Method for producing coated cathode active material, and coated cathode active material

A core-shell structured cathode active material is produced through a method involving an aqueous buffer treatment and heat treatment to reduce gassing, improving energy density and cycle life in lithium-ion batteries.

JP2024536359AActive Publication Date: 2024-10-04BASF SE
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024520683
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-04
Filing Date
2022-09-28
Publication Date
2024-10-04
Estimated Expiration
2042-09-28

AI Technical Summary

Technical Problem

Lithium-ion batteries with high manganese cathode active materials suffer from gassing issues, leading to capacity loss and voltage drop due to oxygen generation, which affects their energy density retention and cycle life.

Method used

A method involving a core-shell structured cathode active material is produced by treating a particulate electrode active material with an aqueous buffer, followed by solid-liquid separation and heat treatment, resulting in a spinel-like surface layer with reduced nickel content to minimize gassing.

Benefits of technology

The method produces cathode active materials with high energy density retention and reduced gassing tendencies, enhancing the cycle life and performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536359000001
    Figure 2024536359000001
  • Figure 2024536359000002
    Figure 2024536359000002
  • Figure 2024536359000003
    Figure 2024536359000003
Patent Text Reader

Abstract

1. A method for making a cathode active material having a core-shell structure, the method comprising the steps of: (a) General formula Li 1+x TM 1-x O 2 providing a particulate electrode active material according to the method of claim 1, wherein T M is a combination of metals comprising Ni and Mn and optionally at least one element selected from Al, Mg, Ba, and transition metals other than Ni and Mn, x is in the range of 0.075 to 0.2, and at least 50 mol % of the metal in T M is Mn; (b) treating the particulate electrode active material with an aqueous buffer having a pH value in the range of 2.0 to 10.5; (c) removing the liquid phase by solid-liquid separation; (d) treating the residue from step (c) at a temperature in the range of 180 to 750°C; Includes.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a cathode active material having a core-shell structure, the method comprising the steps of: (a) General formula Li 1+x TM 1-x providing a particulate electrode active material from O2, where T M is a combination of metals comprising Ni and Mn, and optionally at least one element selected from Al, Mg, Ba, and transition metals other than Ni and Mn, where x is in the range of 0.075 to 0.2, and at least 50 mol % of the metals in T M is Mn; (b) treating the particulate electrode active material with an aqueous buffer having a pH value in the range of 2.0 to 10.5; (c) removing the liquid phase by solid-liquid separation; (d) treating the residue from step (c) at a temperature in the range of 180 to 750°C; Includes. [Background technology]

[0002] Lithium-ion secondary batteries are modern devices for storing energy. Many applications have been considered, from small devices such as mobile phones and laptop computers to car batteries and other e-mobility batteries. Various battery components such as electrolytes, electrode materials and separators have important roles in the performance of the battery. Cathode materials have received particular attention. Several materials have been proposed, such as lithium iron phosphate, lithium cobalt oxide, and lithium nickel cobalt manganese oxide. Extensive research has been conducted, but the solutions found so far still leave room for improvement.

[0003] Lithiated transition metal oxides are currently used as electrode active materials in lithium-ion batteries. Extensive research and development has been carried out over the past few years to improve properties such as charge density, specific energy, and other properties such as cycle life degradation and capacity loss that adversely affect the life or applicability of lithium-ion batteries. Further efforts are being made to improve the manufacturing methods.

[0004] Many of the electrode active materials currently under discussion are of the lithiated nickel-cobalt-manganese oxide ("NCM material") or lithiated nickel-cobalt-aluminum oxide ("NCA material") type.

[0005] In a typical process for the preparation of cathode materials for lithium-ion batteries, a so-called precursor is first formed by co-precipitation of a transition metal as a carbonate, oxide or preferably as an (oxy)hydroxide. This precursor is then mixed with a lithium compound, such as but not limited to LiOH, Li2O or Li2CO3, and calcined at high temperature. The lithium compound(s) can be used as hydrate(s) or in dehydrated form. The calcination or calcination, also commonly referred to as thermal or heat treatment of the precursor, is usually carried out at temperatures in the range of 600-1000°C. If hydroxides or carbonates are used as precursors, removal of water or carbon dioxide is first carried out, followed by the lithiation reaction. The heat treatment is carried out in a heated zone of an oven or kiln.

[0006] Many studies have been conducted on improving various properties of cathode active materials, such as energy density, charge / discharge performance such as capacity fade, etc. However, many cathode active materials have problems with limited cycle life and voltage fade, especially for many Mn-rich cathode active materials.

[0007] EP 3 486 980 discloses certain high manganese materials with high energy density retention. However, the disclosed cathode active materials suffer from such limited energy density. WO 2021 / 037678 discloses high manganese cathode active materials with high energy density.

[0008] However, it has been observed that high manganese cathode active materials suffer from gassing, which is the evolution of oxygen from the cathode active material, resulting in the formation of an oxygen-deficient near-surface layer on the electrode. The reaction of oxygen with the electrolyte produces gases such as CO, CO2, and H2. The gassing occurs during cycling and can cause cell swelling, capacity loss, and voltage loss. T. Teufl et al., J. Electrochem. Soc. 2018, 165, A2718-A2731, describe a method for producing cathode active materials with a shell layer of spinel-type compounds. However, the formation of the spinel usually results in oxygen release during the first charge cycle. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] EP 3 486 980 [Patent Document 2] WO 2021 / 037678 [Non-patent literature]

[0010] [Non-Patent Document 1] T. Teufl et al., J. Electrochem. Soc. 2018, 165, A2718-A2731 Summary of the Invention [Problem to be solved by the invention]

[0011] It was therefore an object of the present invention to provide electrochemical cells and batteries having high energy density retention but reduced tendency to gassing. It was further an object of the present invention to provide a method for producing a cathode active material that exhibits high energy density retention and reduced tendency to gassing. It was further an object of the present invention to provide a method for producing a cathode active material that has high energy density retention and reduced tendency to gassing. [Means for solving the problem]

[0012] Thus, a method as defined at the outset has been found, hereinafter also referred to as the "inventive method", which comprises at least three steps, namely steps (a), (b), (c) and (d), or simply (a), (b), (c) and (d), which are explained in more detail below. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Step (a) is a compound of the general formula Li 1+x TM 1-x The present invention relates to a method for producing an electrode active material comprising: providing an electrode active material with O2, wherein TM is a combination of metals comprising Ni and Mn, and optionally at least one element selected from Al, Mg, Ba, and transition metals other than Ni and Mn, x is in the range of 0.075-0.2, and at least 50 mol %, preferably 60-85 mol %, of the metals in TM is Mn. The cathode active material is also referred to as a basic cathode active material.

[0014] In one embodiment of the present invention, TM is a combination of elements of general formula (I): (Ni a Co b Mn c ) 1-d M d (I) (In the formula, a is in the range of 0.25 to 0.40, b is in the range of 0 to 0.15, more preferably b is zero; c is in the range of 0.60 to 0.70; d is in the range of 0 to 0.02; M is selected from Al, Ti, Zr, W, Mo, Mg, Nb, and combinations of at least two of the foregoing; a+b+c=1).

[0015] Some metal elements are ubiquitous, e.g., sodium, calcium or zinc, and trace amounts of these are present practically everywhere, but such trace amounts are not taken into account in the present specification, trace amounts in this context meaning amounts of 0.05 mol % or less relative to the total metal content TM.

[0016] M may be uniformly or non-uniformly distributed within the particles of the basic cathode active material provided in step (a). Preferably, M is distributed non-uniformly, and even more preferably as a gradient (higher concentration of M in the outer shell than in the center of the particle).

[0017] In one embodiment of the present invention, the basic cathode active material provided in step (a) has a pH of 0.7 to 4.0 μm. 2 / g or 6m 2 / g and has a specific surface area (BET) determined in accordance with DIN-ISO 9277:2003-05 in the range of 0.1 to 3.8 m 2 / g or 3.0 or less to 5.5m 2 / g is preferred.

[0018] In one embodiment of the present invention, the basic cathode active material provided in step (a) is composed of spherical particles, i.e., particles having a spherical shape, including not only particles that are precisely spherical, but also particles in which the difference between the maximum and minimum diameters of at least 90% (number average) of a representative sample is 10% or less.

[0019] In one embodiment of the present invention, the basic cathode active material provided in step (a) is composed of secondary particles that are aggregates of primary particles. Preferably, the electrode active material provided in step (a) is composed of spherical secondary particles that are aggregates of primary particles. Even more preferably, the electrode active material provided in step (a) is composed of spherical secondary particles that are aggregates of platelet-shaped primary particles.

[0020] In another embodiment of the present invention, the basic cathode active material provided in step (a) is a so-called monolithic material. Monolithic materials are also called single crystal materials and do not exhibit primary particles as described above. Monolithic materials preferably have a slightly irregular shape. Preferably, such monolithic materials have an average particle size in the range of 0.5 to 2.5 μm and a mean particle size of 0.5 to 2.5 μm. 2 / g range of specific surface area.

[0021] In one embodiment of the present invention, the electrode active material provided in step (a) has an average diameter in the range of 1 to 2000 nm, preferably 10 to 1000 nm, particularly preferably 50 to 500 nm. The average primary particle size can be determined, for example, by SEM or TEM. SEM is an abbreviation for scanning electron microscope, and TEM is an abbreviation for transmission electron microscope.

[0022] In one embodiment of the invention, the basic cathode active material provided in step (a) has a unimodal particle size distribution. In an alternative embodiment, the cathode active material of the invention has a bimodal particle size distribution, for example with a maximum in the range of 3 to 6 μm and another maximum in the range of 9 to 12 μm.

[0023] In one embodiment of the present invention, the pressed density of the electrode active material provided in step (a) is 2.75 to 3.1 g / cm, determined at a pressure of 250 MPa. 3 The range is 2.85 to 3.10 g / cm 3 is preferred.

[0024] The basic cathode active material provided in step (a) can be prepared according to various methods, including but not limited to those disclosed in WO 2021 / 037678.

[0025] In step (b), the basic cathode active material provided in step (a) is treated with an aqueous buffer having a pH value in the range of 2.0 to 10.5, preferably 4.0 to 9.5. The pH values ​​relate to a temperature of 25° C. and refer to the start of step (b). An increase in the pH value is observed during step (b).

[0026] An example of a suitable buffer is B(OH)4 with a pH value of 9.2. - / B(OH)3, H2PO4 with a pH value of 7.2 - / HPO4 2- , acetate / acetic acid with a pH value of 4.8, and H3PO4 / H2PO4 with a pH value of 2.2. - The pH values ​​correspond to a 1:1 molar aqueous solution at 25°C. B(OH)4 - / B(OH)3, PO4 - / HPO4 2- , and acetate / acetic acid are preferred, H2PO4 - / HPO4 2- and acetate / acetic acid are more preferred, H2PO4 - / HPO4 2- is even more preferred. The counter ion may be an alkali metal, such as lithium, sodium, and potassium. PO4 - / HPO4 2- In this case, potassium is preferred.

[0027] In one embodiment of the invention, step (b) is carried out at a temperature in the range of 25 to 100° C., preferably 50 to 90° C., more preferably 70 to 90° C. Higher temperatures, for example up to 120° C., can likewise be carried out under elevated pressure, for example 1.5 to 2 bar.

[0028] In one embodiment of the invention, the buffer has a concentration in the range of 0.1-1M.

[0029] In one embodiment of step (b), the volume ratio of the basic cathode active material provided in step (a) to the buffer solution ranges from 2:1 to 1:20, preferably from 1:1 to 1:5.

[0030] In one embodiment of the present invention, step (b) has a duration in the range of from 10 minutes to 10 hours, preferably from 20 minutes to 8 hours, more preferably from 30 minutes to 4 hours.

[0031] Preferably, step (b) may be supported by a mixing operation, such as stirring or tumbling. On a laboratory scale, shaking can also be used.

[0032] From step (b) a suspension is obtained having a solid phase and a liquid phase.

[0033] Step (c) comprises separating the liquid phase from the suspension obtained after step (b) by a solid-liquid separation method, for example by decantation in a centrifuge or by filtration.

[0034] In one embodiment of the invention, after or during step (b) the liquid phase is removed by any type of filtration, for example on a band filter or in a filter press.

[0035] In a preferred embodiment of the present invention, steps (b) and (c) are carried out in a filter press or a stirred filter apparatus, such as a stirred pressure filter or a stirred suction filter. Removal of the aqueous medium is started by starting the filtration at most 3 minutes after combining the starting material and the aqueous medium according to step (b), or immediately thereafter. On a laboratory scale, steps (b) and (c) may be carried out in a centrifuge or a Büchner funnel, and steps (b) and (c) may be supported by manual stirring.

[0036] In a preferred embodiment, steps (b) and (c) are carried out in a filter apparatus, such as an agitated filter apparatus, which allows for agitation of the slurry or filter cake within the filter apparatus.

[0037] In one embodiment of the present invention, step (c) is carried out at a temperature in the range of 10 to 65° C. Room temperature is preferred.

[0038] In one embodiment of the invention, step (c) is a filtration supported by pressure, for example a positive pressure in the range of 1 to 500 mbar, hi another embodiment, step (c) is a filtration performed by suction.

[0039] In one embodiment of the invention, the removal of the liquid phase according to step (c) has a duration ranging from 1 minute to 1 hour.

[0040] By carrying out step (c), a solid residue and a liquid phase are obtained.

[0041] In one embodiment of the invention, the liquid phase obtained from step (c) is at least partially recycled. Said recycling can be carried out by adding freshly prepared buffer to all or part of the liquid phase obtained from step (c), for example in a mass ratio of 10:1 to 1:10, and then using it in a new batch step (b). It is likewise possible to add the liquid phase obtained from step (c) to freshly prepared buffer, for example in a mass ratio of 10:1 to 1:10, and then use it in a new batch step (b).

[0042] In step (d), the residue from step (c) is treated at a temperature in the range of 140-750°C, preferably 180-300°C.

[0043] Step (d) can be carried out under air, oxygen, oxygen-enriched air, nitrogen, nitrogen-enriched air, or a noble gas such as argon. Nitrogen and air are preferred. In another embodiment, step (d) is carried out in a vacuum.

[0044] In one embodiment of the present invention, step (d) has a duration ranging from 15 minutes to 24 hours, preferably from 1 to 15 hours. From step (d) a cathode active material is obtained.

[0045] In one embodiment of the present invention, step (d) is carried out under an atmosphere having a reduced CO2 content, for example, a carbon dioxide content in the range of 0.01 to 500 ppm by mass, preferably 0.1 to 50 ppm by mass. The CO2 content can be determined, for example, by optical methods using infrared light. It is even more preferred to carry out step (d) under an atmosphere having a carbon dioxide content below the detection limit of, for example, an optical method based on infrared light.

[0046] Step (d) may be carried out in a fluidized bed, furnace or oven, such as a rotary kiln, roller hearth kiln or pusher kiln.

[0047] By practicing the method of the present invention, a cathode active material is obtained that has high energy density retention and reduced tendency to gass. The cathode active material resulting from the method of the present invention has a high energy density retention and reduced tendency to gass. 1+x TM 1-x It has a lower relative lithium content than O2. When produced according to the method of the present invention, it can be shown that lithium leaches from the electrode active material provided in step (a).

[0048] In one embodiment of the invention, between steps (c) and (d) there is an additional step: (e) washing the residue from step (c) with water 1 to 4 times. will be carried out.

[0049] More than five washing steps are disadvantageous in terms of time consumption and wastewater generation.

[0050] Step (e) is preferably carried out at water temperatures in the range of 5 to 50°C, more preferably 10 to 30°C.

[0051] In one embodiment of the present invention, the mass ratio of the electrode active material to be treated to the washing water per washing step is in the range of 2:1 to 1:20, preferably 1:1 to 1:15.

[0052] Another (optional) step involves drying the solid residue obtained from step (c) or (e), respectively, under reduced pressure or vacuum at a temperature below 140° C. to remove most of the water.

[0053] The water used in step (e) is preferably deionized, for example by ion exchange or distillation, and more preferably is decarbonated.

[0054] By carrying out step (e), it is possible to remove water-soluble salts that originate from the buffer solution and that may dissolve in the electrolyte when the cell is assembled.

[0055] By carrying out the method of the present invention, a cathode active material having excellent properties can be obtained. The cathode active material has the general formula Li 1+x1 TM 1-x1 O2, where TM is a combination of metals comprising Ni and Mn and optionally at least one element selected from Al, Mg, Ba, and transition metals other than Ni and Mn, x1 is in the range of 0.05-0.15, and at least 50 mol % of the metals in TM is Mn, wherein the surface is at least partially covered with a layer of spinel-like material, which layer may comprise a phosphate or borate, and the nickel content in the spinel-like material is lower than that of TM. The cathode active material of the present invention can be described as a core-shell material, or a partially coated material having a core and a coating.

[0056] When present, the content of phosphate or borate is in the range of 0.05 to 2 wt %, based on the total weight of the cathode active material of the present invention.

[0057] The cathode active material of the present invention is Li 1+x TM 1-x It has a lower relative lithium content than O2. The method of the present invention can be shown to leach lithium from the electrode active material provided in step (a). However, preferably, TM does not leach.

[0058] The surface of the cathode active material produced by the method of the present invention is at least partially covered with a layer of spinel-like material, which may comprise a phosphate or borate, and the content of nickel in the spinel-like material is lower than that of TM. The material obtained by the method of the present invention can therefore also be considered as a core-shell material, the shell of which comprises a spinel-like material with reduced nickel content and the core of which has the composition Li 1+x TM 1-x O2, but advantageously, dissolution of the TM is avoided.

[0059] In one embodiment of the invention, the surface of the cathode active material of the invention is covered to an extent of 60-100% with said spinel-like material.Preferably, 85-100% of the particles of a sample of the cathode active material of the invention are covered by such a shell.

[0060] In one embodiment of the invention, the average thickness of the shell is very thin, for example 0.1-5 nm, preferably 1-3 nm. In other embodiments, the thickness may be in the range of 6-15 nm. In further embodiments, the thickness of such a shell is in the range of 16-50 nm. A typical range may be 1.5-10 nm.

[0061] The term "spinel-like" includes true spinel structures and structures that deviate from spinel depending on the ratio of lithium to non-lithium metals.

[0062] In one embodiment of the present invention, the cathode active material according to the present invention has a molecular weight of 1.5 to 8 m 2 / g, which can be determined by nitrogen adsorption after outgassing the sample at 200 ° C for 30 min and beyond, according to DIN ISO 9277:2010.

[0063] In one embodiment of the invention, the spinel-like material corresponds to the formula LiTM'2O4, where TM' comprises the metal combination of Ni and Mn and optionally at least one element selected from Al, Mg, Ba, and transition metals other than Ni and Mn, x is in the range of 0.075-0.2, and the content of nickel in TM' is 2-6 mol % lower than in the respective TM from the core, relative to the sum of the metals other than lithium.

[0064] Further disclosed herein are electrodes comprising at least one electrode active material produced according to the present invention. These are particularly useful for lithium ion batteries. Lithium ion batteries comprising at least one electrode produced according to the present invention exhibit good discharge behavior. Electrodes comprising at least one electrode active material produced according to the present invention: (A) at least one electrode active material made according to the present invention; (B) Carbon in a conductive state; (C) a binder material, also called binder or binding agent (C), and preferably (D) Current collector Contains:

[0065] In a preferred embodiment, such a cathode comprises, based on the sum of (A), (B) and (C): (A) 80 to 98% by mass of an electrode active material produced according to the present invention; (B) 1 to 17 mass% carbon, (C) 1 to 15 mass % of a binder material Contains:

[0066] The electrodes according to the present invention may include further components. They may include a current collector, such as, but not limited to, aluminum foil. They may further include conductive carbon and a binder.

[0067] The electrode according to the invention contains a conductively modified carbon, also called carbon (B) for short, which can be selected from soot, activated carbon, carbon nanotubes, graphene, graphite, and a combination of at least two of the foregoing.

[0068] Suitable binders (C) are preferably selected from organic (co)polymers. Suitable (co)polymers, i.e. homopolymers or copolymers, can be selected, for example, from (co)polymers obtainable by anionic, catalytic or free radical (co)polymerization, in particular from polyethylene, polyacrylonitrile, polybutadiene, polystyrene and copolymers of at least two comonomers selected from ethylene, propylene, styrene, (meth)acrylonitrile and 1,3-butadiene. Polypropylene is also suitable. Polyisoprene and polyacrylates are furthermore suitable. Polyacrylonitrile is particularly preferred.

[0069] In a particularly preferred embodiment of the present invention, the binder (C) is selected from halogenated (co)polymers, in particular fluorinated (co)polymers.Halogenated or fluorinated (co)polymers are understood to mean (co)polymers that contain at least one (co)polymerized (co)monomer with at least one halogen atom or at least one fluorine atom per molecule, more preferably at least two halogen atoms or at least two fluorine atoms per molecule.Examples include polyvinyl chloride, polyvinylidene chloride, polytetrafluoroethylene, polyvinylidene fluoride (PVdF), tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), vinylidene fluoride-tetrafluoroethylene copolymer, perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, and ethylene-chlorofluoroethylene copolymer.

[0070] Suitable binders (C) are especially polyvinyl alcohol and halogenated (co)polymers such as polyvinyl chloride or polyvinylidene chloride, especially fluorinated (co)polymers such as polyvinyl fluoride and especially polyvinylidene fluoride and polytetrafluoroethylene.

[0071] The cathode of the present invention may contain 1 to 15% by weight of binder(s) relative to the electrode active material. In other embodiments, the cathode of the present invention may contain 0.1 to less than 1% by weight of binder(s).

[0072] A further aspect of the invention is a battery containing at least one cathode comprising an electrode active material made according to the invention, carbon and a binder, at least one anode, and at least one electrolyte.

[0073] Such cathode embodiments have already been described in detail above.

[0074] The anode may contain at least one anode active material, such as lithium, carbon (graphite), TiO2, lithium titanium oxide, silicon, or tin. The anode may further contain a current collector, such as a metal foil, such as copper foil.

[0075] The electrolyte may include at least one non-aqueous solvent, at least one electrolyte salt, and optionally, additives.

[0076] The non-aqueous solvent for the electrolyte can be liquid or solid at room temperature and is preferably selected from polymers, cyclic or acyclic ethers, cyclic and acyclic acetals, and cyclic or acyclic organic carbonates.

[0077] Examples of suitable polymers are in particular polyalkylene glycols, preferably poly-C1-C4-alkylene glycols and in particular polyethylene glycols, where the polyethylene glycols may contain up to 20 mol % of one or more C1-C4-alkylene glycols.The polyalkylene glycols are preferably polyalkylene glycols with two methyl or ethyl end caps.

[0078] The molecular weight M of suitable polyalkylene glycols, particularly suitable polyethylene glycols, W may be at least 400 g / mol.

[0079] The molecular weight M of suitable polyalkylene glycols, particularly suitable polyethylene glycols, W can be up to 5,000,000 g / mol, preferably up to 2,000,000 g / mol.

[0080] Examples of suitable acyclic ethers are, for example, diisopropyl ether, di-n-butyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, with 1,2-dimethoxyethane being preferred.

[0081] Examples of suitable cyclic ethers are tetrahydrofuran and 1,4-dioxane.

[0082] Examples of suitable acyclic acetals are, for example, dimethoxymethane, diethoxymethane, 1,1-dimethoxyethane and 1,1-diethoxyethane.

[0083] An example of a suitable cyclic acetal is 1,3-dioxane, and especially 1,3-dioxolane.

[0084] Examples of suitable acyclic organic carbonates are dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate.

[0085] Examples of suitable cyclic organic carbonates are compounds according to the general formulae (II) and (III): [ka] (In the formula, R 1 , R 2 and R 3 can be the same or different and are selected from hydrogen and C1-C4-alkyl, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl, preferably R 2 and R 3 (Both cannot be tert-butyl).

[0086] In a particularly preferred embodiment, R 1 is methyl, R 2 and R 3 are each hydrogen or R 1 , R 2 and R 3 are respectively In another embodiment, R 1 is fluorine, R 2 and R 3 are hydrogen.

[0087] Another preferred cyclic organic carbonate is vinylene carbonate of formula (IV).

[0088] [ka]

[0089] Preferably, the solvent or solvents are used in an aqueous state, ie with a water content in the range of 1 ppm to 0.1% by weight, which can be determined, for example, by Karl Fischer titration.

[0090] The electrolyte further comprises at least one electrolyte salt. Suitable electrolyte salts are in particular lithium salts. Examples of suitable lithium salts are LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC(C n F 2n+1SO2)3, lithium imide, e.g. LiN(C n F 2n+1 SO2)2 (wherein n is an integer ranging from 1 to 20), LiN(SO2F)2, Li2SiF6, LiSbF6, LiAlCl4, and compounds of the general formula (C n F 2n+1 SO2) t Salt of YLi where t=1 when Y is selected from oxygen and sulfur; when Y is selected from nitrogen and phosphorus, t=2; When Y is selected from carbon and silicon, t=3).

[0091] Preferred electrolyte salts are selected from LiC(CF3SO2)3, LiN(CF3SO2)2, LiPF6, LiBF4, LiClO4, with LiPF6 and LiN(CF3SO2)2 being particularly preferred.

[0092] The battery according to the invention comprises one or more separators by which the electrodes are mechanically separated. Suitable separators are polymer films, especially porous polymer films, which are unreactive towards metallic lithium. Particularly suitable materials for the separators are polyolefins, especially film-forming porous polyethylene and film-forming porous polypropylene.

[0093] A separator made of polyolefin, particularly polyethylene or polypropylene, may have a porosity in the range of 35 to 45%. A suitable pore size is, for example, in the range of 30 to 500 nm.

[0094] In another embodiment of the present invention, the separator can be selected from PET nonwoven fabrics filled with inorganic particles. Such separators can have a porosity in the range of 40-55%. Suitable pore sizes are, for example, in the range of 80-750 nm.

[0095] The battery according to the invention further comprises a housing which may have any shape, for example a cube, or the shape of a cylindrical disk or can. In one variant, a metal foil configured as a pouch is used as the housing.

[0096] The battery according to the invention exhibits good discharge behaviour, for example very good discharge and cycling behaviour at low temperatures (below 0° C., for example −10° C. or less).

[0097] The battery according to the present invention may comprise two or more electrochemical cells that are combined with each other, for example, connected in series or connected in parallel. A series connection is preferred. In the battery according to the present invention, at least one electrochemical cell contains at least one cathode according to the present invention. Preferably, in the electrochemical cell according to the present invention, the majority of the electrochemical cells contain the cathode according to the present invention. Even more preferably, in the battery according to the present invention, all the electrochemical cells contain the cathode according to the present invention.

[0098] The battery according to the invention is used in a device, in particular a mobile device. Examples of mobile devices are vehicles, such as automobiles, bicycles, aircraft, or water vehicles, such as boats or ships. Other examples of mobile devices are manually operated, such as computers, in particular laptops, phones, or powered hand tools, for example in the construction sector, in particular drills, battery-powered drivers, or battery-powered staplers. EXAMPLES

[0099] The present invention is further illustrated by the following examples.

[0100] The average particle size (D50) was determined by dynamic light scattering ("DLS"). Percentages are by weight unless otherwise stated.

[0101] I. Preparation of the Cathode Active Material of the Present Invention I.1 Preparation of Basic Cathode Active Material, Step (a.1) The stirred tank reactor was charged with deionized water and heated to 55°C. The pH was then adjusted to 8.05 by adding aqueous sodium hydroxide. The coprecipitation reaction was started by simultaneously feeding aqueous transition metal sulfate and aqueous sodium carbonate solutions at a flow ratio of 1.3 and a mean residence time of 13.5 hours at total flow rate. The aqueous transition metal solution contained Ni and Mn in a molar ratio of 1:2 and a total transition metal concentration of 1.65 mol / kg. The aqueous sodium carbonate solution was a 27% by weight aqueous sodium carbonate solution. The pH value was maintained at 8.05 by separately feeding aqueous sodium carbonate. Starting from the start of all feeds, the mother liquor was continuously removed. The resulting suspension was filtered, washed with distilled water, dried at 120°C in air and sieved to obtain the mixed transition metal (TM) carbonate precursor.

[0102] This precursor was mixed with Li2CO3 in a molar ratio of Li / (TM) of 1.30. The mixture was heated to 930 °C and kept in a mixed gas flow of 20% oxygen and 80% nitrogen (volume ratio) for 5 h. After cooling to room temperature, the resulting powder was deagglomerated and sieved through a 32 μm mesh to obtain the basic electrode active material B-CAM.1.

[0103] I.2 Treatment with aqueous buffers I.2.1 Treatment with buffer K2HPO4 / KH2PO4 Step (b.1): 5 g of B-CAM.1 was placed in a flask. A preset amount of buffer solution with a concentration and temperature according to Table 1 was added. The resulting slurry was stirred for 4 hours. The change in pH value from the beginning to the end of step (b.1) was less than 1.5 units.

[0104] Step (c.1): The liquid phase was then removed using a centrifuge to obtain a solid residue.

[0105] Step (e.1): The residue from step (d.1) was washed three times with 25 ml of deionized water each time. The water was removed by centrifugation.

[0106] Step (d.1): The residue from step (e.1) was heated at 300° C. in vacuum for 12 hours to obtain a cathode active material treated according to the present invention.

[0107] The conditions for the separate experiments are summarized in Table 1.

[0108] [Table 1]

[0109] In a comparative example, the K2HPO4 / KH2PO4 buffer solution was replaced with distilled water (25 ml) and washing was carried out for 24 hours at 70° C. Steps (c) and (d) were carried out in the same manner as above.

[0110] I.2.2 Treatment with sodium acetate / acetic acid buffer Step (b.1) was repeated, but using a sodium acetate / acetic acid buffer instead. A similar procedure was followed to obtain the treated cathode active material.

[0111] II. Electrode Fabrication (B.1): Conductive carbon (Super C65, Imerys, Switzerland) (C.1): Polyvinylidene fluoride binder (PVDF, Solef 5130, Solvay, Belgium) Cathodes were prepared by dispersing 92.5%, 4.0%, and 3.5% by weight of each CAM or B-CAM.1 or comparative cathode active material in NMP. Each cathode active material was weighed in an argon-filled glove box (O2 and H2O less than 0.1 ppm, MBraun, Germany). (B.1) and (C.1) were mixed in a planetary mixer (ARV-310, Thinky, USA) at 1000 rpm for 1 x 5 min. NMP was then added in three portions under air and the slurry was mixed again at 2000 rpm for 3 x 5 min. Cathode active material was added to the resulting slurry and mixed for 1 x 5 min. The resulting electrode ink was coated onto aluminum foil (18 μm thick, MTI Corporation, USA) using a four-blade blade (RK PrintCoat Instruments, UK). The coating was subsequently dried in a convection oven (T = 55 °C) for at least 3 h to remove the NMP. Electrodes with a diameter of 14 mm were punched out, pressed with a KBr-Press at 2.5 tonnes each, and dried at 120 °C under dynamic vacuum in a glass oven (Drying Oven 585, Büchi, Switzerland) for 12 h, from where they were transferred to a glove box (O2 and H2O < 0.1 ppm, MBraun, Germany). The cathode loading was 8.5 mg. CAM / cm 2 and 2.1mAh / cm 2 Corresponds to.

[0112] The graphite anode was prepared by mixing graphite (T750, SGL carbon, Germany) and (C.1) in a mass ratio of 95:5. To prepare the ink, graphite and (C.1) were dispersed in NMP and mixed in a planetary mixer (ARV-310, Thinky, USA; 2000 rpm for 15 min). The resulting ink was coated on a copper foil (12 μm thick, MTI Corporation, USA). The coating was dried in a convection oven (T=55 °C) for at least 3 h to evaporate the NMP. Electrodes with a diameter of 15 mm were punched out, pressed with a KBr-Press at 0.5 ton and dried overnight at 120 °C under dynamic vacuum in a glass oven (Drying Oven 585, Büchi, Switzerland) without exposure to the atmosphere, from where the samples were transferred to a glove box (O2 and H2O < 0.1 ppm, MBraun, Germany). To minimize the risk of lithium plating, 6.7 mg of 1000 μl ... グラファイト / cm 2 The anode electrode with a loading of 1.0 μg / g had a larger surface capacity than the cathode electrode (nominal specific capacity 355 mAh / g グラファイト Based on 2.4mAh / cm 2 ).

[0113] III. Electrochemical Testing Full-cell coin cells (2032 type) were assembled in a glove box using a 17 mm diameter Celgard C2500 separator, a 14 mm diameter cathode, and a 15 mm diameter anode, by adding 80 μL of electrolyte (1 M LiPF6 in 2:8 g:g FEC:DEC; note that no additives were used here). After assembly, all cells were given a 2-hour rest period before charge / discharge cycling, with C-rates based on the nominal LMR-NCM capacity of 250 mAh / g. The full cells with LRM-NCM cathodes were activated in a constant current procedure (CC) at a C-rate of C / 15 to a full cell voltage of 4.7 V in the first cycle, and then discharged (CC) at C / 15 to 2.0 V; the upper cut-off cell voltage was lowered to a full cell voltage of 4.6 V in the subsequent cycles. Then, 3 cycles of 0.1 C CC charge and 0.1 C CC discharge were applied.

[0114] Following these initial formation cycles, the cells were rate tested by charging / discharging for two cycles at 0.3C(CCCV) / 0.5C(CC), 0.7C(CCCV) / 1C(CC), 0.7C(CCCV) / 2C(CC), 0.7C(CCCV) / 3C(CC), and 0.7C(CCCV) / 1C(CC), respectively, where all CV steps were terminated after 1 hour or when the current dropped below 0.01C. After the rate test, a cycle life test was conducted, starting with 3 cycles of 0.1C CC charge and 0.1C CC discharge, followed by 30 cycles of 0.7C (CCCV) charge rate and 1C (CC) discharge rate, where the CV steps are as defined above. This sequence of 3 slow discharges and 30 fast discharges was repeated several times.

[0115] [Table 2]

Claims

1. 1. A method for making a cathode active material having a core-shell structure, comprising the steps of: (a) General formula Li 1+x T.M. 1-x O 2 wherein TM is a combination of metals comprising Ni and Mn, and optionally at least one element selected from Al, Mg, Ba, and transition metals other than Ni and Mn, x is in the range of 0.075 to 0.2, and at least 50 mol % of the metals in TM is Mn; (b) treating the particulate electrode active material with an aqueous buffer having a pH value in the range of 2.0 to 10.5; (c) removing the liquid phase by solid-liquid separation; (d) treating the residue from step (c) at a temperature in the range of 140 to 750° C.; A method comprising:

2. TM is a compound represented by the general formula (I): (Ni a Co b Mr c ) 1-d M d (I) (wherein a is in the range of 0.25 to 0.4; b is 0 or in the range of 0.01 to 0.2; c is in the range of 0.6 to 0.75; d is in the range of 0 to 0.1; M is at least one of Al, Mg, Ti, Mo, W, and Zr; a + b + c = 1) The method of claim 1, wherein the metal combination is

3. 3. The process according to claim 1 or 2, wherein the solid-liquid separation step in step (c) is a filtration.

4. The method according to claim 1 or 2, wherein the buffer in step (b) has a pH value in the range of 4.0 to 9.

5.

5. Step (d) is followed by step (e): (e) washing the heat treated material from step (d) with water 1 to 4 times. The method of claim 1 or 2, comprising:

6. The process according to claim 1 or 2, wherein step (b) is carried out at a temperature in the range of from 25 to 90°C.

7. 3. The process according to claim 1 or 2, wherein the liquid phase obtained from step (c) is at least partially recycled.

Citation Information

Patent Citations

  • Core-shell structure positive electrode material and preparation method thereof

    CN112968153A

  • Production of positive electrode active material nickel acid lithium for nun-aqueous secondary battery and non- aqueous secondary battery

    JP2000128546A

  • Positive electrode active material for lithium secondary batteries, method for manufacturing the same, positive electrode of a lithium secondary battery containing the same, and lithium secondary battery

    JP2011519142A

  • Positive electrode active material for nonaqueous electrolyte secondary batteries, manufacturing method thereof, and nonaqueous electrolyte secondary battery

    JP2015144105A

  • Positive electrode active material for lithium secondary battery, method of producing the same, and lithium secondary battery

    JP2018092793A