Novel Photoinitiators

Bifunctional photoinitiators responsive to UVA, UVB, and UVC wavelengths address the issues of poor surface curability and yellowing in existing photoinitiators, enhancing reactivity and reducing post-curing yellowing, particularly under LED light sources.

JP2024537185AInactive Publication Date: 2024-10-10IGM RESINS ITAL

Patent Information

Application Number
JP2024520895
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-08
Filing Date
2022-08-04
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing photoinitiators suffer from poor surface curability and significant yellowing after curing, making them unsuitable for applications requiring transparency and high reactivity, such as transparent varnishes.

Method used

Development of bifunctional photoinitiators responsive to UVA, UVB, and UVC wavelength ranges, particularly effective under LED light sources, with formulations that minimize yellowing and enhance surface curing.

Benefits of technology

The new photoinitiators exhibit improved reactivity and reduced yellowing, achieving better surface curing performance compared to prior art compounds, especially under LED lamps.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to novel photoinitiators and photopolymerization compositions having improved performance, as well as methods for photopolymerizing compositions containing the photoinitiators and their use in products including printed, coated, and assembled parts.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to novel photoinitiators that have improved reactivity and surface cure properties and / or reduced yellowing after cure, and the use of the photoinitiators in photopolymerizable compositions. The present invention also relates to methods of photopolymerizing compositions that include the photoinitiators, and the use of the photoinitiators in products, including printed, coated, and assembled assemblies. [Background technology]

[0002] In recent years, the design and development of new photoinitiators (Pls) has attracted attention because many photoinitiators have been banned or are scheduled to be banned as toxic or reproductive toxicants.

[0003] There have been many attempts to develop new photoinitiators that can mimic standard photoinitiators or overcome issues such as yellowing, faster line speeds, and curing under LED lamps. Some examples are glyoxylic acid 3-ketocoumarin (WO2021 / 070152), benzoyl phenyl telluride PIs (Macromolecules, 2014, 47(16), 5526-5531), silicon-based PIs (JP2010-229169; Macromolecules, 2009, 42(16), 6031-6037; Macromolecules 2007, 40(24), 8527-8530; Macromol. Rapid Commun. 2017, 38, 1600470; Macromolecules, 2017, 50(17), 6911-6923), and fluorine-based PIs (US2019 / 0155153). For sensitive applications, e.g. food packaging, photoinitiators that can photocrosslink within the matrix are preferred, besides good reactivity and low yellowing, to avoid possible migration of the photoinitiator into the food. Only a few examples exist in the literature, the most recent being reported in EP 2 617 705 A1. Summary of the Invention [Problem to be solved by the invention]

[0004] Unfortunately, these photoinitiators also have several limitations when used in standard applications, such as poor surface cure and, most importantly, yellowing after curing, which makes the abovementioned PIs unsuitable for use in polymerization systems that include clear varnishes.

[0005] Therefore, there is a demand for new technical solutions that can improve the surface curability of PIs and / or limit the yellowing after curing, without affecting the good reactivity of these products.

[0006] It is a first object of the present invention to provide novel PIs, their use as photoinitiators, and photocurable compositions containing them.

[0007] It is a further object of the present invention to provide photocurable compositions containing the novel PIs of the present invention.

[0008] It is a further object of the present invention to provide a method for photocuring ethylenically unsaturated compounds using the novel PIs, and products produced thereby. [Means for solving the problem]

[0009] Surprisingly, we have discovered that certain bifunctional photoinitiators respond well to the UVA, UVB, and UVC wavelength ranges, and even more preferably to LED light sources emitting in the 350-420 nm range. Maintaining low post-cure yellowing represents a technological advancement compared to prior art.

[0010] In fact, improved performance under LED lamps is always associated with increased yellowing after curing.

[0011] According to one aspect, the present invention relates to a compound of formula (I) Formula (I) [ka] wherein R1 is selected from aryl and heteroaryl, each of which is optionally substituted with one or more substituents selected from: halogen, substituted or unsubstituted C1-C20 alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted C1-C20 alkylthio, substituted or unsubstituted (C1-C12 alkyl)2amino, morpholino, piperidino, piperazino and N(C1-C12 alkyl)piperazino; n is 1 to 7; R2 is a group of formula (II) Formula (II) [ka] where G is an optionally ethoxylated and / or propoxylated monomeric, oligomeric or polymeric polyol G-(OH) m+n+p where m+n+p is from 2 to 8, m is 1 to 7; p is 0 to 6; R3 is selected from CH2=CH-C(=O) and CH2=C(CH3)-C(=O); The wavy line indicates a bond to a compound of formula (I); Z is selected from (i), (ii), and (iii) below: (i) [ka] (ii) [ka] (iii) [ka] Where: X is selected from O, S and C(R4)(R5); Y is selected from O, S, C(R4)(R5) and NR6; R4 and R5 are each independently selected from H, C1-C12 alkyl, OH, and C1-C10 alkoxy; R6 is selected from H and C1-C8 alkyl; The wavy line characterizes the bond attached to the keto group in formula (I).

[0012] According to the present invention, G-(OH) m+n+p is selected from monomeric polyols, oligomeric polyols, polymeric polyols and mixtures thereof, which may be optionally ethoxylated or propoxylated.

[0013] Suitable examples of monomeric and oligomeric polyols include ethylene glycol, propylene glycol, 1,2-butanediol, 1,2-propanediol, 1,2-hexanediol, diethanolamine, N-methyldiethanolamine, glycerol, diglycerol, triglycerol, triethanolamine, trimethylolpropane, ditrimethylolpropane, pentaerythritol, dipentaerythritol, sorbitol, mannitol, xylitol, and other sugar alcohols, and mixtures thereof.

[0014] Examples of polymer polyols are polyhydroxy polyethers, which can be both aliphatic or aromatic, polyhydroxy polyesters, polyhydroxy polyamides, polyhydroxy polyimides, polyhydroxy polycarbonates, styrene-allyl alcohol copolymers.

[0015] Alkoxylated polyols are particularly preferred for the realization of the present invention. Examples of such alkoxylated polyols are the above-mentioned monomeric, oligomeric and polymeric polyols that are alkoxylated, for example ethoxylated and / or propoxylated and / or butoxylated. Other suitable examples are alkoxylated linear or branched polyamines and polyalkoxylated diamines, such as ethoxylated ethylenediamine and ethoxylated 1,3-propylenediamine. In the alkoxylated compounds of the present invention, each group reactive towards alkylene oxide can provide 0 to 15 alkoxy units, preferably 1 to 6 alkoxy units.

[0016] In a preferred embodiment, G-(OH) m+n+p is selected from monomeric and oligomeric polyols.

[0017] In another preferred embodiment, G-(OH) m+n+p is selected from ethoxylated and / or propoxylated monomeric and oligomeric polyols.

[0018] Preferably, G-(OH) m+n+p teeth, - 1,500 Da or less, more preferably 1,000 Da or less, most preferably 800 Da or less, and - 100 Da or more, preferably 200 Da or more The number average molecular weight is

[0019] Preferably, G-(OH) m+n+pis selected from glycerol, ethoxylated and / or propoxylated glycerol, diglycerol, ethoxylated and / or propoxylated diglycerol, trimethylolpropane, ethoxylated and / or propoxylated trimethylolpropane, ditrimethylolpropane, ethoxylated and / or propoxylated ditrimethylolpropane, pentaerythritol, ethoxylated and / or propoxylated pentaerythritol, dipentaerythritol, ethoxylated and / or propoxylated dipentaerythritol, sorbitol, ethoxylated and / or propoxylated sorbitol, triethanolamine, and ethoxylated and / or propoxylated triethanolamine.

[0020] Preferably, m+n+p is 2 to 8, more preferably 3 to 6, for example 3, 4, 5 or 6. Preferably, m is 1 to 6, more preferably 1 to 4, for example 1, 2, 3 or 4. Preferably, n is 1 to 6, more preferably 1 to 4, for example 1, 2, 3 or 4. Preferably, p is 0 to 6, more preferably 0 to 3, for example 0, 1, 2 or 3. When p is not 0, the compound of formula (I) has a free alcohol group.

[0021] When R1 is aryl or heteroaryl substituted with two or more substituents, the substituents may be the same or different. Preferably, R1 is aryl, more preferably phenyl unsubstituted or substituted with C1-C20 alkyl.

[0022] Preferably, R1 is selected from phenyl, trimethylphenyl, halophenyl, preferably fluorophenyl, biphenyl, coumarin-3-yl, naphthyl and thiophenyl.

[0023] According to one embodiment, R1 is an unsubstituted coumarin or benzocoumarin.

[0024] According to another preferred embodiment, R1 is selected from substituted or unsubstituted phenyl, preferably trimethylphenyl, fluorophenyl, biphenyl, and halophenyl, such as coumarin-3-yl. - Z is (i) and X is S or O, or - Z is (ii), Y is O and X is dimethylmethylene; or Z is (iii) and X is methylene.

[0025] Mixtures of compounds of formula (I) are also within the scope of the invention, including, but not limited to, mixtures of compounds of formula (I) where p is zero and compounds of formula (I) where p is other than zero, when R2 is a group of formula (II).

[0026] According to a preferred embodiment, Z is (i) and X is S or O, preferably S. When X is S, the oxidized forms of sulfur to sulfone or sulfoxide are also included in the scope of protection of the present invention.

[0027] According to another preferred embodiment of the present invention, n is 1 to 4, more preferably 1 to 3, for example 1, 2 or 3. R2 is a group of formula (II). p is 0 to 3, more preferably 0 to 2, for example, 0, 1 or 2. m is 1 to 6, more preferably 2 to 4, for example 2, 3 or 4. m+n+p is an integer of 2 to 6, more preferably 3 to 5, for example 3, 4 or 5.

[0028] According to an embodiment, referred to herein as embodiment (1), Z is (i), R2 is a group of formula (II), and the other variables are as defined above.

[0029] According to a preferred embodiment (1), G-(OH) m+n+pis an ethoxylated and / or propoxylated monomeric or oligomeric polyol.

[0030] According to a preferred embodiment (1), n ​​is 1 to 4, more preferably 1 to 3, for example 1, 2 or 3; R2 is a group of formula (II); p is 0 to 3, more preferably 0 to 2, for example 0, 1 or 2; m is 1 to 6, more preferably 2 to 4, for example 2, 3 or 4; and m+n+p is 2 to 6, more preferably 3 to 5, for example 3, 4 or 5.

[0031] According to a preferred embodiment (1), R1 is aryl, more preferably phenyl unsubstituted or substituted with C1-C20 alkyl.

[0032] According to an embodiment, herein referred to as embodiment (2), Z is (ii), R2 is a group of formula (II), and the other variables are as defined above.

[0033] According to a further preferred embodiment (2), X is O and Y is C(R4)(R5), where R4 and R5 are C1-C12 alkyl.

[0034] According to a preferred embodiment (2), G-(OH) m+n+p is an ethoxylated and / or propoxylated monomeric or oligomeric polyol.

[0035] According to a preferred embodiment (2), n is 1 to 4, more preferably 1 to 3, for example 1, 2 or 3; R2 is a group of formula (II); p is 0 to 3, more preferably 0 to 2, for example 0, 1 or 2; m is 1 to 6, more preferably 2 to 4, for example 2, 3 or 4; and m+n+p is 2 to 6, more preferably 3 to 5, for example 3, 4 or 5.

[0036] According to a preferred embodiment (2), R1 is aryl, more preferably phenyl unsubstituted or substituted with C1-C20 alkyl.

[0037] According to an embodiment, herein referred to as embodiment (3), Z is (iii), R2 is a group of formula (II), and the other variables are as defined above.

[0038] According to a further preferred embodiment (3), X is O or S.

[0039] According to a preferred embodiment (3), G-(OH) m+n+p is an ethoxylated and / or propoxylated monomeric or oligomeric polyol.

[0040] According to a preferred embodiment (3), n is 1 to 4, more preferably 1 to 3, for example 1, 2 or 3; R2 is a group of formula (II); p is 0 to 3, more preferably 0 to 2, for example 0, 1 or 2; m is 1 to 6, more preferably 2 to 4, for example 2, 3 or 4; and m+n+p is 2 to 6, more preferably 3 to 5, for example 3, 4 or 5.

[0041] According to a preferred embodiment (3), R1 is aryl, more preferably phenyl unsubstituted or substituted with C1-C20 alkyl.

[0042] If possible, within each of the embodiments (1) to (3), all preferred embodiments can be combined.

[0043] As used herein, the term "alkyl" or "alkyl group", unless otherwise indicated, means a straight or branched saturated alkyl chain containing the specified number of carbon atoms, including all possible isomers for each number of carbon atoms in the alkyl group, i.e., n-propyl and isopropyl for three carbon atoms, n-butyl, isobutyl, and tert-butyl for four carbon atoms, n-pentyl, 1,1-dimethyl-propyl, 2,2-dimethylpropyl, and 2-methyl-butyl, etc. for five carbon atoms.

[0044] "Alkenyl" or "alkenyl group" means an unsaturated group containing 2 to 12 carbon atoms, preferably C3 to C12 carbon atoms, for example, allyl, methallyl, or undecenyl.

[0045] The term "cycloalkyl" or "cycloalkyl group", unless otherwise specified, means an aliphatic ring preferably containing 5 or 6 carbon atoms, for example, cyclopentyl or cyclohexyl.

[0046] The term "aryl" or "aryl group" includes, but is not limited to, substituted or unsubstituted phenyl, substituted or unsubstituted naphthyl, anthracenyl, indenyl, fluorenyl, gem-dialkylfluorenyl, phenanthracenyl groups, preferably substituted or unsubstituted phenyl, substituted or unsubstituted naphthyl, or substituted or unsubstituted phenanthracenyl groups, more preferably phenyl.

[0047] The term "heteroaryl" or "heteroaryl group" includes, but is not limited to, furan, thiophene, pyrrole, N-substituted pyrrole, oxazole, isoxazole, thiazole, isothiazole, imidazole, pyrazole, pyran, pyridine, pyrrolidine, indole, N-substituted indole, dibenzofuran, benzocarbazole, quinoline, isoquinoline, coumarin, etc. Preferably, heteroaryl is substituted or unsubstituted furan, thiophene, pyrrole coumarin and benzocoumarin, each of which is unsubstituted or substituted, preferably substituted or unsubstituted coumarin.

[0048] Coumarin has the formula: [ka] It is attached to the rest of the molecule at position 3, as indicated by the asterisk.

[0049] Benzocoumarin has the formula: [ka] [ka] [ka] It is attached to the rest of the molecule at position 3, as indicated by the asterisk.

[0050] When a group is defined as substituted, unless otherwise defined, the term "substituted" as used herein means that the group has one or more substituents, which are preferably selected from halogen atoms, alkyl, aryl, cycloalkyl, alkoxy, aryloxy, alkylamino, dialkylamino, alkylthio or arylthio, heterocyclic groups, and phosphorus- or silicon-containing groups. More preferably, the term "substituted" as used herein denotes one or more groups selected from methyl, ethyl, isopropyl, tert-butyl, phenyl, trifluoromethyl, cyano, acetyl, ethoxycarbonyl, carboxyl, carboxylate, amino, methylamino, dimethylamino, ethylamino, diethylamino, isopropylamino, diisopropylamino, cyclohexylamino, dicyclohexylamino, acetylamino, piperidino, pyrrolidyl, methoxy, ethoxy, propoxy, isopropoxy, butoxy, pentyloxy, phenoxy, hydroxyl, acetoxy, -POH, methylthio, ethylthio, i-propylthio, n-propylthio, phenylthio, mercapto, acetylthio, thiocyano, methylsulfinyl, methylsulfonyl, dimethylsulfonyl, sulfonate group, fluorine atom, chlorine atom, bromine atom, iodine atom, trimethylsilyl, pentamethyldisilyl, triethylsilyl, trimethylstannyl, furyl, thienyl, pyridyl, and morpholino.

[0051] According to one embodiment, when Z is (iii) and X is C(R4)(R5), R1 is a heteroaryl selected from optionally substituted coumarin or benzocoumarin.

[0052] The compounds of the present invention can be prepared according to any suitable method, for example, they can be prepared by double Friedel-Crafts acylation and optionally transesterification according to Scheme 1 below. Scheme 1 [ka]

[0053] According to a preferred embodiment, the compound of formula (I) is the reaction product of: [ka] Here, A is OH or a halogen atom, preferably chlorine.

[0054] In another aspect, the present invention relates to a process for the preparation of compounds of formula (I) comprising Friedel-Crafts acylation of Z group (i), (ii) or (iii) and, optionally, transesterification according to Scheme 1 above.

[0055] The chemical reactions of Scheme 1 can be fully carried out by those skilled in the art according to known methods.

[0056] Details of the method of the invention are reported in the experimental section herein.

[0057] Preferred PIs according to the present invention are as follows: TIFF2024537185000012.tif220144 TIFF2024537185000013.tif148142

[0058] Throughout this specification, the letters (a), (a'), (a"), (a'") and subsequent letters represent the number of ethoxy units, each independently ranging from 0 to 15, more preferably 1 to 8.

[0059] According to another aspect, the present invention relates to a photopolymerizable composition comprising: a) 50 to 99.9% by weight, preferably 70 to 98.9% by weight (based on the total weight of the composition) of at least one ethylenically unsaturated compound, b) 0.1 to 35% by mass, preferably 0.1 to 20% by mass, more preferably 0.2 to 15% by mass (based on the total mass of the composition) of at least one compound of formula (I) above, and c) 0 to 20% by mass, preferably 0 to 15% by mass, more preferably 0.2 to 15% by mass of an accelerator and / or coinitiator (based on the total mass of the composition).

[0060] According to the present invention, the terms "photocuring" and "photopolymerization" and related terms are synonymous.

[0061] The expression "based on the total weight of the composition" means that the % weight of each component is calculated with respect to the total weight of the components of the composition, including the above components a), b), and c) plus any further additional components, and water and / or solvents that may be present in the composition are not taken into account for the calculation of said % weight.

[0062] According to another aspect, the present invention relates to a method for photocuring photopolymerizable composition coatings, adhesives and inks, the method comprising: i) providing a coating of a photopolymerizable composition; i providing the photopolymerizable composition; ii. coating or printing the photopolymerizable composition onto a substrate; and iii. photocuring said coated or printed composition on said substrate with a light source.

[0063] According to another aspect, the present invention relates to a three-dimensional printing method comprising photocuring a mixture comprising the above-described photopolymerizable composition with a light source.

[0064] According to another aspect, the present invention relates to a product obtainable by the process of the present invention.

[0065] The photocurable compositions of the present invention may also comprise, in addition to the compounds a), b) and, if present, c), one or more of the following components: d) photosensitizers, and / or e) further photoinitiators, and / or f) general additives.

[0066] According to a preferred embodiment, the photopolymerizable composition used in the method of the present invention comprises at least components a), b), c), more preferably at least a), b), c), and d) above.

[0067] The photoinitiators of the present invention are used in photocurable compositions comprising ethylenically unsaturated compounds a), which may contain one or more olefinic double bonds. These may be low molecular weight (monomeric) or high molecular weight (oligomeric) compounds.

[0068] Examples of suitable low molecular weight monomers (monomeric compounds) with one double bond are alkyl or hydroxyalkyl acrylates or methacrylates, such as methyl-, ethyl-, butyl-, 2-ethylhexyl-, 2-hydroxyethyl-, or isobornyl-acrylate, and methyl or ethyl methacrylate. Further examples are silicon- or fluorine-modified resins, such as silicone acrylates. Further examples of these monomers are acrylonitrile, acrylamide, methacrylamide, N-substituted (meth)acrylamides, styrene, alkylstyrenes, and halogenostyrenes, vinyl esters such as vinyl acetate, vinyl ethers such as isobutyl vinyl ether, N-vinylpyrrolidone, vinyl chloride, or vinylidene chloride.

[0069] Examples of monomers having two or more double bonds are ethylene glycol diacrylate, propylene glycol diacrylate, neopentyl glycol diacrylate, hexamethylene glycol diacrylate, bisphenol A diacrylate, 4,4'-bis-(2-acryloyloxyethoxy)-diphenylpropane, trimethylolpropane triacrylate, pentaerythritol triacrylate or tetraacrylate, vinyl acrylate, divinylbenzene, divinyl succinate, diallyl phthalate, triallyl phthalate, triallyl phosphate, triallyl isocyanurate, or tris-(2-acryloylethyl)isocyanurate.

[0070] Examples of polyunsaturated compounds of high molecular weight (oligomeric) are acrylated epoxy resins, acrylated polyesters or vinyl-ether or epoxy-group-containing polyesters, acrylated polyurethanes, or acrylated polyethers. Further examples of unsaturated oligomers are unsaturated polyester resins, usually prepared from maleic acid, phthalic acid, and one or more diols, and having a molecular weight of about 500 to 3000 Da. Such unsaturated oligomers are also called prepolymers.

[0071] Examples of compounds a) which are particularly suitable for carrying out the invention are esters of ethylenically unsaturated carboxylic acids with polyols or polyepoxides, and polymers which contain in-chain or in side groups ethylenically unsaturated groups, such as unsaturated polyesters, polyamides and polyurethanes and their copolymers, alkyl resins, polybutadienes and butadiene copolymers, polyisoprene and isoprene copolymers, polymers and copolymers which have (meth)acrylic groups in the side chain, and mixtures thereof.

[0072] Illustrative of unsaturated carboxylic acids or anhydrides useful in preparing such esters are acrylic acid, methacrylic acid, maleic anhydride, crotonic acid, itaconic acid, cinnamic acid, and unsaturated fatty acids such as linoleic acid and oleic acid. Acrylic acid and methacrylic acid are preferred.

[0073] Examples of polyols to be esterified are aromatic polyols and aliphatic and cycloaliphatic polyols, preferably aliphatic and cycloaliphatic polyols.

[0074] Aromatic polyols are, for example, hydroquinone, 4,4'-dihydroxydiphenyl, 2,2-di(4-hydroxyphenyl)propane, as well as novolaks and resols. The polyepoxides to be esterified are based on the above polyols, and in particular include the reaction products between aromatic polyols and epichlorohydrin. Polymers and copolymers containing hydroxyl groups in the polymer chain or in the side groups, such as polyvinyl alcohol and its copolymers, or polymethacrylic acid hydroxyalkyl esters or its copolymers, are also suitable as polyols. Further suitable polyols are oligoesters with hydroxy end groups.

[0075] Examples of aliphatic and cycloaliphatic polyols include alkylene diols preferably containing 2 to 12 carbon atoms, such as ethylene glycol, 1,2- or 1,3-propanediol, 1,2-, 1,3- or 1,4-butanediol, pentanediol, hexanediol, octanediol, dodecanediol, diethylene glycol, triethylene glycol, polyethylene glycols preferably having a molecular weight of 200 to 1500 Da, 1,3-cyclopentanediol, 1,2-, 1,3- or 1,4-cyclohexanediol, 1,4-dihydroxymethylcyclohexane, glycerol, tris(β-hydroxyethyl)amine, trimethylolethane, trimethylolpropane, pentaerythritol, dipentaerythritol and sorbitol.

[0076] Further suitable ethylenically unsaturated compounds a) are unsaturated polyamides obtained from unsaturated carboxylic acids, preferably having 2 to 6, preferably 2 to 4, amino groups, and aromatic, aliphatic and cycloaliphatic polyamines. Examples of such polyamines are ethylenediamine, 1,2- or 1,3-propylenediamine, 1,2-, 1,3- or 1,4-butylenediamine, 1,5-pentylenediamine, 1,6-hexylenediamine, octylenediamine, dodecylenediamine, 1,4-diaminocyclohexane, isophoronediamine, phenylenediamine, bisphenylenediamine, di-(β-aminoethyl)ether, diethylenetriamine, triethylenetetramine and di(β-aminoethoxy)- and di(β-aminopropoxy)ethane. Other suitable polyamines are polymers and copolymers which may contain additional amino groups in the side chain and oligoamides containing amino end groups.

[0077] Specific examples of such unsaturated polyamides are methylenebisacrylamide, 1,6-hexamethylenebisacrylamide, diethylenetriaminetrismethacrylamide, bis(methacrylamidopropoxy)ethane, and N-[(β-hydroxyethoxy)ethyl]-acrylamide.

[0078] Unsaturated polyurethanes, such as those derived from saturated or unsaturated diisocyanates and unsaturated or saturated diols, are also suitable as component a) in the practice of the invention. Polybutadiene and polyisoprene and their copolymers can also be used.

[0079] Suitable monomers include, for example, olefins such as ethylene, propene, butene and hexene, (meth)acrylates, acrylonitrile, styrene, and vinyl chloride.

[0080] Polymers having unsaturated (meth)acrylate groups in the side chain are also used as component a), typically the reaction products of novolac epoxy resins and (meth)acrylic acid, homopolymers or copolymers of vinyl alcohol or its hydroxyalkyl derivatives esterified with (meth)acrylic acid, and homopolymers and copolymers of (meth)acrylates esterified with hydroxyalkyl (meth)acrylates.

[0081] According to a preferred embodiment, the photocurable composition further comprises a coinitiator c), also called an accelerator.

[0082] Suitable examples of accelerators / co-initiators c) are alcohols, thiols, thioethers, amines or ethers with an available hydrogen attached to the carbon adjacent to the heteroatom, disulfides and phosphines, as described, for example, in EP 438123 and GB 2180358.

[0083] Suitable examples of amine accelerators / co-initiators include, but are not limited to, aliphatic, cycloaliphatic, aromatic, arylaliphatic, heterocyclic, oligomeric or polymeric amines, including primary, secondary or tertiary amines such as butylamine, dibutylamine, tributylamine, cyclohexylamine, benzyldimethylamine, dicyclohexylamine, N-phenylglycine, triethylamine, phenyldiethanolamine, triethanolamine, piperidine, piperazine, morpholine, pyridine, quinoline, esters of dimethylaminobenzoic acid, Michler's ketone (4,4'-bis-dimethylaminobenzophenone) and corresponding derivatives.

[0084] As amine accelerators / co-initiators, amine-modified acrylate compounds are used, examples of such amine-modified acrylates include acrylates modified by reaction with primary or secondary amines (as described in US 3844916, EP 280222, US 5482649, or US 5734002).

[0085] Multifunctional amines and polymeric amine derivatives are also suitable as coinitiators, some examples being Omnipol®, ASA (IGM Resins BV), Genopol®, AB-2 (Rahn AG), Speedcure® 7040 (Lambson Limited), or those described in US 2013 / 0012611.

[0086] The photocurable compositions of the present invention may also be formulated as compositions that further include water and / or a solvent, such as an organic solvent.

[0087] The photosensitizer d) can be present in an amount of 0.01 to 15% by weight, preferably 0.01 to 10% by weight, based on the total weight of the composition.

[0088] Examples of photosensitizers are those commonly used in the art: aromatic carbonyl compounds, such as benzophenones, thioxanthones, anthraquinones, coumarins, and 3-acylcumarine derivatives, terphenyls, styryl ketones, and 3-(aroylmethylene)-thiazolines, camphorquinones, and eosin, rhodamine, erythrosine dyes.

[0089] Examples of thioxanthone include thioxanthone, 2-isopropylthioxanthone, 2-chlorothioxanthone, 2-dodecylthioxanthone, 2,4-diethylthioxanthone, 2,4-dimethylthioxanthone, 1-methoxycarbonylthioxanthone, 2-ethoxycarbonylthioxanthone, 3-(2-methoxyethoxycarbonyl)thioxanthone, 4-butoxycarbonylthioxanthone, 3-butoxycarbonyl-7-methylthioxanthone, 1-cyano-3-chlorothioxanthone, thioxanthone, 1-ethoxycarbonyl-3-chlorothioxanthone, 1-ethoxycarbonyl-3-ethoxythioxanthone, 1-ethoxycarbonyl-3-aminothioxanthone, 1-ethoxycarbonyl-3-phenylsulfurylthioxanthone, 3,4-di[2-(2-methoxyethoxy)ethoxycarbonyl]thioxanthone, 1-ethoxycarbonyl-3-(1-methyl-1-morpholinoethyl)thioxanthone, 2-methyl-6-dimethoxymethylthioxanthone, 2-methyl -6-(1,1-dimethoxybenzyl)thioxanthone, 2-morpholinomethylthioxanthone, 2-methyl-6-morpholinomethylthioxanthone, N-allylthioxanthone-3,4-dicarboximide, N-octylthioxanthone-3,4-dicarboximide, N-(1,1,3,3-tetramethylbutyl)-thioxanthone-3,4-dicarboximide, 1-phenoxythioxanthone, 6-ethoxycarbonyl-1-2-methoxythioxanthone, 6-ethoxycarbyl-1-2-methoxythioxanthone, Bornyl-2-methylthioxanthone, thioxanthone-2-polyethylene glycol ester, 2-hydroxy-3-(3,4-dimethyl-9-oxo-9H-thioxanthone-2-yloxy)-N,N,N-trimethyl-1-propanaminium chloride, or those described in PCT / EP2011 / 069514, such as n-dodecyl-7-methyl-thioxanthone-3-carboxylate and N,N-diisobutyl-7-methyl-thioxanthone-3-carbamide. Polymeric thioxanthone derivatives, such as Omnipol® TX (IGM Resins BV), Genopol® TX-1 (Rahn AG), Speedcure® 7010 (Lambson Limited), are also suitable.

[0090] Examples of benzophenones are benzophenone, 4-phenylbenzophenone, 4-methoxybenzophenone, 4,4'-dimethoxybenzophenone, 4,4'-dimethylbenzophenone, 4,4'-dichlorobenzophenone, 4,4'-dimethylaminobenzophenone, 4,4'-diethylaminobenzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-(4-methylthiophenyl)benzophenone, 3,3'-dimethyl-4-methoxybenzophenone, methyl 2-benzoylbenzoate, 4-(2-hydroxybenzoyl)benzoate, methyl 4-benzoylbenzoate, methyl 5-(2-hydroxybenzoyl)benzoate, methyl 6-(2-hydroxybenzoyl)benzoate, methyl 7-(2-hydroxybenzoyl)benzoate, methyl 8-(2-hydroxybenzoyl)benzoate, methyl 9-(2-hydroxybenzoyl)benzoate, methyl 10-(2-hydroxybenzoyl)benzoate, methyl 11-(2-hydroxybenzoyl)benzoate, methyl 12-(2-hydroxybenzoyl)benzoate, methyl 13-(2-hydroxybenzoyl)benzoate, methyl 14-(2-hydroxybenzoyl)benzoate, methyl 15-(2-hydroxybenzoyl)benzoate, methyl 16-(2-hydroxybenzoyl)benzoate, methyl 17-(2-hydroxybenzoyl)benzoate, methyl 18-(2-hydroxybenzoyl)benzoate, methyl 19 ... hydroxyethylthio)benzophenone, 4-(4-tolylthio)benzophenone, 4-benzoyl-N,N,N-trimethylbenzenemethanaminium chloride, 2-hydroxy-3-(4-benzoylphenoxy)-N,N,N-trimethyl-1-propanaminium chloride 11 monohydrate, 4-(13-acryloyl-1,4,7,10,13-pentaoxatridecyl)benzophenone, 4-benzoyl-N,N-dimethyl-N-[2-(1-oxo-2-propenyl)oxyethyl-benzenemethanaminium chloride, or those described in US 9938231 (e.g. Omnirad® 991 (IGM Resins BV)).

[0091] Polymeric benzophenone derivatives (e.g., Omnipol® BP, Omnipol® 2702 and Omnipol® 682 (all from IGM Resins BV), Genopol® BP-2 (Rahn AG), and Speedcure® 7005 (Lambson Limited)) are also suitable.

[0092] Examples of 3-acylcoumarin derivatives are 3-benzoylcoumarin, 3-benzoyl-7-methoxycoumarin, 3-benzoyl-5,7-di(propoxy)coumarin, 3-benzoyl-6,8-dichlorocoumarin, 3-benzoyl-6-chlorocoumarin, 3,3'-carbonyl-bis[5,7-di(propoxy)coumarin], 3,3'-carbonyl-bis(7-methoxycoumarin), 3,3'-carbonyl-bis(7-diethylaminocoumarin), 3-isobutyroylcoumarin, 3-benzoyl-5,7-dimethoxycoumarin, 3-benzoyl-5,7-diethoxycoumarin, 3-benzoyl- coumarin, 5,7-dibutoxycoumarin, 3-benzoyl-5,7-di(methoxyethoxy)coumarin, 3-benzoyl-5,7-di(allyloxy)coumarin, 3-benzoyl-7-dimethylaminocoumarin, 3-benzoyl-7-diethylaminocoumarin, 3-isobutyroyl-1,7-dimethylaminocoumarin, 5,7-dimethoxy-3-(1-benzoyl)coumarin, 5,7-dimethoxy-3-(1-benzoyl)-coumarin, 3-benzoylbenzo[f]coumarin, 7-diethylamino-3-thienoylcoumarin, 3-(4-cyanobenzoyl)-5,7-dimethoxycoumarin, or those described in EP 2909243 and WO 2017 / 216699.

[0093] Examples of 3-(aroylmethylene)thiazolines are 3-methyl-1,2-benzoylmethylene-β-benzothiazoline, 3-methyl-2-benzoylmethylene-benzothiazoline, 3-ethyl-2-propionylmethylene-β-benzothiazoline.

[0094] Examples of other aromatic carbonyl compounds are acetophenone, 3-methoxyacetophenone, 4-phenylacetophenone, benzil (for example those described in WO 2013 / 164394), 2-acetylnaphthalene, 2-naphthaldehyde, 9,10-anthraquinone, 9-fluorenone, dibenzosuberone, xanthone, 2,5-bis(4-diethylaminobenzylidene)cyclopentanone, α-(p-dimethylaminobenzylidene), ketones such as 2-(4-dimethylamino-benzylidene)-indan-1-one or 3-(4-dimethylaminophenyl)-1-indan-5-yl-propenone, 3-phenylthiophthalimide, N-methyl-3,5-di(ethylthio)phthalimide.

[0095] Thioxanthones, coumarins, and 3-acylumarins are particularly preferred.

[0096] It has been observed that the above component d) increases the reactivity of the photoinitiator b) without shortening the shelf life of the composition. Moreover, such a composition has the special advantage that the spectral sensitivity of the photoinitiator b) can be shifted to various desired wavelength ranges by appropriately selecting the photosensitizer d). Those skilled in the art can select a suitable photosensitizer d) to make the photoinitiator b) function in various desired wavelength ranges.

[0097] Further possible photoinitiators e) can be present in an amount of 0.5 to 15% by weight, preferably 1 to 10% by weight, of the composition, based on the total weight of the composition.

[0098] Examples of other suitable photoinitiators e) are camphorquinone, benzophenone, benzophenone derivatives, acetophenone, acetophenone derivatives, dialkoxyacetophenones, α-hydroxyketones, α-aminoketones, 4-aroyl-1,3-dioxolanes, benzoin alkyl ethers and benzil ketals, for example benzil dimethyl ketal, ketosulfones, for example 1-[4-[(4-benzoyl-phenyl)-thio]-phenyl]-2-methyl-2-[(4-methyl-phenyl)-sulfonyl]-propan-1-one (Esacure® 1001 (IGM Resins BV)), 3-ketocoumarins, for example those described in EP 2909243 and WO 2017 / 216699, phenylglyoxylates and derivatives thereof, dimeric phenylglyoxylates, peresters, for example benzophenonetetracarboxylic acid peresters, for example EP 126541, acylphosphine photoinitiators (selected from among mono-acylphosphine oxides, bis-acylphosphine oxides, tris-acylphosphine oxides, and polyfunctional mono- or bis-acylphosphine oxides), halomethyltriazines, hexaarylbisimidazole / co-initiator systems such as ortho-chlorohexaphenylbisimidazole in combination with 2-mercaptobenzothiazole, ferrocenium compounds or titanocenes such as dicyclopentadienyl-bis(2,6-difluoro-3-pyrrolo-phenyl)titanium, O-acyloxime ester photoinitiators.

[0099] Examples of α-hydroxyketones and α-aminoketones are 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, 2-hydroxy-1- {4-[4-(2-hydroxy-2-methyl-propionyl)-phenoxy]-phenyl}-2-methyl-propan-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone.

[0100] Examples of O-acyloxime ester photoinitiators are 1,2-octanedione, 1-[4-(phenylthio)phenyl]-2-(O-benzoyloxime), ethanone 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]1-(O-acetyloxime), or those described in GB 2339571.

[0101] Examples of acylphosphine photoinitiators include, but are not limited to, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-(2,4-dipentyloxyphenyl), 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and ethyl(2,4,6-trimethylbenzoyl)phenylphosphinate, phenyl(2,4,6-trimethylbenzoyl)phosphinic acid, glycerol ethoxylated trimester (Omnipol® TP (IGM Resins BV)).

[0102] Examples of halomethyltriazine photoinitiators are 2-[2-(4-methoxy-phenyl)-vinyl]-4,6-bis-trichloromethyl[1,3,5]triazine, 2-(4-methoxy-phenyl)-4,6-bis-trichloromethyl[1,3,5]triazine, 2-(3,4-dimethoxyphenyl)-4,6-bis-trichloromethyl[1,3,5]triazine, 2-methyl-4,6-bis-trichloromethyl[1,3,5]triazine.

[0103] If the photocurable composition according to the invention is used in a hybrid system (hybrid system in this context means a mixture of a free radically curable system and a cationic curable system), cationic photoinitiators can also be used as further photoinitiators e). Examples of suitable cationic photoinitiators are aromatic sulfonium, phosphonium or iodonium salts, as described in US 4950581, or cyclopentadienylarenes-iron(II) complex salts, such as (η 6 -isopropylbenzene)(η 5 -cyclopentadienyl)iron(II) hexafluorophosphate or an oxime-based photolatent acid.

[0104] The photocurable composition according to the invention may also contain common additives in an amount of 0-10%, based on the total weight of the composition. Additives f) are, for example, thermal initiators, binders, stabilizers, and mixtures thereof.

[0105] The choice of additives is determined based on the field of use in question and the properties desired for that field of use. The above additives f) are known in the art and are used in amounts commonly used in the art.

[0106] For example, in particular in the case of pigmented compositions, the composition may also comprise as additional additive f) thermal initiators (compounds which form free radicals when heated), for example azo compounds such as 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), triazenes, diazosulfides, pentazadienes, or peroxy compounds, for example hydroperoxides or peroxycarbonates, for example tert-butyl hydroperoxide (described for example in EP 245639).

[0107] A binder may also be added to the photocurable composition of the present invention. The addition of a binder is particularly advantageous when the photocurable compound is a liquid or viscous substance. The amount of binder may be, for example, 5 to 60% by weight, preferably 10 to 50% by weight, based on the total weight of the composition (excluding water and solvent). The binder is selected according to the field of use and the required properties, such as developability in aqueous and organic solvent systems, adhesion to substrates, and sensitivity to oxygen.

[0108] A suitable binder is, for example, a polymer having a weight average molecular weight (Mw) of about 5,000 to 2,000,000 Da, preferably 10,000 to 1,000,000 Da. Illustrative examples are homopolymers and copolymers of acrylates and methacrylates, such as methyl methacrylate / ethyl acrylate / methacrylic acid copolymers, poly(methacrylic acid alkyl esters), poly(acrylic acid alkyl esters), cellulose esters and ethers, such as cellulose acetate, cellulose acetate butyrate, methyl cellulose, ethyl cellulose, polyvinyl butyral, polyvinyl formal, cyclized rubbers, polyethers, such as polyethylene oxide, polypropylene oxide, polytetrahydrofuran, polystyrene, polycarbonate, polyurethanes, chlorinated polyolefins, such as polyvinyl chloride, vinyl chloride / vinylidene chloride copolymers, vinylidene chloride and acrylonitrile, copolymers of methyl methacrylate and vinyl acetate, polyvinyl acetate, co-poly(ethylene / vinyl acetate), polymers such as polycaprolactam and poly(hexamethylene adipamide), polyesters, such as poly(ethylene glycol terephthalate) and poly(hexamethylene glycol succinate).

[0109] Suitable stabilizers are, for example, thermal inhibitors, such as hydroquinone, hydroquinone derivatives, p-methoxyphenol, β-benzoyl, or sterically hindered phenols, such as 2,6-di(tert-butyl)-p-cresol, which prevent premature polymerization. To increase the dark storage stability, for example, copper compounds, such as copper naphthenate, copper stearate, or copper octenate, phosphorus compounds, such as triphenylphosphine, tributylphosphine, triethyl phosphite, triphenyl phosphite, or tribenzyl phosphite, quaternary ammonium compounds, such as tetramethylammonium chloride or trimethylbenzylammonium chloride, or hydroxylamine derivatives, such as N,N-diethylhydroxylamine, can be used. To remove oxygen from the atmosphere during polymerization, paraffin or similar wax-like substances can be used, which are insoluble in the polymer and migrate to the surface at the beginning of the polymerization, forming a transparent surface layer that prevents air from entering.

[0110] Light stabilizers such as UV absorbers, for example of the hydroxyphenylbenzotriazole, hydroxyphenylbenzophenone, oxalic acid amide or hydroxyphenyl-s-triazine type, can also be used. Such compounds can be used alone or in mixtures, with or without the use of sterically hindered amines (HALS).

[0111] The photocurable compositions according to the invention can also contain as further additives f) photoreducible dyes, such as xanthene, benzoxanthene, benzothioxanthene, thiazine, pyronine, porphyrin or acridine dyes, and / or radiation-cleavable trihalomethyl compounds, which are described, for example, in EP 445624.

[0112] Further customary additives f) are, depending on the intended application, optical brighteners, fillers, pigments (both white and colored pigments), colorants, antistatic agents, wetting agents or flow improvers.Additives commonly used in this technical field, such as antistatic agents, flow improvers and adhesion promoters, can also be used.

[0113] In addition to the above ingredients, other ingredients may be present in compositions according to the present invention.

[0114] It is also possible to add chain transfer agents commonly used in the art to the compositions according to the invention, examples being mercaptans, amines and benzothiazoles.

[0115] The composition of the present invention may include colorants and / or colored pigments. Depending on the intended application, both inorganic and organic pigments can be used. Such additives are known to those skilled in the art. Some examples are carbon black, iron oxides, such as yellow iron oxide, red iron oxide, chrome yellow, chrome green, nickel titanium yellow, ultramarine blue, cobalt blue, bismuth vanadate, cadmium yellow, and cadmium red. Examples of organic pigments are mono- or bis-azo pigments and their metal complexes, phthalocyanine pigments, polycyclic pigments, such as perylene, anthraquinone, thioindigo, quinacridone, or triphenylmethane pigments, and diketo-pyrrolo-pyrrole, isoindolinone, such as tetrachloroisoindolinone, isoindoline, dioxazine, benzimidazolone, and quinophthalone pigments. In the formulation, the pigments can be used alone or as mixtures in the formulation.

[0116] Depending on the intended use, pigments can be added to the formulation in amounts commonly used in the art, for example, from 0.1 to 30% by weight, or from 10 to 25% by weight, based on the total weight of the composition.

[0117] The composition may also contain, for example, a wide variety of organic colorants. Examples are azo dyes, methine dyes, anthraquinone dyes, and metal complex dyes. Typical concentrations are, for example, 0.1 to 20% by weight, in particular 1 to 5% by weight, based on the total weight of the composition.

[0118] The photocurable composition of the present invention may contain water.

[0119] The photocurable compositions of the invention can be used for various purposes, for example as printing inks, e.g. screen printing inks, flexographic printing inks, offset printing inks and inkjet printing inks, as clear coats, e.g. as pigmented coats for wood or metal, as powder coatings, in particular as coating materials for paper, wood, metal or plastics, for construction and road markings, for photocopying, for holographic recording materials, for image recording or in the production of printing plates using organic solvents or aqueous alkaline media, as sunlight-curable paints for the production of screen printing masks, as dental filling materials, as adhesives, as pressure-sensitive adhesives, as laminating resins, as photoresists, e.g. galvano-resists, as etch resists or permanent resists (both liquid and dry film), as photostructurable dielectrics and as solder masks for electronic circuits, in the production of color filters for various types of display screens or in the formation of structures during the production of plasma displays and electroluminescent displays, in the production of optical switches, optical gratings (interference gratings), by bulk curing (UV curing in transparent moulds) or in stereolithography methods (e.g. US The present invention is also suitable as a resist in coatings or encapsulations for electronic components or coatings for optical fibers, in the manufacture of three-dimensional articles by the process described in US Pat. No. 4,575,330, in the manufacture of composite materials (e.g., styrene polyesters which may contain glass fibers and / or other fibers and other auxiliaries) and other methods of three-dimensional printing known to those skilled in the art.

[0120] The photocurable compositions according to the invention are also suitable for the manufacture of optical lenses, such as contact lenses or Fresnel lenses, for example, and for the manufacture of medical devices, aids or implants, and also for dry film paints.

[0121] The photocurable compositions of the invention are also suitable for the preparation of gels having thermotropic properties, such as those described, for example, in DE 19700064 and EP 678534.

[0122] Articles comprising the compounds of formula (I) according to the invention or comprising the photocurable compositions according to the invention are further subject matter of the present invention.

[0123] The compounds and compositions according to the invention can also be used as free radical photoinitiators or photoinitiating systems for radiation curable powder coatings.

[0124] The photocurable compositions according to the invention are suitable, for example, as coating materials for all kinds of substrates, such as wood, textiles, paper, ceramics, glass, plastics (e.g. polyesters, polyethylene terephthalate, polyolefins, and cellulose acetate, especially in film form), and metals (e.g. Al, Cu, Ni, Fe, Zn, Mg, or Co), and also GaAs, Si or SiO2 (to which a protective layer is applied or to which an image is exposed, for example by imagewise exposure).

[0125] In the method according to the invention, a large number of light sources of the most diverse types can be used, which emit at wavelengths from about 200 nm to about 800 nm. Both point sources and flat radiators (lamp carpets) are suitable. Examples are carbon arc lamps, xenon arc lamps, medium, high and low pressure mercury arc radiators, optionally doped with metal halides (metal halide lamps), microwave excited metal vapor lamps, excimer lamps, super actinic fluorescent tubes, fluorescent lamps, argon incandescent lamps, flash lamps, photographic floodlight lamps, light emitting diodes (LEDs), electron beams, X-rays and lasers.

[0126] According to one embodiment, the light source includes ultraviolet light in at least one of the UVA, UVB, and UVC ranges.

[0127] According to a preferred embodiment, the light source is an LED light source, with LED light sources emitting light at wavelengths of 365 to 420 nm, more preferably 365 nm, 385 nm, and 395 nm being particularly preferred.

[0128] According to the invention, the distance between the lamp and the substrate to be exposed can vary depending on the intended application, the type and strength of the lamp, and is, for example, from 0.1 to 150 cm, preferably from 1 to 50 cm.

[0129] The photopolymerizable compositions described above can also be applied over a substrate that already contains a coated or printed layer, and after the photopolymerizable composition has been photopolymerized with the light source, it can be overprinted or overcoated with one or more compositions suitable for printing or coating.

[0130] Articles obtained by applying said photopolymerizable composition onto said substrate by said coating or printing means and photopolymerizing by said light source, with or without further finishing of the article by further coating or printing, are further subjects of the present invention.

[0131] As described above, the inventors have surprisingly found that the compound of formula (I) exhibits very high reactivity under UVA, UVB and UVC wavelengths and exhibits low post-cure yellowing compared to the prior art. The novel compound exhibits a significant improvement in surface curability under LED and Hg lamps in both clear and pigmented systems.

[0132] The present invention will now be described in more detail with reference to the following examples, which are illustrative and not limiting.

[0133] Experimental Section Throughout this specification, in the event of a conflict between a chemical name and a chemical formula, the chemical formula shall control.

[0134] The compound of Example 15 is a mixture of compounds obtained by reaction of the indicated starting materials.

[0135] 1 1 H NMR spectra were recorded on a Bruker Ascend 300 MHz NMR spectrometer. Example 1

[0136] Synthesis of the following [ka] To an ice-cooled mixture of 10.00 g (53.686 mmol) diphenyl sulfide and 7.92 g (56.342 mmol) benzoyl chloride in 120 mL dichloromethane was carefully added in portions, 7.87 g (59.022 mmol) anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and 9.53 g (69.802 mmol) ethyl chlorooxoacetate was carefully added followed by 10.88 g (81.596 mmol) anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and an additional 1.47 g (10.767 mmol) ethyl chlorooxoacetate was carefully added followed by 1.65 g (12.374 mmol) anhydrous aluminum chloride. The reaction was then stirred at room temperature for an additional 1.5 hours and poured into 400 mL ice / water. The mixture was extracted with dichloromethane, the organic layer was separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation to give the crude product, which was purified by crystallization from ethanol to give 15.70 g of an off-white solid (75% yield). 1 H-NMR (DMSO-d6, δppm): 1.33 (t, 3H), 4.42 (q, 2H), 7.51 (d, 2H), 7.54~7.74 (m, 5H), 7.76~7.82 (m, 4H), 7.97 (d, 2H). Example 2

[0137] Synthesis of the following [ka] To an ice-cooled mixture of 5.00 g (29.375 mmol) diphenyl ether and 4.33 g (30.803 mmol) benzoyl chloride in 60 mL dichloromethane was carefully added in portions, 4.31 g (32.323 mmol) anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and 5.21 g (38.160 mmol) ethyl chlorooxoacetate was carefully added followed by 5.95 g (44.623 mmol) anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and an additional 0.80 g (5.860 mmol) ethyl chlorooxoacetate was carefully added followed by 0.90 g (6.750 mmol) anhydrous aluminum chloride. The reaction was then stirred at room temperature for an additional 1.5 hours and poured into 200 mL ice / water. The mixture was extracted with dichloromethane, the organic layer was separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give the crude product, which was purified by crystallization from ethanol followed by flash column chromatography on silica gel (toluene / ethyl acetate 98:2) to give 7.97 g of a white solid (72% yield). 1 H-NMR (DMSO-d6, δppm): 1.34 (t, 3H), 4.42 (q, 2H), 7.30 (m, 4H), 7.58 (t, 2H), 7.67 (tt, 1H), 7.75 (dd, 2H), 7.86 (d, 2H), 8.06 (d, 2H). Example 3

[0138] Synthesis of the following [ka] To an ice-cooled mixture of 10.00 g (47.556 mmol) of 9,9-dimethylxanthene and 7.02 g (49.940 mmol) of benzoyl chloride in 120 mL of dichloromethane was carefully added in portions, 6.98 g (52.347 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and 8.44 g (61.818 mmol) of ethyl chlorooxoacetate was carefully added in succession, followed by 9.64 g (72.297 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and an additional 1.30 g (9.522 mmol) of ethyl chlorooxoacetate was carefully added in succession, followed by 1.46 g (10.949 mmol) of anhydrous aluminum chloride. The reaction was then stirred at room temperature for an additional 1.5 hours and poured into 400 mL of ice / water. The mixture was extracted with dichloromethane, the organic layer was separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give the crude product, which was purified by flash column chromatography on silica gel (toluene / ethyl acetate 98:2) to give 16.74 g of a yellow oil (85% yield). 1 H-NMR (DMSO-d6, δppm): 1.33 (t, 3H), 1.64 (s, 6H), 4.43 (q, 2H), 7.26 (d, 1H), 7.31 (d, 1H), 7.54 (t, 2H), 7.62~7.75 (m, 4H), 7.88 (dd, 1H), 7.99 (d, 1H), 8.18 (d, 1H). Example 4

[0139] Synthesis of the following [ka]

[0140] Step a) Synthesis of [ka] To an ice-cooled mixture of 5.00 g (26.843 mmol) of diphenyl sulfide and 2.21 g (28.153 mmol) of acetyl chloride in 50 mL of dichloromethane was carefully added in portions 3.94 g (29.549 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was poured into 200 mL of ice / water. The mixture was extracted with dichloromethane, the organic layer separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give 5.97 g of an off-white solid (97% yield). 1 H-NMR (DMSO-d6, δppm): 2.53 (s, 3H), 7.25 (d, 2H), 7.48 (m, 5H), 7.87 (d, 2H).

[0141] Step b) Synthesis of [ka] 4.73 g (26.268 mmol) of sodium methoxide in 30% w / w methanol solution was slowly added in portions over 10 minutes to a mixture containing 5.00 g (21.900 mmol) of the compound prepared in the previous step and 19.73 g (219.028 mmol) of dimethyl carbonate in 18.4 mL of toluene with stirring at 90° C. The mixture was stirred at 90° C. for 1 hour to remove methanol by distillation. After completion of the reaction, the mixture was allowed to cool, poured into 200 mL of 3M hydrochloric acid, and extracted with ethyl acetate. The organic layer was washed with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give 6.25 g of a yellow oil (100% yield). 1 H-NMR (DMSO-d6, δppm): 3.65 (s, 3H), 4.15 (s, 2H), 7.25 (d, 2H), 7.51 (m, 5H), 7.87 (d, 2H).

[0142] Step c) Synthesis of [ka] 0.178g (2.090mmol) of piperidine was added to a mixture containing 6.00g (20.953mmol) of the compound prepared in the previous step and 2.56g (20.963mmol) of salicylaldehyde in 80mL of ethanol. The mixture was stirred under reflux for 1 hour and then cooled to room temperature. The reaction product was collected by filtration to give 6.63g of a yellow solid (yield 88%). 1 H-NMR (DMSO-d6, δppm): 7.23 (d, 2H), 7.42 (td, 1H), 7.47~7.58 (m, 6H), 7.73 (m, 1H), 7.83~7.88 (m, 3H), 8.40 (s, 1H).

[0143] Step d) Synthesis of [ka] To an ice-cooled mixture of 5.00 g (13.951 mmol) of the compound prepared in the previous step and 2.48 g (18.165 mmol) of ethyl chlorooxoacetate in 100 mL of dichloromethane, 6.55 g (49.123 mmol) of anhydrous aluminum chloride was carefully added in portions. After stirring at room temperature for 1.5 hours, the reaction was poured into 200 mL of ice / water. The mixture was extracted with dichloromethane, the organic layer was separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give the crude product. The crude product was dissolved in 120 mL of ethanol, washed under reflux with vigorous stirring for 30 minutes, and then cooled to room temperature. The reaction product was collected by filtration to give 6.00 g of a canary yellow solid (94% yield). 1 H-NMR (DMSO-d6, δppm): 1.33 (t, 3H), 4.41 (q, 2H), 7.43 (td, 1H), 7.48~7.60 (m, 5H), 7.75 (m, 1H), 7.88 (dd, 1H), 7.95~8.01 (m, 4H), 8.47 (s, 1H). Example 5

[0144] Synthesis of the following [ka] To a warm solution of 5.00 g (10.906 mmol) of the compound of Example 4 and 4.26 g (32.711 mmol) of 2-ethyl-1-hexanol in 40 mL of toluene was added 0.53 g (1.087 mmol) of zirconium(IV) acetylacetonate with stirring. The reaction mixture was stirred at 110° C. for 2 hours to remove ethanol by distillation. The progress of the reaction was monitored by TLC. After completion of the reaction, the mixture was allowed to cool, diluted with ethyl acetate, and washed successively with 50 mL (×2) of 3 M hydrochloric acid, water, and brine, respectively. The organic layer was separated, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to obtain the crude product. The crude product was purified by crystallization from ethanol to obtain 5.09 g of a canary yellow solid (86% yield). 1 H-NMR (DMSO-d6, δppm): 0.85 (m, 6H), 1.32 (m, 8H), 1.66 (m, 1H), 4.30 (d, 2H), 7.41 (td , 1H), 7.48~7.60(m, 5H), 7.75(m, 1H), 7.88(dd, 1H), 7.93~8.00(m, 4H), 8.47(s, 1H). Example 6

[0145] Synthesis of the following [ka]

[0146] Step a) Synthesis of [ka] To an ice-cooled mixture of 5.00 g (30.081 mmol) of fluorene and 2.48 g (31.592 mmol) of acetyl chloride in 50 mL of dichloromethane was carefully added in portions, 4.41 g (33.073 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and an additional 0.118 g (1.503 mmol) of acetyl chloride and 0.240 g (1.800 mmol) of anhydrous aluminum chloride were carefully added in succession. The reaction was then stirred at room temperature for an additional 45 minutes and poured into 200 mL of ice / water. The mixture was extracted with dichloromethane, the organic layer separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give 6.25 g of an off-white solid (100% yield). 1 H-NMR (DMSO-d6, δppm): 2.63 (s, 3H), 4.01 (s, 2H), 7.41 (m, 2H), 7.64 (m, 1H), 8.00 (m, 3H), 8.17 (s, 1H).

[0147] Step b) Synthesis of [ka] 5.19 g (28.823 mmol) of sodium methoxide in 30% w / w methanol solution was slowly added in portions over 10 minutes to a mixture of 5.00 g (24.008 mmol) of the compound from the previous step and 21.63 g (240.120 mmol) of dimethyl carbonate in 20.2 mL of toluene with stirring at 90° C. The mixture was stirred at 90° C. for 1 hour to remove the methanol by distillation. After the reaction was complete, the mixture was allowed to cool, poured into 200 mL of 3M hydrochloric acid, and extracted with ethyl acetate. The organic layer was washed with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give 6.27 g of a yellow oil (98% yield). 1 H-NMR (DMSO-d6, δppm): 3.68 (s, 3H), 4.02 (s, 2H), 4.26 (s, 2H), 7.43 (m, 2H), 7.65 (m, 1H), 8.01 (m, 3H), 8.18 (s, 1H).

[0148] Step c) Synthesis of [ka] 0.192 g (2.255 mmol) of piperidine was added to a mixture of 6.00 g (22.531 mmol) of the compound from the previous step and 2.75 g (22.519 mmol) of salicylaldehyde in 120 mL of ethanol. The mixture was stirred under reflux for 1 hour and then cooled to room temperature. The reaction product was collected by filtration to give 5.96 g of a canary yellow solid (78% yield). 1 H-NMR (DMSO-d6, δppm): 4.02 (s, 2H), 7.40~7.48 (m, 3H), 7.51 (d, 1H), 7.66 (m, 1H), 7.75(m, 1H), 7.88(dd, 1H), 7.99~8.08(m, 3H), 8.18(s, 1H), 8.43(s, 1H).

[0149] Step d) Synthesis of [ka] To an ice-cooled mixture of 5.00 g (14.777 mmol) of the compound from the previous step and 2.62 g (19.190 mmol) of ethyl chlorooxoacetate in 100 mL of dichloromethane was carefully added in portions with 6.94 g (52.047 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and an additional 0.404 g (2.959 mmol) of ethyl chlorooxoacetate and 0.453 g (3.397 mmol) of anhydrous aluminum chloride were carefully added in succession. The reaction was then stirred at room temperature for an additional hour and poured into 200 mL of ice / water. The mixture was extracted with dichloromethane, the organic layer separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give the crude product. This crude product was dissolved in 70 mL of toluene and washed under reflux with vigorous stirring for 30 minutes, then cooled to room temperature. The reaction product was collected by filtration to give 4.66 g of a yellow solid (72% yield). 1H-NMR (DMSO-d6, δppm): 1.37 (t, 3H), 4.15 (s, 2H), 4.48 (q, 2H), 7.45 (td, 1H), 7.5 3(d, 1H), 7.75(m, 1H), 7.88(dd, 1H), 8.05(m, 2H), 8.21~8.29(m, 4H), 8.47(s, 1H). Example 7

[0150] Synthesis of the following [ka] 0.501 g (1.027 mmol) of zirconium(IV) acetylacetonate was added to a warm solution of 4.50 g (10.264 mmol) of the compound of Example 6 and 4.01 g (30.792 mmol) of 2-ethyl-1-hexanol in 35 mL of toluene with stirring. The reaction mixture was stirred at 110° C. for 2.5 hours to remove ethanol by distillation. The progress of the reaction was monitored by TLC. After completion of the reaction, the mixture was allowed to cool, diluted with dichloromethane, washed with 50 mL (×2) of 3 M hydrochloric acid, water, and brine, respectively. The organic layer was separated, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to obtain the crude product. The crude product was dissolved in 100 mL of ethanol, washed under reflux with vigorous stirring for 30 minutes, and then cooled to room temperature. The reaction product was collected by filtration to obtain 4.45 g of a yellow solid (83% yield). 1 H-NMR (DMSO-d6, δppm): 0.88 (m, 6H), 1.33 (m, 8H), 1.70 (m, 1H), 4.15 (s, 2H), 4.37 (d, 2H), 7.45 ( td, 1H), 7.53(d, 1H), 7.75(m, 1H), 7.88(dd, 1H), 8.05(td, 2H), 8.22~8.30(m, 4H), 8.47(s, 1H). Example 8

[0151] Synthesis of the following [ka]

[0152] Step a) Synthesis of [ka] To an ice-cooled mixture of 5.00 g (29.375 mmol) diphenyl ether and 2.42 g (30.828 mmol) acetyl chloride in 50 mL dichloromethane was carefully added in portions 4.31 g (32.323 mmol) anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was poured into 200 mL ice / water. The mixture was extracted with dichloromethane, the organic layer separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give 6.12 g of a white solid (98% yield). 1 H-NMR (DMSO-d6, δppm): 2.55 (s, 3H), 7.05 (d, 2H), 7.12 (d, 2H), 7.25 (t, 1H), 7.47 (t, 2H), 7.99 (d, 2H).

[0153] Step b) Synthesis of [ka] 5.09 g (28.267 mmol) of sodium methoxide in 30% w / w methanol solution was added slowly in portions over 10 minutes to a mixture of 5.00 g (23.557 mmol) of the compound from the previous step and 21.22 g (235.568 mmol) of dimethyl carbonate in 19.8 mL of toluene with stirring at 90° C. The mixture was stirred at 90° C. for 1 hour to remove the methanol by distillation. After the reaction was complete, the mixture was allowed to cool, poured into 200 mL of 3M hydrochloric acid, and extracted with ethyl acetate. The organic layer was washed with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give 6.34 g of a yellow oil (100% yield). 1 H-NMR (DMSO-d6, δppm): 3.66 (s, 3H), 4.16 (s, 2H), 7.05 (d, 2H), 7.13 (d, 2H), 7.28 (t, 1H), 7.47 (t, 2H), 7.99 (d, 2H).

[0154] Step c) Synthesis of [ka] 0.189g (2.220mmol) of piperidine was added to a mixture of 6.00g (22.199mmol) of the compound from the previous step and 2.71g (22.191mmol) of salicylaldehyde in 80mL of ethanol. The mixture was stirred under reflux for 1 hour and then cooled to room temperature. The reaction product was collected by filtration to give 6.74g of a white solid (yield 89%). 1 H-NMR (DMSO-d6, δppm): 7.05 (d, 2H), 7.15 (d, 2H), 7.28 (t, 1H), 7.42~7.51 (m, 4H), 7.72 (m, 1H), 7.85 (dd, 1H), 7.99 (d, 2H), 8.40 (s, 1H).

[0155] Step d) Synthesis of [ka] To an ice-cooled mixture of 5.00 g (14.605 mmol) of the compound from the previous step and 2.59 g (18.970 mmol) of ethyl chlorooxoacetate in 100 mL of dichloromethane, 6.85 g (51.372 mmol) of anhydrous aluminum chloride was carefully added in portions. After stirring at room temperature for 1.5 hours, the reaction was poured into 200 mL of ice / water. The mixture was extracted with dichloromethane, the organic layer was separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give the crude product. The crude product was dissolved in 100 mL of ethanol, washed under reflux with vigorous stirring for 30 minutes, and then cooled to room temperature. The reaction product was collected by filtration to give 5.96 g of a white solid (92% yield). 1 H-NMR (DMSO-d6, δppm): 1.34 (t, 3H), 4.42 (q, 2H), 7.28 (m, 4H), 7.44 (td, 1H), 7.50 (d, 1H), 7.75 (m, 1H), 7.88 (dd, 1H), 8.06 (m, 4H), 8.44 (s, 1H). Example 9

[0156] Synthesis of the following [ka] 0.646 g (1.325 mmol) of zirconium(IV) acetylacetonate was added to a warm solution of 5.86 g (13.245 mmol) of the compound of Example 8 and 5.17 g (39.699 mmol) of 2-ethyl-1-hexanol in 46 mL of toluene with stirring. The reaction mixture was stirred at 110° C. for 2 hours to remove ethanol by distillation. The progress of the reaction was monitored by TLC. After completion of the reaction, the mixture was allowed to cool, diluted with ethyl acetate, and washed successively with 50 mL (×2) of 3 M hydrochloric acid, water, and brine, respectively. The organic layer was separated, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to obtain the crude product. The crude product was purified by crystallization from ethanol to obtain 5.63 g of a white solid (81% yield). 1 H-NMR (DMSO-d6, δppm): 0.86 (m, 6H), 1.33 (m, 8H), 1.70 (m, 1H), 4.30 (d, 2H), 7.28 (m, 4H), 7.44(td, 1H), 7.51(d, 1H), 7.75(m, 1H), 7.88(dd, 1H), 8.06(m, 4H), 8.44(s, 1H). Example 10

[0157] Synthesis of the following [ka] To an ice-cooled mixture of 5.00 g (26.843 mmol) of diphenyl sulfide and 4.47 g (28.191 mmol) of 4-fluorobenzoyl chloride in 60 mL of dichloromethane was carefully added in portions, 3.94 g (29.549 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and 5.50 g (40.284 mmol) of ethyl chlorooxoacetate was carefully added, followed by 6.26 g (46.948 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and an additional 3.57 g (26.774 mmol) of anhydrous aluminum chloride was carefully added. The reaction was then stirred at room temperature for an additional 30 minutes and poured into 200 mL of ice / water. The mixture was extracted with dichloromethane, the organic layer was separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation to obtain a crude product. The crude product was dissolved in 110 mL of ethanol and washed under reflux with vigorous stirring for 30 minutes, then cooled to room temperature. The reaction product was collected by filtration to obtain 9.80 g of a white solid (yield 89%). 1 H-NMR (DMSO-d6, δppm): 1.33 (t, 3H), 4.42 (q, 2H), 7.40 (t, 2H), 7.52 (d, 2H), 7.64 (d, 2H), 7.78 (d, 2H), 7.85 (m, 2H), 7.95 (d, 2H). Example 11

[0158] Synthesis of the following [ka] To an ice-cooled mixture of 5.00 g (26.843 mmol) of diphenyl sulfide and 6.11 g (28.201 mmol) of biphenyl-4-carbonyl chloride in 60 mL of dichloromethane was carefully added in portions, 3.94 g (29.549 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and an additional 0.29 g (1.339 mmol) of biphenyl-4-carbonyl chloride was carefully added followed by 0.21 g (1.575 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 30 minutes, the reaction was cooled again and 4.76 g (34.864 mmol) of ethyl chlorooxoacetate was carefully added followed by 8.23 ​​g (61.722 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was poured into 200 mL of ice / water. The mixture was extracted with dichloromethane, the organic layer was separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent was removed by vacuum distillation to obtain a crude product. The crude product was dissolved in 110 mL of ethanol and washed under reflux with vigorous stirring for 30 minutes, then cooled to room temperature. The reaction product was collected by filtration, and the solid was purified by crystallization from toluene to obtain 8.90 g of a white solid (71% yield). 1 H-NMR (DMSO-d6, δppm): 1.33 (t, 3H), 4.42 (q, 2H), 7.43~57 (m, 5H), 7.66 (d, 2H), 7.78 (d, 2H), 7.83~7.88 (m, 6H), 7.96 (d, 2H). Example 12

[0159] Synthesis of the following [ka] To an ice-cooled mixture of 5.00 g (26.843 mmol) of diphenyl sulfide and 5.15 g (28.196 mmol) of 2,4,6-trimethylbenzoyl chloride in 60 mL of dichloromethane was carefully added in portions, 3.94 g (29.549 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 2 hours, the reaction was cooled again and an additional 0.49 g (2.683 mmol) of 2,4,6-trimethylbenzoyl chloride was carefully added followed by 0.54 g (4.050 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and an additional 0.49 g (2.683 mmol) of 2,4,6-trimethylbenzoyl chloride was carefully added followed by 0.54 g (4.050 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 2 hours, the reaction was heated to reflux and stirred for an additional 45 minutes, then cooled again and 4.76 g (34.864 mmol) of ethyl chlorooxoacetate and 8.23 ​​g (61.722 mmol) of anhydrous aluminum chloride were carefully added in sequence. After stirring at room temperature for 1.5 hours, the reaction was poured into 200 mL of ice / water. The mixture was extracted with dichloromethane, the organic layer was separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give the crude product. The crude product was purified by flash column chromatography on silica gel (toluene / ethyl acetate 97.5:2.5) to give 7.12 g of a yellow oil (61% yield). 1 H-NMR (DMSO-d6, δppm): 1.33 (t, 3H), 2.00 (s, 6H), 2.30 (s, 3H), 4.40 (q, 2H), 6.96 (s, 2H), 7.51~7.58 (m, 4H), 7.70 (d, 2H), 7.96 (d, 2H). Example 13

[0160] Synthesis of the following [ka] To an ice-cooled mixture of 5.00 g (26.843 mmol) of diphenyl sulfide and 5.37 g (28.170 mmol) of 2-benzoyl chloride in 60 mL of dichloromethane was carefully added in portions with 3.94 g (29.549 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and 4.76 g (34.864 mmol) of ethyl chlorooxoacetate and 8.23 ​​g (61.722 mmol) of anhydrous aluminum chloride were carefully added in succession. After stirring at room temperature for 1.5 hours, the reaction was poured into 200 mL of ice / water. The mixture was extracted with dichloromethane, the organic layer was separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give the crude product. The crude product was purified by crystallization from 230 mL of ethanol to give 10.25 g of a white solid (87% yield). 1 H-NMR (DMSO-d6, δppm): 1.33 (t, 3H), 4.42 (q, 2H), 7.53 (d, 2H), 7.60~7.73 (m, 4H), 7.88 (m, 3H), 7.95 (d, 2H), 8.03~8.14 (m, 3H), 8.36 (d, 1H). Example 14

[0161] Synthesis of the following [ka] To an ice-cooled mixture of 5.00 g (26.843 mmol) of diphenyl sulfide and 4.13 g (28.174 mmol) of thiophene-2-carbonyl chloride in 60 mL of dichloromethane was carefully added in portions with 3.94 g (29.549 mmol) of anhydrous aluminum chloride. After stirring at room temperature for 1.5 hours, the reaction was cooled again and 4.76 g (34.864 mmol) of ethyl chlorooxoacetate and 8.23 ​​g (61.722 mmol) of anhydrous aluminum chloride were carefully added in succession. After stirring at room temperature for 1.5 hours, the reaction was poured into 200 mL of ice / water. The mixture was extracted with dichloromethane, the organic layer was separated, washed again with water and brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give the crude product. The crude product was purified by crystallization from ethanol to give 9.14 g of an off-white solid (86% yield). 1 H-NMR (DMSO-d6, δppm): 1.33 (t, 3H), 4.26 (q, 2H), 7.31 (m, 1H), 7.51 (d, 2H), 7.65 (d, 2H), 7.78 (dd, 1H), 7.90 (d, 2H), 7.97 (d, 2H), 8.15 (dd, 1H). Example 15

[0162] The reaction product [ka] 0.375 g (0.769 mmol) of zirconium(IV) acetylacetonate was added to a warm solution of 3.00 g (7.683 mmol) of the compound of Example 1 and 2.72 g (hydroxyl number 634 mg KOH / g) of Polyol 4640 (purchased from Perstorp) in 30 mL of toluene with stirring. The reaction mixture was then stirred at 105-110° C. for 3.5 hours to remove ethanol by distillation. The progress of the reaction was monitored by TLC (toluene / ethyl acetate 95:5). An additional 0.188 g (0.385 mmol) of zirconium(IV) acetylacetonate was then added and the reaction mixture was stirred at 105-110° C. for an additional 2.5 hours to remove ethanol by distillation. After the reaction was complete, the mixture was allowed to cool, poured into 50 mL of 2 M hydrochloric acid, and extracted with dichloromethane. The organic layer was separated, washed again with 50 mL of 2 M hydrochloric acid, then washed with water, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give 4.91 g of crude product, which was used in the next step without further purification. To an ice-cooled mixture of 4.91 g of crude product, 3.19 g (31.525 mmol) of triethylamine, and 0.232 g (1.053 mmol) of 2,6-di-tert-butyl-4-methylphenol in 40 mL of dichloromethane, a solution of 2.48 g (27.400 mmol) of acryloyl chloride in 10 mL of dichloromethane was slowly added over 20 minutes. The reaction mixture was then stirred at room temperature for 3 hours and washed with 50 mL (×2) of 1 M hydrochloric acid. The organic phase was separated, washed with brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation. The residue was dissolved in ethyl acetate and washed with 50 mL (x2) of 0.25 M aqueous sodium carbonate, then with brine, dried over anhydrous sodium sulfate, filtered, and the solvent removed by vacuum distillation to give 5.85 g of a tan oil (88% overall yield). Example 15 is a mixture of different products, 1 H-NMR was calculated by assigning a value of 2 to signals between 7.83 and 8.02 ppm. 1H-NMR (DMSO-d6, δppm): 3.10~3.80 (m, 22.6H), 4.05~4.55 (m, 5.4H), 5.76~5 .97(m, 1.7H), 6.00~6.37(m, 3.4H), 7.37~7.83(m, 11H), 7.83~8.02(m, 2H).

[0163] All of the compounds of Examples 1-14 can be reacted with an appropriate polyol and a (meth)acryloyl derivative, preferably (meth)acryloyl chloride, to give the compounds of the invention.

[0164] Comparative Test The photoinitiators (PIs) of the present invention were compared with the acryloyl compound PI 1 (COMP-1) in Example 1 on page 20 of EP 2617705 A1. Example 16

[0165] Through cure with cyan offset ink Test formulations were prepared by dissolving the components in industrial cyan offset ink at the mass concentrations shown in Table 1. The test formulations were homogenized with a mechanical stirrer at 50°C for 1 hour and then applied to white cardboard at a thickness of 1.5 microns using an IGT Reprotester instrument. Table 1 TIFF2024537185000041.tif80148 The formulations were cured using the following: a) A mercury lamp at a distance of 8 cm b) LED 395nm lamp at a distance of 0.5cm c) LED 365nm lamp at a distance of 0.5cm The through cure test is a measurement of the complete ink cure obtained at a specified speed, checked by the "thumb twist pressure test." Higher speed corresponds to higher reactivity. The results are shown in Table 2. Table 2 TIFF2024537185000042.tif136148 Where no reactivity is indicated in Table 2, it means that no through-cure is achieved at the lowest possible belt speed (10 m / min). These tests confirmed that the compounds of formula (I) are more effective than the prior art photoinitiators: the reactivity of the new compounds is significantly higher in all conditions, achieving the best results in LED lamps where the prior art compounds were either non-reactive or poorly reactive. Example 17

[0166] Tack-free in clear formulations Photopolymerizable compositions for testing were prepared by dissolving the components in the mass concentrations shown in Table 3 in a solution of 50% Photomer 6577 (aromatic urethane acrylate 10F), 15% Photomer 4335 (PETIA), 15% Photomer 4666 (DPHA), and 20% Photomer 4172 (PPTTA). The photopolymerizable composition was applied to a thickness of 12 microns on varnished cardboard using a bar coater. a) A mercury lamp at a distance of 8 cm b) LED 395nm lamp at a distance of 0.5cm c) LED 365nm lamp at a distance of 0.5cm The results were expressed as the maximum speed at which tack-free was achieved in m / min (Table 4). Table 3 TIFF2024537185000043.tif70120 Table 4 TIFF2024537185000044.tif101140 Where no reactivity is indicated in Table 4, it means that no through cure is achieved at the lowest possible belt speed (10 m / min). The reactivity of the new compound was significantly higher in all conditions, achieving the best results in LED lamps where prior art compounds showed no or low reactivity. All these tests confirmed that the compound of formula (I) was more reactive under all lamps and in all conditions than the prior art lamps.

Claims

1. A compound of formula (I): Formula (I) 【Chemistry 1】 wherein R1 is selected from aryl and heteroaryl, each of which is optionally substituted with one or more substituents selected from: halogen, substituted or unsubstituted C1-C20 alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted C1-C20 alkylthio, substituted or unsubstituted (C1-C12 alkyl)2amino, morpholino, piperidino, piperazino and N(C1-C12 alkyl)piperazino; n is 1 to 7; R2 is a group of formula (II) Formula (II) 【Chemistry 2】 where G is an optionally ethoxylated and / or propoxylated monomeric, oligomeric or polymeric polyol G-(OH). m+n+p where m+n+p is from 2 to 8, m is 1 to 7; p is 0 to 6; R3 is selected from CH2=CH-C(=O) and CH2=C(CH3)-C(=O); The wavy line indicates a bond to a compound of formula (I); Z is selected from (i), (ii), and (iii) below: (i) 【Chemistry 3】 (ii) 【Chemistry 4】 (iii) 【Chemistry 5】 Where: X is selected from O, S and C(R4)(R5); Y is selected from O, S, C(R4)(R5) and NR6; R4 and R5 are each independently selected from H, C1-C12 alkyl, OH, and C1-C10 alkoxy; R6 is selected from H and C1-C8 alkyl; A compound of formula (1) characterized in that the wavy line indicates the bond attached to the keto group of formula (I).

2. G-(OH) m+n+p 2. The compound of formula (1) according to claim 1, characterized in that is selected from monomeric polyols, oligomeric polyols and mixtures thereof, which can be optionally ethoxylated or propoxylated.

3. G-(OH) m+n+p 2. The compound of formula (1) according to claim 1, characterized in that it has a number average molecular weight of 1,500 Da or less, more preferably 1,000 Da or less, most preferably 800 Da or less, and a number average molecular weight of 100 Da or more, preferably 200 Da or more.

4. m+n+p is 2 to 8, more preferably 3 to 6; m is 1 to 6, more preferably 1 to 4; n is 1 to 6, more preferably 1 to 4, and A compound of formula (1) according to claim 1, characterized in that p is 0 to 6, more preferably 0 to 4.

5. 2. A compound of formula (1) according to claim 1, characterized in that Z is (i) and X is S or O, preferably S.

6. Compounds of formula (1) according to claim 1, characterized in that R1 is selected from phenyl, trimethylphenyl, halophenyl, preferably fluorophenyl, biphenyl, coumarin-3-yl, naphthyl and thiophenyl.

7. The reaction product: 【Chemistry 6】 Compounds of formula (1) according to claim 1, characterized in that A is OH or a halogen atom, preferably chlorine, and (a'), (b'), (c') and (d') are each independently 0 to 15, preferably 1 to 8.

8. The compound shown below: 【Chemistry 7】 2. The compound of formula (1) according to claim 1, characterized in that (a'), (b'), (c') and (d') are each independently 0 to 15, preferably 1 to 8.

9. a) from 50 to 99.9% by weight, preferably from 70 to 98.9% by weight (based on the total weight of the composition) of at least one ethylenically unsaturated compound; b) 0.1 to 35% by weight, preferably 0.1 to 20% by weight, more preferably 0.2 to 15% by weight (based on the total weight of the composition) of at least one compound of formula (I) as defined in any one of claims 1 to 8, and c) 0 to 20% by weight, preferably 0 to 15% by weight, more preferably 0.2 to 15% by weight, of accelerator and / or coinitiator (based on the total weight of the composition); A photopolymerizable composition comprising:

10. In addition, the following ingredients: d) 0.01 to 15% by weight (based on the total weight of the composition) of one or more photosensitizers, and / or e) 0.5 to 15% by weight (based on the total weight of the composition) of one or more further photoinitiators; 10. The photocurable composition of claim 9, comprising one or more of the following:

11. 10. Photocurable composition according to claim 9, characterized in that the accelerator and / or coinitiator is an amine, preferably a tertiary amine.

12. 1. A method for photocuring photopolymerizable composition coatings, adhesives, and inks, the method comprising: (i) providing a photopolymerizable composition according to claim 9; (ii) coating or printing the photopolymerizable composition onto a substrate; (iii) photopolymerizing the coated or printed composition on the substrate with a light source.

13. A three-dimensional printing method comprising providing the photopolymerizable composition according to claim 9 and photocuring the photopolymerizable composition with a light source.

14. 13. The method of claim 12, wherein the light source is ultraviolet light in at least one of the UVA, UVB, and UVC regions.

15. 13. The method of claim 12, wherein the light source is an LED light source emitting in the range of 350-420 nm.

16. 13. The method of claim 12, further comprising the step of coating the photopolymerizable composition onto a substrate prior to photopolymerization.

17. A product obtainable according to the method of claim 12.

18. 10. An article obtained by three-dimensional printing of the photopolymerizable composition according to claim 9.

Citation Information

Patent Citations

  • Polymerizable free radical II type photoinitiators and preparation method thereof

    CN107629151A

  • Dibenzothiophene formyl formate photoinitiator as well as preparation method and application thereof

    CN108623559A

  • Fluorene photoinitiator and photocured composition comprising same

    CN109503736A

  • Polymerizable II-type photoinitiator and preparation method thereof

    CN109734699A

  • Amino photoreactive binder

    JP2015509099A

Cited By

  • Photocurable resin composition, cured product, laminate, method for producing cured product, method for producing laminate, method for manufacturing semiconductor device, and semiconductor device

    WO2026160330A1