Process for continuous batch production of polyamides
By using end-capping agents and comonomers in controlled amounts, the process addresses heel retention and phase-out issues in high 6T semi-crystalline polyamide production, ensuring consistent quality and efficiency in continuous batch processes.
Patent Information
- Application Number
- JP2024523153
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-22
- Filing Date
- 2022-10-20
- Publication Date
- 2024-10-18
AI Technical Summary
The production of semi-crystalline polyamides containing high mole fractions of hexamethylene terephthalic acid (6T) in continuous batch processes faces challenges such as heel retention, phase-out issues, and poor casting performance due to the formation of high-melting-point crystallites, which are exacerbated by the higher reactivity differences between terephthalic acid and adipic acid during polymerization.
Incorporating 0.5-2.5 mol% of an end-capping agent and 0.5-6.0 mol% of at least one other comonomer into the polymerization process of terephthalic acid, adipic acid, and hexamethylene diamine, while maintaining a maximum pressure of 320 psia and temperature below the melting point of the final polymer, limits the formation of long 6T blocks and reduces heel buildup, ensuring consistent polymer quality.
This approach allows for continuous batch production of semi-crystalline polyamides with maintained or improved tensile strength and impact strength, reduces the need for inter-batch cleaning, and enhances manufacturing efficiency by minimizing solvent use and defective products.
Smart Images

Figure 2024538173000001 
Figure 2024538173000002 
Figure 2024538173000003
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to UK Application No. 2115260.8, filed October 22, 2021, which is incorporated herein by reference.
[0002] FIELD OF THEINVENTION A process for making continuous batches of semi-crystalline polyamides comprising terephthalic acid, adipic acid, and hexamethylenediamine, as well as small amounts of at least one other comonomer (less than 6 mol % each) and an endcapping agent (0.5-2.5 mol %) is disclosed. [Background technology]
[0003] Conventional hydrolytic polymerization for producing polyamides such as PA66 using batch autoclave techniques and resources well known in the art is described by MI Kohan in Nylon Plastics Handbook (Section 2.3, pp. 17-20, ISBN 1-56990-189-9).
[0004] The hydrolysis polymerization process is a two-phase process consisting of liquid and gas. The gas is mostly water vapor (steam) that exists as bubbles within the liquid (hence two phases) or as gas above the liquid. The liquid phase changes its nature during polymerization from that of dissolved monomers, through a mixture of dissolved monomers and oligomers, to molten polymer at the end of the polymerization process. The formation of solids or other inhomogeneities, e.g. gels, either by exceeding the solubility limit, not achieving the melting point as the species is formed, or decomposition giving rise to branched species, is detrimental and is intentionally avoided by careful temperature and pressure control during the polymerization process. The inability to maintain a homogeneous two-phase system can be described as "phasing out".
[0005] Phase-out can manifest in a variety of ways, which may also depend on the degree of phase-out, such as: inhomogeneous melt lacing upon casting with the formation of thick and thin sections (which may be described as "blobs" and "thins"); inhomogeneous viscous behavior upon casting leading to surging, i.e., there is a rapid change in viscosity on a short time scale; entrapment of excessive amounts of gas bubbles; post-casting analysis of the melting behavior of the polymer may find a population of high melting species, "high melts" or "un-melts" that exceed the expected melting point of the polymer; post-casting analysis of the solidification behavior of the polymer may find that the polymer begins to solidify at a higher temperature than would typically be expected to occur for a polymer with a nucleating agent present; or post-casting analysis of the polymer may find that the entire polymer is not soluble in the solvent and exhibits gel formation.
[0006] Some small levels of "unmelt" can be tolerated, but too high a level will result in unacceptable pelletizing performance and low yields due to levels of misshapen pellets, or even the need to "dump" the batch.
[0007] In contrast, good casting performance may be characterized by a homogenous molten race; no surging causing blobs or sins; any viscosity changes being slow and gradual (it is well known in the art that a polymer may exhibit a lower melt viscosity at the beginning of casting than at the end due to continuing polymerization during casting, but this is easily compensated for), and the race being substantially free of visible air bubbles, or at least any air bubbles in the race being small and at an acceptable level so as not to result in poor casting performance.
[0008] In commercial batch operations, when the molten contents of a polymerization autoclave reach a desired degree of polymerization, the contents are discharged from the vessel, which may be as strands of molten polymer that are then cooled, often in a water bath or sluice, and formed into pellets. However, the entire contents of the autoclave vessel are not easily discharged from the vessel, and a portion of the contents remains attached to the walls and other surfaces within the vessel. This small amount of polymer on the inner surface of the reactor is often referred to as the "heel." After discharge, the valve is closed.
[0009] It would be uneconomical to remove the heel after each batch, and therefore it would be desirable to charge the next batch of monomer feed, usually a hot concentrated aqueous feed, to the autoclave in which the heel is present. However, the hot feed is lower than the freezing or melting point of the polymer that constitutes the heel, and therefore the heel will solidify where the heel is present. As a result, when this next batch is processed and polymerized, the heel will undergo a heat treatment. The heat treatment may induce annealing of the heel, a process known in the art of perfecting any polymer crystallites that have formed and increasing their melting point. This additional heat treatment will also contribute to additional pyrolysate levels in the final polymer. At the interface between the heel and the hot feed, hydrolysis may occur, partially dissolving the surface of the heel in the hot liquid. Thus, the heel is returned to this next batch to be fully incorporated only when the heel is fully hydrolyzed or the temperature of the system is high enough for the heel to flow. However, higher melting species than those created during the annealing stage may still be present, and these species will persist until the system reaches a temperature high enough to destroy them.
[0010] Therefore, this mode of making batch-on-batch or successive batches has its own challenges beyond making a single batch on a clean autoclave and may produce a polymer with slightly different properties than that from a clean autoclave.Various approaches have been proposed in the art to address the challenges of making successive batches of copolyamides while keeping the heel in the batch vessel between successive batches.
[0011] Conventionally, the technique for naming the repeat units of polyamides made from diamines and dicarboxylic acids is that the first letter represents (or labels) the diamine and the second letter represents (or labels) the dicarboxylic acid. Polyamides containing repeat units of hexamethylene terephthalamide (6T or PA6T), derived from the monomers hexamethylene diamine (6) and terephthalic acid (T), are commercially available.
[0012] Although these 6T-containing copolyamides are known to be particularly difficult to make and to avoid phasing out, their ability to perform well in high temperature environments, for example due to their oxidation resistance, high melting points, high glass transition temperatures, high heat distortion temperatures, or better flame retardant properties, makes them attractive polymers for use in more extreme applications where polyamides such as PA6 or PA66 would struggle to meet the application demands.
[0013] PA6T homopolymer is intractable by itself, melting at about 350-370°C. Its copolymers are therefore made to reduce the melting point to a level where melt processability is possible and the level of thermal degradation is acceptable. Comonomers that affect such a melting point reduction can be based on additional dicarboxylic acids such as adipic acid (6) or isophthalic acid (I); or additional diamines such as 2-methylpentamethylenediamine (D); or amino acids such as 6-aminocaproic acid (6-ACA); or lactams such as caprolactam, or combinations thereof.
[0014] For commercial manufacture and subsequent melt processing, including but not limited to, by methods such as compounding, injection molding, it is preferred to produce a polymer with a melting point of about 260° C. to 310° C. Below this, there is little advantage over conventional PA66 (hexamethylene adipamide) polymers, and above this temperature range, decomposition reactions become problematic, especially when aliphatic dicarboxylic acids form part of the polymer.
[0015] To avoid large investment costs, it would be highly desirable to be able to produce such 6T-containing polymers in commercial facilities designed to make PA66. PA66 autoclaves are typically designed to operate with contents well within a safety margin at a maximum operating pressure of about 320 psia and about 330°C, but when producing PA66, they can typically be operated at about 265 psia and 290°C.
[0016] It is also desirable to be able to utilize process variables commonly used in the art, such as time, temperature, pressure, vacuum depth, etc., to achieve end product properties, such as solution viscosity. Similarly, utilize normal formulation variables commonly used in the art, such as excess diamine or dicarboxylic acid, to achieve end product properties, such as amine end group (AEG) levels. It is well known in the art that there are interactions between process and formulation variables in achieving end product properties, and measures taken, such as longer periods at high temperatures, can result in higher hexamethylenediamine loss levels, necessitating the addition of additional hexamethylenediamine to compensate for the losses.
[0017] Other additives, such as heat stabilizers, antioxidants, light and UV stabilizers, pigments, lubricants, nucleating agents, catalysts, acid scavengers, and other additives known in the art, may optionally be added during any convenient stage of the polymerization.
[0018] U.S. Patent No. 3,941,755 (RD Chapman et al. Monsanto Co.) claims fiber-forming PA6T / 6I copolymers containing 60-80 m% (i.e., mol%) 6T and having boiling water shrinkage of 10-30%. The phase-out problem is described in paragraph column 2 line 24, and means of preventing phase-out are described, either by using 6T and 6I salts having a pH of 7.2±0.2, optionally conducting the polymerization in the presence of a plasticizer and including a small but effective amount of a heat stabilizer, or by using 6T and 6I salts having a pH between 7.2±0.2, carefully controlling the time it takes to complete the second cycle of polymerization to 35±5 minutes (when the reaction mixture is heated from about 220° C. to 300° C.-310° C. at about 250 psig while maintaining a constant pressure), and optionally conducting the polymerization in the presence of a plasticizer (paragraph column 2 line 36).
[0019] U.S. Pat. No. 4,238,603 (RD Chapman et al., Monsanto Co.) describes the problem of making PA6T / 6I containing more than 60m% 6T in a batch autoclave making successive batches, where the heel does not melt completely in the next batch, resulting in particles in the polymer, a condition referred to as "polymer heterogeneity."
[0020] U.S. Pat. No. 4,501,882 (L.W. Plischke, Monsanto Co.) claims a process for preparing successive (consecutive) batches of PA6T / 6I copolymer containing 45-80m% 6T by adding a base such as sodium hydroxide in an amount sufficient to allow successive batches to be made without washing the vessel between successive batches.
[0021] U.S. Pat. No. 5,302,691 (RR Soelch, Du Pont Canada Inc.) describes problems that arise when making PA6T / DT (D is 2-methylpentamethylenediamine (2-MPMD)) on the same autoclave without taking steps to clean the autoclave between successive batches.
[0022] European Patent No. 655,076 (C. Leboeuf, Dupont Canada Inc.) describes a high pressure process for the manufacture of PA6T / DT on a batch autoclave running successive batches (i.e., without cleaning between batches).
[0023] U.S. Patent No. 5,656,717 (C. Lebouef, Du Pont Canada Inc.) describes the same problem as European Patent No. 655,076.
[0024] Zytel® HTN 501 (Dupont) disclosed in Thermochimica Acta 1998,319,201 (MY Keating) is PA6T / DT 50 / 50 w% (note that in this case it is the same as m%, the entire diacid is terephthalic acid), Grivory® HT XE 3733 (EMS) would be a member of the first subcategory and would therefore be PA6T / 6I 70 / 30 m% disclosed in US Patent Application Publication No. 2002 / 0173584 (M. Ebert et al, EMS), and Zytel® HTN 502 (Dupont) is PA66 / 6T disclosed in US Patent Application Publication No. 2011 / 0015328 (Y. Orihashi, Dupont). 45 / 55 m%, and Amodel® A1000 (Solvay), which is a PA66 / 6T / 6I 10 / 65 / 25 (adipic acid / terephthalic acid / isophthalic acid mole % (m%), respectively), disclosed in U.S. Pat. No. 5,436,294 (GP Desio et al., Amoco Corp.), would fall within the second category.
[0025] Aliphatic dicarboxylic acids, especially adipic acid, are more sensitive to thermal decomposition, so prolonged periods at high melt temperatures will cause undesirable decomposition of fatty acid segments. Furthermore, this problem is more severe than that of PA66 polymerization due to the higher melting points of PA66 / 6T and PA66 / 6T / 6I polyphthalamides. The challenge for manufacturers is to devise a process that minimizes decomposition while still achieving polymerization and satisfactory polymer quality.
[0026] PA66 / 6T is a well-established copolyamide. Schlack (German Patent No. 929151) reported on the hydrolytic melt polymerization preparation of PA66 / 6T copolymers and the melting points of compositions up to 50 mol% 6T (50m% 6T). Making continuous batches of the polymer was not considered.
[0027] Unlike most copolymer systems, which experience a depression of the melting point to a minimum at some composition between the melting points of the pure homopolymers, PA66 / 6T exhibits isomorphism of the 6T repeating units to the PA66 crystal lattice, which means that for PA66 / 6T, at levels above about 20m% 6T, the melting point tends to gradually increase between the melting points of the PA66 and PA6T homopolymers, as reported by AJ Yu and RD Evens (J. Polymn. Sci, 1960, XLII, 249-257).
[0028] British Patent No. 1,114,541 (OBEdgar) claims ternary copolyamides consisting of a major proportion of PA66, at least 20 w% of PA6T, and a minor proportion of a third copolyamide, e.g., PA6I, preferably 20-40 w% PA6T and 5-10 w% of the third copolymer. Example 1 is a PA66 / 6T / 6I 58 / 31.5 / 10.5 w% (60 / 30 / 10 m%) copolymer made with 1 mole of acetic acid and analyzed for 44 moles of acetyl end groups per million grams of polymer. Example 2 is a PA66 / 6T / 6I 72.8 / 21.9 / 5.3 (74.7 / 20.6 / 4.7 m%) copolymer made with 0.55 moles of acetic acid.
[0029] U.S. Reissue Patent No. 34447 (reissue of U.S. Pat. No. 4,603,166, W. Poppe et al., Amoco Corp.) describes a process for producing PA6T / 6I / 66 copolymers having molar ratios in the range of 65-90 / 25-0 / 35-5m%, respectively (6I / 66 molar ratios less than 3:1), in which a first process low molecular weight prepolymer is made, which is converted to a higher molecular weight polymer in a subsequent process. One process exemplified consists of rapidly making a very low molecular weight prepolymer (polyamide oligomer) by heating an aqueous solution of monomers together at high temperature (328° C.) and pressure (1800 psig) for a short period of time (40 seconds) and then feeding it to a flash reactor, where the reaction mixture can reach up to 333° C. while the pressure is reduced to about 0-400 psig with a residence time of about 10 seconds (the flash reactor can be operated in batch, batch continuous, or continuous mode), and then completing the polycondensation in, for example, a twin screw reactor / extruder configured to increase the molecular weight. In another process, a low molecular weight prepolymer is exemplified as being made in a batch reactor at about 315° C. and 130 psig pressure, isolated as granules, and then fed to a twin screw reactor / extruder configured to increase the molecular weight. Such a multi-step process is more complex than a conventional single-step autoclave process.
[0030] Application Publication No. 61,159,422 (K. Koichi et al, Toray Ind Inc.) describes a process for producing PA66 / 6T polymers containing 20-60 w% 6T (about 19-38 m%) by limiting the maximum melting temperature 5-15° C. above the melting point of the resulting copolymer. To control the molecular weight of the polymer, 0.7-4.0 m% of a salt-based viscosity stabilizer, such as acetic acid, is added.
[0031] Application Publication No. 04,337,323 (S. Kataoka et al., Toray Ind Inc.) relates to a method for producing blow molding polyamide resins having good heat resistance, chemical resistance, low water absorption, antifreeze resistance, dimensional stability, and improved melt residence stability.
[0032] European Patent No. 3,502,165 (Rhodia Operations) describes the problem of fouling of used autoclaves when preparing PA66 / 6T copolyamides, which must be removed periodically by thorough cleaning. The patent claims a process for producing copolyamides containing less than 50 mol % of 6T units by polymerizing a concentrated mixture of salts in an autoclave at a pressure of at least 1.2 MPa by increasing the temperature to a temperature higher than the final melting point of the copolyamide before releasing the pressure, and allowing further polymerization to continue before granulating the product.
[0033] US Patent No. 10875962 (MD Benstead, INVISTA North America SARL) describes a method for making polyamide copolymers including PA66 / 6T containing 10-39m% 6T, and a method for making such polymers in a continuous batch mode (i.e., on the heel of a previous batch).Acetic acid is optionally added in an amount of 0.1-10m% as an end-capping agent to limit the molecular weight and improve casting performance.
[0034] The object of the present invention is to address one or more of the above-mentioned problems. In particular, the object of the present invention is to provide an improved process for producing continuous batches of semi-crystalline polyamides containing terephthalic acid, adipic acid, and hexamethylenediamine, particularly at a relatively high mole fraction of 6T. A particular object of the present invention is to address the heel retention problem while retaining good product quality. Advantageously, the process should be operable on existing commercial assets, e.g., commercial assets suitable for producing PA66. Summary of the Invention
[0035] The inventors have surprisingly found that it is possible to carry out a polymerization process for producing continuous autoclave batches of semi-crystalline polyamides comprising terephthalic acid, adipic acid, and hexamethylenediamine by judicious incorporation of 0.5-2.5 m% of an end-capping agent, and incorporation of small amounts of at least one other comonomer (also referred to herein as a breaker) of 0.5-6.0 m%, where m% 6T is 25-45 m% and at a maximum pressure of about 320 psia, limiting the maximum content temperature during the highest pressure stage to below the melting point of the final polymer, and the final content temperature to a maximum of about 320°C.
[0036] Without limiting the scope of the invention by theory, it is the inventors' contention that the problems described herein with respect to the production of copolymers containing 6T are the result of the formation of blocks of 6T repeat units, also meant to be understood as 6T-rich blocks in isomorphic systems along the copolyamide chain. There will be a distribution of such block lengths determined by the statistics and dynamics of the system. In systems with high m% levels of 6T, there is a greater statistical opportunity to form a greater proportion of longer block lengths compared to systems with lower m% of 6T. In systems where there is a significant difference between the reactivity of terephthalic acid and other carboxylic acids undergoing polymerization, such as adipic acid, which is aliphatic and more reactive, this can lead to a kinetic composition drift as the chain grows. For example, in PA66 / 6T, PA66-rich polymers may form first and PA6T-rich segments may form later. Thus, 6T is more likely to be enriched beyond the initial composition and form longer 6T repeat unit blocks than it would be if the reactivity were comparable.
[0037] In semi-crystalline polymers, the thicker the lamellae in the crystallites, the higher their melting point (Gibbs-Thomson equation as in B. Wunderlich & G. Czornyj; Macromolecules, 1977, 19(5), 906-913). The longer the 6T repeating unit blocks, the more capable they are of forming larger crystals and therefore exhibiting higher melting points. Thus, when such blocks are formed during the melt polymerization process, they may clump together and, if the temperature of the mass is not high enough for the length of the 6T repeating unit blocks formed, they may crystallize, i.e., phase out. The amount of phase out may vary from a very small portion of the remaining fluid mass of the molten polymer to the freezing of the entire system.
[0038] As mentioned earlier, when producing polymers in a batch-on-batch (or sequential batch) mode without cleaning between batches, there is a residual heel of polymer from the previous batch that is heated and annealed during the subsequent polymerization. During this annealing process, crystals of the 6T repeating units may grow with sufficient thermal motion to allow rearrangement. As a result, their melting point will increase, which will present a problem in producing a satisfactory polymer that is not observed when making a single batch of polymer on a clean autoclave.
[0039] Other comonomers (or breakers) suitable for use in the present invention, i.e., that are not terephthalic acid, adipic acid, or hexamethylenediamine, include organic diamines, such as (but not limited to) pentamethylenediamine; 2-methylpentamethylenediamine; octanediamine; m-xylylenediamine; 2-methyloctanediamine; bis(p-aminocyclohexyl)methane; nonanediamine; decanediamine; 2,4,4-trimethylhexamethylenediamine; 2,2,4-trimethylhexamethylenediamine; and isophoranediamine. It may be an isophoranediamine, and / or an organic dicarboxylic acid, such as (but not limited to) azelaic acid, isophthalic acid, sebacic acid, dodecanedioic acid, and 2,6-naphthanene dicarboxylic acid, and / or an organic aminocarboxylic acid, such as (but not limited to) 6-aminohexanoic acid, 7-aminoheptanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid, and / or an organic lactam, such as (but not limited to) caprolactam, and laurolactam. Other preferred comonomers used in the present invention are selected from isophthalic acid (I), 2-methylpentamethylenediamine (D), and combinations thereof.
[0040] Typically, no more than two of the comonomers are present in a copolyamide.
[0041] When more than one comonomer is present in the copolyamide, the total amount of comonomers is preferably no more than 12m%, preferably no more than 10m%.
[0042] It will be understood that the comonomer is incorporated into the backbone of the polymer chain of the copolyamide product.
[0043] Without limiting the scope of the invention by theory, it is believed that such comonomers insert into the 6T repeat unit blocks, reducing their length and thus making the lamella thicker, thus reducing their ability to form high melting point crystallites upon crystallization. Therefore, such comonomers may be considered and referred to as breakers herein. If excessive amounts of comonomers are used, the melting point of the polymer may be reduced or the crystallinity of the polymer may be reduced to such an extent that other desirable properties, such as good tensile strength or impact strength, are unattainable.
[0044] Similarly, the endcapping agent may limit the length that the 6T blocks can form, thus making the lamellae thicker and thus reducing the ability to form high melting crystallites upon crystallization. If excessive amounts of endcapping agent are present, the molecular weight of the polymer may be reduced to such an extent that other desirable properties, such as good tensile strength or impact strength, become unattainable.
[0045] The inventors have found that including end cappers and other comonomers in the aforementioned ranges reduces or minimizes heel build-up during the manufacture of the polymer while at the same time providing a high performance end product, in particular where mechanical properties (such as tensile strength and / or impact strength) are maintained or improved and / or there is no significant reduction in the melting point of the polymer.The present invention is a particularly advantageous semi-crystalline polyamide comprising terephthalic acid, adipic acid and hexamethylenediamine, wherein m% 6T is 30-45m%, in particular 35-45m%, in particular 40-45m%.
[0046] The process of the present invention advantageously minimizes or avoids between-batch cleaning, thus sustainably reducing the use of additional solvents and disposal of spent solvents used in such cleaning. Additionally, the present invention improves the sustainability, efficiency, and economics of the manufacturing process by improving productivity and minimizing off-target or defective products.
[0047] The process of the present invention allows for successive batch production of copolyamides, either while at least maintaining or without a significant drop in the relative viscosity of the product in successive batches. As used herein, a significant drop in relative viscosity is defined as a drop in relative viscosity (RVS, defined below) of more than 0.5 within successive batches or over a cycle of up to four successive batches. Preferably, the process of the present invention exhibits a drop in relative viscosity (RVS) within successive batches (and preferably over a cycle of up to four successive batches) of 0.5 or less, preferably 0.4 or less, preferably 0.3 or less, preferably 0.2 or less, preferably 0.1 or less.
[0048] Any suitable endcapping agent known or conventional in the art may be used, including monofunctional organic carboxylic acids, such as acetic acid, benzoic acid, propionic acid, stearic acid, and the like, and monofunctional organic amines, particularly alkylamines, such as n-hexylamine, and the like. 1,4-dicarboxylic acids, such as succinic acid, are also known endcapping agents, as they can react with amine termini to form endcapping five-membered imide ring structures. Other endcapping agents include anhydrides, such as phthalic anhydride, which can form endcapping five-membered imide ring structures, and 1,8-naphthalene anhydride, which can form endcapping six-membered imide ring structures. Particularly useful are monofunctional organic acids (i.e., having one dicarboxylic acid group) and monofunctional organic amines (i.e., having one amine group). A preferred endcapping agent is acetic acid (AcOH). Although one or more endcapping agents may be used, typically only one endcapping agent is used.
[0049] 2-Methylpentamethylenediamine (D) is commercially available under the trade name INVISTA Dytek® A amine. INVISTA DYTEK® A amine is commercially produced by hydrogenating 2-methylglutaronitrile (i.e., "MGN", methylglutaronitrile). MGN is a branched C6 dinitrile obtained as a by-product from the butadiene double hydrocyanation process for adiponitrile (i.e., "ADN", adiponitrile). The MGN by-product, which would otherwise be disposed of, can be recycled and reused in the manufacture of INVISTA Dytek® A amine. Thus, the use of 2-methylpentamethylenediamine in the present invention sustainably and advantageously recycles the amine content.
[0050] The copolyamides produced by the process of the present invention are preferably not block copolymers, but instead are preferably random copolymers, or essentially random copolymers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0051] According to the present invention, semi-crystalline polyamides comprising terephthalic acid, adipic acid and hexamethylenediamine, with m% 6T in the range of 25-45 m%, and with incorporation of small amounts of at least one other comonomer in the range of 0.5-6.0 m%, and 0.5-2.5 m% of an end-capping agent, can be produced in a batch autoclave in a continuous batch mode (batch-on-batch) without cleaning the autoclave between batches.
[0052] The reactants for polymerization can be introduced into the autoclave in any convenient form and at any convenient temperature and pressure. In one embodiment, a concentrated (25 wt % or less water) salt solution containing terephthalic acid, adipic acid, hexamethylenediamine, endcapping agent, and at least one other comonomer is fed from an evaporator vessel at a convenient temperature, pressure, and concentration in a manner similar to that well practiced in the art for PA66. In another embodiment, a moderately concentrated (40 wt % or more water) salt solution containing terephthalic acid, adipic acid, hexamethylenediamine, endcapping agent, and at least one other comonomer is fed into the autoclave at a convenient temperature, pressure, and concentration.
[0053] The batch polymerization can be conveniently described as being carried out in six cycles.
[0054] In the first cycle, the salt water solution containing the above monomers and reactants is introduced into the conditioned autoclave vessel, waiting for the introduction of the salt solution. Optionally, other additives such as antifoam agents, catalysts, etc. may be added at this stage. If the salt solution is moderately dilute, the contents may be heated and vented to evaporate the water, the pressure may be controlled at a set point of about 30 psia to 250 psia, and venting is stopped when the temperature reaches a set point of about 160°C to 200°C. If the salt solution is sufficiently concentrated, the second cycle begins once all the hot solution (which is about 160°C to 200°C) has been added.
[0055] In the second cycle, heating continues to increase the pressure and temperature, and the second cycle ends when the pressure reaches a set point between about 250 psia and 320 psia, the maximum pressure for the process.
[0056] In the third cycle, venting begins while the temperature is increased to a set point between about 245° C. and 290° C. and below the melting point of the final polymer.
[0057] In the fourth cycle, the pressure is reduced from the maximum pressure to atmospheric pressure, and the pressure reduction can be done in stages with intermediate hold pressures and set point temperature targets that can be above the melting point of the final polymer, or it can be a single uniform pressure reduction. The fourth cycle can take about 15 minutes to 120 minutes, preferably about 25 minutes to 40 minutes, more preferably 30 minutes to 35 minutes.
[0058] When the pressure reaches atmospheric pressure during the fifth cycle, the system is allowed to vent freely to evaporate water-containing vapors and bring the molten contents to their final temperature and hold for any desired length of time that results in the final polyamide with the desired properties. Optionally, a vacuum can be applied during this cycle for any length of time and at any depth of vacuum that results in the final polyamide with the desired properties.
[0059] In the sixth cycle, a small pressure is applied to the autoclave, typically by application of nitrogen gas, and the polymer is extruded through a casting valve and formed into pellets by means well known in the art.
[0060] When the casting valve begins to blow nitrogen gas through it, casting is complete and the casting valve is closed. Note that uncast polymer residue, the heel, remains in the autoclave.
[0061] The autoclave is now ready to return to cycle 1 for the next batch and await the introduction of the salt water solution. The optimum times, temperatures, pressures and vacuum depths associated with each run of the cycle will vary somewhat depending on the polymer composition.
[0062] The invention is defined, inter alia, by the following numbered statements: 1. A polymerization process for producing continuous batches of a copolyamide comprising terephthalic acid, adipic acid, and hexamethylenediamine, comprising: a. introducing copolyamide monomer units of terephthalic acid, adipic acid, and hexamethylenediamine into a batch vessel to provide a reaction mixture; b. introducing into the batch vessel an endcapping agent and at least one comonomer other than terephthalic acid, adipic acid, and hexamethylenediamine; c. subjecting the contents of the batch container to conditions sufficient to form the copolyamide; d. recovering the copolyamide product from the vessel; A process in which batch containers are not cleaned between batches. 2. The process of statement 1, wherein the process comprises producing a first batch of the copolyamide and recovering it from the batch container in accordance with steps (a)-(d), and further comprises producing a second batch of the copolyamide and optionally at least one subsequent batch of the copolyamide, wherein each production step of the second and optional subsequent batches corresponds to steps (a)-(d). 3. The process according to statement 1 or 2, wherein upon completion of step (d) in each production batch, a residual copolyamide product, defined as the heel, remains in the batch vessel and said second and optional subsequent batches are processed on the heel of the preceding batch, preferably the amount of said heel representing no more than 10% by weight of the maximum theoretical yield from the batch. 4. The process according to any of statements 1 to 3, wherein the reaction mixture further comprises a solvent, preferably water. 5. The process of any of statements 1-4, wherein the terephthalic acid, adipic acid, hexamethylenediamine, endcapping agent, and other comonomers are contacted in a mixing vessel and then introduced into the batch vessel, preferably in the form of a feed solution. 6. The process of any of statements 1-5, wherein a portion of the total amount of the adipic acid and hexamethylenediamine needed to make a copolyamide is in the form of a nylon salt, preferably the portion being an approximately stoichiometric amount of the hexamethylenediamine relative to the amount of adipic acid. As used herein, the term "approximately stoichiometric amount" means a HMD:AA ratio of 10% or less on either side of 1.00:1.00, i.e., in the range of 1.10:1.00 to 1.00:1.10. Preferably, a stoichiometric salt is used to maximize the molecular weight achievable by the process. 7. The process of statement 6, wherein the terephthalic acid, the salt, and the other comonomers are contacted in a mixing vessel and additional hexamethylenediamine is added thereto, and the endcapping agent can be contacted with the terephthalic acid, the salt, and the other comonomers, or can be added to a mixture containing the terephthalic acid, the salt, and the other comonomers simultaneously or in the same composition as the additional hexamethylenediamine. 8. The process of any of statements 1 to 7, wherein the total amount of diamines in the reaction mixture, preferably the total amount of hexamethylenediamine in the reaction mixture, is in excess relative to the combined molar amounts of adipic acid, terephthalic acid, and any carboxylic acid-containing compounds among the other comonomers, preferably the excess is 0.1 to 5.0 m% relative to the combined molar amounts of adipic acid, terephthalic acid, and any carboxylic acid-containing compounds among the other comonomers. 9. The process of any of statements 1-8, wherein the batch vessel is subjected to a maximum pressure of about 320 psia and the maximum temperature of the vessel contents during the maximum pressure stage is below the melting point of the final copolyamide product. 10. The process of any of statements 1-9, wherein the temperature of the final contents of the batch vessel is limited to a maximum of 320°C. 11. The process of any of statements 1-10, wherein the batch vessel is an autoclave. 12. The process of any of statements 1 to 11, wherein the copolyamide product comprises 0.5 to 2.5 m %, preferably 1.0 to 2.0 m %, of an endcapping agent. 13. The process of any of statements 1-12, wherein the copolyamide product comprises 0.5 to 6.0 m %, preferably 2.0 to 6.0 m %, preferably 2.0 to 5.5 m %, preferably 2.0 to 5.0 m %, preferably 2.0 to 4.5 m % of each of the one or more comonomers other than terephthalic acid, adipic acid, or hexamethylenediamine. 14. The process of any of statements 1-12, wherein the copolyamide product contains no more than 4.5 m%, preferably from 0.5 to 4.5 m%, preferably from 2.0 to 4.5 m%, of each of the one or more comonomers other than terephthalic acid, adipic acid, or hexamethylenediamine. 15. The process according to any of statements 1 to 14, wherein the copolyamide product comprises a plurality of said comonomers other than terephthalic acid, adipic acid, or hexamethylenediamine, the total amount of said comonomers being 12m% or less, preferably 10m% or less. 16. The process of any of statements 1 to 15, wherein the copolyamide product exhibits a hexamethylene terephthalamide mole fraction, defined as the 6T component, of 25 to 45 m%. 17. The process of any of statements 1 to 16, wherein the copolyamide product exhibits a hexamethylene adipamide mole fraction, defined as the 66 component, of 50 to 70 m%. 18. The process according to any of statements 1 to 17, wherein when the copolyamide product exhibits a hexamethylene terephthalamide mole fraction (6T component) of 35 to 45 m%, in particular 40 to 45 m%, the amount of at least one of the one or more comonomers, preferably each of the one or more comonomers, other than terephthalic acid, adipic acid, or hexamethylenediamine present in the copolyamide is in the range of 2.5 to 6.0 m%, preferably 3.0 to 6.0 m%, preferably 3.5 to 6.0 m%, and preferably 4.0 to 6.0 m%. 19. The process according to any of statements 1 to 18, wherein when the copolyamide product exhibits a hexamethylene terephthalamide mole fraction (6T component) of 35 to 45 m%, in particular 40 to 45 m%, the total amount of hexamethylene diamine in the reaction mixture is in excess over the combined molar amounts of adipic acid, terephthalic acid, and any carboxylic acid-containing compounds among the other comonomers, said excess being 3.0 to 5.0 m% over the combined molar amounts of adipic acid, terephthalic acid, and any carboxylic acid-containing compounds among the other comonomers. 20. The process according to any of statements 1 to 17, wherein the copolyamide product exhibits a hexamethylene terephthalamide mole fraction (6T component) of less than 35 m%, and the total amount of hexamethylene diamine in the reaction mixture is in excess relative to the combined molar amounts of adipic acid, terephthalic acid, and any carboxylic acid-containing compounds among the other comonomers, the excess being less than 0.1 to 3.0 m%, preferably 0.1 to 1.0 m%, relative to the combined molar amounts of adipic acid, terephthalic acid, and any carboxylic acid-containing compounds among the other comonomers. 21. The process of any of statements 1-20, wherein the endcapping agent is selected from a monofunctional organic carboxylic acid, such as acetic acid, benzoic acid, propionic acid, stearic acid, and the like; a monofunctional organic amine, preferably an alkyl amine, such as n-hexylamine; a 1,4-dicarboxylic acid, such as succinic acid, which reacts with the amine terminus to form an endcapping 5-membered imide ring structure; an anhydride, such as phthalic anhydride, which reacts with the amine terminus to form an endcapping 5-membered imide ring structure; and an anhydride, such as 1,8-naphthalene anhydride, which reacts with the amine terminus to form an endcapping 6-membered imide ring structure, and preferably the endcapping agent is acetic acid. 22. The at least one comonomer other than terephthalic acid, adipic acid, and hexamethylenediamine is selected from organic diamines, organic dicarboxylic acids, organic aminocarboxylic acids, and organic lactams, preferably, the organic diamine is selected from pentamethylenediamine, 2-methylpentamethylenediamine, octanediamine, m-xylylenediamine, 2-methyloctanediamine, bis(p-aminocyclohexyl)methane, nonanediamine, decanediamine, 2,4,4-trimethylhexamethylenediamine, 2, ... 23. The process according to any of statements 1 to 22, wherein the organic dicarboxylic acid is selected from azelaic acid, isophthalic acid, sebacic acid, dodecanedioic acid, and 2,6-naphthalenedicarboxylic acid, and / or preferably the organic amino carboxylic acid is selected from 6-aminohexanoic acid, 7-aminoheptanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid, and / or preferably the organic lactam is selected from caprolactam and laurolactam. 23. The process of any of statements 1-22, wherein the at least one comonomer other than terephthalic acid, adipic acid, and hexamethylenediamine is selected from isophthalic acid (I), 2-methylpentamethylenediamine (D), and combinations thereof. 24. The process according to any of statements 1 to 23, wherein the at least one comonomer other than terephthalic acid, adipic acid, and hexamethylenediamine is isophthalic acid (I), preferably the copolyamide product comprises up to 4.5 m%, preferably 0.5 to 4.5 m%, preferably 2.0 to 4.5 m%, of the isophthalic acid (I), optionally in combination with 2-methylpentamethylenediamine (D). 25. The process according to any of statements 1 to 24, wherein the at least one comonomer other than terephthalic acid, adipic acid, and hexamethylenediamine is 2-methylpentamethylenediamine (D), preferably wherein the copolyamide product comprises 0.5 to 6.0 m%, preferably 2.0 to 6.0 m%, preferably 2.0 to 5.5 m%, preferably 2.0 to 5.0 m%, preferably 2.0 to 4.5 m% of the 2-methylpentamethylenediamine (D), optionally in combination with isophthalic acid (I). 26. The process of any of statements 1 to 25, wherein the copolyamide product is a semicrystalline copolyamide. 27. The process of any of statements 1 to 26, wherein the copolyamide product exhibits a relative viscosity, measured in a 1.0 wt. / vol.% solution of the copolyamide sample in 96% sulfuric acid according to ASTM D789 method, in the range of 1.8 to 2.8 and an amine end group content in the range of 15 to 100 mpmg. 28. The process according to any of statements 1 to 27, wherein the copolyamide product exhibits a crystallization temperature of greater than 220.0°C, preferably at least 222.0°C, preferably greater than 225.0°C, preferably at least 227.0°C, preferably at least 230.0°C, and preferably equal to or less than 260.0°C, preferably equal to or less than 255.0°C, preferably equal to or less than 250.0°C, preferably the crystallization temperature of the copolyamide product is in the range of greater than 220.0°C to equal to or less than 260.0°C, preferably in the range of at least 222.0°C to equal to or less than 260.0°C, preferably in the range of greater than 225.0°C to equal to or less than 260.0°C, preferably in the range of at least 227.0°C to equal to or less than 260.0°C, preferably at least 230.0°C, preferably equal to or less than 255.0°C, preferably equal to or less than 250.0°C. 29. The process of any of statements 1 to 28, wherein the copolyamide product exhibits a melting point of less than or equal to 320.0°C, preferably at least 250.0°C, and preferably the melting point of the copolyamide product is in the range of 250.0 to 320.0°C. 30. A copolyamide made according to the process described in any of statements 1 to 29. 31. A copolyamide containing monomer units derived from terephthalic acid, adipic acid, hexamethylenediamine, at least one comonomer other than terephthalic acid, adipic acid, and hexamethylenediamine, and an endcapping agent, wherein the copolyamide has a relative viscosity in the range of 1.8 to 2.8, as measured in a 1.0 wt. / vol.% solution of a sample of the copolyamide in 96% sulfuric acid according to ASTM D789 method, and an amine end group content preferably in the range of 15 to 160 mpmg. 32. The copolyamide according to statement 31, wherein the copolyamide is as defined in any of statements 12 to 30. Measurement and testing
[0063] The molecular weight of polyamide resins is typically estimated by measuring solution viscosity. The two most common methods are (i) ASTM D789 for measuring relative viscosity (RV), and (ii) ISO 307, which uses sulfuric acid to obtain viscosity number (VN) values. The viscosity values and trends considered are determined by the same method, regardless of which method is chosen.
[0064] The terms "RV" or "RVF" as used herein in the Examples refer to the relative viscosity of a polymer sample measured in an 8.4 wt. % solution in 90% formic acid according to ASTM D789 (unless otherwise indicated).
[0065] The term "RVS" refers to the relative viscosity measured in a 1.0 w / v % solution of a polymer sample in 96% sulfuric acid according to ASTM D789.
[0066] The term "VNF" refers to the viscosity number obtained from a 0.5 w / v % solution of a polymer sample in 90% formic acid, according to ISO 307.
[0067] The term "VNS" refers to the viscosity number obtained from a 0.5% w / v solution of a polymer sample in 96% sulfuric acid, according to ISO 307.
[0068] Polymer amine ends can be measured by direct titration of a weighed sample of polymer taken in solution with a standardized perchloric acid solution. In a preferred method, approximately 1.5000 g of accurately weighed dry polyamide is dissolved in 50 mL of a 68 w / v% solution of phenol in methanol at approximately 75° C. The cooled solution (approximately 25° C.) is titrated with a standardized solution of 0.05 M perchloric acid in 1-propanol using an automatic titrator (Metrohm 905 Titranado, Tiamo Software and accessories). The results of the amine end group (AEG) concentration are reported in moles per million grams (mpmg), which is equivalent to mmol / Kg. Other suitable solvents include 80 w% phenol in methanol, or m-cresol. A few drops of an indicator such as a mixture of 0.1 w% methyl orange and 0.1 w% xylene cyanol in water can be added to aid in visual detection of the end point.
[0069] Melting and crystallization transitions were determined by differential scanning calorimetry on a Perkin Elmer DSC 8500 under nitrogen atmosphere. Accurately weighed amounts of 5-20 mg of polymer were used. The following heating method was used: (i) Initial heating at 10°C / min to 30°C to 300°C (or a higher temperature at least 10°C above the end of the melting process); (ii) holding at the final temperature from step (i) for 1 minute, then cooling at 50°C / min back to 30°C; (iii) reheating at 10°C / min to 300°C (or at least 10°C higher than the end of the melting process); (iv) Hold at the final temperature from step (iii) for 1 minute then cool at 50°C / min back to 30°C.
[0070] The enthalpy of melting (ΔHm) was determined for each heating step. From the first cooling step, the crystallization onset temperature (Tc1,o) was determined, which is referred to herein as the "crystallization temperature" of the polymer unless otherwise indicated. From the reheating step, the melting process end temperature (Tm2,e) was determined, which is referred to herein as the "melting temperature" (or "melting point") of the polymer unless otherwise indicated. EXAMPLES
[0071] Example 1 (E1.1) PA66 / 6T / 6I 58 / 40 / 2m% 40m% 6T formulation containing hexamethylenediamine, adipic acid, and isophthalic acid as a comonomer other than terephthalic acid. Acetic acid [AcOH] was used as the end-capping agent.
[0072] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 6361 g of demineralized water, 4110 g (15.67 mol) of nylon 66 salt, 1794 g (10.8 mol) of terephthalic acid, 89.7 g (0.54 mol) of isophthalic acid, and 24.3 g (0.4 mol) of acetic acid. 2375 g of a 56 wt % solution of hexamethylenediamine (1330 g, 11.44 mol) in water was added via a peristaltic pump while maintaining the temperature at 80°C. This produced a solution having a 66 / 6T / 6I molar ratio of about 58 / 40 / 2, containing 1.5 m% additional acetic acid based on the combined moles of adipic acid, terephthalic acid, and isophthalic acid, and 0.4 m% excess hexamethylenediamine based on the combined moles of adipic acid, terephthalic acid, and isophthalic acid, at a concentration of about 49 w%.
[0073] This solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 4.6 g sodium hypophosphite hydrate (0.43 moles, equivalent to 212 ppm P in the final polymer) and 0.59 g of a 50 wt % aqueous solution of Silwet L7605 antifoam agent (47 ppm active ingredient on a final polymer basis).
[0074] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 198°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 14 minutes, by which time the temperature of the contents had risen to approximately 217°C. In the third cycle, the venting continued for 48 minutes while the system was kept at 265 psia until the temperature of the contents reached 254°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 35 minutes and the temperature of the contents increased to 290°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 500 mbar over 11 minutes, held at 500 mbar for 4 minutes, the vacuum was released with nitrogen over 1 minute, and the temperature reached 294°C. In the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 80 psia. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The vessel contains the residual polymer, the heel, and is ready for the next batch for processing.
[0075] The second batch (E1.2) processed on the first heel was processed in essentially the same manner as the first. The polymer cast well without thick / thin race issues, was of good and consistent viscosity, had no visible signs of unmelted material, and was pelletizable.
[0076] Four more batches (E1.3, E1.4, E1.5, E1.6) continued to be processed in this continuous batch mode, with the final batch (the fifth batch as a batch-on-heel batch) casting as well as the second batch (the first batch on the heel) had. Comparative Example 1A (CE1A.1) PA66 / 6T 60 / 40m% [No "I" or "D" comonomer]
[0077] 40m% 6T formulation containing no comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid. Acetic acid was used as the endcapping agent.
[0078] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere were added 6467 g of demineralized water, 4250 g (16.2 moles) of nylon 66 salt, 1794 g (10.8 moles) of terephthalic acid, and 24.3 g (0.4 moles) of acetic acid. While maintaining a temperature of 80° C., 2113 g of a 60 wt % aqueous solution of hexamethylenediamine (1268 g, 10.91 moles) was added via a peristaltic pump. This produced a solution with a 66 / 6T molar ratio of about 60 / 40, containing 1.5 m% additional acetic acid based on the combined moles of adipic acid and terephthalic acid, and 0.4 m% excess hexamethylenediamine based on the combined moles of adipic acid and terephthalic acid, at a concentration of about 49 wt %.
[0079] This solution was added to the 24 L autoclave used in Example 1 along with 4.55 g (0.04 mol) of sodium hypophosphite hydrate (yielding 210 ppm P in the final polymer) and 0.57 g of Silwet L7605 (50%, yielding 45 ppm active defoamer on a final polymer basis).
[0080] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 198°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 15 minutes, by which time the temperature of the contents had risen to approximately 218°C. In the third cycle, the venting continued for 54 minutes while the system was held at 265 psia until the temperature of the contents reached 255°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 35 minutes and the temperature of the contents increased to 297°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 500 mbar over 11 minutes, held at 500 mbar for 4 minutes, the vacuum was released with nitrogen over 1 minute, and the temperature reached 299°C. On the sixth cycle, upon casting, there was a small plug of material initially, this plug was removed and good casting took place thereafter without any thick / thin race issues, the extruded polymer was of good, consistent viscosity and had no visible signs of unmelted material. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The vessel contained residual polymer, heel and was ready for the next batch for processing.
[0081] A second batch (CE1A.2) was processed on the first heel in essentially the same manner as the first. Casting failure ensued, evident in the formation of thick and thin laths due to apparent viscosity fluctuations as the lath was extruded from the autoclave, with the thick sections described as "gel-like." It was not possible to form a lath that was consistent enough to pelletize the material, and the remainder of the polymer contents in the autoclave was discarded into a metal bucket.
[0082] This comparative example shows that it was not possible to carry out successive batches and achieve good casting performance, as compared to Example 1, which had the advantage of incorporating small amounts of another comonomer in addition to hexamethylenediamine, adipic acid, and terephthalic acid. Comparative Example 1B (CE1B.1) PA66 / 6T 60 / 40m% [No "I" or "D" comonomer]
[0083] 40m% 6T formulation containing no comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid. Acetic acid was used as the endcapping agent.
[0084] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere, 4464 g of demineralized water, 1622 g (11.08 moles) of adipic acid, 1228 g (7.39 moles) of terephthalic acid were added, 2650 g of an 80 wt % aqueous solution of hexamethylenediamine (HMD) was added via a peristaltic pump (2120 g, 18.24 moles) while maintaining the temperature at 80° C., and the pH was adjusted to 7.50 (diluted to a 9.5 wt % solution, 25° C.) by adding an additional 58 g of 80% HMD solution (total HMD 2178 g, 18.64 moles). This produced a solution of approximately 50 wt % concentration with a 66 / 6T molar ratio of approximately 60 / 40.
[0085] This solution was added to a clean 15 L electrically heated autoclave along with 16.7 g (0.28 moles) of acetic acid [1.5 m% acetic acid based on the combined moles of adipic and terephthalic acids] and 1.74 g (0.016 moles) of sodium hypophosphite hydrate (yielding 115 ppm P in the final polymer) and 0.4 g of Silwet L7605 (50%, yielding 46 ppm active defoamer on a final polymer basis).
[0086] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 206°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 20 minutes, by which time the temperature of the contents had risen to approximately 228°C. In the third cycle, the venting continued for 34 minutes while the system was held at 265 psia until the temperature of the contents reached 260°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 30 minutes and the temperature of the contents increased to 294°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 350 mbar over 12 minutes, held at 350 mbar for 3 minutes, the vacuum was released with nitrogen over 1 minute, and the temperature reached 301°C. In the sixth cycle, using a maximum nitrogen pressure of 30 psia, the polymer was extruded from the autoclave through the bottom extrusion valve and the cast was of good, consistent viscosity with no visible signs of unmolten material. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The vessel contained the residual polymer, the heel, and was ready for the next batch for processing.
[0087] A second batch (CE1B.2) was processed on the first heel and in essentially the same manner as the first. Casting failure ensued, evident in the formation of thick and thin laths due to apparent viscosity fluctuations as the lath was extruded from the autoclave, with the thick sections described as "lumpy." It was not possible to form a sufficiently consistent lath to pelletize the material.
[0088] This comparative example shows that compared to Example 1, which had the advantage of incorporating a small amount of another comonomer in addition to the hexamethylenediamine, adipic acid, and terephthalic acid monomers, and acetic acid as an endcapper, it was not possible to run successive batches at the 40m% 6T level and achieve good casting performance when the endcapping agent was present but no other comonomer was present. Example 2 (E2.1) PA66 / 6T / 6I 63 / 35 / 2m%
[0089] 35m% 6T formulation containing hexamethylenediamine, adipic acid, and isophthalic acid as a comonomer other than terephthalic acid. Acetic acid was used as the endcapping agent.
[0090] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 6333 g of demineralized water, 4616 g (17.59 mol) of nylon 66 salt, 1624 g (9.78 mol) of terephthalic acid, 93.0 g (0.56 mol) of isophthalic acid, and 25.2 g (0.4 mol) of acetic acid. 2425 g of a 50 wt % solution of hexamethylenediamine (1213 g, 10.34 mol) in water was added via a peristaltic pump while maintaining the temperature at 80°C. This produced a solution of about 50 wt % concentration having a 66 / 6T / 6I molar ratio of about 63 / 35 / 2, containing 1.5 m % additional acetic acid based on the combined moles of adipic acid, terephthalic acid, and isophthalic acid, and 0.35 m % excess hexamethylenediamine based on the combined moles of adipic acid, terephthalic acid, and isophthalic acid.
[0091] This solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 4.69 g sodium hypophosphite hydrate (0.44 moles, equivalent to 210 ppm P in the final polymer) and 0.59 g of a 50 wt % aqueous solution of Silwet L7605 antifoam agent (45 ppm active ingredient based on final polymer).
[0092] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 198°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 15 minutes, by which time the temperature of the contents had risen to about 217°C. In the third cycle, the venting was continued for 60 minutes while the system was kept at 265 psia until the temperature of the contents reached 254°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 35 minutes, the temperature of the contents reached 296°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 500 mbar over 9 minutes, held at 500 mbar for 2 minutes, the vacuum was released with nitrogen over 1 minute, and the temperature reached 298°C. In the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 25 psia. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The vessel contains the residual polymer, the heel, and is ready for the next batch for processing.
[0093] A second batch (E2.2) processed on the first heel was processed in essentially the same manner as the first. The polymer cast well without thick / thin race issues, was of good and consistent viscosity similar to the first batch, had no visible signs of unmelted material, and was pelletizable.
[0094] Two more batches (E2.3, E2.4) continued to be processed in this continuous batch mode, and the final batch (the fourth batch, i.e. the third batch as a batch-on-heel batch) cast as well as the second batch (the first batch on the heel) had cast. Comparative Example 2A (CE2A.1) PA66 / 6T 65 / 35m% [No "I" or "D" comonomer]
[0095] A 35m% 6T formulation containing no comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid. Acetic acid was used as the endcapping agent.
[0096] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere were added 6412 g of demineralized water, 4604 g (17.5 moles) of nylon 66 salt, 1570 g (9.45 moles) of terephthalic acid, and 24.3 g (0.35 moles) of acetic acid. While maintaining a temperature of 80° C., 1981 g of a 56 wt % aqueous solution of hexamethylenediamine (1109 g, 9.55 moles) was added via a peristaltic pump. This produced a solution of approximately 50 wt % concentration having a 66 / 6T molar ratio of approximately 65 / 35, containing 1.5 m % additional acetic acid based on the combined moles of adipic acid and terephthalic acid, and 0.35 m % excess hexamethylenediamine based on the combined moles of adipic acid and terephthalic acid.
[0097] This solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 4.53 g sodium hypophosphite hydrate (0.44 moles, equivalent to 210 ppm P in the final polymer) and 0.57 g of a 50 wt % aqueous solution of Silwet L7605 antifoam agent (45 ppm active ingredient based on final polymer).
[0098] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 198°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 16 minutes, by which time the temperature of the contents had risen to about 217°C. In the third cycle, the venting continued for 70 minutes while the system was held at 265 psia until the temperature of the contents reached 253°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 35 minutes, the temperature of the contents reached 299°C. In the fifth cycle, a vacuum was applied and the pressure was reduced to 500 mbar over 11 minutes, held at 500 mbar for 4 minutes, the vacuum was released with nitrogen over 1 minute, and the temperature was 300°C. In the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 38 psia.
[0099] The polymer cast well without thick / thin race issues, was of good, consistent viscosity, and had no visible signs of unmelted material. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The container contained residual polymer, heel, and was ready for the next batch for processing.
[0100] A second batch (CE2A.2) was processed on the first heel and in essentially the same manner as the first. The polymer gave good casts but was clearly of lower melt viscosity than the first batch.
[0101] A third batch (CE2A.3) was processed on a second heel and in essentially the same manner as the first. The casting performance of the polymer was similar to the second batch and was of reasonable quality, but had a lower melt viscosity.
[0102] A fourth batch (CE2A.4) was processed on the third heel and in essentially the same manner as the first. The fourth batch (CE2A.4) could be cast but had signs of air bubbles and "unmelted material" during racing.
[0103] This comparative example shows that at the 35m% 6T level, with the endcapping agent present but no other comonomers present, as the number of successive batches increases, the casting performance deteriorates after only a few successive batches are performed, as compared to Example 2, in which there was incorporation of a small amount of another comonomer in addition to hexamethylenediamine, adipic acid, and terephthalic acid monomers, and acetic acid as an endcapper, and the casting performance remained good without signs of bubbles or "unmelt". Comparative Example 2B (CE2B.1) PA66 / 6T 65 / 35m% [No "I" or "D" comonomer]
[0104] A 35m% 6T formulation containing no comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid. Acetic acid was used as the endcapping agent.
[0105] In a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere, a solution containing 7500 g of demineralized water, 2645 g of adipic acid (18.10 moles), 1619 g (9.75 moles) of terephthalic acid, and 3236 g of hexamethylenediamine (27.85 moles) was prepared at a temperature of 80° C. This produced a solution of approximately 50 wt % concentration with a 66 / 6T molar ratio of approximately 65 / 35.
[0106] This solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 2.60 g of sodium hypophosphite hydrate (0.025 moles, equivalent to 117 ppm P in the final polymer), 25.37 g of acetic acid (0.42 moles, which was 1.5 m% based on the combined moles of adipic acid and terephthalic acid), and 1.8 g of a 10 wt % solution of Ambersil AF 1316 defoamer in water (28 ppm active ingredient based on final polymer).
[0107] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 198 °C. In the second cycle, venting was stopped and the pressure was increased to 265 psia over 12 minutes, by which time the temperature of the contents had risen to approximately 221 °C. In the third cycle, venting was continued for 49 minutes while the system was held at 265 psia until the temperature of the contents reached 258 °C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 35 minutes, the temperature of the contents reached 284 °C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 350 mbar over 15 minutes, held at 350-400 mbar for 5 minutes, the vacuum was released with nitrogen over 5 minutes, and the temperature was 293 °C. In the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 35 psia.
[0108] The polymer cast well without thick / thin race issues, was of good, consistent viscosity, and had no visible signs of unmelted material. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The container contained residual polymer, heel, and was ready for the next batch for processing.
[0109] A second batch (CE2B.2) was processed on the first heel and in essentially the same manner as the first. Upon extrusion, "high melt" was visible and the batch could not be cast and pelletized.
[0110] This comparative example shows that at the 35m% 6T level, when the endcapping agent was present but no other comonomers were present, the casting performance was very poor, even for the first batch on the heel, compared to Example 2, where there was incorporation of a small amount of another comonomer in addition to hexamethylenediamine, adipic acid, and terephthalic acid monomers, and acetic acid as an endcapper, and the casting performance remained good without any signs of bubbles or "unmelt". Comparative Example 3A (CE3A) PA66 / 6T 70 / 30m% [No "I" or "D" Comonomer]
[0111] A 30m% 6T formulation containing no comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid, and no acetic acid as an end-capping agent.
[0112] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 5000 g of demineralized water, 3422 g (13.04 moles) of nylon 66 salt, and 1578 g (5.59 moles) of anhydrous nylon 6T salt. This produced a solution of approximately 50 wt % concentration with a 66 / 6T molar ratio of approximately 70 / 30. This solution was transferred to a clean 15 L electrically heated autoclave.
[0113] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 209°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 18 minutes, by which time the temperature of the contents had risen to approximately 229°C. In the third cycle, the venting continued for 38 minutes while the system was held at 265 psia until the temperature of the contents reached 270°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 30 minutes and the temperature of the contents was increased to 285°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 660 mbar over 10 minutes, held at 660 mbar for 6 minutes, the vacuum was released with nitrogen over 1 minute, and the temperature was 285°C. In the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 30 psia, and the cast was good and consistent, but with a visibly high melt viscosity and no visible signs of unmolten material. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The polymer was found to have an RVS of 2.43. Comparative Example 3B (CE3B) PA66 / 6T 70 / 30m% [No "I" or "D" Comonomer]
[0114] A 30m% 6T formulation containing no comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid, and containing 0.5m% acetic acid as an end-capping agent.
[0115] The same salt procedure as in Comparative Example 3A was used, except for the addition of 5.6 g (0.093 moles) of acetic acid. This produced a solution with a concentration of about 50 w% with a 66 / 6T molar ratio of about 70 / 30 and 0.5 m% acetic acid based on the combined moles of terephthalic acid and adipic acid making up the salt. This solution was transferred to a clean 15 L electrically heated autoclave.
[0116] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 211°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 20 minutes, by which time the temperature of the contents had risen to approximately 232°C. In the third cycle, the venting continued for 32 minutes while the system was held at 265 psia until the temperature of the contents reached 270°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 30 minutes and the temperature of the contents was increased to 281°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 645 mbar over 10 minutes, held at 645 mbar for 7 minutes, the vacuum was released with nitrogen over 1 minute, and the temperature was 281°C. On the sixth cycle, using a maximum nitrogen pressure of 30 psia, the polymer was extruded from the autoclave through the bottom extrusion valve and the cast was good, with consistent melt viscosity, no thinning or bubbles, and no visible signs of unmelted material. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The polymer was found to have an RVS of 2.22. Comparative Example 3C (CE3C) PA66 / 6T 70 / 30m% [No "I" or "D" Comonomer]
[0117] A 30m% 6T formulation containing no comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid, and containing 1.5m% acetic acid as an end-capping agent.
[0118] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 7500 g of demineralized water, 5133 g (19.56 moles) of nylon 66 salt, and 2367 g (8.38 moles) of anhydrous nylon 6T salt, producing a solution of approximately 50 wt % concentration with a 66 / 6T molar ratio of approximately 70 / 30.
[0119] This solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 25.0 g (0.417 moles) of acetic acid, 2.61 g of sodium hypophosphite hydrate (0.025 moles, equivalent to 117 ppm P in the final polymer), and 1.8 g of Ambersil AF 1316 (10% antifoam as an aqueous emulsion, 28 ppm active additive based on final weight polymer).
[0120] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 199 °C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 10 minutes, by which time the temperature of the contents had risen to approximately 217 °C. In the third cycle, the venting continued for 45 minutes, while the system was held at 265 psia, until the temperature of the contents reached 257 °C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 36 minutes, and the temperature of the contents increased to 292 °C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 300 mbar over 15 minutes, held at 300-350 mbar for 9 minutes, the vacuum was released with nitrogen over 1 minute, and the temperature was 298 °C. On the sixth cycle, using a maximum nitrogen pressure of 30 psia, the polymer was extruded from the autoclave through the bottom extrusion valve and the cast was good, with consistent melt viscosity, no thinning or bubbles, and no visible signs of unmelted material. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The polymer was found to have an RVS of 2.05.
[0121] Comparative Examples 3A, 4 3B, and 3C are single batches on a clean autoclave (no continuous batches) and they demonstrate the well-known effect in the art of how adding an endcapping agent (as done in GB 1,114,541, Published Application No. 61,159,422, EP 3,502,165) limits the molecular weight, even in the presence of a catalyst, and thereby the melt viscosity as reflected in the relative viscosity value of the solution (RVS). What has not been disclosed, suggested, or explored in the art is whether the use of sufficient endcapping agent alone would allow the process for continuous batches. Comparative Example 3D (CE3D) PA66 / 6T 70 / 30m% [No "I" or "D" Comonomer]
[0122] A 30m% 6T formulation containing no comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid, and no acetic acid as an end-capping agent.
[0123] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 6871 g of demineralized water, 5132 g (19.56 moles) of nylon 66 salt, 1392 g (8.38 moles) of terephthalic acid, and 1620 g of 60% hexamethylenediamine (8.31 moles), producing a solution of approximately 50 wt % concentration with a 66 / 6T molar ratio of approximately 70 / 30.
[0124] This solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 4.70 g of sodium hypophosphite hydrate (0.044 moles, equivalent to 212 ppm P in the final polymer) and 1.8 g of Ambersil AF 1316 (10% antifoam as an aqueous emulsion, 28 ppm active additive based on final weight polymer).
[0125] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 198°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 15 minutes, by which time the temperature of the contents had risen to approximately 217°C. In the third cycle, the venting continued for 67 minutes while the system was held at 265 psia until the temperature of the contents reached 256°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 30 minutes and the temperature of the contents increased to 292°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 620 mbar over 3 minutes, held at 620 mbar for 17 minutes, the vacuum was released with nitrogen over 1 minute, and the temperature was 297°C. In the sixth cycle, an attempt was made to extrude the polymer from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 88 psia, but the polymer was too viscous and would not form a race for casting, and a small sample for analytical purposes was all that was recovered. The polymer had an RV of 3.13 and an AEG of 31.6 mpmg.
[0126] Comparative Example 3D (CE3D) demonstrates that even at a 30m% 6T level for a single batch made on a clean autoclave where no endcapping agent was used, overpolymerization of the polymer can occur, rendering the polymer uncastable. Thus, one skilled in the art would have to select polymerization conditions and formulations that would allow a first batch to be made and cast before attempting to make and cast a successive batch on the heel of the previous batch. Comparative Example 3E (CE3E.1) PA66 / 6T 70 / 30m% [No "I" or "D" Comonomer]
[0127] A 30m% 6T formulation containing no comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid, and containing 0.5m% acetic acid as an end-capping agent.
[0128] The same salt procedure as in Comparative Example 3D (CE3D) was used, except for the addition of 8.4 g (0.14 moles) of acetic acid, which produced a solution of approximately 50 wt % concentration with a 66 / 6T molar ratio of approximately 70 / 30 and 0.5 m % acetic acid based on the combined moles of terephthalic and adipic acids making up the salt.
[0129] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 198°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 13 minutes, by which time the temperature of the contents had risen to approximately 217°C. In the third cycle, the venting continued for 50 minutes while the system was held at 265 psia until the temperature of the contents reached 256°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 30 minutes and the temperature of the contents increased to 281°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 620 mbar over 3 minutes, held at 620 mbar for 17 minutes, the vacuum was released with nitrogen over 1 minute, and the temperature was 287°C. In the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 71 psia, and the cast was good and consistent in that it was not too viscous and showed no signs of unmelted, bubbles, or thins. The RV of the batch was found to be 2.68.
[0130] A second batch (CE3E.2) was processed on the heel of the first and in essentially the same manner as the first. The second batch (CE3E.2) produced good casting performance like the first batch, but had a reduced RV of 2.16.
[0131] Comparative Example 3E demonstrates that at a 6T level of 30m%, with the endcapping agent present but no other comonomer present, at least one successive batch could be made on the heel of the previous batch with good casting performance, but other undesirable effects also occurred, in this case a drop in RV from the first batch to the second batch. Example 4 (E4.1) PA 66 / 6T / 6I 69 / 29 / 2m%
[0132] A 29m% 6T formulation in which isophthalic acid is used as the comonomer other than hexamethylenediamine, adipic acid, and terephthalic acid, along with 1.5m% acetic acid as an end-capping agent.
[0133] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 7260 g of demineralized water, 5059 g (19.28 moles) of nylon 66 salt, 1346 g (8.10 moles) of terephthalic acid, and 93 g (0.56 moles) of isophthalic acid. While maintaining a temperature of 80° C., 1258 g of an 80 w% aqueous solution of hexamethylenediamine (1006 g, 8.66 moles) was added via a peristaltic pump. This produced a solution of approximately 50 w% concentration with a 66 / 6T / 6I molar ratio of approximately 69 / 29 / 2 m%.
[0134] This solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 25.2 g (0.42 moles) of acetic acid (1.5 m% based on total terephthalic, isophthalic, and adipic acid) and 1.8 g of Ambersil AF 1316 (10% solution, 28 ppm active ingredient based on final polymer).
[0135] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 194°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 9 minutes, by which time the temperature of the contents had risen to approximately 216°C. In the third cycle, the venting continued for 48 minutes while the system was held at 265 psia until the temperature of the contents reached 253°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 35 minutes and the temperature of the contents increased to 288°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 500 mbar over 10 minutes, held at 500 mbar for 2 minutes, the vacuum was released with nitrogen over 5 minutes, and the temperature was 293°C. On the sixth cycle, using a maximum nitrogen pressure of 35 psia, the polymer was extruded from the autoclave through the bottom extrusion valve, the cast was good, with consistent melt viscosity, no thinning or bubbles, and no visible signs of molten material. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed.
[0136] A second batch (E4.2) was processed on the first heel and in essentially the same manner as the first. The polymer gave a good cast.
[0137] A third batch (E4.3) was processed on a second heel in essentially the same manner as the first. The polymer gave a good cast.
[0138] A fourth batch (E4.4) was processed on the third heel in essentially the same manner as the first. The polymer gave a good cast.
[0139] Example 4 demonstrates that at a 6T level of 29m%, when an endcapping agent and at least one other comonomer are present, the commoner does not impair the ability to use a process that allows successive batches to be made on the heel of the previous batch while still providing good and acceptable casting performance. Example 5 (E5.1) PA66 / 6T / 6I 62 / 32 / 6m%
[0140] A 32m% 6T formulation in which isophthalic acid is used as the comonomer other than hexamethylenediamine, adipic acid, and terephthalic acid, along with 1.5m% acetic acid as an end-capping agent.
[0141] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 7260 g of demineralized water, 4546 g (17.33 moles) of nylon 66 salt, 1485 g (8.94 moles) of terephthalic acid, and 278 g (1.67 moles) of isophthalic acid. While maintaining a temperature of 80° C., 1542 g of an 80 w% aqueous solution of hexamethylenediamine (1234 g, 10.62 moles) was added via a peristaltic pump. This produced a solution of approximately 50 w% concentration with a 66 / 6T / 6I molar ratio of approximately 62 / 32 / 6 m%.
[0142] This solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 25.2 g (0.42 moles) of acetic acid (1.5 m% based on total terephthalic, isophthalic, and adipic acid) and 1.8 g of Ambersil AF 1316 (10% solution, 29 ppm active ingredient based on final polymer).
[0143] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 194°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 9 minutes, by which time the temperature of the contents had increased to about 216°C. In the third cycle, the venting continued for 52 minutes while the system was kept at 265 psia until the temperature of the contents reached 253°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 35 minutes and the temperature of the contents increased to 289°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 500 mbar over 9 minutes, held at 500 mbar for 2 minutes, the vacuum was released with nitrogen over 1 minute, and the temperature was 292°C. In the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 35 psia. When extruded, the molten race was of consistent melt viscosity, without any thin or air bubbles, and no visible signs of unmelted material. Cooling of the polymer race in the water chute provided an amorphous race that was optimized for pelletization by slightly extending the cooling length of the water chute relative to other inventive examples reported herein. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed.
[0144] The second batch (E5.2), when processed and cast on the first heel, gave crystalline lacy on cooling in the water chute. The polymer gave good casting and was easily pelletized.
[0145] A third batch (E5.3) was processed on a second heel and in essentially the same manner as the second. The polymer gave a good cast.
[0146] The fourth batch (E5.4) was processed with a third heel and in essentially the same manner as the second batch. The polymer gave a good cast.
[0147] Example 5 shows that at relatively higher levels of comonomer, the rate of crystallization of the copolyamide may be suppressed, so that relatively more cooling may be appropriate for optimal pelletization. Example 5 also shows that the heel of a previous batch may affect the crystallization behavior of a subsequent batch, thereby inducing nucleation and crystallization, which is beneficial for pelletization in this example. Example 6 (E6.1) PA 66 / 6T / 6I 64 / 34 / 2m%
[0148] A 34m% 6T formulation in which isophthalic acid is used as the comonomer other than hexamethylenediamine, adipic acid, and terephthalic acid, along with 1.5m% acetic acid as an end-capping agent.
[0149] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 7260 g of demineralized water, 4692 g (17.88 moles) of nylon 66 salt, 1578 g (9.50 moles) of terephthalic acid, and 93 g (0.56 moles) of isophthalic acid. While maintaining a temperature of 80° C., 1461 g of an 80 w% aqueous solution of hexamethylenediamine (1169 g, 10.06 moles) was added via a peristaltic pump. This produced a solution of approximately 50 w% concentration with a 66 / 6T / 6I molar ratio of approximately 64 / 34 / 2 m%.
[0150] This solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 25.2 g (0.42 moles) of acetic acid (1.5 m% based on total terephthalic, isophthalic, and adipic acid) and 1.8 g of Ambersil AF 1316 (10% solution, 28 ppm active ingredient based on final polymer).
[0151] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 194°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 11 minutes, by which time the temperature of the contents had risen to approximately 216°C. In the third cycle, the venting was continued for 47 minutes, while the system was kept at 265 psia, until the temperature of the contents reached 253°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 36 minutes, and the temperature of the contents increased to 286°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 500 mbar over 9 minutes, held at 500 mbar for 2 minutes, the vacuum was released with nitrogen over 1 minute, and the temperature was 292°C. In the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 35 psia. The polymer solidified in the water chute into a semi-crystalline polymer. Once the nitrogen blow-through had occurred, the pressure was released and the extrusion valve was sealed.
[0152] The second batch (E6.2), when processed on the first heel and cast, gave crystalline lace upon cooling in the water chute and occasional high melts were observed. The polymer cast well and was easily pelletized.
[0153] A third batch (E6.3) was processed on a second heel in essentially the same manner as the second, with occasional high melts observed. The polymer cast well and was easily pelletized.
[0154] A fourth batch (E6.4) was processed on a third heel in essentially the same manner as the second, and although some high melt was observed, the polymer cast well and was easily pelletized.
[0155] Example 6 demonstrates that at the 34m% 6T level, the presence of an endcapping agent and at least one other comonomer allows successive batches to be made on the heel of the previous batch, and these successive batches cast well without issues of thick / thin races and good, consistent viscosity. Example 7 (E7.1) PA 66 / 6T / DI 63 / 35 / 2m%
[0156] A 35m% 6T formulation containing isophthalic acid (I) and 2-methylpentamethylenediamine (D) as comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid. Acetic acid was used as the end-capping agent. Isophthalic acid and 2-methylpentamethylenediamine were both added at 2m% levels.
[0157] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 6731 g of demineralized water, 4628 g (17.64 moles) of nylon 66 salt, 1628 g (9.80 moles) of terephthalic acid, 93.0 g (0.56 moles) of isophthalic acid, 65.0 g of Dytek A (2-methylpentamethylenediamine, 0.56 moles), and 25.2 g (0.4 moles) of acetic acid. While maintaining the temperature at 80° C., 1912 g of a 60 wt % solution of hexamethylenediamine (1147 g, 9.87 moles) in water was added via a peristaltic pump. This produced a solution having a 66 / 6T / DI molar ratio of about 63 / 35 / 2, containing 1.5 m% additional acetic acid based on the combined moles of adipic acid, terephthalic acid, and isophthalic acid, and 0.26 m% excess hexamethylenediamine based on the combined moles of adipic acid, terephthalic acid, and isophthalic acid, at a concentration of about 50 wt %.
[0158] This solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 4.70 g sodium hypophosphite hydrate (0.44 moles, equivalent to 210 ppm P in the final polymer) and 0.59 g of a 50 wt % aqueous solution of Silwet L7605 antifoam agent (45 ppm active ingredient based on final polymer).
[0159] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 198°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 15 minutes, by which time the temperature of the contents had risen to about 217°C. In the third cycle, the venting continued for 70 minutes while the system was held at 265 psia until the temperature of the contents reached 255°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 35 minutes, and the temperature of the contents reached 297°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 550 mbar over 3 minutes, held at 550 mbar for 7 minutes, the vacuum was released with nitrogen, and the temperature reached 297°C. In the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 42 psia. The polymer cast well with no significant unmelted material or excessive bubbles in the lace. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The vessel contained the residual polymer, heel, and was ready for the next batch to be processed.
[0160] The second batch (E7.2) processed on the first heel was processed in essentially the same manner as the first. Although a small amount of thin lacing occurred (within acceptable limits), the polymer cast well, was of good and consistent viscosity, had no visible signs of unmelted material, and was pelletizable.
[0161] Two more batches (E7.3, E7.4) continued to be processed in this continuous batch mode, with the final batch (the fourth batch, i.e. the third batch as a batch-on-heel batch) casting as well as the first batch.
[0162] Example 7 demonstrates that at the 34m% 6T level, the presence of the endcapping agent and two other comonomers allows successive batches to be made on the heel of the previous batch, and these successive batches cast well without issues of thick / thin races, and generally good, consistent viscosity. Example 8 (E8.1) PA 66 / 6T / DI 58 / 40 / 2m%
[0163] A 40m% 6T formulation containing isophthalic acid (I) and 2-methylpentamethylenediamine (D) as comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid. Acetic acid was used as the end-capping agent. Isophthalic acid and 2-methylpentamethylenediamine were both added at 2m% levels.
[0164] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 6651 g of demineralized water, 4261 g (16.24 moles) of nylon 66 salt, 1861 g (11.2 moles) of terephthalic acid, 93.0 g (0.56 moles) of isophthalic acid, 65.0 g of Dytek A (2-methylpentamethylenediamine, 0.56 moles), and 25.2 g (0.4 moles) of acetic acid. 2186 g of a 60 wt % solution of hexamethylenediamine (1312 g, 11.29 moles) in water was added via a peristaltic pump while maintaining the temperature at 80°C. This produced a solution having a 66 / 6 T / DI molar ratio of about 58 / 40 / 2, containing 1.5 m% additional acetic acid based on the combined moles of adipic acid, terephthalic acid, and isophthalic acid, and 0.30 m% excess hexamethylenediamine based on the combined moles of adipic acid, terephthalic acid, and isophthalic acid, at a concentration of about 50 wt %.
[0165] This solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 4.70 g sodium hypophosphite hydrate (0.44 moles, equivalent to 210 ppm P in the final polymer) and 0.59 g of a 50 wt % aqueous solution of Silwet L7605 antifoam agent (45 ppm active ingredient based on final polymer).
[0166] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 198°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 17 minutes, by which time the temperature of the contents had risen to about 217°C. In the third cycle, the venting continued for 76 minutes while the system was held at 265 psia until the temperature of the contents reached 265°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 35 minutes, the temperature of the contents reached 306°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 550 mbar over 10 minutes, the vacuum was released with nitrogen, and the temperature was 305°C. In the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 44 psia. The polymer cast was good in that some development of thin lace was observed, but there was no significant unmelting. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The vessel contained the residual polymer, heel, and was ready for the next batch to be processed.
[0167] The second batch (E8.2) processed on the first heel was processed in essentially the same manner as the first. The polymer cast well, in that there was no significant unmelting, although some development of thin lace was observed.
[0168] Example 8 demonstrates that at the 40m% 6T level, the presence of the endcapping agent and two other comonomers allows successive batches to be made on the heel of the previous batch, with some occurrence of thin lace, but within acceptable limits. Example 9 (E9.1) PA 66 / 6T / DI 56 / 40 / 4m%
[0169] A 40m% 6T formulation containing isophthalic acid (I) and 2-methylpentamethylenediamine (D) as comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid. Acetic acid was used as the end-capping agent. Isophthalic acid and 2-methylpentamethylenediamine were both added at a level of 4m%.
[0170] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 6587 g of demineralized water, 4114 g (15.68 moles) of nylon 66 salt, 1861 g (11.2 moles) of terephthalic acid, 186.0 g (1.12 moles) of isophthalic acid, 130.0 g of Dytek A (2-methylpentamethylenediamine, 1.12 moles), and 25.2 g (0.4 moles) of acetic acid. 2186 g of a 60 wt % solution of hexamethylenediamine (1312 g, 11.29 moles) in water was added via a peristaltic pump while maintaining the temperature at 80°C. This produced a solution having a 66 / 6T / DI molar ratio of about 56 / 40 / 4, containing 1.5 m% additional acetic acid based on the combined moles of adipic acid, terephthalic acid, and isophthalic acid, and 0.30 m% excess hexamethylenediamine based on the combined moles of adipic acid, terephthalic acid, and isophthalic acid, at a concentration of about 50 wt %.
[0171] This solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 4.70 g sodium hypophosphite hydrate (0.44 moles, equivalent to 210 ppm P in the final polymer) and 0.59 g of a 50 wt % aqueous solution of Silwet L7605 antifoam agent (45 ppm active ingredient based on final polymer).
[0172] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 198°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 14 minutes, by which time the temperature of the contents had risen to about 217°C. In the third cycle, the venting continued for 70 minutes while the system was held at 265 psia until the temperature of the contents reached 265°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 34 minutes, the temperature of the contents reached 302°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 670 mbar over 3 minutes, held at 670 mbar for 10 minutes, the vacuum was released with nitrogen, and the temperature was 301°C. In the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 50 psia. The polymer cast was good in that there was no significant unmelt and few thin lace events were observed. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The vessel contained the residual polymer, heel, and was ready for the next batch to be processed.
[0173] The second batch (E9.2) processed on the first heel was processed in essentially the same manner as the first. The polymer cast well, in that there was no significant unmelt, very few thin lace events, and very few air bubbles.
[0174] Example 9 demonstrates that at a 6T level of 40m%, the presence of the endcapping agent and two other comonomers makes it possible to make successive batches on the heel of the previous batch, and that by increasing the levels of the two other comonomers compared to Example 8, the casting performance was very acceptable.
[0175] In the above examples and comparative examples, the temperature at the end of the high pressure cycle was always well below the melting point of the final polymer, as determined by either DSC analysis of the polymer produced in the example or comparative example, or from data generated by polymers of the same formulation. Example 10 (E10.1) PA 66 / 6T / 6I 63 / 35 / 2m%
[0176] A 35m% 6T formulation in which isophthalic acid is used as the comonomer other than hexamethylenediamine, adipic acid, and terephthalic acid, along with 1.5m% acetic acid as an end-capping agent.
[0177] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 6742 g of demineralized water, 4616 g (17.59 mol) of nylon 66 salt, 1624 g (9.78 mol) of terephthalic acid, and 93 g (0.56 mol) of isophthalic acid. 2009 g of a 60 wt % solution of hexamethylenediamine (1205 g, 10.37 mol) in water was added via a peristaltic pump while maintaining the temperature at 80°C.
[0178] This produced a solution of approximately 50 w% concentration with a 66 / 6T / 6I molar ratio of approximately 63 / 35 / 2 m%. 5 g of a 60 w% aqueous solution of hexamethylenediamine was added. A small sample of the salt mixture was diluted to 9.5 w% and the pH was measured to be 7.60.
[0179] The salt solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 25.2 g (0.42 moles) of acetic acid (1.5 m% based on total terephthalic, isophthalic, and adipic acid), 41 g of 60 wt % hexamethylenediamine (0.21 moles) to balance the acetic acid addition, 4.69 g of sodium hypophosphite (0.04 moles, 210 ppm phosphorus based on final polymer) added as catalyst, an additional 80 g of 60 wt % hexamethylenediamine in water (0.41 moles) added to increase the amine end group content in the final polymer, and 0.59 g of Silwet L7605 defoamer (50% solution, 45 ppm active ingredient based on final polymer).
[0180] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 198°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 14 minutes, by which time the temperature of the contents had risen to approximately 219°C. In the third cycle, the venting continued for 42 minutes while the system was held at 265 psia until the temperature of the contents reached 255°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 31 minutes and the temperature of the contents increased to 287°C. In the fifth cycle, a vacuum was applied, the pressure was reduced to 410 mbar over 2 minutes, held at 480 mbar for 10 minutes, the vacuum was released with nitrogen over 5 minutes, and the temperature was 287°C. On the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 45 psia; the cast was of good, consistent viscosity and no visible signs of unmolten material. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The polymer had an RVS of 2.40 and an AEG of 80.7 mpmg.
[0181] A second batch (E10.2) was processed on the first heel and was processed in essentially the same manner as the first.
[0182] A third batch (E10.3) was processed on a second heel in essentially the same manner as the first. The polymer gave a good cast.
[0183] A fourth batch (E10.4) was processed on the third heel and in essentially the same manner as the first. The polymer gave a good cast.
[0184] Example 10 demonstrates that at the 35m% 6T level, the presence of an endcapping agent and one other comonomer (isophthalic acid in this example), and excess hexamethylenediamine, allowed for successive batches to be made on the heel of the previous batch while still providing good and acceptable casting performance and also resulting in a product with high amine end group levels. Example 11 (E11.1) PA 66 / 6T / DI 63 / 35 / 2m%
[0185] A 35m% 6T formulation in which isophthalic acid and 2-methylpentamethylenediamine are used as comonomers other than hexamethylenediamine, adipic acid, and terephthalic acid, along with 1.5m% acetic acid as an end-capping agent.
[0186] To a 20 L temperature controlled jacketed glass vessel equipped with an overhead stirrer and condenser and maintained under a nitrogen atmosphere was added 6333 g of demineralized water, 4616 g (17.59 moles) of nylon 66 salt, 1624 g (9.78 moles) of terephthalic acid, 93 g (0.56 moles) of isophthalic acid, and 65 g of 2-methylpentamethylenediamine (0.56 moles, Dytek A®). 1895 g of a 60 wt % solution in water of hexamethylenediamine (1137 g, 9.79 moles) was added via a peristaltic pump while maintaining a temperature of 80°C.
[0187] This produced a solution of approximately 50 w% concentration with a 66 / 6T / DI molar ratio of approximately 63 / 35 / 2 m%. A small sample of the salt mixture was diluted to 9.5 w% and the pH was measured to be 7.60.
[0188] The salt solution was added to a clean 24 L oil heated autoclave equipped with a stirrer along with 25.2 g (0.42 moles) of acetic acid (1.5 m% based on total terephthalic, isophthalic, and adipic acid), 41 g of 60 wt % hexamethylenediamine (0.21 moles) to balance the acetic acid addition, 4.69 g of sodium hypophosphite (0.04 moles, 210 ppm phosphorus based on final polymer) added as catalyst, an additional 80 g of 60 wt % hexamethylenediamine in water (0.41 moles) added to increase the amine end group content in the final polymer, and 0.59 g of Silwet L7605 defoamer (50% solution, 45 ppm active ingredient based on final polymer).
[0189] In the first cycle, the solution was heated and vented when the pressure reached 170 psia and continued until the temperature reached 198°C. In the second cycle, the venting was stopped and the pressure was increased to 265 psia over 15 minutes, by which time the temperature of the contents had risen to about 217°C. In the third cycle, the venting continued for 49 minutes while the system was held at 265 psia until the temperature of the contents reached 255°C. In the fourth cycle, the pressure was reduced to atmospheric pressure over 33 minutes and the temperature of the contents increased to 291°C. In the fifth cycle, a vacuum was applied and the pressure was reduced to 480 mbar over 12 minutes, the vacuum was released with nitrogen over 5 minutes, and the temperature was 292°C. In the sixth cycle, the polymer was extruded from the autoclave through the bottom extrusion valve using a maximum nitrogen pressure of 45 psia and the cast was of good, consistent viscosity and no visible signs of unmelted material. When the nitrogen blow-through occurred, the pressure was released and the extrusion valve was sealed. The polymer had an RVS of 2.34 and an AEG of 86.6 mpmg.
[0190] A second batch (E11.2) was processed on the first heel and was processed essentially in the same manner as the first. The polymer had an RVS of 2.18 and an AEG of 85.5 mpmg.
[0191] A third batch (E11.3) was processed on the second heel in essentially the same manner as the first. The polymer gave a good cast. The polymer had an RVS of 2.50 and an AEG of 87.4 mpmg.
[0192] Example 11 demonstrates that at the 35m% 6T level, the presence of an endcapping agent and two other comonomers (isophthalic acid and 2-methylpentamethylenediamine), as well as excess hexamethylenediamine, allowed for successive batches to be made on the heel of the previous batch while still providing good and acceptable casting performance and also resulting in a product with high amine end group levels.
[0193] The DSC, RVS, and AEG results for the above examples are shown below in Tables 1A, 1B, and 1C.
[0194] [Table 1]
[0195] [Table 2]
[0196] [Table 3]
[0197] [Table 4]
[0198] [Table 5]
[0199] [Table 6]
[0200] [Table 7]
Claims
1. 1. A polymerization process for producing continuous batches of a copolyamide comprising terephthalic acid, adipic acid, and hexamethylenediamine, comprising: (a) introducing copolyamide monomer units of terephthalic acid, adipic acid, and hexamethylenediamine into a batch vessel to provide a reaction mixture; (b) introducing into said batch vessel an endcapping agent and at least one comonomer other than terephthalic acid, adipic acid, and hexamethylenediamine; (c) subjecting the batch container contents to conditions sufficient to form said copolyamide; (d) recovering the copolyamide product from said vessel; A polymerization process wherein the batch vessel is not cleaned between batches.
2. 2. The process of claim 1, wherein the process comprises producing a first batch of the copolyamide and recovering it from the batch vessel in accordance with steps (a)-(d), and further comprises producing a second batch of the copolyamide and optionally at least one subsequent batch of the copolyamide, the production steps of each of the second and optional subsequent batches corresponding to steps (a)-(d).
3. 3. The process according to claim 1 or 2, wherein, upon completion of step (d) in each production batch, a residual copolyamide product, defined as heel, remains in the batch vessel and the second and optional subsequent batches are processed on the heel of the preceding batch, preferably the amount of heel representing no more than 10% by weight of the maximum theoretical yield from the batch.
4. The process according to any one of claims 1 to 3, wherein the reaction mixture further comprises a solvent, preferably water.
5. 5. The process of any one of claims 1 to 4, wherein the terephthalic acid, adipic acid, hexamethylenediamine, endcapping agent, and other comonomers are contacted in a mixing vessel and then introduced into the batch vessel, preferably in the form of a feed solution.
6. 6. The process of any one of claims 1 to 5, wherein the adipic acid and a portion of the total amount of the hexamethylenediamine required to make the copolyamide are in the form of a nylon salt, preferably said portion being approximately stoichiometric amounts of the hexamethylenediamine relative to the amount of adipic acid.
7. 7. The process of claim 6, wherein the terephthalic acid, the salt, and the other comonomers are contacted in a mixing vessel and additional hexamethylenediamine is added thereto, and the endcapping agent can be contacted with the terephthalic acid, the salt, and the other comonomers, or can be added to a mixture comprising the terephthalic acid, the salt, and the other comonomers at the same time or in the same composition as the additional hexamethylenediamine.
8. 8. The process of any one of claims 1 to 7, wherein the total amount of diamines in the reaction mixture, preferably the total amount of hexamethylenediamine in the reaction mixture, is in excess relative to the combined molar amount of adipic acid, terephthalic acid, and any carboxylic acid containing compounds among the other comonomers, preferably the excess is 0.1 to 5.0 m % relative to the combined molar amount of adipic acid, terephthalic acid, and any carboxylic acid containing compounds among the other comonomers.
9. 9. The process of any one of claims 1 to 8, wherein the batch vessel is subjected to a maximum pressure of about 320 psia and the maximum temperature of the vessel contents during the maximum pressure stage is below the melting point of the final copolyamide product.
10. 10. The process of any one of claims 1 to 9, wherein the temperature of the final contents of the batch vessel is limited to a maximum of 320°C.
11. The process of any one of claims 1 to 10, wherein the batch vessel is an autoclave.
12. The process according to any one of claims 1 to 11, wherein the copolyamide product comprises 0.5 to 2.5m%, preferably 1.0 to 2.0m% of an endcapping agent.
13. 13. The process of any one of claims 1 to 12, wherein the copolyamide product comprises 0.5 to 6.0 m%, preferably 2.0 to 6.0 m%, preferably 2.0 to 5.5 m%, preferably 2.0 to 5.0 m%, preferably 2.0 to 4.5 m% of each of one or more comonomers other than terephthalic acid, adipic acid, or hexamethylenediamine.
14. 13. The process of any one of claims 1 to 12, wherein the copolyamide product comprises up to 4.5 m %, preferably from 0.5 to 4.5 m %, preferably from 2.0 to 4.5 m %, of each of the one or more comonomers other than terephthalic acid, adipic acid, or hexamethylenediamine.
15. 15. The process of any one of claims 1 to 14, wherein the copolyamide product comprises a plurality of said comonomers other than terephthalic acid, adipic acid, or hexamethylenediamine, the total amount of said comonomers being equal to or less than 12m%, preferably equal to or less than 10m%.
16. 16. The process of any one of claims 1 to 15, wherein the copolyamide product exhibits a hexamethylene terephthalamide mole fraction, defined as the 6T component, of 25 to 45m%.
17. 17. The process of any one of claims 1 to 16, wherein the copolyamide product exhibits a hexamethylene adipamide mole fraction, defined as 66 components, of 50 to 70m%.
18. 18. The process according to any one of the preceding claims, wherein when the copolyamide product exhibits a hexamethylene terephthalamide mole fraction (6T component) of 35 to 45m%, in particular 40 to 45m%, the amount of at least one of, preferably each of, the one or more comonomers other than terephthalic acid, adipic acid, or hexamethylenediamine present in the copolyamide is in the range of 2.5 to 6.0m%, preferably 3.0 to 6.0m%, preferably 3.5 to 6.0m%, preferably 4.0 to 6.0m%.
19. 19. The process according to any one of claims 1 to 18, wherein the total amount of hexamethylenediamine in the reaction mixture is in excess over the combined molar amount of adipic acid, terephthalic acid and any carboxylic acid-containing compounds among the other comonomers, said excess being 3.0 to 5.0 m % over the combined molar amount of adipic acid, terephthalic acid and any carboxylic acid-containing compounds among the other comonomers, when the copolyamide product exhibits a hexamethylene terephthalamide mole fraction (6T component) of 35 to 45 m %, in particular 40 to 45 m %.
20. 18. The process of any one of claims 1 to 17, wherein the copolyamide product exhibits a hexamethylene terephthalamide mole fraction (6T component) of less than 35 m%, and the total amount of hexamethylene diamine in the reaction mixture is in excess over the combined molar amount of adipic acid, terephthalic acid, and any carboxylic acid-containing compounds among the other comonomers, the excess being 0.1 to less than 3.0 m%, preferably 0.1 to 1.0 m%, based on the combined molar amount of adipic acid, terephthalic acid, and any carboxylic acid-containing compounds among the other comonomers.
21. 21. The process of any one of claims 1 to 20, wherein the endcapping agent is selected from monofunctional organic carboxylic acids such as acetic acid, benzoic acid, propionic acid, stearic acid, etc.; monofunctional organic amines, preferably alkyl amines such as n-hexylamine; 1,4-dicarboxylic acids such as succinic acid which react with the amine terminus to form an endcapping 5-membered imide ring structure; anhydrides such as phthalic anhydride which react with the amine terminus to form an endcapping 5-membered imide ring structure; and anhydrides such as 1,8-naphthalene anhydride which react with the amine terminus to form an endcapping 6-membered imide ring structure, preferably the endcapping agent is acetic acid.
22. The at least one comonomer other than terephthalic acid, adipic acid, and hexamethylenediamine is selected from organic diamines, organic dicarboxylic acids, organic aminocarboxylic acids, and organic lactams, and preferably, the organic diamine is selected from pentamethylenediamine, 2-methylpentamethylenediamine, octanediamine, m-xylylenediamine, 2-methyloctanediamine, bis(p-aminocyclohexyl)methane, nonanediamine, decanediamine, 2,4,4-trimethylhexamethylenediamine, 2, ...
22. The process according to any one of claims 1 to 21, wherein the organic dicarboxylic acid is selected from azelaic acid, isophthalic acid, sebacic acid, dodecanedioic acid, and 2,6-naphthalenedicarboxylic acid, and / or preferably the organic amino carboxylic acid is selected from 6-aminohexanoic acid, 7-aminoheptanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid, and / or preferably the organic lactam is selected from caprolactam and laurolactam.
23. 23. The process of any one of claims 1 to 22, wherein the at least one comonomer other than terephthalic acid, adipic acid, and hexamethylenediamine is selected from isophthalic acid (I), 2-methylpentamethylenediamine (D), and combinations thereof.
24. 24. The process according to any one of claims 1 to 23, wherein the at least one comonomer other than terephthalic acid, adipic acid and hexamethylenediamine is isophthalic acid (I), preferably the copolyamide product comprises up to 4.5m%, preferably 0.5 to 4.5m%, preferably 2.0 to 4.5m% of said isophthalic acid (I), optionally in combination with 2-methylpentamethylenediamine (D).
25. 25. The process according to any one of claims 1 to 24, wherein the at least one comonomer other than terephthalic acid, adipic acid and hexamethylenediamine is 2-methylpentamethylenediamine (D), preferably the copolyamide product comprises 0.5 to 6.0 m%, preferably 2.0 to 6.0 m%, preferably 2.0 to 5.5 m%, preferably 2.0 to 5.0 m%, preferably 2.0 to 4.5 m% of said 2-methylpentamethylenediamine (D), optionally in combination with isophthalic acid (I).
26. The process of any one of claims 1 to 25, wherein the copolyamide product is a semi-crystalline copolyamide.
27. 27. The process of any one of claims 1 to 26, wherein the copolyamide product exhibits a relative viscosity, measured in a 1.0 wt. / vol. % solution of the copolyamide sample in 96% sulfuric acid according to ASTM D789 method, in the range of 1.8 to 2.8 and an amine end group content in the range of 15 to 100 mpmg.
28. 28. The process according to any one of claims 1 to 27, wherein the copolyamide product exhibits a crystallization temperature of above 220.0°C, preferably at least 222.0°C, preferably above 225.0°C, preferably at least 227.0°C, preferably at least 230.0°C, and preferably equal to or less than 260.0°C, preferably equal to or less than 255.0°C, preferably equal to or less than 250.0°C.
29. The process according to any one of claims 1 to 28, wherein the copolyamide product exhibits a melting point of less than or equal to 320.0°C, preferably at least 250.0°C.
30. A copolyamide made according to the process of any one of claims 1 to 29.
31. A copolyamide containing monomer units derived from terephthalic acid, adipic acid, hexamethylenediamine, at least one comonomer other than terephthalic acid, adipic acid, and hexamethylenediamine, and an endcapping agent, the copolyamide having a relative viscosity in the range of 1.8 to 2.8 as measured in a 1.0 wt. / vol.% solution of a sample of said copolyamide in 96% sulfuric acid according to ASTM D789 method, and an amine end group content preferably in the range of 15 to 160 mpmg.
32. Copolyamide according to claim 31, wherein the copolyamide is as defined in any one of claims 12 to 30.
Citation Information
Patent Citations
Fiber formable random copolyamide
JP1977078298A
Polyamide blow molding
JP1992288341A
Production of polyamide resin for blow molding
JP1992337323A
Ternary and multinary polyamides containing amide units of 2-methylpentamethylenediamine and products made therefrom
JP1994502671A
Polyamide copolymer, its production and fiber and plastic therefrom
JP2000038445A