Silica reinforced rubber compositions and articles made therefrom

A rubber composition with diene-based polymers, precipitated silica, and specific silanes enhances processing and rolling resistance, addressing high Mooney viscosities and scorch safety issues in silica-reinforced rubbers, ensuring improved tire performance.

JP2024538710APending Publication Date: 2024-10-23MOMENTIVE PERFORMANCE MATERIALS INC

Patent Information

Application Number
JP2024520967
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-06
Filing Date
2022-10-06
Publication Date
2024-10-23

AI Technical Summary

Technical Problem

Existing silica-reinforced rubber compositions face challenges such as high Mooney viscosities and scorch safety issues during processing, leading to difficulties in mixing, grinding, extruding, and tire curing, while compromising rolling resistance and other performance characteristics like handling and abrasion.

Method used

A rubber composition comprising diene-based polymers, precipitated silica, mercapto-functional alkyl alkoxysilane, blocked mercapto-functional alkyl alkoxysilane, a deblocking agent, a vulcanization package, and a scorch modifier, which synergistically improve processing properties and rolling resistance.

Benefits of technology

The composition achieves low rolling resistance with improved handling and abrasion resistance, while maintaining high Mooney viscosity and scorch safety, making it suitable for industrial tire production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538710000001
    Figure 2024538710000001
  • Figure 2024538710000002
    Figure 2024538710000002
  • Figure 2024538710000003
    Figure 2024538710000003
Patent Text Reader

Abstract

Provided herein is a rubber composition comprising at least one diene-based polymer, precipitated silica, a coupling agent package comprising a mercapto-functional alkylalkoxysilane and a blocked mercapto-functional alkylalkoxysilane, a deblocking agent, a vulcanization package comprising at least one vulcanizing agent comprising sulfur and at least one accelerator, and a scorch modifier.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a rubber composition comprising at least one diene-based polymer, precipitated silica, a coupling agent package comprising a mercapto-functional alkylalkoxysilane and a blocked mercapto-functional alkylalkoxysilane, a deblocking agent, a vulcanization package, and a scorch modifier, and to the cured composition thereof. [Background technology]

[0002] Tire companies are constantly searching for new rubber technologies to reduce tire rolling resistance and improve automobile fuel economy without compromising tire safety, handling, traction, service life, and industrial feasibility.One approach to achieve this need is to use silica-reinforced rubber, where silica is bonded to the rubber using a coupling agent that contains an alkoxysilyl group that can react with the silica filler and a functional group that can react with the rubber during processing and / or curing.

[0003] A wide variety of coupling agents have been used, and some of the silicon-based coupling agents include amino-functional alkylalkoxysilanes, bis-(alkylalkoxysilane) disulfides, bis-(alkylalkoxysilane) polysulfides, blocked mercapto-functional alkylalkoxysilanes, and mercapto-functional alkylalkoxysilanes. These coupling agents are generally used with non-functionalized solution styrene butadiene rubber and precipitated silica. Although these compositions improve rolling resistance compared to carbon black reinforced rubber, these compositions often suffer from the loss of other properties such as handling and wear, and still do not meet the need for further improvement in rolling resistance.

[0004] Furthermore, the use of silica rubber compounds containing mercapto-functional alkylalkoxysilanes during tire pre-cure processing has historically been very difficult, resulting in unacceptably high Mooney viscosities and inadequate scorch safety even in the presence of scorch modifiers.

[0005] Another approach is to use diene-based rubbers that contain at least one functional group capable of interacting with the silica surface. However, the processing of rubber compositions containing mercaptoalkylalkoxysilanes, precipitated silica, and diene-based rubbers that contain at least one functional group is accompanied by unacceptably high Mooney viscosity and short scorch times. This results in unfavorable or unacceptable processing characteristics and difficulties in mixing, grinding, extrusion, tire building, and tire curing. These problems are generally contraindicated for industrializing rubber compositions containing diene-based rubbers that contain functional groups, and for most mercapto-functional alkylalkoxysilane compounds. Thus, there is a need for rubber compositions that have improved rolling resistance behavior while balancing other key performance characteristics such as tread, grip (traction and braking), wear, and handling, while overcoming industrial processing difficulties such as high Mooney viscosity and poor scorch safety. Summary of the Invention

[0006] The rubber composition disclosed herein comprises: (i) at least one diene-based polymer; (ii) precipitated silica; (iii) at least one coupling agent package comprising a mercapto-functional alkylalkoxysilane (iii)(a) and a blocked mercapto-functional alkylalkoxysilane (iii)(b); (iv) at least one deblocking agent; (v) a vulcanization package comprising at least one vulcanizing agent containing sulfur and at least one accelerator; and (vi) containing at least one scorch modifier;

[0007] In some embodiments, the at least one diene-based polymer is selected from the group consisting of (i)(a) a diene-based polymer that contains at least one functional group, (i)(b) a diene-based polymer that does not contain a functional group, and combinations thereof.

[0008] In another embodiment, the at least one diene-based polymer is a diene-based polymer that contains at least one functional group and a diene-based polymer that does not contain a functional group.

[0009] In another embodiment, the at least one diene-based polymer is a diene-based polymer (i)(a) that contains at least one functional group.

[0010] In some embodiments, at least one functional group is selected from the group consisting of amino group, alkoxysilyl group, stanyl group, hydroxyl group, thiol group, sulfide group, thioisocyanate group, isocyanate group, imino group, pyridino group, epoxy group, thioepoxy group, thioketone group, ketone group, ketimine group, isocyanuric acid group, amide group, silazane group, hydroxysilyl (silanol) group, siloxane group, phthalocyanino group, silane-sulfide group, carboxylic acid group, carboxylic acid ester group, and combinations thereof.In some embodiments, at least one functional group is an alkoxysilyl group.

[0011] In some embodiments, the diene-based polymer containing at least one functional group is a solution styrene butadiene rubber containing a functional group selected from the group consisting of amino, alkoxysilyl, stanyl, hydroxyl, thiol, sulfide, thioisocyanate, isocyanate, imino, pyridino, epoxy, thioepoxy, thioketone, ketone, ketimine, isocyanuric acid, amide, silazane, hydroxysilyl (silanol), siloxane, phthalocyanino, silane-sulfide, carboxylic acid, and / or carboxylic acid ester groups. The functional groups can be used alone or can be combined at terminal or pendant positions to form two functional terminals or two functional pendant groups, such as, for example, the terminal position of the diene-based polymer can include an alkoxysilyl group and a primary amino group, or an alkoxysilyl group and a thiol group.

[0012] In some embodiments, the diene-based polymer is one that reacts with the precipitated silica. In further embodiments, the diene-based polymer containing at least one functional group is reacted with the precipitated silica. In some embodiments, the diene-based polymer is a solution styrene butadiene rubber containing an alkoxysilyl group. In some embodiments, the diene-based polymer contains at least one functional group capable of bonding with the precipitated silica and / or itself to reduce or eliminate dangling ends. Each diene-based polymer chain (or a mole of polymer) in the polymer matrix has two dangling ends, also known as terminal groups or polymer chain ends. When the polymer chain ends are functionalized with chemical groups reactive with the silica surface, the covalent bond between the polymer chain ends and the silica surface essentially eliminates one dangling end. Dangling ends have more freedom compared to the polymer chain length between crosslinks and the covalently bonded chain ends, and therefore contribute significantly to the hysteresis of the polymer matrix, which degrades the rolling resistance properties of the rubber tread compound.

[0013] In some embodiments, the mercapto-functional alkylalkoxysilane, hereinafter referred to as mercaptosilane, in the compositions disclosed herein is a difunctional silane having a thiol (mercaptan) functionality and an alkoxysilane functionality bonded to an alkane via a single covalent bond.

[0014] In some embodiments, the blocked mercapto-functional alkylalkoxysilane in the rubber composition disclosed herein, hereinafter referred to as blocked mercaptosilane, is a bifunctional silane, in which one functional group is a thiol (mercaptan), in which the hydrogen atom of mercapto is replaced with another group (hereinafter referred to as "blocking group"), and another functional group is an alkoxysilyl group, in which the blocked mercapto group and the alkoxysilyl group are bonded to an alkane via a single covalent bond.Specifically, the silane can be a blocked mercaptosilane, in which the blocking group comprises an acyl group bonded directly to the sulfur via a single bond to form a thioester functional group, or in which the blocking group is a thiocarboxyl group bonded directly to the sulfur via a single bond to form a xanthate functional group (-OC=S)S-.

[0015] In some embodiments, the weight ratio of the blocked mercapto-functional alkylalkoxysilane (iii)(b) to the mercapto-functional alkylalkoxysilane (iii)(a) in the rubber compositions disclosed herein is from about 0.25:1 to about 50:1. In some embodiments, the weight ratio of the blocked mercapto-functional alkylalkoxysilane (iii)(b) to the mercapto-functional alkylalkoxysilane (iii)(a) in the rubber compositions disclosed herein is from about 0.5:1 to about 20:1. In some embodiments, the weight ratio of the blocked mercapto-functional alkylalkoxysilane (iii)(b) to the mercapto-functional alkylalkoxysilane (iii)(a) in the rubber compositions disclosed herein is from about 1:1 to about 10:1.

[0016] In some embodiments, the weight ratio of blocked mercaptosilane to mercaptosilane in the rubber compositions disclosed herein is from about 0.25:1 to about 50:1.

[0017] In some embodiments, at least one coupling agent package (iii) is used in an amount of from about 0.5 to about 20 parts by weight of coupling agent package per 100 parts by weight of rubber, more specifically from about 1 to about 10 parts by weight of coupling agent package (iii) per 100 parts by weight of rubber, and even more specifically from about 3 to about 8 parts by weight of coupling agent package (iii) per 100 parts by weight of rubber.

[0018] In some embodiments, the scorch modifier may be selected from the group consisting of scorch modifiers including tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrapropylthiuram disulfide, tetrabutylthiuram disulfide, tetraphenylthiuram disulfide, tetramethylthiuram monosulfide, zinc dibenzyldithiocarbamate, and tetrabenzylthiuram disulfide, and combinations thereof.

[0019] In some embodiments, the scorch modifier is a thiuram disulfide scorch modifier, hi some embodiments, the scorch modifier is tetrabenzyl thiuram disulfide or tetramethyl thiuram disulfide.

[0020] In some embodiments, the rubber composition comprises: (i) about 100 parts rubber, where the weight of rubber is the total weight of each diene based polymer (i)(a) that contains at least one functional group plus the total weight of each diene based polymer (i)(b) that does not contain the at least one functional group used in the formulation; (ii) from about 5 to about 140 parts by weight of precipitated silica per 100 parts of rubber (i); (iii) from about 1 to about 20 parts by weight per 100 parts of rubber (i) of a coupling agent package comprising a mercapto-functional alkylalkoxysilane and a blocked mercapto-functional alkylalkoxysilane; (iv) from about 0.1 to about 20 parts by weight of a deblocking agent per 100 parts of rubber (i); (v) from about 0.1 to about 10 parts by weight per 100 parts of rubber (i) of a vulcanization package comprising sulfur and at least one accelerator; and (vi) about 0.1 to about 5 parts by weight of a scorch modifier per 100 parts of rubber (i).

[0021] The units for parts by weight per 100 parts of rubber (i) are often indicated as phr. The sum of the weights of each of the diene-based polymers (i)(a) that contain at least one functional group comprises from 0 to about 100 parts by weight per 100 parts of rubber (i), more specifically from about 10 to about 100 parts by weight per 100 parts of rubber (i), even more specifically from about 20 to about 95 parts by weight per 100 parts of rubber (i), and even more specifically from about 50 to about 90 parts by weight per 100 parts of rubber, with the remainder of the rubber component (i) being the sum of the weights of the diene-based polymers (i)(b) that do not contain at least one functional group.

[0022] In some embodiments, the rubber composition is cured.

[0023] The rubber compositions disclosed herein exhibit a synergistic effect between diene-based polymers containing at least one functional group, precipitated silica, coupling agent packages containing mercapto-functional alkylalkoxysilanes and blocked mercapto-functional alkylalkoxysilanes, and thiuram disulfide scorch modifiers. This synergy has been observed for many different diene-based polymers containing different functional groups, resulting in low rolling resistance while maintaining or improving other performance characteristics. In some embodiments, this synergy is exemplified by high performance index values.

[0024] In some embodiments, the compositions of the present disclosure have a higher performance index value compared to the same composition without the mercaptosilane. In some embodiments, the compositions have a higher performance index value compared to the same composition without the blocked mercaptosilane. In some embodiments, the compositions have a higher performance index value compared to the same composition in which the functionalized polymer is replaced with a non-functionalized polymer.

[0025] The present disclosure further provides a composition prepared by the process of the present disclosure. In some embodiments, the composition prepared by the process of the present disclosure is a rubber composition. In some embodiments, the rubber composition is used to manufacture tires. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] As used above, and throughout the detailed description, the following terms, unless otherwise stated, shall be understood to have the following meanings:

[0027] Unless otherwise stated, the terms "a," "that," and "the," and similar references used in the context of describing particular embodiments of this application (particularly in the context of the claims) may be construed as including both the singular and the plural. References to ranges of values ​​herein are merely intended to serve as a shorthand method of referring individually to each separate value falling within the range. Unless otherwise stated herein, each separate value is included in the specification as if it were individually referred to in this application.

[0028] Furthermore, when "and / or" is used herein, it is to be understood that each of the two specified features or components is specifically disclosed with or without the other. Thus, the term "and / or" used herein in phrases such as "A and / or B" is intended to include "A and B," "A or B," "A (only)," and "B (only)." Similarly, the term "and / or" used in phrases such as "A, B, and / or C" is intended to encompass each of the following embodiments: A, B, and C; A, B, or C; A or C; A or B; B or C; A and C; A and B; B and C; A (only); B (only); and C (only).

[0029] It will be understood that where embodiments are described herein using the term "comprising," otherwise similar embodiments described using the terms "consisting of" and / or "consisting essentially of" are also provided.

[0030] The term "polymer" refers to a substance, chemical compound, or mixture of compounds having a molecular structure consisting primarily or entirely of a large number of similar units (e.g., monomeric units) bonded together.

[0031] The term "functionalized diene-based polymer" is synonymous with, and therefore interchangeable with, "diene-based polymer (i)(a) that contains at least one functional group."

[0032] The term "non-functionalized diene-based polymer" is synonymous with, and therefore interchangeable with, "diene-based polymer (i)(b) that does not contain any functional groups."

[0033] As used herein, the term "about" encompasses the range of experimental error that occurs in measurements.

[0034] The term "elastomer" is synonymous with "rubber" and is therefore interchangeable.

[0035] The term "vulcanization" is synonymous with "curing" and is therefore interchangeable.

[0036] The expression "blocked mercaptosilane" should be understood to include partial hydrolysates, which may result from some of the methods for its preparation and / or upon its storage, especially under conditions of high humidity.

[0037] The expression "coupling agent" means an agent capable of establishing an effective chemical and / or physical bond between a diene polymer and a filler, or an agent capable of establishing an effective chemical and / or physical bond between two diene polymers. An effective coupling agent has functional groups capable of physically and / or chemically bonding with the filler or with a second diene polymer, for example between the silanol groups of the coupling agent and the hydroxyl (OH) groups on the surface of the filler (for example the surface silanols in the case of silica), or between the silanol groups bonded to one diene polymer and the silanol groups of another polymer, and for example sulfur atoms capable of physically and / or chemically bonding with the diene polymer as a result of vulcanization (curing).

[0038] The term "filler" refers to a substance added to a diene polymer (rubber) to extend the rubber or reinforce the elastomer network. Reinforcing fillers are materials that have a higher modulus than the diene polymer of the elastomeric composition and can absorb strain from the diene polymer when the elastomer is strained. Fillers include fibers, needles, nanotubes, particles, and sheet-like structures and can be composed of inorganic minerals, silicates, silica, clays, ceramics, carbon, organic polymers, and diatomaceous earth.

[0039] The term "hydrocarbon" as used herein means any chemical structure containing hydrogen and carbon atoms.

[0040] As used herein, "alkyl" includes straight-chain, branched-chain, and cyclic alkyl groups; "alkenyl" includes any straight-chain, branched-chain, or cyclic alkenyl group containing one or more carbon-carbon double bonds, where the points of substitution can be at either the carbon-carbon double bonds or elsewhere in the group; and "alkynyl" includes any straight-chain, branched-chain, or cyclic alkynyl group containing one or more carbon-carbon triple bonds, and optionally one or more carbon-carbon double bonds, where the points of substitution can be at either the carbon-carbon triple bonds, carbon-carbon double bonds, or elsewhere in the group.

[0041] Specific non-limiting examples of alkyl groups include methyl, ethyl, propyl, and isobutyl. Specific non-limiting examples of alkenyl groups include vinyl, propenyl, allyl, and methallyl. Specific non-limiting examples of alkynyl groups include acetylenyl, propargyl, and methylacetylenyl.

[0042] As used herein, "aryl" includes any aromatic hydrocarbon having one hydrogen atom removed; "aralkyl" includes any alkyl group as described above having one or more hydrogen atoms replaced with an equal number of similar and / or different aryl (as defined herein) substituents; and "arenyl" includes any aryl group as described above having one or more hydrogen atoms replaced with an equal number of similar and / or different alkyl (as defined herein) substituents. Specific non-limiting examples of aryl groups include phenyl and naphthalenyl. Specific non-limiting examples of aralkyl groups include benzyl and phenethyl. Specific non-limiting examples of arenyl groups include tolyl and xylyl.

[0043] As used herein, an "alkylene" is a divalent saturated aliphatic radical derived by removing two hydrogen atoms from an alkane.

[0044] Other than in the examples, or unless otherwise noted, all numbers expressing quantities of ingredients, reaction conditions, lengths of time, quantified properties of materials, and the like set forth in the specification and claims are understood to be modified in all instances by the term "about."

[0045] Any numerical range recited herein is understood to include all subranges within that range, and any combination of the various endpoints of that range or subrange.

[0046] Furthermore, all compounds, materials or substances explicitly or implicitly disclosed and / or claimed herein as belonging to a group of structurally, compositionally and / or functionally related compounds, materials or substances are understood to include the individual members of that group and all combinations thereof.

[0047] The compositions of the present disclosure exhibit a synergistic effect between the diene-based polymer (i)(a) containing at least one functional group, the blocked mercaptosilane, the mercaptosilane, and the scorch modifier in silica rubber compounds, which is achieved with various diene-based polymers (i)(a). In some embodiments, this synergistic effect is exemplified by high performance index values.

[0048] In one embodiment, the composition comprising the diene-based polymer (i)(a), the mercaptosilane and the blocked mercaptosilane reacts on the surface of the silica during mixing. Both the diene-based polymer (i)(a) and the mercaptosilane form chemical or physical bonds between the silica and the polymer during mixing. The high reactivity of the mercaptosilane thiol may result in bonding with the diene-based polymer during mixing, but not all thiols will have sufficient reaction time during the rubber mixing schemes contemplated for commercial tire manufacturing.

[0049] The rubber composition disclosed herein comprises: (i) at least one diene-based polymer; (ii) precipitated silica; (iii) a coupling agent package comprising a mercapto-functional alkylalkoxysilane and a blocked mercapto-functional alkylalkoxysilane; (iv) a deblocking agent; (v) a vulcanization package comprising sulfur and at least one accelerator; and (vi) Contains a scorch modifier.

[0050] In some embodiments, the rubber composition is cured.

[0051] In some embodiments, the at least one diene-based polymer is selected from the group consisting of diene-based polymer (i)(a) containing at least one functional group, diene-based polymer (i)(b) not containing a functional group, and combinations thereof. In some embodiments, the at least one diene-based polymer is a combination of at least one diene-based polymer (ia) containing at least one functional group and diene-based polymer (i)(b) not containing a functional group.

[0052] In some embodiments, the rubber composition comprises: (i) a diene-based polymer, where the diene-based polymer is a combination of at least one diene-based polymer (i)(a) that contains at least one functional group and a diene-based polymer (i)(b) that does not contain a functional group; (ii) precipitated silica; (iii) at least one coupling agent package comprising a mercapto-functional alkylalkoxysilane (iii)(a) and a blocked mercapto-functional alkylalkoxysilane (iii)(b); (iv) at least one deblocking agent; (v) a vulcanization package comprising at least one vulcanizing agent comprising elemental sulfur and at least one accelerator; and (vi) at least one scorch modifier; Diene polymers (i)

[0053] (i)(a) a diene-based polymer containing at least one functional group

[0054] The diene-based polymer (i)(a) containing at least one functional group is a compound whose functional group is selected from the group consisting of an amino group, an alkoxysilyl group, a stannyl (tin) group, a hydroxyl group, a thiol group, a sulfide group, a thioisocyanate group, an isocyanate group, an imino group, a pyridino group, an epoxy group, a thioepoxy group, a thioketone group, a ketone group, a ketimine group, an isocyanuric acid group, an amide group, a silazane group, a hydroxysilyl (silanol) group, a siloxane group, a phthalocyanino group, a silane-sulfide group, a carboxylic acid group, a carboxylic acid ester group, and a combination of these functional groups.

[0055] In certain embodiments, the diene-based polymer (i)(a) that includes at least one functional group can include the functional group(s) at one end of the polymer, at both ends of the polymer, at one end of the polymer and pendant to the polymer backbone, at both ends of the polymer and pendant to the polymer backbone, or only pendant to the polymer backbone. The functional group at the end of the polymer (end group) or within the polymer chain (pendant group) can be one functional group, or two or more functional groups that can be present at one end of the polymer or pendant to the polymer backbone.

[0056] In certain embodiments, the diene-based polymer (i)(a) containing at least one functional group can be prepared by solution anionic polymerization, solvent-free radical polymerization, or free radical emulsion polymerization.

[0057] In an embodiment, the diene-based polymer (i)(a) containing at least one functional group is prepared by polymerizing monomers, including, but not limited to, aromatic compounds containing alkenyl groups, in which the carbon-carbon double bond is conjugated with an aromatic ring, and dienes, such as 1,3-butadiene or isoprene, of 8 to 20 carbon atoms, and compounds containing an alkenyl group and a functional group and / or a protected functional group. A protected functional group is a functional group that reacts with a protecting agent to form a protected functional group, which does not participate in or prevents the participation of the protected functional group in the polymerization reaction, but can be removed after the polymerization reaction to regenerate the functional group. The polymerization reaction is initiated by an initiator and terminated by a terminating compound. The initiator and / or the terminating compound may contain a functional group and / or a protected functional group.

[0058] In an embodiment, the diene-based polymer (i)(a) containing at least one functional group can be prepared according to US Patent Publication No. 2010 / 0186869A1, US Patent No. 7,342,070B2 and / or International Publication No. WO2007 / 047943, the entire contents of each of which are incorporated herein by reference. The diene-based polymer (i)(a) containing at least one functional group can be a styrene butadiene rubber functionalized with an alkoxysilane group and at least one of a primary amine group and / or a thiol group. The styrene butadiene rubber is obtained by copolymerizing styrene and butadiene, and is characterized in that the styrene butadiene rubber has a primary amino group and / or a thiol group and an alkoxysilyl group attached to the polymer chain. The alkoxysilyl group can be at least one of a methoxysilyl group and / or an ethoxysilyl group. The primary amino group and / or thiol group may be bonded to any of the polymerization initiation end, polymerization termination end, main chain, and side chain of the styrene-butadiene rubber, so long as it is bonded to the chain of the styrene-butadiene rubber. The primary amino group and / or thiol group may be introduced to the polymerization initiation end or polymerization termination end.

[0059] In one embodiment, the content of alkoxysilyl groups attached to the polymer chains of the (co)polymer rubber is preferably from about 0.5 to about 200 millimoles per kilogram (mmol / kg) of diene-based polymer (i)(a) containing at least one functional group, more particularly the content is from about 1 to about 100 mmol / kg of diene-based polymer (i)(a) containing at least one functional group, and especially from about 2 to about 50 mmol / kg of diene-based polymer (i)(a) containing at least one functional group.

[0060] The diene-based polymer (i)(a) containing at least one functional group can be prepared by anionic polymerization of styrene and butadiene in a hydrocarbon solvent using an organic alkali metal and / or organic alkaline earth metal initiator, adding a terminator compound having a protected primary amino group and / or a protected thiol group and an alkoxysilyl group, reacting the terminator with the living polymer chain end when the polymerization is substantially complete, and then deblocking, for example by hydrolysis or other suitable procedure.

[0061] In some embodiments, the diene-based polymer (i)(a) containing at least one functional group has the formula (I): [ka] During the ceremony P is a conjugated diolefin or a (co)polymer chain of a conjugated diolefin and an aromatic vinyl compound; R 1 is an alkylene group having 1 to 12 carbon atoms; R 2 and R 3 each of which is independently an alkyl group, an aryl group, or an aryl group having from 1 to 20 carbon atoms; and k, m and n are each an integer, where n is 1 or 2, m is 1 or 2, and k is 1 or 2, with the proviso that n+m+k is an integer of 3 or 4; or having the formula (II): [ka] During the ceremony P is a conjugated diolefin or a (co)polymer chain of a conjugated diolefin and an aromatic vinyl compound; R 1 is an alkylene group having 1 to 12 carbon atoms; R 2 and R 3 each of which is independently an alkyl group having 1 to 20 carbon atoms, an aryl group, or an aryl group having 6 to 12 carbon atoms; and j and h are each an integer, where j is an integer from 1 to 3 and h is an integer from 1 to 3, with the proviso that j+h is an integer from 2 to 4.

[0062] The terminator having a protected primary amino group and an alkoxysilyl group may be any compound of formula (III): [ka] During the ceremony R 1 is an alkylene group having 1 to 12 carbon atoms; R 2 and R 3 each independently is an alkyl group, an aryl group, or an aryl group having 1 to 20 carbon atoms; R 4 , R 5 and R 6 each independently represents an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, provided that R 4 and R 5 may be bonded to each other via a covalent bond to form a ring together with the silicon atom to which they are attached; k, m and n are each an integer, where n is 1 or 2, m is 1 or 2, and k is 1 or 2, with the proviso that n+m+k is an integer of 3 or 4; or any compound of formula (IV): [ka] During the ceremony R 1 is an alkylene group having 1 to 12 carbon atoms; R 2 and R 3 each independently is an alkyl group, an aryl group, or an aryl group having 1 to 20 carbon atoms; R 4 , R 5 and R 6 each independently represents an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, provided that R 4 and R 5 may be bonded to each other via a covalent bond to form a ring together with the silicon atom to which they are attached; m is 1 or 2.

[0063] The terminator is a compound having a protected primary amino group and an alkoxysilyl group, and may be any of various compounds known in the art.In some embodiments, the terminator is a compound having a protected primary amino group and an alkoxysilyl group, and may include, for example, N,N-bis(trimethylsilyl)aminopropyl-methyldimethoxysilane, 1-trimethylsilyl-2,2-dimethoxy-1-aza-2-silacyclopentane, N,N-bis(trimethylsilyl)aminopropyltrimethoxysilane, N,N-bis-(trimethylsilyl)aminopropyl-triethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane, N,N-bis-(trimethylsilyl)aminoethyltrimethoxysilane, N,N-bis-(trimethylsilyl)-aminoethyltriethoxysilane, N,N-bis-(trimethylsilyl)aminoethylmethyldimethoxysilane, and N,N-bis-(trimethylsilyl)aminoethylmethyldiethoxysilane. More particularly, the terminating agent is 1-trimethylsilyl-2,2-dimethoxy-1-aza-2-silacyclopentane, N,N-bis-(trimethylsilyl)aminopropylmethyldimethoxysilane or N,N-bis-(trimethylsilyl)aminopropylmethyldiethoxysilane.

[0064] A suitable work-up to obtain a primary amine means reaction of the living polymer with a compound having a protected primary amino group and an alkoxysilyl group followed by removal of the protecting group. For example, in the case of a bis-(trialkylsilyl) protecting group, hydrolysis is used to remove the trialkylsilyl group, as in N,N-bis(trimethylsilyl)aminopropyltriethoxysilane, leaving the primary amine.

[0065] In another embodiment, the solution of styrene and butadiene monomers polymerized and functionalized with alkoxysilane groups and thiols is disclosed in International Publication WO 2007 / 047943, the entire contents of which are incorporated herein by reference. The diene-based polymer (i)(a) containing at least one functional group has the formula (V): [ka] During the ceremony P is a conjugated diolefin or a (co)polymer chain of a conjugated diolefin and an aromatic vinyl compound; R 1 is an alkylene group having 1 to 12 carbon atoms; R 2 and R 3 each of which is independently an alkyl group, an aryl group, or an aryl group having from 1 to 20 carbon atoms; and k, m and n are each integers, where n is 1 or 2, m is 1 or 2, and k is 1 or 2, with the proviso that n+m+k is an integer of 3 or 4.

[0066] The reaction product having the formula (V) is prepared from the reaction of a living anionic polymer with a silane-sulfide terminator (modifier) ​​having the formula (VI): (R 2 O)bR 3 4-(n+b)Si-[R 1 S-SiR 4 R 5 R 6 ]n (VI) During the ceremony R 1 is an alkylene group having 1 to 12 carbon atoms; R 2 and R 3 each independently is an alkyl group, an aryl group, or an aryl group having 1 to 20 carbon atoms; R 4 , R 5 and R 6 each independently represents an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, provided that R 4 and R 5 may be bonded to each other via a covalent bond to form a ring with the silicon atom to which they are attached; and n and b are each an integer, where n is 1 or 2 and b is 1, 2 or 3, with the proviso that n+b is an integer from 2 to 4.

[0067] The protecting group is removed by any reaction which generates a free thiol group, such as hydrolysis or transesterification.

[0068] Representative, non-limiting examples of compounds of formula (V) include (CH3O)3Si-(CH2)3-S-Si(CH3)3, (CH3CH2O)3Si-(CH2)3-S-Si(CH3)3, (CH3CHO)3Si-(CH2)2-S-Si(CH3)3, (CH3CH2O)3Si-CH2-S-Si(CH3)3, (CH3CH2O)3Si-CH2CH(CH3)CH2-S-Si(CH3)3, (CH3CH2O)3Si-CH2CH(CH3)CH2-S-Si(CH3)3, (CH3CH2O)2(CH3)Si-( CH2)3-S-Si(CH3)3, (CH3CH2CH2O)3Si-CH2-S-Si(CH3)2C(CH3)3, (CH3O)3Si-CH2-C(CH3)2-CH2-S-Si(CH3)2C(CH3)3 , (CH3CH2O)3Si-CH2C(CH3)2CH2-S-Si(CH3)2C(CH3)3 and (CH3CH2O)3Si-CH2C(CH3)2CH2-S-Si(CH3)2C(CH3)3.

[0069] In some embodiments, the living anionic elastomeric polymer is selected from the group consisting of homopolymers of isoprene, homopolymers of butadiene, copolymers of butadiene and styrene, copolymers of isoprene and styrene, terpolymers of butadiene and isoprene and styrene, and combinations thereof.

[0070] In another embodiment, the living anionic elastomeric polymer is selected from the group consisting of homopolymers of butadiene and copolymers of butadiene and styrene.

[0071] Useful monomers for preparing the diene-based polymer (i) include conjugated olefins and olefins selected from the group including alpha-olefins, internal olefins, cyclic olefins, polar olefins, and non-conjugated diolefins.

[0072] Suitable conjugated unsaturated monomers are in particular conjugated dienes such as 1,3-butadiene, 2-alkyl-1,3-butadienes, in particular isoprene (2-methyl-1,3-butadiene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2,4-hexadiene, 1,3-hexadiene, 1,3-heptadiene, 1,3-octadiene, 2-methyl-2,4-pentadiene, cyclopentadiene, 2,4-hexadiene, 1,3-cyclooctadiene. Alpha olefins include, but are not limited to, long chain polymeric alpha olefins, more particularly aromatic vinyl compounds. Aromatic vinyl compounds include styrene, alkyl-substituted styrenes such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,4,6-trimethylstyrene, stilbene, 2,4-diisopropylstyrene, 4-tert-butylstyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, N,N-dimethylaminoethylstyrene, tert-butoxystyrene, vinylpyridine, and mixtures thereof.

[0073] Suitable polar olefins include acrylonitrile, methacrylate, methyl methacrylate. Suitable non-conjugated olefins include diolefins having from 4 to 20 carbon atoms, particularly norbornadiene, ethylidene norbornene, 1,4-hexadiene, 1,5-hexadiene, 1,7-octadiene, 4-vinylcyclohexene, divinylbenzene including 1,2-divinylbenzene, 1,3-divinylbenzene, 1,4-divinylbenzene, and mixtures thereof.

[0074] Preferred conjugated dienes include 1,3-butadiene, isoprene, and cyclopentadiene, and preferred aromatic alpha-olefins include styrene and 4-methylstyrene.

[0075] Non-limiting examples of diene-based polymers (i)(a) include homopolymers of conjugated dienes, especially butadiene or isoprene, as well as random or block copolymers and terpolymers of at least one conjugated diene, especially butadiene or isoprene, with at least one aromatic alpha-olefin, especially styrene and 4-methylstyrene, or aromatic diolefin, especially divinylbenzene. Particularly preferred are random copolymers, optionally terpolymers, of at least one conjugated diene with at least one aromatic alpha-olefin and / or aliphatic alpha-olefin, especially butadiene or isoprene with styrene and / or 4-methylstyrene.

[0076] In general, the polymerization of diene monomer(s) or copolymerization of diene monomer(s) with alpha-olefin monomer(s) may be accomplished under conditions well known for anionic living polymerization type polymerization reaction techniques, for example at temperatures of about -50 to about 250°C, preferably about 0 to about 120°C. This reaction temperature may be the same as the polymerization initiation temperature. The polymerization may be carried out continuously or discontinuously at atmospheric pressure, below atmospheric pressure, or at elevated pressures up to or even above 500 MPa. Preferably, the polymerization is carried out at pressures of about 0.01 to about 500 MPa, most preferably about 0.01 to about 10 MPa, and in particular about 0.1 to about 2 MPa. Higher pressures may also be applied. Initiators may also be used with good results in such high pressure processes.

[0077] Solution polymerization is usually carried out at lower pressures, preferably less than about 10 MPa. The polymerization can be carried out in gas phase as well as in a liquid reaction medium. The polymerization is generally carried out under batch, continuous or semi-continuous polymerization conditions. The polymerization process can be carried out as a gas phase polymerization, for example in a fluidized bed or stirred bed reactor, as a solution polymerization, where the polymer formed is substantially soluble in the reaction mixture, as a suspension / slurry polymerization, where the polymer formed is substantially insoluble in the reaction mixture, or as a so-called bulk polymerization process, where an excess of the monomers to be polymerized is used as the reaction medium.

[0078] Polymerization of the above-mentioned monomers is typically initiated with an anionic initiator such as, but not limited to, an organometallic compound having at least one lithium, sodium, potassium, or magnesium atom, such organometallic compound having from 1 to about 20 carbon atoms. Preferably, the organometallic compound has at least one lithium atom, such as ethyllithium, propyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, phenyllithium, hexyllithium, 1,4-dilithio-n-butane, 1,3-di(2-lithio-2-hexyl)benzene, and preferably n-butyllithium and sec-butyllithium. These organolithium initiators may be used alone or in combination as a mixture of two or more different types.

[0079] The amount of organolithium initiator used will vary based on the monomers being polymerized and the targeted molecular weight of the polymer being produced; however, this amount is typically from about 0.1 to about 5 mmol, preferably from about 0.3 to about 3 mmol, per 100 grams of monomer, where 100 grams of monomer is the total polymerizable monomers.

[0080] In order to adjust the microstructure, such as the content of vinyl bonds in the conjugated diolefin portion of a homopolymer, copolymer or terpolymer of the diolefin type, or to adjust the composition distribution of aromatic vinyl compounds in a copolymer or terpolymer containing a conjugated diene monomer, a polar coordinator compound may be optionally added to the polymerization mixture, thus acting, for example, as a randomizing component. Polar coordinator compounds include, for example, ether compounds such as diethyl ether, di-n-butyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, and propylene glycol dibutyl ether; alkyl tetrahydrofuryl ethers, such as methyl tetrahydrofuryl ether, ethyl tetrahydrofuryl ether, propyl tetrahydrofuryl ether, butyl tetrahydrofuryl ether, hexyl tetrahydrofuryl ether, and octyl tetrahydrofuryl ether; tetrahydrofuran; 2,2-( tertiary amine compounds such as bis-tetrahydrofurfuryl)propane, bis-tetrahydrofurfuryl formal, methyl ether of tetrahydrofurfuryl alcohol, ethyl ether of tetrahydrofurfuryl alcohol, butyl ether of tetrahydrofurfuryl alcohol, alpha-methoxytetrahydrofuran, dimethoxybenzene, and / or dimethoxyethane and / or butyl ether of triethylamine, pyridine, N,N,N',N'-tetramethylethylenediamine, dipiperidinoethane, methyl ether of N,N-diethylethanolamine, ethyl ether of N,N-diethylethanolamine, and / or N,N-diethylethanolamine.

[0081] The polar coordinator compound is typically added in a molar ratio of polar coordinator compound to lithium initiator within the range of about 0.012:1 to about 5:1, but typically from about 0.1:1 to about 4:1, preferably from about 0.25:1 to about 3:1, and most preferably from about 0.5:1 to about 3:2.

[0082] The polymerization can optionally be carried out using oligomeric oxolanyl alkanes as polar coordinator compounds, examples of which are provided in U.S. Patent Nos. 6,790,921 and 6,664,328, each of which is incorporated herein by reference.

[0083] The polymerization can optionally include an accelerator to increase the reactivity of the initiator, to randomly place the vinyl aromatic compounds incorporated into the polymer, or to result in single chains of vinyl aromatic compounds, thus influencing the compositional distribution of the vinyl aromatic compounds in the diene-based polymer (i).

[0084] Examples of applicable accelerators include sodium and potassium alkoxides or potassium phenoxides, such as potassium isopropoxide, potassium t-butoxide, potassium t-amyl oxide, potassium n-heptyl oxide, potassium benzyl oxide, potassium phenoxide; potassium salts of carboxylic acids, such as isovaleric acid, caprylic acid, lauric acid, palmitic acid, stearic acid, oleic acid, linoleic acid, benzoic acid, phthalic acid, or 2-ethylhexanoic acid; potassium salts of organic sulfonic acids, such as dodecylbenzenesulfonic acid, tetradecylbenzenesulfonic acid, hexadecylbenzenesulfonic acid, or octadecylbenzenesulfonic acid; and potassium salts of organic phosphoric acids, such as diethyl phosphite, diisopropyl phosphite, diphenyl phosphite, dibutyl phosphite, dilauryl phosphite. These potassium compounds may be added in an amount of about 0.005 to about 0.5 moles per 1.0 gram-atom equivalent of the lithium initiator. If less than 0.005 moles is added, typically no full effect is achieved, whereas if the amount of potassium compound exceeds 0.5 moles, the productivity and efficiency of the chain end modification reaction will be significantly reduced.

[0085] An alkali metal alkoxide compound may be added together with the polymerization initiator to improve the polymerization reactivity. The alkali metal alkoxide compound may be prepared by reacting an alcohol with an organic alkali metal compound. This reaction may be carried out in a hydrocarbon solvent in the presence of monomers, preferably conjugated diolefin monomers and aromatic vinyl compound monomers, prior to the copolymerization of these monomers.

[0086] The alkali metal alkoxide compound is illustratively represented by tetrahydrofurfuryl alcohol, N,N-dimethylethanolamine, N,N-diethylethanolamine, 1-piperazineethanolamine, or other metal alkoxides. The organic alkali metal compound may preferably be an organolithium compound, which can be used as a reactant for the alcohol compound to prepare the alkali metal alkoxide. For example, ethyllithium, propyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, hexyllithium, and mixtures thereof can be mentioned. Among these, n-butyllithium and sec-butyllithium are preferred. The molar ratio of the alcohol compound to the organolithium compound is about 1:0.7 to about 1:5.0, preferably about 1:0.8 to about 1:2.0, and most preferably about 1:0.9 to about 1:1.2. If the molar ratio of the organolithium compound to the alcohol compound exceeds 5.0, the effect of improving tensile strength, wear resistance, and hysteresis is impaired. On the other hand, if the molar ratio of the organolithium compound is less than 0.8, the polymerization rate slows down, productivity drops significantly, and the efficiency of the modification reaction of the chain ends decreases.

[0087] Coupling or linking agents may be used to further control the molecular weight and properties of the polymer. For example, if asymmetric coupling is desired, tin halides, silicon halides, tin alkoxides, silicon alkoxides, or mixtures of these compounds may be added continuously during polymerization.

[0088] This continuous addition is usually done in a reaction zone separate from the zone where the majority of the polymerization is occurring. The coupling agent can be added to the polymerization mixture in a hydrocarbon solvent, such as cyclohexane, with adequate mixing for dispersion and reaction. The coupling agent is typically added only after a high degree of conversion has already been achieved. For example, the coupling agent is usually added only after greater than 85 percent monomer conversion has been realized. It is typically preferred that the monomer conversion reach at least 90% before the addition of the coupling agent.

[0089] Common halide coupling agents include tin tetrachloride, tin tetrabromide, tin tetrafluoride, tin tetraiodide, silicon tetrachloride, silicon tetrabromide, silicon tetrafluoride, silicon tetraiodide; tin and silicon trihalides, or tin and silicon dihalides can also be used. Polymers coupled with tin or silicon tetrahalides have a maximum of four arms (or four polymer bond chains), tin and silicon trihalides have a maximum of three arms, and tin and silicon dihalides have a maximum of two arms. Hexahalodisilanes or hexahalodisiloxanes can also be used as coupling agents, resulting in polymers with a maximum of six arms. Useful tin and silicon halide coupling agents include SnCl4, (R 7 )3SnCl, (R 7 )2SnCl2, SiCl4, (R 7 )SiCl, (R 7 )2SiCl2,R 7 SiCl3, Cl3Si-SiCl3, Cl3Si-O-SiCl3, Cl3Sn-SnCl3, Cl3Sn-O-SnCl3, where R 7 is an alkyl group of 1 to 12 carbon atoms.

[0090] Examples of tin and silicon alkoxide coupling agents include Si(OCH3)4, Sn(OCH3)4, Sn(OCH2CH3)4 or Si(OCH2CH3)4. The most preferred coupling agents are SiCl4, Sn(OCH3)4 and Si(OCH3)4.

[0091] Combinations with tin or silicon compounds can optionally be used to bond to the polymer. By using such combinations of tin and silicon coupling agents, improved properties, such as low hysteresis, can be achieved for the diene-based polymer (i)(a) used in tires.

[0092] The combination of tin and silicon coupling agents is particularly desirable for use in tire tread compounds containing both silica and carbon black. In such cases, the molar ratio of tin to silicon compound used in coupling the diene-based polymer (i)(a) is typically in the range of about 20:80 to about 95:5; more typically about 40:60 to about 90:10, and preferably about 60:40 to about 85:15. Most typically, a range of about 0.01 to about 4.5 milliequivalents of coupling agent (tin and silicon compound) is used per 100 grams of diene-based polymer (i)(a). To obtain the desired Mooney viscosity, it is usually preferred to use about 0.01 to about 1.5 milliequivalents of coupling agent per 100 grams of diene-based polymer (i)(a). Higher amounts tend to produce polymers containing terminal reactive groups or that are poorly coupled. When between zero and less than one equivalent of tin and / or silicon coupling group is used per equivalent of lithium initiator, it allows for subsequent functionalization of the remaining living polymer moieties. For example, when tin or silicon tetrachloride, or a mixture of these compounds, is used as the coupling agent, between 0 and less than 1.0 mole, preferably between 0 and about 0.8 mole, and more preferably between 0 and about 0.6 mole of coupling agent is used for every 4.0 moles of living lithium polymer chain ends.

[0093] The coupling agent may be added in a hydrocarbon solution, such as cyclohexane, to the polymerization mixture in the reactor with adequate mixing for dispersion and reaction.

[0094] For the solution-based polymerization process, the polymerization is carried out in a suitable solvent, dispersant or diluent. Non-coordinating inert liquids are preferred, including but not limited to straight-chain and branched-chain hydrocarbons such as propane, butane, isobutane, pentane, hexane, heptane, octane, cyclic and cyclic aliphatic hydrocarbons such as cyclohexane, cycloheptane, methylcyclohexane, methylcycloheptane, aromatic and alkyl-substituted aromatic compounds such as benzene, toluene, and xylene, their isomers, their mixtures, and pentamethylheptane or mineral oil fractions, such as light or regular gasoline, naphtha, kerosene, or diesel. Fluorinated hydrocarbon fluids, such as perfluorinated alkanes containing 4 to 10 carbon atoms, are also suitable.

[0095] Additionally, suitable solvents, including liquid olefins, which may act as monomers or comonomers in the polymerization process include propylene, 1-butene, 1-pentene, cyclopentene, 1-hexene, 3-methyl-1-pentene, 4-methyl-1-pentene, butadiene, isoprene, 1,4-hexadiene, 1,7-octadiene, 1-octene, 1-decene, styrene, divinylbenzene, ethylidenenorbornene, allylbenzene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-vinylcyclohexane, and vinylcyclohexane.

[0096] Mixtures of solvents are also suitable. Aromatic hydrocarbons, such as benzene and toluene, can be used.

[0097] Suitable diene-based polymers (i)(a) containing at least one functional group, the functional groups being alkoxysilane and thiol groups, are commercially available, for example from Dow Olefin Compounds, and are of the type described in International Publication No. WO 2007 / 047943, the entire contents of which are incorporated herein by reference.

[0098] The diene-based polymer (i)(a) containing at least one functional group can be prepared according to US Patent Publication No. 2013 / 0165578A1, the entire contents of which are incorporated herein by reference. The diene-based polymer (i)(a) containing at least one functional group is an in-chain functionalized polybutadiene elastomer that contains a copolymer of in-chain repeat units derived from 1,3-butadiene monomer and a functionalizing monomer in an amount of about 0.2 to about 1.5 wt % based on the total weight of the monomers (1,3-butadiene monomer, and optionally styrene monomer and isoprene monomer). The functionalizing monomer has the structure of formula (VII): [ka] During the ceremony R 9 is hydrogen or an alkyl group of 1 to 4 carbon atoms; R 10 is a functional group having the formula (VIII): [ka] wherein p and o are each integers, where p is from 2 to 10 and o is from 0 to 10, or having the formula (IX): -(CH2) g NR 12 2(IX) During the ceremony R 12 each independently represents an alkyl group of 1 to 10 carbon atoms, an aryl group of 6 to 10 carbon atoms, or R 12 The group is connected to another R via an oxygen atom. 12 -(CH2) bonded to the nitrogen atom by the group qO-(CH2) r -group, where q and r are each integers, q is 1 to 10 and r is 1 to 10; and g is an integer from 0 to 10.

[0099] Representative non-limiting examples of functional monomers include pyrrolidine ethyl styrene, vinylbenzyl pyrrolidine, vinylbenzyl dimethylamine.

[0100] In some embodiments, the intrachain functionalized polybutadiene includes repeat units derived from 1,3-butadiene and / or isoprene, and at least one of pyrrolidine ethyl styrene, vinylbenzyl dimethylamine, and vinylbenzyl pyrrolidine. The repeat units of isoprene may, for example, comprise from 0 to about 25 weight percent, more specifically from about 2 to about 15 weight percent, the weight percent being based on the total weight of the copolymer.

[0101] In one embodiment, the functionalized polybutadiene rubber is a copolymer of 1,3-butadiene and a functionalized monomer, prepared by anionic copolymerization of 1,3-butadiene and the functional monomer in a hydrocarbon solvent in the presence of a polymerization initiator including n-butyllithium to initiate the copolymerization, and optionally in the presence of a polymerization modifier to facilitate the incorporation and / or dispersion of the functional monomer units along the polybutadiene chain, such as, but not limited to, tetramethylethylenediamine.

[0102] In another embodiment, the diene-based polymer (i)(a) containing at least one functional group, when prepared according to U.S. Patent No. 6,664,328, the entirety of which is incorporated herein by reference, has a cis 1,4-isomer content in the range of about 30 to about 50 percent, a trans 1,4-isomer content in the range of about 40 to about 60 percent, and a vinyl content in the range of about 5 to about 20 percent, a glass transition temperature (Tg) in the range of about -85°C to about -95°C, and a number average molecular weight (Mn) in the range of, for example, about 75,000 to about 350,000, and a weight average to number average dispersity (MW / Mn) in the range of, for example, about 1 to about 2.5, or about 1.5 to about 2.5. The number average molecular weight and weight average molecular weight are determined by ASTM D6474-20, Standard Test Method for Determination of Molecular Weight Distribution and Average Molecular Weight of Polyolefins by High Temperature Gel Permeation Chromatography.

[0103] The diene-based polymer (i)(a) containing at least one functional group includes a polymer in which the functional group reacts with at least one silicic acid functional group to form a silicic acid functionalized polymer, as disclosed in DE102013100009A1, the entire contents of which are incorporated herein by reference. In particular, the solution-polymerized diene-based polymer (i)(a) containing at least one functional group reacts with silicic acid to form a silicic acid functionalized styrene butadiene polymer. These diene-based polymers (i)(a) show a good effect on wear properties.

[0104] In one embodiment, the silicic acid functionalized styrene butadiene polymer has a vinyl content of from about 10 to about 80 weight percent, more preferably from about 10 to about 70 weight percent, and a styrene content of from 0 to about 50 weight percent, and especially preferably from 0 to about 35 weight percent, where the weight percent is based on the total weight of the diene-based polymer (i)(a).

[0105] The functionalization of silica in this application is effected by reaction with hydroxyl, epoxy, siloxane, phthalocyanine, aminosiloxane and / or carboxy groups. The functional groups include -OH, -COOH, -COCl, -SH, -CSSH, -NCO, amino, epoxy, silyl, silanol or siloxane groups, including polysiloxanes. The siloxane groups are attached to the diene-based polymer chain with or without a linking group.

[0106] Silyl, silanol, and siloxane groups are represented by -ASiH2(OH), -ASi(R 13 )2(OH), -ASiH(OH)2, -ASiR 13 (OH)2, -ASi(OH)3, -ASi(OR 13 )3, -A(SiR 13 R 14 O) u -R 15 , -ASi(R 15 )3 or -ASi(A 1 N(R 15 )2) v (OR 13 ) w (R 15 ) 3-(v+w) where R 13 and R 14 each of R15 is independently an alkoxy group, a straight chain alkyl group containing 1 to 12 carbon atoms, a branched chain alkyl group containing 3 to 12 carbon atoms, a cyclic alkyl group containing 5 to 12 carbon atoms, an aryl group containing 6 to 12 carbon atoms, an alkylaryl group containing 7 to 12 carbon atoms, an aralkyl group containing 7 to 12 carbon atoms, or vinyl, each R15 is independently a straight chain alkyl group containing 1 to 12 carbon atoms, a branched chain alkyl group containing 3 to 12 carbon atoms, a cyclic alkyl group containing 5 to 12 carbon atoms, or hydrogen, each of u, v and w is an integer, where u is 1 to 1500, v is 0 to 3, and w is 0 to 3, with the proviso that v+w is less than or equal to 3; and A and A 1 Each of is an alkylene group of 1 to 12 carbon atoms or a single covalent bond.

[0107] One embodiment includes a diene-based polymer (i) having a number average molecular weight of about 150,000 to about 400,000, more specifically about 200,000 to about 300,000, and even more specifically about 225,000 to about 275,000, prior to functionalization with silicic acid, the diene-based polymer (i)(a) having at least one terminal functional group comprising a styrene-butadiene copolymer, a butadiene homopolymer having a cis-1,4 bond content of 90 percent or greater, a syndiotactic-1,2-polybutadiene, an isoprene rubber, a styrene-isoprene copolymer, or a butadiene-isoprene copolymer.

[0108] As for the diene-based polymer (i)(a) having a terminal functional group, the functional group can be derived from various compounds, in particular from tin compounds, aminobenzophenone compounds, isocyanate compounds, diglycidylamine compounds, cyclic imine compounds, alkoxysilane halide compounds, glycidoxypropylalkoxysilane compounds, and neodymium compounds.

[0109] The living diene polymer used to prepare the diene polymer (i)(a) with at least one functional group has a number average molecular weight (Mn) of about 150,000 to about 400,000, and more preferably about 150,000 to about 250,000, prior to functionalization. If the Mn is less than 150,000, the diene polymer (i)(a) cannot exhibit sufficient strength. Conversely, if the Mn is greater than about 400,000, the diene polymer (i)(a) is insufficiently effective in improving low fuel consumption characteristics. In addition, if the diene polymer (i)(a) is bonded to each other due to terminal functional groups, resulting in a doubling or tripling of the molecular weight, it is difficult to process. The number average molecular weight and weight average molecular weight are determined by ASTM D6474-20, Standard Test Method for Determination of Molecular Weight Distribution and Average Molecular Weight of Polyolefins by High Temperature Gel Permeation Chromatography.

[0110] To prepare the diene-based polymer (i)(a) containing silicic acid functionalization, a conjugated diene compound or a vinyl-substituted aromatic compound is copolymerized in the presence of an organolithium initiator. The resulting conjugated diene polymers and copolymers containing a conjugated diene compound and a vinyl-substituted aromatic compound have an initial weight average molecular weight of about 1,000 to about 300,000 as measured by ASTM D6474-20. The conjugated diene polymers or copolymers may have a weight average molecular weight in the range of about 1,000 to about 1,200,000, and more specifically about 10,000 to about 500,000.

[0111] An organolithium initiator is used as a polymerization initiator.The organolithium initiator is a hydrocarbon compound having at least one lithium atom, and specific examples thereof may include ethyllithium, propyllithium, n-butyllithium, sec-butyllithium, tert-butyllithium, phenyllithium, propenyllithium, hexyllithium, 1,4-dilithio-n-butane, and l,3-di(2-lithio-2-hexyl)benzene, preferably n-butyllithium and sec-butyllithium.These organolithium initiators may be used alone or in combination as a mixture of two or more different types.

[0112] The amount of organolithium initiator will vary based on the targeted molecular weight of the polymer being produced, but will typically be from about 0.1 to about 5 mmol, preferably from about 0.3 to about 4 mmol, per 100 grams of the total weight of the monomers used.

[0113] Non-limiting examples of hydrocarbon solvents for polymerization, as used herein, include n-butane, isopentane, n-hexane, n-heptane, isooctane, cyclohexane, methylcyclopentane, benzene, and toluene, preferably n-hexane, n-heptane, and cyclohexane. The hydrocarbon solvent is used in an amount of about 0.1 to about 25 parts by weight per part by weight of monomer, more specifically in an amount of about 1 to about 20 parts by weight per part by weight of monomer, and even more specifically in an amount of about 5 to about 15 parts by weight per part by weight of monomer.

[0114] Suitable conjugated diene compounds include isoprene and 1,3-butadiene, and suitable vinyl-substituted aromatic compounds include styrene and alpha-methylstyrene. The diene-based polymer (i)(a) may contain about 10 to 100% by weight of conjugated diene monomer and 0 to about 90% by weight of vinyl-substituted aromatic monomer, more specifically about 20 to about 80% by weight of conjugated diene monomer and about 20 to about 80% by weight of vinyl-substituted aromatic monomer, and even more specifically about 30 to about 50% by weight of conjugated diene monomer and about 50 to about 70% by weight of vinyl-substituted aromatic monomer, based on the total weight of monomers used.

[0115] The ends of the living diene polymer are then reacted in the presence of a coupling agent which is an organic compound, where the coupling agent has a group, such as a hydrolyzable silyl group, capable of reacting with the carbanion of the living polymer.

[0116] One embodiment is a diene-based polymer (i)(a) in which both ends contain functional groups. These diene-based polymers (i)(a) are prepared according to U.S. Patent No. 9,328,176 B2, the entire contents of which are incorporated herein by reference.

[0117] The difunctional initiator may be obtained by a general method that describes the addition of a monoorganolithium initiator to a reactor in the presence of a non-polar hydrocarbon solvent and a polar additive, followed by the slow addition of a divinylaromatic material to the solution. For the preparation of the difunctional initiator, examples of divinylaromatic materials are selected from the group consisting of 1,3-divinylbenzene, 1,4-divinylbenzene, 1,3-diisopropenylbenzene, 1,3-dipropenylbenzene, 1,4-diisopropenylbenzene, 2,4-diisopropenyltoluene, 2,4-divinyltoluene, 1,3-distyrylbenzene, 1,4-distyrylbenzene, 1,2-distyrylbenzene, 1,3-diisobutenylbenzene, and 1,3-diisopentenylbenzene; among these compounds, 1,3-diisopropenylbenzene is most preferably selected.

[0118] Non-limiting examples of organolithium initiators include n-butyllithium, sec-butyllithium, and t-butyllithium; preferably, 2 to 2.5 equivalents of t-butyllithium are used proportionally to 1 equivalent of divinyl aromatic material.

[0119] Additionally, non-polar hydrocarbon solvents may be used alone or in mixture with cycloaliphatic hydrocarbon solvents such as cyclohexane or cyclopentane, or aliphatic hydrocarbon solvents such as n-hexane or n-heptane; among these compounds, cyclohexane is the most preferred choice.

[0120] Examples of polar additives include dialkyl ethers, cyclic ethers, and trialkylamines. The polar additive is used in the range of about 0.3 to about 2.0 equivalents relative to one equivalent of lithium ion of the organolithium initiator, and more particularly in the range of about 0.5 to about 1.5 equivalents. It is preferred that triethylamine is used in the range of about 0.5 to about 1.5 equivalents, and more preferably in the range of about 0.7 to about 1.2 equivalents, relative to one equivalent of lithium ion of the organolithium initiator.

[0121] The first reaction step for preparing the difunctional initiator is carried out at a temperature of about -40 to about 40° C. for about 1 to about 10 hours, more preferably at a temperature of about -40 to about 20° C. for about 1 to about 3 hours. The second reaction step is that the difunctional initiator thus prepared is added to the conjugated diene-aromatic vinyl monomer in the presence of a non-polar hydrocarbon solvent and a polar additive to activate one end of the difunctional initiator, thus synthesizing a random copolymer.

[0122] Preferred examples of non-polar hydrocarbon solvents include cyclohexane, n-hexane, and n-heptane, or mixtures thereof. Cyclic ethers and dialkyl ethers are used as randomizers in the most preferred range of 0.2 to 5 wt %.

[0123] Additionally, the conjugated diene monomer of 4 to 8 carbon atoms may be selected from the group consisting of 1,3-butadiene, 2-methyl-1,3-butadiene, 1,3-pentadiene, or 1,3-hexadiene. Non-limiting examples of aromatic vinyl monomers include styrene or alpha methyl styrene.

[0124] The second step reaction is carried out at a temperature of about -40 to about 70°C until the conversion of monomer to polymer exceeds 90 percent. It is preferred to carry out the reaction until the conversion exceeds 95 percent, and most preferred to carry out the reaction until the conversion exceeds 99 percent. The random copolymer prepared through the second step reaction preferably has a styrene content in the range of about 10 to about 30 weight percent, more preferably in the range of about 15 to about 25 weight percent. Furthermore, the vinyl content is in the range of about 40 to about 70 weight percent, more preferably in the range of about 40 to about 50 weight percent. The final third step reaction is the addition of a polar material to the random polymer, followed by the addition of an electrophilic material to the active sites on both ends of the polymer, thus forming a polymer with functional groups at both ends.

[0125] Ethers and tertiary amines can be used as polar materials. Specific examples of polar materials include diethyl ether, di-n-propyl ether, diisopropyl ether, di-n-butyl ether, tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, trimethylamine, triethylamine, N',N,N',N'-tetramethylethylenediamine, and N,N,N',N',N''-pentamethyldiethylenetriamine. Relative to one equivalent of lithium ion, less than 100 equivalents of polar material may be used, most preferably less than 10 equivalents.

[0126] Further, examples of electrophilic materials added to both ends of the polymer include aminoketones, aminoaldehydes, thioaminoketones, thioaminoaldehydes, and amides. The electrophilic material is added to the polymer in the range of about 0.5 to about 3 equivalents relative to one equivalent of lithium ion. In particular, in the case of 4-dimethylaminobenzophenone, 4-diethylaminobenzophenone, or 4,4'-bis-(diethylamino)benzophenone, it is most preferable to use about 0.8 to about 1.5 equivalents relative to one equivalent of lithium ion.

[0127] The third step reaction is carried out at a temperature of about -40 to about 80° C. for about 1 to about 6 hours, and more specifically at a temperature of about 60 to about 80° C. for about 1 to about 2 hours.

[0128] Applicable weight average molecular weights for the random copolymers prepared from this three-step reaction are in the range of about 100,000 to about 500,000, preferably in the range of about 200,000 to about 400,000.

[0129] An embodiment provides a diene-based polymer (i)(a) containing at least one functional group, where the polymer is prepared by radical polymerization in emulsion of styrene monomer, butadiene monomer, and epoxy acrylate monomer, and ring-opening of styrene-butadiene-epoxy acrylate copolymer. Such diene-based polymer (i)(a) containing at least one functional group is prepared according to U.S. Patent No. 9,328,176 B2, the entire contents of which are incorporated herein by reference. Such diene-based polymer contributes to wet braking properties and wear resistance when blended with silica.

[0130] Among the monomers used in the polymerization reaction, the styrene monomer may be one or more selected from styrene, methylstyrene, and dimethylstyrene, and is used in an amount of about 10 to about 50% by weight, more specifically about 20 to about 40% by weight, based on the total weight of the monomers. If used in an amount less than 10% by weight, the tensile properties and other mechanical properties may be insufficient. On the other hand, if used in an amount greater than 50% by weight, the elasticity and abrasion resistance may be insufficient. The butadiene monomer may be one or more of 1,3-butadiene and isoprene, and is used in an amount of about 45 to about 85% by weight, and more specifically about 60 to about 80% by weight, based on the total weight of the monomers. If used in an amount less than 45% by weight, the elasticity and abrasion resistance may be insufficient. On the other hand, if used in an amount greater than 85% by weight, the tensile properties and other mechanical properties may be insufficient. In the copolymers produced from styrene and butadiene monomers, the butadiene units may have a trans or cis configuration.

[0131] The epoxy acrylate monomer may be glycidyl acrylate or glycidyl methacrylate, and is preferably used in an amount of about 0.1 to about 10% by weight, more particularly about 1 to about 8% by weight, and even more particularly about 2 to about 5% by weight, based on the total weight of the monomers. If used in an amount less than 0.1% by weight, the styrene-butadiene-acrylate copolymer may have insufficient hydrophilicity. On the other hand, if used in an amount greater than 10% by weight, the elasticity may decrease and strength may increase, making processing difficult.

[0132] Radical initiators commonly used in the technical field may be used.The radical initiator system used in emulsion polymerization may be selected from persulfates such as potassium persulfate and ammonium persulfate, acetylacetone peroxide, benzoyl peroxide, dicumyl peroxide, p-menthane hydroperoxide, 2,4-dichlorobenzoyl peroxide, t-butyl peracetate, 2,2'-azobis(isobutylamidine) dihydrochloride, azobisisobutyronitrile, hydrogen peroxide, redox systems, ferrous sulfate, and others.

[0133] In the polymerization of styrene, butadiene, and epoxy acrylate monomers, the hydroxyl functional group can participate in the opening of the epoxy ring. In the first step of the radical polymerization of styrene, butadiene, and epoxy acrylate monomers, an emulsion state is carried out to prepare the copolymer, and in the second step, the epoxy ring is opened under acidic or alkaline conditions. As a result of the opening of the epoxy ring, the copolymer has a pendant ester containing a 1,2-dihydroxypropyl group.

[0134] In the preparation of diene-based polymer (i)(a), the radical initiator is used in an amount of about 0.05 to about 3 parts by weight, and more particularly about 0.1 to about 2 parts by weight, based on the total weight of the monomers. If used in an amount less than 0.05 parts by weight, sufficient polymerization may not occur. On the other hand, if used in an amount more than 3 parts by weight, a low molecular weight copolymer may be obtained.

[0135] Furthermore, anionic, cationic or nonionic surfactants may be used as emulsifiers. Anionic surfactants may be selected from metal alkyl sulfates, metal alkylaryl sulfonates, metal alkyl phosphates, ammonium alkyl sulfates, ammonium alkylaryl sulfonates, ammonium alkylaryl sulfonates, ammonium allyl sulfonates, or ammonium alkyl phosphates. In particular, metal or ammonium salts of dodecylbenzene sulfonic acid, rosin acid, fatty acids, lauryl sulfonic acid, or hexadecyl sulfonic acid may be used. Cationic surfactants include tetra-substituted ammonium halides such as dodecyltrimethylammonium chloride. Nonionic surfactants are polyalkylene oxide polymers starting from hydroxyl-terminated hydrocarbons.

[0136] The emulsifier is used in an amount of from about 0.1 to about 10 parts by weight, and more specifically from about 1 to about 5 parts by weight, based on 100 parts by weight of total monomers.

[0137] Furthermore, in the preparation of the diene-based polymer (i)(a), a mercaptan compound having 8 to 20 carbon atoms may be used as a molecular weight regulator. Preferably, one or more selected from octyl mercaptan, decyl mercaptan, dodecyl mercaptan, and hexadecyl mercaptan may be used. The average molecular weight of the styrene-butadiene copolymer may be adjusted by controlling the amount of the molecular weight regulator. When the mercaptan-based molecular weight regulator is used in an amount of about 0.001 to about 2 parts by weight based on 100 parts by weight of the total monomers, a high molecular weight styrene monomer-butadiene copolymer may be prepared. On the other hand, when the mercaptan-based molecular weight regulator is used in an amount of about 0.5 to about 2 parts by weight, a low molecular weight styrene-butadiene copolymer may be prepared. When the mercaptan-based molecular weight regulator is used in an amount of less than 0.0001 parts by weight, gelation may occur. On the other hand, when it is used in an amount of more than 2 parts by weight, a decrease in physical properties may occur.

[0138] In preparing the diene-based polymer (i)(a), diethylhydroxylamine, N-isopropylhydroxylamine, monoethylhydroxylamine, sodium dimethyldithiocarbamate, or the like may be used as a polymerization terminator. Preferably, the polymerization terminator may be used in an amount of about 0.01 to about 2 parts by weight, more specifically about 0.1 to about 1 part by weight, based on 100 parts by weight of the total monomers.

[0139] The method for preparing the diene-based polymer includes multiple steps. First, styrene monomer, butadiene monomer, and epoxy acrylate monomer are radically polymerized in emulsion at about 0 to about 70° C., more specifically about 15 to about 60° C., for about 4 to about 48 hours. As a result, a styrene-butadiene copolymer is prepared having an average molecular weight of about 100,000 to about 2,000,000 grams per mole, more specifically about 200,000 to about 1,000,000 grams per mole.

[0140] The epoxy group is ring-opened in the presence of a nucleophile such as an acid, a base or an amine, thereby improving the compatibility with silica. The acid can be sulfuric acid, phosphoric acid, hydrochloric acid, acetic acid, hydrofluoric acid or others, and the base can be sodium hydroxide, potassium hydroxide, ammonium hydroxide or others. Preferably, the ring-opening acid or base is used in an amount of about 1 to about 20 parts by weight, more specifically about 2 to about 10 parts by weight, based on 100 parts by weight of the total monomer.

[0141] The diene-based polymer (i)(a) prepared by emulsion polymerization has particles within the range of about 20 to about 2000 nanometers and has an average molecular weight of about 100,000 to about 3,000,000 grams per mole, and more specifically has an average molecular weight of about 40 to about 1500 nanometers and about 150,000 to about 2,000,000 grams per mole.

[0142] One embodiment is to provide a diene-based polymer (i)(a) containing at least one functional group, where the functional group is a stannyl functional group. The diene-based polymer (i)(a) containing at least one functional group can be prepared according to U.S. Pat. No. 5,514,757, the entirety of which is incorporated herein by reference. Anionic polymerization of the monomers is carried out as described above. The living anionic polymer is then reacted with a tin compound. Useful tin compounds include SnCl4, (R 16 )3SnCl, (R 16 )2SnCl2, SiCl4, (R 16 )SiCl, (R 16 )2SiCl2,R 16 SiCl3, Cl3Si-SiCl3, Cl3Si-O-SiCl3, Cl3Sn-SnCl3, Cl3Sn-O-SnCl3, where R 16 contains an alkyl group of 1 to 12 carbon atoms, Sn(OCH3)4 or Sn(OCH2CH3)4. The most preferred coupling agents are SiCl4, Sn(OCH3)4, and Si(OCH3)4. Diene-based polymers not containing functional groups (i)(b)

[0143] In some embodiments, the diene-based polymer may include a diene-based polymer that does not contain functional groups.

[0144] The other rubber component, the non-functional diene-based polymer (i)(b), is any suitable vulcanizable, i.e., curable, rubber (organic polymer) well known in the art and described in numerous references, to name just two, "The Vanderbilt Rubber Handbook," edited by RF Ohm (Vanderbilt, Norwalk, Conn., 1990), and "The Rubber Industry Manual," edited by T. Kempermann, S. Koch and J. Sumner (Bayer, Leverkusen, Germany, 1993), the contents of which are incorporated herein in their entirety to the extent not inconsistent with the present disclosure.

[0145] Representative examples of suitable vulcanizable polymers include solution polymerization prepared styrene butadiene rubber (S-SBR), emulsion polymerization prepared styrene butadiene rubber (E-SBR), natural rubber (NR), polybutadiene (BR), ethylene-propylene copolymers and terpolymers (EP, EPDM), and acrylonitrile-butadiene rubber (NBR). The rubber composition of the present application contains at least one diene-based elastomer, i.e., rubber. Suitable conjugated dienes are isoprene and 1,3-butadiene, and suitable vinyl aromatic compounds are styrene and alpha-methylstyrene.

[0146] The diene-based polymer (i)(b), i.e., rubber, may be selected from, for example, at least one of cis-1,4-polyisoprene rubber (natural and / or synthetic, and preferably natural rubber), emulsion polymerization prepared styrene / butadiene copolymer rubber, organic solution polymerization prepared styrene / butadiene rubber, 3,4-polyisoprene rubber, isoprene / butadiene rubber, styrene / isoprene / butadiene terpolymer rubber, cis-1,4-polybutadiene, medium vinyl content polybutadiene rubber (35 percent to 50 percent vinyl), high vinyl content polybutadiene rubber (50 percent to 75 percent vinyl), styrene / isoprene copolymer, emulsion polymerization prepared styrene / butadiene / acrylonitrile terpolymer rubber, and butadiene / acrylonitrile copolymer rubber. Also useful are styrene / butadiene (E-SBR) derived from emulsion polymerization prepared and having a relatively conventional styrene content of 20 to 28 percent bound styrene, and for some applications, E-SBR having a medium to relatively high bound styrene content, i.e., 30 to 45 percent bound styrene. Styrene / butadiene / acrylonitrile terpolymer rubbers prepared by emulsion polymerization and containing 2 to 40 weight percent bound acrylonitrile in the terpolymer are also considered diene-based polymers.

[0147] Solution polymerization prepared SBR (S-SBR) typically has a bound styrene content within the range of from about 5 to about 50 percent, preferably from about 9 to about 36 percent. The polybutadiene elastomer may, for example, be conveniently characterized by having at least a 90 weight percent cis-1,4-content.

[0148] The total weight of the rubber composition is the sum of the sum of the weights of each of the diene-based polymers (i)(a) that contain at least one functional group and the sum of the weights of each of the diene-based polymers (i)(b) that do not contain functional groups. The total weight of the rubber composition is set to 100 parts by weight of rubber. This weight includes only the weights of the diene-based polymers (i)(a) and (i)(b) and does not include the weights of processing oils, solvents or other additives that may be blended with the polymers. Of each 100 parts by weight of rubber, the total weight of each of the diene-based polymers (i)(a) containing at least one functional group may be from 0 to about 100 parts by weight of diene-based polymer (i)(a) based on 100 total parts by weight of rubber (phr), more specifically from about 5 to about 100 parts by weight of diene-based polymer (i)(a), even more specifically from about 20 to about 90 parts by weight of diene-based polymer (i)(a) based on 100 total parts by weight of rubber (phr), and even more specifically from about 40 to about 80 parts by weight of diene-based polymer (i)(a) based on 100 total parts by weight of rubber (phr). and the total weight of each of the diene-based polymers (i)(b) that do not contain functional groups is from 0 to about 100 parts by weight of diene-based polymer (i)(b) based on 100 total parts by weight of rubber, more specifically from 0 to about 95 parts by weight of diene-based polymer (i)(b) based on 100 total parts by weight of rubber, even more specifically from about 10 to about 80 parts by weight of diene-based polymer (i)(b) based on 100 total parts by weight of rubber (phr), and still even more specifically from about 20 to about 60 parts by weight of diene-based polymer (i)(b) based on 100 total parts by weight of rubber (phr).

[0149] In some embodiments, the compositions of the present disclosure may comprise about 20% to about 50%, about 25% to about 50%, about 30% to about 50%, about 35% to about 50%, about 40% to about 50%, about 45% to about 50%, about 20% to about 45%, about 25% to about 45%, about 30% to about 45%, about 35% to about 45%, about 40% to about 45%, about 20% to about 40%, about 25% to about 40%, about 30% to about 40%, about 35% to about 40%, about 20% to about 35%, about 25% to about 35%, about 30% to about 35%, about 20% to about 30%, or about 25% to about 30% by weight of at least one diene-based polymer. Precipitated Silica Component (ii)

[0150] In one embodiment, precipitated silica (ii) is used as the silane-reactive filler. The preferred silica may be characterized by a BET specific surface area measured using nitrogen gas, preferably from about 40 to about 600 m. 2 / g, and more usually in the range of about 50 to about 300 m 2 / g range. Preferred silicas may also be characterized by having a dibutyl phthalate (DBP) adsorption value ranging from about 100 to about 350, and more usually from about 150 to about 300. Furthermore, the silica fillers, as well as the alumina and aluminosilicate fillers mentioned above, may be characterized by having a cetyltrimethylammonium bromide (CTAB) specific surface area ranging from about 100 to about 240. CTAB specific surface area is the external specific surface area measured using cetyltrimethylammonium bromide at pH 9 using the method of ASTM D3849.

[0151] The mercury pore surface area is the specific surface area determined by the mercury porosimetry method. According to this method, mercury is allowed to penetrate into the pores after a heat treatment to remove volatiles from the measured sample of particulate filler. A typical set of conditions includes a 100 mg sample, 2 hours of removal of volatiles at 105°C and atmospheric pressure, and pressures ranging from atmospheric to 2000 bar. The mercury porosimetry method may be carried out according to Winslow and Shapiro, ASTM Proceedings, p. 39 (1959), or according to DIN 66133. For such a method, a CARLO-ERBA Porosimeter 2000 may be used. The average mercury pore specific surface area for a typical silica filler is about 100 to about 300 m 2 / g.

[0152] Suitable pore size distributions for silica, alumina, and aluminosilicates by the above-mentioned mercury porosimetry methods are: 5 percent or less of the pores have a diameter less than 10 nm; about 60 percent to about 90 percent of the pores have a diameter of about 10 to about 100 nm; about 10 percent to about 30 percent of the pores have a diameter of about 100 to about 1,000 nm; and about 5 percent to about 20 percent of the pores have a diameter greater than 1,000 nm.

[0153] The silica may be expected to have an average final particle size within the range of about 0.01 to about 0.05 μm, for example, as determined by electron microscopy, although the silica particles may be smaller or larger in size. A variety of commercially available silicas are useful, such as those available under the trademark HI-SIL from PPG Industries, Inc., such as HI-SIL 190, 210, 243, and other designations; those available from Solvay (formerly known as Rhodia), such as ZEOSIL 1165MP, Zeosil 195HR, and Zeosil Premium 200MP; those available from Evonik Industries, Inc., such as VN2 and VN3, and Ultrasil 7000GR, and other designations; and those available from Huber, Inc., such as HUBERSIL 8745.

[0154] In one embodiment, when it is desired that the rubber composition contains both precipitated silica (ii) and other fillers, non-limiting representative examples are titanium dioxide, alumina, and siliceous materials such as aluminosilicates, clays, and talc, and mixtures thereof. Inert, i.e., non-reactive with silane, filler(s), such as carbon black, acetylene black, calcium carbonate, and barium sulfate, may be used with the silane-reactive particulate filler(s) (ii). For use in rubber products such as tire treads, a combination of silica and carbon black is particularly advantageous. Alumina may be used alone or in combination with silica. In this application, the term "alumina" refers to aluminum oxide, i.e., Al2O3. The filler may be in the hydrated or anhydrous form. The use of alumina in rubber compositions is described, for example, in U.S. Pat. No. 5,116,886 and European Patent 0631982, each of which is incorporated herein by reference in its entirety.

[0155] In another embodiment, with precipitated silica (ii) and carbon black as fillers / reinforcing pigments, the weight ratio of precipitated silica to carbon black is often preferred to be at least about 3 / 1, preferably at least about 10 / 1 to about 30 / 1. The filler can comprise about 15 to about 95% by weight of precipitated silica and correspondingly about 5 to about 85% by weight of carbon black, where the carbon black has a CTAB value in the range of about 80 to about 150. Alternatively, the filler can comprise about 60 to about 95% by weight of precipitated silica and correspondingly about 40 to about 5% by weight of carbon black. The precipitated silica and carbon black fillers can be preblended or blended together during the preparation of the vulcanized rubber.

[0156] The precipitated silica (ii) is used in an amount of about 5 to about 140 parts by weight of precipitated silica per 100 parts by weight of rubber (phr). In another embodiment, the precipitated silica (ii) can be used specifically in an amount of about 40 to about 110 phr, more specifically in an amount of about 60 to about 80 phr. When carbon black is used, the amount can vary from about 0.5 to about 50 parts by weight of carbon black per 100 parts by weight of rubber, more specifically from about 1 to about 10 phr, and even more specifically from about 2 to about 5 phr. Carbon black is used to impart a black color to the rubber composition, as an ultraviolet (UV) stabilizer, and to discharge static electricity formed from the use of articles such as tires.

[0157] Other fillers, such as titanium dioxide, clays, siliceous fillers such as aluminates, aluminosilicates, particulate iron oxide and others, can be used at various addition levels including, for example, from about 1 to about 50 parts by weight of filler per 100 parts by weight of rubber, and more specifically, from about 5 to about 25 phr.

[0158] In some embodiments, the compositions of the present disclosure may comprise about 20% to about 50%, about 25% to about 50%, about 30% to about 50%, about 35% to about 50%, about 40% to about 50%, about 45% to about 50%, about 20% to about 45%, about 25% to about 45%, about 30% to about 45%, about 35% to about 45%, about 40% to about 45%, about 20% to about 40%, about 25% to about 40%, about 30% to about 40%, about 35% to about 40%, about 20% to about 35%, about 25% to about 35%, about 30% to about 35%, about 20% to about 30%, or about 25% to about 30% precipitated silica by weight. Coupling Agent Package (iii)

[0159] At least one coupling agent package includes a mercapto-functional alkylalkoxysilane and a blocked mercapto-functional alkylalkoxysilane.

[0160] The coupling agent package (iii) includes a mercaptosilane (iii)(a) and a blocked mercaptosilane (iii)(b).

[0161] In one embodiment, the mercaptosilane (iii)(a) has the general formula (X): [ka] During the ceremony R 17 independently a straight chain alkylene group of 1 to 6 carbon atoms or a branched chain alkylene group of 3 to 6 carbon atoms; R 18 each of which is a straight chain alkylene group of from 2 to 8 carbon atoms or a branched chain alkylene group of from 3 to 8 carbon atoms; R 19 each independently is a straight chain alkylene group of 1 to 6 carbon atoms or a branched chain alkylene group of 3 to 6 carbon atoms; X 1 -OR 20 Group, where R 20 is an alkyl group of 1 to 4 carbon atoms, -OR 21 OH group, where R21 is a straight chain alkylene group having 2 to 8 carbon atoms or a branched chain alkylene group having 3 to 8 carbon atoms, or X 1 -OR 22 (OR 23 ) c OR 24 , where R 22 is a linear alkylene group of 2 to 6 carbon atoms or a branched alkylene group of 3 to 6 carbon atoms, preferably 3 carbon atoms; each R 23 are independently an alkylene group of 2 to 4 carbon atoms, and R 24 is hydrogen, a straight chain alkyl group of 1 to 16 carbon atoms or a branched chain alkyl group of 3 to 16 carbon atoms, and c is an integer from 1 to 20; X 2 and X 3 is independent of X 1 or methyl; X 4 Each of X is independent. 1 or methyl; and a is an integer from 0 to 8, (i)X 1 and X 2 -OR 20 When , two -OR 20 are bonded together via covalent bonds to the same silicon atom -OR 20 -R 20 O-groups to form a ring structure containing 2 to 8 carbon atoms, 2 oxygen atoms, and a silicon atom; and (ii) a is 1 to 8 and X 3 and X 4 -OR 20 When , two -OR 20 The groups are linked together via covalent bonds and attached to the same silicon atom -OR 20 -R 20 The O-groups may be formed to form a ring structure containing from 2 to 8 carbon atoms, two oxygen atoms and a silicon atom group.

[0162] In another embodiment, the mercaptosilane (iii)(a) has the structure of formula (I), where R 17is a linear alkylene group having 1 to 6 carbon atoms or a branched alkylene group having 3 to 6 carbon atoms; X 1 -OR 20 is a group, where R 20 is an alkyl group of 1 to 4 carbon atoms, X 2 and X 3 is independent of X 1 or methyl, and a is 0.

[0163] In yet another embodiment, the mercaptosilane has the structure of formula (I), where R 17 are independently a linear alkylene group having 1 to 6 carbon atoms or a branched alkylene group having 3 to 6 carbon atoms; R 18 each of R is a linear alkylene group having 2 to 8 carbon atoms or a branched alkylene group having 3 to 8 carbon atoms; 19 each independently represents a linear alkylene group of 1 to 6 carbon atoms or a branched alkylene group of 3 to 6 carbon atoms; 1 and X 2 -OR 20 , where R 20 is an alkyl group of 1 to 4 carbon atoms, and X 1 and X 2 Two-OR 20 The groups are linked together via covalent bonds and attached to the same silicon atom -OR 20 -R 20 O-groups to form a ring structure containing 2 to 8 carbon atoms, 2 oxygen atoms and a silicon atom group, or X 1 and X 2 Each of -OR 21 is an OH group, where R 21 is a linear alkylene group having 2 to 8 carbon atoms or a branched alkylene group having 3 to 8 carbon atoms; X 3 and X 4 are independent -OR 20 Group, where R 20 is an alkyl group of 1 to 4 carbon atoms, -OR 21 OH group, where R 21 is a linear alkylene group of 2 to 8 carbon atoms or a branched alkylene group of 3 to 8 carbon atoms, where X 3 and X4 -OR 20 When , two -OR 20 The groups are covalently bonded together to the same silicon atom -OR 20 -R 20 O-groups may be formed, forming a ring structure containing 2 to 8 carbon atoms, two oxygen atoms and a silicon atom, where a is 1 to 8, preferably 1 to 3.

[0164] Representative, non-limiting examples of mercaptosilanes (iii)(a) include 3-mercapto-1-propyltriethoxysilane, 2-mercapto-1-ethyltriethoxysilane, mercaptomethyltriethoxysilane, 6-mercapto-1-hexyltriethoxysilane, 4-mercapto-1-butyltriethoxysilane, 1-mercapto-1-ethyltriethoxysilane, 3-mercapto-1-propylmethyldiethoxysilane, 3-mercapto-1-propyldimethylethoxysilane, 3-mercapto-1-propyldimethylethoxysilane, 3-mercapto-1-propyltri ... Pyrtrimethoxysilane, 2-mercapto-1-ethyltrimethoxysilane, mercaptomethyltrimethoxysilane, 6-mercapto-1-hexyltrimethoxysilane, 4-mercapto-1-butyltrimethoxysilane, 1-mercapto-1-ethyltrimethoxysilane, 3-mercapto-1-propylmethyldimethoxysilane, 3-mercapto-1-propyldimethylmethoxysilane, 3-mercapto-1-propyltripropoxysilane, 3-mercapto-1-propyltriisopropoxysilane, 3-mercapto-1-propyltriisopropoxysilane, mercapto-1-propyltributoxysilane; 4-(3,6,9,12,15-penta-oxaoctacosyloxy)-4-ethoxy-5,8,11,14,17,20-hexaocta-4-silatritriacontane-1-thiol; 3-(2-{3-[2-(3-mercapto-propyl)-5-methyl-[1,3,2]dioxasilinan-2-yloxy]-2-methyl-propoxy}-5-methyl-[1,3,2]dioxasilinan-2-yl)-propane-1-thiol; 3-(2-{3-[2-(3- mercapto-propyl)-4,4,6-trimethyl-[1,3,2]dioxasilinan-2-yloxy]-2-methyl-propoxy}-4,4,6-trimethyl-[1,3,2]dioxasilinan-2-yl)-propane-thiol;3-(2-{3-[2-(3-mercapto-propyl)-4,4,6-trimethyl-[1,3,2]dioxasilinan-2-yloxy]-1,1-dimethyl-butoxy}-4,4,6-trimethyl-[1,3,2]dioxasilinan-2-yl)-propane-1-thiol;3-({3-[2-mercaptopropyl)-5-methyl-[1,3,2]dioxasilinane-yloxy]-2-methyl-propoxy}-bis-[3-hydroxy-2-methyl-propoxy]-silanyl)-propane-1-thiol;3-[{3-[{3-bis-(3-hydroxy-2-methyl-propyl)-(3-mercaptopropyl)-silanyloxy]-1-methyl-propoxy}-(3-hydroxy-2-methyl-propoxy)-(3-mercaptopropyl)-silanyloxy]-1-methyl-propoxy}-(3-hydroxy-2-methyl-propoxy)-(3-mercaptopropyl)-silanyloxy] 3-[[3-((3-hydroxy-3-methyl-propoxy)-3-mercapto-propyl)-{3-[2-(3-mercapto-propyl)-5-methyl-[1,3,2]dioxasilinan-2-yloxy]-1-methyl-propoxy}-silanyloxy)-methyl-propoxy-(3-hydroxy-2-methyl-propoxy)-3-mercapto-propyl)-silanyl]-2-methylpropan-1-ol;3-(2-{3-[2-(3-mercaptopropyl)-5-methyl-[1,3,2]dioxasilinan-2-yloxy]-1-methyl-propoxy}-silanyloxy)-methyl-propoxy-(3-hydroxy-2-methyl-propoxy)-3-mercapto-propyl)-silanyl]-2-methylpropan-1-ol 3-({3-[2-mercapto-methyl)-5-methyl-[1,3,2]dioxasilinan-2-yloxy]-2-methyl-propoxy}-diethoxy]-silanyl)-methane-1-thiol;3-[{3-[{3-bis-(3-hydroxy-2,2-dimethyl-propyl)-(3-mercapto-propyl)-silanyloxy] -2,2-dimethyl-propoxy}-(3-hydroxy-2,2-dimethyl-propoxy)-(3-mercapto-propyl)-silanyloxy]-2,2-dimethyl-propan-1-ol; 3-[{3-[(methyl)-(3-hydroxy-2-methyl-propoxy)-(3-mercapto-propyl)-silanyloxy]-2-methyl-propoxy}-methyl)-(3-mercapto-propyl)-silanyloxy]-2-methyl-propan-1-ol, and combinations thereof.

[0165] In another embodiment, the blocked mercaptosilane (iii)(b) has the general formula (XI): [ka] During the ceremony R 17 independently a straight chain alkylene group of 1 to 6 carbon atoms or a branched chain alkylene group of 3 to 6 carbon atoms; R 18 each of which is a straight chain alkylene group of from 2 to 8 carbon atoms or a branched chain alkylene group of from 3 to 8 carbon atoms; R 19 each independently is a straight chain alkylene group of 1 to 6 carbon atoms or a branched chain alkylene group of 3 to 6 carbon atoms; X 1 -OR 20 Group, where R 20 is an alkyl group of 1 to 4 carbon atoms, -OR 21 OH group, where R 21 is a straight chain alkylene group having 2 to 8 carbon atoms or a branched chain alkylene group having 3 to 8 carbon atoms, or X 1 -OR 22 (OR 23 ) c OR 224 , where R 22 is a linear alkylene group having 2 to 6 carbon atoms or a branched alkylene group having 3 to 6 carbon atoms, preferably 3 carbon atoms; R 23 each independently represents an alkylene group of 2 to 4 carbon atoms, and R 24 is a linear alkyl group of 1 to 16 carbon atoms or a branched alkyl group of 3 to 16 carbon atoms, and c is an integer from 1 to 20; X 2 and X 3 is independent of X 1 or methyl; X 4 Each of X is independent. 1 or methyl; Y 1 Each of these is -C(=O)R 25 OR -C(=S)OR 25 , where R 25are independently a straight chain alkylene group of 1 to 16, more particularly 5 to 11, and even more particularly 6 to 9 carbon atoms, or a branched chain alkylene group of 3 to 16, more particularly 5 to 11, and even more particularly 6 to 9 carbon atoms; and a is an integer from 0 to 8, (i)X 1 and X 2 -OR 20 When , two -OR 20 are bonded together via covalent bonds to the same silicon atom -OR 20 -R 20 O-groups to form a ring structure containing 2 to 8 carbon atoms, 2 oxygen atoms, and a silicon atom; and (ii) a is 1 to 8 and X 3 and X 4 -OR 20 When , two -OR 20 The groups are linked together via covalent bonds and attached to the same silicon atom -OR 20 -R 20 The O-groups form a ring structure containing 2 to 8 carbon atoms, two oxygen atoms and a silicon atom.

[0166] In another embodiment, the blocked mercaptosilane (iii)(b) has the structure of formula (I), where R 17 is a linear alkylene group having 1 to 6 carbon atoms or a branched alkylene group having 3 to 6 carbon atoms; Y 1 is -C(=O)R 25 OR -C(=S)OR 25 , where each R 25 are independently a straight chain alkylene group of 1 to 16 carbon atoms, more particularly 5 to 11 carbon atoms, and even more particularly 6 to 9 carbon atoms, or a branched chain alkylene group of 3 to 16 carbon atoms, more particularly 5 to 11 carbon atoms, and even more particularly 6 to 9 carbon atoms; X 1 -OR 20 is a group, where R 20 is an alkyl group of 1 to 4 carbon atoms, X2 and X 3 is independent of X 1 Or methyl and a is 0.

[0167] In yet another embodiment, the blocked mercaptosilane (iii)(b) has the structure of formula (I), where R 17 are independently a linear alkylene group having 1 to 6 carbon atoms or a branched alkylene group having 3 to 6 carbon atoms; R 18 each of R is a linear alkylene group having 2 to 8 carbon atoms or a branched alkylene group having 3 to 8 carbon atoms; 19 each independently represents a linear alkylene group of 1 to 6 carbon atoms or a branched alkylene group of 3 to 6 carbon atoms; Y 1 is -C(=O)R 25 OR -C(=S)OR 25 , where each R 25 are independently a straight chain alkylene group of 1 to 16 carbon atoms, more particularly 5 to 11 carbon atoms, and even more particularly 6 to 9 carbon atoms, or a branched chain alkylene group of 3 to 16 carbon atoms, more particularly 5 to 11 carbon atoms, and even more particularly 6 to 9 carbon atoms; X 1 and X 2 -OR 20 , where R 20 is an alkyl group of 1 to 4 carbon atoms, and X 1 and X 2 Two-OR 20 The groups are linked together via covalent bonds and attached to the same silicon atom -OR 20 -R 20 O-groups to form a ring structure containing 2 to 8 carbon atoms, 2 oxygen atoms and a silicon atom group, or X 1 and X 2 Each of -OR 21 is an OH group, where R 21 is a linear alkylene group having 2 to 8 carbon atoms or a branched alkylene group having 3 to 8 carbon atoms; X 3 and X 4 are independent -OR 20 Group, where R 20is an alkyl group of 1 to 4 carbon atoms, -OR 21 OH group, where R 21 is a linear alkylene group of 2 to 8 carbon atoms or a branched alkylene group of 3 to 8 carbon atoms, where X 3 and X 4 -OR 20 When , two -OR 20 The groups are covalently bonded together to the same silicon atom -OR 20 -R 20 O-groups may be formed, forming a ring structure containing 2 to 8 carbon atoms, two oxygen atoms and a silicon atom, where a is 1 to 8, preferably 1 to 3.

[0168] Representative, non-limiting examples of blocked mercaptosilanes (iii)(b) include triethoxysilylmethyl thioformate, 2-triethoxysilylethyl thioacetate, 3-triethoxysilylpropyl thiopropanoate, 3-triethoxysilylpropyl thiohexanoate, 3-triethoxysilylpropyl thio-(2-ethyl)-hexanoate, 3-triethoxysilylpropyl thiooctanoate, 3-diethoxymethylsilylpropyl thiooctanoate, 3-ethoxydimethylsilylpropyl thiooctanoate, 3-ethoxydimethylsilylpropyl thiooctanoate, 3-tri ... Silylpropylthiooctanoate, 3-triethoxysilylpropylthiododecanoate, 3-triethoxysilylpropylthiooctadecanoate, 3-trimethoxysilylpropylthiooctanoate, 3-triacetoxysilylpropylthioacetate, 3-dipropoxymethylsilylpropylthiopropanoate, 4-oxa-hexyloxydimethylsilylpropylthiooctanoate, 3-(2-{3-[2-(4-thia-5-oxo-dodecyl)-5-methyl-[1,3,2] 3-(2-{3-[2-(4-thia-5-oxo-dodecyl)-4,4,6-trimethyl-[1,3,2]dioxasilinan-2-yloxy]-2-methyl-propoxy}-4,4,6-trimethyl-[1,3,2]dioxasilinan-2-yl)-4-thia-5-oxo-dodecane;3-(2-{3-[2-(4-thia-5-oxo-dodecyl)-4,4,6-trimethyl-[1,3,2]dioxasilinan-2-yloxy]-2-methyl-propoxy}-4,4,6-trimethyl-[1,3,2]dioxasilinan-2-yl)-4-thia-5-oxo-dodecane oxo-dodecyl)-4,4,6-trimethyl-[1,3,2]dioxasilinan-2-yloxy]-1,1-dimethyl-butoxy}-4,4,6-trimethyl-[1,3,2]dioxasilinan-2-yl)-4-thia-5-oxo-dodecane;3-({3-[2-thia-3-oxo-decyl)-5-methyl-[1,3,2]dioxasilinan-yloxy]-2-methyl-propoxy}-bis-[3-hydroxy-2-methyl-propoxy]-silanyl)-2-thia-3-oxo-decane;3-[{3-[{3-bis-(3-hydroxy-2-methyl-propyl)-(4-thia-5-oxo-dodecyl)-silanyloxy]-1-methyl-propoxy}-(3-hydroxy-2-methyl-propoxy)-(4-thia-5-oxo-dodecyl)-silanyloxy]-2-methyl-propan-1-ol;3-[[3-((3-hydroxy-3-methyl-propoxy)-4-thia-5-oxo-dodecyl)-{3-[2-(4-thia-5-oxo-dodecyl) -5-Methyl-[1,3,2]dioxasilinan-2-yloxy]-1-methyl-propoxy}-silanyloxy)-2-methyl-propoxy-(3-hydroxy-2-methyl-propoxy)-4-thia-5-oxo-dodecyl)-silanyl]-2-methylpropan-1-ol;3-(2-{3-[2-(4-thia-5-oxo-6-ethyl-decyl)-[1,3,2]dioxasilinan-2-yloxy]-propoxy}-[1,3,2]dioxasilinan- 2-yl)-4-thia-5-oxo-6-ethyl-decane;3-({3-[2-thia-3-oxo-octyl)-5-methyl-[1,3,2]dioxasilinan-2-yloxy]-2-methyl-propoxy}-diethoxy]-silanyl)-2-thia-3-oxo-octane;3-[{3-[{3-bis-(3-hydroxy-2,2-dimethyl-propyl)-(4-thia-5-oxo-dodecyl)-silanyloxy]-2,2-dimethyl-propoxy}-(3-hydroxy hydroxy-2,2-dimethyl-propoxy)-(4-thia-5-oxo-dodecyl)-silanyloxy]-2,2-dimethyl-propan-1-ol; 3-[{3-[(methyl)-(3-hydroxy-2-methyl-propoxy)-(4-thia-5-oxo-dodecyl)-silanyloxy]-2-methyl-propoxy}-methyl)-(4-thia-5-oxo-dodecyl)-silanyloxy]-2-methyl-propan-1-ol, and combinations thereof.

[0169] In some embodiments, the blocked mercaptosilane in the composition of the present disclosure is a bifunctional silane having a blocked thiol functionality and an alkoxysilane functionality. In some embodiments, the blocked mercaptosilane is octanoylthio-1-propyltriethoxysilane.

[0170] In some embodiments, the mercaptosilane in the process of the present disclosure is a bifunctional silane having a blocked thiol functionality and an alkoxysilane functionality. In some embodiments, the mercaptosilane is mercaptopropyltriethoxysilane. In some embodiments, the mercaptosilane is 4-(3,6,9,12,15-penta-oxaoctacosyloxy)-4-ethoxy-5,8,11,14,17,20-hexaoxa-4-silatritriacontane-1-thiol.

[0171] In some embodiments, the weight ratio of the blocked mercaptosilane to the mercaptosilane in the process of the present disclosure is from about 75 to about 25. In some embodiments, the weight ratio of the blocked mercaptosilane to the mercaptosilane is from about 4.8 to about 1.6, from about 7 to about 0.35, from about 6.25 to about 0.7, from about 5.75 to about 1, from about 5.2 to about 1.3, from about 4.4 to about 1.9, or from about 3.6 to about 2.4. In some embodiments, the weight ratio of the blocked mercaptosilane to the mercaptosilane is about 3. In some embodiments, the weight ratio of the blocked mercaptosilane to the mercaptosilane is from about 2.85 to about 3.15.

[0172] Blocked mercaptosilanes are coupling agents for vulcanizable organic polymer(s), such as diene-based polymers (i)(a) containing at least one functional group and diene-based polymers (i)(b) not containing functional groups, and silane-reactive particulate filler(s), such as precipitated silica (ii). A mixture of mercaptosilane (iii)(a) and blocked mercaptosilane (iii)(b) is unique in that it takes advantage of the high performance of the mercapto group without the deleterious side effects typically associated with the use of mercaptosilanes, such as high processing viscosity, less than desirable filler dispersion, and premature curing (scorch). These advantages are achieved by initially providing a concentration of mercaptan groups below the amount required to cause undesirable effects. Blocked mercaptosilane (iii)(b) is not available to react with the rubber component(s) as a result of its blocking group. Generally, during the first stage of the compounding process, the silane-SiX 1 X 2 X 3 Only reaction of the groups with the silane-reactive filler can occur. Thus, substantial coupling of the filler to the polymer during mixing is prevented, thereby minimizing undesirable premature curing (scorch) and the associated undesirable increase in viscosity. As a result of preventing, inhibiting, or minimizing premature curing, better performance of the cured filled rubber, such as a balance of handling, rolling resistance, and grip, can be achieved.

[0173] The blocked mercaptosilane (iii)(b) is capable of reacting with the silica surface during mixing, but remains partially or completely blocked during the non-productive mixing stage, thereby preventing reaction with the diene polymer. The diene polymer reacts with the thiol group of the blocked mercaptosilane (iii)(b) only after the blocking group is removed. Removal of the blocking group is accomplished when the blocked mercaptosilane reacts with a nucleophile to form a thiol group.

[0174] In some embodiments, at least one coupling agent package (iii) is used in an amount of from about 0.5 to about 20 parts by weight of coupling agent package per 100 parts by weight of rubber, more specifically from about 1 to about 10 parts by weight of coupling agent package (iii) per 100 parts by weight of rubber, and even more specifically from about 3 to about 8 parts by weight of coupling agent package (iii) per 100 parts by weight of rubber.

[0175] In some embodiments, the weight ratio of the blocked mercapto-functional alkylalkoxysilane (iii)(b) to the mercapto-functional alkylalkoxysilane (iii)(a) in the rubber compositions disclosed herein is from about 0.25:1 to about 50:1. In some embodiments, the weight ratio of the blocked mercapto-functional alkylalkoxysilane (iii)(b) to the mercapto-functional alkylalkoxysilane (iii)(a) in the rubber compositions disclosed herein is from about 0.5:1 to about 20:1. In some embodiments, the weight ratio of the blocked mercapto-functional alkylalkoxysilane (iii)(b) to the mercapto-functional alkylalkoxysilane (iii)(a) in the rubber compositions disclosed herein is from about 1:1 to about 10:1.

[0176] In some embodiments, the weight ratio of blocked mercaptosilane to mercaptosilane in the rubber compositions disclosed herein is from about 0.25:1 to about 50:1.

[0177] In some embodiments, the mercapto-functional alkylalkoxysilane (iii)(a) can be used in an amount ranging from about 0.1 to about 10 parts by weight of mercapto-functional alkylalkoxysilane (iii)(a) per 100 parts by weight of rubber, more specifically in an amount ranging from 0.5 to about 5 parts by weight of mercapto-functional alkylalkoxysilane (iii)(a) per 100 parts by weight of rubber, and even more specifically in an amount ranging from 1 to 3 parts by weight of mercapto-functional alkylalkoxysilane (iii)(a) per 100 parts by weight of rubber. In some embodiments, the blocked mercapto-functional alkylalkoxysilane (iii)(b) can be used in an amount ranging from about 0.1 to about 15 parts by weight of the mercapto-functional alkylalkoxysilane (iii)(b) per 100 parts by weight of rubber, more specifically in an amount ranging from about 1 to about 10 parts by weight of the blocked mercapto-functional alkylalkoxysilane (iii)(b) per 100 parts by weight of rubber, and even more specifically in an amount ranging from 3 to 8 parts by weight of the blocked mercapto-functional alkylalkoxysilane (iii)(b) per 100 parts by weight of rubber.

[0178] In some embodiments, the compositions of the present disclosure comprise from about 0.01% to about 10%, about 0.05% to about 10%, about 0.1% to about 10%, about 0.5% to about 10%, about 1% to about 10%, about 2% to about 10%, about 5% to about 10%, about 7% to about 10%, about 0.01% to about 7%, about 0.05% to about 7%, about 0.1% to about 7%, about 0.5% to about 7%, about 1% to about 7%, about 2% to about 7%, about 5% to about 7%, about 0.01% to about 5%, about 0.05% to about from about 5%, from about 0.1% to about 5%, from about 0.5% to about 5%, from about 1% to about 5%, from about 2% to about 5%, from about 0.01% to about 2%, from about 0.05% to about 2%, from about 0.1% to about 2%, from about 0.5% to about 2%, from about 1% to about 2%, from about 0.01% to about 1%, from about 0.05% to about 1%, from about 0.1% to about 1%, from about 0.5% to about 1%, from about 0.01% to about 0.5%, from about 0.05% to about 0.5%, or from about 0.1% to about 0.5% mercaptosilane. Deblocking Agent (iv)

[0179] When it is desired to react a coupling agent package comprising a mixture of mercaptosilane (iii)(a) and blocked mercaptosilane (iii)(b) to bond the precipitated silica (ii) and other silane-reactive filler(s) to the diene-based polymer(s) (i)(a) and (i)(b), at least one deblocking agent (iv) is also present in the rubber composition.

[0180] The deblocking agent(s) (iv) may be present in an amount ranging from about 0.05 to about 20 phr, more particularly from about 0.1 to about 5 phr, and most particularly from about 0.5 to about 3 phr. If alcohol or water is present in the mixture (as is usually the case), a catalyst (e.g., a tertiary amine, Lewis acid, or thiol) may be used to initiate and promote the release of the blocking group by hydrolysis or alcoholysis, thus liberating the corresponding active mercaptosilane. Alternatively, the deblocking agent (iv) may be a nucleophile containing a sufficiently labile hydrogen atom that is transferred to the position of the original blocking group to provide the corresponding active mercaptosilane. Thus, in the presence of a blocking group acceptor molecule, exchange of hydrogen from the nucleophile with the blocking group of the blocked mercaptosilane occurs to form a mercaptosilane and the corresponding nucleophile derivative containing the original blocking group. This transfer of the blocking group from the mercaptosilane to the nucleophile can be driven, for example, by the greater thermodynamic stability of the product (mercaptosilane and blocking group-containing nucleophile) relative to the initial reactants (blocked mercaptosilane and nucleophile). For example, when the nucleophile is an amine containing an N-H bond, the transfer of the blocking group from the blocked mercaptosilane (ii)(b) results in the mercaptosilane and an amide corresponding to the acyl group or a thiocarbamate corresponding to the xanthate group.

[0181] What is important about the blocking groups initially present in the blocked mercaptosilane (iii)(b), and the deblocking agent (iv) employed, is that the initially substantially inactive (in terms of bonding to the organic polymer) blocked mercaptosilane (iii)(b) is substantially converted to an active mercaptosilane at the desired point in the rubber compounding procedure. It is noted that a partial amount (i.e., a stoichiometric deficiency) of nucleophile may be used if it is to deblock only a portion of the blocked mercaptosilane (iii)(b) to control the degree of vulcanization of a particular formulation.

[0182] Water can be a deblocking agent and is typically present on the filler as water of hydration or bonded to the filler in the form of hydroxyl groups.

[0183] The deblocking agent (iv) can be added to the cure package or, alternatively, can be added as the sole component at any other stage of the compounding process. The deblocking agent (iv) can be the sole agent or can be generated in situ as a by-product of the reaction.

[0184] In one embodiment, the deblocking agent (iv) has the formula (XII): R 26 [A 3 -H] d (XII) During the ceremony: R 26 is a monovalent or polyvalent organic radical containing 1 to 30 carbon atoms or hydrogen, A 3 Each of the is independently an oxygen, a sulfur, or a -NR 27 Group, where each R 27 are independently a monovalent or polyvalent organic radical containing 1 to 30 carbon atoms or hydrogen; and d is an integer from 1 to 100, preferably from 1 to 3.

[0185] More specifically, R 26each of which is a radical derived by removing one or more hydrogen atoms from a hydrocarbon containing from 1 to 30 carbon atoms, optionally containing at least one heteroatom selected from the group consisting of oxygen, nitrogen, sulfur, and phosphorus; and R 26 each of A is an alkyl or aryl group (when d is 1), an alkylene or arylene group (when d is 2), or a -C(=NH)- group (when d is 2); 3 -NR 27 - where R 27 is phenyl or an alkyl group of 1 to 10 carbon atoms, e.g., diphenylguanidine.

[0186] Examples of deblocking agents (iv) according to the above formula include water or monohydric alcohols or glycols or polyols, any primary or secondary amines or amines containing a C=N double bond such as imines or guanidines, provided that such amines contain at least one NH (nitrogen-hydrogen) bond. Specific examples of many such guanidines, amines, and imines as rubber components are well known in the art and are disclosed, for example, in J. Van Alphen's Rubber Chemistry (TNO, Plastics and Rubber Research Association, Delft, The Netherlands, 1973), which is incorporated herein by reference to the extent that it does not conflict with this disclosure. Some examples include N,N'-diphenylguanidine, N,N',N''-triphenylguanidine, N,N'-di-ortho-tolylguanidine, orthobiguanide, hexamethylenetetramine, cyclohexylethylamine, dibutylamine, and 4,4'-diaminodiphenylmethane.

[0187] Any of the common acid catalysts used in the transesterification of esters can be used as the catalyst, such as Bronsted or Lewis acids.

[0188] The blocking groups of the blocked mercaptosilanes can be removed during the elevated temperature cure of the rubber after the vulcanization chemicals have been added at low temperature.

[0189] In some embodiments, the compositions of the present disclosure comprise about 0.01% to about 10%, about 0.05% to about 10%, about 0.1% to about 10%, about 0.5% to about 10%, about 1% to about 10%, about 2% to about 10%, about 5% to about 10%, about 7% to about 10%, about 0.01% to about 7%, about 0.05% to about 7%, about 0.1% to about 7%, about 0.5% to about 7%, about 1% to about 7%, about 2% to about 7%, about 5% to about 7%, about 0.01% to about 5%, about 0.05% to about 5%, about 0.1% to about 5%, about 0.5% to about 5%, about 1% to about 5%, about 2% to about 5%, about 0.01% to about 2%, about 0.05% to about 2%, about 0.1% to about 2%, about 0.5% to about 2%, about 1% to about 2%, about 0.01% to about 1%, about 0.05% to about 1%, about 0.1% to about 1%, about 0.5% to about 1%, about 0.01% to about 0.5%, about 0.05% to about 0.5%, or about 0.1% to about 0.5% of the blocked mercaptosilane. Vulcanization Package(v)

[0190] The vulcanization of the vulcanizable component(s) present in the rubber composition of the present application can be carried out in the presence of one or more sulfur-containing vulcanizing agents, examples of which include elemental sulfur (free sulfur) or sulfur-donor vulcanizing agents, such as polysulfide polymers and sulfur olefin adducts. Other useful sulfur donors include, for example, morpholine derivatives. Representative examples of such donors include, for example, but are not limited to, dimorpholine disulfide, dimorpholine tetrasulfide, benzothiazyl-2,N-dithiomorpholide, thioplasts, and disulfide caprolactam.

[0191] The selected vulcanizing agent(s) are conventionally added to the final mix or at the productive rubber composition mix stage. Vulcanizing agents may be added at the productive mix stage in amounts ranging from about 0.1 to about 6 phr, with a range of about 0.5 to about 5 phr being preferred, and in some cases about 1.0 to about 3.0 phr being preferred.

[0192] The vulcanization of the vulcanizable component(s) present in the rubber composition of the present application can also be carried out in the presence of one or more vulcanization accelerators, which are compounds that increase the rate of vulcanization, allowing the vulcanization to proceed at low temperatures and with high efficiency.

[0193] Representative non-limiting examples include benzothiazoles, guanidine derivatives, and thiocarbamates. Specific accelerators of these and other types include, but are not limited to, mercaptobenzothiazole, benzothiazole disulfide, diphenylguanidine, zinc dithiocarbamate, alkylphenol disulfide, zinc butyl xanthate, N-dicyclohexyl-2-benzothiazole sulfenamide, N-cyclohexyl-2-benzothiazole sulfenamide, N-oxydiethylenebenzothiazole-2-sulfenamide, N,N-diphenylthiourea, dithiocarbamylsulfenamide, N,N-diisopropylbenzothiazole-2-sulfenamide, zinc-2-mercapto toluimidazole, dithiobis(N-methylpiperazine), dithiobis(N-beta-hydroxyethylpiperazine), and dithiobis(dibenzylamine).

[0194] Accelerators may be used to control the time and / or temperature required for vulcanization and to improve the properties of the vulcanizate. In one embodiment, a single accelerator system, i.e., a primary accelerator, may be used. Traditionally and preferably, a primary accelerator(s) is used in a total amount ranging from about 0.5 to about 4 phr, preferably from about 0.8 to about 1.5 phr. A combination of a primary accelerator and a secondary accelerator may also be used, where the secondary accelerator is used in a smaller amount (e.g., ranging from about 0.05 to about 3 phr) to activate the vulcanizate and improve its properties. Delayed action accelerators and / or vulcanization retarders may also be used. Suitable types of accelerators include amines, disulfides, guanidines, thioureas, thiazoles, sulfenamides, dithiocarbamates, and xanthates. Preferably, the primary accelerator is a sulfenamide. If a secondary accelerator is used, the secondary accelerator is preferably a guanidine or dithiocarbamate compound.

[0195] In certain embodiments, a vulcanization accelerator is used alone. In certain embodiments, two or more vulcanization accelerators are used in combination. Representative non-limiting examples of guanidine vulcanization accelerators include 1,3-diphenylguanidine, 1,3-di-ortho-tolylguanidine, 1-ortho-tolylbiguanide, di-ortho-tolylguanidine salt of dicatechol borate, 1,3-di-ortho-cumenylguanidine, 1,3-di-ortho-biphenylguanidine, and 1,3-di-ortho-cumenyl-2-propionylguanidine. In some embodiments, the vulcanization package in the composition of the present disclosure includes sulfur and a sulfenamide primary accelerator. This accelerator may also be -A. 3 When it has an H group, it can also function as a deblocking agent (iv) in the same manner as in the case of diphenylguanidine. Scorch Modifiers (vi)

[0196] The rubber composition may include a scorch modifier (vi). In certain embodiments, the scorch modifier is a thiuram disulfide scorch modifier. In some embodiments, the scorch modifier has the general formula (XIII): R 28 2NC(=S)SSC(=S)NR 28 2(XIII) R in the formula 28 are independently a straight chain alkyl group of 1 to 12 carbon atoms, a branched chain alkyl group of 3 to 12 carbon atoms, a cycloalkyl group of 5 to 12 carbon atoms, an aryl group of 6 to 12 carbon atoms, or an aralkyl group of 7 to 12 carbon atoms.

[0197] Representative non-limiting examples of scorch modifiers include tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrapropylthiuram disulfide, tetrabutylthiuram disulfide, tetraphenylthiuram disulfide, tetramethylthiuram monosulfide, zinc dibenzyldithiocarbamate, and tetrabenzylthiuram disulfide.

[0198] The scorch modifier (vi) can be used in an amount ranging from about 0.05 to about 10 parts by weight of scorch modifier (vi) per hundred parts of rubber (phr), more specifically from about 0.1 to about 5 parts by weight of scorch modifier (vi) per hundred parts of rubber (phr), and in some cases from about 0.15 to about 1.0 parts by weight of scorch modifier (vi) per hundred parts of rubber (phr) is preferred.

[0199] In some embodiments, the compositions of the present disclosure comprise about 0.01% to about 10%, about 0.05% to about 10%, about 0.1% to about 10%, about 0.5% to about 10%, about 2% to about 10%, about 5% to about 10%, about 7% to about 10%, about 0.01% to about 7%, about 0.05% to about 7%, about 0.1% to about 7%, about 0.5% to about 7%, about 2% to about 7% by weight. , about 5% to about 7%, about 0.01% to about 5%, about 0.05% to about 5%, about 0.1% to about 5%, about 0.5% to about 5%, about 2% to about 5%, about 0.01% to about 2%, about 0.05% to about 2%, about 0.1% to about 2%, about 0.5% to about 2%, about 0.01% to about 0.5%, or about 0.01% to about 0.05% of a scorch modifier. Other Ingredients

[0200] When tackifying resins are used, typical amounts are from about 0.1 to about 15 parts by weight of tackifying resin per hundred parts by weight of rubber (phr), and more particularly from about 0.5 to about 10 parts by weight of tackifying resin per hundred parts by weight of rubber (phr), usually from about 1 to about 5 parts by weight of tackifying resin per hundred parts by weight of rubber (phr). Such tackifying resins include rosin and its derivatives, terpenes and modified terpenes, aliphatic, cycloaliphatic, and aromatic resins, hydrogenated hydrocarbon resins, and mixtures thereof, terpene-phenolic resins, and novolacs. Typical amounts of processing aids are from about 1 to about 50 parts by weight of processing aid per hundred parts by weight of rubber (phr). Such processing aids include, for example, aromatic, naphthenic, and / or paraffinic processing oils. Typical amounts of antioxidants are from about 1 to about 5 parts by weight of antioxidant per hundred parts by weight of rubber (phr). Representative antioxidants may be, for example, diphenyl-p-phenylenediamine and others disclosed in the Vanderbilt Rubber Handbook (1978) at pp. 344-46, which is incorporated herein by reference in its entirety. A typical amount of antiozonant is about 1 to about 5 parts by weight antiozonant per 100 parts by weight rubber (phr). A typical amount of fatty acid, which may include stearic acid, if used, is about 0.5 to about 3 parts by weight fatty acid per 100 parts by weight rubber (phr). A typical amount of zinc oxide is about 2 to about 5 parts by weight zinc oxide per 100 parts by weight rubber (phr). A typical amount of wax is about 1 to about 5 parts by weight wax per 100 parts by weight rubber (phr). Often microcrystalline waxes are used. A typical amount of peptizer is about 0.1 to about 1 part by weight peptizer per 100 parts by weight rubber (phr). Typical peptizers are, for example, pentachlorothiophenol and dibenzamidodiphenyl disulfide.

[0201] The addition of an alkylsilane to the coupling agent package, typically in the range of 1 / 50 to 1 / 2 molar ratio of alkylsilane to the total amount of blocked mercaptosilane (iii)(b), facilitates better control of the processing and aging of the rubber composition.

[0202] In another embodiment, the present disclosure provides: about 30% to about 40% by weight of at least one diene-based polymer containing at least one functional group; about 30% to about 40% by weight of precipitated silica; about 0.05% to about 5% by weight of a blocked mercapto-functional alkylalkoxysilane; about 0.05% to about 5% by weight of a mercapto-functional alkylalkoxysilane, and Compositions containing from about 0.1% to about 10% by weight of the scorch modifier are directed.

[0203] In some embodiments, the composition further comprises a vulcanizing agent, which comprises at least one vulcanizing agent and at least one accelerator comprising sulfur. Any vulcanizing agent and vulcanization accelerator may be used, including those commonly used in the tire industry. Examples of vulcanization accelerators include, but are not limited to, guanidine, sulfonamide, thiazole, thiuram, dithiocarbamate, thiourea, and xanthate. In certain embodiments, a vulcanization accelerator is used alone. In certain embodiments, two or more vulcanization accelerators are used in combination. Examples of guanidine vulcanization accelerators include 1,3-diphenylguanidine, 1,3-di-ortho-tolylguanidine, 1-ortho-tolylbiguanide, di-ortho-tolylguanidine salt of dicatechol borate, 1,3-di-ortho-cumenylguanidine, 1,3-di-ortho-biphenylguanidine, and 1,3-di-ortho-cumenyl-2-propionylguanidine. In some embodiments, the sulfur in the vulcanization agent is selected from the group consisting of elemental sulfur, sulfur donor compounds, and combinations thereof. In some embodiments, the composition also includes sulfur and a sulfenamide primary accelerator.

[0204] A single performance index value (or performance index, or "PIV") represents the benefit of a composition by averaging together several properties of the rubber compound, which represent various important aspects in the tire and rubber industry. The main reason that PIV is important is that the performance of rubber compounds is interdependent; that is, the performance of many rubber compounds can only be improved by negatively affecting another property of the rubber compound. As an example, for bifunctional silanes, there is a known trade-off in which the improvement of rolling resistance properties comes at the expense of the processing properties of the rubber. Thus, the improved balance of several performance properties for a composition, as represented by a performance index value, illustrates the inventive nature of the composition.

[0205] Figure of merit value or performance index or PIV are used interchangeably throughout this disclosure.

[0206] Table 1 shows the performance items that make up the performance index value. [Table 1]

[0207] A performance index, or multiple performance indices, can be used to evaluate rubber compositions. For example, U.S. Patent No. 10,494,510 discloses such values ​​for evaluating rubber compositions, including rolling resistance and grip performance among the multiple performance indices.

[0208] In some embodiments, the rubber composition may have a Mooney viscosity of about 40 MU to about 150 MU, as measured using the ASTM D-1646 method. In further embodiments, the rubber composition may have a Mooney viscosity of about 120 MU to about 140 MU. In another embodiment, the rubber composition may have a Mooney viscosity of about 40 MU to about 100 MU. In some embodiments, the rubber composition may have a Mooney viscosity of about 40, about 45, about 50, about 55, about 60, about 65, about 70, about 75, about 80, about 85, about 90, about 95, about 100, about 105, about 110, about 115, about 120, about 125, about 130, about 135, about 140, about 145, or about 150 MU.

[0209] In some embodiments, the rubber composition may have a Mooney scorch of about 2 minutes to about 40 minutes at 3 points up as measured using ASTM D-1646 method. In further embodiments, the rubber composition may have a Mooney scorch of about 30 minutes to about 40 minutes at 3 points up. In another embodiment, the rubber composition may have a Mooney scorch of about 20 minutes to about 30 minutes at 3 points up. In some embodiments, the rubber composition may have a Mooney scorch of about 2, about 5, about 10, about 15, about 20, about 25, about 30, about 35, or about 40 at 3 points up.

[0210] In some embodiments, the rubber composition may have a tensile strength of about 5 MPa to about 25 MPa as measured by ASTM D-412 method. In further embodiments, the rubber composition may have a tensile strength of about 15 MPa to about 20 MPa. In other embodiments, the rubber composition may have a tensile strength of about 10 MPa to about 15 MPa. In some embodiments, the rubber composition may have a tensile strength of about 5, about 10, about 15, about 20, or about 25 MPa.

[0211] In some embodiments, the rubber composition may have a Shore A hardness of about 50 to about 80 Shore A as measured using ASTM D-2240 method. In a further embodiment, the rubber composition may have a Shore A hardness of about 55 to about 65 Shore A. In another embodiment, the rubber composition may have a Shore A hardness of about 65 to about 75 Shore A. In some embodiments, the rubber composition may have a Shore A hardness of about 50, about 55, about 60, about 65, about 70, about 75, or about 80 Shore A.

[0212] In some embodiments, the rubber composition may have a rebound resilience at 0° C. of about 5 to about 20 as measured using ASTM D-7121. In further embodiments, the rubber composition may have a rebound resilience at 0° C. of about 5 to about 10. In other embodiments, the rubber composition may have a rebound resilience at 0° C. of about 10 to about 15. In some embodiments, the rubber composition may have a rebound resilience at 0° C. of about 5, about 10, about 15, or about 20.

[0213] In some embodiments, the rubber composition may have a DMA (dynamic mechanical analysis) TS (temperature sweep) tan δ max of about 0.50 to about 1.00 as measured by using ASTM D6049 03 (2017). In further embodiments, the rubber composition may have a DMA TS tan δ max of about 0.50 to about 0.75. In another embodiment, the rubber composition may have a DMA TS tan δ max of about 0.75 to about 1.00. In some embodiments, the rubber composition may have a DMA TS tan δ max of about 0.50, about 0.55, about 0.60, about 0.65, about 0.70, about 0.75, about 0.80, about 0.85, about 0.90, about 0.95, or about 1.00.

[0214] In some embodiments, the rubber composition may have an RPA (rubber processability measurement) SS (strain sweep) tan delta max at 60°C of about 0.05 to about 0.20 as measured by using ASTM D-6601. In further embodiments, the rubber composition may have an RPA SS 60°C tan delta max of about 0.05 to about 0.10. In another embodiment, the rubber composition may have an RPA SS 60°C tan delta max of about 0.10 to about 0.20. In some embodiments, the rubber composition may have an RPA SS 60°C tan delta max of about 0.05, about 0.06, about 0.07, about 0.08, about 0.09, about 0.10, about 0.11, about 0.12, about 0.13, about 0.14, about 0.15, about 0.16, about 0.17, about 0.18, about 0.19, or about 0.20.

[0215] In some embodiments, the rubber composition may have a DMA TS tan δ at 60° C. of about 0.05 to about 0.20 as measured by using ASTM D6049 03(2017). In further embodiments, the rubber composition may have a DMA TS 60° C. tan δ of about 0.05 to about 0.10. In another embodiment, the rubber composition may have a DMA TS 60° C. tan δ of about 0.10 to about 0.20. In some embodiments, the rubber composition may have a DMA TS 60° C. tan δ of about 0.05, about 0.06, about 0.07, about 0.08, about 0.09, about 0.10, about 0.11, about 0.12, about 0.13, about 0.14, about 0.15, about 0.16, about 0.17, about 0.18, about 0.19, or about 0.20.

[0216] In some embodiments, the rubber composition has a DIN abrasion of about 70 mm as measured using ASTM D-5963. 3 From about 130 mm 3 In a further embodiment, the rubber composition has a DIN abrasion of about 80 mm 3 From about 100 mm 3 In another embodiment, the rubber composition may have a DIN abrasion of about 100 mm 3 From about 120 mm 3In some embodiments, the rubber composition may have a DIN abrasion of about 70 mm 3 , about 75mm 3 , about 80mm 3 , about 85mm 3 , about 90mm 3 , about 95mm 3 , about 100 mm 3 , about 105mm 3 , about 110mm 3 , about 115mm 3 , about 120mm 3 , about 125mm 3 , or about 130 mm 3 It may be. Process for preparing rubber composition

[0217] In some embodiments, the present disclosure provides a rubber composition comprising a composition comprising at least one diene-based polymer (i), silica (ii), a coupling agent package comprising mercaptosilane (iii)(a) and blocked mercaptosilane (iii)(b), at least one deblocking agent (iv), a vulcanization package comprising accelerator and sulfur (v), and a scorch modifier (vi). The rubber composition may be prepared by known methods, such as by mixing the ingredients using a rubber mixer, such as an open roll mill or a Banbury mixer, and vulcanizing the mixture. The rubber composition of the present disclosure may be used for various tire components, and is particularly suitable for example for treads and sidewalls.

[0218] The tire formed from the rubber composition can be manufactured by a conventional method using the rubber composition. Specifically, the unvulcanized rubber composition containing various required additives is extruded into the shape of a tire component, such as a tread, and then assembled with other tire components in a conventional manner in a tire manufacturing machine to build an unvulcanized tire. The unvulcanized tire is heat pressed in a vulcanizing machine to manufacture a tire. In some embodiments, a pneumatic tire or a non-pneumatic tire can be manufactured from the rubber composition. Such pneumatic tires can be used, for example, for passenger cars, trucks and buses, or motorcycles, or high-performance tires. As used herein, high-performance tires refer in particular to tires with excellent grip performance, including racing tires for automobile racing. They have excellent performance on ice, and are therefore suitable as studless tires for winter use.

[0219] The process of the present disclosure comprises adding silica (ii), mercaptosilane (iii)(a), and blocked mercaptosilane (iii)(b) to at least one diene-based polymer (i), where the diene-based polymer (i) comprises at least one diene-based polymer (i)(a) that contains at least one functional group and / or at least one diene-based polymer (i)(b) that does not contain a functional group, to prepare a composition.

[0220] In some embodiments, the weight ratio of the blocked mercaptosilane to the mercaptosilane is greater than 1. In some embodiments, the weight ratio of the blocked mercaptosilane to the mercaptosilane in the compositions of the present disclosure is about 1, about 2, about 3, about 4, about 5, about 6, about 7, about 8, about 9, about 10, about 11, about 12, about 15, about 20, about 25, or about 30. In some embodiments, the weight ratio of blocked mercaptosilane to mercaptosilane in the compositions of the present disclosure is from about 10 to about 1, from about 10 to about 2, from about 10 to about 3, from about 10 to about 4, from about 10 to about 5, from about 10 to about 6, from about 10 to about 7, from about 10 to about 8, from about 10 to about 9, from about 9 to about 1, from about 9 to about 2, from about 9 to about 3, from about 9 to about 4, from about 9 to about 5, from about 9 to about 6, from about 9 to about 7, from about 9 to about 8, from about 8 to about 1, from about 8 to about 1, or from about 8 to about 2. about 2, about 8 to about 3, about 8 to about 4, about 8 to about 5, about 8 to about 6, about 8 to about 7, about 7 to about 1, about 7 to about 2, about 7 to about 3, about 7 to about 4, about 7 to about 5, about 7 to about 6, about 6 to about 1, about 6 to about 2, about 6 to about 3, about 6 to about 4, about 6 to about 5, about 5 to about 1, about 5 to about 2, about 5 to about 3, about 5 to about 4, about 4 to about 1, about 4 to about 2, about to about 3, about 3 to about 1, about 3 to about 2, or about 2 to about 1.

[0221] In some embodiments, at least one coupling agent package (iii) is used in an amount of from about 0.5 to about 20 parts by weight of coupling agent package per 100 parts by weight of rubber, more specifically from about 1 to about 10 parts by weight of coupling agent package (iii) per 100 parts by weight of rubber, and even more specifically from about 3 to about 8 parts by weight of coupling agent package (iii) per 100 parts by weight of rubber.

[0222] In some embodiments, the weight ratio of the blocked mercapto-functional alkylalkoxysilane (iii)(b) to the mercapto-functional alkylalkoxysilane (iii)(a) in the rubber compositions disclosed herein is from about 0.25:1 to about 50:1. In some embodiments, the weight ratio of the blocked mercapto-functional alkylalkoxysilane (iii)(b) to the mercapto-functional alkylalkoxysilane (iii)(a) in the rubber compositions disclosed herein is from about 0.5:1 to about 20:1. In some embodiments, the weight ratio of the blocked mercapto-functional alkylalkoxysilane (iii)(b) to the mercapto-functional alkylalkoxysilane (iii)(a) in the rubber compositions disclosed herein is from about 1:1 to about 10:1.

[0223] In some embodiments, the weight ratio of blocked mercaptosilane to mercaptosilane in the rubber compositions of the present disclosure is from about 0.25:1 to about 50:1.

[0224] In some embodiments, the mercapto-functional alkylalkoxysilane (iii)(a) can be used in an amount ranging from about 0.1 to about 10 parts by weight of mercapto-functional alkylalkoxysilane (iii)(a) per 100 parts by weight of rubber, more specifically from about 0.5 to about 5 parts by weight of mercapto-functional alkylalkoxysilane (iii)(a) per 100 parts by weight of rubber, and even more specifically from about 1 to about 3 parts by weight of mercapto-functional alkylalkoxysilane (iii)(a) per 100 parts by weight of rubber. In some embodiments, the blocked mercapto-functional alkylalkoxysilane (iii)(b) can be used in an amount ranging from about 0.1 to about 15 parts by weight of blocked mercapto-functional alkylalkoxysilane (iii)(b) per 100 parts by weight of rubber, more specifically from about 1 to about 10 parts by weight of blocked mercapto-functional alkylalkoxysilane (iii)(b) per 100 parts by weight of rubber, and even more specifically from 3 to 8 parts by weight of blocked mercapto-functional alkylalkoxysilane (iii)(b) per 100 parts by weight of rubber.

[0225] In some embodiments, the process includes adding the scorch modifier (vi) simultaneously with the other vulcanization chemicals. In some embodiments, the step of adding the scorch modifier (vi) simultaneously with the other vulcanization chemicals is after the steps of adding the silica (ii), the mercaptosilane (iii)(a), and the blocked mercaptosilane (iii)(b) to the at least one diene based polymer (i)(a) and / or the at least one diene based polymer (i)(b). In some embodiments, the step of adding the scorch modifier (vi) simultaneously with the other vulcanization chemicals is a final mix.

[0226] In practice, sulfur-vulcanized rubber articles are typically prepared by thermomechanically mixing the rubber and various ingredients in a continuous and stepwise manner, followed by molding and curing the compounded rubber to form a vulcanized product. First, for said mixing of the rubber and various ingredients, the rubber(s) and various rubber compound additives, typically excluding vulcanizing agents and vulcanization accelerators (collectively "curing agents"), are typically blended in a suitable mixer in at least one, and often (in the case of silica-filled low rolling resistance tires) two, preliminary thermomechanical mixing stage(s). Deblocking agents and scorch modifiers can be added either in the preliminary thermomechanical mixing stage or in the final mixing stage. Such preliminary mixing is called non-productive mixing or non-productive mixing step or stage. Such preliminary mixing is usually carried out at a temperature of about 100°C to about 200°C, and often about 140°C to about 180°C. Following such premixing stages, in a final mix stage, sometimes referred to as the production mix stage, the vulcanizing agent(s), the deblocking agent(s) if not added in the premixing stage, the scorch modifier(s) if not added in the premixing stage, and possibly one or more additional ingredients are mixed with the rubber composition at a temperature lower than that used in the premixing stage, typically within the range of about 50° C. to about 130° C., to prevent or retard premature hardening of the curable rubber, sometimes referred to as scorching. This rubber mixture, variously referred to as a rubber compound or rubber composition, is typically allowed to cool, for example to a temperature of about 50° C. or less, during or after intermediate mill mixing, which is performed during the various mixing steps described above. When it is desired to mold and cure the rubber, the rubber is placed in a suitable mold at at least about 130° C. and up to about 200° C., and vulcanization of the diene-based polymer(s) occurs with the mercapto groups of the deblocked mercaptosilane and any other vulcanizing agent(s), such as free sulfur source(s), that may be present in the rubber mixture.

[0227] Thermomechanical mixing means that the rubber compound, i.e. the composition of rubber and rubber compounding ingredients, is mixed under high shear conditions in a rubber mixer where it autogenously heats up as a result of mixing, primarily due to shear and associated friction within the rubber mixture in the rubber mixer. During various steps in the mixing and curing process, several chemical reactions may occur.

[0228] The first reaction is a relatively fast reaction and may be considered to occur between the filler and the alkoxysilyl groups of the mercaptosilane and blocked mercaptosilane. Such a reaction may occur at a relatively low temperature, for example, about 120° C. The second and third reactions considered herein are the deblocking of the mercaptosilane and the subsequent reaction between the sulfur moiety of the mercaptosilane, including the deblocked mercaptosilane, and the sulfur vulcanizable rubber(s), which occurs at a higher temperature, for example, above about 140° C.

[0229] Other sulfur sources may also be used, for example in the form of elemental sulfur S8. Sulfur donors are considered herein to be sulfur-containing compounds that release free or elemental sulfur at temperatures ranging from about 140 to about 190°C. Examples of such sulfur donors may be, but are not limited to, polysulfide vulcanization accelerators and organosilane polysulfides, having at least two linked sulfur atoms in the polysulfidic linkage. The amount of free sulfur source added to the mixture can be controlled or manipulated as a matter of choice, relatively independently of the addition of the blocked mercaptosilane described above. Thus, for example, the independent addition of the sulfur source may be manipulated by its amount and by the order of addition relative to the addition of other components to the rubber mixture.

[0230] In one embodiment, the rubber composition is prepared by a process comprising: a) In at least one pre-mixing step, the following are thermomechanically mixed at a first elevated temperature, e.g., from about 140° C. to about 200° C., preferably from about 160° C. to about 190° C., and more preferably from about 155° C. to about 170° C., for a suitable time, e.g., 20 minutes, preferably from about 4 to about 15 minutes: at least one diene-based polymer (i)(a) containing at least one functional group and / or at least one diene-based polymer (i)(b) not containing a functional group, for example 100 parts by weight thereof; (ii) precipitated silica, for example from about 5 to about 140 phr (parts by weight per 100 parts by weight of rubber), preferably from about 25 to about 110 phr, or a mixture of precipitated silica and other fillers; a coupling agent package (iii) which is a mixture of at least one mercaptosilane (iii)(a) and at least one blocked mercaptosilane (iii)(b), e.g., from about 1 to about 20 phr of the mixture (coupling agent package (iii)); and optionally some or all of the deblocking agent (iv) and / or scorch modifier (vi); b) in a final thermomechanical mixing step, blending the mixture resulting from (a) at a second elevated temperature lower than the first elevated temperature, e.g., from about 50° C. to about 130° C., for a suitable time, e.g., up to about 30 minutes, and preferably from about 1 to about 3 minutes, with at least one deblocking agent (iv), preferably from about 0.05 to about 20 phr, if not included in step (a), at least one scorch modifier (vi), if not included in step (a), and from about 0.1 to about 10 phr of a vulcanization package; and, optionally, c) curing the mixture from step (b) at a third elevated temperature, such as from about 130° C. to about 200° C., for a suitable time, such as from about 5 to about 60 minutes. In another embodiment, the above process may also include the additional step of preparing an assembly of a tire or vulcanizable rubber and a tread comprised of the rubber composition prepared according to the process described herein, and vulcanizing the assembly at a temperature in the range of from about 130° C. to about 200° C.

[0231] In one embodiment, the rubber composition is prepared by a process comprising: a) In at least one pre-mixing step, the following are thermomechanically mixed at a first elevated temperature, e.g., from about 140° C. to about 200° C., preferably from about 160° C. to about 190° C., and more preferably from about 155° C. to about 170° C., for a suitable time, e.g., 20 minutes, preferably from about 4 to about 15 minutes: at least one diene-based polymer (i)(a) containing at least one functional group and at least one diene-based polymer (i)(b) not containing a functional group, for example 100 parts by weight thereof; (ii) precipitated silica, for example from about 5 to about 140 phr (parts by weight per 100 parts by weight of rubber), preferably from about 25 to about 110 phr, or a mixture of precipitated silica and other fillers; a coupling agent package (iii) which is a mixture of at least one mercaptosilane (iii)(a) and at least one blocked mercaptosilane (iii)(b), e.g., from about 1 to about 20 phr of the mixture (coupling agent package (iii)); and optionally some or all of the deblocking agent (iv) and / or scorch modifier (vi); b) in a final thermomechanical mixing step, blending the mixture resulting from (a) at a second elevated temperature lower than the first elevated temperature, e.g., from about 50° C. to about 130° C., for a suitable time, e.g., up to about 30 minutes, and preferably from about 1 to about 3 minutes, with at least one deblocking agent (iv), preferably from about 0.05 to about 20 phr, if not included in step (a), at least one scorch modifier (vi), if not included in step (a), and from about 0.1 to about 10 phr of a vulcanization package; and, optionally, c) curing the mixture from step (b) at a third elevated temperature, such as from about 130° C. to about 200° C., for a suitable time, such as from about 5 to about 60 minutes. In another embodiment, the above process may also include the additional step of preparing an assembly of a tire or vulcanizable rubber and a tread comprised of the rubber composition prepared according to the process described herein, and vulcanizing the assembly at a temperature in the range of from about 130° C. to about 200° C.

[0232] In yet another embodiment, the rubber composition can be used to manufacture a variety of articles. For example, it can be used for various tire compounds such as treads, sidewalls, beads, and others. Such tires can be constructed, formed, molded, and cured by a variety of methods known and readily apparent to those having skill in the art. Others include hoses, belts, rollers, insulating jackets, industrial products, shoe soles, bushings, damping pads, and others.

[0233] The invention may be better understood by reference to the following examples, in which parts and percentages are by weight unless otherwise specified. Working Example

[0234] The ingredients for preparing the rubber composition are as follows:

[0235] A non-functionalized solution styrene butadiene rubber is available as Sprintan® from Trinseo (dba Synthos SA). TM It is an oil-extended polymer designated SLR4630 and has a Mooney viscosity (ML1+4(100°C)) of 55MU, a bound styrene content of 25.0%, a vinyl content of 62.0%, a TDAE (treated distillate aromatic extract) oil content of 37.5 phr, and a glass transition temperature of the dry polymer of -19°C.

[0236] Carbon black activated functionalized solution styrene butadiene is Sprintan available from Trinseo TMThe dry polymer is designated SLR4601 and has a Mooney viscosity (ML1+4(100°C)) of 50MU, a bound styrene content of 21.0%, a vinyl content of 62.0%, no oil, and a glass transition temperature of the dry polymer of -25°C.

[0237] Silica and carbon black activated functionalized solution styrene butadiene is Sprintan available from Trinseo. TM The dry polymer is designated SLR4602 and has a Mooney viscosity (ML1+4(100°C)) of 50MU, a bound styrene content of 21.0%, a vinyl content of 62.0%, no oil, and a glass transition temperature of the dry polymer of -25°C.

[0238] Butadiene rubber is a neodymium (Nd) catalyzed high cis polybutadiene, sold by Chimei under the trade name KIBIPOL 登録商標 It is available under the HBR PR-040G with a Mooney viscosity (ML1+4(100°C)) range of 39-49MU, cis-butadiene content >97%, and vinyl content <1%.

[0239] Precipitated synthetic amorphous silica is sold under the trade name ZEOSIL by Solvay (formerly known as Rhodia). 登録商標 Highly disperse silica (HDS) micropearls available under 1165MP, with a BET specific surface area of ​​165 m2 / g under nitrogen.

[0240] The carbon black is a medium reinforcing black filler designated N330 available from Tokai Carbon CB via Harwick Standard, with a BET specific surface area of ​​78 m2 on nitrogen. 2 / g.

[0241] Silane 1 is octanethioic acid S-[3-(triethoxysilyl)propyl] ester, CAS No. 220727-26-4, available from Momentive Performance Materials under the trade name Silquest*NXT* silane.

[0242] Silane 2 is 3-triethoxysilylpropane-1-thiol, CAS No. 13814-09-6, available from Momentive under the tradename Silquest* A-1891 silane.

[0243] The process oil is a treated distillate aromatic extract (TDAE) oil, available from H&R Group under the trade name Vivatec 500.

[0244] The processing aid is a zinc soap of a rubber-soluble high molecular weight fatty acid, available from Struktol Corporation under the trade name Struktol 登録商標 Available under A60.

[0245] Antidegradant 1 is N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, available from Harwick & Co. under the trade name Stangard. 登録商標 Available under 6PPD.

[0246] Degradation inhibitor 2 is a paraffin blend microcrystalline wax, available from Acrochem under the trade name AKROWAX 登録商標 Available under 5084.

[0247] Antidegradant 3 is a 2,2,4-trimethyl-1,2-dihydroquinoline polymer sold by Harwick under the trade name Stangard. 登録商標 Available under TMQ.

[0248] Activator 1 is zinc oxide, available from Harwick Corporation under the name Zinc Oxide CR-40.

[0249] Enhancer 2 is stearic acid, available from Harwick & Co. under the trade name Stearic Acid F-2000.

[0250] The curing agent is sulfur, available from Georgia Gulf Sulfur Company under the trade name Rubber Makers Sulfur.

[0251] The accelerator is N-cyclohexyl-2-benzothiazole sulfonamide, available from Harwick under the trade name KEMAI CBS GR.

[0252] The tackifying resin is an unsaturated aromatic hydrocarbon resin derived from the polymerization of unsaturated aromatic olefins and diolefins, and also from the polymerization of diolefins derived from the thermal cracking of naphtha, and is sold by Akrochem under the trade name 登録商標 Available under P-90 resin.

[0253] The scorch modifier is tetrabenzyl thiuram disulfide, sold by Akrochem under the trade name AKROCHEM 登録商標 Available under Accelerator TBzTD.

[0254] The test procedures for evaluating the vulcanized (cured) rubber compositions of the present application are described below by ASTM or DIN methods (Table 2): [Table 2]

[0255] Rolling resistance is abbreviated as RR, strain sweep is abbreviated as SS, temperature sweep is abbreviated as TS, rubber processability measurement is abbreviated as RPA, and dynamic mechanical properties measurement is abbreviated as DMA. Comparative Example 1 Preparation and Evaluation of Rubber Compositions [Table 3] [Table 4]

[0256] The rubber composition was prepared by mixing the ingredients as follows: 登録商標The rubber is prepared by mixing in a mixer (Model BR-1600, ASTM 3182 Certified Laboratory Mixer, Farrell Co.). The mixing of the rubber is done in three stages.

[0257] The mixer was set at a rotor speed of 75 rpm and a temperature of 130°F + / - 10°F (55°C) and maintained at this temperature using cooling water. In the first mixing stage, called Masterbatch 1, the rubber polymer is added to the mixer and ram mixed for 40 seconds. Half of the silica and Silane 1 and / or Silane 2 are added to the mixer and ram mixed for 50 seconds, where Silane 1 is NXT* silane and Silane 2 is Silquest* A-1891. The remaining silica and the other ingredients of Masterbatch 1, except for the carbon black and process oil, are added and mixed to a temperature of 257°F (125°C). The carbon black and process oil are added to the mixer and mixed to a temperature of 275°F (135°C). The mixer is swept to ensure all materials are added to the mixing chamber. The ingredients are mixed at a speed of less than 95 rpm to a temperature of 302°F (150°C) and held at that temperature for 90 seconds. The total mixing time is between 420 and 430 seconds.

[0258] The material is removed from the mixing chamber and compounded on a two-roll mill (Farrell, Two Cylinder Roll Mill) set at a temperature of approximately 140°F (60°C). The rubber is wrapped around one cylinder to form a bank of rubber that rotates in the nip between the two cylinders. As the rubber leaves the mill, the compounded rubber is cross-cut from left to right at 1 inch per revolution, starting with a 1 inch wide ribbon. This compounding step is repeated five times and then allowed to cool to ambient temperature. The compounded rubber is designated as Masterbatch 1, which is the non-productive mix step.

[0259] In the second mixing stage, called Masterbatch 2, or the remix dispersion process, the rubber composition of Masterbatch 1 is charged back into the mixer. The mixer speed is 75 rpm, the mixer temperature is 140°F + / - 10°F (60°C), and the mix time is 40 seconds. The temperature is raised to 275°F (135°C) and held at that temperature for 30 seconds. The mixer is swept. The rubber is then mixed at less than 95 rpm to a temperature of 302°F (150°C) and held at that temperature for 90 seconds. The total mix time is between 300 and 315 seconds.

[0260] The material leaves the mixing chamber and is compounded and dispersed on a two-roll mill set at a temperature of approximately 140°F (60°C). The rubber is wrapped around one cylinder to form a bank of rubber that rotates in the nip between the two cylinders. As the rubber leaves the mill, the compounded rubber is cross-cut from left to right at 1 inch per revolution, starting with a 1 inch wide ribbon. This compounding stage is repeated five times and then allowed to cool to ambient temperature. The compounded rubber is designated as Masterbatch 2, which is the non-productive mix stage.

[0261] In the third mix stage, called Masterbatch 3, or Final Mix (FM), the mixer temperature is set at 100°F + / - 10°F (38°C). Masterbatch 2 and vulcanization chemicals are charged to the mixer along with the curatives and mixed at 50 rpm. The rubber is mixed until a temperature of 200°F (93°C) is reached and then held at that temperature for a total mix time of 170 seconds. The rubber is further mixed at a speed of less than 75 rpm until the temperature reaches 212°F (100°C). The rubber is mixed for a total of between 210 and 215 seconds.

[0262] After mixing, Masterbatch 3 is discharged from the mixing chamber and milled and dispersed on a two-roll mill set at a temperature of about 140° F. (60° C.) to form a sheet, which is then cooled to ambient temperature and used to measure green properties such as Mooney viscosity and Mooney scorch.

[0263] The sheet is cured under the conditions of 160° C. for 20 minutes. The cured sheet is used to measure the cured properties of the rubber composition.

[0264] Performance index values ​​are used to evaluate rubber compositions. Performance index values ​​are calculated by first determining the ratio of index performance values ​​(PIPi) measured for each index for the rubber composition. Performance index properties (PIPi) for processability index 1 (Mooney scorch, 3 point increase), handling index 2 (Shore A hardness), grip index 3 (rebound resilience at 0°C), and grip index 4 (DMA TS tan δ maximum value) are calculated. i ) is the ratio of the measured performance index value (PIP i ) was compared with the index value (PIP io ) for processability index 5 (Mooney viscosity, ML(1+4)100℃), rolling resistance index 6 (RPA SS 60℃ tan δ maximum), rolling resistance index 7 (DMA TS 60℃ tan δ), and abrasion index 8 (DIN abrasion). i ) is the ratio of the performance index value (PIP) measured for the control rubber composition. io ) to the measured performance index value (PIP i ) The formula for calculating the figure of merit is:

number

[0265] The data from the examples support the synergistic effect of combining silanes 1 and 2 with different weight ratios and the use of functionalized polymers. For example, the performance index for compounds 11-15 shows an improvement with the blend of silanes 1 and 2 compared to the individual silanes when compared to the control compounds 1-14, where the SSBR used in compounds 1-14 is non-functionalized for silica and the SSBR used in compounds 11-15 is functionalized for silica. These performance index values ​​show that the functionalized polymer rubber composition with both silanes 1 and 2 provides improvements in many important parameters such as wear, rolling resistance, grip, and handling when compared to rubber compositions based on non-functionalized polymers and only silanes 1 or 2. The ΔTan δ (0°C-60°C) values ​​of the examples further illustrate the advantages of the present invention. The blend of silanes 1 and 2 shows improved ΔTan δ (0°C-60°C) values ​​over rubber compositions containing only silanes 1 or 2. An additional advantage is observed for the wet traction tan δ at 0° C. (Metravib - 0.5% at 60° C. temperature sweep, 2% DSA). The compositions of the present invention show a statistically significant improvement in wet traction performance. The compositions of the present invention also show a synergistic effect in that the rubber compositions containing only Silane 1 or only Silane 2 have a worse Wet Traction Index (lower values) than the rubber compositions containing both Silane 1 and Silane 2. Example 2 Preparation of 3-(2-ethylhexanoylthio)-1-propyltriethoxysilane

[0266] The reactor consisted of a 5-liter round-bottom reaction flask fitted with a mechanical stirring impeller, an addition funnel, a thermocouple, a nitrogen inlet, and a gas outlet. The gas outlet fed into a scrubber of aqueous sodium hydroxide to trap hydrogen sulfide released by the process. The thermocouple was fitted with an electronic temperature controller. A stripping apparatus was also assembled to remove residual water from the product. This apparatus consisted of a 1-liter round-bottom flask fitted with a thermocouple and a 5-plate bubble plate (Oldershaw) column. The column was fitted with a short-path distillation head, against which was fitted a collection flask to collect the distillate. Vacuum was applied to the head via a mechanical vacuum pump. A cold trap cooled with dry ice was placed between the distillation head and the pump to capture volatiles. An electronic pressure gauge monitored the absolute pressure between the cold trap and the vacuum pump. The contents of the flask were stirred with a magnetic stir bar and a stirring motor.

[0267] The reaction flask was initially charged with 785 grams of 45% aqueous sodium hydrogen sulfide solution (NaSH 6.30 moles) and deionized water (676 grams; 37.5 moles). The mixture was slowly stirred with a mechanical stirrer, and then tetrabutylammonium bromide crystals (0.0057 moles; 3.7 grams) were added. Stirring was continued for 5 minutes, producing a clear yellow homogeneous solution. The addition funnel was charged with 2-ethylhexanoyl chloride (471 grams; 2.89 moles). A first amount of 2-ethylhexanoyl chloride was then introduced into the reactor in the amount of 25 mL. The reaction that followed was slow. The temperature of the reactor was then raised to 48° C. A second amount of 2-ethylhexanoyl chloride, about 55 mL, was then introduced through the addition funnel, resulting in the liberation of gas (hydrogen sulfide), as indicated by the bubbling observed in the scrubber. The dropwise addition of 2-ethylhexanoyl chloride was then begun and maintained at a rate to provide a steady bubbling of hydrogen sulfide, which was completed after 2.5 hours.

[0268] The set point of the electronic temperature controller was set to 95°C and the reactor contents continued to be stirred. When the temperature reached 79°C, additional crystals of tetrabutylammonium bromide (11 grams; 0.017 moles) were added, which quickly dissolved. 3-chloro-1-propyltriethoxysilane (682 grams; 2.83 moles) was then added all at once to the reactor. The stirring speed was increased to and maintained at 635 revolutions per minute. Within approximately 10 minutes the temperature reached 95°C and rose briefly 2-3°C before settling constant at 95°C. After 2 hours, the external heating and stirring were discontinued. The mixture quickly separated into two distinct phases.

[0269] The reactor contents were immediately transferred, while still hot, to a separatory funnel via a cannula tube. The liquid quickly separated into three distinct layers. The bottom aqueous layer and the middle layer were poured off and discarded. Approximately 2 / 3 of the remaining organic phase was then immediately transferred to the stripper. Vacuum was gradually applied while slowly stirring the flask contents until the absolute pressure reading was 0.5 torr. Sufficient boiling resulted in no distillate being collected. Vapors consisting mainly of residual water were collected as solids in the trap. Once boiling ceased, the temperature was gradually increased. At approximately 90°C, condensate began to appear in the lower portion of the column. The temperature was then increased to 160°C while distillate was collected in the collection vessel. When no additional liquid was being collected, stripping was stopped. The remaining contents of the distillation flask were allowed to cool, and the resulting cloudy, nearly colorless liquid was decanted, ultimately resulting in a clear, nearly colorless liquid product and a thin layer of white precipitate remaining. The remaining organic phase in the separatory funnel was then treated in the same manner.

[0270] The final product was first analyzed by gas chromatography (GC, area %) and mass spectrometry (GCMS) to confirm that the desired product had been obtained. Purity was determined by gas chromatography (GC, mass %) of the product containing a known amount of an internal standard (heptadecane). The composition of this product was determined to be: 96.03% 3-(2-ethylhexanoylthio)-1-propyltriethoxysilane (target product), 1.94% 3-chloro-1-propyltriethoxysilane, 0.79% 3-mercapto-1-propyltriethoxysilane, 0.18% bis(3-triethoxysilyl-1-propyl) disulfide (TESPD), and 1.06% uneluted weights (mostly siloxanes). Example 3 Preparation of amyl-(3-triethoxysilyl-1-propyl) xanthate

[0271] The reactor consisted of a 250 mL three-neck round-bottom flask equipped with a water condenser fitted with a nitrogen bubbler, an addition funnel, a Teflon-coated magnetic stir bar, a magnetic stirring motor, and a heating mantle controlled by an electronic temperature controller.

[0272] 3-Chloro-1-propyltriethoxysilane (12.2 grams; 0.5 moles) was charged to the reactor. Potassium amyl xanthate (10.1 grams; 0.05 moles) and potassium iodide (1.6 grams; 0.01 moles) were added to the reaction flask while stirring vigorously to prevent the formation of lumps. The potassium iodide had previously been ground to a fine powder using a mortar and pestle. The mixture was stirred and heated. The temperature was set at 175°C. The progress of the reaction was monitored by removing aliquots and obtaining gas chromatography traces. The GC trace showed that after 3 hours of heating at 175°C, only 26% of the product was obtained in addition to increasing formation of undissolved components.

[0273] All publications, patents, and patent applications mentioned in this specification are incorporated by reference in their entirety to the same extent as if each individual publication, patent, or patent application was specifically and individually indicated to be incorporated by reference in its entirety. In the event that a term in this application is found to have a different definition than in a document incorporated by reference, the definition provided in this application is to be used as the definition for that term.

Claims

1. 1. A rubber composition comprising: a. at least one diene-based polymer; b. precipitated silica; c. at least one coupling agent package comprising a mercapto-functional alkylalkoxysilane and a blocked mercapto-functional alkylalkoxysilane; d. at least one deblocking agent; e. a vulcanization package comprising at least one vulcanizing agent comprising sulfur and at least one accelerator; f. at least one scorch modifier; and g. Optionally, at least one filler A rubber composition comprising:

2. 2. The rubber composition of claim 1, wherein the at least one diene-based polymer is a diene-based polymer containing at least one functional group, a diene-based polymer not containing a functional group, or a combination thereof.

3. The diene-based polymer containing at least one functional group is a compound of formula (I): [C10] During the ceremony P is a (co)polymer chain of a conjugated diolefin or a conjugated diolefin and an aromatic vinyl compound; R 1 is an alkylene group having 1 to 12 carbon atoms; R 2 and R 3 each independently is an alkyl, aryl, or aryl group having 1 to 20 carbon atoms; and k, m and n are each integers, where n is 1 or 2, m is 1 or 2, and k is 1 or 2, with the proviso that n+m+k is an integer of 3 or 4; Or a compound of formula (II): [C11] During the ceremony P is a (co)polymer chain of a conjugated diolefin or a conjugated diolefin and an aromatic vinyl compound; R 1 is an alkylene group having 1 to 12 carbon atoms; R2 and R 3 each independently is an alkyl group having 1 to 20 carbon atoms, an aryl group, or an aryl group having 6 to 12 carbon atoms; and 2. The rubber composition of claim 1, wherein j and h are each an integer, where j is an integer from 1 to 3 and h is an integer from 1 to 3, with the proviso that j+h is an integer from 2 to 4.

4. The diene-based polymer containing at least one functional group is a compound of formula (V): [C12] During the ceremony P is a (co)polymer chain of a conjugated diolefin or a conjugated diolefin and an aromatic vinyl compound; R 1 is an alkylene group having 1 to 12 carbon atoms; R 2 and R 3 each independently is an alkyl, aryl, or aryl group having 1 to 20 carbon atoms; and 2. The rubber composition of claim 1, wherein k, m and n are each integers, where n is 1 or 2, m is 1 or 2, and k is 1 or 2, with the proviso that n+m+k is an integer of 3 or 4.

5. The diene-based polymer comprising at least one functional group further comprises a terminating agent, wherein the terminating agent is of formula (iii): [C13] During the ceremony R 1 is an alkylene group having 1 to 12 carbon atoms; R 2 and R 3 independently an alkyl, aryl, or aryl group having 1 to 20 carbon atoms; R 4 , R 5 , and R 6 each independently represents an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, provided that R 4 and R 5 may be bonded to each other via a covalent bond to form a ring with the silicon atom to which they are attached; and k, m and n are each an integer, where n is 1 or 2, m is 1 or 2, and k is 1 or 2, with the proviso that n+m+k is an integer of 3 or 4; or of formula (IV): [C14] During the ceremony R 1 is an alkylene group having 1 to 12 carbon atoms; R 2 and R 3 each independently is an alkyl, aryl, or aryl group having 1 to 20 carbon atoms; R 4 , R 5 , and R 6 each independently represents an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, provided that R 4 and R 5 may be bonded to each other via a covalent bond to form a ring with the silicon atom to which they are attached; and 3. The rubber composition of claim 2, wherein m is an integer of 1 or 2.

6. The mercapto-functional alkylalkoxysilane is a mercaptosilane of formula (X): [C15] During the ceremony R 17 are independently a straight chain alkylene group of 1 to 6 carbon atoms or a branched chain alkylene group of 3 to 6 carbon atoms; R 18 each of which is a straight chain alkylene group of from 2 to 8 carbon atoms or a branched chain alkylene group of from 3 to 8 carbon atoms; R 19each independently is a straight chain alkylene group of 1 to 6 carbon atoms or a branched chain alkylene group of 3 to 6 carbon atoms; X 1 Yes - OR 20 Group, where R 20 is an alkyl group having 1 to 4 carbon atoms; -OR 21 OH group, where R 21 is a linear alkylene group having 2 to 8 carbon atoms or a branched alkylene group having 3 to 8 carbon atoms, or X 1 Yes - OR 22 (OR 23 ) c OR 224 , where R 22 is a linear alkylene group having 2 to 6 carbon atoms or a branched alkylene group having 3 to 6 carbon atoms; R 23 each independently represents an alkylene group of 2 to 4 carbon atoms; R 24 is a linear alkyl group of 1 to 16 carbon atoms or a branched alkyl group of 3 to 16 carbon atoms, and c is an integer from 1 to 20; X 2 and X 3 is independent of X 1 or methyl; X 4 Each of X is independently 1 or methyl; and a is an integer from 0 to 8, (iii) X 1 and X 2 -OR 20 When , two -OR 20 are bonded together via covalent bonds to the same silicon atom, 20 -R 20 O-groups may be formed to form a ring structure containing 2 to 8 carbon atoms, two oxygen atoms, and a silicon atom; and (iv) a is 1 to 8 and X 3 and X 4 -OR 20 When , two -OR 20 The groups are bonded together via covalent bonds and attached to the same silicon atom. 20 -R 202. The rubber composition of claim 1, wherein the O-groups may be formed to form a cyclic structure containing from 2 to 8 carbon atoms, two oxygen atoms, and a silicon atom.

7. The blocked mercapto-functional alkylalkoxysilane is a blocked mercaptosilane of formula (XI): [C16] During the ceremony R 17 are independently a straight chain alkylene group of 1 to 6 carbon atoms or a branched chain alkylene group of 3 to 6 carbon atoms; R 18 each of which is a straight chain alkylene group of from 2 to 8 carbon atoms or a branched chain alkylene group of from 3 to 8 carbon atoms; R 19 each independently is a straight chain alkylene group of 1 to 6 carbon atoms or a branched chain alkylene group of 3 to 6 carbon atoms; X 1 Yes - OR 20 Group, where R 20 is an alkyl group having 1 to 4 carbon atoms; -OR 21 OH group, where R 21 is a linear alkylene group having 2 to 8 carbon atoms or a branched alkylene group having 3 to 8 carbon atoms, or X 1 Yes - OR 22 (OR 23 ) c OR 24 , where R 22 is a linear alkylene group having 2 to 6 carbon atoms or a branched alkylene group having 3 to 6 carbon atoms, preferably 3 carbon atoms; R 23 each independently represents an alkylene group of 2 to 4 carbon atoms; R 24 is a linear alkyl group of 1 to 16 carbon atoms or a branched alkyl group of 3 to 16 carbon atoms, and c is an integer from 1 to 20; X 2 and X 3 is independent of X 1 or methyl; X 4 Each of X is independently 1 or methyl; Y 1Each of the formulas is -C(=O)R 25 Or -C(=S)OR 25 , where each R 25 are independently a straight chain alkylene group of 1 to 16 carbon atoms, more specifically 5 to 11 carbon atoms, and even more specifically 6 to 9 carbon atoms, or a branched chain alkylene group of 3 to 16 carbon atoms, more specifically 5 to 11 carbon atoms, and even more specifically 6 to 9 carbon atoms; and a is an integer from 0 to 8, (iii) X 1 and X 2 -OR 20 When , two -OR 20 are bonded together via covalent bonds to the same silicon atom, 20 -R 20 O-groups may be formed to form a ring structure containing 2 to 8 carbon atoms, two oxygen atoms, and a silicon atom; and (iv) a is 1 to 8 and X 3 and X 4 -OR 20 When , two -OR 20 The groups are bonded together via covalent bonds and attached to the same silicon atom. 20 -R 20 2. The rubber composition of claim 1, wherein the O-groups may be formed to form a cyclic structure containing from 2 to 8 carbon atoms, two oxygen atoms, and a silicon atom.

8. 2. The rubber composition of claim 1, wherein the weight ratio of the blocked mercapto-functional alkylalkoxysilane to the mercapto-functional alkylalkoxysilane is from about 0.25:1 to about 50:

1.

9. At least one deblocking agent is a compound of formula (XII): R 26 [A 3 -H] d (XII) During the ceremony: R 26 is a monovalent or polyvalent organic radical containing 1 to 30 carbon atoms or hydrogen, A 3 each independently represents oxygen, sulfur, or -NR 27 group, where each R 27 are independently a monovalent or polyvalent organic radical containing 1 to 30 carbon atoms or hydrogen; and 2. The rubber composition of claim 1, wherein d is an integer from 1 to 100, preferably from 1 to 3.

10. 2. The rubber composition of claim 1, wherein the sulfur in the vulcanizing agent is selected from the group consisting of elemental sulfur, sulfur donor compounds, and combinations thereof.

11. 2. The rubber composition of claim 1, wherein the at least one accelerator is selected from the group consisting of benzothiazoles, guanidine derivatives, thiocarbamates, and combinations thereof.

12. The at least one scorch modifier is a compound of formula (XIII): R 28 2 NC(=S)SSC(=S)NR 28 2 (XIII) During the ceremony R 28 2. The rubber composition of claim 1, wherein: are independently a straight chain alkyl group of 1 to 12 carbon atoms, a branched chain alkyl group of 3 to 12 carbon atoms, a cycloalkyl group of 5 to 12 carbon atoms, an aryl group of 6 to 12 carbon atoms, or an aralkyl group of 7 to 12 carbon atoms.

13. 2. The rubber composition of claim 1, wherein the at least one diene based polymer is reactive with precipitated silica.

14. 2. The rubber composition of claim 1, wherein the composition has a Mooney viscosity of from about 40 MU to about 150 MU, as measured using ASTM D-1646 method.

15. 2. The rubber composition of claim 1, wherein the composition has a Mooney scorch at 3 points increase from about 5 minutes to about 40 minutes as measured using ASTM D-1646 method.

16. 10. The rubber composition of claim 1, wherein the composition has a tensile strength of about 5 MPa to about 25 MPa as measured using ASTM D-412 method.

17. 1. A rubber composition comprising: (i) about 100 parts rubber, where the weight of rubber is the sum of the weight of each diene based polymer used in the compounding that contains at least one functional group and the weight of each diene based polymer used in the compounding that does not contain at least one functional group; (ii) from about 5 to about 140 parts by weight of precipitated silica per 100 parts of rubber (i); (iii) from about 1 to about 20 parts by weight per 100 parts of rubber (i) of a coupling agent package comprising a mercapto-functional alkylalkoxysilane and a blocked mercapto-functional alkylalkoxysilane; (iv) from about 0.1 to about 20 parts by weight of a deblocking agent per 100 parts of rubber (i); (v) from about 0.1 to about 10 parts by weight per 100 parts of rubber (i) of a vulcanization package comprising sulfur and at least one accelerator; and (vi) a rubber composition comprising from about 0.1 to about 5 parts by weight of a scorch modifier per 100 parts of rubber (i).

18. 1. A process for preparing a composition comprising adding silica, a mercapto-functional alkylalkoxysilane, a blocked mercapto-functional alkylalkoxysilane, and optionally at least one scorch modifier to at least one diene-based polymer simultaneously with a vulcanization package comprising at least one vulcanizing agent comprising sulfur and at least one accelerator.

19. The composition comprises: a. about 30% to about 40% by weight of at least one diene-based polymer containing at least one functional group; b. about 30% to about 40% by weight of precipitated silica; c. about 0.05% to about 5% by weight of a blocked mercapto-functional alkylalkoxysilane; d. about 0.05% to about 5% by weight of a mercapto-functional alkylalkoxysilane; e. about 0.1% to about 10% by weight of a scorch modifier; and f. The process of claim 18, further comprising a vulcanization package comprising at least one vulcanizing agent, optionally including sulfur, and at least one accelerator.

20. 20. A composition prepared by the process of claim 18, wherein the composition is a rubber composition.

21. 21. The rubber composition of claim 20, wherein the rubber composition is a tire composition.

Citation Information

Patent Citations

  • Production of granulated body of silica by precipitation method and filler for reinforcing elastomer

    JP1996133720A

  • Conjugated diolefin (CO)polymer rubber and method for producing the same, rubber composition and tire

    JP2004018795A

  • Modified conjugated diene-based polymer composition

    JP2013082778A

  • Rubber composition for tire, and pneumatic tire

    JP2013087181A

  • Method of producing rubber composition

    JP2013129696A

Cited By

  • Rubber composition for tire treads and tires

    JP2026119851A

  • Rubber composition for tire treads and tires

    JP7904505B2

  • Rubber composition for tire treads, and tire

    WO2026150867A1