High Loft Nonwoven Fabric
The use of crimped bicomponent fibers with polypropylene, polyethylene, and a copolymer in nonwoven fabrics addresses the issue of loft and thickness, enhancing comfort and fluid distribution in hygiene products.
Patent Information
- Application Number
- JP2024523124
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-18
- Filing Date
- 2022-10-18
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional nonwoven fabrics lack loft and thickness in the z-direction, which affects user comfort and fluid distribution in hygiene-related products.
A nonwoven fabric comprising crimped bicomponent fibers made from a combination of polypropylene, polyethylene, and a polypropylene-polyethylene copolymer, formed through melt spinning and crimping processes to enhance loft and thickness.
The crimped bicomponent fibers provide a high-loft, low-density fabric that improves user comfort and fluid distribution in hygiene products by increasing thickness and reducing density.
Smart Images

Figure 2024536545000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority under 35 U.S.C. §119(e) to U.S. Provisional Application No. 63 / 256,796, filed October 18, 2021, which is specifically incorporated by reference in its entirety.
[0002] Inventive embodiments of the present disclosure generally relate to a nonwoven fabric having a plurality of crimped bicomponent fibers having a first component comprising a first polymeric material comprising a first polymer or a first polymer blend and a second component comprising a second polymeric material, wherein the second polymeric material comprises a second polymer blend of (i) at least one polypropylene polymer, (ii) at least one polyethylene polymer, and (iii) at least one compatibilizer comprising or consisting of at least one polypropylene-polyethylene copolymer. [Background technology]
[0003] In nonwoven fabrics, the fibers forming the nonwoven fabric are generally oriented in the xy plane of the web. Thus, the resulting nonwoven fabric is relatively thin and lacks loft or significant thickness in the z direction. The loft or thickness of nonwoven fabrics suitable for use in hygiene-related molded articles (e.g., personal care absorbents) promotes user comfort (softness), spillage management, and fluid distribution to adjacent components of the molded article. In this regard, high-loft, low-density nonwoven fabrics are used for various end-use applications, such as hygiene-related products (e.g., sanitary pads and napkins, disposable diapers, incontinence care pads, etc.). High-loft and low-density nonwoven fabrics can be used in products such as towels, industrial wipes, incontinence products, baby care products (e.g., diapers), feminine absorbent care products, and commercial health care molded articles. Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made to solve the problems in the conventional techniques described above. [Means for solving the problem]
[0005] One or more embodiments of the present invention may address one or more of the problems described above. Certain embodiments according to the present invention provide a nonwoven fabric comprising a plurality of crimped bicomponent fibers having a first component comprising a first polymer material comprising a first polymer or a first polymer blend and a second component comprising a second polymer material, wherein the second polymer material comprises a second polymer blend of (i) at least one polypropylene polymer, (ii) at least one polyethylene polymer, and (iii) at least one compatibilizer comprising or consisting of at least one polypropylene-polyethylene copolymer.
[0006] In another embodiment, the present invention provides a method of making a nonwoven fabric, which may include: (a) forming a first polymer melt comprising a first polymer or a first polymer blend, (b) forming a second polymer melt comprising a second polymer blend of (i) at least one polypropylene polymer, (ii) at least one polyethylene polymer, and (iii) at least one compatibilizer comprising a polypropylene-polyethylene copolymer, (c) forming a plurality of bicomponent fibers by melt spinning the first polymer melt and the second polymer melt through a bicomponent spinneret pack, (d) allowing the plurality of bicomponent fibers to crimp prior to or during deposition on a collecting surface or subjecting the plurality of bicomponent fibers to a crimping process to provide a plurality of crimped bicomponent fibers, and (e) consolidating the plurality of crimped bicomponent fibers to form a nonwoven fabric.
[0007] In another aspect, the present invention provides a method of making a nonwoven fabric, which may include: (a) forming a first polymer melt comprising a first polymer or a first polymer blend, (b) forming a second polymer melt comprising a second polymer blend of (i) at least one polypropylene polymer, (ii) at least one polyethylene polymer, and (iii) at least one compatibilizer comprising a polypropylene-polyethylene copolymer, (c) forming a plurality of bicomponent fibers by melt spinning the first polymer melt and the second polymer melt through a bicomponent spinneret pack, (d) consolidating the plurality of bicomponent fibers to form an intermediate nonwoven fabric, and (e) subjecting the plurality of bicomponent fibers of the intermediate nonwoven fabric to a crimping process to provide a nonwoven fabric.
[0008] In yet another aspect, the present invention provides a shaped article comprising one or more of the nonwoven fabrics described and disclosed herein. The shaped article may comprise an adult diaper, a baby diaper, a pull-up, or of a feminine hygiene pad. According to certain embodiments of the present invention, the shaped article may comprise a topsheet comprising the nonwoven fabrics described and disclosed herein.
[0009] The present invention will now be described more fully hereinafter with reference to the accompanying drawings, in which some, but not all, embodiments of the invention are shown. Indeed, the invention may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will satisfy applicable legal requirements. Like numbers will refer to like elements throughout. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 illustrates a crimped bicomponent fiber according to certain embodiments of the present invention. [Diagram 2]2A-2H illustrate example cross-sectional images of some example bicomponent fibers according to certain embodiments of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will now be described in more detail hereinafter with reference to the accompanying drawings, in which some, but not all, embodiments of the present invention are shown. Indeed, the present invention may be embodied in many different forms and should not be construed as being limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will satisfy applicable legal requirements. As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.
[0012] The terms "substantial" or "substantially" may encompass a given total amount according to certain embodiments of the invention, or approximately but not to a given total amount (e.g., 95%, 96%, 97%, 98%, or 99% of a given total amount) according to other embodiments of the invention.
[0013] The terms "polymer" or "polymeric" as used interchangeably herein may include homopolymers, copolymers, such as block, graft, random, and alternating copolymers, terpolymers, and the like, as well as blends and modifications thereof. Furthermore, unless specifically limited otherwise, the terms "polymer" or "polymeric" include all possible structural isomers, stereoisomers, including without limitation, geometric isomers, optical isomers, or enantiomers, and / or any chiral molecular configurations of such polymer or polymeric material. Such configurations include, but are not limited to, isotactic, syndiotactic, and atactic configurations of such polymer or polymeric material. The terms "polymer" or "polymeric" also include polymers made from various catalyst systems, including without limitation Ziegler-Natta catalyst systems and metallocene / single-site catalyst systems. The terms "polymer" or "polymeric", according to certain embodiments of the present invention, also include polymers that are produced by fermentation processes or that are biosourced.
[0014] As used herein, the terms "nonwoven" and "nonwoven web" may include webs having a structure of individual fibers, filaments, and / or threads that are layered over one another rather than in an identifiable repeating manner, such as knitted or woven fabrics. Nonwoven fabrics or webs according to certain embodiments of the present invention may be formed by any process conventionally known in the art, such as, for example, meltblowing processes, spunbonding processes, needlepunching, hydroentangling, airlaid, and bonded carded web processes. As used herein, a "nonwoven web" may include a plurality of individual fibers that have not been subjected to a consolidation process.
[0015] As used herein, the terms "fabric" and "nonwoven fabric" may include a web of fibers in which a plurality of fibers are mechanically entangled or otherwise interconnected, fused together, and / or chemically bonded together. For example, a nonwoven web of individually layered fibers may be subjected to a bonding or consolidation process to bond at least some of the individual fibers together to form a coherent (e.g., consolidated) web of interconnected fibers.
[0016] As used herein, the terms "consolidated" and "consolidation" may include the closer approach or attachment between at least some of the fibers of a nonwoven web (e.g., heat-sealed together, chemically bonded together, and / or mechanically entangled together) to form a bond site(s), which functions to increase resistance to external forces (e.g., abrasion and tensile forces) compared to a non-consolidated web. The bond site(s) may include, for example, discrete or localized regions of web material that have been softened or melted and optionally subsequently or simultaneously compressed to form discrete or localized deformations of the web material. Furthermore, the term "consolidation" can include an entire nonwoven web that has been treated such that at least some portion of the fibers are brought into closer proximity or attachment therebetween (e.g., heat-sealed together, chemically bonded together, and / or mechanically entangled together), for example, by thermal bonding or mechanical entanglement (e.g., hydroentanglement), just to name a few. Such webs can be considered "consolidated nonwovens," "nonwoven fabrics," or simply "fabrics" according to certain embodiments of the present invention.
[0017] The term "staple fibers" as used herein may include fibers cut from a filament. According to certain embodiments, any type of filament material may be used to form the staple fibers. For example, the staple fibers may be formed from polymeric and / or elastomeric fibers. Non-limiting examples of materials may include polyolefins (e.g., polypropylene or polypropylene-containing copolymers), polyethylene terephthalate, and polyamides. The average length of the staple fibers may include, by way of example only, from about 2 centimeters to about 15 centimeters.
[0018] The term "spunbond" as used herein may include fibers formed by extruding a molten thermoplastic material as filaments from a plurality of thin, usually circular capillaries of a spinneret, the diameter of the extruded filaments then rapidly reducing. In accordance with certain embodiments of the present invention, spunbond fibers are generally not tacky when they accumulate on a collecting surface and may be generally continuous as described and disclosed herein. It is noted that spunbonds used in certain composites of the present invention may include nonwoven fabrics described in the literature as SPINLACE®. Spunbond fibers may include, for example, continuous fibers.
[0019] The term "continuous fibers" as used herein refers to fibers that are not cut from their original length prior to being formed into a nonwoven web or fabric. Continuous fibers can have an average length ranging from greater than about 15 centimeters to more than one meter, up to the length of the web or fabric to be formed. For example, continuous fibers as used herein can include fibers in which the length of the fiber is at least 1,000 times longer than the average diameter of the fiber. For example, the length of the fiber is at least about 5,000, 10,000, 50,000, or 100,000 times greater than the average diameter of the fiber.
[0020] The term "meltblown" as used herein may include fibers formed by extruding molten thermoplastic material as molten threads or filaments through multiple thin die capillaries into a converging high velocity, usually hot, gas (e.g., air) stream that attenuates the filaments of molten thermoplastic material to reduce their diameter, which may be a microfiber diameter according to certain embodiments of the invention. According to certain embodiments of the invention, the die capillaries may be circular. The meltblown fibers are then carried by the high velocity gas stream and accumulate on a collecting surface to form a web of randomly spun meltblown fibers. Meltblown fibers may include microfibers that may be continuous or discontinuous and are generally tacky when they accumulate on a collecting surface. However, meltblown fibers are shorter in length than those of spunbond fibers.
[0021] The term "layer" as used herein may include any commonly recognizable combination of similar material types and / or functions that reside in the XY plane.
[0022] The term "multicomponent fiber" as used herein may include fibers formed from at least two different polymeric materials (e.g., two or more) extruded from separate extruders but spun together to form one fiber. The term "bicomponent fiber" as used herein may include fibers formed from two different polymeric materials extruded from separate extruders but spun together to form one fiber. The polymeric materials or polymers are disposed at substantially constant locations in distinct zones on the cross section of the multicomponent fiber and extend continuously along the length of the multicomponent fiber. The configuration of such multicomponent fibers may be, for example, a sheath / core configuration in which one polymer is surrounded by another, an eccentric sheath-core configuration that includes a sheath component and a core component, where the core component defines at least a portion of the outer surface of the bicomponent fiber having an eccentric sheath-core configuration, or a side-by-side configuration, or a pie configuration, or an "islands in the sea" configuration, as are known in the art of multicomponent fibers that each include a bicomponent.
[0023] As used herein, the term "monocomponent fiber" may include fibers formed from a single polymer or polymer blend (e.g., a blend or mixture of two or more polymers) extruded from a single extruder. The single polymer or polymer blend may, for example, define a polymer matrix within which one or more additives (e.g., fillers) may be dispersed.
[0024] As used herein, the term "high loft" includes materials that may have a z-direction thickness generally greater than about 0.3 mm and a relatively low bulk density. The thickness of a "high loft" nonwoven and / or layer may be greater than 0.3 mm (e.g., greater than 0.4 mm, greater than 0.5 mm, greater than 0.6 mm, greater than 0.8 mm, or greater than 1 mm). The thickness is determined utilizing a ProGage Thickness Tester (Model 89-2009) available from Thwig-Albert Instrument, Inc. (West Berlin, NJ 08091), which utilizes a 2" diameter foot with an applied force of 1.45 kPa during measurement. According to certain embodiments of the present invention, the thickness of the "Hi-Loft" nonwoven fabric and / or layers may be up to about any of the following: 3, 2.75, 2.5, 2.25, 2, 1.75, 1.5, 1.25, 1.0, 0.75, and 0.5 mm, and / or at least about any of the following: 0.3, 0.4, 0.5, 0.75, 1.0, 1.25, 1.5, 1.75, and 2.0 mm. In addition, as used herein, a "high loft" nonwoven fabric and / or layer has a relatively low density (e.g., bulk density of weight per unit volume), e.g., less than about 60 kg / m 3 Less than, for example, up to about any of the following: 70, 60, 55, 50, 45, 40, 35, 30, and 25 kg / m 3 , and / or at least about any of the following: 10, 15, 20, 25, 30, 35, 40, 45, 50, and 55 kg / m 3 may have:
[0025] As used herein, the term "machine direction" or "MD" includes the direction in which the fabric is produced or transported. As used herein, the term "cross-machine direction" or "CD" includes the direction of the fabric substantially perpendicular to the MD.
[0026] As used herein, the term "aspect ratio" includes the ratio of the length of the major axis to the length of the minor axis of the cross-section of the subject fiber.
[0027] All integer endpoints disclosed herein that may create smaller ranges within a given range disclosed herein are within the scope of certain embodiments of the invention. For example, a disclosure of about 10 to about 15 includes disclosures of intermediate ranges, such as about 10 to about 11, about 10 to about 12, about 13 to about 15, about 14 to about 15, etc. Moreover, all single decimal endpoints (e.g., numbers reported to one decimal place after rounding) that may create smaller ranges within a given range disclosed herein are within the scope of certain embodiments of the invention. For example, a disclosure of about 1.5 to about 2.0 includes disclosures of intermediate ranges, such as about 1.5 to about 1.6, about 1.5 to about 1.7, about 1.7 to about 1.8, etc.
[0028] In one aspect, the present invention provides a nonwoven fabric comprising a plurality of crimped bicomponent fibers having a first component comprising a first polymeric material comprising a first polymer or a first polymer blend, and a second component comprising a second polymeric material, wherein the second polymeric material comprises a second polymer blend of (i) at least one polypropylene polymer, (ii) at least one polyethylene polymer, and (iii) at least one compatibilizer comprising or consisting of at least one polypropylene-polyethylene copolymer. According to certain embodiments of the present invention, the nonwoven fabric comprises a high loft nonwoven fabric, wherein the plurality of crimped bicomponent fibers impart a desired loft property (e.g., thickness in the z-direction perpendicular to the cross-machine and machine directions of the nonwoven fabric).
[0029] Figure 1, for example, illustrates a crimped bicomponent fiber 50 according to certain embodiments of the present invention, where the crimped bicomponent fiber 50 includes a plurality of three-dimensional coil or helix shaped crimped portions. Although the crimped bicomponent fiber 50 of Figure 1 illustrates a plurality of three-dimensional coil or helix shaped crimped portions, the crimped bicomponent fiber may additionally or alternatively include at least one discrete zigzag configured crimped portion, at least one discrete helix configured crimped portion, or combinations thereof.
[0030] According to certain embodiments of the present invention, the plurality of crimped bicomponent fibers can comprise an average free state crimp percentage of about 30% to about 300%, for example, up to about any of the following: 300, 275, 250, 225, 200, 175, 150, 125, 100, and 75%, and / or at least about any of the following: 20, 30, 40, 50, 75, 100, 125, 150, 175, and 200%. Additionally or alternatively, the plurality of crimped bicomponent fibers may include an average free state crimp length of about 10 mm to about 50 mm, such as at least about any of the following: 10, 12, 14, 15, 16, 18, 20, 22, 24, and 25 mm, and / or at most about any of the following: 50, 45, 40, 38, 35, 32, 30, 28, and 25 mm. The average free state crimp percentage may be ascertained by determining the free state crimp length of the subject fiber with an Instron 5565 equipped with a 2.5N load cell. At this point, the free or unstretched fiber bundle may be placed in the clamps of the machine. The free state crimp length may be measured at the point where the load (e.g., 2.5N load cell) on the fiber bundle becomes constant. The following parameters are used to determine the free state crimp length: (i) record the approximate free state fiber bundle weight in grams (e.g., xxxg ± 0.002 grams), (ii) record the unstretched bundle length in inches, (iii) set the gauge length of the Inston (i.e., the distance or gap between the clamps holding the fiber bundle) to 1 inch, and (iv) set the crosshead speed to 2.4 inches / minute. The free state crimp length of a given fiber can then be ascertained by recording the stretched length of the fiber at the point where the load becomes constant (i.e., the fiber is fully stretched). The average free state crimp percentage can be calculated from the free state crimp length of the given fiber and the unstretched fiber bundle length (e.g., the gauge length). For example, a measured free state crimp length of 32 mm would provide an average free state crimp percentage of about 126% when using the 1 inch (25.4 mm) gauge length discussed above. The foregoing method for determining average free state crimp percentage can be particularly useful when evaluating continuous fibers having a helical coil crimp.For example, conventional textile fibers can be mechanically crimped and optically measured, but continuous fibers having helical coil crimped portions introduce errors when attempting to optically count the "crimp" of such fibers.
[0031] According to certain embodiments of the present invention, a plurality of crimped bicomponent fibers may include a plurality of three-dimensional crimped portions having an average diameter (e.g., based on an average of the longest lengths defining the individual crimped portions) of about 0.5 mm to about 5 mm, e.g., up to about any of the following: 5, 4.75, 4.5, 4.25, 4, 3.75, 3.5, 3.25, 3, 2.9, 2.8, 2.7, 2.6, 2.5, 2.4, 2.3, 2.2, 2.1, 2, 1.9, 1.8, 1.7, 1.6, and 1.5 mm, and / or at least about any of the following: 0.5, 0.6, .07, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, and 2 mm. According to certain embodiments of the present invention, the average diameter of the plurality of three-dimensional crimped portions may be ascertained by use of a digital optical microscope (KH-7700, manufactured by Hirox Corporation, Japan) to view a sample of the multicomponent fiber and obtain digital measurements of the loop diameters of the three-dimensional crimped portions of the SMF. Typically, a magnification range of 20x to 40x may be used to facilitate evaluation of the loop diameters formed from the three-dimensional crimps of the multicomponent fiber.
[0032] According to certain embodiments of the present invention, the plurality of crimped bicomponent fibers may include a plurality of three-dimensional crimped portions having an average diameter (e.g., based on an average of the longest length defining the individual crimped portions) of about 10 mm to about 40 mm, e.g., up to about any of the following: 40, 38, 35, 32, 30, 28, and 25 mm, and / or at least about any of the following: 10, 12, 15, 18, 20, 22, and 25 mm. According to certain embodiments of the present invention, the average diameter of the plurality of three-dimensional crimped portions may be ascertained by using a digital optical microscope (KH-7700, manufactured by Hirox Co., Ltd., Japan) to view a sample of the multicomponent fiber and obtain digital measurements of the loop diameters of the three-dimensional crimped portions of the SMF. Typically, a magnification range of 20x to 40x can be used to facilitate evaluation of the loop diameters formed from the three-dimensional crimp of the multicomponent fiber.
[0033] According to certain embodiments of the present invention, the first polymeric material may include a polyolefin, such as one or more polypropylenes, one or more polyethylenes, or any combination thereof. For example, the first polymeric material may include a single polymer or a total polymer content attributable to a first polymer blend, such as a first polypropylene having a first melt flow rate (MFR) and a second polypropylene having a second MFR, where the second MFR is greater than or equal to the first MFR. According to certain embodiments of the invention, the first MFR ratio between the second MFR and the first MFR is at least about 1:1, such as at least about any of the following: 1:1, 1.2:1, 1.4:1, 1.5:1, 1.6:1, 1.8:1, 2:1, 4:1, 5:1, 6:1, 8:1, 10:1, 12:1, 14:1, 16:1, 18:1, 20:1, 22:1, 24:1, and 25:1, and / or at most about any of the following: 60:1, 55:1, 50:1, 48:1, 46:1, 45:1, 44:1, 42:1, 40:1, 38:1, 36:1, 35:1., 34:1, 32:1, 30:1, 28:1, 26:1, and 25:1.
[0034] According to certain embodiments of the present invention, the first polymeric material may comprise about 70 wt.% to about 99 wt.% of a first polypropylene, for example, at least about any of the following: 70, 75, 80, 85, and 90 wt.%, and / or up to about any of the following: 99, 98, 97, 96, 95, 94, 93, 92, 91, and 90 wt.%. Additionally or alternatively, the first polymeric material may comprise about 1 wt.% to about 10 wt.% of a second polypropylene, for example, at least about any of the following: 1, 2, 3, 4, and 5 wt.%, and / or up to about any of the following: 10, 9, 8, 7, 6, and 5 wt.%.
[0035] According to certain embodiments of the present invention, the first polypropylene of the first polymeric material may have an MFR (i.e., a first MFR) of about 10 g / 10 min to about 100 g / 10 min as determined by ASTM-D1238 (230° C. / 2.16 kg), for example, at least about any of the following: 10, 15, 20, 22, 25, 28, 30, 32, 35, 38, and 40 g / 10 min as determined by ASTM-D1238 (230° C. / 2.16 kg), and / or at most about any of the following: 100, 90, 80, 70, 60, 50, and 40 g / 10 min as determined by ASTM-D1238 (230° C. / 2.16 kg). Additionally or alternatively, the second polypropylene of the first polymeric material may have an MFR (i.e., a second MFR) of about 500 g / 10 min to about 2500 g / 10 min as determined by ASTM-D1238 (230° C. / 2.16 kg), for example, at least about any of the following: 500, 550, 600, 700, 800, 900, 1000, 1200, 1500, and 1800 g / 10 min as determined by ASTM-D1238 (230° C. / 2.16 kg), and / or at most about any of the following: 2500, 2400, 2300, 2200, 2100, 2000, 1900, and 1800 g / 10 min as determined by ASTM-D1238 (230° C. / 2.16 kg).
[0036] According to certain embodiments of the present invention, the second polymer blend may comprise about 60 wt.% to about 90 wt.% of at least one polypropylene polymer (e.g., a single polypropylene polymer or a combination of polypropylene polymers), for example, at least about any of the following: 60, 62, 64, 65, 66, 68, 70, 72, 74, 77, 78, and 80 wt.% of at least one polypropylene polymer, and / or up to about any of the following: 90, 88, 86, 85, 84, 83, 82, 81, and 80 wt.% of at least one polypropylene polymer. For example, the at least one polypropylene polymer may be a first polypropylene polymer that may be the same or different from the first polypropylene used in the first polymer blend, and / or a second polypropylene polymer that may be the same or different from the second polypropylene used in the first polymer blend). According to certain embodiments of the present invention, at least one polypropylene polymer of the second polymer blend (e.g., a single polypropylene polymer or a combination of polypropylene polymers) has a melt flow rate (MFR) of about 10 to about 150 g / 10 min as determined by ASTM-D1238 (230° C. / 2.16 kg), e.g., at least about any of the following: 10, 12, 14, 16, 18, 20, 22, 24, 25, 26, 28, 30, 32, 34, 35, 36, 38, 40, 42, 44, 45, 46, 48, and 50 g / 10 min, and / or up to about any of the following: 150, 140, 130, 120, 110, 100, 95, 90, 85, 80, 75, 70, 65, 60, 58, 56, 55, 54, 52, and 50 g / 10 min. For example, the second polymer blend can include a plurality of different polypropylene polymers, and the weight average MFR of the combination of the plurality of different polypropylene polymers can fall within any of the aforementioned ranges.
[0037] According to certain embodiments of the invention, the second polymer blend may comprise about 5 to about 30 wt.% of at least one polyethylene polymer, such as at least about any of the following: 5, 6, 8, 10, 12, 14, and 15 wt.% of at least one polyethylene polymer, and / or up to about any of the following: 30, 28, 26, 25, 24, 22, 20, 18, 16, and 15 wt.% of at least one polyethylene polymer. For example, the at least one polyethylene polymer may be the first polyethylene polymer. According to certain embodiments of the present invention, the at least one polyethylene polymer may have a melt flow rate (MFR) as determined by ASTM-D1238 (190°C / 2.16 kg) of about 1 to about 40 g / 10 min, for example, at least about any of the following: 1, 2, 4, 5, 6, 8, 10, 12, 14, and 15 g / 10 min, and / or up to about any of the following: 40, 35, 30, 25, 20, 18, 16, and 15 g / 10 min.
[0038] According to certain embodiments of the present invention, the second polymer blend may comprise about 1 wt.% to about 10 wt.% of at least one polypropylene-polyethylene copolymer (e.g., a compatibilizer), for example, at least about any of the following: 1, 2, 3, 4, and 5 wt.% of at least one polypropylene-polyethylene copolymer, and / or up to about any of the following: 10, 9, 8, 7, 6, and 5 wt.% of at least one polypropylene-polyethylene copolymer. The at least one polypropylene-polyethylene copolymer may be, for example, a first polypropylene-polyethylene copolymer (e.g., a single polypropylene-polyethylene copolymer). The first polypropylene-polyethylene copolymer may comprise a first block copolymer or a first random copolymer. According to certain embodiments of the present invention, the first polypropylene-polyethylene copolymer is an EP-iPP diblock polymer.
[0039] The first polypropylene-polyethylene copolymer according to certain embodiments of the invention may have an ethylene monomer content of from about 5 to about 60% by weight, for example, at least about any of the following: 5, 6, 8, 10, 12, 14, 15, 16, 18, 20, 22, 24, 25, 26, 28, 30, 32, 34, 35, 26, 38, 40, 42, 44, and 45% by weight, and / or up to about any of the following: 60, 58, 56, 55, 54, 52, 50, 48, 46, and 45% by weight. Additionally or alternatively, at least one polypropylene-polyethylene copolymer (e.g., the first polypropylene-polyethylene copolymer) has a melt flow rate (MFR) of about 0.5 g / 10 min to about 20 g / 10 min as determined by ASTM-D1238 (230° C. / 2.16 kg), for example, at least about any of the following: 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, and 10 g / 10 min as determined by ASTM-D1238 (230° C. / 2.16 kg), and / or up to about any of the following: 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, and 10 g / 10 min as determined by ASTM-D1238 (230° C. / 2.16 kg). According to certain embodiments of the present invention, the second MFR ratio between the third MFR of the at least one polypropylene polymer as determined by ASTM-D1238 (230° C. / 2.16 kg) and the fourth MFR of the at least one polyethylene polymer as determined by ASTM-D1238 (230° C. / 2.16 kg) in the second polymeric material can be from about 5:1 to about 20:1, such as at least about any of the following: 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, and 12:1, and / or up to about any of the following: 20:1, 19:1, 18:1, 17:1, 16:1, 15:1, 14:1, 13:1, and 12:1.Additionally or alternatively, the second polymer blend may have a MFR of about 20 to about 120 g / 10 min as determined by ASTM-D1238 (230° C. / 2.16 kg), e.g., at least about any of the following: , 36, 38, and 40 g / 10 min, and / or up to about any of the following: 120, 110, 100, 90, 80, 70, 60, 59, 58, 56, 55, 54, 52, 50, 49, 48, 47, 46, 45, 44, 43, 42, 41, and 40 g / 10 min as determined by ASTM-D1238 (230° C. / 2.16 kg).
[0040] In this regard, recent advances in single-site catalysts (e.g., metallocene catalysts) have allowed the creation of various polymer structures that were difficult or impossible to produce economically. In this regard, the first polypropylene-polyethylene copolymer may include copolymers formed from single-site catalysts, such as metallocene-catalyzed copolymers. For example, polypropylene-based polymers having significant amounts of ethylene content may be produced in various configurations (e.g., distinct blocks) to further improve the copolymer's ability to bridge typically incompatible polymers. Examples of such materials include polypropylene-based elastomers, including propylene and ethylene copolymers, Vistamaxx™ (e.g., Vistamaxx™ 6202). Such propylene-based elastomers include, for example, isotactic polypropylene microcrystalline regions and random amorphous regions (e.g., ethylene). Such olefin copolymers may include hard and soft blocks, where the hard block is primarily propylene and the soft block is primarily ethylene. In this regard, the hard block (e.g., propylene) may comprise 10-90% by weight of the copolymer, and the soft block may comprise 90-10% by weight of the copolymer. In this regard, such copolymers include a random ethylene distribution throughout the copolymer. Vistamaxx™ (e.g., Vistamaxx™ 6202) copolymers are commercially available from ExxonMobil. Vistamaxx™ 6202 has a density of 0.862 g / cc, an MI (190C / 2.16 kg) of 9.1, an MFR (230C / 2.16 kg load) of 20, and an ethylene content of 15% by weight. Additional examples include olefin diblock copolymers, including EP-iPP diblock polymers such as Intune™, which are polypropylene-based block copolymers that include ethylene monomers.According to certain embodiments of the present invention, the first polypropylene-polyethylene copolymer disclosed herein may be prepared, for example, by a process comprising contacting an addition-polymerizable monomer or mixture of monomers under addition polymerization conditions with a composition comprising at least one addition polymerization catalyst, a cocatalyst, and a chain shuttling agent ("CSA"). Here, the process is characterized by the formation of at least some of the growing polymer chains by two or more reactors operating at steady-state polymerization conditions at distinct process conditions or by two or more zones of a reactor operating at plug-flow polymerization conditions. According to certain embodiments of the present invention, the first polypropylene-polyethylene copolymer may comprise an olefin block copolymer formed from a single-site catalyst or other catalyst system. Thus, the first polypropylene-polyethylene copolymer may not be produced from a single-site catalyst according to certain embodiments of the present invention. According to certain embodiments of the present invention, the first polypropylene-polyethylene copolymer lacks anhydride functionality, such as maleic anhydride functionality.
[0041] According to certain embodiments of the present invention, the copolymers formed from the single-site catalysts discussed above can be distinguished from conventional random copolymers, physical blends of polymers, and block copolymers prepared by sequential monomer addition. These copolymers can be distinguished from random copolymers by characteristics such as higher melting temperatures for equivalent amounts of comonomer, block composite index, described below; from physical blends by characteristics such as block composite index, better tensile strength, improved fracture strength, thinner morphology, improved optics, and greater impact strength at lower temperatures; and from block copolymers prepared by sequential monomer addition by molecular weight distribution, rheology, shear thinning, rheology ratio, and block polydispersity.
[0042] As a further example, the first polypropylene-polyethylene copolymer may comprise an EP-iPP diblock polymer having an ethylene content of 43 to 48%, or 43.5 to 47%, or 44 to 47% by weight, based on the weight of the diblock copolymer. In example embodiments, the EP-iPP diblock polymer may have a propylene content of 57 to 52%, or 56.5 to 53%, or 56 to 53% by weight, based on the weight of the EP-iPP diblock polymer.
[0043] According to certain embodiments of the present invention, the plurality of crimped bicomponent fibers have an average diameter (e.g., fiber diameter) of about 10 to about 30 microns, such as at least about any of the following: 10, 12, 14, 15, 16, 18, and 20 microns, and / or up to about any of the following: 30, 28, 26, 25, 24, 22, and 20 microns. Additionally or alternatively, the plurality of crimped bicomponent fibers may include continuous fibers, such as spunbond fibers, staple fibers, or combinations thereof.
[0044] According to certain embodiments of the present invention, the plurality of crimped bicomponent fibers may include a side-by-side configuration (e.g., circular or non-circular cross-section), a sheath-core configuration, a pie configuration, an islands-in-the-sea configuration, a multilobal configuration, or any combination thereof, etc. For example, the sheath-core configuration may include an eccentric sheath-core configuration including a sheath component and a core component, where the core component defines at least a portion of an outer surface of the plurality of bicomponent fibers having the eccentric sheath-core configuration.
[0045] 2A-2H illustrate example cross-sectional images of some non-limiting examples of multiple crimped bicomponent fibers according to certain embodiments of the present invention. As illustrated in FIG. 2A-2H, multiple crimped bicomponent fibers 50 can include a first polymer component 52 of a first polymer composition A, for example as disclosed and described herein, and a second polymer component 54 of a second polymer composition B, for example as disclosed and described herein. The first and second components 52 and 54 can be arranged in substantially distinct zones within the cross-section of the multiple crimped bicomponent fibers that extend substantially continuously along the length of the bicomponent fiber. The first and second components 52 and 54 can be arranged in a side-by-side arrangement in a circular cross-sectional fiber as illustrated in FIG. 2A, or in a ribbon-shaped (e.g., non-circular) cross-sectional fiber as illustrated in FIG. 2G and 2H. Additionally or alternatively, the first and second components 52 and 54 may be arranged in a sheath / core arrangement, such as the eccentric sheath / core arrangement illustrated in Figures 2B and 2C. In an eccentric sheath / core bicomponent fiber illustrated in Figure 2B, one component completely encloses or surrounds the other, but is located asymmetrically in the multicomponent fiber to allow fiber crimp (e.g., first component 52 surrounds component 54). The eccentric sheath / core configuration illustrated by Figure 2C includes a first component 52 (e.g., sheath component) that substantially but not completely surrounds a second component 54 (e.g., core component), since some portion of the second component may be exposed and form part of the outermost surface of the fiber 50. As an additional example, the bicomponent fiber may include a hollow fiber, as illustrated in Figures 2D and 2E, or a multilobal fiber, as illustrated in Figure 2F. It should be pointed out, however, that numerous other cross-sectional configurations and / or fiber shapes may be suitable in accordance with certain embodiments of the present invention.
[0046] In a multiply crimped bicomponent fiber, the respective polymer components may be present in a ratio (by volume or by weight (my)) of about 85:15 to about 15:85 according to certain embodiments of the present invention. A ratio (by volume or weight) of approximately 50:50 may be desirable according to certain embodiments of the present invention. However, the specific ratio employed may vary as desired. For example, up to about any of the following: 85:15, 80:20, 75:25, 70:30, 65:35, 60:40, 55:45, and 50:50 by volume or weight, and / or at least about any of the following: 50:50, 45:55, 40:60, 35:65, 30:70, 25:75, 20:80, and 15:85 by volume or weight. Additionally or alternatively, the first polymeric material may comprise about 20 wt.% to about 80 wt.% of the plurality of crimped bicomponent fibers, such as at least about any of the following: 20, 25, 30, 35, 40, 45, 50, and 55 wt.%, and / or up to about any of the following: 80, 75, 70, 65, 60, and 55 wt.%. Additionally or alternatively, the second polymeric material may comprise about 20 wt.% to about 80 wt.% of the plurality of crimped bicomponent fibers, such as at least about any of the following: 20, 25, 30, 35, 40, 45, 50, and 55 wt.%, and / or up to about any of the following: 80, 75, 70, 65, 60, and 55 wt.%.
[0047] According to certain embodiments of the invention, the first polymer blend, the second polymer blend, or both may comprise less than about 10% by weight of the total polypropylene-polyethylene copolymer, such as at least about any of the following: 0, 0.5, 1, 2, 3, 4, and 5% by weight, and / or at most about any of the following: 10, 9, 8, 7, 6, and 5% by weight. In this regard, the bicomponent fiber may comprise a total polymer component having less than about 10% by weight of the total polypropylene-polyethylene copolymer, such as at least about any of the following: 0, 0.5, 1, 2, 3, 4, and 5% by weight, and / or at most about any of the following: 10, 9, 8, 7, 6, and 5% by weight.
[0048] According to certain embodiments of the present invention, the second polymeric material may optionally further comprise a compatibilizer comprising anhydride functionality, such as maleic anhydride or a maleic anhydride modified polymer. Additionally or alternatively, the first polymeric material, the second polymeric material, or both may further comprise one or more fillers, such as one or more organic fillers and / or one or more inorganic fillers (e.g., calcium carbonate particulates, pigments, etc.). According to certain embodiments of the present invention, the first polymeric material, the second polymeric material, or both may further comprise one or more slip agents, such as amides. The one or more slip agents may comprise, for example, primary amides, secondary amides, tertiary amides, bisamides, or any combination thereof. According to certain embodiments of the present invention, the one or more slip agents may comprise one or more primary amides. By way of example, primary amides suitable as slip agents according to certain embodiments of the present invention may include erucamide, oleamide, strearamide, behenamide, or any combination thereof. Alternatively or in addition, certain embodiments of the present invention may include one or more slip agents comprising one or more secondary amides. By way of example, secondary amides suitable as slip agents according to certain embodiments of the present invention may include oleyl palmitamide, stearyl erucamide, or any combination thereof. Alternatively or in addition, certain embodiments of the present invention may include one or more slip agents comprising one or more bisamides, such as ethylene bisamides. By way of example, bisamides suitable as slip agents according to certain embodiments of the present invention may include ethylene bis strearamide, ethylene bis oleamide, or any combination thereof. Slip agents according to certain embodiments of the present invention may include amides (e.g., primary amides, secondary amides, tertiary amides, bisamides, etc.) that include one or more saturated or unsaturated aliphatic chains. According to certain embodiments of the invention, the one or more aliphatic chains can each independently contain from about 1 to about 30 carbon atoms (e.g., from about 5 to about 30 carbon atoms). For example, secondary amides and bisamides can contain two saturated and / or unsaturated carbon chains, each independently containing from about 1 to about 30 carbon atoms (e.g., from about 5 to about 30 carbon atoms).By way of example only, the one or more aliphatic chains may each independently contain at least about any of the following: 1, 5, 10, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, and 25 carbon atoms, and / or up to about 30, 29, 28, 27, 26, 25, 20, and 15 carbon atoms (e.g., from about 15 to about 25 carbon atoms, from about 20 to 30 carbon atoms, etc.). In accordance with certain embodiments of the present invention, the slip agent may include an amide that includes an unsaturated aliphatic chain having one or more elements of unsaturation. An element of unsaturation corresponds to two fewer hydrogen atoms than a saturated formula. For example, a single double bond would correspond to one element of unsaturation, and a triple bond would correspond to two elements of unsaturation. According to certain embodiments of the invention, the slip agent includes an unsaturated aliphatic chain containing from about 1 to about 10 elements of unsaturation (eg, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 elements of saturation).
[0049] As noted above, the plurality of crimped bicomponent fibers may include circular cross-sections, non-circular cross-sections, or both. For example, the non-circular cross-sections may include pie-shaped cross-sections, multi-lobal cross-sections, or ribbon-shaped cross-sections. According to certain embodiments of the present invention, the plurality of crimped bicomponent fibers include non-circular cross-sections having an aspect ratio of at least about 1.5:1, for example, from about 1.5:1 to about 10:1.
[0050] According to certain embodiments of the present invention, the plurality of crimped bicomponent fibers may comprise about 0 to about 100 wt.% circular cross-section fibers, such as at least about any of the following: 0, 5, 10, 20, 30, 40, and 50 wt.%, and / or at most about any of the following: 100, 95, 90, 80, 70, 60, and 50 wt.%. Additionally or alternatively, the plurality of crimped bicomponent fibers may comprise about 0 to about 100 wt.% non-circular cross-section fibers, such as at least about any of the following: 0, 5, 10, 20, 30, 40, and 50 wt.%, and / or at most about any of the following: 100, 95, 90, 80, 70, 60, and 50 wt.%.
[0051] According to certain embodiments of the present invention, the plurality of crimped bicomponent fibers defines a first nonwoven layer, and the nonwoven fabric further comprises one or more additional nonwoven layers, including, for example, at least a second nonwoven layer. In this regard, the nonwoven fabric may comprise a multi-layer nonwoven fabric. The one or more additional layers may include, for example, a spunbond layer, a meltblown layer, a carded layer, a hydroentangled layer, a cellulosic layer, or any combination thereof. According to certain embodiments of the present invention, the nonwoven fabric comprises one or more cellulosic layers located directly or indirectly between the first nonwoven layer and the second nonwoven layer, where the second nonwoven layer comprises a second spunbond layer or a spunbond-meltblown-spunbond layer.
[0052] According to certain embodiments of the present invention, the nonwoven fabric may have a basis weight of at least about 14 grams per square meter (gsm), such as at least about any of the following: 14, 16, 18, 20, 22, 25, 28, 30, 32, 35, 38, 40, 42, 45, 48, 50, 52, 55, 58, and 60 gsm, and / or up to about any of the following: 100, 95, 90, 85, 80, 75, 70, 65, and 60 gsm.
[0053] In another embodiment, the present invention provides a method of making a nonwoven fabric, which may include: (a) forming a first polymer melt comprising a first polymer or a first polymer blend, (b) forming a second polymer melt comprising a second polymer blend of (i) at least one polypropylene polymer, (ii) at least one polyethylene polymer, and (iii) at least one compatibilizer comprising a polypropylene-polyethylene copolymer, (c) forming a plurality of bicomponent fibers by melt spinning the first polymer melt and the second polymer melt through a bicomponent spinneret pack, (d) allowing the plurality of bicomponent fibers to crimp prior to or during deposition on a collecting surface or subjecting the plurality of bicomponent fibers to a crimping process to provide a plurality of crimped bicomponent fibers, and (e) consolidating the plurality of crimped bicomponent fibers to form a nonwoven fabric. Alternatively, the method may include: (a) forming a first polymer melt comprising a first polymer or a first polymer blend, (b) forming a second polymer melt comprising a second polymer blend of (i) at least one polypropylene polymer, (ii) at least one polyethylene polymer, and (iii) at least one compatibilizer comprising a polypropylene-polyethylene copolymer, (c) forming a plurality of bicomponent fibers by melt spinning the first polymer melt and the second polymer melt through a bicomponent spinneret pack, (d) consolidating the plurality of bicomponent fibers to form an intermediate nonwoven fabric, and (e) subjecting the plurality of bicomponent fibers of the intermediate nonwoven fabric to a crimping process to provide a nonwoven fabric. According to certain embodiments of the present invention, the bicomponent spinneret pack includes an orifice through which the plurality of bicomponent fibers are extruded.
[0054] According to certain embodiments of the invention, the step of forming the second polymer melt includes selecting and blending at an elevated temperature at least one polypropylene polymer, at least one polyethylene polymer, and at least one polypropylene-polyethylene copolymer, wherein the MFR of the at least one polyethylene polymer is less than the MFR of the at least one polypropylene polymer at the elevated temperature, and the difference between the MFR of the at least one polypropylene polymer and the MFR of the at least one polyethylene polymer is less than about 35. For example, the difference between the MFR of the at least one polypropylene polymer and the MFR of the at least one polyethylene polymer can be from about 1 to about 35, such as at least about any of the following: 1, 3, 5, 8, 10, 12, 15, 18, and 20, and / or up to about any of the following: 35, 32, 20, 28, 26, 25, 24, 22, and 20. According to certain embodiments of the invention, the elevated temperature can be from about 190° C. to about 250° C., for example, at least about any of the following: 190, 200, 210, and 215° C., and / or up to about any of the following: 250, 245, 240, 235, 230, 225, 220, and 215° C. According to certain embodiments of the invention, the first polymer blend and the second polymer blend can be extruded and / or melt spun at one or more of the elevated temperatures or temperature ranges referenced above. According to certain embodiments of the invention, the first polymer blend and the second polymer blend can be extruded and melt spun at the same elevated temperature.
[0055] According to certain embodiments of the present invention, the step of consolidating the plurality of bicomponent fibers or consolidating the plurality of crimped bicomponent fibers may include a thermal bonding process, an ultrasonic bonding process, a mechanical bonding process, an adhesive bonding process, or any combination thereof. The consolidation step may include forming a plurality of individual bond sites, for example, by a thermal bonding process or an ultrasonic process. In this regard, the plurality of individual bond sites define a bond area. The bond area may comprise, for example, about 3% to about 30% of the nonwoven fabric, for example, at least about any of the following: 3, 4, 5, 6, 8, 10, 12, 14, and 15%, and / or up to about any of the following: 30, 28, 26, 25, 24, 22, 20, 18, 16, and 15%. Additionally or alternatively, the step of forming the plurality of individual bond sites may be performed at a temperature of about 120° C. to about 170° C., e.g., at least about any of the following: 120, 122, 124, 125, 126, 128, 130, 132, 134, and 135° C., and / or at most about any of the following: 170, 160, 150, 148, 146, 145, 144, 142, 140, 138, 136, and 135° C.
[0056] In yet another aspect, the present invention provides a shaped article comprising one or more of the nonwoven fabrics described and disclosed herein. The shaped article may comprise an adult diaper, a baby diaper, a pull-up, or of a feminine hygiene pad. According to certain embodiments of the present invention, the shaped article may comprise a topsheet comprising the nonwoven fabrics described and disclosed herein. EXAMPLES
[0057] The present disclosure is further illustrated by the following examples, which should not be construed as limiting in any way, and thus the specific features described in the following examples are merely illustrative and not limiting.
[0058] Example set 1 Nine (9) differently crimped bicomponent fibers (i.e., Samples 1-9) were produced and their average free state crimp length was measured. Each of the bicomponent fibers was a side-by-side bicomponent fiber, where the first polymeric material represented 60 wt.% of the bicomponent fiber and the second polymeric material represented 40 wt.% of the bicomponent fiber. The average free state crimp length was measured for each of the differently crimped bicomponent fibers. The results are summarized in Table 1 below.
[0059] Sample 1 was the control sample. All polymeric materials consisted of 100 wt% polypropylene homopolymer (i.e., PP3155E5 from Exxon) with a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). In Sample 2, the first polymeric material consisted of 100 wt% polypropylene homopolymer (i.e., PP3155E5 from Exxon) with a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of 100 wt% polypropylene copolymer commercially available as SV956 from LyondellBasell.
[0060] In Sample 3, the first polymeric material consisted of 100 wt. % polypropylene homopolymer (ie, PP3155E5 from Exxon) having a MFR of 36 g / 10 min according to ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of a blend of (i) 80 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), (ii) 15 wt. % linear low density polyethylene (i.e., PE-Dowlex 2036.01G from Dow) having a MFR of 2.5 g / 10 min per ASTM-D1238 (190° C. / 2.16 kg), and (iii) 5 wt. % EP-iPP diblock polymer (i.e., Intune™-Dow D5545) having a MFR of 9.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg).
[0061] In Sample 4, the first polymeric material consisted of a blend of (1) 97 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), and (ii) 3 wt. % meltblown polypropylene having a MFR of 500 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of a blend of (i) 80 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), (ii) 15 wt. % linear low density polyethylene (i.e., PE-Dowlex 2036.01G from Dow) having a MFR of 2.5 g / 10 min per ASTM-D1238 (190° C. / 2.16 kg), and (iii) 5 wt. % EP-iPP diblock polymer (i.e., Intune™-Dow D5545) having a MFR of 9.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg).
[0062] In Sample 5, the first polymeric material consisted of 100 wt.% polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min according to ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of 100 wt.% polypropylene random copolymer commercially available as RP448S from LyondellBasell.
[0063] In Sample 6, the first polymeric material consisted of 100 wt.% polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), and the second polymeric material consisted of 100 wt.% polypropylene copolymer commercially available as Pro-Fax-SDS242 from LyondellBasell.
[0064] In sample 7, the first polymeric material consisted of 100 wt.% polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of 97 wt.% polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg) and 3 wt.% Dowlex polyethylene.
[0065] In Sample 8, the first polymeric material consisted of 100 wt.% polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of: (i) 92 wt.% polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), (ii) 6 wt.% Dowlex polyethylene, and (iii) 2 wt.% EP-iPP diblock polymer (i.e., Intune™-Dow D5545) having a MFR of 9.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg).
[0066] In Sample 9, the first polymeric material consisted of 100 wt% polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of: (i) 86.5 wt% polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), (ii) 10 wt% Dowlex polyethylene, and (iii) 3.5 wt% EP-iPP diblock polymer (i.e., Intune™-Dow D5545) having a MFR of 9.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg).
[0067] As shown in Table 1, Sample 3 was capable of providing an average free state crimp length while using a blend of polypropylene, polyethylene, and a small amount of compatibilizer. In this regard, the improved average free state crimp achieved by Sample 3 was achieved while using significantly less polypropylene copolymer. Details regarding the specific composition of the first and second polymeric materials of each sample are more briefly summarized in Table 2.
[0068] Example set 2 Thirteen (13) additional differently crimped bicomponent fibers (i.e., Samples 10-22) were produced and their average free state crimp length was measured. In these samples, each of the bicomponent fibers was a side-by-side bicomponent fiber, but the weight percentages of the first polymeric material of the bicomponent fiber and the second polymeric material of the bicomponent fiber were varied as shown in Table 2. The average free state crimp length was measured for each of the differently crimped bicomponent fibers. The results are summarized in Table 1 below.
[0069] In Sample 10, the first polymeric material consisted of 100 wt. % polypropylene homopolymer (ie, PP3155E5 from Exxon) having a MFR of 36 g / 10 min according to ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of 80 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), 15 wt. % Dowelex polyethylene (i.e., PE-Dowlex 2036.01G from Dow) having a MFR of 2.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), and 5 wt. % EP-iPP diblock polymer (i.e., Intune™-Dow D5545) having a MFR of 9.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The first polymeric material represented 70% by weight of the bicomponent fibers, and the second polymeric material represented 30% by weight of the bicomponent fibers.
[0070] In Sample 11, the first polymeric material and the second polymeric material were the same as those in Sample 10. However, in Sample 11, the first polymeric material represented 50% by weight of the bicomponent fibers, and the second polymeric material represented 50% by weight of the bicomponent fibers.
[0071] In Sample 12, the first polymeric material and the second polymeric material were the same as those in Sample 10. However, in Sample 12, the first polymeric material represented 30% by weight of the bicomponent fibers and the second polymeric material represented 70% by weight of the bicomponent fibers.
[0072] In Sample 13, the first polymeric material consisted of a blend of (i) 97 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), and (ii) 3 wt. % meltblown polypropylene having a MFR of 1800 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of a blend of (i) 80 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), (ii) 15 wt. % linear low density polyethylene (i.e., PE-Dowlex 2036.01G from Dow) having a MFR of 2.5 g / 10 min per ASTM-D1238 (190° C. / 2.16 kg), and (iii) 5 wt. % EP-iPP diblock polymer (i.e., Intune™-Dow D5545) having a MFR of 9.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The first polymeric material represented 70% by weight of the bicomponent fibers, and the second polymeric material represented 30% by weight of the bicomponent fibers.
[0073] In Sample 14, the first polymeric material and the second polymeric material were the same as those in Sample 13. However, in Sample 14, the first polymeric material represented 50% by weight of the bicomponent fibers, and the second polymeric material represented 50% by weight of the bicomponent fibers.
[0074] In Sample 15, the first polymeric material and the second polymeric material were the same as those in Sample 13. However, in Sample 15, the first polymeric material represented 30% by weight of the bicomponent fibers and the second polymeric material represented 70% by weight of the bicomponent fibers.
[0075] In Sample 16, the first polymeric material consisted of 100 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of (i) 77 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), (ii) 15 wt. % linear low density polyethylene (i.e., PE-Dow from Dow) having a MFR of 2.5 g / 10 min per ASTM-D1238 (190° C. / 2.16 kg). lex2036.01G), (iii) 5 wt. % EP-iPP diblock polymer (i.e., Intune™-Dow D5545) having a MFR of 9.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), and (iv) 3 wt. % meltblown polypropylene having a MFR of 1800 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The first polymer material represented 70 wt. % of the bicomponent fibers and the second polymer material represented 30 wt. % of the bicomponent fibers.
[0076] In Sample 17, the first polymeric material and the second polymeric material were the same as those in Sample 16. However, in Sample 16, the first polymeric material represented 50% by weight of the bicomponent fibers, and the second polymeric material represented 50% by weight of the bicomponent fibers.
[0077] In Sample 18, the first polymeric material and the second polymeric material were the same as those in Sample 16. However, in Sample 18, the first polymeric material represented 30% by weight of the bicomponent fibers and the second polymeric material represented 70% by weight of the bicomponent fibers.
[0078] In Sample 19, the first polymeric material consisted of a blend of (i) 99 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), and (ii) 1 wt. % meltblown polypropylene having a MFR of 1800 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of a blend of (i) 80 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), (ii) 15 wt. % Dowelex polyethylene (i.e., PE-Dowlex 2036.01G from Dow) having a MFR of 2.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), and (iii) 5 wt. % EP-iPP diblock polymer (i.e., Intune™-Dow D5545) having a MFR of 9.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The first polymeric material represented 50% by weight of the bicomponent fibers, and the second polymeric material represented 50% by weight of the bicomponent fibers.
[0079] In Sample 20, the first polymeric material consisted of a blend of (i) 98 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), and (ii) 2 wt. % meltblown polypropylene having a MFR of 1800 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of a blend of (i) 80 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), (ii) 15 wt. % Dowelex polyethylene (i.e., PE-Dowlex 2036.01G from Dow) having a MFR of 2.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), and (iii) 5 wt. % EP-iPP diblock polymer (i.e., Intune™-Dow D5545) having a MFR of 9.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The first polymeric material represented 50% by weight of the bicomponent fibers, and the second polymeric material represented 50% by weight of the bicomponent fibers.
[0080] For Sample 21, the first polymeric material consisted of a blend of (i) 97 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), and (ii) 3 wt. % meltblown polypropylene having a MFR of 1800 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of a blend of (i) 82 wt. % polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), (ii) 15 wt. % Dowelex polyethylene (i.e., PE-Dowlex 2036.01G from Dow) having a MFR of 2.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg), and (iii) 3 wt. % EP-iPP diblock polymer (i.e., Intune™-Dow D5545) having a MFR of 9.5 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The first polymeric material represented 50% by weight of the bicomponent fibers, and the second polymeric material represented 50% by weight of the bicomponent fibers.
[0081] In sample 22, the first polymeric material consisted of 100 wt.% polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The second polymeric material consisted of 100 wt.% polypropylene homopolymer (i.e., PP3155E5 from Exxon) having a MFR of 36 g / 10 min per ASTM-D1238 (230° C. / 2.16 kg). The first polymeric material represented 50 wt.% of the bicomponent fibers and the second polymeric material represented 50 wt.% of the bicomponent fibers.
[0082] [Table 1]
[0083] [Table 2A] [Table 2B]
[0084] These and other modifications and variations of the present invention may be practiced by those of ordinary skill in the art without departing from the spirit and scope of the present invention as more particularly set forth in the appended claims. In addition, it should be understood that aspects of the various embodiments may be interchanged in whole or in part. Furthermore, those skilled in the art will appreciate that the foregoing description is by way of example only and is not intended to limit the invention as further set forth in such appended claims. Thus, the spirit and scope of the appended claims should not be limited to the illustrative descriptions of the variations contained herein. [Explanation of symbols]
[0085] A. First Polymer Composition B. Second Polymer Composition 50 Crimped bicomponent fibers 52 First Polymer Component 54 Second Polymer Component
Claims
1. 1. A nonwoven fabric comprising a plurality of crimped bicomponent fibers having a first component comprising a first polymeric material comprising a first polymer or a first polymer blend, and a second component comprising a second polymeric material, wherein the second polymeric material comprises a second polymer blend of (i) at least one polypropylene polymer, (ii) at least one polyethylene polymer, and (iii) at least one compatibilizer comprising or consisting of at least one polypropylene-polyethylene copolymer.
2. 10. The nonwoven fabric of claim 1, wherein the first polymeric material comprises a polyolefin, such as one or more polypropylenes, one or more polyethylenes, or any combination thereof.
3. 10. The nonwoven fabric of claim 1, wherein the first polymeric material comprises a first polypropylene having a first melt flow rate (MFR) and a second polypropylene having a second MFR, wherein the second MFR is greater than or equal to the first MFR.
4. A first MFR ratio between the second MFR and the first MFR is at least about 1:1, for example at least about any of the following: 1:1, 1.2:1, 1.4:1, 1.5:1, 1.6:1, 1.8:1, 2:1, 4:1, 5:1, 6:1, 8:1, 10:1, 12:1, 14:1, 16:1, 18:1, 20:1, 22:1, 24:1, and 25:1, and / or at most about any of the following: 60:1, 55:1, 50:1, 48:1, 46:1, 45:1, 44:1, 42:1, 40:1, 38:1, 36:1, 35:
1.
4. The nonwoven fabric of claim 3, wherein the .lambda. / .lambda. ratio is 34:1, 32:1, 30:1, 28:1, 26:1, and 25:
1.
5. 5. The nonwoven fabric of claims 3-4, wherein the first polymeric material comprises about 70 wt.% to about 99 wt.% of the first polypropylene, such as at least about any of the following: 70, 75, 80, 85, and 90 wt.%, and / or at most about any of the following: 99, 98, 97, 96, 95, 94, 93, 92, 91, and 90 wt.%, and the first polymeric material comprises about 1 wt.% to about 10 wt.% of the second polypropylene, such as at least about any of the following: 1, 2, 3, 4, and 5 wt.%, and / or at most about any of the following: 10, 9, 8, 7, 6, and 5 wt.%.
6. 6. The nonwoven fabric of claims 1-5, wherein the second polymer blend comprises about 60 to about 90 wt.% of the at least one polypropylene polymer, about 5 to about 30 wt.% of the at least one polyethylene polymer, and about 1 to about 10 wt.% of the at least one polypropylene-polyethylene copolymer.
7. 7. The nonwoven fabric of claim 6, wherein the at least one polypropylene polymer is a first polypropylene polymer having a melt flow rate (MFR) of about 10 to about 100 g / 10 min as determined by ASTM-D1238 (230 C / 2.16 kg), the at least one polyethylene polymer is a first polyethylene polymer having a MFR of about 1 to about 40 g / 10 min as determined by ASTM-D1238 (190 C / 2.16 kg), and the at least one polypropylene-polyethylene copolymer is a first polypropylene-polyethylene copolymer, such as an EP-iPP diblock polymer, having a MFR of about 0.5 to about 20 g / 10 min as determined by ASTM-D1238 (230 C / 2.16 kg).
8. 8. The nonwoven fabric of claim 7, wherein the first polypropylene-polyethylene copolymer has an ethylene monomer content of from about 5 to about 60 weight percent, for example, at least about any of the following: 5, 6, 8, 10, 12, 14, 15, 16, 18, 20, 22, 24, 25, 26, 28, 30, 32, 34, 35, 26, 38, 40, 42, 44, and 45 weight percent, and / or up to about any of the following: 60, 58, 56, 55, 54, 52, 50, 48, 46, and 45 weight percent.
9. The nonwoven fabric of claims 1-8, wherein the plurality of crimped bicomponent fibers comprises continuous fibers, such as spunbond fibers, staple fibers, or a combination thereof.
10. 10. The nonwoven fabric of claims 1-9, wherein the plurality of crimped bicomponent fibers comprises a side-by-side configuration, a sheath-core configuration, a pie configuration, an islands-in-the-sea configuration, a multilobal configuration, or any combination thereof.
11. 11. The nonwoven fabric of claims 1-10, wherein the first polymeric material comprises about 20% to about 80% by weight of the plurality of crimped bicomponent fibers, such as at least about any of the following: 20, 25, 30, 35, 40, 45, 50, and 55 wt.%, and / or up to about any of the following: 80, 75, 70, 65, 60, and 55 wt.%, and the second polymeric material comprises about 20% to about 80% by weight of the plurality of crimped bicomponent fibers, such as at least about any of the following: 20, 25, 30, 35, 40, 45, 50, and 55 wt.%, and / or up to about any of the following: 80, 75, 70, 65, 60, and 55 wt.%.
12. 12. The nonwoven fabric of claims 1-11, wherein the plurality of crimped bicomponent fibers defines a first nonwoven layer, and the nonwoven fabric further comprises one or more additional nonwoven layers including at least a second nonwoven layer, the one or more additional layers comprising a spunbond layer, a meltblown layer, a carded layer, a hydroentangled layer, a cellulosic layer, or any combination thereof.
13. 13. The nonwoven fabric of claim 12, wherein the nonwoven fabric comprises one or more cellulosic layers located directly or indirectly between the first nonwoven layer and the second nonwoven layer, wherein the second nonwoven layer comprises a spunbond layer or a spunbond-meltblown-spunbond layer.
14. A method of making a nonwoven fabric, including: (a) forming a first polymer melt comprising a first polymer or a first polymer blend; (b) forming a second polymer melt comprising a second polymer blend of (i) at least one polypropylene polymer, (ii) at least one polyethylene polymer, and (iii) at least one compatibilizer comprising a polypropylene-polyethylene copolymer; (c) forming a plurality of bicomponent fibers by melt spinning the first polymer melt and the second polymer melt through a bicomponent spinneret pack; (d) allowing the plurality of bicomponent fibers to crimp prior to or during deposition on a collecting surface or subjecting the plurality of bicomponent fibers to a crimping step to provide a plurality of crimped bicomponent fibers; and (e) consolidating the plurality of crimped bicomponent fibers to form the nonwoven fabric of any one of claims 1-42.
15. A method of making a nonwoven fabric, including: (a) forming a first polymer melt comprising a first polymer or a first polymer blend; (b) forming a second polymer melt comprising a second polymer blend of (i) at least one polypropylene polymer, (ii) at least one polyethylene polymer, and (iii) at least one compatibilizer comprising a polypropylene-polyethylene copolymer; (c) forming a plurality of bicomponent fibers by melt spinning the first polymer melt and the second polymer melt through a bicomponent spinneret pack; (d) consolidating the plurality of bicomponent fibers to form an intermediate nonwoven fabric; and (e) subjecting the plurality of bicomponent fibers of the intermediate nonwoven fabric to a crimping process to provide the nonwoven fabric of any one of claims 1-42.
Citation Information
Patent Citations
Crimped multicomponent fiber and method of making same
JP2002529617A
Latent crimpable composite fiber and manufacturing method therefor, conjugate fiber and nonwoven fabric
JP2017179621A
Multicomponent fibers with improved intercomponent adhesion
JP2021503048A
Self-crimping multicomponent fibers and methods for making same
JP2022503858A