Electrets containing substituted cyclotriphosphazene compounds and articles obtained therefrom
Patent Information
- Application Number
- JP2023536847
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-12-18
- Filing Date
- 2021-11-29
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2041-11-29
AI Technical Summary
Existing electret materials used in microfiber webs for aerosol filtration do not effectively enhance particle capture, and there is a need for improved charge-enhancing additives that maintain a semi-permanent charge under standard atmospheric conditions.
Incorporation of substituted cyclotriphosphazene cores with at least three amino-cyclic carbon groups as charge-enhancing additives in thermoplastic resins, which are blended into fibers and charged through triboelectric methods to form electret materials.
The cyclotriphosphazene cores provide a semi-permanent electret charge, enhancing filtration performance by maintaining high charge levels over the product's life, as evidenced by improved Quality Factor (QF) values and effective particle capture.
Smart Images

Figure 2022130080000001 
Figure 2022130080000002 
Figure 2022130080000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to the use and applications of substituted cyclotriphosphazene compounds as charge-enhancing additives for electret webs, including nonwoven fibrous webs. Summary of the Invention
[0002] Electrets are dielectric materials that have a permanent or semi-permanent electric charge or dipole polarization. Electrets are useful in a variety of devices, including, for example, food packaging wraps, air filters, filtering facepieces, and respirator devices, and as electrostatic elements in electroacoustic devices such as microphones, headphones, and electrostatic recording devices.
[0003] The performance of microfiber webs used in aerosol filtration can be improved by imparting an electric charge to the fibers and forming an electret material. In particular, electrets are effective in enhancing particle capture in aerosol filters. Many methods are known for forming electret materials in microfiber webs. Such methods include, for example, bombarding meltblown fibers with charged particles, such as electrons or ions, as the fibers are formed and emerge from the die orifice. Other methods include, for example, charging the fibers after the web is formed by corona discharge or imparting an electric charge to a fiber mat by carding and / or needle tacking (tribocharging). Additionally, methods have been described in which a water jet or a stream of water droplets is impinged on a nonwoven web at a pressure sufficient to enhance the electret charge by filtration (hydrocharging).
[0004] Various charge enhancing additives have been developed for use in electret materials. US Patent No. 9,815,068 describes an electret web comprising a thermoplastic resin and a charge enhancing additive, the charge enhancing additive being a divalent metal-containing substituted mercaptobenzoimidazolate salt. US Patent No. 10,240,269 describes an electret web comprising a thermoplastic resin and a charge enhancing additive, the charge enhancing additive being a condensed aromatic thiourea, a condensed aromatic urea compound, or a combination thereof. The charge enhancing additive may also include a hindered amine light stabilizer compound.
[0005] In one aspect, the present disclosure describes a composition including a substituted cyclotriphosphazene core as a charge enhancing additive in a thermoplastic resin.
[0006] In one embodiment, the compositions disclosed herein can be used in filtration articles, such as respirators.
[0007] In another aspect, a method of making an electret is described, comprising providing a composition comprising (i) a thermoplastic resin and (ii) a substituted cyclotriphosphazene core having at least three amino-cyclic carbon groups, and charging the composition by corona treatment, hydrocharging, tribocharging, or a combination thereof to form an electret.
[0008] The above summary of the invention is not intended to describe every embodiment. The details of one or more embodiments of the invention are also set forth in the following detailed description. Other features, objects, and advantages will be apparent from the detailed description and claims. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view of an exemplary core-sheath fiber according to the present disclosure.
[0010] [Diagram 2] 1 is a schematic perspective view of a nonwoven fibrous web according to the present disclosure.
[0011] [Diagram 3] FIG. 1 is a schematic front view of an exemplary respirator 40 according to one embodiment of the present disclosure.
[0012] [Figure 4] 4 is a schematic cross-sectional view of the mask body 42 of FIG. 3.
[0013] Repeated use of reference characters in the specification and drawings is intended to represent the same or similar features or elements of the present disclosure. It is to be understood that those skilled in the art can devise numerous other modifications and embodiments that are within the spirit and scope of the principles of the present disclosure. The figures may not be drawn to scale. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] As used herein, The terms "a," "an," and "the" are used interchangeably and mean one or more; "And / or" is used to indicate that either or both of the stated cases may occur; for example, A and / or B includes (A and B) as well as (A or B).
[0015] Further herein, the recitation of ranges by endpoints includes all numbers subsumed within that range (eg, 1 to 10 includes 1.4, 1.9, 2.33, 5.75, 9.98, etc.).
[0016] Further, as used herein, references to "at least one" include all numbers greater than or equal to one (e.g., at least 2, at least 4, at least 6, at least 8, at least 10, at least 25, at least 50, at least 100, etc.).
[0017] As used herein, "comprising at least one of" A, B, and C refers to a single element A, a single element B, a single element C, A and B, A and C, B and C, and combinations of all three.
[0018] The compositions of the present disclosure include cyclophosphazene compounds, which are used as electrostatic enhancing additives in thermoplastic resins.
[0019] The charge enhancing additives disclosed herein are cyclotriphosphazene cores substituted with at least three amino-carbocyclic groups.
[0020] In one embodiment, the amino-carbocyclic group comprises an amino group and a cycloalkyl group. The cycloalkyl group may be substituted or unsubstituted with an alkyl chain. In one embodiment, the amino-cycloalkyl group comprises, for example, 5, 6, 7, or 8 carbon atoms.
[0021] In one embodiment, the amino-carbocyclic group comprises an amino group and an aryl group. The amino-carbocyclic group comprising an aryl group may further comprise an ether, an amine, an alkyl group, and combinations thereof. In one embodiment, the amino-aryl group comprises, for example, 6, 7, 8, 9, 10, 11, or even 12 carbon atoms. Exemplary amino-aryl groups include phenylamino, alkylphenylamino, alkoxyphenylamino, phosphoramino indane, or alkylaminophenoxy groups.
[0022] In one embodiment, the charge enhancing additive has Formula I: [ka] where L is selected from NH or N(R), R is an alkyl group optionally containing at least one catenated atom selected from N (amino) or O (ether), and X comprises a carbocyclic group containing 5-6 cyclic carbon atoms. As a common convention, the lines intersecting the cyclotriphosphazene core are substituents attached to any of the phosphorus atoms of the ring, with the remainder of the phosphorus atoms being bonded to -H to satisfy valences.
[0023] In other embodiments, the charge enhancing additive has formula (II): [ka] [wherein X comprises an amino group and a cyclic carbocyclic group containing at least 5 to 6 carbon atoms].
[0024] In one embodiment, the charge enhancing additive is at least one of the following: [ka] [ka]
[0025] Cyclotriphosphazene cores substituted with at least three amino-carbocyclic groups may be commercially available or can be synthesized, for example, by substituting 1,3,5,2,4,6-triazatriphosphorine-2,2,4,4,6,6-hexachloride with phenols or arylamines, as shown in the Examples section below. Generally, the amino-carbocyclic groups substituted in the cyclotriphosphazene core are synthetically identical.
[0026] The cyclotriphosphazene cores substituted with at least three amino-cyclic carbon groups disclosed herein can be used as charge enhancing additives, which are materials that improve the quality factor (QF) as described below.
[0027] Preferably, the cyclotriphosphazene core substituted with at least three amino-cyclic carbon groups used as the charge enhancing additive is solid at ambient conditions to prevent migration within the resin and does not decompose at moderate temperatures (such as processing temperatures). In one embodiment, the charge enhancing additive is solid at temperatures of at least 25°C, 30°C, 40°C, 50°C, 60°C, 80°C, or even 100°C. In one embodiment, the charge enhancing additive does not decompose. For example, when heated to 220°C, 235°C, or even 250°C, there is no significant weight loss (i.e., less than 5% by weight, less than 1% by weight, or even less than 0.1% by weight) as measured under nitrogen by thermogravimetric analysis using a heating rate of 10°C / min.
[0028] The cyclotriphosphazene core substituted with at least three amino-carbocyclic groups disclosed herein does not need to be covalently bonded to the thermoplastic resin, but instead is blended into the thermoplastic resin. The cyclotriphosphazene core substituted with at least three amino-carbocyclic groups of the present disclosure can be effective as a charge enhancing additive in relatively small amounts. Typically, the cyclotriphosphazene core substituted with at least three amino-carbocyclic groups is present in the thermoplastic resin in an amount up to about 10% by weight, more typically in the range of 0.01 to 5% by weight, based on the total weight of the blend. In some embodiments, the cyclotriphosphazene core substituted with at least three amino-carbocyclic groups is present in the electret composition in an amount ranging from 0.1 to 3% by weight, 0.1 to 2% by weight, 0.2 to 1.0% by weight, or 0.25 to 0.5% by weight.
[0029] Typically, the at least three amino-carbocyclic group substituted cyclotriphosphazene cores disclosed herein are blended with a thermoplastic resin and made into fibers.
[0030] Thermoplastic resins useful in the present disclosure include any thermoplastic non-conductive polymer that is capable of retaining a significant amount of trapped electrostatic charge when formed into a web and charged. Typically, such polymeric resins will have a thermal conductivity of 10 to 40% at the temperature of the intended application.14 It has a DC (direct current) resistivity of more than Ω-cm. Polymers capable of acquiring trapped charges include polypropylene; polyethylene (e.g., HDPE, LDPE, LLDPE, VLDPE; ULDPE, UHMW-PE grades); polyolefins such as poly(1-butene); poly(3-methylbutene); poly(4-methyl-1-pentene); polyvinyl chloride; polystyrene; polycarbonate; polyesters including polylactide; and perfluorinated polymers and copolymers. Preferably, the thermoplastic resin comprises polypropylene.
[0031] Examples of suitable thermoplastic resins include, for example, polypropylene resins: ESCORENE PP 3746G available from Exxon-Mobil Corporation (Irving, TX); TOTAL PP3960, TOTAL PP3860, and TOTAL PP3868 available from Total Petrochemicals USA Inc. (Houston, TX); and METOCENE MF 650W available from LyondellBasell Industries, Inc. (Rotterdam, Netherlands); and poly-4-methyl-1-pentene resins TPX-DX820, TPX-DX470, and TPX-MX002 available from Mitsui Chemicals (Tokyo).
[0032] The blend of thermoplastic resin and charge enhancing additive can be prepared by well-known methods. Typically, the blend of charge enhancing additive and thermoplastic resin is processed using melt extrusion technology, so the blend can be pre-blended to form pellets in a batch process, or the thermoplastic resin and charge enhancing additive can be mixed in an extruder in a continuous process. When using a continuous process, the thermoplastic resin and charge enhancing additive can be pre-blended as solids, or added separately to the extruder and mixed in a molten state.
[0033] Examples of melt mixers that can be used to form pre-blended pellets include those that provide dispersive mixing, distributive mixing, or a combination of dispersive and distributive mixing. Examples of batch processes include those that use a BRABENDER (e.g., BRABENDER PREP CENTER available from CW Brabender Instruments, Inc.; South Hackensack, New Jersey) or a BANBURY internal mixing and roll milling device (e.g., equipment available from Farrel Co.; Ansonia, Connecticut). After batch mixing, the resulting mixture may be immediately quenched and stored below the melting temperature of the mixture for later processing.
[0034] Examples of continuous processes include single screw extrusion, twin screw extrusion, disk extrusion, reciprocating single screw extrusion, and pin barrel single screw extrusion. Continuous processes can include the use of both cavity transfer mixers (e.g., CTM available from RAPRA Technology, Ltd., Shrewsbury, England) and distributive or dispersive mixing elements such as pin mixing elements, static mixing elements (e.g., available from MADDOCK mixing elements or SAXTON mixing elements).
[0035] Examples of extruders that can be used to extrude the pre-blended pellets prepared by the batch process include the same types of equipment described above for continuous processing. Useful extrusion conditions are generally those suitable for extruding the resin without additives.
[0036] In one embodiment, the resin containing the electrostatic enhancing additive is a fiber. The fiber may have any cross-sectional shape, for example, triangular, square, rectangular, pentagonal, hexagonal, heptagonal, octagonal, star, elliptical, trilobal, and tetralobal.
[0037] In one embodiment, the fiber is a fiber core encapsulated with a sheath, a so-called sheath-core fiber as shown in FIG. 1. In FIG. 1, the sheath-core fiber 100 includes a core 110 with a sheath layer 120 disposed thereon. Although not shown, the sheath layer 120 is coextensive along the fiber length (fiber ends excluded). The core can have any average diameter, but preferably ranges from 1 to 100 microns, more preferably 5 to 50 microns, and even more preferably 10 to 25 microns. In one embodiment, the sheath layer can be a thin layer, for example, having an average thickness of at least 0.05, 0.1, 0.2, 0.4, 0.5, or even 0.6 microns thick, and up to 0.8, 1.0, 1.5, 2.0, 2.5, 2.8, or even 3.0 microns thick.
[0038] In one embodiment, the composition may include a secondary charge enhancing additive in addition to the substituted cyclotriphosphazene core disclosed herein. Such secondary charge enhancing additives are known in the art and include hindered amine light stabilizer additives, triazine additives, and hindered phenol additives.
[0039] Specific examples of hindered amine or triazine additives include poly[[6-(1,1,3,3-tetramethylbutyl)amino]-s-triazine-2,4-diyl][[(2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidyl)imino]] available under the trade name "CHIMASSORB 944" from BASF, Ludwigshafen, Germany; dimethyl succinate-1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate available under the trade name "TINUVIN 622" from BASF; di-tert-butyl-4-hydroxybenzyl)-2-n-butylmalonate bis(1,2,2,6,6-pentamethyl-4-piperidyl) available under the trade name "CHIMASSORB 2020" from BASF; polycondensates of dibutylamine-1,3,5-triazine-N,N'-bis(2,2,6,6-tetramethyl-4-piperidyl-1,6-hexamethylenediamine-N-(2,2,6,6-tetramethyl-4-piperidyl)butylamine available under the trade name "TINUVIN 1577" from BASF; 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-((hexyl)oxy)-phenol available under the trade name "UVINUL N-substituted amino aromatic compounds, particularly the triamino substituted compounds, such as 2,4,6-trianilino-p-(carbo-2'-ethylhexyl-1'-oxy)-1,3,5-triazine, available under the tradename "T-150"; and 2,4,6-tris-(octadecylamino)triazine, also known as tristearylmelamine ("TSM").
[0040] The hindered phenol additive has a hydroxyl group as a terminal functional group. The hindered phenol additive is not particularly limited, and specific examples thereof include pentaerythrityl-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (Irganox 1010, manufactured by BASF), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (Irganox 1076, manufactured by BASF), tris-(3,5-di-tert-butyl-4-hydroxybenzyl)-isocyanurate (Irganox 3114, manufactured by BASF), and 3,9-bis-{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)-propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro-[5,5]undecane (Sumilizer-GA-80, manufactured by Sumitomo Chemical Co., Ltd.).
[0041] Triazine-based charge enhancing additives include thermally stable organic triazine compounds or oligomers containing at least one nitrogen atom in addition to the nitrogen atom in the triazine ring, as disclosed in U.S. Pat. Nos. 6,268,495, 5,976,208, 5,968,635, 5,919,847, and 5,908,598 to Rousseau et al.
[0042] Further examples of charge enhancing additives are provided in U.S. Patent Application Publication No. 2011 / 0137082 (Li et al.), U.S. Pat. No. 8,613,795 (Li et al.), U.S. Pat. No. 7,390,351 (Leir et al.), U.S. Pat. No. 5,057,710 (Nishiura et al.), and U.S. Pat. Nos. 4,652,282 and 4,789,504 (both to Susumu et al.), and U.S. Pat. No. 8,790,449(B2) (Li et al.).
[0043] Generally, the charge enhancing additive does not include hindered amine compounds that include ether-linked groups attached to nitrogen atoms in a NOR-type configuration (typically referred to as NOR-HALS). Exemplary NOR-HALS are disclosed in U.S. Pat. No. 7,947,767 (Chin et al.), which is incorporated herein by reference. Exemplary commercially available NOR-HALS include the hindered amine NOR stabilizer available from BASF under the trade name "TINUVIN NOR371". In one embodiment, the composition is substantially free of NOR-HALS (i.e., contains less than 0.05 wt.%, or even less than 0.01 wt.%, or even contains no NOR-HALS).
[0044] In one embodiment, the composition may include one or more conventional adjuvants such as antioxidants, light stabilizers, plasticizers, acid neutralizers, fillers, antibacterial agents, surfactants, antiblocking agents, pigments, primers, dispersants, and other adhesion promoters.The incorporation of antibacterial agents and strengthening agents discussed in U.S. Patent No. 7,879,746 (Klun et al.) (hereby incorporated by reference) may be particularly beneficial for medical applications.The incorporation of surfactants discussed in U.S. Patent Application Publication No. 2012 / 0077886 (Scholz et al.) (hereby incorporated by reference) may be particularly beneficial for certain applications.
[0045] In one embodiment, additive compounds can be added to the resin to modify the surface properties of the fiber, such as stain release or oil repellency. For example, the fiber is fluorinated. In one embodiment, a fluorinated compound (e.g., a fluorinated compound available as Repellent Polymer Melt Additive PM-870 from 3M Co., Maplewood, MN) can be added to the polymer resin. In another embodiment, the fiber can be placed in an atmosphere containing a fluorine-containing species and an inert gas, and then discharged to modify the surface chemistry of the fiber. The discharge can be in the form of a plasma, such as an AC corona discharge. This plasma fluorination process results in the presence of fluorine atoms on the surface of the polymer article. The plasma fluorination process is described in many U.S. Patents 6,397,458, 6,398,847, 6,409,806, 6,432,175, 6,562,112, 6,660,210, and 6,808,551 to Jones / Lyons et al. Electret articles having a high fluorosaturation ratio are described in U.S. Pat. No. 7,244,291 to Spartz et al., and electret articles having a low fluorosaturation ratio with heteroatoms are described in U.S. Pat. No. 7,244,292 to Kirk et al. Other publications disclosing fluorination techniques include: U.S. Pat. Nos. 6,419,871, 6,238,466, 6,214,094, 6,213,122, 5,908,598, 4,557,945, 4,508,781, and 4,264,750; U.S. Patent Application Publication Nos. 2003 / 0134515(A1) and 2002 / 0174869(A1); and WO 01 / 07144.
[0046] Generally, the fibers disclosed herein do not include fiber finishes. Fiber finishes are treatments used to change the surface properties of fibers to allow easier / improved processing of the fibers. In one embodiment, the fibers of the present disclosure are substantially free of sorbitan fatty acid esters or polyoxyalkylene alkyl esters (including less than 30% by weight, less than 20% by weight, less than 10% by weight, less than 5% by weight, less than 1% by weight, less than 0.5% by weight, or even less than 0.1% by weight).
[0047] The fibers used in the practice of the present disclosure may have any average fiber diameter and may be continuous, random, and / or staple fibers. For example, in some embodiments, the fibers (i.e., individual fibers) may have an average fiber diameter of at least 5, 6, 8, or even 10 micrometers, and up to 15, 18, 20, 22, or even 25 micrometers.
[0048] In one embodiment, the diameter of the fibers can be determined by microscopy (e.g., optical microscopy or scanning electron microscopy), where the fibers are cross-sectioned and viewed under magnification to determine the diameter of the fiber.
[0049] In one embodiment, the fiber diameter can be calculated by measuring the pressure drop across the fiber web. The effective fiber diameter (EFD) can be calculated as described in CNDavies, The Separation of Airborne Dust and Particulates, Institution of Mechanical Engineers, London Proceedings, IB (1952). In practice, fiber thickness may show some experimental variation as a result of routine experimental variation and the averaging nature of EFD.
[0050] The fibers (filaments) described herein can generally be made using techniques known in the art for making filaments, including wet spinning, dry spinning, melt spinning, melt blowing, or gel spinning.
[0051] Particularly advantageous is melt spinning. In melt spinning, a polymer is heated and passed through a spinneret, and the fiber solidifies upon cooling. For example, a melt spinning process can be carried out to collect multicomponent filaments. As used herein, the term "melt spinning" refers to filaments formed by extruding molten filaments from a set of orifices, cooling and (at least partially) solidifying the filaments to form filaments, where the filaments pass through an air space (which may include a moving air stream) to aid in the cooling and solidification of the filaments, and then passing the thus formed fibers through an attenuation (i.e., drawing) unit to draw the fibers.
[0052] Melt spinning can be distinguished from melt blowing in that melt blowing involves the extrusion of molten filaments into a converging high-velocity air stream introduced by an air-blowing orifice located in close proximity to the extrusion orifice. Melt spinning can also be distinguished from electrospinning in that electrospinning can be described as extrusion from a desired solvent solution. Spinneret modifications result in multicomponent (e.g., core-sheath) fibers (see, for example, U.S. Pat. Nos. 4,406,850 (Hills), 5,458,972 (Hagen), 5,411,693 (Wust), 5,618,479 (Lijten), and 5,989,004 (Cook)). Filaments according to the present disclosure can also be made by fibrillation of a film, which can provide filaments with a rectangular cross section.
[0053] 2, an exemplary nonwoven fibrous web 200 includes fibers 210 and optional secondary fibers 220. Fibers 210 have an average fiber diameter between 2 and 100 microns and include a substituted cyclotriphosphazene compound according to the present disclosure. The optional secondary fibers may be any fiber type and / or have any average fiber diameter.
[0054] Nonwoven fibrous webs can be made, for example, by conventional airlaid, carded, stitchbonded, spunbonded, wetlaid, airlaid and / or meltblown procedures.
[0055] Spunbond nonwoven fibrous webs can be formed according to well-known conventional methods in which melt-spun fibers are deposited on a moving belt, where they form a nonwoven continuous fibrous web with interfiber bonds. Meltblown nonwoven fibrous webs are made by a similar process, except that high-velocity gas impinges on the extruded fibers, thereby stretching and thinning them, before they are collected on a rotating drum. Meltblown fibrous webs also have interfiber bonds, but they generally do not have the cohesive strength of the corresponding spunbond fibrous webs.
[0056] In some embodiments, the nonwoven web can be produced by air laying of fibers. Airlaid nonwoven fibrous webs can be made using equipment such as those available from Rando Machine Company (Macedon, New York) as RANDO WEBBER. In some embodiments, a type of airlaying process called gravity laying can be used, for example, as disclosed in U.S. Patent Application Publication No. 2011 / 0247839 (Lalouch), the disclosure of which is incorporated herein by reference. Nonwoven fibrous webs can be densified and strengthened by techniques such as, for example, cross-lap, stitch-bonding, needle-tuck, hydroentanglement, chemical bonding, and / or thermal bonding. In other embodiments, the nonwoven web is not an airlaid fibrous web.
[0057] The nonwoven fibrous web according to the present disclosure may have any basis weight, thickness, porosity, and / or density unless otherwise specified. In some embodiments, the nonwoven fibrous web is a bulky open nonwoven fibrous web. In some embodiments, the fibers of the nonwoven fibrous web have an effective fiber diameter of at least 3, 4, 5, 10, 15, 20 micrometers, or 25 micrometers and up to 125, 100, 90, 80, 75, 50, 40 micrometers, or even 30 micrometers.
[0058] In one embodiment, the web comprises a distribution of fiber lengths. In one embodiment, the distribution comprises long fiber stands. For example, fibers having lengths greater than 40, 60, 100, 500, or even 1000 millimeters. These long fiber strands can theoretically be of infinite length, but are typically less than 2000 meters, or even less than 1000 meters in length.
[0059] The fibers of the present disclosure and / or nonwoven fibrous webs containing the fibers of the present disclosure may be charged as formed or may be charged after formation. In the case of electret filtration media (e.g., nonwoven fibrous webs), the media is generally charged after the fibrous web is formed.
[0060] Generally, any standard charging method known in the art can be used. For example, charging can be performed in a variety of ways, including tribocharging, hydrocharging, and corona discharge. A combination of methods can also be used. As mentioned above, in some embodiments, the electret web of the present disclosure has the desirable feature that it can be charged by corona discharge alone, particularly DC corona discharge, without the need for additional charging methods. Examples of suitable corona discharge processes are described in U.S. Pat. No. Re. 30,782 (van Turnhout), U.S. Pat. No. Re. 31,285 (van Turnhout), U.S. Pat. No. Re. 32,171 (van Turnhout), U.S. Pat. No. 4,215,682 (Davis et al.), U.S. Pat. No. 4,375,718 (Wadsworth et al.), U.S. Pat. No. 5,401,446 (Wadsworth et al.), U.S. Pat. No. 4,588,537 (Klaase et al.), U.S. Pat. No. 4,592,815 (Nakao), U.S. Pat. No. 6,365,088 (Knight et al.), British Pat. No. 384,052 (Hansen), U.S. Pat. No. 5,643,525 (McGinty et al.), and Japanese Pat. No. 4,141,679(B2) (Kawabe et al.). Further methods are discussed by M. Paajanen et al. in Journal of Physics D: Applied Physics (2001), vol. 34, pp. 2482-2488, and by GM Essler and JE West in Journal of Electrostatics (1975), 1, pp. 111-123.
[0061] Another technique that can be used to charge an electret web is hydrocharging. Hydrocharging of a web is performed by contacting the fibers with water in a manner sufficient to impart an electric charge to the fibers, and then drying the web. One example of hydrocharging involves applying a water jet or a stream of water droplets to the web at a pressure sufficient to enhance the electret charge by filtration into the web, and then drying the web. The pressure required to achieve optimal results will vary depending on the type of sprayer used, the type of polymer from which the web is formed, the type and concentration of additives added to the polymer, the thickness and density of the web, and whether a pretreatment such as a corona surface treatment is performed before hydrocharging. Generally, water pressures in the range of about 10 to 500 psi (69 to 3450 kPa) are suitable. The water jet or stream of water droplets can be provided by any suitable spray device. One example of a useful spray device is a device used for hydroentangling of fibers. An example of a suitable method of hydrocharging is described in U.S. Pat. No. 5,496,507 (Angadjivand et al.). Other methods are described in U.S. Patent No. 6,824,718 (Eitzman et al.), U.S. Patent No. 6,743,464 (Insley et al.), U.S. Patent No. 6,454,986 (Eitzman et al.), U.S. Patent No. 6,406,657 (Eitzman et al.), and U.S. Patent No. 6,375,886 (Angadjivand et al.) Hydrocharging of the web may also be accomplished using the method disclosed in U.S. Patent No. 7,765,698 (Sebastian et al.).
[0062] Surprisingly, it has been discovered that compositions comprising a cyclotriphosphazene core substituted with at least three amino-cyclic carbon groups can have an electret charge. By electret charge, it is meant that there is at least a semi-permanent charge, and by "semi-permanent" it is meant that the charge exists for a period long enough to be significantly measurable under standard atmospheric conditions (22°C, atmospheric pressure of 101,300 Pascals, and 50% relative humidity). The charge can be characterized by an X-ray discharge test as described in U.S. Pat. No. 9,815,067 (Schultz et al.), column 18, lines 12-42, which is incorporated herein by reference. Unlike static charges that dissipate immediately (such as those that may be generated as a result of friction), the electret charge of a (e.g., nonwoven) web article is a semi-permanent charge that is substantially maintained over the intended product life of the article. Thus, sufficient charge is evident during use as well as at least 6 or 12 months after manufacture.
[0063] To ensure that a particular filter material is electrostatically charged in nature, its performance may be examined after exposure to ionizing X-ray radiation. As described in the literature (Air Filtration by RC Brown (Pergamon Press, 1993 and "Application of Cavity Theory to the Discharge of Electrostatic Dust Filters by x-Rays", AJ WAKER and RC BROWN, Applied Radiation and Isotopes, Vol. 39, No. 7, pp. 677-684, 1988), if a filter that is electrostatically charged is exposed to X-rays, the aerosol will penetrate the filter more after exposure than before, because the ions generated by the X-rays in the pores between the fibers have neutralized some of the charge. Thus, a plot of transmission versus cumulative X-ray exposure can be obtained that steadily increases to a certain level and then does not change further with irradiation. At this point, all the charge has been removed from the filter. In some embodiments, the electret charge of a (for example, single) fiber web can be characterized by exhibiting a % transmission of at least 50%.
[0064] In one embodiment, the composition comprising the cyclotriphosphazene core substituted with at least three amino-cyclic carbon groups of the present disclosure is not flame retardant. As used herein, "flame retardant" means that the composition is more flame resistant than the same composition made without the cyclotriphosphazene core substituted with at least three amino-cyclic carbon groups of the present disclosure. Many tests are known to measure the flame retardancy of a material. For example, oxygen index, ASTM D-635 (horizontal) and UL94 tests are often used to evaluate the flammability properties of polymers. Any one of these tests can be used to determine the (lack of) flame retardancy of the present composition.
[0065] Fibers according to the present disclosure are useful, for example, in the manufacture of nonwoven filtration media, particularly nonwoven electret filtration media.
[0066] In one embodiment, the fibers of the present disclosure may be included in filtration articles such as air filter elements of respirators, such as filtering masks, or filtration articles such as home and commercial air conditioners, air purifiers, vacuum cleaners, medical air line filters, air conditioning systems for vehicles and general appliances such as computers, computer disk drives and electronic devices. In some embodiments, the filtration article is combined with a respirator assembly to form an artificial respiratory device designed for use by a person. In respirator applications, the filtration article may be in the form of a molded, pleated or folded half-face respirator, a replaceable cartridge or canister, or a pre-filter. As used herein, the term "respiratory" refers to a system or device worn over a person's airway to prevent contaminants from entering the wearer's airway and / or to protect other people or objects from exposure to pathogens or other contaminants expelled by the wearer during breathing, including, but not limited to, a filtering face mask.
[0067] 3 and 4 are an example of a respirator. The respirator 40 includes a mask body 42 that may be curved, hemispherical, or may have other shapes as desired (see, for example, U.S. Pat. Nos. 5,307,796 (Kronzer et al.) and 4,827,924 (Japuntich)). In the mask 40, an electret nonwoven fibrous web (i.e., filtration material) 200 according to the present disclosure is sandwiched between a cover web 43 and an inner molding layer 45. The molding layer 45 provides structure to the mask body 42 and provides support for the filtration material 200.
[0068] The shaped layer 45 can be disposed on either side of the filter medium 200 and can be made, for example, from a nonwoven web of thermally bondable fibers molded into a cup-shaped configuration. The shaped layer can be molded according to known procedures (see, for example, U.S. Pat. No. 5,307,796 (Kronzer et al.), the disclosure of which is incorporated herein by reference). The shaped layer is typically made from bicomponent fibers having a core of a high melting point material, such as polyethylene terephthalate, surrounded by a sheath of a lower melting point material, such that when heated in a mold, the shaped layer conforms to the shape of the mold and retains this shape when cooled to room temperature. When pressed together with another layer, such as a filter layer, the low melting point sheath material can also serve to bond the layers together.
[0069] To hold the mask 40 snugly against the wearer's face, the mask body 42 may have straps 52, ties, mask harnesses, or the like attached thereto. Flexible, soft bands 54 made of metal, such as aluminum, may be provided on the mask body 42 so that they may be shaped to hold the mask 40 in a desired fitting relationship over the wearer's nose (see, e.g., U.S. Pat. No. 5,558,089 to Castiglione et al.). Respirators according to the present disclosure may also include additional layers, valves (see, e.g., U.S. Pat. No. 5,509,436 to Japuntich et al.), shaped masks, or the like. Examples of respirators that can incorporate electret filtration media according to the present disclosure include those described in U.S. Pat. Nos. 4,536,440 (Berg), 4,827,924 (Japuntich), 5,325,892 (Japuntich et al.), 4,807,619 (Dyrud et al.), 4,886,058 (Brostrom et al.), and U.S. Reissue Pat. No. 35,062 (Brostrom et al.).
[0070] A variety of filtration test protocols have been developed to evaluate filtration performance. These tests involve measuring the aerosol penetration of the filter web (usually expressed as the percentage of aerosol that penetrates the filter web (%Pen)) using a standard challenge aerosol such as dioctyl phthalate (DOP), and measuring the pressure drop (ΔP) across the filter web. From these two measurements, a quantity called the Quality Factor (QF) can be calculated by the following formula: QF = -ln(%Pen / 100) / ΔP (wherein ln represents the natural logarithm). A higher QF value indicates better filtration performance, and a decrease in QF value correlates effectively with a decrease in filtration performance. Details on the measurement of these values are provided in the Examples section. Typically, the filtration media of the present disclosure have a face velocity of 0.3 (mmH2O) at a face velocity of 13.8 centimeters per second (cm / s) or 6.9 cm / s. -1 The measured QF value is equal to or greater than 1.
[0071] The initial quality factor (Q0) is typically at least 0.2, preferably at least 0.3, 0.4, or even 0.5, for a face velocity of 13.8 cm / s or 6.9 cm / s, when tested according to the filtration performance test method as described in the following examples. More preferably, the initial quality factor is at least 0.6 or 0.7. In some embodiments, the initial quality factor is at least 0.8, at least 0.90, at least 1.0, or even greater than 1.0. To test the performance of the filter web, the filter web is exposed to X-rays at room temperature (e.g., 23°C) for a certain time, and the quality factor is measured again. In one embodiment, the quality factor after 40 minutes of X-ray exposure is typically at least 50% less than the initial quality factor.
[0072] For the web to have sufficient charge to be used as a filter, the percent transmittance is typically at least 50%. As the percent transmittance increases, the filtration performance of the web also increases. In some embodiments, the percent transmittance is at least 55%, 60%, or 70%. In preferred embodiments, the percent transmittance is at least 75% or 80%. In some embodiments, a single web exhibits a percent transmittance of at least 85%, at least, or at least 95%. EXAMPLES
[0073] Unless otherwise noted, all parts, percentages, ratios, etc. in the examples and the rest of the specification are by weight, and all reagents used in the examples were obtained or available from general chemical suppliers, such as Sigma-Aldrich Company (Saint Louis, Missouri), or can be synthesized by conventional methods. [Table 1-1] [Table 1-2]
[0074] Test Method
[0075] Thermal Gravimetric Analysis (TGA)
[0076] The thermal stability of selected phosphazenes was measured by thermogravimetric analysis (TGA) (Model Q500, TA Instruments, New Castle, Del.). Approximately 5 milligrams (mg) of dried sample were heated under nitrogen from a starting temperature of about 35° C. to 450° C. at a rate of 10° C. / min. The samples were weighed and the temperatures at which 5% and 10% weight loss occurred are reported in Table 3.
[0077] Filtration performance test method
[0078] Samples were tested for % aerosol penetration (%Pen) and pressure drop (ΔP), and the quality factor (QF) was calculated from these two values. An automated filter tester AFT Model 8130 (available from TSI, Inc. St. Paul, MN) was used to evaluate the filtration performance (%Pen and QF) of the nonwoven microfiber webs using dioctyl phthalate (DOP) as the challenge aerosol and a pressure transducer measuring the pressure drop across the filter (ΔP (mmH2O)). DOP aerosols were nominally 50-200 mg / m 3 Upstream concentration of 100 mg / m 3 The aerosol was monodisperse with a target value of 0.33 micrometer mass median diameter (MMD). The aerosol was passed through the media samples at a calibrated flow rate of 85 or 42.5 lpm (liters per minute) (face velocity of 13.8 cm / s or 6.9 cm / s as described in the following examples). In these tests, the aerosol ionizer was turned off. The total test time was 23 seconds (rise time 15 seconds, sample time 4 seconds, and purge time 4 seconds). A calibrated photometer was used to measure the concentration of DOP aerosol by light scattering both upstream and downstream of the media. DOP %Pen is defined as follows: %Pen=100×(DOP concentration downstream / DOP concentration upstream). For each material, six separate measurements were made at different points on the web, and the results were averaged to determine the QF value.
[0079] Preparation of fibrous and nonwoven samples
[0080] Step A - Fiber and Web Formation:
[0081] For each sample, a filtration medium was formed by first dry blending the substituted cyclotriphosphazene compound shown in Tables 4-5 with the indicated polypropylene resin (PP-1 or PP-2) and forming it into a meltblown fibrous web. The extrusion temperature was 250°C and the web properties were as follows: 65 g / m 2 basis weight, 5.5% solidity, and an effective fiber diameter of 8 microns.
[0082] Step B - Preparation of electrets:
[0083] Each of the meltblown webs was charged by one of two electret charging methods: corona charging or hydrocharging, which are designated charging methods C and H, respectively.
[0084] Charging method C - Corona charging:
[0085] Corona charging was achieved by passing the web on a grounded surface under a corona brush source at a speed of about 3 centimeters per second with a corona current of about 0.01 milliamps per centimeter of discharge source length. The corona source was located about 3.5 centimeters above the grounded surface on which the web rested. The corona source was driven by a positive DC voltage.
[0086] Charging method H-Hydrocharging:
[0087] A fine spray of high purity water having a conductivity of less than 5 microSiemens / cm was generated continuously from a nozzle operating at a pressure of 896 kilopascals (130 psig) and a flow rate of approximately 1.4 liters / minute. Selected webs prepared in step A were conveyed by a porous belt through the water spray at a velocity of approximately 10 centimeters / second while a vacuum was drawn from below through the web. Each web was passed through the hydrocharger twice (once on each side in turn) and then allowed to dry thoroughly overnight before filter testing.
[0088] Synthesis of selected cyclotriphosphazene compounds.
[0089] Scheme A. General scheme for the synthesis of nitrogen and oxygen derivatives. [ka]
[0090] Preparation of compound 4: Synthesis of hexa-4-ethylanilinecyclotriphosphazene (6).
[0091] To a stirred solution of hexachlorocyclotriphosphazene (20.0 grams (g), 57.5 mmol) in dry toluene (400 milliliters (mL)) and trimethylamine (200 mL, 1430 mmol) was added 4-ethylaniline (85 mL, 681 mmol) at room temperature. The formation of a white precipitate indicated the start of the reaction. The solution was heated to reflux overnight. An aliquot was then removed for analysis by liquid chromatography / mass spectrometry (LC / MS), which indicated complete conversion to the hexa-substituted product. The mixture was cooled to room temperature, filtered, and the precipitate was rinsed with ethyl acetate. The solvent was removed under reduced pressure by rotary evaporation. The remaining viscous oil was then distilled to remove excess triethylamine and aniline. The remaining dark solid was triturated with methanol, filtered, rinsed with methanol, and dried in a vacuum oven to give a white solid (28.4 g, 57% yield).
[0092] Preparation of compound 5: Synthesis of hexaanisidylcyclotriphosphazene (8).
[0093] To a stirred solution of hexachlorocyclotriphosphazene (10.0 g, 28.7 mmol) in dry toluene (200 mL) and trimethylamine (100 mL, 717 mmol) was added para-anisidine (42.5 mL, 345 mmol) at room temperature. The formation of a white precipitate indicated the start of the reaction. The solution was heated to reflux overnight. An aliquot was then removed for analysis by LCMS, which indicated complete conversion to the hexa-substituted product. The mixture was cooled to room temperature, filtered, and the precipitate was rinsed with ethyl acetate. The solvent was removed under reduced pressure by rotary evaporation. The remaining viscous oil was then distilled to remove excess triethylamine and anisidine. The remaining dark solid was triturated with methanol, filtered, rinsed with methanol, and dried in a vacuum oven to give a white solid (10 g, 40% yield).
[0094] Preparation of compound 6: Synthesis of hexa-4-dimethylaminophenoxycyclotriphosphazene (9).
[0095] Dimethylaminophenol was synthesized according to the procedure disclosed by Seim, KL et al. in J. Am. Chem. Soc. 2011, 133, pages 16970-16976, except using sodium cyanoborohydride instead of sodium borohydride. To a flame-dried 500 mL two-neck flask, NaH (12 g, 300 mmol) was added. Under a nitrogen atmosphere, dioxane (100 mL) was added. The solution was cooled to 0° C. and 4-dimethylaminophenol (31 g, 226 mmol) was added slowly in small portions as a solution in dioxane (50 mL). The solution turned brown and was stirred for 20 min. Hexachlorocyclotriphosphazene (10 g, 28.7 mmol) was added dropwise via an addition funnel as a solution in dioxane (50 mL). After the addition was complete, the ice bath was removed and replaced with an oil bath, a condenser was placed on the flask, and the mixture was refluxed (110° C.) overnight. An aliquot was removed for analysis by LCMS, which showed nearly complete conversion to the hexa-substituted product. Saturated ammonium chloride solution was added slowly to quench any remaining NaH. The solution was dark red / brown. The mixture was extracted with EtOAc, and the combined organic layers were washed with brine, dried (MgSO4), and concentrated to give a white solid in a pink slurry. The slurry was triturated with MeOH for 30 min, then filtered through a Buchner funnel, washed with cold MeOH, and dried using a vacuum oven to give a white solid (14 g, 51% yield).
[0096] The TGA results showing the temperatures at which 5% and 10% weight loss occurs for various compounds are shown in Table 3 below. [Table 2]
[0097] Select the compound that is blended with polypropylene, meltblown into web, and charged after preparing the above-mentioned fiber and nonwoven sample. Test the QF value of the nonwoven web using the filtration performance test method. The results are shown in Table 4 for the sample tested at a face velocity of 13.8 cm / s, and the sample in Table 5 was tested at a face velocity of 6.9 cm / s. [Table 3] [Table 4]
[0098] Foreseeable modifications and variations of the present invention will become apparent to those skilled in the art without departing from the scope and spirit of the present invention. The present invention is not limited to the embodiments described in this application for illustrative purposes. In the event of any discrepancy or inconsistency between the description of this specification and the disclosure in any document mentioned in this specification or incorporated by reference, the description of this specification shall prevail.
Claims
1. (a) a thermoplastic resin; (b) a charge enhancing additive comprising a cyclotriphosphazene core substituted with at least three amino-carbocyclic groups; A composition comprising an electrostatically charged fiber comprising:
2. The composition of claim 1, wherein the amino-carbocyclic group comprises an amino-cycloalkyl group, optionally the amino-cycloalkyl group comprises a cycloalkyl group containing from 5 to 8 carbon atoms.
3. The composition of claim 1 , wherein the amino-carbocyclic group comprises an amino-aryl group.
4. The composition of claim 3, wherein the amino-aryl group comprises at least one aromatic ring optionally substituted with at least one of an ether, an amine, and an alkyl group.
5. The composition of claim 3, wherein the amino-aryl group comprises at least one of a phenylamino group, an alkylphenylamino group, an alkoxyphenylamino group, a phosphoroaminoindane, or an alkylaminophenoxy group.
6. The charge enhancing additive has Formula I: 【Chemistry 1】 2. The composition of claim 1, wherein L is selected from NH or N(R), R is an alkyl group, optionally containing at least one catenated atom selected from N or O, and X comprises a cyclic carbocyclic group.
7. The charge enhancing additive has Formula II: 【Chemistry 2】 2. The composition of claim 1, wherein X comprises a cyclic carbocyclic group that contains an amino group.
8. 10. The composition of claim 1, wherein the charge enhancing additive comprises at least one of the following: 【Chemistry 3】 【Chemistry 4】
9. 10. The composition of claim 1, wherein the charge enhancing additive does not decompose below 220°C.
10. The composition of claim 1 , wherein said electrostatically charged fiber comprises at least 0.01% and up to 5.0% by weight of said electrostatic enhancing additive.
11. 10. The composition of claim 1, wherein said electrostatically charged fiber is substantially free of a second electrostatic enhancing additive, and optionally, said second electrostatic enhancing additive is a hindered amine.
12. A nonwoven fibrous web comprising fibers comprising the electrostatically charged fibers of claim 1.
13. A medical article comprising the nonwoven fibrous web of claim 12.
14. 13. A filtration article comprising the nonwoven fibrous web of claim 12, optionally wherein the filtration article is a respirator.
15. A method of making an electret, comprising the steps of: Providing a composition according to claim 1; charging the composition via corona treatment, hydrocharging, tribocharging, or a combination thereof to form the electret.
16. Use of a cyclotriphosphazene core substituted with at least three amino-carbocyclic groups as a charge enhancing additive.