Lithium secondary battery
By employing SiOx and perlithium manganese oxide with controlled usage depth and composition, the lithium secondary battery achieves high energy density and extended life characteristics, addressing the limitations of carbon-based and silicon-based materials.
Patent Information
- Application Number
- JP2024519732
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-05
- Filing Date
- 2022-10-05
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2042-10-05
AI Technical Summary
Lithium secondary batteries face limitations in achieving high energy density and rapid charging due to the use of carbon-based negative electrode active materials, which have a small capacity, and silicon-based materials that expand rapidly during charging, leading to performance deterioration.
The use of SiOx and perlithium manganese oxide as active materials, with specific ratios and compositions, including a manganese content exceeding 50 mol% and a lithium mole ratio exceeding 1, and controlling the SiOx usage depth between 1 to 15% in a fully discharged state, to minimize volume expansion and non-uniform reactions.
This configuration results in lithium secondary batteries with excellent energy density, rapid charging performance, and improved life characteristics by stabilizing the silicon-based negative electrode and compensating for irreversible capacity.
Smart Images

Figure 2024536253000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0131947 filed on October 5, 2021 and Korean Patent Application No. 10-2022-0127247 filed on October 5, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated as part of this specification.
[0002] The present invention relates to a lithium secondary battery, and more specifically, to a lithium secondary battery that uses a layered perlithium manganese oxide as a positive electrode active material and a mixture of silicon oxide and a carbon-based negative electrode active material as a negative electrode active material. [Background technology]
[0003] Recently, lithium secondary batteries have been attracting attention as an energy source for electric vehicles. As the use of electric vehicles increases, there is an increasing need for lithium secondary batteries that can travel longer distances on a single charge and can be quickly charged in a shorter time. This has led to a demand for the development of lithium secondary batteries that have high energy density and can be quickly charged.
[0004] Lithium secondary batteries are generally manufactured by forming an electrode assembly by interposing a separator between a positive electrode including a positive electrode active material made of a lithium-containing transition metal oxide and a negative electrode including a negative electrode active material capable of storing lithium ions, inserting the electrode assembly into a battery case, injecting a non-aqueous electrolyte that serves as a medium for transferring lithium ions, and then sealing the battery case. The non-aqueous electrolyte is generally composed of a lithium salt and an organic solvent capable of dissolving the lithium salt.
[0005] Conventionally, carbon-based materials such as natural graphite and artificial graphite have been mainly used as the negative electrode active material of lithium secondary batteries. However, since such carbon-based negative electrode active materials have a small capacity, there has been a limit in achieving high capacity in secondary batteries applying this material. Therefore, the development of lithium secondary batteries applying silicon-based negative electrode active materials, which have a theoretical capacity more than 10 times larger than that of carbon-based materials, has been attempted. In the case of silicon-based negative electrode active materials, there is an advantage that a higher capacity can be achieved compared to carbon-based materials. However, during the charging process, the volume expands rapidly, and damage to the negative electrode and interruption of the conduction path may occur. Therefore, there is a problem that the battery performance deteriorates rapidly.
[0006] Therefore, the development of lithium secondary batteries applying silicon-based negative electrode active materials and having excellent life characteristics is required.
Summary of the Invention
Problems to be Solved by the Invention
[0007] The present invention is for solving the above problems, and by including SiOx and over-lithiated manganese-based oxides having excellent capacity characteristics as active materials, it aims to provide a lithium secondary battery having a high energy density and excellent life characteristics.
Means for Solving the Problems
[0008] In one aspect, the present invention includes a negative electrode, a positive electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte. The negative electrode includes SiOx (where 0 < x < 2) and a carbon-based negative electrode active material. The positive electrode includes a positive electrode active material containing an over-lithiated manganese-based oxide in which the content of manganese exceeds 50 mol% of the total metals other than lithium and the ratio (Li / Me) of the number of moles of lithium to the number of moles of the total metals other than lithium exceeds 1. It provides a lithium secondary battery in which the SiOx usage depth defined by the following formula (1) is 1 to 15, preferably 3 to 15, in the state of SOC 0%. Formula (1): SiOx usage depth = (capacity of Li remaining in the negative electrode / capacity of SiOx in the negative electrode) × 100
[0009] On the one hand, the over-lithiated manganese-based oxide can be represented by the following [Chemical Formula 1]. [Chemical Formula 1] Li a Ni b Co c Mn d M e O2 In Chemical Formula 1, 1 < a, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.1, 0.5 ≤ d < 1.0, 0 ≤ e ≤ 0.2, and M can be at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr. Preferably, 1.1 ≤ a ≤ 1.5, 0.1 ≤ b ≤ 0.4, 0 ≤ c ≤ 0.05, 0.5 ≤ d ≤ 0.80, 0 ≤ e ≤ 0.1.
[0010] On the other hand, the positive electrode active material is D 50 can be 2 μm to 10 μm, and the BET specific surface area can be 1 to 10 m 2 / g.
[0011] Also, the initial irreversible capacity of the positive electrode can be 5% to 70%, and the electrode density can be 2.5 to 3.8 g / cc.
[0012] The negative electrode can contain a SiOx: carbon-based negative electrode active material in a weight ratio of 1:99 to 50:50.
[0013] The degree of prelithiation of the negative electrode represented by the following formula (2) can be 1% to 30%. Formula (2): Degree of prelithiation (%) = {Capacity per unit area of Li inserted into the negative electrode by prelithiation / Negative electrode loading amount} × 100
[0014] The negative electrode further contains a conductive material and a binder, and the conductive material can include single-walled carbon nanotubes.
[0015] The negative electrode may include a lower negative electrode mixture layer formed on a negative electrode current collector, and an upper negative electrode mixture layer formed on the lower negative electrode mixture layer.
[0016] The SiOx D 50 can be 3 μm to 8 μm.
[0017] The SiOx is M b Metal (where M b The metal can be doped with Group 1 alkali metal elements and / or Group 2 alkaline earth metal elements.
[0018] The lithium secondary battery may have an N / P ratio of 100% to 150%. Effect of the Invention
[0019] The lithium secondary battery of the present invention is designed so that the ratio of the remaining Li capacity to the SiOx capacity in the negative electrode in a fully discharged state (SOC=0) satisfies a specific range, thereby suppressing the expansion of SiOx during charging and discharging, and providing excellent safety and life characteristics.
[0020] In addition, the present invention uses a perlithium manganese-based oxide in which a rock-salt Li2MnO3 phase and a layered LiMO2 phase (where M is Ni, Co, or Mn) are mixed as the positive electrode active material, and a silicon-based negative electrode active material as the negative electrode active material, so that the excess lithium generated from the LiMO2 phase during the activation process can compensate for the irreversible capacity of the silicon-based negative electrode active material. Therefore, the use of a sacrificial positive electrode material or prelithiation for negative electrode compensation can be minimized, and the positive electrode capacity can be maximized.
[0021] In addition, the perlithium manganese oxide can be stably driven even at a relatively high voltage compared to the conventionally used lithium nickel cobalt manganese oxide. Therefore, when a positive electrode active material containing the perlithium manganese oxide is used together with a silicon-based negative electrode active material, a high energy density can be achieved by increasing the driving voltage.
[0022] Furthermore, the lithium secondary battery of the present invention is excellent in energy density and rapid charging performance since it contains, as the negative electrode active material, a silicon-based negative electrode active material that is excellent in capacity and rate characteristics. [Brief description of the drawings]
[0023] [Figure 1] 1 is an image showing the formation of a conductive path on the surface of a negative electrode active material when single-walled carbon nanotubes are used as a conductive material. [Diagram 2] 1 is an image showing the formation of a conductive path on the surface of a negative electrode active material when multi-walled carbon nanotubes are used as a conductive material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to best describe his / her invention.
[0025] In the present invention, the term "primary particle" refers to a particle unit that does not have grain boundaries when observed at a magnification of 5,000 to 20,000 times using a scanning electron microscope. The term "average particle size of primary particles" refers to the arithmetic average value calculated after measuring the particle sizes of primary particles observed from a scanning electron microscope image.
[0026] In the present invention, the "secondary particles" refer to particles formed by agglomeration of a plurality of primary particles.
[0027] In the present invention, the "average particle size D 50 " means the particle diameter at 50% of the volume cumulative particle size distribution of the particle powder to be measured (e.g., positive electrode active material powder, negative electrode active material powder, etc.). 50can be measured using the laser diffraction method. For example, the powder of the particles to be measured is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), where it is irradiated with ultrasonic waves of about 28 kHz at an output of 60 W, and a volume cumulative particle size distribution graph is obtained, and the particle diameter corresponding to 50% of the volume cumulative amount is calculated.
[0028] In the present invention, the "N / P ratio" refers to the percentage of the negative electrode loading amount to the positive electrode loading amount, that is, (negative electrode loading amount / positive electrode loading amount)×100.
[0029] In this specification, the term "positive electrode loading amount" refers to the discharge capacity per unit area of the positive electrode (unit: mAh / cm 2 ), "negative electrode loading amount" is the discharge capacity per unit area of the negative electrode (unit: mAh / cm 2 )
[0030] The present invention will be specifically described below.
[0031] As a result of extensive research into the development of a lithium secondary battery with excellent energy density and life characteristics, the inventors discovered that high energy density and excellent life characteristics can be achieved by using a perlithium manganese-based oxide with excellent capacity characteristics and SiOx as active materials, and designing the battery so that the depth of use of SiOx in a fully discharged state (SOC=0) satisfies a specific range, thereby completing the present invention.
[0032] The lithium secondary battery according to the present invention includes a negative electrode, a positive electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte. The negative electrode contains SiOx (where 0 < x < 2) and a carbon-based negative electrode active material as the negative electrode active material. The positive electrode contains a hyper-lithium manganese-based oxide in which the content of manganese exceeds 50 mol% among all metals other than lithium, and the ratio (Li / Me) of the number of moles of lithium to the number of moles of all metals other than lithium exceeds 1. In the state of SOC 0%, the depth of use of SiOx defined by the following formula (1) satisfies 1 to 15. Formula (1): Depth of use of SiOx (%) = (Capacity of Li remaining in the negative electrode / Capacity of SiOx in the negative electrode) × 100
[0033] Hereinafter, each component of the lithium secondary battery according to the present invention will be specifically described.
[0034] negative electrode The negative electrode according to the present invention contains silicon oxide (i.e., SiOx (where 0 < x < 2)) and a carbon-based negative electrode active material as the negative electrode active material. For example, the negative electrode according to the present invention includes a negative electrode current collector and a negative electrode active material layer formed on at least one surface of the negative electrode current collector, and the negative electrode active material layer contains SiOx (where 0 < x < 2) and a carbon-based negative electrode active material as the negative electrode active material.
[0035] SiOx (where 0 < x < 2) has a higher theoretical capacity than the carbon-based negative electrode active material and a faster reaction rate with lithium. Therefore, when SiOx is included as the negative electrode active material, the energy density and rapid charging performance are improved. However, SiOx has a large irreversible capacity and a large volume expansion during charge and discharge, so it is inferior in terms of life characteristics. In particular, when used in combination with a hyper-lithium manganese-based oxide in which an oxygen-redox reaction occurs, there is a problem that the deterioration of the life characteristics becomes more serious. In addition, when SiOx and a carbon-based negative electrode active material are mixed and used, non-uniformity occurs in the negative electrode due to the difference in the reaction rate between the silicon-based negative electrode active material and the carbon-based negative electrode active material, resulting in deterioration of the negative electrode.
[0036] In order to solve the above problems, the present invention minimizes the volume expansion and non-uniformity of the reaction between the negative electrode active materials during charging and discharging by controlling the depth of SiOx used in the negative electrode within a specific range.
[0037] Specifically, in the lithium secondary battery according to the present invention, the usage depth of SiOx defined by the following formula (1) at SOC 0%, i.e., in a fully discharged state, can be 1 to 15%, preferably 3 to 15%, and more preferably 5 to 15%.
[0038] Formula (1): SiOx usage depth (%) = (Li capacity remaining in negative electrode / SiOx capacity in negative electrode) × 100
[0039] According to the research of the present inventors, when the SiOx usage depth is less than 1% or exceeds 15% in the SOC 0% state (i.e., fully discharged state), the life characteristics are rapidly degraded. Specifically, when the SiOx usage depth is less than 1% in the fully discharged state, the volume of SiOx changes rapidly during the charge and discharge process, which causes a decrease in energy density and life characteristics, and when the SiOx usage depth exceeds 15% in the fully discharged state, the electrical connectivity of the electrode is reduced, which causes a decrease in life characteristics.
[0040] The SiOx usage depth is influenced by a ratio of the negative electrode loading amount to the positive electrode loading amount (N / P ratio), the composition of the negative electrode active material, the composition of the positive electrode active material, the degree of prelithiation of the negative electrode, activation conditions, etc., and the SiOx usage depth can be adjusted by appropriately controlling these factors.
[0041] On the other hand, the capacity of Li remaining in the negative electrode and the capacity of SiOx in the negative electrode at an SOC of 0% can be measured by the following method.
[0042] First, the lithium secondary battery is fully discharged, and then disassembled to separate the negative electrode. Then, a coin-half cell is manufactured using the separated negative electrode and a Li metal counter electrode, and the cell is delithiated at 0.1 C to 1.0 V to measure the discharge capacity. The discharge capacity measured at this time is the capacity generated by the Li remaining in the negative electrode, and therefore it can be evaluated as the capacity of Li remaining in the negative electrode.
[0043] Next, the capacity of SiOx in the negative electrode can be obtained by charging and discharging the coin-half cell at 0.1C in a voltage range of 0.005V to 1.0V to obtain a voltage-capacity graph, and then using the voltage-capacity graph.
[0044] Specifically, the SiOx capacity in the negative electrode can be determined by the following method.
[0045] When measuring a voltage-capacity graph of a coin half cell manufactured using a negative electrode containing a carbon-based negative electrode active material and SiOx, the gradient of the voltage-capacity graph changes abruptly around 0.25V, and the capacity realized at a voltage below the voltage at which the gradient changes abruptly (e.g., 0.25V) is the capacity attributable to the carbon-based negative electrode active material, and the capacity realized at a voltage above the voltage at which the gradient changes abruptly (e.g., 0.25V) is the capacity attributable to SiOx. Therefore, if the capacity at the point where the gradient changes abruptly in the capacity-voltage graph of the coin half cell is A and the total discharge capacity of the coin half cell is B, the capacity of SiOx in the negative electrode can be calculated as BA.
[0046] On the other hand, the SiOx may be, if necessary, b It can be doped with a metal, where M b The metal can be a Group 1 alkali metal element and / or a Group 2 alkaline earth metal element, such as Li, Mg, etc. bMetal-doped SiOx has high efficiency and can achieve high energy density, although the capacity of the active material is reduced by the doping element.
[0047] In addition, the SiOx may further include a carbon coating layer on the surface of the particles, if necessary. Here, the amount of carbon coating may be 20 wt% or less, preferably 0.1 to 20 wt%, based on the total weight of the SiOx active material. When the carbon coating is applied, the electrical conductivity of the SiOx surface is improved, the uniformity of the SEI layer is improved, and the initial efficiency and life characteristics can be improved. Here, the carbon coating layer may be formed by a method such as dry coating, wet coating, chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD), etc.
[0048] On the other hand, the SiOx preferably has a capacity of 1000 to 4000 mAh / g, preferably 1000 to 3800 mAh / g, and more preferably 1200 to 3800 mAh / g. When SiOx that satisfies the above capacity range is used, high capacity characteristics can be realized.
[0049] The SiOx may have an initial efficiency of 60 to 95%, 70 to 95%, and preferably 75 to 95%. Here, the initial efficiency of the SiOx means a percentage of a discharge capacity relative to a charge capacity measured by manufacturing a half cell with a negative electrode using 100% SiOx as a negative electrode active material and a Li metal counter electrode, and then charging and discharging the half cell in a voltage range of 0.01 V to 1.5 V at a 0.1 C rate. When the initial efficiency of the SiOx satisfies the above range, lithium provided from the positive electrode can be reversibly used, and excellent rapid charging performance can be realized.
[0050] The SiOx has an average particle size D 50can be 3 μm to 8 μm, preferably 4 μm to 7 μm, and Dmin to Dmax can be 0.01 μm to 30 μm, preferably 0.01 μm to 20 μm, and more preferably 0.5 μm to 15 μm. When the particle size of SiOx satisfies the above range, sufficient electrode density can be ensured when mixed with a carbon-based negative electrode active material.
[0051] Meanwhile, the carbon-based negative electrode active material may be any of various carbon-based negative electrode active materials used in the art, such as artificial graphite, natural graphite, graphitized carbon fiber, amorphous carbon, soft carbon, hard carbon, or a combination thereof. Preferably, artificial graphite, natural graphite, or a combination thereof may be used.
[0052] The carbon-based negative electrode active material has an average particle size D 50 However, the particle size of the carbon-based negative electrode active material may be in the range of 2 μm to 30 μm, and preferably 5 μm to 30 μm. When the particle size of the carbon-based negative electrode active material falls within the above range, sufficient electrode density can be ensured when mixed with SiOx.
[0053] Meanwhile, the SiOx and the carbon-based negative electrode active material can be contained in the negative electrode at a weight ratio (SiOx:carbon-based negative electrode active material) of 1:99 to 50:50, preferably 3:97 to 50:50, more preferably 5:95 to 50:50, and further preferably 5:95 to 30:70. When the mixing ratio of SiOx and the carbon-based negative electrode active material satisfies the above range, a secondary battery excellent in energy density, life characteristics, and rapid charging performance can be realized. If the ratio of SiOx is too low, the effect of improving the energy density and rapid charging performance is insufficient, and if the ratio of SiOx is too high, the life characteristics may be deteriorated.
[0054] Meanwhile, the negative electrode active material layer may further include a conductive material and a binder, if necessary.
[0055] Examples of the conductive material include spherical or flaky graphite; carbonaceous materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, single-walled carbon nanotubes, and multi-walled carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives. Of these, one type alone or a mixture of two or more types can be used. The conductive material can be included in an amount of 0.1 to 30% by weight, 0.1 to 20% by weight, or 0.1 to 10% by weight based on the total weight of the negative electrode active material layer.
[0056] Preferably, the conductive material may be a single-walled carbon nanotube. When the conductive material is a carbon nanotube, a conductive path is formed widely, which increases durability and reduces resistance, thereby realizing excellent life characteristics.
[0057] FIG. 1 shows an image illustrating the formation of conductive paths on the surface of a negative electrode active material when single-walled carbon nanotubes are used as the conductive material, and FIG. 2 shows an image illustrating the formation of conductive paths on the surface of a negative electrode active material when multi-walled carbon nanotubes are used as the conductive material.
[0058] As shown in Figures 1 and 2, when single-walled carbon nanotubes are used as a conductive material, conductive paths are uniformly formed on the surface of the negative electrode active material, thereby improving cycle characteristics.
[0059] Examples of the binder include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylic acid, polyacrylamide, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and among these, one type alone or a mixture of two or more types can be used. The binder can be contained in an amount of 1 to 20% by weight, 2 to 20% by weight, or 2 to 10% by weight based on the total weight of the negative electrode active material layer.
[0060] Meanwhile, the negative electrode may have a single negative electrode active material layer or a multi-layer structure composed of two or more layers. For example, the negative electrode may include a first negative electrode active material layer formed on a negative electrode current collector and a second negative electrode active material layer formed on the first negative electrode active material.
[0061] When the negative electrode active material layer has a multi-layer structure composed of two or more layers, each layer may have a different type and / or content of the negative electrode active material, binder, and / or conductive material.
[0062] For example, the first negative electrode active material layer (lower layer) may have a higher carbon-based negative electrode active material content than the second negative electrode active material layer (upper layer) and the second negative electrode active material layer may have a higher silicon-based negative electrode active material content than the first negative electrode active material layer, or the second negative electrode active material layer (upper layer) may have a higher conductive material content than the first negative electrode active material layer (lower layer).
[0063] By forming the negative electrode active material layer in a multi-layer structure and varying the composition of each layer, the performance characteristics of the battery can be improved. For example, when the upper layer is formed to have a higher content of conductive material or silicon-based negative electrode active material than the lower layer, the effect of improving the fast charging performance can be obtained.
[0064] On the other hand, in the present invention, the negative electrode may be a prelithiated negative electrode, if necessary.
[0065] The prelithiation of the negative electrode can be performed, for example, by a method of pressing or depositing lithium metal on a negative electrode active material layer, a method of inserting lithium into a negative electrode active material layer by an electrochemical method, a method of inserting excess lithium contained in a sacrificial positive electrode material contained in a positive electrode into the negative electrode by an activation process, or a method of providing excess lithium to the positive electrode by an electrochemical method or a method of pressing or depositing lithium metal, and then inserting the excess lithium provided to the positive electrode by the activation process into the negative electrode, or the like. Two or more of the above methods can be combined.
[0066] When the prelithiation process is performed, the SiOx use depth in a fully discharged state can be adjusted by adjusting the degree of prelithiation, and even when the SiOx content in the negative electrode is high compared to when prelithiation is not performed, the SiOx use depth that satisfies the range of the present invention can be realized. When the SiOx content in the negative electrode is high, the energy density increases, so that when a prelithiation negative electrode is used, a higher energy density can be realized than when a non-prelithiation negative electrode is used. That is, when a prelithiation negative electrode is applied, the SiOx content in the negative electrode can be increased and the SiOx use depth can be adjusted within the range of the present invention, thereby further improving the energy density and life characteristics.
[0067] Preferably, the negative electrode of the present invention has a degree of prelithiation represented by the following formula (2) of 1 to 30%, preferably 1 to 20%, and more preferably 3 to 20%.
[0068] Formula (2): Degree of prelithiation (%) = {Capacity per unit area of Li inserted into the negative electrode by prelithiation / negative electrode loading amount} × 100
[0069] When the degree of prelithiation of the negative electrode satisfies the above range, a lithium secondary battery having excellent energy density and life characteristics can be realized.
[0070] Meanwhile, the negative electrode active material layer may have a porosity of 20% to 70% or 20% to 50%. If the porosity of the negative electrode active material layer is too small, the electrolyte impregnation property may decrease, and the lithium mobility may decrease, whereas if the porosity is too large, the energy density may decrease.
[0071] positive electrode The positive electrode according to the present invention includes, as a positive electrode active material, a perlithium manganese-based oxide in which the manganese content of all metals other than lithium exceeds 50 mol % and the ratio of the number of moles of lithium to the number of moles of all metals other than lithium (Li / Me) exceeds 1. Specifically, the positive electrode of the present invention includes a positive electrode current collector and a positive electrode active material layer formed on at least one surface of the positive electrode current collector, and the positive electrode active material layer includes a perlithium manganese-based oxide in which the manganese content of all metals other than lithium exceeds 50 mol % and the ratio of the number of moles of lithium to the number of moles of all metals other than lithium (Li / Me) exceeds 1.
[0072] In the case of perlithium manganese oxides that contain excess lithium, they have a structure in which the layered phase (LiM'O2) and rock salt phase (Li2MnO3) are mixed, and the rock salt phase is activated during the initial activation process to generate excess lithium ions, achieving high capacity. In addition, because the lithium ions generated during the activation process compensate for the negative electrode irreversible capacity, there is no need to add a separate compensating material such as a sacrificial positive electrode material, and the capacity of the positive electrode can be increased.
[0073] Preferably, the lithium manganese-based oxide may be represented by Chemical Formula 1.
[0074] [Chemical Formula 1] Li a Ni b Co c Mn d M e O2
[0075] In Chemical Formula 1 above, M can be at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr.
[0076] On the other hand, a is the molar ratio of Li in the over-lithiated manganese-based oxide, and can be 1 < a, 1.1 ≤ a ≤ 1.5, or 1.1 ≤ a ≤ 1.3. When a satisfies the above range, the irreversible capacity of SiOx can be sufficiently compensated, and high-capacity characteristics can be realized.
[0077] The b is the molar ratio of Ni in the over-lithiated manganese-based oxide, and can be 0 ≤ b ≤ 0.5, 0.1 ≤ b ≤ 0.4, or 0.2 ≤ b ≤ 0.4.
[0078] The c is the molar ratio of Co in the over-lithiated manganese-based oxide, and can be 0 ≤ c ≤ 0.1, 0 ≤ c ≤ 0.08, or 0 ≤ c ≤ 0.05. When c exceeds 0.1, it is difficult to ensure high capacity, and gas generation and deterioration of the positive electrode active material may become serious, resulting in a decrease in life characteristics.
[0079] The d is the molar ratio of Mn in the over-lithiated manganese-based oxide, and can be 0.5 ≤ d < 1.0, 0.50 ≤ d ≤ 0.80, or 0.50 ≤ d ≤ 0.70. When d is less than 0.5, the ratio of the rock salt phase becomes excessively small, and the effects of negative electrode irreversible compensation and capacity improvement are not significant.
[0080] The e is the molar ratio of the doping element M in the over-lithiated manganese-based oxide, and can be 0 ≤ e ≤ 0.2, 0 ≤ e ≤ 0.1, or 0 ≤ e ≤ 0.05. If the content of the doping element is too much, it may have an adverse effect on the active material capacity.
[0081] Meanwhile, in the perlithium manganese oxide represented by the formula 1, the ratio of the number of moles of Li to the number of moles of all metal elements other than Li (Li / Me) can be 1.2 to 1.5, 1.25 to 1.5, or 1.25 to 1.4. When the Li / Me ratio satisfies the above range, the rate characteristic and capacity characteristic are excellent. If the Li / Me ratio is too high, the electrical conductivity decreases and the rock salt phase (Li2MnO3) increases, which may lead to a high rate of deterioration, and if the Li / Me ratio is too low, there is little effect in improving the energy density.
[0082] Meanwhile, the composition of the lithium manganese oxide may be represented by the following [Chemical Formula 2].
[0083] [Chemical formula 2] XLi2MnO3·(1-X)Li[Ni 1-y-z-w Mn y Co z M w ]O2
[0084] In the above [Chemical Formula 2], M may be at least one selected from the group consisting of metal ions Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr.
[0085] The X means the ratio of the Li2MnO3 phase in the perlithium manganese oxide, and may be 0.2≦x≦0.5, 0.25≦x≦0.5, or 0.25≦x≦0.4. When the ratio of the Li2MnO3 phase in the perlithium manganese oxide satisfies the above range, the irreversible capacity of the SiOx negative electrode active material can be sufficiently compensated, and high capacity characteristics can be achieved.
[0086] The y is a molar ratio of Mn in the LiM'O2 layer phase, and can be 0.4≦y<1, 0.4≦y≦0.8, or 0.4≦y≦0.7.
[0087] The z is a molar ratio of Co in the LiM'O2 phase and may be 0≦z≦0.1, 0≦z≦0.08, or 0≦z≦0.05. If z exceeds 0.1, gas generation and deterioration of the positive electrode active material may become serious, resulting in reduced life characteristics.
[0088] The w is the molar ratio of the doping element M in the LiM'O2 layer phase, and can be 0≦w≦0.2, 0≦w≦0.1, or 0≦w≦0.05.
[0089] Meanwhile, the positive electrode active material according to the present invention may further include a coating layer on the surface of the perlithium manganese-based oxide, if necessary. When the positive electrode active material includes a coating layer, the coating layer can suppress contact between the perlithium manganese-based oxide and the electrolyte, thereby reducing electrolyte side reactions, thereby improving the life characteristics.
[0090] The coating layer is a coating element M 1 The coating element M 1 For example, the coating element M may be at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr and Zr, and may be preferably Al, Co, Nb, W and combinations thereof, and more preferably Al, Co and combinations thereof. 1 can contain two or more kinds, for example, Al and Co.
[0091] The coating elements are in the oxide form in the coating layer, i.e., M 1 It can exist as Oz (1≦z≦4).
[0092] The coating layer can be formed by dry coating, wet coating, chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD), etc. Among them, the coating layer is preferably formed by atomic layer deposition, since it can be formed to have a large area.
[0093] The area of the coating layer formed may be 10 to 100%, preferably 30 to 100%, and more preferably 50 to 100% of the total surface area of the perlithium manganese oxide particles. When the area of the coating layer formed satisfies the above range, the effect of improving the life characteristics is excellent.
[0094] Meanwhile, the positive electrode active material according to the present invention may be in the form of secondary particles in which a plurality of primary particles are aggregated, and the average particle diameter D 50 However, the thickness of the positive electrode active material may be 2 μm to 10 μm, preferably 2 μm to 8 μm, and more preferably 4 μm to 8 μm. 50 When satisfies the above range, excellent electrode density can be achieved and the deterioration of capacity and rate characteristics can be minimized.
[0095] The positive electrode active material has a BET specific surface area of 1 m 2 / g~10m 2 / g, 3-8m 2 / g or 4~6m 2 If the BET specific surface area of the positive electrode active material is too low, the reaction area with the electrolyte is insufficient, making it difficult to achieve sufficient capacity, whereas if the specific surface area is too high, moisture absorption is rapid, accelerating side reactions with the electrolyte, making it difficult to ensure the life characteristics.
[0096] In addition, the positive electrode according to the present invention preferably has an initial irreversible capacity of about 5 to 70%, 5 to 50%, or 5 to 30%. The initial irreversible capacity of the positive electrode is a percentage of the discharge capacity when a half cell is charged and discharged at a voltage range of 2.5 to 4.4 V relative to the charge capacity when the half cell is charged at a high voltage of 4.6 V or more after preparing the half cell from the positive electrode and a lithium counter electrode, and is a value measured based on 0.1 C. When the initial irreversible capacity of the positive electrode satisfies the above range, the irreversible capacity of the silicon-based negative electrode active material can be sufficiently compensated for without using a separate compensation material such as a sacrificial positive electrode material.
[0097] Meanwhile, the perlithium manganese oxide may be prepared by mixing a transition metal precursor and a lithium source material and then calcining the mixture.
[0098] Examples of the lithium source material include lithium-containing carbonates (e.g., lithium carbonate, etc.), hydrates (e.g., lithium hydroxide hydrate (LiOH·H2O), etc.), hydroxides (e.g., lithium hydroxide), nitrates (e.g., lithium nitrate (LiNO3), etc.), and chlorides (e.g., lithium chloride (LiCl), etc.), and among these, one kind may be used alone or two or more kinds may be used in combination.
[0099] Meanwhile, the transition metal precursor may be in the form of a hydroxide, oxide or carbonate. When a precursor in the form of a carbonate is used, it is more preferable in that a positive electrode active material having a relatively high specific surface area can be prepared.
[0100] The transition metal precursor can be prepared by a co-precipitation process. For example, the transition metal precursor can be prepared by dissolving each transition metal-containing raw material in a solvent to prepare a metal solution, mixing the metal solution, an ammonium cation complexing agent and a basic compound, and then performing a co-precipitation reaction. If necessary, an oxidizing agent or oxygen gas can be further added during the co-precipitation reaction.
[0101] Here, the transition metal-containing raw material may be acetate, carbonate, nitrate, sulfate, halide, sulfide, etc. of each transition metal. Specifically, the transition metal-containing raw material may be NiO, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, Mn2O3, MnO2, Mn3O4MnCO3, Mn(NO3)2, MnSO4·H2O, manganese acetate, manganese halide, Mn2O3, MnO2, Mn3O4, MnCO3, Mn(NO3)2, MnSO4·H2O, manganese acetate, manganese halide, etc.
[0102] The ammonium cation complexing agent may be at least one selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and NH4CO3.
[0103] The basic compound may be at least one selected from the group consisting of NaOH, Na2CO3, KOH, and Ca(OH)2. The form of the precursor may vary depending on the type of basic compound used. For example, when NaOH is used as the basic compound, a hydroxide-form precursor can be obtained, and when Na2CO3 is used as the basic compound, a carbonate-form precursor can be obtained. In addition, when a basic compound and an oxidizing agent are used together, an oxide-form precursor can be obtained.
[0104] Meanwhile, the transition metal precursor and the lithium source material may be mixed in an amount such that the total transition metal (Ni+Co+Mn):Li molar ratio is 1:1.05 to 1:2, preferably 1:1.1 to 1:1.8, and more preferably 1:1.25 to 1:1.8.
[0105] Meanwhile, the firing may be performed at a temperature of 600° C. to 1000° C. or 700° C. to 950° C., and the firing time may be 5 hours to 30 hours or 5 hours to 20 hours. The firing atmosphere may be an air atmosphere or an oxygen atmosphere, for example, an atmosphere containing 20 to 100 volume % oxygen.
[0106] Meanwhile, the positive electrode active material layer may further include a conductive material and a binder in addition to the positive electrode active material.
[0107] Examples of the conductive material include spherical or flaky graphite; carbonaceous materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, single-walled carbon nanotubes, and multi-walled carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and among these, one type alone or a mixture of two or more types can be used. The conductive material can be included in an amount of 0.1 to 20 wt%, 1 to 20 wt%, or 1 to 10 wt% based on the total weight of the positive electrode active material layer.
[0108] Examples of the binder include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and among these, one type alone or a mixture of two or more types can be used. The binder can be included in an amount of 1 to 20% by weight, 2 to 20% by weight, or 2 to 10% by weight based on the total weight of the negative electrode active material layer.
[0109] Meanwhile, the positive electrode according to the present invention may have an electrode density of about 2.5 to 3.8 g / cc, about 2.5 to 3.5 g / cc, or about 3.0 to 3.3 g / cc. When the electrode density of the positive electrode satisfies the above range, a high energy density can be realized.
[0110] As described above, the lithium secondary battery of the present invention using the perlithium manganese oxide represented by Chemical Formula 1 as a positive electrode active material can stably operate the cell and achieve high capacity characteristics even if the end-of-charge voltage is set high to a level of 4.3V to 4.5V during operation of the battery.
[0111] Separator In the lithium secondary battery of the present invention, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular restrictions. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent humidification ability of the electrolyte solution is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting point glass fiber, polyethylene terephthalate fiber, etc., can be used. In addition, a coated separator containing a ceramic component or a polymeric substance can be used to ensure heat resistance or mechanical strength, and can be selectively used as a single layer or multilayer structure.
[0112] electrolyte In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.
[0113] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0114] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of solvents that can be used include carbonate-based solvents such as polycarbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; and sulfolanes.
[0115] The lithium salt can be used without any particular limitation as long as it is a compound that can provide lithium ions used in lithium secondary batteries. Specifically, the anion of the lithium salt is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 -, CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - The lithium salt may be at least one selected from the group consisting of LiPF6, LiN(FSO2)2, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2, etc. The lithium salt may be used in a concentration range of 0.1 to 5.0M.
[0116] The electrolyte may contain additives for the purpose of improving the life characteristics of the battery, suppressing the capacity decrease, suppressing gas generation, etc. Examples of the additives include various additives used in the technical field, such as fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinyl ethylene carbonate (VEC), ethylene sulfate (ESa), lithium difluorophosphate (LiPO2F2), lithium bisoxalate borate (LiBOB), lithium tetrafluoroborate (LiBF4), lithium difluorooxalate borate (LiDFOB), lithium difluorobisoxalate phosphate (LiDFBP), lithium tetrafluorooxalate phosphate (LiTFOP), lithium methyl sulfate (LiMS), lithium ethyl sulfate (LiES), propane sultone (PS), propene sultone (PRS), succinonitrile (SN), adiponite, etc. Tolyl (AND), 1,3,6-hexanetricarbonitrile (HTCN), 1,4-dicyano-2-butene (DCB), fluorobenzene (FB), ethyl di(prop-2-ynyl)phosphate (EDP), 5-methyl-5 propargyloxylcarbonyl-1,3-dioxane-2-one (MPOD), a compound represented by the following formula A (e.g., cyanoethyl polyvinyl alcohol, PVA-CN), a compound represented by the following formula B (e.g., heptafluorobutyl cyanoethyl polyvinyl alcohol, PF-PVA-CN), a compound represented by the following formula C (e.g., propargyl 1H-imidazole-1-carboxylate, PAC), and / or a compound represented by the following formula D (e.g., aryl imidazole such as C6H8N2), may be used.
[0117] [ka]
[0118] In the above chemical formula A, n and m each independently represent an integer of 1-100.
[0119] [ka]
[0120] [ka]
[0121] In the above chemical formula C, R 16 is a linear or non-linear alkylene group having 1 to 3 carbon atoms; R 17 ~R 19 are each independently at least one selected from the group consisting of hydrogen, an alkyl group having 1 to 3 carbon atoms, and a cyano group (-CN), and D is CH or N.
[0122] [ka]
[0123] In the above chemical formula D, R1, R2, R3, and R4 can each independently include hydrogen; or an alkyl group having 1 to 5 carbon atoms, a cyano group (CN), an allyl group, a propargyl group, an amine group, a phosphate group, an ether group, a benzene group, a cyclohexyl group, a silyl group, an isocyanate group (-NCO), or a fluoro group (-F).
[0124] Preferably, the additive may be a compound that acts as an oxygen scavenger. For example, a substance having a phosphite structure (see formula E) such as tristri(methylsilyl)phosphite (TMSPi), tristrimethylphosphite (TMPi), tris(2,2,2-trifluoroethyl)phosphite (TTFP), tristri(methylsilyl)phosphate (TMSPa), polyphosphate trimethylsilyl ester (PPSE), tris(pentafluorophenyl)borane (TPFPB), coumarin-3-carbonitrile (CMCN), 7-ethynylcoumarin (ECM), 3- Compounds containing a coumarin structure such as acetyl coumarin (AcCM) and 3-[(trimethylsilyl)coumarin (TMSCM) (see chemical formula F); 3-[(trimethylsilyl)oxyl]-2H-1-benzopyran-2-one (TMSOCM), 3-(2-propyn-1-yloxyl)-2H-1-benzopyran-2-one (POCM), 2-propyn-1-yl-2-iodo-2H-1-benzopyran-3-carboxylate (OBCM), etc. can be used as compounds that act as oxygen scavengers.
[0125] [ka]
[0126] [ka]
[0127] In the chemical formulas E and F, R1 to R6 can each independently include a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms and a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a cyano group (-CN), a fluoro group (F), an ether group (COC), a carboxyl group (OC=O), a trimethylsilyl group (-TMS), an isocyanate group (-NCO), and / or an isothiocyanate group (-NCS).
[0128] On the other hand, the lithium secondary battery according to the present invention may have an N / P ratio of 100% to 150%, preferably 105% to 130%, and more preferably 105% to 120%. If the N / P ratio is less than the above range, when it is less than 100%, lithium deposition may occur in the negative electrode, and when it exceeds 150%, it is difficult to realize the depth of use of SiOx within the range of the present invention.
[0129] On the other hand, the lithium secondary battery according to the present invention can realize excellent energy density and rapid charging performance by containing SiOx, and shows excellent life characteristics. Specifically, the lithium secondary battery according to the present invention can achieve 80% life reaching times of 510 times or more, preferably 530 times or more, more preferably 550 times or more, and can have an energy density of 460Wh / L or more, preferably 470Wh / L or more, more preferably 480Wh / L or more.
[0130] The present invention will now be described in more detail with reference to specific examples.
[0131] Example 1 <Production of positive electrodes> The positive electrode active material, conductive material, and PVDF binder were mixed in a weight ratio of 96:1:3 in N-methylpyrrolidone to prepare a positive electrode slurry. 1.143 [Ni 0.33 Mn 0.67 ] 0.857 O2 was used, and carbon nanotubes were used as the conductive material.
[0132] The positive electrode slurry was applied onto an aluminum collector sheet, dried, and then rolled to obtain a loading capacity of 4.30 mAh / cm 2 A positive electrode having the formula:
[0133] <Production of negative electrodes> Anode active material: Conductive material: Styrene-butadiene rubber (SBR): carboxymethyl cellulose (CMC) was mixed in water in a weight ratio of 96.2:0.8:2:1 to prepare anode slurry. Here, the anode active material was SiOx:graphite (Gr) mixed in a weight ratio of 5.5:94.5, and the conductive material was single-walled carbon nanotubes.
[0134] The negative electrode slurry was applied onto a copper current collector sheet, dried, and then rolled to obtain a loading capacity of 4.95 mAh / cm 2 A negative electrode having the formula:
[0135] <Manufacturing lithium secondary batteries> A separator was interposed between the positive and negative electrodes to prepare an electrode assembly, and the electrode assembly was inserted into a battery case and an electrolyte was injected to prepare a battery cell. The battery cell was then charged at a constant current of 0.1 C at 45° C. to 4.6 V, and then discharged at a constant current of 0.1 C to 2.0 V to activate the Li2MnO3 phase of the positive electrode active material, thereby preparing a lithium secondary battery.
[0136] Example 2 During the manufacture of the negative electrode, the negative electrode loading was 4.52 mAh / cm 2 A lithium secondary battery was produced in the same manner as in Example 1, except that the above-mentioned
[0137] Example 3 During the manufacture of the positive electrode, Li was coated with 1500 ppm of Al as the positive electrode active material. 1.167 [Ni 0.25 Mn 0.75 ] 0.833 A lithium secondary battery was produced in the same manner as in Example 1, except that O2 was used.
[0138] Example 4 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the activation step was performed by charging at a constant current of 0.1 C at 45° C. to 4.7 V, and then discharging at a constant current of 0.1 C to 2.0 V.
[0139] Examples 5 to 8 A lithium secondary battery was manufactured in the same manner as in Example 1, except that a negative electrode active material was prepared by mixing SiOx:graphite in a weight ratio of 10:90, and a prelithiation process was further performed by an electrochemical method after the preparation of the negative electrode so that the negative electrode had a prelithiation degree shown in Table 1 below.
[0140] Comparative Example 1 A lithium secondary battery was manufactured in the same manner as in Example 1, except that a mixture of SiOx and graphite in a weight ratio of 10:90 was used as the negative electrode active material during the manufacture of the negative electrode.
[0141] Comparative Example 2 During the manufacture of the negative electrode, the negative electrode loading was 5.16 mAh / cm 2 A lithium secondary battery was produced in the same manner as in Example 1, except that the above-mentioned
[0142] Comparative Example 3 A lithium secondary battery was manufactured in the same manner as in Example 1, except that a prelithiation process was further performed by an electrochemical method after the preparation of the negative electrode so that the negative electrode had a prelithiation degree shown in Table 1 below.
[0143] Comparative Example 4 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the activation step was performed by charging at a constant current of 0.1 C at 45° C. to 4.3 V, and then discharging at a constant current of 0.1 C to 2.0 V.
[0144] Comparative Example 5 When manufacturing the positive electrode, Li[Ni 0.8 Co 0.1 Mn 0.1 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the activation process was performed by charging the battery at a constant current of 0.1 C to 4.2 V using 1024×1000 and discharging the battery at a constant current of 0.1 C to 2.0 V using 1024×1000.
[0145] [Table 1]
[0146] Experimental Example 1 After the lithium secondary batteries of the Examples and Comparative Examples were fully discharged, the lithium secondary batteries were disassembled to separate the negative electrodes, and coin-half cells were fabricated using the separated negative electrodes and Li metal counter electrodes. The coin-half cells were delithiated to 1.0 V at a constant current of 0.1 C, and the discharge capacity up to the point of full discharge was measured, which was measured as the capacity of Li remaining in the negative electrode.
[0147] Next, the coin-half cell was charged and discharged at 25° C. and 0.1 C in the voltage range of 0.005 V to 1.0 V, and the discharge capacity of the negative electrode at 1 V was measured. The capacity due to SiOx in the negative electrode was measured using the measured discharge capacity of the negative electrode.
[0148] The measured values were substituted into the following formula (1) to calculate the usage depth of SiOx at SOC 0%.
[0149] Formula (1): SiOx usage depth = (capacity of Li remaining in the negative electrode / capacity of SiOx in the negative electrode) x 100
[0150] Experimental example 2: Number of times the life span reaches 80% The secondary batteries manufactured in the examples and comparative examples were charged at 25° C. at a constant current of 0.33 C to 4.35 V and then discharged at a constant current of 0.33 C to 2.5 V, which constitutes one cycle. The number of cycles at which the discharge capacity after the cycle reached 80% of the initial discharge capacity was measured. The measurement results are shown in Table 2 below.
[0151] Experimental example 3: Energy density (unit: Wh / L) The secondary batteries manufactured in the above examples and comparative examples were measured for energy density per unit volume in the voltage range of 4.35 to 2.5 V. The measurement results are shown in Table 2 below.
[0152] [Table 2]
[0153] As shown in Table 2, the batteries of Examples 1 to 8, which use a perlithium manganese oxide as a positive electrode active material and have a SiOx usage depth that falls within the range of the present invention in a fully discharged state, have excellent life characteristics compared to the batteries of Comparative Examples 1 to 4, which have a SiOx usage depth that falls outside the range of the present invention. Also, it can be seen that Comparative Example 5, which uses NCM instead of a perlithium manganese oxide as the positive electrode active material, has significantly lower life characteristics and energy density compared to the batteries of the Examples.
Claims
1. A lithium secondary battery including a negative electrode, a positive electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte, the negative electrode comprises SiOx (where 0<x<2) and a carbon-based negative electrode active material, The positive electrode includes, as a positive electrode active material, a perlithium manganese-based oxide in which a manganese content of all metals other than lithium exceeds 50 mol % and a ratio of the number of moles of lithium to the number of moles of all metals other than lithium (Li / Me) exceeds 1; A lithium secondary battery having an SiOx usage depth of 1 to 15, defined by the following formula (1), at an SOC of 0%. Formula (1): SiOx usage depth = (capacity of Li remaining in negative electrode / capacity of SiOx in negative electrode) x 100
2. 2. The lithium secondary battery according to claim 1, wherein the SiOx usage depth defined by the formula (1) is 3 to 15 at an SOC of 0%.
3. 2. The lithium secondary battery of claim 1, wherein the perlithium manganese oxide is represented by the following formula 1: [Chemical formula 1] Li a Ni b Co c Mn d M e O 2 In the above formula 1, 1<a, 0≦b≦0.5, 0≦c≦0.1, 0.5≦d<1.0, 0≦e≦0.2, and M is at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr.
4. 4. The lithium secondary battery according to claim 3, wherein, in Chemical Formula 1, 1.1≦a≦1.5, 0.1≦b≦0.4, 0≦c≦0.05, 0.5≦d≦0.80, and 0≦e≦0.
1.
5. The positive electrode active material is D 50 The lithium secondary battery according to claim 1, wherein the thickness is 2 μm to 10 μm.
6. The positive electrode active material has a BET specific surface area of 1 to 10 m 2 The lithium secondary battery according to claim 1, wherein the capacitance is 1 / g.
7. 2. The lithium secondary battery according to claim 1, wherein the positive electrode has an initial irreversible capacity of 5% to 70%.
8. 2. The lithium secondary battery according to claim 1, wherein the positive electrode has an electrode density of 2.5 to 3.8 g / cc.
9. 9. The lithium secondary battery according to claim 1, wherein the negative electrode comprises SiOx:carbon-based negative electrode active material in a weight ratio of 1:99 to 50:
50.
10. The lithium secondary battery according to claim 1, wherein the negative electrode has a degree of prelithiation represented by the following formula (2) of 1 to 30%. Formula (2): Degree of prelithiation (%)={capacity per unit area of Li inserted into the negative electrode by prelithiation / loading amount of the negative electrode}×100
11. The negative electrode further comprises a conductive material and a binder, The lithium secondary battery according to claim 1 , wherein the conductive material comprises single-walled carbon nanotubes.
12. D of the SiOx 50 The lithium secondary battery according to claim 1, wherein the average particle diameter is 3 μm to 8 μm.
13. 2. The lithium secondary battery according to claim 1, wherein the negative electrode includes a lower negative electrode mixture layer formed on a negative electrode current collector, and an upper negative electrode mixture layer formed on the lower negative electrode mixture layer.
14. The SiOx is M b Metal (where M b 2. The lithium secondary battery according to claim 1, wherein the metal is doped with an alkali metal element of Group 1 and / or an alkaline earth metal element of Group 2.
15. 2. The lithium secondary battery according to claim 1, wherein the lithium secondary battery has an N / P ratio of 100% to 150%.
16. 2. The lithium secondary battery according to claim 1, wherein the lithium secondary battery has an 80% life reaching number of 510 or more times and an energy density of 460 Wh / L or more.
Citation Information
Patent Citations
Lithium secondary battery
JP2016126976A
Lithium metal oxides with multiple phases and stable high energy electrochemical cycling
US20130149609A1
Nonaqueous electrolyte secondary battery
WO2016143543A1
KR20200089182A