Lithium secondary battery
A lithium cobalt-based oxide with a core-shell structure and a specific non-aqueous electrolyte composition stabilizes the electrode surface, addressing structural instability and elution issues, thereby enhancing battery performance at high voltages.
Patent Information
- Application Number
- JP2024520757
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-04
- Filing Date
- 2022-11-07
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2042-11-07
AI Technical Summary
Lithium cobalt-based oxide positive electrodes in lithium secondary batteries suffer from structural instability and rapid gas and cobalt elution at high voltages, limiting their use in high-capacity applications.
A lithium cobalt-based oxide with a core-shell structure containing doping elements like Al, Zr, and Ti, combined with a non-aqueous electrolyte containing lithium difluorophosphate and a dinitrile compound, forms a stable film on the electrode surface, enhancing structural stability and preventing side reactions.
The solution improves high-temperature durability and cycle characteristics of lithium secondary batteries, minimizing interfacial resistance and suppressing gas and cobalt elution, especially at high voltages.
Smart Images

Figure 2024537150000001 
Figure 2024537150000002 
Figure 2024537150000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0152273 filed on November 8, 2021 and Korean Patent Application No. 10-2022-0146338 filed on November 4, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated as part of this specification.
[0002] The present invention relates to a lithium secondary battery having improved high-temperature durability and cycle characteristics under high voltage conditions. [Background technology]
[0003] Recently, with the development of the information society, personal IT devices and networks have developed, and as a result, society as a whole has become more dependent on electrical energy, which has created a demand for technological development to efficiently store and utilize electrical energy.
[0004] In particular, with growing interest in solving environmental problems and realizing a sustainable recycling-based society, extensive research is being conducted on lithium-ion batteries, which are in the spotlight as a clean energy source with low carbon dioxide emissions.
[0005] Lithium-ion batteries can be miniaturized to a level suitable for use in personal IT devices, and because they have a high energy density and operating voltage, they are used not only as power sources for laptop computers and mobile phones, but also for power storage and electric vehicles.
[0006] Meanwhile, one of the positive electrode active materials for lithium secondary batteries that are currently being actively researched, developed, and used is a lithium-cobalt-based positive electrode active material with a layered structure, such as LiCoO2. LiCoO2 is the most widely used because it is easy to synthesize and has excellent electrochemical performance, including life characteristics, but it has low structural stability and is limited in its application to high-capacity battery technology.
[0007] Furthermore, as there is a demand for high-capacity batteries, active materials with high energy per unit volume of the battery are required. To meet this requirement, the packing density of the active material must be high, and to increase the packing density, an active material with a large particle size is advantageous. However, in the case of large-particle-size lithium cobalt-based oxide particles, the surface area is relatively low, so the active area in contact with the electrolyte is narrow, and the lithium migration rate is slow due to the two-dimensional layer structure, so there are problems with the rate characteristics and initial capacity being low.
[0008] Therefore, a technique has been proposed in which a dopant having high reactivity with lithium is added during the production of lithium-cobalt-based oxide so that the dopant reacts with the lithium on the surface, thereby forming lithium defects on the surface of the lithium-cobalt-based oxide.
[0009] However, the lithium-cobalt-based positive electrode active material having the lithium defects does not cause any problems when applied to batteries operated at a voltage of less than 4.45 V. However, when applied to batteries operated at a voltage of 4.45 V or more, gas and cobalt elution occurs rapidly due to a side reaction with the electrolyte, and as a result, the life characteristics and high-temperature storage properties are significantly reduced, making it impossible to apply the material to batteries operated at 4.45 V or more.
[0010] Therefore, there is a demand for the development of a lithium secondary battery that can suppress gas and cobalt elution and improve cycle characteristics even when driven at 4.45 V or higher. Summary of the Invention [Problem to be solved by the invention]
[0011] In order to solve the above-mentioned problems, an object of the present invention is to provide a lithium secondary battery capable of realizing excellent high-temperature durability and cycle characteristics by using a positive electrode containing a lithium cobalt-based oxide containing a doping element in a specific concentration range as a positive electrode active material in combination with a nonaqueous electrolyte solution containing an additive capable of forming a highly durable coating on the surface of the electrode. [Means for solving the problem]
[0012] According to one embodiment, the present invention comprises: a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; a separator interposed between the positive electrode and the negative electrode; and a non-aqueous electrolyte for a lithium secondary battery, The positive electrode active material includes a core including a lithium cobalt-based oxide represented by the following formula 1, and a shell including a lithium cobalt-based oxide represented by the following formula 2 disposed on a surface of the core, the core and the shell including at least one doping element selected from the group consisting of Al, Zr, Mg, and Ti, The non-aqueous electrolyte provides a lithium secondary battery, comprising a lithium salt, an organic solvent, lithium difluorophosphate, and a dinitrile compound represented by the following Chemical Formula 3: [Chemical formula 1] Li a Co 1-b M b O2 (In the above Chemical Formula 1, M is at least one selected from the group consisting of Al, Zr, Mg and Ti; 1≦a≦1.2, 0.005≦b≦0.05.) [Chemical formula 2] Li x Co 1-y M y O2 (In the above Chemical Formula 2, M 1 is at least one selected from the group consisting of Al, Zr, Mg and Ti; 0.5≦x<1, 0≦y≦0.002.)
[0013] [ka]
[0014] (In the above Chemical Formula 3, R1, R2, R3, and R4 each independently represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or -R-CN, wherein R represents an alkylene group having 1 to 12 carbon atoms; At least one of R1 and R2 is -R-CN; At least one of R3 and R4 is -R-CN.
[0015] The doping element may be present in a concentration gradient that decreases from the center of the core towards the core-shell interface.
[0016] The doping element includes zirconium (Zr) and may optionally further include at least one selected from the group consisting of aluminum (Al), magnesium (Mg) and titanium (Ti).
[0017] Specifically, zirconium (Zr) among the doping elements may be included in an amount of 0.025 wt % to 0.085 wt % based on the total weight of the positive electrode active material.
[0018] In addition, the doping elements, aluminum (Al), may be included in an amount of 0.5 wt % to 0.55 wt % based on the total weight of the positive electrode active material, the doping elements, magnesium (Mg), may be included in an amount of 0.1 wt % to 0.15 wt % based on the total weight of the positive electrode active material, and the doping elements, titanium (Ti), may be included in an amount of 0.01 wt % to 0.05 wt % based on the total weight of the positive electrode active material.
[0019] Meanwhile, the lithium difluorophosphate may be included in an amount of 0.1 wt % to 1.5 wt % based on the total weight of the non-aqueous electrolyte for lithium secondary batteries.
[0020] Meanwhile, the lithium difluorophosphate and the dinitrile-based compound may be included in a weight ratio of 1:0.25 to 1:3. Effect of the Invention
[0021] The lithium secondary battery of the present invention uses a positive electrode containing a lithium cobalt-based oxide containing a doping element in a specific concentration range as a positive electrode active material in combination with a nonaqueous electrolyte containing a dinitrile-based compound and lithium difluorophosphate as additives, thereby ensuring the structural stability of the positive electrode active material and forming a highly durable coating on the surface of the positive electrode, thereby minimizing an increase in interface resistance and preventing side reactions between the positive electrode and the electrolyte, thereby maximizing the effects of improving high-temperature storage characteristics, high-temperature durability, and cycle characteristics.
[0022] Such a lithium secondary battery of the present invention can be effectively used in particular in automobile batteries and the like which require high driving voltage and high output characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings, in order to enable those skilled in the art to easily carry out the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.
[0024] As a result of extensive research into developing a lithium secondary battery with improved high-temperature storage characteristics and cycle characteristics, the inventors have discovered that the performance characteristics of a secondary battery can be improved by using, as a positive electrode active material, a lithium cobalt-based oxide containing a doping element in a specific concentration range, in combination with a nonaqueous electrolyte solution containing an additive of a specific composition, and have thus completed the present invention.
[0025] The lithium secondary battery of the present invention according to one embodiment comprises: a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; a separator interposed between the positive electrode and the negative electrode; and a non-aqueous electrolyte for a lithium secondary battery, The positive electrode active material includes a core including a lithium cobalt-based oxide represented by the following formula 1, and a shell including a lithium cobalt-based oxide represented by the following formula 2 disposed on a surface of the core, the core and the shell including at least one doping element selected from the group consisting of Al, Zr, Mg, and Ti, The non-aqueous electrolyte provides a lithium secondary battery, comprising a lithium salt, an organic solvent, lithium difluorophosphate, and a dinitrile compound represented by the following Chemical Formula 3: [Chemical formula 1] Li a Co 1-b M b O2 In the above Chemical Formula 1, M is at least one selected from the group consisting of Al, Zr, Mg and Ti; 1≦a≦1.2, 0.005≦b≦0.05. [Chemical formula 2] Li x Co 1-y M y O2 In the above Chemical Formula 2, M 1 is at least one selected from the group consisting of Al, Zr, Mg and Ti; 0.5≦x<1, 0≦y≦0.002.
[0026] [ka]
[0027] In the above Chemical Formula 3, R1, R2, R3, and R4 each independently represent a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or -R-CN, wherein R represents an alkylene group having 1 to 12 carbon atoms; At least one of R1 and R2 is -R-CN; At least one of R3 and R4 is -R-CN.
[0028] The configuration of the lithium secondary battery of the present invention will be specifically described below.
[0029] (1) Positive electrode The positive electrode of the present invention may include a positive electrode active material layer containing a positive electrode active material, and if necessary, the positive electrode active material layer may further include a conductive material and / or a binder.
[0030] The positive electrode active material has a core-shell structure in which a core is located at the center of a particle and a shell is disposed on an outer surface of the core, and the core and the shell may be classified according to the concentration of a doping element.
[0031] Specifically, the positive electrode active material includes a core including a lithium cobalt-based oxide represented by the following formula 1, and a shell including a lithium cobalt-based oxide represented by the following formula 2 disposed on the surface of the core, and the core and the shell may include at least one doping element selected from the group consisting of Al, Zr, Mg, and Ti.
[0032] [Chemical formula 1] Li a Co 1-b M b O2
[0033] In the above Chemical Formula 1, M is at least one selected from the group consisting of Al, Zr, Mg and Ti; 1≦a≦1.2, 0.005≦b≦0.05.
[0034] [Chemical formula 2] Li xCo 1-y M y O2
[0035] In the above Chemical Formula 2, M 1 is at least one selected from the group consisting of Al, Zr, Mg and Ti; 0.5≦x<1, 0≦y≦0.002.
[0036] Meanwhile, in Formula 1, a represents the lithium atomic ratio in the lithium cobalt-based oxide of Formula 1, and may be 1≦a≦1.2, preferably 1≦a≦1.1.
[0037] In addition, in the formula 1, the b represents the atomic ratio of the doping element M in the lithium cobalt-based oxide of the formula 1, and may be 0.001≦b≦0.05, preferably 0.01≦b≦0.02. When the atomic ratio of the doping element in the lithium cobalt-based oxide forming the core portion satisfies the above range, the structural stability of the positive electrode active material is improved, no phase transition to a monoclinic system occurs during charging and discharging, and gas generation and cobalt elution can be reduced even when driven at a high voltage of 4.45V or more.
[0038] In addition, in Formula 2, x represents the lithium atomic ratio in the lithium cobalt-based oxide of Formula 2, and may be 0.5≦x<1, preferably 0.55≦x<1, and more preferably 0.9≦x≦0.99. When the lithium atomic ratio in the lithium cobalt-based oxide of the shell portion satisfies the above range, the lithium cobalt-based oxide of the shell portion has a three-dimensional crystal structure such as a spinel-like structure, and thus the migration speed of lithium ions in the shell portion is increased, improving the output characteristics and rate characteristics.
[0039] In addition, in Formula 2, y represents the atomic ratio of the doping element in the lithium cobalt-based oxide of Formula 2, and may be 0≦y≦0.002, preferably 0.0005≦y≦0.0017. It is preferable that the lithium cobalt-based oxide forming the shell contains a small amount or a very small amount of the doping element compared to the lithium cobalt-based oxide forming the core.
[0040] Specifically, the concentration of cobalt contained in the positive electrode active material may increase with a continuous concentration gradient from the center of the active material particle to the surface of the particle, or may be constant from the center to the surface of the positive electrode active material particle. In this way, when the active material particle contains a concentration gradient in which the cobalt concentration is high at the center of the particle and increases toward the surface, a decrease in capacity can be prevented.
[0041] In the present invention, "having a concentration gradient" means that the concentration of a metal or the like exists in a concentration distribution that gradually changes in one direction throughout the entire particle.
[0042] In addition, the positive electrode active material of the present invention can have a concentration gradient in which the concentration of the doping element decreases from the center of the core toward the interface between the core and the shell by introducing a doping element having a high bonding strength with oxygen, thereby rapidly forming particles from the center of the core.
[0043] Specifically, the positive electrode active material may include a doping element in a core located at the center of a particle, and a small or trace amount of the doping element may be included in a shell.
[0044] The doping element may include zirconium (Zr) and may further include at least one selected from the group consisting of aluminum (Al), magnesium (Mg) and titanium (Ti).The doping element may include zirconium (Zr) and aluminum (Al) and may further include at least one selected from the group consisting of magnesium (Mg) and titanium (Ti).
[0045] Specifically, zirconium (Zr) among the doping elements is substituted for Li ion sites in a layered structure and is located at vacant sites from which Li ions are released during discharge. This reduces stress accompanying expansion and contraction of the positive electrode active material, thereby increasing the stability of the active material. That is, the c-axis lattice constant increases, thereby improving the efficiency and life characteristics of the battery. Here, the weight ratio of zirconium (Zr) to the total weight of the positive electrode active material may be 0.025 wt% to 0.085 wt%, specifically 0.03 wt% to 0.08 wt%, and more preferably 0.03 wt% to 0.06 wt%. When the content of Zr in the positive electrode active material satisfies the above range, the cycle performance is further improved and the decrease in discharge capacity can be prevented.
[0046] In addition, aluminum (Al) among the doping elements is a component capable of suppressing Co elution and improving high temperature durability, and may be included in an amount of 0.5 wt% to 0.55 wt%, specifically, 0.51 wt% to 0.55 wt%, based on the total weight of the positive electrode active material. When the Al content in the positive electrode active material satisfies the above range, cycle performance is further improved and a decrease in discharge capacity can be prevented.
[0047] Among the doping elements, magnesium (Mg) is a component that can stabilize the structure of the positive electrode active material and increase durability at high voltage, and may be included in the positive electrode active material at 0.1 wt % to 0.15 wt %, specifically 0.11 wt % to 0.15 wt %, based on the total weight of the positive electrode active material.
[0048] Among the doping elements, titanium (Ti) is substituted at the Me-O site in the layered structure to increase the crystallinity, thereby increasing the lattice constant of the a-axis, and improving the life characteristics of the battery by increasing and stabilizing the crystallinity of the layered structure. The titanium may be included in an amount of 0.01 wt% to 0.05 wt%, specifically 0.01 wt% to 0.05 wt%, specifically 0.01 wt% to 0.04 wt%, based on the total weight of the positive electrode active material.
[0049] Meanwhile, the positive electrode active material of the present invention contains at least one doping element selected from the group consisting of Al, Zr, Mg, and Ti, which ensures the structural stability of the positive electrode active material and reduces the surface exposure of the positive electrode active material to prevent side reactions, thereby minimizing an increase in the interface resistance of the positive electrode active material and improving the capacity characteristics and high temperature durability of the battery. In particular, when the element concentrations of Al, Zr, Mg, and / or Ti in the positive electrode active material satisfy the above ranges, both the durability increase effect and the surface modification effect of the positive electrode active material can be ensured.
[0050] On the other hand, the positive electrode active material of the present invention has a concentration gradient in which the doping element having a high bond strength with oxygen forms particles in the center and the doping element concentration decreases from the center to the surface, so that the doping element concentration is insufficient on the surface of the positive electrode active material, which may increase side reactions with the electrolyte during operation or cause the structure of the positive electrode active material to collapse. Therefore, in the present invention, as described below, a nonaqueous electrolyte containing an additive capable of forming a stable coating on the surface of the positive electrode is used in combination to prevent side reactions between the positive electrode and the electrolyte, thereby improving high-temperature storage characteristics and cycle characteristics.
[0051] On the other hand, the positive electrode active material of the present invention can be formed by a conventional method.
[0052] Specifically, the method may be carried out by a solid phase method in which a first lithium cobalt-based oxide and a doping source are mixed and a first heat treatment is performed to form a core part including the lithium cobalt-based oxide represented by the formula 1, and then a second lithium cobalt-based oxide and a selective doping source are mixed with the obtained lithium cobalt-based oxide represented by the formula 1 and a second heat treatment is performed to form a shell part. Here, the mixing ratio of the doping source may be appropriately adjusted so that the core and shell-type lithium cobalt-based oxide represented by the formula 1 and / or 2 is formed. Specifically, when forming the core part, the lithium cobalt-based oxide and the doping source may be mixed in an amount such that the atomic ratio of Li / (Co+M) of the core part is 1.0 to 1.2, specifically 1.0 to 1.1. The lithium cobalt-based oxide and the doping source may be added at the same time or may be added separately so that the atomic ratio of Li / (Co+M) decreases with a time lag. In the latter case, it is possible to form a core portion having a concentration gradient in which the lithium concentration decreases from the center of the core portion toward the surface.
[0053] In addition, during the formation of the shell portion, lithium present on the surface of the lithium cobalt-based oxide represented by Chemical Formula 1 reacts with the second lithium cobalt-based oxide and / or the source to form a lithium cobalt-based oxide having an atomic ratio of Li / (Co+M) less than 1. Here, the second lithium cobalt-based oxide may be mixed in an amount such that the atomic ratio of Li / (Co+M) of the shell portion is 0.50 or more and less than 1, preferably 0.55 or more and less than 1, more preferably 0.90 to 0.99. The ratio of the first lithium cobalt-based oxide and the second lithium cobalt-based oxide may be such that the ratio of the first lithium cobalt-based oxide / second lithium cobalt-based oxide is 0.1 or more and less than 4, more preferably 0.5 or more and less than 2. Meanwhile, the second lithium cobalt-based oxide and / or the doping source may be added at the same time, or may be added in portions so that the Li / Co atomic ratio decreases with a time lag. In the latter case, it is possible to form a core portion having a concentration gradient in which the lithium concentration decreases from the center of the shell portion toward the surface.
[0054] Meanwhile, the first and second lithium cobalt-based oxides may be LiCoO2.
[0055] The doping source may be at least one element selected from the group consisting of Al, Zr, Mg, and Ti, or an oxide, hydroxide, oxyhydroxide, halide, nitrate, carbonate, acetate, oxalate, citrate, or sulfate containing the same, or a mixture of two or more of these may be used.
[0056] Specifically, the Al source may be an oxide containing Al, such as Al(NO3)3·9H2O.
[0057] As the Zr source, an oxide containing Zr, for example, Zr(NO3)2·xH2O (x is an integer of 1 to 6), etc. may be used.
[0058] The Mg source may be an oxide containing Mg, such as MgO.
[0059] The Ti source may be an oxide containing Ti, such as TiO2.
[0060] The respective sources may be used in a mixed amount that can realize the concentration range contained in the final coating layer.
[0061] In addition, by adjusting the heat treatment temperature, the mixing speed, and the ratio of the doping elements during the heat treatment, the precursor particles can have a desired doping element concentration from the center to the surface.
[0062] Specifically, the primary and secondary heat treatments are preferably performed at a temperature of 650° C. to 1100° C., specifically 850° C. to 1100° C. If the heat treatment temperature is less than 650° C., there is a risk of a decrease in discharge capacity per unit weight, a decrease in cycle characteristics, and a decrease in operating voltage due to the remaining unreacted doping source, and if it exceeds 1100° C., there is a risk of a decrease in discharge capacity per unit weight, a decrease in cycle characteristics, and a decrease in operating voltage due to the generation of by-products due to high-temperature reactions.
[0063] The heat treatment is preferably carried out in air or an oxygen atmosphere for 5 to 30 hours, which allows the diffusion reaction between the particles of the mixture to proceed sufficiently.
[0064] As another method, the positive electrode active material can be formed by dissolving or dispersing a doping source in a solvent to prepare a doping composition, and then surface-treating a lithium-cobalt-based oxide using the doping composition, drying it, and heat-treating it at a temperature of 200°C to 600°C.
[0065] The surface treatment can be carried out by a method such as coating, spraying, or immersion, or by a deposition method such as chemical vapor deposition.
[0066] The doping sources may be as described above.
[0067] In addition, the solvent may be any solvent that does not affect the lithium cobalt oxide and is generally used in surface treatment using a metal source material. Specifically, N-methylpyrrolidone (NMP), acetone, isopropyl alcohol, etc. may be used.
[0068] As described above, the lithium secondary battery of the present invention includes a core containing a lithium cobalt-based oxide represented by the following chemical formula 1, and a shell containing a lithium cobalt-based oxide represented by the chemical formula 2 arranged on the surface of the core, and the core and shell are provided with a positive electrode containing a positive electrode active material containing at least one doping element selected from the group consisting of Al, Zr, Mg, and Ti, thereby improving the structural stability of the positive electrode active material even when driven under high voltage.
[0069] Meanwhile, in the positive electrode active material according to the present invention, the ratio of the radius of the core part to the thickness of the shell part may be, for example, about 1:0.01 to 1:0.1. If the thickness of the shell part is too thin, the effect of increasing the movement of lithium ions may not be sufficient, and if the thickness of the shell part is too thick, the structural stability of the active material particles may be reduced. More specifically, under the above-mentioned condition of the ratio of the radius of the core part to the thickness of the shell part, the thickness of the shell part may be 1 to 500 nm, or 10 to 450 nm.
[0070] Meanwhile, the positive electrode active material may be, in addition to the lithium cobalt-based oxide represented by Chemical Formula 1 or 2, a lithium manganese-based oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium nickel-based oxide (e.g., LiNiO2, etc.), a lithium nickel-manganese-based oxide (e.g., LiNi1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-z Ni z O4 (where 0 < Z < 2), etc.), or lithium - nickel - cobalt - transition metal (M) oxides (e.g., Li(Ni p2 Co q2 Mn r3 M s2 )O2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r3, and s2 are, as atomic fractions of independent elements, 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1, and p2 + q2 + r3 + s2 = 1)) can be further included, etc.
[0071] The positive electrode active material can be contained in an amount of 90% to 99% by weight, specifically 93% to 98% by weight, based on the total weight of the solid content in the positive electrode active material layer.
[0072] On the other hand, the positive electrode active material layer contained in the positive electrode of the present invention can further contain a conductive material and / or a binder, if necessary.
[0073] The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, carbon powders such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powders such as natural graphite, artificial graphite, or graphite with a highly developed crystal structure; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc. can be used.
[0074] The conductive material is usually added in an amount of 1% to 30% by weight based on the total weight of the solid content in the positive electrode active material layer.
[0075] The binder is a component that plays a role in improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector, and is usually added in an amount of 1% by weight to 30% by weight based on the total weight of the solid content of the positive electrode active material layer. Examples of such binders include fluororesin-based binders including polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene butadiene rubber (SBR), acrylonitrile butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders including polyvinyl alcohol; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; and silane-based binders.
[0076] The positive electrode of the present invention as described above may be manufactured according to a method for manufacturing a positive electrode well known in the art. For example, the positive electrode may be manufactured by a method of dissolving or dispersing a positive electrode active material, a binder, and / or a conductive material in a solvent to prepare a positive electrode slurry, coating the positive electrode current collector with the positive electrode slurry, drying and rolling the positive electrode slurry to form a positive electrode active material layer, or by a method of casting the positive electrode active material layer on a separate support, peeling off the support, and laminating the resulting film on the positive electrode current collector.
[0077] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel whose surface is treated with carbon, nickel, titanium, silver, or the like can be used.
[0078] The solvent may include an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a preferred viscosity when the positive electrode active material and, optionally, a binder and a conductive material are included. For example, the solvent may be included so that the solids concentration in the active material slurry that includes the positive electrode active material and, optionally, a binder and a conductive material, is 10 wt % to 70 wt %, preferably 20 wt % to 60 wt %.
[0079] (2) Negative electrode Next, the negative electrode will be described.
[0080] The negative electrode according to the present invention includes a negative electrode active material layer including a negative electrode active material, and the negative electrode active material layer may further include a conductive material and / or a binder, if necessary.
[0081] The negative electrode active material may include at least one selected from the group consisting of lithium metal, a carbon material capable of reversibly intercalating / deintercalating lithium ions, a metal or an alloy of these metals and lithium, a metal composite oxide, a material capable of doping and dedoping lithium, and a transition metal oxide.
[0082] The carbonaceous material capable of reversibly intercalating / deintercalating lithium ions may be any carbonaceous negative electrode active material commonly used in lithium ion secondary batteries, and representative examples thereof include crystalline carbon, amorphous carbon, or both. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide, and calcined coke.
[0083] As the metal or an alloy of these metals and lithium, a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn, or an alloy of these metals and lithium can be used.
[0084] As the metal composite oxide, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, Li x Fe2O3(0≦x≦1), Li x WO2(0≦x≦1), and Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Group 1, Group 2, Group 3 elements of the periodic table, halogen; 0<x≦1; 1≦y≦3; 1≦z≦8) selected from the group consisting of can be used.
[0085] As the substance capable of doping and undoping lithium, Si, SiO x (0<x<2), Si-Y alloy (wherein Y is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, and a combination thereof, and is not Si), Sn, SnO2, Sn-Y (wherein Y is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, and a combination thereof, and is not Sn), etc. can be mentioned, and at least one of these can also be used in mixture with SiO2. As the element Y, it can be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db (dubnium), Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, and a combination thereof.
[0086] Examples of the transition metal oxide include lithium-containing titanium oxide (LTO), vanadium oxide, and lithium vanadium oxide.
[0087] The negative electrode active material may be contained in an amount of 80% by weight to 99% by weight based on the total weight of the solid content in the negative electrode active material layer.
[0088] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 1% by weight to 20% by weight based on the total weight of the solid content of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of such conductive materials include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0089] The binder is a component that helps to bond between the conductive material, the active material, and the current collector, and is usually added in an amount of 1% by weight to 30% by weight based on the total weight of the solid content of the negative electrode active material layer. Examples of such binders include fluororesin-based binders including polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders including polyvinyl alcohol; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; and silane-based binders.
[0090] The negative electrode may be manufactured according to a method for manufacturing a negative electrode well known in the art. For example, the negative electrode may be manufactured by applying a negative electrode active material slurry, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, onto a negative electrode current collector, rolling and drying the slurry to form a negative electrode active material layer, or by casting the negative electrode active material layer onto another support, peeling off the support, and laminating the resulting film onto the negative electrode current collector.
[0091] The negative electrode current collector generally has a thickness of 3 μm to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, like the positive electrode current collector, the surface can be formed with fine irregularities to strengthen the binding force of the negative electrode active material, and it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0092] The solvent may include water or an organic solvent such as NMP or alcohol, and may be used in an amount that provides a preferred viscosity when the negative electrode active material and, optionally, a binder and a conductive material are included. For example, the solvent may be included so that the solids concentration in the active material slurry including the negative electrode active material and, optionally, a binder and a conductive material is 50% by weight to 75% by weight, preferably 50% by weight to 65% by weight.
[0093] (3) Separator The lithium secondary battery according to the present invention includes a separator interposed between the positive electrode and the negative electrode.
[0094] The separator separates the negative electrode and the positive electrode and provides a path for lithium ion migration. Any separator that is normally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion migration of the electrolyte and has excellent electrolyte humidification ability is preferred.
[0095] Specifically, the separator may be a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof. Also, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, or the like, may be used. Also, in order to ensure heat resistance or mechanical strength, a coated separator containing a ceramic component or a polymer material may be used, and may be selectively used in a single layer or multilayer structure.
[0096] (4) Non-aqueous electrolyte The non-aqueous electrolyte for a lithium secondary battery of the present invention may include a lithium salt, an organic solvent, lithium difluorophosphate, and a dinitrile compound represented by the following Chemical Formula 3.
[0097] [ka]
[0098] In the above Chemical Formula 3, R1, R2, R3, and R4 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or -R-CN, wherein R is an alkylene group having 1 to 12 carbon atoms, and one of R1 and R2 and one of R3 and R4 is necessarily -R-CN.
[0099] (4-1) Lithium salt The lithium salt may be any one that is commonly used in electrolytes for lithium secondary batteries without any restrictions. For example, Li + The anion is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - , BF2C2O4 - , BC4O8 - , PF4C2O4 - , PF2C4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - and SCN - At least one selected from the group consisting of:
[0100] Specifically, the lithium salt is LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10, LiAlCl4, LiAlO4, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiN(SO2F)2(Lithium bis(fluorosulfonyl)imide, LiFSI), LiN(SO2CF2CF3)2(lithium bis(pentafluoroethanesulfonyl)imide, LiBETI) and LiN(SO2CF3)2(lithium bis(trifluoromethanesulfonyl)imide, LiTFSI). In addition to these, lithium salts commonly used in electrolytes for lithium secondary batteries can be used without any restrictions.
[0101] The lithium salt can be appropriately changed within a range that is normally usable, but in order to obtain an optimal effect of forming a corrosion prevention coating on the surface of the electrode, it can be contained in the electrolyte at a concentration of 0.8 M to 3.0 M, specifically, at a concentration of 1.0 M to 3.0 M.
[0102] If the concentration of the lithium salt is less than 0.8 M, the mobility of lithium ions may decrease, resulting in a decrease in capacity characteristics. If the concentration of the lithium salt is more than 3.0 M, the viscosity of the non-aqueous electrolyte may increase excessively, resulting in a decrease in electrolyte impregnation, and a decrease in the film formation effect.
[0103] (4-2) Organic Solvent As the organic solvent, various organic solvents commonly used in lithium electrolytes can be used without limitation. Specifically, the type of the organic solvent is not limited as long as it can minimize decomposition due to an oxidation reaction during the charge / discharge process of the secondary battery and can exhibit the desired properties together with the additive.
[0104] For example, the organic solvent may be a cyclic carbonate organic solvent having a high dielectric constant and a high viscosity that easily dissociates the lithium salt in the electrolyte. In addition, the organic solvent may be a mixture of the cyclic carbonate organic solvent and at least one of a linear carbonate organic solvent and a linear ester organic solvent in order to produce an electrolyte having high ionic conductivity.
[0105] The cyclic carbonate organic solvent is a high-viscosity organic solvent that has a high dielectric constant and can effectively dissociate the lithium salt in the electrolyte. Specific examples of the cyclic carbonate organic solvent include at least one organic solvent selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate, and among these, ethylene carbonate can be included.
[0106] In addition, the linear carbonate organic solvent is an organic solvent having low viscosity and low dielectric constant, and a representative example thereof is at least one organic solvent selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, and specifically, ethyl methyl carbonate (EMC) can be included.
[0107] Specific examples of the linear ester-based organic solvent include at least one organic solvent selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate.
[0108] Specifically, the organic solvent of the present invention can be at least one of a cyclic carbonate organic solvent, a linear carbonate organic solvent, and a linear ester organic solvent in a volume ratio of 10:90 to 80:20, specifically, a volume ratio of 30:70 to 50:50.
[0109] Meanwhile, in the nonaqueous electrolyte of the present invention, components other than the organic solvent, for example, the remainder other than the lithium salt, lithium difluorophosphate, dinitrile compound and other additives, may be an organic solvent unless otherwise specified.
[0110] (4-3) Lithium difluorophosphate The non-aqueous electrolyte of the present invention may contain lithium difluorophosphate as a first additive in order to achieve an effect of improving the long-term life characteristics of the secondary battery.
[0111] The lithium difluorophosphate is decomposed during initial charging to generate lithium ion components, which can form a stable SEI film on the surface of the negative electrode, and the formation of such an SEI film can improve Li mobility at the negative electrode and reduce interface resistance. In addition, the difluorophosphate anions generated during initial charging are present on the surface of the positive electrode, which can stabilize the positive electrode and improve discharge characteristics.
[0112] The lithium difluorophosphate may be included in an amount of 0.1% by weight to 1.5% by weight based on the total weight of the non-aqueous electrolyte.
[0113] When the lithium difluorophosphate is contained in the above content range, a stable film is formed, and the elution of transition metals from the positive electrode at high temperatures can be effectively suppressed, and excellent high-temperature durability can be achieved. That is, when the lithium difluorophosphate is contained in the non-aqueous electrolyte at 0.1 wt % or more, the film forming effect is improved, and a stable SEI film is formed even during high-temperature storage, so that an increase in resistance and a decrease in capacity can be prevented even after high-temperature storage, and various performances can be improved. In addition, when the lithium difluorophosphate is contained in an amount of 1.5 wt % or less, an excessively thick film is prevented from being formed during initial charging, an increase in resistance can be prevented, and a decrease in the initial capacity and output characteristics of the secondary battery can be prevented.
[0114] Specifically, the lithium difluorophosphate may be contained in an amount of 0.1% by weight to 1.0% by weight based on the total weight of the non-aqueous electrolyte.
[0115] (4-4) Dinitrile compounds In addition, the non-aqueous electrolyte of the present invention may contain the dinitrile compound represented by Chemical Formula 3 as a second additive in order to improve the cycle performance and output performance of the secondary battery.
[0116] The dinitrile compound represented by the chemical formula 3 is a compound containing one or more polar nitrile groups (-CN) having a high dipole moment at both ends, and the polar nitrile groups bind to transition metal ions eluted from the positive electrode, preventing the transition metal ions from precipitating on the surface of inorganic particles on the organic-inorganic composite separator. In addition, when the dinitrile compound binds to a transition metal, its volume increases and its mobility in the electrolyte decreases, which is also a factor that can suppress side reactions caused by the transition metal. In particular, the dinitrile compound contained in the nonaqueous electrolyte of the present invention contains an unsaturated double bond, which further increases the binding force between the nitrile groups at both ends and the transition metal, and has excellent effects of capturing and preventing the release of transition metals even under high voltage conditions, effectively preventing side reactions in the electrolyte, and ensuring the stability of the battery.
[0117] Exemplary dinitrile compounds according to the present invention include 1,4-dicyano-2-butene, 1,4-dicyano-2-methyl-2-butene, 1,4-dicyano-2-ethyl-2-butene, 1,4-dicyano-2,3-dimethyl-2-butene, 1,4-dicyano-2,3-diethyl-2-butene, 1,6-dicyano-3-hexene, 1,6-dicyano-2-methyl-3-hexene, 1,6-dicyano-2-methyl-5-methyl-3-hexene, and the like, which may be used alone or in combination of two or more thereof, and specifically may include 4-dicyano-2-butene.
[0118] The dinitrile compound may have two or more nitrile groups in the cis or trans positions relative to the double bond, and preferably in the trans positions.
[0119] Furthermore, compared with common nitrile additives such as succinonitrile or adiponitrile, the dinitrile compound further contains a double bond in the middle of the structure, and thus forms an organic polymer-type coating by oxidative decomposition of the double bond, and forms a complex structure or ligand on the surface of the positive electrode by strong bonding with metal ions, and can form a very stable ion-conductive coating. As a result, side reactions between the electrolyte and the positive electrode can be prevented and gas generation can be suppressed. Furthermore, the non-shared electron pair of N in the nitrile group stabilizes the anion of the lithium salt and suppresses the generation of HF due to the decomposition of the lithium salt, thereby further improving the high-temperature storage characteristics of the secondary battery.
[0120] On the other hand, when a dinitrile-based compound is included alone as a non-aqueous electrolyte additive, it has the advantage of improving cycle characteristics and high-temperature storage characteristics, but when included in a specific content range, it has the disadvantage of deteriorating cycle characteristics due to an increase in resistance. In order to solve this problem, the present invention uses the lithium difluorophosphate compound, which can reduce battery resistance as an essential electrolyte additive component, together with the dinitrile-based compound in a specific mixing ratio, thereby suppressing the increase in resistance and improving the deterioration of cycle characteristics due to the synergistic effect of these additives.
[0121] Specifically, the non-aqueous electrolyte of the present invention may contain the lithium difluorophosphate and the dinitrile compound in a weight ratio of 1:0.25 to 1:3.
[0122] When the lithium difluorophosphate and the dinitrile-based compound are contained in the above content ratio, a coating film having a lower resistance and a higher stability is selectively formed than when the dinitrile-based compound is introduced alone onto the surface of the positive electrode active material not coated with a metal element, and therefore, it is possible to suppress the elution of transition metals from the positive electrode at high temperatures and realize a battery having excellent high-temperature durability.
[0123] Specifically, the lithium difluorophosphate and the dinitrile-based compound may be included in a weight ratio of 1:0.25 to 1:2.
[0124] In this way, the lithium secondary battery of the present invention includes a core including a lithium cobalt-based oxide represented by Chemical Formula 1, and a shell including a lithium cobalt-based oxide represented by Chemical Formula 2 arranged on the surface of the core, and the core and shell include a positive electrode including a positive electrode active material including at least one doping element selected from the group consisting of Al, Zr, Mg, and Ti, and a nonaqueous electrolyte including lithium difluorophosphate and a dinitrile compound as an additive, thereby forming a thin, low-resistance, stable passivation film on the surface of the positive electrode, thereby reducing the resistance of the surface of the positive electrode and suppressing side reactions during high-temperature storage, thereby improving durability. Therefore, the capacity characteristics and high-temperature durability of the lithium secondary battery can be maximized.
[0125] (4-5) Other additives Meanwhile, the nonaqueous electrolyte of the present invention may further include other additives that can act as a complement to form a stable coating on the surface of the negative electrode and the positive electrode without significantly increasing the initial resistance along with the effects exerted by the additives when used together with the first and second additives, or inhibit decomposition of a solvent in the nonaqueous electrolyte and improve the mobility of lithium ions.
[0126] The other additives are not particularly limited as long as they can form stable coatings on the surfaces of the positive and negative electrodes. Representative examples of the other additives include at least one additive selected from the group consisting of cyclic carbonate compounds, halogen-substituted carbonate compounds, sultone compounds, nitrile compounds, phosphate compounds, borate compounds, and lithium salt compounds.
[0127] Specifically, the cyclic carbonate-based compound forms a stable SEI film mainly on the surface of the negative electrode during battery activation, thereby improving the durability of the battery. Such a cyclic carbonate-based compound may be vinylene carbonate (VC) or vinyl ethylene carbonate (VEC), and may be contained in an amount of 3 wt% or less based on the total weight of the non-aqueous electrolyte. If the content of the cyclic carbonate-based compound in the non-aqueous electrolyte exceeds 3 wt%, the cell swelling suppression performance and initial resistance may be deteriorated.
[0128] The halogen-substituted carbonate-based compound may be fluoroethylene carbonate (FEC) and may be included in an amount of 5 wt% or less based on the total weight of the non-aqueous electrolyte. If the content of the halogen-substituted carbonate-based compound exceeds 5 wt%, the cell swelling performance may be deteriorated.
[0129] Furthermore, the sultone-based compound may be, for example, at least one compound selected from the group consisting of 1,3-propane sultone (PS), 1,4-butane sultone, ethene sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone.
[0130] In addition, the nitrile compound may be at least one compound selected from the group consisting of succinonitrile (SN), adiponitrile (Adn), acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonitrile, hexanetricarbonitrile (HTCN), cyclohexanecarbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile.
[0131] The nitrile-based compound may act as a complement to form a negative electrode SEI film, may inhibit decomposition of the solvent in the electrolyte, and may improve the mobility of lithium ions. The nitrile-based compound may be included in an amount of 8 wt% or less based on the total weight of the non-aqueous electrolyte. If the total content of the nitrile-based compound in the non-aqueous electrolyte exceeds 8 wt%, the resistance increases due to an increase in the film formed on the surface of the electrode, and battery performance may be deteriorated.
[0132] In addition, the phosphate-based compound stabilizes PF6 anions in the electrolyte and is useful for forming the positive and negative electrode coatings, thereby improving the durability of the battery. Such phosphate-based compounds include one or more compounds selected from the group consisting of lithium difluoro(bisoxalato)phosphate (LiDFOP), tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphite, and may be contained in an amount of 3% by weight or less based on the total weight of the non-aqueous electrolyte.
[0133] The borate-based compound can promote the separation of ion pairs of lithium salts, improve the mobility of lithium ions, reduce the interface resistance of the SEI coating, and dissociate substances such as LiF that are generated during battery reactions and are difficult to separate, thereby resolving problems such as the generation of hydrofluoric acid gas. Examples of such borate-based compounds include lithium bisoxalatoborate (LiBOB, LiB(C2O4)2), lithium oxalyl difluoroborate (LiODFB), and tetramethyltrimethylsilylborate (TMSB), and can be included in an amount of 3 wt % or less based on the total weight of the nonaqueous electrolyte.
[0134] The lithium salt compound may be LiBF4 as a compound different from the lithium salt contained in the non-aqueous electrolyte, and may be contained in an amount of 3 wt % or less based on the total weight of the non-aqueous electrolyte.
[0135] The other additives can be used in combination of two or more kinds, and can be contained in an amount of 10% by weight or less, specifically 0.01% by weight to 10% by weight, and preferably 0.1% by weight to 5.0% by weight, based on the total amount of the electrolyte.
[0136] If the content of the other additives is less than 0.01 wt%, the high-temperature storage characteristics and gas reduction effects that the additives are intended to achieve are not sufficient, and if the content of the other additives is more than 10 wt%, excessive side reactions may occur in the electrolyte during charging and discharging of the battery. In particular, if the other additives are added in excess, they may not be sufficiently decomposed and may remain in an unreacted or precipitated state in the electrolyte at room temperature. This may increase resistance and reduce the life characteristics of the secondary battery.
[0137] Such a nonaqueous electrolyte solution of the present invention, by containing an additive of a specific composition, selectively forms a highly durable coating on the surface of the positive electrode active material, prevents the elution of transition metals from the positive electrode, ensures the structural stability of the positive electrode active material, and prevents sustained decomposition reactions of the electrolyte solution, thereby making it possible to realize a lithium secondary battery with improved high-temperature durability, cycle characteristics, and output characteristics.
[0138] In the present invention, a lithium secondary battery having improved cycle characteristics and output characteristics can be provided by including a positive electrode containing a lithium cobalt-based oxide containing a doping element in a specific concentration range as a positive electrode active material and a non-aqueous electrolyte containing an additive capable of forming a highly durable coating on the surface of the electrode. Such a lithium secondary battery according to the present invention is useful in portable devices such as mobile phones, notebook computers, and digital cameras, and in the field of electric vehicles such as hybrid electric vehicles (HEVs).
[0139] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may be embodied in various different forms and should not be construed as limited to the embodiments set forth herein.
[0140] [Example] Example 1. (Production of non-aqueous electrolyte) LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC): propylene carbonate (PC): ethylene propionate (EP): propylene propionate (PP) were mixed in a weight ratio of 20:10:25:45 to a concentration of 1.2 M, and then 0.25 wt% lithium difluorophosphate (hereinafter abbreviated as "LiDFP"), 0.5 wt% 1,4-dicyano-2-butene (hereinafter abbreviated as "DCB"), and other A non-aqueous electrolyte was prepared by adding 16.5 wt% of additives (0.5 wt% vinyl ethylene carbonate (VEC), 4 wt% 1,3-propane sultone (PS), 7 wt% fluoroethylene carbonate (FEC), 1.5 wt% succinonitrile (SN), 3 wt% hexanetricarbonitrile (HTCN), 0.3 wt% lithium oxalyl difluoroborate (LiODFB), and 40.2 wt% LiBF) (see Table 1 below).
[0141] (Production of positive electrodes) (i) Production of positive electrode active material LiCoO2 powder was mixed with Al(NO3)3·9H2O, Zr(NO3)2·xH2O (x is an integer between 1 and 6), MgO, and TiO2 in a weight ratio of 1:0.085:0.0015:0.0026:0.0006, and then a primary heat treatment was carried out at 900 °C for more than 3 h.
[0142] Then, the material obtained by the first heat treatment was mixed with LiCoO2 powder, Al(NO3)3·9H2O, Zr(NO3)2·xH2O (x is an integer from 1 to 6), MgO and TiO2 in a weight ratio of 1:0.0085:0.00015:0.00026:0.00006, and then a second heat treatment was performed at 900℃ for more than 3 hours to obtain Li 1.02Co 0.9849 Al 0.0113 Zr 0.0003 Mg 0.0031 Ti 0.0004 The surface of the core (Li / (Co+M) ratio = 1.02) made of O2 is covered with Li 0.94 Co 0.99848 Al 0.00113 Zr 0.00003 Mg 0.00031 Ti 0.00005 A positive electrode active material was produced in which a shell portion made of O2 (Li / (Co+M) ratio = 0.94) was formed.
[0143] Here, in the positive electrode active material, the doping elements, that is, the Al content is 0.52 wt %, the Zr content is 0.05 wt %, the Mg content is 0.13 wt %, and the Ti content is 0.03 wt %.
[0144] (ii) Manufacture of the positive electrode The positive electrode active material, conductive material (carbon black), and binder (polyvinylidene fluoride) were added to a solvent, N-methyl-2-pyrrolidone (NMP), in a weight ratio of 97.5:1:1.5 to prepare a positive electrode active material slurry (solid concentration 60 wt%). The positive electrode active material slurry was applied to a positive electrode current collector (aluminum thin film) having a thickness of 15 μm, dried, and then roll pressed to prepare a positive electrode.
[0145] (Production of negative electrodes) A negative electrode active material slurry (solid concentration 50 wt%) was prepared by adding a negative electrode active material (graphite), a conductive material (carbon black) and a binder (polyvinylidene fluoride) to distilled water in a weight ratio of 96:0.5:3.5. The negative electrode active material slurry was applied to a negative electrode current collector (Cu thin film) having a thickness of 8 μm, dried, and then roll pressed to prepare a negative electrode.
[0146] (Secondary battery manufacturing) The positive and negative electrodes prepared by the above-mentioned method were laminated together with a polyethylene porous film as a separator to prepare an electrode assembly, which was then placed in a battery case, into which 5 mL of the non-aqueous electrolyte was poured, and the battery case was sealed to prepare a pouch-type lithium secondary battery (battery capacity 6.24 mAh).
[0147] Example 2. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.2 M, and then 0.5 wt % of LiDFP, 0.5 wt % of DCB, and 16.5 wt % of other additives were added to prepare a non-aqueous electrolyte solution.
[0148] Example 3. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.2 M, and then 1.0 wt % LiDFP, 0.5 wt % DCB, and 16.5 wt % other additives were added to prepare a non-aqueous electrolyte solution.
[0149] Example 4. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.2 M, and then 1.5 wt % LiDFP, 0.5 wt % DCB, and 16.5 wt % other additives were added to prepare a non-aqueous electrolyte solution.
[0150] Example 5. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.2 M, and then 0.255 wt % of LiDFP, 0.5 wt % of DCB, and 16.5 wt % of other additives were added to prepare a non-aqueous electrolyte solution.
[0151] Example 6. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.2 M, and then 1.0 wt % LiDFP, 2.0 wt % DCB, and 16.5 wt % other additives were added to prepare a non-aqueous electrolyte solution.
[0152] Example 7. A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.2 M, and then 1.5 wt % LiDFP, 3.0 wt % DCB, and 16.5 wt % other additives were added to prepare a non-aqueous electrolyte solution.
[0153] Example 8. (Production of positive electrodes) (i) Production of positive electrode active material LiCoO2 powder was mixed with Al(NO3)3·9H2O, Zr(NO3)2·xH2O (x is an integer between 1 and 6), MgO, and TiO2 in a weight ratio of 1:0.078:0.00064:0.0022:0.0005, and then a primary heat treatment was carried out at 900 °C for more than 3 h.
[0154] Then, the material obtained by the first heat treatment was mixed with LiCoO2 powder, Al(NO3)3·9H2O, Zr(NO3)2·xH2O (x is an integer from 1 to 6), MgO and TiO2 in a weight ratio of 1:0.0078:0.000064:0.00022:0.00005, and then a second heat treatment was performed at 900℃ for more than 3 hours to obtain Li 1.02 Co 0.9851 Al 0.0113 Zr 0.0002 Mg 0.0031 Ti 0.0004 The surface of the core (Li / (Co+M) ratio = 1.02) made of O2 is covered with Li 0.94 Co 0.9985 Al 0.00113 Zr 0.00002 Mg 0.00031 Ti 0.00004 A positive electrode active material was produced in which a shell portion made of O2 (Li / (Co+M) ratio = 0.94) was formed.
[0155] Here, in the positive electrode active material, the doping elements, that is, the Al content is 0.52 wt %, the Zr content is 0.025 wt %, the Mg content is 0.13 wt %, and the Ti content is 0.03 wt %.
[0156] (ii) Manufacture of the positive electrode The positive electrode active material, conductive material (carbon black), and binder (polyvinylidene fluoride) were added to a solvent, N-methyl-2-pyrrolidone (NMP), in a weight ratio of 97.5:1:1.5 to prepare a positive electrode active material slurry (solid concentration 60 wt%). The positive electrode active material slurry was applied to a positive electrode current collector (aluminum thin film) having a thickness of 15 μm, dried, and then roll pressed to prepare a positive electrode.
[0157] (Secondary battery manufacturing) A lithium secondary battery was manufactured in the same manner as in Example 1, except that the prepared positive electrode was used.
[0158] Example 9. (Production of positive electrodes) (i) Production of positive electrode active material LiCoO2 powder was mixed with Al(NO3)3·9H2O, Zr(NO3)2·xH2O (x is an integer between 1 and 6), MgO, and TiO2 in a weight ratio of 1:0.078:0.0022:0.0022:0.0005, and then a primary heat treatment was carried out at 900 °C for more than 3 h.
[0159] Then, the material obtained by the first heat treatment was mixed with LiCoO2 powder, Al(NO3)3·9H2O, Zr(NO3)2·xH2O (x is an integer from 1 to 6), MgO and TiO2 in a weight ratio of 1:0.0078:0.00022:0.00022:0.00005, and then a second heat treatment was performed at 900℃ for more than 3 hours to obtain Li 1.02 Co 0.9847 Al 0.0113 Zr 0.0005 Mg 0.0031 Ti 0.0004 The surface of the core (Li / (Co+M) ratio = 1.02) made of O2 is covered with Li 0.94 Co 0.9985 Al 0.0011 Zr 0.00005 Mg 0.00031 Ti 0.00004 A positive electrode active material was produced in which a shell portion made of O2 (Li / (Co+M) ratio = 0.94) was formed.
[0160] Here, in the positive electrode active material, the doping elements, that is, the Al content is 0.52 wt %, the Zr content is 0.085 wt %, the Mg content is 0.13 wt %, and the Ti content is 0.03 wt %.
[0161] (ii) Manufacture of the positive electrode The positive electrode active material, conductive material (carbon black), and binder (polyvinylidene fluoride) were added to a solvent, N-methyl-2-pyrrolidone (NMP), in a weight ratio of 97.5:1:1.5 to prepare a positive electrode active material slurry (solid concentration 60 wt%). The positive electrode active material slurry was applied to a positive electrode current collector (aluminum thin film) having a thickness of 15 μm, dried, and then roll pressed to prepare a positive electrode.
[0162] (Secondary battery manufacturing) A lithium secondary battery was manufactured in the same manner as in Example 1, except that the prepared positive electrode was used.
[0163] Comparative Example 1 A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.2 M, and then 1.5 wt % of LiDFP and 16.5 wt % of other additives were added to prepare a non-aqueous electrolyte solution.
[0164] Comparative Example 2 A lithium secondary battery was manufactured in the same manner as in Example 1, except that LiPF6 was dissolved in a non-aqueous organic solvent to a concentration of 1.2 M, and then 0.5 wt % of DCB and 16.5 wt % of other additives were added to prepare a non-aqueous electrolyte solution.
[0165] Comparative Example 3. (Production of positive electrodes) A positive electrode active material (LiCoO2), a conductive material (carbon black), and a binder (polyvinylidene fluoride) were added to a solvent, N-methyl-2-pyrrolidone (NMP), in a weight ratio of 97.5:1:1.5 to prepare a positive electrode active material slurry (solid concentration 60 wt%). The positive electrode active material slurry was applied to a positive electrode current collector (aluminum thin film) with a thickness of 15 μm, dried, and then roll pressed to prepare a positive electrode.
[0166] (Secondary battery manufacturing) A lithium secondary battery was manufactured in the same manner as in Example 1, except that the prepared positive electrode was used.
[0167] Comparative Example 4. (Production of positive electrodes) Cathode active material (Li(Ni) 0.6 Co 0.2 Mn 0.2 A cathode active material slurry (solid concentration 60 wt%) was prepared by adding N-methyl-2-pyrrolidone (NMP) as a solvent to the cathode active material slurry (carbon black; NCM622) in a weight ratio of 97.5:1:1.5. The cathode active material slurry was applied to a cathode current collector (aluminum thin film) with a thickness of 15 μm, dried, and then roll pressed to prepare a cathode.
[0168] (Secondary battery manufacturing) A lithium secondary battery was manufactured in the same manner as in Example 1, except that the prepared positive electrode was used.
[0169] Experimental Example Experimental Example 1. Evaluation of initial capacity The lithium secondary batteries manufactured in Examples 1 to 9 and Comparative Examples 1 to 4 were each activated at 0.1 C CC. Then, using a PESC05-0.5 charger / discharger (PNE Solutions, 5V, 500mA) at room temperature, the batteries were charged to 4.5V at 0.5 C CC under constant current-constant voltage (CC-CV) charging conditions, and then discharged to 2.5V at 0.5 C CC under CC conditions with a 0.05 C current cut-off. After three cycles of charging and discharging, the third discharge capacity was selected as the initial capacity and is shown in Table 1 below.
[0170] Experimental example 2: Evaluation of high temperature cycle The lithium secondary batteries prepared in Examples 1 to 9 and Comparative Examples 1 to 4 were each charged at 45° C. under constant current / constant voltage conditions at a 0.33 C rate to 4.2 V, and then discharged at a 0.33 C rate under constant current conditions to 3 V for one cycle. The initial discharge capacity and initial resistance after one cycle were measured.
[0171] After that, 200 cycles of charge and discharge were performed under the above-mentioned conditions for one cycle, and then the capacity retention rate (%) and resistance value (mOhm) were measured. The capacity retention rate (%) was calculated by the following formula 1, and the measurement results are shown in Table 1 below.
[0172] [Formula 1] Capacity retention rate (%) = (discharge capacity after 100 cycles / discharge capacity after 1 cycle) x 100
[0173] [Table 1]
[0174] Referring to Table 1, it can be seen that the initial capacity, the capacity retention rate (%) after 200 cycles at high temperature (45°C), and the resistance value of the secondary batteries of Examples 1 to 9 of the present invention were improved compared to the secondary batteries of Comparative Examples 1 to 4.
[0175] Experimental Example 3: Evaluation of high-temperature storage The lithium secondary batteries prepared in Examples 1 to 9 and Comparative Examples 1 to 4 were each charged to 4.2 V at room temperature (25° C.) under constant current / constant voltage conditions at a rate of 0.33 C, and then discharged to a depth of discharge (DOD) of 50% to adjust the SOC to 50%, and then discharged at a rate of 2.5 C for 10 seconds, and the initial capacity was measured.
[0176] Then, each lithium secondary battery was stored at 85° C. for 8 hours, and then discharged, charged, and discharged at 0.33 C to evaluate the recovery capacity. The results are shown in Table 2 below.
[0177] [Table 2]
[0178] Referring to Table 2, it can be seen that the secondary batteries of Examples 1 to 9 of the present invention have improved initial capacity and recovered capacity (%) compared to the secondary batteries of Comparative Examples 1 to 4.
[0179] Experimental Example 4: Evaluation of metal elution amount The lithium secondary batteries prepared in Examples 1 to 9 and Comparative Examples 1 to 4 were stored at 85° C. for 8 hours, and then decomposed in a fully discharged state to analyze the amounts of Ni, Co, and Mn deposited on the negative electrodes (ICP-OES, Perkin Elmer, AVIO 500), and the results are shown in Table 3 below (unit of dissolved metal content: ppm).
[0180] [Table 3]
[0181] Referring to Table 3, it can be seen that in the case of the secondary batteries of Examples 1 to 9 of the present invention, the amount of metal ions eluted after high-temperature storage was reduced compared to the secondary batteries of Comparative Examples 1 to 4.
[0182] In particular, in the case of the lithium secondary batteries of Comparative Examples 1 and 2 equipped with non-aqueous electrolytes not containing the additive composition of the present invention, it was confirmed that it was impossible to form a polymer coating on the positive electrode or to form a coating by strong adsorption, and the elution of transition metals was significantly increased compared to the lithium secondary batteries of Examples 1 to 9.
[0183] From these results, it can be seen that the lithium secondary battery using the nonaqueous electrolyte of the present invention has improved capacity retention rate (%) after cycling and metal elution suppression effect, and has reduced resistance value.
[0184] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the following claims also fall within the scope of the present invention.
Claims
1. a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; a separator interposed between the positive electrode and the negative electrode; and a non-aqueous electrolyte for a lithium secondary battery, The positive electrode active material includes a core including a lithium cobalt-based oxide represented by the following Chemical Formula 1, and a shell including a lithium cobalt-based oxide represented by the following Chemical Formula 2 disposed on a surface of the core, the core and the shell including at least one doping element selected from the group consisting of Al, Zr, Mg, and Ti, The non-aqueous electrolyte solution of the lithium secondary battery includes a lithium salt, an organic solvent, lithium difluorophosphate, and a dinitrile-based compound represented by the following Chemical Formula 3: [Chemical formula 1] Li a Co 1-b M b O 2 (In the above Chemical Formula 1, M is at least one selected from the group consisting of Al, Zr, Mg and Ti; 1≦a≦1.2, 0.005≦b≦0.05.) [Chemical formula 2] Li x Co 1-y M y O 2 (In the above Chemical Formula 2, M 1 is at least one selected from the group consisting of Al, Zr, Mg and Ti; 0.5≦x<1, 0≦y≦0.002.) 【Chemistry 1】 (In the above Chemical Formula 3, R 1 , R 2 , R 3 and R 4 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or -R-CN, wherein R is an alkylene group having 1 to 12 carbon atoms; The R 1 and R 2 At least one of is -R-CN; The R 3 and R 4 At least one of the groups is -R-CN.
2. 2. The lithium secondary battery of claim 1, wherein the doping element is present in a concentration gradient that decreases from the center of the core toward the core-shell interface.
3. 2. The lithium secondary battery according to claim 1, wherein the doping element comprises zirconium (Zr), and optionally further comprises at least one selected from the group consisting of aluminum (Al), magnesium (Mg) and titanium (Ti).
4. 2. The lithium secondary battery according to claim 1, wherein the zirconium (Zr) among the doping elements is contained in an amount of 0.025% by weight to 0.085% by weight based on the total weight of the positive electrode active material.
5. The lithium secondary battery according to claim 4, wherein the zirconium (Zr) among the doping elements is contained in an amount of 0.03 wt % to 0.08 wt % based on the total weight of the positive electrode active material.
6. 2. The lithium secondary battery according to claim 1, wherein the aluminum (Al) among the doping elements is contained in an amount of 0.5% by weight to 0.55% by weight based on the total weight of the positive electrode active material.
7. 2. The lithium secondary battery according to claim 1, wherein the doping element, magnesium (Mg), is contained in an amount of 0.1% by weight to 0.15% by weight based on the total weight of the positive electrode active material.
8. 2. The lithium secondary battery according to claim 1, wherein the doping element titanium (Ti) is contained in an amount of 0.01% by weight to 0.05% by weight based on the total weight of the positive electrode active material.
9. 2. The lithium secondary battery according to claim 1, wherein the lithium difluorophosphate is contained in an amount of 0.1% by weight to 1.5% by weight based on the total weight of the non-aqueous electrolyte for lithium secondary batteries.
10. 2. The lithium secondary battery according to claim 1, wherein the --R--CN groups in the dinitrile compound are in trans positions relative to each other.
11. 2. The lithium secondary battery according to claim 1, wherein the dinitrile compound is at least one selected from the group consisting of 1,4-dicyano-2-butene, 1,4-dicyano-2-methyl-2-butene, 1,4-dicyano-2-ethyl-2-butene, 1,4-dicyano-2,3-dimethyl-2-butene, 1,4-dicyano-2,3-diethyl-2-butene, 1,6-dicyano-3-hexene, 1,6-dicyano-2-methyl-3-hexene, and 1,6-dicyano-2-methyl-5-methyl-3-hexene.
12. 2. The lithium secondary battery according to claim 1, wherein the dinitrile compound is 1,4-dicyano-2-butene.
13. 2. The lithium secondary battery according to claim 1, wherein the weight ratio of the lithium difluorophosphate and the dinitrile-based compound is 1:0.25 to 1:
3.
14. 2. The lithium secondary battery according to claim 1, wherein a weight ratio of the lithium difluorophosphate and the dinitrile-based compound is 1:0.25 to 1:2.
Citation Information
Patent Citations
Non-aqueous electrolyte additive having cyano group and electrochemical device using the same
JP2009543318A
Positive electrode active material for lithium secondary battery, method for producing the same, and lithium secondary battery including the same
JP2017536649A
Lithium-ion batteries for automotive applications
JP2019509605A
Lithium-cobalt-based positive electrode active material, its manufacturing method, positive electrode and secondary battery including the same
JP2020537308A
Nonaqueous electrolyte secondary battery
WO2014034043A1
Cited By
Electrochemical and Electronic Devices
JP2024542588A
Electrochemical and electronic devices
JP7780645B2