Electrolytic copper foil for secondary battery collectors

The electrolytic copper foil addresses issues of high production costs and non-uniform coating by providing high tensile strength, elongation, and controlled surface properties, ensuring stable and uniform active material adhesion, thus enhancing battery performance and lifespan.

JP2024538307AActive Publication Date: 2024-10-18LOTTE ENERGY MATERIALS CO LTD

Patent Information

Application Number
JP2024525742
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-29
Filing Date
2022-10-07
Publication Date
2024-10-18
Estimated Expiration
2042-10-07

AI Technical Summary

Technical Problem

Existing copper foils for secondary battery current collectors face issues such as high production costs, contamination from lubricating oil, reduced adhesion to active materials, volume changes leading to wrinkles and cracks, and non-uniform coating on both sides, which affect battery performance and lifespan.

Method used

An electrolytic copper foil with specific mechanical properties, including high tensile strength, high elongation, controlled surface roughness, and uniform wetting angles on both sides, achieved through a combination of additives in the electrolytic solution, ensuring good contact with active materials and stability under varying temperatures.

Benefits of technology

The electrolytic copper foil provides stable performance in secondary batteries by maintaining mechanical integrity, ensuring uniform coating, and enhancing adhesion and contact with active materials, thereby improving cycle characteristics and lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538307000001_ABST
    Figure 2024538307000001_ABST
Patent Text Reader

Abstract

The present invention provides an electrodeposited copper foil for use as a current collector for secondary batteries, characterized in that the room-temperature elongation rate relative to thickness is 1.3-2.0% / μm and the ratio of the surface wetting angle (θM) on the M plane to the surface wetting angle (θS) on the S plane is 1 or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolytic copper foil, and more particularly to an electrolytic copper foil for use as a current collector for a secondary battery. [Background technology]

[0002] Copper foil is generally used as a current collector for secondary batteries. The copper foil is mainly rolled copper foil produced by rolling, but the manufacturing cost is high and it is difficult to produce wide copper foil. In addition, rolled copper foil requires the use of lubricating oil during rolling, and the adhesion to the active material decreases due to contamination of the lubricating oil, which may result in a decrease in the charge / discharge cycle characteristics of the battery.

[0003] Lithium batteries undergo volumetric changes during charging and discharging and heat generation due to overcharging. In addition, the surface roughness of the copper foil must be low so as to improve adhesion with the electrode active material, to have a relatively small effect on the copper foil base material in relation to the expansion and contraction of the active material layer due to the charge and discharge cycle, and to prevent the occurrence of wrinkles and breakage in the copper foil as a current collector. Therefore, a copper foil that can withstand the volumetric changes and heat generation phenomenon of lithium batteries and has excellent adhesion with the active material, high elongation, high strength, and low roughness is required. In addition, when used as a negative electrode current collector for secondary batteries, both sides of the copper foil are coated with electrode active material. In this case, if the roughness of both sides of the electrolytic copper foil is different, the battery characteristics will differ, so it is necessary to maintain the roughness of both sides of the electrolytic copper foil at the same or similar level.

[0004] In the manufacturing process of a secondary battery using such an electrolytic copper foil, the copper foil is vacuum-dried. However, since vacuum drying is a process that is performed at high temperature for a long time, the adhesive strength and stress between the copper foil and the active material coating surface change during the vacuum drying of the copper foil, which may shorten the life of the battery or cause cracks.

[0005] When the electrolytic copper foil is used as a negative electrode current collector for a secondary battery, both sides of the copper foil are coated with an electrode active material. Therefore, it is preferable that the surface of the electrolytic copper foil provides good contact with the active material. However, conventional approaches to provide good contact with the active material are limited to controlling the surface roughness of the electrolytic copper foil.

[0006] Therefore, there is a demand for electrolytic copper foils for use as current collectors for secondary batteries that have high mechanical properties over a wide range of temperatures and, at the same time, can provide good contact properties with active materials. Summary of the Invention [Problem to be solved by the invention]

[0007] In order to solve the above-mentioned problems of the prior art, an object of the present invention is to provide an electrodeposited copper foil having high mechanical strength and high elongation in a wide temperature range.

[0008] Another object of the present invention is to provide an electrolytic copper foil having high mechanical strength and high elongation even when a high-temperature drying process is applied.

[0009] Another object of the present invention is to provide an electrolytic copper foil for a current collector of a secondary battery, which can provide good contact performance to an active material coating containing a water-based binder.

[0010] Another object of the present invention is to provide an electrolytic copper foil for use as a current collector for a secondary battery, which enables uniform coating of an active material on both sides of the electrolytic copper foil. [Means for solving the problem]

[0011] In order to achieve the above technical objectives, the present invention provides a sheet having a room temperature thickness elongation ratio of 1.3 to 2.0% / μm and a surface wetting angle (θ S ) on the M surface relative to the surface wetting angle (θ M ) is 1 or more.

[0012] The electrolytic copper foil of the present invention has a room temperature tensile strength of 40 kgf / mm 2 The surface wetting angle on the S surface (θ S ) on the M surface relative to the surface wetting angle (θ M ) may be 1 or more. In this case, θ M is 60° to 70°, and θ S may be 50° to 60°.

[0013] In addition, the surface wetting angle of the electrolytic copper thin film of the present invention is 0.7 <cosθ M / cosθ S < 1.

[0014] Furthermore, the three-dimensional surface roughness Sz of the M plane of the electrolytic copper foil of the present invention may be smaller than the three-dimensional surface roughness Sz of the S plane.

[0015] In this case, the three-dimensional surface roughness Sz of the M plane may be 0.7 to 1.0 μm, and the three-dimensional surface roughness Sz of the S plane may be 1.3 to 2.0 μm.

[0016] The electrodeposited copper foil of the present invention can exhibit the above-mentioned high elongation rate relative to thickness in the thickness range of 2 to 12 μm.

[0017] Furthermore, the static friction coefficient of the M side of the electrolytic copper foil of the present invention may be 0.2 to 0.3, and the static friction coefficient of the S side may be 0.17 to 0.21.

[0018] The electrodeposited copper foil of the present invention may have a TOC content of 5 to 8 ppm.

[0019] In addition, the electrolytic copper foil of the present invention has a tensile strength of 36 kgf / mm after heat treatment at 200°C for 1 hour. 2 It may be more than that.

[0020] Moreover, the electrolytic copper foil of the present invention may have a thickness-to-thickness elongation ratio after heat treatment at 200° C. for 1 hour of 1.4% / μm or more. Effect of the Invention

[0021] According to the present invention, it is possible to provide an electrolytic copper foil having high mechanical strength and a high elongation rate in various temperature ranges.

[0022] Furthermore, according to the present invention, it is possible to provide a current collector that can provide good contact performance to an active material coating that contains a water-based binder.

[0023] Furthermore, according to the present invention, it is possible to provide a secondary battery current collector that enables uniform coating of active material on both sides of the electrolytic copper foil. [Brief description of the drawings]

[0024] [Figure 1A] 1A and 1B are photographs showing an example of measurement of wetting angles on the M and S faces, respectively, of a copper foil produced according to an embodiment of the present invention. [Figure 1B] 1A and 1B are photographs showing an example of measurement of wetting angles on the M and S faces, respectively, of a copper foil produced according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The embodiments described in this specification and the configurations shown in the drawings are merely the most preferred embodiments of the present invention and do not represent all of the technical ideas of the present invention, so it should be understood that there are various equivalents and modifications that can replace them at the time of filing this application. Hereinafter, the embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0026] In the present specification, the S side refers to the side that comes into contact with the drum during the production process of the electrodeposited copper foil and is generally referred to as the gloss side, and the M side refers to the opposite side, which is generally referred to as the deposit side or matte side. These terms do not express the roughness of the respective sides, and it goes without saying that the S side may have a lower gloss or a higher surface roughness than the M side.

[0027] In the present invention, the electrodeposited copper foil has a tensile strength at room temperature (hereinafter referred to as "room temperature tensile strength") of 40 kgf / mm 2 The electrolytic copper foil preferably has a room temperature tensile strength of 50 kgf / mm 2 Less than or equal to 45kgf / mm 2 It is preferable that:

[0028] The room temperature tensile strength of copper foil is 40kgf / mm 2 If it is less than 50 kgf / mm, there is a high possibility that defects such as wrinkles, distortions, and bending may occur due to plastic deformation when the anode active material is coated on the copper foil at high speed in the anode electrode formation process in lithium secondary batteries. 2 If the temperature exceeds 100° C., the occurrence of distortion or wrinkles may be reduced, but there is a high possibility that a high tension imbalance may occur during high-speed coating of the negative active material, and the brittleness of the copper foil itself may increase, which may cause cracks and breaks.

[0029] The electrolytic copper foil of the present invention has high tensile strength even after high-temperature heat treatment. The electrolytic copper foil of the present invention has a tensile strength of 36 kgf / mm after heat treatment at 200° C. for 1 hour (hereinafter referred to as "high-temperature tensile strength"). 2 The electrolytic copper foil preferably has a high-temperature tensile strength of 45 kgf / mm 2 Less than or equal to 42kgf / mm 2 It is preferable that:

[0030] In the present specification, the high-temperature tensile strength is a measured value that imitates the process of high-temperature processes such as coating dry and vacuum dry during the process of forming the anode of a lithium secondary battery. The high-temperature tensile strength of copper foil is 36 kgf / mm 2 If it is less than 45kgf / mm, deformation occurs due to the stress caused by the volume expansion of the negative electrode during charging and discharging of the lithium secondary battery, causing a decrease in lifespan during charging and discharging. 2If it exceeds this value, the deformation due to stress caused by volume expansion decreases, but the brittleness of the copper foil increases, and cracks and electrode detachment due to accumulation of stress occur, shortening the life of the electrode. Electrodeposited copper foil is required to have a high elongation rate with appropriate strength.

[0031] In the present invention, the ratio of the high-temperature tensile strength to the room-temperature tensile strength is preferably 0.9 or more, and the tensile strength ratio is less than 1, preferably less than 0.95. In the present invention, the electrodeposited copper foil is characterized in that the deterioration of the tensile strength due to high-temperature heat treatment is suppressed as much as possible.

[0032] In the present invention, the electrolytic copper foil has a high elongation ratio of the electrolytic copper foil. Specifically, the electrolytic copper foil of the present invention has a higher value obtained by dividing the elongation ratio by the thickness (hereinafter referred to as "elongation per unit thickness") than that of conventional electrolytic copper foils. For example, the elongation ratio relative to the thickness at room temperature (hereinafter referred to as "elongation per unit thickness at room temperature") may have a value of 1.3% / μm or more or 1.5% / μm or more. In addition, the elongation ratio relative to the thickness at room temperature may have a value of 2.0% / μm or less, 1.9% / μm or less, or 1.8% / μm or less. In addition, in the present invention, the electrolytic copper foil exhibits a high elongation ratio even after high-temperature heat treatment. The electrolytic copper foil of the present invention may have a thickness-to-thickness elongation ratio after heat treatment at 200° C. for 1 hour (hereinafter referred to as “high-temperature thickness-to-thickness elongation ratio”) of 1.4% / μm or more, 1.5% / μm or more, or 1.6% / μm or more. The high-temperature thickness-to-thickness elongation ratio of the electrolytic copper foil may be 2.4% / μm or less, 2.2% / μm or less, or 2.0% / μm or less.

[0033] In order to improve the energy density of a lithium secondary battery, the content of active materials must be increased and the thickness of non-active materials such as copper foil, aluminum foil, and separator must be reduced. Therefore, the higher the energy density of a lithium secondary battery, the thinner the required copper foil thickness. However, as the copper foil becomes thinner, the physical energy content of the foil decreases. Therefore, the thinner the thickness, the more likely it is to break or crack even when a small external stress is applied. Therefore, only if the copper foil has a certain or higher elongation rate per thickness can a stable product be manufactured in a copper foil manufacturing process or a secondary battery electrode manufacturing process using the copper foil, and a stable life performance can be realized during charging and discharging of the secondary battery. As described below, the electrolytic copper foil of the present invention has a high elongation rate per thickness even at a thin thickness.

[0034] If the elongation rate relative to thickness at room temperature is below the lower limit, breakage and cracks may occur during the copper foil manufacturing process and the secondary battery electrode manufacturing process, and if it exceeds the upper limit, excessive deformation may cause defects due to wrinkles, distortion, etc. If the elongation rate relative to thickness at high temperature is below the lower limit, the electrode may break during charging and discharging of the secondary battery, reducing its life characteristics, and if it exceeds the upper limit, charge and discharge performance may be reduced due to electrode deformation. Therefore, an appropriate range of elongation rate relative to thickness is required.

[0035] In the present invention, the electrodeposited copper foil exhibits a high elongation ratio relative to thickness even at a thickness as small as 2 μm or 4 μm. For example, the thickness range in which the copper foil of the present invention exhibits the above-mentioned elongation ratio relative to thickness may be in the range of 2 to 12 μm, 4 to 12 μm, 2 to 10 μm, or 4 to 10 μm.

[0036] In addition, in the present invention, the elongation ratio relative to thickness of the electrolytic copper foil shows a narrow deviation over the range of copper foil thicknesses. For example, an electrolytic copper foil having a thickness of 4 μm may have a similar elongation ratio relative to thickness value to an electrolytic copper foil having a thickness of 12 μm.

[0037] In addition, the electrodeposited copper foil of the present invention has a ratio of the high-temperature elongation rate to the room-temperature elongation rate (elongation rate ratio) of 1 or more, or 1.05 or more. In addition, the ratio of the high-temperature elongation rate to the room-temperature elongation rate (elongation rate ratio) may be 1.25 or less, or 1.2 or less.

[0038] The electrodeposited copper foil of the present invention preferably has an MIT folding number of 240 or more. For example, the electrodeposited copper foil of the present invention may have an MIT folding number of 240 to 300. When contracting and expanding during charging and discharging of a secondary battery, the copper foil base material used as a current collector also contracts and expands, and the larger the MIT value, the more it can withstand stress caused by bending, so that a copper foil with a high MIT value can improve cycle characteristics and ensure high capacity performance.

[0039] (blank paragraph)

[0040] The M and S faces of the electrolytic copper foil of the present invention have hydrophilic surfaces to provide good contact properties to an active material paste containing an aqueous binder. For example, in the present invention, the wetting angle or contact angle of the M and S faces of the electrolytic copper foil to water is preferably 70° or less, 69° or less, 68° or less, 67° or less, 66° or less, or 65° or less. In addition, in the present invention, the wetting angle of the M and S faces is preferably 50° or more, 51° or more, 52° or more, 53° or more, 54° or more, or 55° or more.

[0041] According to one embodiment of the present invention, the electrodeposited copper foil of the present invention is characterized in that the wetting angle of the M plane is equal to or greater than the wetting angle of the S plane. For example, the wetting angle of the M plane of the electrodeposited copper foil may be 60° or more, and the wetting angle of the S plane may be 60° or less.

[0042] In the present invention, the two surfaces of the electrolytic copper foil have a very small difference in wettability. The difference in wettability (D) between the two surfaces of the copper foil may be expressed in various ways, but can be expressed using a wetting angle as follows:

[0043] (mathematical formula 1)

[0044] D=cosθ M / cosθ S

[0045] (Here, θ M is the wetting angle on the M surface, θ S is the wetting angle on the S surface)

[0046] (blank paragraph)

[0047] In the electrolytic copper foil of the present invention, the wettability difference (D) may be 0.7 or more, 0.75 or more, or 0.8 or more, and the wettability difference (D) may be 1 or less, 0.95 or less, 0.90 or less, or 0.85 or less.

[0048] Within the above-mentioned numerical ranges, the electrolytic copper foil of the present invention can ensure good contact characteristics with the active material paste on the M and S sides and can provide uniform application.

[0049] The electrolytic copper foil of the present invention has low surface roughness. For example, the three-dimensional surface roughness (Sz) of the electrolytic copper foil of the present invention may be 2.0 μm or less, 1.5 μm or less, or 1.0 μm or less. It is preferable that the three-dimensional surface roughness (Sz) of the M surface is 1.0 μm or less, and the S surface is 2.0 μm or less.

[0050] When the electrolytic copper foil is used as a current collector for the anode of a secondary battery, if the surface roughness (Sz) of the M side, which is the deposition surface of the electrolytic copper foil, is 1.0 μm or less and flat, the thickness of the coated electrode is also flat, which can improve the performance of the battery by making the distribution of lithium ions in the electrode uniform. However, if the surface roughness (Sz) is less than 0.7 μm, the adhesive strength between the active material and the electrolytic copper foil interface decreases, which can deteriorate the performance of the electrode.

[0051] According to one embodiment of the present invention, the M-side of the electrolytic copper foil has a lower three-dimensional surface roughness (Sz) value than the S-side. For example, the S-side may have an Sz value of 1.3 to 2.0 μm, whereas the M-side may have an Sz value of 0.7 to 1.0 μm.

[0052] The static friction coefficient of the electrolytic copper foil of the present invention is preferably in the range of 0.2 to 0.3 for the M surface and 0.17 to 0.21 for the S surface. If the static friction coefficient is less than the lower limit, the friction coefficient is too small, which may cause a decrease in coating adhesion performance during coating of the secondary battery electrode active material, and if it exceeds the upper limit, the friction coefficient is too large, which may cause a decrease in coating uniformity during coating of the active material.

[0053] (blank paragraph)

[0054] In order to realize high strength and high elongation, minimize changes in mechanical properties between room temperature and high temperature, and minimize differences in surface properties between M-plane and S-plane, the present invention may be prepared using an electrolyte containing a combination of additives selected from the following Additives A to Additive C.

[0055] (blank paragraph)

[0056] Additive A

[0057] Additive A is a thiourea compound, a compound in which a thiol group is linked to a nitrogen-containing heterocycle, or a mixture thereof.

[0058] Here, the thiourea compound is ethylenethiourea, diethylthiourea, acetylenethiourea, dipropylthiourea, dibutylthiourea, N-trifluoroacetylthiourea, N-ethylthiourea, N-cyanoacetylthiourea, N-allylthiourea, o-tolylthiourea, N,N'-butylene ... The thiourea compound may be at least one selected from the group consisting of 4-thiourea, thiazolidinethiol, 4-thiazolinethiol, 4-methyl-2-pyrimidinethiol, and 2-thiouracil, but is not necessarily limited thereto, and various thiourea compounds that can be used as additives in the field of the art may be used.

[0059] The compound having a thiol group linked to a nitrogen-containing heterocycle of the additive A may be at least one selected from the group consisting of 2-mercapto-5-benzoimidazole sulfonic acid sodium salt, sodium 3-(5-mercapto-1-tetrazolyl)benzene sulfonate, and 2-mercapto benzothiazole, but is not necessarily limited thereto. Any compound having a thiol group linked to a nitrogen-containing heterocycle that can be used as an additive in the field of the art may be used.

[0060] In the present invention, the additive A is preferably added to the electrolyte solution at a concentration of less than 2 ppm, and more preferably, the additive A is added at 0.5 to 1.9 ppm.

[0061] In the present invention, Additive A can improve the strength of the electrolytic copper foil. If the content of Additive A exceeds 1.9 ppm, the surface roughness of the deposit side increases, making it difficult to produce an electrolytic copper foil with low roughness, and the elongation rate may decrease.

[0062] (blank paragraph)

[0063] Additive B

[0064] Additive B is a sulfonic acid or a metal salt thereof, which is a compound containing a sulfur atom.

[0065] For example, sulfonic acids or metal salts thereof of compounds containing sulfur atoms include bis-(3-sulfopropyl)-disulfide disodium salt (SPS), 3-mercapto-1-propanesulfonic acid (MPS), 3-(N,N-dimethylthiocarbamoyl)-thiopropanesulfonate sodium salt (DPS), 3-[(amino-iminomethyl)thio]-1-propanesulfonate sodium salt (UPS), o-ethyldithiocarbonate-S-(3-sulfopropyl)-ester sodium salt (OPX), 3-(benzothiazolyl-2-mercapto)-propylsulfonic acid sodium salt (ZPS), ethylenedithiodipropylsulfonic acid sodium salt, thioglycolic acid, thiophosphoric acid-o-ethyl-bis-(ω-sulfopropyl)ester disodium salt, The sulfonic acid may be at least one selected from the group consisting of thiophosphoric acid-tris-(ω-sulfopropyl)ester trisodium salt, and thiophosphoric acid-tris-(ω-sulfopropyl)ester trisodium salt, but is not necessarily limited thereto, and any sulfonic acid or metal salt thereof of a compound containing a sulfur atom that can be used as an additive in the field of the art may be used.

[0066] In the present invention, the additive B is preferably added to the electrolytic solution in an amount of 5 to 20 ppm.

[0067] In the copper electrolyte, the additive B can improve the surface gloss of the electrolytic copper foil. If the content of the additive B is less than 5 ppm, the gloss of the electrolytic copper foil may be reduced, and if the content of the additive B is more than 20 ppm, the surface roughness of the deposit surface increases, making it difficult to manufacture an electrolytic copper foil with low roughness, and the tensile strength of the electrolytic copper foil may be reduced.

[0068] (blank paragraph)

[0069] Additive C

[0070] Additive C is a non-ionic water-soluble polymer.

[0071] The nonionic water-soluble polymer may be polyethylene glycol, polyglycerin, nonylphenol polyglycol ether, octanediol-bis-(polyalkylene glycol ether), octanol polyalkylene glycol ether, oleic acid polyglycol ether, polyethylene propylene glycol, polyethylene glycol dimethyl ether, polyoxypropylene glycol, polyvinyl alcohol, β-naphthol polyglycol ether, stearic acid polyglycol ether, and stearyl alcohol polyglycol ether. However, the present invention is not limited thereto, and any water-soluble polymer usable as an additive in the field of the art may be used. For example, the molecular weight of the polyethylene glycol may be 100 to 20,000.

[0072] The nonionic water-soluble polymer may be at least one selected from the group consisting of hydroxyethyl cellulose and carboxymethyl cellulose, but is not necessarily limited thereto.

[0073] The nonionic water-soluble polymer is a water-soluble proteinaceous gelatin such as gelatin and collagen, and has a structure in which glycine, hydroxylysine, and hydroxyproline are repeated, and there are six or more types including type I, type II, and type V. A chain in which three types of amino acids are repeated is called an alpha chain, and a triple helix is ​​formed when three alpha chains are wound around each other. In general, the complex structure of collagen is formed by cross-linking the triple helices. The nonionic water-soluble polymer of the present invention may be one or more selected from the group consisting of collagen and gelatin, but is not necessarily limited thereto.

[0074] In the present invention, the additive C is preferably added to the electrolytic solution in an amount of 5 to 15 ppm. In the copper electrolytic solution, the additive C can reduce the surface roughness of the electrolytic copper foil and improve the surface gloss. If the content of the additive C is less than 5 ppm, the surface roughness of the deposit surface increases, making it difficult to produce an electrolytic copper foil with a low roughness, and the gloss of the electrolytic copper foil may decrease. If the content of the additive C is more than 15 ppm, the high-temperature strength and high-temperature hardness of the electrolytic copper foil may decrease.

[0075] In the present invention, the ratios of additives A, B and C in the electrolyte may be controlled.

[0076] The effects of the additives A, B, and C in the electrolyte on the physical properties of the electrolytic copper foil have been described above, but the above description is merely illustrative. It is understood that the type, content, or combination of each additive of the present invention may affect other physical properties of the electrolytic copper foil produced by the present invention through unknown mechanisms. EXAMPLES

[0077] <Electrolytic copper foil production example 1>

[0078] (Examples 1 to 5)

[0079] In an electrolyte solution containing 200-452g / L CuSO45H2O, 30-250g / L sulfuric acid, and 10-30ppm chloride ion concentration, at 50-60℃ and 50-70A / dm 2 Electrolytic plating was performed at a current density of 100000 (ASD). 0.5 to 1.5 ppm of ETU (ethylene thiourea) was added as additive A, 5 to 20 ppm of DPS (3-(N,N-dimethylthiocarbamoyl)-thiopropanesulfonate sodium salt) was added as additive B, and 5 to 10 ppm of PEG (polyethylene glycol, molecular weight Mw: 500 to 4000) was added as additive C to the electrolyte. The composition of the electrolyte used in each example is shown in Table 1. The thickness of the plating film was varied depending on the example.

[0080] (blank paragraph)

[0081] Comparative Example 1

[0082] In an electrolyte solution of Cu 100g / L, sulfuric acid 150g / L, and chloride ion concentration 20ppm, at 50-60℃, 50-70A / dm 2 Electrolytic plating was performed at a current density of 100000 (ASD) to produce a plating film with a thickness of 18 μm. 2 ppm of DET (diethylthiourea) was added as additive A, 45 ppm of SPS (bis-(3-sulfopropyl)-disulfide disodium salt) and 10 ppm of ZPS (3-(benzothiazolyl-2-mercapto)-propylsulfonic acid sodium salt) were added as additive B, 20 ppm of PEG (polyethylene glycol, molecular weight Mw: 500-4000) was added as additive C, and 3 ppm of JGB (Janus Green B) was added as additive D to the electrolyte.

[0083] (blank paragraph)

[0084] Comparative Example 2

[0085] In an electrolyte solution of Cu 90g / L, sulfuric acid 120g / L, and chloride ion concentration 30ppm, 50-60℃, 50-70A / dm 2Electrolytic plating was performed at a current density of 10000 ppm (ASD) to produce a 4 μm-thick plating film. The electrolyte contained 3 ppm DET (diethylthiourea) as additive A, 60 ppm SPS (bis-(3-sulfopropyl)-disulfide disodium salt) and 40 ppm ZPS (3-(benzothiazolyl-2-mercapto)-propylsulfonic acid sodium salt) as additive B, and 20 ppm PEG (polyethylene glycol, molecular weight Mw: 500-4000) as additive C, 10 ppm PGL (polyglycerin), 375 ppm Zn, and 75 ppm Fe.

[0086] (blank paragraph)

[0087] Comparative Example 3

[0088] In an electrolyte solution of Cu 100g / L, sulfuric acid 130g / L, and chloride ion concentration 30ppm, 50-60℃, 50-70A / dm 2 Electrolytic plating was performed at a current density of 10000 (ASD) to produce a plating film with a thickness of 6 μm. The electrolyte contained 26 ppm DET (diethylthiourea) as additive A, 80 ppm SPS (bis-(3-sulfopropyl)-disulfide disodium salt) and 40 ppm ZPS (3-(benzothiazolyl-2-mercapto)-propylsulfonic acid sodium salt) as additive B, and 20 ppm PEG (polyethylene glycol, molecular weight Mw: 500-4000) and 10 ppm PGL (polyglycerin) as additive C.

[0089] (blank paragraph)

[0090] Comparative Example 4

[0091] In an electrolyte solution of Cu 80g / L, sulfuric acid 140g / L, and chloride ion concentration 10ppm, at 50-60℃, 50-70A / dm 2 Electrolytic plating was performed at a current density of ASD to produce a plating film with a thickness of 12 μm. 5 ppm of MPS (3-mercapto-1-propanesulfonic acid) as additive B and DDAC (diallyldimethylammonium chloride) as additive E were added to the electrolyte.

[0092] (blank paragraph)

[0093] Comparative Example 5

[0094] In an electrolyte solution of Cu 80g / L, sulfuric acid 140g / L, and chloride ion concentration 10ppm, at 50-60℃, 50-70A / dm 2 Electrolytic plating was performed at a current density of ASD to produce a plating film with a thickness of 12 μm. 5 ppm of MPS (3-mercapto-1-propanesulfonic acid) as additive B and DDAC (diallyldimethylammonium chloride) as additive E were added to the electrolyte.

[0095] The plating solution compositions for each example are shown in Table 1 below.

[0096] (blank paragraph)

[0097] [Table 1]

[0098] (blank paragraph)

[0099] <Physical property evaluation>

[0100] The physical properties of each surface-treated foil specimen prepared in the Examples and Comparative Examples were measured and are shown in Tables 1 and 2. The physical property evaluation items and measurement methods are as follows.

[0101] (blank paragraph)

[0102] a. Tensile strength / elongation rate

[0103] Tensile test pieces were taken from the electrolytic copper foil with a width of 12.7 mm and a gauge length of 50 mm, and a tensile test was carried out at a crosshead speed of 50.8 mm / min according to the IPC-TM-650 2.4.18B standard, and the maximum load of the measured tensile strength was taken as the tensile strength, and the elongation at the time of failure was taken as the elongation. The tensile strength and elongation of each test piece were measured at room temperature, and after heat treatment at a high temperature of 200°C for 1 hour, the tensile strength and elongation were measured, and the results are shown in Table 1 below.

[0104] (blank paragraph)

[0105] b. TOC measurement of copper foil

[0106] The TOC content in the electrodeposited copper foil was analyzed by dissolving the electrodeposited copper foil test pieces obtained in the examples and comparative examples in 60 ml of hydrochloric acid (35%) and 40 ml of hydrogen peroxide solution (30%) using a Shimadzu TOC-V WP. The results are shown in Table 2 below.

[0107] (blank paragraph)

[0108] c.3D roughness

[0109] A 3D Profiler, NV-2200, manufactured by Nano Systems, was used to measure the shape of minute steps on an object in a non-contact manner, and the three-dimensional roughness was measured. Specifically, a contact light-emitting element and a light-receiving element such as a camera were used to precisely measure the minute distance between the contact light-emitting element and the object being measured. Here, Sz is the roughness of the maximum height of a three-dimensional surface, which is the distance between the highest point and the lowest point within a single surface, and this parameter is a three-dimensional expansion of the profile (line roughness) parameter Rz. The maximum height Sz is equal to the sum of the maximum peak height Sp and the maximum valley depth Sv.

[0110] The three-dimensional surface roughness (Sz) was measured at five points on the manufactured copper foil, and the average values ​​are shown in Table 2 below.

[0111] [Table 2]

[0112] (blank paragraph)

[0113] As shown in Table 2, the electrodeposited copper foils of Examples 1 to 5 of the present invention exhibit low TOC contents of 5.1 to 8.

[0114] As listed in Table 2, the test pieces of Examples 1 to 5 had a compressive strength of 40 kgf / mm at room temperature. 2 It shows high strength characteristics and maintains high strength even after high-temperature heat treatment at 200°C.

[0115] Also, as shown in Table 2, Examples 1 to 5 show high values ​​of elongation ratio relative to thickness at room temperature of 1.3 to 2.0% / μm. Furthermore, it can be seen that even in Example 1 with a thickness of 4 μm, the elongation ratio relative to thickness shows a value of 1.3% / μm, while the comparative examples show values ​​of 1.2 or less.

[0116] Furthermore, the test pieces of Examples 1 to 5 of the present invention have a three-dimensional surface roughness (Sz) of the M surface of 0.73 to 0.82 and a three-dimensional surface roughness (Sz) of the S surface of 1.36 to 1.8, indicating that the deviation in surface roughness between the M surface and the S surface is small.

[0117] (blank paragraph)

[0118] d. Wetting angle

[0119] The wetting angle (or contact angle) of water on the surface of the copper foil test piece manufactured in the examples and comparative examples was measured. The wetting angle was measured using Phoenix-300 manufactured by SEO Co., Ltd. according to the standard of ASTM D5946, and deionized water was used as the water droplet. The measurement conditions were as follows.

[0120] (blank paragraph)

[0121] Three test pieces were taken from the produced copper foil, and the wetting angles of each were measured and averaged, as shown in Table 4. Figures 1A and 1B are photographs showing an example of measuring the wetting angles on the M and S sides of the copper foil produced according to Example 2 of the present invention, respectively, and Table 3 shows the measurement data from the measurements.

[0122] [Table 3]

[0123] e.Static friction coefficient

[0124] The test method was performed according to ASTM D1894 (Standard Test Methode for Static and Kinetic Coefficients of Friction of Plastic Film and Sheeting), and the test equipment was a Shimadzu AGS-X universal testing machine. The specific measurement conditions are as follows:

[0125] (1) Test speed: 150 mm / min

[0126] (2) Load cell: 29N

[0127] (3) Test environment: (23±2)℃, (45±5)% RH

[0128] (4) Vertical load: 1.96N (200g)

[0129] (5) Average range: (30~120)mm

[0130] (6) Friction material: SUS (provided by Koptri)

[0131] (blank paragraph)

[0132] The measurement results are shown in Table 4 below.

[0133] [Table 4]

[0134] The electrolytic copper foils according to the examples of the present invention have a hydrophilic surface. For example, the copper foil surfaces of Examples 1 to 5 have a wetting angle of 70° or less. This is distinct from the M or S surface of the copper foils of Comparative Examples 1 to 5, which have a wetting angle of more than 70°.

[0135] In addition, the electrodeposited copper foil according to the embodiment of the present invention has a wetting angle (θ M ) is the wetting angle on the S surface (θ S On the other hand, the electrodeposited copper foils of Comparative Examples 1 to 3 have a value larger than θ M <θ S In the embodiment of the present invention, θ M and θ S The difference between the wettability and the wettability of the electrodeposited copper foils is smaller than those of Comparative Examples 1 to 3. As described above, the electrodeposited copper foils produced according to the examples of the present invention have a significantly reduced wettability deviation between the M side and the S side.

[0136] The wettability characteristics of the electrolytic copper foil of the present invention provide good contact performance for active material coatings containing aqueous binders and allow for uniform active material coating on both sides of the electrolytic copper foil.

[0137] (blank paragraph)

[0138] Although the preferred embodiment of the present invention has been described in detail above, those skilled in the art will understand that various modifications can be made to the above-described embodiment without departing from the scope of the present invention. Therefore, the scope of the present invention should not be limited to the described embodiment, but should be determined by the following claims and their equivalents. [Industrial Applicability]

[0139] The present invention is applicable to electrolytic copper foils.

Claims

1. The room temperature thickness elongation ratio is 1.3 to 2.0% / μm. Surface wetting angle on the S surface (θ S ) to the M-plane surface wetting angle (θ M ) is 1 or more.

2. Room temperature tensile strength is 40 kgf / mm 2 That's all. Surface wetting angle on the S surface (θ S ) to the M-plane surface wetting angle (θ M ) is 1 or more.

3. θ M The electrolytic copper foil according to claim 1 or 2, wherein the angle is 60° to 70°.

4. θ S The electrolytic copper foil according to claim 3, wherein the angle is 50° to 60°.

5. 0.7<cosθ M / cosθ S The electrolytic copper foil according to claim 1 or 2, characterized in that < 1.

6. 3. The electrolytic copper foil according to claim 1, wherein the three-dimensional surface roughness Sz of the M-side is smaller than the three-dimensional surface roughness Sz of the S-side.

7. The electrolytic copper foil according to claim 6, characterized in that the three-dimensional surface roughness Sz on the M side is 0.7 to 1.0 μm.

8. The electrolytic copper foil according to claim 6, characterized in that the three-dimensional surface roughness Sz on the S-side is 1.3 to 2.0 μm.

9. The electrolytic copper foil according to claim 1 or 2, characterized in that the thickness is 2 to 12 μm.

10. 3. The electrolytic copper foil according to claim 1, wherein the static friction coefficient of the M side is 0.2 to 0.3, and the static friction coefficient of the S side is 0.17 to 0.

21.

11. The electrolytic copper foil according to claim 1 or 2, characterized in that the TOC content is 5 to 8 ppm.

12. The tensile strength after heat treatment at 200°C for 1 hour is 36 kgf / mm 2 The electrolytic copper foil according to claim 1 or 2, characterized in that

13. The electrolytic copper foil according to claim 1 or 2, characterized in that the elongation relative to the thickness after heat treatment at 200° C. for 1 hour is 1.4% / μm or more.

Citation Information

Patent Citations

  • Copper foil for current collector of lithium secondary battery

    JP2012038700A

  • Electrolytic copper foil, and electrical component and battery comprising the same

    JP2016160503A

  • Electrolytic copper foil, current collector containing same, negative electrode and lithium battery

    JP2017517637A

  • Roughened copper foil, copper clad laminate and printed wiring board

    JP2019218602A

  • Electrolytic copper foil for secondary batteries and its manufacturing method

    JP2019536211A

Cited By

  • Electrolytic copper foil for secondary battery current collector

    JP2024538308A