Hot stamping forming method for pre-coated steel sheet

A preliminary heat treatment process for pre-coated steel sheets enhances alloying and fracture performance by refining the microstructure, addressing the limitations of existing hot stamping methods and improving industrial production efficiency.

JP2024538806APending Publication Date: 2024-10-23THE UNIVERSITY OF HONG KONG
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024523689
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-21
Filing Date
2022-10-11
Publication Date
2024-10-23

AI Technical Summary

Technical Problem

Existing hot stamping processes for pre-coated steel sheets face challenges in simultaneously improving the degree of alloying of the precoat layer and the fracture performance of the steel plate base material, leading to issues such as scale adhesion, wear, poor coating performance, and inadequate corrosion resistance, while also having narrow temperature and time process windows that hinder industrial production efficiency.

Method used

A preliminary heat treatment process involving heating and cooling cycles is applied to pre-coated steel sheets, including heating at specific temperatures for defined times and cooling at controlled rates to refine the microstructure, thereby enhancing alloying and fracture performance.

Benefits of technology

The method improves the degree of alloying and fracture performance of pre-coated steel sheets, reducing mold wear, crack formation, and expanding the process window for hot stamping, resulting in improved industrial production stability and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538806000001_ABST
    Figure 2024538806000001_ABST
Patent Text Reader

Abstract

The present invention provides a hot stamping forming method for a precoated steel sheet, which includes pre-heat treating the precoated steel sheet before hot stamping, and the pre-heat treatment includes (1) heating the precoated steel sheet to 850-920°C and keeping the temperature for 7-15 minutes, or heating the precoated steel sheet to 920-960°C and keeping the temperature for 5-10 minutes, (2) cooling the precoated steel sheet to 300°C or less at a cooling rate of 5°C / s or more after the heating and keeping step, and (3) optionally repeating the heating and keeping and cooling steps one or more times. The pre-heat treatment can increase the degree of alloying of the precoat layer, reduce the carbide structure in the steel sheet substrate, and obtain a substrate structure of martensite and / or bainite, thereby reducing the wear of the precoat layer against the stamping die during high-temperature stamping deformation, and refine the crystal grains, thereby improving the fracture performance of the final hot stamping formed member.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to Chinese patent application No. 20211226071.X filed on October 21, 2021, and the entire contents of the above Chinese patent application are incorporated herein by reference as part of this application.

[0002] The present invention relates to a hot stamping forming method for pre-coated steel sheets. [Background technology]

[0003] With the proposal of the goals of "peaking CO2 emissions" and "carbon neutral," energy conservation and emission reduction in automobiles have become an urgent task, and the weight reduction of automobiles has become an effective means of achieving this. Among the many lightweight materials, ultra-high strength steel is an ideal material for realizing the weight reduction of automobiles while ensuring vehicle safety due to its advantages of high strength, low cost, and mature processing.

[0004] Hot stamping is a forming process in which fully austenitized steel plate is stamped and deformed under high temperature, and then cooled rapidly at the same time to obtain ultra-high strength steel components. Hot stamping has the advantages of high forming precision and good weight reduction effect, and is particularly suitable for processing and forming complex integrated thin-walled parts such as A-pillars, B-pillars, and back-top cross beams of automobile white body.

[0005] In the actual hot stamping process, in order to avoid oxidation and decarbonization of the steel surface due to high temperature, the steel sheet surface is usually pre-coated. Among them, the most widely applied is the high temperature resistant Al-Si plating layer patent invented by ArcelorMittal in 1999, and the hot forming steel sheet pre-coated with the above Al-Si plating layer was commercialized in 2007. However, even after more than 20 years since the invention of the Al-Si plating layer, the contradiction between the degree of alloying of the pre-coated layer and the fracture performance of the steel sheet substrate could not be resolved.

[0006] The first problem is how to increase the degree of alloying of the precoat layer.

[0007] If the degree of alloying is insufficient, the pre-coated steel sheet will have problems such as scale adhesion and wear at the furnace rolls, forming dies, etc., which is very disadvantageous for practical production. At the same time, if the degree of alloying is insufficient, the proportion of tough phase in the intermetallic compound of the pre-coated layer will be low and the proportion of brittle phase will be high, making it easy for cracks to form in the coating layer, which will affect the paintability, corrosion resistance, and other performance of the pre-coated steel sheet.

[0008] In the process of hot stamping forming of precoated steel sheet, a relatively high heating temperature and a relatively long heat retention time are usually required to ensure the degree of alloying. For example, CN 101583486 B (hereinafter referred to as Patent Document 1) discloses a hot stamping forming process of precoated steel, which is the main production process of the current precoated steel, and clarifies that when the thickness of the Al-Si coating layer is 20-33 μm, the austenitizing heating and heat retention process is limited to the inside of a rectangle consisting of (3 minutes, 930 ° C), (6 minutes, 930 ° C), (13 minutes, 880 ° C), and (4.5 minutes, 880 ° C) when the thickness of the steel sheet is 0.7-1.5 mm, and the temperature and time are limited to the inside of a rectangle consisting of (4 minutes, 940 ° C), (8 minutes, 940 ° C), (13 minutes, 900 ° C), and (6.5 minutes, 900 ° C) when the thickness of the steel sheet is 1.5-3 mm. The above-mentioned invention patent further specifies the ratio of Fe2Al5 phase and FeAl phase in the microstructure of the pre-coated layer after hot stamping, so as to ensure the performance of the pre-coated steel member after hot stamping, such as painting, welding, corrosion resistance, etc.

[0009] The second problem is how to improve the fracture performance of pre-coated steel substrates.

[0010] In order to improve the rupture performance, it is usually necessary to adopt a low heating temperature and a short heat retention time so as to avoid excessive growth of austenite grains at high temperatures. However, the above requirement is in conflict with the requirement to increase the degree of alloying of the precoat layer. Conventional techniques have no choice but to strike a balance between the two, and it is not possible to simultaneously improve the degree of alloying of the precoat layer and the rupture performance of the steel sheet substrate.

[0011] It is noteworthy that the current pre-coated steel hot stamping formed parts cannot meet the fracture performance standards of all automobile factories. The above fracture performances include low temperature fracture, bending fracture, hydrogen delayed fracture, etc. Non-ideal low temperature fracture, bending fracture, or hydrogen delayed fracture performance may cause local fracture failure in the body parts during the service or collision of the automobile, which may endanger the safety of passengers. In particular, the Al-Si plating layer alloys at high temperatures to form brittle intermetallic compounds, brittle high aluminum high silica ferrite, and brittle high carbon martensite, and these brittle structures further reduce the fracture performance of the hot stamping formed steel parts. In actual industrial production, after hot forming, the fracture performance of the pre-coated steel sheet was obviously lower than that of the steel sheet without the pre-coated layer.

[0012] In addition, the temperature and time process window of the conventional hot forming process is narrow, and the requirements for actual industrial production are relatively high.

[0013] For example, CN 10646697 B (hereinafter referred to as Patent Document 2) discloses another hot stamping forming process of Al-Si plating layer precoated steel sheet, clarifying a heating and keeping process of 900-950°C for 2.5-10 minutes, preferably with a heating furnace temperature of 935-950°C or 945-950°C, and a preferred residence time of 2.5-5 minutes. Although the heating and keeping process in Patent Document 2 is slightly higher than that in Patent Document 1, in actual production, the heating and keeping process in Patent Document 2 leads to excessive enlargement of the austenite grains of the steel sheet substrate, resulting in less than ideal fracture performance, making it difficult to apply to car body parts.

[0014] As described above, the conventional hot forming process cannot simultaneously improve the alloying degree of the precoat layer and the rupture performance of the steel sheet substrate, and in particular, the rupture performance of the precoated steel sheet still needs to be strongly improved so as to meet the rupture performance standards of the automobile industry. In addition to the conventional hot forming process, it is also advantageous for practical industrial production to expand the window of the hot forming process. Summary of the Invention [Problem to be solved by the invention]

[0015] Therefore, the object of the present invention is to provide a hot stamping method for solving the bottleneck problem of the above technology, improving the degree of alloying of the precoat layer of the hot stamping steel sheet, improving the fracture performance of the hot stamping steel sheet, or simultaneously improving the degree of alloying of the precoat layer and the fracture performance of the hot stamping steel sheet. Another object of the present invention is to expand the temperature and time process interval of the hot stamping process and improve the stability of the hot stamping process. [Means for solving the problem]

[0016] The inventors have found that the above object can be effectively achieved by subjecting the pre-coated steel sheet to a pre-heat treatment prior to hot stamping, which mainly includes a heating and keeping step and a cooling step.

[0017] In addition, the present invention provides a hot stamping method including hot stamping a pre-coated steel sheet using a die at a hot stamping temperature to obtain a hot stamped member, The method further includes pre-heat treating the pre-coated steel sheet before hot stamping, the pre-heat treatment being (1) Heating and keeping the precoated steel sheet at 850 to 920°C and keeping it at that temperature for 7 to 15 minutes, or at 920 to 960°C and keeping it at that temperature for 5 to 10 minutes, so that the precoated steel sheet base material is austenitized and the precoat layer is alloyed; (2) After the heating and keeping step is completed, the pre-coated steel sheet is cooled to 300°C or less at a cooling rate of 5°C / s or more; and (3) There is provided a hot stamping method for pre-coated steel sheet, which includes optionally repeating the above heating, keeping at a constant temperature, and cooling steps one or more times.

[0018] In one embodiment of the present invention, the precoated steel sheet substrate further contains, in addition to iron element, by weight percent, 0.2 to 0.4% carbon, 0.5 to 1.5% manganese, 0 to 0.005% boron, 1% or less of one or more alloy elements selected from aluminum, silicon, chromium, molybdenum, niobium, and vanadium, and other unavoidable impurity elements.

[0019] In another embodiment of the present invention, the precoated steel sheet substrate further contains, in addition to iron element, by weight %, 0.3 to 0.5% carbon, 0.5 to 2.5% manganese, 0 to 0.005% boron, 3% or less of one or more alloy elements selected from aluminum, silicon, chromium, molybdenum, niobium, and vanadium, and other unavoidable impurity elements.

[0020] Increasing the content of carbon, manganese, and silicon can increase the hardening capacity of the steel plate substrate, and can more easily obtain martensite after the pre-heat treatment, thereby realizing the effect of refining the crystal grains. However, if the content of carbon, manganese, and silicon is too high, it will have a negative effect on the fracture performance of the steel plate substrate. Adding a very small amount of boron can increase the hardening capacity of the steel plate substrate without affecting the fracture performance. Aluminum can deoxidize during the smelting process and protect the effectiveness of boron at the same time. Other elements such as chromium and molybdenum can also increase the hardening capacity, but disadvantageously, they can greatly increase the cost of the steel plate. Vanadium and niobium can refine the austenite grains on the one hand, and produce a precipitation strengthening effect on the other hand, which can increase the strength of the hot stamping formed member. As a preferred example, the pre-coated steel plate substrate can be selected and used from those commercially available as 22MnB5 steel or 34MnB5 steel.

[0021] In an embodiment of the present invention, the precoated steel sheet substrate has a thickness of 0.8-2.5 mm, and the precoat layer has a thickness of 6-36 μm. In some embodiments, the precoat layer has a thickness of 15-27 μm. In some specific embodiments, the precoated steel sheet substrate has a thickness of 1.0-1.3 mm, which is a typical thickness of steel sheets for vehicle safety components.

[0022] In some embodiments of the present invention, the precoat layer is aluminum or an aluminum alloy, the precoat layer is disposed on at least one surface of the precoated steel sheet, and the initial thickness of the precoat layer on each surface is less than 36 μm.

[0023] In some specific embodiments, the precoat layer is an Al-Si alloy plating layer, which typically contains, by weight, 8-11% Si, 2-4% Fe, 85-90% Al, and unavoidable impurities. Al mainly provides high temperature stability and oxidation resistance of the plating layer, but disadvantageously, Al alloys with the steel sheet substrate at high temperature to form brittle intermetallic compounds, while Si can inhibit the growth of the intermetallic compounds and reduce the harm of the brittle intermetallic compounds to the fracture performance of the steel sheet.

[0024] As an example, a commercially available 22MnB5 steel precoated with an Al-Si plating layer can be used, in which the C content, expressed in weight percent, of the 22MnB5 steel sheet substrate is 0.20-0.23%, the Mn content is 0.9-1.4%, the Si content is 0.20-0.28%, and the thickness of the precoated Al-Si plating layer is about 25 μm.

[0025] In a preferred embodiment, when the thickness of the precoat layer is less than 20 μm, the heating and maintaining step is performed at 850 to 920° C. for 7 to 15 minutes, and when the thickness of the precoat layer is 20 μm or more, the heating and maintaining step is performed at 920 to 960° C. for 5 to 10 minutes. In some embodiments, the precoat layer is an Al-Si plating layer, and when the thickness of the Al-Si plating layer is less than 20 μm, the maintaining temperature range is 870 to 915° C. and the total time is 2 to 7 minutes, and when the thickness of the Al-Si plating layer is 20 μm or more, the maintaining temperature range is 890 to 935° C. and the total time is 4 to 9 minutes.

[0026] The selection of the heating and heat-retention process in the pre-heat treatment process is mainly to ensure the alloying of the coating layer and obtain a suitable intermetallic compound structure. When the pre-coat layer is aluminum or an aluminum alloy, the intermetallic compound contains FeAl phase with a volume fraction of 60% or more. Compared with other intermetallic compounds, FeAl phase has the advantages of a higher melting point and good fracture toughness, which can reduce die wear and simultaneously reduce cracks in the coating layer and improve the fracture performance and corrosion resistance of the steel sheet.

[0027] In addition, the adverse effects of austenite growth in the steel sheet substrate during the preliminary heat treatment can be eliminated or mitigated by the martensite or bainite structure obtained after cooling. The martensite or bainite structure can provide more austenite nucleation sites and refine the austenite structure so as to improve the fracture performance of the steel sheet substrate during the subsequent hot stamping. Therefore, the process range of the preliminary heat treatment of the present invention is wider than that of the conventional hot stamping process, which is advantageous in improving the process stability.

[0028] The cooling rate in the preliminary heat treatment mainly depends on the quench hardenability of the steel sheet substrate. In particular, it should be pointed out that a cooling rate of about 5°C / s cannot completely avoid the formation of carbides, and it is not possible to obtain a microstructure that is entirely martensite or bainite. However, the inventors have found that a small amount of martensite or bainite microstructure (30% or more, or the sum of the volume fractions of both is 30% or more) can also play a role in refining the austenite grains in the subsequent hot stamping forming process. At the same time, the uniformly distributed carbides can also provide a large amount of austenite nucleation sites during the heating process, and play a role in refining the austenite grains.

[0029] Preferably, the cooling rate is 10°C / s or more, in which case the martensite volume fraction after cooling can reach 50% or more, without forming pearlite, and the carbide particle size is 0.1 μm or less. More preferably, the cooling rate is 25°C / s or more, in which case the martensite volume fraction after cooling is close to 100%. However, when the cooling rate is increased to 50°C / s, the effect of further refining the austenite grains is not obvious, and the fracture performance after the subsequent hot stamping is hardly further improved. Therefore, optimally, the cooling rate is 25°C / s to 50°C / s.

[0030] In actual production process, it takes a long time to cool the steel plate after the above pre-heat treatment to room temperature, and the cooling rate is extremely slow especially below 200°C. In order to improve production efficiency, as a preferred embodiment, when the steel plate is cooled to 300°C or below or 200°C or above after the pre-heat treatment step, the steel plate is transferred to a heating furnace and reheating is started. In this case, the transformation to martensite during the cooling process is all or almost complete, and the austenite grains are refined to a sufficient extent to improve the final rupture performance of the steel plate.

[0031] Preferably, the steel sheet can be deformed through the stamping die during the cooling process of the preliminary heat treatment. On the one hand, it can reduce the deformation amount in the subsequent hot stamping forming process, reduce the temperature requirement in the subsequent hot stamping forming process, and make the window of the heating and keeping process in the subsequent hot stamping forming process larger. On the other hand, the heating and keeping in the subsequent hot stamping forming process can fill the cracks in the coating layer caused by the preliminary deformation, and at the same time, the deformation amount required in the subsequent hot forming process can be reduced, thereby reducing the number and depth of the cracks in the coating layer, and further improving the corrosion resistance of the precoat layer and reducing the adverse effect of the cracks in the coating layer on the fracture performance.

[0032] Preferably, the steel sheet is pre-heated multiple times, and the same or different process parameters can be used during the multiple pre-heat treatments. The reciprocating transformation between high-temperature austenite and room-temperature martensite can enhance the degree of grain refinement. At the same time, the adoption of different process parameters during the multiple pre-heat treatments can provide more possibilities for designing the Fe-Al diffusion layer and intermetallic compound layer in the pre-coat layer (e.g., Al-Si plating layer). Therefore, after multiple pre-heat treatments, the chemical composition and microstructure of the steel sheet substrate are more uniform, the grains are more refined, and the degree of alloying of the pre-coat layer is higher.

[0033] In addition, the adverse effects of austenite growth in the steel substrate during the preliminary heat treatment process can be eliminated or mitigated by the martensite or bainite structure obtained after cooling. The martensite or bainite structure can provide more austenite nucleation sites and refine the austenite structure so as to improve the fracture performance of the steel substrate during the subsequent hot stamping. Therefore, the process range of the preliminary heat treatment of the present invention is wider than that of the conventional hot stamping process, which is advantageous in improving the process stability.

[0034] According to the hot stamping forming method for pre-coated steel plate provided by the present invention, the microstructure of the pre-coated steel plate substrate after preliminary heat treatment is: (a) The volume fraction of martensite or bainite or the sum of both is 30% or more, (b) It is characterized in that there are no spherical carbide particles having a particle size exceeding 0.5 μm, and there are no sheet-like pearlite regions having a particle size exceeding 1 μm.

[0035] Here, the microstructure of the precoat layer after the preliminary heat treatment is composed of ferrite and one or more intermetallic compounds in which the volume fraction of the FeAl phase in all intermetallic compounds is 60% or more.

[0036] In some embodiments of the present invention, the hot stamping forming method further includes, after the preliminary heat treatment, reheating the pre-coated steel sheet to 780 to 940°C and keeping the temperature for 1 to 7 minutes so as to completely austenitize the pre-coated steel sheet substrate, and then transferring the pre-coated steel sheet to a mold while maintaining a temperature of 500°C or higher, and performing hot stamping forming.

[0037] Preferably, the hot stamping forming method further includes, after the preliminary heat treatment, reheating the precoated steel sheet to 830 to 900°C and keeping the temperature for 1 to 4 minutes so as to completely austenitize the precoated steel sheet substrate, and then transferring the precoated steel sheet to a mold while maintaining a temperature of 600°C or higher, and performing hot stamping forming.

[0038] Preferably, in the reheating step, the temperature is maintained in the range of 830 to 900° C., and the total heating and maintaining time is 1 to 4 minutes.

[0039] More importantly, with the refinement of prior austenite grains in the hot stamping steel, the martensite slat bundles, slat chunks and slats are refined, which ultimately improves the fracture performance of the hot stamping formed parts.

[0040] In some embodiments of the present invention, the microstructure of the pre-coated steel sheet substrate after hot stamping is a full martensitic structure.

[0041] In some other embodiments of the present invention, the microstructure of the precoated steel sheet substrate after hot stamping is a mixed structure consisting of two or more phases selected from the group consisting of ferrite, bainite, martensite, and austenite. In this case, the strength of the hot stamped member is reduced and the fracture performance is improved.

[0042] Furthermore, the prior austenite grain size of the microstructure of the pre-coated steel sheet substrate after hot stamping does not exceed 18 μm. In a preferred embodiment, the prior austenite grain size in the microstructure of the hot stamping formed part does not exceed 10 μm. In this case, the grain refinement is higher, so that the fracture performance of the hot stamping formed steel is better.

[0043] The microstructure of the above hot stamping steel sheet substrate is usually an all martensite structure, in which case the strength of the hot stamping steel can reach 1.5 GPa.

[0044] In some embodiments of the present invention, after the preliminary heat treatment, the steel sheet is transferred to a heating furnace to be reheated and hot stamping formed. In a preferred embodiment, after the preliminary heat treatment step, the steel sheet is transferred to a heating furnace and reheating begins when the steel sheet is cooled to 300°C or less and 200°C or more. In this case, the transformation to martensite during the cooling process is all or almost complete, and the austenite grains are refined to perform a sufficient function of improving the final rupture performance of the steel sheet. By transferring the steel sheet to a heating furnace at 200°C or more, production efficiency can be improved and energy can be saved.

[0045] In another preferred embodiment, after the preliminary heat treatment step, the steel sheet is transferred to a heating furnace and reheating is started when the steel sheet is cooled to 200° C. or less and 100° C. or more. This embodiment is more suitable than the above embodiment when the precoated steel sheet substrate has a high alloy content and a low martensite transformation temperature.

[0046] The reason why the hot stamping method of the present invention can refine the prior austenite grains is mainly related to the following factors: (A) In the heating and keeping process of the preliminary heat treatment, the precoat layer has already been alloyed and formed an intermetallic compound layer and a diffusion layer, and the alloying of the precoat layer does not need to be the main consideration in the hot stamping process, so a relatively low heating and keeping temperature and a relatively short heating and keeping time can be adopted to suppress the growth of austenite grains; (B) In the cooling process of the preliminary heat treatment, the steel plate substrate forms a complete or partial martensite or bainite structure, which has the characteristics of fine grains, high defect density, etc., and the distribution of carbides in the steel plate substrate is finer and more uniform, which provides more austenite nucleation sites in the reheating process of the hot stamping process, and finally refines the prior austenite grains.

[0047] The reason why the technology of the present invention improves the fracture performance is as follows: The hot stamping technology of the present invention can refine the prior austenite grains, martensite slat bundles, martensite slat chunks and martensite slats in the microstructure of the hot stamping formed member. On the one hand, the refinement of the grains reduces the concentration of impurity elements such as phosphorus and sulfur and hydrogen elements at the grain boundaries, and alleviates the adverse effects of impurity elements and hydrogen elements on grain boundary fracture, thereby suppressing brittle grain boundary fracture. On the other hand, due to the refinement of the grains, the crack needs to pass through more high-angle grain boundaries during the expansion process, including prior austenite grain boundaries, martensite slat bundle interfaces, martensite slat chunk interfaces, etc., so that the crack expansion requires more energy and is more difficult, and finally improves the fracture performance of the hot stamping formed member.

[0048] Therefore, according to the hot stamping method provided by the present invention, the pre-heat treatment can increase the degree of alloying of the pre-coat layer, reduce the carbide structure in the steel plate substrate, and obtain a martensite and / or bainite substrate structure, thereby reducing the wear of the pre-coat layer against the stamping die during high-temperature stamping deformation, refine the crystal grains, and improve the fracture performance of the final hot stamped part.

[0049] The hot stamping molding method of the present invention can be used for automobile safety structures, reinforcement structures, wheel components, high-strength automobile structures, etc., including, but not limited to, the A-pillars, B-pillars, back top cross beams, etc. of automobile white body.

[0050] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. [Brief description of the drawings]

[0051] [Figure 1] FIG. 1 is a schematic diagram of a conventional hot stamping molding method. [Diagram 2]FIG. 2 is a schematic diagram of the hot stamping molding method of the present invention. [Diagram 3] FIG. 3 is a diagram showing the initial microstructure of the precoat layer and the steel sheet substrate of the 22MnB5 steel sheet used in the examples. [Figure 4] FIG. 4 is a schematic diagram of the microstructure of the Al—Si plating layer after the preliminary heat treatment in Examples 1 to 3 of the present invention. [Diagram 5] FIG. 5 is a graph showing the change in the total volume fraction ratio value of the FeAl phase and the intermetallic compound in the precoat layer after the preliminary heat treatment with respect to the heat retention time in Examples 1 to 3 of the present invention. [Figure 6] FIG. 6 is a microstructure diagram of the steel sheet substrate after the preliminary heat treatment in Example 2 of the present invention. [Figure 7] FIG. 7 is a microstructure diagram of the steel sheet substrate after hot stamping in Example 4 of the present invention. [Figure 8] FIG. 8 is an inverse pole figure of the microstructure of the steel sheet substrate after hot stamping in Example 4 of the present invention. [Figure 9] FIG. 9 is an inverse pole figure of the microstructure of a steel sheet substrate after hot stamping using conventional technology. [Figure 10] FIG. 10 is a graph showing a comparison between the three-point bending test results of Example 4 of the present invention and the precoated hot stamping formed steel sheet obtained by the prior art. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0052] The present invention will be described in more detail below based on specific embodiments. The embodiments provided are provided only to illustrate the present invention, without limiting the scope of the present invention.

[0053] In order to specifically explain the hot stamping method of the present invention, an embodiment of the hot stamping method of the present invention and a conventional hot stamping method are shown together in Figures 1 and 2. Note that the present invention is not limited to the embodiment shown in the figures, and the slope in the figure is merely used to explain the average heating or cooling rate, and does not represent the actual heating or cooling curve.

[0054] The precoat Al-Si layer of the 22MnB5 steel sheet used in the examples and the original microstructure of the steel sheet substrate are shown in FIG. 3. Here, the precoat layer is, in order from the steel sheet substrate side, a Si-rich intermetallic compound layer and an Al layer. This precoat Al-Si plating layer structure is a typical precoat plating layer structure of commercially available 22MnB5 steel. The steel sheet substrate mainly consists of ferrite, pearlite, and carbides. Of these, the size of the sheet-like pearlite region can be 2 μm or more, and the particle size of the spherical carbide can be 0.5 μm or more. EXAMPLES

[0055] Examples 1 to 3 The precoated 22MnB5 steel sheet was subjected to the following preliminary heat treatment. (1) The three precoated steel plates were heated to 930°C and kept at that temperature for 1 minute (Example 1), 5 minutes (Example 2), and 10 minutes (Example 3), respectively, to austenitize the precoated steel plate substrate and alloy the precoat layer. (2) After the heating and keeping step was completed, the steel plate was cooled to room temperature at a cooling rate of 300° C. / s.

[0056] After the preliminary heat treatment, the Al-Si plating layer in the above steel sheet was alloyed, and its microstructure became as shown in Figure 4. From the steel sheet substrate side, there was an Fe-Al diffusion layer mainly containing ferrite structure, and an intermetallic compound layer mainly containing FeAl and Fe2Al5. However, the thickness of the Fe-Al diffusion layer was 4 to 30 μm, and the thickness of the intermetallic compound layer was 15 to 40 μm.

[0057] Figure 5 shows the change in the total volume fraction ratio of the FeAl phase and intermetallic compounds with the temperature retention time. FeAl has a higher melting point and fracture toughness than the Fe2Al5 phase, and can reduce the adverse effects of problems such as scale adhesion to the furnace rollers and die wear. In this example, the volume fraction of the FeAl phase in the entire Fe-Al intermetallic compounds was 60% or more.

[0058] As shown in FIG. 6, the microstructure of the steel plate substrate after the preliminary heat treatment in Example 2 had no spheroidal carburized particles having a particle size of more than 0.5 μm, no sheet-like pearlite regions having a particle size of more than 1 μm, and the volume fraction of martensite or bainite, or the sum of the volume fraction of both, was 30% or more.

[0059] Through multiple parallel tests, it has become clear that although the cooling rate and temperature of this example are not within the optimum range of the present invention, this does not affect the microstructure and conclusion of this example. That is, the microstructure and conclusions obtained in the optimum cooling rate range and temperature range of the present invention are almost similar to those of the above examples. However, the range of these optimum conditions is more favorable for industrial production.

[0060] Example 4 The steel plate obtained in Example 2 was reheated and hot stamped. (3) The steel plate was reheated to 850° C. and held at that temperature for a total time of 1.5 minutes to fully austenitize the steel plate. (4) The heated steel plate was transferred to the mold so as to ensure that the temperature of the heated steel plate was above 500°C when transferred to the mold. (5) The heated steel plate was subjected to hot stamping in the die to obtain a final hot stamped steel part.

[0061] FIG. 7 shows the microstructure of the steel sheet substrate after the hot stamping process. After hot stamping, the steel sheet substrate obtains a martensite structure, and the prior austenite grains in the microstructure are significantly refined, and the prior austenite grain size is reduced from 15-25μm after pre-heat treatment to 3-8μm after hot stamping. At the same time, the alloying degree and microstructure of the Al-Si coating layer no longer change obviously because the hot stamping process adopts a relatively low temperature and a relatively short heat retention time.

[0062] FIG. 8 is an inverse pole figure of the microstructure of the steel sheet substrate after the hot stamping process, in which the prior austenite grain size in the microstructure of the steel sheet substrate, which corresponds to the prior austenite grain size of 3 to 8 μm observed in FIG. 7, is more clearly observed.

[0063] For comparison, FIG. 9 is a microstructure inverse pole figure of the steel plate substrate obtained by using the conventional hot stamping forming technology shown in FIG. 2. Here, the prior austenite grain size is about 20 μm. The conventional hot stamping forming process does not undergo preliminary heat treatment, and a relatively high heating and holding temperature and a relatively long heating and holding time, for example, 900-940°C, 5-10 minutes, must be adopted. In addition, the initial microstructure of the conventional hot stamping forming process is a ferrite + sheet-like pearlite + globular carbide structure, and the martensite or bainite structure cannot play the role of refining the austenite grains. Therefore, the prior austenite grains in the steel plate substrate obtained by the conventional hot stamping forming process are much larger than those of the hot stamping forming process of the present invention.

[0064] FIG. 10 compares the three-point bending test results of the steel sheet after hot stamping formed by the conventional hot stamping method and the method of the present invention. The three-point bending test results of the steel sheet after hot stamping formed can embody the fracture performance of the hot stamping formed member. The three-point bending test results show that the steel sheet after hot stamping formed by the technology of the present invention can achieve a larger bending load and a larger bending angle than the conventional hot stamping forming technology, among which the technology of the present invention can achieve a maximum bending load of about 1100N and a bending angle of about 58.4°, while the conventional technology can only achieve a maximum bending load of about 1000kN and a bending angle of about 52.2°, that is, the maximum bending load is improved by 10% and the bending angle is improved by 11.9% at the same time. Therefore, the three-point bending performance of the steel sheet after hot stamping formed by the method of the present invention is better, and the fracture performance of the hot stamping formed member is also better accordingly.

[0065] As can be seen from the above examples, the method of the present invention can simultaneously improve the alloying degree of the precoat layer and the fracture performance of the steel plate substrate. The reasons for improving the fracture performance of the steel plate substrate are as follows: The hot stamping forming technology of the present invention can distribute carbon elements more uniformly in the substrate, and refine the prior austenite grains, martensite slat bundles, martensite slat clusters and martensite slats in the microstructure of the hot stamping formed member. On the one hand, the refinement of the grains reduces the concentration of impurity elements such as phosphorus and sulfur and hydrogen elements at the grain boundaries, and alleviates the adverse effects of impurity elements and hydrogen elements on the grain boundary fracture, thereby suppressing brittle grain boundary fracture. On the other hand, due to the refinement of the grains, the crack needs to pass through more high-angle grain boundaries during the expansion process, including prior austenite grain boundaries, martensite slat bundle interfaces, martensite slat cluster interfaces, etc., so that the crack expansion requires more energy and is more difficult, and finally improves the fracture performance of the hot stamping formed member.

[0066] The above description of the examples is provided for the purpose of illustration and description. It should be clear to those skilled in the art that the present invention is not limited to these examples or experimental data. The data and various parameters described in the examples are merely illustrative and do not constitute limitations on the present invention.

Claims

1. A hot stamping method comprising: hot stamping a precoated steel sheet using a die at a hot stamping temperature to obtain a hot stamped part, The method further includes pre-heat treating the pre-coated steel sheet before hot stamping, the pre-heat treatment being (1) Heating and keeping the precoated steel sheet at 850-920°C and keeping it at that temperature for 7-15 minutes, or at 920-960°C and keeping it at that temperature for 5-10 minutes, so that the precoated steel sheet base material is austenitized and the precoat layer is alloyed; (2) After the heating and maintaining step is completed, the pre-coated steel sheet is cooled to 300°C or less at a cooling rate of 5°C / s or more; and (3) A hot stamping forming method for pre-coated steel sheet, which comprises optionally repeating the above heating and cooling steps one or more times.

2. The pre-coated steel sheet substrate further contains, in addition to the iron element, 0.2 to 0.4% by weight of carbon, 0.5 to 1.5% by weight of manganese, 0 to 0.005% by weight of boron, 1% or less of one or more alloy elements selected from aluminum, silicon, chromium, molybdenum, niobium, and vanadium, and other unavoidable impurity elements; or The precoated steel sheet substrate further contains, by weight percent, 0.3 to 0.5% carbon, 0.5 to 2.5% manganese, 0 to 0.005% boron, 3% or less of one or more alloy elements selected from aluminum, silicon, chromium, molybdenum, niobium, and vanadium, and other unavoidable impurity elements; The hot stamping method according to claim 1, wherein the thickness of the pre-coated steel sheet substrate is preferably 0.8 to 2.5 mm.

3. The hot stamping forming method according to claim 1, wherein the precoat layer is aluminum or an aluminum alloy, preferably an aluminum alloy, more preferably an Al-Si alloy, and preferably the thickness of the precoat layer is 6-36 μm, more preferably 15-27 μm.

4. 4. The hot stamping molding method according to claim 1, wherein the heating and keeping step is performed at 850 to 920°C for 7 to 15 minutes when the thickness of the precoat layer is less than 20 μm, and at 920 to 960°C for 5 to 10 minutes when the thickness of the precoat layer is 20 μm or more.

5. the cooling rate is 10° C. / s or more, more preferably the cooling rate is 25° C. / s or more, and most preferably the cooling rate is 25° C. / s to 50° C. / s; The hot stamping method according to any one of claims 1 to 3, wherein the pre-coated steel sheet is deformed by a stamping die during the cooling process in step (2).

6. The microstructure of the pre-coated steel sheet substrate after the preliminary heat treatment is (a) The volume fraction of martensite or bainite or the sum of both is 30% or more; (b) the hot stamping method according to any one of claims 1 to 3, characterized in that there are no spherical carbide particles having a particle size exceeding 0.5 μm, and there are no sheet-like pearlite regions having a particle size exceeding 1 μm.

7. 4. The hot stamping method according to claim 1, wherein the microstructure of the precoat layer after the preliminary heat treatment is composed of ferrite and one or more intermetallic compounds in which the volume fraction of FeAl phase in all intermetallic compounds is 60% or more.

8. The method further includes, after the preliminary heat treatment, reheating the pre-coated steel sheet to 780 to 940°C and holding the temperature for 1 to 7 minutes so as to completely austenitize the pre-coated steel sheet substrate, and then transferring the pre-coated steel sheet to a mold and hot stamping forming the pre-coated steel sheet while maintaining a temperature of 500°C or higher; Preferably, the method further comprises, after the preliminary heat treatment, reheating the pre-coated steel sheet to 830-900°C and keeping the temperature for 1-4 minutes so as to completely austenitize the pre-coated steel sheet substrate, and then transferring the pre-coated steel sheet to a die while maintaining a temperature of 600°C or higher, and performing hot stamping. The hot stamping method according to any one of claims 1 to 3.

9. The microstructure of the precoated steel sheet substrate after hot stamping is a full martensite structure, or 4. The hot stamping method according to claim 1, wherein the microstructure of the precoated steel sheet substrate after hot stamping is a mixed structure consisting of two or more phases selected from the group consisting of a ferrite structure, a bainite structure, a martensite structure, and an austenite structure.

10. The hot stamping method according to any one of claims 1 to 3, wherein the prior austenite grain size of the pre-coated steel sheet substrate microstructure after hot stamping does not exceed 18 μm, preferably does not exceed 10 μm.

Citation Information

Patent Citations

  • Hot stamped components, pre-coated steel sheets used for hot stamping and the hot stamping process

    JP2020524211A

  • Hot press member and method for producing the same

    JP2021179002A

  • Highly productive method for manufacturing press-hardened parts

    JP2021517204A

  • Steel for hot press forming having excellent formability and method for manufacturing the same

    KR1020140084872A

  • Hot stamp molded body and method for producing same

    WO2018134874A1