Positive electrode piece and lithium ion secondary battery including the same
The positive electrode piece with a specific composition and electrolyte additives enhances lithium-ion secondary battery performance by stabilizing the positive electrode and efficiently replenishing lithium, addressing the challenges of energy density and cycle life.
Patent Information
- Application Number
- JP2024524757
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-25
- Filing Date
- 2021-11-18
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2041-11-18
AI Technical Summary
Existing lithium-ion secondary batteries face challenges in maintaining high energy density and cycle life due to irreversible capacity loss during the formation of the solid electrolyte interface (SEI) on the negative electrode, and methods to replenish lithium at the cathode are not sufficiently safe or efficient.
A positive electrode piece comprising a specific composition of a first cathode active material (Li1+xMn y M2-yO4-tA t ) and a second lithium supplement material (Li1+rMn1-pNpO2-sB s ) with controlled resistance, compressed density, and areal density ratios, along with an electrolyte containing vinylene carbonate and 1,3-propane sultone, to stabilize the positive electrode and enhance lithium replenishment.
The synergistic effect of the specified materials and compositions improves the energy density, rate characteristics, and cycle life of lithium-ion secondary batteries by stabilizing the positive electrode and effectively replenishing lithium, resulting in improved performance.
Smart Images

Figure 2024536612000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode piece and a lithium ion secondary battery including the same. [Background technology]
[0002] In the process of initial charge and discharge of lithium-ion secondary batteries, a solid electrolyte interface (SEI) is formed on the surface of the negative electrode, which causes irreversible capacity loss and reduces the energy density of lithium-ion energy storage devices. In devices using graphite negative electrodes, about 10% of the active lithium source is consumed in the first cycle. When negative electrodes made of high specific capacity materials, such as alloys (silicon, tin, etc.), oxides (silicon oxide, tin oxide), and amorphous carbon, are used, the consumption of the active lithium source becomes even more rapid. Therefore, a suitable lithium replenishment method is of great significance for further improving the energy density of lithium-ion secondary batteries.
[0003] In Patent Document 1, a method of replenishing lithium in the negative electrode is presented. Specifically, metallic lithium powder, a negative electrode material and a non-aqueous liquid are mixed to form a slurry, and the slurry is applied to a current collector. This method can improve the energy density of the battery, but the control of moisture in the production process is very strict, and the process is difficult. FMC, an American company, has made some improvements to the lithium powder, and the stabilized lithium metal powder (SLMP) produced has better stability. However, it can only remain stable for a few hours even in dry air, and there is a large potential danger. When a wet process is adopted, there are also problems with the selection of non-aqueous solvents and the control of moisture.
[0004] The method of replenishing lithium at the negative electrode faces great difficulties, so the industry is increasingly paying attention to a method of replenishing lithium at the positive electrode that is safer and easier to operate. Patent Document 2 discloses a positive electrode replenishing lithium material based on a lithium oxygen compound, a lithium source and an alkyl lithium. However, the decomposition potential of the lithium-containing compound is high, and oxygen and other by-products are generated during the decomposition process, which affects the battery life. Patent Document 3 discloses a Li2NiO2-type lithium replenishing material. The free lithium content on the surface of this type of material is very high, and the slurry has a strong tendency to form a gel during the process of preparing the slurry, which greatly affects the processing performance and causes a continuous increase in impedance, affecting the cycle characteristics. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Chinese patent CN1427490A [Patent Document 2] China patent CN104037418A [Patent Document 3] China patent CN101877417A [Patent Document 4] China patent CN110265627A Summary of the Invention
[0006] The present invention aims to overcome the shortcomings of the prior art by providing a positive electrode piece and a lithium ion secondary battery including the same, and aims to stabilize the positive electrode piece, simplify the processing method, and at the same time, provide the lithium ion secondary battery with high energy density, rate characteristics, and cycle life.
[0007] To achieve the above object, in a first aspect, the present invention provides a positive electrode sheet, the positive electrode sheet including a positive electrode current collector and a positive electrode active material layer provided on at least one surface of the positive electrode current collector, the positive electrode active material layer including a first positive electrode active material and a second positive electrode lithium supplement material, the positive electrode sheet satisfying 1.5 ≦ R·P / Q ≦ 30, where R is the resistance of the positive electrode sheet, the unit of R being Ω, P is the compression density of the positive electrode sheet, the unit of P being g / cm 3 and Q is the areal density per side of the positive electrode sheet, the unit of Q being g / 1540.25 mm 2 .
[0008] Preferably, the first positive electrode active material is Li 1+x Mn y M 2-y O 4-t A t where x, y, and t satisfy -0.1 < x < 0.2, 1 < y ≦ 2, 0 ≦ t < 0.5, M is at least one of Ni, Fe, Zn, Mg, Al, Ti, and Zr, and A is at least one of S, N, F, Cl, and Br.
[0009] Preferably, the second positive electrode lithium supplement material is Li 1+r Mn 1-p N p O 2-s B s where r, p, and s satisfy -0.1 < r < 0.2, 0 ≦ p < 0.2, 0 ≦ s < 0.2, N is at least one of Fe, Co, Ni, Ti, Zn, Mg, Al, V, Cr, and Zr, and B is at least one of S, N, F, Cl, and Br.
[0010] Preferably, the positive electrode sheet satisfies at least one of the following characteristics (a) to (d): (a) The positive electrode sheet satisfies 3.0 ≦ R·P / Q ≦ 15, (b) R satisfies R ≦ 5 Ω, preferably R ≦ 2 Ω, (c) P is 2.5 g / cm 3<P<3.2g / cm 3 Fulfilling (d) The Q is 0.3 g / 1540.25 mm 2 <Q<0.55g / 1540.25mm 2 Meet the following.
[0011] Preferably, the ratio of the weight of the first positive electrode active material to the weight of the second positive electrode lithium supplement material is 5:1 to 99:1 (first positive electrode active material:second positive electrode lithium supplement material). More preferably, the ratio of the weight of the first positive electrode active material to the weight of the second positive electrode lithium supplement material is 9:1 to 99:1 (first positive electrode active material:second positive electrode lithium supplement material).
[0012] Preferably, the weight content of the first positive electrode active material in the positive electrode active material layer is 80% to 98%, and more preferably, the weight content of the first positive electrode active material in the positive electrode active material layer is 85% to 98%.
[0013] In a second aspect, the present invention provides a lithium ion secondary battery, the lithium ion secondary battery comprising the positive electrode pieces, a negative electrode piece, a separator and an electrolyte.
[0014] Preferably, the electrolyte contains, on a weight content basis, 0.001% to 5% vinylene carbonate and / or 0.001% to 5% 1,3-propane sultone.
[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: the second positive electrode lithium supplementary material in the positive electrode piece of the present invention has a very low content of surface free lithium, good slurry stability, and good processing properties; and due to the synergistic effect of the first positive electrode active material and the second positive electrode lithium supplementary material, and by defining the positive electrode piece to satisfy 1.5≦R·P / Q≦30, the resulting lithium ion secondary battery has high energy density, rate characteristics, and cycle life. [Brief description of the drawings]
[0016] [Figure 1]FIG. 1(b) is a partial enlarged view of FIG. 1(a) of the XRD spectrum of the second positive electrode lithium supplementary material in Example 1 before and after the first charge. [Diagram 2] 4 is the initial charge-discharge curve of the second positive electrode lithium supplementary material in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] In order to better illustrate the objectives, technical solutions and advantages of the present invention, the present invention will be further described below with reference to specific examples. Those skilled in the art should understand that the specific examples described herein are only for illustrating the present invention, and are not intended to limit the present invention.
[0018] In the examples, unless otherwise specified, all test methods used are conventional methods, and all materials, reagents, etc. used are available from commercial sources, unless otherwise specified.
[0019] positive electrode piece The positive electrode piece according to the present invention includes a positive electrode current collector and a positive electrode active material layer provided on at least one surface of the positive electrode current collector. In one example, the positive electrode current collector includes two surfaces facing each other in a thickness direction thereof, and the positive electrode active material layer is provided on one or both of the two surfaces.
[0020] In the positive electrode piece of the present invention, the positive electrode active material layer includes a first positive electrode active material and a second positive electrode lithium supplementary material, and the positive electrode piece satisfies 1.5≦R P / Q≦30, where R is the resistance of the positive electrode piece, and the unit of R is Ω; P is the compression density of the positive electrode piece, and the unit of P is g / cm 3 Q is the surface density of the positive electrode piece on one side, and the unit of Q is g / 1540.25 mm 2 It is.
[0021] The first positive electrode active material is Li 1+x Mn y M 2-y O 4-t A twherein x, y, and t satisfy -0.1 < x < 0.2, 1 < y ≤ 2, 0 ≤ t < 0.5, M is at least one of Ni, Fe, Zn, Mg, Al, Ti, and Zr, and A is at least one of S, N, F, Cl, and Br.
[0022] The second positive electrode lithium supplement material is Li 1+r Mn 1-p N p O 2-s B s wherein r, p, and s satisfy -0.1 < r < 0.2, 0 ≤ p < 0.2, 0 ≤ s < 0.2, N is at least one of Fe, Co, Ni, Ti, Zn, Mg, Al, V, Cr, and Zr, and B is at least one of S, N, F, Cl, and Br.
[0023] The positive electrode piece of the present invention uses a first positive electrode active material and a second positive electrode lithium supplementary material with a specific composition. The first positive electrode active material has a stable structure, good cycle stability and high initial coulombic efficiency. The second positive electrode lithium supplementary material has a low content of surface free lithium and good processing characteristics. Compared with the first positive electrode active material, the second positive electrode lithium supplementary material has a high initial charge specific capacity and a low initial discharge specific capacity. That is, the initial coulombic efficiency is low, and a large amount of lithium ions are released from the second positive electrode lithium supplementary material during the first charge to replenish the loss of active lithium due to the formation of SEI, and during the first discharge, sufficient lithium ions are absorbed back into the first positive electrode active material, improving the energy density of the battery. The synergistic effect of the first positive electrode active material and the second positive electrode lithium supplementary material effectively improves the energy density, rate characteristics and cycle life of the lithium ion secondary battery. Compared with the combination of the first positive active material and the second positive active material in the previously filed Patent Publication 4, the combination of the first positive active material and the second positive lithium supplementary material used in the present invention can more significantly improve the energy density, rate characteristics and cycle life of the lithium ion secondary battery. At the same time, the present invention specifically designs the resistance R, compression density P and single-sided area density Q of the positive electrode piece, which can further improve the energy density, rate characteristics and cycle life of the lithium ion secondary battery, and realizes the organic integration of high energy density, good rate characteristics and long cycle life.
[0024] In order to realize the function of lithium supplementation, the second positive electrode lithium supplement material in the present invention satisfies 1-p>0.8 (i.e., 0≦p<0.2). Specifically, the second positive electrode lithium supplement material in the present invention has two phase structures, which belong to the Pmmn space group and the C2 / m space group, respectively, the Pmmn space group corresponds to the characteristic diffraction peak A appearing at 15°-16° in the line diffraction spectrum, the C2 / m space group corresponds to the characteristic diffraction peak B appearing at 18°-19° in the line diffraction spectrum, and the intensity I of the characteristic diffraction peak B B Intensity of characteristic diffraction peak A vs. I A Ratio I A / I B is 0 A / I B After the first charge, the characteristic diffraction peak A and the characteristic diffraction peak B both shift to lower angles, and the shift widths are both <0.5°.
[0025] In the present invention, in order to ensure that the lithium ion secondary battery has high energy density, rate characteristics and cycle life, the positive electrode piece needs to satisfy 1.5≦R·P / Q≦30. In some embodiments of the present invention, R·P / Q is one of the following values: 1.5, 3, 6, 9, 12, 15, 18, 21, 24, 27, 30, etc. In some preferred embodiments of the present invention, R·P / Q is 3.0≦R·P / Q≦15, so that the obtained lithium ion secondary battery has longer cycle life and rate characteristics. For example, R·P / Q is one of the following values: 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, etc.
[0026] In this specification, the calculation of R P / Q involves only numerical calculations. For example, the resistance R of the positive electrode strip is 1.0 Ω and the compaction density P is 3.0 g / cm 3 The surface density Q of the positive electrode piece on one side is 0.35 g / 1540.25 mm 2 Then, R P / Q = 8.57.
[0027] The resistance R of the positive electrode is the resistance measured by the DC two-probe method, of which the contact area between the probe and the positive electrode is 49πmm 2 In the present invention, the resistance R of the positive electrode piece was measured using a HIOKI BT23562 type internal resistance measuring device during research, and the specific operation is as follows: the upper and lower sides of the positive electrode piece were sandwiched between two conductive terminals of the measuring device, and pressure was applied to fix the positive electrode piece, the diameter of the conductive terminal was 14 mm, and the pressure applied was 15 MPa to 27 MPa, and the resistance R of the positive electrode piece was measured.
[0028] The compressed density P of the positive electrode piece can be calculated from the formula P=m / v, where m is the weight of the positive electrode active material layer, m is in g, and v is the volume of the positive electrode active material layer, v is in cm. 3The volume v of the positive electrode active material layer is the area A of the positive electrode active material layer. r and the thickness of the positive electrode active material layer.
[0029] The surface density Q of one side of the positive electrode piece is calculated by the formula Q = 1540.25 m / A r In this formula, m is the weight of the positive electrode active material layer, and the unit of m is g, and A r is the area of the positive electrode active material layer, and A r The unit is mm 2 It is.
[0030] In addition, the film resistance R, compression density P, and surface density Q of the positive electrode piece are important parameters in the design and manufacture of lithium ion secondary batteries. If the film resistance R of the positive electrode piece is too large, the cycle characteristics and rate characteristics of the lithium ion secondary battery will deteriorate. If the compression density P is too large or too small, the cycle characteristics and rate characteristics of the lithium ion secondary battery will deteriorate. If the surface density Q of one side of the positive electrode piece is too large, the cycle life of the lithium ion secondary battery will be reduced, affecting the penetration of the electrolyte, and further affecting the rate characteristics of the battery, especially reducing the high-rate discharge capacity of the battery. If the surface density Q of one side of the positive electrode is too small, the length of the current collector and separator will increase for the same battery capacity, and the internal resistance of the electrochemical device will increase. Therefore, in order to obtain the expected results of the electrochemical characteristics of the lithium ion secondary battery, it is necessary to comprehensively design these parameters during the manufacture of the battery so that the positive electrode piece reaches the expected design value.
[0031] Since it is advantageous to improve the cycle characteristics and rate characteristics of the lithium ion secondary battery, it is preferable that the film resistance R of the positive electrode piece satisfies R≦5Ω. In order to further improve the cycle characteristics and rate characteristics of the lithium ion secondary battery, it is more preferable that the film resistance R of the positive electrode piece satisfies R≦2Ω.
[0032] Preferably, the positive electrode piece has a compressed density P of 2.5 g / cm 3 <P<3.2g / cm 3which is favorable for the transfer of electrons and ions in the positive electrode piece, thereby improving the cycle characteristics of the lithium ion secondary battery.
[0033] Preferably, the surface density Q of one side of the positive electrode piece is 0.3 g / 1540.25 mm 2 <Q<0.55g / 1540.25mm 2 This satisfies the above requirements, and while ensuring the charge / discharge capacity, it is possible to improve the cycle characteristics and rate characteristics of the lithium ion secondary battery.
[0034] Preferably, the weight ratio of the first positive active material to the weight of the second positive lithium supplementary material is 5:1 to 99:1, and such positive pieces are mostly the first positive active material, which has higher structural stability, reduces capacity loss and resistance increase due to structural destruction of the positive active material, and can maintain cycle stability and dynamic characteristics. Preferably, the weight ratio of the first positive active material to the weight of the second positive lithium supplementary material is 9:1 to 99:1, which further improves cycle stability and dynamic characteristics.
[0035] The weight content of the first positive electrode active material in the positive electrode active material is 80% to 98%, and more preferably 85% to 98%.
[0036] In the positive electrode chip of the embodiment of the present invention, the positive electrode active material layer further includes a conductive agent and a binder. The present invention does not have any particular limitations on the types of the conductive agent and the binder, and they can be selected according to actual needs.
[0037] For example, the conductive agent may be at least one of graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, carbon nanofibers, and the like, and the binder may be at least one of styrene butadiene rubber (SBR), water based acrylic resin, carboxymethyl cellulose (CMC), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer (EVA), polyvinyl alcohol (PVA), and the like.
[0038] In some optional embodiments, the weight content of the conductive agent in the positive electrode active material layer is ≧0.5%, which is advantageous for obtaining low positive electrode film resistance.
[0039] In some alternative embodiments, the weight content of the binder in the positive electrode active material layer is ≦2.0%, which is advantageous for obtaining low positive electrode film resistance.
[0040] The positive electrode current collector may be a metal foil material or a porous metal plate, for example, a foil material or a porous plate formed using a metal such as aluminum, copper, nickel, titanium, or silver, or an alloy thereof, for example, aluminum foil.
[0041] The thickness of the positive electrode current collector is preferably 5 μm to 20 μm, more preferably 6 μm to 18 μm, and further preferably 8 μm to 16 μm.
[0042] Lithium-ion secondary battery The positive electrode piece of the present invention can be used as the positive electrode of lithium ion secondary battery. The lithium ion secondary battery includes a positive electrode piece, a negative electrode piece, a separator and an electrolyte, of which the positive electrode piece is the positive electrode piece of the present invention. By using the positive electrode piece of the present invention, the lithium ion secondary battery of the present invention has high energy density, cycle characteristics and rate characteristics at the same time.
[0043] The negative electrode pieces may be metallic lithium pieces and may include a negative electrode current collector and a negative electrode active material layer provided on at least one surface of the negative electrode current collector.
[0044] The negative electrode active material layer usually includes a negative electrode active material, a conductive agent, a binder, and a thickener. Examples of the negative electrode active material include natural graphite, artificial graphite, mesocarbon microbeads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, SiO, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, and lithium titanate with a spinel structure Li4Ti5O. 12 , Li-Al alloy, and metallic lithium, etc., the conductive agent may be at least one of graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, carbon nanofibers, etc., the binder may be at least one of styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), water-based acrylic resin, carboxymethyl cellulose (CMC), etc., and the thickener may be carboxymethyl cellulose (CMC), etc. However, the present invention is not limited to these materials, and other materials that can be used as negative electrode active materials, conductive agents, binders, and thickeners for lithium ion secondary batteries can also be used.
[0045] The negative electrode current collector may be a metal foil material or a porous metal plate, for example, a foil material or a porous plate formed using a metal such as copper, nickel, titanium, iron, or an alloy thereof, for example, copper foil.
[0046] The negative electrode pieces can be manufactured according to conventional methods in the art. Typically, the negative electrode active material, and any conductive agent, binder, and thickener are dispersed in a solvent to form a uniform negative electrode slurry. The solvent may be N-methylpyrrolidone (NMP) or deionized water. The negative electrode slurry is applied to a negative electrode current collector, and the negative electrode pieces are obtained through processes such as drying and cold pressing.
[0047] The separator is not particularly limited, and any known separator having a porous structure and having electrochemical and chemical stability may be selected and used, for example, a single-layer or multi-layer film of at least one of glass fiber, nonwoven fabric, polyethylene (PE), polypropylene (PP), and polyvinylidene fluoride (PVDF).
[0048] The electrolyte includes an organic solvent, an electrolyte lithium salt, and an additive. The present invention does not limit the types of the organic solvent and the electrolyte lithium salt, and may be selected according to actual needs.
[0049] For example, the organic solvent may be at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), and diethyl sulfone (ESE), and preferably two or more of these.
[0050] The electrolyte lithium salt may be one or more of LiPF6 (lithium hexafluorophosphate), LiBF4 (lithium tetrafluoroborate), LiClO4 (lithium perchlorate), LiAsF6 (lithium hexafluoroarsenate), LiFSI (lithium bis(fluorosulfonyl)imide), LiTFSI (lithium bis(trifluoromethanesulfonyl)imide), LiTFS (lithium trifluoromethanesulfonate), LiDFOB (lithium difluoro(oxalato)borate), LiBOB (lithium bis(oxalato)borate), LiPO2F2 (lithium difluorophosphate), LiDFOP (lithium difluoro(oxalato)phosphate), LiTFOP (lithium tetrafluoro(oxalato)phosphate), and the like.
[0051] The additive of the electrolyte includes vinylene carbonate (VC), and the weight content of the vinylene carbonate is 0 to 5% based on the total weight of the electrolyte, but not 0. By adding the additive of vinylene carbonate to the electrolyte, a more uniform and dense SEI film is formed on the negative electrode, and the continuous loss of active lithium is suppressed.
[0052] The additive of the electrolyte includes 1,3-propane sultone (PS), and the content by weight of the 1,3-propane sultone relative to the total weight of the electrolyte is 0 to 5%, but not 0. By adding 1,3-propane sultone to the electrolyte, an interface protection layer is formed on the positive electrode side, and the cycle life of the lithium ion secondary battery can be further improved.
[0053] The electrolyte may optionally contain other additives, which may be any additives that can be used as additives in lithium ion batteries, and the present invention is not particularly limited and may be selected according to actual needs. For example, the additives may further include one of vinyl ethylene carbonate (VEC), succinonitrile (SN), adiponitrile (AND), 1,3-propene sultone (PST), sulfonic acid ester cyclic quaternary ammonium salt, tris(trimethylsilyl)phosphate (TMSP), and tris(trimethylsilyl)borate (TMSB).
[0054] The above-mentioned electrolyte solution can be prepared according to the conventional method in the art. The organic solvent, the electrolyte lithium salt, the vinylene carbonate, the 1,3-propane sultone and other optional additives are mixed uniformly to obtain the electrolyte solution, and the order of adding each material is not particularly limited. For example, the electrolyte lithium salt, the vinylene carbonate, the 1,3-propane sultone and other optional additives are added to the organic solvent, and mixed uniformly to obtain the electrolyte solution. The electrolyte lithium salt can be added to the organic solvent, and then the vinylene carbonate, the 1,3-propane sultone and other optional additives can be added to the organic solvent separately or simultaneously.
[0055] The positive electrode piece, separator, and negative electrode piece are stacked in order, and the separator is placed between the positive electrode and the negative electrode to serve as an insulator to obtain a cell. Alternatively, the cell is wound up to obtain a cell. The cell is placed in an outer case, and an electrolyte is poured in and sealed to obtain a lithium ion secondary battery.
[0056] In the study of the present invention, the charge / discharge curve, high-temperature cycle characteristics and rate characteristics of the lithium ion secondary battery are measured by the following methods.
[0057] Measurement of charge-discharge curve: At 45°C, the lithium-ion secondary battery was charged at a constant current of 0.1C to 4.3V, then charged at a constant voltage until the current reached or was less than 0.025C, and then discharged at a constant current of 0.1C to 3.0V, and the charge-discharge curve of the lithium-ion secondary battery was recorded.
[0058] High-temperature cycle characteristic measurement: At 45°C, the lithium-ion secondary battery was charged at a constant current of 1.5C up to 4.3V, and then charged at a constant voltage until the current became 0.05C or less, and then discharged at a constant current of 3.0V at a rate of 1C, which was regarded as one charge-discharge cycle. The discharge capacity of the first cycle of the lithium-ion secondary battery was recorded. The lithium-ion secondary battery was subjected to charge-discharge cycles according to the above method, and the discharge capacity of each cycle was recorded. When the discharge capacity of the lithium-ion secondary battery was attenuated to 80% of the discharge capacity of the first cycle, the cycle was terminated, and the number of charge-discharge cycles was recorded.
[0059] Rate characteristic measurement: At 25°C, the lithium ion secondary battery was charged at a constant current of 0.2C to 4.3V, and then charged at a constant voltage until the current became 0.05C or less, and then discharged at a constant current of 0.2C to 3.0V, and the discharge capacity at the 0.2C rate was recorded. At 25°C, the lithium ion secondary battery was charged at a constant current of 0.2C to 4.3V, and then charged at a constant voltage until the current became 0.05C or less, and then discharged at a constant current of 2C to 3.0V, and the discharge capacity at the 2C rate was recorded. Discharge capacity retention rate (%) at the 2C rate of the lithium ion secondary battery = discharge capacity at the 2C rate / discharge capacity at the 0.2C rate × 100%.
[0060] Example 1 Preparation of the positive electrode piece: The first positive electrode active material LiMn2O4, the second positive electrode lithium supplement material LiMnO2, the binder PVDF and conductive carbon black are mixed, in which the weight ratio of LiMn2O4, LiMnO2, PVDF and conductive carbon black is 92.5:4.0:1.5:2.0, the solvent NMP is added in a ratio of 7:3 of material to liquid, and the mixture is stirred under vacuum stirring until it becomes a uniform and transparent system, to obtain a positive electrode slurry. The positive electrode slurry is uniformly applied to the aluminum foil of the positive electrode current collector, and then transferred to an oven to dry, the drying temperature is 120°C, and the positive electrode is obtained by cold pressing and slitting. The weight content of the first positive electrode active material LiMn2O4 in the positive electrode active material layer is 92.5%, and the weight content of the second positive electrode lithium supplement material LiMnO2 in the positive electrode active material layer is 4.0%.
[0061] Preparation of negative electrode pieces: The negative electrode active material artificial graphite, the thickener sodium carboxymethylcellulose (CMC), the binder (SBR) and the conductive carbon black were mixed in a mass ratio of 95.7:1.0:1.8:1.5, and the solvent deionized water was added in a material to liquid ratio of 4:6, and the negative electrode slurry was obtained by the action of a vacuum stirrer. The negative electrode slurry was uniformly applied to the copper foil of the negative electrode current collector, and then transferred to an oven for drying, the drying temperature was 120°C, and the negative electrode pieces were obtained by cold pressing and slitting.
[0062] Preparation of electrolyte: Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were mixed uniformly in a volume ratio of 1:1:1 to obtain an organic solvent. LiPF6 was dissolved in the above organic solvent, and the concentration of LiPF6 was 1 mol / L. 3% by weight of vinylene carbonate and 3% by weight of 1,3-propane sultone were further added based on the total mass of the electrolyte, and mixed uniformly to obtain an electrolyte.
[0063] Preparation of lithium ion secondary battery: A positive electrode piece, a separator, and a negative electrode piece were laminated in this order. The separator was a polypropylene (PP) film (provided by Celgard) with a thickness of 14 μm, and was located between the positive electrode piece and the negative electrode piece to serve as an insulator. Then, the separator was wound around the electrode assembly, a tab was welded, the electrode assembly was placed in an outer case, an electrolyte was injected, and the case was sealed. After that, the battery was left to stand, formed, shaped, and other processes to obtain a lithium ion secondary battery.
[0064] Examples 2 to 27 The difference from Example 1 is that the material components in the positive electrode and the correlation parameters in the manufacturing steps are adjusted, as shown in Table 1 (in this table, the weight content of the first positive electrode active material is the weight content of the first positive electrode active material in the positive electrode active material, and the weight content of the second positive electrode lithium supplementary material is the weight content of the second positive electrode lithium supplementary material in the positive electrode active material).
[0065] Comparative Example 1 The difference from Example 1 was that the positive electrode contained only LiMn2O4.
[0066] Comparative Example 2 The difference from Example 1 was that the positive electrode contained only LiMnO2.
[0067] Comparative Examples 3 to 4 The difference from Example 1 was that the ratio of the weight of the first positive electrode active material to the weight of the second positive electrode lithium supplement material in the positive electrode was different.
[0068] Comparative Examples 5 to 6 The difference from Example 1 was that the film resistance, compression density, and surface density of the positive electrode piece were different.
[0069] Comparative Examples 7 to 8 The difference from Example 1 was that the weight contents of vinylene carbonate and 1,3-propane sultone in the electrolyte were different.
[0070] Comparative Examples 9 to 10 The difference from Example 26 was that the electrolyte contained only vinylene carbonate or only 1,3-propane sultone.
[0071] In each of the Examples and Comparative Examples, except for Example 18, in which the content of the conductive carbon black and the content of the PVDF as the binder in the positive electrode active material were each 0.5 wt%, the content of the conductive carbon black in the positive electrode active material was 2.0 wt%, and the content of the PVDF as the binder was 1.5 wt%.
[0072] According to the above-mentioned methods, the high-temperature cycle characteristics and rate characteristics of the lithium ion secondary batteries obtained in each of the Examples and Comparative Examples were measured. The results are shown in Table 2.
[0073] [Table 1-1] [Table 1-2]
[0074] [Table 2-1] [Table 2-2] [Table 2-3]
[0075] As can be seen from the above examples and comparative examples, (1) in the present invention, a synergistic effect is obtained by using the first positive electrode active material and the second positive electrode lithium supplement material together. First, the second positive electrode lithium supplement material used in the present invention has a low content of surface free lithium, and when it is added to the positive electrode, the resulting slurry has good stability and good processing properties. Second, the second positive electrode lithium supplement material used in the present invention has a high initial charge specific capacity and a low initial coulombic efficiency, and can better supplement the loss of active lithium due to the formation of SEI, and during discharge, more lithium ions are absorbed back into the crystal lattice of the first positive electrode active material, effectively improving the energy density of the lithium ion secondary battery. Third, the first positive electrode active material has a stable structure and good cycle stability, and by controlling the film resistance R, compression density P, and single-sided areal density Q of the positive electrode piece within the range of the present invention, the lithium ion secondary battery can have good cycle characteristics and rate characteristics. (2) The lithium replenishment method using vinylene carbonate, the first positive electrode active material, and the second lithium replenishment active material added to the electrolyte can exert a synergistic effect. During the first charge, a large amount of active lithium released from the second positive electrode lithium replenishment material is absorbed into the negative electrode, which further reduces the true potential of the negative electrode and causes the solvent in the electrolyte to continue to undergo a reduction reaction, affecting the cycle characteristics. The use of the vinylene carbonate additive within the scope of the present invention can induce the formation of a denser and thinner SEI layer and prevent continuous consumption of the electrolyte. In addition, the addition of 1,3-propane sultone additive to the electrolyte can form an interface protection layer on the surface of the positive electrode active material, further improving the cycle characteristics.
[0076] Finally, it should be noted that the above embodiments are only used to describe the technical solutions of the present invention, and do not limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, it should be understood that those skilled in the art can modify or replace the technical solutions of the present invention without departing from the spirit and scope of the present invention.
Claims
1. A positive electrode piece, A positive electrode current collector and a positive electrode active material layer provided on at least one surface of the positive electrode current collector, the positive electrode active material layer includes a first positive electrode active material and a second positive electrode lithium supplement material; The positive electrode piece satisfies 1.5≦R·P / Q≦30, R is the resistance of the positive pole piece, R is in Ω; P is the compressed density of the positive electrode piece, and P is expressed in g / cm 3 and Q is the surface density of one side of the positive electrode piece, and the unit of Q is g / 1540.25 mm 2 Characterized in that Positive electrode piece.
2. The first positive electrode active material is Li 1+x Mn y M 2-y O 4-t A t and x, y, and t satisfy −0.1<x<0.2, 1<y≦2, 0≦t<0.5; M is at least one of Ni, Fe, Zn, Mg, Al, Ti, and Zr; 2. The cathode piece of claim 1, wherein A is at least one of S, N, F, Cl, and Br.
3. The second positive electrode lithium supplement material is Li 1+r Mn 1-p N p O 2-s B s and r, p, and s satisfy −0.1<r<0.2, 0≦p<0.2, 0≦s<0.2, N is at least one of Fe, Co, Ni, Ti, Zn, Mg, Al, V, Cr, and Zr; The cathode piece of claim 1 , wherein B is at least one of S, N, F, Cl, and Br.
4. Satisfying at least one of the following characteristics (a) to (d): (a) the positive electrode piece satisfies 3.0≦R·P / Q≦15; (b) the R satisfies R≦5Ω, preferably R≦2Ω; (c) The P is 2.5 g / cm 3 <P<3.2g / cm 3 Fulfilling (d) The Q is 0.3 g / 1540.25 mm 2 <Q<0.55g / 1540.25mm 2 Fulfilling The positive electrode piece according to claim 1 .
5. 2. The positive electrode piece according to claim 1, wherein a ratio of the weight of the first positive electrode active material to the weight of the second positive electrode lithium supplement material is 5:1 to 99:
1.
6. 6. The positive electrode piece according to claim 5, wherein a weight ratio of the first positive electrode active material to the second positive electrode lithium supplement material is 9:1 to 99:
1.
7. The positive electrode piece according to claim 1 , wherein the weight content of the first positive electrode active material in the positive electrode active material layer is 80% to 98%.
8. The positive electrode piece according to claim 7, wherein the weight content of the first positive electrode active material in the positive electrode active material layer is 85% to 98%.
9. A lithium ion secondary battery, The battery includes a positive electrode piece, a negative electrode piece, a separator, and an electrolyte. A lithium ion secondary battery, characterized in that the positive electrode piece is the positive electrode piece according to any one of claims 1 to 8.
10. 10. The lithium ion secondary battery according to claim 9, wherein the electrolyte contains, by weight, 0.001% to 5% vinylene carbonate and / or 0.001% to 5% 1,3-propane sultone.
Citation Information
Patent Citations
Secondary battery with non-aqueous electrolyte
CN102637894A
Positive electrode piece and lithium ion secondary battery
CN110265627A
Positive electrode active material containing additive for improving overdischarge performance and lithium secondary battery using the same
JP2006512747A
Nonaqueous electrolyte secondary battery
JP2015018599A
Increased energy density and swelling control in batteries for portable electronic devices
US20140065462A1