Silicone Urethane (Meth)Acrylates and Their Use in 3D Printing Resins and Coating Compositions
Patent Information
- Application Number
- JP2023542979
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-01-15
- Filing Date
- 2022-01-13
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2042-01-13
AI Technical Summary
Silicone urethane (meth)acrylates in the prior art exhibit moderate photocuring rates, are highly viscous or solid at room temperature, making processing difficult, and often require higher temperatures or solvents, leading to increased energy consumption and adverse effects on product properties.
Development of silicone urethane (meth)acrylates with at least 3 (meth)acrylate groups and no more than (meth)acrylate groups, prepared by reacting hydroxy-functional silicone (meth)acrylates with isocyanate-functional urethane (meth)acrylates, resulting in compositions with improved processability and mechanical properties.
The new compositions demonstrate low viscosity, fast photocuring reactions, and excellent mechanical properties, including high elongation at break, allowing for the production of flexible, elastomeric materials without the need for solvents or elevated temperatures.
Smart Images

Figure 2022152775000001 
Figure 2022152775000002 
Figure 2022152775000003
Abstract
Description
[Technical field]
[0001] The present invention relates to silicone urethane (meth)acrylates, in particular having at least three (meth)acrylate groups and not more urethane groups than (meth)acrylate groups, to a process for preparing said silicone urethane (meth)acrylates, to compositions comprising said silicone urethane (meth)acrylates, and to their use in the production of release coatings, protective films, protective coatings, and in the manufacture of 3D printed objects by stereolithography.
[0002] The use of silicone urethane (meth)acrylates as components of 3D printing resins and coating compositions is known in the art.
[0003] Korean Patent Publication No. 20170128955 discloses silicone urethane (meth)acrylate as a photocurable polymer for 3D printing. In Example 1, silicone urethane acrylate is prepared by reacting 1 mole of hydroxy-terminated polydimethylsiloxane with 2 moles of hexamethylene diisocyanate (HDI) followed by 2 moles of hydroxyethyl acrylate (HEA). In Example 2, silicone urethane acrylate is prepared in the same manner except that isophorone diisocyanate (IPDI) is used instead of HDI. These silicone urethane acrylates in Examples 1 and 2 have 2 acrylate groups and 4 urethane groups. In Example 3, silicone urethane methacrylate is prepared by reacting 1 mole of hydroxy-terminated polydimethylsiloxane with 2 moles of 2-isocyanatoethyl methacrylate, which is a dangerous and toxic compound. The polymer in Example 3 has 2 methacrylate groups and 2 urethane groups. These photocurable polymers are further described as being flexible, having a high photocuring speed, and being easy to process.
[0004] Chinese Patent Publication No. 106519182 discloses a silicone urethane acrylate for use in the field of release coatings. The silicone urethane acrylate is: (1) reacting an organosilicon glycol with a diisocyanate in a molar ratio of hydroxyl groups to isocyanate groups of 1:2; (2) reacting hydroxyethyl acrylate or hydroxyethyl methacrylate with the prepolymer obtained in step (1) in a molar ratio of hydroxyl groups to isocyanate groups of 1:1; It is prepared by a method comprising:
[0005] The organosilicon glycol is a chain-type silicon glycol having an organic radical containing two hydroxyl groups at one of its chain ends.The diisocyanate is preferably selected from toluene diisocyanate, hexamethylene diisocyanate, or isophorone diisocyanate.The obtained silicone urethane acrylate has two (meth)acrylate groups and four urethane groups.
[0006] CN109577077 relates to a method for preparing a self-adhesive release paper by electron beam curing. The release paper comprises a base paper layer and a release coating, the latter of which is obtained by electron beam curing of a release coating composition containing 50-100 parts of silicone modified urethane acrylate, 0-50 parts of silicone modified polyacrylate and 10-20 parts of reactive diluent.
[0007] However, silicone urethane (meth)acrylates known in the art usually only show moderate photocuring speeds, or have high viscosities, or even are solid at room temperature, which makes them difficult to process. To improve their processability, silicone urethane (meth)acrylates are processed at higher temperatures or higher amounts of solvents or reactive diluents are added, which may result in other drawbacks such as increased energy consumption, additional process steps to remove the solvent, and / or possible adverse effects on the desired properties of the cured product. To facilitate processing, it is also preferable to have high curing speeds and increased cure depths. In addition, it is preferable for the cured product to be flexible and have good mechanical properties, such as high elongation at break. It is also preferable for the cured product to be an elastomeric material, i.e., the product should return to its original shape after deformation, such as elongation. The surface of the cured product should be smooth and have good release properties. It is also necessary to avoid highly toxic or hazardous compounds in the synthesis of silicone urethane (meth)acrylates.
[0008] Therefore, there remains a need to provide silicone urethane (meth)acrylates that have advantages over the prior art. Accordingly, the problem addressed by the present invention was to overcome at least one of the shortcomings of the prior art.
[0009] Surprisingly, it has been found that at least one of the disadvantages of the prior art is overcome by the subject matter of the independent claims.
[0010] The object of the present invention is therefore achieved by the subject matter of the independent claims. Preferred embodiments of the invention are specified in the dependent claims, the examples and the description.
[0011] According to a first aspect of the present invention, - at least 3 (meth)acrylate groups, - no more urethane groups than (meth)acrylate groups, preferably just as many as (meth)acrylate groups; A silicone urethane (meth)acrylate having the formula:
[0012] According to a second aspect of the present invention, a compound of formula (A): [ka] containing the group During the ceremony, Z 1 is, in each case, independently selected from the group consisting of CH3 or H, preferably H; Z 2 is a divalent organic radical, preferably an alkylene radical, preferably OCN-Z 2 is an alkylene radical derived from isophorone diisocyanate as the diisocyanate of -CNO, Z 3 is a (q+1)-valent organic radical, where q is an organic radical which is an integer from 1 to 3, preferably an alkylene radical, preferably -(C2H4)-; Z 4 is, in each occurrence, independently selected from the group consisting of -CH3 and -H, preferably H; wherein each dotted line represents a covalent bond. A silicone urethane (meth)acrylate, preferably also according to the first aspect of the present invention, is provided.
[0013] According to a third aspect of the present invention, there is provided a method for preparing the silicone urethane (meth)acrylate, wherein the silicone urethane (meth)acrylate is formed by reacting at least one hydroxy-functional silicone (meth)acrylate with at least one isocyanate-functional urethane (meth)acrylate.
[0014] According to a fourth aspect of the present invention, a composition comprising the following ingredients: (a) at least one silicone urethane (meth)acrylate according to the present invention, (b) optionally, at least one organic (meth)acrylate that does not contain any silicon atoms; (c) optionally at least one silicone (meth)acrylate that does not have any urethane groups; (d) optionally, at least one curing catalyst; (e) optionally, at least one additive; (f) optionally, at least one solvent; A composition comprising or consisting of is provided.
[0015] According to a fifth aspect of the invention, there is provided a method for preparing said composition, comprising the steps of: (i) preparing a mixture of component (a) and component (f); (ii) preparing a mixture by adding at least one of components (b) to (e), preferably components (b) and / or (c), to the mixture of step (i); (iii) (essentially) removing component (f) from the mixture of step (ii); (iv) optionally preparing a mixture by adding at least one of components (b)-(e) to the mixture of step (iii), if said component was not added in step (ii); A method is provided that includes:
[0016] According to a fifth aspect of the invention there is provided a release coating, protective film or protective coating obtainable by curing the composition, or a 3D printed object obtainable by 3D printing the composition.
[0017] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly indicates otherwise.
[0018] As used herein, the terms "comprising" and "comprises" are synonymous with "including," "includes," "containing," or "contains," and are inclusive or open-ended and do not exclude additional, unrecited components, elements, or method steps.
[0019] When amounts, concentrations, dimensions, and other parameters are expressed in the form of ranges, preferred ranges, upper values, lower values, or preferred upper and lower values, it is to be understood that any range that can be obtained by combining any upper or preferred value with any lower limit or preferred value is also specifically disclosed, whether or not the resulting range is expressly stated in the context.
[0020] Hereinafter, when numerical ranges are reported in the format "X to Y," where X and Y represent the limits of the numerical range, this is equivalent to saying "from at least X to Y, inclusive," unless otherwise stated. Thus, the statement of a range includes the range limits X and Y, unless otherwise stated.
[0021] The words "preferred" and "preferably" are frequently used herein to refer to embodiments of the present disclosure that may provide certain benefits, under certain circumstances. However, the recitation of one or more preferred embodiments does not imply that other embodiments are not useful, and is not intended to exclude these other embodiments from the scope of the present disclosure.
[0022] Where measurements, parameters or material properties determined by measurement are reported below, these are measurements, parameters or material properties measured at 25° C. and preferably at a pressure of 101325 Pa (standard pressure), unless otherwise stated.
[0023] As used herein, room temperature (RT) is 23°C ± 2°C.
[0024] The term "(meth)acrylic" refers to "methacrylic" and / or "acrylic". Thus, the term "(meth)acrylate" refers to "methacrylate" and / or "acrylate". As used herein, "acrylate" refers to "acrylic acid ester" and "methacrylate" refers to "methacrylic acid ester".
[0025] In the context of this invention, silicone urethane (meth)acrylates are understood to mean organosiloxanes which contain urethane groups and have methacrylic acid ester groups and / or acrylic acid ester groups, also referred to below as (meth)acrylic acid ester groups. Organosiloxanes are also referred to below simply as siloxanes.
[0026] Organosiloxanes are compounds consisting of an organic radical bonded to a silicon atom and a compound of the formula: [ka] Also has the structural unit [ka] is understood to mean a compound in which M=[RSiO 1 / 2 ], D = [RSiO 2 / 2 ], T = [RSiO 3 / 2 ] and optionally having the formula Q=[SiO 4 / 2
[0023] , where R is a monovalent organic radical. Here, the radicals R can be selected independently of each other and are identical or different when compared in pairs. The radicals R can also be partially replaced by non-organic monovalent radicals, such as, for example, hydroxyl groups or chlorine. References cited in connection with the M, D, T, Q nomenclature used herein to describe the structural units of organosiloxanes are: W. Noll, Chemie und Technologie der Silicone [Chemistry and Technology of the Silicones], Verlag Chemie GmbH, Weinheim (1960), page 2 ff.
[0027] The various repeating units in the following formulas (C), (F), (Q) and (S) may be statistically distributed. The statistical distribution may have a block-wise structure with any number of blocks and any sequence, or may be a random distribution, which may have an alternating structure or form a gradient along the chain, if any, and in particular, they may also form any mixed form thereof, in which groups of different distributions may optionally follow each other. Specific embodiments may be defined below in that features such as index, or structural components, or ranges, or statistical distributions are subject to limitations according to the embodiments. All other features not affected by the limitations remain unchanged.
[0028] Where a molecule / molecular fragment has one or more stereocenters (stereogenic centers) or can be separated into isomers based on symmetry or other effects, e.g. restricted rotation, all possible isomers are encompassed by the present invention.
[0029] Molecular weights given in this document are number average molecular weights (M n). All molecular weight data refers to values obtained by gel permeation chromatography (GPC), as described in the examples.
[0030] Where documents are cited within the context of this specification, it is intended that their entire contents are part of the disclosure of the present invention.
[0031] In a first aspect of the present invention, - at least 3 (meth)acrylate groups, - no more urethane groups than (meth)acrylate groups, preferably just as many as (meth)acrylate groups; A silicone urethane (meth)acrylate having the formula:
[0032] It is preferred that the silicone urethane (meth)acrylate has m (meth)acrylate groups and n urethane groups; m is an integer of at least 3, preferably 3 to 5, more preferably 4; n is an integer of at least 2, preferably 2 to 4, more preferably 4; However, m≧n, and preferably m=n.
[0033] Examples of possible combinations (m;n) of m (meth)acrylate groups and n urethane groups include, but are not limited to, (3;1), (3;2), (3;3), (4;1), (4;2), (4;3), (4;4), (5;1), (5;2), (5;3), (5;4), (5;5); (6;1), (6;2), (6;3), (6;4), (6;5), or (6;6); preferably (3;2), (3;3), (4;2), (4;3), (4;4), (5;2), (5;3), (5;4), or (5;5), particularly preferably (4;4).
[0034] The silicone urethane (meth)acrylate has the formula (B): X(-Y) p Formula (B) is represented by During the ceremony, X is a p-valent silicone radical; Y is bonded to the silicon atom of the silicone radical, in each case, independently selected from the group consisting of a monovalent organic radical having at least one urethane group and at least one (meth)acrylate group; Preferably, in each case, independently selected from the group consisting of monovalent organic radicals having two (meth)acrylate groups and one or two urethane groups, More preferably, in each case, independently selected from the group consisting of a monovalent organic radical having two (meth)acrylate groups and two urethane groups, p is an integer of at least 1, preferably 2 to 4, and more preferably 2. It is preferred.
[0035] The silicone radicals can be linear, branched, cyclic, or a combination thereof. It is preferred that the silicone radicals are linear. It is particularly preferred that the silicone radicals are divalent polydimethylsiloxane radicals.
[0036] The silicone urethane (meth)acrylate has the formula (C): [R a Y b SiO (4-a-b) / 2 ] Formula (C) Including units represented by During the ceremony, a is an integer of 0 to 2, preferably 1 or 2; b is an integer from 1 to 3, preferably 1; However, a+b is 1 to 3, R, in each instance, is independently selected from the group consisting of monovalent organic radicals that are free of any urethane groups; Preferably, in each case, independently selected from the group consisting of monovalent hydrocarbon radicals having 1 to 30 carbon atoms, More preferably, it is a methyl radical. Y is as defined above It is preferred.
[0037] Preferably, the silicone urethane (meth)acrylate has exactly two units represented by formula (C) as defined above, and it is particularly preferred that each of these units has two radicals R and one radical Y, i.e. a=2 and b=1.
[0038] In a further aspect of the present invention, it is preferably also a silicone urethane (meth)acrylate according to the first aspect of the present invention, more preferably comprising, contained in said radical Y, a compound of formula (A): [ka] containing the group During the ceremony, Z 1 is, in each case, independently selected from the group consisting of CH3 or H, preferably H; Z 2 is a divalent organic radical, preferably an alkylene radical, preferably OCN-Z 2 is an alkylene radical derived from isophorone diisocyanate as the diisocyanate of -CNO, Z 3 is a (q+1)-valent organic radical, where q is an organic radical which is an integer from 1 to 3, preferably an alkylene radical, preferably -(C2H4)-; Z 4 is, in each occurrence, independently selected from the group consisting of -CH3 and -H, preferably H; wherein each dotted line represents a covalent bond. Silicone urethane (meth)acrylates are provided.
[0039] Examples of covalent bonds represented by dotted lines are bonds to a hydrogen radical or to an organic radical, such as an alkyl or alkylene radical, which may be linear, branched or cyclic and may optionally be interrupted by an oxygen atom. Preferably, at least one of said dotted lines represents a covalent bond to an organic radical which itself has a covalent bond to a silicon atom, said organic radical being preferably a divalent hydrocarbon radical which may be interrupted by an oxygen atom.
[0040] Z 2 In each case, it is preferred that Z is independently selected from the group consisting of divalent, saturated or unsaturated, linear, branched or cyclic hydrocarbon radicals having 1 to 30 carbon atoms. 2 is the formula OCN-Z 2 The residue of a diisocyanate may be of the formula (D) -CNO. The term "residue of a diisocyanate" is defined herein as the molecular structure of a diisocyanate from which all isocyanate groups have been removed. Examples of suitable diisocyanates are shown below. 2 However, the formula OCN-Z 2 It is particularly preferred that the divalent radical is derived from a diisocyanate of -CNO, said diisocyanate being IPDI.
[0041] Z 3 In each case, it is preferred that Z is independently selected from the group consisting of (q+1)-valent, saturated or unsaturated, linear, branched or cyclic hydrocarbon radicals having 2 to 30 carbon atoms. 3 is expressed by the formula (E): [ka] may be the residue of a hydroxy-functional (meth)acrylate.
[0042] Examples of suitable hydroxy-functional (meth)acrylates are given below: Hydroxyethyl acrylate is particularly preferred.
[0043] The silicone urethane (meth)acrylate has the formula (F): M m1 M UA m2 M A m3 D d1 D UA d2 D A d3 T t Q q Formula (F) is represented by During the ceremony, M = [RSiO 1 / 2 ], M UA =[R2(R UA )SiO 1 / 2 ], M A =[R2(R A )SiO 1 / 2 ], D = [R2SiO 2 / 2 ], D UA =[R(R UA )SiO 2 / 2 ], D A =[R(R A )SiO 2 / 2 ], T = [RSiO 3 / 2 ], Q = [SiO 4 / 2 ], m1 is an integer of 0 to 32, preferably 0 to 22, more preferably 0; m2 is an integer of 0 to 32, preferably 1 to 10, more preferably 2; m3 is an integer of 0 to 32, preferably 0 to 22, more preferably 0; d1 is an integer of 1 to 1000, preferably an integer of 5 to 500, more preferably an integer of 10 to 400, d2 is an integer of 0 to 10, preferably 0 to 5, and more preferably 0; d3 is an integer of 0 to 10, preferably 0 to 5, and more preferably 0; t is an integer of 0 to 10, preferably 0 to 5, more preferably 1 to 5; q is an integer of 0 to 10, preferably 0 to 5, more preferably 1 to 5; however, m1+m2+m3 is at least 2, preferably 2 to 20, more preferably 2 to 10; m2+d2 is at least 1, preferably 2 to 10, more preferably 2 to 6; During the ceremony, R is, in each case, independently selected from the group consisting of monovalent organic radicals that do not contain any urethane or (meth)acrylate groups; Preferably, in each case, independently selected from the group consisting of monovalent hydrocarbon radicals having 1 to 30 carbon atoms, More preferably, it is a methyl radical. R UA are independently selected in each case from the group consisting of monovalent organic radicals having at least one (meth)acrylate group and at least one urethane group; Preferably, in each case, independently selected from the group consisting of monovalent organic radicals having two (meth)acrylate groups and one or two urethane groups, More preferably, in each case, the compound has the formula (G): [ka] and independently selected from the group consisting of monovalent organic radicals represented by x1 is an integer from 1 to 3, preferably 3; R 1 In each case, R is a hydrogen radical, a monovalent hydrocarbon radical having 1 to 6 carbon atoms, 2 , and R 3 are independently selected from the group consisting of: Preferably, in each case, independently selected from the group consisting of a hydrogen radical and a monovalent hydrocarbon radical having 1 to 6 carbon atoms, More preferably, it is a hydrogen radical. R 2 In both cases, the hydrogen radical, R 3 and a monovalent organic radical having at least one (meth)acrylate group; Preferably, in each case, R 3 and a monovalent organic radical having at least one (meth)acrylate group; More preferably, in each case, the compound has the formula (H): [ka] are independently selected from the monovalent radicals x2=(1-x3), R 3 are independently selected in each case from the group consisting of monovalent organic radicals having at least one urethane group and at least one (meth)acrylate group; Preferably, in each case, independently selected from the group consisting of monovalent organic radicals having exactly two urethane groups and exactly one (meth)acrylate group, More preferably, in each case, the compound has the formula (I): [ka] and independently selected from the group consisting of monovalent organic radicals of x3 is an integer selected from 0 or 1, preferably 0; R 4 is in each case independently selected from a hydrogen radical or a methyl radical, preferably a hydrogen radical; R 5 are independently selected from the group of divalent, saturated or unsaturated, linear, branched or cyclic hydrocarbon radicals having in each case 1 to 30 carbon atoms; Preferably, the compound of formula (J): [ka] is a divalent radical of R A are independently selected in each case from the group consisting of monovalent organic radicals having at least one (meth)acrylate group and no urethane groups; Preferably, in each case, independently selected from the group consisting of monovalent radicals represented by formula (K) or (L): More preferably, in each case, independently selected from the group consisting of monovalent radicals represented by formula (K): [ka] In the formula, x1 and R 4 is as defined above It is preferred.
[0044] Radical R UA or Y each has the formula (M), (N), (O), and (P): [ka] It is even more preferred that the .alpha.-alkyl group is represented by:
[0045] Preferably, the following applies to the silicone urethane (meth)acrylates according to formula (F): m1=d2=t=q=0, m2=2, and d1 is in the range of 1 to 1,000, preferably 5 to 500, more preferably 10 to 400, and further more preferably 20 to 100.
[0046] It is preferred that the (meth)acrylate group of the silicone urethane (meth)acrylate is an acrylate group.
[0047] Preferably, the silicone urethane (meth)acrylates of the present invention do not contain groups containing a moiety of the formula -(C=O)-NH- other than urethane groups.
[0048] It is preferred that the silicone urethane (meth)acrylate has a viscosity of less than 200 Pa·s, preferably from 0.5 to 150 Pa·s, more preferably from 10 to 100 Pa·s at 25° C. The glass transition temperature is preferably determined as described in the examples.
[0049] The silicone urethane (meth)acrylates preferably have a weight average molecular weight Mw of 1000 to 20000 g / mol, preferably 2000 to 15000 g / mol, more preferably 3000 to 10000 g / mol. The weight average molecular weight is preferably determined as described in the examples.
[0050] The silicone urethane (meth)acrylates preferably have a number average molecular weight Mn of 1000 to 10000 g / mol, preferably 1500 to 7500 g / mol, more preferably 2000 to 5000 g / mol. The number average molecular weight is preferably determined as described in the examples.
[0051] The cured silicone urethane (meth)acrylate has a glass transition temperature (T g The glass transition temperature is preferably determined by differential scanning calorimetry (DSC) according to DSC method DIN 53765 at a heating rate of 10 K / min.
[0052] Silicone urethane (meth)acrylate is (1) reacting at least one hydroxy-functional silicone (meth)acrylate with at least one diisocyanate while forming at least one urethane group to obtain an isocyanate-functional prepolymer; (2) reacting at least one hydroxy-functional (meth)acrylate with the isocyanate-functional prepolymer obtained in step (1) while forming at least one urethane bond; It can be prepared by a method comprising:
[0053] Those skilled in the art know how to carry out the reaction and select suitable reaction conditions to achieve high yields, for example as described in Korean Patent Publication No. 20170128955 and Chinese Patent Publication No. 106519182. For example, it is preferred that the molar ratio of hydroxyl groups to isocyanate groups is about 1:2 in step (1) and about 1:1 in step (2).
[0054] Surprisingly, an alternative method for producing silicone urethane (meth)acrylate is much more preferable.According to this method, hydroxyl-functional silicone (meth)acrylate is reacted with isocyanate-functional urethane (meth)acrylate.By applying this method, viscosity can be further reduced.
[0055] Thus, a further aspect of the present invention is a method for preparing a silicone urethane (meth)acrylate, said silicone urethane (meth)acrylate being formed by reaction of at least one hydroxy-functional silicone (meth)acrylate with at least one isocyanate-functional urethane (meth)acrylate.
[0056] The reaction of hydroxy-functional silicone (meth)acrylates with isocyanate-functional urethane (meth)acrylates involves the reaction of free NCO groups with hydroxyl groups and has already been described extensively (WO 2010 / 072439 and references cited therein). This reaction can take place with or without a solvent. It is generally carried out in a temperature range between 40° C. and 80° C. The reaction generally takes 4 to 8 hours. It can be advantageously catalyzed by common catalysts known in urethane chemistry, such as organometallic compounds and tertiary amines. Examples of suitable organometallic compounds are dibutyltin dilaurate (DBTL), dibutyltin dineodecanoate, zinc octoate, and bismuth neodecanoate. Examples of suitable tertiary amines are triethylamine or diazobicyclooctane. Suitable reaction assemblies include all conventional equipment, tanks, static mixers, extruders, etc., preferably assemblies with mixing or stirring functions. The NCO / OH ratio is typically 2:1 to 1:2, preferably 1.5:1 to 1:1.5, more preferably 1:1. The reaction can be carried out in the presence of a solvent, preferably without the presence of a solvent. A suitable solvent is, for example, acetone. To avoid polymerization of the (meth)acrylate groups, it can be advantageous to carry out the reaction in the presence of an antioxidant / polymerization inhibitor. The inhibitor can be added to the reaction mixture together with the isocyanate-functional urethane (meth)acrylate that can react with the hydroxyl groups of the hydroxy-functional silicone (meth)acrylate. If a solvent is used, it can preferably be removed after completion of the reaction, preferably under vacuum, or after preparation of the composition according to the invention.
[0057] The examples of hydroxy-functional silicone (meth)acrylates that can be used to prepare the silicone urethane (meth)acrylates of the present invention are also known to those skilled in the art.Preferably, said hydroxy-functional silicone (meth)acrylates are formed by the reaction of at least one epoxy-functional silicone with (meth)acrylic acid and / or at least one hydroxy-functional (meth)acrylate.Even more preferably, said hydroxy-functional silicone (meth)acrylates are formed by the reaction of at least one epoxy-functional silicone with methacrylic acid and / or acrylic acid, especially acrylic acid.This is described in U.S. Pat. No. 4,978,726 and the references cited therein.The examples of suitable hydroxy-functional (meth)acrylates that can be used are the same as those that can be used to synthesize isocyanate-functional urethane (meth)acrylates as follows:
[0058] Examples of isocyanate-functional urethane (meth)acrylates that can be used to prepare the silicone urethane (meth)acrylates of the present invention are also known from the prior art and are described, for example, in WO 2010 / 072439 and WO 2010 / 115644. Commercially available isocyanate-functional urethane (meth)acrylates that can be used are, for example, VESTANAT® EP DC-1241 (available from Evonik Industries AG, Germany). Isocyanate-functional urethane (meth)acrylates can be prepared by reacting diisocyanates with hydroxy-functional (meth)acrylates while forming urethane bonds, as described in WO 2010 / 072439.
[0059] Preferred diisocyanates are described, for example, by Houben-Weyl, Methoden der organischen Chemie, Volume 14 / 2, on pages 61 to 70, and by W.As described by the paper by Siefken, aliphatic, cycloaliphatic, and araliphatic (i.e., aryl-substituted aliphatic) diisocyanates, such as 1,2-ethylene diisocyanate, 1,4-tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate (HDI), 2,2,4-trimethyl-1,6-hexamethylene diisocyanate (TMDI), 2,4,4-trimethyl-1,6-hexamethylene diisocyanate (TMDI), 1,9-diisocyanato-5-methylnonane, 1,8-Diisocyanato-2,4-dimethyloctane, 1,12-dodecane diisocyanate, ω,ω'-Diisocyanatodipropyl ether, Cyclobutene 1,3-diisocyanate, Cyclohexane 1,3-diisocyanate, Cyclohexane 1,4-diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (Isophorone diisocyanate, IPDI), 1,4-Diisocyanatomethyl-2,3,5,6-tetramethylcyclohexane, Decahydro-8-methyl( 1,4-methano-naphthalene)-2,5-ylene dimethylene diisocyanate, decahydro-8-methyl(1,4-methano-naphthalene)-3,5-ylene dimethylene diisocyanate, hexahydro-4,7-methanoindan-1,5-ylene dimethylene diisocyanate, hexahydro-4,7-methanoindan-2,5-ylene dimethylene diisocyanate, hexahydro-4,7-methanoindan-1,6-ylene dimethylene diisocyanate, hexahydro-4,7-methanoindan-2,5-ylene diisocyanate Methylene diisocyanate, hexahydro-4,7-methanoindan-1,5-ylene diisocyanate, hexahydro-4,7-methanoindan-2,5-ylene diisocyanate, hexahydro-4,7-methanoindan-1,6-ylene diisocyanate, hexahydro-4,7-methanoindan-2,6-ylene diisocyanate, 2,4-hexahydrotolylene diisocyanate, 2,6-hexahydrotolylene diisocyanate, 4,4'-methylenedicyclohexyl diisocyanate (4,4'-H. 12 MDI), 2,2'-methylenedicyclohexyl diisocyanate (2,2'-H 12MDI), 2,4-methylenedicyclohexyl diisocyanate (2,4-H 12 MDI), or other mixtures, 4,4'-diisocyanato-3,3',5,5'-tetramethyldicyclohexylmethane, 4,4'-diisocyanato-2,2',3,3',5,5',6,6'-octamethyldicyclohexylmethane, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,4-diisocyanatomethyl-2,3,5,6-tetramethylbenzene, 2-methyl-1,5-diisocyanatopentane (MPDI), 2-ethyl-1,4-diisocyanatobutane, 1,10-diisocyanatodecane, 1,5-diisocyanatohexane, 1,3-diisocyanatomethylcyclohexane, 1,4-diisocyanatomethylcyclohexane, and any desired mixtures of these compounds. Further suitable isocyanates are described in the above-mentioned article in Justus Liebigs Annalen der Chemie on page 122 f. 2,5-bis(isocyanatomethyl)bicyclo[2.2.1]heptane (NBDI) and / or 2,6-bis(isocyanatomethyl)bicyclo[2.2.1]heptane (NBDI) are also preferred. Particularly preferred are industrially readily available aliphatic and cycloaliphatic diisocyanates, such as IPDI, HDI, and H 12 MDI and the like, as well as also their isomeric mixtures, in particular IPDI, are used. The diisocyanates are embodiments of the diisocyanates of formula (D) as given above.
[0060] Preferred hydroxy-functional (meth)acrylates are all compounds that have at least one methacrylate or acrylate functional group, but also exactly one hydroxyl group. The further constituents can be aliphatic, cycloaliphatic, aromatic, or heterocyclic alkyl groups. Oligomeric or polymeric compounds are also conceivable. For example, readily available products such as hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, and hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl methacrylate, glycerol diacrylate, pentaerythritol triacrylate, trimethylolpropane diacrylate, glycerol dimethacrylate, pentaerythritol trimethacrylate, and trimethylolpropane dimethacrylate, and also hydroxylethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, hydroxypentyl vinyl ether, and hydroxyhexyl vinyl ether are preferred. Hydroxyethyl acrylate is particularly preferred. It is also possible to use mixtures of two or more of these hydroxy-functional (meth)acrylates. The hydroxy-functional (meth)acrylate is an embodiment of the hydroxy-functional (meth)acrylate of formula (E) as shown above.
[0061] The silicone urethane (meth)acrylates according to the present invention are typically used as components in compositions for a variety of applications.
[0062] Thus, a further aspect of the present invention is a composition comprising: (a) at least one silicone urethane (meth)acrylate according to the invention and / or prepared by the method according to the invention, (b) optionally, at least one organic (meth)acrylate that does not contain any silicon atoms; (c) optionally at least one silicone (meth)acrylate that does not have any urethane groups; (d) optionally, at least one curing catalyst; (e) optionally, at least one additive A composition comprising or consisting essentially of:
[0063] said composition being based on the total weight of the sum of components (a)-(e) and / or based on the total weight of the composition, preferably based on the total weight of the composition; - 5 to 100, preferably 5 to 20, more preferably 10 to 20% by weight of at least component (a), - 0 to 60, preferably 0 to 30, more preferably 5 to 15% by weight of at least component (b), - 0 to 95, preferably 65 to 85, more preferably 70 to 80% by weight of at least component (c), - 0 to 5, preferably 0.1 to 3, more preferably 0.5 to 2.5% by weight of component (d), - 0 to 20, preferably 0 to 10, more preferably 0 to 5% by weight of component (e), - 0 to 10, preferably 0 to 5, more preferably 0 to 1 wt.-% of component (f), It is preferred that the composition comprises or consists essentially of:
[0064] The one or more silicone urethane (meth)acrylates according to the present invention are also referred to herein as component (a).
[0065] It is preferred that the amount of silicone urethane (meth)acrylate (component (a)) present in the composition of the present invention is from 5 to 100% by weight, preferably from 5 to 20% by weight, more preferably from 10 to 20% by weight, based on the total weight of the sum of components (a) to (e) and / or based on the total weight of the composition, preferably based on the total weight of the composition.
[0066] It is preferred that the composition according to the invention further comprises component (b). Component (b) can be used as a reactive diluent to reduce and adjust the viscosity of the composition. Alternatively, component (b) can be used as a crosslinking agent. Component (b) of the composition consists of one or more organic (meth)acrylates that do not have any silicon atoms. Thus, the organic (meth)acrylates are silicon-free. It is preferred that the organic (meth)acrylates consist only of the elements carbon, hydrogen, oxygen and nitrogen. It is also preferred that the organic (meth)acrylates have 2 to 6 (meth)acrylate groups. Such compounds are described in the European Coatings Tech Files by Patrick Gloeckner et al. in ''Radiation Curing: Coatings and Printing Inks'', 2008, Vincentz Network, Hanover, Germany.
[0067] Particularly preferred organic (meth)acrylates are disclosed in WO 2016 / 096595 and WO 2018 / 001687. Examples of organic (meth)acrylates may be selected from the group consisting of, but are not limited to, trimethylolpropane triacrylate (TMPTA), tripropylene glycol diacrylate (TPGDA), dipropylene glycol diacrylate (DPGDA), isobornyl acrylate (IBOA), lauryl acrylate, 1,6-hexanediol diacrylate (HDDA), tridecyl acrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, propoxylated glyceryl triacrylate, polyethylene glycol diacrylate, and ethoxylated and / or propoxylated derivatives thereof.
[0068] Suitable organic (meth)acrylates are Ebecryl® TMPTA (Allnex SA, Germany), Ebecryl® OTA480 (propoxylated glyceryl triacrylate, Allnex SA, Germany), Ebecryl® TPGDA (Allnex SA, Germany), Ebecryl® DPGDA (Allnex SA, Germany), Ebecryl® 892 (Allnex SA, Germany), Ebecryl® 11 (polyethylene glycol 600 diacrylate with Mw 700 g / mol, Allnex SA, Germany), Ebecryl® 45 (Allnex SA, Germany), PETIA (mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate, Allnex SA, Germany), Ebecryl® 150 (bisphenol A derivative diacrylate, Allnex SA, Germany), Germany), Ebecryl® 605 (a mixture of 80% bisphenol A diepoxy acrylate and 20% TPGDA, Allnex SA, Germany), Ebecryl® 40 (ethoxylated and propoxylated (total of 1.2 propylene oxide and 5 ethylene oxide units) pentaerythritol tetraacrylate, Allnex SA, Germany), Laromer® TMPTA (BASF, Germany), Miramer® M200 (HDDA, Rahn AG, Germany), Miramer® M220 (TPGDA, Rahn AG, Germany), Miramer® 3130 (ethoxylated trimethylolpropane triacrylate (total of 3 ethylene oxide units), Rahn AG, Germany), SR 415 (ethoxylated (total of 20 ethylene oxide units)) trimethylolpropane triacrylate, Sartomer, It is also commercially available under the trade names SR 489 (tridecyl acrylate, Sartomer, France) and SR 489 (tridecyl acrylate, Sartomer, France).
[0069] Suitable organic (meth)acrylates are also commercially available from Evonik Industries AG (Germany) as part of the VISIOMER® product line. Preferred compounds are glycerol formal methacrylate (VISIOMER® GLYFOMA), diurethane dimethacrylate (VISIOMER® HEMA TMDI), butyl diglycol methacrylate (VISIOMER® BDGMA), polyethylene glycol 200 dimethacrylate (VISIOMER® PEG200DMA), trimethylolpropane methacrylate (VISIOMER® TMPTMA), tetrahydrofurfuryl methacrylate (VISIOMER® THFMA), isobornyl methacrylate (VISIOMER® Terra IBOMA), isobornyl acrylate (VISIOMER® IBOA), methacrylic acid esters of fatty alcohols having an average of 13.0 carbon atoms (VISIOMER® Terra C13-MA) or methacrylic acid esters of fatty alcohols having an average of 17.4 carbon atoms (VISIOMER® Terra C17.4-MA).
[0070] The composition of the present invention more preferably comprises an organic (meth)acrylate selected from the group consisting of isobornyl methacrylate (VISIOMER® Terra IBOMA), isobornyl acrylate (VISIOMER® IBOA), lauryl acrylate, Ebecryl® 45, hexanediol diacrylate, and trimethylolpropane triacrylate.
[0071] Organic (meth)acrylate (component (b)) It is preferred that the (meth)acrylate group of the silicone (meth)acrylate is an acrylate group.
[0072] It is also preferred that the (meth)acrylate group of the organic (meth)acrylate (component (b)) silicone (meth)acrylate is a (meth)acrylate group.
[0073] It is preferred that the amount of organic methacrylate (component (b)) present in the composition of the present invention is from 0 to 60% by weight, preferably from 0 to 30% by weight, more preferably from 5 to 15% by weight, based on the total weight of the sum of components (a) to (e) and / or based on the total weight of the composition, preferably based on the total weight of the composition.
[0074] The composition according to the invention preferably comprises component (c). Component (c) consists of at least one silicone (meth)acrylate which does not have any urethane groups. The silicone (meth)acrylate is therefore free of urethane groups.
[0075] At least one silicone (meth)acrylate of component (c) is represented by formula (Q) and / or at least one silicone (meth)acrylate of component (c) is represented by formula (S), M A m1 D d1 Formula (Q) During the ceremony, M A =[R2(R A )SiO 1 / 2 ], D = [R2SiO 2 / 2 ], m1 is an integer equal to 2; d1 is an integer of 1 to 10,000, preferably 50 to 5,000, and more preferably 70 to 2,000; During the ceremony, R is, in each case, independently selected from the group consisting of monovalent organic radicals that do not contain any urethane or (meth)acrylate groups; Preferably, in each case, independently selected from the group consisting of monovalent hydrocarbon radicals having 1 to 30 carbon atoms, More preferably, it is a methyl radical. R A are independently selected in each case from the group consisting of monovalent organic radicals having at least one (meth)acrylate group and no urethane groups; Preferably, in each case, the compound has the formula (R): [ka] and independently selected from the group consisting of monovalent radicals represented by x1 is as defined above, x4 is an integer of 0 or 1, preferably 0; R 6 are independently selected in each occurrence from the group consisting of monovalent hydrocarbon radicals having 1 to 6 carbon atoms; Preferably, it is an ethyl radical, R 7 are independently selected in each case from the group consisting of monovalent organic radicals having at least one (meth)acrylate group and no urethane groups; Preferably, in each case, independently selected from monovalent radicals of formula (H), as defined above, M m1 D d1 D A d2 D AC d3 Formula(S) During the ceremony, M = [RSiO 1 / 2 ], D = [R2SiO 2 / 2 ], D A =[R(R A )SiO 2 / 2 ], D AC =[R(R AC )SiO 2 / 2 ], During the ceremony, R, m1, and d1 are as defined above for formula (Q); d2 is an integer of 1 to 20, preferably 2 to 10, more preferably 3 to 8; d3 is an integer of 0 to 3, preferably 0 to 2, more preferably 0 to 1; R Aare independently selected in each case from the group consisting of monovalent organic radicals having at least one (meth)acrylate group and no urethane groups; Preferably, in each case, independently selected from the group consisting of monovalent radicals represented by formula (K) or (L): More preferably, in each case, independently selected from the group consisting of monovalent radicals represented by formula (K): [ka] In the formula, x1 and R 4 is as previously defined, R AC are independently selected from the group consisting of monovalent organic radicals having at least one carboxylic acid ester group and no (meth)acrylate groups and no urethane groups; Preferably, in each case, the compound has the formula (T) or (U): [ka] and independently selected from the group consisting of monovalent radicals represented by where x1 is as defined above, R 5 are independently selected in each occurrence from the group consisting of monovalent hydrocarbon radicals having 1 to 22 carbon atoms; Preferably, it is a methyl radical. It is preferred.
[0076] At least one silicone (meth)acrylate of component (c) represented by formula (Q) is referred to herein as component (c1). At least one silicone (meth)acrylate of component (c) represented by formula (S) is referred to herein as component (c2). Thus, component (c) is composed of component (c1) and / or component (c2), component (c1) is composed of at least one silicone (meth)acrylate represented by formula (Q), and component (c2) is composed of at least one silicone (meth)acrylate represented by formula (S).
[0077] Examples of silicone (meth)acrylates according to formula (Q) (component (c1)) are known to the person skilled in the art and can be prepared, for example, as described in EP-A-0 940 422.
[0078] Examples of silicone (meth)acrylates (component (c2)) according to formula (S) are also known to those skilled in the art and can be prepared, for example, as described in EP 3168273 A and WO 2017187030 A1.
[0079] It is preferred that the amount of silicone (meth)acrylate (component (c)) present in the composition of the present invention is from 0 to 95% by weight, preferably from 65 to 85% by weight, more preferably from 70 to 80% by weight, based on the total weight of the sum of components (a) to (e) and / or based on the total weight of the composition, preferably based on the total weight of the composition.
[0080] It is particularly preferred that the amount of silicone (meth)acrylate according to formula (Q) (component (c1)) present in the composition of the present invention is from 0 to 95 wt.-%, preferably from 65 to 85 wt.-%, more preferably from 70 to 80 wt.-%, based on the total weight of the sum of components (a) to (e) and / or based on the total weight of the composition, preferably based on the total weight of the composition.
[0081] It is particularly preferred that the amount of silicone (meth)acrylate according to formula (S) (component (c2)) present in the composition of the present invention is 0 to 95 wt.-%, preferably 65 to 85 wt.-%, more preferably 70 to 80 wt.-%, based on the total weight of the sum of components (a) to (e) and / or based on the total weight of the composition, preferably based on the total weight of the composition.
[0082] It is preferred that the (meth)acrylate group of the silicone (meth)acrylate (component (c1)) represented by the general formula (Q) is an acrylate group. Similarly, it is preferred that the (meth)acrylate group of the silicone (meth)acrylate (component (c2)) represented by the general formula (S) is an acrylate group. It is more preferred that the (meth)acrylate group of the silicone (meth)acrylate (component (c1)) represented by the formula (Q) and the (meth)acrylate group of the silicone (meth)acrylate (component (c1)) represented by the formula (S) are acrylate groups.
[0083] It is particularly preferred that the (meth)acrylate groups of components (a), (b), and (c) (such as components (c1) and (c2)) are acrylate groups.
[0084] It is also particularly preferred that the (meth)acrylate groups of components (a) and (c) (such as (c1) and (c2)) are acrylate groups and the (meth)acrylate groups of component (b) are (meth)acrylate groups.
[0085] Component (d) of the composition according to the present invention consists of one or more curing catalysts.Preferably, the curing catalyst is a compound that generates a reactive species, such as a free radical, a cation, or an anion, more preferably a radical, when exposed to an external trigger, such as actinic radiation, preferably UV light and / or visible light, or heat.Accordingly, the curing catalyst can be a catalyst for photocuring (photoinitiator) or a catalyst for thermal curing (thermal curing catalyst).
[0086] It may be advantageous to have one or more thermal curing catalysts present in the composition of the present invention. Thermal curing catalysts are compounds that generate reactive species, such as free radicals, cations, or anions, when exposed to heat. It is preferred that the thermal curing catalyst comprises an organic peroxide, such as 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane (e.g., LUPEROX 101®), dilauroyl peroxide (e.g., LUPEROX LP®), dibenzoyl peroxide (e.g., LUPEROX A98®), and bis(tert-butyldioxyisopropyl)benzene (e.g., VulCUP R®). Such organic peroxides are available from a variety of sources, including, but not limited to, Arkema (France). Preferred examples include ketone peroxides such as methyl ethyl ketone peroxide, diacyl peroxides such as benzoyl peroxide, hydroperoxides such as cumene hydroperoxide, as well as peroxyketals, dialkyl peroxides, peroxydicarbonates, and peroxyesters. Examples of thermal curing catalysts also include inorganic peroxides such as peroxydisulfates including sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), and ammonium persulfate ((NH4)2S2O8). Examples of thermal curing catalysts further include azobisisobutyronitrile (AIBN).
[0087] It may be advantageous for one or more photoinitiators to be present in the composition of the present invention. Photoinitiators are compounds that generate reactive species, such as free radicals, cations, or anions, when exposed to actinic radiation, preferably UV or visible light, more preferably UV light. Any suitable photoinitiator may be present in the composition of the present invention, including, but not limited to, Norrish Type I and Norrish Type II photoinitiators, and including, for example, commonly used UV photoinitiators, including acetophenone (e.g., diethoxyacetophenone), phosphine oxide, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (PPO), Irgacure 369, and the like (see, for example, U.S. Patent No. 9,453,142 to Rolland et al.). Preferred photoinitiators according to the present invention are those that generate free radicals. The most preferred photoinitiator is bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, available under the trade name OMNIRAD® 819 from IGM resins (previously known as IRGACURE® 819 from BASF SE). Other photoinitiators that may be used in the compositions of the invention are available under the product names OMNIRAD® TPO (diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide) and OMNIRAD® TPO-L (ethyl(2,4,6-trimethylbenzoyl)phenylphosphinate) from IGM resins. Photoinitiators of the Norrish 1 type, such as benzophenone, benzoin, α-hydroxyalkylphenone, acylphosphine oxide, or derivatives thereof, are particularly preferred. Conventional photoinitiators are described, for example, in ''A Compilation of Photoinitiators Commercially available for UV today'' (K. Dietliker, SITA Technology Ltd., London 2002).
[0088] It is preferred that the amount of curing catalyst (component (d)) present in the composition of the present invention is from 0 to 5 wt.%, preferably from 0.1 to 3 wt.%, more preferably from 0.5 to 2.5 wt.%, based on the total weight of the sum of components (a)-(e) and / or based on the total weight of the composition, preferably based on the total weight of the composition.
[0089] Component (e) of the composition according to the invention consists of one or more additives.
[0090] Component (e) may include solid particles suspended or dispersed therein as additives. Any suitable solid particles may be used depending on the final product to be produced. The particles may be metallic, organic / polymeric, inorganic, or composites or mixtures thereof. The particles may be non-conductive, semi-conductive, or conductive (including metallic and non-metallic or polymeric conductors), and the particles may be magnetic, ferromagnetic, paramagnetic, or non-magnetic. The particles may be of any suitable shape including spherical, ellipsoidal, cylindrical, etc. The particles may be of any suitable size (e.g., average diameter ranging from 1 nm to 200 μm). The particles may include active agents or detectable compounds, which may also be provided dissolved / solubilized in the compositions of the invention. For example, magnetic or paramagnetic particles or nanoparticles may be used.
[0091] Component (e) may again include as additives pigments, dyes, active compounds, detectable compounds (eg fluorescent, phosphorescent) depending on the particular purpose of the product being manufactured.
[0092] It is particularly preferred that component (e) contains a non-reactive pigment or dye that absorbs light as an additive. Suitable examples of such light absorbers include, but are not limited to, (i) titanium dioxide (e.g., in an amount of 0.05 or 0.1 to 1 or 5 weight percent), (ii) carbon black (e.g., in an amount of 0.05 or 0.1 to 1 or 5 weight percent), and / or organic ultraviolet light absorbers (UV blockers), such as hydroxybenzophenone, hydroxyphenylbenzotriazole, oxanilide, benzophenone, thioxanthone, hydroxyphenyltriazine, thiophene and / or benzotriazole ultraviolet light absorbers (e.g., Mayzo BLS1326) (e.g., in an amount of 0.001 or 0.005 to 1, 2, or 4 weight percent). Examples of suitable organic ultraviolet light absorbers include, but are not limited to, those described in U.S. Patent Nos. 3,213,058, 6,916,867, 7,157,586, and 7,695,643, the disclosures of which are incorporated herein by reference.Another example of a suitable organic ultraviolet light absorber is 2,5-bis(5-tert-butyl-2-benzoxazolyl)thiophene (BBOT).
[0093] When the composition includes component (d) containing a thermal curing catalyst, it is preferred that component (e) is also present and includes a curing accelerator for thermal curing. Examples of such curing accelerators include organic acid metal salts such as cobalt naphthenate, and N-substituted aromatic amines such as N,N-dimethylaniline and N,N-dimethyl-para-toluidine.
[0094] When the composition includes component (d) containing a photoinitiator, component (e) is also present and preferably includes a photosensitizer. Examples of such photosensitizers include, but are not limited to, amines such as n-butylamine, triethylamine, N-methyldiethanolamine, piperidine, N,N-dimethylaniline, and triethylenetetramine, sulfur compounds such as S-benzyl-isothiuronium-p-toluenesulfinate, nitriles such as N,N-dimethyl-p-aminobenzonitrile, and phosphorus compounds such as sodium diethylthiophosphate.
[0095] The composition according to the invention may include any suitable filler as additive (component (e)) depending on the desired properties of the part or object to be fabricated. Thus, the filler may be solid or liquid, organic or inorganic, and may include, but is not limited to, reactive and non-reactive rubbers, siloxanes, acrylonitrile butadiene rubbers, reactive and non-reactive thermoplastics (including but not limited to poly(etherimides), maleimide-styrene terpolymers, polyacrylates, polysulfones, and polyethersulfones, etc.), inorganic fillers such as silicates (talc, clay, silica, mica, etc.), glass, carbon nanotubes, graphene, cellulose nanocrystals, combinations of all of the foregoing, etc. Suitable fillers include, but are not limited to, reinforcing agents such as core-shell rubbers. The filler is preferably selected from inorganic particles, more preferably from carbon black and / or silica. Most preferably, silica functionalized with methacrylate groups is present as a filler in the composition according to the invention. Suitable silicas functionalized with methacrylate groups are available, for example, from Evonik Industries AG, Germany, under the trade names AEROSIL® 701, AEROSIL® 711, AEROSIL® R 7200, and AEROSIL® R 8200. It is preferred that the amount of filler present in the composition of the present invention is 0 to 20% by weight, preferably 0 to 10% by weight, more preferably 0 to 5% by weight, based on the total weight of the sum of components (a) to (e) and / or based on the total weight of the composition, preferably based on the total weight of the composition.
[0096] The composition according to the invention preferably comprises a polymerization inhibitor and / or antioxidant as an additive (component (e)). By using a polymerization inhibitor and / or antioxidant, polymerization of the composition during its preparation and / or its storage can be prevented. Suitable polymerization inhibitors are, for example, 2,6-di-tert-butyl-4-methylphenol, catechol, 4-methoxyphenol, 4-tert-butyloxyphenol, 4-benzyloxyphenol, naphthol, phenothiazine, 10-10-dimethyl-9,10-dihydroacridine, bis[2-hydroxy-5-methyl-3-cyclohexylphenyl]methane, bis[2-hydroxy-5-methyl-3-tert-butylphenyl]methane, hydroquinone, pyrogallol, 3,4-dihydroxy-1-tert-butylbenzol, 4-methoxy-2(3)-tert-butylphenol (BHA), as well as BHA in combination with bis[2-carboxyethyl]sulfide (TDPA), 4-methyl-2,6-di-tert-butylphenol (BHT), bis[4- hydroxy-2-methyl-5-tert.-butylphenyl]sulfide, 4-butylmercaptomethyl-2,6-di-tert.-butylphenol, 4-hydroxy-3,5-di-tert.-butylphenyl methanesulfonic acid dioctadecyl ester, 2,5-dihydroxytoluene, 2,5-dihydroxy-1-tert.-butylbenzene, 2,5-dihydroxy-1,4-di-tert.-butylbenzene, 3,4-dihydroxy-1-tert.-butylbenzene and 2,3-dimethyl-1,4-bis[3,4-dihydroxyphenyl]butane, 2,2'-thiobis(4-tert.-octylphenol), (2,2,6,6)-tetramethylpiperidin-1-yl)oxyl (TEMPO), and also TEMPO derivatives such as, for example, 4-hydroxy-TEMPO. A preferred polymerization inhibitor is 2,6-di-tert-butyl-4-methylphenol (BHT) sold under the trade name IONOL® CP by Oxiris Chemicals SA. The amount of polymerization inhibitor present in the composition of the present invention is preferably 0.001 to 1% by weight, more preferably 0.01 to 0.5% by weight, based on the total composition.
[0097] It is preferred that the total amount of additives (component (e)) present in the composition of the present invention is from 0 to 20% by weight, preferably from 0 to 10% by weight, more preferably from 0 to 5% by weight, based on the total weight of the sum of components (a) to (e) and / or based on the total weight of the composition, preferably based on the total weight of the composition.
[0098] Component (f) of the composition according to the invention consists of one or more solvents. Examples of solvents include, but are not limited to, aprotic solvents, preferably acetone, tetrahydrofuran (THF), dimethylformamide (DMF), acetonitrile (MeCN) or dimethylsulfoxide (DMSO), more preferably acetone. However, it is preferred that the composition according to the invention is essentially solvent-free. It is therefore preferred that the amount of solvent present in the composition according to the invention is 0-10% by weight, preferably 0-5% by weight, more preferably 0-1% by weight, based on the total weight of the sum of components (a)-(e) and / or based on the total weight of the composition, preferably based on the total weight of the composition.
[0099] The composition according to the invention is preferably used to produce a release coating, a protective film, a protective coating, or a 3D printed object by curing said composition.
[0100] It is therefore preferred that the composition is curable, preferably curable by radical reactions, which can be initiated thermally, by UV radiation and / or by electron beam. The composition according to the invention can be crosslinked three-dimensionally by free radicals and can be cured thermally in a very short time, for example by adding peroxides, or under the influence of high-energy radiation, such as UV or electron beam, to form mechanically and chemically durable layers with predeterminable adhesive properties and also adhesive properties, taking into account the suitable formulation of the composition according to the invention. If the radiation used is UV radiation, the crosslinking / curing preferably takes place in the presence of a photoinitiator and / or photosensitizer. Photoinitiators of the Norrish 1 type, such as benzophenone, benzoin, α-hydroxyalkylphenone, acylphosphine oxide or derivatives thereof, are preferred. Conventional photoinitiators are described, for example, in ''A Compilation of Photoinitiators Commercially available for UV today'' (K. Dietliker, SITA Technology Ltd., London 2002). A preferred composition according to the invention comprises a photoinitiator and / or photosensitizer in a mass proportion of 0.01% to 10%, in particular 0.1% to 5%, based on the mass of the total composition. The photoinitiator and / or photosensitizer is preferably soluble in the composition according to the invention, more preferably in a mass proportion of 0.01% to 10%, in particular 0.1% to 5%, based on the mass of the total composition.
[0101] The composition according to the invention can be prepared by any suitable method, for example by mixing component (a) with one or more of the optional components (b) to (f) in any order. The solvent (component (f)) is mainly used to reduce the viscosity of the composition and facilitate mixing of the components. Component (f) facilitates the preparation of the composition and the application of the composition. However, it is generally preferred to provide a composition that is essentially solvent-free, i.e., essentially free of component (f). Consequently, it is preferred to (essentially) remove the solvent (component (f)) from the composition after or at some point during its preparation.
[0102] Thus, a further aspect of the present invention is (i) preparing a mixture of component (a) and component (f); (ii) preparing a mixture by adding at least one of components (b) to (e), preferably components (b) and / or (c), to the mixture of step (i); (iii) (essentially) removing component (f) from the mixture of step (ii); (iv) optionally preparing a mixture by adding at least one of components (b)-(e) to the mixture of step (iii), if said component was not added in step (ii); A method for preparing a composition according to the invention, comprising or consisting of:
[0103] The process steps (i) to (iv) are carried out in a given order. However, they can be interrupted by additional intermediate process steps. In addition to the solvent component (g) or as an alternative to the solvent (component (g)), it is also possible to use a reactive diluent (component (b)). The preparation of the mixture can be carried out at room temperature or at elevated temperature. Mixing can be carried out using conventional mixing devices, for example speed mixers.
[0104] The composition according to the invention can be used in various fields. It is particularly suitable for use in the production of release coatings, protective films, protective coatings, as well as in the manufacture of 3D printed objects by stereolithography.
[0105] A further aspect of the present invention is therefore a release coating, protective film or protective coating obtainable by curing of a composition according to the invention or a 3D printed object obtainable by 3D printing of a composition according to the invention.
[0106] It is preferred to use the compositions according to the invention to produce release coatings. Release coatings (often also called adhesive coatings) are known from the prior art. They are used in various ways for the production of labels, adhesive tapes or sanitary articles. Release coatings are characterized by low adhesion in contact with adhesives and consist of radiation-cured silicones. Two mechanisms are typically used for the curing of functional silicones: in the case of cationic curing, epoxy-functional organosiloxanes are polymerized using photoinitiators that release acids on irradiation. In the case of free-radical curing, silicone (meth)acrylates are polymerized using photoinitiators that form radicals on irradiation.
[0107] It is also preferred to use the composition according to the invention for 3D printing. "3D printing" is often called "additive manufacturing" and vice versa. Therefore, in the context of this invention, the terms "3D printing" and "additive manufacturing" are used synonymously and refer to a method of building an object by adding layers of material. The object thus obtained is called a 3D printed object in the context of the present invention. It is preferred that the 3D printing method / additive manufacturing method is a method of creating an object from three-dimensional digital information.
[0108] Lithography-based additive manufacturing, such as stereolithography, as well as 3D printing methods in general, have traditionally been used primarily to generate prototypes and functional patterns ("rapid prototyping"). As a result of technological advances, real production applications, such as transparent orthotics or hearing aid shells, are becoming increasingly important. In this application, the mechanical and thermal properties of the printing material are of great importance. However, the materials currently available for additive manufacturing do not yet possess the mechanical properties of traditional production materials (see, for example, T. Swetly, J. Stampfl, G. Kempf, and R.-M. Hucke, ''Capabilities of Additive Manufacturing Technologies (AMT) in the Validation of the Automobile Cockpit'', RTejournal - Forum for Rapid Technology 2014 (1)).
[0109] These materials (resins) for lithography-based additive manufacturing are based on reactive components that can be cured by exposure. For this purpose, radical (e.g. acrylates) or cationic (e.g. epoxides) polymerization is frequently used. For this purpose, special photoinitiators are added to the resins, which cause the polymerization of the reactive components by changing their state by exposure.
[0110] Various methods are available for additively manufacturing objects from these resins, such as stereolithography, digital light processing, and multijet modeling. All procedures involve the curing of several layers of these resins, thus producing three-dimensional objects. Generally, resins with low viscosities, for example 20-40 mPa·s, are required (see I. Gibson, DW Rosen, B. Stucker et al., ''Additive manufacturing technologies'', vol. 238, Springer Verlag (2010)). To improve the mechanical properties of the products cured in this way, especially the toughness and elongation at break, the crosslink density can be reduced or the molecular weight of the monomers can be increased. However, this increases the viscosity or the melting point of the uncured resins, and until recently, for the latter reason, it was not possible to cure these using additive manufacturing methods. In addition, the curing speed can be too low.
[0111] However, new developments make it possible to process resins with higher viscosities. For example, WO 2015 / 075094 and WO 2016 / 078838 disclose stereolithography devices in which layers of polymerizable material that are successively cured are heated, allowing processing even with highly viscous resins. WO 2015 / 074088 discloses photopolymerizable compositions with a viscosity of at least 20 Pa·s at room temperature, which are heated to at least 30° C. during curing. For comparison: 20 Pa·s corresponds roughly to the viscosity of ethylene glycol or viscous honey, while butter, with a viscosity of about 30 Pa·s, is barely flowable. However, this is advantageous if there is no need to heat the polymerizable material during the additive manufacturing process.
[0112] The compositions of the present invention exhibit low viscosity, fast photocure response, and good mechanical properties, especially with respect to tensile strength at break and elongation at break.
[0113] The compositions used in the present invention have the advantage that they can be processed at room temperature below 50° C., preferably below 25° C., since the viscosity of the composition at the processing temperature is preferably below 20 Pa·s.
[0114] The compositions used in the present invention have the advantage that they can be processed without the presence of solvents, therefore no organic volatiles are produced during the additive manufacturing process.
[0115] The compositions used in the present invention have the further advantage that they can be produced in a simple manner.
[0116] The compositions used in the present invention have the advantage that they may contain fillers which provide better properties, especially better tensile strength at break and elongation at break.
[0117] The composition used in the present invention has a low T g and has the further advantage that the use of this composition makes it possible to obtain, by additive manufacturing, products which are elastomers or have one or more properties typical of elastomers, for example an elongation at break of preferably more than 40%, more preferably more than 60%, and most preferably more than 100%.
[0118] The composition according to the present invention can be used as a photopolymerizable material in additive manufacturing / 3D printing methods, preferably based on stereolithography.The composition according to the present invention can be applied as a raw material in additive manufacturing methods, such as those described in WO2015 / 075094 or WO2016 / 078838.
[0119] In general, additive manufacturing / 3D printing methods are based on the following technology: the production of shaped bodies by processing multiple layers of photopolymerizable material, in which a freshly supplied layer of photopolymerizable material is polymerized with the desired contour in each case, and by successively defining its individual contour for each layer, the desired object is formed with its three-dimensional shape resulting from the succession of layers produced.
[0120] Thus, the method for preparing a release coating or 3D printed object preferably comprises the following indirect or direct successive steps: a. applying a composition to a surface; b. curing the composition, preferably by exposure to UV radiation. Includes.
[0121] In the production of a 3D printed object by the 3D printing method, the method steps a and b are preferably performed repeatedly in alternating order, in this way the 3D printed object is built up step by step.
[0122] Suitable sources of UV radiation for curing the compositions according to the invention are optionally doped medium- or low-pressure mercury vapor lamps, UV-LED lamps or so-called excimer emitters. The UV emitters may be polychromatic or monochromatic. The emission range of the emitter is preferably within the absorption range of the photoinitiator and / or photosensitizer.
[0123] In the production of release coatings, the surface is preferably the surface of a carrier, preferably a sheet-like carrier. Here, the composition of the present invention can be applied to the sheet-like carrier on one or both sides. The sheet-like carrier is preferably selected from the group consisting of paper, fabric, metal foil, and polymer film. The carrier can be smooth or provided with a surface structure. Particularly preferred carriers are polypropylene and polyethylene films.
[0124] The release coating is applied, for example, to adhesive tapes, labels, self-adhesive hygiene product packaging, food packaging, self-adhesive thermal paper, or liners for asphalt roofing membranes. The release coating has good release effect for the adhesive materials used in these applications.
[0125] The peeling effect for adhesive materials, usually adhesive tapes or labels for industrial use, is expressed by the peeling force, with a low peeling force representing a good peeling effect. The peeling force is determined according to the FINAT Handbook 8th Edition, The Hague / NL, 2009, under the name FTM10, with the modification that the storage is carried out under pressure at 40°C. The peeling force depends on the quality of the release coating (e.g. the uniformity, thickness and / or smoothness of the coating), the adhesive material or adhesive, and the test conditions. Therefore, for the evaluation of the release coating, the adhesive or adhesive material present and the test conditions should be the same. The peeling force is checked using the 2.5 cm wide adhesive tape TESA® 7475, a trademark of Tesa SE, Germany, Hamburg.
[0126] The release coating of the present invention preferably has a release force of at most 20 cN / 2.5cm, more preferably at most 10 cN / 2.5cm, very preferably at most 8 cN / 2.5cm, the release force being at least 0.5 cN / 2.5cm, preferably at least 1 cN / 2.5cm.
[0127] It is believed that those skilled in the art can make the most of the above description without further elaboration. Therefore, the preferred embodiments and examples should be interpreted merely as an explanatory disclosure, and are in no way limiting.
[0128] Without further elaboration, it is believed that a person skilled in the art can utilize the above description to the fullest extent possible. Therefore, the preferred embodiments and examples should be interpreted merely as an explanatory disclosure, and are in no way limiting.
[0129] All definitions, embodiments and elaborations applicable to one aspect of the invention are applicable, mutatis mutandis, to other aspects of the invention and vice versa.
[0130] The present subject matter will be more particularly detailed with reference to Figures 1 and 2, without it being intended in any way that the present subject matter is limited thereto. [Brief description of the drawings]
[0131] [Figure 1] FIG. 1 shows a reaction scheme for the synthesis of a silicone urethane (meth)acrylate (7) according to formula (A) formed by the reaction of a hydroxy-functional silicone (meth)acrylate (5) with an isocyanate-functional urethane (meth)acrylate (6), the hydroxy-functional silicone (meth)acrylate (5) being formed by the reaction of a (meth)acrylic acid (1) with an epoxy-functional silicone (2), and the isocyanate-functional urethane (meth)acrylate (6) being formed by the reaction of a diisocyanate (3) of formula (D) with a hydroxy-functional (meth)acrylate (4) of formula (E). [Diagram 2] FIG. 14 shows tensile tests (dotted lines) and cyclic measurements (solid lines) of 3D printed test samples based on formulations F16 and F17.
[0132] The present invention will be illustratively described in the following examples, but the scope of the present invention is clear from the entire specification and claims, and it is not possible to interpret the present invention as being limited to the embodiments described in the examples. Therefore, the following examples are only useful for explaining the present invention in detail to those skilled in the art, and do not constitute any limitations on the claimed subject matter.
[0133] Working Example The following examples serve only to illustrate the invention to one of ordinary skill in the art and are not intended to constitute any limitation of the claimed subject matter.
[0134] method Epoxide Value: The epoxide number was determined in weight percent according to DIN EN ISO 3001 (1999-11) and ASTM D 1652 (2011).
[0135] viscosity: The viscosity was measured at 25° C. with a Brookfield R / S-CPS Plus rheometer using a RP75 measuring plate. The test method is described in DIN 53019 (DIN 53019-1 (2008-09), DIN 53019-2 (2001-02) and DIN 53019-3 (2008-09)).
[0136] Acid Number: The acid number was determined in mg KOH / g polymer by titration means according to DIN EN ISO 2114 (2002-06).
[0137] Hydroxyl number (OH number): The OH number was determined in mg KOH / g polymer by titration means according to DIN EN ISO 4629-2 (2016-12).
[0138] Isocyanate value (NCO value): The NCO number was determined in % by weight by titration according to DIN EN 1242 (2013-05).
[0139] Gel Permeation Chromatography (GPC): Weight average molecular weight Mw and number average molecular weight M n The GPC measurements are carried out under the following measurement conditions: column combination SDV1000 / 10000 Å (length 55 cm), temperature 35° C., THF as mobile phase, flow rate 0.35 ml / min, sample concentration 10 g / l, RI detector, evaluation of the polymer against polystyrene standards (162-2520000 g / mol).
[0140] material VESTANAT® AT EP-DC 1241: VESTANAT® AT EP-DC 1241 (Evonik Industries AG) is a commercially available adduct of 2-hydroxyethyl-propenoate (2-hydroxyethyl acrylate, HEA) with 5-isocyanato(isocyanatomethyl)-1,3,3-trimethylcyclohexane (isophorone diisocyanate, IPDI) and contains the following isomers: [ka] Component (a) - a silicone urethane (meth)acrylate according to formula (F)
[0141] synthesis S1) Preparation of silicone urethane acrylates according to formula (F), where m1=0, m2=2, m3=0, d1=28, d2=t=q=0, x1=3, (x2=1 and x3=0) or (x2=1 and x3=0), R=CH3, R 1 =H, R 2 =Formula (H), R 3 =Formula (I), R 4 =H, and R 5 =Formula(J) A 2 L four-neck flask equipped with a mechanical stirrer, reflux condenser, and internal thermometer is charged with 94.4 g acrylic acid, 0.3 g methylhydroquinone, 69.5 g n-butanol, 41.7 g methyl isobutyl ketone, and 3 g of 50% aqueous chromium(III) acetate solution with stirring. To this is added 1291 g polydimethylsiloxane modified with terminal epoxy groups and having an epoxide oxygen value of 1.32 wt.%. Stirring at 115-120 °C is continued until the conversion of the epoxy groups, as determined by the acid value, is greater than 99%. All volatiles are then distilled off at 120 °C and full vacuum. Filtration gives a liquid silicone acrylate with a viscosity of less than 200 mPa·s at 25 °C and a hydroxyl value of 52 mg KOH / g.
[0142] In a 2 L four-neck flask equipped with a mechanical stirrer, a reflux condenser and an internal thermometer, 1078.8 g of the silicone acrylate thus prepared are mixed with 356.2 g of VESTANAT® EP-DC 1241 and 2.87 g of TIB KAT 716 LA and stirred for 6 hours at 60° C. The high-viscosity silicone urethane acrylate has a residual NCO content of less than 0.03% and a number average molecular weight M determined by GPC of 4395 g / mol. n and a weight average molecular weight Mw of 6513 g / mol.
[0143] S2) Preparation of silicone urethane acrylates according to formula (F), where m1=0, m2=1, m3=1, d1=28, d2=t=q=0, x1=3, (x2=1 and x3=0) or (x2=1 and x3=0), R=CH3, R 1 =H, R 2 =Formula (H), R 3 =Formula (I), R 4 =H, R 5 = Formula (J), and R A = Formula (K) or (L) In a 2 L four-neck flask equipped with a mechanical stirrer, a reflux condenser and an internal thermometer, 253 g of the silicone acrylate prepared according to Example S1 having a hydroxyl number of 51 mg KOH / g are mixed with 40.96 g of VESTANAT® EP-DC 1241 and 0.59 g of TIB KAT 716 LA and stirred for 6 hours at 60° C. The resulting silicone urethane acrylate had a viscosity of 1837 mPa·s at 25° C. and a number average molecular weight M determined by GPC of 2872 g / mol. n and a weight average molecular weight Mw of 5377 g / mol.
[0144] S3) Preparation of silicone urethane acrylates according to formula (F), where m1=0, m2=2, m3=0, d1=48, d2=d3=t=q=0, x1=3, (x2=1 and x3=0) or (x2=1 and x3=0), R=CH3, R 1 =H, R 2 =Formula (H), R 3=Formula (I), R 4 =H, and R 5 =Formula(J) A 2 L four-neck flask equipped with a mechanical stirrer, reflux condenser and internal thermometer is charged with 131.69 g acrylic acid, 0.6 g methylhydroquinone, 86.9 g n-butanol, 3.6 g 2-(((3-(octyloxy)propyl)imino)methyl)phenol prepared according to EP 3168273, and 1.7 g 50% aqueous chromium(III) acetate solution with stirring. To this is added 2763.5 g polydimethylsiloxane modified with terminal epoxy groups and having an epoxide oxygen value of 0.92% by weight, while heating to 115°C. Stirring at 115-120°C is continued until the conversion of the epoxy groups, determined by the acid value, is greater than 99%. All volatiles are then distilled off at 120°C and 3 mbar vacuum with a slight bleed. Filtration gives a liquid silicone acrylate with a hydroxyl number of 30 mg KOH / g.
[0145] In a 2 L four-neck flask equipped with a mechanical stirrer, a reflux condenser and an internal thermometer, 3140.8 g of the silicone acrylate thus prepared are mixed with 1123.5 g of acetone, 604.2 g of VESTANAT® EP-DC 1241 and 7.5 g of TIB KAT 716 LA and stirred for 6 hours at 60° C. Distillation at 60° C. and 3 mbar with a slight air bleed gives a greenish-brown transparent product having a viscosity of 18216 mPa·s at 25° C.
[0146] S4) Preparation of silicone urethane acrylate according to formula (F), where m1=0, m2=2, m3=0, d1=8, d2=d3=t=q=0, x1=3, x3=1, R=CH3, R 1 =C2H5,R 2 =R 3 =Formula (I), R 4 =H, R 5 =Formula(J) A 5 L four-neck flask equipped with a mechanical stirrer, reflux condenser and internal thermometer is charged with 47.7 g of a hydroxy-functional siloxane having a hydroxyl number of 200 mg KOH / g prepared according to Example 1 of EP 0940422 and 57.7 g of VESTANAT® EP-DC 1241, and the mixture is heated to 80° C. with stirring. To this, 0.21 g of TIB® KAT 716 LA is added, and the mixture is stirred at 80° C. for 5 hours. During this time, the viscosity increases sharply. This results in a polymer that is transparent yellow and highly viscous at 80° C., and solidifies into a glassy mass at room temperature.
[0147] S5) Preparation of silicone urethane acrylate according to formula (F), where m1=0, m2=2, m3=0, d1=78, d2=d3=t=q=0, x1=3, x3=1, R=CH3, R 1 =C2H5,R 2 =R 3 =Formula (I), R 4 =H, R 5 =Formula(J) In a 5 L four-neck flask equipped with a mechanical stirrer, a reflux condenser and an internal thermometer, 1055.21 g of a hydroxy-functional siloxane having a hydroxyl number of 42 mg KOH / g prepared according to the prior art disclosed in EP 0940422 and 281.41 g of VESTANAT® EP DC 1241 are dissolved in 2004.94 g of toluene and 2.67 g of TIB® KAT 716 LA are added.
[0148] The reaction mixture is heated to 60° C. and stirred for 4 h. Toluene is distilled off at 70° C. and the target pressure of 20 mbar is reached after 2 h, yielding a polymer that is very viscous at 70° C. and solidifies into a glassy mass at room temperature. The number average molecular weight M determined by GPC is n is 8638 g / mol, and the weight average molecular weight Mw is 28731 g / mol.
[0149] S6) Preparation of silicone urethane acrylate according to formula (F), where m1=0, m2=2, m3=0, d1=48, d2=d3=t=q=0, x1=3, x3=0, R=CH3, R 1 =R 2 =H, R 3 =Formula (I), R 4 =H, R 5 =Formula(J) A 0.5 L four-neck flask equipped with a mechanical stirrer, a reflux condenser and an internal thermometer is charged with 179.0 g of polydimethylsiloxane modified with terminal hydroxyl groups and having a hydroxyl number of 47 mg KOH / g, and 53.3 g of VESTANAT® EP DC 1241 and 116.1 g of toluene are added with stirring. To this, 0.23 g of TIB® KAT 716 LA is added. The reaction mixture is heated to 60° C. and stirred at 60° C. for 4 hours. The solvent is then distilled off in a rotary evaporator at 80° C. and 2 mbar over a period of 1 hour. A very viscous polymer is obtained that solidifies at room temperature.
[0150] S7) Preparation of silicone urethane acrylates according to formula (F), where m1=1, m2=1, m3=0, d1=28, d2=d3=t=q=0, x1=3, (x2=1 and x3=0) or (x2=1 and x3=0), R=CH3, R 1 =H, R 2 =Formula (H), R 3 =Formula (I), R 4 =H, and R 5 =Formula(J) A 0.5 L four-neck flask equipped with a mechanical stirrer, reflux condenser, and internal thermometer is charged with 12.4 g acrylic acid, 0.032 g methylhydroquinone, 9.5 g n-butanol, 0.38 g 2-(((3-(octyloxy)propyl)imino)methyl)phenol prepared according to EP 3168273, and 0.19 g 50% aqueous chromium(III) acetate solution with stirring. To this is added 303.7 g linear polydimethylsiloxane with 0.79 wt% epoxide oxygen value modified with one terminal epoxy group and one terminal trimethylsiloxy group while heating to 120°C. Stirring at 115-120°C is continued until the conversion of the epoxy groups, as determined by the acid value, is greater than 99%. All volatile substances are then distilled off with a slight air bleed at 120° C. and a vacuum of 3 mbar. Filtration gives a liquid silicone acrylate with a hydroxyl number of 27 mg KOH / g.
[0151] In a 0.5 L four-neck flask equipped with a mechanical stirrer, a reflux condenser and an internal thermometer, 200.6 g of the silicone acrylate thus prepared are mixed with 70.3 g of acetone, 33.8 g of VESTANAT® EP-DC 1241 and 0.23 g of TIB KAT 716 LA and stirred for 4 h at 60° C. Distillation at 60° C. and 1-2 mbar with a slight air bleed gives a greenish transparent product with a viscosity of 857 mPa·s at 25° C.
[0152] S8) Preparation of silicone urethane acrylates according to formula (F), where m1=2, m2=0, m3=0, d1=65, d2=4, d3=t=q=0, x1=3, (x2=1 and x3=0) or (x2=1 and x3=0), R=CH3, R 1 =H, R 2 =Formula (H), R 3 =Formula (I), R 4 =H, and R 5 =Formula(J) A 2 L four-neck flask equipped with a mechanical stirrer, reflux condenser, and internal thermometer is charged with 37.29 g acrylic acid, 0.073 g methylhydroquinone, 21.13 g n-butanol, 0.887 g 2-(((3-(octyloxy)propyl)imino)methyl)phenol prepared according to EP 3168273, and 0.422 g 50% aqueous chromium(III) acetate solution with stirring. To this is added 666.64 g of a statistically distributed [poly-dimethyl(methyl-,glycidoxypropyl)]siloxane-copolymer with an epoxide oxygen value of 1.08 wt.% and a viscosity of 145 mPa·s at 25°C while heating to 115°C. Stirring at 115-120°C is continued until the conversion of the epoxy groups as determined by the acid value is greater than 99%. All volatile substances are then distilled off with a slight air bleed at 120° C. and a vacuum of 3 mbar. Filtration gives a liquid silicone acrylate with a hydroxyl number of 33.8 mg KOH / g.
[0153] In a 1 L four-neck flask equipped with a mechanical stirrer, a reflux condenser and an internal thermometer, 215.8 g of the silicone acrylate thus prepared are mixed with 77.9 g of acetone, 43.9 g of VESTANAT® EP-DC 1241 and 0.25 g of TIB KAT 716 LA and stirred for 4 hours at 60° C. Distillation at 60° C. and 3 mbar with a slight air bleed gives a brown transparent product having a viscosity of 20004 mPa·s at 25° C.
[0154] S9) Preparation of silicone urethane acrylates according to formula (F), where m1=2, m2=0, m3=0, d1=65, d2=2, d3=2, t=q=0, x1=3, (x2=1 and x3=0) or (x2=1 and x3=0), R=CH3, R 1 =H, R 2 =Formula (H), R 3 =Formula (I), R 4 =H, R 5 = Formula (J), and R A = Formula (K) or (L) In a 1 L four-neck flask equipped with a mechanical stirrer, a reflux condenser and an internal thermometer, 183.6 g of the silicone acrylate prepared in Example S8 are mixed with 60.7 g of acetone, 18.7 g of VESTANAT® EP-DC 1241 and 0.20 g of TIB KAT 716 LA and stirred for 4 hours at 60° C. Distillation at 60° C. and 3 mbar with a slight air bleed gives a brown transparent product with a viscosity of 2146 mPa·s at 25° C.
[0155] Silicone urethane (meth)acrylates are listed in Table 1. Silicone urethane (meth)acrylates according to the invention have lower viscosities than silicone urethane (meth)acrylates not according to the invention.
[0156] [Table 1]
[0157] [Table 2]
[0158] Component (b) - Organic (meth)acrylate (reactive diluent) The organic (meth)acrylates used as component (b) are listed in Table 2.
[0159] [Table 3]
[0160] Component (c) - Silicone (meth)acrylate without urethane groups Component (c1): Silicone (meth)acrylate according to formula (Q) Silicone (meth)acrylates S10, S12, and S13 according to formula (Q) are prepared by prior art methods, for example as described in EP 0 940 422. Silicone (meth)acrylates according to formula (Q) are listed in Table 3.
[0161] [Table 4]
[0162] Component (c2): Silicone (meth)acrylate according to formula (S) The silicone (meth)acrylate according to formula (S) is prepared by a method according to the prior art, for example as disclosed in EP 3168273 or WO 2017187030. The silicone (meth)acrylate according to formula (S) is listed in Table 4.
[0163] [Table 5]
[0164] Preparation of mixtures with organic acrylates Provided that this is acceptable in terms of viscosity, the resulting silicone urethane (meth)acrylate is mixed with an organic acrylate as a reactive diluent while heating and stirring. In the case of low-boiling or heat-sensitive reactive diluents, diluent exchange is carried out immediately after synthesis. This is carried out in each case by adding the amount of organic (meth)acrylate (reactive diluent) required for the desired mixture and distilling off acetone at room temperature under full vacuum. The mixtures according to the invention are shown in Table 5.
[0165] [Table 6]
[0166] Hardening Test UV-curable silicones or their blends were mixed with 2% by weight of the photoinitiator TEGO® A18. 30 g of this mixture was placed on an aluminum lid with a diameter of 5 cm to obtain a layer several millimeters thick. The lid was placed under an 80 W / cm mercury UV lamp from Eltosch. Curing generally occurred within a few seconds. The specimens were left at room temperature for a day, after which they were visually inspected and tested for surface scraping and tackiness. If the specimens were satisfactory in terms of mechanical stability, they were removed from the lid and subjected to manual bending and tearing. The mixtures used for the curing tests are shown in Table 6.
[0167] [Table 7]
[0168] From the results of the curing test, it is clear that the cured composition based on the silicone urethane (meth)acrylate of the present invention has superior properties compared to the composition based on the silicone (meth)acrylate without urethane groups.The cured composition according to the present invention shows a smooth surface and can be bent, while the composition not according to the present invention has either a soft, sticky surface or a wrinkled surface.In addition, the composition not according to the present invention fails the tear test.
[0169] Casting test The mechanical properties of the silicones were evaluated by measuring the cured formulations prepared by casting. Crosslinking occurs by adding 1% by weight of a photoinitiator (TPO-L) and irradiating the composition with a UV lamp or projector. The components of the formulations were weighed out on a balance with an accuracy of ±0.001 g and homogenized in a SpeedMixer at 2300 rpm for 10 minutes. The quantities were set according to the required volume. During mixing, the entire setup is heated to 40° C. The formulations were named FX (X=test number).
[0170] Viscosity (η) measurements of uncured samples were performed on a Malvern Kinexus Lab+ rheometer using a cone-plate geometry (4°) after equilibration at room temperature (RT). The reported values are obtained using a frequency of 10 Hz.
[0171] The cast samples were exposed to UV radiation with a wavelength of 405 nm (2400 mW / cm 2 ) for 2 h. The exposure time was 5 min. The object was then washed in isopropanol for 10 min and placed in a curing station at 80 °C for 2 h (light intensity 18 mW / cm 2 and wavelength 405 nm).
[0172] The mechanical properties of the cured samples were evaluated on a universal testing machine according to DIN EN ISO 527 5A. As used herein, "DIN EN ISO 527 5A" refers to the test conditions of DIN EN ISO 527, as described in Part 1 of said standard, testing specimens having a size and shape corresponding to "5A" as described in Part 2 of said standard. Parameters of interest are Young's modulus (E), tensile strength at break (σ b ), and elongation at break (ε b ).
[0173] Table 7 shows the ingredients, content (%) and mechanical properties of the evaluated formulations.
[0174] [Table 8]
[0175] As can be seen in Table 7, the combination of the silicone urethane (meth)acrylate according to the invention with the silicone (meth)acrylate without urethane groups makes it possible to obtain an elastomeric material that is very elastic and can recover its original shape after deformation. It is also clear that the viscosity and mechanical properties can be easily adjusted as required by simply adjusting the amount of the silicone urethane (meth)acrylate according to the invention, the silicone (meth)acrylate without urethane groups, and the organic (meth)acrylate. Furthermore, it is clear from the comparison of F12 and F14, and F13 and F15 that the composition based on silicone urethane acrylate S1 (having 4 acrylate groups and 4 urethane groups) results in an elastomeric material with better mechanical properties compared to the similar composition based on silicone urethane acrylate S7 (having 2 acrylate groups and 2 urethane groups).
[0176] Additive Manufacturing using Stereolithography (SLA) and Digital Light Processing (DLP) In general, the formulations can be printed using an SLA or DLP printer with a projector with a wavelength of 365-405 nm. In the following example, the formulations are printed using a 15 mW / cm 2 The formulations were processed using a DLP printer (Station 5, Atum3D) equipped with a projector with a light intensity of 1000 and a wavelength of 405 nm. To ensure the flowability of the material while the build platform is moving, the viscosity of the formulation should not exceed 30000 mPa s. Table 8 shows an example of the most important parameters of a print job.
[0177] [Table 9]
[0178] Table 9 shows the formulation of the test specimens according to standard DIN EN ISO 527 5A. The photo package was adapted to the wavelength and light intensity of the printer (photoinitiator: 1-2% by weight, UV-blocker: 0.01-0.05% by weight). After printing, all objects were washed in isopropanol for 10 min and placed in a curing station at 80 °C for 2 h (light intensity: 18 mW / cm2). 2 and wavelength: 405 nm).
[0179] [Table 10]
[0180] As can be seen in Table 9, DLP of formulations containing silicone urethane (meth)acrylates and silicone (meth)acrylates without urethane groups makes it possible to obtain elastomeric materials that are very elastic and can recover their original shape after deformation. F10, F11, F12, and F13 showed that the addition of silicone urethane acrylate (L) to silicone acrylate (S13 or S12) transforms the materials into elastomers (E). From rigid formulations (F1) or flexible formulations (F6, F7, F8, and F9) to rubber-like materials, they are able to recover their initial shape. F10 vs. F11 showed that increasing the content of S1 increases the tensile strength and Young's modulus. These results are similar to those of F12 vs. F13. The printability is improved by the addition of an organic (meth)acrylate (IBOMA). In addition, this monomer has a high glass transition temperature (T g ), which could increase the tensile strength and Young's modulus of the soft (S) sample. Furthermore, from a comparison of F12 and F14, and F13 and F15, it is clear that the composition based on the silicone urethane acrylate S1 (having 4 acrylate groups and 4 urethane groups) results in an elastomeric material with better mechanical properties compared to a similar composition based on the silicone urethane acrylate S7 (having 2 acrylate groups and 2 urethane groups).
[0181] Cycle measurements of printed silicone formulations To demonstrate the suitability of silicone urethane acrylate (S1) for generating elastomeric (E) materials, cyclic measurements were performed to determine the recovery rate of the material after elongation. Table 10 shows the formulation content, viscosity, and mechanical properties of the samples. The samples were printed according to the procedure previously described in the Additive Manufacturing using Stereolithography (SLA) and Digital Light Processing (DLP) section.
[0182] The tensile tests were performed according to the standard DIN EN ISO 527 5A. For comparative purposes, the same test conditions were maintained in the cyclic measurements. In each cycle, the sample was deformed to half of its elongation at break (εb) in Table 10. The procedure was as follows: - For the F16, a maximum force of 11.6N is applied initially. The force is then reduced to 1.1N.
[0183] - For the F17, a maximum force of 5N is applied initially. Then the force is reduced to 0.7N.
[0184] This cycle was repeated 10 times. None of the specimens broke during the cycle measurements. The recovery for each cycle was calculated as follows: Recovery(%)=(ε max -ε min )×100 / ε max In the formula, ε max refers to the maximum elongation observed during each cycle, and ε min refers to the minimum elongation observed during each cycle.
[0185] The results of the cycle measurements are shown in Table 11 and Figure 2. For F16, the recovery is 52% in the first cycle and 44% in the tenth cycle. This behavior shows the plastic and irrecoverable deformation typical of flexible materials (F). Although evident, the yield point is beyond the mechanical curve (left plot) and with each cycle, a displacement occurs that reduces the recovery value, indicating further plastic deformation. In contrast, for F17, the recovery is 89% in the first cycle and 87% in the tenth cycle, with almost no displacement. Elastomeric materials (E) typically do not show a yield point. This shows that the flexible material (F) can be transformed into an elastomeric material (E) by adding S1 to the formulation.
[0186] [Table 11]
[0187] curing kinetics The curing kinetics was evaluated by measuring the cure depth (layer thickness) of the resin exposed to irradiation at different time intervals. The resin thickness (cure depth) is measured using a gauge length with an accuracy of ±1 μm. Placed on a microscope slide, the formulation is irradiated using a projector from a DLP printer (light intensity: 15 mW / cm2). 2 (Wavelength: 405 nm). Remove excess resin and measure thickness.
[0188] Formulations F4, F8, and F12, corresponding to S1, S12, and a mixture of S1 / S12, were compared. Table 12 shows selected formulations from Table 7. The cure time reported is the initial time that the layer is measured, and the cure depth is the amount of thickness that this layer was able to cure to in the time stated.
[0189] [Table 12]
[0190] From Table 12, it is clear that the silicone urethane (meth)acrylate of the present invention provides increased cure depth and decreased cure time (i.e., increased cure speed). Therefore, the silicone urethane (meth)acrylate can be used to facilitate 3D printing methods.
[0191] Table 13 shows the time dependence of cure depth after exposing the resin to UV radiation. The cure time will determine the print speed target.
[0192] [Table 13]
[0193] F4 showed a cure depth of 390 μm in 5 seconds. In the same time interval, F8 has zero cure depth. F8 requires at least 60 seconds to show 73 μm. The cure efficiency of S1 in F4 (very rigid) is better than S12 in F8 (flexible). Compared to F8, the mixture of S1 and S12 in F12 (elastomeric) can reduce the required cure time to 10 seconds and increase the cure depth to 117 μm. By including 10 wt% S1, the cure efficiency is improved and the printing speed can be increased to produce more parts per minute.
[0194] Release Coating Preparation of release coating: The performance test of the synthesis example S1 of the present invention is carried out in the formulation for release coating.Release coating is known from the prior art, especially for its use in adhesive tape or label laminate, on sheet carrier, specifically in the form of adhesive coating therein.
[0195] The formulations for the release coatings are prepared in each case by vigorously mixing 78 g of the silicone urethane acrylate from Synthesis Example S1, 20 g of hexanediol diacrylate, and 2 g of the photoinitiator TEGO® A 18 (Evonik Industries AG, Germany).
[0196] The coating composition thus prepared is applied to a sheet-like carrier, which consists of a 50 cm wide biaxially oriented polypropylene film (BoPP), which has been subjected to a corona pretreatment with a generator power of 1 kW in each case before application of the coating composition. The coating composition is applied at a rate of about 1 g / m2 using a 5-roll coating unit from COATEMA® (Coating Machinery GmbH, Dormagen, Germany). 2 and cured by exposure to UV light from a medium pressure mercury lamp from IST® Metz GmbH (Nuertingen, Germany) under a nitrogen atmosphere with a residual oxygen content of less than 50 ppm at 60 W / cm and a belt speed of 100 m / min.
[0197] The specimens thus coated are subjected to tests for rub-off, peel strength, and residual adhesion.
[0198] Scrub off: The adhesion of the cured coating to the carrier material is checked by rubbing vigorously with a thumb on the coating. If the adhesion is poor, rub-off occurs in the form of a rubbery crumb. Such crumb should not form even with vigorous rubbing. The test is carried out by a trained panel. The results are assessed by classification into a range of 1 to 5, with 1 being very good and 5 being fairly poor adhesion to the carrier material.
[0199] Separation force: The peeling effect for adhesive materials, which are usually in the form of adhesive tapes or labels in industrial applications, is expressed by the peeling force (RF), a low peeling force representing a good peeling effect. The peeling force depends on the quality of the release coating, the adhesive itself and the test conditions. The evaluation of the release coating therefore requires the use of the same adhesive and the same test conditions. To determine the peeling force, the adhesive tape or label laminate is cut to a width of 2.5 cm and then the adhesive side is applied in each case to the silicone coating and subjected to the test. The test is carried out according to test protocol FTM 10 of the FINAT Handbook, 8th Edition, The Hague / NL, 2009, with the modification that the storage is at 40° C. and under pressure. The adhesive tape used is tesa® 7475 (trademark of Tesa SE, Hamburg, Germany). The reported values are average values from 5 measurements and are reported in cN / 2.5 cm.
[0200] Residual adhesive strength: The residual adhesion (RAF) is determined by test protocol FTM 11 of the FINAT Handbook 8th Edition, The Hague / NL, 2009, with the difference that the storage of the test adhesive strip in contact with the silicone is for a period of 1 minute and that the standard surface is an untreated BoPP surface. The adhesive tape used is tesa® 7475 (a trademark of Tesa SE, Hamburg, Germany). The residual adhesion is a measure of the crosslinking of the silicone. If silicone components are present that are unpolymerized and therefore mobile, the residual adhesion value decreases as the proportion of such components increases. The results for the rub-off test, the peel force and the residual adhesion (RAF) are presented in Table 14.
[0201] [Table 14]
[0202] Table 14 clearly shows that example S1 according to the invention allows acceptable peel forces with good adhesion. Adhesion to the substrate is also good.
[0203] Thus, the components prepared according to the invention meet all the important requirements for use in release coatings: by appropriate tailoring to the respective system, they can be used either as adhesive components or as components with medium to high release forces.
Claims
1. at least 3 (meth)acrylate groups, - not more urethane groups than (meth)acrylate groups; A silicone urethane (meth)acrylate having the formula:
2. having m (meth)acrylate groups and n urethane groups; m is an integer of at least 3; n is an integer of at least 2; Here, m≧n. The silicone urethane (meth)acrylate according to claim 1 .
3. Formula (B): X (-Y) p Formula (B) is represented by During the ceremony, X is a p-valent silicone radical; Y is bonded to the silicon atom of the silicone radical, in each case, independently selected from the group consisting of monovalent organic radicals having at least one urethane group and at least one (meth)acrylate group; p is an integer of at least 1 3. The silicone urethane (meth)acrylate according to claim 1 or 2.
4. Formula (C): [R a Y b SiO (4-a-b)/2 formula (C) Including units represented by During the ceremony a is an integer from 0 to 2; b is an integer from 1 to 3; provided that a+b is 1 to 3; R, in each instance, is independently selected from the group consisting of monovalent organic radicals that are free of any urethane groups; Y in each case is independently selected from the group consisting of monovalent organic radicals having at least one urethane group and at least one (meth)acrylate group.
3. The silicone urethane (meth)acrylate according to claim 1 or 2.
5. Formula (A): 【Chemistry 1】 containing the group During the ceremony, Z 1 In either case, CH 3 or H; Z 2 is a divalent organic radical, Z 3 is a (q+1)-valent organic radical, where q is an organic radical which is an integer from 1 to 3; Z 4 In either case, -CH 3 and -H, In the formula, each dotted line represents a covalent bond.
1. A silicone urethane (meth)acrylate comprising:
6. Formula (F): M m1 M UA m2 M A m3 D d1 D UA d2 D A d3 T t Q q Formula (F) is represented by During the ceremony, M=[R 3 SiO 1/2 ]、 M UA =[R 2 (R UA )SiO 1/2 ]、 M A =[R 2 (R A )SiO 1/2 ]、 D=[R 2 SiO 2/2 ]、 D UA =[R(R UA )SiO 2/2 ]、 D A =[R(R A )SiO 2/2 ]、 T=[RSiO 3/2 ]、 Q=[SiO 4/2 ]、 m1 is an integer from 0 to 32; m2 is an integer from 0 to 32; m3 is an integer from 0 to 32, d1 is an integer from 1 to 1000; d2 is an integer from 0 to 10; d3 is an integer from 0 to 10, t is an integer from 0 to 10; q is an integer from 0 to 10; however, m1+m2+m3 is at least 2; m2+d2 is at least 1; During the ceremony, R is independently selected in each case from the group consisting of monovalent organic radicals that do not contain any urethane or (meth)acrylate groups; R UA are independently selected from the group consisting of monovalent organic radicals having at least one (meth)acrylate group and at least one urethane group; R A are each independently selected from the group consisting of monovalent organic radicals having at least one (meth)acrylate group and no urethane group.
3. The silicone urethane (meth)acrylate according to claim 1 or 2.
7. Y is selected from the group consisting of the formulas (M), (N), (O), and (P): 【Chemistry 2-1】 【Chemistry 2-2】 The silicone urethane (meth)acrylate of claim 3, characterized in that it is represented by at least one of the following:
8. 3. A method for preparing the silicone urethane (meth)acrylate of claim 1 or 2, wherein the silicone urethane (meth)acrylate is formed by reacting at least one hydroxy-functional silicone (meth)acrylate with at least one isocyanate-functional urethane (meth)acrylate.
9. 9. The method of claim 8, wherein the hydroxy-functional silicone (meth)acrylate is formed by reacting at least one epoxy-functional silicone with (meth)acrylic acid and / or at least one hydroxy-functional (meth)acrylate.
10. Ingredients below: (a) at least one silicone urethane (meth)acrylate according to claim 1 or 2; (b) optionally, at least one organic (meth)acrylate that does not have any silicon atoms; (c) optionally at least one silicone (meth)acrylate that does not have any urethane groups; (d) optionally, at least one curing catalyst; (e) optionally, at least one additive; (f) optionally, at least one solvent; A composition comprising or consisting of:
11. based on the total weight of components (a)-(f) combined and / or based on the total weight of the composition, - 5 to 100% by weight of at least component (a), - 0 to 60% by weight of at least component (b), - 0 to 95% by weight of at least component (c), - 0 to 5% by weight of component (d), 0 to 20% by weight of component (e), 0 to 10% by weight of component (f) The composition of claim 10 comprising or consisting of:
12. At least one silicone (meth)acrylate of component (c) is represented by formula (Q) and / or at least one silicone (meth)acrylate of component (c) is represented by formula (S), M A m1 D d1 Formula (Q) During the ceremony, M A =[R 2 (R A )SiO 1/2 ]、 D=[R 2 SiO 2/2 ]、 m1 is an integer of 2; d1 is an integer from 1 to 10,000; During the ceremony, R is independently selected in each case from the group consisting of monovalent organic radicals that do not contain any urethane or (meth)acrylate groups; R A are independently selected from the group consisting of monovalent organic radicals having at least one (meth)acrylate group and no urethane groups; M m1 D d1 D A d2 D AC d3 Formula (S) During the ceremony, M=[R 3 SiO 1/2 ]、 D=[R 2 SiO 2/2 ]、 D A =[R(R A )SiO 2/2 ]、 D AC =[R(R AC )SiO 2/2 ]、 During the ceremony, R, m1, and d1 are as defined for formula (Q); d2 is an integer from 1 to 20; d3 is an integer from 0 to 3, R A are independently selected from the group consisting of monovalent organic radicals having at least one (meth)acrylate group and no urethane groups; R AC in each case, independently selected from the group consisting of monovalent organic radicals having at least one carboxylic acid ester group but no (meth)acrylate groups and no urethane groups. The composition according to claim 10 .
13. The composition of claim 10, wherein the composition is curable.
14. 11. A method for preparing the composition of claim 10, comprising: (i) preparing a mixture of component (a) and component (f); (ii) preparing a mixture by adding at least one of components (b)-(e) to the mixture of step (i); (iii) removing said component (f) from said mixture of step (ii); (iv) optionally preparing a mixture by adding at least one of said components (b)-(e) to said mixture of step (iii), if said component was not added in step (ii); 13. A method comprising or consisting of:
15. A release coating, protective film or protective coating obtainable by curing the composition of claim 10, or a 3D printed object obtainable by 3D printing the composition of claim 10.