Positive electrode and method for preparing same, and lithium ion secondary battery
A positive electrode with a first material for stability and a second material for lithium replenishment addresses SEI-related capacity loss, enhancing energy density and cycle life in lithium-ion batteries.
Patent Information
- Application Number
- JP2024524620
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-25
- Filing Date
- 2021-11-17
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2041-11-17
AI Technical Summary
The formation of a solid electrolyte interface (SEI) on the negative electrode during the charging and discharging of lithium-ion secondary batteries leads to irreversible capacity loss and reduced energy density, especially when high-specific-capacity negative electrode materials like silicon or tin-based alloys are used, necessitating an effective lithium replenishment method.
A positive electrode comprising a first material with high cycling stability and a second material with high initial charge specific capacity and low coulombic efficiency, where the second material undergoes a phase transition to replenish lithium, increasing energy density by compensating for SEI losses and participating in subsequent cycles as an active material.
The proposed positive electrode design enhances energy density by replenishing lithium through a phase transition in the second material, improving cycle life and rate characteristics of lithium-ion secondary batteries.
Smart Images

Figure 2024536607000001_ABST
Abstract
Description
[Technical field]
[0001] The present application relates to the field of battery positive electrode materials, in particular to a positive electrode and a method for preparing the same, and to a lithium-ion secondary battery. [Background technology]
[0002] In the process of the first charge and discharge of lithium-ion secondary batteries, a solid electrolyte interface (SEI) is formed on the surface of the negative electrode, which causes irreversible capacity loss and reduces the energy density of lithium-ion energy storage devices. In devices using graphite as the negative electrode, about 10% of the active lithium source is consumed in the first cycle. When using negative electrode materials with high specific capacity, such as alloys (silicon, tin, etc.), oxides (silicon oxide, tin oxide), and amorphous carbon, the consumption of the active lithium source increases further. Therefore, in order to further improve the energy density of lithium-ion secondary batteries, a suitable lithium replenishment method is very important.
[0003] In the prior art, the industry has been increasingly paying attention to a method of lithium replenishment to the positive electrode, which is relatively safe and easy to operate compared to the many problems caused by lithium replenishment to the negative electrode. For example, the prior art discloses lithium replenishment materials to the positive electrode based on lithium oxygen compounds, lithium sources, and alkyl lithiums. The prior art also discloses lithium replenishment by Li2NiO2-based lithium replenishment materials. Summary of the Invention
[0004] This application discloses a positive electrode. The positive electrode comprises a first positive electrode material having excellent cycle stability and high initial coulombic efficiency and a second material having high initial charge specific capacity and low initial coulombic efficiency, thereby compensating for the loss of active lithium due to the formation of SEI. After releasing the excess absorbed lithium, the second material undergoes a phase transition to the R-3m phase and participates in the subsequent cycles as an active material, thereby increasing the energy density of the secondary battery.
[0005] A positive electrode, wherein the positive electrode contains a first positive electrode material and a second material, wherein the first positive electrode material contains any one represented by Formula I,
Chemical formula
Chemical formula
[0006] Specifically, the second material must contain the B phase. Only the B phase can provide additional charge specific capacity. After releasing excess lithium, the B phase undergoes a phase transition to the A phase. Since the second material can be used as a material for replenishing lithium, it will necessarily have the effects of a high initial charge specific capacity and a low initial Coulomb efficiency.
[0007] The prerequisite for lithium replenishment is that the initial efficiency of the positive electrode is higher than that of the negative electrode. Therefore, a part of the positive electrode material is not fully utilized. In the present application, the first positive electrode material is not fully utilized. In order to fully utilize the first positive electrode material (increase the energy density), it is necessary to replenish lithium to the first positive electrode material. In the present application, a second material is used to replenish lithium. The second material must have a high initial charge specific capacity and a low initial Coulomb efficiency. Otherwise, it cannot be combined with the first positive electrode material, and the effect of lithium replenishment cannot be obtained. In addition, the second material is relatively special. After releasing lithium, it participates in subsequent cycles as an active material (i.e., the A phase), thereby further increasing the energy density.
[0008] Optionally, in the first positive electrode material, M 1 contains at least one selected from the group consisting of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, and Rh, and / or A contains at least one selected from the group consisting of S and F, and / or x satisfies -0.05 ≤ x ≤ 0.1, and / or y satisfies 0 ≤ y ≤ 0.1.
[0009] Optionally, in the second material, M 2 and M 3 each independently contain at least one selected from the group consisting of Co, Mn, and Al, and / or D contains at least one selected from the group consisting of S and F, and / or p and q satisfy 0 < p ≤ 0.2, 0 < q ≤ 0.2, 0 < p + q ≤ 0.5, and / or r satisfies 0 < r ≤ 1, and / or s satisfies 0 ≤ s < 0.1.
[0010] Optionally, the second material is a B phase belonging to the F-3m1 space group. That is, the second material consists of the B phase. At this time, the chemical formula of the second material is the following formula II-1,
Chemical formula
[0011] Alternatively, the second material includes at least two distinct phases, one of which is a B phase belonging to the F-3m1 space group. For example, the second material may include two, three, four, or five distinct phases.
[0012] Optionally, the second material includes two distinct phases, one of the two distinct phases being a B phase.
[0013] Optionally, the second material includes phase A and phase B, the phase A belongs to the R-3m space group and has a characteristic diffraction peak A of the (003) plane at 17° to 19° in the X-ray diffraction spectrum, and the phase B belongs to the F-3m1 space group and has a characteristic diffraction peak A of the (001) plane at 16° to 18° in the X-ray diffraction spectrum.
[0014] Optionally, the intensity I of the characteristic diffraction peak A A and the intensity of characteristic diffraction peak B I B The relationship is shown in Formula III. [ka]
[0015] Optionally, in the second material, the space group of the B phase is changed from F-3m1 to R-3m after releasing the excess absorbed lithium.
[0016] Optionally, the weight ratio of the first cathode material to the second material is 2-99:1.
[0017] Optionally, the weight ratio of the first cathode material to the second material is 3-99:1.
[0018] Optionally, the positive electrode further includes a binder, a conductive agent, and a solvent, and the content of the first positive electrode material in the positive electrode is 80 wt % to 98 wt %.
[0019] Specifically, when the positive electrode includes a current collector, the content of the first positive electrode material in the positive electrode means the content of the first positive electrode material in the remaining material after removing the current collector from the positive electrode.
[0020] Optionally, the content of the first positive electrode material in the positive electrode is 85wt% to 98wt%.
[0021] Optionally, the positive electrode satisfies Formula IV: [ka] In formula IV, R represents the resistance of the positive electrode (Ω), P represents the compressed density of the positive electrode (g / cm 3 ), and Q is the surface density (g / 1540.25 mm 2 )
[0022] Optionally, the positive electrode satisfies formula IV-1: [ka] In formula IV-1, the meanings of R, P, and Q are the same as those in formula IV.
[0023] Optionally, the resistance R of the positive electrode satisfies R≦3.
[0024] Optionally, the resistance R of the positive electrode satisfies R≦1.5.
[0025] Alternatively, the range of the value of the compressed density P of the positive electrode is 3.4 <P<4.2である。
[0026] Alternatively, the surface density Q of one side of the positive electrode is in the range of 0.16 <Q<0.38である。
[0027] According to a second aspect of the present application, there is further provided a lithium ion secondary battery. The lithium ion secondary battery has the advantages of high energy density, good rate characteristics, and long cycle life. Specifically, the energy density of the battery is increased by selecting a first positive electrode material and a second material containing a B phase. A lithium ion secondary battery having good rate characteristics and long cycle life can be obtained by designing parameter conditions such as P, Q, and R of the positive electrode piece.
[0028] The lithium ion secondary battery includes the positive electrode according to any one of the above, a negative electrode, a separator, and an electrolyte solution.
[0029] Optionally, the electrolyte contains fluoroethylene carbonate, and the content of the fluoroethylene carbonate in the electrolyte is m. The range of the value of m is 0 wt%. <m≦15wt%である。
[0030] In the present application, the electrolyte of the lithium ion secondary battery contains fluoroethylene carbonate, which replenishes lithium and forms a more uniform and dense SEI in the negative electrode, thereby reducing the continuous consumption of active lithium, better protecting the interface, and improving the cycle life.
[0031] According to a third aspect of the present application, there is further provided a method for preparing a positive electrode, comprising mixing a first positive electrode material and a second material and then coating the mixture to obtain the positive electrode, The second material comprises at least a) obtaining a precursor a, said precursor a comprising any of the formula V; [ka] In formula V, M 2 , M 3 , D, p, and q each have the same meaning as in formula II; b) preparing a solution a of a lithium-containing organic compound containing any one selected from the group consisting of lithium naphthalenide, dibiphenyl lithium, and n-butyl lithium; The solvent in the solution a is tetrahydrofuran or ethylene glycol dimethyl ether; and c) Reacting precursor a with solution a to obtain a precipitate of a second material. This is what is obtained.
[0032] Specifically, the method for preparing the second material includes: Conventional solid-phase sintering method 1-p-q M 2 p M 3 q O 2-s D s A first step of preparing a second step of preparing a solution of lithium naphthalenide (or dibiphenyllithium, or n-butyllithium) in tetrahydrofuran (or ethylene glycol dimethyl ether) having a concentration of 0.2M to 2M; LiNi obtained in the first step 1-p-q M 2 p M 3 q O 2-s D s a third step of immersing the powder in the solution prepared in the second step for 3 to 30 minutes; and a fourth step of discarding the supernatant in the third step, washing the precipitate with a large amount of tetrahydrofuran (or ethylene glycol dimethyl ether) solvent, and drying it in a vacuum oven to obtain the second material.
[0033] The beneficial effects of the present application include the following:
[0034] 1) The positive electrode active material in this application is a material for replenishing lithium to the positive electrode, and the second material includes a B phase that belongs to the F-3m1 space group and has a very high specific capacity. The B phase releases a large amount of lithium ions during the first charge to compensate for the loss of active lithium. After releasing the excess lithium, the B phase undergoes a phase transition from the F-3m1 phase to the R-3m phase and participates in the subsequent cycles as an active material.
[0035] The second material containing phase B has a high first charge specific capacity and a low first coulombic efficiency, and when combined with the first positive electrode material having a high specific capacity, a high discharge platform and a high first efficiency (i.e., first coulombic efficiency), it realizes the effect of replenishing lithium and increases the energy density. And in the second material, only phase B can provide additional charge specific capacity. After releasing the excess lithium, phase B undergoes a phase transition to the R-3m phase and participates in subsequent cycles as an active material, thus further increasing the energy density.
[0036] 2) The second material used in the present application can include phase A and phase B. Phase A belongs to the R-3m space group and can be a positive electrode active material with a high specific capacity. Phase B with a high specific capacity belongs to the F-3m1 space group and can release a large amount of lithium ions during the first charge to replenish lithium to the first positive electrode material. After releasing lithium, phase B undergoes a phase transition to the R-3m phase and can participate in subsequent cycles as an active material. Expand the scope of use of the second material.
[0037] 3) The present invention can significantly improve the cycle life and rate characteristics of a lithium ion secondary battery by designing the sheet resistance, compression density and areal density of the positive electrode piece.
[0038] 4) In the present application, by adding fluoroethylene carbonate as an additive to the electrolyte, a uniform and dense SEI film containing a large amount of LiF is formed on the negative electrode, thereby suppressing the continuous loss of active lithium. At the same time, since fluoroethylene carbonate has high resistance to high-pressure oxidation on the positive electrode side, the cycle life of the lithium-ion secondary battery can be further improved. [Brief description of the drawings]
[0039] In order to more clearly describe the technical solutions of the embodiments of the present application, the following briefly describes the drawings used in the embodiments. Obviously, the drawings in the following description are only some embodiments of the present application, and those skilled in the art can also obtain other drawings based on these drawings without inventive work. [Figure 1] FIG. 1 is an XRD pattern of Li1.2Ni0.8Co0.1Mn0.1O2, which is the first second material used in the positive electrode according to Example 1 of the present application. [Diagram 2] FIG. 2 shows the charge-discharge curves of the first cycle of the first second material Li1.2Ni0.8Co0.1Mn0.1O2 in Example 1 of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0040] In order to clarify the purpose, technical solution and beneficial technical effects of the present invention, the present invention will be described in more detail below with examples. It should be noted that the examples described in this specification are merely for the purpose of illustrating the present invention and do not limit the scope of the claims of the present invention. The scope of the present invention is defined only by the appended claims and their equivalents. Any modifications, equivalent replacements and improvements made within the spirit and principle of the present invention should be included within the protection scope of the present invention.
[0041] For example, the first positive electrode material and the second material according to the present invention may be directly mixed when preparing a slurry, or a slurry may be prepared using the second material according to the present invention and applied as an upper or lower layer to the first positive electrode material.
[0042] Also, for convenience, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form a range that is not explicitly stated. Also, any lower limit can be combined with another lower limit to form a range that is not explicitly stated. Similarly, any upper limit can be combined with any other upper limit to form a range that is not explicitly stated. Also, although not explicitly stated, each point or individual value between the endpoints of a range is included in the range. Therefore, each point or individual value can be combined with any other point or individual value as its own lower limit or upper limit, or with other lower limits or upper limits to form a range that is not explicitly stated.
[0043] In the present description, unless otherwise specified, the terms "greater than or equal to" and "less than or equal to" include the numerical values. The term "SEI" in this application refers to a solid electrolyte interface.
[0044] In this specification, the meaning of "xx to xx" includes the two end values. For example, "80wt% to 98wt%" means 80wt% or more and 98wt% or less.
[0045] In the prior art, Li2NiO2-based lithium supplement materials are used. Such materials have a high specific capacity, are easy to prepare, and can sufficiently supplement active lithium. However, such materials belong to the Immm space group, and the lithium release process is irreversible. After releasing lithium during the first cycle charge, inactive components remain in the electrode strip, which is disadvantageous for further increasing the energy density of the battery. In addition, during the first charge, a large amount of active lithium is absorbed into the negative electrode, which further reduces the true potential of the negative electrode, and the solvent in the electrolyte continues to undergo a reduction reaction at the negative electrode, causing a continuous increase in impedance and affecting the cycle characteristics.
[0046] In order to solve the problem that the effect of improving the energy density of a battery by the lithium supplementary material in the prior art is limited, the inventors have found that the lithium release process of the lithium supplementary material in the prior art is irreversible, and inactive components remain on the electrode strip after releasing lithium by the first cycle charging. Therefore, the present application provides a positive electrode active material including a first positive electrode material and a second material including a B phase belonging to the F-3m1 space group. Specifically, on the one hand, the B phase provides additional lithium to supplement the first positive electrode material with lithium (i.e., to compensate for the loss of active lithium due to the formation of SEI), thereby increasing the energy density of the battery. On the other hand, the B phase undergoes a phase transition to the R-3m phase after releasing the excess lithium, and participates in the subsequent cycles as an active material, thereby further increasing the energy density.
[0047] Positive Electrode (also referred to herein as positive piece) A first aspect of the embodiment of the present invention provides a positive electrode including a positive electrode current collector and a positive electrode material layer provided on at least one surface of the positive electrode current collector. As an example, the positive electrode current collector includes two surfaces facing each other in a thickness direction thereof, and the positive electrode material layer is provided by laminating on either one or both of the two surfaces of the positive electrode current collector.
[0048] The positive electrode material layer includes a positive electrode active material including a first positive electrode material and a second material.
[0049] [ka]
[0050] In the above formula I, x, y, and t satisfy −0.1≦x≦0.2, 0≦y≦0.2, and 0≦t≦0.2; M 1 is at least one selected from the group consisting of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, Ru, Rh, Ga, Pd, Pt, Mo, W, Sb, Nb, Se, Te, and Ce, and A is at least one selected from the group consisting of S, N, F, Cl, and Br.
[0051] [Chemical formula]
[0052] In the above chemical formula II, r, p, q, and s satisfy 0 < r ≤ 1, 0 < p < 1, 0 < q < 1, 0 < p + q ≤ 0.5, 0 ≤ s < 0.2, and M 2 and M 3 are each independently at least one selected from the group consisting of Co, Mn, Fe, Ti, Al, V, Cr, Nb, Zr, La, and Y, and D is at least one selected from the group consisting of S, N, F, Cl, and Br.
[0053] The second material includes a B phase belonging to the F-3m1 space group.
[0054] In one possible example, the second material consists of a B phase.
[0055] In another possible example, the second material can include an A phase and a B phase. The A phase belongs to the R-3m space group, and a characteristic diffraction peak A of the (003) plane appears at 17° - 19° in the X-ray diffraction spectrum. The B phase belongs to the F-3m1 space group, and a characteristic diffraction peak B of the (001) plane appears at 16° - 18° in the X-ray diffraction spectrum. The intensity I A of the characteristic diffraction peak A and the intensity I B of the characteristic diffraction peak B satisfy Equation III. [Chemical formula]
[0056] In this application, the second material includes both an A phase and a B phase, thereby increasing the energy density of the battery.
[0057] Furthermore, the technical parameters of the positive electrode sheet satisfy 1.0 ≤ R·P / Q ≤ 32, where R is the resistance (Ω) of the positive electrode sheet, P is the compression density (g / cm 3 ) of the positive electrode sheet, and Q is the areal density (g / 1540.25 mm of one side of the positive electrode sheet2 ).
[0058] In this specification, the calculation of R·P / Q is a numerical calculation only. For example, if the resistance R of the positive electrode piece is 1.0 Ω and the compaction density P is 4.0 g / cm 3 The surface density Q of the positive electrode piece on one side is 0.30 g / 1540.25 mm 2 If so, then R P / Q = 13.33.
[0059] The resistance R of the positive electrode piece is the resistance value measured using the DC double probe method. Here, the contact area between the probe and the positive electrode piece is 49π mm 2 As an example, the top and bottom of the positive electrode piece are sandwiched between two conductive terminals of an electrode resistance measuring device, and pressure is applied to fix the electrode piece, the diameter of the conductive terminal is 14 mm, and the applied pressure is 15 MPa to 27 MPa. The electrode resistance measuring device is a HIOKI BT3562 type internal resistance meter.
[0060] The packed density of the positive electrode strip can be calculated by the formula P=m / v, where m is the weight of the positive electrode layer (g) and v is the volume of the positive electrode layer (cm 3 ) Here, the volume v of the positive electrode material layer may be the product of the area Ar of the positive electrode material layer and the thickness of the positive electrode material layer.
[0061] The areal density Q of one side of the positive electrode piece can be calculated by the formula Q = 1540.25 m / Ar. In the above formula, m is the weight (g) of the positive electrode material layer, and Ar is the area (mm 2 ).
[0062] The positive electrode piece of the embodiment of the present invention can fully exert the synergistic effect of the first positive electrode material and the second material. First, the second material used in the present invention can include phase A and phase B, phase A belongs to the R-3m space group and can be a positive electrode active material with high specific capacity, and phase B belongs to the F-3m1 space group and has a very high specific capacity, and releases a large amount of lithium ions during the first charge to compensate for the loss of active lithium, and after releasing lithium, it can be changed to the R-3m phase and participate in the subsequent cycles as an active material. Second, the first positive electrode material used in the present invention has a high specific capacity, a high discharge platform and a high initial efficiency, and can effectively increase the energy density of the battery by combining with the second material. Third, the present invention can significantly improve the cycle life and rate characteristics of the lithium ion secondary battery by designing the sheet resistance, compression density and areal density of the electrode piece. Fourth, by adding fluoroethylene carbonate as an additive to the electrolyte, a uniform and dense SEI film that is rich in LiF components is formed on the negative electrode, thereby suppressing the continuous loss of active lithium. At the same time, fluoroethylene carbonate has high resistance to high-pressure oxidation on the positive electrode side, which can further improve the cycle life of the lithium-ion secondary battery.
[0063] Note that the sheet resistance, compression density, and areal density per side of the positive electrode sheet are important parameters in the design and preparation of lithium-ion secondary batteries. If the sheet resistance of the positive electrode sheet is too large, it will affect the cycle characteristics and rate characteristics of the lithium-ion secondary battery. If the compression density is too large or too small, the cycle characteristics and rate characteristics of the battery will deteriorate. If the areal density per side of the positive electrode sheet is too large, the cycle life of the battery will decrease, which will also affect the penetration of the electrolyte, and further affect the rate characteristics of the battery, especially reducing the discharge capacity of the battery at high rates. And if the areal density per side of the positive electrode sheet is too small, it means that for the same battery capacity, the lengths of the current collector and separator will increase, and the ohmic internal resistance of the battery will increase. Therefore, in order to achieve the expected results of the electrochemical performance of the lithium-ion secondary battery, these parameters need to be comprehensively designed during the manufacture of the battery so that the positive electrode sheet reaches the expected design values.
[0064] More preferably, the technical parameters of the positive electrode sheet should satisfy 5.0 ≦ R·P / Q ≦ 15. The design of R·P / Q is mainly aimed at further improving the cycle life and rate characteristics of the battery.
[0065] The sheet resistance R of the positive electrode sheet is preferably R ≦ 3, and more preferably R ≦ 1.5. This is advantageous for improving the cycle characteristics and rate characteristics of the lithium-ion secondary battery.
[0066] The compression density P of the positive electrode sheet is preferably 3.4 < P < 4.2. This is advantageous for the movement of electrons and ions in the positive electrode sheet, thereby improving the cycle characteristics of the lithium-ion secondary battery.
[0067] The areal density Q per side of the positive electrode sheet is preferably 0.16 < Q < 0.38. This can improve the cycle characteristics and rate characteristics of the lithium-ion secondary battery while ensuring the charge and discharge capacity.
[0068] In the positive electrode, the weight ratio of the first positive electrode material to the second material is preferably 2:1 to 99:1, more preferably 3:1 to 99:1. Since the majority of such positive electrode pieces is the first positive electrode material, it has higher structural stability, reduces capacity loss and impedance increase caused by structural destruction of the positive electrode material, and can maintain cycle stability and dynamic performance.
[0069] The specific ratio of the first cathode material to the second material depends on the initial efficiency and specific capacity of the cathode and anode of the applied system. This ratio should not be too large (too little second material), otherwise the active lithium consumed by the SEI will not be sufficiently replenished. This ratio should also not be too small (too much second material), otherwise there will be an excess of active lithium that is not fully utilized. Also, the second material has a low compaction density, so adding too much of it is detrimental to achieving a higher volumetric energy density.
[0070] In the positive electrode, the weight ratio of the first positive electrode material is 80 wt % to 98 wt %, and more preferably 85 wt % to 98 wt %.
[0071] The positive electrode piece of the embodiment of the present invention can further include a conductive agent and a binder. The present invention does not have any particular limitations on the types of conductive agent and binder, and can be selected according to actual needs.
[0072] As an example, the conductive agent may be one or more selected from the group consisting of graphite, superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The binder may be one or more selected from the group consisting of styrene butadiene rubber (SBR), water based acrylic resin, carboxymethyl cellulose (CMC), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), ethylene vinyl acetate copolymer (EVA), and polyvinyl alcohol (PVA).
[0073] In some optional embodiments, the weight percentage of the conductive agent in the positive electrode is 0.5 wt% or more, which is advantageous for obtaining a relatively low sheet resistance of the positive electrode. When the positive electrode includes a current collector, the content of the conductive agent in the positive electrode means the content of the conductive agent in the remaining material after removing the current collector from the positive electrode.
[0074] In some optional embodiments, the weight percentage of the binder in the positive electrode is 2.0 wt% or less, which is advantageous for obtaining a relatively low sheet resistance of the positive electrode. When the positive electrode includes a current collector, the binder content in the positive electrode refers to the binder content in the remaining material after removing the current collector from the positive electrode.
[0075] The positive electrode current collector may be a metal foil or a porous metal plate. For example, a foil or a porous plate made of a metal such as aluminum, copper, nickel, titanium, or silver, or an alloy thereof, such as aluminum foil, may be used.
[0076] The thickness of the positive electrode current collector is preferably 5 μm to 20 μm, more preferably 6 μm to 18 μm, and even more preferably 8 μm to 16 μm.
[0077] Lithium-ion secondary battery Another aspect of the present invention further provides a lithium ion secondary battery including a positive electrode, a negative electrode, a separator, and an electrolyte.
[0078] The positive electrode uses a positive electrode piece according to the first aspect of the embodiment of the present invention.
[0079] The negative electrode may be a metallic lithium sheet, or may include a negative electrode current collector and a negative electrode material layer provided on at least one surface of the negative electrode current collector.
[0080] The negative electrode layer typically includes a negative electrode material and optional conductive agents, binders, and thickeners. Examples of the negative electrode material include natural graphite, artificial graphite, mesocarbon microbeads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composites, SiO, Li-Sn alloys, Li-Sn-O alloys, Sn, SnO, SnO2, and lithium titanate with a spinel structure, Li4Ti5O. 12 The conductive agent may be one or more selected from the group consisting of graphite, superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The binder may be one or more selected from the group consisting of styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin, and carboxymethyl cellulose (CMC). The thickener may be carboxymethyl cellulose (CMC). However, the present application is not limited to these materials, and other materials that can be used as negative electrode materials, conductive agents, binders, and thickeners for lithium ion secondary batteries may also be used.
[0081] The negative electrode current collector can be made of a material such as a metal foil or a porous metal plate. For example, a foil or a porous plate made of a metal such as copper, nickel, titanium, or iron, or an alloy thereof, such as copper foil, is used.
[0082] The negative electrode pieces can be prepared according to conventional methods in the art. Typically, the negative electrode material, optional conductive agent, binder, and thickener are dispersed in a solvent such as N-methylpyrrolidone (NMP) or deionized water to form a uniform negative electrode slurry, which is then applied to a negative electrode current collector, and the negative electrode pieces are obtained through processes such as drying and cold pressing.
[0083] The separator is not particularly limited, and any known separator having a porous structure and electrochemical stability and chemical stability can be selected. The separator is, for example, one or more single-layer or multi-layer films selected from the group consisting of glass fiber, nonwoven fabric, polyethylene (PE), polypropylene (PP), and polyvinylidene fluoride (PVDF).
[0084] The electrolyte solution includes an organic solvent, an electrolyte lithium salt, and an additive. The present invention does not limit the types of the organic solvent and the electrolyte lithium salt, and can be selected according to actual needs.
[0085] As an example, the organic solvent may be one or more selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), vinylene carbonate (VC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE), and is preferably two or more selected from the group consisting of them.
[0086] The electrolyte lithium salt may be one or more selected from the group consisting of LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiClO4 (lithium perchlorate), LiAsF6 (lithium hexafluoroarsenate), LiFSI (lithium bis(fluorosulfonyl)imide), LiTFSI (lithium bis(trifluoromethanesulfonyl)imide), LiTFS (lithium trifluoromethanesulfonate), LiDFOB (lithium difluoro(oxalato)borate), LiBOB (lithium bis(oxalato)borate), LiPO2F2 (lithium difluorophosphate), LiDFOP (lithium difluorobis(oxalato)phosphate), and LiTFOP (lithium tetrafluoro(oxalato)phosphate).
[0087] The electrolyte additive contains fluoroethylene carbonate (FEC), and the content of the fluoroethylene carbonate is 0 to 15% by weight based on the total weight of the electrolyte.
[0088] The electrolyte solution may further include other additives, if desired. The additives may be any additives that can be used as additives for lithium ion secondary batteries, and are not particularly limited in the present invention and may be selected according to actual needs. As an example, the additives may be one or more selected from the group consisting of vinyl ethylene carbonate (VEC), succinonitrile (SN), adiponitrile (AND), 1-propene 1,3-sultone (PST), sulfonic acid ester cyclic quaternary ammonium salt, tris(trimethylsilane)phosphate (TMSP) and tris(trimethylsilane)borate (TMSB).
[0089] The electrolyte can be prepared according to conventional methods in the art. The electrolyte can be obtained by uniformly mixing an organic solvent, an electrolyte lithium salt, fluoroethylene carbonate and any other additives. Here, the order of addition of each material is not particularly limited. For example, the electrolyte lithium salt, fluoroethylene carbonate and any other additives are added to an organic solvent, and then uniformly mixed to obtain an electrolyte. Wherein, the electrolyte lithium salt can be added to the organic solvent, and then the fluoroethylene carbonate and any other additives can be added to the organic solvent separately or simultaneously.
[0090] The positive electrode piece, the separator, and the negative electrode piece are stacked in this order, and a separator is positioned between the positive electrode piece and the negative electrode piece to provide an isolating function, to obtain a cell, or the cell can be obtained after winding, or the cell can be placed in a case, an electrolyte is injected, and the case is sealed to obtain a lithium ion secondary battery.
[0091] The lithium ion secondary battery of the present invention uses the positive electrode piece according to the first embodiment of the present invention, and therefore has high energy density, good cycle characteristics, and good rate characteristics at the same time.
[0092] Working Example Various substances and materials used in the examples of this application are commercially available, unless otherwise specified.
[0093] Method for preparing the second material 1) 1st second material Li 1.2 Ni 0.8 Co 0.1 Mn 0.1 O 2 Method for preparing Step 1: LiNi by conventional solid-state sintering 0.8 Co 0.1 Mn 0.1 O2 was prepared.
[0094] Step 2: Prepare a 0.5M lithium naphthalenide tetrahydrofuran solution in a glove box (water and oxygen content are both less than 0.1 ppm). Specifically, add an appropriate amount of tetrahydrofuran into a container, then weigh out an appropriate amount of naphthalene powder into the container, and then cut lithium sheet into small pieces and slowly add it to the container and stir for 5 minutes.
[0095] Step 3: The LiNi obtained in step 1 0.8 Co 0.1 Mn 0.1 9.728 g of O2 powder was weighed out and immersed in 40 ml of the solution prepared in step 2 for 5 minutes.
[0096] Step 4: The supernatant in step 3 was discarded, and the precipitate was washed with a large amount of solvent tetrahydrofuran, and dried in a vacuum oven at 80° C. for 5 minutes to obtain a sample, which was recorded as the first second material.
[0097] 2) The second material Li 1.2 Ni 0.8 Co 0.08 Mn 0.1 Al 0.02 O 2 Method for preparing was similar to the first second material, but in step 1, LiNi was prepared by conventional solid-state sintering. 0.8 Co 0.08 Mn 0.1 Al 0.02 O2 was prepared and differed in step 3 in that the mass of the powder was 9.664 g.
[0098] 3) The third second material Li 1.2 Ni 0.8 Co 0.1 Mn 0.1 O 1.95 F 0.05 Method for preparingwas similar to the first second material, but in step 1, LiNi was prepared by conventional solid-state sintering. 0.8 Co 0.1 Mn 0.1 O 1.95 F 0.05 was prepared, differing in that in step 3 the mass of the powder was 9.743 g.
[0099] 4) 5th second material Li 1.2 Ni 0.8 Co 0.1 Mn 0.1 O 1.9 S 0.05 F 0.05 Method for preparing was similar to the first second material, but in step 1, LiNi was prepared by conventional solid-state sintering. 0.8 Co 0.1 Mn 0.1 O 1.9 S 0.05 F 0.05 was prepared, differing in that in step 3 the mass of the powder was 9.823 g.
[0100] 5) 6th second material Li 1.2 Ni 0.5 Co 0.3 Mn 0.2 O 2 Method for preparing was similar to the first second material, but in step 1, LiNi was prepared by conventional solid-state sintering. 0.5 Co 0.3 Mn 0.2 O2 was prepared and differed in step 3 in that the mass of powder was 9.695 g.
[0101] 6) 7th second material Li 2 Ni 0.8 Co 0.1 Mn 0.1 O 2 Method for preparing was similar to the first second material, but in step 1, LiNi was prepared by conventional solid-state sintering. 0.8 Co 0.1 Mn 0.1 O2 was prepared and differed in step 3 in that the volume of the solution was 200 ml.
[0102] XRD measurement of the second material XRD measurements were performed on the first to seventh second materials, and the results showed that all of the first to seventh second materials contained phases A and B.
[0103] 1st Secondary Material Li 1.2 Ni 0.8 Co 0.1 Mn 0.1 The XRD data of LiO2 are shown in Fig. 1. 1.2 Ni 0.8 Co 0.1 Mn 0.1 In O2, a diffraction peak A characteristic of the (003) plane appeared at about 18.7°, and a diffraction peak B characteristic of the (001) plane appeared at about 17.4°. Therefore, the first second material contains phases A and B, and the chemical formula of A is LiNi 0.8 Co 0.1 Mn 0.1 O2, and the chemical formula of B is Li2Ni 0.8 Co 0.1 Mn 0.1 O2. And the intensity of the characteristic diffraction peak A was I A and the intensity of characteristic diffraction peaks B and I B Ratio I A / I B was 8.1.
[0104] Measurement of the charge-discharge characteristics of the first cycle of the second material The measurement method was as follows: At 45° C., the lithium ion secondary battery was charged at a constant current of 0.1 C up to 4.4 V, then charged at a constant voltage until the current was 0.025 C or less, and further discharged at a constant current of 0.1 C up to 3.0 V, and the charge / discharge curve of the battery was recorded.
[0105] The measurement results show that the first to seventh second materials all have high initial charge specific capacity and low initial coulombic efficiency. The charge-discharge characteristics of the first cycle are shown in FIG. 2, taking the first second material as a typical representative. From the figure, it is known that the first second material has high initial charge specific capacity and low initial coulombic efficiency.
[0106] Example 1 Preparation of the positive electrode pieces: The first positive electrode material, LiCoO2, and the second material, Li 1.2 Ni 0.8 Co 0.1 Mn 0.1 The positive electrode slurry was obtained by mixing O2, the binder PVDF, and conductive carbon black in a weight ratio of 87.6:10.0:1.3:1.1, adding the solvent NMP, and stirring with a vacuum mixer until it became a uniform and transparent system. The positive electrode slurry was evenly applied to an aluminum foil positive electrode current collector, then transferred to an oven and dried at 120°C, and further subjected to cold pressing and cutting to obtain positive electrode pieces. The weight percentage of LiCoO2, the first positive electrode material in the positive electrode material layer, was 87.6%, and the weight percentage of LiCoO2, the second material in the positive electrode material layer, was 10.0%. 1.2 Ni 0.8 Co 0.1 Mn 0.1 The weight percentage of O2 was 10.0%.
[0107] Preparation of negative electrode pieces: The negative electrode active material is artificial graphite, silicon monoxide, and the binder is polyacrylic acid (PAA, molecular weight 1×10 3 ~1×10 6 The negative electrode slurry was uniformly applied to the negative electrode current collector, copper foil, and then transferred to an oven to dry at 120°C. The negative electrode pieces were then obtained by cold pressing and cutting.
[0108] Preparation of electrolyte: Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain an organic solvent. 1 mol / L of LiPF6 was dissolved in the organic solvent, and 5% by weight of fluoroethylene carbonate was further added to the total mass of the electrolyte, and the mixture was mixed uniformly to obtain an electrolyte.
[0109] Preparation of lithium ion secondary battery: A positive electrode piece, a separator, and a negative electrode piece are laminated once, where the separator is a 14 μm thick polypropylene (PP) film (manufactured by Celgard), and is positioned between the positive electrode piece and the negative electrode piece to perform the function of isolation. Then, the electrode assembly is wound up, the tab is welded, the bare cell is placed in a case, the electrolyte is injected and sealed, and then the process of standing, chemical conversion, shaping, etc. is carried out to obtain a lithium ion secondary battery.
[0110] Examples 2 to 17 The difference from Example 1 is that the components of the materials in the positive electrode and the related parameters in the preparation process are adjusted, the details of which are shown in Table 1.
[0111] Comparative Example 1 The difference from Example 1 is that the positive electrode contains only LiCoO2, and the details are shown in Table 1.
[0112] Comparative Example 2 The difference from Example 1 is that the positive electrode is Li 1.2 Ni 0.8 Co 0.1 Mn 0.1 The purpose of the present invention is to contain only O2, see Table 1 for details.
[0113] Comparative Example 3 The difference from Example 1 is that the second material in the positive electrode does not contain phase B. See Table 1 for details.
[0114] Comparative Examples 4 to 5 The difference from Example 1 is that the weight ratio of the first positive electrode material to the second material in the positive electrode is different. See Table 1 for details.
[0115] Comparative Examples 6 to 7 The difference from Example 1 is that the sheet resistance, compression density, and surface density of the positive electrode pieces are different. See Table 1 for details.
[0116] Comparative Examples 8 to 9 The difference from Example 1 is that the weight percentage of fluoroethylene carbonate in the electrolyte is different. See Table 1 for details.
[0117] Measurement of the sheet resistance of the positive electrode strip The sheet resistance of the positive electrode piece was measured using a HIOKI BT3562 type resistance meter. Specifically, the positive electrode piece was sandwiched between two conductive terminals of an internal resistance meter, pressure was applied to fix it, and the resistance R of the positive electrode piece was measured. Here, the diameter of the conductive terminal was 14 mm, the pressure was 15 MPa to 27 MPa, and the sampling time ranged from 5 s to 17 s. See Table 1 for details of the measurement results.
[0118] Measurement of high-temperature cycle characteristics of lithium-ion secondary batteries At 45°C, the lithium-ion secondary battery was charged at a constant current of 1.5C up to 4.4V, then charged at a constant voltage until the current fell to 0.05C or less, and then discharged at a constant current of 1C up to 3.0V. This process was counted as one charge / discharge cycle, and the discharge capacity of the first cycle of the lithium-ion secondary battery was recorded. The lithium-ion secondary battery was subjected to charge / discharge cycles according to the above method, and the discharge capacity of each charge / discharge cycle was recorded until the discharge capacity of the lithium-ion secondary battery decayed to 80% of the discharge capacity of the first cycle, and the number of charge / discharge cycles was recorded. See Table 2 for details of the measurement results.
[0119] Measurement of rate characteristics of lithium-ion secondary batteries At 25°C, the lithium-ion secondary battery was charged at a constant current of 0.2C up to 4.4V, then charged at a constant voltage until the current fell to 0.05C or less, and further discharged at a constant current of 0.2C down to 3.0V, and the discharge capacity at 0.2C was recorded.
[0120] At 25°C, the lithium-ion secondary battery was charged at a constant current of 0.2C up to 4.4V, then charged at a constant voltage until the current fell to 0.05C or less, and further discharged at a constant current of 2C down to 3.0V, and the discharge capacity at 2C was recorded.
[0121] Discharge capacity retention rate (%) of lithium ion secondary battery at 2C=discharge capacity at 2C / discharge capacity at 0.2C×100%. See Table 2 for details of the measurement results.
[0122] [Table 1]
[0123] [Table 2]
[0124] The following can be understood from Table 2: a) As can be seen from the comparison between Example 1 and Comparative Examples 1, 2, and 3, by adding a second material to a first positive electrode material and by including a B phase in the second material, it is possible to increase the energy density and also improve the cycle characteristics and rate characteristics.
[0125] b) In Comparative Examples 4 to 5, the weight ratio of the first positive electrode material to the second material in Example 1 was adjusted. As can be seen from the comparison between Example 1 and Comparative Examples 4 to 5, an appropriate weight ratio of the first positive electrode material to the second material can increase the energy density, improve cycle characteristics, and improve rate characteristics. As shown in Comparative Example 5, if the amount of the second material added is too large, the lithium source becomes excessive, and the overall energy density is also lost.
[0126] c) In Comparative Examples 6 to 7, the values of P, Q, and R in Example 1 were adjusted so that R·P / Q was different. As can be seen from a comparison between Example 1 and Comparative Examples 6 to 7, the number of high-temperature cycles was reduced from 475 in Example 1 to 308 / 281, the rate characteristics were reduced from 96.9% to 93.7% / 93.6%, and the energy density was reduced from 778 Wh / L to 641 Wh / L / 722 Wh / L. This shows that an appropriate range of R·P / Q values enhances high-temperature cycle characteristics, rate characteristics, and energy density.
[0127] d) In Comparative Examples 8 to 9, the weight percentage of fluoroethylene carbonate in the electrolyte in Example 1 was adjusted. As can be seen from a comparison between Example 1 and Comparative Examples 8 to 9, the number of high-temperature cycles was reduced from 475 in Example 1 to 276 / 425. This shows that an appropriate fluoroethylene carbonate content is advantageous for improving cycle characteristics, and is also advantageous for improving rate characteristics and energy density.
[0128] e) As can be seen from a comparison of Examples 12 to 13 with Examples 1, 10, 11, 14, and 15, when R·P / Q is 5 to 15 (e.g., 7.31, 7.98), better high-temperature cycle characteristics and rate characteristics are obtained than when R·P / Q is 1 to 32 (e.g., 4.44, 20.36). Therefore, it is more preferable that R·P / Q is in the range of 5 to 15.
[0129] f) The second material in Example 9 was made of phase B. This shows that the second material made of phase B can achieve high energy density, good cycle characteristics, and good rate characteristics.
[0130] As can be seen from the above examples and comparative examples, the combination of the first positive electrode material and the second material produces a synergistic effect. First, the surface of the second material used in the present invention has a low content of free lithium, and by adding it to the positive electrode, the resulting slurry has good stability and excellent processability. Second, the second material used in the present invention has a high initial charge specific capacity and a low initial efficiency, and can better compensate for the loss of active lithium due to the formation of SEI, so that more lithium ions are re-occluded in the lattice of the first positive electrode material during discharge, thereby effectively improving the energy density of the lithium ion secondary battery. Third, the first positive electrode material has good cycle characteristics and a high specific capacity, and the sheet resistance R, compression density P, and single-sided areal density Q of the positive electrode piece can be controlled to be within the range of the present application, thereby providing the lithium ion secondary battery with good cycle characteristics and rate characteristics. Fourth, the fluoroethylene carbonate added to the electrolyte and the lithium supplementary solution can exert a synergistic effect. Specifically, during the first charge, a large amount of active lithium released from the second material is absorbed into the negative electrode, which further reduces the true potential of the negative electrode, and the solvent in the electrolyte continues to undergo a reduction reaction, affecting the cycle characteristics. The use of fluoroethylene carbonate within the scope of the present application as an additive can induce the formation of a denser and thinner SEI layer and prevent the continuous consumption of the electrolyte. In addition, fluoroethylene carbonate has a high resistance to high-pressure oxidation, which makes it more advantageous to combine it with the high-voltage first positive electrode material.
[0131] The above-described embodiments are merely preferred embodiments of the present application, and do not limit the scope of the present application. Any modifications and improvements made by those skilled in the art to the technical solutions of the present application within the scope of the design spirit of the present application should fall within the scope of protection defined by the claims of the present application.
Claims
1. A positive electrode, the positive electrode comprises a first positive electrode material and a second material; The first positive electrode material comprises any of those represented by Formula I: 【Chemistry 1】 In formula I, M 1 contains at least one selected from the group consisting of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn, Ru, Rh, Ga, Pd, Pt, Mo, W, Sb, Nb, Se, Te, and Ce, A contains at least one selected from the group consisting of S, N, F, Cl and Br; x, y, and t satisfy −0.1≦x≦0.2, 0≦y≦0.2, and 0≦t≦0.2; the second material comprises any of those represented by Formula II, 【Chemistry 2】 In Formula II, M 2 and M. 3 each independently contains at least one selected from the group consisting of Co, Mn, Fe, Ti, Al, V, Cr, Nb, Zr, La, and Y, 2 and M. 3 are different elements, D comprises at least one selected from the group consisting of S, N, F, Cl and Br; r, p, q, and s satisfy 0<r≦1, 0<p<1, 0<q<1, 0<p+q≦0.5, 0≦s<0.2, The second material includes a B phase belonging to the F-3m1 space group; A positive electrode comprising:
2. In the first positive electrode material, M 1 contains at least one selected from the group consisting of Ni, Mn, Al, Mg, Ti, Zr, La, Y, Fe, Cr, V, Zn and Rh, and / or A comprises at least one member selected from the group consisting of S and F, and / or x satisfies −0.05≦x≦0.1, and / or y satisfies 0≦y≦0.1; The positive electrode according to claim 1 .
3. In the second material, M 2 and M. 3 each independently contains at least one selected from the group consisting of Co, Mn and Al, and / or D comprises at least one member selected from the group consisting of S and F; and / or p and q satisfy 0<p≦0.2, 0<q≦0.2, 0<p+q≦0.5, and / or r satisfies 0<r≦1, and / or s satisfies 0≦s<0.1; The positive electrode according to claim 1 .
4. the second material is a B-phase belonging to the F-3m1 space group, or the second material includes at least two distinct phases, one of the at least two distinct phases being a B phase belonging to the F-3m1 space group; The positive electrode according to claim 1 .
5. the second material includes two distinct phases, one of the two distinct phases being phase A and the other being phase B; The A phase belongs to the R-3m space group, and in the X-ray diffraction spectrum, a characteristic diffraction peak A of the (003) plane appears at 17° to 19°; The B phase belongs to the F-3m1 space group, and a characteristic diffraction peak of the (001) plane appears at 16° to 18° in the X-ray diffraction spectrum. The positive electrode according to claim 4 .
6. Intensity I of characteristic diffraction peak A A and the intensity of characteristic diffraction peak B I B The relationship between 【Chemistry 3】 Fulfilling The positive electrode according to claim 5 .
7. The positive electrode is (a) in the second material, after the B phase releases excess absorbed lithium, the space group is changed from F-3m1 to R-3m; (b) a weight ratio of the first cathode material to the second material is from 2 to 99:1; and (c) a weight ratio of the first cathode material to the second material is between 3 and 99:1; At least one of the following is satisfied: The positive electrode according to claim 1 .
8. The positive electrode is (i) the positive electrode further includes a binder, a conductive agent, and a solvent, and the content of the first positive electrode material in the positive electrode is 80 wt % to 98 wt %; (ii) the content of the first positive electrode material in the positive electrode is 85 wt % to 98 wt %; (iii) the positive electrode satisfies the following formula IV: 【Chemistry 4】 In Formula IV, R represents the resistance (Ω) of the positive electrode; P is the compressed density of the positive electrode (g / cm 3 ) Q is the surface density (g / 1540.25 mm 2 ) (iv) The positive electrode satisfies the following formula IV-1: 【Chemistry 5】 In formula IV-1, the meanings of R, P, and Q are the same as those in formula IV; (v) the resistance R of the positive electrode satisfies R≦3; (vi) the resistance R of the positive electrode satisfies R≦1.5; (vii) the range of the compressed density P of the positive electrode is 3.4<P<4.2; and (viii) the range of the area density Q of one surface of the positive electrode is 0.16<Q<0.38; At least one of the following is satisfied: The positive electrode according to claim 1 .
9. A lithium ion secondary battery, the lithium ion secondary battery includes a positive electrode, a negative electrode, a separator, and an electrolyte; The positive electrode is any one of the positive electrodes according to any one of claims 1 to 8, the electrolyte solution comprises fluoroethylene carbonate, When the content of the fluoroethylene carbonate in the electrolytic solution is m, the range of the value of m is 0 wt% < m ≦ 15 wt%; A lithium ion secondary battery comprising:
10. A method for preparing a positive electrode according to claim 1, comprising the steps of: A first positive electrode material and a second material are mixed and then coated to obtain the positive electrode; The second material comprises at least a) obtaining a precursor a, said precursor a comprising any of the following formula V: 【Chemistry 6】 In formula V, M 2 , M. 3 , D, p, and q each have the same meaning as in formula II; b) preparing a solution a of a lithium-containing organic compound containing any one selected from the group consisting of lithium naphthalenide, dibiphenyl lithium, and n-butyl lithium, wherein the solvent in the solution a is tetrahydrofuran or ethylene glycol dimethyl ether; and c) immersing precursor a in solution a and reacting to obtain a precipitate of the second material; This is what is obtained by A method for preparing a positive electrode comprising the steps of:
Citation Information
Patent Citations
Positive electrode piece and lithium ion secondary battery
CN110265627A
Lithium ion battery cathode material and preparation method thereof
CN112382749A
Nonaqueous secondary battery
JP2000340229A
Over-lithiated cathodes for lithium ion batteries and processes of manufacture
US20200313157A1
Positive-electrode active material, positive electrode, battery, battery pack, electronic device, electric vehicle, electricity storage apparatus, and power system
WO2016017077A1