Manufacturing method of superabsorbent resin

By using a reducing agent and sodium dodecyl sulfate during polymerization, the method addresses the inefficiencies in drying superabsorbent resin production, enhancing water absorption and retention capacity through controlled micropore formation.

JP2024536008APending Publication Date: 2024-10-04LG CHEM LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024514554
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-20
Filing Date
2022-10-21
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods for producing superabsorbent resins face challenges in achieving efficient drying due to the cohesive force of hydrogel polymers, leading to decreased porosity and inadequate drying of the inner layers, which affects water absorption properties.

Method used

Incorporating a specific reducing agent, such as oxalic acid, sodium metabisulfite, or sodium benzoate, in combination with sodium dodecyl sulfate during the polymerization stage to enhance polymerization rate and create micropores, improving drying efficiency and controlling the undried ratio of the base resin.

Benefits of technology

The method results in superabsorbent resins with excellent water absorption properties, particularly high centrifugal water retention capacity and drying efficiency, by forming appropriate voids during the drying process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536008000001
    Figure 2024536008000001
  • Figure 2024536008000002
    Figure 2024536008000002
  • Figure 2024536008000003
    Figure 2024536008000003
Patent Text Reader

Abstract

The present invention relates to a method for producing a superabsorbent resin, more specifically, to a method for producing a superabsorbent resin in which a specific reducing agent compound and sodium dodecyl sulfate are used in combination in the polymerization step to achieve excellent drying efficiency, thereby improving the water absorption properties of the resin.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0141344 filed on October 21, 2021 and Korean Patent Application No. 10-2022-0135391 filed on October 20, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.

[0002] The present invention relates to a method for producing a superabsorbent resin, more specifically, to a method for producing a superabsorbent resin in which a specific reducing agent compound is included in the polymerization step to realize excellent drying efficiency, thereby improving the water absorption properties of the resin. [Background technology]

[0003] Super absorbent polymer (SAP) is a synthetic polymeric substance that has the ability to absorb 500 to 1,000 times its own weight in water, and is given different names by different developers, such as SAM (Super Absorbency Material) and AGM (Absorbent Gel Material). These super absorbent polymers first came into practical use as sanitary products, and are now widely used as soil water retention agents for horticulture, water stoppers for civil engineering and construction, seedling sheets, freshness preserving agents in the food distribution field, and materials for packs.

[0004] Such superabsorbent polymers are widely used in the field of sanitary materials, such as diapers and sanitary napkins. In the sanitary materials, the superabsorbent polymers are generally contained in a dispersed state in the pulp. However, in recent years, efforts have been made to provide sanitary materials, such as diapers, with thinner thicknesses, and as part of these efforts, the pulp content has been reduced, or even going a step further, the development of so-called pulpless diapers, which do not use pulp at all, has been actively promoted.

[0005] In this way, in the case of sanitary materials in which the pulp content is reduced or no pulp is used, the superabsorbent polymer is contained at a relatively high ratio, and the superabsorbent polymer particles are inevitably contained in multiple layers in the sanitary materials. In order for the overall superabsorbent polymer particles contained in multiple layers in this way to more efficiently absorb a large amount of liquid such as urine, the superabsorbent polymer basically needs to exhibit not only high water absorption performance but also a fast water absorption speed.

[0006] Meanwhile, such superabsorbent resins are generally manufactured by polymerizing monomers to prepare a hydrogel polymer containing a large amount of water, drying the hydrogel polymer, and then pulverizing the hydrogel polymer into resin particles having a desired particle size. The hydrogel polymers have the property of agglomerating with each other, and when they are manufactured into agglomerated fine particles, there is a problem that the drying is not performed well in the subsequent drying process. Specifically, the porosity in the drying layer is significantly reduced during the drying process due to the increase in the cohesive force of the hydrogel polymer, and this increases the hot air differential pressure, resulting in a problem that only the outer periphery of the drying layer is dried and the inside is not sufficiently dried. In this case, the water absorption properties of the final superabsorbent resin are affected, and the water retention capacity, water absorption speed, etc. are reduced, so there is a continuous demand for the development of a technology to improve drying efficiency. Summary of the Invention [Problem to be solved by the invention]

[0007] Therefore, the present invention provides a method for producing a superabsorbent resin that can produce a hydrogel polymer using a specific additive in the polymerization stage, thereby showing excellent drying efficiency in the subsequent drying process and finally realizing excellent water absorption properties. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention provides forming a hydrogel polymer by cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group in the presence of an internal cross-linking agent, a polymerization initiator, sodium dodecyl sulfate and a reducing agent; and drying the hydrogel polymer to produce a base resin; The reducing agent is at least one selected from the group consisting of oxalic acid, sodium metabisulfite, and sodium benzoate; After classifying the base resin with a 4 mesh sieve according to ASTM E11, the wet ratio, defined as the mass ratio of the base resin not filtered through the sieve, is 3 wt% or less; A method for producing a superabsorbent resin is provided. Effect of the Invention

[0009] According to the method for producing a superabsorbent polymer of the present invention, a specific reducing agent and sodium dodecyl sulfate are combined in the polymerization step to produce a hydrogel polymer, which increases the polymerization rate to form micropores inside the polymer, thereby providing excellent drying efficiency in the subsequent drying step and controlling the wet rate of the base resin within a desired range, thereby providing a method for producing a superabsorbent polymer that can ultimately achieve excellent water absorption properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention.

[0011] The singular expression includes the plural expression unless the context clearly indicates otherwise. It should be understood that, in this specification, the terms "comprise", "comprise", "have" and the like are intended to specify the presence of embodied features, steps, components, or combinations thereof, and do not preclude the possibility of the presence or addition of one or more other features, steps, components, or combinations thereof.

[0012] The terms first, second, third, etc. are used to describe various elements, and such terms are used only to distinguish one element from another.

[0013] Although the present invention can be modified in various ways and has various forms, specific embodiments are exemplified and described in detail below. However, it is not intended to limit the present invention to the specific disclosed embodiments, and it should be understood that the present invention includes all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.

[0014] The term "polymer" or "polymeric polymer" as used herein means a state in which a water-soluble ethylenically unsaturated monomer is polymerized, and may include any range of water content or particle size. Among the above polymers, a polymer having a water content (water content) of about 40% by weight or more in a state after polymerization and before drying may be called a hydrogel polymer, and particles of such a hydrogel polymer that have been crushed and dried may be called a crosslinked polymer.

[0015] In addition, the term "crosslinked polymer" means a polymer obtained by crosslinking polymerization in the presence of the water-soluble ethylenically unsaturated monomer and an internal crosslinking agent, and the term "base resin" means a material containing such a crosslinked polymer.

[0016] In addition, the term "super absorbent polymer" refers to a crosslinked polymer obtained by polymerizing a water-soluble ethylenically unsaturated monomer containing an acidic group and at least a part of the acidic group being neutralized, or a base resin obtained by drying the crosslinked polymer, or is used to encompass all of the crosslinked polymers or base resins that have been subjected to additional processes, such as surface crosslinking, fine powder regranulation, drying, pulverization, classification, etc., to be in a state suitable for commercialization.

[0017] In addition, the term "super absorbent resin powder" refers to a particulate material that includes a crosslinked polymer obtained by polymerizing a water-soluble ethylenically unsaturated monomer that contains acidic groups and at least a portion of the acidic groups have been neutralized, and crosslinking the polymer with an internal crosslinking agent.

[0018] A method for producing a superabsorbent resin according to one embodiment of the present invention includes the steps of: cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group in the presence of an internal cross-linking agent, a polymerization initiator, sodium dodecyl sulfate, and a reducing agent to form a hydrogel polymer; and drying the hydrogel polymer to produce a base resin.

[0019] Recently, as sanitary materials such as diapers and sanitary napkins are becoming thinner, high water absorption performance is required from superabsorbent resins. In particular, various methods are being considered to improve the centrifugation retention capacity (CRC), which is a physical property that indicates the basic water absorption and water retention capacity of superabsorbent resins. However, in order to improve the centrifugation retention capacity (CRC) of superabsorbent resins even after surface crosslinking, it is necessary to further improve the centrifugation retention capacity (CRC) of the base resin, and for this purpose, a method of controlling the content of the internal crosslinking agent to a low level is being considered. However, when the content of the internal crosslinking agent is reduced, there is a problem that the stickiness of the polymer increases and drying is not performed well in the subsequent drying process. Specifically, there is a problem that the porosity in the drying layer is significantly reduced during the drying process due to the increase in the cohesive force of the hydrogel polymer, and only the outer periphery of the drying layer is dried, and the inside is not sufficiently dried. In addition, there is a problem that the hot air differential pressure of the drying layer increases due to the decrease in the porosity of the drying layer, and in order to achieve the desired degree of drying rate, the drying temperature must be excessively increased or the drying time must be long, resulting in a significant decrease in process efficiency. Ultimately, it was difficult to achieve the desired water absorption properties.

[0020] Therefore, the present inventors discovered that by using a combination of a specific reducing agent and sodium dodecyl sulfate in the hydrogel polymer formation stage, the polymerization rate can be increased to effectively form fine pores inside the polymer, and appropriate voids can be formed in the drying layer in the subsequent drying process, thereby making it possible to control the wet rate of the base resin within a desired range, and thus completed the present invention.

[0021] The superabsorbent resin produced by the present invention can realize excellent water absorption properties, and in particular has excellent drying rate and centrifuge retention capacity (CRC).

[0022] Hereinafter, each step of the method for producing a superabsorbent resin according to an embodiment of the present invention will be described in detail.

[0023] (Polymerization stage) A method for producing a superabsorbent resin according to an embodiment of the present invention includes a step of cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group in the presence of an internal cross-linking agent, a polymerization initiator, sodium dodecyl sulfate, and a reducing agent to form a hydrogel polymer.

[0024] Specifically, the process involves thermally or photopolymerizing a monomer composition containing an internal crosslinking agent, a polymerization initiator, sodium dodecyl sulfate, a specific reducing agent, and a monomer mixture to form a hydrogel polymer.

[0025] Here, the use of sodium dodecyl sulfate can promote the formation of fine bubbles during the formation of a hydrogel polymer, and at the same time, the use of a specific reducing agent in combination can promote the polymerization reaction and effectively capture the fine pores formed inside the polymer at a high polymerization rate, thereby enabling the wet rate of the base resin to be controlled within a desired range with excellent drying efficiency in the subsequent drying process.

[0026] The reducing agent can be one or more selected from the group consisting of oxalic acid, sodium metabisulfite, and sodium benzoate.

[0027] The reducing agent is contained in the range of 500 ppmw to 10,000 ppmw based on the weight of the water-soluble ethylenically unsaturated monomer, and within the range, the aggregation of the hydrogel polymer can be controlled within an appropriate range.Preferably, the reducing agent is contained in the range of 500 ppmw or more, 800 ppmw or more, 900 ppmw or more, or 1,000 ppmw or more, and 10,000 ppmw or less, 8,000 ppmw or less, 7,000 ppmw or less, or 5,000 ppmw or less, and may be contained in the range of 800 ppmw to 8,000 ppmw, 900 ppmw to 7,000 ppmw, or 1,000 ppmw to 5,000 ppmw, and within the range, the above-mentioned effects can be further improved.

[0028] The sodium dodecyl sulfate may be contained in an amount of 500 ppmw to 10,000 ppmw based on the weight of the water-soluble ethylenically unsaturated monomer, and when used together with a reducing agent in the above range, it can effectively form micropores inside the hydrogel polymer.Preferably, it is 500 ppmw or more, 800 ppmw or more, 900 ppmw or more, or 1,000 ppmw or more, and 10,000 ppmw or less, 8,000 ppmw or less, 7,000 ppmw or less, or 5,000 ppmw or less, and may be contained in an amount of 800 ppmw to 8,000 ppmw, 900 ppmw to 7,000 ppmw, or 1,000 ppmw to 5,000 ppmw, and within the above range, the above-mentioned effects can be further improved.

[0029] The water-soluble ethylenically unsaturated monomer may be any monomer commonly used in the manufacture of superabsorbent resins. As a non-limiting example, the water-soluble ethylenically unsaturated monomer may be a compound represented by the following formula 1:

[0030] [Chemical formula 1] R1-COOM 1

[0031] In the above Chemical Formula 1, R1 is an alkyl group having 2 to 5 carbon atoms and containing an unsaturated bond, M 1 is a hydrogen atom, a monovalent or divalent metal, an ammonium group, or an organic amine salt.

[0032] Preferably, the monomer may be at least one selected from the group consisting of acrylic acid, methacrylic acid, and monovalent metal salts, divalent metal salts, ammonium salts, and organic amine salts of these acids. In this way, when acrylic acid or a salt thereof is used as the water-soluble ethylenically unsaturated monomer, it is advantageous to obtain a highly water-absorbent resin having improved water absorption. In addition, the monomer may be at least one selected from the group consisting of anionic monomers and salts thereof, such as maleic anhydride, fumaric acid, crotonic acid, itaconic acid, 2-acryloylethanesulfonic acid, 2-methacryloylethanesulfonic acid, 2-(meth)acryloylpropanesulfonic acid, or 2-(meth)acrylamido-2-methylpropanesulfonic acid; nonionic hydrophilic monomers, such as (meth)acrylamide, N-substituted (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, or polyethylene glycol (meth)acrylate; and amino group-containing unsaturated monomers, such as (N,N)-dimethylaminoethyl (meth)acrylate or (N,N)-dimethylaminopropyl (meth)acrylamide, and quaternized products thereof.

[0033] Here, the water-soluble ethylenically unsaturated monomer has an acidic group, and at least a part of the acidic group is partially neutralized using the neutralizing solution of the present invention described above.

[0034] At this time, the neutralization degree of the monomer may be 40 to 95 mol%, or 40 to 80 mol%, or 45 to 75 mol%, as described above. The range of the neutralization degree varies depending on the final properties, but if the neutralization degree is too high, the neutralized monomer may precipitate and the polymerization may not proceed smoothly, and conversely, if the neutralization degree is too low, the water absorption of the polymer may be significantly reduced and the polymer may exhibit properties similar to elastic rubber, which are difficult to handle.

[0035] The term "internal crosslinking agent" used in this specification is used to distinguish it from the "surface crosslinking agent" for crosslinking the surface of the base resin, and plays a role in crosslinking and polymerizing the unsaturated bonds of the water-soluble ethylenically unsaturated monomers described above. The crosslinking in this step is performed regardless of whether it is on the surface or inside, but the surface of the superabsorbent resin particles finally produced by the surface crosslinking process of the base resin described below has a structure crosslinked by the surface crosslinking agent, and the inside has a structure crosslinked by the internal crosslinking agent.

[0036] The internal crosslinking agent may be a polyfunctional component, and for example, one or more selected from the group consisting of N,N'-methylenebisacrylamide, trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol (meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipentaerythritol pentaacrylate, glycerin tri(meth)acrylate, pentaerythritol tetraacrylate, triarylamine, ethylene glycol diglycidyl ether, propylene glycol, glycerin, and ethylene carbonate may be used. Preferably, ethylene glycol diglycidyl ether can be used.

[0037] The internal crosslinking agent can be used at 50 ppmw to 1,000 ppmw based on the weight of the water-soluble ethylenically unsaturated monomer. When the content is within the above range, sufficient crosslinking can be achieved to achieve strength above an appropriate level, and sufficient water retention can be achieved by introducing an appropriate crosslinked structure. Preferably, the content is 100 ppmw or more, 200 ppmw or more, 300 ppmw or more, or 600 ppmw or more, and 1,000 ppmw or less or 800 ppmw or less, and includes 200 ppmw to 1,000 ppmw, 200 ppmw to 800 ppmw, or 600 ppmw to 800 ppmw. If the content of the internal crosslinking agent is too low, crosslinking may not occur sufficiently, making it difficult to achieve strength above an appropriate level, and drying efficiency may be significantly reduced, and if the content of the internal crosslinking agent is too high, the internal crosslinking density may be high, making it difficult to achieve the desired water retention.

[0038] The polymerization initiator may be a radical polymerization initiator, which initiates the polymerization reaction and, when used together with the reducing agent component, facilitates the formation of fine bubbles in the polymer by increasing the polymerization reaction rate.

[0039] Examples of the polymerization initiator include 2,2-azobis(2-amidinopropane) dihydrochloride, 2,2-azobis-(N,N-dimethylene)isobutyramidine dihydrochloride, 2-(carbamoylazo)isobutylonitrile, and 2,2-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 4,4-azobis-(4-cyanovaleric acid), One or more compounds selected from the group consisting of azo compounds such as 2,2-azobis-(2-amidinopropane) dihydrochloride and sodium persulfate can be used.

[0040] The polymerization initiator may be included in an amount of 500 ppmw to 10,000 ppmw based on the weight of the water-soluble ethylenically unsaturated monomer, and when used together with a reducing agent in the above range, it can promote the polymerization reaction and effectively form micropores inside the hydrogel polymer. Preferably, it is 500 ppmw or more, 750 ppmw or more, 800 ppmw or more, or 1,000 ppmw or more, and 10,000 ppmw or less, 8,000 ppmw or less, 7,000 ppmw or less, 5,000 ppmw or less, or 1,000 ppmw or less, and may be 500 ppmw to 8,000 ppmw, 500 ppmw to 1,000 ppmw, 750 ppmw to 1,000 ppmw, 800 ppmw to 8,000 ppmw, 1,000 ppmw to 5,000 ppmw, or 1,500 ppmw to 4,500 ppmw, and within the above ranges, the above-mentioned effects can be further improved.

[0041] As the polymerization initiator, in addition to the above-mentioned radical initiators, a photopolymerization initiator or the like can be used.

[0042] The photopolymerization initiator may be, for example, one or more compounds selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyl alkyl ketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone. Specific examples of acylphosphine include diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and ethyl(2,4,6-trimethylbenzoyl)phenylphosphinate. More various photoinitiators are described in detail in "UV Coatings: Basics, Recent Developments and New Application" (Elsevier, 2007), p. 115, by Reinhold Schwalm, and are not limited to the above-mentioned examples.

[0043] Such a photopolymerization initiator can be added in an amount of 10 ppmw to 30,000 ppmw, preferably 30 ppmw to 10,000 ppmw, or 50 ppmw to 5,000 ppmw, based on the weight of the water-soluble ethylenically unsaturated monomer.

[0044] In addition, the monomer composition may further contain additives such as a foaming agent, a thickener, a plasticizer, a storage stabilizer, and an antioxidant, if necessary.

[0045] The foaming agent plays a role in increasing the surface area by forming pores in the hydrogel polymer through foaming during polymerization. The foaming agent may be a carbonate, for example, sodium bicarbonate, sodium carbonate, potassium bicarbonate, potassium carbonate, calcium bicarbonate, calcium carbonate, magnesium bicarbonate, or magnesium carbonate. A commercially available foaming agent that can be used is, but is not limited to, F-36D, which is an encapsulated foaming agent.

[0046] In addition, the foaming agent is preferably used in an amount of 1,500 ppmw or less based on the weight of the water-soluble ethylenically unsaturated monomer. If the amount of foaming agent used exceeds 1,500 ppmw, the number of pores may be excessively increased, the gel strength of the superabsorbent resin may decrease, and the density may decrease, which may cause problems in distribution and storage. In addition, the foaming agent is preferably used in an amount of 500 ppmw or more, or 1,000 ppmw or more based on the weight of the water-soluble ethylenically unsaturated monomer.

[0047] The monomer composition may be prepared in the form of a solution in which raw materials such as the reducing agent, the internal crosslinking agent, the water-soluble ethylenically unsaturated monomer, and the polymerization initiator are dissolved in a solvent.

[0048] In this case, the solvent that can be used is not limited in composition as long as it can dissolve the above-mentioned raw materials. For example, the solvent may be water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, N,N-dimethylacetamide, or a mixture thereof.

[0049] The step of forming the hydrogel polymer by polymerization of the monomer composition is carried out by a conventional polymerization method, and the process is not particularly limited. As a non-limiting example, the polymerization method is largely divided into thermal polymerization and photopolymerization according to the type of polymerization energy source, and when the thermal polymerization is carried out, it is carried out in a reactor having a stirring shaft such as a kneader, and when the photopolymerization is carried out, it is carried out in a reactor equipped with a movable conveyor belt.

[0050] As an example, the monomer composition is charged into a reactor such as a kneader equipped with an agitator shaft, and hot air is supplied thereto or the reactor is heated to thermally polymerize the monomer composition, thereby obtaining a hydrogel polymer. At this time, depending on the type of the agitator shaft equipped in the reactor, the hydrogel polymer discharged from the outlet of the reactor is obtained as particles of several millimeters to several centimeters in size. Specifically, the obtained hydrogel polymer is obtained in various forms depending on the concentration of the monomer composition injected and the injection speed, but usually, a hydrogel polymer having a (weight average) particle size of 2 to 50 mm is obtained.

[0051] As another example, when the photopolymerization of the monomer composition is carried out in a reactor equipped with a movable conveyor belt, a sheet-like hydrogel polymer is obtained. In this case, the thickness of the sheet varies depending on the concentration and injection speed of the monomer composition to be injected, but it is generally preferable to adjust the thickness to 0.5 to 10 cm in order to ensure the production speed while allowing the entire sheet to be evenly polymerized.

[0052] The water content of the hydrogel polymer obtained by this method may be 40% to 80% by weight. Meanwhile, throughout this specification, the term "water content" refers to the water content relative to the weight of the entire hydrogel polymer, and means the weight of the hydrogel polymer minus the weight of the polymer in a dry state. Specifically, it is defined as a value calculated by measuring the weight loss due to evaporation of water in the polymer during the process of drying by increasing the temperature of the polymer using infrared heating. At this time, the drying conditions are a method of increasing the temperature from room temperature to 180°C and then maintaining it at 180°C, and the total drying time is set to 20 minutes, including 5 minutes for the temperature increase stage, and the water content is measured.

[0053] (Drying stage) Next, the hydrogel polymer is dried to produce a base resin.

[0054] If necessary, the hydrogel polymer may be coarsely pulverized before drying in order to increase the efficiency of the drying step. The pulverizer used is not limited in structure, and may include any one selected from the group of pulverizing devices consisting of a vertical pulverizer, a turbo cutter, a turbo grinder, a rotary cutter mill, a cutter mill, a disc mill, a shred crusher, a crusher, a chopper, and a disc cutter, but is not limited to the above examples.

[0055] The drying step is a step of removing water from the hydrogel polymer to produce a base resin having a desired particle size. By using a specific reducing agent in the polymerization step, fine pores are easily formed inside the polymer, which forms appropriate voids in the structure and improves the drying efficiency of the drying step.

[0056] At this time, the drying temperature in the drying step may be 150° C. to 250° C. As described above, by using a specific reducing agent in the polymerization step, excellent drying efficiency can be achieved even under relatively mild drying conditions, and thus the wet rate of the base resin can be controlled within a desired range.

[0057] On the other hand, if the drying temperature is less than 150°C, the drying time becomes too long, which may deteriorate the properties of the final superabsorbent resin, and if the drying temperature exceeds 250°C, only the surface of the polymer may be dried excessively, which may cause fine powder to be generated in the subsequent pulverization process, resulting in increased process costs and reduced economic efficiency. The drying is preferably performed at a temperature of 150°C to 200°C, more preferably at a temperature of 150°C to 185°C. The drying can be performed in multiple stages at different temperatures within the above temperature range.

[0058] The drying step is performed for 30 to 60 minutes. If the drying step time is less than 30 minutes, the inside of the drying layer to be dried is not sufficiently dried, making it difficult to achieve the desired non-drying rate, and if it exceeds 60 minutes, the drying efficiency is reduced and polymer deterioration may occur in some particles. If drying is performed in multiple stages, the time of the drying step is the sum of the implementation times of each stage.

[0059] The drying step is preferably performed by hot air drying, which means drying with hot air satisfying the above-mentioned temperature range. The number of times hot air is introduced in the drying step is not particularly limited, and hot air may be introduced several times as long as the total drying time satisfies the above-mentioned range.

[0060] The drying is performed in a fixed-bed type, which refers to a method in which the material to be dried is suspended at the bottom of a perforated plate through which air can pass, and hot air passes over the material from bottom to top. Specifically, the drying is performed using a ventilated belt dryer equipped with a perforated plate. Specifically, the chopped mixture to be dried is placed on a perforated plate, whereby upward airflow means airflow from below the perforated plate to the top, and downward airflow means airflow from above the chopped mixture placed on the perforated plate to the bottom.

[0061] The hot air drying is carried out by introducing hot air having a linear velocity of 0.5 m / s to 3.0 m / s, 0.7 m / s to 2.5 m / s, or 0.85 m / s to 2.0 m / s. When the above speed range is satisfied, the object to be dried can be dried uniformly to the inside, which is preferable. When the linear velocity is less than 0.5 m / s, it is difficult for the hot air to reach the inside of the object to be dried, and when it exceeds 3.0 m / s, the object to be dried may be scattered inside the dryer.

[0062] The wet ratio of the base resin produced through the drying step is 3 wt% or less. The wet ratio indicates the degree of drying of crumb-shaped powder, which is relatively large in size and difficult to dry in the base resin, and is one of the indicators of drying efficiency.

[0063] Specifically, it means the mass ratio of the base resin that is not filtered through a 4 mesh sieve according to ASTM E11, and the particles that are not filtered after 10 minutes or more of classification through a 4 mesh sieve are not sufficiently dried and re-agglomerated due to internal moisture. In fact, the moisture content of the particles that are not filtered through a 4 mesh sieve after 10 minutes or more of classification is 10% or more.

[0064] The smaller the wet ratio, the better, and the lower limit of the wet ratio is 0wt%. Preferably, the wet ratio is 0wt% or more, 0.001wt% or more, 0.001wt% or more, 0.1wt% or more, 3wt% or less, 1wt% or less, 0.7wt% or less, 0.5wt% or less, 0wt% to 3wt%, 0wt% to 1wt%, 0.01wt% to 3w%, 0.01wt% to 1wt%, or 0.01wt% to 0.7wt%. The method for measuring the wet ratio of the base resin will be described in more detail in the experimental examples described later.

[0065] The base resin has a centrifugation water retention capacity (CRC) of 60.0 g / g or more, preferably 62.0 g / g or more, 90.0 g / g or less, 87.0 g / g or less, 60 g / g to 90 g / g, or 62 g / g to 87 g / g, as measured by EDENA method WSP241.3. A specific method for measuring the centrifugation water retention capacity will be described in more detail in the experimental examples described later.

[0066] (Crushing and classification stage) As described above, the base resin thus prepared exhibits excellent drying efficiency, and allows the production of a resin having a desired particle size by only a sieve classification process. Therefore, the process may optionally further include a step of crushing and classifying the base resin.

[0067] The polymer powder obtained after the pulverization step may have a particle size of 150 to 850 μm. Specifically, the pulverizer used for pulverizing to such a particle size may be a pin mill, a hammer mill, a screw mill, a roll mill, a disc mill, a jog mill, or the like, but is not limited to the above examples.

[0068] After the pulverization step, a separate process of classifying the polymer powder obtained after pulverization according to particle size can be performed in order to control the physical properties of the superabsorbent resin powder to be manufactured into a final product. Preferably, the polymer having a particle size of 150 to 850 μm is classified, and only the polymer powder having such a particle size can be manufactured into a product through a surface crosslinking reaction step. More specifically, the base resin that has been classified has a particle size of 150 to 850 μm and may contain 50% by weight or more of particles having a particle size of 300 to 600 μm.

[0069] (Surface cross-linking stage) Next, the method for preparing a superabsorbent resin according to an embodiment of the present invention further includes a step of heat-treating the base resin in the presence of a surface cross-linking agent to cross-link a portion of the surface of the base resin.

[0070] The surface cross-linking step induces a cross-linking reaction on the surface of the base resin in the presence of a surface cross-linking agent, and the unsaturated bonds of the water-soluble ethylenically unsaturated monomer remaining on the surface without being cross-linked are cross-linked by the surface cross-linking agent to form a superabsorbent resin with a high surface cross-linking density.

[0071] Specifically, a surface cross-linked layer is formed in a heat treatment process in the presence of a surface cross-linking agent, and the heat treatment process increases the surface cross-linking density, i.e., the external cross-linking density, while the internal cross-linking density remains unchanged. Thus, the produced superabsorbent resin having a surface cross-linked layer has a structure in which the external cross-linking density is higher than the internal cross-linking density.

[0072] In the surface cross-linking step, a surface cross-linking agent composition containing an alcohol-based solvent and water in addition to a surface cross-linking agent may be used.

[0073] On the other hand, as the surface cross-linking agent contained in the surface cross-linking agent composition, any cross-linking agent component that has been used in the manufacture of superabsorbent resins can be used without any particular limitation. For example, the surface cross-linking agent can include one or more polyols selected from the group consisting of ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,2-hexanediol, 1,3-hexanediol, 2-methyl-1,3-propanediol, 2,5-hexanediol, 2-methyl-1,3-pentanediol, 2-methyl-2,4-pentanediol, tripropylene glycol and glycerol; one or more carbonate-based compounds selected from the group consisting of ethylene carbonate and propylene carbonate; epoxy compounds such as ethylene glycol diglycidyl ether; oxazoline compounds such as oxazolidinone; polyamine compounds; mono-, di- or polyoxazolidinone compounds; or cyclic urea compounds; and the like. Preferably, the same internal crosslinking agent as described above can be used, for example, a diglycidyl ether compound of an alkylene glycol such as ethylene glycol diglycidyl ether can be used.

[0074] Such a surface cross-linking agent can be used in an amount of 0.001 to 2 parts by weight per 100 parts by weight of the base resin. Preferably, the amount is 0.005 parts by weight or more, 0.01 parts by weight or more, or 0.02 parts by weight or more and 0.5 parts by weight or less, or 0.3 parts by weight or less. By adjusting the content range of the surface cross-linking agent to the above-mentioned range, a highly water-absorbent resin exhibiting various physical properties such as excellent water absorption performance and liquid permeability can be produced.

[0075] Meanwhile, the surface crosslinking agent is added to the base resin in the form of a surface crosslinking agent composition containing the surface crosslinking agent, and the method of adding such a surface crosslinking agent composition is not particularly limited in its constitution. For example, a method of putting the surface crosslinking agent composition and the base resin in a reaction tank and mixing them, a method of spraying the surface crosslinking agent composition to the base resin, a method of continuously supplying the base resin and the surface crosslinking agent composition to a continuously operated mixer, and the like can be used.

[0076] The surface crosslinking agent composition may further include water and / or a hydrophilic organic solvent as a medium. This has the advantage that the surface crosslinking agent can be uniformly dispersed on the base resin. At this time, the content of water and the hydrophilic organic solvent can be adjusted and applied by controlling the addition ratio with respect to 100 parts by weight of the base resin for the purpose of inducing uniform dissolution / dispersion of the surface crosslinking agent and preventing the clumping phenomenon of the base resin, while optimizing the surface penetration depth of the surface crosslinking agent.

[0077] The surface cross-linking step can be carried out by heat treatment for 30 minutes or more at a temperature of 110° C. to 200° C., or 110° C. to 150° C. More specifically, the surface cross-linking can be carried out by setting the above-mentioned temperature as the maximum reaction temperature and heat treating at such maximum reaction temperature for 30 to 80 minutes, or 40 to 70 minutes to allow the surface cross-linking reaction to proceed.

[0078] By satisfying such surface cross-linking step conditions (particularly, the temperature rise conditions and the reaction conditions at the maximum reaction temperature), a highly water-absorbent resin that appropriately satisfies physical properties such as excellent pressurized liquid permeability can be produced.

[0079] The temperature raising means for the surface crosslinking reaction is not particularly limited. Heating can be performed by supplying a heat medium or directly supplying a heat source. At this time, the type of heat medium that can be used can be a heated fluid such as steam, hot air, hot oil, etc., but is not limited to these, and the temperature of the heat medium to be supplied can be appropriately selected in consideration of the means of the heat medium, the heating rate, and the target temperature of the heat raising. On the other hand, the heat source to be directly supplied can be, but is not limited to the above-mentioned examples, heating by electricity and heating by gas.

[0080] Meanwhile, in the method for producing a superabsorbent resin according to an embodiment of the present invention, various polyvalent metal salts, such as aluminum salts, such as aluminum sulfate salts, may be further used during surface cross-linking in order to further improve liquid permeability, etc. Such polyvalent metal salts may be included on the surface cross-linked layer of the finally produced superabsorbent resin.

[0081] (Super absorbent resin) The superabsorbent resin produced according to the above-mentioned embodiment may have a particle size of 150 to 850 μm. More specifically, at least 95% by weight of the superabsorbent resin may have a particle size of 150 to 850 μm, and may contain 50% by weight or more of particles having a particle size of 300 to 600 μm, and may contain less than 3% by weight of fine powder having a particle size of less than 150 μm.

[0082] The highly absorbent resin produced according to the embodiment described above realizes excellent water absorption properties, and in particular has excellent centrifugal water retention capacity and pressurized water absorption capacity.

[0083] The functions and effects of the present invention will be described in more detail below through specific examples of the present invention, however, these examples are merely presented as examples of the present invention and do not define the scope of the invention.

[0084] [Example] <Production of superabsorbent resin> Example 1 (Stage 1) In a 3L glass container equipped with a stirrer and a thermometer, 500g of acrylic acid, 600ppmw of ethylene glycol diglycidyl ether as an internal crosslinking agent (relative to 100 parts by weight of acrylic acid), 5,000ppmw of oxalic acid as an acrylic acid reducing agent, and 80ppmw of diphenyl(2,4,6-trimethylbenzoyl)-phosphine oxide as a photopolymerization initiator (relative to 100 parts by weight of acrylic acid) were added and dissolved, and then 627g of 31.5wt% caustic soda solution was added to prepare a water-soluble unsaturated monomer aqueous solution (neutralization degree: 70mol%; solid content: 44.9wt%). When the temperature of the water-soluble unsaturated monomer aqueous solution rises due to the heat of neutralization and reaches 40°C, the mixture is placed in a container containing 750 ppmw (based on 100 parts by weight of acrylic acid) of the radical polymerization initiator 2,2-azobis-(2-amidinopropane) dihydrochloride, 1,000 ppmw (based on 100 parts by weight of acrylic acid) of the blowing agent F36D, and 1,000 ppmw (based on 100 parts by weight of acrylic acid) of sodium dodecyl sulfate, and then irradiated with ultraviolet light for 1 minute (irradiation dose: 10 mV / cm 2 ) and UV polymerization was carried out to obtain a hydrous gel-like polymer sheet.

[0085] The obtained hydrogel polymer sheet was passed through a chopper with a hole size of 16 mm to produce crumbs.

[0086] Next, the crumbs were dried in an oven capable of shifting airflow from up to down. The drying was carried out in multiple stages, specifically, using an air flow oven at 150°C for 13 minutes, 170°C for 5 minutes, 175°C for 5 minutes, 180°C for 5 minutes, and 160°C for 5 minutes. Through the drying process, a superabsorbent resin containing a base resin was produced.

[0087] Examples 2 to 5 and Comparative Examples 1 to 7 A superabsorbent resin was prepared in the same manner as in Example 1, except that the components and amounts shown in Table 1 below were used in the polymerization step.

[0088] [Table 1]

[0089] <Experimental Example> The properties of the superabsorbent resins containing the base resin produced in the above Examples and Comparative Examples were evaluated by the following methods. The results are shown in Table 2.

[0090] (1)Centrifuge Retention Capacity (CRC) The base resins prepared in the examples and comparative examples were sampled to have a particle size of 150 to 850 μm, and the centrifuge retention capacity (CRC) was measured based on the no-load water absorption capacity according to the European Disposables and Nonwovens Association (EDANA) standard EDANA WSP241.2.

[0091] Specifically, the base resin obtained in each of the examples and comparative examples was classified with a sieve of #30-50 to obtain a resin. Such resin W0(g) (about 0.2g) was evenly placed in a nonwoven fabric envelope, sealed, and then immersed in physiological saline (0.9% by weight) at room temperature. After 30 minutes, the envelope was drained for 3 minutes under conditions of 250G using a centrifuge, and the mass W2(g) of the envelope was measured. The same operation was also performed without using the resin, and the mass W1(g) at that time was measured. Using each of the obtained masses, the CRC(g / g) was calculated according to the following formula 1.

[0092] [Formula 1] CRC(g / g)={[W2(g)-W1(g)] / W0(g)}-1

[0093] (2) Wetness rate evaluation The wet ratio of the base resins prepared in the examples and comparative examples was evaluated according to Equation 2, and the results are shown in Table 2.

[0094] Specifically, the base resin sample (A1) was classified for 10 minutes using a 4 mesh sieve according to ASTM E11 to obtain a sample (A2) that was not filtered through the sieve relative to the initial weight A'1 (g) of the base resin sample (A1), and the ratio of the weight A'2 (g) of the sample that was not filtered through the sieve was measured.

[0095] [Formula 2] Undried rate (wt%)={[A'1(g)-A'2(g)] / A'1(g)}×100

[0096] [Table 2]

[0097] As can be seen from the data in Table 2, it was confirmed that the embodiment of the manufacturing method of the present invention can simultaneously achieve excellent drying efficiency and CRC properties by using a combination of a specific reducing agent compound and sodium dodecyl sulfate in the polymerization step.

[0098] In the case of Comparative Example 1, where the reducing agent of the present invention was not used, it was confirmed that internal air bubbles of the polymer were not sufficiently formed, and the wet ratio increased due to re-agglomeration of particles during the drying process.

[0099] In the case of Comparative Examples 2 to 6, which contained the same reducing agent compound as the present invention but were used in the grinding step rather than the polymerization step, it was confirmed that the wet ratio increased significantly and the CRC value of the base resin was slightly lower than that of the Examples.

[0100] In addition, in the case of Comparative Example 7 which did not contain SDS, it was confirmed that the wet rate value increased because it was difficult to form bubbles inside the polymer, and the CRC value also decreased compared to the Examples.

Claims

1. forming a hydrogel polymer by cross-linking and polymerizing a water-soluble ethylenically unsaturated monomer having at least a partially neutralized acidic group in the presence of an internal cross-linking agent, a polymerization initiator, sodium dodecyl sulfate and a reducing agent; and drying the hydrogel polymer to produce a base resin; the reducing agent is at least one selected from the group consisting of oxalic acid, sodium metabisulfite, and sodium benzoate; The base resin is classified using a 4 mesh sieve according to ASTM E11, and then the wet ratio, which is defined as the mass ratio of the base resin that is not filtered through the sieve, is 3 wt % or less. A method for producing a superabsorbent resin.

2. The wet ratio of the base resin is 1 wt % or less. A method for producing the highly water-absorbent resin according to claim 1.

3. The base resin has a centrifugal retention capacity (CRC) according to EDENA method WSP241.3 of 60.0 g / g or more; A method for producing the highly water-absorbent resin according to claim 1.

4. The reducing agent is contained in an amount of 500 ppmw to 10,000 ppmw based on the weight of the water-soluble ethylenically unsaturated monomer. A method for producing the highly water-absorbent resin according to claim 1.

5. The sodium dodecyl sulfate is contained in an amount of 500 ppmw to 10,000 ppmw based on the weight of the ethylenically unsaturated monomer. A method for producing the highly water-absorbent resin according to any one of claims 1 to 4.

6. The internal crosslinking agent is at least one selected from the group consisting of N,N'-methylenebisacrylamide, trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol (meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol (meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipentaerythritol pentaacrylate, glycerin tri(meth)acrylate, pentaerythritol tetraacrylate, triarylamine, ethylene glycol diglycidyl ether, propylene glycol, glycerin, and ethylene carbonate. A method for producing the highly water-absorbent resin according to claim 1.

7. The internal crosslinking agent is contained in an amount of 50 ppmw to 1,000 ppmw based on the weight of the water-soluble ethylenically unsaturated monomer. A method for producing the highly water-absorbent resin according to claim 1.

8. The polymerization initiator is 2,2-azobis(2-amidinopropane) dihydrochloride, 2,2-azobis(N,N-dimethylene)isobutyramide dihydrochloride azo compounds such as 2,2-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2-(carbamoylazo)isobutyronitrile, and 2,2-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 4,4-azobis-(4-cyanovaleric acid); and Selected from the group consisting of persulfate compounds including sodium persulfate, potassium persulfate, and ammonium persulfate; A method for producing the highly water-absorbent resin according to claim 1.

9. The polymerization initiator is contained in an amount of 500 ppmw to 10,000 ppmw based on the weight of the water-soluble ethylenically unsaturated monomer. A method for producing the highly water-absorbent resin according to claim 1.

10. The method further comprises the step of heat-treating the base resin in the presence of a surface cross-linking agent to cross-link a portion of the surface of the base resin. A method for producing the highly water-absorbent resin according to claim 1.

Citation Information

Patent Citations

  • Absorbent polymer with high liquid permeability and low caking tendency and preparation method thereof

    CN113004550A