High molecular weight functionalized polymers for electrochemical cells.

High molecular weight functionalized polymers with high dielectric constants and low glass transition temperatures address safety and conductivity issues in lithium ion batteries, enhancing performance and manufacturing efficiency.

JP2024537025AInactive Publication Date: 2024-10-10IONIC MATERIALS INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024518513
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-27
Filing Date
2022-09-27
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional electrolytes in lithium ion batteries face safety issues due to flammability and require high temperatures for effective conductivity, while polymer electrolytes like PEO suffer from low conductivity at room temperature and inefficient ion transport.

Method used

Development of high molecular weight functionalized polymers with high dielectric constants and low glass transition temperatures, produced through addition polymerization or anionic ring opening, which are used as polymer electrolytes in lithium ion batteries, enhancing ion dissociation and conductivity.

Benefits of technology

The high dielectric polymers improve safety and conductivity at lower temperatures, enabling solvent-free electrode manufacturing and reducing manufacturing costs, while maintaining high ionic conductivity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024537025000001_ABST
    Figure 2024537025000001_ABST
Patent Text Reader

Abstract

Disclosed herein are high molecular weight functionalized polymers ("high dielectric polymers") along with associated methods of use and manufacture. High dielectric polymers have a relatively high dielectric constant (e.g., greater than 10) as well as a relatively low glass transition temperature (e.g., less than -30°C). The polymers can be produced utilizing addition polymerization or anionic ring opening to yield linear or branched polymer backbones containing a number of residual nucleophilic groups. Nucleophilic substitution can then be performed to functionalize the residual nucleophilic groups. The functionalized polymers can then be purified and used as needed as polymer electrolytes in electrochemical cells (e.g., as non-aqueous polymer electrolytes in secondary Li-ion batteries).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to polymer electrolytes, and more particularly to high molecular weight functionalized polymers for electrochemical cells (e.g., lithium ion batteries). [Background technology]

[0002] Non-aqueous batteries such as lithium-ion batteries are widely used as power sources in small and portable device applications due to their high energy density. More recently, the energy density and reliability of such batteries have improved to a level that allows them to be used in all electric vehicles. In parallel with these developments, it is also important to ensure safety.

[0003] Modern Li-ion batteries typically consist of three components: (1) a positive electrode, (2) a negative electrode, and (3) an electrically insulating but ionically conductive intermediate layer (i.e., the separator). Summary of the Invention [Means for solving the problem]

[0004] High molecular weight functionalized polymers are disclosed herein along with related methods of use and manufacture. The high molecular weight functionalized polymers of the present disclosure have a relatively high dielectric permittivity (e.g., greater than 10) as well as a relatively low glass transition temperature (e.g., less than -30°C). These properties represent unique advantages when the polymers are used as polymer electrolytes in electrochemical cells such as lithium ion batteries. For example, the high dielectric constant of the material allows for strong dissociation of ions, which in turn leads to high solubility of lithium salts.

[0005] The glass transition temperature (T g) indicates how easily or difficult it is for the polymer chains in a structure to move about freely, and therefore how easily ions can be transported through the structure. The glass transition temperature of an amorphous polymer represents the temperature at which the polymer transitions from a hard, brittle state to a soft, rubbery state. Therefore, lowering the glass transition temperature of a polymer allows for more segmental motion and improves electrical conductivity.

[0006] The use of branched polymers instead of linear polymers in the disclosed polymeric materials is also advantageous compared to previous approaches, since the branches prevent (i.e., hinder) the chain packing and prevent the polymer from crystallizing. This is manifested by the polymer becoming a relatively viscous liquid-like polymer rather than a solid due to a reduction in the glass transition temperature of the polymer. The high molecular weight functionalized polymers of the present disclosure (alternatively referred to herein as "high dielectric polymers") have both high dielectric constants and low glass transition temperatures, making them highly suitable for use as polymer electrolytes in lithium-ion batteries.

[0007] The disclosed high dielectric polymers can be produced using addition polymerization or anionic ring opening to produce linear or branched polymer backbones containing multiple residual nucleophiles. The residual nucleophiles can then be functionalized by nucleophilic substitution. While Michael addition is a suitable method for nucleophilic substitution, the more standard S N It is also possible to use alkyl halides for type 2 nucleophilic substitution. In the Michael addition, the linear or branched polymer starting material containing protic nucleophilic groups (-OH, -SH, -NH2) produced in the first step acts as a polymeric Michael donor. A functional group with an α,β-unsaturated C=C bond attached to a strong electron-withdrawing group (EWG) acts as a Michael acceptor. The donor and acceptor react in the presence of a catalyst to attach the Michael acceptor to the polymer starting material. This functionalized polymer can then be purified.

[0008] In one aspect, a method for producing a high dielectric polymer is disclosed, comprising reacting a starting material containing at least three nucleophilic sites with a crosslinker to produce a polydonor, the polydonor being a branched polymer containing multiple reactive nucleophilic sites, functionalizing the multiple reactive nucleophilic sites of the polydonor to produce the high dielectric polymer, and purifying the high dielectric polymer. In the disclosed method, the starting material may be selected from the group consisting of polyalcohols (polyols), sorbitol, pentaerythritol, inositol, pentaerythritol, dipentaerythritol, amino alcohols, tris(hydroxymethyl)aminomethane, 2-amino-2-methyl-1-propanol, 2-amino-2-methyl-1,3-propanediol, cysteine, dithiothreitol, other thiols, and / or polyethyleneimine. In these and other methods, the starting material may be a Michael donor. In some embodiments, the multiple nucleophilic sites may include -OH, -NH2, and / or -SH groups. In these and other embodiments, the crosslinker may be a bifunctional crosslinker. In some such embodiments, the crosslinker may be a diglycidyl ether, dichloride, dibromide, diisocyanate, epichlorohydrin, diacrylate, divinyl, and / or dialdehyde (e.g., divinyl sulfone, glycerol diglycidyl ether, PEG-diglycidyl ether, and / or epichlorohydrin). The disclosed methods may further include purifying the polydonor, as required. In these and other embodiments, functionalizing the multiple reactive nucleophilic sites may be accomplished by nucleophilic addition. In selected embodiments, functionalizing the multiple reactive nucleophilic sites may be accomplished by Michael addition. The method may also include combining the high dielectric polymer with an electrochemically active material to form a polymer electrolyte.In some such embodiments, the method may also include incorporating the polymer electrolyte into the lithium ion battery as an anolyte or catholyte.

[0009] In another aspect, an electrochemical cell is disclosed that includes an anode having a first electrochemically active material, a cathode having a second electrochemically active material, a first electrolyte disposed on either the anode or the cathode, and a second electrolyte interposed between the anode and the cathode. At least one of the first electrolyte and the second electrolyte includes a high dielectric polymer having a dielectric constant greater than 10 and a glass transition temperature less than -30°C. In some such embodiments, the high dielectric polymer has a dielectric constant greater than 20 and a glass transition temperature less than -70°C. In these and other embodiments, the second electrochemically active material includes lithium ions. In some such embodiments, the first electrolyte may include a high dielectric polymer.

[0010] In yet another aspect, a high dielectric polymer is disclosed that includes a branched functionalized polymer backbone, the high dielectric polymer having a dielectric constant greater than 10 and a glass transition temperature less than -30°C. The high dielectric polymer can be produced in some embodiments by functionalizing multiple nucleophilic sites of a polydonor. An electrochemical cell can be formed that includes a polymer electrolyte that contains the high dielectric polymer of the present disclosure. In some such embodiments, the electrochemical cell can be a lithium ion cell. [Brief description of the drawings]

[0011] [Figure 1] 1 illustrates an exemplary method of forming a polymer electrolyte constructed in accordance with the present disclosure. [Diagram 2] 1 illustrates an example of a chemical reaction scheme for forming a high dielectric polymer configured in accordance with an embodiment of the present disclosure. [Diagram 3] 1 shows an exemplary reaction scheme for forming a polydonor as disclosed herein. [Figure 4] 1 shows exemplary chemical reaction schemes for various bifunctional crosslinkers that can be used according to the disclosed methods. [Diagram 5] FIG. 1 shows an exemplary chemical reaction scheme for the production of hyperbranched polyglycerol using n-butanol as the starting molecule and glycidol as the monomer. [Figure 6] 1 shows a Michael addition between an alcohol and an amine. [Figure 7] 1 shows the Michael addition of various acceptors to primary alcohols. [Figure 8] An example of nucleophilic addition between a nucleophilic group and an alkyl halide is shown. [Figure 9A] FIG. 2 is a diagram showing the chemical structure of the highly dielectric polymer obtained in Example 1. [Figure 9B] 9B shows a differential scanning calorimetry (DSC) curve of the highly dielectric polymer of FIG. 9A. [Figure 9C] 9B shows the FTIR spectrum of the highly dielectric polymer of FIG. 9A. [Figure 10] 1 shows a chemical reaction scheme for producing the polydonor of Example 5. [Figure 11] 1 shows a chemical reaction scheme for producing the polydonor of Example 7. [Figure 12] 1 shows a cross-sectional micrograph image of a composite cathode electrode containing the high dielectric polymer electrolyte of Example 8. [Figure 13] FIG. 13 shows exemplary cycling behavior of a cathode half-cell using the composite cathode electrode described in Example 8 and shown in FIG. [Figure 14] 1 shows a chart of the dielectric constants measured for the high dielectric polymer of Example 1 and the high dielectric polymer produced from the polydonor described in Example 7. [Figure 15] 1 shows a chart of measured ionic conductivity as a function of salt concentration for two different salts of a polymer electrolyte made from the polymer of Example 1. [Figure 16]1 shows a chart of the measured conductivity of the high dielectric polymer described in Example 1 when made into a polymer electrolyte containing 40% by weight LiTFSI. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] So that those skilled in the art to which the disclosed system pertains can more readily understand how to make and use it, reference can be made to the following drawings. Previous and current electrolytes for rechargeable lithium-ion batteries (as well as other types of electrochemical batteries) have significant drawbacks. The specific drawbacks of conventional liquid, polymer, and ceramic electrolytes are discussed in detail below, followed by a complete description of the disclosed high dielectric polymers and associated methods of making and using.

[0013] The positive electrode has typically been prepared by, but not limited to, mixing one or more positive electrode active materials in single crystal or particulate form with an electrochemically inert but electronically conductive material, a polymeric binder, and a solvent to form a slurry. The slurry was then coated onto both sides of a suitable substrate, such as, but not limited to, aluminum foil. The coated substrate was then dried to remove the solvent. The assembly was then calendered, typically by passing the as-coated substrate between rollers, to densify the electrode.

[0014] The process for fabricating the negative electrodes was similar, but with a negative active material and different substrates, such as, but not limited to, copper foil. By design, the as-assembled electrodes have a certain porosity, average pore size, and pore size distribution that allows contact with the non-aqueous electrolyte while providing the desired energy density. The electrodes are separated by a separator, an electronically insulating but ionically conductive membrane with pre-designed porosity and pore characteristics, and the pore space is filled with a liquid organic solvent containing a dissolved lithium salt. The mixture of organic solvent and lithium salt is known as the electrolyte and is necessary for the transport of lithium ions to and from the positive and negative electrodes. The separator may have two or more layers. It typically contains a polyolefin layer that can melt at a temperature well below the temperature of thermal runaway (a type of catastrophic failure of the battery) and stop the electrochemical reaction by closing its pores during melting. Unfortunately, these membranes have poor dimensional stability and can shrink at high temperatures, which can allow physical contact between the positive and negative electrodes. This creates a short circuit that can lead to a catastrophic thermal runaway event. To mitigate this failure, one or two heat-resistant layers are attached to the shutdown layer. The heat-resistant layer consists of a binder and heat-resistant particulates, typically in the range of 0.2 to 2.0 microns (0.2 to 2.0 μm), including but not limited to Al2O3, SiO2, or TiO2, present in a concentration that can minimize the shrinkage of the assembled separator layers to an amount that prevents the battery's electrodes from touching each other.

[0015] Conventional electrolytes used in Li-ion batteries contain a mixture of highly flammable liquids, including but not limited to cyclic carbonates, such as ethylene carbonate, and linear carbonates, such as diethyl carbonate, which can result in a thermal runaway event if the battery is shorted, overcharged, overheated, or experiences some other malfunction. The flammability of the electrolyte and the general safety of Li-ion batteries is exacerbated by the presence of the positive electrode, which is usually, but not limited to, some type of lithium-containing transition metal oxide. These transition metal oxides act as a solid oxygen source, releasing oxygen when heated, allowing the lithium-ion battery to continue burning even when air is no longer supplied.

[0016] To overcome these safety concerns, researchers have focused on replacing traditional flammable liquid electrolytes with thermally robust polymer and ceramic electrolytes. -3 ~10 -2 They offer high intrinsic conductivity on the order of S / cm, but require high processing temperatures, are very sensitive to air / moisture, and are often brittle and rigid, resulting in problems with the interfacial contact with the positive and negative electrodes. Polymer electrolytes have been studied since the 70s, with polyethylene oxide (PEO) being by far the most studied. However, PEO suffers from a relatively low electrical conductivity at room temperature, with most PEO-salt formulations exhibiting only a 10 -6 ~10 -4 The conductivity reaches 1.5 S / cm and only shows significant conductivity at temperatures >60°C. This is due, in part, to the Li + PEO, which has a relatively low dielectric constant of about 6-7, is a material that is highly resistant to the four ether-centered Li + Wrapped around Li + This chelation structure is dependent on the formation of a strong chelation complex with Li + Because the number of Li transitions is relatively low, most of the measured conductivity is due to anion transport, which does not contribute significantly to the performance of the battery. This chelation structure also allows for a large number of Li +This results in the interchain transport of Li dominating over the intrachain transport of Li in PEO. + The transport of lithium is primarily via segmental (or segmented) motion within the chains, and therefore requires high temperatures to achieve useful electrical conductivity. One way to increase the amount of segmental motion at a given temperature is to lower the glass transition temperature of the polymer. This can be achieved to some extent by decreasing the molecular weight of the polymer or by creating a branched polymer structure. Polymers with a high degree of branching generally pack less efficiently (i.e., have more excess free volume, and lower density) and, as a result, have lower glass transition temperatures than their linear counterparts. The use of branched structures instead of linear chains can effectively increase the conductivity of polymer gel electrolytes (polymer gels consist of a polymer matrix swollen with a small molecule liquid containing dissolved lithium salts), with higher degrees of branching indicating better electrical conductivity.

[0017] One important aspect of a solvent for battery electrolytes is that it should have a relatively high dielectric constant to promote a high degree of ionic dissociation, which allows for high electrical conductivity. Standard organic solvents such as ethylene carbonate (ε ≈ 90), propylene carbonate (ε ≈ 64), and acetonitrile (ε ≈ 36) have dielectric constants 6-15 times higher than PEO. For polymer electrolytes to reach sufficient electrical conductivity for practical applications, the dielectric constant should be >10, preferably >20, and the dielectric constant should be >10 at a frequency on the order of the ion hopping rate, i.e. >10. 6 It has been proposed that the dielectric constant remains high at 1000 Hz. To achieve high dielectric constants in polymers, functional groups containing high dipole moments can be incorporated, which should have relatively high mobility to maintain high dielectric constants at higher frequencies. Through molecular dynamics simulations, it has been demonstrated that an optimal balance of high dipole functional group density exists that allows for a large amount of ion pair dissociation without excessive dipole-dipole interactions in the polymer, which results in low free volume and a decrease in dielectric constant at higher frequencies.

[0018] In addition to improved safety, the development of bulk polymer electrolytes enables new electrode processing and manufacturing methods. Because the polymers are available in a molten state, electrodes can be manufactured in solvent-free processes such as extrusion. This allows for simplified electrode manufacturing methods and lowers manufacturing costs. In some aspects, the present disclosure provides polymers that have a dielectric constant >10, and in many embodiments >20, and that maintain this high dielectric constant at relevant frequencies and temperatures. In other aspects, the present disclosure provides methods for manufacturing these polymers into electrodes and secondary Li-ion batteries.

[0019] definition As used herein, the following terms should be understood to have the meanings set forth below as well as their conventional technical meanings, unless such conventional meanings conflict with a definition provided herein.

[0020] Polymer - a molecule consisting of several repeating units covalently bonded together. Used herein to refer to the reaction product of a Michael donor with a crosslinker (defined below in Polydonors) and the reaction product of a Michael acceptor with a Polydonor (defined below).

[0021] Michael Addition − Conjugate addition reaction between a Michael donor and a Michael acceptor. Michael Donor - any molecule that contains a protonated nucleophile or carbanion. Examples of nucleophiles include alcohols (-OH), amines (-NH2, -NH-), and thiols (-SH). Other nucleophiles include -PH x O 3-x where 0≦x<4, as well as active methylenes such as malonates and nitroalkanes.

[0022] Michael acceptor - any molecule containing an α,β-unsaturated carbon with a strong electron-withdrawing group attached. Both the α and β carbons to the electron-withdrawing group may be unsubstituted, although this is not strictly necessary, merely allowing for a faster, more efficient reaction due to a more favorable stereochemistry.

[0023] Crosslinker - any difunctional molecule that can react with a Michael donor to produce oligomers and polymers. Examples of crosslinkers include, but are not limited to, diglycidyl ethers, dihalogenated organic compounds, diisocyanates, divinyls and diacrylates.

[0024] Catalyst--Any molecule or energy source used to enhance the rate of reaction between the crosslinker and the Michael donor, or between the nucleophilic group of the Michael donor and the Michael acceptor. Examples of bases that can be used include lithium hydroxide (LiOH), sodium hydroxide (NaOH), potassium hydroxide (KOH), cesium carbonate (Cs2CO3), potassium carbonate (K2CO3), lithium methoxide (LiOMe), lithium tert-butoxide (LiOt-Bu), potassium tert-butoxide (KOt-Bu). However, strong Bronsted acids such as bistriflimidic acid (HTFSI), tetrafluoroboric acid (HBF4), hexafluorophosphoric acid (HPF6), triflic acid (HOTf), as well as strong Lewis acids, have also been shown to be efficient catalysts for Michael addition and can also be used. Ultraviolet radiation, infrared radiation, and / or heat may also be used as catalysts for any suitable chemical reaction described herein.

[0025] Polydonor - the polymeric reaction product of one or more Michael donors and one or more crosslinkers as defined above. High Dielectric Polymer - A purified polymeric reaction product of a polydonor and one or more Michael acceptors.

[0026] Salt - a compound that contains two or more ionically bonded moieties and can be dissociated by a suitable solvent. Polymer Electrolyte - a mixture of one or more high dielectric polymers and one or more lithium salts, with or without the presence of one or more additives.

[0027] Additive - any compound added to a polymer electrolyte in an amount less than 10 wt. % to obtain more desirable properties of the resulting polymer electrolyte and battery (e.g., to improve processability, mechanical properties, or electrochemical performance).

[0028] Plasticizer--a subclass of additives that act to reduce the viscosity and / or glass transition temperature of high dielectric polymers and / or polymer electrolytes. Co-solvent - a subclass of additives used to facilitate dissociation of lithium salts when, for a given loading of salt, the high dielectric polymer is unable to completely dissociate the salt.

[0029] Methods for forming high dielectric polymers: As previously mentioned, the present disclosure describes unique high dielectric polymers, as well as methods of using the high dielectric polymers in electrochemical batteries (e.g., lithium ion batteries). Figure 1 shows an exemplary method of producing the high dielectric polymers according to various embodiments of the present disclosure.

[0030] As shown in FIG. 1, the method 100 includes reacting a starting material with a crosslinker to generate a polydonor (block 102). The starting material can be any compound with three or more reactive nucleophilic sites. In some embodiments, the starting material can be a Michael donor molecule. In selected embodiments, the starting material can be a polyhydric alcohol (polyol), such as sorbitol, pentaerythritol, inositol, pentaerythritol, dipentaerythritol, or other polyols, tris(hydroxymethyl)aminomethane, 2-amino-2-methyl-1-propanol, 2-amino-2-methyl-1,3-propanediol, or other amino alcohols, cysteine, dithiothreitol, other thiols, and / or polyethyleneimine. The crosslinker can be any suitable type of bifunctional molecule (i.e., reactive with the nucleophilic sites of the starting material). Exemplary crosslinkers include, but are not limited to, diglycidyl ethers, dichlorides, dibromides, diisocyanates, epichlorohydrin, diacrylates, divinyls, and / or dialdehydes.

[0031] To complete the reaction between the starting materials and the crosslinker (block 102), the starting materials are dissolved in a suitable solvent with or without a catalyst, such as potassium hydroxide (KOH), sodium hydroxide (NaOH), lithium hydroxide (LiOH), potassium carbonate (K2CO3), cesium carbonate (Cs2CO3), triethylamine (TEA), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), magnesium oxide (MgO), barium oxide (BaO), or aluminum oxide (Al2O3).

[0032] The crosslinker can be added dropwise to the starting material mixture under vigorous stirring at a temperature suitable for the reaction. Adding the crosslinker dropwise to the starting material solution ensures that there is always an excess of starting material (e.g., Michael donor) so that, statistically, each reactive group on the crosslinker will react with two different starting material molecules. When the crosslinker is added dropwise to a vigorously mixing solution of starting materials, oligomers will form and eventually begin to link together to form a polymer. Because oligomers and polymers contain a large number of residual reactive sites, addition polymerization will result in randomly branched polymer structures. Depending on the starting materials, crosslinker, and temperature, a catalyst may or may not be necessary or desired to drive the reaction. Additionally, for certain crosslinkers such as chlorides and bromides, compounds such as NaOH or triethylamine should be present in at least an equimolar ratio to the chloride / bromide concentration to neutralize or capture the HCl and HBr generated from the reaction of the chloride / bromide with the Michael donor. The reaction is allowed to proceed for a sufficient time to ensure that all reactive groups on the crosslinker have reacted. The polymer produced in this step is called a polydonor (because it is a polymeric version of the Michael donor starting material used).

[0033] An alternative method to addition polymerization for producing branched polydonors is by anionic ring-opening polymerization of glycidol, modified glycidyl ethers, oxiranes, oxetanes, and mixtures thereof. In these embodiments, the preparation of hyperbranched polydonors is carried out using seeding monomers containing one or more alcohols, amines (primary or secondary), or thiols, followed by the addition of a strong base such as lithium methoxide, followed by the addition of glycidol. The ring structure of glycidol reacts with the deprotonated nucleophilic group, opening the ring to form a carbon-nucleophilic group bond, producing secondary and primary alcohols simultaneously. The primary and secondary alcohols produced from this reaction then provide two new nucleophilic sites for more glycidol to react. This process results in a hyperbranched polyether structure with a large number of residual nucleophilic groups. The molecular weight of the resulting hyperbranched polymer can be controlled by varying the ratio of seeding monomers to glycidol, oxiranes, and oxetanes. The lower the ratio of seeding monomer to glycidol, oxirane and oxetane, the higher the molecular weight of the polymer produced.

[0034] A typical example of a branched polydonor produced in this way is hyperbranched polyglycerol (HPG). HPG is produced via anionic ring-opening polymerization of glycidol in the presence of various seeding monomers such as butanol, ethanediol, tris(hydroxymethyl)propane. This results in HPG with various degrees of branching and high density of alcohols in the structure. By copolymerizing glycidol with oxiranes or oxetanes that do not contain nucleophilic groups such as hydroxides, it is possible to tune the final concentration of nucleophilic groups in the structure, and therefore to control the final concentration of functionalized high dielectric groups in the final high dielectric polymer.

[0035] After the polydonor scaffold is generated, it can be purified (block 104). Although discussed herein and shown in FIG. 1, purification of the polydonor may not be necessary. Purification can be advantageous when the reaction solvent or catalyst used in the generation of the polydonor is not suitable for the functionalization step (block 106). If both the solvent and catalyst for the polydonor synthesis (block 102) are suitable for the functionalization step (block 106), purification of the polydonor (block 104) can be avoided to minimize the number of steps and maximize the yield.

[0036] If performed, purification of the polydonor (block 104) can typically be accomplished by (1) neutralizing the base catalyst, (2) removing the solvent, and (3) removing any non-polymeric compounds (e.g., salts from the neutralization, oligomers from the reaction, or residual monomers). For ease of processing, the polydonor can be redissolved in a solvent, although this is not strictly necessary.

[0037] The method 100 continues with functionalizing the nucleophilic sites of the polydonor (Block 106). In some embodiments, the nucleophilic sites of the polydonor may be functionalized via Michael addition with one or more Michael acceptors. Michael acceptors include, but are not limited to, acrylonitrile, 2-sulfolene, methyl vinyl sulfone, ethyl vinyl sulfone, fumaronitrile, ethenesulfonyl fluoride, N-methylmaleimide, vinyl phosphonic acid, dimethyl vinyl phosphonate, methyleneflutaronitrile, lithium vinyl sulfonate, and methyl vinyl ether. Michael acceptors are more generally compounds that include an α,β-unsaturated carbon bond with an electron-withdrawing group attached.

[0038] Similar to the reaction of the starting material with the crosslinker (block 102), base catalysis may or may not be required to proceed with the functionalization reaction of the nucleophilic sites of the polydonor (block 106). Catalysts may be useful when the active nucleophilic groups are alcohols or thiols. If a catalyst is used for the reaction, the base catalyst is first added to the polydonor and mixed thoroughly. The polydonor-catalyst mixture is then added dropwise to a solution of Michael acceptor, with the Michael acceptor being present in a molar ratio of 1.2 to 10 times excess relative to the number of moles of nucleophilic sites present in the polydonor. Adding the polydonor dropwise to the excess Michael acceptor with vigorous stirring may be advantageous as it ensures that the nucleophilic sites on the polydonor react quickly. However, the reaction can also be carried out by adding the Michael acceptor dropwise to a vigorously mixed solution of polydonor and catalyst.

[0039] The polydonor functionalization reaction (block 106) can be carried out at ambient temperature. However, in other embodiments, the reaction proceeds when cooled below ambient temperature or when heated above ambient temperature, depending on the reactivity of a given polydonor, catalyst, and Michael acceptor. For example, when acrylonitrile is used as the Michael acceptor and NaOH is used as the base catalyst, OH - It is preferred to maintain the reaction temperature <30°C to avoid anionic attack of acrylonitrile by the anions. In the highly polar case of using aprotic solvents such as dimethylsulfoxide (DMSO) and acrylonitrile as the Michael acceptor, it is preferred to maintain the temperature below ambient with active cooling to avoid runaway reaction of excess acrylonitrile. If the temperature is not carefully controlled or if too much catalyst is used, the polymerization solution may discolor due to excessive side reactions between the catalyst and the Michael acceptor. Once the polydonor and Michael acceptor are fully coupled, the reaction is allowed to proceed to completion. The final product, consisting of a polydonor functionalized with a Michael acceptor, is called a highly dielectric polymer.

[0040] If a catalyst is used to produce the high dielectric polymer, an equimolar amount of acid may be added to neutralize the system. After neutralization, any solvent and residual Michael acceptor may be removed. The high dielectric polymer may then be purified (block 108). To purify the high dielectric polymer, various purification techniques may be used, including redissolving the high dielectric polymer in a solvent and removing residual salts from the neutralization and any by-products of the reaction. After this initial purification is complete, final purification may be performed by removing the solvent, redissolving the high dielectric polymer in an anhydrous solvent, and adding a drying agent (e.g., but not limited to, MgSO4, Na2SO4, CaH2, or molecular sieves) to reduce the moisture content to less than 100 ppm, preferably less than 20 ppm, and more preferably less than 2 ppm. Once dried, the solvent may be removed from the high dielectric polymer or may be left in place to facilitate further processing.

[0041] It is important to note that the polydonor may be functionalized (block 106) by methods other than Michael addition. For example, in some embodiments, the polydonor may be functionalized via nucleophilic substitution using an alkyl halide. This process is similar to Michael addition in that a base catalyst is used, but requires the use of at least an equimolar amount of base relative to the alkyl halide added. Suitable alkyl halides for this process include, but are not limited to, 4-bromobutyronitrile, 3-bromopropionitrile, 4-chloropropionitrile, 1-bromo-2-(methylsulfonyl)ethane, and 1-bromo-2-(methylsulfonyl)propane. To carry out this functionalization, the polydonor is first dissolved in an aprotic solvent such as acetonitrile (ACN), tetrahydrofuran (THF), dioxane, dioxolane, dimethylsulfoxide (DMSO), dimethylformamide (DMF), or another suitable solvent. Then, an equimolar amount of base relative to the alkyl halide used is added. Suitable bases include, but are not limited to, alkali metal carbonates (e.g., lithium carbonate, sodium carbonate, potassium carbonate), alkali metal hydroxides (e.g., lithium hydroxide, sodium hydroxide, potassium hydroxide), alkali alkoxides (e.g., lithium methoxide, sodium ethoxide, potassium terbutoxide), or tertiary amines (e.g., triethylamine (TEA)). Other suitable bases include lithium diisopropylamide (LDA), lithium hydride, and sodium hydride. An alkyl halide is added to the solution containing the polydonor and base and allowed to react. The products of this reaction are the highly dielectric polymer and the salt of the utilized halide with the base. For example, when TEA is used as the base and 3-bromopropionitrile is used as the alkyl halide, the by-product is triethylammonium bromide, i.e., the bromine salt of triethylamine.Once the polydonor has been functionalized via nucleophilic addition of an alkyl halide to produce a highly dielectric polymer, it can be purified (block 108), taking special care to ensure complete removal of excess halide salts.

[0042] The high dielectric polymers produced by method 100 may have unique characteristics compared to other polymers. For example, in some embodiments, the disclosed high dielectric polymers may have a dielectric constant greater than 10, and in some embodiments, greater than 20, 25, 30, 35, 40, 45, or 50. In these and other embodiments, the high dielectric polymers of the present disclosure have a glass transition temperature (T) of less than -30°C, e.g., less than -70°C, -80°C, -90°C, or -100°C. g High dielectric polymers that also have relatively low glass transition temperatures can offer significant advantages as polymer electrolytes compared to conventional electrolytes.

[0043] Figure 2 shows a chemical reaction scheme in which a high dielectric polymer is produced using the method 100 of Figure 1. In particular, Figure 2 shows the reaction of sorbitol (starting material) with butanediol diglycidyl ether (crosslinker) to form a branched polydonor, followed by Michael addition functionalization with acrylonitrile to form a high dielectric polymer. Figure 3 shows an exemplary reaction scheme for forming a polydonor via the reaction of dipentaerythritol (starting material) with divinyl sulfone (crosslinker). Although the polydonor product is shown linear, in reality the structure is randomly branched since all of the primary alcohols are equally likely to react with divinyl sulfone.

[0044] FIG. 4 shows chemical reaction schemes for various bifunctional crosslinkers. In particular, diglycidyl ether, dichloride (alcohol donor), dichloride (amine donor), diisocyanate (alcohol donor), diisocyanate (amine donor), divinyl and diacrylate are shown in FIG. 4. As used in FIG. 4, "X" represents any core molecular structure and "R" represents any donor molecule. FIG. 5 shows an exemplary reaction for the production of hyperbranched polyglycerol using n-butanol as the starting molecule and glycidol as the monomer. The molecular weight of the final polymer in FIG. 5 is determined by the ratio of starting molecule to glycidol. FIG. 6 shows the Michael addition between an alcohol, -OH (note that this reaction is equivalent to if a thiol, -SH, was used) and an amine, -NH2.

[0045] Figure 7 shows the Michael addition of various acceptors to primary alcohols. In particular, Figure 7 shows the reactions of fumaronitrile, 2-sulfolene, vinylene carbonate, and lithium vinylsulfonate.

[0046] FIG. 8 shows an example of nucleophilic addition between a nucleophilic group (-OH, -SH, NH2) and an alkyl halide (alkyl bromide). Methods for preparing polymer electrolytes: To produce a polymer electrolyte from the high dielectric polymer of the present disclosure, the high dielectric polymer is mixed with one or more lithium salts, and optionally one or more additives. Exemplary lithium salts include, but are not limited to, the following: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(oxalato)borate (LiBOB), lithium difluoro(oxalato)borate (LiDFOB), lithium difluorophosphate (LiDFP), lithium triflate (LiOTf), and lithium nitrate (LiNO3). Typical ranges of lithium salt concentration for high dielectric polymers are 5-40 wt%, depending on the solubility of the salt and the performance of the final mixture. Polymer-in-salt electrolytes can also be produced by increasing the salt concentration to >50 wt%. For example, LiFSI is soluble in several high dielectric polymers to at least 75% by weight. The nature of ionic conduction in these polymer-in-salt mixtures is expected to be different from that in standard polymer electrolytes.

[0047] Apart from lithium salts, additives can be added to high dielectric polymers to obtain higher electrical conductivity, more stable cycling of the battery, improve the mechanical properties of the resulting electrodes, improve safety, reduce flammability, and / or provide more desirable rheological properties that facilitate downstream processing. For example, the addition of triethyl phosphate can reduce flammability while also increasing the conductivity of the electrolyte. The addition of dimethyl carbonate (a low boiling, low dielectric, highly volatile solvent) can be used to reduce the viscosity to allow better film formation during slurry coating of the electrodes, which can be easily removed later with heat. The addition of fumed silica can be used to increase the viscosity and stiffness of the polymer electrolyte, facilitating calendering of the electrode mixture.

[0048] The disclosed polymer electrolytes can be incorporated into electrochemical cells as needed. The polymer electrolytes can be used in electrodes, stand-alone dielectrics, or as non-electrochemically active electrolytes interposed between electrodes. In lithium-ion batteries, the polymer electrolytes can be used in the anode, cathode, and / or as stand-alone dielectric non-electrochemically active electrolytes interposed between the anode and cathode electrodes. The stand-alone dielectric non-electrochemically active electrolytes can be thermoformed onto the anode or cathode by heating and attaching the polymer electrode to the anode or cathode using a lamination process or the like. In other embodiments, the polymer electrolytes can be bonded to the anode or cathode by a co-extrusion process. In embodiments where the polymer electrolyte is used as an anolyte or catholyte, the polymer electrolyte can be laminated to a current collector using conventional techniques known to those skilled in the art.

[0049] Lithium salts may be used for the polymers to function as electrolytes in Li-ion batteries and can be generalized as "LiA", where A represents any anion species. These salts can be added in any suitable amount (e.g., 25% to 50% by weight) to obtain optimal characteristics for battery performance.

[0050] Additives can be used to further improve the ionic conductivity of the polymer, to passivate the active material surface, to enhance safety, or to obtain certain rheological properties required for processing. These additives include, but are not limited to, oligomeric (short chain polymers, generally less than 10 mer units) versions of the polymer, small molecule additives (diethyl carbonate, sulfolane, pivalonitrile, ethylene carbonate, phosphazene, triethyl phosphate, etc.), and ceramic powders (fumed silica, nano lithium lanthanum zirconate (LLZO), nano alumina). As described in detail herein, the term polymer electrolyte refers to a mixture of the aforementioned polymer, lithium salt(s), and any additive(s) present.

[0051] The polymer electrolyte thus produced can then be mixed with active materials, conductive additives, and binder materials if necessary or desired. This mixture can then be processed to produce a thin film-like structure that will become an electrode (either positive or negative). Once the film is produced, it may be applied to a metal substrate to act as a current collector.

[0052] In some aspects, an electrochemical battery is disclosed that includes a polymer electrolyte containing a high dielectric polymer as described herein. In some embodiments, the electrochemical battery is a lithium ion battery. The electrochemical battery can include an anode that includes a first electrochemically active material, a cathode that includes a second electrochemically active material, a first electrolyte disposed within either the anode or the cathode, and a second electrolyte interposed between the anode and the cathode. In some such embodiments, at least one of the first electrolyte and the second electrolyte can include a high dielectric polymer as described herein (e.g., a high dielectric polymer having a dielectric constant greater than 10 and a glass transition temperature less than -30°C). In these and other embodiments, the high dielectric polymer can have a dielectric constant greater than 20 and a glass transition temperature less than -70°C. The second electrochemically active material can include lithium ions in some embodiments. In these and other embodiments, the first electrolyte can include a high dielectric polymer. EXAMPLES

[0053] Example 1: Preparation of high dielectric polymer: To a 500 mL round bottom flask, magnetic stir beads were added. Then, 20.0 g (110 mmol) of sorbitol, 3.25 g (10 mmol) of cesium carbonate, and 100.0 g of dimethylformamide (DMF) were added to the flask. The flask was then capped with a silicone septum stopper and placed in an oil bath on a heated stir plate. A temperature probe was connected to the heated stir plate and submerged in the oil. The temperature was set to 100° C. and the stirring was set to 600 rpm. Two stainless steel needles (20 gauge) were used to puncture the septum stopper. One of the needles was connected to a Schlenk line and used to purge the headspace of the round bottom flask with nitrogen gas at a rate of 1 standard cubic foot per hour (SCFH) (0.42 L / min). The second needle acted as a relief to prevent pressure buildup. The mixture of sorbitol, cesium carbonate, and DMF was mixed for 1 hour.

[0054] Meanwhile, in a 50 mL round-bottom flask, add polyethylene glycol diglycidyl ether (M n A flask was filled with 48.3 g (109 mmol based on the epoxide number provided on the Certificate of Analysis (COA)) of 100% sorbitol (=400) and capped with a silicone septum stopper. The silicone septum stopper was punctured with two needles. One needle was used for pressure equalization of the flask, and the other needle was used to insert a capillary tube into the bottom of the flask, which was then connected to a 1 / 16 inch (1.59 mm) inner diameter, 1 / 8 inch (3.18 mm) outer diameter peristaltic pump tubing, which was then connected to an Ismatec® Reglo compact cassette pump. The other end of the tubing was connected via needle to the flask containing the sorbitol, cesium carbonate, DMF mixture. The peristaltic pump was then set to 2 rpm and run overnight or for 14-24 hours. All needles and tubing were then removed, and the flask containing the polydonor in DMF was removed from the heat. The silicone stopper was removed from the flask, and a PTFE sleeve was inserted. The flask was then attached to a rotary evaporator equipped with a bump trap and all of the DMF was removed from the mixture.

[0055] The product was a mixture of polydonor and cesium carbonate. This mixture was then dissolved in 10.0 g of methanol and 60.0 g of tetrahydrofuran and connected to a peristaltic pump in the same manner as described for polyethylene glycol diglycidyl ether. A second 500 mL flask was added with magnetic stirring beads along with 200 g of acrylonitrile and then capped with a silicone septum stopper. The flask containing acrylonitrile was then placed in a 35° C. oil bath. The polydonor, cesium carbonate, dissolved in MeOH / THF, was then added via the peristaltic pump at 15 rpm. Once complete, the reaction was allowed to continue overnight.

[0056] Upon completion, the precipitated cesium carbonate was filtered off and the mixture was neutralized using 1M HCl. The residual solvent, THF, and acrylonitrile were removed by rotary evaporation using the same method used previously. After all the solvent was removed, the CsCl salt was observed to precipitate. The high dielectric polymer was then dissolved in excess acetone and centrifuged to remove the CsCl. The acetone was then removed by rotary evaporation.

[0057] The resulting high dielectric polymer was transferred to a drying chamber, dissolved in acetonitrile to about 50% by weight, and a few grams of MgSO4 was added and mixed to act as a drying agent. The mixture was centrifuged to separate the MgSO4 from the solution. The polymer-acetonitrile solution was decanted from the MgSO4. The sample was dried to remove the acetonitrile and the structure was confirmed using FTIR and 100% FTIR was measured using a Keysight E4980AL precision LCR meter. 2 ~10 6 The dielectric constant was measured in the range of 1000 to 2000 Hz. At 1 MHz, the dielectric constant was 33.22. Differential scanning calorimetry was used to determine the glass transition temperature, which was found to be about -50°C. Figure 9A shows the chemical structure of the high dielectric polymer obtained in this example, and Figure 9B shows the differential scanning calorimetry (DSC) curve of the high dielectric polymer. Figure 9C shows the FTIR spectrum of the high dielectric polymer, which shows that there is substantially no residual alcohol in the structure (3000-3500 cm -1the absence of a peak between 2250 cm -1 ), and a strong ether peak (1100 cm -1 ) is shown.

[0058] Example 2: Preparation of polymer electrolyte: A polymer electrolyte was prepared using the high dielectric polymer produced in Example 1. All solvent was removed from the high dielectric polymer using a rotary evaporation unit prior to use. The electrolyte was prepared using a FlackTek Speedmixer™ equipped with a Max40 cup. 10.0 g of the high dielectric polymer from Example 1 was added to a plastic cup, followed by 2.50 g of LiTFSI salt. The cup was covered and mixed at 800 rpm for 15 seconds, 1400 rpm for 15 seconds, 2000 rpm for 1 minute, and 2600 rpm for 1 minute. After mixing, the solution was checked for clarity. If there was any sign of undissolved salt, the cup was placed in a 60° C. oven for 5 minutes, returned to the Speedmixer™, and mixed again using the mixing profile described above. This process was repeated until all the lithium salt was dissolved. The product was 12.5 g of a highly viscous, transparent polymer electrolyte containing 20 wt % LiTFSI salt. The conductivity of the produced electrolyte was measured to be about 0.4 mS / cm at 25°C.

[0059] Example 3: Preparation of polymer electrolyte: All solvent was removed from the high dielectric polymer prior to use. The electrolyte was prepared using a FlackTek Speedmixer™ equipped with a Max40 cup. 5.0 g of the high dielectric polymer of Example 1 was added to the plastic cup, followed by 9.286 g of LiFSI salt. The cup was covered and mixed at 800 rpm for 15 seconds, 1400 rpm for 15 seconds, 2000 rpm for 1 minute, and 2600 rpm for 1 minute. After mixing, the solution was checked for clarity. If there was any sign of undissolved salt, the cup was placed in a 50°C vacuum oven for 5 minutes while vacuum was applied to degas the solution, and then placed back in the Speedmixer™ and mixed again using the mixing profile described above. This process was repeated until all the lithium salt was dissolved. The product was 14.286 g of glassy, ​​ultra-high viscosity, transparent polymer electrolyte containing 65 wt% LiFSI salt. To obtain the proper rheology for further processing into a positive electrode, 1.587 g of diethyl carbonate (DEC) was added to the mixing cup and the above mixing steps were repeated. The product was 15.873 g of highly viscous polymer in salt electrolyte.

[0060] Example 4: Preparation of high dielectric polymer: To a 250 mL round bottom flask, magnetic stirring beads were added. Then, 20.0 g (110 mmol) of sorbitol, 1.4 g (10 mmol) of potassium hydroxide (40 wt % in water), and 20.0 g of deionized water were added to the flask. The flask was then capped with a silicone septum stopper. The flask was placed in an oil bath on a heated stir plate. A temperature probe was connected to the heated stir plate and submerged in the oil. The temperature was set to 60° C. and the stirring was set to 600 rpm. Two stainless steel needles (20 gauge) were used to puncture the septum stopper. One of the needles was connected to a Schlenk line and used to purge the headspace of the round bottom flask with nitrogen gas at a rate of 1 SCFH (0.42 L / min). The second needle acted as a relief to prevent pressure buildup. The sorbitol, potassium hydroxide solution was mixed for 1 hour. Meanwhile, in a 50 mL round-bottom flask, add polyethylene glycol diglycidyl ether (M nA flask was filled with 48.3 g (109 mmol based on the epoxide number provided on the Certificate of Analysis (COA)) of 100% sorbitol (E = 400) and capped with a silicone septum stopper. The silicone septum stopper was punctured with two needles. One needle was used for pressure equalization of the flask. The other needle was used to insert a capillary tube into the bottom of the flask, which was then connected to a 1 / 16 inch (1.59 mm) inner diameter, 1 / 8 inch (3.18 mm) outer diameter peristaltic pump tubing, which was then connected to an Ismatec® Reglo compact cassette pump. The other end of the tubing was connected to the flask containing the sorbitol solution via a needle. The peristaltic pump was then set to 2 rpm and run overnight or for 14-24 hours. All needles and tubing were then removed and the flask containing the polydonor in deionized water was removed from the heat and allowed to come to room temperature.

[0061] To a second 500 mL flask, magnetic stirring beads were added along with 200 g of acrylonitrile, then capped with a silicone septum stopper. The flask containing acrylonitrile was then placed in a 35° C. oil bath. Polydonor, aqueous potassium hydroxide was then added via a peristaltic pump at 10 rpm. Once complete, the reaction was allowed to continue overnight. Once complete, the mixture was neutralized using 1M HCl. Residual acrylonitrile and water were removed by rotary evaporation in the same manner as in Example 1. After all the solvent was removed, the KCl salt was observed to precipitate. The high dielectric polymer was then dissolved in excess acetone and centrifuged to remove the KCl. The acetone was then removed by rotary evaporation. Finally, the high dielectric polymer was transferred to a drying chamber and dissolved in acetonitrile to approximately 50% by weight, with enough anhydrous MgSO4 added to remove any remaining moisture (if MgSO4 was used as a drying agent, it was added until it began to disperse evenly throughout the solution without clumping). The mixture was centrifuged and decanted through a grade 4 Whatman™ filter paper to separate the MgSO4 from the solution. The high dielectric polymer was left dissolved in acetonitrile for further processing.

[0062] Example 5: Preparation of polydonors: To a 250 mL round bottom flask, magnetic stir beads were added along with 20.0 g sorbitol (110 mmol), 20.0 g deionized water, and 19.0 g epichlorohydrin (205 mmol). The flask was capped with a silicone septum and placed in an oil bath with the temperature set to 60° C. It was purged with inert gas as described in Example 1. To a 40 mL septum vial, 28 g of potassium hydroxide solution (45 wt%) (225 mmol) was added. The potassium hydroxide was added at a rate of 5 rpm following the same settings of the peristaltic pump described in Example 1. Once all of the potassium hydroxide was added, the solution was mixed overnight. After completion of the reaction, the solution was neutralized with 1 M HCl and the solution was cooled to room temperature. The solution was then transferred to dialysis tubing with a 1 kDa cutoff and placed in a 1 gallon (3.8 liter) plastic jar filled with deionized water and a stir bar. The jar was placed on a stir plate and mixed for 2 days, changing the deionized water twice a day. After dialysis, the polymer solution was collected and excess water was removed by rotary evaporation. The final product was 21 g of viscous, clear polydonor. Figure 10 shows the chemical reaction scheme for making the polydonor of this example.

[0063] Example 6: Preparation of hyperbranched polyglycerol as polydonor: For the generation of hyperbranched polyglycerol as polydonor, lithium methoxide solution in methanol (2.2 M) was transferred to a single-neck round-bottom flask. The round-bottom flask was then attached to a rotary evaporation unit at 80 °C to remove the methanol. After removing the methanol, n-butanol (starting monomer) was added to the flask and heated to 80 °C under nitrogen gas. The molar ratio of butanol to lithium methoxide was 10:1.

[0064] The flask was then connected to a nitrogen gas line and a bubbler outlet. The mixture was maintained at 80° C. to allow time for the methanol produced from the reaction between butanol and methoxide anion to exit through the bubbler. 25 g of glycidol was then pumped into the round-bottom flask at 0.2 mL / min using a syringe pump, also under nitrogen gas. The reaction was allowed to proceed for 16 hours under a nitrogen blanket before being quenched by the addition of 1 mL of deionized water.

[0065] Next, 20-50 mL of methanol was added to dilute the viscous polymer, followed by precipitation in 200 mL of acetone. The polymer was recovered by centrifugation and then washed with another 200 mL of acetone. The washed polymer was transferred to a 40 mL vial and attached to a rotary evaporation unit with the oil bath temperature set at 80 °C, vacuum pulled and run overnight. Finally, the solvent-free viscous polymer was analyzed by nuclear magnetic resonance (NMR) to determine the molecular weight (MW) and degree of branching (DB).

[0066] Example 7: Preparation of polydonors: To a 500 mL round bottom flask, magnetic stirring beads were added. Next, 10.0 g (83 mmol) of tris(hydroxymethyl)aminomethane (tris) and 100.0 g of dimethylformamide (DMF) were added to the flask. Since tris contains a primary amine, it was not necessary to add cesium carbonate or other base catalyst to drive the reaction since the amine acts as a base. The flask was then capped with a silicone septum stopper. The flask was placed in an oil bath on a heated stir plate. A temperature probe was connected to the heated stir plate and submerged in the oil. The temperature was set to 100° C. and stirring was set to 600 rpm. Two stainless steel needles (20 gauge) were used to puncture the septum stopper. One of the needles was connected to a Schlenk line and used to purge the headspace of the round bottom flask with nitrogen gas at a rate of 1 SCFH (0.42 L / min). The second needle acted as a relief to prevent pressure buildup. The Tris-DMF mixture was mixed for 1 hour.

[0067] Meanwhile, 36.6 g (82 mmol based on the number of epoxides provided in the COA) of polyethylene glycol diglycidyl ether (Mn=400) was added to a 60 mL metered addition funnel. The stopper attached to the flask containing the Tris-DMF solution was then removed, the addition funnel was connected, and the stopper was reconnected to the top of the addition funnel to continue purging with inert gas. The addition funnel was purged with inert gas for 15 minutes, then the metered stopcock was opened and the needle valve was adjusted until one drop of crosslinker was added every 6-10 seconds. The addition funnel was left open overnight and the polyethylene glycol diglycidyl ether was added dropwise over several hours. After approximately 20 hours, the heating and stirring were stopped. The silicone stopper and addition funnel were removed from the flask and a PTFE sleeve was inserted. The flask was then connected to a rotary evaporator equipped with a bump trap and all of the DMF was removed from the mixture. The product was a light brown viscous liquid. Figure 11 shows the chemical reaction scheme for producing the polydonor of this example (where "n" represents the number of repeat units in the PEG-diglycidyl ether crosslinker).

[0068] Example 8: Preparation of positive electrode by solvent-based method: The electrode slurry was made using a FlackTek Speedmixer™ equipped with a Max20 cup. 1.57 g of N-methyl-2-pyrrolidone (NMP) and 0.63 g of solvent-free high dielectric polymer electrolyte containing 25 wt % lithium salt, such as lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), were added to the plastic cup to act as an ionically conductive catholyte. The cup was then capped and mixed at 800 rpm for 15 seconds, 1200 rpm for 15 seconds, 1600 rpm for 15 seconds, 2000 rpm for 30 seconds, and 2750 rpm for 2 minutes. 0.50 g of an electronically conductive carbon additive, such as LITX™ 200 (Cabot), was then added and mixed three times at 800 rpm for 15 seconds, 1200 rpm for 15 seconds, 1600 rpm for 15 seconds, 2200 rpm for 30 seconds, and 2750 rpm for 3 minutes. Then, 8.98 g of lithium-containing cathode active material such as Lithium Nickel Cobalt Manganese Oxide (NCM811, POSCO N83MA11, D50 11.8 μm), 1.57 g of NMP, and 0.02 g of premixed binder solution consisting of 20 wt % polyvinylidene fluoride (PVDF, Arkema Kynar® HSV1810) were added to the cup and then mixed twice at 800 rpm for 15 seconds, 1000 rpm for 15 seconds, 1400 rpm for 15 seconds, 1800 rpm for 30 seconds, and 2000 rpm for 5 minutes. Finally, 0.95 g of NMP was added and then mixed at 800 rpm for 15 seconds, 1000 rpm for 15 seconds, 1400 rpm for 15 seconds, 1800 rpm for 30 seconds, and 2000 rpm for 5 minutes. The resulting slurry was then cast onto a carbon-coated aluminum foil (BlueNano, 17 μm) at the target loading using an adjustable doctor blade with a gap height setting of 60 μm. The coated foil was then dried in a forced convection oven (Yamato DNK402) at 100° C. for 16 hours to remove the NMP, resulting in a dry composite electrode with a composition of 89.8 wt % NCM811, 5 wt % LITX™ 200 carbon black, 5 wt % dielectric polymer electrolyte, and 0.3 wt % HSV1810 PVDF.The dried composite electrode was then densified using a heated calendar roll (TOB-JS-250L) at 55° C. to reduce the porosity of the electrode. The resulting electrode had a thickness of 20 μm and a mass of approximately 1.15 mAh / cm, assuming full utilization of NCM811 (208 mAh / g). 2 The cathode had an areal loading of about 1000 μm. The completed electrode sheet was then punched to precise dimensions and then aluminum tabs pre-applied with hot melt adhesive were ultrasonically welded (Branson MWX100) onto the punched electrode tab areas to create the complete cathode assembly. FIG. 12 shows a cross-sectional micrograph image of a composite cathode electrode (NCM811) with high dielectric polymer electrolyte as described in Example 8. The electrode coating thickness was about 17 μm.

[0069] Small factor pouch cells (2.526 cm) consisted of a lithium anode (Honjo, 20 μm Li on 8 μm Cu), a ceramic filled separator (Entek, CF9), and a bulk electrolyte composed of a solvent-free high dielectric polymer electrolyte containing 60 wt% lithium bis(fluorosulfonyl)imide (LiFSI) and 10 wt% diethyl carbonate (DEC) as an additive. 2 Electrochemical testing of the composite cathode containing catholyte was performed using a 0.05C constant current (CC) C rate to 4.3 V. A polymer electrolyte was applied to the CF9 separator as the cell was constructed to ensure complete wetting of the separator layer. The assembled stack was vacuum sealed at 100 kpa, clamped in a pressure fixture at 3 bar (300 kPa) and left at 45° C. for 6 hours before cycling. FIG. 13 shows an exemplary cycling behavior of a cathode half cell using an NCM811 composite cathode electrode as described in Example 8. Cycling was performed between 3 and 4.3 V, using a constant current (CC) C rate of 0.05 C to 4.3 V and held at constant voltage (CV) until the current dropped below 0.025 C. Constant current discharge was performed at 0.05 C rate to 3 V. Cycling was performed at 45° C.

[0070] Example 9: Preparation of positive electrode by solvent-free method: The electrode paste was made using a Resodyn Lab RAM I™ with a Max10 cup. In a plastic cup, 0.29 g of lithium salt such as lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), 0.20 g of conductive carbon additive such as LITX™ 200 (Cabot), 17.15 g of lithium-containing cathode active material such as lithium nickel cobalt manganese oxide (NCM811, POSCO N83MA11, D50 11.8 μm), 1.59 g of high dielectric polymer, and 0.78 g of additive such as triethyl phosphate (TEP) were mixed using a LabRAM I™ acoustic mixer system. The acceleration force was ramped from 30 g to 70 g to ensure that the power level remained low and stable during mixing. The mixing time was about 12 minutes and was done in such a way as to ensure that the container temperature reached and stabilized at about 70° C. The resulting electrode paste was then applied to a suitable current collector, such as carbon-coated aluminum foil (BlueNano, 17 μm), followed by lamination with a Kapton® film (polyimide film) to act as a release liner. A heated calendar roll (TOB-JS-250L) was used to calendar the laminate at 70° C. to flatten the applied paste and create an electrode with uniform thickness and low porosity. The thickness reduction was reduced in steps such that the gap was set to be approximately 10% smaller than the measured thickness and was calendared several times before decreasing the gap setting. This process was repeated several times until the target thickness and areal loading were achieved. To remove the release liner, the sample was cooled to <−40° C. in an environmental chamber (Test Equity, Model 115A-F) and the Kapton® release liner was pulled 180° in the opposite direction so that it was parallel to the surface to help ensure a clean release. These electrodes were then punched to the correct dimensions and then aluminum tabs with pre-applied hot melt adhesive were ultrasonically welded (Branson MWX100) onto the punched electrode tab areas to create the complete cathode assembly.

[0071] Comparative Test: The dielectric constant as a function of frequency was measured for two different high dielectric polymers. Figure 14 shows test data for the high dielectric polymer of Example 1 (dielectric constant of about 33 at 1 MHz) and for a high dielectric polymer produced from a polydonor described in Example 7 (acrylonitrile was used as the Michael acceptor and the measured dielectric constant was about 26 at 1 MHz).

[0072] The ionic conductivity of the polymer electrolyte made from the polymer described in Example 1 was measured as a function of salt concentration for two different salts. The results are shown in Figure 15. The error bars represent the standard deviation of the three different conductivity cells. The peak conductivity is seen at about 0.5 mS / cm for 40 wt% LiTFSI.

[0073] The electrical conductivity of the high dielectric polymer described in Example 1 was measured when made into a polymer electrolyte containing 40 wt % LiTFSI, and the measurements obtained are shown in FIG. Although the present technology has been described with respect to certain specific embodiments, those skilled in the art will readily appreciate that various changes and / or modifications may be made thereto by those skilled in the art without departing from the inventive nature of the present disclosure.Furthermore, it should be understood that the concepts of the present disclosure are intended to be encompassed by the following claims, unless those claims are otherwise expressly set forth in their language.

Claims

1. 1. A method for producing a high dielectric polymer, the method comprising: reacting a starting material containing at least three nucleophilic sites with a crosslinker to produce a polydonor, said polydonor being a branched polymer containing multiple reactive nucleophilic sites; functionalizing the plurality of reactive nucleophilic sites of the polydonor to produce a high dielectric polymer; purifying the high dielectric polymer; A method comprising:

2. 2. The method of claim 1, wherein the starting material is selected from the group consisting of polyalcohols (polyols), sorbitol, pentaerythritol, inositol, pentaerythritol, dipentaerythritol, amino alcohols, tris(hydroxymethyl)aminomethane, 2-amino-2-methyl-1-propanol, 2-amino-2-methyl-1,3-propanediol, cysteine, dithiothreitol, other thiols, and / or polyethyleneimine.

3. The method of claim 1 , wherein the starting material is a Michael donor.

4. The plurality of nucleophilic sites are -OH, -NH 2 4. The method of claim 1, wherein the aryl group comprises -CH 2 , -CH 3 , and / or -SH groups.

5. The method of claim 1 , wherein the crosslinking agent is a bifunctional crosslinking agent.

6. 10. The method of claim 1, wherein the crosslinking agent is a diglycidyl ether, a dichloride, a dibromide, a diisocyanate, an epichlorohydrin, a diacrylate, a divinyl, and / or a dialdehyde.

7. The method of claim 6, wherein the cross-linking agent is selected from the group consisting of divinyl sulfone, glycerol diglycidyl ether, PEG-diglycidyl ether, and epichlorohydrin.

8. The method of claim 1 , further comprising purifying the polydonor.

9. The method of claim 1 , wherein functionalizing the plurality of reactive nucleophilic sites is accomplished by nucleophilic addition.

10. 10. The method of claim 1, wherein functionalizing the multiple reactive nucleophilic sites is accomplished by Michael addition.

11. The method of claim 1 further comprising combining the high dielectric polymer with an electrochemically active material to form a polymer electrolyte.

12. 12. The method of claim 11, further comprising incorporating the polymer electrolyte into a lithium ion battery as an anolyte or catholyte.

13. 1. An electrochemical cell comprising: an anode comprising a first electrochemically active material; a cathode comprising a second electrochemically active material; and a first electrolyte disposed within either the anode or the cathode; a second electrolyte interposed between the anode and the cathode; Including, An electrochemical cell, wherein at least one of the first electrolyte and the second electrolyte comprises a high dielectric polymer having a dielectric constant greater than 10 and a glass transition temperature less than -30°C.

14. 14. The electrochemical cell of claim 13, wherein said high dielectric polymer has a dielectric constant greater than 20 and said glass transition temperature less than -70°C.

15. 14. The electrochemical cell of claim 13, wherein the second electrochemically active material comprises lithium ions.

16. 16. The electrochemical cell of claim 15, wherein the first electrolyte comprises the high dielectric polymer.

17. A high dielectric polymer comprising a branched and functionalized polymer backbone, said high dielectric polymer having a dielectric constant greater than 10 and a glass transition temperature less than -30°C.

18. 20. The high dielectric polymer of claim 17, wherein said high dielectric polymer is produced by functionalizing multiple nucleophilic sites on a polydonor.

19. 20. An electrochemical cell comprising a polymer electrolyte containing the high dielectric polymer of claim 17.

20. 20. The electrochemical cell of claim 19, wherein the electrochemical cell is a lithium ion battery.

Citation Information

Patent Citations

  • Aqueous polyepoxide resin composition

    JP1995048434A

  • Polymeric solid electrolytic lithium ion secondary battery

    JP2001176555A

  • Polymeric compound, polymer for polyelectrolyte, and composition for ionically conductive polyelectrolyte

    WO2000035991A1