Process for producing bis-2-hydroxyethyl terephthalate via continuous depolymerization
The method of coextrusion and multi-stage depolymerization in continuous reactors addresses inefficiencies in producing BHET from waste polyester, achieving high purity and efficiency by reducing molecular weight and minimizing by-products.
Patent Information
- Application Number
- JP2024525115
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-07-11
- Filing Date
- 2023-06-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-06-15
AI Technical Summary
Existing methods for depolymerizing waste polyester to produce bis(2-hydroxyethyl) terephthalate (BHET) face inefficiencies in terms of time and purity, with batch reactors requiring excessive time and not adequately suppressing by-product formation.
A method involving coextrusion of waste polyester through a coextruder, followed by depolymerization in a stirred shaft reactor and multiple stages of continuous reactors (CSTR) to reduce molecular weight and purify BHET efficiently.
This approach allows for the production of highly purified BHET in a shorter time with minimized by-product formation, enhancing production efficiency and quality.
Smart Images

Figure 2024538257000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for efficiently preparing high-purity bis(2-hydroxyethyl) terephthalate (BHET) using waste polyester. [Background technology]
[0002] Among polymers, polyester is used as a material in various fields due to its excellent mechanical strength, heat resistance, transparency and gas barrier properties. In particular, polyester sheets or plates have good transparency and excellent mechanical strength, and as a result, polyester sheets or plates are widely used for cases, boxes, partitions, shelves, panels, packaging materials, building materials, interior materials, exterior materials, etc.
[0003] As a result, waste plastics such as polyester are generated at unmanageable levels worldwide each year. Recently, countries around the world have been preparing regulations and programs to recycle waste plastic resources, including waste polyester.
[0004] Physical and chemical methods are used to recycle waste polyester, but physical recycling methods are not widely used because they cannot guarantee purity. On the other hand, chemical recycling methods depolymerize waste polyester by breaking the ester bonds of the waste polyester. Reactions such as glycolysis, hydrolysis, methanolysis, and aminolysis are used. Among these, glycolysis is a method of decomposing waste polyester by adding glycols such as ethylene glycol or diethylene glycol at high temperatures. A reaction product containing mainly bis(2-hydroxyethyl) terephthalate (BHET) is obtained. The bis(2-hydroxy) terephthalate contained in the reaction product can be used as a raw material for preparing unsaturated polyester or ester polyol after crystallization or purification.
[0005] In order to use bis(2-hydroxyethyl)terephthalate as the raw material, it is necessary to increase the purity of bis(2-hydroxyethyl)terephthalate by minimizing the formation of by-products such as diethylene glycol esters (DEG esters) during the depolymerization process. For this purpose, a method of carrying out the depolymerization by using a multi-stage continuous stirred tank reactor (CSTR) is currently being adopted.
[0006] However, this method requires more than twice as long to depolymerize the waste polyester as the batch reactor, which reduces the process efficiency. In addition, this method of depolymerizing the waste polyester does not sufficiently suppress the generation of by-products, and there is a limit to obtaining bis(2-hydroxyethyl) terephthalate with the desired purity. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Korean Patent Publication No. 2022-0068991 Summary of the Invention [Problem to be solved by the invention]
[0008] The present inventors have conducted various studies to solve the above-mentioned problems of the prior art. As a result, it has been found that when waste polyester is subjected to molecular weight reduction and short-term depolymerization before depolymerization in a continuous stream reactor (CSTR), high-purity bis(2-hydroxyethyl) terephthalate can be prepared with high efficiency (improved productivity).
[0009] Therefore, the object of the present invention is to provide a method for preparing bis(2-hydroxyethyl) terephthalate by continuous depolymerization of waste polyester, which method makes it possible to improve the purity and production efficiency (productivity) of bis(2-hydroxyethyl) terephthalate. [Means for solving the problem]
[0010] In order to achieve the above object, the present invention provides a method for preparing bis(2-hydroxyethyl) terephthalate, the method comprising the steps of: (1) feeding waste polyester raw material into a co-extruder to obtain a co-extrudate; (2) feeding the co-extrudate into an agitated shaft reactor and depolymerizing the co-extrudate to obtain a first reactant; (3) feeding the first reactant into a first continuous reactor and depolymerizing the first reactant to obtain a second reactant; and (4) feeding the second reactant into a second continuous reactor and depolymerizing the second reactant to obtain a third reactant. Effect of the Invention
[0011] According to the preparation method of the present invention, waste polyester can be coextruded and depolymerized in a stirred shaft reactor for a short period to reduce the molecular weight, followed by depolymerization in a continuous multi-stage reactor (CSTR) to prepare bis(2-hydroxyethyl) terephthalate (BHET) in a relatively short time while minimizing the formation of by-products (e.g., DEG and DEG esters) that may be considered as impurities. Therefore, the present invention can provide high-purity bis(2-hydroxyethyl) terephthalate (BHET) with high efficiency, and the bis(2-hydroxyethyl) terephthalate (BHET) prepared as described above can be used as a raw material for preparing polyesters having excellent quality and products using the same. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 illustrates an example of a method for preparing bis(2-hydroxyethyl) terephthalate according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing methods for preparing bis(2-hydroxyethyl) terephthalate according to Comparative Examples 1 to 3. [Diagram 3]FIG. 1 is a diagram showing methods for preparing bis(2-hydroxyethyl) terephthalate according to Comparative Examples 4 to 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below. The present invention in this specification is not limited to the disclosure contents shown below, and can be modified in various forms without changing the gist of the present invention.
[0014] As used herein, the term "comprising" is intended to specify certain features, regions, steps, processes, elements, and / or components, and does not exclude the presence or addition of other features, regions, steps, processes, elements, and / or components, unless specifically stated to the contrary.
[0015] Throughout this specification, the terms first, second, etc. are used to distinguish one element from another, but the components should not be limited by the terms.
[0016] All numbers and expressions relating to quantities of ingredients, reaction conditions, and the like used in this specification should be understood to be modified by the term "about" unless otherwise specified.
[0017] The number average molecular weight and weight average molecular weight of the compounds (reactants or products) described herein are, as is well known, carbon-12 ( 12 C) as a reference. The unit is not given, but it may be understood as the molar mass (g / mol) of the same value if necessary.
[0018] For illustrative purposes, the size of individual elements in the accompanying drawings may be exaggerated and may differ from the actual size.
[0019] Method for preparing bis(2-hydroxyethyl) terephthalate The present invention relates to a method for preparing bis(2-hydroxyethyl) terephthalate, which is one of the raw materials for preparing recycled resin (post-consumer resin), by depolymerization of waste polyester. The present invention is characterized in that the waste polyester is subjected to molecular weight reduction and short-term depolymerization, and then depolymerized in multiple stages through a continuous reactor.
[0020] Specifically, the method for preparing bis(2-hydroxyethyl) terephthalate according to the present invention includes the steps of: (1) feeding waste polyester raw material into a co-extruder to obtain a co-extrudate; (2) feeding the co-extrudate into a stirred shaft reactor and depolymerizing the co-extrudate to obtain a first reactant; (3) feeding the first reactant into a first continuous reactor and depolymerizing the first reactant to obtain a second reactant; and (4) feeding the second reactant into a second continuous reactor and depolymerizing the second reactant to obtain a third reactant.
[0021] The method for preparing bis(2-hydroxyethyl) terephthalate according to the present invention may further comprise a step (5) of purifying the third reactant of step (4).
[0022] Each step of this method is explained in detail below with reference to FIG.
[0023] Step (1): Obtaining a co-extrusion According to the present invention, in step (1), waste polyester raw material is fed into a co-extruder (10) to obtain a co-extrudate. Specifically, in step (1), the molecular weight reduction of the waste polyester raw material is achieved by physical and / or chemical methods through the co-extruder (10).
[0024] The waste polyester raw material can be obtained from polyester material products that are discarded after use. Specifically, the waste polyester can be obtained by pre-treating waste products such as beverage bottles, fabrics, films, cases, boxes, partitions, shelves, protective panels, packaging materials, building materials, interior materials, and exterior materials that contain various polyester materials (e.g., polyethylene terephthalate (PET) materials) that are discarded after use by consumers.
[0025] The pretreatment may be carried out by removing other plastics, metals, and foreign objects contained in the waste, washing the waste polyester, and then crushing it in a grinder. As a result of the pretreatment, the waste polyester raw material may be in a flake form. Furthermore, the waste polyester raw material may have a fine structure like fibers.
[0026] In step (1), the first glycol-based compound may be continuously fed to the co-extruder (10). When the first glycol-based compound is fed to the co-extruder (10), the molecular weight of the waste polyester raw material can be reduced more efficiently.
[0027] The first glycol compound is not particularly limited. Specifically, the first glycol compound may be at least one selected from the group consisting of ethylene glycol (monoethylene glycol), propylene glycol, and diethylene glycol.
[0028] The amount of the first glycol compound fed may be 0.01 to 100 parts by weight, 1 to 80 parts by weight, 3 to 60 parts by weight, or 5 to 50 parts by weight, relative to 100 parts by weight of the waste polyester raw material. When the amount of the first glycol compound fed is within the above range, the molecular weight of the waste polyester raw material can be reduced to the utmost limit through the co-extruder (10).
[0029] On the other hand, the co-extrusion may be carried out at 170 to 290°C, specifically, 173 to 275°C, 175 to 250°C, 180 to 230°C, 185 to 215°C, or 190 to 200°C. When the co-extrusion is carried out within the above temperature range, the molecular weight of the waste polyester raw material can be stably reduced. Furthermore, the extrusion speed (screw rpm) during co-extrusion may be 130 to 250 rpm, 135 to 220 rpm, 140 to 200 rpm, or 145 to 185 rpm.
[0030] The co-extruder (10) is not particularly limited as long as it is capable of co-extruding the waste polyester raw material. Specifically, the co-extruder (10) may be a conventionally known single-screw co-extruder or a multi-screw (e.g., twin-screw) co-extruder.
[0031] The coextrudate obtained through step (1) may have a relatively low weight average molecular weight and number average molecular weight. That is, the coextrudate may have a weight average molecular weight of 3,000 to 36,000, specifically, 3,500 to 30,000, 3,800 to 25,000, or 4,000 to 20,000. Furthermore, the coextrudate may have a number average molecular weight of 500 to 10,000, 800 to 8,000, 1,000 to 6,500, or 1,100 to 5,500.
[0032] Since the coextrudate obtained through step (1) has a relatively low molecular weight as described above, the time required for the depolymerization procedure in steps (2) to (4) can be reduced, and the production of by-products (e.g., DEG and DEG esters) is minimized.
[0033] Step (2): Obtaining the first reactant by a stirred shaft reactor According to the present invention, in step (2), the coextrudate is fed to a stirring shaft reactor and depolymerized (first depolymerization) to obtain a first reactant. Specifically, in step (2), a glycolysis reaction in which polymer chains and the like present in the coextrudate are decomposed by the first glycol compound can be carried out in a short time.
[0034] In step (1), if the first glycol-based compound is not fed to the co-extruder (10), the first glycol-based compound may be fed continuously to the stirred shaft reactor (20).
[0035] In order to promote the depolymerization of the coextrudate through the stirred shaft reactor (20), a catalyst for promoting the depolymerization reaction may be further fed to the stirred shaft reactor (20). The catalyst is not particularly limited as long as it is a known catalyst. Specifically, the catalyst may be a catalyst including a metal acetate, an anhydride of an acetate, or a hydrate of an acetate. More specifically, the catalyst may be at least one acetate selected from the group consisting of zinc acetate, sodium acetate, cobalt acetate, and manganese acetate, or a hydrate or anhydride thereof.
[0036] The amount of catalyst supplied to the stirring shaft reactor (20) may be 0.01 to 5 parts by weight, 0.1 to 3 parts by weight, or 0.2 to 1 part by weight, based on 100 parts by weight of the waste polyester raw material.
[0037] The depolymerization of the coextrudate may be carried out at 180 to 210°C (specifically, 183 to 208°C, 185 to 205°C, 186 to 204°C, 188 to 203°C, 190 to 200°C, or 193 to 198°C) for 50 minutes or less (specifically, 5 to 50 minutes, 10 to 50 minutes, 20 to 50 minutes, 22 to 45 minutes, 25 to 40 minutes, or 30 to 35 minutes). In particular, the depolymerization temperature of the coextrudate may be higher than the depolymerization temperature in steps (3) and (4), and the time spent on depolymerization may be shorter than the time spent on depolymerization in steps (3) and (4). As a result, high-purity bis(2-hydroxyethyl) terephthalate can be prepared with high efficiency.
[0038] Meanwhile, the stirred shaft reactor (20) is not particularly limited as long as it is for mixing the coextrudate, the first glycol-based compound, and the catalyst. Specifically, the stirred shaft reactor (20) may include at least one selected from the group consisting of a kneader, a paddle mixer, a plow shear mixer, a screw mixer, and a ribbon blender. More specifically, the stirred shaft reactor may be a kneader or a paddle mixer.
[0039] The first reaction product obtained through step (2) may have a peak area fraction of bis(2-hydroxyethyl) terephthalate (BHET) of 50 to 75%, specifically, 55 to 75%, 58 to 73%, or 65 to 70%, when analyzed by high performance liquid chromatography (HPLC).
[0040] Furthermore, the first reaction product may have a peak area fraction of oligomers having a weight average molecular weight of less than 2,000 (>Mw2,000) of 11.0% or less, specifically, 0.5 to 10.5%, 0.8 to 10%, 1.0 to 8.0%, 1.3 to 7.5%, or 1.5 to 7.3%, when analyzed by gel permeation chromatography (GPC).
[0041] Step (3): Obtaining the second reactant through the first continuous reactor According to the present invention, in step (3), the first reactant is supplied to the first continuous reactor and depolymerized (second depolymerization) to obtain a second reactant. Specifically, in step (3), the second glycol-based compound may be continuously supplied to the first continuous reactor (30) as well. As a result, a glycolysis reaction can be carried out in which polymer chains and the like present in the first reactant are decomposed by the second glycol-based compound.
[0042] The second glycol compound is not particularly limited, and specifically may be at least one selected from the group consisting of ethylene glycol (monoethylene glycol), propylene glycol, and diethylene glycol.
[0043] The amount of the second glycol-based compound supplied to the first continuous reactor (30) may be 50 to 340 parts by weight relative to 100 parts by weight of the first reactant. Specifically, the second glycol-based compound may be continuously supplied to the first continuous reactor (30) in an amount of 50 to 300 parts by weight, 50 to 250 parts by weight, 50 to 200 parts by weight, or 50 to 100 parts by weight relative to 100 parts by weight of the first reactant. When the supply amount of the second glycol-based compound is within the above range, the depolymerization of the first reactant can be efficiently carried out, and thus the proportion of oligomers, dimers, or trimers contained in the second reactant obtained via step (3) can be significantly reduced.
[0044] The depolymerization of the first reactant may be carried out at 170 to 195°C (specifically, 173 to 194°C, 175 to 193°C, 177 to 192°C, 180 to 191°C, 183 to 191°C, or 185 to 190°C) for 30 to 50 minutes (specifically, 32 to 45 minutes, 35 to 43 minutes, or 38 to 40 minutes). When the depolymerization of the first reactant is carried out under the above conditions, the depolymerization is efficiently carried out and the overall process time is shortened, so that the purity and preparation efficiency (productivity) of bis(2-hydroxyethyl) terephthalate can be improved.
[0045] The depolymerization of the first reactant may be carried out in the presence of a catalyst that is continuously fed to the stirred shaft reactor (20) in step (2) or directly fed to the first continuous reactor (30). The catalyst may be a catalyst comprising a metal acetate, anhydride or hydrate thereof.
[0046] On the other hand, the first continuous reactor (30) is not particularly limited as long as it is a conventional continuous flow tank reactor designed to carry out depolymerization.
[0047] The second reaction product obtained through step (3) may have a peak area fraction of bis(2-hydroxyethyl)terephthalate (BHET) of 50 to 85%, specifically, 55 to 84%, 65 to 83.5%, or 75 to 83%, when analyzed by high performance liquid chromatography (HPLC). Here, the HPLC peak area fraction of bis(2-hydroxyethyl)terephthalate (BHET) in the second reaction product can be changed depending on the amount of the second glycol compound supplied to the first continuous reactor (30).
[0048] Step (4): Obtaining a third reactant through a second continuous reactor According to the present invention, in step (4), the second reactant is supplied to the second continuous reactor (40) and depolymerized (third depolymerization) to obtain a third reactant. Specifically, in step (4), the unreacted second glycol-based compound discharged from the first continuous reactor (30) in step (1) and supplied to the second continuous reactor (40) can perform a glycolysis reaction in which polymer chains and the like present in the second reactant are decomposed. In addition, in the case where the unreacted second glycol-based compound is not supplied to the second continuous reactor (40) to an extent that the depolymerization is sufficiently performed or in the case where the purity of the unreacted second glycol-based compound decreases, a third glycol-based compound may be additionally supplied to the second continuous reactor (40) in preparation for a decrease in depolymerization efficiency.
[0049] The third glycol compound is not particularly limited, and specifically may be at least one selected from the group consisting of ethylene glycol (monoethylene glycol), propylene glycol, and diethylene glycol.
[0050] The amount of the third glycol-based compound supplied to the second continuous reactor (40) may be 50 to 150 parts by weight relative to 100 parts by weight of the second reactant. Specifically, the third glycol-based compound may be continuously supplied to the second continuous reactor (40) in an amount of 50 to 130 parts by weight, 55 to 110 parts by weight, 60 to 90 parts by weight, or 65 to 80 parts by weight relative to 100 parts by weight of the second reactant. When the supply amount of the third glycol-based compound is within the above range, the depolymerization of the second reactant can be efficiently carried out, and thus the proportion of oligomers, dimers, or trimers contained in the third reactant obtained via step (4) can be significantly reduced.
[0051] The depolymerization of the second reactant may be carried out at 140 to 170°C (specifically, 143 to 168°C, 145 to 165°C, 148 to 160°C, 149 to 158°C, or 150 to 155°C) for 30 to 50 minutes (specifically, 35 to 45 minutes, 38 to 43 minutes, or 40 to 42 minutes). When the depolymerization of the second reactant is carried out under the above conditions, the depolymerization is carried out efficiently and the overall process time is shortened, so that the purity and preparation efficiency (productivity) of bis(2-hydroxyethyl) terephthalate can be improved.
[0052] The depolymerization of the second reactant may be carried out in step (2) in the presence of a catalyst that is continuously fed to the stirred shaft reactor (20), continuously fed to the first continuous reactor (30), or fed directly to the second continuous reactor (40). The catalyst may be a catalyst comprising a metal acetate, an anhydride thereof, or a hydrate thereof.
[0053] On the other hand, the second continuous reactor (40) is not particularly limited so long as it is a conventional continuous flow tank reactor designed to carry out depolymerization.
[0054] The third reaction product obtained via step (4) may have a peak area fraction of bis(2-hydroxyethyl) terephthalate (BHET) of 80 to 90%, specifically, 83.5 to 90%, 84 to 89.5%, or 84.5 to 89%, when analyzed by high performance liquid chromatography (HPLC).
[0055] Furthermore, the third reaction product may have a peak area fraction of oligomers having a weight average molecular weight of less than 2,000 (>Mw2,000) of 2.0% or less, specifically, 0.0 to 2.0%, 0.0 to 1.8%, 0.0 to 1.7%, 0.0 to 1.5%, or 0.0 to 1.0%, when analyzed by gel permeation chromatography (GPC).
[0056] Meanwhile, the third reactant is subjected to a filtration step to remove unreacted materials and impurities (contaminants). In such a case, the third reactant contains almost no oligomers, which have a significant effect on the time required for the filtration step, so that the filtration step can be performed in a relatively short time in the present invention. That is, in the present invention, before the waste polyester is directly fed to the continuous reactor and depolymerized in multiple stages, the molecular weight of the waste polyester raw material is reduced through the co-extruder (10) in step (1) and depolymerized in a short time through the stirring shaft reactor (20) in step (2), so that the reactant obtained by the final depolymerization contains almost no oligomers that would otherwise increase the filtration time or delay the filtration step. In addition, when the multi-stage depolymerization is performed through the above steps (3) and (4), the residence time of the high-temperature reaction of the reactants obtained in each step is shortened, and the generation of by-products is minimized, so that high-purity bis(2-hydroxyethyl) terephthalate can be prepared in a high yield.
[0057] Specifically, when the third reactant is filtered using a membrane filter having a pore size of 0.1 μm, the flow rate (filtration flow rate) passing through the membrane filter may be 10 kg / hr or more, specifically, 10 to 100 kg / hr, 12 to 90 kg / hr, 13 to 80 kg / hr, or 14 to 70 kg / hr. When the filtration flow rate is within the above range, it is possible to significantly improve the preparation efficiency (productivity) of bis(2-hydroxyethyl) terephthalate.
[0058] Further, the third reactant may have a filtration loss rate according to the following formula 1 of less than 8 wt %, specifically, 0.1-7.5 wt %, 0.5-7.0 wt %, 1.0-6.0 wt %, or 1.3-5.0 wt %. [Formula 1] Filtration loss rate (weight%)=(m1-m2 / m1)×100 m1: initial weight of the third reactant m2: weight of the third reactant that passed through a filter membrane having a pore size of 0.1 μm
[0059] Step (5): Purification of the third reactant According to the present invention, in step (5), the third reactant is purified. Step (5) can be optionally performed as necessary.
[0060] Purification of the third reactant may be carried out via commonly known methods, specifically, purification may include one or more steps of filtration, ion exchange, distillation, decolorization, and adsorption.
[0061] The filtration step may include processes such as membrane filtration, filter aid filtration, reduced pressure flash (cooling), and solid-liquid separation. When such a filtration step is performed, fine particles and insoluble foreign matter contained in the third reaction liquid can be removed.
[0062] Ion exchange is a step carried out using a commonly known ion exchange resin. Examples of ion exchange resins include cation exchange resins, anion exchange resins, amphoteric ion exchange resins, chelating resins, and the like. Specifically, the cation exchange resin may be a strongly acidic cation exchange resin having a sulfonic acid group (-SO3H), or a weakly acidic cation exchange resin having a carboxyl group (-COOH). The anion exchange resin may be a strongly basic anion exchange resin in the form of a quaternary ammonium salt, or a weakly basic anion exchange resin having an amino group. When such an ion exchange step is carried out, the catalyst and metal foreign matter can be removed.
[0063] The distillation may include steps such as vacuum distillation, thin film evaporation, falling film evaporation, short path evaporation, etc. If such a distillation step is performed, unreacted glycol-based compounds may be removed.
[0064] Bleaching is a step that is generally carried out using a known bleaching agent. Specifically, examples of the bleaching agent include activated carbon, activated clay, diatomaceous earth, etc. When such a bleaching step is carried out, colored substances can be removed.
[0065] Adsorption is a step carried out using an adsorbent known in the art. When such an adsorption step is carried out, other foreign substances can be removed and the crystallized final reactant (bis(2-hydroxyethyl) terephthalate) can be obtained.
[0066] Method of the invention The present invention will be described in more detail below with reference to the following embodiments. However, these embodiments are provided for illustrative purposes only and are not intended to limit the present invention.
[0067] Preparation Example 1 Crushed waste PET (flake-like PET) and monoethylene glycol (MEG) were fed into a single-screw co-extruder at a feed rate of 15.5 kg / hr each, and co-extruded at a temperature of 180°C and 150 rpm (to reduce molecular weight) to obtain a co-extrudate.
[0068] Preparation Examples 2 to 7 Each coextrudate was obtained in the same manner as in Preparation Example 1, except that the feed flow rate and coextrusion conditions were adjusted as shown in Table 1 below.
[0069] Test Example 1 The coextrusion products obtained in Preparation Examples 1 to 7 were analyzed by gel permeation chromatography (GPC) under the following conditions, and the results are shown in Table 1 below. GPC analyzer: HLC-8420GPC Elite of TOSOH Mobile phase: Chloroform / phenol mixed solvent Temperature: 40℃ Column: Individual gel type x 4EA Sample pretreatment: The sample concentration in the solution was adjusted to 0.5 wt / v% using a chloroform / phenol mixed solvent.
[0070] [Table 1]
[0071] Example 1 Application of the co-extruder, kneader, first continuous reactor and second continuous reactor Following the coextrusion process of Preparation Example 1, depolymerization was continuously carried out through the kneader, the first continuous reactor (CSTR-1), and the second continuous reactor (CSTR-2) according to the design conditions of Fig. 1. Specifically, the coextrusion product of Preparation Example 1 (feed flow rate: 31.0 kg / hr) and zinc acetate anhydride as a catalyst (feed flow rate: 0.065 kg / hr) were fed to the kneader, and a first depolymerization reaction was carried out at 195°C for 35 minutes to obtain a first reactant.
[0072] The first reactant thus obtained and additional monoethylene glycol (MEG-2) (feed rate: 15.5 kg / hr) were fed to a first continuous reactor (CSTR-1) to carry out a second depolymerization reaction at 190° C. for 40 minutes to obtain a second reactant.
[0073] The second reactant thus obtained and additional monoethylene glycol (MEG-3) (feed rate: 31.0 kg / hr) were fed to a second continuous reactor (CSTR-1) to carry out a third depolymerization reaction at 150° C. for 40 minutes to obtain a third reactant.
[0074] The third reaction product thus obtained was purified by a conventional method to prepare bis(2-hydroxyethyl) terephthalate.
[0075] Examples 2 to 7 Application of the co-extruder, kneader, first continuous reactor, and second continuous reactor Bis(2-hydroxyethyl) terephthalate was prepared in the same manner as in Example 1, except that the feed flow rate and reaction temperature in each depolymerization reaction were adjusted as shown in Table 2 below.
[0076] Comparative Examples 1 to 3 Application of the Kneader, the First Continuous Reactor, and the Second Continuous Reactor According to the design conditions in Figure 2, depolymerization of shredded waste PET (flake-like PET) was continuously carried out through a kneader, a first continuous reactor (CSTR-1) and a second continuous reactor (CSTR-2) in the presence of anhydrous zinc acetate catalyst, without going through a co-extrusion process of the shredded waste PET. Bis(2-hydroxyethyl) terephthalate was prepared by adjusting the feed flow rate and reaction temperature in each depolymerization reaction as shown in Table 3 below.
[0077] Comparative Examples 4 to 6 Application of the First Continuous Reactor, the Second Continuous Reactor, and the Third Continuous Reactor According to the design conditions in Figure 3, depolymerization of shredded waste PET (flake-like PET) was continuously carried out in the presence of zinc acetate anhydride catalyst through the first continuous reactor (CSTR-1), the second continuous reactor (CSTR-2) and the third continuous reactor (CSTR-3) without going through the co-extrusion process of the shredded waste PET and depolymerization using a kneader. Bis(2-hydroxyethyl) terephthalate was prepared by adjusting the feed flow rate and reaction temperature in each depolymerization reaction as shown in Table 3 below.
[0078] [Table 2]
[0079] [Table 3]
[0080] Test Example 2 The reaction products obtained in Examples 1 to 7 and Comparative Examples 1 to 6 were analyzed by gel permeation chromatography (GPC) under the following conditions. The results are shown in Tables 4 and 5 below. GPC analyzer: HLC-8420GPC Elite of TOSOH Mobile phase: Chloroform / phenol mixed solvent Temperature: 40℃ Column: Individual gel type x 4EA Sample pretreatment: The sample concentration in the solution was adjusted to 0.5 wt / v% using a chloroform / phenol mixed solvent.
[0081] Test Example 3 The third reaction products obtained by depolymerization in the second continuous reactor (CSTR-2) in Examples 1 to 7 and Comparative Examples 1 to 3, and the third reaction products obtained by depolymerization in the third continuous reactor (CSTR-3) in Comparative Examples 4 to 6 were each filtered through a circular glass fiber filter, and the filtration time and flow rate were measured. The results are shown in Tables 4 and 5 below. Here, the evaluation conditions and evaluation criteria were as follows. Glass fiber filter pore size: 0.1 μm Diameter of glass fiber filter: 320mm Filtration temperature: 100~150℃ Judgment of success or failure of filtration - ◎: Filtration time within 20 minutes, ○: Filtration time from 20 minutes to 60 minutes or less, ×: Filtration time over 60 minutes
[0082] Test Example 4 The reaction products (filtrates) obtained in Test Example 3 were analyzed by high performance liquid chromatography (HPLC) under the following conditions. The results are shown in Tables 4 and 5 below. Pretreatment: Approximately 0.01 g of a sample was diluted with approximately 20 mL of methanol and measured by HPLC. HPLC analyzer (model): Waters e2695 Column: C18 (4.6 x 250 mm), 5 μm UV detector: 242 nm Injection volume: 10μL Eluent (gradient) - A: H2O + H3PO4, B: Acetonitrile
[0083] Test Example 5 After carrying out Test Example 3, the filtration loss rate of the reaction product (filtrate) was calculated according to the following formula 1. [Formula 1] Filtration loss rate (weight%)=(m1-m2 / m1)×100 m1: initial weight of the third reactant (initial weight of the third reactant obtained by depolymerization in the second continuous reactor (CSTR-2) in Examples 1 to 7 and Comparative Examples 1 to 3, and initial weight of the reactant obtained by depolymerization in the third continuous reactor (CSTR-3) in Comparative Examples 4 to 6). m2: weight of the third reactant that has passed through a filtration membrane having a pore size of 0.1 μm (in Examples 1 to 7 and Comparative Examples 1 to 3, the weight of the third reactant obtained by depolymerization in the second continuous reactor (CSTR-2) that has passed through a filtration membrane having a pore size of 0.1 μm, and in Comparative Examples 4 to 6, the weight of the reactant obtained by depolymerization in the third continuous reactor (CSTR-3) that has passed through a filtration membrane having a pore size of 0.1 μm)
[0084] [Table 4]
[0085] [Table 5]
[0086] Referring to Table 4, in Examples 1 to 7 in which the preparation method according to the present invention was applied, when multi-stage depolymerization was performed after coextrusion and kneader depolymerization, the depolymerization was performed in a relatively short time, minimizing the generation of by-products that are considered to be impurities, and high-purity bis(2-hydroxyethyl) terephthalate was produced. In addition, since the waste PET was satisfactorily depolymerized and there was almost no remaining oligomer, the filtration process for removing unreacted materials and impurities could be efficiently performed.
[0087] In contrast, referring to Table 5, in Comparative Examples 1 to 3 in which the coextrusion process was not performed, the molecular weight of the waste PET was not reduced as compared with Examples 1 to 7, so that the residual oligomers increased and the amount of by-products produced increased. Also, in Comparative Examples 4 to 6 in which multi-stage depolymerization was performed without reducing the molecular weight of the waste PET, the residual oligomers were large and the filtration loss rate was high, so that the efficiency of the method for preparing bis(2-hydroxyethyl) terephthalate was significantly deteriorated. [Explanation of symbols]
[0088] 10: Co-extrusion machine 20: Stirred shaft reactor 30: First continuous reactor 40: Second continuous reactor
Claims
1. (1) feeding waste polyester raw material into a co-extruder to obtain a co-extrudate; (2) feeding the co-extrudate into a stirred shaft reactor and depolymerizing the co-extrudate to obtain a first reactant; (3) feeding the first reactant to a first continuous reactor and depolymerizing the first reactant to obtain a second reactant; (4) feeding the second reactant to a second continuous reactor and depolymerizing the second reactant to obtain a third reactant; A method for preparing bis(2-hydroxyethyl) terephthalate comprising:
2. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, wherein the first glycol-based compound is continuously fed into the co-extruder in step (1) in an amount of 0.01 to 100 parts by weight based on 100 parts by weight of the waste polyester raw material.
3. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, wherein the co-extrusion in step (1) is carried out at 170-290°C.
4. 2. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, wherein the coextrudate has a weight average molecular weight of 3,000 to 36,000.
5. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, wherein the depolymerization in step (2) is carried out at 180-210°C.
6. 2. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, wherein in step (2), a catalyst comprising a metal acetate or its anhydride or hydride is further fed into the stirred shaft reactor.
7. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, wherein the first reaction product obtained through step (2) has a peak area fraction of bis(2-hydroxyethyl) terephthalate (BHET) of 50 to 75% when analyzed by high performance liquid chromatography (HPLC).
8. 2. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, wherein the stirred shaft reactor comprises at least one selected from the group consisting of a kneader, a paddle mixer, a plowshare mixer, a screw mixer, and a ribbon blender.
9. 2. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, wherein a second glycol-based compound is continuously fed to the first continuous reactor in step (3) in an amount of 50 to 340 parts by weight per 100 parts by weight of the first reactant.
10. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, wherein the third reaction product obtained through step (4) has a peak area fraction of bis(2-hydroxyethyl) terephthalate (BHET) of 80 to 90% when analyzed by high performance liquid chromatography (HPLC).
11. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, wherein the depolymerization in step (3) is carried out at 170-195° C. for 30-50 minutes, and the depolymerization in step (4) is carried out at 140-170° C. for 30-50 minutes.
12. 2. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, wherein a third glycol-based compound is continuously fed to the second continuous reactor in step (4) in an amount of 50 to 150 parts by weight relative to 100 parts by weight of the second reactant.
13. 2. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, wherein when the third reactant in step (4) is filtered using a membrane filter having a pore size of 0.1 μm, the flow rate through the membrane filter is 10 kg / hr or more.
14. The third reactant in step (4) is represented by the following formula 1: [Formula 1] Filtration loss rate (weight %) = (m 1 -m 2 / m 1 )×100 m 1 : initial weight of the third reactant m 2 : Weight of the third reactant that passed through a filter membrane having a pore size of 0.1 μm 2. The method for preparing the bis(2-hydroxyethyl) terephthalate of claim 1, having a filtration loss rate of less than 8% by weight according to
15. 2. The method for preparing bis(2-hydroxyethyl) terephthalate according to claim 1, further comprising a step (5) of purifying the third reactant of step (4).
Citation Information
Patent Citations
Method for depolymerizing polyethylene terephthalate
JP2002332379A
METHOD FOR PRODUCING BIS-beta-HYDROXYETHYL TEREPHTHALATE
JP2003055300A
Recovery method for waste polyester by continuous alcoholysis
JP2021532197A
Recovery method for waste polyester materials by continuous alcoholysis and continuous transesterification
JP2021532198A
Process for the depolymerization of a polyester comprising opaque polyethylene terephthalate
US20190161595A1