Antibacterial composition and method for producing same
The antimicrobial composition with Si-bonded hydrogen atoms and excipients stabilizes silver-containing agents, addressing discoloration issues in wound care dressings by inhibiting silver oxide formation, ensuring color stability and efficacy.
Patent Information
- Application Number
- JP2024513741
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-10-13
- Publication Date
- 2024-10-04
AI Technical Summary
Wound care dressings containing silver-containing compounds suffer from discoloration due to the dissociation of silver ions, which is undesirable in hospital settings.
An antimicrobial composition comprising an organopolysiloxane with Si-bonded hydrogen atoms, a silver-containing antimicrobial agent, and an excipient, where the excipient inhibits the formation of elemental silver or silver oxide, maintaining the composition's color stability.
The composition maintains color stability under humid conditions, preventing undesirable discoloration and providing effective antimicrobial properties for wound care applications.
Smart Images

Figure 2024536000000001 
Figure 2024536000000002 
Figure 2024536000000003
Abstract
Description
[Technical field]
[0001] The present invention relates to antimicrobial compositions, methods of making such compositions, and uses thereof. [Background technology]
[0002] Wound care dressings often contain an adhesive layer that includes silver-containing compounds and other antimicrobial agents to help prevent infection and promote wound healing. However, over time, such silver-containing compounds dissociate. The resulting dissociation produces silver ions, which can be reduced and oxidized, resulting in discoloration of the dressing. Such discoloration is undesirable, especially in hospitals. Summary of the Invention [Problem to be solved by the invention]
[0003] It would therefore be desirable to provide a composition that can overcome the aforementioned shortcomings. Methods for making such compositions would also be beneficial. [Means for solving the problem]
[0004] An embodiment of an antimicrobial composition is provided.
[0005] In one embodiment, the antimicrobial composition includes component (A). Component (A) includes an organopolysiloxane having one or more groups that include a silicon atom bonded to a hydrogen atom. The antimicrobial composition also includes a silver-containing antimicrobial agent and an excipient. The antimicrobial composition has a discontinuous phase, and the antimicrobial agent and the excipient are present in the discontinuous phase.
[0006] Preferably, the silver-containing antimicrobial agent is a silver salt.
[0007] In some embodiments, the excipient has an average molecular weight of 300 g / mol or more. In certain embodiments, the average molecular weight of the excipient is 300-2,000 g / mol. In certain embodiments, the excipient is an alcohol, glycol, polyether, or organopolysiloxane polyoxyalkylene. In one such embodiment, the excipient is a polyether having an average molecular weight of 300-2,000 g / mol. In another embodiment, the average molecular weight of the excipient is 300-1000 g / mol.
[0008] In certain embodiments, the excipient inhibits the silver-containing antimicrobial agent from forming elemental silver or silver oxide in the presence of air having 50% relative humidity at 20°C.
[0009] In some embodiments, the weight percentage of the excipient is greater than the weight percentage of the silver-containing antimicrobial agent, based on the total weight of the composition. In some embodiments, the weight percentage of the excipient in the composition is at least twice the weight percentage of the silver-containing antimicrobial agent. Preferably, the weight percentage of the excipient is 2-10 times greater than the weight percentage of the silver-containing antimicrobial agent.
[0010] In other embodiments, the antimicrobial composition comprises 0.5% or more by weight of excipients, based on the total weight of the composition, hi one such embodiment, the antimicrobial composition comprises 0.5-15% by weight of excipients, based on the total weight of the composition.
[0011] In some embodiments, the antimicrobial composition further comprises a hydrophilic additive compound.
[0012] In other embodiments, the antimicrobial composition exhibits no observable color change after exposure to air at 50% relative humidity for 24 hours at 20°C.
[0013] In other embodiments, the antimicrobial composition further comprises component (B), which comprises an organopolysiloxane compound having one or more end groups containing a carbon-carbon multiple bond.
[0014] In some embodiments, the antimicrobial composition has a continuous phase that includes a polysiloxane network formed by the product of combining component (A) and component (B). In some of these embodiments, the average molecular weight of the excipient is between 300 and 1000 g / mol.
[0015] In other embodiments, the antimicrobial composition further comprises a hydrosilylation catalyst provided as part of component (A) or component (B).
[0016] In some embodiments, the antimicrobial composition further comprises component (C), hi some embodiments, component (C) comprises an organopolysiloxane and a filler.
[0017] In some embodiments, a gel adhesive may comprise said antimicrobial composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] It is to be understood that the invention may contemplate various alternative adaptations and step sequences unless expressly specified to the contrary. It is also to be understood that the specific materials, compositions, articles, and methods described in the following specification are merely exemplary embodiments of the concepts of the invention. Thus, specific characteristics, conditions, or other physical characteristics relating to the disclosed embodiments are not to be considered as limiting, unless expressly stated to the contrary.
[0019] In certain embodiments, an antimicrobial composition is provided. The antimicrobial composition is suitable for use in wound care dressings. For example, the composition can be utilized to provide an adhesive portion for wound care dressings. However, the antimicrobial composition is not limited to wound care applications and can be utilized in other applications where it is desired to inhibit the growth of microorganisms. Such applications can be of a medical or non-medical type.
[0020] The antimicrobial composition includes component (A). Component (A) includes an organopolysiloxane having one or more groups containing a silicon atom bonded to a hydrogen atom. The silicon atom bonded to a hydrogen atom may be referred to herein as Si-bonded hydrogen or by using the designation "SiH". In some embodiments, at least one of the one or more groups containing a silicon atom bonded to a hydrogen atom is a terminal group. In other embodiments, at least one of the one or more groups containing a silicon atom bonded to a hydrogen atom is a pendant group. In still other embodiments, the organopolysiloxane of component (A) has two or more groups containing a silicon atom bonded to a hydrogen atom, at least one of the two or more groups is a terminal group and at least one of the two or more groups is a pendant group. In some embodiments, component (A) may include a mixture of the above organopolysiloxanes. For example, in some embodiments, component (A) may comprise a mixture of organopolysiloxanes, which may include an organopolysiloxane having at least one end group comprising a silicon atom bonded to a hydrogen atom and an organopolysiloxane having at least one pendant group comprising a silicon atom bonded to a hydrogen atom. Additional organopolysiloxanes may also be suitable for use in component (A).
[0021] Preferably, the organopolysiloxane of component (A) has two or more silicon-bonded hydrogen atoms, is linear, cyclic or branched, and is composed of units of general formula (I). R 4 c H d SiO (4-c-d) / 2 (I) [In the formula, R 4 is, independently in each occurrence, a group that does not contain an aliphatic carbon-carbon multiple bond; c is 0, 1, 2, or 3; d is 0, 1, or 2; However, the sum of c+d is 3 or less, and there are at least two silicon-bonded hydrogen atoms per molecule.
[0022] In some embodiments, R 4 may contain one or more monovalent or polyvalent groups, where the polyvalent groups, e.g., divalent, trivalent, and tetravalent groups, link together, for example, two or more, e.g., two, three, or four, siloxy units of formula (I).
[0023] In other embodiments, R 4 -F, -Cl, -Br, OR 6 , -CN, -SCN, -NCO, and a monovalent radical from the group comprising oxygen atoms or radicals -C(O)- and SiC-bonded substituted or unsubstituted hydrocarbon radicals which may be interrupted on both sides by Si-bonded divalent radicals according to formula (I). 4 When contains a SiC-bonded substituted hydrocarbon group, preferred substituents are halogen atoms, phosphorus-containing groups, cyano groups, -OR 6 , -NR 6 -, -NR 6 2 , -NR 6 -C(O)-NR 6 2 , -C(O)-NR 6 2 , -C(O)R 6 , -C(O)OR 6 , -SO 2 -Ph and -C 6 F 5 In such an embodiment, R 6 are independently in each occurrence the same or different and represent a hydrogen atom or a monovalent hydrocarbon radical having 1 to 20 carbon atoms, and Ph is a phenyl group.
[0024] R 4Further embodiments of the present invention include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, hexyl groups such as n-hexyl, heptyl groups such as n-heptyl, octyl groups such as n-octyl and isooctyl groups such as 2,2,4-trimethylpentyl, nonyl groups such as n-nonyl, decyl groups such as n-decyl, n-oct ... dodecyl groups such as decyl groups, and octadecyl groups such as n-octadecyl groups; cycloalkyl groups such as cyclopentyl, cyclohexyl, cycloheptyl, and methylcyclohexyl groups; aryl groups such as phenyl, naphthyl, anthryl, and phenanthryl groups; alkaryl groups such as o-, m-, and p-tolyl, xylyl, and ethylphenyl groups; and aralkyl groups such as benzyl, α-, and β-phenylethyl groups.
[0025] R 4 When is a substituted group, suitable examples include haloalkyl groups such as 3,3,3-trifluoro-n-propyl, 2,2,2,2',2',2'-hexafluoroisopropyl, heptafluoroisopropyl, haloaryl groups such as o-, m-, and p-chlorophenyl groups, -(CH 2 )-N(R 6 )C(O)NR 6 2 , -(CH 2 ) o -C(O)NR 6 2 , -(CH 2 ) o -C(O)R 6 , -(CH 2 ) o -C(O)OR 6 , (CH 2 ) o -C(O)NR 6 2 , -(CH 2 )-C(O)-(CH 2 ) p C(O)CH 3 , -(CH 2 )-O-CO-R 6, -(CH 2 )-NR 6 -(CH 2 ) p -NR 6 2 , -(CH 2 ) o -O-(CH 2 ) p CH(OH)CH 2 OH, -(CH 2 ) o (OCH 2 CH 2 ) p OR 6 , (CH 2 ) o -SO 2 -Ph, and (CH 2 ) o -OC 6 F 5 Including R 6 and Ph correspond to the definitions given above, and o and p are the same or different integers between 0 and 10.
[0026] R as a divalent group bonded to Si on both sides according to formula (I) 4 Examples of R are the additional bonds that occur due to the replacement of hydrogen atoms. 4 Examples of such groups are -(CH 2 )-, -CH(CH 3 )-, -C(CH 3 ) 2 -, -CH(CH 3 )-CH 2 -, -C 6 H 4 -, -CH(Ph)-CH 2 -, -C(CF 3 ) 2 -, (CH 2 ) o -C 6 H 4 -(CH 2 ) o -, -(CH 2 ) o -C 6 H 4 -C 6 H 4 -(CH2 ) o -, -(CH 2 O) p , (CH 2 CH 2 O) o , -(CH 2 ) o -O x -C 6 H 4 -SO 2 -C 6 H 4 -O x -(CH 2 ) o -, where x is 0 or 1, and Ph, o and p have the above definitions.
[0027] Preferably, R 4 includes a monovalent SiC-bonded, optionally substituted hydrocarbon group having 1 to 18 carbon atoms and containing no aliphatic carbon-carbon multiple bonds, more preferably a monovalent SiC-bonded hydrocarbon group having 1 to 6 carbon atoms and containing no aliphatic carbon-carbon multiple bonds, and more specifically a methyl group or a phenyl group.
[0028] In one particular embodiment, the organopolysiloxane of component (A) preferably contains Si-bonded hydrogen in the range of 0.04 to 1.7 weight percent (wt %), based on the total weight of the organopolysiloxane.
[0029] The molecular weight of the organopolysiloxane of component (A) may likewise be within a wide range, e.g., 10 2 ~10 6 The organopolysiloxane of component (A) can thus be, for example, a relatively low molecular weight SiH-functional oligosiloxane, such as tetramethyldisiloxane, or it can be a silicone resin or polymeric polydimethylsiloxane having in-chain or terminal SiH groups.
[0030] The molecular structure of component (A) is also not fixed, and in particular the relatively high molecular weight SiH-containing organopolysiloxanes, i.e. oligomeric or polymeric structures, may be linear, cyclic, branched, or resinous or network-like. The linear and cyclic organopolysiloxanes are preferably of the formula R 4 3 SiO 1 / 2 , H.R. 4 2 SiO 1 / 2 , H.R. 4 SiO 2 / 2 , and R 4 2 SiO 2 / 2 It is composed of units of R 4 has the definition given above. The branched and network organopolysiloxanes further contain trifunctional and / or tetrafunctional units and are represented by the formula R 4 SiO 3 / 2 , HSiO 3 / 2 and SiO 4 / 2 R 4 has the definition given above.
[0031] In some embodiments, component (A) may contain a mixture of two or more different organopolysiloxane-containing molecules. Particularly preferred is the use of low molecular weight SiH-functional compounds such as tetrakis(dimethylsiloxy)silane and tetramethylcyclotetrasiloxane, as well as higher molecular weight SiH-containing siloxanes such as poly(hydrogenmethyl)siloxanes and poly(dimethylhydrogenmethyl)siloxanes having a viscosity at 25° C. of 10 to 20000 mPa·s, or similar SiH-containing compounds in which some of the methyl groups have been replaced by 3,3,3-trifluoropropyl or phenyl groups.
[0032] The amount of component (A) in the antimicrobial composition is preferably such that the molar ratio of SiH groups to aliphatically unsaturated groups in the composition is between 0.1 and 20, more preferably 0.3 and 2.0.
[0033] In some embodiments, the antimicrobial composition may be of the one-component type. In other embodiments, the antimicrobial composition may be of the two-component type. In these embodiments, the antimicrobial composition may be formed by providing component (B).
[0034] Component (B) may include an organopolysiloxane compound or another compound. In some embodiments, component (B) may include a linear organopolysiloxane compound or another linear compound. In these embodiments, the organopolysiloxane compound may have one or more end groups that include a carbon-carbon multiple bond, which may also be referred to herein as an aliphatic multiple bond. In one such embodiment, the organopolysiloxane compound may include a SiC bond group with an aliphatic carbon-carbon multiple bond, which may also be referred to herein as an aliphatic unsaturated group. When component (B) includes another linear compound, such a compound may include an aliphatic carbon-carbon multiple bond.
[0035] As mentioned above, component (B) may comprise an organopolysiloxane compound or another compound. In embodiments where component (B) comprises a silicon-free organic compound, such a compound may comprise at least two aliphatically unsaturated groups. It is further noted that component (B) may comprise an organopolysiloxane having at least two aliphatically unsaturated groups. In certain embodiments, component (B) may comprise a mixture of compounds. In one such embodiment, component (B) may comprise an organopolysiloxane compound having at least two aliphatically unsaturated groups and a silicon-free organic compound having at least two aliphatically unsaturated groups. In yet other embodiments, component (B) may comprise a mixture of different organopolysiloxane compounds, each of which may comprise an aliphatic carbon-carbon multiple bond. In these embodiments, the aliphatic carbon-carbon multiple bond may be included in the end group of the organopolysiloxane compound or may be located in a separate group.
[0036] Examples of silicon-free organic compounds suitable for use in component (B) are 1,3,5-trivinylcyclohexane, 2,3-dimethyl-1,3-butadiene, 7-methyl-3-methylene-1,6-octadiene, 2-methyl-1,3-butadiene, 1,5-hexadiene, 1,7-octadiene, 4,7-methylene-4,7,8,9-tetrahydroindene, methylcyclopentadiene, 5-vinyl-2-nor Bornene, bicyclo[2.2.1]hepta-2,5-diene, 1,3-diisopropenylbenzene, polybutadiene containing vinyl groups, 1,4-divinylcyclohexane, 1,3,5-triallylbenzene, 1,3,5-trivinylbenzene, 1,2,4-trivinylcyclohexane, 1,3,5-triisopropenylbenzene, 1,4-divinylbenzene, 3-methylhepta-1,5-diene, 3-phenyl and 4,5-dimethyl-4,5-diethylocta-1,7-diene, N,N'-methylenebisacrylamide, 1,1,1-tris(hydroxymethyl)propane triacrylate, 1,1,1-tris(hydroxymethyl)propane trimethacrylate, tripropylene glycol diacrylate, diallyl ether, diallylamine, diallyl carbonate, N,N'-diallyl urea, triallylamine, tris(2-methylallyl)amine, 2,4,6-triallyloxy-1,3,5-triazine, triallyl-s-triazine-2,4,6(1H,3H,5H)-trione, diallyl malonate, polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, and poly(propylene glycol) methacrylate.
[0037] Organopolysiloxane compounds known in the art are suitable for use in component (B). Examples of such organopolysiloxanes include, for example, silicone block copolymers having urea segments, silicone block copolymers having amide segments and / or imide segments and / or ester-amide segments and / or polystyrene segments and / or silarylene segments and / or carborane segments, and silicone graft copolymers having ether groups.
[0038] Organopolysiloxane compounds suitable for use in component (B) are preferably linear or branched organopolysiloxanes containing units of the general formula (II). R 4 a R 5 b SiO (4-a-b) / 2 (II) [In the formula, R 4 is, independently in each occurrence, a group that does not contain an aliphatic carbon-carbon multiple bond; R 5 are independently in each occurrence the same or different and are monovalent substituted or unsubstituted SiC-bonded hydrocarbon radicals having at least one aliphatic carbon-carbon multiple bond; a is 0, 1, 2, or 3; b is 0, 1, or 2; However, the sum of a+b is 3 or less, and there are at least two groups R per molecule. 5 exists.]
[0039] R 4 has the definition given above. In some embodiments, R 5 contains any desired group suitable for addition reaction (hydrosilylation) with SiH-functional compounds.
[0040] R 5 When contains a SiC-bonded substituted hydrocarbon group, preferred substituents are halogen atoms, cyano groups, and -OR 6Where R 6 has the definition given above.
[0041] Preferably, R 5 includes alkenyl and alkynyl groups having 2 to 16 carbon atoms, such as vinyl, allyl, methallyl, 1-propenyl, 5-hexenyl, ethynyl, butadienyl, hexadienyl, cyclopentenyl, cyclopentadienyl, cyclohexenyl, vinylcyclohexylethyl, divinylcyclohexylethyl, norbornenyl, vinylphenyl and styryl groups, with vinyl, allyl and hexenyl groups being particularly preferred for use.
[0042] The molecular weight of the organopolysiloxane compound(s) of component (B) can be within a wide range, for example, 10 2 ~10 6 Thus, for example, component (B) can be an organopolysiloxane that is a relatively low molecular weight alkenyl-functional oligosiloxane, such as 1,2-divinyltetramethyldisiloxane, or a 10- to 12-hydroxypropyl siloxane having in-chain or terminal Si-bonded vinyl groups. 5 The organopolysiloxane of component (B) may comprise a polydimethylsiloxane having a molecular weight (number average as measured by NMR) of 10 ... 4 3 SiO 1 / 2 , R 5 R 4 2 SiO 1 / 2 , R 5 R 4 SiO 1 / 2 , and R 4 2 SiO 2 / 2 In the formula, R 4 and R 5has the definition given above. The branched and reticulated polysiloxanes further comprise trifunctional and / or tetrafunctional units and have the formula R 4 SiO 3 / 2 , R 5 SiO 3 / 2 and SiO 4 / 2 Also, as mentioned above, mixtures of these different organopolysiloxanes may be utilized in component (B).
[0043] Preferred organopolysiloxane compounds for use in component (B) are vinyl-functional substantially linear polydiorganosiloxanes having a viscosity of 0.01 to 500,000 Pa·s, more preferably 0.1 to 100,000 Pa·s, in each case measured at 25°C.
[0044] In some embodiments, the antimicrobial composition may contain 30-95% by weight, preferably 30-80% by weight, more preferably 40-70% by weight of the organopolysiloxane compound(s) of component (B). In other embodiments, the antimicrobial composition may contain 0.1-60% by weight, preferably 0.5-50% by weight, more preferably 1-30% by weight of the organopolysiloxane(s) of component (A). When the antimicrobial composition includes a substitute for the organopolysiloxanes of components (A) and (B), it may be present in the antimicrobial composition at 30-95% by weight, preferably 30-80% by weight, more preferably 40-70% by weight.
[0045] In certain embodiments, the antimicrobial composition has a continuous phase and a discontinuous phase. In these embodiments, the antimicrobial composition may be an emulsion. In one embodiment, the continuous phase comprises a polysiloxane network and the discontinuous phase is dispersed in the continuous phase. In some embodiments, the discontinuous phase is uniformly dispersed in the continuous phase. In certain embodiments, the polysiloxane network may be formed by utilizing a single component, such as component (A). In other embodiments, the polysiloxane network is formed by the product of combining the organopolysiloxane from component (A) with the organopolysiloxane from component (B). In certain embodiments, the continuous phase may also be formed by utilizing component (C).
[0046] Component (C) may include an organopolysiloxane. In some embodiments, the organopolysiloxane may have one or more end groups containing a silicon atom bonded to a hydrogen atom. In other embodiments, the organopolysiloxane may have one or more end groups containing a carbon-carbon multiple bond. In yet other embodiments, component (C) may include a mixture of organopolysiloxanes. For example, in some embodiments, component C may include an organopolysiloxane compound having one or more end groups containing a silicon atom bonded to a hydrogen atom, an organopolysiloxane compound having one or more end groups containing a carbon-carbon multiple bond, and / or an organopolysiloxane compound that does not contain a reactive group. Component (C) may also include a reinforcing filler. In other embodiments, component (C) may include non-silicone oligomeric compounds, such as polyethers, or polymeric compounds, such as acrylates, urethanes, polyesters, and copolymers thereof with siloxanes.
[0047] Alternatively, instead of utilizing different organopolysiloxanes in components (A) and (B), the polysiloxane network can be formed by providing a single component that includes an organopolysiloxane that simultaneously has aliphatic carbon-carbon multiple bonds and Si-bonded hydrogen atoms.
[0048] When using an organopolysiloxane having simultaneously aliphatic carbon-carbon multiple bonds and Si-bonded hydrogen atoms, suitable examples are preferably composed of units of the general formulae (III), (IV) and (V). R 4 f SiO 4 / 2 (III) R 4 g R 5 SiO 3-g / 2 (IV) R 4 h HSiO 3-h / 2 (V) [In the formula, R 4 and R 5 have the definitions given therefor above, f is 0, 1, 2, or 3; g is 0, 1, or 2; h is 0, 1, or 2; However, there are at least two groups R per molecule. 5 and there are at least two Si-bonded hydrogen atoms.]
[0049] Examples of suitable organopolysiloxanes include SiO 2 , also known as MQ resins. 4 / 2 Units, R 4 3 SiO 1 / 2 Units, R 4 2 R 5 SiO 1 / 2 Units and R 4 2 HSiO 1 / 2 These resins include those containing R 4 SiO 3 / 2 Units and R 4 2 Further comprising SiO units, and R 4 2 R 5 SiO 1 / 2 Units, R 4 2 SiO units, and R 4 Also included are linear organopolysiloxanes substantially composed of HSiO units, and R4 and R 5 satisfies the above definition. Organopolysiloxanes having both aliphatic carbon-carbon multiple bonds and Si-bonded hydrogen atoms have an average viscosity at 25°C of preferably 0.01 to 500,000 Pa·s, more preferably 0.1 to 100,000 Pa·s in any case. Such organopolysiloxanes can be prepared by techniques known in the art. It is also possible to provide both Si-bonded hydrogen atoms and aliphatic carbon-carbon multiple bonds in a single compound.
[0050] Preferably, the antimicrobial composition is crosslinkable. In some embodiments, the antimicrobial composition is formed by addition crosslinking. Crosslinking occurs when the antimicrobial composition cures. A hydrosilylation catalyst can be provided to crosslink the organopolysiloxane provided in the antimicrobial composition. The hydrosilylation catalyst can be provided as part of one of the components utilized to form the antimicrobial composition.
[0051] In the case of a two-component silicone composition, the two components can generally comprise all the components mentioned above in any desired combination, with the proviso that one component does not simultaneously comprise an organopolysiloxane compound having an aliphatic multiple bond, an organopolysiloxane compound having a Si-bonded hydrogen atom, and a hydrosilylation catalyst.Thus, in the case of a two-component composition, the hydrosilylation catalyst can be provided as part of component (A) or component (B).
[0052] Any hydrosilylation catalyst known in the art is suitable for use in the antimicrobial composition. The hydrosilylation catalyst may comprise, for example, a platinum group metal such as platinum, rhodium, ruthenium, palladium, osmium, or iridium, or may be an organometallic compound, or a combination thereof. Suitable examples of hydrosilylation catalysts are compounds such as hexachloroplatinic (IV) acid, platinum dichloride, platinum acetylacetonate, and complexes of said compounds encapsulated in a matrix or core / shell-like structure. Other suitable platinum complexes with low molecular weight organopolysiloxanes include 1,3-diethenyl-1,1,3,3-tetramethyldisiloxane complexes with platinum. Other examples of suitable hydrosilylation catalysts are platinum-phosphite complexes, platinum-phosphine complexes, or alkyl platinum complexes such as cyclopentadienyltrimethylplatinum(IV), derivatives of cyclooctadienyldimethylplatinum(II), or diketonato complexes such as bisacetylacetonatoplatinum(II). In certain embodiments, the platinum-containing compound may be encapsulated within a resin matrix.
[0053] The concentration of the catalyst for catalyzing the hydrosilylation crosslinking reaction can be between 0.1 and 1000 parts per million (ppm), between 0.5 and 100 ppm, or between 1 and 25 ppm of platinum group metal, based on the total weight of the antimicrobial composition.
[0054] In the above-mentioned embodiments, the antimicrobial composition may be provided as a gel. In these embodiments, the gel has a crosslinked structure. A crosslinked structure may be formed when the total number of reactive groups is greater than four. Thus, in the case of a gel formed by a platinum-catalyzed hydrosilylation reaction, crosslinking may occur, for example, between a first organopolysiloxane containing more than two Si-bonded hydrogen atoms and a second organopolysiloxane having at least two reactive aliphatically unsaturated groups, or between a first organopolysiloxane containing two Si-bonded hydrogen atoms and a second organopolysiloxane having more than two aliphatically unsaturated groups. Preferably, in these embodiments, the first and second organopolysiloxanes are crosslinked to the gel point of the mixture. In such embodiments, prior to curing, the antimicrobial composition may exhibit a viscosity of 50 to 100,000 centipoise.
[0055] The antimicrobial composition includes a silver-containing antimicrobial agent. In certain embodiments, the silver-containing antimicrobial agent is a silver salt having antimicrobial properties. 2 SO 4 , Ag 2 SO 3 , AgNO 3 , Ag 2 CO 3 , Ag 3 PO 4 Silver-containing antimicrobial agents may be selected from the group including silver zirconium, silver citrate, silver acetate, silver lactate, and / or other organic silver salts, and / or combinations or mixtures thereof. Other compounds suitable for providing silver ions are also suitable as silver-containing antimicrobial agents, if desired. The silver-containing antimicrobial agent may be provided in the antimicrobial composition at about 1 weight percent (wt%) to about 30 wt%, preferably about 2-20 wt%, in all cases based on the total weight of the composition. The silver-containing antimicrobial agent may be provided as part of component (A), component (B), component (C), in two or more of these components, or as a separate additive to the composition.
[0056] The antimicrobial composition includes an excipient. Based on the total weight of the composition, the antimicrobial composition may include 0.5 wt.% or more of the excipient. Preferably, based on the total weight of the composition, the antimicrobial composition includes 0.5-15 wt.% of the excipient. More preferably, based on the total weight of the composition, the antimicrobial composition includes 0.5-10 wt.% of the excipient. The excipient may be provided as part of component (A), component (B), component (C), or in two or more of these components.
[0057] Preferably, the weight percentage of the excipient in the antimicrobial composition is greater than the weight percentage of the silver-containing antimicrobial agent in the antimicrobial composition, based on the total weight of the composition. For example, the weight percentage of the excipient present in the antimicrobial composition can be more than twice the weight percentage of the silver-containing antimicrobial agent. In some embodiments, the weight percentage of the excipient present in the antimicrobial composition is 2-10 times greater than the weight percentage of the silver-containing antimicrobial agent.
[0058] In some embodiments, the excipient is an alcohol and contains one or more hydroxyl groups. In other embodiments, the excipient can be a glycol. In these embodiments, the excipient has two or more hydroxyl groups, and two of the two or more hydroxyl groups can be linked to different carbon atoms. In one such embodiment, two of the two or more hydroxyl groups are terminal groups. In some embodiments, the excipient is a polyether.
[0059] In some embodiments, the excipient has a number average molecular weight of 100 g / mol or more. In other embodiments, the excipient may have a number average molecular weight of 300 g / mol or more. Preferably, the excipient has a relatively low number average molecular weight. In one such embodiment, the excipient has a number average molecular weight of 300-2,000 g / mol. In another embodiment, the number average molecular weight of the excipient is 300-1000 g / mol. Preferably, in these embodiments, the number average molecular weight of the excipient is 300-600 g / mol.
[0060] In some embodiments, the excipient may be selected from the group consisting of poly(propylene glycol), 1,2-propanediol, di(propylene glycol), di(propylene glycol) monomethyl ether, di(propylene glycol) dimethyl ether, organopolysiloxane polyoxyalkylenes having a number average molecular weight of 400-2000 g / mol, copolymers and mixtures thereof. In certain embodiments, it may be preferred that the excipient is a poly(propylene glycol) having a number average molecular weight of 400-2000 g / mol. Preferably, in these embodiments, the excipient is a poly(propylene glycol) having a number average molecular weight of 400 g / mol. In other embodiments, it may be preferred that the excipient is an organopolysiloxane polyoxyalkylene. Preferably, in these embodiments, the excipient is an organopolysiloxane polyoxyalkylene of the following general formula: [ka]
[0061] In certain embodiments, the organopolysiloxane polyoxyalkylene may be covelantly bonded. An example of a commercially available organopolysiloxane polyoxyalkylene suitable as an excipient is sold by Wacker Chemie AG under the name Belsil® OW1500.
[0062] As described above, the antimicrobial composition has a discontinuous phase. The antimicrobial agent and excipients are present in the discontinuous phase. Without wishing to be bound by a particular theory, it is believed that the silver-containing compound in the conventional antimicrobial composition dissociates and forms silver oxide or elemental silver in the presence of air. The resulting dissociation produces silver ions, which can be reduced and / or oxidized, resulting in undesirable discoloration of the composition. Typically, the discoloration is a dark color, such as black or brown. In the present antimicrobial composition, the excipient inhibits the silver-containing antimicrobial agent from forming elemental silver or silver oxide in the presence of air. Preferably, the excipient inhibits the silver-containing antimicrobial agent from forming elemental silver or silver oxide to the extent that the antimicrobial composition does not show an observable color change after exposure to air having a relative humidity of 50% at 25° C. for 24 hours. In certain embodiments, the antimicrobial composition does not show an observable color change after exposure to air having a relative humidity of 50% at 25° C. for 168 hours. Also, when the antimicrobial composition is provided as a gel, the composition may not exhibit an observable color change after exposure to air having a relative humidity of 50% at 25° C. for 12 months. Moreover, in embodiments in which the antimicrobial composition exhibits an observable color change, the color change is significantly reduced from the color change observed in known compositions. Moreover, the color change results in a color exhibited by the antimicrobial composition that is visually pleasing.
[0063] The antimicrobial composition may include one or more additives, which may be provided as part of component (A), component (B), or component (C). For example, as described above, the antimicrobial composition may include a reinforcing filler. Suitable reinforcing fillers include those having at least 50 ml of reinforcing filler. 2 Examples of suitable fillers include fumed or precipitated silicas having a BET specific surface area of 1000 nm / g, carbon black, activated carbon such as furnace black and acetylene black, or mixtures thereof. The silica fillers described may be hydrophilic or may be made hydrophobic by known methods. Based on the total weight of the antimicrobial composition, the amount of reinforcing filler in the antimicrobial composition may be in the range of 0 to 70% by weight, preferably 0 to 50% by weight.
[0064] In certain embodiments, the fillers utilized are preferably surface-treated. The surface treatment is obtained by methods known in the art for hydrophobizing finely divided fillers. As a result of the surface treatment, the fillers utilized may have a carbon content of at least 0.01 and up to 20% by weight, preferably between 0.1 and 10% by weight, more preferably between 0.5 and 5% by weight. Preferably, in these embodiments, the filler is a surface-treated silica having 0.01 to 2% by weight of Si-bonded aliphatic unsaturated groups. These groups are, for example, Si-bonded vinyl groups. In the antimicrobial composition, the filler is provided as a single species or as a mixture of two or more finely divided fillers.
[0065] Based on the total weight of the composition, further additives may be provided in the antimicrobial composition in a proportion of up to 70% by weight, preferably 0.0001 to 40% by weight. These additives may be, for example, inert fillers, resinous polyorganosiloxanes different from the abovementioned siloxanes, reinforcing and non-reinforcing fillers, fungicides, fragrances, rheological additives, corrosion inhibitors, antioxidants, light stabilizers, flame retardants, and agents for influencing electrical properties, dispersing aids, solvents, adhesion promoters, pigments, dyes, plasticizers, organic polymers, heat stabilizers, etc. These are additives such as finely ground quartz, diatomaceous earth, clays, chalk, lithopone, carbon black, graphite, metal oxides, metal carbonates, metal sulfates, metal salts of carboxylic acids, metal dust, glass fibers, polymer fibers, and other fibers, polymer powders, metal dust, dyes, pigments, etc. The further fillers may be thermally conductive or electrically conductive. Combinations of fillers with different particle sizes and different particle size distributions may also be utilized.
[0066] In addition, the antimicrobial composition may include additional additives. For example, the antimicrobial composition may include one or more solvents and / or one or more inhibitors. In other embodiments, the antimicrobial composition may include a hydrophilic additive compound that may enhance silver release from the composition. Hydrophilic additive compounds known in the art are suitable for use in the antimicrobial composition. These hydrophilic additive compounds, when crosslinked, are known to produce an antimicrobial composition that swells at least 5% after 24 hours in an aqueous solution containing 8.298 g / L sodium chloride and 0.368 g / L calcium chloride dihydrate, as measured by free swelling absorption method.
[0067] When provided as a gel, the antimicrobial composition may also function as an adhesive. In these embodiments, the antimicrobial composition may be utilized as an adhesive portion of a wound care dressing. In this embodiment, the tack exhibited by the gel may be greater than 50 grams of force (gf). Preferably, the tack exhibited by the gel is greater than 100 gf. However, the tack should not be so strong that the skin of the user is damaged when the dressing is removed. Thus, in some embodiments, the tack exhibited by the gel is less than 800 gf. In these embodiments, the tack exhibited by the gel may be between 50 and 800 gf. The tack exhibited by the gel may be measured by known methods. For example, the tack of the gel may be measured with a TA.XT Plus Texture Analyzer using a TA-57R probe and a TA-303 instrument.
[0068] In addition to suitable adhesion, the gel is preferably cohesive. A cohesive gel will not crumble when removed from the surface to which it is adhered. In some embodiments, the gel may exhibit a post-cure penetration hardness of 25 to 500 1 / 10 mm, measured according to DIN ISO 2137 using a 62.5 gram hollow cone for 60 seconds, after curing at 120° C. for 60 minutes.
[0069] The gel can be combined with or incorporated into a wound care dressing prior to application of the dressing to a user, or can be applied directly to the user. In such applications, in certain embodiments, the gel does not exhibit an observable color change over an extended period of time. For example, the gel may not exhibit an observable color change after 24 hours of exposure to air at 25° C. with a relative humidity of 50%. Indeed, in gel form, the antimicrobial composition may not exhibit an observable color change after 365 days of exposure to air at 25° C. with a relative humidity of 50%. However, in other embodiments, when the antimicrobial composition is in gel form, the composition may exhibit an observable color change. In these embodiments, the color change is significantly reduced from the color change observed in known compositions. Furthermore, the color change results in a color exhibited by the antimicrobial composition that is visually pleasing.
[0070] The antimicrobial composition may be formed as a gel after being applied to a substrate. In some embodiments, the antimicrobial composition may coat a substrate, such as, for example, a dressing. In these embodiments, the antimicrobial composition may be cast onto the substrate and allowed to harden to form a gel. The antimicrobial composition may be applied to the substrate to provide any desired thickness, pattern, or form. Suitable substrates are known in the art.
[0071] Prior to forming the gel, the antimicrobial composition may be made by preparing component (A). Preferably, component (A) includes the organopolysiloxane(s) described above for component (A). Additionally, component (A) may include a silver-containing antimicrobial agent, an excipient, a hydrosilylation catalyst, and / or one or more additives. If included in component (A), the silver-containing antimicrobial agent, the excipient, the hydrosilylation catalyst, and one or more additives may be mixed with the organopolysiloxane(s) to form a mixture. Mixing may be performed at a predetermined speed and for a predetermined period of time, for example, utilizing a commercially available mixing device such as a Speedmixer® or Dispermat® equipped with a dissolver blade. The silver-containing antimicrobial agent, the excipient, the hydrosilylation catalyst, and one or more additives may be as described above.
[0072] In certain embodiments, the antimicrobial composition can be made by preparing component (B). Preferably, component (B) includes an organopolysiloxane as described above for component (B). In addition, component (B) can include a silver-containing antimicrobial agent, an excipient, a hydrosilylation catalyst, and / or one or more additives. When included in component (B), the silver-containing antimicrobial agent, the excipient, the hydrosilylation catalyst, and one or more additives can be mixed with the organopolysiloxane to form a mixture. Mixing can be performed at a predetermined speed and for a predetermined period of time, for example, utilizing a commercially available mixing device such as the mixing device described above. The silver-containing antimicrobial agent, the excipient, the hydrosilylation catalyst, and one or more additives can be as described above.
[0073] In embodiments in which the antimicrobial composition includes component (C), the antimicrobial composition is made by preparing component (C). In these embodiments, the antimicrobial composition can be made by preparing three mixtures and combining these mixtures. Preferably, component (C) includes an organopolysiloxane, such as those described above for component (C). Additionally, component (C) can include a silver-containing antimicrobial agent, an excipient, a hydrosilylation catalyst, and / or one or more additives. If included in component (C), the silver-containing antimicrobial agent, the excipient, the hydrosilylation catalyst, and one or more additives can be mixed with the organopolysiloxane to form a mixture. Thus, in these embodiments, the antimicrobial composition can be made by first preparing three mixtures. Mixing can be performed at a predetermined speed and for a predetermined period of time utilizing the commercially available mixing equipment described above. The silver-containing antimicrobial agent, the excipient, the hydrosilylation catalyst, and one or more additives can be as described above.
[0074] In certain embodiments, component (A) and component (B) can be mixed to form a mixture prior to coating the substrate. Mixing can be performed at a predetermined rate and for a predetermined period of time, utilizing commercially available mixing equipment, such as the mixing equipment described above. In some embodiments, the mixture can also include component (C). If not included in components (A), (B) or (C), or if it is desired to include additional amounts in the antimicrobial composition, the silver-containing antimicrobial agent, excipient, hydrosilylation catalyst, and / or one or more additives can be added to the mixture. Addition of the silver-containing antimicrobial agent, excipient, hydrosilylation catalyst, and / or one or more additives to the mixture can be accomplished upon mixing of components (A), (B), and (C), or can be performed simultaneously or sequentially with further mixing. After mixing, one or more portions of the substrate can be coated with the antimicrobial composition, and the composition can be cured at a predetermined temperature for a predetermined period of time. For example, the mixture can be cured at a temperature of 40 to 140° C., preferably 60 to 130° C., for 5 seconds to 2 hours, preferably 10 seconds to 30 minutes.
[0075] In a particular embodiment, component (A) is prepared to include an organopolysiloxane having one or more groups that include a silicon atom bonded to a hydrogen atom. In this embodiment, the antimicrobial composition is made by mixing a silver-containing antimicrobial agent with an organopolysiloxane having one or more groups that include a silicon atom bonded to a hydrogen atom and an excipient. Preferably, the excipient includes a polyether or organopolysiloxane polyoxyalkylene having an average molecular weight of 300 to 2,000 g / mol. In one embodiment, component (B) is prepared to include an organopolysiloxane having one or more groups, an organopolysiloxane having one or more end groups that include a carbon-carbon multiple bond. Preferably, component (B) also includes one or more additives, such as, for example, a reinforcing filler. In this embodiment, a mixture is formed. The mixture includes component (A), component (B), a silver-containing antimicrobial agent, an excipient, and a hydrosilylation catalyst. An antimicrobial gel is formed by curing the mixture. EXAMPLES
[0076] The following examples are presented solely for the purpose of further illustrating and disclosing embodiments of the antibacterial composition. Examples of the antibacterial composition include Examples 1-16, which are described below. Comparative Examples 1 and 2, which are not part of the present invention, are also described below.
[0077] [Comparative Example 1] A composition was formed by mixing 3 grams of component (A), which includes an organopolysiloxane having a molecular weight of about 1000 g / mol and one or more groups containing a silicon atom bonded to a hydrogen atom, with 0.5 grams of a mixture of silver sulfate and pyrogenic silica at 2350 rpm using a SpeedMixer® for 5 minutes. Based on the total weight of the mixture, the mixture of silver sulfate and pyrogenic silica was 99% silver sulfate and 1% pyrogenic silica. The composition was initially white, but was observed to change color rapidly when exposed to air at a temperature of about 25°C. After 60 seconds of exposure to air at 25°C, the composition was dark brown to black.
[0078] [Example 1] An antimicrobial composition was formed by mixing 3 grams of component (A), which includes an organopolysiloxane having a molecular weight of about 1000 g / mol and one or more groups containing a silicon atom bonded to a hydrogen atom, with 0.5 grams of a mixture of poly(propylene glycol) having a number average molecular weight of about 400 g / mol, silver sulfate, and pyrogenic silica at 2350 rpm for 5 minutes using a SpeedMixer®. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. The resulting antimicrobial composition included a continuous phase and a discontinuous phase. The continuous phase included the organopolysiloxane, and the discontinuous phase included silver sulfate and poly(propylene glycol). The presence of silver sulfate and poly(propylene glycol) in the discontinuous phase was confirmed by optical microscopy and was evident by light scattering and the white color of the composition. The color of the antimicrobial composition did not undergo any observable change after exposure to air for 60 seconds at a temperature of 25°C.
[0079] [Comparative Example 2] The mixture of silver sulfate and pyrogenic silica was mixed with component (B) comprising an organopolysiloxane having one or more end groups containing carbon-carbon multiple bonds using a SpeedMixer® at 2350 rpm for 5 minutes. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) comprising an organopolysiloxane having one or more groups containing a silicon atom bonded to a hydrogen atom was then added using a SpeedMixer® at 2350 rpm for 30 seconds. The resulting composition comprised 2% by weight of the mixture of silver sulfate and pyrogenic silica, with the remainder of the composition formed from equal parts of components (A) and (B). Before curing, the composition was white in color. A portion of the composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured at 120° C. for 12 minutes. The remaining portion of the composition was cured by exposure to air at a temperature of about 25° C. for 24 hours. After curing, the composition was a gel that appeared brown in color.
[0080] [Example 2] A poly(propylene glycol) having a number average molecular weight of about 400 g / mol, a mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 2% by weight of the mixture of silver sulfate and pyrogenic silica and 5% by weight of poly(propylene glycol), with the remaining portion of the antimicrobial composition formed from equal parts of component (A) and component (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel that showed no observable color change.
[0081] [Example 3] A poly(propylene glycol) having a number average molecular weight of about 725 g / mol, a mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 2% by weight of the mixture of silver sulfate and pyrogenic silica and 5% by weight of poly(propylene glycol), with the remaining portion of the antimicrobial composition formed from equal parts of component (A) and component (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel exhibiting a slight yellow tint.
[0082] [Example 4] A poly(propylene glycol) having a number average molecular weight of about 1000 g / mol, a mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 2% by weight of the mixture of silver sulfate and pyrogenic silica and 5% by weight of poly(propylene glycol), with the remaining portion of the antimicrobial composition formed from equal parts of component (A) and component (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel exhibiting a slight yellow tint.
[0083] [Example 5] A poly(propylene glycol) having a number average molecular weight of about 2000 g / mol, a mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 2% by weight of the mixture of silver sulfate and pyrogenic silica and 5% by weight of poly(propylene glycol), with the remaining portion of the antimicrobial composition formed from equal parts of component (A) and component (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel exhibiting a slight yellow tint.
[0084] [Example 6] A poly(ethylene glycol) having a number average molecular weight of about 400 g / mol, a mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 2% by weight of the mixture of silver sulfate and pyrogenic silica and 5% by weight of poly(ethylene glycol), with the remaining portion of the antimicrobial composition formed from equal parts of component (A) and component (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel exhibiting a slight pink tint.
[0085] [Example 7] 1,2-propanediol, a mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 2% by weight of the mixture of silver sulfate and pyrogenic silica and 5% by weight of 1,2-propanediol, with the remaining portion of the antimicrobial composition formed from equal parts of component (A) and component (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel exhibiting a slight yellow tint.
[0086] [Example 8] Di(propylene glycol), a mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 2% by weight of the mixture of silver sulfate and pyrogenic silica and 5% by weight of di(propylene glycol), with the remaining portion of the antimicrobial composition formed from equal parts of components (A) and (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel that was observed to be colorless.
[0087] [Example 9] The di(propylene glycol) monomethyl ether, the mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 2% by weight of the mixture of silver sulfate and pyrogenic silica and 5% by weight of di(propylene glycol) monomethyl ether, with the remaining portion of the antimicrobial composition formed from equal parts of components (A) and (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 25° C. After curing, the antimicrobial composition was a gel exhibiting a yellowish tint.
[0088] [Example 10] Di(propylene glycol) dimethyl ether, a mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 2% by weight of the mixture of silver sulfate and pyrogenic silica and 5% by weight of di(propylene glycol) dimethyl ether, with the remaining portion of the antimicrobial composition formed from equal parts of components (A) and (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel that exhibited a stronger yellowish tint than that observed in Example 7.
[0089] [Example 11] A mixture of poly(propylene glycol) having a number average molecular weight of about 400 g / mol, silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 2% by weight of the mixture of silver sulfate and pyrogenic silica and 2.5% by weight of poly(propylene glycol), with the remaining portion of the antimicrobial composition formed from equal parts of component (A) and component (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel that showed no observable color change.
[0090] [Example 12] A poly(propylene glycol) having a number average molecular weight of about 400 g / mol, a mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 2% by weight of the mixture of silver sulfate and pyrogenic silica and 1.0% by weight of poly(propylene glycol), with the remaining portion of the antimicrobial composition formed from equal parts of component (A) and component (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel that showed no observable color change.
[0091] [Example 13] A poly(propylene glycol) having a number average molecular weight of about 400 g / mol, a mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 2% by weight of the mixture of silver sulfate and pyrogenic silica and 0.5% by weight of poly(propylene glycol), with the remaining portion of the antimicrobial composition formed from equal parts of component (A) and component (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel exhibiting a slight pink tint.
[0092] [Example 14] A poly(propylene glycol) having a number average molecular weight of about 400 g / mol, a mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 5% by weight of the mixture of silver sulfate and pyrogenic silica and 0.5% by weight of poly(propylene glycol), with the remaining portion of the antimicrobial composition formed from equal parts of component (A) and component (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel exhibiting a slight pink tint.
[0093] [Example 15] A poly(propylene glycol) having a number average molecular weight of about 400 g / mol, a mixture of silver sulfate and pyrogenic silica, and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds were mixed with a SpeedMixer® at 2350 rpm for 5 minutes to form a first mixture. The mixture of silver sulfate and pyrogenic silica was as described above in Comparative Example 1. Component (A) including an organopolysiloxane having one or more groups including a silicon atom bonded to a hydrogen atom was then added to the first mixture with a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition included 10% by weight of the silver sulfate and pyrogenic silica mixture and 1.0% by weight of poly(propylene glycol), with the remaining portion of the antimicrobial composition formed from equal parts of component (A) and component (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast onto a biaxially oriented PET substrate to achieve a wet film thickness of 15 mils and then cured for 12 minutes at 120° C. The remaining portion of the composition was cured by exposure to air for 24 hours at a temperature of about 20° C. After curing, the antimicrobial composition was a gel exhibiting a slight pink tint.
[0094] [Example 16] A first mixture was formed. The first mixture included organopolysiloxane polyoxyalkylene sold by Wacker Chemie AG as Belsil® OW1500 and component (B) including an organopolysiloxane having one or more end groups including carbon-carbon multiple bonds. The first mixture was formed using a SpeedMixer® at 2350 rpm. A second mixture of silver sulfate, pyrogenic silica, and component (B) was formed using a SpeedMixer® at 2350 rpm. An antimicrobial composition was formed by mixing the first mixture, the second mixture, and component (A) including an organopolysiloxane having one or more groups including silicon atoms bonded to hydrogen atoms using a SpeedMixer® at 2350 rpm for 30 seconds. The resulting antimicrobial composition contained 3.1 parts silver sulfate, 0.6 parts pyrogenic silica, 14.3 parts Belsil® OW1500, with the remaining portion of the antimicrobial composition formed from equal parts of component (A) and component (B). Before curing, the antimicrobial composition was white in color. A portion of the antimicrobial composition was cast, drawn down, and then cured at 120° C. for 12 minutes. After curing, each portion of the antimicrobial composition was a gel having a thickness between 8-9 mils. The gel portion showed no observable color change.
[0095] From the foregoing detailed description, it will be apparent that various modifications, additions, and other alternative embodiments are possible without departing from the true scope and spirit. The embodiments and examples discussed herein have been selected and described to provide the best illustration of the principles of the invention and its practical application, thereby enabling those skilled in the art to use the invention in various embodiments and with various modifications as appropriate for the particular use contemplated. It should be understood that all such modifications and variations are within the scope of the invention.
Claims
1. Component (A) comprising an organopolysiloxane having one or more groups containing silicon atoms bonded to hydrogen atoms; Silver-containing antimicrobial agents, and Excipients An antimicrobial composition comprising: the antimicrobial composition has a discontinuous phase, and the antimicrobial agent and the excipients are present in the discontinuous phase; Antibacterial composition.
2. The composition of claim 1 , wherein the silver-containing antimicrobial agent is a silver salt.
3. The composition of claim 1 , wherein the excipient is an alcohol, a glycol, a polyether, or an organopolysiloxane polyoxyalkylene.
4. The composition of claim 1 , wherein the excipient has an average molecular weight of 300 g / mol or greater.
5. The composition of claim 1 further comprising a hydrophilic additive compound.
6. 10. The composition of claim 1, wherein the excipient inhibits the silver-containing antimicrobial agent from forming elemental silver or silver oxide in the presence of air having a relative humidity of 50% at 20°C.
7. 10. The composition of claim 1, which exhibits no observable color change after exposure to air at 50% relative humidity for 24 hours at 20°C.
8. 10. The composition of claim 1 further comprising component (B) comprising an organopolysiloxane compound having one or more end groups containing a carbon-carbon multiple bond.
9. 10. The composition of claim 1, wherein the weight percentage of said excipient is greater than the weight percentage of said silver-containing antimicrobial agent, based on the total weight of said composition.
10. 10. The composition of claim 1, comprising 0.5% by weight or more of said excipient, based on the total weight of said composition.
11. The composition of claim 3, wherein the excipient is a polyether having an average molecular weight of 300 to 2,000 g / mol.
12. The composition of claim 4, wherein the average molecular weight of the excipient is from 300 to 2,000 g / mol.
13. 9. The composition of claim 8 having a continuous phase comprising a polysiloxane network formed by the product of combining said component (A) and said component (B).
14. 9. The composition of claim 8, further comprising a hydrosilylation catalyst provided as part of said component (A) or said component (B).
15. 9. The composition of claim 8, further comprising component (C), said component (C) comprising an organopolysiloxane and a filler.
16. 10. The composition of claim 9, wherein the weight percentage of said excipient in said composition is greater than or equal to two times the weight percentage of said silver-containing antimicrobial agent.
17. The composition of claim 10, comprising 0.5 to 15% by weight of said excipient, based on the total weight of the composition.
18. The composition according to claim 11, wherein the average molecular weight of the excipient is from 300 to 1000 g / mol.
19. 17. The composition of claim 16, wherein the weight percentage of the excipient is 2 to 10 times greater than the weight percentage of the silver-containing antimicrobial agent.
20. A gel adhesive comprising the composition of claim 1.
Citation Information
Patent Citations
Antibacterial anticoagulant high polymer material, and preparation method and application thereof
CN103965639A
Antifungal silicone rubber composition
JP2002038011A
Antibacterial gel
JP2013523879A
Hydrophilic and antibacterial silicone gel adhesive
JP2016507598A