Composition for sealing organic light-emitting element and organic light-emitting element display device including organic layer produced therefrom

A composition with (meth)allylic and (meth)acrylate photocurable monomers and a photocurable monomer of chemical formula 4 addresses the issues of high plasma etching rate and dielectric constant in OLED encapsulation, ensuring uniformity and reliability through inkjet application.

JP2024535979APending Publication Date: 2024-10-04SAMSUNG SDI CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024502036
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-04-20
Filing Date
2022-05-16
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing encapsulation compositions for organic light-emitting devices (OLEDs) face challenges in achieving a low plasma etching rate, high dielectric constant, and poor inkjet properties, leading to potential damage and malfunction due to external factors and stacking effects.

Method used

A composition comprising a (meth)allylic photocurable monomer, a (meth)acrylate photocurable monomer, and a photocurable monomer of specific chemical formula 4, with a balanced ratio, forms an organic layer with low plasma etching rate and dielectric constant, ensuring uniformity and reliability through inkjet application.

Benefits of technology

The composition achieves an organic layer with a low plasma etching rate, low dielectric constant, and excellent inkjet properties, minimizing wrinkles and enhancing the reliability of OLEDs by forming a highly reliable sealing layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024535979000001_ABST
    Figure 2024535979000001_ABST
Patent Text Reader

Abstract

The present invention provides a composition for sealing an organic light-emitting device, the composition including an allyl-based photocurable monomer, a (meth)acrylate-based photocurable monomer, a photocurable monomer of Chemical Formula 4, and a photoinitiator, wherein the sum of the allyl-based photocurable monomer and the (meth)acrylate-based photocurable monomer is greater than the photocurable monomer of Chemical Formula 4, by weight, and an organic layer formed therefrom.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for sealing an organic light emitting device and an organic light emitting device display device including an organic layer manufactured using the composition. More particularly, the present invention relates to a composition for sealing an organic light emitting device, which can realize an organic layer having a low plasma etching rate after curing and a low dielectric constant (permittivity, ε), and has excellent ink jetting properties, and an organic light emitting device display device including the organic layer manufactured using the composition. [Background technology]

[0002] When external moisture, oxygen, etc. penetrate into an organic light-emitting element, the element is easily damaged, and its function may be lost, resulting in a decrease in reliability. Therefore, the organic light-emitting element needs to be sealed with a sealing layer including an inorganic layer (a laminate of an organic layer and an inorganic layer) in addition to an organic layer formed from a composition for sealing an organic light-emitting element.

[0003] The organic layer can be formed by applying a composition for sealing an organic light-emitting device to a predetermined thickness and then curing it. In recent years, an ink jet method has been considered as a method for applying a composition for sealing an organic light-emitting device. In the ink jet method, a composition for sealing an organic light-emitting device is placed in a nozzle and then dropped at a predetermined temperature and dropping speed.

[0004] Meanwhile, in an organic light emitting diode display device, in addition to an encapsulation layer, various display elements are additionally stacked on the upper and lower parts of the organic light emitting element. However, various electricity, static electricity, or electromagnetic waves emitted from the display elements may affect the organic light emitting element. The various electricity, static electricity, or electromagnetic waves emitted from the display elements may cause the organic light emitting element to malfunction or cancel its function. Therefore, it is necessary to have a basic function of encapsulating the organic light emitting element, while having a low dielectric constant and minimizing the effect even when additional elements are stacked on the organic light emitting element.

[0005] There are already known methods to lower the dielectric constant, but most of them are applied to semiconductor devices and are not suitable for processes such as inkjet coating for sealing organic light emitting devices and low-temperature photocuring, which is a manufacturing process for OLED panels.

[0006] The background art of the present invention is described in Korean Patent Publication No. 10-2016-0150255 and the like. Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a composition for sealing an organic light emitting device which realizes an organic layer having a low plasma etching rate and a low dielectric constant.

[0008] Another object of the present invention is to provide a composition for sealing an organic light emitting device, which has excellent ink jetting properties and realizes an organic layer having a uniform surface.

[0009] Another object of the present invention is to provide a composition for sealing an organic light emitting device, which can form an organic layer having excellent reliability by minimizing the occurrence of wrinkles in the organic layer even when an inorganic layer is repeatedly formed by chemical vapor deposition (CVD). [Means for solving the problem]

[0010] One aspect of the present invention is a composition for sealing an organic light-emitting device.

[0011] The composition for sealing an organic light-emitting element includes a (meth)allyl-based photocurable monomer, a (meth)acrylate-based photocurable monomer, a photocurable monomer of the following chemical formula 4, and a photoinitiator, and the sum of the (meth)allyl-based photocurable monomer and the (meth)acrylate-based photocurable monomer is greater than the photocurable monomer of the following chemical formula 4 by weight:

[0012] [ka]

[0013] (In the above Chemical Formula 4, R 1 is hydrogen or a methyl group, R 2 , R 3 , R 4 , R 5 , R 6 are each independently a hydrogen atom, a linear or branched, substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or a substituted or unsubstituted arylalkyl group having 7 to 20 carbon atoms; R 2 , R 3 , R 4 , R 5 , R 6 may each independently have one of an epoxy group, a urethane group, and an alkoxy group at its terminal.

[0014] The organic light-emitting element display device of the present invention includes an organic layer formed from the composition for sealing an organic light-emitting element of the present invention. Effect of the Invention

[0015] The present invention provides a composition for sealing an organic light emitting device that realizes an organic layer having a low plasma etching rate and a low dielectric constant.

[0016] The present invention provides a composition for sealing an organic light-emitting device, which has excellent ink-jetting properties and realizes an organic layer with a uniform surface.

[0017] The present invention provides a composition for sealing an organic light emitting device that can form an organic layer having excellent reliability by minimizing the occurrence of wrinkles in the organic layer despite repeated formation of inorganic layers by CVD. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a cross-sectional view of an organic light-emitting display device according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of an organic light-emitting display device according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] [Best Mode for Carrying Out the Invention] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings, in which: FIG.

[0020] In order to clearly explain the present invention in the drawings, parts that are not relevant to the explanation are omitted, and the same or similar components are given the same reference numerals throughout the specification. The length and size of each component in the drawings are for explaining the present invention, and the present invention is not limited to the length and size of each component shown in the drawings.

[0021] As used herein, "(meth)allyl" can mean allyl and / or methallyl.

[0022] As used herein, "(meth)acrylic" can mean acrylic and / or methacrylic.

[0023] In this specification, unless otherwise defined, "substituted" may mean that one or more hydrogen atoms of the functional group of the present invention are substituted with a halogen (F, Cl, Br or I), a hydroxy group, a nitro group, a cyano group, an imino group (=NH, =NR, and R are alkyl groups having 1 to 10 carbon atoms), an amino group (-NH, -NH(R'), -N(R"(R"'), R', R", and R"' are each independently alkyl groups having 1 to 10 carbon atoms), an amidino group, a hydrazine or hydrazone group, a carboxy group, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, a cycloalkyl group having 3 to 30 carbon atoms, a heteroaryl group having 3 to 30 carbon atoms, or a heterocycloalkyl group having 2 to 30 carbon atoms.

[0024] When describing a numerical range in this specification, "X to Y" means X or more and Y or less (X≦and ≦Y).

[0025] The composition for sealing an organic light emitting device (hereinafter, also referred to as "composition") according to an embodiment of the present invention can realize an organic layer having a low plasma etching rate and a low dielectric constant.

[0026] In one embodiment, the composition of the present invention may realize an organic layer having an etching rate of 6.5% or less, specifically 0% to 6.5%, by plasma after curing, as shown in the following formula 1. In this range, the organic layer is not damaged when forming an inorganic layer on the organic layer, thereby extending the life of the organic light emitting device:

[0027]

number

[0028] (In the above formula 1, T1 is a time series in which the composition is evaporated onto a silicon (Si) wafer and exposed to 100 mW / cm 2 The initial thickness of the organic layer obtained by photocuring with UV irradiation for 20 seconds (T1, unit: μm) T2 is the thickness of the organic layer after inductively coupled plasma treatment under the following conditions: ICP power: 2500 W, RE power: 300 W, DC bias: 200 V, Ar flow: 50 sccm, etching time: 1 min, pressure: 10 mtorr (T2, unit: μm).

[0029] The thickness (or height) of the organic layer can be measured by, but is not limited to, FE-SEM (Hitachi High Technologies Corporation).

[0030] In one embodiment, the composition of the present invention may have a dielectric constant of 3.2 or less, specifically 1.5 to 3.2, more specifically 2 to 3.15 after curing. In this range, the composition is not affected by external static electricity or electricity, and the performance of the organic light-emitting device can be well realized. In particular, the composition of the present invention forms an organic layer that is laminated alternately with an inorganic layer, which will be described in detail below. In such an alternating laminate structure, in order to form an organic layer that has plasma resistance while ensuring a low dielectric constant, the composition of the present invention is designed to have a dielectric constant of 3.2 or less after curing.

[0031] The composition of the present invention has excellent inkjet jetting properties and can form an organic layer with a uniform surface. The inkjet method is a method in which a composition for sealing an organic light-emitting element is placed in a nozzle and then dropped at a predetermined temperature and dropping speed.

[0032] The composition of the present invention can form an organic layer with excellent reliability by minimizing the occurrence of wrinkles even when the inorganic layer is repeatedly deposited. In general, an organic light emitting device sealing layer can seal an organic light emitting device by repeatedly forming an organic layer and an inorganic layer. The inorganic layer can be formed by chemical vapor deposition (CVD), without being particularly limited. The present invention provides a composition for sealing an organic light emitting device that can form an organic layer with excellent reliability by minimizing the occurrence of wrinkles in the organic layer despite the repeated formation of an inorganic layer by CVD. To this end, the organic layer can have a pencil hardness of 3H or more, for example, 3H to 6H.

[0033] The composition of the present invention includes a (meth)allyl-based photocurable monomer (A), a (meth)acrylate-based photocurable monomer (B), a photocurable monomer (C) of Chemical Formula 4, and a photoinitiator (D). On a weight basis, the sum of the (meth)allyl-based photocurable monomer (A) and the (meth)acrylate-based photocurable monomer (B) is greater than the photocurable monomer (C) of Chemical Formula 4.

[0034] The composition of the present invention has a relationship of (A)+(B)>(C) in the amount of the content, and therefore, even if it is a solvent-free composition, the composition can have excellent inkjet jetting properties. This relationship allows some components in the composition, particularly component (C), to dissolve well in (A) and (B). If the inkjet jetting properties are poor, when the composition is inkjet-jetted, the droplets of the composition do not completely expand from their spherical shape, and an organic layer cannot be formed well. In addition, by satisfying the above relationship, an organic layer having a low plasma etching rate and dielectric constant and excellent strength can be easily realized.

[0035] In one embodiment, the ratio of (A)+(B) to (C) can be 2 to 10, specifically, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, for example, 2 to 9. Within this range, the effects of the present invention can be easily realized.

[0036] Each component in the composition of one embodiment of the present invention will be described in detail below.

[0037] (Meth)allyl-based photocurable monomers The (meth)allyl-based photocurable monomer has one or more, preferably 1 to 3, (meth)allyl groups, and can form an organic layer by being cured with a photoinitiator described in detail below.

[0038] The (meth)allylic photocurable monomer may have a nitrogen-containing ring structure. The (meth)allylic photocurable monomer having a nitrogen-containing ring structure may be combined with the photocurable monomer of formula 4 described below to help form an organic layer with a significantly lower dielectric constant and a lower plasma etching rate.

[0039] The nitrogen-containing ring structure may include an alicyclic ring structure formed of one or more nitrogens and carbons. In one specific example, the ring structure may include an alicyclic ring structure having 3 to 10 carbon atoms forming the ring structure, which is a single ring or a heterocyclic ring. Preferably, the ring structure has two or more, for example, two to three carbonyl groups (-C=O-), which may make it easier to realize the effects of the present invention.

[0040] In one embodiment, the nitrogen-containing ring structure may include one or more of an isocyanurate group, a piperidine group, a piperidinone group, a piperidinedione group, a pyrrolidine group, a pyrrolidinedione group, a pyridine group, an indole group, an at least partially hydrogenated indole group, an indoledione group, an at least partially hydrogenated isoindoledione group, a pyridinedione group, and a pyrroledione group. Preferably, the nitrogen-containing ring structure may be an isocyanurate group.

[0041] In one embodiment, the (meth)allylic photocurable monomer may include one or more of the following formula 1 and formula 2:

[0042] [ka]

[0043] (In the above Chemical Formula 1, R 1 , R 2 , R 3 respectively represent an allyl group, a methallyl group, hydrogen, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 10 carbon atoms, or a glycidyl group, R 1 , R 2 , R 3 is an allyl or methallyl group).

[0044] [ka]

[0045] (In the above Chemical Formula 2, R 4 is an allyl group or a methallyl group, R 5 is a nitrogen-containing ring-type functional group, R 6 is an allyl group, a methallyl group, hydrogen, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 10 carbon atoms, or a glycidyl group, R 5 and R 6 are linked together to form a substituted or unsubstituted nitrogen-containing ring-type functional group.

[0046] In the above formula 2, R 5 or R 5 and R 6 The nitrogen-containing cyclic functional group formed by linking together may be one or more of a piperidine group, a piperidinone group (including but not limited to the following Chemical Formula 2-1), a piperidinedione group (including but not limited to the following Chemical Formula 2-2), a pyrrolidine group, a pyrrolidinedione group (including but not limited to the following Chemical Formula 2-3), a pyridine group (including but not limited to the following Chemical Formula 2-10), an indole group, an at least partially hydrogenated indole group, an indoledione group, an at least partially hydrogenated isoindoledione group (including but not limited to the following Chemical Formula 2-4, 2-5, 2-8, or 2-9), a pyridinedione group (including but not limited to the following Chemical Formula 2-6), and a pyrroledione group (including but not limited to the following Chemical Formula 2-7).

[0047] [ka]

[0048] [ka]

[0049] (In the above Chemical Formula 2-1 to Chemical Formula 2-10, * represents R 4 (This is the linking site with Preferably, the (meth)allyl-based photocurable monomer may include one or more of the following Chemical Formula 3-1 to Chemical Formula 3-11:

[0050] [ka]

[0051] [ka]

[0052] The (meth)allyl-based photocurable monomer is 40 to 90 parts by weight, specifically, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90 parts by weight, based on 100 parts by weight of the total of (A), (B), and (C). For example, it may be included in an amount of 40 to 80 parts by weight. Within this range, the dielectric constant of an organic layer formed from the composition may be reduced, which may help improve the plasma etching rate.

[0053] (Meth)acrylate-based photocurable monomers The (meth)acrylate-based photocurable monomer has a (meth)acrylate group and can form an organic layer by being cured with a photoinitiator, which will be described in detail below.

[0054] The (meth)acrylate-based photocurable monomer can be a monofunctional (meth)acrylate having one acrylate or methacrylate group. When a multifunctional (meth)acrylate having two or more acrylate or methacrylate groups is combined with a (meth)allyl-based photocurable monomer or a photocurable monomer of Chemical Formula 4 and cured with a photoinitiator, the organic layer becomes too hard, which can cause problems such as cracking and being unsuitable for application in flexible devices. In addition, the hard organic layer can cause cracks and damage the inorganic layer, shortening its lifespan.

[0055] In the composition, the content of the polyfunctional (meth)acrylate having two or more acrylate groups or methacrylate groups can be 0 part by weight to 1 part by weight, preferably 0 part by weight, in 100 parts by weight of the total of (A), (B) and (C), that is, (A)+(B)+(C).

[0056] The (meth)acrylate photocurable monomer can be a mono(meth)acrylate having a substituted or unsubstituted, linear or branched alkyl group having 1 to 30 carbon atoms. Here, the "number of carbon atoms" does not include the carbons in the (meth)acrylate group, but refers to the number of carbon atoms in the alkyl group bonded to the oxygen (O) of the ester group.

[0057] Preferably, the (meth)acrylate photocurable monomer can be a mono(meth)acrylate having a substituted or unsubstituted, linear or branched alkyl group having 10 to 30 carbon atoms, more preferably 12 to 25 carbon atoms.

[0058] When such a mono(meth)acrylate-based photocurable monomer having a long-chain alkyl group is combined with the (meth)allyl-based photocurable monomer of the present invention and the monomer of Chemical Formula 4, the organic layer is not damaged when an inorganic layer is formed on the organic layer, thereby further realizing the effect of extending the life of the organic light-emitting device.

[0059] More preferably, the (meth)acrylate-based photocurable monomer can be a mono(meth)acrylate having a straight-chain or branched-chain alkyl group having 10 to 30 carbon atoms, and further preferably having 12 to 25 carbon atoms, which is unsubstituted or substituted with an alkyl group having 1 to 20 carbon atoms.

[0060] For example, the (meth)acrylate-based photocurable monomer may include, but is not limited to, one or more of 2-propenoic acid 2-decyltetradecyl ester, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, dodecyl-substituted tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, and nonadecyl (meth)acrylate.

[0061] The (meth)acrylate-based photocurable monomer may be included in an amount of 5 parts by weight to 55 parts by weight, specifically 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55 parts by weight, for example, 10 parts by weight to 50 parts by weight, in the total amount (A) + (B) + (C) of (A), (B) and (C) of 100 parts by weight. When the (meth)allyl-based photocurable monomer and the photocurable monomer of Chemical Formula 4 are combined within the above range, the photocurable monomer can be cured by the photoinitiator to form an organic layer, and the organic layer can be prevented from becoming an excessively hard type.

[0062] Photocurable monomer of formula 4 The photocurable monomer of Chemical Formula 4 has a vinyl group and can form an organic layer by being cured with a photoinitiator, which will be described in detail below.

[0063] [ka]

[0064] (In the above Chemical Formula 4, R 1 is hydrogen or a methyl group, R 2 ,R 3 ,R 4 ,R 5 ,R 6 are each independently a hydrogen atom, a linear or branched, substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or a substituted or unsubstituted arylalkyl group having 7 to 20 carbon atoms; R 2 ,R 3 ,R 4 ,R 5 ,R 6 may each independently have one of an epoxy group, a urethane group, and an alkoxy group at its terminal.

[0065] In the above chemical formula 4, the "epoxy group" is

[0066] [ka]

[0067] It could be the same.

[0068] In the above Chemical Formula 4, the "urethane group" can be *-R-(NH)-(C=O)-OR' or *-NH-(C=O)-OR' (* is a linking site to an element, and R and R' are each independently a substituted or unsubstituted alkyl group having 1 to 12 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 18 carbon atoms).

[0069] In the above Chemical Formula 4, the "alkoxy group" can be an alkoxy group having 1 to 10 carbon atoms.

[0070] The photocurable monomer of Chemical Formula 4 has an aromatic group, particularly a benzene group, and thus when combined with a (meth)allyl-based photocurable monomer, it can help form an organic layer with a significantly low dielectric constant and low plasma etching rate. The present inventors have confirmed that by using a (meth)allyl-based photocurable monomer and a photocurable monomer of Chemical Formula 4 together, an organic layer and an organic layer with a significantly low plasma etching rate can be realized, and in this case, by including a (meth)acrylate-based photocurable monomer together and satisfying the relationship of the content (A)+(B)>(C), the curing rate is high and the inkjet jetting property is excellent.

[0071] For example, the photocurable monomer of formula 4 can include one or more of phenylstyrenes, including 4-phenylstyrene, etc.; tert-butylstyrenes, including 4-tert-butylstyrene, etc.; and alpha-methylstyrene.

[0072] In one embodiment, the photocurable monomer of formula 4 may have a boiling point of 90°C to 150°C, specifically 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, for example 90°C to 95°C, and a melting point of -50°C to -10°C, specifically -50°C, -45°C, -40°C, -35°C, -30°C, -25°C, -20°C, -15°C, -10°C, for example -40°C to -20°C. By providing a composition that is liquid at room temperature and has a low viscosity within the above range, the composition of the present invention may be produced in a solvent-free form without causing any problems in the jetting properties of the inkjet. The boiling point and melting point may be measured by a conventional method known to those skilled in the art.

[0073] The photocurable monomer of Chemical Formula 4 may be included in an amount of 5 to 35 parts by weight, specifically 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35 parts by weight, for example 10 to 30 parts by weight, in the total of (A), (B) and (C) (A) + (B) + (C) 100 parts by weight. When combined with a (meth)allyl-based photocurable monomer in the above range, it may help form an organic layer with a significantly low dielectric constant and a low plasma etching rate, and the viscosity of the composition may be low, resulting in excellent inkjet jetting properties.

[0074] The total amount of the (meth)allyl-based photocurable monomer, the (meth)acrylate-based photocurable monomer, and the photocurable monomer of Chemical Formula 4 may be 95 parts by weight or more, for example, 98 parts by weight to 100 parts by weight, for example, 100 parts by weight, based on 100 parts by weight of the total photocurable monomers in the composition.

[0075] Photoinitiators The photoinitiator may include, without limitation, one or more of a general photoradical initiator and a photoacid generator capable of carrying out a photocuring reaction.

[0076] The photoradical initiator may include a triazine type, an acetophenone type, a benzophenone type, a thioxanthone type, a benzoin type, a phosphorus type, an oxime type, or a mixture thereof.

[0077] The photoradical initiator may include a phosphorus-based initiator having a maximum absorption wavelength of 360 nm to 400 nm. When the phosphorus-based initiator is used, the composition of the present invention may exhibit better initiation performance in long wavelength UV (e.g., 300 nm to 400 nm). The phosphorus-based initiator may be ethyl (2,4,6-trimethylbenzoyl) phenylphosphine oxide, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide, 2,4,6-trimethylbenzoyl diphenyl phosphinate, (2,4,6-trimethylbenzoyl) ethoxyphenyl phosphinate, (2,4,6-trimethylbenzoyl) methoxyphenyl phosphinate, bisacylphosphine oxide, methyl (2,4,6-trimethylbenzoyl) phenyl phosphinate, or a mixture thereof. For example, the initiator may be included alone or in a mixture of two or more kinds. The "maximum absorption wavelength" may be measured by a conventional method known to those skilled in the art, or may be a value obtained by referring to a product catalog.

[0078] The photoradical initiator may be included in an amount of 0.01 to 10 parts by weight, specifically 0.01, 0.05, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by weight, for example 1 to 5 parts by weight, relative to a total of 100 parts by weight of the (meth)allyl-based photocurable monomer, the (meth)acrylate-based photocurable monomer, and the photocurable monomer of Chemical Formula 4. Within the above range, the curing rate of the composition is increased, and it is possible to prevent a decrease in light transmittance due to a remaining amount of the initiator remaining.

[0079] The photoacid generator is a compound that, when exposed to light, generates a cationic species to initiate a curing reaction of a cationically polymerizable compound and may include a cationic moiety that absorbs light and an anionic moiety that serves as a source of acid generation.

[0080] The photoacid generator may include one or more of sulfonate-based, sulfonium-based, diazonium salt-based, iodonium salt-based, sulfonium salt-based, phosphonium salt-based, selenium salt-based, oxonium salt-based, ammonium salt-based, and bromide salt-based compounds. For example, the photoacid generator may be N-hydroxynaphthalimide trifluoromethanesulfonate, thio-p-phenylenebis(4,4'-dimethyldiphenylsulfonium)bistetrakis(pentafluorophenyl)borate, (4-hydroxyphenyl)methylbenzylsulfonium tetrakis(pentafluorophenyl)borate, 4-(4-biphenylylthio)phenyl-4-biphenylylphenylsulfonium tetrakis(pentafluorophenyl)borate, 4-(phenylthio)phenyldiphenylsulfonium phenyltris(pentafluorophenyl)borate, [4-(4-biphenylylthio)phenyl]-4-biphenylylphenylsulfonium phenyltris(pentafluorophenyl)borate, diphenyl[4-(phenylthio)phenylsulfonium]hexafluoroantimonium, The sulfonyl group may include, but is not limited to, one or more of the following: diphenyl[4-(phenylthio)phenyl]sulfonium tris(pentafluoroethyl)trifluorophosphate, diphenyl[4-(phenylthio)phenyl]sulfonium tetrakis(pentafluorophenyl)borate, diphenyl[4-(phenylthio)phenyl]sulfonium hexafluorophosphate, 4-(4-biphenylylthio)phenyl-4-biphenylylphenylsulfonium tris(pentafluoroethyl)trifluorophosphate, bis[4-(diphenylsulfonio)phenyl]sulfidophenyltris(pentafluorophenyl)borate, and [4-(2-thioxanthonylthio)phenyl]phenyl-2-thioxanthonylsulfonium phenyltris(pentafluorophenyl)borate.

[0081] Preferably, the photoacid generator may include one or more of N-hydroxynaphthalimide trifluoromethanesulfonate, thio-p-phenylenebis(4,4'-dimethyldiphenylsulfonium)bistetrakis(pentafluorophenyl)borate.

[0082] The photoacid generator may be included in an amount of 0.01 to 5 parts by weight, specifically 0.01, 0.05, 0.1, 0.5, 1, 2, 3, 4, or 5 parts by weight, for example 0.01 to 1 part by weight, based on a total of 100 parts by weight of the (meth)allyl-based photocurable monomer, the (meth)acrylate-based photocurable monomer, and the photocurable monomer of Chemical Formula 4. Within this range, the curing rate is high, and it is possible to prevent a residual amount from remaining and lowering the light transmittance of the organic layer.

[0083] The photoinitiator may be included in an amount of 0.01 to 15 parts by weight, preferably 1 to 5 parts by weight, based on a total of 100 parts by weight of the (meth)allyl-based photocurable monomer, the (meth)acrylate-based photocurable monomer, and the photocurable monomer of Chemical Formula 4. Within this range, the curing rate of the composition is increased, and it is possible to prevent a decrease in light transmittance due to a residual amount of the initiator remaining.

[0084] The composition of the present invention may be formed by mixing a (meth)allyl-based photocurable monomer, a (meth)acrylate-based photocurable monomer, a photocurable monomer of Chemical Formula 4, and a photoinitiator. For example, the composition of the present invention may be formed into a solventless type that does not contain a solvent. The solventless type can reduce the amount of outgassing after forming an organic layer, thereby minimizing the effect on the organic light-emitting device.

[0085] The composition of the present invention is a photocurable composition having a UV wavelength of 10 mW / cm 2 ~500mW / cm 2 The resin is photocured by UV irradiation for 1 to 50 seconds at 80° C., thereby forming a sealing layer.

[0086] The composition of the present invention may further contain conventional additives known to those skilled in the art, including, but not limited to, heat stabilizers, antioxidants, UV absorbers, etc.

[0087] The composition of the present invention may have a viscosity of 7 cps to 100 cps, preferably 7 cps to 60 cps, and more preferably 7 cps to 50 cps at 25±2° C. (23° C. to 27° C.) in the above range, which may help improve the inkjet properties of the sealing composition.

[0088] The composition of the present invention can be used to encapsulate an organic light-emitting device. Specifically, the composition can form an organic layer in an encapsulation structure in which an inorganic layer and an organic layer are formed in that order.

[0089] The composition of the present invention can also be used for sealing device components, particularly display device components, which may be decomposed or become defective due to the permeation of gases or liquids in the surrounding environment, such as atmospheric oxygen and / or moisture and / or water vapor, and chemicals used in processing electronic products. For example, the device components can be, but are not limited to, lighting devices, metal sensor pads, microdisk lasers, electrochromic devices, photochromic devices, microelectromechanical systems, solar cells, integrated circuits, charge-coupled devices, light-emitting polymers, etc.

[0090] The organic light emitting device display device of the present invention may include an organic layer formed from the composition for sealing an organic light emitting device according to an embodiment of the present invention. Specifically, the organic light emitting device display device includes an organic light emitting device, and a barrier stack formed on the organic light emitting device and including an inorganic layer and an organic layer, and the organic layer may be formed from the composition for sealing an organic light emitting device according to an embodiment of the present invention. As a result, the reliability of the organic light emitting device display device may be improved.

[0091] Hereinafter, an organic light emitting diode display device according to an embodiment of the present invention will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view of an organic light emitting diode display device according to an embodiment of the present invention.

[0092] Referring to FIG. 1, an organic light emitting device display 100 includes a substrate 10, an organic light emitting device 20 formed on the substrate 10, and a barrier stack 30 formed on the organic light emitting device 20 and including an inorganic layer 31 and an organic layer 32, the inorganic layer 31 being in contact with the organic light emitting device 20, and the organic layer 32 being formed from a composition for sealing an organic light emitting device according to an embodiment of the present invention.

[0093] The substrate 10 is not particularly limited as long as it is a substrate on which an organic light emitting device can be formed, and may be made of, for example, transparent glass, a plastic sheet, a silicon or metal substrate, or the like.

[0094] The organic light emitting element 20 is a type commonly used in organic light emitting element display devices, and although not shown in FIG. 1, includes a first electrode, a second electrode, and an organic light emitting film formed between the first electrode and the second electrode. The organic light emitting film may be a layer including a hole injection layer, a hole transport layer, a light emitting layer, an electron transport layer, and an electron injection layer stacked in this order, but is not limited thereto.

[0095] The barrier stack 30 includes an organic layer and an inorganic layer, and the organic layer and the inorganic layer have different components constituting each layer, and each layer can realize a function of sealing the organic light emitting device.

[0096] The inorganic layer can complement the effect of the organic layer by being different from the organic layer in composition. For example, the inorganic layer can be a metal, a nonmetal, a compound or alloy between metals, a compound or alloy between nonmetals, an oxide of a metal or a nonmetal, a fluoride of a metal or a nonmetal, a nitride of a metal or a nonmetal, a carbide of a metal or a nonmetal, an oxynitride of a metal or a nonmetal, a boride of a metal or a nonmetal, an oxyboride of a metal or a nonmetal, a silicide of a metal or a nonmetal, or a mixture thereof. The metal or nonmetal can be, but is not limited to, silicon (Si), aluminum (Al), selenium (Se), zinc (Zn), antimony (Sb), indium (In), germanium (Ge), tin (Sn), bismuth (Bi), a transition metal, a lanthanum group metal, etc. Specifically, the inorganic layer can be silicon oxide (SiOx), silicon nitride (SiNx), silicon oxynitride (SiOxNy), ZnSe, ZnO, Sb2O3, AlOx, including Al2O3, In2O3, SnO2, etc.

[0097] The inorganic layer can be deposited by plasma processes, vacuum processes such as sputtering, chemical vapor deposition, plasma enhanced chemical vapor deposition, evaporation, sublimation, electron cyclotron resonance-plasma vapor deposition and combinations thereof.

[0098] When the organic layer is alternately deposited with the inorganic layer, it can ensure the smoothing properties of the inorganic layer and prevent defects in the inorganic layer from being propagated to another inorganic layer.

[0099] The organic layer can be formed by a combination of coating, vapor deposition, curing, etc., of the composition for sealing an organic light-emitting element according to the embodiment of the present invention. For example, the composition for sealing an organic light-emitting element is coated to a thickness of 1 μm to 50 μm, and irradiated with 10 mW / cm 2 ~500mW / cm 2 It can be cured by exposing it to UV light for 1 to 50 seconds.

[0100] The barrier stack includes an organic layer and an inorganic layer, but the total number of the organic layers and the inorganic layers is not limited. The total number of the organic layers and the inorganic layers can be changed depending on the level of permeation resistance to oxygen and / or moisture and / or water vapor and / or chemicals. For example, the total number of the organic layers and the inorganic layers can be 10 layers or less, for example, 2 to 7 layers, and specifically, 7 layers can be formed in the order of inorganic layer / organic layer / inorganic layer / organic layer / inorganic layer / organic layer / inorganic layer.

[0101] The organic and inorganic layers in the barrier stack can be deposited alternately due to the effect on the organic layers produced by the physical properties of the compositions described above, whereby the organic and inorganic layers can complement or enhance the encapsulation effect on the device.

[0102] Hereinafter, an organic light emitting diode display device according to another embodiment of the present invention will be described with reference to Fig. 2. Fig. 2 is a cross-sectional view of an organic light emitting diode display device according to another embodiment of the present invention.

[0103] 2, an organic light emitting device display 200 includes a substrate 10, an organic light emitting device 20 formed on the substrate 10, and a barrier stack 30 formed on the organic light emitting device 20 and including an inorganic layer 31 and an organic layer 32, the inorganic layer 31 sealing an internal space 40 in which the organic light emitting device 20 is accommodated, and the organic layer 32 may be formed of a composition for sealing an organic light emitting device according to an embodiment of the present invention. Except for the fact that the inorganic layer does not contact the organic light emitting device, the organic light emitting device display 200 is substantially the same as the organic light emitting device display of an embodiment of the present invention.

[0104] [Mode for carrying out the invention] The present invention will be described in more detail with reference to the following preferred embodiments, which are merely illustrative of the present invention and should not be construed as limiting the present invention in any way. The specific specifications of the components used in the examples and comparative examples are as follows.

[0105] (A) (Meth)allyl-based photocurable monomer (A1) Triallyl isocyanurate (Aldrich) (A2) 1,3-Diallyl-5-glycidyl isocyanurate (Shikoku) (A3) Diallyl n-propyl isocyanurate (TCI) (A4) Trimethallyl isocyanurate (Aldrich) (B) (Meth)acrylate-based photocurable monomer (B1) 2-Propenonic acid 2-decyltetradecyl ester (Light acrylate, DTD-A, Kyoeisha Chemical) (B2) Dodecyl methacrylate (Sartomer) (C) Photocurable monomer of formula 4 (C1) 4-tert-butylstyrene (TCI) (C2) 4-vinylbiphenyl (4-phenylstyrene, TCI) (D) Photoinitiator (D1) Phosphorus initiator (Irgacure TPO-L, BASF) (D2) Photoacid generator (N-hydroxynaphthalimide trifluoromethanesulfonate, H1136, Miwon Shoji).

[0106] Example 1 50 parts by weight of (A2), 30 parts by weight of (B1), 20 parts by weight of (C1), 4 parts by weight of (D1), and 0.1 parts by weight of (D2) were placed in a 125 ml brown polypropylene bottle and mixed at room temperature using a shaker for 3 hours to prepare a sealing composition.

[0107] Examples 2 to 5 and Comparative Examples 1 to 4 An encapsulating composition was prepared in the same manner as in Example 1, except that the content of each component was changed as shown in the following Table 1 (unit: weight part). In the following Table 1, "-" means that the corresponding component is not included.

[0108] The following physical properties were measured for the compositions produced in the Examples and Comparative Examples, and the results are shown in Table 1.

[0109] (1) Viscosity (unit: cps): The viscosity of the sealing compositions of the examples and comparative examples was measured at 24.8° C. using a viscosity measuring device LV DV-II Pro (Brookfield Corporation) with a spindle number of 40.

[0110] (2) Dielectric constant (no unit): The sealing compositions of the examples and comparative examples were applied to a chromium (Cr) plate in a predetermined thickness, and the dielectric constant was 100 mW / cm 2 The coating was then photocured by irradiating the coating with UV light at 400 V for 10 seconds to form a coating film with a thickness of 8 μm. An aluminum electrode (electrode for measuring the dielectric constant) was vapor-deposited on the coating film, and the dielectric constant was measured at 200 kHz and 25° C. using an impedance measuring device (RDMS-200).

[0111] (3) Inkjet jetting properties: 16 pL (picoliters) of the sealing compositions of the examples and comparative examples were jetted with an inkjet at a drop speed of 2.5 to 4.5 μm / sec and an inkjet head temperature of 25 to 50° C. When the inkjet was jetted, if the drop shape was a precise sphere, it was evaluated as OK, and if it was not a sphere, it was evaluated as NG.

[0112] (4) Pencil hardness: The sealing compositions of the examples and comparative examples were coated on a glass substrate, and the pencil hardness was 100 mW / cm 2 The organic layer specimen is then photocured by irradiating with UV light at 400° for 10 seconds to obtain an organic layer specimen. The pencil hardness of the organic layer specimen was measured. When measuring the pencil hardness, an electric pencil hardness tester (CT-PC2) and Mitsubishi pencils 6B~9H were used. The pencil load on the specimen was 500g, the pencil scratch angle was 45°, and the pencil scratching speed was 48mm / min. If a scratch occurred at least once out of five evaluations, a pencil of the lower pencil hardness level was used for measurement, and the maximum pencil hardness value was the value when no scratches occurred in all five evaluations.

[0113] (5) Plasma etching rate (unit: %): The sealing compositions of the examples and comparative examples were deposited on a silicon (Si) wafer, and etched at 100 mW / cm 2The organic layer was then photocured by irradiating with UV light for 20 seconds at 4000 V, and the initial thickness (T1, unit: μm) of the organic layer obtained by photocuring was measured. The organic layer was treated with inductively coupled plasma using ICP CVD (BMR Technology) under the conditions of ICP power: 2500 W, RE power: 300 W, DC bias: 200 V, Ar flow: 50 sccm, etching time: 1 min, and pressure: 10 mtorr, and the thickness (T2, unit: μm) of the organic layer was measured. The etching rate of the organic layer by plasma was calculated using the following formula 1. The thickness of the organic layer was measured using FE-SEM (Hitachi High Technologies Corporation). The lower the value of formula 1, the better the plasma resistance.

[0114]

number

[0115] [Table 1]

[0116] *In Table 1, "--" means that the composition was not curable or some of the components in the composition were not dissolved, so that the corresponding physical properties could not be evaluated.

[0117] As shown in Table 1, the composition for sealing an organic light emitting device according to the present invention realizes an organic layer having a low plasma etching rate and dielectric constant, excellent pencil hardness, and excellent inkjetability.

[0118] On the other hand, the compositions of the comparative examples which do not satisfy the composition constitution of the present invention were unable to obtain all the effects of the present invention.

[0119] Simple modifications or alterations of the present invention can be easily implemented by a person having ordinary skill in the art, and all such modifications and alterations can be considered to be included within the scope of the present invention.

Claims

1. A composition for sealing an organic light-emitting element, comprising: a (meth)allyl-based photocurable monomer, a (meth)acrylate-based photocurable monomer, a photocurable monomer of the following Chemical Formula 4, and a photoinitiator, wherein the total of the allyl-based photocurable monomer and the (meth)acrylate-based photocurable monomer is greater than the photocurable monomer of the following Chemical Formula 4 by weight: [Formula 1] (In the above Chemical Formula 4, R 1 is hydrogen or a methyl group, R 2 , R 3 , R 4 , R 5 , R 6 are each independently a hydrogen atom, a linear or branched, substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 20 carbon atoms, or a substituted or unsubstituted arylalkyl group having 7 to 20 carbon atoms; R 2 , R 3 , R 4 , R 5 , R 6 may each independently have one of an epoxy group, a urethane group, and an alkoxy group at its terminal.

2. The composition for sealing an organic light-emitting element according to claim 1, wherein the (meth)allyl-based photocurable monomer includes at least one of the following chemical formulas 1 and 2: [Case 2] (In the above Chemical Formula 1, R 1 , R 2 , R 3 respectively represent an allyl group, a methallyl group, hydrogen, a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted cycloalkyl group having 3 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, a substituted or unsubstituted arylalkyl group having 7 to 10 carbon atoms, or a glycidyl group, R 1 , R 2 , R 3 is an allyl or methallyl group). [C3] (In the above Chemical Formula 2, R 4 is an allyl group or a methallyl group, R 5 and R 6 are linked together to form a substituted or unsubstituted nitrogen-containing ring structure.

3. The composition for sealing an organic light-emitting element according to claim 1, wherein the (meth)allyl-based photocurable monomer comprises at least one of triallyl isocyanurate, 1,3-diallyl-5-glycidyl isocyanurate, diallyl n-propyl isocyanurate, and trimethallyl isocyanurate.

4. The composition for sealing an organic light-emitting element according to claim 1 , wherein the (meth)acrylate photocurable monomer is a monofunctional (meth)acrylate.

5. The composition for sealing an organic light-emitting element according to claim 1, wherein the (meth)acrylate-based photocurable monomer contains a mono(meth)acrylate having a substituted or unsubstituted, linear or branched alkyl group having 1 to 30 carbon atoms.

6. 2. The composition for sealing an organic light emitting device according to claim 1, wherein the photocurable monomer of Formula 4 includes at least one of phenylstyrene, tert-butylstyrene, and alpha-methylstyrene.

7. 2. The composition for sealing an organic light-emitting element according to claim 1, wherein the composition comprises 40 to 90 parts by weight of the (meth)allyl-based photocurable monomer, 5 to 55 parts by weight of the (meth)acrylate-based photocurable monomer, 5 to 35 parts by weight of the photocurable monomer of Chemical Formula 4, and 0.01 to 15 parts by weight of the photoinitiator, relative to a total of 100 parts by weight of the (meth)allyl-based photocurable monomer, the (meth)acrylate-based photocurable monomer, and the photocurable monomer of Chemical Formula 4.

8. The composition for sealing an organic light-emitting element according to claim 1 , wherein the composition is a solvent-free composition.

9. 2. The composition for sealing an organic light-emitting element according to claim 1, wherein the composition has a viscosity of 7 cps to 100 cps at 25±2° C.

10. 10. An organic light-emitting element display device comprising an organic layer formed from the composition for sealing an organic light-emitting element according to claim 1.

Citation Information

Patent Citations

  • Solid acrylic matting resin with improved mechanical property

    CN105418827A

  • Addition polymers from nitrogen heterocycle containing monomers and vinyl arylcyclobutene-containing monomers

    CN109748997A

  • Multifunctional resins, their manufacturing methods and applications

    JP2021520443A

  • A method for manufacturing acrylic graft copolymer having improved impact strength, coloring properties and weather resistance

    KR101868800B1

  • Polymer Particles, Conductive Particles, and an Anisotropic Conductive Packaging Materials Containing the Same

    US20070252112A1