Positive electrode and secondary battery including same
The positive electrode with a lithium composite transition metal oxide and optimized conductive material ratio addresses conductivity issues, enhancing energy density and stability in secondary batteries.
Patent Information
- Application Number
- JP2024519912
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-08
- Filing Date
- 2022-10-07
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2042-10-07
AI Technical Summary
Lithium cobalt oxide-based positive electrodes face limitations due to rising cobalt prices and supply issues, and NCM-based lithium composite transition metal oxides suffer from conductivity challenges, leading to decreased energy density and stability in secondary batteries.
A positive electrode design featuring a lithium composite transition metal oxide with nickel, cobalt, and manganese, in single particle form, and a specific ratio of BET specific surface areas of the active material and conductive material, forming a conductive network to enhance conductivity and energy density.
The design achieves high energy density and improved lifetime performance by optimizing the conductive network, preventing resistance increases and ensuring stable battery operation.
Smart Images

Figure 2024536293000001 
Figure 2024536293000002 
Figure 2024536293000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0134107 filed on October 8, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference. The present invention relates to a positive electrode and a secondary battery including the same. [Background technology]
[0002] In recent years, with the rapid spread of electronic devices that use batteries, such as mobile phones, notebook computers, and electric vehicles, the demand for secondary batteries that are small, lightweight, and have relatively high capacity is rapidly increasing. In particular, lithium secondary batteries, which are lightweight and have high energy density, have been attracting attention as a driving power source for portable electronic devices.
[0003] In general, a lithium secondary battery includes a positive electrode, a negative electrode, a separator between the positive electrode and the negative electrode, an electrolyte, an organic solvent, etc. In addition, the positive electrode and the negative electrode may have an active material layer including a positive electrode active material or a negative electrode active material formed on a current collector. In general, a lithium transition metal oxide is used as a positive electrode active material in the positive electrode, and thus, a carbon-based active material or a silicon-based active material not containing lithium is used as a negative electrode active material in the negative electrode.
[0004] In this regard, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMn2O4, etc.), lithium iron phosphate compound (LiFePO4), etc. have been used as the lithium transition metal oxide. Among them, lithium cobalt oxide (LiCoO2) is widely used due to its advantages of high operating voltage and excellent capacity characteristics, and is applied as a high voltage positive electrode active material. However, due to the rising price and unstable supply of cobalt (Co), there is a limit to its large-scale use as a power source in fields such as electric vehicles, and therefore the need for the development of a positive electrode active material that can replace it has arisen.
[0005] For this reason, nickel-cobalt-manganese-based lithium composite transition metal oxides (hereinafter simply referred to as "NCM-based lithium composite transition metal oxides") have been developed in which part of the cobalt (Co) is replaced with nickel (Ni) and manganese (Mn). Although such "NCM-based lithium composite transition metal oxides" have the advantage of being superior in charging speed compared to the lithium cobalt oxide, they have a problem in that a large specific surface area is required to ensure conductivity compared to the lithium cobalt oxide, and therefore a large amount of conductive material must be used to ensure conductivity, which makes it difficult to ensure the energy density of the positive electrode. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Korean Patent Publication No. 10-2019-0042992 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a positive electrode having high energy density and excellent life characteristics. Another object of the present invention is to provide a secondary battery including the above-mentioned positive electrode. [Means for solving the problem]
[0008] The present invention relates to a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, the positive electrode active material layer including a positive electrode active material and a conductive material, the conductive material including a linear conductive material, the positive electrode active material including a lithium composite transition metal oxide including nickel (Ni), cobalt (Co), and manganese (Mn), the lithium composite transition metal oxide being in a single particle form, and an average particle diameter (D 50 ) is 2 μm to 10 μm, and satisfies the following mathematical formula 1.
[0009] [Mathematical formula 1] 1.2≦B / A≦4.7
[0010] In the above mathematical formula 1, A is the weight percentage of the positive electrode active material relative to the BET specific surface area of the positive electrode active material × the weight of the positive electrode active material layer, and B is the weight percentage of the linear conductive material relative to the BET specific surface area of the linear conductive material × the weight of the positive electrode active material layer.
[0011] The present invention also provides a secondary battery including the above-mentioned positive electrode, a negative electrode facing the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte. Effect of the Invention
[0012] According to the present invention, the positive electrode includes a positive electrode active material including a lithium composite transition metal oxide including nickel, cobalt, and manganese, and a linear conductive material, and the positive electrode active material satisfies a specific average particle size range, and the lithium composite transition metal oxide has a single particle shape, and the content of the positive electrode active material and the linear conductive material in the positive electrode active material layer and the BET specific surface area satisfy a specific mathematical formula. The linear conductive material in the positive electrode active material layer is disposed between the positive electrode active materials to form a conductive network, so that an increase in resistance and a decrease in life performance due to insufficient conductivity can be prevented. In addition, the positive electrode that satisfies the specific mathematical formula 1 prevents a decrease in the energy density of the positive electrode due to the excessive addition of the conductive material, so that the positive electrode of the present invention has a high energy density and improved life performance, and can significantly prevent gas generation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0014] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. The singular expressions include the plural expressions unless otherwise clearly indicated in the context.
[0015] It should be understood that, as used herein, terms such as "comprises," "comprising," or "having" are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, but do not preclude the presence or additional possibility of one or more other features, numbers, steps, components, or combinations thereof.
[0016] In this specification, the average particle size (D 50 The average particle size (D) can be defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. 50 ) can be measured, for example, by using a laser diffraction method. The laser diffraction method generally allows measurement of particle sizes from the submicron range to about several mm, and can provide results with high reproducibility and high resolution.
[0017] In this specification, the BET specific surface area can be measured by a BET (Brunauer-Emmett-Teller) measurement method using an adsorption gas such as nitrogen and a BELSORP (BET apparatus) manufactured by BEL JAPAN.
[0018] The present invention will be specifically described below. <Positive electrode> The present invention relates to a positive electrode. Specifically, the positive electrode can be preferably used as a positive electrode for a lithium secondary battery.
[0019] Specifically, the positive electrode of the present invention includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, the positive electrode active material layer includes a positive electrode active material and a conductive material, the conductive material includes a linear conductive material, the positive electrode active material includes a lithium composite transition metal oxide including nickel (Ni), cobalt (Co), and manganese (Mn), the lithium composite transition metal oxide is in a single particle form, and the average particle size (D 50 ) is 2 μm to 10 μm and is characterized in that the following mathematical formula 1 is satisfied.
[0020] [Mathematical formula 1] 1.2≦B / A≦4.7
[0021] In the above mathematical formula 1, A is the weight percentage of the positive electrode active material relative to the BET specific surface area of the positive electrode active material × the weight of the positive electrode active material layer, and B is the weight percentage of the linear conductive material relative to the BET specific surface area of the linear conductive material × the weight of the positive electrode active material layer.
[0022] According to the present invention, the positive electrode includes a positive electrode active material including a lithium composite transition metal oxide including nickel, cobalt, and manganese, and a linear conductive material, and the positive electrode active material satisfies a specific average particle size range, and the lithium composite transition metal oxide has a single particle shape, and the content of the positive electrode active material and the linear conductive material in the positive electrode active material layer and the BET specific surface area satisfy a specific mathematical formula. The linear conductive material in the positive electrode active material layer is disposed between the positive electrode active materials to form a conductive network, so that an increase in resistance and a decrease in life performance due to insufficient conductivity can be prevented. In addition, the positive electrode that satisfies the specific mathematical formula 1 prevents a decrease in the energy density of the positive electrode due to the excessive addition of the conductive material, so that the positive electrode of the present invention has a high energy density and improved life performance, and can significantly prevent gas generation.
[0023] [Positive electrode current collector] The positive electrode current collector is not particularly limited as long as it does not induce a chemical change in the battery and has high conductivity. Specifically, the positive electrode current collector may include at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and an aluminum-cadmium alloy, and may specifically include aluminum.
[0024] The positive electrode current collector may usually have a thickness of 3 μm to 500 μm. The positive electrode current collector may have a surface with fine projections and recesses to strengthen the bonding force of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, a sheet, a foil, a mesh, a porous body, a foam, a nonwoven fabric, etc.
[0025] [Cathode active material layer] The positive electrode active material layer may be disposed on at least one surface of the positive electrode current collector. More specifically, the positive electrode active material layer may be disposed on one surface or both surfaces of the positive electrode current collector.
[0026] The positive electrode active material layer may include a positive electrode active material and a conductive material. The positive electrode active material may include a lithium composite transition metal oxide including nickel (Ni), cobalt (Co), and manganese (Mn). Specifically, the positive electrode active material may be a lithium composite transition metal oxide.
[0027] The molar ratio (Li / M) of lithium to all metal elements (M) excluding lithium in the lithium composite transition metal oxide may be 0.98 to 1.05, specifically 1.0 to 1.04. When it is in the above range, it is preferable in terms of improving the capacity and preventing an increase in resistance due to an increase in lithium residue.
[0028] Specifically, the lithium composite transition metal oxide may include a compound represented by the following Chemical Formula 1:
[0029] [Chemical formula 1] Li 1+p [Ni 1-(x1+y1+z1) Co x1Mn y1 M a z1 1-p O2
[0030] In Chemical Formula 1 above, M a is at least one element selected from the group consisting of Al, Ti, Zr, Mg, Nb, Ba, Ca, Ta, Sr, Zr, and Y, and -0.02 ≦ p ≦ 0.05, 0 < x1 < 1, 0 < y1 < 1, 0 ≦ z1 ≦ 0.1 may be satisfied.
[0031] In the lithium composite transition metal oxide of Chemical Formula 1 above, Li may be contained in an amount corresponding to 1 + p, that is, 0.98 ≦ 1 + p ≦ 1.05, 1.0 ≦ 1 + p ≦ 1.04. When within the above range, it is preferable in terms of preventing capacity degradation and preventing resistance due to an increase in Li residues.
[0032] In the lithium composite transition metal oxide of Chemical Formula 1 above, Ni may be contained in an amount corresponding to 1 - (x1 + y1 + z1), for example, 0 < 1 - (x1 + y1 + z1) < 1. More preferably, Ni may be contained in an amount of 0.5 ≦ 1 - (x1 + y1 + z1) ≦ 0.95. When contained within the above content range, it is possible to achieve high capacity and ensure excellent stability.
[0033] In the lithium composite transition metal oxide of Chemical Formula 1 above, Co may be contained in an amount corresponding to x1, that is, 0 < x1 < 1, specifically 0.1 ≦ x1 ≦ 0.4.
[0034] In the lithium composite transition metal oxide of Chemical Formula 1 above, Mn may be contained in an amount corresponding to y1, that is, 0 < x1 < 1, specifically 0.1 ≦ x1 ≦ 0.4. When within the above range, it is preferable in terms of improving the stability of the positive electrode active material and, as a result, being able to improve the stability of the battery.
[0035] In the lithium composite transition metal oxide of Chemical Formula 1 above, M a may be a doping element contained in the crystal structure of the lithium composite transition metal oxide, and Ma may be contained in an amount corresponding to z1, that is, 0≦z1≦0.1.
[0036] The lithium composite transition metal oxide or the positive electrode active material according to the present invention is in the form of a single particle. When the lithium composite transition metal oxide is in the form of a single particle, it has the advantage of having a lower initial resistance and less cracking of particles during rolling compared to when it is in the form of secondary particles, but has the disadvantage of a high resistance increase rate due to cycling. For this reason, when the lithium composite transition metal oxide is in the form of a single particle, the positive electrode according to the present invention is preferable in that it can ensure conductivity, improve energy density, and improve life characteristics by satisfying the mathematical formula 1 described below, and can prevent resistance increase due to cycling. When the lithium composite transition metal oxide or the positive electrode active material is in the form of a secondary particle, the specific surface area is relatively large and the electrolyte side reaction is excessive, so that even if the above mathematical formula 1 is satisfied, it is not possible to achieve the intended life performance, rate characteristic improvement effect, and gas generation suppression effect.
[0037] In this specification, the term "single particle" refers to a primary structure of a single particle, which is composed of primary particles and not of secondary particles. In addition, in this specification, the term "secondary particle" refers to an aggregate of primary particles aggregated together by physical or chemical bonds between the primary particles, i.e., a secondary structure, even if there is no intentional aggregation or granulation process for the primary particles that constitute the secondary particle.
[0038] The average particle size (D 50 ) is 2 μm to 10 μm. If the average particle size (D 50 If the average particle diameter (D) of the positive electrode active material is less than 2 μm, the specific surface area increases relatively, and the side reaction of the electrolyte becomes serious. Even if the above-mentioned mathematical formula 1 is satisfied, the life performance, rate characteristic, and gas generation prevention effect cannot be obtained. 50) exceeds 10 μm, the lithium ion diffusion path becomes longer as the average particle size becomes excessively large, so that even if the above mathematical formula 1 is satisfied, the rate characteristic is significantly reduced and no improvement in life performance can be expected.
[0039] The average particle size (D 50 ) may be specifically 3 μm to 8 μm, more specifically 3.5 μm to 6.0 μm. When it is in the above range, the strength of the particles is increased, and cracking of the particles during rolling can be suppressed, the rolling density can be improved, the specific surface area can be reduced, lithium by-products can be reduced, and the amount of gas generated due to a side reaction with the electrolyte can be reduced.
[0040] The BET specific surface area of the positive electrode active material is 0.2 m 2 / g~3m 2 / g, specifically 0.4m 2 / g~1m 2 / g, more specifically 0.7m 2 / g~1m 2 When the content is within the above range, it is preferable in terms of suppressing gas generation due to a side reaction on the positive electrode surface, and in particular, by satisfying mathematical formula 1 described later, it is possible to more preferably achieve the effects of ensuring the conductivity of the positive electrode, improving the energy density, and improving the life characteristics.
[0041] The positive electrode active material may be contained in the positive electrode active material layer in an amount of 90% by weight to 99% by weight, specifically 92% by weight to 98% by weight. When the amount is within the above range, the capacity and energy density of the positive electrode can be improved, and the effect of ensuring the conductivity of the positive electrode, improving the energy density, and improving the life characteristics by satisfying the mathematical formula 1 described below can be more preferably realized.
[0042] The conductive material can be used to assist and improve the electrical conductivity of the positive electrode. The conductive material includes a linear conductive material. The term "linear conductive material" is used to distinguish it from conductive materials such as dot-shaped, particulate-shaped, and plate-shaped conductive materials. The linear conductive material is a long fibrous conductive material and can contribute to the electrical contact between the positive electrode active materials and the formation of a conductive network. The formation of a conductive network by the linear conductive material can minimize the content of the conductive material in the positive electrode, thereby increasing the content of the positive electrode active material and improving the energy density of the positive electrode. In particular, according to the present invention, by satisfying the mathematical formula 1 described below, the conductivity of the positive electrode, the energy density, and the life characteristics can be more preferably achieved.
[0043] The linear conductive material may be at least one selected from conductive fibers and carbon nanotubes. More specifically, it may be carbon nanotubes. The conductive fibers may be carbon fibers, metal fibers, etc., and the carbon nanotubes may be single-walled carbon nanotubes, multi-walled carbon nanotubes, etc. More specifically, the linear conductive material may be carbon nanotubes, which have a long fiber length and a high degree of graphitization and crystallinity, and are therefore preferable for electrical contact of the positive electrode active material and for forming a conductive network.
[0044] The BET specific surface area of the linear conductive material is 150m 2 / g~300m 2 / g, specifically 170m 2 / g~210m 2 When the specific surface area is within the above range, it is preferable in that gas generation is suppressed due to the specific surface area being reduced to a preferable level, and by satisfying the mathematical formula 1 described later, it is possible to more preferably achieve the effects of ensuring the conductivity of the positive electrode, improving the energy density, and improving the life characteristics.
[0045] The BET specific surface area of the linear conductive material may be 150 to 450 times, more specifically 180 to 300 times, as compared with the BET specific surface area of the positive electrode active material. This is preferable in terms of realizing battery capacity while ensuring sufficient conductivity.
[0046] The pellet density of the linear conductive material may be 0.09 g / cc to 0.16 g / cc, specifically 0.095 g / cc to 0.145 g / cc. When the pellet density is within the above range, the rolling density of the electrode can be adjusted to a preferred level, which is preferable in that the energy density can be improved.
[0047] The pellet density may refer to the density measured by placing 5 g of the linear conductive material in a mold having a diameter of 22 mm and measuring the density at a pressure of 2 tons using a powder resistance meter (device name: HPRM-A2, manufacturer: HANTECH).
[0048] The average length of the linear conductive material may be 1 μm to 100 μm, specifically 5 μm to 30 μm. When it is in the above range, it is preferable because the conductive network between the active materials can be smoothly maintained.
[0049] In this specification, the average length of the linear conductive material is measured by the following method. A solution (solid content is 1% by weight based on the total weight of the solution) in which the linear conductive material and carboxymethyl cellulose (CMC) are added to water in a weight ratio of 40:60 is diluted 1,000 times with water. Then, 20 ml of the diluted solution is filtered through a filter, and the filter from which the linear conductive material has been filtered is dried. 100 images of the dried filter are taken with a scanning electron microscope (SEM), and the length of the linear conductive material is measured using the imageJ program, and the average value of the lengths is defined as the average length of the linear conductive material.
[0050] The linear conductive material may have an average diameter of 5 nm to 30 nm, preferably 10 nm to 20 nm. When the average diameter of the linear conductive material is within the above range, it is preferable in terms of preventing breakage of the linear conductive material and ensuring flexibility.
[0051] In this specification, the average diameter of the linear conductive material is measured by the following method. A solution (solid content is 1% by weight based on the total weight of the solution) in which linear conductive material and carboxymethyl cellulose (CMC) are added to water in a weight ratio of 40:60 is diluted 1,000 times with water. A drop of the diluted solution is placed on a TEM grid, and the TEM grid is dried. The dried TEM grid is observed with a TEM device (product name: H7650, manufacturer: Hitachi) to measure the average diameter of the linear conductive material.
[0052] The linear conductive material may be included in the positive electrode active material layer in an amount of 0.50 wt% to 1.75 wt%, specifically 0.8 wt% to 1.7 wt%, more specifically 1.0 wt% to 1.5 wt%. When the amount is within the above range, the conductivity of the positive electrode is maintained at a desired level, and the problem of the linear conductive material being agglomerated due to the addition of an excessive amount of the linear conductive material, which results in the formation of a non-uniform conductive network in the positive electrode, is prevented, and the content of the positive electrode active material is increased, thereby improving the energy density of the positive electrode.
[0053] The weight percentage of the linear conductive material with respect to the total weight of the positive electrode active material layer may be 0.006 to 0.019 times, specifically 0.013 to 0.018 times, and more specifically 0.014 to 0.017 times the weight percentage of the positive electrode active material with respect to the total weight of the positive electrode active material layer. When it is within the above range, it is possible to more preferably realize the effects of ensuring the conductivity of the positive electrode, improving the energy density, and improving the life characteristics by satisfying the mathematical formula 1 described later.
[0054] The conductive material may further include dot-shaped conductive materials in addition to the linear conductive materials. The dot-shaped conductive materials may refer to, for example, particulate conductive materials. Specifically, the dot-shaped conductive materials may include at least one selected from the group consisting of graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; fluorocarbon; metal powder such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives.
[0055] More specifically, the conductive material may be a linear conductive material. For example, the conductive material may include only linear conductive material without including dot-shaped conductive material. According to the present invention, excellent conductivity and improved life performance can be ensured by satisfying the relationship of Mathematical Equation 1, but if both linear conductive material and dot-shaped conductive material are included, it is difficult to form a uniform conductive network due to the addition of dot-shaped conductive material, or the content of positive electrode active material is reduced, resulting in insufficient improvement in energy density.
[0056] The positive electrode active material layer may further include a binder. The binder is a component that assists in binding the active material and conductive material, etc., and in binding to the current collector, and specifically may include at least one selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, and fluororubber, preferably at least one selected from the group consisting of polyvinylidene fluoride and carboxymethyl cellulose, and more preferably polyvinylidene fluoride.
[0057] In order to ensure sufficient binding strength between components such as the positive electrode active material, the binder may be contained in the positive electrode active material layer in an amount of 0.1 wt % to 10 wt %, preferably 0.1 wt % to 3 wt %, and more specifically 0.5 wt % to 2.5 wt %.
[0058] When the positive electrode active material layer further includes a binder, the binder may be included in the positive electrode active material layer in an amount remaining after excluding the positive electrode active material and the linear conductive material.
[0059] The positive electrode active material layer may further include a thickener. The thickener is used for smooth dispersion of the active material, conductive material, binder, etc., and is not particularly limited as long as it is used in the relevant field. For example, the thickener may be carboxymethyl cellulose. The thickener may be contained in the positive electrode active material layer in an amount of 0.1% by weight to 10% by weight, preferably 0.1% by weight to 3% by weight.
[0060] When the positive electrode active material layer further includes the thickener, the thickener may be included in the positive electrode active material layer in an amount remaining after excluding the positive electrode active material and the linear conductive material. Specifically, when the positive electrode active material layer further includes the binder and the thickener, the binder and the thickener may be included in the positive electrode active material layer in an amount remaining after excluding the positive electrode active material and the linear conductive material.
[0061] In the present invention, the positive electrode is characterized in that it satisfies the following mathematical formula 1:
[0062] [Mathematical formula 1] 1.2≦B / A≦4.7
[0063] In the above mathematical formula 1, A is the weight percentage of the positive electrode active material relative to the BET specific surface area of the positive electrode active material × the weight of the positive electrode active material layer, and B is the weight percentage of the linear conductive material relative to the BET specific surface area of the linear conductive material × the weight of the positive electrode active material layer.
[0064] According to the above mathematical formula 1, the relationship between the specific surface area and the content of the positive electrode active material and the conductive material can be optimally adjusted in terms of improving the conductivity, energy density, and life performance of the positive electrode. If B / A is less than 1.2, the conductive material is contained in an excessively small amount, resulting in a decrease in conductivity or insufficient electrical contact of the positive electrode active material, resulting in an increase in the resistance of the positive electrode and a significant decrease in cycle characteristics. If B / A is more than 4.7, the conductive material is added in an excessive amount, resulting in a decrease in the content of the positive electrode active material, resulting in a decrease in energy density, and the formation of a uniform conductive network in the positive electrode may be difficult due to the occurrence of aggregation of the linear conductive material.
[0065] In the above mathematical formula 1, the B / A may be specifically 1.8 to 4.2, more specifically 2.7 to 4.2, and even more specifically 3.2 to 3.7. When it is in the above range, the above-mentioned effects of ensuring the conductivity of the positive electrode and improving the life characteristics are further improved.
[0066] In the above mathematical formula 1, the units of the weight percentage and the BET specific surface area of the positive electrode active material and the linear conductive material are the same. For example, the unit of the weight percentage of the positive electrode active material and the linear conductive material in the above mathematical formula 1 may be "wt%" with respect to the weight of the positive electrode active material, and the unit of the BET specific surface area of the positive electrode active material and the linear conductive material in the above mathematical formula 1 may be "m 2 / g".
[0067] The positive electrode may be manufactured by a typical method for manufacturing a positive electrode, except that it is manufactured to satisfy the mathematical formula 1 according to the present invention. For example, the positive electrode may be manufactured by dissolving or dispersing components constituting a positive electrode active material layer, i.e., a positive electrode active material, a conductive material, a binder, etc., in a solvent to prepare a positive electrode slurry, applying the positive electrode slurry to at least one surface of a positive electrode current collector, and then drying and rolling the positive electrode slurry, or by casting the positive electrode slurry on a separate support, peeling it off from the support, and laminating the resulting film on the positive electrode current collector.
[0068] <Secondary battery> The present invention also provides a secondary battery including the above-described positive electrode. Specifically, the secondary battery according to the present invention includes the above-mentioned positive electrode, a negative electrode facing the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte. The positive electrode has been described above.
[0069] The negative electrode faces the positive electrode. The negative electrode may include a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector.
[0070] The negative electrode current collector is not particularly limited as long as it does not induce a chemical change in the battery and has high conductivity. Specifically, the negative electrode current collector may include at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and an aluminum-cadmium alloy, and may specifically include copper.
[0071] The negative electrode current collector may usually have a thickness of 3 μm to 500 μm. The negative electrode current collector may have a surface with fine projections and recesses to strengthen the binding force of the negative electrode active material. For example, the negative electrode current collector may be used in various forms such as a film, a sheet, a foil, a mesh, a porous body, a foam, a nonwoven fabric, etc.
[0072] The negative electrode active material layer may be disposed on at least one surface of the negative electrode current collector. Specifically, the negative electrode active material layer may be disposed on one surface or both surfaces of the negative electrode current collector.
[0073] The negative electrode active material layer may include a negative electrode active material. The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiOv (0 < v < 2), metal oxides capable of lithium doping and undoping, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compound and the carbonaceous material, such as Si-C composites or Sn-C composites, etc. may be mentioned, and any one or a mixture of two or more of these may be used. Further, a thin film of metallic lithium may be used as the negative electrode active material. Further, as the carbon material, any of low-crystalline carbon and high-crystalline carbon may be used. Representative examples of the low-crystalline carbon are soft carbon and hard carbon, and representative examples of the high-crystalline carbon are amorphous, plate-like, flaky, spherical, or fibrous natural graphite or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.
[0074] In addition to the negative electrode active material described above, the negative electrode active material layer may further contain a negative electrode binder, a negative electrode conductive material, and / or a thickener. The negative electrode binder is a component that assists in the bonding between the active material and / or the current collector, and may usually be contained in the negative electrode active material layer at 1 wt% to 30 wt%, preferably 1 wt% to 10 wt%.
[0075] The negative electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, and fluororubber, preferably at least one selected from polyvinylidene fluoride and styrene-butadiene rubber.
[0076] As the thickener, any thickener used in conventional lithium secondary batteries may be used, and an example thereof is carboxymethyl cellulose (CMC).
[0077] The negative electrode conductive material is a component for further improving the conductivity of the negative electrode active material, and may be contained in the negative electrode active material layer in an amount of 1 wt % to 30 wt %, preferably 1 wt % to 10 wt %.
[0078] The negative electrode conductive material is not particularly limited as long as it does not induce a chemical change in the battery and has conductivity, and examples of the negative electrode conductive material that can be used include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber and metal fiber; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. Specific examples of commercially available conductive materials include acetylene black-based products from Chevron Chemical Company, Denka Singapore Private Limited, Gulf Oil Company, Ketjenblack, EC-based products (from Armak Company), Vulcan XC-72 (from Cabot Company), and Super P (from Timcal).
[0079] The negative electrode may be manufactured by a conventional method for manufacturing a negative electrode that is generally known in the art. For example, the negative electrode may be manufactured by dissolving or dispersing components constituting the negative electrode active material layer, i.e., the negative electrode active material, the negative electrode conductive material, and / or the negative electrode binder, in a solvent to prepare a negative electrode slurry, applying the negative electrode slurry to at least one surface of a negative electrode current collector, and then drying and rolling the negative electrode slurry, or by casting the negative electrode slurry on another support, peeling it off from the support, and laminating the resulting film on the negative electrode current collector.
[0080] Meanwhile, in the secondary battery, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a secondary battery can be used without any particular restrictions, and it is particularly preferable that the separator has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, in order to ensure heat resistance or mechanical strength, a coated separator containing a ceramic component or a polymeric substance may be used, and may be selectively used as a single layer or multilayer structure.
[0081] On the other hand, examples of the electrolyte include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used when manufacturing a secondary battery, but are not limited to these.
[0082] Specifically, the electrolyte may include an organic solvent and a lithium salt. The organic solvent may be used without any particular limitation as long as it can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Carbonate-based solvents such as ethylene carbonate (PC) and the like; alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as Ra-CN (Ra is a hydrocarbon group having a linear, branched, or cyclic structure with 2 to 20 carbon atoms, and may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among them, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant capable of improving the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferred. In this case, the cyclic carbonate and the chain carbonate are mixed in a volume ratio of about 1:1 to 9 to show excellent electrolyte performance.
[0083] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 may be used as the lithium salt. The concentration of the lithium salt is preferably within the range of 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has suitable conductivity and viscosity, so that excellent electrolyte performance can be exhibited and lithium ions can be effectively transferred.
[0084] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, or pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, in order to improve the life characteristics of the battery, suppress the decrease in battery capacity, and improve the discharge capacity of the battery. In this case, the additives may be contained in an amount of 0.1% by weight to 5% by weight based on the total weight of the electrolyte.
[0085] As described above, the secondary battery including the positive electrode active material according to the present invention has excellent electrical characteristics and high-temperature storage properties, and can be usefully applied to portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs), etc. In particular, the secondary battery according to the present invention can be usefully used as a high-voltage battery having a voltage of 4.45 V or more.
[0086] In addition, the secondary battery according to the present invention can be used as a unit cell of a battery module, and the battery module can be applied to a battery pack. The battery module or the battery pack can be used as a power source for any one or more medium- to large-sized devices including power tools, electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs), and power storage systems.
[0087] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings, in which: FIG. 1 is a schematic diagram of a semiconductor device according to an embodiment of the present invention;
[0088] [Examples and Comparative Examples] [Example 1: Production of positive electrode] As the positive electrode active material, Li[Ni 0.83 Co 0.11 Mn 0.06 A single particle lithium transition metal oxide was prepared, which was represented by the chemical formula: 2 / g, and the average particle size (D 50 ) was 4.4 μm.
[0089] Carbon nanotubes were prepared as linear conductive materials. The BET specific surface area of the carbon nanotubes was 185 m 2 / g and the pellet density was 0.12 g / cc.
[0090] The positive electrode active material, the linear conductive material, PVdF as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in an N-methylpyrrolidone solvent in a weight ratio of 97.00:0.68:1.20:1.12 to prepare a positive electrode slurry, which was then applied to an aluminum current collector, dried, and rolled to prepare the positive electrode of Example 1.
[0091] [Example 2: Production of positive electrode] A positive electrode was manufactured in the same manner as in Example 1, except that the positive electrode active material, linear conductive material, binder, and thickener used in Example 1 were mixed in a weight ratio of 97.00:1.47:1.20:0.33.
[0092] [Example 3: Production of positive electrode] A positive electrode was manufactured in the same manner as in Example 1, except that the positive electrode active material, linear conductive material, binder, and thickener used in Example 1 were mixed in a weight ratio of 97.00:1.68:1.20:0.12.
[0093] [Example 4: Production of positive electrode] The positive electrode active material, linear conductive material, binder, thickener, and dot-shaped conductive material, carbon black (BET specific surface area: 135 m) used in Example 1 were used. 2 A positive electrode was prepared in the same manner as in Example 1, except that the above-mentioned materials (w / g) were mixed in a weight ratio of 97.0:1.1:1.2:0.2:0.5.
[0094] [Example 5: Production of positive electrode] The positive electrode active material, linear conductive material, binder, thickener, and dot-shaped conductive material, carbon black (BET specific surface area: 135 m) used in Example 1 were used. 2 A positive electrode was prepared in the same manner as in Example 1, except that the above-mentioned materials (w / g) were mixed in a weight ratio of 97.00:0.75:1.20:0.05:1.00.
[0095] Comparative Example 1: Production of Positive Electrode A positive electrode was manufactured in the same manner as in Example 1, except that the positive electrode active material, linear conductive material, binder, and thickener used in Example 1 were mixed in a weight ratio of 97.00:0.42:1.20:1.38.
[0096] Comparative Example 2: Production of Positive Electrode A positive electrode was manufactured in the same manner as in Example 1, except that the positive electrode active material, linear conductive material, binder, and thickener used in Example 1 were mixed in a weight ratio of 97.00:1.89:1.00:0.11.
[0097] Comparative Example 3: Production of Positive Electrode Comparative Example 3 differs from Example 1 in that no linear conductive material is used. Specifically, the positive electrode active material, binder, and thickener similar to those in Example 1, and carbon black (BET specific surface area: 135 m) as a dot-shaped conductive material were used. 2 A positive electrode was prepared in the same manner as in Example 1, except that the materials (w / g) were mixed in a weight ratio of 96.6:1.2:0.2:2.0.
[0098] Comparative Example 4: Production of Positive Electrode As the positive electrode active material, Li[Ni 0.83 Co 0.11 Mn 0.06 A single particle lithium transition metal oxide was prepared, which was represented by the chemical formula: 2 / g, and the average particle size (D 50 ) was 1.5 μm. A positive electrode was produced in the same manner as in Example 1, except that the positive electrode active material prepared above was used.
[0099] Comparative Example 5: Production of Positive Electrode As the positive electrode active material, Li[Ni 0.83 Co 0.11 Mn 0.06 A single particle lithium transition metal oxide was prepared, which was represented by the chemical formula: 2 / g, and the average particle size (D 50 ) was 1.5 μm.
[0100] A positive electrode was manufactured in the same manner as in Example 1, except that the positive electrode active material prepared above was used, and the positive electrode active material, linear conductive material, binder, and thickener were mixed in a weight ratio of 95.0:3.0:1.5:0.5.
[0101] Comparative Example 6: Production of Positive Electrode As the positive electrode active material, Li[Ni 0.83 Co 0.11 Mn 0.06 A single particle lithium transition metal composite oxide represented by the chemical formula of 0.6 m2 was prepared. The BET specific surface area of the positive electrode active material was 0.6 m2. 2 / g, and the average particle size (D 50 ) was 12.0 μm. A positive electrode was produced in the same manner as in Example 1, except that the positive electrode active material prepared above was used.
[0102] Comparative Example 7: Production of Positive Electrode As the positive electrode active material, Li[Ni 0.83 Co 0.11 Mn 0.06 A single particle lithium transition metal composite oxide represented by the chemical formula of 0.6 m2 was prepared. The BET specific surface area of the positive electrode active material was 0.6 m2. 2 / g, and the average particle size (D 50 ) was 12.0 μm.
[0103] A positive electrode was manufactured in the same manner as in Example 1, except that the positive electrode active material prepared above was used, and the positive electrode active material, linear conductive material, binder, and thickener were mixed in a weight ratio of 96:1:2:1.
[0104] Comparative Example 8: Production of Positive Electrode As the positive electrode active material, Li[Ni 0.83 Co 0.11 Mn 0.06 A lithium composite transition metal oxide in the form of secondary particles in which two or more single particles are aggregated was prepared, and the secondary particle was represented by the chemical formula of 2 / g, and the average particle size (D 50 ) was 8.0 μm. A positive electrode was produced in the same manner as in Example 1, except that the positive electrode active material prepared above was used.
[0105] [Table 1]
[0106] [Experimental Example] <Manufacturing lithium secondary batteries> 1. Manufacturing of negative electrode Graphite as the negative electrode active material, carbon black as the conductive material, styrene-butadiene rubber (SBR) as the binder, and carboxymethyl cellulose (CMC) as the thickener were mixed in a weight ratio of 95.35:0.5:3:1.15 with water as the solvent to prepare a negative electrode slurry, which was then applied to a copper current collector, dried and rolled to prepare the negative electrode.
[0107] 2. Secondary battery manufacturing An electrode assembly was prepared by interposing a porous polyethylene separator between the positive electrode and the negative electrode prepared in Examples 1 to 5 and Comparative Examples 1 to 3, and the electrode assembly was placed inside a battery case, and an electrolyte was injected into the battery case to prepare half-cell lithium secondary batteries of Examples 1 to 5 and Comparative Examples 1 to 3. In this case, the electrolyte was prepared by dissolving lithium hexafluorophosphate (LiPF6) at a concentration of 1.0 M in an organic solvent in which ethylene carbonate (EC), propylene carbonate (PC), and propylene propionate (PP) were mixed in a volume ratio of 4:4:2.
[0108] Experimental example 1: Evaluation of life characteristics The secondary batteries produced in Examples 1 to 5 and Comparative Examples 1 to 8 were evaluated for cycle capacity retention using an electrochemical charger / discharger.
[0109] The cycle capacity retention rate was measured by charging and discharging at 0.1C in the first and second cycles, and at 1.0C from the third cycle onwards (charge conditions: CC / CV, 4.25V / 0.005C cutoff, discharge conditions: CC, 3.0V cutoff).
[0110] The capacity retention rate was calculated as follows. Capacity retention rate (%) = {(discharge capacity at Nth cycle) / (discharge capacity at first cycle)} x 100 (In the above formula, N is an integer of 1 or more). The capacity retention rates (%) at the 150th cycle for Examples 1 to 5 and Comparative Examples 1 to 8 are shown in Table 2 below.
[0111] Experimental example 2: Evaluation of rate characteristics The lithium secondary batteries of Examples 1 to 5 and Comparative Examples 1 to 8 were charged at 0.1 C in CC / CV mode at 25° C. up to 4.25 V and discharged to 3.0 V in 0.1 C CC mode to determine the discharge capacity at 0.1 C discharge.
[0112] Next, lithium secondary batteries of other Examples 1 to 5 and Comparative Examples 1 to 8 were prepared, and the lithium secondary batteries were charged at 0.1 C in CC / CV mode at 25° C. up to 4.25 V, and discharged to 3.0 V in 0.1 C CC mode, and the discharge capacity at 2.0 C discharge was determined.
[0113] Thereafter, the rate characteristics were calculated and evaluated using the following formula. In this case, excellent rate characteristics means that the decrease rate of normalized capacity (i.e., capacity retention rate) due to an increase in discharge rate (C-rate) is small. The results are shown in Table 2 below. Rate characteristic (%) = (discharge capacity at 2.0C discharge / discharge capacity at 0.1C discharge) x 100
[0114] Experimental Example 3: Evaluation of cell thickness increase rate The secondary batteries produced in Examples 1 to 5 and Comparative Examples 1 to 8 were subjected to 150 charge / discharge cycles using an electrochemical charger / discharger.
[0115] In the case of cycle charging and discharging, the first and second cycles were charged and discharged at 0.1C, and from the third cycle onwards, the charge and discharge were performed at 1.0C (charge conditions: CC / CV, 4.25V / 0.005C cutoff, discharge conditions: CC, 3.0V cutoff).
[0116] The cell thickness increase rate due to cycle charging and discharging was evaluated by the following formula. In the following formula, the thickness of the secondary battery was measured using an 800gf PPHG (flat plate thickness measuring device). The results are shown in Table 2 below.
[0117] Cell thickness increase rate (%) = {(thickness of secondary battery at 100% SOC at the 150th cycle) / (thickness of secondary battery at 100% SOC at the first cycle)} × 100
[0118] [Table 2]
[0119] Referring to Table 2, it can be seen that the lithium secondary batteries of Examples 1 to 5, which satisfy the mathematical formula 1 according to the present invention, exhibit significantly improved capacity retention and rate characteristics and a low cell thickness increase rate, compared to Comparative Examples 1 to 3, which do not satisfy the mathematical formula 1.
[0120] On the other hand, the average particle size (D 50 In Comparative Examples 4 to 7 in which a positive electrode active material having an excessively small or large value of ) was used, and in Comparative Example 8 in which a positive electrode active material that was not in a single particulate state was used, it was confirmed that even if Equation 1 was satisfied, the effects of improving the capacity retention rate, improving the rate characteristics, and reducing the cell thickness increase rate, which are the objectives of the present invention, could not be achieved.
Claims
1. A positive electrode current collector; a positive electrode active material layer disposed on at least one surface of the positive electrode current collector; Including, the positive electrode active material layer includes a positive electrode active material and a conductive material, The conductive material includes a linear conductive material, The positive electrode active material includes a lithium transition metal oxide including nickel (Ni), cobalt (Co), and manganese (Mn), The lithium composite transition metal oxide is in a single particle form, The average particle size (D 50 ) is 2 μm to 10 μm, A positive electrode that satisfies the following mathematical formula 1. [Mathematical formula 1] 1.2≦B / A≦4.7 In Equation 1, A is the weight percentage of the positive electrode active material relative to the BET specific surface area of the positive electrode active material × the weight of the positive electrode active material layer, and B is the weight percentage of the linear conductive material relative to the BET specific surface area of the linear conductive material × the weight of the positive electrode active material layer.
2. The positive electrode according to claim 1 , wherein the positive electrode active material is contained in the positive electrode active material layer in an amount of 90% by weight to 99% by weight.
3. The BET specific surface area of the positive electrode active material is 0.2 m 2 / g to 3m 2 / g.
4. The positive electrode according to claim 1 , wherein the linear conductive material is a carbon nanotube.
5. The positive electrode according to claim 1 , wherein the conductive material comprises the linear conductive material.
6. The BET specific surface area of the linear conductive material is 150 m 2 / g to 300m 2 / g.
7. 2. The positive electrode according to claim 1, wherein the pellet density of the linear conductive material is 0.09 g / cc to 0.16 g / cc.
8. The positive electrode according to claim 1 , wherein the linear conductive material is contained in the positive electrode active material layer in an amount of 0.50% by weight to 1.75% by weight.
9. 2. The positive electrode according to claim 1, wherein the BET specific surface area of the linear conductive material is 150 to 450 times larger than the BET specific surface area of the positive electrode active material.
10. 2. The positive electrode according to claim 1, wherein a weight percentage of the linear conductive material with respect to a total weight of the positive electrode active material layer is 0.006 to 0.018 times a weight percentage of the positive electrode active material with respect to a total weight of the positive electrode active material layer.
11. The positive electrode of claim 1 , wherein the positive electrode active material layer further comprises a binder.
12. The positive electrode according to claim 11 , wherein the binder is contained in the positive electrode active material layer in an amount remaining after excluding the positive electrode active material and the linear conductive material.
13. The positive electrode according to any one of claims 1 to 12, a negative electrode facing the positive electrode; a separator interposed between the positive electrode and the negative electrode; An electrolyte; A secondary battery comprising:
Citation Information
Patent Citations
Cathode electrode for lithium secondary battery
JP2018107007A
Positive electrode and secondary battery including the positive electrode
JP2021508158A
Positive electrode active material for secondary battery, method for producing the same, and lithium secondary battery including the same
JP2021514524A
Lithium Secondary Battery
KR1020190042992A