Carbon composite for positive electrode of lithium-sulfur battery and method for producing same

A carbon composite with vanadium nitride particles on a porous carbon material addresses the issue of lithium polysulfide elution in lithium-sulfur batteries by catalyzing its conversion to lithium sulfide, enhancing battery performance and stability.

JP2024536011AActive Publication Date: 2024-10-04LG ENERGY SOLUTION LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024514707
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-12-28
Filing Date
2023-03-30
Publication Date
2024-10-04
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Lithium polysulfide elution during charging and discharging in lithium-sulfur batteries leads to decreased battery capacity and cell deterioration, and existing efforts to support sulfur in porous carbon materials have limitations in promoting the conversion of lithium polysulfide to lithium sulfide.

Method used

A carbon composite comprising a porous carbon material with vanadium nitride particles on its surface, which acts as a catalyst to rapidly convert lithium polysulfide to lithium sulfide, enhancing the performance of lithium-sulfur batteries.

Benefits of technology

The carbon composite effectively prevents lithium polysulfide elution by promoting its conversion to lithium sulfide, improving the battery's performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536011000001_ABST
    Figure 2024536011000001_ABST
Patent Text Reader

Abstract

The present invention relates to a carbon composite for use in a positive electrode of a lithium-sulfur battery and a method for producing the same, the carbon composite comprising a porous carbon material and vanadium nitride particles located on a surface of the porous carbon material. The lithium-sulfur battery using the carbon composite can rapidly convert lithium polysulfide into lithium sulfide, thereby improving the stability of the lithium-sulfur battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a carbon composite material for use in a positive electrode of a lithium-sulfur battery, and a method for producing the same.

[0002] This application claims priority to Korean Patent Application No. 2022-0110385 filed on August 31, 2022 and Korean Patent Application No. 2022-0187899 filed on December 28, 2022, and the contents disclosed in the specification and drawings of said applications are incorporated herein in their entirety. [Background technology]

[0003] Lithium-sulfur batteries refer to battery systems that use sulfur-based materials with sulfur-sulfur bonds as the positive electrode active material and lithium metal as the negative electrode active material. Sulfur, the main material of the positive electrode active material, is an abundant resource worldwide, is non-toxic, and has the advantage of having a low atomic weight.

[0004] As the application areas of secondary batteries expand to electric vehicles (EVs) and energy storage systems (ESSs), lithium-sulfur battery technology is in the spotlight because it can theoretically achieve a relatively high energy storage density (~2,600Wh / kg) relative to its weight, compared to lithium-ion secondary batteries, which have a relatively low energy storage density (~250Wh / kg) relative to their weight.

[0005] During discharge, lithium, the negative electrode active material, is oxidized as it gives off electrons and is ionized into lithium cations, while the positive electrode active material, the sulfur-based material, receives electrons and is reduced. Here, the S-S bond receives two electrons and is converted into the form of a sulfur anion through the reduction reaction of the sulfur-based material. The lithium cations generated by the oxidation reaction of lithium are transferred to the positive electrode via the electrolyte, and combine with the sulfur anions generated by the reduction reaction of the sulfur-based compound to form a salt. Specifically, sulfur before discharge has a cyclic S8 structure, which is converted into lithium polysulfide (Li2S) through a reduction reaction. x , x=8, 6, 4, 2, and the lithium polysulfides are completely reduced to produce lithium sulfide (Li2S).

[0006] However, lithium polysulfide generated during charging and discharging is easily dissolved into the electrolyte, causing a decrease in battery capacity and cell degradation. In order to solve the problem of lithium polysulfide dissolution, various efforts have been made to support sulfur in the pores of various porous carbon materials and use them as positive electrodes. In particular, since there is a problem with production costs in synthesizing and using carbon with a large specific surface area, efforts have been made to physically and chemically modify carbon materials with a low specific surface area and use them as positive electrodes.

[0007] However, although these efforts have solved the problem of lithium polysulfide leaching to some extent, there is still a problem that the reaction of converting lithium polysulfide into lithium sulfide (Li2S) cannot be promoted. Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a carbon composite for a positive electrode of a lithium-sulfur battery, which can promote the conversion of lithium polysulfide to lithium sulfide, and a method for producing the same. [Means for solving the problem]

[0009] In order to achieve the above object, according to one aspect of the present invention, there is provided a carbon composite having the following features.

[0010] A carbon composite according to a first embodiment includes a porous carbon material and vanadium nitride particles located on a surface of the porous carbon material.

[0011] According to a second aspect, the specific surface area of ​​the carbon composite is 250 m 2 / g or more.

[0012] According to a third aspect, the pore volume of the carbon composite is less than 1.0 cm 3 / g or more.

[0013] According to a fourth aspect, the carbon composite may be the carbon composite according to any one of the first to third aspects, in which the average pore size of the carbon composite is 10 nm or more.

[0014] According to a fifth aspect, the carbon composite may be the one according to any one of the first to fourth aspects, in which the vanadium nitride particles have an average particle size of 200 nm or less.

[0015] According to a sixth aspect, the carbon composite may be the carbon composite according to any one of the first to fifth aspects, in which the vanadium nitride particles are contained in an amount of 3 to 50 parts by weight per 100 parts by weight of the carbon composite.

[0016] According to a seventh aspect, the porous carbon material may be the carbon composite according to any one of the first to sixth aspects, comprising carbon nanotubes (CNTs), reduced graphene oxide (rGO), or a mixture thereof.

[0017] According to another aspect of the present invention, there are provided a positive electrode active material, a positive electrode, and a battery having the following embodiments.

[0018] A positive electrode active material according to an eighth aspect includes the carbon composite according to any one of the first to seventh aspects, and a sulfur-containing compound supported in pores of the carbon composite.

[0019] According to a ninth aspect, the positive electrode active material may be as described in the eighth aspect, in which a weight ratio of the sulfur-containing compound to the carbon composite is 1:1 to 9:1.

[0020] A positive electrode according to a tenth aspect includes a current collector and a positive electrode active material layer located on at least one surface of the current collector, the positive electrode active material layer including the positive electrode active material according to the eighth or ninth aspect and a binder.

[0021] The battery according to an eleventh aspect includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and the positive electrode is the positive electrode according to the tenth aspect.

[0022] A positive electrode according to a twelfth aspect includes a current collector and a positive electrode active material layer located on at least one surface of the current collector and including a positive electrode active material, a binder, and a positive electrode additive, the positive electrode active material including a sulfur-containing compound, and the positive electrode additive including the carbon composite according to any one of the first to seventh aspects.

[0023] According to a thirteenth aspect, the positive electrode may be the positive electrode according to the twelfth aspect, in which the positive electrode additive is contained in an amount of 0.01 to 30 parts by weight per 100 parts by weight of the positive electrode active material layer in total.

[0024] The battery according to a fourteenth aspect includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and the positive electrode is the positive electrode according to the twelfth or thirteenth aspect.

[0025] According to still another aspect of the present invention, there is provided a method for producing a carbon composite having the following features.

[0026] A method for producing a carbon composite according to a fifteenth aspect includes a first step of introducing and dispersing a porous carbon material, vanadium nitride or a precursor thereof, and a reducing agent into a solvent, a second step of filtering the result of the first step to remove the solvent and drying the result, and a third step of heat-treating the result of the second step in an inert atmosphere, the third step including a first process of heat-treating at 350 to 650°C and a second process of heat-treating at 650 to 1400°C. Effect of the Invention

[0027] The carbon composite according to the present invention can be used as a positive electrode additive in a lithium-sulfur battery or as a support for a sulfur-containing compound in a lithium-sulfur battery, thereby quickly converting lithium polysulfide into lithium sulfide.

[0028] In addition, the method for producing a carbon composite according to the present invention can uniformly support a catalyst on a porous carbon support without using harmful gases such as NH3 and strong acids such as hydrogen fluoride (HF).

[0029] The following drawings attached to this specification are intended to illustrate preferred embodiments of the present invention and serve to facilitate a further understanding of the technical ideas of the present invention as well as the contents of the invention. Therefore, the present invention should not be interpreted as being limited to only the matters described in the drawings. [Brief description of the drawings]

[0030] [Figure 1] 1 is a graph showing the specific surface area of ​​a carbon composite according to an embodiment of the present invention. [Diagram 2] 1 is a scanning electron microscope (SEM) photograph of a carbon composite according to an embodiment of the present invention. [Diagram 3] 1 is a SEM photograph of a carbon composite according to an embodiment of the present invention. [Figure 4] 1 is a SEM photograph of a carbon composite according to a comparative example of the present invention. [Diagram 5] 1 is a graph showing an evaluation of charge / discharge performance of a lithium-sulfur battery according to an embodiment of the present invention. [Figure 6] 1 is a graph showing an evaluation of charge / discharge performance of a lithium-sulfur battery according to a comparative example of the present invention. [Figure 7] 1 is an evaluation graph of charge / discharge performance of a lithium-sulfur battery according to a comparative example of the present invention. [Figure 8] 1 is a graph showing an evaluation of the performance of a lithium-sulfur battery according to an embodiment of the present invention. [Figure 9] 1 is a graph showing an evaluation of the performance of a lithium-sulfur battery according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] The present invention will be described in detail below. However, the present invention is not limited to the following content, and each component may be modified or mixed selectively as necessary. Therefore, it should be understood that the present invention includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention.

[0032] Throughout this specification, when a certain configuration "comprises" certain components, this does not mean that it excludes certain other components, but that it may further include other components, unless otherwise specified.

[0033] Throughout this specification, the phrase "A and / or B" means "A or B or both."

[0034] Unless the measurement conditions and methods are specifically described for the physical properties described in this specification, the physical properties are measured according to the measurement conditions and methods commonly used by those of ordinary skill in the art.

[0035] The term "polysulfide" as used in this specification means "polysulfide ion (S x 2- ,x=8,6,4,2) and Lithium polysulfide (Li2S x or LiS x ,x=8,6,4,2".

[0036] The term "composite" as used in this specification means a material in which two or more materials are combined to form physically and chemically different phases and thereby exhibit a more effective function.

[0037] The present invention provides a carbon composite that can be used in lithium-sulfur batteries.

[0038] According to one aspect of the present invention, the carbon composite can be used in a positive electrode of a lithium-sulfur battery.

[0039] In one embodiment of the present invention, the carbon composite may be used as a positive electrode additive that is added separately from a positive electrode active material to a positive electrode of a lithium-sulfur battery.

[0040] In another embodiment of the present invention, the carbon composite can be used as a positive electrode active material, specifically, a porous carbon support supporting a sulfur-containing compound, in the positive electrode of a lithium-sulfur battery.

[0041] In yet another embodiment of the present invention, the carbon composite may be used as the above-mentioned cathode additive and cathode active material in the cathode of a lithium-sulfur battery.

[0042] A carbon composite according to one aspect of the present invention includes a porous carbon material and vanadium nitride particles located on a surface of the porous carbon material.

[0043] During the charge and discharge process of a typical lithium-sulfur battery, lithium polysulfide is dissolved from the positive electrode. When the carbon composite according to one aspect of the present invention is used as one or more of a positive electrode additive and a support for a sulfur-containing compound of a lithium-sulfur battery, the vanadium nitride particles contained in the carbon composite act as a catalyst to quickly convert lithium polysulfide to lithium sulfide, thereby preventing the lithium polysulfide from being dissolved into the electrolyte.

[0044] In one embodiment of the present invention, the "porous carbon material" may function as a support for supporting vanadium nitride particles as a catalyst.

[0045] In one embodiment of the present invention, the porous carbon material may be at least partially or entirely crystalline in order to improve the catalytic activity of vanadium nitride particles. For example, when an amorphous porous carbon material is used as at least a part of a positive electrode additive and / or a positive electrode active material, the amorphous carbon portion may act as a resistor in the electrochemical reaction of a battery, causing a decrease in battery performance. Thus, when the porous carbon material is at least partially or entirely crystalline, it can reduce the resistance in an electrode using the porous carbon material and improve the catalytic activity of vanadium nitride particles, but the mechanism of the present invention is not limited thereto.

[0046] In one embodiment of the present invention, the crystallinity of the porous carbon material can be measured by X-ray diffraction (XRD) analysis. "XRD" is a method for analyzing diffraction (Brugh condition: 2dsinθ=nλ: d is the distance between two planes, θ is the angle between the X-ray and the plane, n is an arbitrary integer, and λ is the wavelength of the X-ray) that occurs as a result of scattering and interference of the X-ray by electrons around the atoms when the X-ray is irradiated onto a sample, and this makes it possible to identify and quantify the constituent components, and to specify the crystal size, crystallinity, etc.

[0047] For example, an at least partially crystalline material can be found when at least one distinct peak occurs in an XRD spectrum, where the distinct peak has a measured signal greater than or equal to 1, 1.5, 2, 5, or 10 times the noise.

[0048] In one aspect of the present invention, when the porous carbon material is at least partially crystalline, it may have a higher elasticity than an amorphous carbon material, for example, the amorphous carbon material may be the carbon material disclosed in Liuatal Nanoscale, 2018, 105246-5253.

[0049] In one aspect of the present invention, when the porous carbon material is entirely crystalline, it is possible for the porous carbon material to have even higher elasticity than an amorphous carbon material.

[0050] In one embodiment of the present invention, the porous carbon material includes a large number of micropores on the outer surface and inside, and the average diameter of the micropores can be, for example, in the range of 1 nm to 200 nm, for example, 1 to 100 nm, 10 to 80 nm, or 20 to 50 nm. The average diameter of the pores can be measured according to ISO 15901:2019, which is well known in the art, but is not limited thereto.

[0051] In one embodiment of the present invention, the porosity (or attack rate) of the porous carbon material may be in the range of 10 to 90 vol% of the total volume of the porous carbon material. The porosity of the porous carbon material may be measured according to a method conforming to ISO 15901:2019, which is known in the art, but the measurement method is not limited thereto.

[0052] In one embodiment of the present invention, the pore volume of the porous carbon material is, for example, 1 cm 3 / g~20cm 3 / g or 1cm 3 / g~10cm 3 / g. The pore volume may be a value calculated and measured using N2 isotherm analysis obtained based on the adsorption of liquid nitrogen. When the pore volume of the porous carbon material is within the above range, it may be advantageous in terms of sufficiently positioning the vanadium nitride particles acting as a catalyst on the surface of the porous carbon material, but the present invention is not limited thereto.

[0053] The pore volume can be measured using AUTOSORB iQ series (manufacturer: Quantachrome) based on ASTM D 4641, and the pore volume can be a value calculated and measured using N2 isotherm analysis obtained based on the adsorption of liquid nitrogen.

[0054] In one embodiment of the present invention, the average particle size (D 50 For example, a plurality of porous carbon materials may be used as primary particles to form a secondary particle-like porous carbon material, and the average particle diameter (D 50 ) can fall within the above numerical range.

[0055] The average particle size (D 50 ) means the particle size at 50% of the cumulative distribution of particle volume according to particle size. The particle size can be measured using a laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and the difference in the diffraction pattern according to the particle size when the particles pass through a laser beam is measured to calculate the particle size distribution. The diameter of the particle at 50% of the cumulative distribution of particle volume according to particle size in the measuring device is calculated, and the D 50 can be measured.

[0056] In one embodiment of the present invention, the porous carbon material has a thickness of, for example, 100 to 2000 m 2 / g, 300-2000m 2 / g, 400-1800m 2 / g, 450-1500m 2 / g or 500~1200m 2 The specific surface area may be measured according to a BET method according to ISO 15901:2019, which is known in the art, but is not limited thereto. When the specific surface area of ​​the porous carbon material is within the above-mentioned range, the vanadium nitride particles can be sufficiently supported, but the present invention is not limited thereto.

[0057] In one embodiment of the present invention, the porous carbon material may include, for example, carbon nanotubes (CNTs), graphene, graphene oxide (GO), reduced graphene oxide (rGO), carbon black, graphite, graphite nano fiber (GNF), carbon nano fiber (CNF), activated carbon fiber (ACF), natural graphite, artificial graphite, expanded graphite, activated carbon, fullerene, or a material selected from two or more of these materials.

[0058] In one embodiment of the present invention, the porous carbon material may include at least one selected from the group consisting of carbon nanotubes and reduced graphene oxide.

[0059] In one embodiment of the present invention, the porous carbon material may be doped with at least one element selected from the group consisting of nitrogen, oxygen, and phosphorus.

[0060] In another aspect of the invention, the porous carbon material may comprise carbon nanotubes doped with at least one of nitrogen, oxygen and phosphorus, reduced graphene oxide doped with at least one of nitrogen, oxygen and phosphorus, or a mixture thereof.

[0061] The carbon nanotube is a tube-shaped structure of carbon atoms connected in a hexagonal shape. According to one aspect of the present invention, the carbon nanotube may be a single-walled carbon nanotube (SWCNT), a multi-walled carbon nanotube (MWCNT), or a combination thereof, depending on the number of carbon atom layers (also called "carbon walls") that compose the carbon nanotube. Here, the length of each carbon nanotube is not particularly limited.

[0062] In another embodiment of the present invention, the carbon nanotubes may be present in a form in which two or more carbon nanotubes are tightly intertwined with each other due to the cohesive forces therebetween.

[0063] Specifically, in one embodiment of the present invention, the carbon nanotubes may be provided in the form of a carbon nanotube dispersion in which the carbon nanotubes are dispersed as single strands in a dispersion medium or the like, or may be provided in the form of a secondary structure in which primary structure carbon nanotubes are aggregated together. In this respect, when the porous carbon material includes carbon nanotubes, the carbon nanotubes may be in the form of a bundle-shaped secondary structure, an entangled secondary structure, or both. The bundle-shaped secondary structure of carbon nanotubes refers to a single carbon nanotube as a primary structure, and the multiple primary structures are aligned in the longitudinal direction of the carbon nanotube due to the cohesive force between carbons, and are aggregated together to form a mass, and may also be referred to as a bundled CNT.

[0064] In this way, the carbon nanotubes contained in the carbon composite are formed by one or more carbon nanotubes being twisted or entangled, which enables the carbon composite to have a porous structure in which spaces are formed between the carbon nanotubes.

[0065] The reduced graphene oxide may be formed in a structure in which one reduced graphene oxide is bent, or in a structure in which a plurality of reduced graphene oxides are bent and entangled with each other. Alternatively, a plurality of reduced graphene oxides may be formed in a crumpled shape. In this way, the reduced graphene oxide contained in the carbon composite is formed by one or more reduced graphene oxides being entangled or crumpled, and the carbon composite can have a porous structure in which spaces are formed between the reduced graphene oxides.

[0066] The carbon composite includes vanadium nitride particles located on the surface of the porous carbon material described above.

[0067] The vanadium nitride (VN) is a compound of nitrogen and vanadium. The vanadium nitride particles are located on the surface of the porous carbon material.

[0068] In one embodiment of the present invention, the vanadium nitride particles may have catalytic activity for the oxidation and reduction reactions of sulfur (S8), lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 2≦x≦8), disulfide compounds, or mixtures of two or more of these.

[0069] In one aspect of the present invention, the vanadium nitride particles may be located on at least one of an outer surface of the porous carbon material and an inner surface of the pores, and more specifically, the vanadium nitride particles may be adsorbed and present on the outer surface of the porous carbon material.

[0070] In one aspect of the present invention, since the carbon nanotube is a tube-shaped carbon nanotube formed of carbon connected in a hexagonal shape, the carbon composite may have a structure in which the vanadium nitride particles are located on the inner surface and / or outer surface of the tube-shaped carbon nanotube. In particular, the vanadium nitride particles may be located on the outer surface of the carbon nanotube. Here, the method of positioning the vanadium nitride on the surface of the porous carbon material is not particularly limited, and may be, for example, by adhering or depositing the vanadium nitride on the surface of the porous carbon material.

[0071] In one embodiment of the present invention, the average particle size (D 50 ) may be 200 nm or less, specifically, the average particle size (D 50 ) may be 190 nm or less, 180 nm or less, 170 nm or less, 160 nm or less, or 20 nm or less. 50 ) may be 1 nm or more or 2 nm or more. When the average particle size of the vanadium nitride particles is within the above range, the specific surface area of ​​the vanadium nitride particles acting as a catalyst is increased, so that the particles can react more effectively with lithium polysulfide, and the surface is no longer completely covered by lithium sulfide generated during discharge, so that the reaction can proceed reversibly, and more catalyst can be located on the surface of the porous carbon material. 50 ) can be measured in the same manner as the method for measuring the particle size of the porous carbon material.

[0072] In one embodiment of the present invention, the vanadium nitride particles may be included in an amount of, for example, 3 to 50 parts by weight relative to 100 parts by weight of the carbon composite, specifically, 3 to 40 parts by weight, 3 to 30 parts by weight, 40 to 50 parts by weight, 35 to 50 parts by weight, 10 to 40 parts by weight, or 20 to 30 parts by weight relative to 100 parts by weight of the carbon composite. When the vanadium nitride particles are included in an amount within the above range, the vanadium nitride particles can quickly convert lithium polysulfide to lithium sulfide, prevent lithium polysulfide from dissolving in the electrolyte, and maintain appropriate resistance and weight.

[0073] In one embodiment of the present invention, at least a part of the surface of the vanadium nitride may be coated with a carbon layer. Alternatively, the entire surface of the vanadium nitride may be coated with a carbon layer. Specifically, when the carbon layer is present, the thickness of the carbon layer may be 5 nm or less. The thickness of the carbon layer may be measured by a transmission electron microscope (TEM). The thickness of the carbon layer satisfying the above range is advantageous in terms of increasing the stability of the catalyst while maintaining the effect of the vanadium nitride catalyst.

[0074] In one embodiment of the present invention, the carbon layer coated on the vanadium nitride may be formed of 1 to 3 or 1 to 5 layers, and the total thickness of the carbon layer may be 5 nm or less.

[0075] In one embodiment of the present invention, the specific surface area of ​​the carbon composite is, for example, 250 m 2 / g or more, specifically, 260m 2 / g or more, 270m 2 / g or more, 280m 2 / g or more, 290m 2 / g or more or 300m 2 / g or more, and 2 / g or less or 500m 2When the specific surface area of ​​the carbon composite falls within the above range, a sufficient amount of vanadium nitride located on the surface can sufficiently convert lithium polysulfide to lithium sulfide, and the surface of the carbon composite is not entirely covered with lithium polysulfide or lithium sulfide generated during discharge, allowing the reaction to occur reversibly.

[0076] The specific surface area is measured by the BET method, and specifically, can be calculated from the amount of nitrogen gas adsorbed at liquid nitrogen temperature (77K) using BELSORP-mino II manufactured by BEL Japan.

[0077] In one embodiment of the present invention, the pore volume of the carbon composite is, for example, 1.0 cm 3 Specifically, the pore volume of the carbon composite may be 1.1 cm3 or more. 3 / g or more, 1.2cm 3 / g or more, 1.3cm 3 / g or more or 1.4cm 3 / g or more, and 3 / g or less, 2.7cm 3 / g or less, 3.0cm 3 When the pore volume of the carbon composite is within the above-mentioned range, the electrolyte of a battery using the carbon composite as a positive electrode can be sufficiently impregnated into the pores to improve ion conductivity, and the pores of the carbon composite can be used to improve the loading efficiency of sulfur (S8) and the electrical conductivity of the positive electrode, but the present invention is not limited thereto.

[0078] In one embodiment of the present invention, the average pore size of the carbon composite may be 10 nm or more. Specifically, the average pore size of the carbon composite may be 15 nm or more, 50 nm or less, 70 nm or less, or 100 nm or less. When the average pore size of the carbon composite satisfies such a range, lithium polysulfide can be effectively adsorbed, and it is advantageous in terms of improving reactivity by making the electrolyte easily approach the pores and appropriately maintaining ionic conductivity.

[0079] The average pore diameter can be a value measured by being calculated through, for example, N2 isotherm analysis obtained based on the adsorption of liquid nitrogen.

[0080] In one aspect of the present invention, the carbon composite contains V formed as a by-product during the formation of vanadium nitride particles x O y (0 < x < 2.0 < y < 5) in trace amounts. However, V x O y (0 < x < 2.0 < y < 5) can be less than 1% by weight based on the total weight of the vanadium nitride particles contained in the carbon composite. At this time, the content can be measured by calculating the residual mass at 950 °C using thermogravimetric analysis (TGA: Thermo Gravimetric Analysis).

[0081] In one aspect of the present invention, the carbon composite is characterized in that an XRD (X-Ray Diffraction) peak occurs at 2θ.

[0082] In one aspect of the present invention, the intensity ratio (I D / I G ratio) of the Raman spectrum peak of the carbon composite can be 2.0 or less. Specifically, the I D / I G ratio can be 0.5 or more and 2.0 or less. The intensity ratio (I D / I G ratio) can be measured using the peak intensities I G and I D obtained from the spectrum of the carbon composite obtained using Raman spectroscopy. The I G means the peak (G-peak, 1573 / cm) of the crystalline part, and I D means the peak (D-peak, 1309 / cm) of the amorphous part. Therefore, at this time, I D / I GA smaller ratio indicates higher crystallinity. When the ratio satisfies the above range, electrical conductivity and mechanical strength can be appropriately maintained.

[0083] In one embodiment of the present invention, the crystallinity of the carbon composite may be, for example, 70% or more. The crystallinity is characterized in that it is measured using at least one of Raman spectroscopy and XRD analysis. The crystallinity falling within the above range is advantageous in terms of preventing a decrease in catalyst performance and maintaining resistance at a certain level or less while maintaining appropriate electrical conductivity.

[0084] According to another aspect of the present invention, there is provided a positive electrode active material comprising the above-mentioned carbon composite.

[0085] Specifically, the cathode active material can be for use in a lithium-sulfur battery.

[0086] A positive electrode active material according to one aspect of the present invention may include the above-described carbon composite as a support, and a sulfur-containing compound supported within pores of the carbon composite.

[0087] In one embodiment of the present invention, the sulfur-containing sulfide supported in the pores of the carbon composite is inorganic sulfur (S8), Li2S n (n≧1), 2,5-dimercapto-1,3,4-thiadiazole, 1,3,5-trithiocyanuic acid, and other disulfide compounds, and organic sulfur compounds. Preferably, inorganic sulfur (S8) may be included.

[0088] In one embodiment of the present invention, the weight ratio of the sulfur-containing compound to the carbon composite may be, for example, 1:1 to 9:1. Specifically, the weight ratio of the sulfur-containing compound to the carbon composite may be 2:1 to 8:1, 5:1 to 9:1, or 8:1 to 9:1. When the weight ratio satisfies such a range, the agglomeration phenomenon between the sulfur-containing compounds is prevented and the sulfur-containing compounds are easily able to accept electrons, so that they can directly participate in the electrode reaction, and the amount of binder added required in the preparation of the positive electrode slurry can be appropriately controlled, so that problems such as an increase in the surface resistance of the electrode and a decrease in cell performance can be prevented.

[0089] According to another aspect of the present invention, there is provided a positive electrode comprising the above-described positive electrode active material.

[0090] The positive electrode comprises a current collector and a positive electrode active material layer located on at least one surface of the current collector, the positive electrode active material layer including the positive electrode active material and a binder as described above. Optionally, the positive electrode active material layer may further include a conductive material.

[0091] In one aspect of the present invention, the binder holds the positive electrode active material on the positive electrode current collector and organically connects the positive electrode active materials to each other to further enhance the binding strength therebetween, and any binder known in the art can be used. For example, the binder may be one or a mixture or copolymer of two or more selected from the group consisting of fluororesin-based binders including polyvinylidene fluoride (PVdF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene butadiene rubber (SBR), acrylonitrile-butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; polyacrylic-based binders; and silane-based binders.

[0092] In one embodiment of the present invention, the content of the binder may be, for example, 0.5 to 30 parts by weight when the total weight of the positive electrode active material layer is 100 parts by weight. When the content of the binder satisfies this range, the physical properties of the positive electrode are improved, and the phenomenon that the active material and the conductive material in the positive electrode are removed can be prevented, and the ratio of the active material and the conductive material in the positive electrode can be appropriately controlled, thereby ensuring the capacity of the battery.

[0093] In one aspect of the present invention, the conductive material is a material that electrically connects the electrolyte and the positive electrode active material and serves as a path through which electrons move from the current collector to the positive electrode active material, and can be used without any restrictions as long as it has electrical conductivity. In one embodiment, the conductive material can be carbon black such as Super-P, Denka Black, acetylene black, Ketjen Black, channel black, furnace black, lamp black, thermal black, carbon black, etc.; carbon derivatives such as carbon nanotubes, graphene, and fullerene; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; or conductive polymers such as polyaniline, polythiophene, polyacetylene, and polypyrrole, either alone or in combination. In addition, the carbon composite according to the present invention can be used as the conductive material.

[0094] In one embodiment of the present invention, when the conductive material is included, the content of the conductive material may be 0.01 to 30 parts by weight based on 100 parts by weight of the total positive electrode active material layer.

[0095] In one embodiment of the present invention, the current collector is not particularly limited as long as it supports the positive electrode active material layer, does not cause chemical changes in the battery, and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, palladium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, silver, etc., aluminum-cadmium alloy, etc. can be used.

[0096] In one aspect of the present invention, the current collector can have minute projections and recesses on its surface to strengthen the bonding force with the positive electrode active material, and a wide variety of forms such as a film, sheet, foil, mesh, net, porous body, foam, and nonwoven fabric can be used.

[0097] In one embodiment of the present invention, the thickness of the current collector is not particularly limited, but may be, for example, 3 to 500 μm.

[0098] According to another aspect of the present invention, there is provided a battery using the above-described positive electrode, particularly a battery for a lithium secondary battery, specifically a lithium-sulfur battery.

[0099] The battery includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.

[0100] The above-mentioned items are applicable to the positive electrode.

[0101] In one embodiment of the present invention, the negative electrode and the separator can be used without any particular limitation as long as they are usable in a lithium-sulfur battery, as long as the object of the present invention is not impaired. The negative electrode can be, for example, lithium metal.

[0102] In one embodiment of the present invention, the separator can be any separator that can be used without limitation as long as it is generally usable as a separator for a lithium-sulfur battery.

[0103] In one embodiment of the present invention, the separator may include a porous polyolefin substrate, and may further include inorganic particles on at least one surface of the porous polyolefin substrate, and may further include a binder that binds the inorganic particles, if necessary.

[0104] In another embodiment of the present invention, the separator may be a film-like electrolyte membrane containing a solid electrolyte, and may further contain a binder for binding the solid electrolyte, if necessary. The solid electrolyte may be any solid electrolyte that can be used in lithium-sulfur batteries without any restrictions, such as a polymer solid electrolyte, an inorganic solid electrolyte, or a mixture thereof.

[0105] In one embodiment of the present invention, the electrolyte includes any electrolyte that can be used in lithium-sulfur batteries. The electrolyte may include a lithium salt and a non-aqueous solvent.

[0106] The lithium salt can be used without any restrictions as long as it is generally usable as an electrolyte for a lithium-sulfur battery. Examples of the lithium salt include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiC4BO8, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, (C2F5SO2)2NLi, (SO2F)2NLi, (CF3SO2)3CLi, lithium chloroborane, lithium lower aliphatic carboxylate, lithium 4-phenylborate, lithium imide, or two or more of these, but are not limited thereto.

[0107] The non-aqueous solvent can be used without any limitation as long as it can be used in the electrolyte of a lithium-sulfur battery. The non-aqueous solvent can include, for example, a cyclic carbonate solvent, a linear carbonate solvent, an ester solvent, a ketone solvent, or a mixed solvent of two or more of these, but is not limited thereto.

[0108] In one embodiment of the present invention, the electrolyte may include (CF3SO2)2NLi as a lithium salt and a dioxolane (DOL) / dimethoxyethane (DME) binary system as a non-aqueous solvent. For example, the electrolyte may further include a common additive such as LiNO3.

[0109] In one aspect of the present invention, the lithium-sulfur battery may have an outer shape, for example, a coin shape, a cylindrical shape, a pouch shape, a rectangular shape, etc., and the outer shape of the battery is not particularly limited. In addition, the lithium-sulfur battery can be used not only as a battery cell used as a power source for a small device, but also as a unit battery for a medium- to large-sized battery module including a number of battery cells, and the usage form is not particularly limited.

[0110] According to yet another aspect of the present invention, there is provided a positive electrode to which the above-mentioned carbon composite is added as a positive electrode additive.

[0111] In one aspect of the present invention, the positive electrode comprises a current collector and a positive electrode active material layer located on at least one surface of the current collector and including a positive electrode active material, a binder, and a positive electrode additive, the positive electrode active material including a sulfur-containing compound, and the positive electrode additive including the carbon composite described above.

[0112] In one embodiment of the present invention, when the positive electrode additive is the carbon composite described above, the positive electrode additive may be included, for example, in an amount of 0.1 to 30 parts by weight relative to a total of 100 parts by weight of the positive electrode active material layer. Specifically, the positive electrode additive may be included in an amount of 0.5 to 20 parts by weight, 1 to 10 parts by weight, or 1 to 5 parts by weight relative to a total of 100 parts by weight of the positive electrode active material layer. When the positive electrode additive is included in the above range, it is advantageous in improving the electrical conductivity between active material particles or between the active material and the current collector, and reducing the resistance in the electrode. In addition, the positive electrode additive is dispersed between the compressed active material particles, thereby maintaining micropores between the active material particles and facilitating the penetration of the electrolyte.

[0113] According to yet another aspect of the present invention, there is provided a battery including a positive electrode using the above-mentioned carbon composite as a positive electrode additive.

[0114] The battery includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and the positive electrode includes the above-mentioned carbon composite as a positive electrode additive.

[0115] In this case, the above-mentioned items are applicable to the negative electrode, the separator, and the electrolyte.

[0116] According to yet another aspect of the present invention, there is provided a method for producing the above-mentioned carbon composite.

[0117] The carbon composite, as described above, includes a porous carbon material and vanadium nitride particles located on a surface of the porous carbon material.

[0118] The method for producing the carbon composite includes a first step of introducing and dispersing a porous carbon material, vanadium nitride or a precursor thereof, and a reducing agent into a solvent, a second step of filtering the result of the first step to remove the solvent and drying the result, and a third step of heat-treating the result of the second step in an inert atmosphere.

[0119] In one embodiment of the present invention, the vanadium nitride precursor may include one or more selected from the group consisting of dicyandiamide, ammonium metavanadate (NH4VO3), vanadium oxides, ammonia (NH3), and ammonium chloride.

[0120] For example, the vanadium nitride may be produced by a synthetic reaction between dicyandiamide and ammonium metavanadate.

[0121] In one embodiment of the present invention, the reducing agent may include one or more selected from the group consisting of glucose, sucrose, lactose, fructose, starch, polydopamine, and tannic acid.

[0122] In one embodiment of the present invention, the solvent used in the first step may be one or more organic solvents selected from the group consisting of dimethyl carbonate, dimethylformamide, N-methylformamide, sulfolane (tetrahydrothiophene-1,1-dioxide), 3-methylsulfolane, N-butylsulfone, dimethylsulfoxide, pyrrolidinone (HEP), dimethylpiperidone (DMPD), N-methylpyrrolidinone (NMP), N-methylacetamide, dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), diethylacetamide (DEAc), dipropylacetamide (DPAc), ethanol, propanol, butanol, hexanol, ethylene glycol, tetrachloroethylene, propylene glycol, toluene, turpentine, methyl acetate, ethyl acetate, petroleum ether, acetone, cresol, and glycerol.

[0123] In one embodiment of the present invention, based on 100 parts by weight of the porous carbon material added in the first step, the content of the vanadium nitride or its precursor may be 1 to 100 parts by weight or 5 to 40 parts by weight, and the content of the reducing agent may be 10 to 100 parts by weight or 20 to 80 parts by weight. When the vanadium nitride or its precursor and the reducing agent satisfy the above range, an appropriate level of vanadium nitride catalyst particles can be uniformly formed on the surface of the porous carbon material. In addition, the amount of amorphous carbon with low electrical conductivity is minimized, and the catalyst surface can be exposed to the maximum while maintaining a large specific surface area, which is advantageous in maximizing the reactivity of lithium polysulfide and preventing it from being dissolved in the electrolyte, but the present invention is not limited thereto.

[0124] In one embodiment of the invention, in said first step, dispersion may be performed by ultrasonication and / or magnetic stirring.

[0125] In one embodiment of the present invention, in the second step, the removal of the solvent may be performed by vacuum filtration. Furthermore, the drying may be performed under a temperature condition of 50° C. to 150° C. Furthermore, the drying may be performed for, for example, 1 to 48 hours.

[0126] In one aspect of the present invention, the third step includes a first process of heat treatment at a low temperature and a second process of heat treatment at a high temperature. Specifically, the first process may be performed so that a vanadium nitride precursor is thermally decomposed and reduced to produce vanadium nitride, and the second process may be performed so that a carbonization reaction is promoted to bind vanadium nitride particles to the surface of the porous carbon material.

[0127] In one embodiment of the present invention, the third step may include a first process of heat treatment at 350 to 650°C and a second process of heat treatment at 650 to 1400°C.

[0128] In one embodiment of the present invention, the first step can be carried out at a temperature of 350 to 650°C, 500 to 650°C, or 550 to 650°C.

[0129] In one embodiment of the present invention, the second step can be carried out at a temperature of 650 to 1400°C, 700 to 900°C, or 750 to 850°C.

[0130] In one aspect of the invention, the third step may be carried out under an inert atmosphere, and the inert atmosphere may be formed using one or more gases selected from helium, neon, argon, carbon dioxide and nitrogen.

[0131] In one embodiment of the present invention, the method for producing the above-mentioned carbon composite may be characterized in that it does not use NH3, HF, or an acid having an acid dissociation constant (pKa) of 4.0 or less.

[0132] The present invention will be described in more detail below with reference to examples. However, the following examples are merely for the purpose of illustrating the present invention, and the scope of the present invention is not limited to these examples in any way.

[0133] [Manufacturing of carbon composites] Example 1 1.6 g of carbon nanotubes, 24 g of dicyanodiamide, 0.8 g of ammonium metavanadate, and 0.2 g of glucose were mixed in 500 mL of a solvent consisting of a 1:1 volumetric ratio of ethanol and water, and dissolved and dispersed by ultrasonic treatment and magnetic stirring.

[0134] This was followed by vacuum filtration to remove the solvent except for the vanadium nitride precursor adsorbed on the surface of the carbon nanotubes.

[0135] Then, it was dried in an oven at 80° C. for 12 hours.

[0136] Then, the carbon nanotube was heat-treated in an inert atmosphere tube furnace at 600°C for 3 hours and at 800°C for 2 hours to obtain a carbon composite having vanadium nitride particles located on the surface of the carbon nanotube. The vanadium nitride particle content was 20 parts by weight per 100 parts by weight of the obtained carbon composite. The vanadium nitride particle content was measured using a thermogravimetric analyzer (TGA).

[0137] Example 2 A carbon composite having vanadium nitride particles located on the surface of reduced graphene oxide was obtained in the same manner as in Example 1, except that reduced graphene oxide was used instead of carbon nanotubes. At this time, the content of the vanadium nitride particles was 20 parts by weight per 100 parts by weight of the obtained carbon composite. The content of the vanadium nitride particles was measured using a thermogravimetric analyzer (TGA).

[0138] Comparative Example 1 24 g of dicyanodiamide, 0.8 g of ammonium metavanadate, and 0.8 g of glucose were mixed in 500 mL of a solvent in which ethanol and water were mixed in a volume ratio of 1:1, and dissolved and dispersed by ultrasonic treatment and magnetic stirring.

[0139] Thereafter, the solvent other than dicyanodiamide and ammonium metavanadate was removed by filtration under reduced pressure.

[0140] Then, it was dried in an oven at 80° C. for 12 hours.

[0141] After that, the mixture was heat-treated in an inert atmosphere tube furnace at 600°C for 3 hours and then at 800°C for 2 hours to obtain a carbon composite in which vanadium nitride particles were located on the surface of amorphous carbon formed from glucose through a carbonization process.

[0142] At this time, the content of the vanadium nitride particles was 20 parts by weight based on 100 parts by weight of the obtained carbon composite. The content of the vanadium nitride particles was measured using a thermogravimetric analyzer (TGA).

[0143] Evaluation of the physical properties of carbon composites For the carbon composites produced in Example 1, Example 2, and Comparative Example 1, the specific surface area, pore volume, and average pore diameter were measured using a BELSORP-mino II manufactured by BEL Japan, according to a method of calculation from the amount of nitrogen gas adsorbed at liquid nitrogen temperature (77 K).

[0144] In addition, the crystallinity of the carbon in the carbon composite produced above was measured using Raman spectroscopy, and the spectrum obtained as a result of the measurement was used to determine the crystallinity of the carbon in the carbon composite produced above. D / I G The ratio was derived.

[0145] The physical properties evaluated according to the above methods are shown in Table 1 below.

[0146] [Table 1]

[0147] FIG. 1 shows the results of measuring the 77K N2 isotherms of the carbon composites according to Example 1, Example 2 and Comparative Example 1.

[0148] Fig. 2 is an SEM photograph of the carbon composite of Example 1 in which vanadium nitride particles are located on the surface of the carbon nanotubes. The SEM image in Fig. 2 was obtained at a magnification of 2,000 times for an area of ​​10 µm x 10 µm.

[0149] Fig. 3 is an SEM photograph of the carbon composite of Example 2 in which vanadium nitride particles are located on the surface of reduced graphene oxide. The SEM image in Fig. 3 was obtained at a magnification of 2,000 times over an area of ​​10 µm x 10 µm.

[0150] Fig. 4 is an SEM photograph of the carbon composite of Comparative Example 1 in which vanadium nitride particles are located on the surface of carbon nanotubes, which are amorphous carbon. The SEM image in Fig. 4 was obtained at a magnification of 2,000 times for an area of ​​10 μm x 10 μm.

[0151] 2 to 4, it was confirmed that vanadium nitride particles were uniformly formed on the surfaces of the carbon nanotubes, reduced graphene oxide, and amorphous carbon, respectively. The average particle size (D 50 ) is 1 μm, and it can be seen that the vanadium nitride particles are considerably aggregated and form clumps. In contrast, the vanadium nitride particles formed on the surface of reduced graphene oxide or carbon nanotubes have an average particle size (D 50 ) can be confirmed to be 0.1 μm or less.

[0152] [Manufacturing lithium-sulfur batteries] Example 3 <Production of positive electrodes> A porous carbon support in which sulfur is supported on carbon nanotubes was prepared as a positive electrode active material. The weight ratio of the carbon composite to sulfur (S8) was 1:3. The carbon composite of Example 1 was used as a positive electrode additive, and polyacrylic acid (PAA) was mixed as a binder to prepare a positive electrode slurry.

[0153] At this time, the weight ratio of the positive electrode active material, the positive electrode additive, and the binder was 88:5:7.

[0154] The slurry was coated on an aluminum foil using a Mathis coating device, dried at 50° C. for 24 hours, and then rolled to prepare a positive electrode.

[0155] <Manufacturing lithium-sulfur batteries> A 45 μm-thick lithium metal thin film was prepared as the negative electrode, and a mixed solution was prepared as the electrolyte by dissolving 1 M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 1 wt % lithium nitrate (LiNO3) in an organic solvent consisting of 1,3-dioxolane and dimethyl ether (DOL:DME = 1:1 (volume ratio)).

[0156] The prepared positive and negative electrodes were placed facing each other, a polyethylene separator having a thickness of 16 μm and a porosity of 46% was interposed between them, and 70 μl of the electrolyte was injected to prepare a lithium-sulfur battery.

[0157] Example 4 A lithium-sulfur battery was manufactured in the same manner as in Example 3, except that the carbon composite of Example 2 was used instead of the carbon composite of Example 1 as a positive electrode additive.

[0158] Example 5 <Production of positive electrodes> As a positive electrode active material, sulfur was supported on the carbon composite produced in Example 1 using a melt support method. Specifically, the carbon composite was mixed with sulfur (S8) and mixed uniformly. Then, the carbon composite was heat-treated in an oven at 150°C for 30 minutes to impregnate the inside of the carbon composite with sulfur. At this time, the weight ratio of the carbon composite to sulfur was 1:3.

[0159] A polyacrylic acid (PAA) binder and a carbon fiber conductive material were mixed to prepare a positive electrode slurry. In the slurry, the weight ratio of the positive electrode active material, the conductive material, and the binder was 88:5:7.

[0160] The slurry was coated on an aluminum foil using a Matisse coating device, dried at a temperature of 50° C. for 24 hours, and then rolled to prepare a positive electrode.

[0161] <Manufacturing lithium-sulfur batteries> A lithium metal thin film with a thickness of 45 μm was prepared as the negative electrode, and a mixed solution of 1 M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 1 wt % lithium nitrate (LiNO3) dissolved in an organic solvent consisting of 1,3-dioxolane and dimethyl ether (DOL:DME = 1:1 (volume ratio)) was prepared as the electrolyte.

[0162] The prepared positive and negative electrodes were placed facing each other, a polyethylene separator having a thickness of 16 μm and a porosity of 46% was interposed between them, and 70 μl of the electrolyte was injected to prepare a lithium-sulfur battery.

[0163] Comparative Example 2 A lithium-sulfur battery was manufactured in the same manner as in Example 3, except that carbon nanotubes (CNTs) were used instead of the carbon composite of Example 1 as a positive electrode additive.

[0164] Comparative Example 3 A lithium-sulfur battery was manufactured in the same manner as in Example 3, except that the carbon composite of Comparative Example 1 was used instead of the carbon composite of Example 1 as a positive electrode additive.

[0165] Comparative Example 4 A positive electrode and a lithium-sulfur battery were manufactured in the same manner as in Example 5, except that carbon nanotubes (CNTs) were used instead of the carbon composite prepared in Example 1 as a positive electrode additive.

[0166] Comparative Example 5 <Production of positive electrodes> As a positive electrode active material, sulfur was supported on carbon nanotubes (CNTs) using a melting support method. Specifically, the carbon composite was mixed with sulfur (S8) and mixed uniformly. After that, it was heat-treated in an oven at 150°C for 30 minutes to impregnate the inside of the carbon composite with sulfur. At this time, the weight ratio of the carbon composite to sulfur was 1:3.

[0167] Polyacrylic acid (PAA) binder, polyvinyl alcohol, PVA thickener, and carbon nanotube conductive material were further added and mixed to prepare a positive electrode slurry. In the slurry, the weight ratio of the positive electrode active material, binder, thickener, and conductive material was 88:6.5:0.5:5.

[0168] The slurry was coated on an aluminum foil using a Matisse coating device, dried at a temperature of 50° C. for 24 hours, and then rolled to prepare a positive electrode.

[0169] <Manufacturing lithium-sulfur batteries> A 45 μm-thick lithium metal thin film was prepared as the negative electrode, and a mixed solution of 1 M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 1 wt % lithium nitrate (LiNO3) dissolved in an organic solvent consisting of 1,3-dioxolane and dimethyl ether (DOL:DME = 1:1 (volume ratio)) was prepared as the electrolyte.

[0170] The prepared positive and negative electrodes were placed facing each other, a polyethylene separator having a thickness of 16 μm and a porosity of 46% was interposed between them, and 70 μl of the electrolyte was injected to prepare a lithium-sulfur battery.

[0171] [Evaluation of lithium-sulfur battery performance] The performance of the lithium-sulfur batteries of Examples 3 to 5 and Comparative Examples 2 to 5 produced above was evaluated by a circulating current-voltage method (CV), and the results are shown in FIGS.

[0172] Specifically, the battery to be evaluated was charged at 1.7V to 2.8V (vs Li / Li + ), the first three charge / discharge cycles were performed at a current density of 0.1C, the next three charge / discharge cycles at 0.3C, and the remaining three charge / discharge cycles at 0.5C. The capacity-voltage curves for the first cycle (Figures 5, 7, and 8), the voltage-current density curve (Figure 6), and the cycle-specific capacity curve (Figure 9) are shown.

[0173] 5, it was confirmed that the batteries of Example 3 and Example 4, which used a carbon composite containing vanadium nitride particles on a porous carbon material as a positive electrode additive, had improved battery performance due to the catalytic activity of the vanadium nitride particles compared to the battery of Comparative Example 5. This confirmed that the vanadium nitride particles can improve the overvoltage of a lithium-sulfur battery and improve the rate at which lithium polysulfide is converted to lithium sulfide. In particular, it was confirmed that Example 3, which used carbon nanotubes, showed better performance than Example 4, which used reduced graphene oxide.

[0174] In addition, referring to FIGS. 6 and 7, it was confirmed that the battery of Comparative Example 3, which uses the carbon composite of Comparative Example 1 as a positive electrode additive, which has a small specific surface area and small pores and in which vanadium nitride particles are located on the surface of amorphous carbon, has increased resistance due to the low electrical conductivity of amorphous carbon, and as a result, is inferior in performance to Comparative Example 5, which uses a positive electrode that does not contain vanadium nitride particles.

[0175] 8 and 9, it was confirmed that the performance was improved by improving the overvoltage and accelerating the conversion reaction in the lithium-sulfur battery of Example 5. This indicates that the performance of the lithium-sulfur battery can be improved by supporting sulfur (S8) on a carbon composite containing vanadium nitride particles on a porous carbon material and using the carbon composite as a positive electrode active material.

[0176] Although the present invention has been described above using limited embodiments and drawings, it goes without saying that the present invention is in no way limited to these, and that a person having ordinary knowledge in the technical field to which the present invention pertains can make various modifications and variations within the technical spirit of the present invention and the equivalent scope of the claims.

Claims

1. A porous carbon material; vanadium nitride particles located on a surface of the porous carbon material; A carbon composite comprising:

2. The specific surface area of ​​the carbon composite is 250 m 2 The carbon composite according to claim 1, wherein the carbon composite has a molecular weight of 1 / g or more.

3. The pore volume of the carbon composite is 1.0 cm 3 The carbon composite according to claim 1, wherein the carbon composite has a molecular weight of 1 / g or more.

4. The carbon composite according to claim 1 , wherein the average pore size of the carbon composite is 10 nm or more.

5. 2. The carbon composite according to claim 1, wherein the vanadium nitride particles have an average particle size of 200 nm or less.

6. 2. The carbon composite according to claim 1, wherein the vanadium nitride particles are contained in an amount of 3 to 50 parts by weight based on 100 parts by weight of the carbon composite.

7. 10. The carbon composite of claim 1, wherein the porous carbon material comprises carbon nanotubes (CNTs), reduced graphene oxide (rGO), or a mixture thereof.

8. A carbon composite according to any one of claims 1 to 7; a sulfur-containing compound supported within the pores of the carbon composite; A positive electrode active material comprising:

9. The positive electrode active material according to claim 8, wherein a weight ratio of the sulfur-containing compound to the carbon composite is 1:1 to 9:

1.

10. A current collector; a positive electrode active material layer located on at least one surface of the current collector, the positive electrode active material layer comprising the positive electrode active material according to claim 8 and a binder; A positive electrode.

11. The battery includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte; The battery, wherein the positive electrode is the positive electrode of claim 10.

12. A current collector; a positive electrode active material layer located on at least one surface of the current collector and including a positive electrode active material, a binder, and a positive electrode additive; Equipped with The positive electrode active material contains a sulfur-containing compound, The positive electrode additive comprises the carbon composite according to claim 1 .

13. The positive electrode according to claim 12, wherein the positive electrode additive is contained in an amount of 0.01 to 30 parts by weight based on a total of 100 parts by weight of the positive electrode active material layer.

14. The battery includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte; The battery, wherein the positive electrode is the positive electrode of claim 12.

15. A first step of dispersing a porous carbon material, vanadium nitride or a precursor thereof, and a reducing agent in a solvent; a second step of filtering the result of the first step to remove the solvent and drying; a third step of heat treating the result of the second step under an inert atmosphere; Including, The third step includes: A first step of heat treating at 350°C to 650°C; A second step of heat treating at 650°C to 1400°C; The method for producing the carbon composite of claim 1 , comprising:

Citation Information

Patent Citations

  • Cathode material used for lithium-sulfur secondary battery

    CN105932242A

  • Transition metal nitride / nitrogen-doped graphene nanometer composite material and preparation method and application thereof

    CN107610938A

  • Vanadium nitride nanocluster loaded on 3D carbon foam skeleton and preparation method thereof

    CN109205590A

  • Vanadium nitride-hybridized and nitrogen-doped porous carbon material as well as preparation method and application thereof

    CN111892047A

  • Preparation method of vanadium nitride nanoparticle composite material for lithium-sulfur battery