Decorative film and shatterproof film for vehicle interiors

A decorative film with a biaxially oriented polyethylene terephthalate layer and colored adhesive layer using specific acrylic polymers addresses durability and nonflammability issues, ensuring mechanical strength and resistance to heat-induced shrinkage.

JP2024536467AInactive Publication Date: 2024-10-043M INNOVATIVE PROPERTIES CO
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
JP2024521827
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-15
Filing Date
2022-10-10
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Decorative films used in vehicle interiors and building windows face issues with durability, mechanical strength, and nonflammability when exposed to sunlight and high temperatures, leading to adhesive deterioration and shrinkage.

Method used

A decorative film comprising a biaxially oriented polyethylene terephthalate film layer combined with a colored adhesive layer containing carboxy group-containing and amino group-containing (meth)acrylic polymers, which enhances durability, mechanical properties, and nonflammability.

Benefits of technology

The film exhibits improved tensile strength, elongation, and resistance to heat shrinkage, maintaining adhesive strength and preventing glass scattering, while being nonflammable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536467000001_ABST
    Figure 2024536467000001_ABST
Patent Text Reader

Abstract

A decorative film for vehicle interiors according to one embodiment comprises a biaxially oriented polyethylene terephthalate film layer and a colored adhesive layer, the colored adhesive layer comprising a carboxyl group-containing (meth)acrylic polymer, an amino group-containing (meth)acrylic polymer, and a colorant, the pencil hardness of the biaxially oriented polyethylene terephthalate film layer side of the decorative film is B or higher, the tensile strength at 2% elongation of the decorative film is 50 N / 25 mm or higher, the elongation is 60% or higher, and the total heat generation amount for 20 minutes after the start of heating measured in accordance with the ISO5660-1 cone calorimeter heat generation test is 8 MJ / m 2 The following is the result.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to decorative films and shatterproof films for vehicle interiors. [Background technology]

[0002] Decorative films or sheets having an adhesive layer on a film substrate are widely used in the interior decoration of vehicles such as automobiles, trains, and buses, and buildings. In addition, shatterproof films are widely used in window glass of buildings, vehicles, etc., to prevent glass from shattering when broken. Some shatterproof films also have a decorative function.

[0003] Patent Document 1 (JP 2003-138235 A) describes "a pressure-sensitive adhesive composition having a concealing property, comprising (a) 100 parts by weight of a resin component of a copolymer mainly composed of a (meth)acrylic acid alkyl ester monomer having an alkyl group with 1 to 12 carbon atoms, (b) 0.1 to 5 parts by weight of surface-treated aluminum powder having an average particle size of 5 to 50 μm and an aspect ratio of 50 to 200, and (c) 5 to 60 parts by weight of titanium oxide" and "a pressure-sensitive adhesive sheet obtained by applying the pressure-sensitive adhesive composition having a concealing property onto a substrate sheet and drying the composition".

[0004] Patent Document 2 (JP Patent Publication No. 2003-183602) describes a decorative adhesive sheet characterized in that "an adhesive containing 3 to 50 parts by weight of white pigment per 100 parts by weight of the adhesive base polymer, and aluminum metal pieces amounting to 0.3 to 2% by weight of the white pigment added, is laminated on one side of a colored film having a total light transmittance of 3 to 80%."

[0005] Patent Document 3 (JP 2006-88593 A) describes "a decorative metallic adhesive sheet comprising, in this order, an acrylic resin layer (A) which contains an ultraviolet absorber and has a total light transmittance for visible light of 85% or more, a metallic adhesive layer (B) in which an acrylic adhesive contains aluminum metal powder and a pearl pigment, a colored soft polyvinyl chloride resin layer (C), and an acrylic adhesive layer (D) laminated together."

[0006] Patent Document 4 (JP 2008-308646 A) describes "an acrylic colored adhesive containing a carboxyl group-containing (meth)acrylic polymer, a pigment or dye, and an amino group-containing (meth)acrylic polymer not containing an aromatic vinyl monomer" and "a marking film having a base film layer and an adhesive layer made of the acrylic colored adhesive." Summary of the Invention

[0007] When decorative or shatterproof films are applied (applied inside) to the interior side of glass substrates such as window glass in buildings, the film substrates (e.g., polyvinyl chloride films) that are components of these films may deteriorate or shrink due to exposure to sunlight (especially ultraviolet light) and the continuous high temperature environment created by the heat that accumulates in the relatively thick glass substrates.

[0008] Decorative films used in the interiors of trains, buses and other vehicles are required to have durability against external physical forces or influences, such as resistance to breakage, scratching, graffiti, and punctures.

[0009] The performance required for shatterproof films includes tensile strength and elongation. For example, according to JIS A 5759:2016 "Architectural Window Films" 6.8 "Tensile Strength and Elongation Test", solar radiation control films and low emissivity films are required to have a tensile strength of 50N / 25mm or more and an elongation of 60% or more, while impact-resistant glass shatterproof films and interlayer displacement-resistant glass shatterproof films are required to have a tensile strength of 100N / 25mm or more and an elongation of 60% or more.

[0010] Additionally, decorative and shatterproof films desirably have a certain level of flame retardancy when used on vehicles or buildings.

[0011] The present disclosure provides a functional adhesive film that is durable, has excellent mechanical properties, and is non-flammable, for use in shatterproofing glass substrates such as vehicle interiors and building window glass.

[0012] The present inventors have found that the above problems can be solved by combining a biaxially stretched polyethylene terephthalate film as a film substrate with a colored adhesive layer containing a specific combination of (meth)acrylic polymers and a colorant.

[0013] According to one embodiment, a decorative film for vehicle interiors comprising a biaxially oriented polyethylene terephthalate film layer and a colored adhesive layer, the colored adhesive layer comprising a carboxyl group-containing (meth)acrylic polymer, an amino group-containing (meth)acrylic polymer, and a colorant, the pencil hardness of the biaxially oriented polyethylene terephthalate film layer side of the decorative film is B or higher, the tensile strength at 2% elongation of the decorative film is 50 N / 25 mm or higher, the elongation is 60% or higher, and the total heat generation amount for 20 minutes after the start of heating measured in accordance with the ISO5660-1 cone calorimeter heat generation test is 8 MJ / m 2 The following decorative film for vehicle interiors is provided:

[0014] According to another embodiment, there is provided a shatterproof film comprising a biaxially oriented polyethylene terephthalate film layer and a colored adhesive layer, the colored adhesive layer comprising a carboxyl group-containing (meth)acrylic polymer, an amino group-containing (meth)acrylic polymer, and a colorant, the pencil hardness of the biaxially oriented polyethylene terephthalate film layer side of the shatterproof film is B or higher, the tensile strength at 2% elongation of the shatterproof film is 50 N / 25 mm or higher, the elongation is 60% or higher, and the total heat generation amount for 20 minutes after the start of heating measured in accordance with the ISO5660-1 cone calorimeter heat generation test is 8 MJ / m 2 A shatterproof film is provided, which is as follows:

[0015] According to the present disclosure, there is provided a non-flammable functional adhesive film having excellent durability and mechanical properties, which is used for preventing glass substrates such as vehicle interiors and building window glass from shattering.

[0016] It should be noted that the above description should not be construed as a disclosure of all embodiments of the present invention and all advantages related to the present invention. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view of a decorative film (vehicle interior decorative film and shatterproof film) according to one embodiment. [Diagram 2] 1 is a graph showing the relationship between elongation (%, horizontal axis) and tensile strength (N / 25 mm, vertical axis) of the decorative films of Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, the present invention will be described in more detail with reference to the drawings for the purpose of illustrating typical embodiments of the present invention, but the present invention is not limited to these embodiments.

[0019] In this disclosure, "(meth)acrylic" means acrylic or methacrylic, and "(meth)acrylate" means acrylate or methacrylate.

[0020] In this disclosure, the term "film" also encompasses an article called a "sheet."

[0021] In this disclosure, "pressure sensitive adhesion" refers to the property of a material or composition to adhere to a variety of surfaces with only slight pressure applied for a short period of time within the temperature range of use, e.g., from 0° C. to 50° C., and not to exceed this temperature, and not to exhibit a phase change (liquid to solid). In this disclosure, "tack" is used interchangeably with "pressure sensitive adhesion."

[0022] In the present disclosure, "disposed on" includes not only the case of being directly disposed on, but also the case of being indirectly disposed on, that is, disposed on via another material or layer.

[0023] The decorative film and shatterproof film for vehicle interiors of one embodiment include a biaxially oriented polyethylene terephthalate film layer (hereinafter, in this disclosure, also referred to as a "biaxially oriented PET film layer") and a colored adhesive layer. Hereinafter, in this disclosure, the decorative film and the shatterproof film for vehicle interiors are collectively referred to simply as "decorative film".

[0024] The biaxially oriented PET film layer and the colored adhesive layer may be in direct contact with each other, or other layers, such as a colored layer, a printed layer, a bulk layer, etc., may be interposed between these layers. Other layers, such as a colored layer, a printed layer, a bulk layer, a surface protective layer, etc., may be disposed on the biaxially oriented PET film layer.

[0025] In one embodiment, the decorative film is composed of a biaxially oriented PET film layer and a colored adhesive layer. "Composed of a biaxially oriented PET film layer and a colored adhesive layer" means that the decorative film does not include any layer other than the biaxially oriented PET film layer, the colored adhesive layer, and the liner that is removed during use.

[0026] Fig. 1 shows a schematic cross-sectional view of a decorative film (vehicle interior film and shatterproof film) according to one embodiment. The decorative film 10 includes a biaxially oriented PET film layer 12 and a colored adhesive layer 14. The decorative film 10 in Fig. 1 further includes a liner 16 as an optional component. The liner 16 is removed before the decorative film 10 is attached to an adherend.

[0027] The present inventors have found that biaxially stretched PET film is superior to acrylic resin films commonly used for decorative films in terms of durability against external mechanical forces, strength, and non-flammability (oxygen consumption during combustion), and that, like acrylic resin films, it is less susceptible to thermal shrinkage in high-temperature environments than polyvinyl chloride films commonly used for decorative films. Based on this finding, the present inventors have adopted a biaxially stretched PET film as the film substrate for the decorative film of the present disclosure. Due to these properties of the biaxially stretched PET film, even if the thickness of the biaxially stretched PET film is reduced, it is possible to satisfy the durability and mechanical properties required for use as a decorative film for vehicle interiors or a shatterproof film, and by making it even thinner, it is possible to obtain even better non-flammability.

[0028] The biaxially stretched PET film layer may contain only polyethylene terephthalate as a resin component, or may contain polyethylene terephthalate and other resins, for example, polyesters such as polybutylene terephthalate (PBT) and polyethylene naphthalate (PEN), polyolefins such as polycarbonate, polyethylene, and polypropylene, acrylic resins, polystyrene, polyamide, or polyurethane, or two or more of these. From the viewpoints of transparency and mechanical properties, the biaxially stretched PET film layer preferably contains more than 50 mass% of polyethylene terephthalate as a main component as a resin component, and more preferably contains only polyethylene terephthalate.

[0029] The stretch ratio of the biaxially stretched PET film layer may vary depending on the application, and for example, the MD (Machine Direction: resin flow direction) / TD (Transverse Direction: resin width direction) may be about 0.1 or more, about 0.2 or more, or about 0.5 or more, and about 10 or less, about 5 or less, or about 2 or less.

[0030] The thickness of the biaxially stretched PET film layer may vary, for example, about 10 μm or more, about 12 μm or more, or about 15 μm or more, and about 200 μm or less, about 150 μm or less, or about 100 μm or less. From the viewpoint of the elongation and non-flammability of the decorative film, the thickness of the biaxially stretched PET film layer is preferably about 80 μm or less, more preferably about 50 μm or less.

[0031] The biaxially stretched PET film layer is preferably colorless and transparent, or has a transparency to such an extent that the color of the colored adhesive layer can be visually recognized through the biaxially stretched PET film layer. In one embodiment, the total light transmittance of the biaxially stretched PET film layer in the wavelength range of 380 to 780 nm is about 80% or more, about 85% or more, or about 90% or more and 100% or less. In the present disclosure, the total light transmittance is measured in accordance with JIS A 5759:2008.

[0032] In one embodiment, the biaxially stretched PET film layer contains an ultraviolet absorbing agent. Examples of ultraviolet absorbing agents include benzotriazole compounds, hydroxyphenyltriazine compounds, and cyanoacrylate compounds, and specific product names include Tinuvin® 99-2, Tinuvin® 928, Tinuvin® P, Tinuvin® 479, and Tinuvin® 1130 (all from BASF Japan Ltd., Chuo-ku, Tokyo, Japan). The content of the ultraviolet absorbing agent can be about 0.5% by weight or more, or about 1% by weight or more, and about 10% by weight or less, or about 5% by weight or less, based on the weight of the biaxially stretched PET film layer.

[0033] The biaxially stretched PET film layer may contain a hindered amine light stabilizer (HALS) such as Tinuvin® 292, Tinuvin® 123, Tinuvin® 622SF, Tinuvin® 770 (all available from BASF Japan Ltd., Chuo-ku, Tokyo, Japan) in place of or in addition to the UV absorber.

[0034] The surface of the biaxially stretched PET film layer in contact with the colored adhesive layer may be subjected to a surface treatment such as a primer treatment, a corona treatment, a plasma treatment, etc. Examples of the primer treatment include treatment using a primer agent containing a carbodiimide compound, an amine compound, or an epoxy compound.

[0035] The biaxially stretched PET film layer may be colored with a coloring agent such as a pigment or dye. The biaxially stretched PET film layer may have a printed layer including a picture, a design, a character, or the like on its surface. The biaxially stretched PET film layer may have a matte or clear hard coat layer, a hydrophilic coat layer, a hydrophobic coat layer, a transparent overlaminate film layer, or the like on its surface opposite to the colored adhesive layer. The surface of the biaxially stretched PET film layer in contact with these printed layers, or the like, may be subjected to a surface treatment such as a primer treatment, a corona treatment, or a plasma treatment.

[0036] The colored adhesive layer contains a carboxy group-containing (meth)acrylic polymer, an amino group-containing (meth)acrylic polymer, and a colorant. By containing the carboxy group-containing (meth)acrylic polymer and the amino group-containing (meth)acrylic polymer in the colored adhesive layer, the colorant can be contained in the colored adhesive layer in a high concentration and uniformly dispersed state by utilizing the interaction between the colorant and the carboxy group or the amino group. Therefore, even if the colored adhesive layer is made relatively thin, it is possible to provide a decorative film having various saturations and brightnesses. In addition, being able to make the colored adhesive layer thin is advantageous from the viewpoint of non-flammability.

[0037] The carboxyl group-containing (meth)acrylic polymer can increase the cohesive strength of the colored adhesive layer due to the presence of the carboxyl group, thereby improving the adhesive strength. In some cases, the carboxyl group-containing (meth)acrylic polymer can increase the adhesion between the biaxially oriented PET film layer and the colored adhesive layer.

[0038] The carboxyl group-containing (meth)acrylic polymer can be obtained by copolymerizing a polymerizable composition containing a (meth)acrylic monomer, a carboxyl group-containing monomer, and, if necessary, other monomers having monoethylenically unsaturated groups. In the present disclosure, the (meth)acrylic monomer, the carboxyl group-containing monomer, the amino group-containing monomer, and other monomers having monoethylenically unsaturated groups are collectively referred to as polymerizable components. The (meth)acrylic monomer, the carboxyl group-containing monomer, and other monomers having monoethylenically unsaturated groups may each be used alone or in combination of two or more.

[0039] The (meth)acrylic monomer generally contains an alkyl (meth)acrylate, the alkyl group of which may have 1 to 12 carbon atoms. Examples of the alkyl (meth)acrylate include linear or branched alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-methylbutyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, and n-dodecyl (meth)acrylate; and alicyclic (meth)acrylates such as cyclohexyl (meth)acrylate, 4-t-butylcyclohexyl (meth)acrylate, and isobornyl (meth)acrylate. Preferably, the alkyl (meth)acrylate comprises methyl (meth)acrylate, n-butyl (meth)acrylate, 2-ethylhexyl acrylate, or a combination thereof.

[0040] The alkyl (meth)acrylate constitutes the main component of the carboxy group-containing (meth)acrylic polymer. In one embodiment, the carboxy group-containing (meth)acrylic polymer is obtained by copolymerizing a polymerizable composition containing the alkyl (meth)acrylate in an amount of about 50 mass % or more, about 70 mass % or more, or about 80 mass % or more, about 99.5 mass % or less, about 99 mass % or less, or about 98 mass % or less, based on the mass of the polymerizable component, and contains the alkyl (meth)acrylate-derived constitutional unit in the above mass ratio.

[0041] The (meth)acrylic monomer may include aromatic (meth)acrylates such as phenyl (meth)acrylate, p-tolyl (meth)acrylate, etc.; phenoxyalkyl (meth)acrylates such as phenoxyethyl (meth)acrylate, etc.; alkoxyalkyl (meth)acrylates such as methoxypropyl (meth)acrylate, 2-methoxybutyl (meth)acrylate, etc.; or cyclic ether-containing (meth)acrylates such as glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, etc.

[0042] Examples of the carboxyl group-containing monomer include (meth)acrylic acid, monohydroxyethyl phthalate (meth)acrylate, β-carboxyethyl (meth)acrylate, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, crotonic acid, itaconic acid, fumaric acid, citraconic acid, and maleic acid. The carboxyl group-containing monomer is preferably (meth)acrylic acid. In the present disclosure, a monomer that corresponds to both a (meth)acrylic monomer and a carboxyl group-containing monomer, such as (meth)acrylic acid, is treated as a carboxyl group-containing monomer.

[0043] In one embodiment, the carboxy group-containing (meth)acrylic polymer is obtained by copolymerizing a polymerizable composition containing a carboxy group-containing monomer in an amount of about 0.5 mass % or more, about 1 mass % or more, or about 2 mass % or more, about 15 mass % or less, about 10 mass % or less, or about 8 mass % or less, based on the mass of the polymerizable component, and contains constitutional units derived from the carboxy group-containing monomer in the above-mentioned mass ratio.

[0044] Examples of (meth)acrylic monomers or other monomers having a monoethylenically unsaturated group include amide group-containing monomers such as (meth)acrylamide, N-vinylpyrrolidone, and N-vinylcaprolactam; hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; unsaturated nitriles such as (meth)acrylonitrile; aromatic vinyl monomers such as styrene, α-methylstyrene, and vinyl toluene; and vinyl esters such as vinyl acetate.

[0045] The copolymerization of the carboxyl group-containing (meth)acrylic polymer can be carried out by radical polymerization. As the radical polymerization, known polymerization methods such as solution polymerization, suspension polymerization, emulsion polymerization, and bulk polymerization can be used. It is advantageous to use solution polymerization, which can easily synthesize a polymer with a high molecular weight. As the polymerization initiator, for example, an organic peroxide such as benzoyl peroxide, lauroyl peroxide, or bis(4-tert-butylcyclohexyl)peroxydicarbonate; or an azo polymerization initiator such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), dimethyl-2,2-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), dimethyl 2,2'-azobis(2-methylpropionate), or azobis(2,4-dimethylvaleronitrile)(AVN) can be used. The amount of the polymerization initiator used is generally about 0.01 parts by mass or more, or about 0.05 parts by mass or more, and about 5 parts by mass or less, or about 3 parts by mass or less, based on 100 parts by mass of the polymerizable component.

[0046] The amino group-containing (meth)acrylic polymer can enhance the cohesive strength of the colored adhesive layer by interacting with the carboxy group-containing (meth)acrylic polymer, thereby improving the adhesive properties of the colored adhesive layer. The amino group-containing (meth)acrylic polymer has the ability to capture trace amounts of metal ions, such as iron ions, contained in the glass to be adhered, with the amino group. This makes it possible to suppress the depolymerization reaction of the (meth)acrylic polymer, which may be catalyzed by metal ions activated by ultraviolet rays contained in sunlight in a high-temperature environment, when the decorative film is applied to a glass substrate, and to maintain the adhesive strength of the colored adhesive layer at a desired level.

[0047] The amino group-containing (meth)acrylic polymer can be obtained by copolymerizing a polymerizable composition containing a (meth)acrylic monomer, an amino group-containing monomer, and, if necessary, other monomers having a monoethylenically unsaturated group. The (meth)acrylic monomer, the amino group-containing monomer, and the other monomers having a monoethylenically unsaturated group may each be used alone or in combination of two or more kinds.

[0048] As for the (meth)acrylic monomer and other monomers having a monoethylenically unsaturated group, the same ones as those explained for the carboxy group-containing (meth)acrylic polymer can be used.

[0049] The alkyl (meth)acrylate constitutes the main component of the amino group-containing (meth)acrylic polymer. In one embodiment, the amino group-containing (meth)acrylic polymer is obtained by copolymerizing a polymerizable composition containing the alkyl (meth)acrylate in an amount of about 50 mass % or more, about 70 mass % or more, or about 80 mass % or more, about 99.5 mass % or less, about 99 mass % or less, or about 98 mass % or less, based on the mass of the polymerizable component, and contains the alkyl (meth)acrylate-derived constitutional unit in the above mass ratio.

[0050] Examples of the amino group-containing monomer include aminoalkyl(meth)acrylates such as aminoethyl(meth)acrylate; monoalkylaminoalkyl(meth)acrylates such as butylaminoethyl(meth)acrylate; dialkylaminoalkyl(meth)acrylates such as N,N-dimethylaminoethylacrylate (DMAEA) and N,N-dimethylaminoethylmethacrylate (DMAEMA); dialkylaminoalkyl(meth)acrylamides such as N,N-dimethylaminopropylacrylamide (DMAPAA) and N,N-dimethylaminopropylmethacrylamide; and dialkylaminoalkylvinylethers such as N,N-dimethylaminoethylvinylether and N,N-diethylaminoethylvinylether. The amino group-containing monomer is preferably a dialkylaminoalkyl(meth)acrylate such as N,N-dimethylaminoethylacrylate (DMAEA) and N,N-dimethylaminoethylmethacrylate (DMAEMA). In the present disclosure, a monomer that falls under both the (meth)acrylic monomer and the amino group-containing monomer, such as aminoethyl (meth)acrylate, is treated as an amino group-containing monomer.

[0051] In one embodiment, the amino group-containing (meth)acrylic polymer is obtained by copolymerizing a polymerizable composition containing an amino group-containing monomer in an amount of about 0.5% by mass or more, about 1% by mass or more, or about 2% by mass or more, about 20% by mass or less, about 15% by mass or less, or about 10% by mass or less, based on the mass of the polymerizable components, and contains constitutional units derived from the amino group-containing monomer in the above-mentioned mass ratio.

[0052] The amino group-containing (meth)acrylic polymer is preferably an amino group-containing (meth)acrylic polymer that does not contain a monomer unit derived from an aromatic vinyl monomer (hereinafter, in this disclosure, also referred to as "amino group-containing non-aromatic (meth)acrylic polymer"). Since the amino group-containing non-aromatic (meth)acrylic polymer has excellent compatibility with the carboxy group-containing (meth)acrylic polymer, the above-mentioned interaction with the carboxy group-containing (meth)acrylic polymer can be made more effective.

[0053] The amino group-containing non-aromatic (meth)acrylic polymer does not contain a constituent unit derived from an aromatic vinyl monomer. Examples of aromatic vinyl monomers include styrene, α-methylstyrene, vinyltoluene, vinylnaphthalene, vinylanthracene, vinylanthraquinone, (meth)acrylamides of aromatic amines, and (meth)acrylates of hydroxyl group-containing aromatic compounds. Examples of aromatic amines include aniline, benzylamine, naphthylamine, aminoanthracene, aminoanthraquinone, and derivatives thereof. Examples of hydroxyl group-containing aromatic compounds include hydroxyl group-containing compounds corresponding to the above aromatic amines.

[0054] Copolymerization of amino group-containing (meth)acrylic polymers can be carried out by radical polymerization, similar to copolymerization of carboxyl group-containing (meth)acrylic polymers. The polymerization method, polymerization initiator and amount thereof are the same as those described for copolymerization of carboxyl group-containing (meth)acrylic polymers.

[0055] In the colored adhesive layer, at least one of the carboxyl group-containing (meth)acrylic polymer and the amino group-containing (meth)acrylic polymer functions as an acrylic adhesive polymer, which imparts pressure-sensitive adhesiveness to the colored adhesive layer at a usage temperature (e.g., 5°C to 35°C).

[0056] The glass transition temperature (Tg) of the acrylic adhesive polymer can be about -70°C to about -20°C. In one embodiment, the glass transition temperature of the acrylic adhesive polymer is about -65°C or higher, or about -60°C or higher, and about -25°C or lower, or about -30°C or lower. By setting the glass transition temperature of the acrylic adhesive polymer to about -70°C or higher, it is possible to impart adhesive strength and holding strength to the colored adhesive layer. By setting the glass transition temperature of the acrylic adhesive polymer to about -20°C or lower, it is possible to effectively impart initial adhesiveness (tack) to the colored adhesive layer.

[0057] The glass transition temperature (Tg) of acrylic adhesive polymers is calculated by the following FOX formula (Fox, TG, Bull. Am. Phys. Soc., 1 (1956), p. 123), assuming that each polymer is copolymerized with n kinds of monomers.

number

number

[0058] In one embodiment, the weight average molecular weight (Mw) of the acrylic adhesive polymer is about 150,000 or more, about 200,000 or more, or about 250,000 or more, and about 2,000,000 or less, about 1,500,000 or less, or about 1,000,000 or less. In the present disclosure, the "weight average molecular weight" refers to the molecular weight calculated using standard polystyrene by gel permeation chromatography (GPC).

[0059] The mass ratio of the carboxy group-containing (meth)acrylic polymer to the amino group-containing (meth)acrylic polymer can be 100:about 0.1-50, 100:about 1-40, or 100:about 2-30 (when the carboxy group-containing (meth)acrylic polymer functions as an acrylic adhesive polymer), or about 0.1-50:100, about 1-40:100, or about 2-30:100 (when the amino group-containing (meth)acrylic polymer functions as an acrylic adhesive polymer).

[0060] When a general decorative film is applied (interior application) to the inside or indoor side of a glass substrate such as a window glass of a vehicle or building, the adhesive contained in the adhesive layer constituting the decorative film may deteriorate. The deterioration of the adhesive is specifically caused by the decomposition of the adhesive polymer, which is the main component of the adhesive, such as an acrylic adhesive polymer, and is considered to be mainly caused by exposure to sunlight (especially exposure to ultraviolet light) that penetrates the glass substrate, and a continuous high temperature environment created by heat accumulated in a relatively thick glass substrate. It is generally known that the weather resistance of a decorative film can be improved by incorporating an ultraviolet absorbing agent into the film substrate of the decorative film. However, in the case of interior application, since the film substrate is located on the back side of the adhesive layer with respect to sunlight, the ultraviolet absorbing agent contained in the film substrate does not directly contribute to reducing the amount of ultraviolet light incident on the adhesive layer. Thus, the deterioration of the adhesive in the decorative film is more of a problem in interior application than in exterior application (the decorative film is applied to the outside or outdoor side of the glass substrate). When the adhesive deteriorates, the cohesive force of the adhesive decreases, and the internal stress of the film substrate generated during application overcomes the cohesive force of the adhesive, causing the decorative film to shrink, or air bubbles may be generated between the decorative film and the glass substrate.

[0061] In one embodiment, a (meth)acrylic polymer other than the (meth)acrylic polymer that functions as the acrylic adhesive polymer may function as the acrylic polymer additive. That is, when a carboxy group-containing (meth)acrylic polymer functions as the acrylic adhesive polymer, an amino group-containing (meth)acrylic polymer may function as the acrylic polymer additive, and when an amino group-containing (meth)acrylic polymer functions as the acrylic adhesive polymer, a carboxy group-containing (meth)acrylic polymer may function as the acrylic polymer additive. The acrylic polymer additive can suppress the decrease in cohesive strength caused by depolymerization of the acrylic adhesive polymer caused by exposure to sunlight, etc., through the acid (carboxy group)-base (amino group) interaction with the acrylic adhesive polymer, thereby maintaining the adhesive strength at a desired level.

[0062] In one embodiment, the carboxy group-containing (meth)acrylic polymer is the acrylic adhesive polymer and the amino group-containing (meth)acrylic polymer is the acrylic polymer additive.

[0063] The glass transition temperature (Tg) of the acrylic polymer additive can be about 20°C to about 120°C. In one embodiment, the glass transition temperature of the acrylic polymer additive is about 30°C or more, or about 45°C or more, and about 100°C or less, or about 80°C or less. By setting the glass transition temperature of the acrylic polymer additive to about 20°C or more, it is possible to suppress the decrease in cohesive force caused by depolymerization of the acrylic adhesive polymer caused by exposure to sunlight, etc., and to maintain the adhesive force at a desired level. By setting the glass transition temperature of the acrylic polymer additive to about 100°C or less, it is possible to ensure the adhesiveness in the normal temperature range. The glass transition temperature of the acrylic polymer additive can be determined using the FOX formula in the same manner as the acrylic adhesive polymer.

[0064] In one embodiment, the weight average molecular weight (Mw) of the acrylic polymer additive is about 1,000 or more, about 5,000 or more, or about 10,000 or more and about 200,000 or less, about 100,000 or less, or about 80,000 or less.

[0065] In one embodiment, the glass transition temperature of the carboxyl group-containing (meth)acrylic polymer or amino group-containing (meth)acrylic polymer functioning as the acrylic adhesive polymer is about -70 ° C to about -20 ° C, the glass transition temperature of the carboxyl group-containing (meth)acrylic polymer or amino group-containing (meth)acrylic polymer functioning as the acrylic polymer additive is 20 ° C to 120 ° C, and the content of the acrylic polymer additive in the colored adhesive layer is about 11 parts by mass to about 40 parts by mass based on 100 parts by mass of the acrylic adhesive polymer. The content of the acrylic polymer additive is preferably about 12 parts by mass or more, or about 15 parts by mass or more, and about 30 parts by mass or less, or about 25 parts by mass or less, based on 100 parts by mass of the acrylic adhesive polymer. By setting the content of the acrylic polymer additive to about 11 parts by mass or more based on 100 parts by mass of the acrylic adhesive polymer, the acrylic polymer additive having a high glass transition temperature of 20°C to 120°C can suppress the decrease in the cohesive strength of the acrylic adhesive polymer caused by exposure to sunlight, and the adhesive strength of the colored adhesive layer can be maintained at a desired level. By setting the content of the acrylic polymer additive to about 40 parts by mass or less based on 100 parts by mass of the acrylic adhesive polymer, the adhesiveness can be ensured even at low temperatures.

[0066] Examples of colorants include pigments and dyes. The pigments and dyes can be used alone or in combination of two or more. The form of the pigments and dyes is not particularly limited, and they may be subjected to a dispersion treatment.

[0067] Examples of pigments include inorganic pigments such as zinc carbonate, zinc oxide, zinc sulfide, talc, kaolin, calcium carbonate, titanium oxide, carbon black, yellow lead, yellow iron oxide, red iron oxide, barium sulfate, alumina, zirconia, iron oxide pigments, iron hydroxide pigments, chromium oxide pigments, spinel-type calcined pigments, chromate pigments, chrome vermilion pigments, Prussian blue pigments, aluminum powder pigments, bronze powder pigments, and calcium phosphate; and organic pigments such as phthalocyanine pigments such as phthalocyanine blue and phthalocyanine green, azo pigments, condensed azo pigments, azo lake pigments, anthraquinone pigments, indigo pigments, thioindigo pigments, isoindolinone pigments, azomethine azo pigments, aniline black pigments, triphenylmethane pigments, perinone pigments, perylene pigments, quinophthalone pigments, dioxazine pigments, and quinacridone pigments such as quinacridone red.

[0068] Examples of dyes include azo dyes, anthraquinone dyes, quinonephthalone dyes, styryl dyes, diphenylmethane dyes, triphenylmethane dyes, oxazine dyes, triazine dyes, xanthan dyes, azomethine dyes, acridine dyes, and diazine dyes.

[0069] The content of the colorant can be about 0.1 parts by mass or more, about 0.5 parts by mass or more, or about 1 part by mass or more, and about 100 parts by mass or less, about 75 parts by mass or less, or about 50 parts by mass or less, based on 100 parts by mass in total of the carboxy group-containing (meth)acrylic polymer and the amino group-containing (meth)acrylic polymer.

[0070] At least one of the carboxyl group-containing (meth)acrylic polymer and the amino group-containing (meth)acrylic polymer may function as a dispersant for the colorant. In this embodiment, the colorant and the (meth)acrylic polymer functioning as a dispersant may be mixed to prepare a premix (also called a mill base), and the obtained premix may be mixed with other components of the colored adhesive composition used to form the colored adhesive layer. This allows a large amount of colorant to be stably dispersed in the colored adhesive layer. In addition, a premix may be prepared for each of a plurality of colorants, and these premixes may be appropriately mixed to facilitate color matching.

[0071] The carboxyl group-containing (meth)acrylic polymer or amino group-containing (meth)acrylic polymer functioning as a dispersant may be the same as or different from the one functioning as the acrylic adhesive polymer or acrylic polymer additive. In the latter case, the colored adhesive layer contains two or more carboxyl group-containing (meth)acrylic polymers or amino group-containing (meth)acrylic polymers, i.e., a carboxyl group-containing (meth)acrylic polymer or amino group-containing (meth)acrylic polymer functioning as a dispersant and a carboxyl group-containing (meth)acrylic polymer or amino group-containing (meth)acrylic polymer functioning as an acrylic adhesive polymer or acrylic polymer additive.

[0072] The weight average molecular weight (Mw) of the carboxy group-containing (meth)acrylic polymer or amino group-containing (meth)acrylic polymer that functions as a dispersant can generally be about 1,000 or more, or about 10,000 or more, and about 1,500,000 or less, or about 800,000 or less.

[0073] The pigmented adhesive layer can be formed on the biaxially oriented PET film layer or liner using a pigmented adhesive composition containing a carboxy group-containing (meth)acrylic polymer, an amino group-containing (meth)acrylic polymer, and a colorant, as well as, if necessary, a crosslinker, a solvent, and / or other additives.

[0074] Before preparing the colored adhesive composition, a premix may be prepared by mixing a colorant with a carboxyl group-containing (meth)acrylic polymer or an amino group-containing (meth)acrylic polymer that functions as a dispersant. The mixing may be performed, for example, using a paint shaker, a sand grind mill, a ball mill, an attritor mill, or a three-roll mill. During mixing, an aqueous solvent or an organic solvent may be added as necessary. The obtained premix may be mixed with other components of the colored adhesive composition to prepare the colored adhesive composition. When multiple colorants are used, a premix may be prepared for each colorant, and the premix mixture may be mixed appropriately to tone the color, and then mixed with other components of the colored adhesive composition.

[0075] The mass ratio of the colorant to the dispersant can be about 1-100: about 5-1000, about 1-100: about 10-700, or about 1-100: about 10-500. The entire amount of the dispersant may be used when preparing the premix, or a portion of the dispersant may be used when preparing the premix and the remainder may be used when preparing the colored adhesive composition.

[0076] The crosslinking agent is not particularly limited as long as it can form a crosslink between polymer chains of a carboxyl group-containing (meth)acrylic polymer or an amino group-containing (meth)acrylic polymer. For example, an epoxy-based crosslinking agent, a bisamide-based crosslinking agent, an aziridine-based crosslinking agent, a carbodiimide-based crosslinking agent, an isocyanate-based crosslinking agent, etc. can be used as the crosslinking agent for a carboxyl group-containing (meth)acrylic polymer.

[0077] Examples of epoxy crosslinking agents include N,N,N',N'-tetraglycidyl-1,3-benzenedi(methaneamine) (trade names include TETRAD-X (Mitsubishi Gas Chemical Company, Inc., Chiyoda-ku, Tokyo, Japan), E-AX, and E-5XM (all of which are manufactured by Soken Chemical & Engineering Co., Ltd., Toshima-ku, Tokyo, Japan)), and N,N'-(cyclohexane-1,3-diylbismethylene)bis(diglycidylamine) (trade names include TETRAD-C (Mitsubishi Gas Chemical Company, Inc., Chiyoda-ku, Tokyo, Japan), and E-5C (Soken Chemical & Engineering Co., Ltd., Toshima-ku, Tokyo, Japan)).

[0078] Examples of bisamide crosslinking agents include 1,1'-isophthaloyl-bis(2-methylaziridine), 1,4-bis(ethyleneiminocarbonylamino)benzene, 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane, and 1,8-bis(ethyleneiminocarbonylamino)octane.

[0079] Examples of aziridine-based crosslinking agents include 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate (trade names: Chemitite (registered trademark) PZ-33 (Nippon Shokubai Co., Ltd., Osaka City, Osaka Prefecture, Japan)) and Crosslinker CX-100 (DSM Coating Resins BV, Zwolle, Kingdom of the Netherlands)).

[0080] Examples of carbodiimide crosslinking agents include Carbodilite V-03, V-05, and V-07 (all manufactured by Nisshinbo Chemical Inc., Chuo-ku, Tokyo, Japan).

[0081] Examples of isocyanate crosslinking agents include Coronate L and Coronate HK (both available from Tosoh Corporation (Minato-ku, Tokyo, Japan)).

[0082] The crosslinking agent can be used in an amount of about 0.01 parts by mass or more, about 0.02 parts by mass or more, or about 0.05 parts by mass or more, and about 0.5 parts by mass or less, about 0.4 parts by mass or less, or about 0.3 parts by mass or less, based on 100 parts by mass of the carboxy group-containing (meth)acrylic polymer or amino group-containing (meth)acrylic polymer that functions as the acrylic adhesive polymer.

[0083] Examples of the solvent include methanol, ethanol, hexane, heptane, toluene, acetone, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, butyl acetate, and the like, or mixtures of these solvents.

[0084] Examples of other additives include ultraviolet absorbers, antioxidants, heat stabilizers, fillers, and tackifiers.

[0085] The thickness of the colored adhesive layer may vary, for example, about 5 μm or more, about 10 μm or more, or about 20 μm or more, and about 200 μm or less, about 100 μm or less, or about 80 μm or less. From the viewpoint of the non-flammability of the decorative film, the thickness of the colored adhesive layer is preferably about 50 μm or less, and more preferably about 30 μm or less.

[0086] The decorative film can be produced by a known method. For example, the colored adhesive composition is applied onto a liner by knife coating, bar coating, or the like, and dried to form a colored adhesive layer. The colored adhesive layer may be heated during drying using hot air, an oven, or the like to react with the optional crosslinking agent. A biaxially oriented PET film layer may be laminated onto the obtained colored adhesive layer by a method such as dry lamination to produce a decorative film. The colored adhesive composition may also be applied directly onto the biaxially oriented PET film layer and dried to produce a decorative film.

[0087] The decorative film may have a liner on the surface of the colored adhesive layer opposite the biaxially oriented PET film layer. The liner, which is an optional component, may be, for example, a plastic material such as polyethylene, polypropylene, polyester, or cellulose acetate, paper, or a laminated paper of the plastic material. These liners may have a surface that has been subjected to a release treatment using silicone or the like. The thickness of the liner may be generally about 10 μm or more, or about 25 μm or more, and about 500 μm or less, or about 200 μm or less.

[0088] The colored adhesive layer may be solid, porous or foamed. The adhesive surface of the colored adhesive layer may be flat or uneven. The uneven adhesive surface includes an adhesive surface in which a convex portion containing the solid content of the colored adhesive composition or the solid content of the reaction product and a concave portion surrounding the convex portion are formed on the adhesive surface of the colored adhesive layer, and a communication path that communicates with the outside and is defined by the concave portion between the surface of the adherend and the adhesive surface when the colored adhesive layer is adhered to the adherend is formed. An example of a method for forming an uneven adhesive surface is described below.

[0089] A liner having a release surface with a predetermined uneven structure is prepared. A colored adhesive composition is applied to the release surface of the liner and heated as necessary to form a colored adhesive layer. This transfers the uneven structure (negative structure) of the liner to the surface of the colored adhesive layer that contacts the liner (this becomes the adhesive surface of the decorative film), forming an uneven adhesive surface with a predetermined structure (positive structure) on the adhesive surface. As described above, the unevenness of the adhesive surface is designed in advance to include grooves that can form communication paths when the convex parts are adhered to the adherend.

[0090] The grooves of the colored adhesive layer may be formed in a regular pattern by arranging grooves of a certain shape on the adhesive surface along a regular pattern, or may be formed in an irregular pattern by arranging grooves of an indefinite shape. When a plurality of grooves are formed so as to be arranged substantially parallel to each other, the arrangement interval of the grooves is preferably about 10 μm or more, or about 100 μm or more, and about 2000 μm or less, or about 1000 μm or less. The depth of the groove (the distance from the adhesive surface to the bottom of the groove measured toward the direction of the biaxially stretched PET film layer) is usually about 10 μm or more and about 100 μm or less. The shape of the groove is also not particularly limited as long as it does not impair the effects of the present invention. For example, the shape of the groove can be substantially rectangular (including trapezoidal), substantially semicircular, or substantially semielliptical in the cross section of the groove in the direction perpendicular to the adhesive surface.

[0091] In one embodiment, the thickness of the decorative film, excluding the liner, is about 270 μm or less, about 200 μm or less, or about 100 μm or less. The thickness of the decorative film, excluding the liner, can be about 30 μm or more, about 40 μm or more, or about 50 μm or more.

[0092] In one embodiment, the visible light transmittance of the decorative film, excluding the liner, is about 10% or more, about 30% or more, or about 50% or more, and about 99% or less, about 97% or less, or about 95% or less.

[0093] The pencil hardness of the biaxially stretched polyethylene terephthalate film layer side of the decorative film is at least B. The pencil hardness is preferably at least H, and more preferably at least 2H.

[0094] The decorative film has a tensile strength of about 50 N / 25 mm or more at 2% elongation, preferably about 60 N / 25 mm or more, and more preferably about 75 N / 25 mm or more.

[0095] The decorative film has an elongation of about 60% or more, preferably about 70% or more, and more preferably about 80% or more.

[0096] The pencil hardness, tensile strength at 2% elongation and elongation are determined by the procedures described in the Examples.

[0097] The total heat generated by the decorative film for 20 minutes after the start of heating, measured in accordance with the ISO5660-1 cone calorimeter heat generation test, is 8MJ / m 2 In one embodiment, the total calorific value is about 7 MJ / m 2 or less than 6MJ / m 2 The total calorific value is 8 MJ / m or less. 2 If the following is true, the decorative film is determined to be non-flammable:

[0098] The shatterproof film is preferably transparent, which means that the total light transmittance in the wavelength range of 380 to 780 nm is about 80% or more.

[0099] In one embodiment, the decorative film is substantially free of flame retardants. Here, "substantially free" means that the content of flame retardants is less than about 1% by weight, less than about 0.5% by weight, or less than about 0.2% by weight, based on the weight of the decorative film. Examples of flame retardants include organic flame retardants such as bromine-based flame retardants, phosphorus-based flame retardants, and chlorine-based flame retardants, and inorganic flame retardants such as antimony compounds, metal hydroxides, nitrogen compounds, and boron compounds. Addition of a flame retardant may reduce the adhesiveness of the decorative film, so the absence of a flame retardant can ensure the adhesiveness of the decorative film. In addition, addition of a flame retardant may reduce the elongation properties of the decorative film.

[0100] The decorative film of the present disclosure can be suitably used as a decorative film for vehicle interiors for vehicle interior purposes, and as a shatterproof film for the window glass of vehicles, buildings, etc. EXAMPLES

[0101] The following examples illustrate specific embodiments of the disclosure, but do not limit the invention. All parts and percentages are by weight unless otherwise specified.

[0102] The materials used to prepare the decorative film are shown in Table 1.

[0103] [Table 1]

[0104] Table 2 shows the pigments 1 to 4 used in the preparation of the decorative film.

[0105] [Table 2]

[0106] Table 3 shows the formulations of the mill bases 1 to 4 (premixes) used in producing the decorative films.

[0107] [Table 3]

[0108] Table 4 shows the formulations of the colored adhesive compositions CA1 to CA3 and CA6 used in producing the decorative films.

[0109] [Table 4]

[0110] Example 1 Crosslinker 1 (CL1) was mixed into colored adhesive composition CA1. The mass ratio of adhesive polymer 2 (ADH2) to CL1 in CA1 was 100:0.05 based on the non-volatile content. The obtained colored adhesive composition was applied onto a liner having a structured surface (SCW860DNL, 3M Japan Co., Ltd., Minato-ku, Tokyo, Japan) using a knife coater and dried at 95°C for 3 minutes. After drying, a colored adhesive layer with a thickness of 25 μm was obtained. The colored adhesive layer was laminated with film 1 (FL1) to obtain the decorative film of Example 1.

[0111] Example 2 and Example 3 A decorative film was obtained in the same manner as in Example 1, except that the colored adhesive composition was changed as shown in Table 5.

[0112] Example 4 A white pigment premix was prepared containing a white pigment, pigment 1 (PG1), (meth)acrylic polymer 1 (AP1), and methyl ethyl ketone (MEK). The mass ratio of PG1 to AP1 was 5:1 based on the nonvolatile content. The solid content of the white pigment premix was about 66% by mass. A colored adhesive composition CA4 was prepared containing a white pigment premix and adhesive polymer 1 (ADH1). The mass ratio of ADH1, PG1, and AP1 was 100:50:10 based on the nonvolatile content. CL1 was mixed with CA4 to obtain a white adhesive composition. The mass ratio of ADH1 to CL1 was 100:0.2 based on the nonvolatile content. The solid content of the white adhesive composition was about 35% by mass.

[0113] The white adhesive composition was applied onto a silicone-coated polyethylene laminated paper liner using a knife coater and dried at 95°C for 5 minutes. After drying, a white adhesive layer with a thickness of 30 μm was obtained. The white adhesive layer and FL1 were laminated together to obtain the decorative film of Example 4.

[0114] Example 5 A white pigment premix was prepared in the same manner as in Example 4. Then, a pigmented adhesive composition CA5 was prepared containing the white pigment premix and ADH2. The mass ratio of ADH2, PG1, and AP1 was 100:40:8 based on the non-volatile content. CL2 was mixed with CA5 to obtain a white adhesive composition. The mass ratio of ADH2 to CL2 was 100:0.05 based on the non-volatile content. The solid content of the white adhesive composition was about 38% by mass.

[0115] The white adhesive composition was applied onto a silicone-coated polyethylene laminated paper liner using a knife coater and dried at 95°C for 5 minutes. After drying, a white adhesive layer with a thickness of 40 μm was obtained. The white adhesive layer and FL1 were laminated together to obtain the decorative film of Example 5.

[0116] Example 6 CL1 was mixed with the colored adhesive composition CA6. The mass ratio of ADH1 to CL1 in CA6 was 100:0.2 based on the non-volatile content. The obtained colored adhesive composition was coated on a silicone-coated polyethylene laminated paper liner using a knife coater and dried at 95°C for 3 minutes. After drying, a colored adhesive layer with a thickness of 21 μm was obtained. The colored adhesive layer was laminated with FL2 to obtain the decorative film of Example 6.

[0117] Example 7 A decorative film was obtained in the same manner as in Example 6, except that FL2 was changed to FL3.

[0118] Comparative Example 1 As the decorative film of Comparative Example 1, 3M (registered trademark) Scotchtint (registered trademark) window film SH2CLAR-R5 (3M Japan Ltd., Minato-ku, Tokyo, Japan) was used.

[0119] Comparative Example 2 As the decorative film of Comparative Example 2, 3M (registered trademark) Scotchcal (registered trademark) Paint Film PF121AP (3M Japan Ltd., Minato-ku, Tokyo, Japan) was used.

[0120] Example 8 A decorative film was obtained in the same manner as in Example 3, except that FL1 was changed to FL4.

[0121] Example 9 A decorative film was obtained in the same manner as in Example 3, except that FL1 was changed to FL5.

[0122] Example 10 A decorative film was obtained in the same manner as in Example 5, except that the thickness of the white adhesive layer after drying was changed to 80 μm.

[0123] The decorative films were evaluated for the following items.

[0124] Tensile strength at 1.2% elongation The decorative film was cut to a width of 25 mm and a length of 150 mm to prepare a test piece. Using a tensile tester (Tensilon (registered trademark) universal testing machine, model number: RTC-1210A, A&D Co., Ltd., Toshima-ku, Tokyo, Japan), the stress at 2% elongation at a temperature of 20°C was recorded as the 2% tensile strength. The tensile speed was 300 mm / min, and the chuck distance was 100 mm.

[0125] 2. Tensile strength at yield The decorative film was cut into a test piece with a width of 25 mm and a length of 150 mm. The stress at the yield point at a temperature of 20°C was recorded as the tensile strength at yield using a tensile tester (Tensilon (registered trademark) universal testing machine, model number: RTC-1210A, A&D Co., Ltd., Toshima-ku, Tokyo, Japan). The tensile speed was 300 mm / min, and the chuck distance was 100 mm.

[0126] 3. Breaking strength and elongation The decorative film was cut to a width of 25 mm and a length of 150 mm to prepare a test specimen. Using a tensile tester (Tensilon (registered trademark) universal testing machine, model number: RTC-1210A, A&D Co., Ltd., Toshima-ku, Tokyo, Japan), the strength and elongation at the time when the test specimen broke (= (length of test specimen at break - length of test specimen before test) / length of test specimen before test) were recorded as the breaking strength and elongation, respectively. The tensile speed was 300 mm / min, and the chuck distance was 100 mm.

[0127] 4.Adhesive strength The decorative film was cut to a width of 25 mm and a length of 150 mm to prepare a test specimen. The test specimen was attached to a melamine-coated board (Partec Co., Ltd., Hiratsuka, Kanagawa Prefecture, Japan), an A5052P aluminum panel, a SUS304BA panel (Partec Co., Ltd., Hiratsuka, Kanagawa Prefecture, Japan), or a 3 mm-thick float glass panel (AGC Co., Ltd., Chiyoda-ku, Tokyo, Japan) at 20°C. The attachment method was in accordance with JIS Z 0237:2009 8.2.3. The test specimen was left at 20°C for 48 hours. The adhesive strength (N / 25mm) was measured using a tensile tester (Tensilon (registered trademark) universal testing machine, model number: RTC-1210A, A&D Co., Ltd., Toshima-ku, Tokyo, Japan) at a temperature of 20°C, a peeling speed of 300 mm / min, and a 180° peeling angle.

[0128] 5.Heat shrinkability The decorative film was cut to a width of 50 mm and a length of 100 mm to prepare a test specimen. The test specimen was attached to an A5052P aluminum panel with a roller in a 23°C environment and left for 24 hours in a 23°C environment. A cross cut was made in the test specimen with a cutter. The test specimen was then heated at 65°C for 48 hours. After heat aging, the shrinkage (mm) of the film was measured under a microscope and the maximum value was recorded.

[0129] 6. Pencil hardness (scratch resistance) The test was conducted according to JIS K5600-5-4 (ISO / DIN 15184). The hardness of the hardest pencil that did not leave a scratch was taken as the scratch hardness. 4H or higher was rated as "A", B to 3H was rated as "B", and 2B or lower was rated as "C". A and B were considered to be pass.

[0130] 7. Non-flammability test A decorative film was attached to a zinc-plated steel sheet (thickness 0.27 mm). The test was conducted in accordance with ISO5660-1 Cone Calorimeter Heat Release Test. The heat release rate (kW / m 2 ) and total calorific value (MJ / m 2 ) was measured using a cone calorimeter (manufactured by Toyo Seiki Seisakusho Co., Ltd.). The total calorific value for 20 minutes after the start of heating was 8 MJ / m 2Less than or equal to 200 kW / m 2 If the total time during which the heat release rate exceeded 10 seconds was 10 seconds or less, the test was judged as passing, and otherwise it was judged as failing.

[0131] The configurations and evaluation results of the decorative films of Examples 1 to 10 and Comparative Examples 1 and 2 are shown in Tables 5 and 6, respectively.

[0132] [Table 5]

[0133] [Table 6]

[0134] FIG. 2 is a graph showing the relationship between elongation (%, horizontal axis) and tensile strength (N / 25 mm, vertical axis) of the decorative films of Example 1 and Comparative Example 1.

[0135] It will be apparent to those skilled in the art that the above-described embodiments and examples can be modified in various ways without departing from the basic principles of the present invention. It will also be apparent to those skilled in the art that various improvements and modifications of the present invention can be made without departing from the spirit and scope of the present invention. [Explanation of symbols]

[0136] 10 Decorative films (vehicle interior decorative films and shatterproof films) 12 biaxially oriented polyethylene terephthalate film layers 14 Colored adhesive layer 16 Liner

Claims

1. A decorative film for vehicle interiors, comprising a biaxially oriented polyethylene terephthalate film layer and a colored adhesive layer, the colored adhesive layer contains a carboxy group-containing (meth)acrylic polymer, an amino group-containing (meth)acrylic polymer, and a colorant; The biaxially oriented polyethylene terephthalate film layer side of the decorative film has a pencil hardness of B or more; The decorative film has a tensile strength of 50 N / 25 mm or more at 2% elongation, an elongation of 60% or more, and a total heat generation amount of 8 MJ / m2 for 20 minutes after the start of heating measured in accordance with ISO 5660-1 Cone Calorimeter Heat Generation Test. 2 The following is a decorative film for vehicle interiors.

2. 2. The decorative film for vehicle interiors according to claim 1, wherein the biaxially oriented polyethylene terephthalate film layer contains an ultraviolet absorbing agent.

3. 3. The decorative film for vehicle interiors according to claim 1, which is substantially free of flame retardants.

4. The decorative film for vehicle interiors according to any one of claims 1 to 3, which comprises the biaxially oriented polyethylene terephthalate film layer and the colored adhesive layer.

5. The decorative film for vehicle interiors according to any one of claims 1 to 4, wherein the biaxially oriented polyethylene terephthalate film layer has a total light transmittance of 80% or more in the wavelength range of 380 to 780 nm.

6. The decorative film for vehicle interiors according to any one of claims 1 to 5, wherein the thickness of the decorative film for vehicle interiors is 270 µm or less.

7. A shatterproof film comprising a biaxially oriented polyethylene terephthalate film layer and a colored adhesive layer, the colored adhesive layer contains a carboxy group-containing (meth)acrylic polymer, an amino group-containing (meth)acrylic polymer, and a colorant; The shatterproof film has a pencil hardness of B or more on the biaxially oriented polyethylene terephthalate film layer side, The shatterproof film has a tensile strength of 50 N / 25 mm or more at 2% elongation, an elongation of 60% or more, and a total heat generation amount of 8 MJ / m2 for 20 minutes after the start of heating as measured in accordance with ISO 5660-1 Cone Calorimeter Heat Generation Test. 2 Below is the shatterproof film.

8. The shatterproof film of claim 7 , wherein the biaxially oriented polyethylene terephthalate film layer comprises an ultraviolet light absorber.

9. 9. The shatterproof film of claim 7 or 8, which is substantially free of flame retardants.

10. The shatterproof film according to any one of claims 7 to 9, which comprises the biaxially oriented polyethylene terephthalate film layer and the colored adhesive layer.

11. The shatterproof film according to any one of claims 7 to 10, wherein the biaxially oriented polyethylene terephthalate film layer has a total light transmittance of 80% or more in the wavelength range of 380 to 780 nm.

12. The shatterproof film according to any one of claims 7 to 11, wherein the thickness of the shatterproof film is 270 μm or less.

Citation Information

Patent Citations

  • Decorative film for glass

    JP2005343055A

  • Fired pencil lead

    JP2006265299A

  • Film for window and its pasting method, and scattering-preventing film and crime-preventing film

    JP2007031658A

  • Ultraviolet absorbing adhesive composition

    JP2007138117A

  • Laminate for forming transparent conductive film, transparent conductive film, touch panel, method for selecting second substrate with adhesive layer, method for manufacturing laminate for forming transparent conductive film, and method for manufacturing transparent conductive film