Conductive contact structure for solar cell, solar cell module and power generation system

A conductive contact structure with a seed layer alloy enhances bonding and light confinement in solar cells, addressing copper peeling and diffusion issues, and improving performance.

JP2024536519AActive Publication Date: 2024-10-04SOLARLAB AIKO EUROPE GMBH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024522471
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-03-11
Filing Date
2022-06-21
Publication Date
2024-10-04
Estimated Expiration
2042-06-21

AI Technical Summary

Technical Problem

The bonding strength between copper and silicon substrates in solar cells is insufficient, leading to peeling and copper diffusion, which deteriorates cell performance, and existing nickel seed layers provide inadequate bonding and poor light reflection.

Method used

A conductive contact structure with a seed layer composed of an alloy material, including a main component with an average refractive index less than 2 and a wavelength range of 850 to 1200 nm, and reinforcing components like Mo, Ni, Ti, W, Cr, Mn, Pd, Bi, Nb, Ta, Pa, Si, and V, enhances bonding and improves light confinement.

Benefits of technology

The seed layer provides strong bonding between the conductive layer and substrate, reducing copper diffusion and enhancing light confinement, thereby improving solar cell efficiency and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536519000001_ABST
    Figure 2024536519000001_ABST
Patent Text Reader

Abstract

The present invention provides a conductive contact structure for a solar cell, comprising: a substrate; a semiconductor region; and an electrode, the semiconductor region being disposed on or within the substrate; the electrode being disposed within the semiconductor region; the electrode comprising a seed layer in contact with the semiconductor region; the seed layer comprising an alloy material, the seed layer comprising a main component and a reinforcing component, the main component being one or more metals having an average refractive index of less than 2 and a wavelength range of 850-1200 nm, and the reinforcing component being any one or more of Mo, Ni, Ti, W, Cr, Mn, Pd, Bi, Nb, Ta, Pa, Si, and V.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of solar cells, and in particular to a conductive contact structure for a solar cell, a solar cell module and a power generation system. [Background technology]

[0002] In solar cells, as shown in Fig. 2, a copper layer 100 is usually used as a conductive layer covering a silicon substrate 200, but the bonding strength between copper and silicon is insufficient, so the conductive layer is easily peeled off from the silicon substrate, and the copper in the conductive layer diffuses into the silicon substrate, which reduces the performance of the solar cell. To solve this problem, the prior art adds a seed layer 300 between the copper conductive layer and the silicon substrate to strengthen the bonding strength between the copper conductive layer 100 and the silicon substrate 200. The seed layer is usually a nickel layer, which strengthens the bonding strength between the copper conductive layer and the silicon substrate, but the strengthening effect is not ideal, and the light reflection effect of the nickel layer is poor, which reduces the light trapping effect of the solar cell. Summary of the Invention

[0003] The present invention aims to strengthen the bonding strength between a conductive layer and a substrate and improve the light trapping effect of a solar cell, and provides a conductive contact structure for a solar cell, a solar cell module and a power generation system.

[0004] To achieve this objective, the present invention adopts the following technical solutions:

[0005] A conductive contact structure for a solar cell is provided, the conductive contact structure for the solar cell comprising: A substrate; A semiconductor region; an electrode; the semiconductor region is disposed on or within the substrate; the electrode is disposed within the semiconductor region; the electrode includes a seed layer in contact with the semiconductor region; The seed layer comprises an alloy material and includes a main component and a reinforcing component, the main component being one or more metals having an average refractive index of less than 2 and a wavelength range of 850 to 1200 nm, and the reinforcing component being one or more of Mo, Ni, Ti, W, Cr, Mn, Pd, Bi, Nb, Ta, Pa, Si, and V.

[0006] In one class of this embodiment, the primary component comprises any one or more of Al, Ag, Cu, and Mg.

[0007] In one class of this embodiment, the reinforcing component may further comprise a non-metallic component.

[0008] In one class of this embodiment, the major component is present in an amount greater than 50 wt.% of the seed layer.

[0009] In one class of this embodiment, the primary component is Al in an amount equal to or greater than 70 wt.% of the seed layer, and the reinforcing component is Ni in an amount equal to or less than 30 wt.% of the seed layer.

[0010] In one class of this embodiment, the major component is Al in an amount equal to or greater than 70 wt.% of the seed layer, and the reinforcing component is W in an amount equal to or less than 30 wt.% of the seed layer.

[0011] In one class of this embodiment, the major component is Al in an amount equal to or greater than 70 wt.% of the seed layer, and the reinforcing component is Ti in an amount equal to or less than 30 wt.% of the seed layer.

[0012] In one class of this embodiment, the major component is Al in an amount equal to or greater than 70 wt.% of the seed layer, and the reinforcing component is Mo in an amount equal to or less than 30 wt.% of the seed layer.

[0013] In one class of this embodiment, the primary component is Al and comprises 70 wt.% or more of the seed layer, and the reinforcing component is Cr and comprises 30 wt.% or less of the seed layer. In one class of this embodiment, the primary component is Al and comprises 70 wt.% or more of the seed layer, and the reinforcing component is Si and comprises 30 wt.% or less of the seed layer.

[0014] In one class of this embodiment, the seed layer is formed on the substrate by any one of the following manufacturing methods: physical vapor deposition, screen printing, chemical vapor deposition, electroplating, or chemical plating.

[0015] In one class of this embodiment, the electrode further includes a conductive layer disposed above the seed layer.

[0016] In one class of this embodiment, the conductive layer comprises any one or more of Cu, Ag, and Al.

[0017] In one class of this embodiment, a passivation film is formed between the seed layer and the semiconductor region, an opening is provided in the passivation film, and the seed layer contacts the semiconductor region through the opening.

[0018] In one class of this embodiment, a transparent conductive oxide (TCO) thin film is further provided between the seed layer and the passivation film, the TCO thin film contacting the semiconductor region through the opening in the passivation film.

[0019] In one class of this embodiment, the TCO thin film is a tin-doped indium oxide or zinc oxide based thin film.

[0020] In one class of this embodiment, the semiconductor region includes a tunnel oxide layer and doped polysilicon.

[0021] In one class of this embodiment, the method of growing the conductive layer on the seed layer includes electroplating, physical vapor deposition, screen printing, or chemical plating.

[0022] In one class of this embodiment, the top of the conductive layer is covered with a protective layer.

[0023] In one class of this embodiment, the protective layer is a Sn layer or an Ag layer.

[0024] In one class of this embodiment, the protective layer is grown on the conductive layer by electroplating or chemical plating methods.

[0025] In one class of this embodiment, the substrate is a silicon substrate.

[0026] In one class of this embodiment, the seed layer is comprised of a plurality of sub-seed layers stacked together.

[0027] In one class of this embodiment, the content of the major component in the subseed layers deposited in a direction away from the substrate gradually decreases.

[0028] In one class of this embodiment, the seed layer has a thickness in the range of 10 nm to 1000 nm.

[0029] In one class of this embodiment, the seed layer has a thickness in the range of 30 nm to 300 nm.

[0030] In one class of this embodiment, the conductive layer has a thickness in the range of 1 μm to 800 μm.

[0031] In one class of this embodiment, the conductive layer has a thickness in the range of 1 μm to 100 μm.

[0032] The present invention further provides a solar cell comprising the conductive contact structure described above.

[0033] The present invention further provides a solar cell module including a plurality of solar cells electrically connected to one another.

[0034] The present invention further provides a photovoltaic power generation system including a plurality of solar cell modules electrically connected to each other.

[0035] The present invention adds a seed layer between the conductive layer and the substrate, the seed layer comprising an alloy material, the main component of which is one or more metals having an average refractive index of less than 2 and a wavelength range of 850 to 1200 nm, and the reinforcing component is one or more of Mo, Ni, Ti, W, Cr, Si, Mn, Pd, Bi, Nb, Ta, Pa, or V. The seed layer formed by the fusion of the main component and the reinforcing component has a strong bond with both the conductive layer and the substrate, and improves the light trapping effect of the solar cell. [Brief description of the drawings]

[0036] In the following, in order to more clearly describe the technical solutions of the embodiments of the present invention, the drawings used in the embodiments of the present invention will be briefly described. Obviously, the drawings described below are only some embodiments of the present invention, and those skilled in the art can think of other drawings from these drawings without creative efforts.

[0037] [Figure 1] 2 is a schematic diagram of a conductive contact structure of a solar cell according to an embodiment of the present invention; [Diagram 2] FIG. 1 is a schematic diagram of a conductive contact structure of a solar cell in the prior art. [Diagram 3] FIG. 1 is a comparison diagram of the diffusion coefficients of Cu and other metals. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0038] The technical solutions of the present invention are further described below through specific embodiments with reference to the drawings.

[0039] Here, the drawings are merely for illustrative purposes, are merely schematic diagrams rather than actual drawings, and should not be understood as limiting the present invention. In order to better explain the embodiments of the present invention, the drawings may omit, enlarge, or reduce some components, do not show the dimensions of the actual products, and those skilled in the art can understand that some of the known structures and their descriptions in the drawings may be omitted.

[0040] The same or similar reference numerals in the drawings of the embodiments of the present invention correspond to the same or similar components. In the description of the present invention, it should be understood that the orientation or positional relationship indicated by the terms "up", "down", "left", "right", "inside", "outside", etc. is the orientation or positional relationship indicated based on the drawings, and is merely for the purpose of easily explaining the present invention and simplifying the description, and does not expressly or imply that the described devices or elements necessarily have a specific orientation, or are configured or operated in a specific orientation, so the terms describing the positional relationship in the drawings are merely for illustrative purposes and should not be understood as limiting the present invention, and a person skilled in the art can understand the specific meaning of the above terms according to the specific situation.

[0041] In the description of the present invention, unless otherwise clearly defined or limited, when a term indicating a connection relationship between members such as "connect" appears, the term should be understood in a broad sense, for example, it may be a fixed connection, a removable connection, or an integral connection, it may be a mechanical connection, an electrical connection, a direct connection, or even an indirect connection via an intermediate medium, or it may be an internal communication between two members or an interaction relationship between two members. Those skilled in the art can understand the specific meaning of the above terms in the present invention according to the specific situation.

[0042] The conductive contact structure of a solar cell provided in the embodiment of the present invention is as shown in FIG. A substrate 1; A semiconductor region disposed on or within a substrate 1; an electrode 100 disposed within the semiconductor region; The electrode includes a seed layer 2 in contact with the semiconductor region; The seed layer 2 includes an alloy material, and includes a main component and a reinforcing component, the main component being one or more metals having an average refractive index of less than 2 and a wavelength range of 850 to 1200 nm (preferably one or more of Al (aluminum), Ag (silver), Cu (copper), or Mg (magnesium)), and the reinforcing component being one or more of Mo (molybdenum), Ti (titanium), W (tungsten), Ni (nickel), Cr, Si, Mn, Pd, Bi, Nb, Ta, Pa, or V. The content of the main component in the seed layer is preferably >50%. More preferably, the main component of the seed layer is Al and the content is 70 wt.% or more of the seed layer, and the reinforcing component is Ti and the content is 30 wt.% or less of the seed layer, or the main component is Al and the content is 70 wt.% or more of the seed layer, and the reinforcing component is W and the content is 30 wt.% or less of the seed layer, or the main component is Al and the content is 70 wt.% or more of the seed layer, and the reinforcing component is Ti and the content is 30 wt.% or less of the seed layer, or the main component is Al and the content is 70 wt.% or more of the seed layer, and the reinforcing component is Mo and the content is 30 wt.% or less of the seed layer.

[0043] Currently, mass-produced crystalline silicon solar cells use Ag paste as the electrode material, and the cost of Ag paste accounts for nearly 30% of the non-silicon cost of the cell. By reducing the amount of Ag used or not using Ag production technology, the production cost of solar cells can be effectively reduced. Among them, Cu is a good substitute for Ag. The advantages of using Cu as a conductive material compared to Ag are shown in Table 1 below.

[0044] [Table 1]

[0045] From Table 1 above, we can see that Cu is an effective substitute for Ag, due to its excellent properties, such as relatively stable chemical properties, excellent ductility, sufficiently low volume resistivity, large availability and low cost (nearly 1 / 72 of the price of Ag material). However, Cu has two important characteristics that limit its application in solar cells, one of which is that the diffusion coefficient of Cu is too large. Figure 3 is a schematic diagram of the diffusion coefficients of common metals, where the abscissa and ordinate represent the inverse of temperature (unit: Kelvin K) and the diffusion coefficient of metal elements, respectively. From Figure 3, it is clear that the diffusion coefficient of Cu is much higher than other metals, and is five orders of magnitude higher than Ag / Al, etc.

[0046] Secondly, Cu defects have a large collection cross section for holes, which significantly shortens the bulk lifetime and further reduces the electrical performance of the solar cell. The effects of Cu content on bulk lifetime and electrical performance are shown in Table 2 below.

[0047] [Table 2]

[0048] From Table 2 above, it can be seen that as the Cu content increases, the bulk lifetime is significantly shortened and the cell efficiency is also significantly reduced. 3 If only one electrode is used, the efficiency of the battery drops by 0.29%.

[0049] In the prior art, Ni (nickel) is usually used as a barrier layer for Cu diffusion, and can adhere well to the substrate and Cu electrode, and the general procedure for its realization is: prepare a coated substrate-laser cut-out-Ni electroplating-Cu layer electroplating. However, the inventors found in the course of their research that Ni has a major defect as a barrier layer for Cu, which is that it has poor reflection effect in the long wavelength range, which reduces the light trapping effect of the cell, and further reduces the conversion efficiency of the cell.

[0050] Please refer to Table 3 below for comparative data on the optical performance of batteries using Ni+Cu and Ag as electrode materials.

[0051] [Table 3]

[0052] From Table 3 above, we can see that the combination of Ni+Cu significantly reduces the short circuit current density of the battery. Simulation results show that the short circuit current density is 0.75mA / cm 2 However, experimental results showed that the short circuit current density was 1.36mA / cm 2 decline, and is greater than theoretically predicted.

[0053] In the following, the light trapping effect of common metals is analyzed.

[0054] Currently, the thickness of the silicon wafer of the finished battery is about 150 μm, and photons with a wavelength of >850 nm can effectively penetrate this thickness. At the same time, since the forbidden band width of Si is 1.12 eV, photons with a wavelength of >1200 nm are unlikely to excite electron-hole pairs. Therefore, when considering the light confinement effect, the inventors mainly focus on the wavelength band of 850 to 1200 nm. Table 4 below shows the interface reflectance of different metals and the market price as of February 2022.

[0055] [Table 4]

[0056] From Table 4 above, it is clear that there is a large difference in interface reflectance between different metals. Among them, Ag / Al / Cu / Mg, the four metals, can obtain relatively ideal short circuit current density results, and when used as a seed layer, they can all form an effective light trapping effect. Further analysis shows that Cu cannot be used as a seed layer, because one of the important roles of the seed layer is to block Cu, Mg is also not a preferred choice because its chemical properties are too active, and Ag is also not a preferred choice because of its high price, while Al has excellent back reflectance effect, is relatively stable in chemical properties, and is inexpensive, only 1 / 223 of Ag and 1 / 3 of Cu, making it an ideal seed layer metal.

[0057] However, using pure Al metal as a seed layer creates another problem: the adhesion between Al and other metals is weak. The technology of using pure Al as a seed layer will result in products that do not meet reliability standards. When the product is subjected to thermal cycling or flexing, or due to stress at the welding points during welding of the parts, both of these can cause separation between the Al and the outer layer metal, resulting in delamination and causing failures.

[0058] The bonding strength between Al and Cu is weak, which is prone to causing large-area finger detachment. To solve this problem, the inventors have tried various improvement methods, such as increasing the contact area between Al and substrate, increasing the temperature of the sample to promote interdiffusion between metals, and sandwiching a new material such as TiW between the Al / Cu materials, but none of the effects are ideal. Finally, they found that by adding a reinforcing component that can form a good interconnection with Cu to the Al material as a seed layer, a good bond between the seed layer / electroplating layer can be formed without even needing an additional annealing treatment after Cu electroplating, and the adhesion of the electroplating layer can be greatly improved, and finally, the problem has been solved.

[0059] Reinforcing elements such as Ni, Mo, Ti, W, Cr, Mn, Pd, Bi, Nb, Ta, Pa, Si, and V significantly enhance adhesion.

[0060] In addition, Ni, Mo, Ti, W, Cr, Mn, Pd, Bi, Nb, Ta, Pa, and Si have low reflectivity. Excessive addition of materials may degrade optical performance. Here, taking W as an example, we simply assume that the performance of the alloying elements is the reinforcement average value of the elements, and obtain the estimated results shown in Table 5 below.

[0061] [Table 5]

[0062] Here, when the W content is 30%, the current loss is 0.36 mA / cm 2 This results in a decrease in the cell conversion efficiency of about 0.2%, which is relatively large, but considering the cost reduction achieved by substituting Cu for Ag and the solution to the reliability problem, it is worth accepting. Therefore, it is recognized that a reinforcing component of 30 wt.% or less in the seed layer is the recommended value.

[0063] In addition, the proportion of the reinforcing component in the seed layer of the present invention may be distributed unevenly, and thus more favorable performance effects can be obtained, the principle of which is that by reducing the content of the reinforcing component in the part close to the substrate, the light reflection can be enhanced, and by containing a relatively large amount of the reinforcing component in the part in contact with the conductive layer metal, the bonding strength with the conductive layer metal can be improved.

[0064] Table 6 below compares the weld pull forces for different electrode technologies.

[0065] [Table 6]

[0066] From Table 6 above, it can be seen that the finger tensile strength of the pure Al seed layer is relatively low, much lower than that of ordinary Ag electrodes, but after the TiW material is directly sandwiched between Al and Cu, the welding tensile strength is improved but still insufficient, whereas the solar cell manufactured with the Al alloy seed layer in the present invention has a higher welding tensile strength than that of ordinary Ag electrodes.

[0067] Al is used as the main component to improve the adhesion between the seed layer and the Cu conductive layer and the light trapping effect of the solar cell. Table 7 shows the data of the technical effects that can be brought about by the combination of each single reinforcing component with the main component Al.

[0068] [Table 7]

[0069] As can be seen from the above experimental data, Cr, Mn, Pd, Bi, Nb, Ta, Pa, Si, and V can also be used as reinforcing components to improve the adhesion between the seed layer and the Cu conductive layer and the light trapping effect of the solar cell. It should be emphasized that any one or more of the reinforcing components Mo, Ni, Ti, W, Cr, Mn, Pd, Bi, Nb, Ta, Pa, Si, and V can be combined with Al in hundreds of combinations, and it is impossible to provide experimental comparison data for all components in the present invention. Therefore, on the premise that the experimental data of Ni, Mo, Ti, W, Cr, Mn, Pd, Bi, Nb, Ta, Pa, Si, and V as individual reinforcing components are given in a specific implementation, it is obvious that other reinforcing components combined with the main component Al can also achieve the desired technical effect.

[0070] Furthermore, the thickness of the seed layer is preferably ≧30 nm. Experiments have shown that a seed layer with a thickness of 30 nm is sufficient to prevent the diffusion of Cu metal. When the thickness is ≦300 nm, the main factor to be considered is cost reduction. For example, even if the seed layer is manufactured using a physical vapor deposition method and the price of Al is lower than other metals, the impact of the cost of the Al target material is still not negligible. In addition, the thicker the seed layer, the lower the production capacity of the equipment, which is unfavorable to the popularization of large-scale production. Therefore, the thickness of the seed layer is preferably 30 nm to 300 nm.

[0071] Furthermore, in order to save the cost of alloy target material and further limit the diffusion of Cu metal into the substrate, a transparent conductive oxide (TCO) layer can be added between the alloy seed layer and the substrate, so that the long wavelength light can be transmitted through the TCO layer and effectively reflected at the alloy layer interface, thus also achieving ideal performance and reliability results.

[0072] In the above-mentioned solution, the seed layer is preferably formed on the substrate by any one of physical vapor deposition (including sputtering and deposition), screen printing, chemical vapor deposition, electroplating, and chemical plating. The seed layer is preferably formed by stacking a plurality of subseed layers, and more preferably, the content of the main component in the subseed layers stacked in the direction away from the substrate is gradually reduced, and the high content of the main component in the subseed layer close to the substrate can enhance the light reflection effect and improve the light trapping effect of the solar cell, and the high content of the reinforcing component and the relatively low content of the main component in the subseed layer farther from the substrate (closer to the conductive layer) can ensure the bonding strength between the subseed layer and the conductive layer.

[0073] The thickness of the seed layer is preferably in the range of 10 nm to 1000 nm, and more preferably in the range of 30 nm to 300 nm.

[0074] The electrode provided in this embodiment further includes a conductive layer 3 disposed above the seed layer 2, as shown in FIG. 1. The material for manufacturing the conductive layer 3 includes any one or more of Cu, Ag, and Al. The method for growing the conductive layer on the seed layer includes electroplating, physical vapor deposition, screen printing, or chemical plating. The thickness of the conductive layer is preferably in the range of 1 to 800 μm, more preferably in the range of 1 to 100 μm.

[0075] In order to protect the conductive layer, the top of the conductive layer is preferably covered with a protective layer 4. More preferably, the protective layer 4 is a Sn layer or an Ag layer. The protective layer 4 is preferably grown on the conductive layer 3 by electroplating or chemical plating.

[0076] 1, a passivation film 6 for protecting the seed layer 2 is preferably formed between the seed layer 2 and the semiconductor region, an opening 7 is provided in the passivation film 6, and the seed layer 2 contacts the semiconductor region through the opening. More preferably, a TCO thin film is further disposed between the seed layer 2 and the passivation film 6, and the TCO thin film contacts the semiconductor region through the opening in the passivation film. The semiconductor region preferably includes a tunnel oxide layer 5 and doped polysilicon 8.

[0077] As described above, the present invention adds a seed layer between the conductive layer and the substrate, and the seed layer contains an alloy material, whose main component is one or more metals having an average refractive index of less than 2 and a wavelength range of 850 to 1200 nm, and whose reinforcing component is one or more of Mo, Ni, Ti, W, Cr, Si, Mn, Pd, Bi, Nb, Ta, Pa, or V. The seed layer formed by the fusion of the main component and the reinforcing component has a strong bonding force with both the conductive layer and the substrate, and improves the light trapping effect of the solar cell.

[0078] Embodiments of the present invention further provide a solar cell including the conductive contact structure described above.

[0079] An embodiment of the present invention further provides a solar cell module including a plurality of solar cells electrically connected to each other and having the above-described conductive contact structures.

[0080] An embodiment of the present invention further provides a photovoltaic power generation system including a plurality of solar cell modules electrically connected to each other.

[0081] It should be explained that the above-mentioned specific embodiment is merely a preferred embodiment of the present invention and the technical principle applied thereto. It is obvious to those skilled in the art that various modifications, equivalent replacements, changes, etc. can be made to the present invention. However, as long as these transformations do not deviate from the spirit of the present invention, they are all included in the protection scope of the present invention. In addition, some terms used in the specification and claims of this application are merely for the purpose of facilitating the description and are not limiting.

Claims

1. A substrate; A semiconductor region; An electrode; 1. A conductive contact structure for a solar cell comprising: the semiconductor region is disposed on or within the substrate; the electrode is disposed within the semiconductor region; the electrode includes a seed layer in contact with the semiconductor region; The seed layer comprises an alloy material and includes a main component and a reinforcing component, the main component being one or more metals having an average refractive index of less than 2 and a wavelength range of 850 to 1200 nm, and the reinforcing component being any one or more of Mo, Ni, Ti, W, Cr, Mn, Pd, Bi, Nb, Ta, Pa, Si, and V.

2. The conductive contact structure of claim 1 , wherein the main components include any one or more of Al, Ag, Cu, and Mg.

3. The conductive contact structure for a solar cell according to claim 1 or 2, wherein the reinforcing component further comprises a non-metallic component.

4. 3. The conductive contact structure for a solar cell according to claim 1, wherein the content of the main component is more than 50 wt. % of the seed layer.

5. 2. The conductive contact structure of claim 1, wherein the main component is Al and the content is 70 wt. % or more of the seed layer, and the reinforcing component is Ni and the content is 30 wt. % or less of the seed layer.

6. 2. The conductive contact structure of claim 1, wherein the main component is Al and the content is 70 wt. % or more of the seed layer, and the reinforcing component is W and the content is 30 wt. % or less of the seed layer.

7. 2. The conductive contact structure of claim 1, wherein the main component is Al and the content is 70 wt. % or more of the seed layer, and the reinforcing component is Ti and the content is 30 wt. % or less of the seed layer.

8. 2. The conductive contact structure of claim 1, wherein the main component is Al and the content is 70 wt. % or more of the seed layer, and the reinforcing component is Mo and the content is 30 wt. % or less of the seed layer.

9. 2. The conductive contact structure of claim 1, wherein the main component is Al and the content is 70 wt. % or more of the seed layer, and the reinforcing component is Cr and the content is 30 wt. % or less of the seed layer.

10. 2. The conductive contact structure of claim 1, wherein the main component is Al and the content is 70 wt. % or more of the seed layer, and the reinforcing component is Si and the content is 30 wt. % or less of the seed layer.

11. The conductive contact structure of a solar cell as described in claim 1, wherein the seed layer is formed on the substrate by using a physical vapor deposition manufacturing method, or a screen printing manufacturing method, or a chemical vapor deposition manufacturing method, or an electroplating manufacturing method, or a chemical plating manufacturing method.

12. The conductive contact structure of claim 1 , wherein the electrode further comprises a conductive layer disposed over the seed layer.

13. 13. The conductive contact structure of claim 12, wherein the conductive layer comprises any one or more of Cu, Ag, and Al.

14. The conductive contact structure of a solar cell according to claim 1 , wherein a passivation film is formed between the seed layer and the semiconductor region, an opening is provided in the passivation film, and the seed layer contacts the semiconductor region through the opening.

15. 15. The conductive contact structure of claim 14, further comprising a transparent conductive oxide (TCO) thin film disposed between the seed layer and the passivation film, the TCO thin film contacting the semiconductor region through the opening in the passivation film.

16. 16. The conductive contact structure of claim 15, wherein the TCO thin film is a tin-doped indium oxide or zinc oxide based thin film.

17. 2. The conductive contact structure of claim 1, wherein said semiconductor region comprises a tunnel oxide layer and doped polysilicon.

18. The conductive contact structure of claim 12 , wherein the method of growing the conductive layer on the seed layer includes electroplating, physical vapor deposition, screen printing, or chemical plating.

19. The conductive contact structure for a solar cell of claim 1 , wherein the conductive layer is covered with a protective layer.

20. 20. The conductive contact structure of claim 19, wherein the protective layer is a Sn layer or an Ag layer.

21. 21. The conductive contact structure for a solar cell according to claim 19 or 20, wherein said protective layer is grown on said conductive layer by electroplating or chemical plating method.

22. The conductive contact structure for a solar cell according to claim 1 , wherein the substrate is a silicon substrate.

23. The conductive contact structure for a solar cell according to claim 1 , wherein the seed layer is formed by stacking a plurality of sub-seed layers.

24. 24. The conductive contact structure of claim 23, wherein the content of the major component in the subseed layer decreases along a direction away from the substrate.

25. 24. The conductive contact structure for a solar cell of claim 23, wherein the seed layer has a thickness in the range of 10 nm to 1000 nm.

26. 24. The conductive contact structure for a solar cell of claim 23, wherein the seed layer has a thickness in the range of 30 nm to 300 nm.

27. The conductive contact structure for a solar cell according to claim 12, wherein the thickness of the conductive layer is in the range of 1 μm to 800 μm.

28. The conductive contact structure for a solar cell according to claim 12, wherein the thickness of the conductive layer is in the range of 1 μm to 100 μm.

29. A solar cell comprising the conductive contact structure of any one of claims 1 to 28.

30. 30. A solar cell module comprising a plurality of the solar cells of claim 29 electrically connected to each other.

Citation Information

Patent Citations

  • Ceramic base copper -clad plate

    CN206790778U

  • Metal contact structure and manufacturing method for solar cells

    JP2006523025A

  • Solar battery cell and manufacturing method thereof

    JP2008004574A

  • Back-surface electrode for compound semiconductor thin-film solar battery, solar battery, and sputtering target for manufacturing the back-surface electrode