Method for manufacturing electrodes for solid-state battery cells

A two-step method for producing gel polymer electrolytes in solid-state batteries by applying a copolymer coating before calendering and forming the electrolyte within the assembled cell addresses inefficiencies in current methods, enhancing production efficiency and stability while reducing costs and thermal risks.

JP2024536783AActive Publication Date: 2024-10-08パワーコエスエー
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024517020
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-17
Filing Date
2022-09-14
Publication Date
2024-10-08
Estimated Expiration
2042-09-14

AI Technical Summary

Technical Problem

Current methods for producing gel polymer electrolytes in solid-state battery cells face inefficiencies such as high manufacturing costs, thermal instability, and handling difficulties due to the sticky nature of gel-like coatings, which complicate processes like cutting and lamination, and require expensive lithium salts and dry environments.

Method used

A two-step method involving the application of a copolymer as a coating on the electrode substrate before calendering, followed by electrolyte addition and gel formation within the assembled battery cell, allowing for easier handling and reduced thermal stress, using cost-effective lithium salts and avoiding high temperatures.

Benefits of technology

This method simplifies the production process, reduces costs, enhances ionic conductivity, and improves the stability of the gel polymer electrolyte, enabling efficient mass production of solid-state batteries with improved handling and reduced risk of thermal runaway.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536783000001_ABST
    Figure 2024536783000001_ABST
Patent Text Reader

Abstract

A method for manufacturing a first electrode (1) of a battery cell (2), the method comprising at least the following steps: a) providing a substrate (3) for the first electrode (1) comprising at least an active material (4) of the first electrode (1) and a copolymer (5); and b) wetting the substrate (3) with a liquid electrolyte (6) and forming a gel polymer electrolyte (7) by reacting the copolymer (5) with the liquid electrolyte (6) to form the first electrode (1).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing an electrode for a solid-state battery cell. The term "solid-state battery cell" is hereinafter also included in the term "battery cell".

[0002] Batteries, in particular lithium-ion batteries, are increasingly being used to drive motor vehicles. In particular, motor vehicles, for example, have electric machines for driving themselves, which can be driven by electrical energy stored in battery cells. Batteries usually consist of battery cells, where each battery cell has a stack of anode sheets, cathode sheets and separator sheets. At least some of the anode and cathode sheets are configured as electrical conductors that conduct the electrical current provided by the cell to an electrical load arranged outside the cell. Battery cells with liquid or solid electrolytes (solid-state batteries) are known.

[0003] The electrodes described herein are used in solid-state battery cells (all-solid-state battery cells and polymer-gel battery cells), i.e. the solid-state battery cells contain exclusively solid components (e.g. polymers, including semi-solid electrolytes, i.e. solid or gel electrolytes, and thus not just liquid electrolytes). These solid or gel electrolytes are not only arranged as ion-conducting separators between the electrodes, but also for ion conduction within the electrodes. These separators are typically made of ceramic materials or polymers, glasses or hybrid materials.

[0004] A solid-state battery cell comprises a particularly gas-tightly constructed casing in which at least one stack of electrode films or electrode layers arranged on top of one another, also referred to as electrodes, is arranged. The casing can be designed as a shape-fixed casing (prismatic cell) or at least partially made of an elastically deformable film material (pouch cell). The two types of casing can also be combined.

[0005] In the manufacture of electrodes for solid-state battery cells, so-called support materials, in particular strip-shaped support materials, such as support films, are at least partially coated on one or both sides with active material (in particular additionally comprising a solid electrolyte, a gel electrolyte being optionally provided later). Electrical conductors (conductor leads) formed in the electrodes are formed in particular by uncoated areas of the support material. Support materials include, for example, copper, copper alloys, aluminum or aluminum alloys.

[0006] The coating formed from the active materials in this way is initially porous, which is reduced by calendering, since in this case the coating is compressed, which is required to increase the specific capacitance (by volume) and the electrical conductivity, or to ensure charge transport through the materials in contact with each other of the active materials.

[0007] During calendering, the active material of the solid-state battery cell is compressed to a porosity of less than 1%, with the gelled electrolyte retaining a particularly large porosity. In this case, the porosity is reduced by 20% to 50% as a result of the calendering. The calendering process is similar to a rolling process. The active material is compressed by applying a calendering force in a deformation zone. The calendering device includes a number of rollers forming at least one gap, through which the electrodes are conveyed along the conveying direction.

[0008] Polymer electrolytes that have been earmarked for application in lithium cells fall into two main categories: (1) those based on pure high polymers that are used both as a solvent to dissolve the lithium salt and as a mechanical matrix to aid processability; and (2) Based on polymers gelled by conventional electrolyte solutions, in which small organic molecules are used as the main solvents, while a small proportion of high polymers completely swollen by these solvents are used only to ensure shape stability; can be distinguished as follows.

[0009] The first polymer electrolyte is usually called Solid Polymer Electrolyte (SPE), and the second is called Gel Polymer Electrolyte (GPE). The poor ionic conductivity at room temperature makes SPE unlikely to be applied. On the other hand, GPE has proven to be of practical value, and second generation lithium-ion cells (e.g. solid-state batteries, i.e. all-solid-state batteries) are already being manufactured with these new electrolytes.

[0010] GPEs are primarily used in the cathode of solid-state batteries and are therefore also called catholytes. For this purpose, a hot polymer solution (at about 90°C) consisting of a polymer (e.g., a polymer based on poly(vinylidene fluoride-co-hexafluoropropylene), i.e., PVdF-HFP) is used mixed with a convective electrolyte, e.g., propylene carbonate (PC), dimethyl carbonate (DMC) and a lithium salt such as lithium hexafluorophosphate (LiPF6) or a new lithium salt such as lithium bis(fluorosulfonyl)imide (LiFSi).

[0011] Conventional methods for introducing GPEs into the cathode can have the following drawbacks: · Typically, GPEs are deposited at high temperatures followed by calendering with an excess of conventional electrolyte to reduce their viscosity and increase wetting of the porous electrode structure. After cooling, the GPE-coated electrodes are difficult to laminate with the cathode and anode and separator due to their gel-like behavior. The sticky nature of the gel-like coating also makes the cathode difficult to handle for further processing. · In conventional methods for producing GPEs, a liquid electrolyte must be heated with a polymer to form a gel, where the thermal instability of the lithium salt (LiPF6 or LiBF4) and the volatility of the solvent (DMC, EMC, etc.) can cause the resulting GPE to deviate from the desired composition or even decompose. Furthermore, conventional electrolytes such as LiPF6 / EC (ethylene carbonate) / DMC cannot be used because, for example, the lithium salt LiPF6 is not stable above 55°C. DMC also starts to boil at 90°C, so expensive lithium salts such as lithium bis(fluorosulfonyl)imide (LiFSi) that are thermally stable at this temperature must be used. Since LiPF6 forms hydrofluoric acid (HF) very quickly in the presence of even traces of moisture, the entire process must be carried out in a dry space after insertion of the GPE into the cathode, which increases production costs. Although it is important for the liquid electrolyte to swell the polymer to form the GPE, the swelling of PVdF-HFP by the liquid electrolyte is not complete due to the semi-crystalline nature of the copolymer, which has a tendency to lead to the formation and separation of microphases after activation with the liquid electrolyte, and the multiphasic nature of the GPE (liquid, gel and crystalline solid) makes it difficult to handle in subsequent processes such as cutting and lamination. During calendering, the porosity in the active material of the electrode is reduced. GPE is currently applied to the cathode after calendering, but due to the small pore size, it is difficult for the liquid electrolyte and GPE to penetrate into the pores of the active material, and high temperatures are required to reduce the viscosity so that the electrolyte and GPE can penetrate into the pores. High temperatures here result in further degradation of the electrolyte.

[0012] In summary, it can be seen that the current methods of introducing GPEs into or onto the cathode are not efficient methods.

[0013] In order to avoid the above problems in the conventional application of GPE, the following measures can be considered: Uses expensive lithium salts such as lithium bis(fluorosulfonyl)imide (LiFSi), which is thermally stable at temperatures around 90°C. Increasing the amount of low viscosity solvent as excess electrolyte (e.g. amount of dimethyl carbonate (DMC) in liquid electrolyte) to improve wettability of electrodes or active materials, however this has the drawback of requiring an additional drying step (which is inefficient and time consuming). Increasing the process temperature to reduce the viscosity. In this case, other solvents or additives must be used to avoid boiling of DMC at, for example, about 90°C. Note that although a low processing temperature can contribute to a stable DMC, it also has a negative effect, since the viscosity of the liquid electrolyte increases and the active material cannot easily penetrate into the pores. Since LiPF6 is sensitive to moisture, the entire process of producing the GPE and its application to the cathode must be carried out in a dry space, with all subsequent processes likewise to be carried out in a dry space. · Handling of GPE-coated cathodes in later processes such as cutting and lamination remains an open problem.

[0014] The most important drawbacks of the above measures are in some cases: · Expensive lithium salts further increase the cost of GPE. Dry space leads to high production costs. The high temperatures required for GPE (approximately 90°C) decompose the other components of the liquid electrolyte, namely the lithium salt LiPF6 and dimethyl carbonate (DMC). The gel-like surface of the cathode creates problems in handling during subsequent processes such as cutting and laminating the electrodes.

[0015] From DE 10020031 A1 a method for producing lithium polymer batteries is known, in which a polymer gel electrolyte is laminated together with the active material for the anode and the active material for the cathode onto a successively occurring collector film.

[0016] From WO 01 / 82403 a method for producing a lithium polymer battery is known.

[0017] From WO 02 / 19450 a method is known for producing a laminate component of a battery cell, the laminate component comprising a layer of gel polymer electrolyte and a layer of active material.

[0018] The object of the present invention is to at least partially solve the problems mentioned in connection with the prior art. In particular, a method for producing electrodes for solid-state battery cells is proposed, in which cutting and / or stacking of the individual electrodes is particularly simplified.

[0019] To achieve this object, a method having the features of the independent claims contributes. Advantageous developments are the subject of the respective dependent claims. The features individually recited in the claims can be combined with one another in a technically significant manner and can be supplemented by facts stated in the description and / or details of the drawings, which show further variant embodiments of the invention.

[0020] A method for manufacturing a first electrode of a solid-state battery cell (hereinafter referred to as battery cell) is proposed. The method comprises at least the following steps: a) providing a first electrode substrate comprising at least an electrode active material and a copolymer; b) wetting the substrate with a liquid electrolyte and reacting the copolymer with the liquid electrolyte to form a gel polymer electrolyte to form a first electrode; Includes.

[0021] Known methods for producing uniform GPE coatings on electrodes are not efficient and are in particular replaced by a two-stage method, in which first an electrode substrate is prepared with only the copolymer as starting material for the gel polymer electrolyte. At least the electrode material is cut in this state to the geometric shape of the electrode present in the solid-state battery cell. Only then, preferably, are the electrodes stacked on top of each other to form a stack, and only after the stack is placed in the casing of the solid-state battery cell is the electrolyte added and the gel polymer electrolyte formed.

[0022] In step a), in particular the active material is prepared and optionally placed on the support material. When producing electrodes for solid-state battery cells, the support material, in particular a strip-shaped support material, for example a support film, can be at least partially coated on one or both sides with the active material. Electrical conductors (conductor leads) formed at the electrodes are formed in particular by uncoated areas of the support material. The support material can, for example, comprise copper or a copper alloy for the anode and aluminum or an aluminum alloy for the cathode. Thus, the substrate can comprise the active material, the support material and the copolymer.

[0023] In particular, in step a), the copolymer is mixed with the active material to form a material mixture, which is then placed on the support material. In particular, the copolymer is substantially uniformly distributed in the material mixture. If the formation of a gel polymer electrolyte is performed in the framework of step b), the gel polymer electrolyte is also uniformly distributed in the material mixture of the subsequently formed first electrode.

[0024] However, such mixing of copolymers may have drawbacks in some cases. For example, the reaction of NMP (N-methyl-2-pyrrolidone; solvent for the preparation of the coating material with active material of the first electrode) with the copolymer may cause an increase in density and thus an increase in viscosity of the coating material. This may cause problems when coating the support material of the first electrode (i.e., for example, aluminum substrate and / or copper substrate) with the coating material, or may irreversibly damage the copolymer of the subsequent gel polymer electrolyte.

[0025] It is desirable that the surface of the first electrode is completely covered by the gel polymer electrolyte, so that the gel polymer electrolyte has good contact with the solid electrolyte separator used in the battery cell, which facilitates ion transfer. Such a gel polymer electrolyte layer on the surface of the first electrode is not manufacturable, especially when the copolymer and the active material are mixed to form a material mixture.

[0026] Thus, preferably, the copolymer is deposited on the active material as a coating in step a1) carried out during step a). In particular, the copolymer is additionally arranged in the active material in the form of a material mixture. Alternatively, the copolymer is exclusively arranged in the coating.

[0027] In solid-state batteries, usually only the cathode is coated with gel polymer electrolyte, while the anode is made of lithium metal. For other polymer gel battery cells or solid-state battery cells, both the anode and the cathode can be coated with gel polymer electrolyte. Since both the cathode compound material and the anode compound material on the support material are coated with the same copolymer (e.g. PVdF-HFP) as a binder, the three elements of the battery cell (anode, cathode, gel polymer electrolyte separator) are effectively fused into an integrated multilayer wafer by gelation after electrolyte activation without showing any physical boundary, so that the interface between the anode and electrolyte or the interface between the cathode and electrolyte reaches deep into the porous structure of these electrodes, which is very similar to the case where the liquid electrolyte reaches the interface. This also improves the ionic conductivity and dimensional stability of the gel polymer electrolyte.

[0028] In particular, if lithium metal is used as the anode, liquid electrolyte can be added only to the substrate formed as the cathode to form a gel polymer electrolyte from the reaction of the copolymer with the liquid electrolyte. If the battery cell is fabricated without lithium metal, the same method can be used for the anode, where liquid electrolyte can also be added to form a gel polymer electrolyte.

[0029] The first electrode is in particular a cathode. The first electrode can also be configured as an anode.

[0030] In one configuration of the method, the active material as a microporous coating is (first) calendered, after which a copolymer, e.g. PVdF-HFP, is deposited onto the active material, in which case calendering can be carried out as a two-stage calendering process with an integrated coating.

[0031] The copolymers (for example PVdF-HFP) can be deposited as coatings in various ways. For example, they can be sprayed (also called high velocity spray or high velocity jet method) onto the surface of the substrate (i.e. onto the active material only) for example by means of a Venturi-based nozzle. The nozzle is pressurized in particular by dry air at high pressure (about 6 bar), and when the copolymer particles are introduced into the nozzle, the high air pressure is converted into a high air velocity, which at high velocities (up to 0.3 Ma to 4 Ma) entrains the copolymer particles and drives them onto the substrate, in particular onto the already calendered surface. In this way, thin coatings of a few micrometers thick can be formed.

[0032] Alternatively or additionally, the copolymer particles are picked up by a deposition roller and pressed onto the substrate, particularly onto an already calendered surface.

[0033] After the substrate has been coated with a coating, for example a thin microporous layer consisting of PVdF-HFP, the substrate consisting of at least the active material and the copolymer is calendered, in particular (for a second time), in step a2) prior to step b).

[0034] In the second calendering process, in particular only the copolymer coating is pressed onto the substrate, in particular the active material, so that the copolymer coating adheres well to the surface of the substrate. The density of the (PVdF-HFP) coating does not increase significantly. After the second calendering, the copolymer (PVdF-HFP) adheres strongly to the surface of the substrate and has a sufficient porosity, which is important for the formation of the gel polymer electrolyte in step b).

[0035] In particular, the active material is calendered in step a0) during step a) and before step a1). Calendering has already been explained at the beginning. The calendering process is similar to a rolling process. The active material (i.e. the material possibly not yet containing the copolymer) is subjected to a calendering force in the deformation zone and is compressed.

[0036] The calendaring device comprises a number of rollers forming at least one gap, through which the substrate of the first electrode (here in particular only the active material and optionally also the support material coated with the active material) is conveyed along the conveying direction.

[0037] In particular, the active material is wetted with the pore-forming material during step a), in this case before or during step a0).

[0038] In particular, the coating is wetted by the pore-forming material during step a).

[0039] For example, the pore-forming material can be evaporated at a certain temperature, so that the pore-forming material can be formed from the substrate, i.e. from the coating and / or active material or material mixture, by heating the substrate. During evaporation, pores are particularly generated in the substrate. The space occupied by the pore-forming material in the substrate here becomes empty after the pore-forming material, which boils at a low temperature, is evaporated. In this way, the porosity required for the formation of a gel polymer electrolyte can be maintained.

[0040] Another way to form porosity is to use a pore-forming material that is soluble in, for example, DMC. The pore-forming material dissolves into the DMC (e.g., into the microporosity formed by the wetting roller) on the surface of the substrate or coating. Such DMC on the surface can be removed by washing the substrate with a wiper roller, which removes the pore-forming agent, and now pores are formed in the copolymer coating on the substrate.

[0041] This means in particular that there are at least two ways to create pores in the coating: one by thermal processes and the other by chemical dissolution processes, but such creation of pores is only necessary if the copolymer coating has a low porosity.

[0042] The substrate is guided through a tank filled with a pore-forming material, in particular for wetting with the pore-forming material. The pore-forming material comprises, for example, DMC (Dimethyl Carbonate). In particular, the tank filled with DMC is under a certain pressure with nitrogen gas, so that outside air cannot penetrate. When the first electrode runs through the tank, the pore-forming material penetrates into the pores of the active material.

[0043] A pressure roller or wetting roller can be provided to apply pressure to the substrate, and the mechanical pressure will drive more of the DMC into the active material of the substrate. The wetting roller will in particular create a microstructure on the surface of the substrate. In this way, more of the DMC will be deposited in the pores or micropores of the substrate surface.

[0044] Furthermore, a wiping roller can be provided for removing excess porous-forming material from the surface of the substrate, which can in particular be returned to the tank.

[0045] The pores of the substrate are then filled, in particular with a pore-forming material.The substrate can then be calendered, in particular in step a2).

[0046] In step a2), the substrate is subjected to a final density, e.g. 3.6 g / cm for a typical NMC material (i.e. material of a lithium-nickel-cobalt-manganese battery cell). 3 (grams per cubic centimeter).

[0047] DMC is especially chosen as the pore-forming material because it has a boiling point of 90° C. DMC is removed again from the substrate at a later point in the method, especially by evaporation.

[0048] When DMC leaves the surface of the substrate, it creates new pores or increases the pore diameter on the surface, which increases the porosity, allowing the copolymer deposited in the form of a coating to penetrate relatively easily into the pores of the first electrode or substrate.

[0049] The microstructure created by the wetting roller specifically contributes to the adhesion of the subsequent copolymer coating to the surface of the substrate.

[0050] During the calendering in step a2), a protective film, for example a polyurethane, can be used on one or both sides, so that the DMC does not spread over the sides of the substrate. The polyurethane film can be placed on the substrate before the introduction to the calender rollers and can be unwound again after exiting the calender. In this way the same film can be reused.

[0051] In particular, the material mixture is wetted with a pore-forming material during step a).

[0052] In particular, the pore-forming material is at least partially removed from the substrate prior to step b).

[0053] In particular, the substrate consisting of at least the active material and the copolymer is calendered in step a2) prior to step b).

[0054] In particular, the substrate does not comprise a gel polymer electrolyte immediately prior to step b).

[0055] In particular, the first electrode is cut prior to step b) into a predetermined geometric shape for operation within the battery cell.

[0056] Cutting of a substrate, in particular formed as a continuous material, includes in particular slitting (extending cut lines along the extension direction of the continuous material, i.e. along the x-direction, to divide the wide starting material of the substrate into a plurality of narrow continuous material strips), notching (cutting conductors out of the continuous material by cut lines, which extend longitudinally along the extension direction of the continuous material and transversely to this extension direction, i.e. for example along the y-direction and the x-direction), and / or separation (cut lines extending transversely to the extension direction of the continuous material along the y-direction, whereby the substrate is cut out of the continuous material to form the individual layers or electrodes of the stack).

[0057] Since before step b) only the copolymer and in particular no gel polymer electrolyte is present, ie in particular no gelling has yet taken place, the substrate can be handled particularly easily.

[0058] In particular, the substrate or the first electrode is dried between steps a) and b).

[0059] In particular, the substrate is heated to a temperature of about 90° C. and dried during this process. If a pore-forming material is arranged in the active material and / or in the material mixture, this pore-forming material boils and evaporates. When bubbles of the pore-forming material are released from the surface of the substrate, new pores are formed or the diameter of existing pores is increased. This increases the porosity in the active material and in the coating, if any.

[0060] If a pore-forming material is disposed within the coating, the pore-forming material is released and removed from the coating by heating, thereby increasing the porosity of the coating.

[0061] Pore-forming materials that are released from the substrate or coating upon drying can be captured and optionally recycled for reuse.

[0062] After heating, the pore-forming material may still remain in the pores of the substrate or coating, which is not particularly detrimental, since the pore-forming material, e.g. DMC, optionally becomes part of the liquid electrolyte used for wetting the first electrode in step b).

[0063] Therefore, in particular DMC or an equivalent suitable pore-forming material is used, i.e. a material which can be used for pore formation and which at the same time constitutes an electrolyte, and which is of no concern from a health point of view and does not contain VOCs (volatile organic compounds).

[0064] After cutting into the predetermined geometric shape, the first electrode can be arranged in a stack, particularly with another electrode, and since there is no gel material on the first electrode at this point, the first electrode can be easily handled during stacking.

[0065] In particular, the first electrodes are arranged after step a) and before step b) in a stacked relationship with at least one second electrode, said electrodes forming a stack.

[0066] In particular, the stack is placed in a casing of the battery cell prior to step b).

[0067] The lamination can be carried out in particular in a known manner, whereby it can be carried out as a Z-fold, i.e. by forming successive layers with alternating folded edges, or in a pick-and-drop method, i.e. with each separate layer, in which a cathode-separator-anode stack is produced.

[0068] After lamination, the conductors on the anode side are connected or welded to one another, in particular using nickel-based connection elements, while on the cathode side the aluminum conductors are connected or welded to one another, in particular by aluminum connection elements.

[0069] The stack, in particular with the respective connected conductors, is then placed in a battery cell casing. The casing can be formed as a pouch cell casing or as a plastically deformable casing (prismatic battery cell). If the casing is a pouch cell casing, the edges of the pouch cell casing are sealed in a known manner to ensure an airtight seal. In particular, the casing has, in a known manner, gas pockets that can collect gas released during the formation of the battery cell.

[0070] A liquid electrolyte is then introduced into the casing after at least partial sealing of the casing.

[0071] In particular in step b), a liquid electrolyte, for example PC (polypropylene carbonate) and / or DMC (dimethyl carbonate) containing a dissolved lithium salt (for example lithium hexafluorophosphate or LiPF6 or lithium bis(fluorosulfonyl)imide or LiFSi), is provided to at least the first electrode, and in particular to the stack. In this case, the amount of liquid electrolyte is very small, since its main function is to form a gel polymer electrolyte together with the copolymer.

[0072] After the electrolyte has been filled, the still open edges of the casing, e.g., a pouch cell casing, are closed or sealed.

[0073] The electrolyte filling is preferably carried out under a nitrogen atmosphere and / or under vacuum, which allows air to escape from the battery cell or casing during electrolyte filling.

[0074] In particular, the formation of the gel polymer electrolyte is activated by the supply of at least thermal or mechanical energy.

[0075] At least the first electrode is wetted, so that the liquid electrolyte penetrates into the pores of the first electrode or the substrate or coating. The liquid electrolyte reacts with the copolymer and is activated. For activation, energy is required, which can be provided, inter alia, by heat or mechanical force. After activation, the liquid electrolyte swells the original microporous film (substrate and / or coating) and finally forms a gel polymer electrolyte.

[0076] The wetting and activation is carried out in particular by applying a mechanical force to the first electrode or the stack. For example, the stack placed in the pouch cell casing can be pressed and compressed between two rotating rollers. The mechanical force causes the liquid electrolyte to penetrate into the pores. This method may be suitable since the possibility of damage to the casing and the separator is relatively small.

[0077] Wetting and activation may (optionally additionally) be performed by thermal energy. For this purpose, at least the first electrode or stack and / or the casing with the stack are supplied with thermal energy, for example by placing them in an oven. For this purpose at least the first electrode is heated to about 50° C. If LiFSi is used as the lithium salt, heating can also be performed up to 80° C. By heating, thermal energy is utilized by the electrolyte, which penetrates into the pores and activates the copolymer to produce a gel polymer electrolyte.

[0078] After the wetting process, the solid-state or polymer battery is ready for molding: the copolymer is in particular at least 90%, preferably at least 95%, particularly preferably completely converted into a gel polymer electrolyte.

[0079] In particular, the stack can be activated with liquid electrolyte (especially including lithium salts) in the same way that conventional polyolefin separators are activated with liquid electrolyte during the electrolyte filling process. Depending on the porosity of the coating or substrate, the liquid electrolyte can penetrate into the coating or substrate. After activation, the liquid electrolyte swells the original microporous coating or substrate, eventually forming a gel polymer electrolyte with the copolymer.

[0080] To accelerate the wetting process of the copolymer, a portion of the liquid electrolyte can be added, especially before calendering.

[0081] In the proposed method, the only step that has to be performed in a humidity-controlled environment is the supply of liquid electrolyte to the stack, so the advantages of the proposed method in terms of manufacturing and equipment costs are clear.

[0082] In battery cells, usually only the cathode is coated with gel polymer electrolyte, while the anode is made of lithium metal. In other polymer gel batteries, both the anode and the cathode can be coated with gel polymer electrolyte. In particular, since both the cathode compound material and the anode compound material on the substrate or support material are coated with the same PVdF-HFP copolymer as a binder, for example, the three elements of the battery cell are effectively fused into an integrated multilayer wafer by gelation after electrolytic activation without showing any physical boundary, so that the interface between the anode and the electrolyte or the interface between the cathode and the electrolyte reaches deep into the porous structure of these electrodes, which is very similar to the case where the liquid electrolyte reaches the interface. This also improves the ionic conductivity and dimensional stability of the gel polymer electrolyte.

[0083] In particular, the method can be used for both solid-state batteries and polymer gel battery cells. In the case of battery cells, lithium metal is used as the anode, so the proposed method is used specifically only for the manufacture of the cathode. In the case of polymer gel battery cells, the method can be used to manufacture the cathode and the anode. Thus, if the battery cell is manufactured without lithium metal, the method can be used for both electrodes.

[0084] The application of the liquid electrolyte and the wetting of the first electrode, in battery cells with lithium as the metallic anode, is carried out especially before the lamination of the electrodes. Problems may arise especially if the liquid electrolyte comes into contact with the lithium metal of the anode, the adhesive film, the nickel plate and the copper substrate. Wetting of the electrodes can also be carried out after lamination, especially if the liquid electrolyte does not have a negative effect on the lithium metal on the anode.

[0085] In particular, the proposed method differs from known methods for manufacturing solid-state battery cells in at least the following respects: In this method, the gel polymer electrolyte is not formed immediately after calendaring, but only after electrolyte filling and activation. The known methods do not envisage filling the casing with a liquid electrolyte. The present method proposes to supply a liquid electrolyte which activates the copolymer to form a gel polymer electrolyte. Only the coating of the active material with the copolymer is at least a new process for producing a battery cell, the other method steps being in particular already known but now proposed for the first time in a different combination. The coating with the copolymer can be carried out in particular by high-speed spraying or by pressing with a deposition roller. In particular, the first electrode configured as a cathode does not have a gelled electrolyte coating during cutting of the electrode and during connection of the electrode with the electrical conductor element as well as during the lamination process. There is no need to manufacture the gel polymer electrolyte externally and then deposit it onto the cathode. The gel polymer electrolyte is manufactured within the battery cell. The porosity of the substrate or coating can be increased by a pore-forming material. In known methods, the porosity is maintained at a relatively low density during calendering. In this method, the calendering of the active material is not altered and the first electrode is in particular completely compressed to the desired density. Pore-forming materials are released especially during the drying process and can be captured and recycled. The gel polymer electrolyte does not have to be applied at high temperatures (approximately 90°C) e.g. onto the cathode. The gel polymer electrolyte is distributed uniformly at a suitable low temperature after wetting of at least the first electrode. Since the wetting here lasts in particular for 3 to 4 hours, a temperature of approximately 50°C may be sufficient. Instead of expensive lithium salts such as LiFSi, "regular" cost-effective lithium salts such as lithium hexafluorophosphate can be used. Other copolymers can also be used, such as, in particular, polyethylene oxide (PEO), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), etc. The method proposes the use of a copolymer of polyvinylidene fluoride (PVdF) together with hexafluoropropylene (HFP) as a preferred configuration.

[0086] Compared to known methods, the following advantages can be achieved in particular: The first electrode can be easily handled during the various steps of the method since the formation of the gel polymer electrolyte occurs at a later phase. · Dry atmosphere for electrode production is no longer required, thus saving energy costs significantly. The gel polymer electrolyte and the liquid electrolyte can be penetrated (as in known methods) into the pores of the first electrode or the substrate or the coating without the need to supply excessive heat energy. No need for expensive lithium salts such as LiFSi. Most of the conventional methods for manufacturing batteries can be used, which reduces the effort required to implement the proposed method. In particular, the stack can be activated with liquid electrolyte (especially containing lithium salts) during the electrolyte filling process, similar to conventional polyolefin separators with liquid electrolyte. The method is better suited for mass production of solid-state battery cells than currently known methods. The relatively low temperatures required to produce the gel polymer electrolyte in the battery cell result in no or only minor degradation of the electrolyte. -Thermal decomposition of lithium salts does not occur. The gel polymer electrolyte inhibits the formation of dendrites in the lithium metal, reducing the risk of thermal runaway. · Conventional calendering can be used to compress the first electrode to a high density, which results in a high volumetric energy density. The higher porosity of the first electrode allows for higher current (higher C-rate) and therefore higher power to be delivered.

[0087] In short, the production of a gel polymer electrolyte in an already assembled battery cell (i.e. when the first electrode is already arranged in a stack and this stack is already present in the battery cell casing) can significantly simplify the production of solid-state or polymer gel batteries.

[0088] The method can in particular be carried out by a data processing system, for example a control device, which system has means adapted or configured or programmed for carrying out the steps of the method or means for carrying out the method, and which at least allows for closed-loop control of the components of the device used in the method.

[0089] The means here include, for example, a processor, a memory storing instructions executed by the processor, and a data line or transmission device capable of transmitting instructions, measurement values, data, etc. between the listed components of the apparatus used in the method.

[0090] Furthermore, a computer program is proposed comprising instructions for causing a computer to carry out the above-mentioned method or the above-mentioned method steps when the program is executed by a computer.

[0091] Furthermore, a computer readable storage medium is proposed, comprising instructions which, when executed by a computer, cause the computer to perform the above-mentioned method or the above-mentioned method steps.

[0092] Furthermore, a battery cell is proposed which comprises at least a casing and, arranged in said casing, an electrode stack which comprises at least one electrode, in particular produced by the method described above.

[0093] A battery cell specifically includes a casing surrounding a volume, and disposed within the volume are at least one first electrode of a first electrode type, a second electrode of a second electrode type, and a separator material or a solid (which may be gelled) electrolyte disposed therebetween.

[0094] The battery cells are in particular pouch cells (with a deformable casing made of a pouch film) or prismatic cells (with a shape-fixed casing). A pouch film is a known deformable casing material that is used as a casing for so-called pouch cells. It is a composite material, for example comprising plastic and aluminum.

[0095] The battery cells are in particular lithium-ion battery cells.

[0096] The individual layers of the electrodes are arranged one on top of the other, in particular forming a stack, and the electrodes are each associated with a different electrode type, i.e. configured as an anode or a cathode, where the anodes and cathodes are arranged alternately and separated from each other by a separator material or an electrolyte, respectively.

[0097] Furthermore, a motor vehicle is proposed which comprises at least a traction drive and a battery with at least one battery cell as described, the traction drive being able to be supplied with energy by the at least one battery cell.

[0098] Descriptions of methods are particularly applicable to battery cells, automobiles, data processing systems, and computer-implemented methods (ie, computers or processors, computer-readable storage media), and vice versa.

[0099] In particular, the use of indefinite articles ("a" and "an") in the claims and the description reflecting them should not be understood as numerals per se, and therefore the concepts or elements introduced with such indefinite articles should be understood as meaning that there is at least one of these concepts or elements, and in particular that there may be a plurality of these concepts or elements.

[0100] For the sake of clarity, numerals used herein ("first", "second", ...) are primarily (only) used to distinguish between multiple similar objects, quantities or processes, i.e., without imposing any particular dependency and / or order between these objects, quantities or processes. Where dependency and / or order is required, it is either explicitly stated herein or will become apparent to one skilled in the art upon consideration of the specifically described configuration. Where components appear multiple times ("at least one"), a description of one of these components applies equally to all or some of these components, but this is not required.

[0101] The present invention and technical environment will be described in detail below with reference to the accompanying drawings. Please note that the present invention is not limited to the described embodiments. In particular, unless otherwise stated, it is also possible to extract partial aspects of the facts shown in the drawings and combine them with other components and findings from this specification. It should be noted that the drawings, especially the scales shown, are merely approximate. [Brief description of the drawings]

[0102] [Figure 1] FIG. 10 shows a flow diagram of a first variant embodiment of the method. [Diagram 2] FIG. 11 shows a flow diagram of a second variant embodiment of the method. [Diagram 3] FIG. 11 shows a flow diagram of a third variant embodiment of the method. [Figure 4] FIG. 2 shows a side view of a first alternative embodiment of an apparatus for applying a coating. [Diagram 5] FIG. 11 is a side view of a second alternative embodiment of the device for applying a coating. [Figure 6] FIG. 2 is a side cross-sectional view showing a battery cell. [Figure 7] FIG. 2 shows a battery cell during step b) of the method. [Figure 8] FIG. 8 shows the battery cell of FIG. 7 after step b). [Figure 9] FIG. [Figure 10] 10 is a view showing the wetting roller of FIG. 9 along the conveying direction. FIG. [Figure 11] FIG. 11 is a side view of the wetting roller of FIG. [Figure 12] FIG. 12 shows the microstructure of the wetting roller of FIGS. 10 and 11.

[0103] In Fig. 1, the flow diagram of a first variant embodiment of the method is shown. In step a) 27, the active material 4 is prepared and possibly placed on a support material 9. The substrate 3 comprises the active material 4 and the support material 9. The active material 4 is moistened with a pore-forming material 11 before step a0) 28. The active material 4 is calendered in step a0) 28 during step a) 27 and before step a1) 29. Calendering has already been described at the beginning. The calendering device 16 comprises a number of calender rollers 17. A calendering force is applied to the active material 4 via the calender rollers 17 in the deformation zone, and the active material 4 is compressed.

[0104] In a subsequent step a1) 29, the copolymer 5 is deposited on the active material 4 as a coating 10. The coating 10 is wetted with a pore-forming material 11 during a step a) 27. The coating 10 wetted with material 11 is calendered again in a step a2) 30.

[0105] The first electrode 1 is cut in step a3) 32 prior to step b) 31 into a geometric shape 12 predetermined for operation in the battery cell 2. The cutting of the substrate 3 formed as a continuous material 39 can include slitting (extending cut lines along the extension direction of the continuous material 39, i.e. along the x-direction or transport direction 46, to divide the wide starting material of the substrate 3 into a plurality of narrow strips of the continuous material 39), notching (cut lines cut out the conductors 38 from the continuous material 39; the cut lines extend longitudinally along the extension direction of the continuous material 39 and transversely to this extension direction, i.e. along the y-direction and the x-direction for example), and / or separation (cut lines extend transversely to the extension direction of the continuous material 39 along the y-direction; separation here cuts the substrate 3 from the continuous material 39 to form the individual layers or electrodes 1, 13 of the stack 14).

[0106] In a next step a4) 33, the cut first electrode 1 or substrate 3 is dried, where the pore-forming material 11 evaporates and pores are formed in the active material 4 and in the coating 10.

[0107] In a next step a5) 34, the electrodes 1, 13 and possibly a separator 40 are laminated to form the stack 14.

[0108] The next step a6) 35 involves placing the stack 14 in the casing 15 .

[0109] The next step b) 31 is divided into a step b1) 36 of adding a liquid electrolyte 6 and a step b2) 37 of forming a gel polymer electrolyte 7 by reacting the copolymer 5 with the liquid electrolyte 6 to form the first electrode 1.

[0110] It should be mentioned here that the addition of the pore-forming material 11 may be performed as an optional step.

[0111] 2 shows the flow diagram of a second variant of the method, in which the second electrode 13 is a lithium metal anode not supplemented by a liquid electrolyte 6 (see also the description of FIG. 1).

[0112] Unlike the first variant embodiment, here the method produces only the cathode as the first electrode 1. Step b) 31 is therefore performed after step a3) 32, i.e. after cutting. Step b) 31 involves the addition of liquid electrolyte 6 and the formation of gel polymer electrolyte 7 by reacting copolymer 5 with liquid electrolyte 6 to form the first electrode 1.

[0113] In a next step a5) 34, the electrodes 1, 13 and possibly a separator 40 are laminated to form the stack 14.

[0114] The next step a6) 35 involves placing the stack 14 in the casing 15 .

[0115] The flow of a third variant of the method is shown in figure 3. Please also refer to the explanations of figures 1 and 2.

[0116] In contrast to the other variants, here the copolymer 5 is mixed with the active material 4 in a step a) 27 to form a material mixture 8, which is then applied to a support material 9. The copolymer 5 is homogeneously distributed in the material mixture 8. When the formation of the gel polymer electrolyte 7 then takes place in the framework of a step b) 31, the gel polymer electrolyte 7 is also homogeneously distributed in the material mixture 8 of the subsequently formed first electrode 1.

[0117] The active material 4 is wetted with a pore-forming material 11 prior to step a0) 28. The active material 4 is calendered in step a0) 28 during step a) 27 and prior to step a1) 29. The first electrode 1 is cut in step a3) 32 prior to step b) 31 into a predetermined geometric shape 12 for operation within the battery cell 2.

[0118] In a next step a4) 33, the cut first electrode 1 or substrate 3 is dried, whereupon the pore-forming material 11 evaporates and pores are formed in the material mixture 8.

[0119] Unlike the first variant embodiment, here the method produces only the cathode as the first electrode 1. Step b) 31 is therefore carried out after step a3) 32, i.e. after cutting. Step b) 31 involves the addition of a liquid electrolyte 6 and the formation of a gel polymer electrolyte 7 by reacting the liquid electrolyte 6 with a copolymer 5 to form the first electrode 1.

[0120] In a next step a5) 34, the electrodes 1, 13 and possibly a separator 40 are laminated to form the stack 14.

[0121] Step a1) 29, ie the placement of the copolymer 5 on the material mixture 8 as a coating 10, does not necessarily have to take place here.

[0122] In FIG. 4 a side view of a first alternative embodiment of an apparatus for applying the coating 10 is shown.

[0123] The copolymer 5 is sprayed (also called high velocity injection or high velocity jet method) onto the surface of the substrate 3 (i.e. only onto the active material 4) by means of a Venturi-based nozzle 21. The nozzle 21 is supplied with dry air 24 at high pressure (about 6 bar). For this purpose, the air 24 is compressed in a compressor 22. The supply of the copolymer 5 is controlled via a valve 23. The copolymer particles flow into the nozzle 21. The high air pressure is converted into a high air velocity. The high velocity (up to 0.3 Ma to 4 Ma) of the air entrains the copolymer particles and drives them into the substrate 3, in particular into the already calendered surface. In this way, thin coatings 10 of a few micrometers thickness can be formed.

[0124] In Fig. 5 a side view of a second variant embodiment of an apparatus for applying a coating 10 is shown. The substrate is fed as a continuous material 39 to a pair of pressure rollers 26. The copolymer 5 fed via the pressure rollers 26 from one outlet 25 in each case is bonded to the support material 9. Further transport of the first electrode 1 takes place via transport rollers 20 to the calender device 16 and step a2) 30. The coating 10 moistened with material 11 is calendered again in step a2) 30.

[0125] 6 shows a battery cell 2 in a cross-sectional side view. The battery cell 2 includes a casing 15 that encloses a volume, and further includes a plurality of first electrodes 1 of a first electrode type, a plurality of second electrodes 13 of a second electrode type, and a separator 40 or a solid (or gel) electrolyte 6 disposed therebetween, disposed within the volume. Electrical conductors 38 of the electrodes 1, 13 extend outwardly from the casing 15. The casing 15 is hermetically closed.

[0126] 7 shows the battery cell 2 during method step b) 31. The casing 15 is already partially closed by a sealing seam 41. The electrical conductors 38 extend beyond the casing 15 to the outside.

[0127] In step a6) 35, the stack 14 is placed in the casing 15. In step b1) 36, the liquid electrolyte 6 is added via the face of the casing 15 that is not yet closed.

[0128] In Fig. 8 the battery cell 2 of Fig. 7 is shown after step b) 31, in which the casing 15 is now finally closed. In step b2) 37 the formation of the gel polymer electrolyte 7 by reacting the copolymer 5 with the liquid electrolyte 6 to form the first electrode 1 is carried out.

[0129] In Fig. 9, a part of the method is shown, where step a0) 28, i.e. the (first) calendering and wetting of the active material 4 with the pore-forming material 11 before step a0) 28, is shown. The active material 4 is calendered in step a0) 28 during step a) 27 and before step a1) 29. The substrate 3 is guided through a tank 42 filled with the pore-forming material 11 for wetting with the pore-forming material 11. The pore-forming material 11 comprises, for example, DMC (dimethyl carbonate). The tank 42 filled with DMC is under a certain pressure by nitrogen gas 43, so that outside air cannot penetrate. When the first electrode 1 runs through the tank 42 as a continuous material 39, the pore-forming material 11 penetrates into the pores of the active material 4. A wetting roller 18 is provided which exerts a pressure on the substrate 3, and by this mechanical pressure more of the pore-forming material 11 penetrates into the active material 4 of the substrate 3. The wetting roller 18 generates a microstructure 44 on the surface of the substrate 3 (see FIG. 12). In this way more of the material 11 is deposited in the pores or micropores of the surface of the substrate 3.

[0130] Additionally, a wiping roller 19 is provided for removing excess porous-forming material from the surface of the substrate 3. Excess porous-forming material 11 can be returned into the tank .

[0131] The pores of the substrate 3 are then filled with a pore-forming material. The substrate 3 is then calendered in step a2) 30.

[0132] In the calendering in step a2) 30, a (polyurethane) protective film 45, for example, is used on both sides, so that the material 11 does not spread over the sides of the substrate 3. The polyurethane protective film 45 is placed on the substrate 3 before it is introduced into the calender rollers 17 and is unwound again after it has been led out of the calender device 16. In this way the same protective film 45 can be used repeatedly.

[0133] In Figure 10 the wetting roller 18 of Figure 9 is shown in a view along the conveying direction 46. In Figure 11 the wetting roller 18 of Figure 10 is shown in a side view. In Figure 12 the microstructure 44 of the wetting roller 18 of Figures 10 and 11 is shown. Figures 10 to 12 are explained together below. See also the explanation for Figure 9.

[0134] The wetting roller 18 is additionally excited by an excitation device 47 to produce vibrations 48. The wetting roller 18 exerts a pressure on the substrate 3, so that due to this mechanical pressure more of the pore-forming material 11 reaches the active material 4 of the substrate 3. The wetting roller 18 has a microstructure 44, which forms a microstructure 44 on the surface of the substrate 3 (see FIG. 12). The individual features of the microstructure 44 have a depth of about 20 μm and a width of up to about 5 μm. In this way more of the material 11 is deposited in the pores or micropores on the surface of the substrate 3. [Explanation of symbols]

[0135] 1 First electrode 2 (Solid-state) battery cells 3 Base 4 Active materials 5. Copolymers 6 Electrolytes 7. Gel polymer electrolyte 8 Material mixture 9 Support material 10 Coating 11 Material 12 Geometric shapes 13 Second electrode 14 Stack 15 Casing 16 Calendar device 17 Calendar Roller 18 Wetting roller 19 Wiping roller 20 Conveyor roller 21 Nozzle 22 Compressor 23 Valve 24 Air 25 Exit 26 Pressure roller 27 Step a) 28 Step a0) 29 Step a1) 30 Step a2) 31 Step b) 32 Step a3) 33 Step a4) 34 Step a5) 35 Step a6) 36 Step b1) 37 Step b2) 38 Conductors 39 Continuous Materials 40 Separator 41 Sealed seam 42 Tank 43 Nitrogen Gas 44 Microstructure 45 Polyurethane protective film 46 Transport direction 47 Excitation Device 48 Vibration

Claims

1. A method for manufacturing a first electrode (1) of a battery cell (2), comprising the steps of: The method comprises at least the following steps: a) producing a substrate (3) of said first electrode (1) comprising at least an active material (4) of said first electrode (1) and a copolymer (5); b) wetting the substrate (3) with a liquid electrolyte (6) and forming a gel polymer electrolyte (7) by reacting the copolymer (5) with the liquid electrolyte (6) to form the first electrode (1); A method comprising:

2. 2. The method according to claim 1, wherein in step a) said copolymer (5) is mixed with said active material (4) to form a material mixture (8) and said material mixture (8) is placed on a support material (9).

3. 3. The method according to claim 1 or 2, wherein in step a1), carried out during step a), the copolymer (5) is deposited as a coating (10) on the active material (4).

4. 4. The method according to claim 3, further comprising calendering the active material (4) during step a) and also prior to step a1) in step a0).

5. 5. The method according to claim 4, wherein during step a), in this case before or during step a0), the active material (4) is moistened with a pore-forming material (11).

6. 6. The method according to claim 3, wherein during step a) the coating (10) is wetted with a pore-forming material (11).

7. 3. The method according to claim 2, wherein during step a) the material mixture (8) is wetted with a pore-forming material (11).

8. The method according to any one of claims 5 to 7, characterized in that prior to step b), the pore-forming material (11) is at least partially removed from the substrate (3).

9. 9. The method according to claim 1, wherein in step a2) before step b), the substrate (3) consisting of at least the active material (4) and the copolymer (5) is calendered.

10. 10. The method according to any one of claims 1 to 9, wherein the substrate (3) does not contain a gel polymer electrolyte immediately prior to step b).

11. 11. The method according to claim 1, further comprising, prior to step b), cutting the first electrode (1) into a predetermined geometric shape (12) for operation within a battery cell (2).

12. 12. The method according to any one of the preceding claims, wherein the first electrode (1) is dried between steps a) and b).

13. 13. The method according to claim 1, further comprising, after step a) and before step b), arranging the first electrode (1) and at least one second electrode (13) in a stacked arrangement on top of each other, forming a stack (14) of the electrodes (1, 13).

14. The method according to claim 11, further comprising, before step b), placing the stack (14) in a casing (15) of the battery cell (2).

15. 15. The method according to any one of the preceding claims, wherein the formation of the gel polymer electrolyte (7) is activated by the supply of at least thermal or mechanical energy.

Citation Information

Patent Citations

  • Electrode for nonaqueous electrolyte battery, and nonaqueous electrolyte battery using the electrode

    JP1997219197A

  • Bipolar type lithium ion secondary battery

    JP2000030746A

  • Nonaqueous electrolyte secondary battery and its manufacture

    JP2000323121A

  • Nonaqueous electrolyte battery and manufacturing method of positive electrode for nonaqueous electrolyte battery

    JP2002216744A

  • Polymer cell

    JP2006286496A