Low film blocking styrene butadiene block copolymers with improved organoleptic properties
A block copolymer with distinct block transitions and cylindrical morphology addresses blocking and odor issues in SBC films, enhancing mechanical properties and organoleptic qualities.
Patent Information
- Application Number
- JP2024515338
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-10
- Filing Date
- 2022-09-09
- Publication Date
- 2024-10-09
AI Technical Summary
Films made from styrene-butadiene block copolymers (SBC) tend to stick together when wound onto a roll during manufacturing, leading to blocking issues and potential tearing, and often have unpleasant odors.
A block copolymer with distinct block transitions and a cylindrical morphology, composed of vinyl aromatic and conjugated diene blocks, is produced through sequential anionic polymerization, ensuring clear composition changes and improved mechanical properties.
The solution results in films with high melt strength, reduced interlayer adhesion, and enhanced organoleptic properties, allowing for easier unwinding and improved sensory characteristics.
Smart Images

Figure 2024536939000001 
Figure 2024536939000002 
Figure 2024536939000003
Abstract
Description
[Technical field]
[0001] explanation The present invention relates to styrene butadiene block copolymers (SBC), to polymer compositions comprising said SBC, and to the use of said polymer compositions for the manufacture of films. [Background technology]
[0002] Stiff and tough styrene butadiene block copolymers (SBC) and compositions containing SBC are known. For the production of shrinkable films, often a mixture of tough and tough SBC components, optionally together with general purpose polystyrene (GPPS), is mixed and extruded into a film. In a subsequent on-line step, the film is heated by hot air and stretched 4-6 times perpendicular (transverse) to the extrusion direction (width direction orientation or TDO) and finally stretched up to 1.1 times perpendicular (parallel) to the machine direction (machine direction orientation or MDO). Finally, the ends are trimmed and the film is wound into a large roll. Later, the film can be cut into smaller rolls, printed and sealed into a long cylindrical hose. Finally, the printed hose is cut to the dimensions of a cylindrical label and shrunk around a container (e.g., a bottle) by applying heat, typically in a heat tunnel. In a separate process, the film is stretched 2-5 times in the MDO direction and finally stretched up to 1.1 times in the TDO direction as well. After cutting the film ends and winding the film on a large roll, the film is cut into smaller rolls and printed. The label is wrapped around the container, cut, glued, and shrunk around the container by applying heat.
[0003] US Pat. No. 5,399,433 describes a mixture of styrene-butadiene block copolymers A and B for the production of heat shrinkable films with high shrink performance and high stiffness / strength. Preferably, the SBC copolymer A has the structure S-(B / S) A -S or a single copolymer block (B / S) A is preferred, where (B / S)A is a random vinyl aromatic / diene copolymer hard block (5-35 wt. % diene, Mn 15,0000-300,000 g / mol) and S is a vinyl aromatic polymer hard block. Preferably, the SBC block copolymer B has short branches S e -(B / S) B ~ and long branches (B / S) A -S i -(B / S) B -S s ~[Here (B / S) B is a soft random copolymer block (80-40% by mass of diene), and S e , S i is long, and S s are short vinyl aromatic polymer blocks.
[0004] Patent Documents 2 and 3 disclose single copolymer block (B / S) Ai (Mn 5,000~15,000g / mol) and two short branches of structure S t -[(B / S) A ] n -(B / S) Ai Or [(B / S) A ] n -(B / S) Ai [Block here [(B / S) A ] n Mn is 50,000-150,000 g / mol, and block S t The present invention describes an SBC mixture for shrinkable packaging films, comprising a rigid star block copolymer A or A1 having two long arms, the Mn of which is 3,000-8,000 g / mol.
[0005] Preferably, structure S e -(B / S) B ~ or S e -(B / S) B -S s ~ 3 or 2 short branches and structure (B / S) Ae -S i -(B / S) B- Or (B / S) Ae-S-(B / S) B -S S Further included are robust star block copolymers B or A2 having one or two long arms of ~; where the block (B / S) B The Mn of is 5,000 to 40,000 g / mol, and the block (B / S) Ae Mn is 30,000-100,000 g / mol, and block S e and S i Mn is 5,000-30,000 g / mol, and block S s The Mn is <2,500 g / mol.
[0006] SBC A, A1, B and A2 (Random) Hard Blocks (B / S) A The diene content of each of the soft blocks (B / S) of SBC B is 35 to 5 mass%. B The diene content of SBC A1 is 80-40% by mass, and the diene content of SBC A2 is 100-75% by mass.
[0007] Films made from the above prior art SBC blends are made up of a soft phase and a hard phase, where the soft phase has a cylindrical morphology.
[0008] Patent Document 4 discloses a mixture containing linear block copolymers made from vinyl aromatic monomers and from dienes of the structures (I) S1-B1-S2 and (II) S3-B2-S4, where S1 is a block made from vinyl aromatic monomers having a number average molecular weight Mn in the range of 40,000 to 100,000 g / mol, S2, S3 and S4 are blocks made from vinyl aromatic monomers having a number average molecular weight Mn in the range of 5,000 to 20,000 g / mol, respectively, B1 and B2 are blocks made from dienes or copolymer blocks made from dienes and from vinyl aromatic monomers having a number average molecular weight Mn in the range of 15,000 to 40,000 g / mol, respectively, and the ratio of block copolymers (I) / (II) is in the range of 0.6 to 2. The transition between the blocks is clear. The examples show simultaneously produced mixtures of SBC(I) (Mn approximately equal to 97,000-100,000 g / mol) and SBC(II) (Mn approximately equal to 45,000-49,000 g / mol), which have butadiene contents in the range of 21.6-35% by weight. Blends of the above mixtures with GPPS have high toughness along with high stiffness and can be used for the production of thin films. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] US 2011 / 098401 [Patent Document 2] WO 2018 / 114569 [Patent Document 3] WO 2018 / 153808 [Patent Document 4] US 2005 / 009990 Summary of the Invention [Problem to be solved by the invention]
[0010] Films made from SBC polymers or polymer compositions according to the prior art often have a tendency to stick when wound onto rolls during the manufacturing process. This blocking of the stretched film can cause various technical problems. In some cases, it is even impossible to unwind it from the roll after a few days. Prior art films often undergo unwanted stretching and eventually tear during processing.
[0011] Furthermore, the prior art materials often have an unpleasant odor. Thus, the blocking and organoleptic properties of the films of said materials still need to be improved.
[0012] One object of the present invention is to provide a material based on styrene butadiene block copolymers (SBC) that allows the extrusion of blown and cast films with high melt strength, which is suitable for the production of shrinkable films with good mechanical properties and reduced interlayer adhesion. Furthermore, the organoleptic properties of the material should be improved. [Means for solving the problem]
[0013] This problem is solved by the block copolymers and polymer compositions according to the claims. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] One aspect of the present invention is a linear block copolymer (A) comprising (or consisting of) at least two polymer blocks S of different number average molecular weights Mn consisting essentially of at least one vinyl aromatic monomer and at least one polymer block B consisting essentially of at least one conjugated diene; where at least two of the blocks S are terminal blocks S1 and S2; The block copolymer (A) here comprises: 65 to 85% by weight, preferably 68 to 80% by weight, more preferably 70 to 75% by weight, based on the entire block copolymer (A), of at least one vinyl aromatic monomer, in particular styrene, and 15-35% by mass, preferably 20-32% by mass, more preferably 25-30% by mass of at least one conjugated diene, in particular butadiene and / or isoprene, more preferably butadiene; wherein the proportion of the soft phase essentially composed of polymerized conjugated dienes is 15-35% by volume based on the entire block copolymer (A), and wherein the soft phase embedded in the hard phase essentially composed of polymerized vinyl aromatic monomers (proportion 65-85% by volume) has a cylindrical morphology; and The block copolymer (A) here has a clear block transition and a number average molecular weight Mn of at least 140,000 g / mol.
[0015] In the context of the present invention, a "distinct block transition" means that the transition between the blocks of the block copolymer is clearly separated (i.e., the composition changes abruptly). The block copolymer (A) does not include a tapered block transition. Preferably, the block copolymer (A) does not contain a random block.
[0016] The morphology is determined by transmission electron microscopy (TEM) on OsO4 stained ultramicrotome samples of the SBC polymer or polymer composition.
[0017] In the context of the present invention, "diene" means a conjugated diene. "Butadiene" means 1,3-butadiene. In the context of the present invention, a (co)polymer comprising a monomer and optionally further comonomers means a (co)polymer comprising structural units derived from said polymerized monomers.
[0018] In the context of the present invention, a polymer (block) "consisting essentially of" at least one vinyl aromatic monomer or at least one conjugated diene means that the polymer consists of 85 to 100% by weight of at least one vinyl aromatic monomer or 85 to 100% by weight of at least one conjugated diene, and optionally 0 to 15% by weight of at least one conjugated diene or 0 to 15% by weight of at least one vinyl aromatic monomer, respectively.
[0019] The polymer block S of the block copolymer (A) preferably consists of 90 to 100% by weight of at least one vinyl aromatic monomer and 0 to 10% by weight of at least one conjugated diene; and the polymer block B of the block copolymer (A) preferably consists of 90 to 100% by weight of at least one conjugated diene and 0 to 10% by weight of at least one vinyl aromatic monomer.
[0020] In the context of the present invention, the number average molecular weight Mn is determined by GPC according to ISO 16014-3:2012 (size exclusion using the relative calibration method against polystyrene standards at temperatures <60° C.).
[0021] Preferably, the block copolymer (A) consists of two terminal polymer blocks S1 and S2 and one polymer block B.
[0022] More preferably, the block copolymer (A) consists of two terminal vinyl aromatic homopolymer blocks S1 and S2 and one diene homopolymer block B. Particularly preferred block copolymers (A) are linear block copolymers (A) of structure (I) S1-B-S2, where S1 and S2 are polystyrene blocks and B is a polybutadiene block.
[0023] Examples of vinyl aromatic monomers that can be used for the preparation of the block copolymer (A) are styrene, alpha-methylstyrene, ring-alkylated styrenes such as p-methylstyrene or tert-butylstyrene, or mixtures thereof. Styrene and / or alpha-methylstyrene are preferred, with styrene being particularly preferred.
[0024] Suitable dienes which may be used for the preparation of the block copolymer (A) are 1,3-butadiene, isoprene, 2,3-dimethylbutadiene, 1,3-pentadiene or 1,3-hexadiene, or mixtures thereof; 1,3-butadiene and isoprene are preferred; 1,3-butadiene is particularly preferred.
[0025] Particularly preferred block copolymers (A) comprise (or consist of) styrene and butadiene. Preferably, the number average molecular weight Mn of the block copolymer (A) is in the range of 140,000 to 1,000,000 g / mol, more preferably 140,000 to 500,000 g / mol, and most preferably 140,000 to 300,000 g / mol.
[0026] The number average molecular weight Mn of the polymer block S1 is preferably within a range of 12,000 to 50,000 g / mol, more preferably 15,000 to 30,000. The number average molecular weight Mn of the polymer block S2 is preferably within a range of 40,000 to 150,000 g / mol, more preferably 60,000 to 140,000 g / mol. The number average molecular weight Mn of the polymer block B is preferably within a range of 15,000 to 80,000 g / mol, more preferably 20,000 to 60,000 g / mol.
[0027] Preference is given to block copolymers (A) of structure (I) S1-B-S2 having a number average molecular weight in the range of 140,000 to 500,000 g / mol, made from 68 to 80% by weight, preferably 70 to 75% by weight, of at least one vinyl aromatic monomer, in particular styrene, and 20 to 32% by weight, preferably 25 to 30% by weight, of at least one diene, in particular butadiene.
[0028] More preferred are block copolymers (A) of structure (I) S1-B-S2 having a number average molecular weight Mn in the range of 140,000 to 300,000 g / mol, made from 70 to 75% by weight of at least one vinyl aromatic monomer, in particular styrene, and 25 to 30% by weight of at least one diene, in particular butadiene.
[0029] The proportion of the soft phase essentially built up from polymerized conjugated dienes is generally 15-35% by volume, preferably 18-32% by volume, more preferably 22-30% by volume, based on the block copolymer (A); accordingly, the proportion of the hard phase essentially built up from vinyl aromatic monomers is 65-85% by volume, more preferably 68-82% by volume, most preferably 70-78% by volume, based on the block copolymer (A).
[0030] The amount of soft and hard phases is determined based on OsO4 stained TEM images and computer processing to calculate the diene rich (hence soft) phase (black in TEM) and the vinyl aromatic rich (hence hard) phase (white in TEM).
[0031] According to the present invention, the block copolymer (A) has a clear block transition, and the soft phase of the block copolymer (A) has a cylindrical morphology.
[0032] The block copolymer (A) according to the present invention can be, and is preferably, prepared by the sequential anionic polymerization of vinyl aromatic monomers and conjugated dienes with an organo-alkali metal initiator.
[0033] Sequential anionic polymerization is known per se. The anionic polymerization initiators used may be any of the conventional mono- or difunctional alkyl, aryl or aralkyl compounds of alkali metals. Preferably, hydrocarbyl monolithium compounds R-Li, where R may be an aliphatic, cycloaliphatic or aromatic hydrocarbon moiety having 1 to 12 C atoms, are used as initiators. It is preferred to use n-butyllithium or sec-butyllithium, more preferably sec-butyllithium.
[0034] The amount of polymerization initiator required depends on the desired molecular weight, and is generally in the range of about 0.01 to about 0.07 mol %, preferably 0.01 to 0.07 mol %, based on the total amount of monomers.
[0035] The polymerization is preferably carried out in the presence of a solvent. Suitable solvents are conventional aliphatic, cycloaliphatic or aromatic hydrocarbons having from 4 to 12 carbon atoms and used in anionic polymerizations, such as pentane, hexane, heptane, cyclohexane, methylcyclohexane, isooctane, benzene, alkylbenzenes, such as toluene, xylene, ethylbenzene or decalin, or suitable mixtures. The use of cyclohexane and methylcyclohexane is preferred.
[0036] The polymerization temperature is generally 0 to 100° C., preferably 30 to 90° C., particularly preferably 40 to 90° C. The polymerization reaction is generally carried out in several stages, in which case the initiator is added at once using a single initiation process.
[0037] The order of monomer addition depends on the block structure selected. For batch processes, it is preferred to start by using all or part of a solvent such as cyclohexane as the initial requirement. Then, the vinyl aromatic monomer required for the first block S1 is added. Then, the initial requirement of an initiator such as sec-butyl lithium required to establish the desired molar mass is added, plus what is known as a titration amount, which serves to destroy traces of impurities in the solvent and in the reaction tank. Part of the monomer required to produce block S1 is used as the initial requirement in the reaction vessel, and then the polymerization reaction is started by adding the initiator. In order to obtain a clear block transition, it is necessary to allow the polymerization to continue until all the monomers have reacted before adding the second monomer. This is typically observed by monitoring the reaction temperature. If the temperature starts to decrease after increasing during the reaction, then all the monomers have reacted. Then, after all the vinyl aromatic monomers have been consumed, a diene monomer is added and polymerized to produce block B.
[0038] Then, after all the diene monomer has been consumed, the remaining amount of vinyl aromatic monomer is added and polymerized to produce block S2.
[0039] Once polymerization is complete, the living polymer chains may be capped using a chain terminator.
[0040] Suitable chain terminators are protonating substances or Lewis acids, such as water, alcohols (eg isopropanol), aliphatic or aromatic carboxylic acids, or inorganic acids, such as carbonic acid or boric acid.
[0041] By using a chain terminator as described above, linear block copolymers S1-B-S2 can be obtained.
[0042] A further aspect of the present invention is a polymer composition comprising a block copolymer (A) as described, and one or more further optional additives and / or processing aids (B) and / or at least one optional thermoplastic polymer (C) different from (A) and (B).
[0043] Generally, the proportion of the soft phase essentially (at least 85% by weight, often 85-100% by weight) built up from polymerized dienes in the polymer composition according to the invention is between 15 and 35% by weight, and the soft phase embedded in the hard phase (proportion 66-85% by weight) essentially (at least 85% by weight, often 85-100% by weight) built up from polymerized vinyl aromatic monomers has a cylindrical morphology.
[0044] The at least one further thermoplastic polymer (C) different from (A) and (B) is in particular at least one vinyl aromatic polymer, preferably at least one styrene polymer, such as standard polystyrene (GPPS).
[0045] Standard polystyrenes suitable as polymer (C) as well as their preparation, structure and properties are described in detail in review literature (A. Echte, F. Haaf, J. Hambrecht, Angew. Chem. (Int. Ed. Engl.) 20, 344-361 (1981); and Kunststoffhandbuch, R. Vieweg and G. Daumiller, eds., Vol. 4 "Polystyrol", Carl-Hanser-Verlag Munich (1996)).
[0046] The incorporation of block copolymer (A) can occur at any desired point once the polymerization is complete, for example after termination, devolatilization, or other post-treatment steps.
[0047] Furthermore, the polymer composition according to the present invention may optionally contain additives and / or processing aids (B). The additives and / or processing aids may be used in an amount of 0.01 to 5% by weight based on the total polymer composition.
[0048] Suitable additives and / or processing aids are in particular stabilizers, antiblocking agents, dyes and UV absorbers. Stabilizers, in particular oxygen radical scavengers, e.g. Irganox (R) 1010, Songnox (R) 1010, Irganox 1076, Irganox 565 and blends thereof, carbon radical scavengers such as Sumilizer (R) GS, Sumilizer GM and blends thereof, and / or secondary stabilizers such as Irgafos (R) It is preferred to use 168. The above stabilizers are commercially available.
[0049] The above-mentioned stabilizers are preferably used in an amount of 0.01 to 0.5% by weight, more preferably 0.1 to 0.3% by weight. The use of antiblocking agents such as high impact polystyrene (HIPS) is even more preferred. The antiblocking agent is preferably used in an amount of 0.1 to 1% by weight.
[0050] The polymer composition according to the invention can be produced by compounding during devolatilization of the block copolymer (A), for example by adding polystyrene to a vented extruder in the form of a "cold feed". A joint work-up results in a homogeneous composition which can also be used directly by processing equipment in a non-mixing injection molding mechanism. Alternatively, however, a mixture of pellets can also be directly processed in a kneader, extruder, or injection molding mechanism which provides mixing, resulting in a polymer composition according to the invention.
[0051] It has been found that materials based on block copolymer (A) allow for the extrusion of blown and cast films with high melt strength.
[0052] A further aspect of the present invention is a molded article, particularly a film, made from the block copolymer (A) or polymer composition according to the present invention.Due to the specific structure with clear block transition and specific increased total molecular weight of block copolymer (A), the film made from block copolymer (A) or polymer composition containing it has good mechanical properties and shows reduced blocking (interlayer adhesion when wound on a roll during the manufacturing process).Furthermore, due to the cylindrical morphology of the soft phase and the specific total diene ratio, it has been found that the organoleptic properties of the material based on block copolymer (A) are significantly improved.
[0053] A further aspect of the present invention is the use of a block copolymer (A) or a polymer composition according to the present invention for the manufacture of a film.The present invention is further illustrated by the claims and the following examples. EXAMPLES
[0054] All solvents and monomers used were dried and purified before use.
[0055] Test Method The melt mass flow index (=MFI, [ml / 10 min]) was measured on the molten polymer at 220° C. and 5 kg load according to ISO1133-1:2011.
[0056] The number average molecular weight Mn was determined by GPC according to ISO16014-3:2012 (size exclusion with relative calibration against T<60° C. polystyrene standards).
[0057] Organoleptic tests were performed in a 100 ml Erlenmeyer flask containing 10 g of SBC polymer granules. Boiling water was prepared and poured directly from the boiler into the Erlenmeyer flask. The steam was gently fanned towards the nose with the hand and graded by a panel of at least three people according to the following criteria: 0 = completely odorless; no odor at all 1 = slight odor indication 2 = detectable but well tolerated odor 3 = Strong odor, still acceptable 4 = Very strong odor, unacceptable.
[0058] The extrudability (melt strength) was graded in a "Rheotens type" test as follows: The polymer melt was heated to T=200° C. and 230° C. and poured from a heated vessel: [Table 1]
[0059] Film blocking (adhesive) was performed by casting 1 mm film from 220°C hot melt onto a chilled roll, followed by 10 cm 2 The adhesive strength was tested by compressing the two film layers with an external weight of 5 kg at 100°C. After one day, the films were separated by hand and the adhesion was graded by a panel of technicians on a value of 0 to 2: 0 = easy separation, no stickiness 1 = slightly sticky but separable 2 = Separable but strongly adhesive, close.
[0060] The tensile properties (elongation at break) were determined according to DIN EN ISO527-3:2019-02. The morphology was determined by transmission electron microscopy on OsO4 stained ultramicrotome samples of the SBC polymers or their polymer compositions.
[0061] General method for producing styrene butadiene block copolymer The SBC block copolymers tested were obtained by living anionic polymerization of styrene and butadiene using sec-butyllithium as initiator in anhydrous cyclohexane with the exclusion of moisture at temperatures of about 50-100° C. Reaction times: between 2.5 and 3.5 hours.
[0062] Tapered blocks of linear SBCs of structure S1-B-S2 or star-shaped SBCs with branches of structure S1-B-S2~ were synthesized by simultaneous addition of styrene and butadiene, which results in polymerization of butadiene first, followed by tapered sequences terminating in short styrene sequences.
[0063] Distinct blocks of linear SBCs of structure S1-B-S2 or branched star-shaped SBCs of structure S1-B-S2~ were synthesized by first adding styrene and polymerizing until monomer consumption was complete, and then adding butadiene and polymerizing until monomer consumption was complete.
[0064] Then, in the case of linear SBC, isopropanol was added as a chain terminator, or in the case of star-shaped SBC, epoxidized soybean oil was added as a chain terminator at a ratio of 1 L epoxidized soybean oil per 9.01 moles of sec-butyllithium initiator used.
[0065] Finally, each SBC polymer solution was acidified with CO2 / water and stabilized with 1500 ppm Irganox 1010, 1500 ppm Sumilzer GS, and 1800 ppm Irgaphos 168.
[0066] The final polymer concentration in cyclohexane was 30% by weight.
[0067] Each individually obtained SBC polymer solution was then fed into a 25 mm twin screw kneading extruder and the cyclohexane and extruder dome were vacuum degassed to a residual cyclohexane content of 2000 mg / kg polymer at a melt temperature of about 200°C.
[0068] The polymer melt of each individual SBC or optionally its blend with polystyrene (PS) (standard radically polymerized styrene with Mw 250,000 g / mol and Mn 100,000 g / mol) was extruded through a die and strands were chopped by a strand pelletizer.
[0069] For the production of films, films of desired thickness were cast from a 220° C. hot melt of SBC or its blends with GPPS onto a chilled roll using a single screw extruder.
[0070] The obtained test data is shown in Table 1. Examples C1 to C5 are comparative examples.
[0071] [Table 2]
[0072] The data show that the SBC block copolymers according to Example 1 of the present invention have improved extrudability (melt strength) compared to linear SBC block copolymers with tapered blocks (see Example C4) or with distinct blocks (see Example C5) with low number average molecular weights Mn of 82,000 g / mol or 74,000 g / mol, respectively.
[0073] Furthermore, the organoleptic properties of the SBC block copolymers according to the invention (see Example 1) are improved compared to the linear SBC block copolymers with tapered blocks (see Example C4), and the elongation at break is improved compared to the linear SBC block copolymer of Example C5.
[0074] Molded articles, especially thin films, made from the example SBC block copolymers have advantageous properties.
Claims
1. At least two polymer blocks S of different number average molecular weights Mn consisting essentially of at least one vinyl aromatic monomer and at least one polymer block B consisting essentially of at least one conjugated diene. wherein at least two of the blocks S are terminal blocks S1 and S2; and wherein the block copolymer (A) comprises, based on the entire block copolymer (A), 65 to 85%, preferably 68 to 80%, more preferably 70 to 75% by weight of at least one vinyl aromatic monomer, and 15 to 35% by weight, preferably 20 to 32% by weight, more preferably 25 to 30% by weight of at least one conjugated diene Consists of; wherein the proportion of the soft phase essentially made up of polymerized conjugated dienes is 15-35% by volume based on the total block copolymer (A), and wherein the soft phase embedded in the hard phase essentially made up of polymerized vinyl aromatic monomers has a cylindrical morphology; And wherein the block copolymer (A) is - have clear block transitions; and having a number average molecular weight Mn of at least 140,000 g / mol; The above block copolymer (A).
2. 2. The block copolymer (A) according to claim 1, having a number average molecular weight of the block copolymer (A) in the range of 140,000 to 1,000,000 g / mol, more preferably 140,000 to 500,000 g / mol, most preferably 140,000 to 300,000 g / mol.
3. 3. Block copolymer (A) according to claim 1 or 2, of structure (I) S1-B-S2.
4. Block copolymer (A) according to any one of claims 1 to 3, comprising 68 to 80% by weight, preferably 70 to 75% by weight, of at least one vinyl aromatic monomer, in particular styrene, and 20 to 32% by weight, preferably 25 to 30% by weight, of at least one conjugated diene, in particular butadiene and / or isoprene.
5. The block copolymer (A) according to any one of claims 1 to 4, wherein the Mn of the polymer block S1 is between 12,000 and 50,000 g / mol, the Mn of the polymer block S2 is between 40,000 and 150,000 g / mol, and the Mn of the polymer block B is between 15,000 and 80,000 g / mol.
6. The block copolymer (A) according to any one of claims 1 to 5, wherein the vinyl aromatic monomer is styrene and the conjugated diene is butadiene.
7. Block copolymer (A) according to any one of the preceding claims, in which the proportion of the soft phase essentially built up of polymerised conjugated dienes is between 18 and 32% by volume.
8. 7. The method according to claim 1, wherein the proportion of the soft phase essentially constituted by polymerized conjugated dienes is between 22 and 30% by volume. 1 Item 2. The block copolymer (A) according to item 1.
9. A process for the preparation of the block copolymer (A) according to any one of claims 1 to 6 by sequential anionic polymerization of monomers.
10. A polymer composition comprising at least one block copolymer (A) according to any one of claims 1 to 8 and one or more further optional additives and / or processing aids (B) and / or at least one thermoplastic polymer (C) different from (A) and (B).
11. 9. The polymer composition of claim 8, wherein the thermoplastic polymer (C) is polystyrene.
12. 12. The polymer composition according to claim 10 or 11, wherein the proportion of the soft phase formed from the polymerized diene is 15 to 35% by weight, based on the total polymer composition, and the soft phase embedded in the hard phase formed from the polymerized vinyl aromatic monomer has a cylindrical morphology.
13. The polymer composition according to claim 10, wherein the proportion of the soft phase formed from the polymerized diene is between 18 and 32% by weight, preferably between 22 and 30% by weight, based on the total polymer composition.
14. A molded article, in particular a film, produced from a block copolymer (A) according to any one of claims 1 to 8 or from a polymer composition according to any one of claims 10 to 13.
15. Use of a block copolymer (A) according to any one of claims 1 to 8 or a polymer composition according to any one of claims 10 to 13 for the manufacture of a film.
Citation Information
Patent Citations
Composition for stretch film
CN102803356A
Method of controlling block copolymer characteristics and articles manufactured therefrom
CN104744947A
Block copolymers composition
JP1977078260A
Manufacturing method of multi-component multi-phase polymer material with three-dimensional co-continuous micro-phase separation structure
JP1993287084A
Manufacturing method of optical member, optical member, electro-optical device, and electronic equipment
JP2004029169A