to produce a hydrated steel slag body.

[0043] The fluidity of the mixture was evaluated based on the fluidity of the mixture when producing the steel slag hydrated solidified body. The slump value at the time of mixing (see JIS A 1101 Slump Test Method for Concrete) was measured. The target value for slump was set at 3.0 cm to 20.0 cm, taking into consideration the slip form method or manual construction. The strength of the steel slag hydrated solidified body was evaluated using the method shown below.

[0044] The strength of the steel slag hydrated body was evaluated by measuring the bending strength at 7 days according to JIS A 1108 2018. The bending strength was evaluated at 4.5 N / mm, which is the nominal strength of pavement concrete specified in JIS A 5308 2019 "Ready Mixed Concrete". 2 The bending strength evaluations of Examples 1 to 6 and Comparative Examples 1 and 2 are shown in Table 3. In the following tables, the strength evaluation is based on the 7-day bending strength (N / mm 2 ) should be written.

[0045] [Table 3]

[0046] In Examples 1 to 6, in which the water volume / main material volume ratio was 0.60 to 0.90, appropriate mixture fluidity was obtained. In addition, the steel slag hydrated bodies obtained by hardening Examples 1 to 6 had appropriate bending strength.

[0047] In contrast, in Comparative Example 1, where the water volume / main material volume ratio was less than 0.60, the mixture had lower fluidity than Invention Examples 1 to 6, and casting was difficult. In Comparative Example 2, where the water volume / main material volume ratio exceeded 0.90, the fluidity was too high and it was not suitable for paving concrete. In addition, the strength of the steel slag hydrated bodies in Comparative Examples 1 and 2 was lower than Invention Examples 1 to 6, and appropriate strength was not obtained.

[0048] By the way, the bending strength of pavement concrete after 28 days is 4.5N / mm 2 In the case of Examples 1 to 6, strength exceeding the prescribed value was achieved seven days after casting. Therefore, when the steel slag hydrated bodies of Examples 1 to 6 are used as a substitute for pavement concrete, it is possible to open the road to traffic early.

[0049] (Test Example 2: Expansion evaluation of hydrated iron and steel slag bodies) By changing the blend ratio of the mixture used to produce the steel slag hydrated solidified body, Examples 7 to 10 and Comparative Example 3 were prepared, and the fluidity and expansiveness of each mixture were evaluated. The mixtures of Examples 7 to 10 and Comparative Example 3 were prepared with the blend ratios shown in Table 4. The mixtures of Examples 1 to 3 and 6 tested in Test Example 1 were also subjected to the test in Test Example 2.

[0050] The mixtures of Examples 7 to 10 and Comparative Example 3 were prepared in the same manner as in Test Example 1. Fluidity was also evaluated in the same manner as in Test Example 1. The mixtures of Examples 7 to 10 and Comparative Example 3 were prepared in the blending amounts shown in Table 4. The mixtures of Examples 1 to 3 and 6 tested in Test Example 1 were also subjected to the test in Test Example 2.

[0051] Specifically, for Examples 6 to 10, the powdered steel slag content of the mixture was 1 m 3 The mixture was prepared so that the content of powdered steel slag in the mixture was 370 kg or less per m3 and the ratio of the volume of water to the volume of the main material was 0.60 to 0.90. 3 The weight of the main material is 370 kg or less per unit area, and the ratio of the volume of water to the volume of the main material is 0.60 to 0.90.

[0052] In addition, in Comparative Example 3, the powdered steel slag content of the mixture was 1m 3 We created a material that did not satisfy any of the following conditions: weight per unit area: 370 kg or less; and the water volume / main material volume ratio: 0.60 to 0.90.

[0053] (Expansion evaluation) The materials were mixed with water to prepare a mixture, which was then poured. The mixture was allowed to harden at room temperature, and the form was removed the next day. The hardened mixture was then cured underwater at 20°C for up to 7 days to produce a hydrated steel slag mass. An expansion test was then conducted on the hydrated steel slag mass.

[0054] The steel slag hydrated solidified bodies were immersed in 80°C water for 10 consecutive days, after which the external appearance of the steel slag hydrated solidified bodies was observed to check for the presence or absence of large cracks. Those for which no cracks were observed during the observation were rated as "passed," and those for which cracks were observed were rated as "failed." In addition, for mixes that had poor fluidity and could not be poured, both the 7-day bending strength and expansiveness were rated as "immeasurable."

[0055] [Table 4]

[0056] In the invention example 1, the ratio of the volume of water to the volume of the main material is 0.60 to 0.90. In the invention examples 2 to 3 and 6 to 10, the content of powdered steel slag in the mixture is 1 m 3 The weight of the container must be 370 kg or less per container, and the ratio of the volume of water to the volume of main material must be 0.60 to 0.90.

[0057] The mixtures of Examples 1 to 3 and 6 to 10 had a slump value in the range of 3.5 to 20.0 and had appropriate fluidity. The bending strength of the steel slag hydrated bodies obtained by hardening the mixtures of Examples 1 to 3 and 6 to 10 was 4.5 N / mm 2 That was all.

[0058] As mentioned above, pavement concrete has a bending strength of 4.5 N / mm2 after 28 days. 2 It is stipulated that. For Examples 1 to 3 and 6 to 10, strength equal to or greater than the stipulated value was obtained 7 days after pouring. Therefore, when the steel slag hydrated solidified bodies of Examples 1 to 3 and 6 to 10 are used as substitutes for pavement concrete, it is possible to open the road to traffic at an early stage. Furthermore, no cracks were found in the steel slag hydrated solidified bodies of Examples 2 to 3 and 6 to 10 in an expansion evaluation. Therefore, the steel slag hydrated solidified bodies of Examples 2 to 3 and 6 to 10 can also be used as roadbed materials.

[0059] In Comparative Example 3, the mixture had low fluidity and was difficult to cast. Therefore, it was impossible to measure the expansion evaluation in Comparative Example 3. In addition, 3 In Example 1, which exceeded 370 kg per unit weight, cracks were confirmed in the expansion property evaluation.

[0060] (Test Example 3: Evaluation of the physical properties of powdered steelmaking slag by particle size) The mixture ratio in producing the iron and steel slag hydrated material was changed to prepare Invention Examples 11 and 8 and Comparative Examples 1 and 2, and the fluidity and expansiveness of each mixture were evaluated.

[0061] The mixtures of Examples 11 and 8 and Comparative Examples 1 and 2 were prepared in the same manner as in Test Example 1. The fluidity was also evaluated in the same manner as in Test Example 1. The mixtures of Examples 11 and 8 and Comparative Examples 1 and 2 were prepared according to the formulations shown in Table 5.

[0062] Specifically, for Example 11, powdered steel slag classified to a maximum particle size of 10 mm or less using a sieve was used as the material, and the water volume / main material volume ratio was set to 0.60 to 0.90. In Table 5, the powdered steel slag is listed as powdered steel slag 1 (0-10 mm). The composition of Example 11 is the same as that of Example 5, except for the maximum particle size of the powdered steel slag.

[0063] In addition, in Table 5, the powdered steelmaking slag of Example 8 is referred to as powdered steelmaking slag 1 (0-40 mm) to make it easier to understand the difference from the maximum particle size of the powdered steelmaking slag of Example 11.

[0064] Comparative Examples 1 and 2 are the same as Test Example 1, so the explanation will be omitted.

[0065] (Expansion evaluation) The appearance of the steel slag hydrated solid was observed to check for the presence or absence of large cracks (cracks that may affect the strength of the structure). In the observation, those that did not have large cracks were rated as "◎", those that did not have large cracks but had small cracks (cracks that do not affect the strength of the structure) or pop-outs (a phenomenon in which the surface peels off like a cone-shaped dish) were rated as "◯", and those that had large cracks were rated as "×". The expansion evaluations of Examples 11 and 8 and Comparative Examples 1 and 2 are shown in Table 5.

[0066] [Table 5]

[0067] The mixture of Example 11 had a slump value in the range of 3.5 to 20.0, and had appropriate fluidity. No cracks were observed in Example 11. The mixture of Example 8 had appropriate fluidity. Although there was a small pop-out in Example 8, no cracks were observed. As mentioned above, Comparative Example 1 had low fluidity and was difficult to cast. Comparative Example 2 had too high fluidity and was not suitable for paving concrete. Comparative Examples 1 and 2 had a unit powdered steel slag amount of 370 kg / m 3 After immersion at 80°C for 10 days, large cracks were observed. The 7-day bending strength was also 4.5N / mm 2 The results were as follows.

[0068] As described above, when it is required to meet high levels of requirements regarding the fluidity of the mixture, the strength of the steel slag hydrated body, and the expansion stability of the steel slag hydrated body, it has been confirmed that it is best to produce the steel slag hydrated body using powdered steelmaking slag with a maximum particle size of 10 mm or less.

Claims

1. CaO, SiO 2 , P 2 O 5 A mixing step of mixing a material containing steel slag and a binder containing ground granulated blast furnace slag with water to generate a mixture; and a curing step of curing the mixture, The steelmaking slag is CaO / SiO 2 The mass ratio of P is 1.4 or more, 2 O 5 The content is 0.3 mass% or less, A method for producing a steel slag hydrated body, wherein in the mixing step, the water, the steelmaking slag, and the binder are added so as to satisfy the following relationship: Volume of water / (volume of binder+volume of steelmaking slag)=0.60-0.90

2. The content of the steel slag in the mixture is 1 m 3 The method for producing an iron and steel slag hydrated solidified body according to claim 1, wherein the weight of the iron and steel slag hydrated solidified body is 370 kg or less per unit time.

3. The method for producing a steel slag hydrated body according to claim 1 or 2, wherein the steelmaking slag has a maximum particle size of 15 mm or less.

Citation Information

Patent Citations

  • Method for fixing fluorine, method for stabilizing industrial waste containing fluorine, and material to be embedded in earth and its production

    JP2000225383A

  • Stabilizing treatment of steel-making slag, embedding material in soil and its production

    JP2000335946A

  • Method for agglomerating steelmaking slag

    JP2001049310A

  • Method for producing steelmaking slag hardened body

    JP2001114550A

  • Production process of steelmaking slag hardened body

    JP2002241169A