Method for manufacturing anisotropic conductive adhesive film with controlled fluidity of conductive particles

The production method for an anisotropic conductive adhesive film with controlled particle movement and aggregation addresses the challenge of maintaining electrical connection reliability in fine-pitch circuits, enhancing capture rates and reducing costs.

JP2024536468AInactive Publication Date: 2024-10-04H&S HIGHTECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024521830
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-20
Filing Date
2022-09-13
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional methods for connecting microcircuits face challenges in maintaining electrical connection reliability and insulation between electrodes, especially in fine-pitch and flexible circuit boards, due to the aggregation of conductive particles in anisotropic conductive adhesives during pressure bonding.

Method used

A method for producing an anisotropic conductive adhesive film involves semi-curing a polymer film layer with conductive particles to create a non-flowable conductive layer, accompanied by non-conductive layers with controlled modulus and thickness, minimizing conductive particle movement and aggregation during crimping.

Benefits of technology

The method enhances connection reliability by increasing the capture rate of conductive particles and reducing electrical short circuits, optimizing the film for various substrate structures, and potentially reducing manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536468000001_ABST
    Figure 2024536468000001_ABST
Patent Text Reader

Abstract

The anisotropic conductive adhesive film according to the present invention fixes the conductive particles with a strong force through the high modulus of the polymer, minimizing the movement of the conductive particles during the compression process. In particular, the non-flowable conductive layer containing the conductive particles is formed through a semi-curing process to fix the conductive particles with the modulus force of the polymer resin, thereby minimizing the movement of the conductive particles when resin flow occurs due to pressure during the compression process. In addition, adhesive layers are formed on the upper and lower parts of the semi-cured polymer film layer to improve physical properties that are reduced by the semi-cured film, such as adhesive strength, reliability, and connection resistance, thereby optimizing the physical properties of the anisotropic conductive adhesive film.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a circuit connection technology using an anisotropic conductive adhesive, and more specifically, to an anisotropic conductive adhesive for circuit connection that, when interconnecting two opposing circuit components, can electrically connect two opposing electrodes in the thickness direction while at the same time maintaining insulation between adjacent electrodes in the surface direction. [Background technology]

[0002] As electronic devices become smaller and thinner, circuit components become denser and more precise. This makes it difficult to connect fine circuits using conventional methods such as welding or soldering. To solve this problem, anisotropic conductive adhesives have been developed (JP Patent Publication 51-21192). Anisotropic conductive adhesives are circuit connection members that can electrically connect two opposing electrodes in the thickness direction and maintain insulation between adjacent electrodes in the surface direction by blending conductive particles with adhesive components containing a cured resin and adjusting the content. Such anisotropic conductive adhesives are widely used for the purpose of electrically connecting and bonding various circuit components when manufacturing display elements, semiconductor elements, etc.

[0003] In recent years, the integration density of electronic circuits has increased, and the pitch between electrodes has become finer, leading to a gradual reduction in the size (area) of circuit electrodes. Furthermore, the development and commercialization of various wearable devices that can be attached to the body has accelerated. Therefore, there is a strong demand for an anisotropic conductive adhesive that can maintain the reliability of electrical connections between circuit members even when the pitch between electrodes is fine and is applied to electronic circuits and / or flexible circuit boards.

[0004] In particular, with the trend towards higher resolution and smaller size of display devices, anisotropic conductive adhesive films applied to COG (chip on glass) and COP (chip on plastic) connection structures have a high density of conductive particles, so it is very important for signal stability to prevent conductive particles from connecting with each other. Also, in anisotropic conductive adhesive films with a high density of conductive particles, if conductive particles aggregate due to the flow of resin during compression, it is fatal to the performance of the anisotropic conductive adhesive film. Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention relates to an anisotropic conductive adhesive film, and more particularly, to a method for manufacturing an anisotropic conductive adhesive film for ultra-fine pitch. The present invention aims to provide a method for manufacturing an anisotropic conductive adhesive film in which a polymer film layer containing conductive particles is fixed by a high modulus force of a resin through semi-curing, and the conductive particles are fixed by a strong fixing force when resin flow occurs due to pressure, thereby minimizing the movement of the conductive particles during the compression process.

[0006] The objects of the present invention are not limited to those mentioned above, and other objects not mentioned will be clearly understood from the following description. [Means for solving the problem]

[0007] The method for producing an anisotropic conductive adhesive film according to the present invention includes a first step of coating a thermosetting resin composition having conductive particles dispersed therein onto a first release film, and then semi-curing the composition so that the curing rate measured by differential scanning calorimetry is 40% or more and 60% or less according to the following formula 1, thereby forming a non-flowable conductive layer; a second step of coating a thermosetting resin composition not containing conductive particles onto a second release film to form a first adhesive non-conductive layer; a third step of coating a thermosetting resin composition not containing conductive particles onto a third release film to form a second adhesive non-conductive layer; a fourth step of laminating the first adhesive non-conductive layer on the top (upper) of the non-flowable conductive layer through a lamination process; and a fifth step of removing the first release film and then laminating the second adhesive non-conductive layer on the bottom (lower) of the exposed non-flowable conductive layer through a lamination process.

[0008] [Formula 1] Cure rate (%) = [1-(initial heat value) / (heat value after semi-curing)] x 100

[0009] The conductive layer has a modulus of 10,000 to 50,000 Pa·s.

[0010] The modulus of the conductive layer is at least twice as high as the modulus of the first and second non-conductive layers.

[0011] The modulus of the first and second non-conductive layers is in the range of 1,000 to 5,000 Pa·s.

[0012] The thermosetting resin composition of the conductive layer, the first and second non-conductive layers may include an epoxy resin.

[0013] It is also preferred that the thickness of the conductive layer does not exceed 2 μm relative to the average particle size of the conductive particles. Effect of the Invention

[0014] According to the present invention, when circuit members are connected using an anisotropic conductive adhesive film, the movement of conductive particles occurring during the compression process is minimized, the number of captured conductive particles between electrodes is increased, and the aggregation of the conductive particles that have been washed away is minimized, thereby improving the connection reliability of electrical elements. In particular, when applied to a COG or COP connection structure, the physical properties of the non-conductive layers disposed above (upper) and below (lower) the conductive layer can be appropriately controlled and formed as necessary, so that an anisotropic conductive adhesive film optimized for substrates with different structures can be manufactured. [Brief description of the drawings]

[0015] [Figure 1] 1 is an image showing a cross section of an anisotropic conductive adhesive film according to the present invention. [Diagram 2] 4 is a differential scanning calorimetry result for the conductive layer of the anisotropic conductive adhesive film according to the present invention, showing a heat capacity graph before and after a semi-curing process. [Diagram 3] 1 is a graph showing the correlation between the capture rate and the connection resistance of an anisotropic conductive adhesive film, which depends on the curing rate of the conductive layer. [Figure 4] Graph (1) showing the change in viscosity depending on temperature for a conductive layer and a non-conductive layer. [Diagram 5] Graph (2) showing the change in viscosity depending on temperature for a conductive layer and a non-conductive layer. [Figure 6] Graph (3) showing the change in viscosity depending on temperature for conductive and non-conductive layers. [Figure 7] 1A to 1C are diagrams illustrating a manufacturing process of an anisotropic conductive adhesive film according to the present invention. [Figure 8] 2A to 2C are diagrams illustrating a lamination process of the anisotropic conductive adhesive film according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] <Best Mode for Carrying Out the Invention> The method for producing an anisotropic conductive adhesive film according to the present invention is characterized by comprising the steps of: a first step of coating a thermosetting resin composition having conductive particles dispersed therein onto a first release film, and semi-curing the composition so that the cure rate measured by differential scanning calorimetry is 40% or more and 60% or less according to the following formula 1; a second step of coating a thermosetting resin composition not containing conductive particles onto a second release film to form a first adhesive non-conductive layer; a third step of coating a thermosetting resin composition not containing conductive particles onto a third release film to form a second adhesive non-conductive layer; a fourth step of laminating the first adhesive non-conductive layer on the top (upper) of the non-flowable conductive layer through a lamination process; and a fifth step of removing the first release film and laminating the second adhesive non-conductive layer on the bottom (lower) of the exposed non-flowable conductive layer through a lamination process.

[0017] [Formula 1] Cure rate (%) = [1-(initial heat value) / (heat value after semi-curing)] x 100

[0018] The conductive layer has a modulus of 10,000 to 50,000 Pa·s.

[0019] The modulus of the conductive layer is at least twice as high as the modulus of the first and second non-conductive layers.

[0020] The modulus of the first and second non-conductive layers is in the range of 1,000 to 5,000 Pa·s.

[0021] The thermosetting resin composition of the conductive layer, the first and second non-conductive layers may include an epoxy resin.

[0022] It is also preferred that the thickness of the conductive layer does not exceed 2 μm relative to the average particle size of the conductive particles.

[0023] <Mode for carrying out the invention> The present invention can be modified in various ways and can have various embodiments, and a specific embodiment will be illustrated in the drawings and described in detail through detailed description. However, this is not intended to limit the present invention to a specific embodiment, and it should be understood that the present invention includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention. In addition, when describing the present invention, if it is determined that a specific description of related publicly known technology may make the gist of the present invention unclear, the detailed description will be omitted.

[0024] The present invention fixes the conductive particles with strong force through the high modulus of the polymer, minimizing the movement of the conductive particles during the compression process. In particular, the non-flowable conductive layer containing the conductive particles is formed through a semi-curing process to fix the conductive particles with the modulus force of the polymer resin, thereby minimizing the movement of the conductive particles when resin flow occurs due to pressure during the compression process. In addition, adhesive layers are formed on the upper and lower parts of the semi-cured polymer film layer to improve physical properties that are reduced by the semi-cured film, such as adhesive strength, reliability, and connection resistance, thereby optimizing the physical properties of the anisotropic conductive adhesive film.

[0025] The anisotropic conductive adhesive film according to the present invention can be manufactured by laminating a conductive layer having conductive particles dispersed therein and an adhesive non-conductive layer not containing conductive particles, wherein the conductive layer and the non-conductive layer are formed of a thermosetting resin composition, in which the conductive layer contains conductive particles and the non-conductive layer does not contain conductive particles.

[0026] The thermosetting resin compositions used in the conductive layer and the non-conductive layer may each contain a curable resin and a curing agent.

[0027] Here, the curable resin may be, but is not limited to, an epoxy resin, an acrylic resin, etc. For example, an epoxy resin such as a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a novolac type epoxy resin, or a modified epoxy resin may be used, and the acrylic resin may be, for example, an acrylic resin such as methyl acrylate, ethyl acrylate, isopropyl acrylate, isobutyl acrylate, epoxy acrylate, or ethylene glycol diacrylate.

[0028] As the curing agent, for example, a radical curing agent such as an organic peroxide, or a latent curing agent such as a sulfonium salt or an onium salt can be appropriately selected and used depending on the type of cured resin.

[0029] The thermosetting resin composition may further contain a phenoxy resin as a film-forming resin, and may further contain a coupling agent to improve adhesion to circuit members as necessary. The coupling agent is not particularly limited, and for example, an epoxy-based silane coupling agent, an acrylic-based silane coupling agent, etc. can be used to improve the connectivity and insulation of the anisotropic conductive adhesive film.

[0030] The conductive particles contained in the conductive layer are used to electrically connect the electrodes facing each other in the bonded body formed by bonding the circuit members, and although the conductive particles are not particularly limited, they are preferably 1 μm to 10 μm in size in order to connect the circuit members having a very fine pitch. The conductive particles may be conductive metal particles or particles in which the surface of resin particles is coated with a metal.

[0031] In the examples described below, 45 to 55 wt.% of epoxy resin was used as the thermosetting resin composition, 5 to 10 wt.% of 4-hydroxyphenylmethyl-1-naphthylmethylsulfonium was used as the initiator, and 10 to 15 wt.% of phenoxy resin was used as the film-forming resin, and 5 to 10 wt.% of nickel balls was used as the conductive particles.

[0032] The anisotropic conductive adhesive film according to the present invention is composed of a conductive layer and a non-conductive layer, and the conductive layer is formed by dispersing conductive particles in a thermosetting resin composition and then semi-curing the composition. The semi-cured conductive layer is electrically connected to the electrodes of the circuit member by flowing the polymer layer surrounding the conductive particles during the bonding process. FIG. 1 shows a cross section of the anisotropic conductive adhesive film according to the present invention. Here, the thickness of the conductive layer is preferably formed not to exceed 2 μm compared to the average particle size of the conductive particles. This is because if the thickness of the conductive layer exceeds 2 μm compared to the average particle size of the conductive particles, the semi-cured resin surrounding the surface of the conductive particles may remain on the surface of the conductive particles during the bonding process, and the pressure load applied to the conductive particles is reduced due to the large thickness of the conductive layer.

[0033] The conductive layer 110 is formed by dispersing conductive particles 130 in a thermosetting resin composition containing an epoxy resin as a curing resin and a curing agent, and then performing a semi-curing process by optimizing the thermal reaction time of the epoxy resin under a drying temperature condition of 50 to 100°C and a coating speed of about 1 to 5 m / min. The non-conductive layer 120 is formed using a thermosetting resin composition containing the same curing resin and curing agent as the conductive layer, and is laminated on the conductive layer that has completed the semi-curing process, and is manufactured using an anisotropic conductive adhesive film.

[0034] In the semi-curing process of the conductive layer, the thermosetting resin composition is applied onto the base film, and then the drying temperature conditions and coating speed in the drying section are adjusted to control the reaction time of the cured resin due to heat. Thus, the semi-cured state of the conductive layer can be confirmed by measuring the curing rate. In order to calculate the curing rate of the conductive layer 110, the heat capacity before and after semi-curing was measured using DSC (Differential Scanning Calorimetry). FIG. 2 shows a graph of the heat capacity measured before (initial heat value of the non-fluid layer) and after (heat value after drying of the non-fluid layer) the semi-curing process under a temperature increase condition of 10° C. per minute. Based on the heat capacity analysis results measured in this way, the curing rate was calculated according to the following [Equation 1].

[0035] [Formula 1] Cure rate (%) = [1-(initial heat value) / (heat value after semi-curing)] x 100

[0036] Each sample (conductive layer film sample) with a cure rate of 30 to 70% was laminated with a non-conductive layer under the same conditions to produce the final anisotropic conductive adhesive film, and then a bump area of ​​1500 μm was used to evaluate the physical properties of each anisotropic conductive adhesive film. 2 The bonding process was carried out on a chip including a circuit component with a pitch of 20 μm, and the capture rate and connection resistance were measured for each sample. The measurement results are shown in Table 1 below.

[0037] [Table 1]

[0038] As is clear from Table 1, when the cure rate is less than 40% (sample 1), the number of captured conductive particles decreases, causing a problem of increased connection resistance. When the cure rate exceeds 60% (sample 5), the connection resistance increases due to insufficient compression. Figure 3 shows the correlation between the capture rate and connection resistance with respect to the cure rate of the conductive layer confirmed in this example.

[0039] Figures 4 to 6 show the results of measuring the viscosity (unit: Pa s) of the conductive layer and non-conductive layer, respectively, using a rheometer machine in the temperature range of 25 to 200°C, when the cure rate of the conductive layer was 40% (Figure 4), 50% (Figure 5), and 60% (Figure 6) (measurement conditions: ramp rate: 10°C / min, angular frequency: 1.0 rad / s). The fluidity of each layer when the anisotropic conductive adhesive film was bonded was confirmed. As is clear from Figs. 4 to 6, the modulus (minimum melt viscosity) of the semi-cured conductive layer 110 increases depending on the curing rate, but if the curing rate is controlled to 40 to 60%, the modulus of the conductive layer can be adjusted to 10,000 to 50,000 Pa·s (it can be seen from Fig. 4 that the modulus of the conductive layer with a curing rate of 40% is 29,800 Pa·s, from Fig. 5 that the modulus of the conductive layer with a curing rate of 50% is 40,100 Pa·s, and from Fig. 6 that the modulus of the conductive layer with a curing rate of 60% is 49,905 Pa·s). In this case, the number of conductive particles that flow away without being involved in the contact between the electrodes due to the resin flow phenomenon that occurs in the bonding process can be minimized, and thus a stable connection resistance can be obtained. If the modulus of the conductive layer is less than 10,000 Pa·s, the resin has high flowability during main compression bonding, so that a large amount of conductive particles present between the electrodes will flow away. Furthermore, if the modulus of the conductive layer exceeds 50,000 Pa·s, the hardness of the resin increases, causing a problem that the compression effect is significantly reduced during main compression and the connection resistance is significantly increased. Furthermore, the modulus of the conductive layer is preferably at least twice as high as that of the non-conductive layer. When the modulus of the conductive layer is at least twice as high as that of the non-conductive layer, the loss of conductive particles due to resin flow in the non-conductive layer during the compression process can be minimized. Furthermore, the modulus (minimum melt viscosity) of the non-conductive layer is preferably within the range of 1,000 to 5,000 Pa·s (in this embodiment, the modulus of the non-conductive layer was confirmed to be 2,178 Pa·s. See Figures 4 to 6).If the modulus of the non-conductive layer is less than 1,000 Pa·s, air bubbles may be generated during the compression process due to high fluidity, and if it exceeds 5,000 Pa·s, the filling ability into the connection structure is reduced due to low fluidity.

[0040] From the viewpoint of the adhesive properties and reliability of the anisotropic conductive adhesive film, the non-conductive layers 120 arranged on the upper and lower parts, which embody the adhesive properties, can improve interlayer compatibility and increase reliability by using the same thermosetting resin as the conductive layer 110.

[0041] The high viscosity of the conductive layer can minimize the loss of conductive particles between the circuit electrodes. In the case of conventional anisotropic conductive adhesive films, the particle capture rate is about 30%, whereas the anisotropic conductive adhesive film according to the present invention can greatly improve the capture rate to a level of 40% to 60%. When using an anisotropic conductive adhesive film having such an improved capture rate, the electrical short circuit phenomenon caused by the flow of conductive particles in fine pitch connections and the resulting aggregation can be fundamentally solved. Therefore, since the same level of capture rate can be realized at fine pitches even if the content of expensive conductive particles is greatly reduced compared to conventional anisotropic conductive adhesive films by the amount of increase in particle capture rate, the manufacturing cost of the anisotropic conductive adhesive film can be greatly reduced.

[0042] In particular, in the case of anisotropic conductive adhesive films for COG and COP, fine pitch is required, so the planar connection cross-sectional area is designed to be narrow, and the number of conductive particles participating in conduction between the bump and the panel is small. Therefore, in the case of conventional anisotropic conductive adhesive films for COG and COP, the density of conductive particles is tens of thousands of pcs / mm 2 When the anisotropic conductive adhesive film according to the present invention is used in the connection structure of COG and COP, the conductive particle flow can be controlled remarkably even if the conductive particle content is significantly reduced, so that a stable number of conductive particles can be captured even at a low conductive density.

[0043] In addition, in the case of COG, the substrate has physical properties in which a rigid lower substrate is applied to an upper substrate having a chip structure, and in the case of COP, the substrate has physical properties in which a lower substrate having a film structure is applied to an upper substrate having a chip structure. In the present invention, a multi-layer structure is designed in which a conductive layer is interposed between two non-conductive layers, and non-conductive layers with different physical properties can be applied to the non-conductive layers disposed above and below the conductive layer, so that an anisotropic conductive adhesive film optimized for substrates with different structures can be provided.

[0044] The anisotropic conductive adhesive film according to the present invention can be manufactured as follows. As is clear from FIG. 7, a thermosetting resin composition in which conductive particles are dispersed is coated on a first release film 210, and then semi-cured so that the curing rate according to Equation 1 measured using differential scanning calorimetry is 40% or more and 60% or less to form a non-fluid conductive layer 110. At this time, the thickness of the conductive layer 110 is formed to a thickness not exceeding 2 μm from the average particle size of the conductive particles. Next, a thermosetting resin composition not containing conductive particles is coated on a second release film 220 to form a first adhesive non-conductive layer 121. Similarly, a thermosetting resin composition not containing conductive particles is coated on a third release film 230 to form a second adhesive non-conductive layer 122. Then, the first adhesive non-conductive layer 121 is laminated on the upper part (above) of the non-fluid conductive layer 110 through a lamination process. Then, after removing the first release film 210, the second adhesive non-conductive layer 122 is laminated on the lower part (bottom) of the exposed non-fluid conductive layer 110 through a lamination process.

[0045] The process of forming the non-fluid conductive layer and the process of laminating the first and second adhesive non-conductive layers are not limited to the above-mentioned process order, and the anisotropic conductive adhesive film can be formed by performing a single lamination process using a film with a non-fluid conductive layer formed in advance, a film with a first adhesive non-conductive layer formed, and a film with a second adhesive non-conductive layer formed, as is clear from Fig. 8. In addition, after removing either one of the second release film and the third release film, the final product can be manufactured as a roll-shaped product.

[0046] Although the preferred embodiment of the present invention has been described above, those skilled in the art may embody the present invention in modified forms without departing from the essential characteristics of the present invention. Therefore, the embodiments of the present invention described herein should be considered in an illustrative rather than a restrictive sense, and the scope of the present invention is set forth in the claims, not in the above description, and all differences within the scope of the equivalents thereto should be understood to be included in the present invention.

Claims

1. A first step of forming a non-fluid conductive layer by coating a thermosetting resin composition having conductive particles dispersed therein on a first release film and semi-curing the composition so that the curing rate is 40% or more and 60% or less according to the following formula 1 measured by differential scanning calorimetry; A second step of coating a thermosetting resin composition not containing conductive particles on a second release film to form a first adhesive non-conductive layer; A third step of coating a thermosetting resin composition not containing conductive particles on the third release film to form a second adhesive non-conductive layer; a fourth step of laminating the first adhesive non-conductive layer on the non-flowable conductive layer through a lamination process; and a fifth step of removing the first release film and then laminating the second adhesive non-conductive layer on the exposed lower part of the non-fluid conductive layer through a lamination process. [Formula 1] Cure rate (%) = [1 - (initial heat value) / (heat value after semi-curing)] x 100

2. 2. The method for producing an anisotropic conductive adhesive film according to claim 1, wherein the modulus of the conductive layer is 10,000 to 50,000 Pa·s.

3. 2. The method for producing an anisotropic conductive adhesive film according to claim 1, wherein the modulus of the conductive layer is at least twice as high as the modulus of the first and second non-conductive layers.

4. 2. The method for producing an anisotropic conductive adhesive film according to claim 1, wherein the modulus of the first and second non-conductive layers is within a range of 1,000 to 5,000 Pa·s.

5. 2. The method for producing an anisotropic conductive adhesive film according to claim 1, wherein the thermosetting resin composition of the conductive layer and the first and second non-conductive layers contains an epoxy resin.

6. 2. The method for producing an anisotropic conductive adhesive film according to claim 1, wherein the thickness of the conductive layer is not more than 2 μm compared to the average particle size of the conductive particles.

Citation Information

Patent Citations

  • Adhesive film and method of manufacturing adhesive film

    JP2005200521A

  • Electric connecting material

    JP2015079603A