Liquid crystal composition, dye compound, liquid crystal layer, and light control element
A liquid crystal composition with a polymerizable compound and non-polymerizable liquid crystal compound forms a polymer network, ensuring effective light-shielding and heat-resistant properties for smart windows.
Patent Information
- Application Number
- JP2023086787
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Liquid crystal layers in light control elements require sufficient light-shielding properties without voltage and must maintain these properties under high-temperature conditions to prevent deterioration due to heat.
A liquid crystal composition containing a polymerizable compound with specific absorption wavelengths and a non-polymerizable liquid crystal compound, forming a polymer network that disperses the liquid crystal, providing a guest-host type liquid crystal layer with enhanced light-shielding properties and heat resistance.
The composition achieves sufficient light-shielding without voltage and maintains these properties under heat, suitable for applications like smart windows with improved contrast and durability.
Smart Images

Figure 2024169924000086 
Figure 2024169924000001 
Figure 2024169924000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystal composition, a dye compound, a liquid crystal layer, and a light control element. [Background technology]
[0002] Liquid crystal materials are not only used in various display elements that display characters, images, and videos, such as those on TVs and smartphones, but are also being put to practical use as light control elements that adjust the transmission of light. Dye compounds with various properties are used for liquid crystal materials depending on the purpose (for example, Patent Document 1).
[0003] In recent years, in the fields of building materials and transportation, so-called polymer-dispersed (polymer network-type) liquid crystal elements have been attracting attention as light-control elements for smart windows and smart glass that adjust the degree of transmission of external light to improve spatial comfort and convenience. Polymer-dispersed liquid crystal elements have a liquid crystal layer (light-control layer) in which liquid crystal material is interposed (or dispersed) in a polymer network, and the degree of light transmission / scattering in the liquid crystal layer can be adjusted by applying a voltage. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] U.S. Pat. No. 5,578,419 [Patent Document 2] International Publication No. 2022 / 138418 Summary of the Invention [Problem to be solved by the invention]
[0005] The liquid crystal layer of the light control element is required to have sufficient light blocking properties when a voltage is applied. In addition, since the light control element may be used in a high-temperature environment, it is important that the light blocking properties of the liquid crystal layer are not deteriorated by heat, that is, that the liquid crystal layer has heat resistance.
[0006] An object of the present invention is to provide a liquid crystal layer that has sufficient light-shielding properties when no voltage is applied and is not susceptible to deterioration of the light-shielding properties due to heat. Another object of the present invention is to provide a liquid crystal composition for forming the liquid crystal layer. Another object of the present invention is to provide a light-adjusting element using the liquid crystal composition. Another object of the present invention is to provide a novel dye compound for use in the liquid crystal composition. [Means for solving the problem]
[0007] Some aspects of the present invention provide the following [1] to
[11] .
[0008] [1] Contains a polymerizable compound, a polymerization initiator, and a non-polymerizable liquid crystal compound; The liquid crystal composition, wherein the polymerizable compound comprises a first polymerizable compound having a maximum absorption wavelength in the range of 370 to 780 nm, and a second polymerizable compound not having a maximum absorption wavelength in the range of 370 to 780 nm.
[0009] [2] The liquid crystal composition according to [1], wherein the first polymerizable compound includes two or more compounds having different maximum absorption wavelengths.
[0010] [3] The liquid crystal composition according to [1] or [2], wherein the first polymerizable compound includes a compound having an anthraquinone skeleton.
[0011] [4] The first polymerizable compound is represented by the following formula (1): [ka] [In the formula, A 1 and A 2 are each independently (a) a 1,4-cyclohexylene group (in this group, one -CH- or two or more non-adjacent -CH- groups may each be independently replaced by -O- or -S-, and -CH= in this group may be replaced by -N=), (b) a 1,4-phenylene group (in which one -CH= or two or more non-adjacent -CH= groups may be replaced by -N=), (c) 1,4-cyclohexenylene group, bicyclo[2.2.2]octane-1,4-diyl group, naphthalene-2,6-diyl group, naphthalene-1,4-diyl group, 1,2,3,4-tetrahydronaphthalene-2,6-diyl group, 5,6,7,8-tetrahydronaphthalene-1,4-diyl group, decahydronaphthalene-2,6-diyl group, anthracene-2,6-diyl group, anthracene-1,4-diyl group, anthracene-9,10-diyl group, phenanthrene-2, 7-diyl group (one -CH= or two or more non-adjacent -CH= present in a naphthalene-2,6-diyl group, a naphthalene-1,4-diyl group, a 1,2,3,4-tetrahydronaphthalene-2,6-diyl group, a 5,6,7,8-tetrahydronaphthalene-1,4-diyl group, an anthracene-2,6-diyl group, an anthracene-1,4-diyl group, an anthracene-9,10-diyl group, or a phenanthrene-2,7-diyl group may be replaced by -N=), and (d) a thiophene-2,5-diyl group, a thiophene-2,4-diyl group, a benzothiophene-2,5-diyl group, a benzothiophene-2,6-diyl group, a dibenzothiophene-3,7-diyl group, a dibenzothiophene-2,6-diyl group, or a thieno[3,2-b]thiophene-2,5-diyl group (one -CH= or two or more non-adjacent -CH=s in these groups may be replaced by -N=). or a single bond, and hydrogen atoms present in the groups (a), (b), (c) and (d) may each independently be replaced by a methyl group, an ethyl group, a propyl group, a 2-propyl group, a butyl group, a 2-butyl group, a methoxy group, an ethoxy group, a methylthio group, an ethylthio group, a dimethylamino group, a diethylamino group, a cyano group, a nitro group, a fluorine atom or a chlorine atom; Z 1 and Z 2 each independently represents a single bond, -N=CH-, -CH=N-, -N=N-, -C≡C-, a linear or branched alkylene group having 1 to 20 carbon atoms, or a linear or branched alkenylene group having 2 to 30 carbon atoms, in which one or more -CH2- in the alkylene group and alkenylene group are optionally substituted with -O-, -COO- or -OCO-, and a hydrogen atom present in the alkylene group and alkenylene group is optionally substituted with a fluorine atom, R 1 and R 2 each independently represents a hydrogen atom, a non-polymerizable group having 1 to 30 carbon atoms, or a polymerizable group having 0 to 20 carbon atoms; R 1 and R 2 At least one of the groups is the polymerizable group, X 1 and X 2 each independently represents -O-, -S-, or -NY-, where Y is a group represented by the following formula (2): [ka] (In the formula, A 3 and Z 3 are the above A 1 and Z 1 is synonymous with R 3 represents a hydrogen atom or a non-polymerizable group having 1 to 30 carbon atoms, and * represents a bond to the nitrogen atom.) is a group represented by n 1 , n 2 and n 3 each independently represents an integer of 0 to 3, m 1 and m2 Each independently represents an integer of 0 to 4, 1 +m 2 is greater than or equal to 1, A 1 , A 2 , A 3 , Z 1 , Z 2 , Z 3 , X 1 , X 2 , R 1 , R 2 , R 3 , n 1 , n 2 and n 3 If there are multiple A's, multiple A's 1 , A 2 , A 3 , Z 1 , Z 2 , Z 3 , X 1 , X 2 , R 1 , R 2 , R 3 , n 1 , n 2 and n 3 may be the same or different from each other. However, in the formula, oxygen atoms are not directly bonded to each other. The liquid crystal composition according to any one of [1] to [3], comprising a compound represented by the following formula:
[0012] [5] The first polymerizable compound is represented by the following formulas (1-1) to (1-3): [ka] [ka] [ka] [In the formula, A 1a , A 2a , A 1b , A2b , A 3b , A 1c and A 2c Each independently represents the A 1 is synonymous with Z 1a , Z 2a , Z 1b , Z 2b , Z 3b , Z 1c and Z 2c Each independently represents Z 1 is synonymous with R 1a , R 2a , R 1b , R 2b , R 3b , R 1c and R 2c Each independently represents the R 1 is synonymous with R 1a and R 2b At least one of R 1b , R 2b and R 3b At least one of, and R 1c and R 2c At least one of the groups is the polymerizable group, X 1a , X 2a and X 1b each independently represents -O- or -S-; n 1a , n 2a , n 1b , n 2b , n 3b , n 1c and n 2c each independently represents an integer of 0 to 3, A 1a , A 2a , A 1b , A 2b , A 3b , A 1c , A 2c , Z 1a , Z 2a , Z 1b , Z 2b , Z 3b , Z 1c and Z 2c If there are multiple A's, multiple A's1a , A 2a , A 1b , A 2b , A 3b , A 1c , A 2c , Z 1a , Z 2a , Z 1b , Z 2b , Z 3b , Z 1c and Z 2c may be the same or different from each other. However, in the formula, oxygen atoms are not directly bonded to each other. The liquid crystal composition according to any one of [1] to [4], comprising at least one compound selected from the group consisting of compounds represented by the following formula:
[0013] [6] The liquid crystal composition according to any one of [1] to [5], further comprising a non-polymerizable dye compound.
[0014] [7] The non-polymerizable liquid crystal compound is represented by the following formula (3): [ka] [In formula (3), R 11 represents an alkyl group having 1 to 10 carbon atoms (a hydrogen atom present in this group may be replaced by a fluorine atom, and one -CH2- or two or more non-adjacent -CH2- groups present in this group may each be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -COO- or -OCO-), R 12 represents a halogen atom, a cyano group, an isothiocyanate group, or an alkyl group having 1 to 10 carbon atoms (a hydrogen atom present in the alkyl group may be replaced by a fluorine atom, and one -CH2- or two or more non-adjacent -CH2- groups present in the alkyl group may each be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -COO- or -OCO-), A11 , A 12 and A 13 are each independently (a3) a 1,4-cyclohexylene group (in which one -CH2- or two or more non-adjacent -CH2- groups may be replaced by -O-), (b3) a 1,4-phenylene group (in which one -CH= or two or more non-adjacent -CH= groups may be replaced by -N=); and (c3) a 1,4-cyclohexenyl group, a tetrahydropyran-2,5-diyl group, a 1,3-dioxane-2,5-diyl group, a decahydronaphthalene-2,6-diyl group, a pyridine-2,5-diyl group, a pyrimidine-2,5-diyl group, a pyrazine-2,5-diyl group, a naphthalene-2,6-diyl group, a 1,2,3,4-tetrahydronaphthalene-2,6-diyl group (one -CH= or two or more non-adjacent -CH=s present in the naphthalene-2,6-diyl group and the 1,2,3,4-tetrahydronaphthalene-2,6-diyl group may be replaced by -N=). wherein hydrogen atoms present in the groups (a3), (b3) and (c3) may each independently be replaced by a cyano group, a methyl group, a trifluoromethyl group, a trifluoromethyloxy group, a fluorine atom or a chlorine atom; Z 11 and Z 12 each independently represents a single bond, -CHCH-, -(CH)-, -OCH-, -CHO-, -COO-, -OCO-, -OCF-, -CFO-, -CH=NN=CH-, -CH=CH-, -CF=CF- or -C≡C-; n 11 represents an integer from 0 to 3, A 11 and Z 11 If there are multiple A's, multiple A's 11 may be the same or different, and multiple Z 11 may be the same or different from each other. However, in the formula, oxygen atoms are not directly bonded to each other. The liquid crystal composition according to any one of [1] to [6], comprising a compound represented by the following formula:
[0015] [8] The liquid crystal composition according to [7], wherein the compound represented by formula (3) includes a compound having a tolan skeleton.
[0016] [9] The following formula (1-2) [ka] [In the formula, A 1b , A 2b and A 3b are each independently (a) a 1,4-cyclohexylene group (in this group, one -CH- or two or more non-adjacent -CH- groups may each be independently replaced by -O- or -S-, and -CH= in this group may be replaced by -N=), (b) a 1,4-phenylene group (in which one -CH= or two or more non-adjacent -CH= groups may be replaced by -N=), (c) 1,4-cyclohexenylene group, bicyclo[2.2.2]octane-1,4-diyl group, naphthalene-2,6-diyl group, naphthalene-1,4-diyl group, 1,2,3,4-tetrahydronaphthalene-2,6-diyl group, 5,6,7,8-tetrahydronaphthalene-1,4-diyl group, decahydronaphthalene-2,6-diyl group, anthracene-2,6-diyl group, anthracene-1,4-diyl group, anthracene-9,10-diyl group, phenanthrene-2, 7-diyl group (one -CH= or two or more non-adjacent -CH= present in a naphthalene-2,6-diyl group, a naphthalene-1,4-diyl group, a 1,2,3,4-tetrahydronaphthalene-2,6-diyl group, a 5,6,7,8-tetrahydronaphthalene-1,4-diyl group, an anthracene-2,6-diyl group, an anthracene-1,4-diyl group, an anthracene-9,10-diyl group, or a phenanthrene-2,7-diyl group may be replaced by -N=), and (d) a thiophene-2,5-diyl group, a thiophene-2,4-diyl group, a benzothiophene-2,5-diyl group, a benzothiophene-2,6-diyl group, a dibenzothiophene-3,7-diyl group, a dibenzothiophene-2,6-diyl group, or a thieno[3,2-b]thiophene-2,5-diyl group (one -CH= or two or more non-adjacent -CH=s in these groups may be replaced by -N=). or a single bond, and hydrogen atoms present in the groups (a), (b), (c) and (d) may each independently be replaced by a methyl group, an ethyl group, a propyl group, a 2-propyl group, a butyl group, a 2-butyl group, a methoxy group, an ethoxy group, a methylthio group, an ethylthio group, a dimethylamino group, a diethylamino group, a cyano group, a nitro group, a fluorine atom or a chlorine atom; Z 1b , Z 2b and Z 3b each independently represents a linear or branched alkylene group having 1 to 20 carbon atoms, a linear or branched alkenylene group having 2 to 30 carbon atoms, -CHO-, -OCH-, -CFO-, -OCF-, -COO-, -OCO-, -N=CH-, -CH=N-, -N=N-, -C≡C-, or a single bond, and a hydrogen atom present in the alkylene group and alkenylene group may be substituted with a fluorine atom, R 1b , R 2b and R 3b each independently represents a hydrogen atom, a non-polymerizable group having 1 to 30 carbon atoms, or a polymerizable group having 0 to 20 carbon atoms; R 1b , R 2b and R 3b At least one of the groups is the polymerizable group, X 1b represents -O- or -S-; n 1b , n 2b and n 3b each independently represents an integer of 0 to 3, A 1b , A 2b , A 3b , Z 1b , Z 2band Z 3b If there are multiple A's, multiple A's 1b , A 2b , A 3b , Z 1b , Z 2b and Z 3b may be the same or different from each other. However, in the formula, oxygen atoms are not directly bonded to each other. A pigment compound represented by the formula:
[0017]
[10] A liquid crystal layer formed from the liquid crystal composition according to any one of [1] to [8], A liquid crystal layer comprising the polymer network derived from the polymerizable compound and the non-polymerizable liquid crystal compound.
[0018]
[11] A pair of transparent electrode substrates; A light control element comprising: a liquid crystal layer according to
[10] disposed between the pair of transparent electrode substrates. Effect of the Invention
[0019] According to the present invention, it is possible to provide a liquid crystal layer that has sufficient light-shielding properties when no voltage is applied and is unlikely to experience a decrease in light-shielding properties due to heat. Also, according to the present invention, it is possible to provide a liquid crystal composition for forming the liquid crystal layer. Also, according to the present invention, it is possible to provide a light-adjusting element using the liquid crystal composition. Also, according to the present invention, it is possible to provide a novel dye compound for use in the liquid crystal composition. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a liquid crystal element according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Preferred embodiments of the present invention will be described below, however, the present invention is not limited to the following embodiments.
[0022] <Liquid crystal composition> One embodiment of the present invention is a liquid crystal composition containing a polymerizable compound, a polymerization initiator, and a non-polymerizable liquid crystal compound, the polymerizable compound including a first polymerizable compound having a maximum absorption wavelength in the range of 370 to 780 nm and a second polymerizable compound not having a maximum absorption wavelength in the range of 370 to 780 nm. Here, the first polymerizable compound can be called a dye compound because it has a maximum absorption wavelength in the range of 370 to 780 nm.
[0023] The polymerizable compound in the liquid crystal composition is polymerized to form a polymer network that disperses the liquid crystal component. According to the liquid crystal composition, a polymer-dispersed type (polymer network type) liquid crystal can be formed by polymerizing the polymerizable compound. Therefore, the liquid crystal composition can be called a polymer-dispersed type (polymer network type) liquid crystal forming composition. In addition, since the liquid crystal composition contains a non-polymerizable liquid crystal compound as a host and a dye compound (a compound having a maximum absorption wavelength in the range of 370 to 780 nm) as a guest, it can also be called a guest-host (GH) type liquid crystal material.
[0024] The liquid crystal composition can form a liquid crystal layer that has sufficient light-shielding properties when no voltage is applied and is not susceptible to deterioration of the light-shielding properties due to heat. Therefore, the liquid crystal composition is suitable for use in light control devices such as smart windows. In addition, the liquid crystal layer formed by the liquid crystal composition tends to have excellent transmittance contrast.
[0025] Components contained in the liquid crystal composition will be described below. In the following, among the components contained in the liquid crystal composition, a component made of a polymerizable compound is referred to as a "polymerizable component", and a component made of a liquid crystal compound is referred to as a "liquid crystal component".
[0026] (Polymerizable component) The polymerizable component includes a first polymerizable compound having a maximum absorption wavelength in the range of 370 to 780 nm, and a second polymerizable compound not having a maximum absorption wavelength in the range of 370 to 780 nm.
[0027] [First polymerizable compound] The first polymerizable compound is a dye compound (polymerizable dye) having one or more polymerizable groups. The polymerizable group may be a radical polymerizable group, a cationic polymerizable group, or an anionic polymerizable group. The number of carbon atoms in the polymerizable group may be, for example, 0 to 20. Specific examples of the polymerizable group include groups represented by the following formulas (P-1) to (P-21). [ka]
[0028] In the formulae (P-1) to (P-21), * indicates a bond to a carbon atom or another atom. In the formulae, the hydrogen atom in the methyl group bonded to the vinyl group may be substituted with one or more fluorine atoms.
[0029] The first polymerizable compound may have one type of polymerizable group or two or more types of polymerizable groups.
[0030] From the viewpoint of enhancing polymerizability and storage stability, the first polymerizable compound preferably has at least one group selected from the group consisting of groups represented by formulae (P-1), (P-2), (P-3), (P-18), and (P-21), and more preferably has at least one group selected from the group consisting of formulae (P-1) and (P-2).
[0031] The first polymerizable compound has a maximum absorption wavelength in the range of 370 to 780 nm. The first polymerizable compound may be a compound having a maximum absorption wavelength in the range of more than 370 nm and not more than 750 nm, not more than 600 nm, or not more than 500 nm. From the viewpoint of adjusting to a desired color such as black, it is preferable to use two or more compounds having different maximum absorption wavelengths as the first polymerizable compound. Among them, it is more preferable to use two or more compounds selected from the group consisting of a compound having a maximum absorption wavelength in the range of more than 370 nm and not more than 500 nm (yellow dye), a compound having a maximum absorption wavelength in the range of more than 500 nm and not more than 600 nm (red dye), and a compound having a maximum absorption wavelength in the range of more than 600 nm and not more than 750 nm (blue dye), and it is even more preferable to use all of these three types of compounds. The number of types of the first polymerizable compound contained in the liquid crystal composition may be six or less (for example, 1 to 6 or 2 to 6), or may be five or less, or four or less.
[0032] The maximum absorption wavelength is measured as follows. First, a sample is prepared by adding and dissolving 1.0 part by mass of the first polymerizable compound to 100 parts by mass of any liquid crystal composition capable of dissolving the first polymerizable compound. Next, using two 2 cm x 2 cm glass substrates having ITO electrodes with an alignment film for horizontal alignment on the ITO electrodes, a cell is created with the ITO electrode layer on the inside of the cell and an injection port whose cell thickness is adjusted to 10 μm using plastic particles. A sample is injected into the cell and the injection port is sealed with a sealant to prepare a device. Next, the absorption spectrum between 370 and 750 nm is measured using the fabricated element at 25°C with no applied voltage using a spectrometer (Otsuka Electronics' "LCD-5200" or Hitachi High-Tech Science's "U-4100"), thereby determining the maximum absorption wavelength of the first polymerizable compound.
[0033] The first polymerizable compound may be, for example, a compound having a skeleton such as an anthraquinone skeleton, an azo skeleton, a quinophthalone skeleton, a diketopyrrolopyrrole skeleton, a benzothiadiazole skeleton, a perylene skeleton, a coumarin skeleton, a quinacridone skeleton, or a porphyrin skeleton. Among these, a compound having an anthraquinone skeleton has excellent radical resistance. Therefore, when the liquid crystal composition contains a compound having an anthraquinone skeleton as the first polymerizable compound, the light resistance of the liquid crystal layer tends to be improved.
[0034] As the first polymerizable compound, from the viewpoint of further improving the light-shielding property and heat resistance, it is preferable to use a compound represented by the following formula (1) (hereinafter, also referred to as "compound (1)"). 1 , A 2 , Z 1 , Z 2 , X 1 , X 2 , R 1 , R 2 , n 1 and n 2 If there are multiple A's, multiple A's 1 , A 2 , Z 1 , Z 2 , X 1 , X 2 , R 1 , R 2 , n 1 and n 2 may be the same or different. In addition, in formula (1), oxygen atoms are not directly bonded to each other. [ka]
[0035] In formula (1), A 1 and A 2 each independently represents a group selected from the group consisting of the following group (a), group (b), group (c) and group (d), or a single bond.
[0036] (a) a 1,4-cyclohexylene group (one -CH- or two or more non-adjacent -CH- groups in this group may each be independently replaced by -O- or -S-, and -CH= in this group may be replaced by -N=).
[0037] (b) a 1,4-phenylene group (in which one -CH= or two or more non-adjacent -CH= groups may be replaced by -N=).
[0038] (c) 1,4-cyclohexenylene group, bicyclo[2.2.2]octane-1,4-diyl group, naphthalene-2,6-diyl group, naphthalene-1,4-diyl group, 1,2,3,4-tetrahydronaphthalene-2,6-diyl group, 5,6,7,8-tetrahydronaphthalene-1,4-diyl group, decahydronaphthalene-2,6-diyl group, anthracene-2,6-diyl group, anthracene-1,4-diyl group, anthracene-9,10-diyl group, phenanthrene-2 ,7-diyl group (one -CH= or two or more non-adjacent -CH=s present in a naphthalene-2,6-diyl group, a naphthalene-1,4-diyl group, a 1,2,3,4-tetrahydronaphthalene-2,6-diyl group, a 5,6,7,8-tetrahydronaphthalene-1,4-diyl group, an anthracene-2,6-diyl group, an anthracene-1,4-diyl group, an anthracene-9,10-diyl group, and a phenanthrene-2,7-diyl group may be replaced by -N=).
[0039] (d) a thiophene-2,5-diyl group, a thiophene-2,4-diyl group, a benzothiophene-2,5-diyl group, a benzothiophene-2,6-diyl group, a dibenzothiophene-3,7-diyl group, a dibenzothiophene-2,6-diyl group, or a thieno[3,2-b]thiophene-2,5-diyl group (one -CH= or two or more non-adjacent -CH=s in these groups may be replaced by -N=).
[0040] Hydrogen atoms present in the groups (a), (b), (c) and (d) may each independently be replaced by a methyl group, an ethyl group, a propyl group, a 2-propyl group, a butyl group, a 2-butyl group, a methoxy group, an ethoxy group, a methylthio group, an ethylthio group, a dimethylamino group, a diethylamino group, a cyano group, a nitro group, a fluorine atom or a chlorine atom.
[0041] The group (a) may be, for example, a group selected from the group consisting of groups represented by the following formulae (a1) to (a5). The wavy line indicates a bond on the X side, and * indicates a bond on the R side. The X side refers to A 1 If X 1 A means side 2 If X 2 The R side means the A side. 1 If R 1 A means side 2 If R 2 It means the side. [ka]
[0042] The group (b) may be, for example, a group selected from the group consisting of groups represented by the following formulae (b1) to (b11): The wavy line indicates a bond on the X side, and * indicates a bond on the R side. [ka]
[0043] R in formulas (b2) to (b6) e R represents a methyl group, an ethyl group, a propyl group (1-propyl group), a 2-propyl group, a butyl group, a 2-butyl group, a methoxy group, an ethoxy group, a methylthio group, an ethylthio group, a dimethylamino group, a diethylamino group, a cyano group, a nitro group, a fluorine atom, or a chlorine atom. e If there are multiple R e may be the same group or different groups.
[0044] The group (c) may be, for example, a group selected from the group consisting of groups represented by the following formulae (c1) to (c14): The wavy line indicates a bond on the X side, and * indicates a bond on the R side. [ka]
[0045] The group (d) may be, for example, a group selected from the group consisting of groups represented by the following formulas (d1) to (d10). e is the same as above. The wavy line indicates a bond on the X side, and * indicates a bond on the R side. [ka]
[0046] From the viewpoint of increasing solubility, A 1 and A 2 is preferably a group selected from the group consisting of group (a) and group (b), and more preferably group (b). 1 and A 2 are each independently preferably a group having a structure represented by the following formula (b-1), more preferably a group having a structure represented by the following formula (b-2) or (b-3), 1 and A 2 and are particularly preferably groups having a structure represented by the following formula (b-2): The wavy line indicates a bond on the X side, and the * indicates a bond on the R side. [ka]
[0047] In formula (b-1), R i1 and R i2 each independently represents a hydrogen atom or a methyl group.
[0048] Z 1 and Z 2each independently represents a single bond, -N=CH-, -CH=N-, -N=N-, -C≡C-, a linear or branched alkylene group having 1 to 20 carbon atoms, or a linear or branched alkenylene group having 2 to 30 carbon atoms. One or more -CH2- in the alkylene group and alkenylene group may be replaced by -O-, -COO- or -OCO-, and a hydrogen atom present in the alkylene group and alkenylene group may be replaced by a fluorine atom.
[0049] Z 1 and Z 2 is preferably a linear or branched alkylene group having 1 to 20 carbon atoms or a single bond from the viewpoint of ease of synthesis and solubility. The alkylene group is preferably linear from the viewpoint of ease of synthesis. The number of carbon atoms in the alkylene group is preferably 2 to 12, more preferably 2 to 8, from the viewpoint of solubility. The alkylene group is preferably unsubstituted or one -CH2- is substituted with -O-. Examples of the alkylene group include an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, and an octylene group. Among these, a group selected from the group consisting of a butylene group, a pentylene group, and a hexylene group is preferred.
[0050] R 1 and R 2 each independently represents a hydrogen atom, a non-polymerizable group having 1 to 30 carbon atoms, or a polymerizable group having 0 to 20 carbon atoms. 1 and R 2 At least one of R is a polymerizable group having 0 to 20 carbon atoms. 1 and R 2 If there are multiple R 1 One or more of R 2 One of the groups may be a polymerizable group having 0 to 20 carbon atoms.
[0051] The non-polymerizable group may be, for example, a linear or branched alkyl group having 1 to 20 carbon atoms, or a linear or branched alkenyl group having 2 to 30 carbon atoms. One -CH2- or two or more non-adjacent -CH2- present in these groups (alkyl and alkenyl groups) are each independently -NR 4 The hydrogen atoms in these groups may be replaced by -, -O-, -S-, -CH=CH-, -CF=CF- or -C≡C-. Furthermore, the hydrogen atoms in these groups may be replaced by fluorine atoms.
[0052] Above R 4 represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an alkenyl group having 2 to 30 carbon atoms. One -CH2- or two or more non-adjacent -CH2- groups present in these groups (alkyl and alkenyl groups) may each be independently replaced by -O-, -S-, -COO-, -OCO-, or -CO-. In addition, a hydrogen atom present in these groups may be replaced by a fluorine atom. R 4 If there are multiple R 4 may be the same or different from each other.
[0053] From the viewpoint of enhancing solubility, the non-polymerizable group is preferably a linear or branched alkyl group having 1 to 20 carbon atoms, and more preferably an unsubstituted linear or branched alkyl group having 1 to 20 carbon atoms. The alkyl group is preferably linear. The number of carbon atoms in the alkyl group is preferably 2 to 16, and more preferably 4 to 12. Note that the above carbon number means the total number of carbon atoms including the number of carbon atoms in the substituent when a part of the alkyl group is replaced with any of the above groups.
[0054] Specific examples of unsubstituted alkyl groups having 1 to 20 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tetradecyl group, and a pentadecyl group.
[0055] R1 is a hydrogen atom or a polymerizable group, R 1 Z directly bonded to 1 may be a linear or branched alkylene group having 1 to 20 carbon atoms; R 1 is a non-polymerizable group, R 1 Z directly bonded to 1 may be a single bond. 2 is a hydrogen atom or a polymerizable group, R 2 Z directly bonded to 2 may be a linear or branched alkylene group having 1 to 20 carbon atoms; R 2 is a non-polymerizable group, R 2 Z directly bonded to 2 may be a single bond.
[0056] X 1 and X 2 each independently represents -O-, -S- or -NY-.
[0057] Y is a group represented by the following formula (2). [ka]
[0058] In formula (2), A 3 and Z 3 are the above A 1 and Z above 1 is synonymous with R 3 represents a hydrogen atom or a non-polymerizable group having 1 to 30 carbon atoms, and * represents a bond to a nitrogen atom. Examples of the non-polymerizable group include the above R 1 The examples of the non-polymerizable group represented by the formula (2) are the same as those of the non-polymerizable group represented by the formula (2). 3 , Z 3 R 3 and n 3 If there are multiple A's, multiple A's 3 , Z 3 R 3 and n 3 may be the same or different from each other.
[0059] n1 , n 2 and n 3 Each independently represents an integer of 0 to 3. In terms of solubility, n 1 , n 2 and n 3 It is preferable that each independently is 0 or 1.
[0060] m 1 and m 2 Each independently represents an integer of 0 to 4. 1 +m 2 is 1 or more. In terms of solubility, m 1 and m 2 are each preferably independently 0 to 2, 1 +m 2 is preferably 2 to 3.
[0061] From the viewpoint of improving the light-shielding property, it is preferable to use, as compound (1), at least one compound selected from the group consisting of compounds represented by the following formulas (1-1) to (1-3) (hereinafter also referred to as "compound (1-1)", "compound (1-2)" and "compound (1-3)"). From the viewpoint of further improving the light-shielding property, it is more preferable to use at least two or more compounds selected from the group consisting of compound (1-1), compound (1-2) and compound (1-3). [ka] [ka] [ka]
[0062] In the formula, A 1a , A 2a , A 1b , A 2b , A 3b , A 1c and A 2c Each independently represents A in the above formula (1). 1is synonymous with Z 1a , Z 2a , Z 1b , Z 2b , Z 3b , Z 1c and Z 2c Each independently represents Z in the above formula (1). 1 is synonymous with R 1a , R 2a , R 1b , R 2b , R 3b , R 1c and R 2c Each independently represents R in the above formula (1). 1 is synonymous with R 1a and R 2b At least one of R 1b , R 2b and R 3b At least one of, and R 1c and R 2c At least one of X is a polymerizable group having 0 to 20 carbon atoms. 1a , X 2a and X 1b each independently represents -O- or -S-; n 1a , n 2a , n 1b , n 2b , n 3b , n 1c and n 2c Each independently represents an integer of 0 to 3; A 1a , A 2a , A 1b , A 2b , A 3b , A 1c , A 2c , Z 1a , Z 2a , Z 1b , Z 2b , Z 3b , Z 1c and Z 2c If there are multiple A's, multiple A's 1a , A 2a , A 1b , A 2b , A 3b , A 1c , A 2c , Z 1a , Z2a , Z 1b , Z 2b , Z 3b , Z 1c and Z 2c may be the same or different, provided that no oxygen atom is directly bonded to another oxygen atom in the formula.
[0063] [Compound (1-1)] The compound (1-1) tends to have a maximum absorption wavelength in the range of more than 370 nm to 500 nm, and therefore, the compound (1-1) can be used as a yellow dye.
[0064] From the viewpoint of the maximum absorption wavelength, the compound (1-1) is preferably a compound represented by the following formula (1-1-1), and more preferably a compound represented by the following formula (1-1-1a). [ka] [ka]
[0065] Z in formula (1-1-1) 1a , Z 2a , R 1a , R 2a , X 1a and X 2a respectively represent Z in the above formula (1-1). 1a , Z 2a , R 1a , R 2a , X 1a and X 2a is synonymous with.
[0066] The compound (1-1) may be used alone or in combination of two or more kinds.
[0067] The content of the compound (1-1) may be, for example, 5 to 90 parts by mass, 10 to 60 parts by mass, or 15 to 45 parts by mass relative to 100 parts by mass of the total amount of the first polymerizable compound.
[0068] Compound (1-1) is a known compound or can be produced from a known compound according to a known production method. Compound (1-1) can be obtained, for example, by a method including a step (1a) of reacting a compound (1,5-dihydroxyanthracene-9,10-dione) represented by the following formula (x1-1) and compounds represented by the following formulas (y1-1) and (y1-2) (hereinafter also referred to as "compound (y1-1)" and "compound (y1-2)") as raw material compounds to obtain compound (1-1). [ka] [ka]
[0069] Here, A in the formula 1a , A 2a , Z 1a , Z 2a , R 1a , R 2a , X 1a , X 2a , n 1a and n 2a is A in formula (1-1) 1a , A 2a , Z 1a , Z 2a , R 1a , R 2a , X 1a , X 2a , n 1a and n 2a The compound (y1-1) and the compound (y1-2) may be the same as each other.
[0070] The conditions of the reaction and post-treatment carried out in step (1a) can be appropriately set according to the structure of the raw material compound. In step (1a), for example, diisopropyl azodicarboxylate is dropped into a mixture containing 1,5-dihydroxyanthracene-9,10-dione, compound (y1-1), compound (y1-2), and triphenylphosphine, and the mixture is stirred to react the raw material compounds, thereby obtaining compound (1-1). If necessary, a solvent can be included in the mixture. Examples of the solvent include tetrahydrofuran, 1,4-dioxane, toluene, benzene, chloroform, dichloromethane, and acetonitrile. Two or more of these solvents may be used in combination. The dropwise addition of diisopropyl azodicarboxylate may be performed under ice cooling. The stirring after the dropwise addition of diisopropyl azodicarboxylate may be performed at room temperature (for example, 0 to 40° C.). The stirring time may be, for example, 1 to 48 hours. The post-treatment can be carried out, for example, by a method including extracting an organic layer containing compound (1-1) from the reaction mixture by a liquid separation operation, washing the extracted organic layer, and drying the washed organic layer. The liquid separation operation can be carried out, for example, by adding water, dichloromethane, or a mixed solvent thereof to the reaction mixture. The organic layer can be washed, for example, by using methanol, ethanol, water, or the like. The organic layer can be dried, for example, by adding a drying agent such as anhydrous sodium sulfate to the organic layer, filtering the drying agent from the organic layer, and then drying the filtrate under reduced pressure. The post-treatment can include a purification treatment. The purification treatment can be carried out, for example, by using silica gel column chromatography. A purification treatment by reprecipitation using dichloromethane, methanol, a mixed solvent thereof, or the like can be carried out.
[0071] [Compound (1-2)] Compound (1-2) tends to have a maximum absorption wavelength in the range of more than 500 nm to 600 nm, and therefore, compound (1-2) can be used as a red dye.
[0072] From the viewpoint of the maximum absorption wavelength, the compound (1-2) is preferably a compound represented by the following formula (1-2-1), and more preferably a compound represented by the following formula (1-2-1a). [ka] [ka]
[0073] Z in formula (1-2-1) 1b , R 1b , R 2b , R 3b and X 1b are Z in the above formula (1-2), 1b , R 1b , R 2b , R 3b and X 1b is synonymous with.
[0074] The compound (1-2) may be used alone or in combination of two or more kinds.
[0075] The content of the compound (1-2) may be, for example, 5 to 90 parts by mass, 10 to 60 parts by mass, or 15 to 45 parts by mass relative to 100 parts by mass of the total amount of the first polymerizable compound.
[0076] The compound (1-2) can be produced, for example, by a method including the following steps (1b) to (3b).
[0077] Step (1b) is a step of using, as raw material compounds, a compound represented by the following formula (x2-1) (hereinafter also referred to as "compound (x2-1)") and a compound represented by the following formula (y2-1) (hereinafter also referred to as "compound (y2-1)"), and reacting these raw material compounds to obtain a compound represented by the following formula (x2-2) (hereinafter also referred to as "compound (x2-2)"). [ka] [ka] [ka]
[0078] Here, A in the formula 3b , Z 3b , R 3b and n 3b is A in formula (1-2) 3b , Z 3b , R 3b and n 3b is synonymous with Q 2b and Q 3b each independently represents a halogen atom. The halogen atom may be a bromine atom or a chlorine atom.
[0079] The conditions of the reaction and post-treatment carried out in step (1b) can be appropriately set according to the structure of the raw material compound. In step (1b), for example, compound (x2-2) can be obtained by reacting compound (x2-1) with compound (y2-1) in a reaction mixture containing them. The reaction mixture can further contain at least one of a solvent, a base, and a catalyst, as necessary. Examples of the solvent include ethylene glycol, normal butanol, isobutanol, normal pentanol, normal hexanol, N-methyl-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), toluene, 1,4-dioxane, ethylene glycol, dimethyl sulfoxide, dichloromethane, etc. Examples of the base include sodium carbonate, potassium carbonate, sodium acetate, potassium acetate, sodium hydroxide, potassium hydroxide, pyridine, triethylamine, disodium hydrogen phosphate, etc. Examples of the catalyst include palladium chloride, palladium acetate, bis(dibenzylideneacetone)palladium, tris(dibenzylideneacetone)dipalladium, tetrakis(triphenylphosphine)palladium, dichlorobis(triphenylphosphine)palladium, bis(di-tert-butyl(4-dimethylaminophenyl)phosphine)dichloropalladium, copper powder, copper acetate monohydrate, copper chloride, copper bromide, copper iodide, copper sulfate pentahydrate, and tin chloride. These solvents, bases, and catalysts may be used in combination of two or more. The temperature of the reaction mixture (reaction temperature) may be, for example, 100° C. or higher, or 100 to 180° C. The time (reaction time) maintained at the reaction temperature may be, for example, 10 minutes or more, or 40 minutes or more, and may be 120 hours or less, or 80 hours or less. The post-treatment can be carried out, for example, by a method including extracting an organic layer containing compound (x2-2) from the reaction mixture by a liquid separation operation, washing the extracted organic layer, drying the washed organic layer, etc. The liquid separation operation for extracting the organic layer containing compound (x2-2) can be carried out, for example, by adding water, an aqueous HCl solution (e.g., a 10 w / w% aqueous HCl solution), toluene, dichloromethane, etc., or a mixed solvent thereof to the reaction mixture.After the liquid separation operation, the extracted organic layer may be neutralized using a saturated aqueous sodium bicarbonate solution or the like before washing the organic layer. The organic layer may be washed using, for example, saturated saline solution or the like. The organic layer may be dried, for example, by adding a drying agent such as anhydrous sodium sulfate to the organic layer, filtering the drying agent from the organic layer, and then drying the filtrate under reduced pressure. The post-treatment may include a purification treatment. The purification treatment may be performed using, for example, silica gel column chromatography. A purification treatment by reprecipitation using dichloromethane, hexane, methanol, a mixed solvent thereof, or the like may be performed.
[0080] Step (2b) is a step of using, as raw material compounds, a compound (x2-2) and a compound represented by the following formula (y2-2) (hereinafter also referred to as “compound (y2-2)”), and reacting these raw material compounds to obtain a compound represented by the following formula (x2-3) (hereinafter also referred to as “compound (x2-3)”). [ka] [ka]
[0081] Here, A in the formula 2b , A 3b , Z 2b , Z 3b , R 2b , R 3b , X 1b , n 2b and n 3b is A in formula (1-2) 2b , A 3b , Z 2b , Z 3b , R 2b , R 3b , X 1b , n 2b and n 3b is synonymous with.
[0082] The conditions of the reaction and post-treatment carried out in step (2b) can be appropriately set according to the structure of the raw material compound. In step (2b), for example, compound (x2-2) and compound (y2-2) can be reacted in a reaction mixture containing them to obtain compound (x2-3). The reaction mixture can further contain at least one of a solvent, a base, and a catalyst as necessary. As the solvent, base, and catalyst, various solvents, bases, and catalysts exemplified in step (1b) can be used. The reaction may be carried out under a nitrogen atmosphere. The temperature of the reaction mixture (reaction temperature) may be, for example, 80° C. or higher, and may be 80 to 160° C. The time (reaction time) for maintaining the reaction temperature may be, for example, 1 hour or more, or 5 hours or more, and may be 1 to 10 hours, or 5 to 8 hours. The post-treatment may be carried out in the same manner as in step (1b).
[0083] Step (3b) is a step of using, as raw material compounds, compound (x2-3) and a compound represented by the following formula (y2-3) (hereinafter also referred to as "compound (y2-3)"), and reacting these raw material compounds to obtain compound (1-2). [ka]
[0084] Here, A in the formula 1b , Z 1b , R 1b and n 1b is A in formula (1-2) 1b , Z 1b , R 1b and n 1b is synonymous with Q 1b represents a halogen atom. The halogen atom may be a bromine atom or a chlorine atom.
[0085] The conditions of the reaction and post-treatment carried out in the step (3b) can be appropriately set according to the structure of the raw material compound. In the step (3b), for example, the compound (x2-3) and the compound (y2-3) can be reacted in a reaction mixture containing them to obtain the compound (1-2). The reaction mixture can further contain any one or more of a solvent, a base, and a catalyst, if necessary. As the solvent, base, and catalyst, various solvents, bases, and catalysts exemplified in the above step (1b) can be used. Two or more of these solvents, bases, and catalysts may be used in combination. The temperature of the reaction mixture (reaction temperature) may be, for example, 100° C. or higher, and may be 100 to 180° C. The time (reaction time) for maintaining the reaction temperature may be, for example, 10 minutes or more, or 40 minutes or more, and may be 120 hours or less, or 80 hours or less. The post-treatment may be carried out in the same manner as in the step (1b).
[0086] [Compound (1-3)] Compound (1-3) tends to have a maximum absorption wavelength in the range of more than 600 nm to 750 nm, and therefore, compound (1-3) can be used as a blue dye.
[0087] From the viewpoint of the maximum absorption wavelength, compound (1-3) is preferably a compound represented by the following formula (1-3-1), and more preferably a compound represented by the following formula (1-3-1a). [ka] [ka]
[0088] Z in formula (1-3-1) 1c , Z 2c , R 1c and R 2c are Z in the above formula (1-3), 1c , Z 2c , R 1c and R 2c is synonymous with.
[0089] The compound (1-3) may be used alone or in combination of two or more kinds.
[0090] The content of the compound (1-3) may be, for example, 5 to 90 parts by mass, 10 to 60 parts by mass, or 15 to 45 parts by mass relative to 100 parts by mass of the total amount of the first polymerizable compound.
[0091] Compound (1-3) is a known compound or can be produced from a known compound according to a known production method. Compound (1-3) can be obtained, for example, by a method including a step (1c) of using a compound represented by the following formula (x3-1) (hereinafter also referred to as "compound (x3-1)") and compounds represented by the following formulas (y3-1) and (y3-2) (hereinafter also referred to as "compound (y3-1)" and "compound (y3-2)") as raw material compounds and reacting these raw material compounds to obtain compound (1-3). [ka] [ka]
[0092] Here, A in the formula 1c , A 2c , Z 1c , Z 2c , R 1c , R 2c , n 1c and n 2c is A in formula (1-3) 1c , A 2c , Z 1c , Z 2c , R 1c , R 2c , n 1c and n 2c is synonymous with Q 1c and Q 2c each independently represents a halogen atom. The halogen atom may be a bromine atom or a chlorine atom. Compound (y3-1) and compound (y3-2) may be the same as each other.
[0093] The conditions of the reaction and post-treatment carried out in step (1c) can be appropriately set according to the structure of the raw material compound. In step (1c), for example, compound (x3-1), compound (y3-1), and compound (y3-2) can be reacted in a reaction mixture containing these compounds to obtain compound (1-3). The reaction mixture can further contain at least one of a solvent, a base, and a catalyst, as necessary. As the solvent, base, and catalyst, various solvents, bases, and catalysts exemplified in step (1b) can be used. Two or more of these solvents, bases, and catalysts may be used in combination. The temperature of the reaction mixture (reaction temperature) may be, for example, 100° C. or higher, and may be 100 to 180° C. The time (reaction time) held at the reaction temperature may be, for example, 10 minutes or more, or 40 minutes or more, and may be 120 hours or less, or 80 hours or less. The post-treatment can be carried out by a method including, for example, precipitating compound (1-3), washing the precipitated compound (1-3), and drying (for example, drying under reduced pressure) the washed compound (1-3). Precipitation of compound (1-3) can be carried out by adding, for example, methanol, ethanol, water, or a mixed solvent thereof to the reaction mixture. Washing of compound (1-3) can be carried out using, for example, methanol, ethanol, an aqueous HCl solution (for example, a 5 w / w% aqueous HCl solution), or the like. The post-treatment can include a purification treatment. The purification treatment can be carried out, for example, by using silica gel column chromatography. A purification treatment by reprecipitation using dichloromethane, hexane, methanol, a mixed solvent thereof, or the like can also be carried out.
[0094] When compound (1-3) is a compound represented by the following formula (1-3') (hereinafter also referred to as "compound (1-3')"), compound (1-3') can also be produced by a method including steps (2c) and (3c) shown below. [ka]
[0095] A in the formula 1c, A 2c , Z 1c , Z 2c , R 1c , R 2c , n 1c and n 2c is A in formula (1-3) 1c , A 2c , Z 1c , Z 2c , R 1c , R 2c , n 1c and n 2c is synonymous with Z 3c and Z 4c represents a linear or branched alkylene group having 1 to 20 carbon atoms, or a linear or branched alkenylene group having 2 to 30 carbon atoms.
[0096] Step (2c) is a step of using, as raw material compounds, compound (x3-1) and compounds represented by the following formulas (y3-3) and (y3-4) (hereinafter also referred to as “compound (y3-3)” and “compound (y3-4)”) to react with each other to obtain a compound represented by the following formula (x3-2) (hereinafter also referred to as “compound (x3-2)”). [ka] [ka]
[0097] Here, A in the formula 1c and A 2c is A in formula (1-3) 1c and A 2c The compound (y3-3) and the compound (y3-4) may be the same as each other.
[0098] The conditions of the reaction and post-treatment carried out in step (2c) can be appropriately set according to the structure of the raw material compound. In step (2c), for example, compound (x3-1), compound (y3-3), and compound (y3-4) can be reacted in a reaction mixture containing these compounds to obtain compound (x3-2). The reaction mixture can further contain at least one of a solvent, a base, and a catalyst, as necessary. As the solvent, base, and catalyst, various solvents, bases, and catalysts exemplified in step (1b) can be used. Two or more of these solvents, bases, and catalysts may be used in combination. The temperature of the reaction mixture (reaction temperature) may be, for example, 100° C. or higher, and may be 100 to 180° C. The time (reaction time) for maintaining the reaction temperature may be, for example, 10 minutes or more, or 40 minutes or more, and may be 120 hours or less, or 80 hours or less. The post-treatment may be carried out in the same manner as in step (1c).
[0099] Step (3c) is a step of using compound (x3-2) and compounds represented by the following formulae (y3-5) and (y3-6) (hereinafter also referred to as "compound (y3-5)" and "compound (y3-6)") as raw material compounds, and reacting these raw material compounds to obtain compound (1-3'). [ka]
[0100] Here, A in the formula 1c , A 2c , Z 1c , Z 2c , Z 3c , Z 4c , R 1c , R 2c , n 1c and n 2c is A in formula (1-3') 1c , A 2c , Z 1c , Z 2c , Z 3c , Z 4c , R 1c , R 2c , n 1c and n 2c is synonymous with Q3c and Q 4c represents a halogen atom. The halogen atom may be a bromine atom or a chlorine atom. Compound (y3-5) and compound (y3-6) may be the same as each other.
[0101] The conditions of the reaction and post-treatment carried out in the step (3c) can be appropriately set according to the structure of the raw material compound. In the step (3c), for example, the compound (x3-2), the compound (y3-5), and the compound (y3-6) can be reacted in a reaction mixture containing these compounds to obtain the compound (1-3'). The reaction mixture can further contain at least one of a solvent, a base, and a catalyst, if necessary. As the solvent, the base, and the catalyst, various solvents, bases, and catalysts exemplified in the above step (1b) can be used. Two or more of these solvents, bases, and catalysts may be used in combination. The temperature of the reaction mixture (reaction temperature) may be, for example, 100°C or higher, and may be 100 to 180°C. The time (reaction time) for maintaining the reaction temperature may be, for example, 10 minutes or more, or 40 minutes or more, and may be 120 hours or less, or 80 hours or less. The post-treatment may be carried out in the same manner as in the step (1c).
[0102] The content (total amount) of compound (1) may be, for example, 5 to 90 parts by mass, 10 to 60 parts by mass, or 15 to 45 parts by mass relative to 100 parts by mass of the total amount of the first polymerizable compound.
[0103] The range of the content (total amount) of the first polymerizable compound may be 0.2 parts by mass or more, 0.5 parts by mass or more, or 1 part by mass or more, based on 100 parts by mass of the total amount of the liquid crystal components in the liquid crystal composition, from the viewpoint of light-shielding property and heat resistance when the voltage is OFF. The content (total amount) of the first polymerizable compound may be 15 parts by mass or less, 13 parts by mass or less, or 10 parts by mass or less, based on 100 parts by mass of the total amount of the liquid crystal components in the liquid crystal composition, from the viewpoint of solubility in the composition and transparency when the voltage is OFF. From these viewpoints, the content (total amount) of the first polymerizable compound may be 0.2 to 15 parts by mass, 0.5 to 13 parts by mass, or 1 to 10 parts by mass, based on 100 parts by mass of the total amount of the liquid crystal components in the liquid crystal composition.
[0104] [Second polymerizable compound] The second polymerizable compound has one or more polymerizable groups. Examples of the polymerizable group of the second polymerizable compound are the same as the examples of the polymerizable group of the first polymerizable compound described above. The polymerizable group of the second polymerizable compound may be one type or two or more types.
[0105] The second polymerizable compound is preferably a (meth)acrylate. Here, "(meth)acrylate" refers to at least one of an acrylate and its corresponding methacrylate.
[0106] As the second polymerizable compound, it is preferable to use at least one of the first to fourth components described below. Among them, it is preferable to use the first component, and it is more preferable to use the first component in combination with at least one of the second and third components. When greater importance is placed on adhesion, it is preferable to use the fourth component.
[0107] -First component- The first component is, for example, a linear monofunctional polymerizable compound represented by the following formula (v).
[0108] [ka]
[0109] In formula (v), P iia1 represents a polymerizable group, R iia2 represents a linear or branched alkyl group having 1 to 22 carbon atoms, and one or more -CH2- in the alkyl group may be each independently replaced with -O-, -CO-, -COO- or -OCO- so that there is no oxygen atom directly adjacent to it, and one or more hydrogen atoms present in the alkyl group may each independently be replaced with a fluorine atom or -OH.
[0110] In the compound represented by formula (v), P iia1represents a polymerizable group, and is preferably a group represented by any one of the above formulas (P-1) to (P-21).
[0111] From the viewpoint of enhancing the polymerizability and storage stability, among the polymerizable groups represented by the above formulas (P-1) to (P-21), the polymerizable groups represented by formula (P-1), formula (P-2), formula (P-7), formula (P-12), formula (P-13) or formula (P-21) are preferred, the polymerizable groups represented by formula (P-1), formula (P-2), formula (P-7) or formula (P-21) are more preferred, and the polymerizable groups represented by formula (P-1), formula (P-2) or formula (P-21) are particularly preferred.
[0112] In the compound represented by formula (v), R iia2 more preferably represents a linear or branched alkyl group having 3 to 30 carbon atoms, and more preferably represents a linear or branched alkyl group having 6 to 28 carbon atoms in particular from the viewpoint of suppressing crystallinity, even more preferably represents a branched alkyl group, even more preferably represents a branched alkyl group having 9 to 24 carbon atoms, and most preferably represents a branched alkyl group having 9 to 24 carbon atoms. The above "linear or branched alkyl group" also includes those in which one or more -CH2- in the alkyl group are replaced with -O- so that the oxygen atom is not directly adjacent.
[0113] R iia2 When represents a branched alkyl group, the compound represented by formula (v) is preferably a mono(meth)acrylate having a branched alkyl chain represented by the following structure, isobutyl(meth)acrylate, isononyl(meth)acrylate, isodecyl(meth)acrylate, isomyristyl(meth)acrylate, or isostearyl(meth)acrylate. [ka]
[0114] In particular, from the viewpoint of achieving a significant effect of reducing the driving voltage while maintaining good transparency when no voltage is applied, it is preferable to use a mono(meth)acrylate having a branched alkyl chain among the compounds represented by formula (v).
[0115] The compound represented by formula (v) may be used alone or in combination of two or more kinds.
[0116] The content of the compound represented by formula (v) is preferably 5% by mass or more, more preferably 10% by mass or more, and particularly preferably 15% by mass or more, based on the total amount of the polymerizable components, from the viewpoint of low-voltage driving and from the viewpoint of improving the compatibility of each component in the liquid crystal composition. The content of the compound represented by formula (v) is preferably 60% by mass or less, more preferably 50% by mass or less, and particularly preferably 40% by mass or less, based on the total amount of the polymerizable components, from the viewpoint of adhesion.
[0117] The first component may be a cyclic monofunctional polymerizable compound represented by the following formula (ii): [ka]
[0118] In formula (ii), P iii1 represents a polymerizable group, Z iii1 represents a single bond or an alkylene group having 1 to 7 carbon atoms, in which one or more non-adjacent -CH- groups may each be independently replaced by -O-, -CO-, -COO- or -OCO- so that oxygen atoms are not directly adjacent to each other; A iii1 represents a group represented by the following formulas (ii-1) to (ii-20). [ka]
[0119] In the formulae (ii-1) to (ii-20), one or more -CH2- may be independently replaced by -O-, -S-, -COO-, -OCO-, -NH-, -NCH3-, or -CO-. However, when a total of two or more oxygen atoms and / or sulfur atoms are present in the formulae (ii-1) to (ii-20), they are not bonded to each other like -OO-, -OS-, or -SS-. Furthermore, one or more -CH2-CH2- may be replaced by -CH=CH- group. Furthermore, the hydrogen atoms in the formulae (ii-1) to (ii-20) may be replaced by an alkyl group having 1 to 8 carbon atoms, which may be linear or branched, and one or more non-adjacent -CH2- in the alkyl group may be independently replaced by -O-, -CO-, -COO-, or -OCO- so that the oxygen atoms are not directly adjacent to each other. Furthermore, the black dots in the formulae represent Z. iii1 Represents a bond to .
[0120] The compound represented by formula (ii) is a material with excellent flexibility, and when this compound is used, it is possible to maintain opacity even in a bent state. In addition, it is possible to increase the adhesion and the compatibility of each component in the liquid crystal composition. The compound represented by formula (ii) is a non-liquid crystal compound.
[0121] In the compound represented by formula (ii), P iii1 A preferred example of the formula (v) is iia1 These are the same as the preferred examples of the polymerizable group represented by the following formula:
[0122] In the compound represented by formula (ii), Z iii1 represents a single bond or an alkylene group having 1 to 7 carbon atoms, in which one or more -CH2- may be independently replaced with -O-, -CO-, -COO- or -OCO- so that no oxygen atom is directly adjacent, and one or more hydrogen atoms in the alkylene group may be independently replaced with a fluorine atom. iii1is preferably a single bond or an alkylene group having 1 to 6 carbon atoms, more preferably a single bond or an alkylene group having 1 to 3 carbon atoms, and particularly preferably a single bond or a -CH2- group.
[0123] In the compound represented by formula (ii), A iii1 From the viewpoint of further improving adhesion, iii1 It is preferable that the ring structure has a heterocyclic structure having a nitrogen atom, an oxygen atom, or a sulfur atom therein, and more specifically, it is preferable that the ring structure is a group represented by the following formulas (ii-a1) to (ii-a11). In particular, when the ring structure has a nitrogen atom, the presence of the nitrogen atom in the ring structure can further improve adhesion. [ka]
[0124] In formulas (ii-a1) to (ii-a11), one or more -CH2- may be each independently replaced by -CO-, and a hydrogen atom in formulas (ii-a1) to (ii-a11) may be each independently replaced by an alkyl group having 1 to 8 carbon atoms, and one or more non-adjacent -CH2- in the alkyl group may each independently be each independently replaced by -O-, -CO-, -COO- or -OCO- so that an oxygen atom is not directly adjacent to the alkyl group.
[0125] In formulas (ii-a1) to (ii-a11), the hydrogen atoms may be substituted with an alkyl group having 1 to 8 carbon atoms, the alkyl group may be linear or branched, and one or more non-adjacent -CH2- in the alkyl group may be each independently substituted with -O-, -CO-, -COO- or -OCO- so that the oxygen atoms are not directly adjacent to each other.
[0126] The black dots in formulas (ii-a1) to (ii-a11) represent Z iii1 Represents a bond to .
[0127] Specifically, the compound represented by formula (ii) is preferably the compounds represented by the following formulae (II-34) to (II-51). [ka]
[0128] In formulas (II-34) to (II-51), X 5 represents a hydrogen atom or a methyl group.
[0129] Among the compounds represented by formulae (II-34) to (II-51), it is more preferable to use a compound represented by formula (II-34), (II-36), (II-38), (II-39), (II-40), (II-41), (II-43), or (II-45).
[0130] The compound represented by formula (ii) may be used alone or in combination of two or more kinds.
[0131] The content of the compound represented by formula (ii) is preferably 10% by mass or more, more preferably 20% by mass or more, and particularly preferably 30% by mass or more, based on the total amount of the polymerizable components, from the viewpoint of improving adhesion and enhancing compatibility of each component in the liquid crystal composition. The content of the compound represented by formula (ii) is preferably 80% by mass or less, more preferably 70% by mass or less, and particularly preferably 60% by mass or less, based on the total amount of the polymerizable components, from the viewpoint of reducing voltage.
[0132] As the first component, when low voltage is important, it is preferable to use a compound represented by formula (v), and when adhesion is important, it is preferable to use a compound represented by formula (ii). As the first component, a compound represented by formula (v) and a compound represented by formula (ii) can also be used in combination.
[0133] -Second component- The second component is a multifunctional (meth)acrylate oligomer having a weight average molecular weight of at least 2000. The multifunctional (meth)acrylate oligomer may be used to introduce a crosslinked structure into the network structure of the polymer and to obtain good adhesion.
[0134] The weight-average molecular weight of the polyfunctional (meth)acrylate oligomer is 2000 or more, preferably 2000 to 60000, more preferably 2500 to 40000, even more preferably 2800 to 35000, and even more preferably 3000 to 30000. This is because if the molecular weight is too small, the degree of cure shrinkage increases due to an increase in the crosslink density caused by an increase in the (meth)acrylic group contained in one molecule, and the adhesion deteriorates, and if the molecular weight is too large, the distance between crosslinks becomes long, the gap becomes large, and the liquid crystal is easily taken in, so the scattering property as a polymer-dispersed liquid crystal decreases. That is, if it is left in a high-temperature environment, the polymer absorbs the liquid crystal, and the characteristics change significantly. In addition, if the molecular weight is too large, the degree of decrease in the transition point Tnm of the polymer-dispersed liquid crystal by the addition of a polymerizable compound becomes small, and in order to make Tnm below room temperature, a material with a low Tni of the liquid crystal compound itself must be used, which results in a problem of a narrow operating temperature range.
[0135] Among the polyfunctional (meth)acrylate oligomers, bifunctional acrylate oligomers are preferred. Furthermore, in order to emphasize adhesion to the substrate, urethane-based or polyester-based (meth)acrylate oligomers are preferred, and urethane (meth)acrylate oligomers are more preferred. The urethane (meth)acrylate oligomer may be a polyester-based urethane (meth)acrylate oligomer, but a polyether-based urethane (meth)acrylate oligomer is preferred.
[0136] The polyfunctional urethane (meth)acrylate oligomer can be obtained by reacting a hydroxyl group-containing (meth)acrylate, a polyol, and a polyisocyanate.
[0137] Examples of the polyol include polyether polyol, polyester polyol, polycarbonate polyol, polycaprolactone polyol, polybutadiene polyol, and the like. Examples of the polyether polyol include polyethylene glycol, polypropylene glycol, polytetramethylene glycol, and the like.
[0138] Polyisocyanates include 2,4- and 2,6-tolylene diisocyanate (TDI), orthotoluidine diisocyanate (TODI), naphthylene diisocyanate (NDI), xylylene diisocyanate (XDI), 4,4'-diphenylmethane diisocyanate (MDI), methylene bis(4-cyclohexyl isocyanate), xylylene diisocyanate, hydrogenated xylylene diisocyanate, hexamethylene diisocyanate, transcyclohexane 1,4-diisocyanate, and cyclohexane 1,4-diisocyanate. Examples of the isocyanate include 1,6,11-undecane triisocyanate, 1,8-diisocyanate-4-isocyanate methyl octane, 1,3,6-hexamethylene triisocyanate, bicycloheptane triisocyanate, trimethylhexamethylene diisocyanate, dicyclopentadiene diisocyanate, norbornene diisocyanate, isophorone diisocyanate, and carbodiimide-modified MDI, polymethylene polyphenyl isocyanate, and polymeric polyisocyanate.
[0139] Examples of hydroxyl group-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, polypropylene glycol mono(meth)acrylate, 1,4-cyclohexanedimethanol monoacrylate, and mono(meth)acrylate modified with ε-caprolactone.
[0140] Specifically, the urethane (meth)acrylate oligomer is preferably an aliphatic urethane (meth)acrylate or an aromatic urethane (meth)acrylate, more preferably an aliphatic urethane acrylate, and more preferably a polyurethane di(meth)acrylate oligomer.
[0141] As the polyol to be used, polyether polyol, polyester polyol, and polycaprolactone polyol are preferred, and polyether polyol and polyester polyol are particularly preferred.
[0142] The polyisocyanate used is preferably a polyisocyanate having a cyclic structure, and particularly preferably a polyisocyanate having an alicyclic structure. More specifically, orthotoluidine diisocyanate (TODI), methylene bis(4-cyclohexyl isocyanate), xylylene diisocyanate, hydrogenated xylylene diisocyanate, transcyclohexane 1,4-diisocyanate, 1,6,11-undecane triisocyanate, bicycloheptane triisocyanate, dicyclopentadiene diisocyanate, norbornene diisocyanate, isophorone diisocyanate, and carbodiimide-modified MDI are preferred, and methylene bis(4-cyclohexyl isocyanate), xylylene diisocyanate, hydrogenated xylylene diisocyanate, transcyclohexane 1,4-diisocyanate, 1,6,11-undecane triisocyanate, bicycloheptane triisocyanate, dicyclopentadiene diisocyanate, norbornene diisocyanate, and isophorone diisocyanate are particularly preferred.
[0143] The hydroxyl group-containing (meth)acrylate used is preferably 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,4-cyclohexanedimethanol monoacrylate, or a mono(meth)acrylate modified with ε-caprolactone, and more preferably 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, or 4-hydroxybutyl (meth)acrylate.
[0144] As the urethane (meth)acrylate oligomer, a compound represented by the following general formula (i-1) is also preferred. [ka]
[0145] In formula (i-1), X i1 each independently represents a hydrogen atom or a methyl group; B 1 each independently represents an alkyl group having 1 to 4 carbon atoms, in which one or more -CH2- may be replaced by an oxygen atom, -CO-, -COO- or -OCO-, and b represents 1 to 20. 2 represents a group selected from the groups represented by the following formulas (i-2) to (i-6), and when b is 2 or more, a plurality of B 2 may be the same or different from each other. [ka]
[0146] B 3 represents a group selected from the groups represented by the following formulas (i-7) to (i-11), and when b is 2 or more, a plurality of B 3 may be the same or different from each other. [ka]
[0147] In formulas (i-7) to (i-11), X i4 , and X i5 each independently represents a hydrogen atom or a methyl group; X i2 , and X i3 each independently represents an alkyl group having 1 to 9 carbon atoms; Y 3 represents an alkylene group having 1 to 15 carbon atoms which may have a branched chain, a divalent aromatic group, or a divalent alicyclic hydrocarbon group, in which one or more -CH2- groups in the alkylene group may be substituted with an oxygen atom, -COO-, or -OCO-, provided that the oxygen atoms are not adjacent to each other, t1 and t2 each independently represent 0 or 1, and t3 represents an integer of 0 to 300.
[0148] The second component may be used alone or in combination of two or more.
[0149] From the viewpoint of improving adhesion, the content of the second component is preferably 5% by mass or more, more preferably 15% by mass or more, and particularly preferably 25% by mass or more, based on the total amount of the polymerizable components. From the viewpoint of reducing voltage, the content of the second component is preferably 80% by mass or less, more preferably 60% by mass or less, and particularly preferably 50% by mass or less, based on the total amount of the polymerizable components.
[0150] -Third component- The third component is a polyfunctional polymerizable compound having a weight average molecular weight of less than 2000 and represented by the following formula (iv). [ka]
[0151] In formula (iv), Y 31 represents a hydrogen atom or a methyl group, X 31represents an alkylene group having 130 or less carbon atoms, the alkylene group may have a cyclic hydrocarbon group or a branched chain, one or more -CH2- groups in the alkylene group or cyclic hydrocarbon group may be each independently substituted with -O-, -NH-, -CO-, -COO-, -OCO-, -CH=CH-, or -C≡C- so that the oxygen atoms are not directly adjacent to each other, and one or more hydrogen atoms present in the alkylene group or cyclic hydrocarbon group may each independently be substituted with a fluorine atom or -OH, n 31 represents an integer from 2 to 6.
[0152] As the polymerizable compound represented by formula (iv), it is preferable to use a polymerizable compound represented by the following formula (iv-1). [ka]
[0153] In formula (iv-1), Y 1 , and Y 2 represents a hydrogen atom or a methyl group, X 1 represents a linear or branched alkylene having 2 to 80 carbon atoms. Any carbon atom of the alkylene may be substituted with -O-, -CO-, -COO-, -OCO-, -CH=CH-, -C≡C-, or OH so that an oxygen atom is not directly adjacent to the alkylene. The number of carbon atoms of the alkylene is preferably in the range of 6 to 70, more preferably in the range of 8 to 60, and particularly preferably in the range of 9 to 50 from the viewpoint of reducing the driving voltage.
[0154] Examples of the polymerizable compound represented by formula (iv-1) include compounds represented by the following formulas (iv-1-1) to (iv-1-10). [ka]
[0155] In formulas (iv-1-1) to (iv-1-10), n and m are integers such that n+m is 1 to 10; 2 is an integer between 1 and 18, n 3 and m 2 is 3 +m 2 n is an integer between 1 and 18 4 is an integer between 1 and 23, n 5 is an integer between 1 and 23, n 6 is an integer between 4 and 30, n 7 is an integer between 2 and 10, n 8 and n 9 represents an integer from 2 to 10.
[0156] The third component may be an oligomer or a monomer. The molecular weight of the third component is preferably 1,500 or less, and more preferably 1,000 or less.
[0157] The third component may be used alone or in combination of two or more thereof, for example, an oligomer and a monomer may be used in combination.
[0158] From the viewpoint of improving heat resistance, the content of the third component is preferably 2% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the total amount of the polymerizable components. From the viewpoint of maintaining adhesion, the content of the third component is particularly preferably 50% by mass or less, 40% by mass or less, 30% by mass or less, or 25% by mass or less, based on the total amount of the polymerizable components.
[0159] -Fourth component- The fourth component is a phosphorus-based (meth)acrylate represented by the following formula (x). [ka]
[0160] In formula (x), Y 31 represents a hydrogen atom or a methyl group, X 31represents an alkylene group having 130 or less carbon atoms and having a divalent group represented by the following formula (x-1), the alkylene group may have a cyclic hydrocarbon group or a branched chain, one or more -CH- groups in the alkylene group or cyclic hydrocarbon group may be each independently substituted with -O-, -NH-, -CO-, -COO-, -OCO-, -CH=CH-, or -C≡C- so that the oxygen atoms are not directly adjacent to each other, and one or more hydrogen atoms present in the alkylene group or cyclic hydrocarbon group may each independently be substituted with a fluorine atom or -OH, n 31 represents an integer from 1 to 6. [ka]
[0161] Specifically, it is preferable to use compounds represented by the following formulae (x-2) and (x-3) as the fourth component. [ka]
[0162] In formulas (x-2) and (x-3), X 6 , X 7 , and X 8 each independently represents a hydrogen atom or a methyl group, and q, r, and s represent an integer of 1 to 4.
[0163] The fourth component may be used alone or in combination of two or more.
[0164] The content of the fourth component is preferably 0.005% by mass or more and 2% by mass or less, more preferably 0.01% by mass or more and 0.5% by mass or less, and even more preferably 0.01% by mass or more and 0.2% by mass or less, based on the total amount of the polymerizable components.
[0165] -Other polymerizable compounds- As the second polymerizable compound, a polymerizable compound other than the above-mentioned first to fourth components (for example, a polymerizable compound having a mesogenic skeleton, etc.) may be used. The content of the second polymerizable compound other than the above-mentioned first to fourth components may be 5% by mass or less, or may be 0% by mass, based on the total amount of the polymerizable components in the liquid crystal composition.
[0166] The content (total amount) of the second polymerizable compound may be 20% by mass or more, 30% by mass or more, or 40% by mass or more based on the total amount of the liquid crystal composition from the viewpoint of high scattering property and high adhesion. The content (total amount) of the second polymerizable compound may be 70% by mass or less, 60% by mass or less, or 50% by mass or less based on the total amount of the liquid crystal composition from the viewpoint of high scattering property and low voltage property. From these viewpoints, the content (total amount) of the second polymerizable compound may be 20 to 70% by mass, 30 to 60% by mass, or 40 to 50% by mass based on the total amount of the liquid crystal composition from the viewpoint of high scattering property. Here, the total amount of the liquid crystal composition is, for example, the total amount of the liquid crystal component, the polymerizable component, and the polymerization initiator in the liquid crystal composition.
[0167] The content (total amount) of the polymerizable components may be 20% by mass or more, 30% by mass or more, or 40% by mass or more based on the total amount of the liquid crystal composition from the viewpoints of high scattering properties and high adhesion. The content (total amount) of the polymerizable components may be 70% by mass or less, 60% by mass or less, or 50% by mass or less based on the total amount of the liquid crystal composition from the viewpoints of high scattering properties and low voltage properties. From these viewpoints, the content (total amount) of the polymerizable components may be 20 to 70% by mass, 30 to 60% by mass, or 40 to 50% by mass based on the total amount of the liquid crystal composition from the viewpoint of high scattering properties.
[0168] (Polymerization initiator) The polymerization initiator is used to polymerize the polymerizable compound. The polymerization initiator is preferably a photopolymerization initiator used when polymerization is performed by light irradiation. As the photopolymerization initiator, it is sufficient to use one that generates an active species corresponding to the polymerizability of the polymerizable compound, and for example, a photoradical polymerization initiator or a photocationic polymerization initiator can be used. As the photopolymerization initiator, a publicly known and commonly used one can be used.
[0169] Examples of photoradical polymerization initiators include 1-hydroxycyclohexyl phenyl ketone (Omnirad 184), 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one (Omnirad 1173), 2-methyl-1-[(methylthio)phenyl]-2-morpholinopropan-1 (Omnirad 907), 2,2-dimethoxy-1,2-diphenylethane-1-one (Omnirad BDK), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone (Omnirad 369), 2 -Alkylphenone-based photoradical polymerization initiators such as dimethylamino-2-(4-methylbenzyl)-1-(4-morpholino-phenyl)butan-1-one (OMNIRAD 379) and 2,2-dimethoxy-2-phenylacetophenone (OMNIRAD 651); 2,2-dimethoxy-1,2-diphenylethane-1-one, bis(2,4,6-trimethylbenzoyl)-diphenylphosphine oxide (OMNIRAD TPO), 2,4,6-trimethylbenzoyl-phenyl-phosphine oxide (OMNIRAD 819) (IGM acylphosphine oxide-based photoradical polymerization initiators such as 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], ethanone ("Irgacure OXE01"), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime) ("Irgacure OXE02"), "Irgacure OXE04" (BASF Ltd.), "ADEKA ARCLES NCI-831", "ADEKA ARCLES NCI-930", "ADEKA ARCLES N-1919" (ADEKA Corporation), and other oxime ester-based photoradical polymerization initiators.Examples of photoradical polymerization initiators that can be used include a mixture of 2,4-diethylthioxanthone ("Kayacure DETX" manufactured by Nippon Kayaku Co., Ltd.) and ethyl p-dimethylaminobenzoate ("Kayacure EPA" manufactured by Nippon Kayaku Co., Ltd.), a mixture of isopropylthioxanthone ("Cantacur-ITX" manufactured by Ward-Plekinsop Co., Ltd.) and ethyl p-dimethylaminobenzoate, "Esacure ONE", "Esacure KIP150", "Esacure KIP160", "Esacure 1001M", "Esacure A198", "Esacure KIP IT", "Esacure KTO46", "Esacure TZT" (manufactured by Lamberti Co., Ltd.), "Speedcure BMS", "Speedcure PBZ", and "Benzophenone" (manufactured by LAMBSON Co., Ltd.). These may be used alone or in combination of two or more.
[0170] Among the above, from the viewpoint of achieving better light-shielding properties and contrast when the voltage is turned off, it is preferable to use an oxime ester-based photoradical polymerization initiator or an acylphosphine oxide-based photoradical polymerization initiator, and it is more preferable to use an acylphosphine oxide-based photoradical polymerization initiator.
[0171] As the photocationic polymerization initiator, a photoacid generator can be used, such as a diazodisulfone-based compound, a triphenylsulfonium-based compound, a phenylsulfone-based compound, a sulfonylpyridine-based compound, a triazine-based compound, and a diphenyliodonium compound.
[0172] The content of the photopolymerization initiator is preferably from 0.1 to 10 parts by mass, more preferably from 0.2 to 6 parts by mass, based on 100 parts by mass of the total amount of the polymerizable components in the liquid crystal composition.
[0173] As the polymerization initiator, a thermal polymerization initiator can also be used. As the thermal polymerization initiator used in thermal polymerization, a known and commonly used one can be used, for example, methyl acetoacetate peroxide, cumene hydroperoxide, benzoyl peroxide, bis(4-t-butylcyclohexyl) peroxydicarbonate, t-butyl peroxybenzoate, methyl ethyl ketone peroxide, 1,1-bis(t-hexylperoxy)3,3,5-trimethylcyclohexane, p-pentahydroperoxide, t-butyl hydroperoxide, dicumyl peroxide, isobutyl peroxide, di(3-methyl-3-methoxybutyl) peroxide, Organic peroxides such as dicarbonate and 1,1-bis(t-butylperoxy)cyclohexane, azonitrile compounds such as 2,2'-azobisisobutyronitrile and 2,2'-azobis(2,4-dimethylvaleronitrile), azoamide compounds such as 2,2'-azobis(2-methyl-N-phenylpropion-amidine) dihydrochloride, azoamide compounds such as 2,2'azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, alkylazo compounds such as 2,2'azobis(2,4,4-trimethylpentane), etc. can be used. These may be used alone or in combination of two or more.
[0174] The content of the thermal polymerization initiator is preferably from 0.1 to 10 parts by mass, more preferably from 1 to 6 parts by mass, based on 100 parts by mass of the total amount of the polymerizable components in the liquid crystal composition.
[0175] (Liquid crystal component) The liquid crystal component contains at least a non-polymerizable liquid crystal compound. As the non-polymerizable liquid crystal compound, a compound represented by the following formula (3) (hereinafter also referred to as "compound (3)") is preferably used from the viewpoints of operating temperature range, operating voltage, light scattering property, solubility, etc. [ka]
[0176] In formula (3), R 11 represents an alkyl group having 1 to 10 carbon atoms (a hydrogen atom present in this group may be replaced by a fluorine atom, and one -CH2- or two or more non-adjacent -CH2- groups present in this group may each be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -COO- or -OCO-), R 12 represents a halogen atom, a cyano group, an isothiocyanate group, or an alkyl group having 1 to 10 carbon atoms (a hydrogen atom present in the alkyl group may be replaced by a fluorine atom, and one -CH2- or two or more non-adjacent -CH2- groups present in the alkyl group may each be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -COO- or -OCO-), A 11 , A 12 and A 13 are each independently (a3) a 1,4-cyclohexylene group (in which one -CH2- or two or more non-adjacent -CH2- groups may be replaced by -O-), (b3) a 1,4-phenylene group (in which one -CH= or two or more non-adjacent -CH= groups may be replaced by -N=); and (c3) a 1,4-cyclohexenyl group, a tetrahydropyran-2,5-diyl group, a 1,3-dioxane-2,5-diyl group, a decahydronaphthalene-2,6-diyl group, a pyridine-2,5-diyl group, a pyrimidine-2,5-diyl group, a pyrazine-2,5-diyl group, a naphthalene-2,6-diyl group, a 1,2,3,4-tetrahydronaphthalene-2,6-diyl group (one -CH= or two or more non-adjacent -CH=s present in the naphthalene-2,6-diyl group and the 1,2,3,4-tetrahydronaphthalene-2,6-diyl group may be replaced by -N=). wherein hydrogen atoms present in the groups (a3), (b3) and (c3) may each independently be replaced by a cyano group, a methyl group, a trifluoromethyl group, a trifluoromethyloxy group, a fluorine atom or a chlorine atom; Z 11 and Z 12 each independently represents a single bond, -CHCH-, -(CH)-, -OCH-, -CHO-, -COO-, -OCO-, -OCF-, -CFO-, -CH=NN=CH-, -CH=CH-, -CF=CF- or -C≡C-; n 11 represents an integer from 0 to 3, A 11 and Z 11 If there are multiple A's, multiple A's 11 may be the same or different, and multiple Z 11 may be the same or different. However, in the formula, oxygen atoms are not directly bonded to each other. As described above, compound (3) may contain unsaturated bonds such as -CH=CH- and -C≡C- in the molecule, but due to the structure of compound (3), groups having such unsaturated bonds (e.g., alkenyl groups) are groups that do not function as polymerizable groups and are not substantially polymerizable groups.
[0177] R 11 is preferably an alkyl group having 1 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, an alkenyl group having 2 to 8 carbon atoms, or an alkenyloxy group having 2 to 8 carbon atoms, preferably an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, or an alkenyloxy group having 2 to 5 carbon atoms, more preferably an alkyl group having 1 to 5 carbon atoms or an alkenyl group having 2 to 5 carbon atoms, still more preferably an alkyl group having 2 to 5 carbon atoms or an alkenyl group having 2 to 3 carbon atoms, and particularly preferably an alkyl group having 2 to 5 carbon atoms.
[0178] R 11 When reliability is important, R is preferably an alkyl group. 11In order to stabilize the nematic phase, the total number of carbon atoms and oxygen atoms is preferably 5 or less, and the structure is preferably linear.
[0179] R 12 is preferably a fluorine atom, a cyano group, or an alkyl group having 1 to 5 carbon atoms (in which one -CH2- or two or more non-adjacent -CH2- may be replaced by -O-).
[0180] A 11 , A 12 and A 13 Each of A preferably independently represents a group selected from the group consisting of the above group (a3) and group (b3). 13 is preferably a group (b3), and more preferably a group having a structure represented by the following formula (b3-1): [ka]
[0181] R i3 , R i4 and R i5 Each independently represents a hydrogen atom or a fluorine atom. 12 The wavy line represents the bond to Z. 12 Represents a bond to .
[0182] A 13 When A is the group (b3), in the case where it is required to increase the refractive index anisotropy (Δn), 11 and A 12 It is preferable that A is aromatic. In order to improve the response speed, 11 and A 12 From these viewpoints, A is preferably aliphatic. 11 and A 12each independently preferably represents a trans-1,4-cyclohexylene group (in which one -CH- or two or more non-adjacent -CH- groups may be replaced by -O-, and in which -CH= may be replaced by -N=), or a 1,4-phenylene group, a 2-fluoro-1,4-phenylene group, a 3-fluoro-1,4-phenylene group, a 3,5-difluoro-1,4-phenylene group or a 2,3-difluoro-1,4-phenylene group (in which one -CH= or two or more non-adjacent -CH= groups may be replaced by -N=).
[0183] Among them, A 11 and A 12 More preferably, each independently represents any one of the following structures: [ka]
[0184] The bond represented by the wavy line in the above structure is R 11 The bond on the side is R 12 It is the connecting part on the side.
[0185] A 11 and A 12 More preferably, each independently represents any one of the following structures: In the following structures, the wavy line and * have the same meaning as above. [ka]
[0186] n 11 is preferably 0, 1 or 2. When emphasis is placed on improving Δε, n 11 is preferably 0 or 1. When the transition temperature (Tni) is important, n 11 is preferably 1 or 2.
[0187] The compound (3) may be used alone or in combination of two or more. For example, the compound (3) may be used in combination of two, three, four, five, six, seven, eight, or nine types, or may be used in combination of ten or more types. There is no particular restriction on the type of compound that can be combined, but the compounds are used in combination according to the desired performance such as solubility at low temperature, transition temperature, electrical reliability, and birefringence.
[0188] The content of compound (3) may be 25% by mass or more, 35% by mass or more, or 45% by mass or more based on the total amount of liquid crystal components, polymerizable compounds, and polymerization initiators in the liquid crystal composition from the viewpoints of scattering properties and low voltage driving. The content of compound (3) may be 80% by mass or less, 70% by mass or less, or 60% by mass or less based on the total amount of liquid crystal components, polymerizable compounds, and polymerization initiators in the liquid crystal composition from the viewpoints of scattering properties and reliability. From these viewpoints, the content of compound (3) may be 25 to 80% by mass, 35 to 70% by mass, or 45 to 60% by mass based on the total amount of liquid crystal components, polymerizable compounds, and polymerization initiators in the liquid crystal composition.
[0189] The compound (3) is a liquid crystal compound having a positive dielectric anisotropy (Δε) at 25° C. (so-called p-type liquid crystal compound) or a liquid crystal compound having a dielectric anisotropy (Δε) of approximately 0 (so-called non-polar type liquid crystal compound).
[0190] In one embodiment, it is preferable to use a compound having a tolan skeleton (hereinafter referred to as a "tolan-based liquid crystal compound") as the compound (3). Specifically, as the compound (3), Z 12 It is more preferable to use a compound in which -C≡C- is used. When the liquid crystal component contains the tolane liquid crystal compound, the liquid crystal element tends to have good adhesion and light scattering properties, and low-voltage driving at room temperature and low temperatures is easily achieved.
[0191] In the tolane liquid crystal compound, R in formula (3) 12 is preferably an alkyl group (including substituted ones) having 1 to 10 carbon atoms.
[0192] In the tolane liquid crystal compound, A in formula (3) 11 is preferably a 1,4-cyclohexylene group or any of the structures represented by the following formulas (A1) to (A12), and A 12 and A 13 are preferably each independently any one of structures represented by the following formulas (A1) to (A12). [ka] [ka]
[0193] The bond represented by the wavy line in the above structure is R 11 The bond on the side is R 12 It is the connecting part on the side.
[0194] A 11 From the viewpoint of high scattering, it is more preferable that A is a 1,4-phenylene group. 12 and A 13 From the viewpoint of high-speed response, it is preferable to select the structure to have any one of the structures represented by the above formulas (A5) to (A8), (A11) and (A12).
[0195] In the tolane liquid crystal compound, Z in formula (3) 11 is preferably -C≡C-, -CF2O-, -OCF2-, trans--CH=CH-, trans--CF=CF-, -COO-, -CH2-CH2-, -CF2-CF2- or a single bond, and more preferably a single bond.
[0196] In the tolane liquid crystal compound, n in formula (3) 11 is preferably 0 or 1.
[0197] A specific example of a suitable tolan-based liquid crystal compound is a compound represented by the following formula (3T). [ka]
[0198] In formula (3T), R T1 and R T2 each independently represents an alkyl group having 1 to 10 carbon atoms (in which one -CH2- or two or more non-adjacent -CH2- groups may be replaced by -CH=CH-, -C≡C-, -O-, -CO-, -COO- or -OCO-), A T1 , A T2 and A T3 each independently represents a 1,4-phenylene group (in which one -CH= or two or more non-adjacent -CH= groups may be replaced by -N=, and a hydrogen atom in this group may be replaced by a methyl group, a cyano group, a fluorine atom or a chlorine atom), n T1 represents 0 or 1.
[0199] R T1 and R T2 The details of the alkyl group represented by the formula (3) (including preferred embodiments) are as follows: 11 The details of the alkyl group are the same as those of the alkyl group represented by the formula (I).
[0200] A T1 and A T2 are each independently preferably a 1,4-phenylene group, a 2-fluoro-1,4-phenylene group, a 3-fluoro-1,4-phenylene group, a 3,5-difluoro-1,4-phenylene group, or a 2,3-difluoro-1,4-phenylene group, and more preferably a 1,4-phenylene group, a 3-fluoro-1,4-phenylene group, or a 3,5-difluoro-1,4-phenylene group. T1 The fourth place is R T2 It is on the side.
[0201] A T3is preferably a 1,4-phenylene group, a 2-fluoro-1,4-phenylene group, a 2,6-difluoro-1,4-phenylene group, a 3-fluoro-1,4-phenylene group, a 3,5-difluoro-1,4-phenylene group, or a 5-fluoro-1,4-phenylene group, and more preferably a 1,4-phenylene group or a 2,6-difluoro-1,4-phenylene group. T1 The fourth place is R T2 It is on the side.
[0202] Preferred specific examples of the tolan-based liquid crystal compound include compounds represented by the following formulae (3T-1) and (3T-2). [ka]
[0203] R in the above formula T1 and R T2 is R in the above formula (3T). T1 and R T2 is synonymous with X T1 , X T2 , X T3 and X T4 Each of X independently represents a hydrogen atom or a fluorine atom. T1 , X T2 , X T3 and X T4 Preferably, any one of X is a fluorine atom. T1 and X T2 When either one of the above is a fluorine atom, X T3 and X T4 is preferably a hydrogen atom.
[0204] Examples of the compounds represented by formula (3T-1) and formula (3T-2) include compounds represented by the following formulas (3T-A) to (3T-D). [ka]
[0205] The tolan-based liquid crystal compounds may be used alone or in combination of two or more.
[0206] From the viewpoint of scattering, the content of the tolan liquid crystal compound may be 0% by mass or more, 20% by mass or more, or 40% by mass or more based on the total amount of the liquid crystal components in the liquid crystal composition. The content of the tolan liquid crystal compound may be 80% by mass or less, 70% by mass or less, or 60% by mass or less based on the total amount of the liquid crystal components in the liquid crystal composition. From these viewpoints, the content of the tolan liquid crystal compound may be 0 to 70% by mass, 20 to 65% by mass, or 40 to 60% by mass based on the total amount of the liquid crystal components in the liquid crystal composition. From the same viewpoint, the content of the compound represented by formula (3T) may be in the above range.
[0207] In one embodiment, compound (3) may be represented by the formula (3): 12 It is preferable to use a compound in which R is a cyano group (hereinafter referred to as a "cyan liquid crystal compound").
[0208] In the cyan liquid crystal compound, Z in formula (3) 11 and Z 12 are each preferably independently a single bond, -COO-, -OCO-, or -CH2-CH2-, and more preferably a single bond or -COO-.
[0209] In the cyan liquid crystal compound, R 11 The number of carbon atoms is preferably 2 to 7, and more preferably 2 to 5.
[0210] In the cyan liquid crystal compound, n in formula (3) 11 is preferably 0 or 1.
[0211] Preferred specific examples of the cyan liquid crystal compound include compounds represented by the following formulas (vi-1) to (vi-11). [ka]
[0212] In the above formulas (vi-1) to (vi-11), R 51 represents an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms; Y 11 ~Y 64 Each of Y independently represents a hydrogen atom or a fluorine atom. 11 ~Y 64 may all represent hydrogen atoms, or one or more of them may represent a fluorine atom.
[0213] More specific examples of the cyan liquid crystal compound include compounds represented by the following formulas (vi-A) to (vi-G).
[0214] [ka]
[0215] In the above formulas (vi-A) to (vi-G), R 511 represents an alkyl group having 2 to 7 carbon atoms or an alkoxy group having 2 to 7 carbon atoms, and preferably represents an alkyl group having 2 to 5 carbon atoms or an alkoxy group having 2 to 5 carbon atoms.
[0216] More specific examples of the cyan liquid crystal compound include the compounds represented by the following formulas (3C-1) to (3C-16). [ka] [ka] [ka] [ka]
[0217] The above cyan liquid crystal compounds may be used alone or in combination of two or more.
[0218] The content of the cyan liquid crystal compound may be 5% by mass or more, 10% by mass or more, or 15% by mass or more based on the total amount of liquid crystal components in the liquid crystal composition from the viewpoint of low driving voltage. The content of the cyan liquid crystal compound may be 100% by mass or less, 97% by mass or less, or 95% by mass or less based on the total amount of liquid crystal components in the liquid crystal composition from the viewpoint of reliability and high-speed response due to low viscosity. From these viewpoints, the content of the cyan liquid crystal compound may be 5 to 100% by mass, 10 to 97% by mass, or 15 to 95% by mass based on the total amount of liquid crystal components in the liquid crystal composition.
[0219] In one embodiment, at least one of the tolane-based liquid crystal compounds and the cyan-based liquid crystal compounds may be used in combination with a compound that does not fall into either the tolane-based liquid crystal compounds or the cyan-based liquid crystal compounds. These compounds may be used alone or in combination of two or more.
[0220] As a compound that does not fall into either the tolane type liquid crystal compound or the cyan type liquid crystal compound, for example, among the compounds (3), R 12 is an alkyl group having 1 to 10 carbon atoms (including substituted ones), and Z in formula (3) 11 and Z 12 is a single bond. Specific examples of such compounds are preferably one or more of the compounds represented by the following formulas (3M-1) to (3M-6). [ka] [ka]
[0221] The liquid crystal component may contain a liquid crystal compound other than the compound (3). The content of the liquid crystal compound other than the compound (3) is preferably 10 mass % or less based on the total amount of the liquid crystal component in the liquid crystal composition.
[0222] The transition temperature (Tni) of the liquid crystal component (all liquid crystal compounds) is preferably 95° C. or higher, more preferably 100 to 150° C., and even more preferably 130 to 140° C. Here, the transition temperature (Tni) means the temperature (upper limit temperature) at which the liquid crystal component (liquid crystal phase) undergoes a phase transition from a nematic phase to an isotropic phase. The higher the transition temperature (Tni), the more the nematic phase can be maintained even at high temperatures, and the wider the operating temperature range can be.
[0223] The refractive index anisotropy (Δn) of the liquid crystal component at 25° C. and 589 nm is preferably from 0.15 to 0.35, more preferably from 0.18 to 0.32, and further preferably from 0.20 to 0.30.
[0224] (Additive ingredients) To the liquid crystal composition, a polymerization inhibitor, an antioxidant, a light stabilizer, a chain transfer agent, a pigment, a particle having a particle diameter of less than 1 μm, a chiral compound, or an alignment material can be added within a range that does not impair practical electro-optical properties and adhesion when a liquid crystal element is produced. Among these, it is preferable to use at least one selected from the group consisting of a polymerization inhibitor, an antioxidant, a light stabilizer, a particle having a particle diameter of less than 1 μm, and a pigment. As these additives, publicly known and commonly used ones can be used, and for example, the compounds described in International Publication No. 2022 / 138418 can be used in the same amount.
[0225] <Liquid crystal layer> Another embodiment of the present invention is a liquid crystal layer formed from the liquid crystal composition of the above embodiment. This liquid crystal layer includes a polymer network derived from the above polymerizable compound (polymerizable component) and a non-polymerizable liquid crystal compound (liquid crystal component). The polymer network is composed of a polymer of the above polymerizable component (a polymer containing each of the polymerizable compounds exemplified as the polymerizable component as a monomer unit). The content of the above first to fourth components relative to the total amount of the polymerizable components in the liquid crystal composition can be interpreted as the content of the monomer units derived from each component relative to the total amount (total mass) of the polymer in the liquid crystal layer. In addition, the content of the above polymerizable component relative to the total amount of the liquid crystal composition can be interpreted as the content of the polymer relative to the total amount of the liquid crystal layer.
[0226] The liquid crystal layer contains a polymer network and a liquid crystal component, and therefore can be called a layer made of polymer-dispersed (polymer network) liquid crystal, that is, a polymer-dispersed liquid crystal layer (polymer network type liquid crystal layer). The polymer-dispersed liquid crystal layer has, for example, a structure in which the liquid crystal component forms a continuous layer in a three-dimensional network structure of a polymer, a structure in which droplets of the liquid crystal component are dispersed in a polymer, or a structure in which both are mixed. The polymer-dispersed liquid crystal layer has a structure in which the liquid crystal component is encapsulated in the polymer component, a structure in which a three-dimensional network structure of the polymer component is formed in the continuous phase of the liquid crystal component, or a structure in which both are mixed, but it is preferable that the polymer component has a three-dimensional network structure formed in the continuous phase of the liquid crystal component. The average particle size of the encapsulated liquid crystal component and the average gap distance of the three-dimensional network structure of the polymer component are preferably 0.1 μm or more, more preferably 0.2 μm or more, most preferably 0.3 μm or more, preferably 3 μm or less, more preferably 2 μm or less, and most preferably 1 μm or less. In the liquid crystal layer, the liquid crystal component and the polymer network are phase-separated from each other, so the liquid crystal layer can also be called a phase-separated liquid crystal layer.
[0227] The liquid crystal layer can be obtained, for example, by applying a liquid crystal composition onto a substrate and polymerizing a polymerizable component in the liquid crystal composition.
[0228] The liquid crystal composition may be applied by a known method such as an applicator method, a bar coating method, a roll coating method, a direct gravure coating method, a reverse gravure coating method, an inkjet method, a die coating method, or a cap coating method.
[0229] The method for polymerizing the polymerizable component in the liquid crystal composition may be a method appropriate for the type of polymerizable component (type of polymerization initiator), but it is preferable to polymerize the polymerizable component by irradiating a liquid crystal composition containing a photopolymerization initiator with ultraviolet light.
[0230] Lamps that generate ultraviolet light include metal halide lamps, high pressure mercury lamps, and ultra-high pressure mercury lamps. The wavelength of the ultraviolet light to be irradiated is preferably within the absorption wavelength range of the photopolymerization initiator contained in the liquid crystal composition, and is not within the absorption wavelength range of the liquid crystal compound contained therein. Specifically, it is preferable to use a metal halide lamp, high pressure mercury lamp, or ultra-high pressure mercury lamp while cutting out ultraviolet light of 330 nm or less. It is also preferable to use a UV-LED lamp that can irradiate a single wavelength.
[0231] The intensity of the ultraviolet light to be irradiated can be appropriately adjusted from the viewpoint of obtaining the desired liquid crystal layer, but is preferably 1 to 200 mW / cm. 2 is preferable, and 5 to 50 mw / cm 2 The time for irradiating with ultraviolet light is appropriately selected depending on the intensity of the ultraviolet light to be irradiated, but is preferably 10 to 300 seconds. The temperature during ultraviolet light irradiation is an important factor that determines the characteristics of the liquid crystal layer, and a temperature higher than the isotropic-nematic transition point (T nm) of the liquid crystal composition is preferable.
[0232] <Liquid crystal elements and light control elements> Another embodiment of the present invention is a liquid crystal element including at least a liquid crystal layer, an electrode, and a substrate supporting the liquid crystal layer and the electrode. Since the liquid crystal layer is the liquid crystal layer of the above embodiment (polymer dispersion type (polymer network type) liquid crystal layer), this liquid crystal element is a so-called polymer dispersion type (polymer network type) liquid crystal element.
[0233] Fig. 1 is a schematic cross-sectional view showing a liquid crystal element according to one embodiment. As shown in Fig. 1, the liquid crystal element 1 according to one embodiment includes a pair of electrode substrates consisting of a first electrode substrate 2 and a second electrode substrate 3, a liquid crystal layer 4 disposed between the pair of electrode substrates (the first electrode substrate 2 and the second electrode substrate 3), and an ultraviolet blocking layer 5 provided on the first electrode substrate 2 on the side opposite to the liquid crystal layer 4. That is, the liquid crystal element 1 according to one embodiment includes the second electrode substrate 3, the liquid crystal layer 4, the first electrode substrate 2, and the ultraviolet blocking layer 5 in this order in the thickness direction (stacking direction).
[0234] The liquid crystal element can be in a light scattering state by the polymer network derived from the polymerizable compound and the liquid crystal molecules (liquid crystal components) present in the gaps therebetween when no voltage is applied. On the other hand, when a voltage is applied, the liquid crystal molecules are oriented perpendicularly to the substrate, so that the liquid crystal element can be in a light transmitting state. In this way, the light transmitting state of the liquid crystal element can be changed depending on the presence or absence of voltage application. In particular, since the liquid crystal layer has a structure derived from the first polymerizable compound, which is a dye compound, the polymer network can be colored or light-shielded even for light transmitted through the polymer network portion as a waveguide, compared to an uncolored polymer network, so that a color corresponding to the absorption wavelength of the first polymerizable compound can be expressed when no voltage is applied, and sufficient light-shielding properties can be expressed. For this reason, the liquid crystal element can be used as a liquid crystal light control element incorporated in a device requiring a light control function, or as a liquid crystal display element used in a display for displaying images.
[0235] The liquid crystal element is preferably used, for example, in building materials, light control glass, smart windows for vehicles, or light control units in OLED displays. The liquid crystal element can be used for the same applications as conventional polymer-dispersed liquid crystal display elements, and is particularly preferably used in transmissive displays, flexible displays, and the like. More specifically, the liquid crystal element can be used in products such as architectural light control elements such as windows, skylights, roofs, walls, partitions, partitions, and doors, transportation light control elements such as doors, windows, doors, helmets, and sunroofs, decorative light control elements such as sunglasses, glasses, sun visors, watches, mirrors, and reflectors, and display members such as flexible liquid crystal display elements, reflective liquid crystal display elements, transparent liquid crystal display elements, and variable diffusion films.
[0236] (Electrode substrate) The first electrode substrate 2 includes a first base material 2a and a first electrode 2b provided on the first base material 2a. Similarly, the second electrode substrate 3 includes a second base material 3a and a second electrode 3b provided on the second base material 3a. In these electrode substrates, the electrodes (the first electrode 2b and the second electrode 3b) are provided so as to generate an electric field capable of controlling the alignment of liquid crystal molecules in the liquid crystal layer.
[0237] The first electrode substrate 2 is a transparent electrode substrate (transparent electrode substrate), and the first base material 2a and the first electrode 2b are made of a transparent material. That is, the first base material 2a is a transparent base material, and the first electrode 2b is a transparent electrode. Here, "transparent" means that the light transmittance in the wavelength range of 400 to 780 nm is 80% or more. In addition, unless otherwise specified, the light transmittance in this specification means the transmittance measured using a spectrophotometer (V-660).
[0238] The first substrate 2a (transparent substrate) is, for example, flat or non-flat (for example, a shape having a curved surface). The material constituting the first substrate 2a (transparent substrate) may be glass or plastic. That is, the first substrate 2a (transparent substrate) may be a glass substrate or a plastic substrate. From the viewpoint of weight reduction and workability in the post-process, the first substrate 2a (transparent substrate) is preferably a plastic substrate. Examples of materials for the plastic substrate include cellulose derivatives, polyolefins, polyesters, polyolefins, polycarbonates, polyacrylates, polyarylates, polyethersulfones, polyimides, polyphenylene sulfides, polyphenylene ethers, nylons, and polystyrenes. Among them, polyesters (for example, PET), polystyrenes, polyolefins, cellulose derivatives, polyarylates, polycarbonates, polyimides, and the like are preferably used.
[0239] The first substrate 2a (transparent substrate) may have a thickness of, for example, 5 to 500 μm.
[0240] The first electrode 2b (transparent electrode) is, for example, in the form of a film. The shape of the first electrode 2b (transparent electrode) is not particularly limited, and the conductive part of the electrode may be formed in a stripe shape, a mesh shape, a random mesh shape, or the like. Examples of materials constituting the first electrode 2b (transparent electrode) include known transparent conductive materials such as ITO (indium tin oxide), IZO (indium zinc oxide), and IZTO (indium zinc tin oxide).
[0241] The thickness of the first electrode 2b (transparent electrode) may be, for example, 5 to 500 nm.
[0242] The second electrode substrate 3 may be a transparent electrode substrate like the first electrode substrate 2, but in some cases may be a non-transparent electrode substrate (for example, a colored electrode substrate, an electrode substrate having light blocking properties, etc.).
[0243] The second substrate 3a is, for example, flat or non-flat (for example, a shape having a curved surface). As the second substrate 3a, a substrate that is usually used for a liquid crystal display element, an organic light-emitting display element, other display elements, optical components, light control elements, colorants, markings, printed matter, or optical films can be used. There is no particular limitation on the material of the second substrate 3a, and, for example, in addition to the glass substrate and plastic substrate used for the first substrate 2a, a metal substrate, a ceramic substrate, a paper substrate, or the like can be used. The second substrate 3a may be transparent or may be a colored substrate. As the second substrate 3a, a substrate with low visible light transmittance (for example, a substrate of gray color, etc.) can also be used in order to impart light shielding properties to the second electrode substrate 3.
[0244] The second electrode 3b is, for example, in the form of a film. The shape of the second electrode 3b is not particularly limited, and for example, the conductive part of the electrode may be formed in a stripe shape, a mesh shape, a random mesh shape, or the like. The material of the second electrode 3b is not particularly limited, and may be a known metal material. As such a metal material, in addition to the transparent conductive material used for the first electrode 2b, for example, Al, Cu, Au, Ag, Cr, Ta, Ti, Mo, W, Ni, or an alloy containing at least one of these can be used.
[0245] The ranges of the thickness of the second base material 3a and the thickness of the second electrode 3b may be the same as the above-mentioned ranges exemplified for the thickness of the first base material 2a and the thickness of the first electrode 2b, respectively.
[0246] The substrates (first substrate 2a and second substrate 3a) of the first electrode substrate 2 and the second electrode substrate 3 may be surface-treated to improve the adhesion of the liquid crystal element. Examples of the surface treatment include ozone treatment, plasma treatment, corona treatment, and silane coupling treatment. In addition, in order to adjust the light transmittance and reflectance, an organic thin film, an inorganic oxide thin film, a metal thin film, or the like may be provided on the substrate surface by a method such as deposition. In addition, in order to add optical value, the substrate may be a pickup lens, a rod lens, an optical disc, a retardation film, a light diffusion film, a microlens sheet, a color filter, or the like. In addition, the substrate may be provided with an anti-reflection function, a reflection function, or the like, as necessary.
[0247] Although not shown, the first electrode substrate 2 and the second electrode substrate 3 may be bonded to each other by a sealant and a sealing material such as an epoxy-based thermosetting composition arranged in the peripheral region. Between the first electrode substrate 2 and the second electrode substrate 3, for example, granular spacers such as glass particles, plastic particles, alumina particles, or spacer pillars made of resin formed by a photolithography method may be arranged to maintain the distance between the substrates.
[0248] (UV blocking layer) The ultraviolet blocking layer 5 is a layer having a light transmittance of 0.1% or less in a wavelength range of 378 nm or less. The light transmittance of the ultraviolet blocking layer 5 in a wavelength range of 412 nm or less is preferably 30% or more, and may be 50% or more. The light transmittance of the ultraviolet blocking layer 5 in a wavelength range of 400 nm or less may be more than 0.1% (for example, more than 0.1% to 90%), but may be 0.1% or less. The light transmittance of the ultraviolet blocking layer 5 in a wavelength range of 394 nm or less may be 0.1% or less. When the light transmittance of the ultraviolet blocking layer 5 in a wavelength range of 394 nm or less is 0.1% or less, the light transmittance of the ultraviolet blocking layer 5 in a wavelength range of 412 nm or less is preferably 50% or more.
[0249] The ultraviolet blocking layer 5 is optically transparent to light in the long wavelength region. The optical transmittance of the ultraviolet blocking layer 5 in the wavelength region of 420 nm or more is, for example, 80% or more.
[0250] The ultraviolet blocking layer 5 is, for example, in the form of a film. Examples of materials constituting the ultraviolet blocking layer 5 include various plastic films mixed with or coated with an ultraviolet absorbing agent, optical interference type substrates, etc. It may also be a coating layer formed by directly coating the electrode substrate 2 with a resin containing an ultraviolet absorbing agent.
[0251] The thickness of the ultraviolet blocking layer 5 may be, for example, 10 μm to 5 mm.
[0252] As the ultraviolet blocking layer 5, for example, ultraviolet blocking films available such as the SC series ultraviolet absorbing filter with a TAC substrate manufactured by Fuji Film Corporation, the acrylic substrate ultraviolet cut filter manufactured by Nitto Plastics Co., Ltd., the colored glass filter manufactured by HOYA Corporation, and the UV cut filter manufactured by 3M Corporation can be used.
[0253] Methods for arranging the ultraviolet blocking layer 5 include a method in which a film substrate serving as the ultraviolet blocking layer is bonded to the first electrode substrate 2, and a method in which the ultraviolet blocking layer is directly formed on the first electrode substrate 2 by a technique such as coating.
[0254] The liquid crystal element of the present invention is not limited to the liquid crystal element of the above embodiment. For example, an ultraviolet blocking layer may be further provided on the opposite side of the second electrode substrate 3 to the liquid crystal layer 4. That is, the liquid crystal element may have a pair of ultraviolet blocking layers so as to sandwich the pair of electrode substrates (the first electrode substrate 2 and the second electrode substrate 3) and the liquid crystal layer 4. In this case, the second electrode substrate 3 may be a transparent electrode substrate. The details of the transparent electrode substrate are the same as those of the first electrode substrate 2. In addition, when the liquid crystal element of the present invention is obtained by laminating an element including a pair of electrode substrates and a liquid crystal layer disposed between the pair of electrode substrates to another substrate, the substrate, a pressure sensitive adhesive (PSA), an intermediate film such as PVB or EVA used for lamination, or the like may be the ultraviolet blocking layer 5. That is, the ultraviolet blocking layer 5 may be formed by imparting an ultraviolet blocking function to these substrates or the like. As a method for imparting an ultraviolet blocking function to intermediate films such as PSA, PVB, or EVA, for example, a method of incorporating an ultraviolet absorbing agent or the like into these materials may be mentioned. The liquid crystal element of the present invention does not necessarily have to include an ultraviolet blocking layer, but the use of an ultraviolet blocking layer can improve the light resistance of the liquid crystal element.
[0255] The liquid crystal element may further include an alignment film so that the liquid crystal molecules in the liquid crystal element are aligned horizontally or vertically, and the substrate may be subjected to an alignment treatment. Examples of the alignment film include films made of compounds such as polyimide, polysiloxane, polyamide, polyvinyl alcohol, polycarbonate, polystyrene, polyphenylene ether, polyarylate, polyethylene terephthalate, polyethersulfone, epoxy resin, epoxy acrylate resin, acrylic resin, azo compound, coumarin compound, chalcone compound, cinnamate compound, fulgide compound, anthraquinone compound, azo compound, and arylethene compound, or polymers or copolymers of the above compounds. Examples of the alignment treatment include stretching, rubbing, polarized ultraviolet-visible light irradiation, ion beam treatment, and oblique deposition of SiO2 on the substrate. When performing rubbing to impart a tilt angle to the liquid crystal molecules, the compound to be aligned by rubbing is preferably one in which crystallization of the material is promoted by adding a heating step during or after the alignment treatment. Among the compounds to be aligned other than rubbing, it is preferable to use a photoalignment material. In general, when a liquid crystal composition is brought into contact with a substrate having an alignment function, the liquid crystal molecules are aligned in the direction of the alignment treatment of the substrate near the substrate. Whether the liquid crystal molecules are aligned parallel to the substrate, tilted, or perpendicular is greatly influenced by the alignment treatment method for the substrate.
[0256] The liquid crystal element can be used as it is, or can be attached to another substrate before use. The liquid crystal element may be laminated with an adhesive, a bonding layer, a pressure sensitive adhesive, a pressure sensitive adhesive layer, a protective film, a polarizing film, or the like.
[0257] The liquid crystal element may be configured so that the orientation of the liquid crystal molecules can be controlled by applying a voltage, and may be a vertical electric field type liquid crystal element, a horizontal electric field type liquid crystal element, or other electric field type liquid crystal element (for example, a fringe electric field type adopted in the FFS drive mode). Among these, it is preferable that the liquid crystal element is configured as a vertical electric field type liquid crystal element.
[0258] A vertical electric field type liquid crystal element is a liquid crystal element in which electrodes are arranged so that an electric field is generated vertically to the alignment film. In a vertical electric field type liquid crystal element, electrodes are usually provided on both of a pair of transparent substrates that sandwich a liquid crystal layer. In other words, a transparent electrode substrate that includes a transparent substrate and an electrode is used.
[0259] A vertical electric field type liquid crystal element has, for example, a pair of transparent electrode substrates (a first transparent electrode substrate and a second transparent electrode substrate) and a liquid crystal layer disposed between the pair of transparent electrode substrates. A liquid crystal element having such a structure is suitably used as a light control element. That is, another embodiment of the present invention is a light control element having a pair of transparent electrode substrates and the liquid crystal layer of the above embodiment disposed between the pair of transparent electrode substrates.
[0260] The light control element may be, for example, an element that electrically controls the transmittance of light. The light control element may be equipped with a voltage application device. The light control element may have a structure in which a laminate of the above-mentioned liquid crystal layer and transparent electrode substrate is sandwiched between two pieces of glass via an intermediate film such as PVB (polyvinyl butyral), EVA (ethylene vinyl acetate copolymer resin), TPU (polyurethane-based), SGP, etc., to form a laminated glass. In addition, the light control element may be provided with a functional film for blocking ultraviolet rays, heat rays, etc.
[0261] From the viewpoint of productivity, it is preferable to fabricate a vertical electric field type liquid crystal element by, for example, using a roll-to-roll method, dropping or applying the liquid crystal composition of the above embodiment onto a substrate by an ODF method or the like, laminating an opposing substrate, and then polymerizing the polymerizable component in the liquid crystal composition to produce a liquid crystal element.
[0262] In the manufacturing process of a liquid crystal element by a roll-to-roll method, a liquid crystal composition is applied onto a first electrode, or onto a glass substrate having an alignment film and a first electrode, or onto a plastic substrate, and then the liquid crystal composition is bonded to a second electrode, or onto a glass substrate having an alignment film and a second electrode, or onto the electrode side or the alignment film side of the plastic substrate so as to be in contact with the liquid crystal composition, and after making the thickness approximately uniform, the polymerizable component in the liquid crystal composition is polymerized to manufacture the liquid crystal element.
[0263] The method for applying the liquid crystal composition and the method for polymerizing the polymerizable component are as described above in the method for producing the liquid crystal layer.
[0264] In the manufacturing process of the liquid crystal element using the ODF method, a sealant such as an epoxy-based photocurable and heat-curable sealant is applied in a closed-loop bank shape using a dispenser on either the backplane or frontplane substrate of the hollow element, and a predetermined amount of the liquid crystal composition is then dropped into the bank under degassing conditions, after which the frontplane and backplane are joined to manufacture the liquid crystal element.
[0265] When preparing a liquid crystal element, the thickness between the substrates (substrate interval) may be adjusted by inserting spacers (particles, etc.) between two substrates to maintain the distance, as in known methods for preparing liquid crystal elements. The thickness between the substrates, i.e., the thickness of the phase separation layer, is preferably 2 to 50 μm, more preferably 10 to 30 μm. The spacers may be dispersed on the substrates in advance, or may be mixed in the liquid crystal composition in advance and applied to the substrates simultaneously with the liquid crystal composition.
[0266] The method for sandwiching the liquid crystal composition between two substrates may be a normal vacuum injection method, but is preferably performed by dropping or coating such as the ODF method. During the period from dropping or coating to polymerization of the polymerizable component, the liquid crystal composition is preferably in a substantially uniform isotropic state.
[0267] When dropping or coating is performed, the liquid crystal composition can be sandwiched between two substrates by, for example, sandwiching the two substrates with a laminator. EXAMPLES
[0268] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the compositions of the following examples and comparative examples, "parts" means "parts by mass".
[0269] <Preparation of first polymerizable compound (polymerizable dye)> (Synthesis Example 1: Synthesis of polymerizable dye 1) Under a dry nitrogen atmosphere, 1,5-dihydroxyanthracene-9,10-dione (3.0 g), 4-hydroxybutyl acrylate (3.6 g), triphenylphosphine (7.21 g), and tetrahydrofuran (60 mL) were mixed and cooled on ice. Diisopropyl azodicarboxylate (5.32 g) was added dropwise under ice cooling, and the mixture was stirred at room temperature for 6 hours. Water (200 mL) was added to the reaction solution, and then dichloromethane (200 mL) was added to separate the liquid. The organic layer was washed with water (100 mL) and dried by adding anhydrous sodium sulfate. After filtering the drying agent, the mixture was concentrated, and the resulting residue was purified by silica gel column chromatography. The obtained crude product was reprecipitated from dichloromethane and methanol to obtain 1.58 g of a compound represented by the following formula (1-1-1a) (1,5-bis(4-acryloxybutane-1-oxy)anthracene-9,19-dione) as polymerizable dye 1. 1 The H-NMR assignments are shown below. 1 H-NMR (400MHz, CDCl3, TMS internal standard) δ(ppm)=7.89(dd,J=7.8,0.9Hz,2H),7.66(t,J=8.0Hz,2H),7.24(d,J=7.8Hz,2H),6.40(dd,J=17.2,1 .6Hz,2H),6.12(dd,J=17.4,10.5Hz,2H),5.81(dd,J=10.3,1.6Hz,2H),4.30(t,J=5.9Hz,4H),4.19(t,J=5.7Hz,4H),2.02-2.07(m,8H) [ka]
[0270] (Synthesis Example 2: Synthesis of polymerizable dye 2) Under a dry nitrogen atmosphere, 1-amino-2,4-dibromoanthracene-9,10-dione (110 g), 4-butylaniline (108 g), copper(II) acetate (10.5 g), potassium acetate (71.0 g) and toluene (1000 mL) were mixed and stirred at 120° C. for 72 hours. After cooling to room temperature, 10% hydrochloric acid (900 mL) and toluene (500 mL) were added and separated. A saturated aqueous solution of sodium bicarbonate (600 mL) was added to the organic layer to neutralize and separate the layers. The organic layer was washed with saturated saline (600 mL) and dried by adding anhydrous sodium sulfate. Sodium sulfate was removed by filtration, and the organic solvent was distilled off under reduced pressure to obtain 1-amino-2-bromo-4-((4-butylphenyl)amino)anthracene-9,10-dione (102 g). 1-amino-2-bromo-4-((4-butylphenyl)amino)anthracene-9,10-dione 1 The H-NMR assignments are shown below. 1 H-NMR (400MHz, CD3COCD3): δ(ppm)=11.94(1H,s), 8.37-8.32(2H,m), 7.88-7.85(3H, m), 7.34-7.28(4H,m), 2.67(2H,t), 1.69-1.61(2H,m), 1.45-1.35(2H,m), 0.95(3H,t)
[0271] Next, under a dry nitrogen atmosphere, 1-amino-2-bromo-4-((4-butylphenyl)amino)anthracene-9,10-dione (90.0 g), 4-butylphenol (90.1 g), potassium hydroxide (33.7 g) and pyridine (800 mL) were mixed and stirred at 110° C. for 22 hours. After cooling to room temperature, toluene (3000 mL) and water (1000 mL) were added and the mixture was separated. After 10% hydrochloric acid (900 mL) was added to the organic layer and the mixture was separated, a saturated aqueous sodium bicarbonate solution (600 mL) was added to the organic layer to neutralize and separate the organic layer. The organic layer was washed with saturated saline (1000 mL) and dried by adding anhydrous sodium sulfate. The sodium sulfate was removed by filtration, and the organic solvent was distilled off under reduced pressure. The resulting residue was purified by silica gel column chromatography, and then reprecipitated with dichloromethane and hexane solvents to obtain 1-amino-2-(4-butylphenoxy)-4-((4-butylphenyl)amino)anthracene-9,10-dione (66.9 g, yield 64%). 1 The H-NMR assignments are shown below. 1 H-NMR (400MHz, CDCl3, TMS internal standard) δ(ppm)=12.33(s,1H),8.36(dt,J=7.0,1.6Hz,2H),7.68-7.75(m,2H),7.16-7.19(m,2H),6.95- 7.03(m,6H),6.79(s,1H),2.59(t,J=7.8Hz,2H),2.53(t,J=7.8Hz,2H),1.50-1.62(m,4H),1.29-1.40(m,4H),0.91-0.97(m,6H)
[0272] Next, under a dry nitrogen atmosphere, 1-amino-2-(4-butylphenoxy)-4-((4-butylphenyl)amino)anthracene-9,10-dione (1.4 g), acryloyl chloride (0.3 g), triethylamine (0.4 g) and dichloromethane (24 mL) were mixed and stirred at room temperature for 26 hours. Water (100 mL) and dichloromethane (100 mL) were added and separated. Anhydrous sodium sulfate was added to the organic layer to dry it. Sodium sulfate was removed by filtration, and the obtained filtrate was purified by silica gel column chromatography. By reprecipitation with dichloromethane and methanol, 0.2 g (yield 16%) of the compound (N-(2-(4-butylphenoxy)-4-((4-butylphenyl)amino)-9,10-dioxo-9,10-dihydroanthracene-1-yl)acrylamide) represented by the following formula (1-2-1a) was obtained as the polymerizable dye 2. Mass spectrum of polymerizable dye 2 and 1 The H-NMR assignments and phase transition temperatures are shown below. MS m / z: 572 [M + ] Phase transition temperature: Cr150Iso 1 H-NMR (400MHz, CDCl3, TMS internal standard) δ(ppm)=11.76(s,1H),10.23(s,1H),8.28(dd,J=7.8,0.9Hz,1H),8 .19(dd,J=7.5,1.1Hz,1H),7.77(td,J=7.5,1.4Hz,1H),7.71(td,J=7.5,1.5Hz,1H),7.12(dt,J=8.8 ,2.3Hz,2H),7.02(dq,J=14.2,2.9Hz,6H),6.86(s,1H),6.34-6.44(m,2H),5.77(q,J=4.0Hz,1H),2 .52-2.58(m,4H),1.51-1.60(m,4H),1.34(tdd,J=14.8,7.4,4.7Hz,4H),0.93(td,J=7.3,4.6Hz,6H) [ka]
[0273] (Synthesis Example 3: Synthesis of polymerizable dye 3) Under dry nitrogen, 1,4-dichloroanthracene-9,10-dione (1.50 g), 4-aminophenol (1.77 g), disodium hydrogen phosphate (1.54 g) and N-methylpyrrolidone (10 mL) were mixed, heated to 160°C and stirred for 16 hours. After cooling to room temperature, methanol (70 mL) was added and the resulting precipitate was filtered. The precipitate was washed with water (50 mL) and then dried to obtain 1,4-bis(4-hydroxyphenylamino)anthracene-9,10-dione (1.90 g).
[0274] Next, 1,4-bis(4-hydroxyphenylamino)anthracene-9,10-dione (1.90 g), potassium carbonate (1.87 g), 6-chloro-1-hexyl acrylate (2.57 g), and dimethyl sulfoxide (40 mL) were mixed and heated to 80° C. After stirring for 15 hours, the mixture was cooled on ice and water (100 mL) was added. The resulting precipitate was filtered and washed with water (50 mL) and methanol (50 mL). The obtained solid was purified by silica gel column chromatography and then reprecipitated from dichloromethane and methanol to obtain 1.21 g of a compound represented by the following formula (1-3-1a) (1,4-bis(4-(6-acryloxyhexane-1-oxy)phenylamino)anthracene-9,10-dione) as polymerizable dye 3. The amount of polymerizable dye 3 was 1.21 g. 1 The H-NMR assignments are shown below. 1 H-NMR (400MHz, CDCl3, TMS internal standard) δ(ppm)=12.19(s,2H),8.39(td,J=6.3,3.0Hz,2H),7.74(td, J=6.3,3.2Hz,2H),7.30(s,2H),7.17(td,J=6.2,3.7Hz,4H),6.90(td,J=6.1,3.8Hz,4H),6.40 (dd,J=17.4,1.8Hz,2H),6.12(dd,J=17.2,10.3Hz,2H),5.81(dd,J=10.5,1.4Hz,2H),4.18(t ,J=6.6Hz,4H),3.97(t,J=6.4Hz,4H),1.78-1.85(m,4H),1.69-1.76(m,4H),1.42-1.55(m,8H) [ka]
[0275] (Measurement of maximum absorption wavelength) The maximum absorption wavelengths of the obtained polymerizable dyes 1 to 3 were measured by the following method. First, 1.0 part by mass of the compound to be measured (polymerizable dyes 1 to 3) was added to 100 parts by mass of any liquid crystal composition capable of dissolving the compound to be measured (polymerizable dyes 1 to 3) and dissolved to prepare a measurement sample. Next, a cell was prepared using two 2 cm x 2 cm glass substrates having an ITO electrode and a horizontal alignment film on the ITO electrode, with the ITO electrode layer as the inside of the cell, and an injection port adjusted to a cell thickness of 10 μm by plastic particles. A sample was injected into the cell, and the injection port was sealed with a sealant to prepare a device. Next, the maximum absorption wavelengths of the polymerizable dyes 1 to 3 were obtained by measuring the absorption spectrum between 370 and 780 nm using the prepared device under conditions of 25°C and no voltage application using a spectrometer (Otsuka Electronics Co., Ltd., "LCD-5200" or Hitachi High-Tech Science Co., Ltd., "U-4100"). The results are shown below. [Maximum absorption wavelength in the range of 370-780 nm] Polymerizable dye 1:377nm Polymerizable dye 2: 535nm Polymerizable dye 3: 641nm
[0276] <Preparation of Polymerizable Mixture (MA)> A polymerizable compound (second polymerizable compound) and a polymerization initiator shown in Table 1 below were mixed in the compounding ratio shown in Table 1, and the polymerization initiator was dissolved in the polymerizable compound while stirring at 50° C., to obtain a polymerizable mixture (PL1). The obtained polymerizable mixture (PL1) was used in the examples and comparative examples described later.
[0277] [Table 1]
[0278] (Synthesis Example 4: Synthesis of urethane acrylate) In a flask equipped with a stirring blade, 44.4 parts (0.2 moles) of IPDI (isophorone diisocyanate) was charged, and while stirring, 810 parts (0.1 moles) of polypropylene glycol (average molecular weight Mw: 8100) was charged while being careful of heat generation, and the temperature was raised to 70°C. The reaction was carried out at this temperature for 7 hours to obtain a urethane polymer having an isocyanate group at the end. Next, 23.2 parts (0.2 moles) of 2-hydroxyethyl acrylate (molecular weight 116) was charged, and the reaction was carried out at this temperature for another 7 hours. After confirming that the absorption of NCO had disappeared in the infrared absorption spectrum, the mixture was taken out and a polymerizable compound (2-1) (average molecular weight Mw: 29800), which is a urethane acrylate, was obtained. The weight average molecular weight (Mw) is a value converted into polystyrene based on GPC measurement. The measurement conditions for GPC are as follows.
[0279] [GPC measurement conditions] Measurement equipment: Tosoh Corporation "HLC-8320 GPC" Column: Tosoh Corporation guard column "SuperHZ-L" + Tosoh Corporation "SuperHZ2000" x 3 + Tosoh Corporation "TSuperHZM-M" Detector: Built-in RI detector Data processing: Tosoh Corporation "EcoSEC-WorkStation Ver2.01" Measurement conditions: column temperature 40°C, developing solvent tetrahydrofuran, flow rate 1.0 ml / min Standard: Monodisperse polystyrene with a known molecular weight was used in accordance with the instrument measurement manual.
[0280] <Preparation of Liquid Crystal Mixture (LC)> A plurality of liquid crystal compounds were mixed together to prepare liquid crystal mixtures (LC1 and LC2) having the compositions shown in Table 2. These liquid crystal mixtures (LC1 and LC2) were used in the examples and comparative examples described later.
[0281] [Table 2]
[0282] In Table 2, the structure of the liquid crystal compound is shown by symbols and numbers. Each symbol represents a group in the structure shown below, and the terminal numbers (1 to 5) represent a linear alkyl group having the same number of carbon atoms as the number. For example, the compound represented by 2-Ph-E-Ph3-CN means the compound represented by the above formula (3C-1). [ka]
[0283] In Table 2, the physical property value "Tni" means the temperature (maximum temperature) at which the liquid crystal component (liquid crystal phase) of the above liquid crystal mixture transitions from a nematic phase to an isotropic phase, and is a value measured using a polarizing microscope.
[0284] In Table 2, the physical property value "Δn" means the refractive index anisotropy of the liquid crystal component of the liquid crystal mixture at 25°C and 589 nm, and is measured using an Abbe refractometer to determine the refractive index (n e ) and the refractive index (n o ) is measured and calculated.
[0285] <Examples 1 to 3 and Comparative Examples 1 to 2> (Preparation of Liquid Crystal Composition) The polymerizable dye, liquid crystal mixture (LC1 or LC2), and polymerizable mixture (PL1) were mixed in the combination and blending ratio (unit: parts by mass) shown in Table 3 below, and the polymerizable dye and the liquid crystal mixture were dissolved in the polymerizable mixture while stirring at 50°C. Then, bead spacers with an average particle size of 15 μm were added thereto to obtain liquid crystal compositions (polymer-dispersed liquid crystal forming compositions) of Examples 1 to 3 and Comparative Examples 1 to 2. The blending amount of the bead spacers was set to 1 mass % based on the total mass of the liquid crystal composition. In addition, "S-428" in Table 3 is a non-polymerizable dye manufactured by Mitsui Chemicals.
[0286] [Table 3]
[0287] (Fabrication of liquid crystal elements) Using the liquid crystal composition obtained above, liquid crystal elements (polymer-dispersed liquid crystal elements) of Examples 1 to 3 and Comparative Examples 1 to 2 were produced, respectively. Specifically, first, two PET films with ITO electrodes were prepared as electrode substrates, and the above composition was applied to the ITO electrode side of one electrode substrate to form a coating film, and the other electrode substrate was placed on the coating film so that the surface on the ITO electrode side was in contact with the coating film. Next, a uniform pressure was applied to the obtained laminate using a laminator (FUJIPLA LPD2313 manufactured by HISAGO CORPORATION), and then the laminate was heated to 15 mw / cm with a UV-LED lamp. 2 The film was irradiated with UV light having a wavelength of 365 nm for 60 seconds to obtain a liquid crystal element (polymer dispersion type liquid crystal display element).
[0288] (Measurement of total light transmittance) Electrode wiring was attached to the liquid crystal element obtained above, and the total light transmittance was measured before and after the heat resistance test with and without voltage application using a haze meter (NDH-7000 manufactured by Nippon Denshoku Industries Co., Ltd.). The heat resistance test was performed by placing the liquid crystal element in a thermostatic chamber at 100°C and heating it for 100 hours. The total light transmittance was measured by applying a square wave voltage of 60 Hz and 0 to 100 V at 25°C in accordance with JIS K 7361-1 and JIS K 7136. Table 4 shows the total light transmittance when no voltage was applied (T0 and T0'), the total light transmittance when AC100V was applied (T100 and T100'), and the rate of change in the total light transmittance (R0 and R100). When the initial total light transmittance T0 when no voltage was applied was 50% or less, the light blocking property was evaluated as sufficient, and when the rate of change R0 in the total light transmittance when no voltage was applied was 15% or less, the heat resistance was evaluated as excellent. The rate of change in the total light transmittance was calculated using the following formula. Rate of change (unit: %) = [(total light transmittance after heat resistance test) / (initial total light transmittance)-1] x 100
[0289] [Table 4] [Explanation of symbols]
[0290] 1...liquid crystal element, 2...first electrode substrate, 3...second electrode substrate, 4...liquid crystal layer, 5...ultraviolet ray blocking layer, 2a...first base material, 2b...first electrode, 3a...second base material, 3b...second electrode.
Claims
1. Contains a polymerizable compound, a polymerization initiator, and a non-polymerizable liquid crystal compound; The liquid crystal composition comprises a first polymerizable compound having a maximum absorption wavelength in the range of 370 to 780 nm, and a second polymerizable compound not having a maximum absorption wavelength in the range of 370 to 780 nm.
2. The liquid crystal composition according to claim 1 , wherein the first polymerizable compound includes two or more compounds having different maximum absorption wavelengths.
3. The liquid crystal composition according to claim 1 , wherein the first polymerizable compound includes a compound having an anthraquinone skeleton.
4. The first polymerizable compound is represented by the following formula (1): 【Chemistry 1】 [In the formula, A 1 and A 2 are each independently (a) a 1,4-cyclohexylene group (one —CH 2 - or two or more non-adjacent -CH 2 Each - may be independently replaced by -O- or -S-, and -CH= in this group may be replaced by -N=. (b) a 1,4-phenylene group (in which one -CH= or two or more non-adjacent -CH= groups may be replaced by -N=); (c) 1,4-cyclohexenylene group, bicyclo[2.2.2]octane-1,4-diyl group, naphthalene-2,6-diyl group, naphthalene-1,4-diyl group, 1,2,3,4-tetrahydronaphthalene-2,6-diyl group, 5,6,7,8-tetrahydronaphthalene-1,4-diyl group, decahydronaphthalene-2,6-diyl group, anthracene-2,6-diyl group, anthracene-1,4-diyl group, anthracene-9,10-diyl group, phenanthrene-2, 7-diyl group (one -CH= or two or more non-adjacent -CH= present in a naphthalene-2,6-diyl group, a naphthalene-1,4-diyl group, a 1,2,3,4-tetrahydronaphthalene-2,6-diyl group, a 5,6,7,8-tetrahydronaphthalene-1,4-diyl group, an anthracene-2,6-diyl group, an anthracene-1,4-diyl group, an anthracene-9,10-diyl group, or a phenanthrene-2,7-diyl group may be replaced by -N=), and (d) a thiophene-2,5-diyl group, a thiophene-2,4-diyl group, a benzothiophene-2,5-diyl group, a benzothiophene-2,6-diyl group, a dibenzothiophene-3,7-diyl group, a dibenzothiophene-2,6-diyl group, or a thieno[3,2-b]thiophene-2,5-diyl group (one -CH= or two or more non-adjacent -CH= in these groups may be replaced by -N=). or a single bond, and hydrogen atoms present in the groups (a), (b), (c) and (d) may each independently be replaced by a methyl group, an ethyl group, a propyl group, a 2-propyl group, a butyl group, a 2-butyl group, a methoxy group, an ethoxy group, a methylthio group, an ethylthio group, a dimethylamino group, a diethylamino group, a cyano group, a nitro group, a fluorine atom or a chlorine atom; Z 1 and Z 2 each independently represents a single bond, -N=CH-, -CH=N-, -N=N-, -C≡C-, a linear or branched alkylene group having 1 to 20 carbon atoms, or a linear or branched alkenylene group having 2 to 30 carbon atoms, 2 - may be substituted by -O-, -COO- or -OCO-, and a hydrogen atom present in the alkylene group or alkenylene group may be substituted by a fluorine atom; R 1 and R 2 each independently represents a hydrogen atom, a non-polymerizable group having 1 to 30 carbon atoms, or a polymerizable group having 0 to 20 carbon atoms; R 1 and R 2 At least one of the groups is the polymerizable group, X 1 and X 2 each independently represents -O-, -S-, or -NY-, where Y is a group represented by the following formula (2): 【Chemistry 2】 (In the formula, A 3 and Z 3 are the above A 1 and Z 1 is synonymous with R 3 represents a hydrogen atom or a non-polymerizable group having 1 to 30 carbon atoms, and * represents a bond to the nitrogen atom. is a group represented by n 1 , n 2 and n 3 each independently represents an integer of 0 to 3, m 1 and m 2 Each independently represents an integer of 0 to 4, 1 +m 2 is 1 or more, A 1 , A 2 , A 3 , Z 1 , Z 2 , Z 3 , X 1 , X 2 , R 1 , R 2 , R 3 , n 1 , n 2 and n 3 If there are multiple A's, 1 , A 2 , A 3 , Z 1 , Z 2 , Z 3 , X 1 , X 2 , R 1 , R 2 , R 3 , n 1 , n 2 and n 3 may be the same or different from each other. However, in the formula, oxygen atoms are not directly bonded to each other. The liquid crystal composition according to claim 1 , comprising a compound represented by the formula:
5. The first polymerizable compound is represented by the following formulas (1-1) to (1-3): 【Chemistry 3】 【Chemistry 4】 【Chemistry 5】 [In the formula, A 1a , A 2a , A 1b , A 2b , A 3b , A 1c and A 2c Each independently represents the A 1 is synonymous with Z 1a , Z 2a , Z 1b , Z 2b , Z 3b , Z 1c and Z 2c Each independently represents Z 1 is synonymous with R 1a , R 2a , R 1b , R 2b , R 3b , R 1c and R 2c Each independently represents the R 1 is the same as R 1a and R 2b At least one of R 1b , R 2b and R 3b At least one of, and R 1c and R 2c At least one of the groups is the polymerizable group, X 1a , X 2a and X 1b each independently represents -O- or -S-; n 1a , n 2a , n 1b , n 2b , n 3b , n 1c and n 2c each independently represents an integer of 0 to 3, A 1a , A 2a , A 1b , A 2b , A 3b , A 1c , A 2c , Z 1a , Z 2a , Z 1b , Z 2b , Z 3b , Z 1c and Z 2c If there are multiple A's, 1a , A 2a , A 1b , A 2b , A 3b , A 1c , A 2c , Z 1a , Z 2a , Z 1b , Z 2b , Z 3b , Z 1c and Z 2c may be the same or different from each other. However, in the formula, oxygen atoms are not directly bonded to each other.
2. The liquid crystal composition according to claim 1, comprising at least one compound selected from the group consisting of compounds represented by the following formula:
6. The liquid crystal composition according to claim 1 , further comprising a non-polymerizable dye compound.
7. The non-polymerizable liquid crystal compound is represented by the following formula (3): 【Chemistry 6】 [In the formula, R 11 is an alkyl group having 1 to 10 carbon atoms (a hydrogen atom in this group may be replaced by a fluorine atom, and one —CH 2 - or two or more non-adjacent -CH 2 Each - may be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -COO- or -OCO-; R 12 represents a halogen atom, a cyano group, an isothiocyanate group, or an alkyl group having 1 to 10 carbon atoms (a hydrogen atom present in the alkyl group may be replaced by a fluorine atom, and one —CH 2 - or two or more non-adjacent -CH 2 Each - may be independently replaced by -CH=CH-, -C≡C-, -O-, -CO-, -COO- or -OCO-; A 11 , A 12 and A 13 are each independently (a3) 1,4-cyclohexylene group (one —CH 2 - or two or more non-adjacent -CH 2 - may be replaced with -O-. (b3) a 1,4-phenylene group (in which one -CH= or two or more non-adjacent -CH= groups may be replaced by -N=); and (c3) 1,4-cyclohexenyl group, tetrahydropyran-2,5-diyl group, 1,3-dioxane-2,5-diyl group, decahydronaphthalene-2,6-diyl group, pyridine-2,5-diyl group, pyrimidine-2,5-diyl group, pyrazine-2,5-diyl group, naphthalene-2,6-diyl group, 1,2,3,4-tetrahydronaphthalene-2,6-diyl group (one -CH= or two or more non-adjacent -CH= in the naphthalene-2,6-diyl group and the 1,2,3,4-tetrahydronaphthalene-2,6-diyl group may be replaced by -N=). wherein hydrogen atoms present in the groups (a3), (b3) and (c3) may each independently be replaced by a cyano group, a methyl group, a trifluoromethyl group, a trifluoromethyloxy group, a fluorine atom or a chlorine atom; Z 11 and Z 12 each independently represents a single bond, —CH 2 CH 2 -, -(CH 2 ) 4 --, --OCH 2 --, --CH 2 O-, -COO-, -OCO-, -OCF 2 -, -CF 2 represents O-, -CH=N-N=CH-, -CH=CH-, -CF=CF- or -C≡C-; n 11 represents an integer from 0 to 3, A 11 and Z 11 If there are multiple A's, 11 may be the same or different, and multiple Z 11 may be the same or different from each other. However, in the formula, oxygen atoms are not directly bonded to each other. The liquid crystal composition according to claim 1 , comprising a compound represented by the formula:
8. The liquid crystal composition according to claim 7 , wherein the compound represented by formula (3) includes a compound having a tolan skeleton.
9. The following formula (1-2) 【Chemistry 7】 [In the formula, A 1b , A 2b and A 3b are each independently (a) a 1,4-cyclohexylene group (one —CH 2 - or two or more non-adjacent -CH 2 Each - may be independently replaced by -O- or -S-, and -CH= in this group may be replaced by -N=. (b) a 1,4-phenylene group (in which one -CH= or two or more non-adjacent -CH= groups may be replaced by -N=); (c) 1,4-cyclohexenylene group, bicyclo[2.2.2]octane-1,4-diyl group, naphthalene-2,6-diyl group, naphthalene-1,4-diyl group, 1,2,3,4-tetrahydronaphthalene-2,6-diyl group, 5,6,7,8-tetrahydronaphthalene-1,4-diyl group, decahydronaphthalene-2,6-diyl group, anthracene-2,6-diyl group, anthracene-1,4-diyl group, anthracene-9,10-diyl group, phenanthrene-2, 7-diyl group (one -CH= or two or more non-adjacent -CH= present in a naphthalene-2,6-diyl group, a naphthalene-1,4-diyl group, a 1,2,3,4-tetrahydronaphthalene-2,6-diyl group, a 5,6,7,8-tetrahydronaphthalene-1,4-diyl group, an anthracene-2,6-diyl group, an anthracene-1,4-diyl group, an anthracene-9,10-diyl group, or a phenanthrene-2,7-diyl group may be replaced by -N=), and (d) a thiophene-2,5-diyl group, a thiophene-2,4-diyl group, a benzothiophene-2,5-diyl group, a benzothiophene-2,6-diyl group, a dibenzothiophene-3,7-diyl group, a dibenzothiophene-2,6-diyl group, or a thieno[3,2-b]thiophene-2,5-diyl group (one -CH= or two or more non-adjacent -CH= in these groups may be replaced by -N=). or a single bond, and hydrogen atoms present in the groups (a), (b), (c) and (d) may each independently be replaced by a methyl group, an ethyl group, a propyl group, a 2-propyl group, a butyl group, a 2-butyl group, a methoxy group, an ethoxy group, a methylthio group, an ethylthio group, a dimethylamino group, a diethylamino group, a cyano group, a nitro group, a fluorine atom or a chlorine atom; Z 1b , Z 2b and Z 3b each independently represents a linear or branched alkylene group having 1 to 20 carbon atoms, a linear or branched alkenylene group having 2 to 30 carbon atoms, -CH 2 O-, -OCH 2 -, -CF 2 O-, -OCF 2 represents -, -COO-, -OCO-, -N=CH-, -CH=N-, -N=N-, -C≡C- or a single bond, and a hydrogen atom present in the alkylene group and alkenylene group may be substituted with a fluorine atom, R 1b , R 2b and R 3b each independently represents a hydrogen atom, a non-polymerizable group having 1 to 30 carbon atoms, or a polymerizable group having 0 to 20 carbon atoms; R 1b , R 2b and R 3b At least one of the groups is the polymerizable group, X 1b represents -O- or -S-; n 1b , n 2b and n 3b each independently represents an integer of 0 to 3, A 1b , A 2b , A 3b , Z 1b , Z 2b and Z 3b If there are multiple A's, 1b , A 2b , A 3b , Z 1b , Z 2b and Z 3b may be the same or different from each other. However, in the formula, oxygen atoms are not directly bonded to each other. A pigment compound represented by the formula:
10. A liquid crystal layer formed from the liquid crystal composition according to any one of claims 1 to 8, A liquid crystal layer comprising the polymer network derived from the polymerizable compound and the non-polymerizable liquid crystal compound.
11. A pair of transparent electrode substrates; A light control element comprising: the liquid crystal layer according to claim 10 disposed between the pair of transparent electrode substrates.
Citation Information
Patent Citations
Dyes for color filters, and photosensitive resist resin composition containing the same
US5578419A
Polymer-dispersed liquid crystal composition, liquid crystal element, and light control element
WO2022138418A1