Method for removing chlorine from waste plastic
A two-step process using a neutralizing agent and copper compound effectively reduces chlorine in waste plastics to refinery-compatible levels by removing 95% or more chlorine, including organic and aromatic forms, addressing the limitations of conventional methods.
Patent Information
- Application Number
- JP2023567178
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-07
- Filing Date
- 2022-09-16
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods struggle to effectively reduce chlorine content in waste plastics to levels suitable for introduction into refinery processes, particularly due to the presence of organic and aromatic chlorine, which are difficult to remove using conventional low-cost neutralizing agents.
A two-step process involving the use of a neutralizing agent followed by a copper compound to react with waste plastics, where the neutralizing agent is mixed with waste plastic at 200 to 320°C and the copper compound is added at 400 to 550°C, effectively removing 95% or more of chlorine, including organic, inorganic, and aromatic forms.
The method significantly reduces chlorine content in waste plastic pyrolysis oil to levels acceptable for refinery processes, achieving less than 100 ppm total chlorine, with organic, inorganic, and aromatic chlorine reduced to low levels.
Smart Images

Figure 2024535964000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for removing chlorine from waste plastics. [Background technology]
[0002] Oil (waste oil) generated by cracking and pyrolysis of waste materials such as waste plastic pyrolysis oil contains a large amount of impurities originating from the waste materials. When using it as fuel, it is necessary to reduce the amount of SO x , NO x In particular, there is a problem that the chlorine (Cl) component is converted to HCl during high-temperature processing, which can corrode equipment, and is then discharged.
[0003] Conventionally, Cl was removed by converting it to HCl using the hydrotreating (HDT) process that utilizes refinery technology, but since waste oils such as waste plastic pyrolysis oil contain a high content of Cl, problems have been reported in which the excess HCl generated in the HDT process causes equipment corrosion, abnormal reactions, and deterioration of product properties, making it difficult to introduce waste oil that has not been pretreated into the HDT process. In order to remove Cl oil using the conventional refinery process, a Cl reduction treatment technology for waste oil that reduces the Cl content to a level that can be introduced into the refinery process is required.
[0004] Prior Patent Document 1 (JP 2019-123771 A) discloses a method for treating chlorine-containing plastics by mixing chlorine-containing plastics with a calcium compound in a pyrolysis process, Prior Patent Document 2 (Korean Patent Registration No. 10-1916404 A) discloses an apparatus for recycling a plastic mixture containing polyvinyl chloride, comprising a serially connected auger reactor; a fluidized bed reactor; and a hot filter filled with calcium oxide, Prior Patent Document 3 (JP 2007-246681 A (Patent Application No. 2006-071995 A)) discloses a method for generating fuel gas from a product of room temperature dechlorination of PVC, which comprises mixing PVC with an oxide, crushing the PVC at room temperature (mechanochemical treatment) to dechlorinate the PVC, and then heating the product to a temperature of 250°C or less.
[0005] The methods for treating chlorine-containing plastics described in the prior patent documents 1 to 3 have the advantage of using a common additive / neutralizer such as a low-cost calcium oxide adsorbent to remove a large amount of chlorine caused by PVC in waste plastics, but have the problem that it is difficult to remove aromatic chlorine (aromatic ring-Cl) caused by waste plastics such as PP, PE, and PET to reduce the chlorine content to a level that can be introduced into the refinery process. In addition, with the diversification of uses, the amount of aromatic chlorine caused by coatings, dyes, adhesive components, and polymer polymerization additives in waste plastics has increased, and a technology for removing organic chlorine in aromatic molecules, which is more difficult than removing inorganic chlorine such as HCl or organic chlorine contained in chain molecules, has become important. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention is a technology for reducing the Cl content of waste plastic raw materials to a level that allows them to be introduced into the refinery process, and aims to remove aromatic chlorine from waste plastics, which originates from coatings, dyes, adhesive components, and polymer polymerization additives, to a very low content level. [Means for solving the problem]
[0007] One embodiment of the present invention provides a method for removing chlorine from waste plastic, comprising: a) reacting waste plastic with a neutralizing agent; and b) reacting the product of step a) with a copper compound, wherein 95% or more by weight of chlorine is removed based on the total weight of the waste plastic.
[0008] The waste plastic preferably includes at least one selected from the group consisting of polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC), and polystyrene (PS). The waste plastic contains organic chlorine, inorganic chlorine, and aromatic chlorine, and preferably contains 10 ppm or more of chlorine.
[0009] The neutralizing agent may be an oxide, hydroxide, carbonate, or combination thereof of a metal, preferably the metal is calcium, aluminum, magnesium, zinc, iron, or combination thereof. The neutralizing agent is preferably mixed at a ratio of 0.5 to 20% by weight based on the total weight of the waste plastic.
[0010] The copper compound preferably includes at least one selected from the group consisting of copper metal (Cu), copper oxide (CuO), copper hydroxide (Cu(OH)2), and copper carbonate (CuCO3). The copper compound is preferably mixed in an amount of 0.1 to 20% by weight based on the total weight of the product of step a).
[0011] In the step a), the neutralizing agent is added to the waste plastic in a molar ratio (N M / N Cl In the step b), the copper compound is mixed in a molar ratio (NCu / N Cl ) 1 to 10 are preferably mixed.
[0012] The ratio (A1 / A) of the chlorine content of the product of step a) to the chlorine content (A) of the waste plastic may be 50% or less, and it is preferable that the ratio (A2 / A) of the chlorine content of the product of step b) is 10% or less. It is preferable that the a) step is carried out at a temperature of 200 to 320°C, and the b) step is carried out at a temperature of 400 to 550°C.
[0013] The steps a) and b) are preferably each independently carried out by at least one step selected from the group consisting of the following steps 1) and 2). 1) Pre-treatment step of waste plastic 2) Pyrolysis of waste plastic
[0014] The 1) pretreatment step is preferably carried out in an auger reactor at 200 to 320°C. The pyrolysis step 2) is preferably carried out in a pyrolysis reactor at 400 to 550° C. under a non-oxidizing atmosphere. Effect of the Invention
[0015] The present invention significantly reduces not only the total chlorine content of waste plastic pyrolysis oil, but also the chlorine content contained in organic chlorine and aromatic molecules, thereby producing pyrolysis oil at a level that can be introduced into the refinery process. [Brief description of the drawings]
[0016] [Figure 1a] 1 is a schematic diagram showing the reaction mechanism between chlorine in waste plastics and a neutralizing agent. [Figure 1b] FIG. 1 is a schematic diagram showing the reaction mechanism between organic chlorine and aromatic chlorine in waste plastics and copper compounds. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Unless otherwise defined, all terms (including technical and scientific terms) used herein may be used as commonly understood by those having ordinary skill in the art to which the present invention belongs. Throughout the specification, when a part is described as "comprising" a certain component, this means that it may further include other components, not excluding other components, unless otherwise specified. In addition, the singular form includes the plural form unless otherwise specified in the text.
[0018] In this specification, "A to B" means "A or more and B or less" unless otherwise specified. In addition, "A and / or B" means at least one selected from the group consisting of A and B, unless otherwise specified.
[0019] One embodiment of the present invention provides a method for removing chlorine from waste plastics. The method includes the steps of a) reacting waste plastics with a neutralizing agent, and b) reacting the product of step a) with a copper compound. Thus, the present invention can treat waste plastic raw material to reduce the Cl content to a level that can be introduced into a refinery process.
[0020] The waste plastic may include at least one selected from the group consisting of polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC), and polystyrene (PS). The waste plastic may include organic chlorine (organic Cl), inorganic chlorine (inorganic Cl), and aromatic chlorine (aromatic Cl), and the chlorine content of the waste plastic may be 10 ppm or more, 50 ppm or more, 100 ppm or more, or 100 to 1,000 ppm, but the present invention is not limited thereto. A large amount of impurities originating from the waste plastic are contained in the waste oil generated by the cracking and pyrolysis reaction of the waste plastic, such as the waste plastic pyrolysis oil. In particular, it is necessary to pretreat the waste oil to remove chlorine components such as organic / inorganic chlorine. The waste plastic may be classified into household waste plastic waste and industrial waste plastic waste. Domestic waste plastics are plastics that contain PVC, PS, PET, PBT, etc., other than PE and PP, and in the present invention, it can mean mixed waste plastics containing 3% by weight or more of PVC together with PE and PP. Since the chlorine derived from PVC has a high ratio of organic Cl and inorganic Cl, Cl in domestic waste plastics can be removed with high efficiency even with inexpensive neutralizing agents (Ca-based, Zn-based, Al-based, etc.). Industrial waste plastics are mostly PE / PP, but they have a high organic Cl content due to adhesive or dye components, and in particular a high ratio of Cl (aromatic chlorine) contained in aromatic rings, which makes it difficult to remove with the above-mentioned general low-cost neutralizing agents.
[0021] The present invention is characterized in that it removes 95% by weight or more, 97% by weight or more, 98% by weight or more, or 99% by weight or more of chlorine based on the total weight of chlorine contained in waste plastics derived from waste plastics. For this purpose, it is preferable to remove chlorine contained in aromatic rings.
[0022] Step a) is a step in which waste plastic is reacted with a neutralizing agent, and a large amount of HCl generated during the melting and thermal decomposition process of PVC and other materials can be removed in the form of neutralizing salt. The reaction mechanism is as shown in Figure 1a.
[0023] The neutralizing agent may be an oxide, hydroxide, carbonate, or combination thereof of a metal, and the metal may be calcium, aluminum, magnesium, zinc, iron, or combination thereof. Specifically, the neutralizing agent may be aluminum oxide, calcium oxide, magnesium oxide, zinc oxide, or iron oxide. The neutralizing agent may include a zeolite component, such as E-cat.
[0024] The neutralizing agent may be mixed in a ratio of 0.5 to 20% by weight, 1 to 10% by weight, or 1 to 5% by weight based on the total weight of the waste plastic. In addition, the ... M / N Cl ) 1 to 25, preferably 0.7 to 15, and more preferably 0.5 to 5.
[0025] Meanwhile, the total moles of chlorine (Cl) in the waste plastics may refer to the total moles of chlorine in the waste plastics solid raw material before pretreatment and pyrolysis.
[0026] In the a) chlorine removal step, the chlorine weight ratio (A1 / A) of the product of the a) step to the chlorine content (A) of the waste plastic may be 50% or less, 40% or less, or 20-30%. Chlorine remaining in the waste plastic after the a) step can be effectively removed in the b) step.
[0027] Step b) is a step in which the product of step a) is reacted with a copper compound, and a small amount of organic chlorine and aromatic chlorine that are not removed in step a) can be removed by the copper compound (catalyst), and the reaction mechanism is as shown in FIG. 1b. When the copper compound is used together with the neutralizing agent in step a) or instead of the neutralizing agent, the copper compound reacts first with the chlorine and inorganic chlorine (HCl) located at the end of the hydrocarbon chain in the organic chlorine, and it may be difficult to contact the aromatic chlorine, which is difficult to remove by the neutralizing agent. In addition, the initial thermal decomposition time point when the temperature inside the reactor is raised for pretreatment or thermal decomposition is relatively low (250 to 300°C), and HCl begins to be generated, so it is preferable to remove chlorine preferentially with a neutralizing agent. After that, when the full-scale thermal decomposition process proceeds, the temperature is relatively high and the reaction of removing aromatic chlorine is activated. Therefore, it is effective to first remove organic Cl and inorganic Cl as HCl using a neutralizing agent, and then remove aromatic chlorine with a copper compound.
[0028] The copper compound may include at least one selected from the group consisting of copper metal (Cu), copper oxide (CuO), copper hydroxide (Cu(OH)2), and copper carbonate (CuCO3), and may preferably include copper metal (Cu) and / or copper oxide (CuO).
[0029] The copper compound may be mixed at a ratio of 0.1 to 20% by weight, 0.5 to 10% by weight, or 1 to 5% by weight based on the total weight of the product of step a). ... In addition, the copper compound may be mixed at a ratio of 0.1 to 20% by weight, 0.5 to 10% by weight, or 1 to 5% by weight based on the total weight of the product of step a) based on the molar ratio (N Cu / N Cl ) 1 to 10, preferably 0.7 to 5, and more preferably 0.5 to 3.
[0030] Meanwhile, the total moles of chlorine (Cl) in the waste plastics may refer to the total moles of chlorine in the waste plastics solid raw material before pretreatment and pyrolysis.
[0031] In the b) chlorine removal step, the ratio (A2 / A) of the chlorine content of the product of the b) step to the chlorine content of the waste plastic (100% by weight) (A) may be 10% or less, 5% or less, or 0.5 to 3%.
[0032] In the method for removing chlorine from waste plastics according to one embodiment of the present invention, the step a) may be carried out at a temperature of 200 to 320° C., and the step b) may be carried out at a temperature of 400 to 550° C. When steps a) and b) are carried out within the above respective temperature ranges, chlorine in the waste plastics can be effectively removed.
[0033] In a method for removing chlorine from waste plastic according to one embodiment of the present invention, the steps a) and b) may each be independently carried out by at least one step selected from the group consisting of the following steps 1) and 2). 1) Pre-treatment step of waste plastic 2) Pyrolysis of waste plastic
[0034] In the present invention, the 1) pretreatment step of the waste plastic may further include a step of feeding the waste plastic into a screw reactor and pulverizing the waste plastic at room temperature. The pulverization of the waste plastic may be performed by applying a pulverization process known in the art, for example, feeding the waste plastic into a pretreatment reactor and heating it to about 300° C. to produce a pellet-shaped precursor of a hydrocarbon flow, but the present invention is not limited thereto.
[0035] As an example, the pulverization process may involve mixing the waste plastic and a neutralizing agent and feeding them into a reactor. When the waste plastic is mixed with calcium oxide or the like as the neutralizing agent and pulverized at room temperature, a mechanochemical reaction occurs to generate hydrocarbons and CaOHCl. This has the effect of stably fixing the chlorine in the waste plastic raw material to CaOHCl.
[0036] Next, the 1) waste plastic pretreatment step is characterized by feeding the pulverized waste plastic into a pretreatment reactor and heating it, and the solid waste plastic raw material may be physicochemically treated to remove chlorine and produce a precursor of a hydrocarbon stream (pyrolysis raw material). The precursor of a hydrocarbon stream means a molten waste plastic, and the molten waste plastic may mean a pulverized or unpulverized solid waste plastic that is entirely or partially converted into liquid waste plastic.
[0037] As an example, the 1) waste plastic pretreatment step may include heating the crushed or uncrushed waste plastic and the neutralizing agent in a reactor. The pretreatment step may include heating the crushed or uncrushed waste plastic and the neutralizing agent in a reactor, and then heating the first pretreatment step. The copper compound may then be added to the reactor to perform a second pretreatment step.
[0038] The heating may be performed at a temperature of 200 to 320° C. under normal pressure conditions, and is preferably performed at a temperature of 250 to 320° C., or 280 to 300° C. In general, the pretreatment temperature for waste plastics is at least 250° C., but the above-mentioned dechlorinated hydrocarbons can be easily pretreated at a lower temperature of 200° C. to generate hydrogen or methane gas.
[0039] The pretreatment reactor may be an extruder, an autoclave reactor, a batch reactor, or the like, and may be an auger reactor, for example, but the present invention is not limited thereto.
[0040] The 2) waste plastic pyrolysis step involves feeding pyrolysis raw materials, which are classified into three material phases, namely, gas phase, liquid phase (oil + wax + water), and solid phase, into a reactor. Specifically, this is a process in which the non-pretreated or pretreated waste plastic is fed into a pyrolysis reactor and heated to produce waste plastic pyrolysis oil.
[0041] As an example, the pyrolysis step may be a step of mixing pretreated waste plastic with a copper compound, feeding the mixture into a reactor and heating the reactor to produce pyrolysis oil. The pyrolysis process may be a step of performing a first pyrolysis in which waste plastic is mixed with a neutralizing agent, feeding the mixture into a reactor and heating the reactor to produce pyrolysis oil, and then performing a second pyrolysis in which a copper compound is fed into the reactor and heated, and at least two pyrolysis steps may be performed continuously or discontinuously.
[0042] The heating may be performed in a non-oxidizing atmosphere at a temperature of 320 to 900° C., preferably 350 to 700° C., and more preferably 400 to 550° C. The heating may be performed at normal pressure. The non-oxidizing atmosphere is an atmosphere in which the waste plastic is not oxidized (burned), and may be, for example, an atmosphere in which the oxygen concentration is adjusted to 1% by volume or less, or an inert gas atmosphere such as nitrogen, water vapor, carbon dioxide, or argon.
[0043] If the heating temperature is 400°C or higher, it is possible to prevent fusion of chlorine-containing plastics. On the other hand, if the heating temperature is 550°C or lower, the chlorine in the waste plastics may remain in the pyrolysis char in the form of CaCl2, CuCl2, etc.
[0044] The pyrolysis step may further include a gas recovery step of recovering pyrolysis gas, and a separation step of separating the pyrolysis solids into fine particles and coarse particles. In the gas recovery step, pyrolysis gas containing low boiling point hydrocarbon compounds such as methane (CH4), ethane (C2H6), and propane (C3H8) is recovered from the gas phase generated in the pyrolysis step. The pyrolysis gas generally contains combustible substances such as hydrogen, carbon monoxide, and low molecular weight hydrocarbon compounds. Examples of the hydrocarbon compounds include methane, ethane, ethylene, propane, propene, butane, and butene. Such pyrolysis gas can be used as fuel because it contains combustible substances.
[0045] In the separation process, the solid phase generated in the pyrolysis process, such as the carbide and the neutralizing agent and / or the copper compound, is separated into fine particles and coarse particles. Specifically, the solid phase generated in the pyrolysis reaction can be separated into fine particles and coarse particles by classifying the solid phase using a sieve that is smaller than the average particle size of the chlorine-containing plastic and larger than the average particle size of the neutralizing agent and the copper compound. In the separation process, the solid phase is preferably separated into fine particles containing a relatively large amount of the chlorine-containing neutralizing agent and the copper compound, and coarse particles containing a relatively large amount of the carbide. The fine particles and the carbide may be reprocessed as necessary, reused in the pyrolysis process, used as fuel, or discarded, but the present invention is not limited thereto.
[0046] The pyrolysis process may be carried out in an autoclave reactor, a batch stirred reactor, a fluidized-bed reactor, a packed-bed reactor, or the like, and may be applied to any reactor capable of controlling stirring and temperature rise. In the present invention, the pyrolysis process may be carried out in a batch reactor, but is not limited thereto.
[0047] The pyrolysis oil produced by the method for removing chlorine from waste plastic according to one embodiment of the present invention has a chlorine content of 100 ppm or less, 70 ppm or less, 65 ppm or less, 60 ppm or less, 50 ppm or less, or 35 ppm or less, and in particular, an organic chlorine content of 50 ppm or less, 30 ppm or less, 20 ppm or less, 15 ppm or less, or 10 ppm or less, an inorganic chlorine content of 30 ppm or less, 15 ppm or less, or 10 ppm or less, and an aromatic chlorine content of 20 ppm or less, 10 ppm or less, 5 ppm or less, or 3 ppm or less, based on the total weight. Therefore, it is possible to produce pyrolysis oil at a level that can be introduced into the refinery process from waste plastics containing a high Cl content.
[0048] Meanwhile, the organic chlorine content, inorganic chlorine content, or aromatic chlorine content may refer to the chlorine content contained in an organic substance, the chlorine content contained in an inorganic substance, or the chlorine content contained in an aromatic ring of an aromatic compound, respectively.
[0049] Preferred examples and comparative examples of the present invention will be described below. However, the following examples are merely preferred examples of the present invention, and the present invention is not limited to the following examples.
[0050] [Example] (Example 1-1) 200g of industrial waste plastic feed was fed into the feed injection section and screw crushing was performed. 200g / hr of crushed waste plastic and 10wt% CaO were fed into the auger reactor, and pretreatment was performed under the following conditions: screw speed 10rpm, nitrogen flow rate 3cc / min, 300℃, residence time 1hr.
[0051] The pretreated waste plastic and 5 wt% CuO were put into a batch pyrolysis reactor and pyrolysis was carried out at 500°C. The pyrolysis gas was collected through a condenser, and then pyrolysis oil was obtained through a recovery section. In this case, the majority of the industrial waste plastic was PE / PP waste vinyl from duty-free shops, and the total Cl content was 853 ppm.
[0052] (Example 1-2) The same procedure as in Example 1-1 was carried out, except that 5 wt % Cu (1.0 mm copper wire) was used instead of 5 wt % CuO.
[0053] (Comparative Example 1-1) A pyrolysis oil was obtained in the same manner as in Example 1-1, except that no pretreatment was performed and no CuO was added during pyrolysis.
[0054] (Comparative Example 1-2) A pyrolysis oil was obtained in the same manner as in Example 1-1, except that CaO was not added during the pretreatment and CuO was not added during the pyrolysis.
[0055] (Comparative Example 1-3) A pyrolysis oil was obtained in the same manner as in Example 1-1, except that E-cat was added instead of CaO during pretreatment and CuO was not added during pyrolysis.
[0056] (Comparative Examples 1-4) A pyrolysis oil was obtained in the same manner as in Example 1-1, except that CaO was not added during pretreatment and CaO was used instead of CuO during pyrolysis.
[0057] (Comparative Examples 1-5) A pyrolysis oil was obtained in the same manner as in Example 1-1, except that CuO was added instead of CaO during pretreatment and CaO was used instead of CuO during pyrolysis.
[0058] (Example 2-1) The same procedure as in Example 1-1 was carried out, except that a household waste plastic feed was used instead of an industrial waste plastic feed.
[0059] The composition of the household waste plastics was 77-80wt% PP, 17-20wt% PE, and 0-6wt% soft PVC (plasticizer + PVC). The total Cl content in the waste PP was 444ppm, the total Cl content in the waste PE was 694ppm, the total Cl content in the waste soft PVC was 243,000ppm, and the total Cl content in the household waste plastics was 8,100ppm.
[0060] (Example 2-2) A pyrolysis oil was obtained in the same manner as in Example 1-2, except that the household waste plastic feed of Example 2-1 was used instead of the industrial waste plastic feed.
[0061] (Comparative Examples 2-1 to 2-5) Pyrolysis oil was obtained in the same manner as in Comparative Examples 1-1 to 1-5, except that the domestic waste plastic feed of Example 2-1 was used instead of the industrial waste plastic feed.
[0062] [Evaluation example]: Evaluation of chlorine content of pyrolysis oil The Cl content of the pyrolysis oils obtained in Examples 1-1, 1-2, 2-1, and 2-2 and Comparative Examples 1-1 to 1-5 and 2-1 to 2-5 was measured and is shown in Table 1 below.
[0063] [Table 1]
[0064] Referring to Table 1, it can be seen from the examples that using CaO during pretreatment and using a copper compound (Cu / CuO) during pyrolysis is more effective in removing aromatic Cl. This result is understood to be due to the fact that at the pyrolysis temperature of 500°C, the reaction between aromatic Cl and copper compounds occurs more actively than between chlorine located at the end of the hydrocarbon chain in organic chlorine and inorganic chlorine (HCl).
[0065] In Example 1-1, it was confirmed that by implementing all the components of the present invention, not only the total Cl content of the pyrolysis oil but also the organic Cl content can be significantly reduced. In contrast, in Comparative Example 1-1, HCl is removed as oil vapor by a simple pyrolysis reaction, so the chlorine content removed is insufficient, and in Comparative Example 1-2, pyrolysis is performed after simple pretreatment in an auger reactor without using a neutralizing agent before pyrolysis, so the chlorine removal rate is better than in Comparative Example 1-1, but it is still not a product of a level that can be introduced into the refinery process. In Comparative Examples 1-3 and 1-4, CaO or E-cat was used instead of the copper compound, but the pyrolysis oil produced contains a relatively high content of organic Cl. It is understood that such results are due to the inability to sufficiently remove aromatic Cl during pyrolysis.
[0066] In Example 2-1, it was confirmed that, even in the pyrolysis of household waste plastics with a high organic Cl content in the feed, by implementing all the components of the present invention, not only the total Cl content of the pyrolysis oil but also the organic Cl content can be reduced to a significantly low content. In Comparative Example 2-1, it was confirmed that only about 70% of the total Cl in the feed can be removed by a simple pyrolysis reaction. In Comparative Example 2-2, it was confirmed that it is possible to reduce Cl to about 94% by simple pretreatment without using a neutralizing agent in an auger reactor before pyrolysis. However, in Comparative Examples 2-1 and 2-2, pyrolysis oil at a level that can be introduced into the refinery process was not obtained. In Comparative Examples 2-3 and 2-4, CaO or E-cat, which are commonly used additives, was used, but the total Cl was higher than in Comparative Example 2-2.
[0067] Comparative Examples 1-5 and 2-5 show higher organic Cl contents than Examples 1-1 and 2-1. This result is understood to be due to the fact that a large amount of inorganic Cl and organic Cl were removed by first treating a feed with a high chlorine content with CuO, but it is difficult to effectively remove aromatic Cl with the CaO neutralizing agent added during pyrolysis, so a relatively large amount of organic Cl remains. Therefore, in order to remove aromatic Cl from waste oil, it is important to contact aromatic chlorine and the like with a copper compound, and for this purpose, it was found that it is preferable to first remove a large amount of organic chlorine and inorganic chlorine with a low-cost neutralizing agent.
[0068] Although the embodiments of the present invention have been described above, the present invention is not limited to the above embodiments, and may be manufactured in various different forms, and a person having ordinary skill in the art to which the present invention belongs can understand that the present invention can be embodied in other specific forms without changing the technical idea or essential features of the present invention. Therefore, it should be understood that the embodiments described above are illustrative in all respects and are not limiting.
Claims
1. a) reacting waste plastic with a neutralizing agent; b) reacting the product of step a) with a copper compound; Including, A method for removing chlorine from waste plastics, characterized in that 95% by weight or more of chlorine is removed based on the total weight of the waste plastics.
2. 2. The method for removing chlorine from waste plastics according to claim 1, wherein the waste plastics include at least one selected from the group consisting of polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyvinyl chloride (PVC), and polystyrene (PS).
3. The method for removing chlorine from waste plastics according to claim 1 , wherein the waste plastics contain organic chlorine, inorganic chlorine, and aromatic chlorine, and contain 10 ppm or more of chlorine.
4. the neutralizing agent is a metal oxide, hydroxide, carbonate, or a combination thereof; The method for removing chlorine from waste plastics according to claim 1 , wherein the metal is calcium, aluminum, magnesium, zinc, iron, or a combination thereof.
5. The method for removing chlorine from waste plastics according to claim 1, wherein the neutralizing agent is mixed in an amount of 0.5 to 20% by weight based on the total weight of the waste plastics.
6. The copper compounds include copper metal (Cu), copper oxide (CuO), copper hydroxide (Cu(OH) 2 ), and copper carbonate (CuCO 3 The method for removing chlorine from waste plastics according to claim 1, comprising at least one selected from the group consisting of:
7. The method for removing chlorine from waste plastics according to claim 1, wherein the copper compound is mixed in an amount of 0.1 to 20% by weight based on the total weight of the product of step a).
8. In the step a), the neutralizing agent is added to the waste plastic in such a manner that the molar ratio of the total chlorine element (Cl) in the waste plastic to the metal element (M) in the neutralizing agent (N M / N Cl ) 1 to 25 are mixed, In the step b), the copper compound is mixed with the waste plastic in a molar ratio (N Cu / N Cl 2. The method for removing chlorine from waste plastics according to claim 1, wherein the mixture is mixed in an amount of 1 to 10.
9. Based on 100% by weight (A) of the chlorine content of the waste plastic, The ratio of the chlorine content of the product of the step a) (A 1 / A) is 50% or less, The ratio of the chlorine content of the product of the step b) (A 2 2. The method for removing chlorine from waste plastics according to claim 1, wherein the ratio of the chlorine content to the total chlorine content is 10% or less.
10. The method for removing chlorine from waste plastics according to claim 1, wherein the step a) is carried out at a temperature of 200 to 320°C, and the step b) is carried out at a temperature of 400 to 550°C.
11. The method for removing chlorine from waste plastics according to claim 1, wherein the steps a) and b) are each independently carried out by at least one step selected from the group consisting of the following steps 1) and 2). 1) Pretreatment step of waste plastic 2) Pyrolysis of waste plastic
12. The method for removing chlorine from waste plastics according to claim 11, wherein the pretreatment step 1) is carried out in an auger reactor at 200 to 320°C.
13. The method for removing chlorine from waste plastics according to claim 11, wherein the 2) pyrolysis step is carried out in a pyrolysis reactor at 400 to 550° C. under a non-oxidizing atmosphere.