Insulating layer composition for lithium secondary battery and lithium secondary battery including same
The use of a conjugated diene copolymer and non-aqueous solvent in the insulating layer composition for lithium secondary batteries addresses insulation and adhesion issues, enhancing battery safety by preventing short circuits and maintaining insulation properties.
Patent Information
- Application Number
- JP2024520042
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-04
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2043-04-04
AI Technical Summary
Conventional separators in lithium secondary batteries face limitations in maintaining electrical insulation under abnormal conditions, leading to potential short circuits and thermal runaway due to insufficient heat resistance and adhesion issues with existing insulating methods, which can compromise battery safety.
An insulating layer composition for lithium secondary batteries using a conjugated diene copolymer as a binder polymer and a non-aqueous organic solvent is applied to form a flexible and insulating layer on the positive electrode tab, allowing simultaneous coating with the positive electrode mixture layer, enhancing adhesion and preventing short circuits.
The insulating layer composition effectively prevents separator shrinkage and electrode bending, maintaining insulation properties and electrolyte resistance, thereby reducing the risk of physical short circuits and improving battery safety.
Smart Images

Figure 2024538871000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an insulating layer composition for a lithium secondary battery and a lithium secondary battery including the same. [Background technology]
[0002] As technological development and demand for mobile devices increases, the demand for secondary batteries as an energy source is growing rapidly, and accordingly, much research is being conducted on batteries that can meet various needs.
[0003] Typically, in terms of battery shape, there is high demand for thin rectangular and pouch-shaped batteries that can be used in products such as mobile phones, and in terms of materials, there is high demand for lithium secondary batteries such as lithium-cobalt polymer batteries, which have excellent energy density, discharge voltage, and safety.
[0004] One of the main research topics for such secondary batteries is to improve their safety. The main cause of safety-related accidents in batteries is the reaching of abnormally high temperatures due to short circuits between the positive and negative electrodes. In other words, under normal circumstances, a separator is located between the positive and negative electrodes to maintain electrical insulation, but in abnormal abuse situations such as when the battery is overcharged or overdischarged, internally short-circuited by dendritic growth of the electrode material or foreign matter, pierced by sharp objects such as nails or screws, or subjected to excessive deformation due to external forces, the conventional separator alone shows its limitations.
[0005] Generally, microporous membranes made of polyolefin resin are mainly used as separators, but their heat resistance is insufficient, with a heat resistance of about 120 to 160°C. Therefore, when an internal short circuit occurs, the separator shrinks due to the short circuit reaction heat, expanding the short circuit area, leading to a thermal runaway state in which a larger amount of reaction heat is generated. Therefore, various methods have been studied to reduce the possibility of cell deformation, external impact, or physical short circuit between the positive and negative electrodes.
[0006] For example, in order to prevent a short circuit caused by the electrode tab coming into contact with the upper end of the electrode assembly due to the movement of the electrode assembly in a completed battery, a method is used in which insulating tape of a predetermined size is attached to the electrode tab adjacent to the upper end of the current collector. However, the winding of such insulating tape is very cumbersome, and if the insulating tape is wound up to a length that extends slightly downward from the upper end of the current collector, such a portion may cause an increase in the thickness of the electrode assembly. Furthermore, there is a problem that the electrode tab is easily loosened when it is bent.
[0007] There is also a method of forming an insulating layer on the tab portion of the positive electrode using a non-aqueous binder (such as PVDF) or an aqueous styrene butadiene copolymer (SBL). However, when a non-aqueous binder (such as PVDF) is used, there is a problem that the wet adhesion is reduced and the migration of lithium ions cannot be prevented in the overlay region of the electrode, resulting in the development of capacity. In particular, when the capacity is developed in the overlay region of the electrode, lithium ions may be precipitated, which may result in a decrease in the stability of the battery cell. In addition, when an aqueous styrene butadiene copolymer (SBL) binder is used, when it is simultaneously coated with the slurry for the positive electrode mixture layer, there is a problem that the battery performance is reduced due to gelation of PVDF, which is an organic binder used as the positive electrode binder, the boundary penetration of the positive electrode slurry into the insulating liquid, and side reactions due to moisture, and simultaneous coating of the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer is impossible.
[0008] Therefore, there is a strong need to develop an insulating liquid that allows for simultaneous coating of a slurry for a positive electrode mixture layer and a slurry for an insulating coating layer while simultaneously satisfying the requirements for flexibility, insulating properties, and electrolyte resistance. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Korean Patent No. 10-1586530 Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide an insulating layer composition for a lithium secondary battery that can perform insulating liquid coating simultaneously with positive electrode coating by replacing water, which is a dispersion solvent for an aqueous conjugated dienes copolymer latex, with a non-aqueous organic solvent (e.g., N-methyl-pyrrolidone).
[0011] Another object of the present invention is to provide a method for producing a positive electrode for a lithium secondary battery using the insulating layer composition for a lithium secondary battery.
[0012] Another object of the present invention is to provide a positive electrode for a lithium secondary battery formed from the insulating layer composition for a lithium secondary battery.
[0013] Another object of the present invention is to provide a lithium secondary battery including the above-mentioned positive electrode for a lithium secondary battery.
[0014] Other objects and advantages of the present invention will be more clearly set forth in the following detailed description of the invention and the appended claims. [Means for solving the problem]
[0015] In order to achieve the above technical objectives, the present invention provides an insulating layer composition for a lithium secondary battery, comprising a conjugated diene copolymer as a binder polymer and a non-aqueous organic solvent as a dispersion solvent, the conjugated diene copolymer having a Tg of -10°C to 40°C.
[0016] In addition, the present invention provides a method for manufacturing a positive electrode for a lithium secondary battery, the method including the steps of: preparing a water-dispersed conjugated diene latex; adding a non-aqueous organic solvent to the water-dispersed conjugated diene latex, and heating and reducing pressure to prepare a slurry for an insulating coating layer; coating a slurry for a positive electrode mixture layer, the slurry including a positive electrode active material, a conductive material, and a non-aqueous binder, on one or both sides of a positive electrode current collector; coating the slurry for the insulating coating layer from a portion of an uncoated portion of the positive electrode current collector to cover a portion of the slurry for the positive electrode mixture layer coated on the current collector; and drying the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer coated on the positive electrode current collector.
[0017] The present invention also provides a positive electrode for a lithium secondary battery, comprising a positive electrode current collector, a positive electrode tab protruding from the positive electrode current collector, and an insulating layer formed by coating an insulating material on the positive electrode tab, the insulating material comprising the insulating layer composition for a lithium secondary battery according to the present invention.
[0018] The present invention also provides a lithium secondary battery including the positive electrode for a lithium secondary battery. Effect of the Invention
[0019] According to one embodiment of the present invention, by forming an insulating layer that simultaneously satisfies flexibility, insulating properties, and electrolyte resistance properties on the tab portion of the positive electrode, it is possible to prevent a physical short circuit between the positive electrode and the negative electrode when defects such as separator shrinkage and electrode breakage occur in a lithium secondary battery.
[0020] According to one embodiment of the present invention, by providing a slurry for an insulating coating layer in which water, which is a dispersion solvent for conjugated diene latex particles used in forming an insulating layer, is replaced with a non-aqueous organic solvent (e.g., N-methyl-pyrrolidone), it is possible to perform insulating liquid coating simultaneously with positive electrode coating.
[0021] The effects of the present invention are not limited to the above-mentioned examples, and more diverse effects are included in the present specification. [Brief description of the drawings]
[0022] [Figure 1] FIG. 13 is a diagram showing the results of evaluating brittleness according to Experimental Example 4. [Diagram 2] FIG. 13 is a diagram showing the results of evaluating the influence of moisture according to Experimental Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The present invention will be described in detail below.
[0024] All terms used in this specification (including technical and scientific terms) may be used in the sense commonly understood by those having ordinary skill in the art to which the present invention belongs, unless otherwise defined. Furthermore, terms defined in commonly used dictionaries are not to be interpreted ideally or excessively, unless clearly and specifically defined.
[0025] Throughout this specification, when a part is said to "comprise" certain elements, this should be understood as an open-ended term that does not exclude other elements, but rather includes the possibility of further including other elements, unless specifically stated to the contrary.
[0026] As used herein, "preferred" and "preferably" refer to embodiments of the invention that may provide certain advantages, under certain circumstances. However, other embodiments may also be preferred, under the same or different circumstances. Furthermore, reference to one or more preferred embodiments does not imply that other embodiments are not useful, and is not intended to exclude other embodiments from the scope of the invention.
[0027] In the present invention, the term "insulating coating layer" refers to an insulating member formed by coating and drying from at least a portion of the uncoated portion of the electrode current collector to at least a portion of the electrode mixture layer.
[0028] In the present invention, "wet adhesion" refers to the adhesion of an insulating coating layer measured in a state where the insulating coating layer is immersed in an electrolyte. If the insulating coating layer swells or falls off in a state where the insulating coating layer is immersed in an electrolyte, the insulating properties of the electrode are difficult to maintain, and this can be confirmed by coating an insulating coating layer on an electrode specimen (electrode test specimen) and measuring the insulating properties.
[0029] In the present invention, the term "metal test piece" refers to a space in which an insulating coating layer is formed, and may refer to a metal current collector used in manufacturing an electrode, and may be a metal current collector punched to have a predetermined width and length. For example, the metal test piece may be aluminum, copper, or an aluminum alloy.
[0030] <Insulating layer composition for lithium secondary batteries>
[0031] One example of the present invention is an insulating layer composition for a lithium secondary battery, comprising a conjugated diene copolymer as a binder polymer and a non-aqueous organic solvent as a dispersion solvent, the conjugated diene copolymer having a Tg of -10°C or more and 40°C or less.
[0032] In the insulating layer composition for lithium secondary batteries according to the present invention, conjugated diene copolymer particles having an average particle size of 50 nm to 500 nm are present in an independent phase, and the conjugated diene copolymer may be contained in an amount of 20 wt% to 100 wt% based on the total solid mass of the composition. When the content of the conjugated diene copolymer is 20 wt% to 100 wt%, the conjugated diene copolymer particles can exert an insulating effect while maintaining adhesive performance even in an electrolyte, thereby providing a certain insulating effect.
[0033] The insulating layer composition may further contain inorganic particles or dyes insofar as the insulating properties are not impaired.
[0034] In one embodiment of the present invention, the inorganic particles may be alumina, boehmite, silica, titanium dioxide, and the like.
[0035] The conjugated diene copolymer may comprise (a) a conjugated diene monomer or a conjugated diene polymer, (b) one or more monomers selected from the group consisting of acrylate monomers, vinyl monomers, and nitrile monomers, and (c) a polymer of one or more monomers selected from the group consisting of unsaturated carboxylic acid monomers and hydroxyl group-containing monomers.
[0036] The conjugated diene monomer may be one monomer selected from the group consisting of 1,3-butadiene, isoprene, chloroprene and piperylene.
[0037] The conjugated diene polymer may be, for example, a polymer of two or more monomers selected from the group consisting of 1,3-butadiene, isoprene, chloroprene, and piperylene, a styrene-butadiene copolymer, an acrylonitrile-butadiene copolymer, a styrene-isoprene copolymer, an acrylate-butadiene rubber, an acrylonitrile-butadiene-styrene rubber, an ethylene-propylene-diene polymer, or a partially epoxidized or brominated polymer of these polymers, or a mixture thereof.
[0038] The acrylate monomer may be one or more monomers selected from the group consisting of methyl ethacrylate, methyl methacrylate, methacryloxyethyl ethylene urea, β-carboxyethyl acrylate, aliphatic monoacrylate, dipropylene diacrylate, ditrimethylolpropane tetraacrylate, dipentaerythriol hexaacrylate, pentaerythriol triacrylate, pentaerythriol tetraacrylate, and glycidyl methacrylate.
[0039] The vinyl monomer may be at least one monomer selected from the group consisting of styrene, α-methylstyrene, β-methylstyrene, pt-butylstyrene, and divinylbenzene.
[0040] The nitrile monomer may be at least one monomer selected from the group consisting of acrylonitrile, methacrylonitrile, and allyl cyanide.
[0041] The unsaturated carboxylic acid monomer may be at least one monomer selected from the group consisting of maleic acid, fumaric acid, methacrylic acid, acrylic acid, glutaric acid, itaconic acid, tetrahydrophthalic acid, crotonic acid, isocrotonic acid, and nadic acid, but is not limited thereto.
[0042] The hydroxy group-containing monomer may be one or more monomers selected from the group consisting of hydroxyacrylate, hydroxyethyl acrylate, hydroxybutyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate, but is not limited thereto.
[0043] The method for producing the conjugate diene copolymer particles is not particularly limited, and may be carried out by a known suspension polymerization method, emulsion polymerization method, seed polymerization method, etc. The mixture of monomers for producing the copolymer particles may contain one or more other components such as a polymerization initiator, a crosslinking agent, a coupling agent, a buffer solution, a molecular weight regulator, and an emulsifier. Specifically, the copolymer particles may be produced by an emulsion polymerization method, and in this case, the average particle size of the copolymer particles may be adjusted by the amount of an emulsifier. In general, the particle size tends to become smaller as the amount of the emulsifier increases, and the particle size tends to become larger as the amount of the emulsifier decreases. The desired average particle size can be achieved by adjusting the amount of the emulsifier used in consideration of the desired particle size, reaction time, reaction stability, etc. The polymerization temperature and polymerization time may be appropriately determined depending on the polymerization method, the type of polymerization initiator, etc. For example, the polymerization temperature may be 10°C to 150°C, and the polymerization time may be 1 to 20 hours.
[0044] The polymerization initiator may be an inorganic or organic peroxide, for example, a water-soluble initiator including potassium persulfate, sodium persulfate, ammonium persulfate, etc., or an oil-soluble initiator including cumene hydroperoxide, benzoyl peroxide, etc. In addition, an activator may be further included to promote the initiation reaction of the peroxide together with the polymerization initiator, and the activator may be at least one selected from the group consisting of sodium formaldehyde sulfoxylate, sodium ethylenediaminetetraacetate, ferrous sulfate, and dextrose.
[0045] The crosslinking agent is a substance that promotes crosslinking of the binder, and examples of the crosslinking agent include amines such as diethylene triamine, triethylene tetramine, diethylamino propylamine, xylene diamine, and isophorone diamine, dodecyl succinic anhydride, and phthalic anhydride. Examples of suitable grafting agents include acid anhydrides such as aryl methacrylate, polyamide resins, polysulfide resins, phenolic resins, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, neopentyl glycol dimethacrylate, trimethylolpropane trimethacrylate, trimethylolmethane triacrylate, and glycidyl methacrylate. Examples of suitable grafting agents include aryl methacrylate (AMA), triaryl isocyanurate (TAIC), triarylamine (TAA), and diarylamine (DAA).
[0046] The coupling agent is a material for increasing the adhesive strength between the active material and the binder, and is characterized by having two or more functional groups, one of which reacts with a hydroxyl group or a carboxyl group on the surface of the silicon, tin or graphite-based active material to form a chemical bond, and the other functional group is a material that forms a chemical bond through a reaction with the nanocomposite according to the present invention, and is not particularly limited. For example, silane-based coupling agents such as triethoxysilylpropyl tetrasulfide, mercaptopropyl triethoxysilane, aminopropyl triethoxysilane, chloropropyl triethoxysilane, vinyltriethoxysilane, methacryloxypropyl triethoxysilane, glycidoxypropyl triethoxysilane, isocyanatopropyl triethoxysilane, and cyanatopropyl triethoxysilane may be used.
[0047] The buffer (buffering agent) may be, for example, one selected from the group consisting of NaHCO3, Na2CO3, K2HPO4, KH2PO4, Na2HPO4, NaOH and NH4OH.
[0048] As the molecular weight regulator, for example, mercaptans, terfins such as terpinolene, dipentene, and t-terpiene, and halogenated hydrocarbons such as chloroform and carbon tetrachloride can be used.
[0049] The emulsifier is a substance having both a hydrophilic group and a hydrophobic group. In one specific example, the emulsifier may be at least one selected from the group consisting of anionic emulsifiers and nonionic emulsifiers.
[0050] Nonionic emulsifiers, when used with anionic emulsifiers, can help control particle size and distribution and provide additional colloidal stabilization of the polymer particles through van der Waals forces in addition to the electrostatic stabilization of the ionic emulsifiers. Nonionic emulsifiers are not often used alone because they produce less stable particles than anionic emulsifiers.
[0051] The anionic emulsifier may be selected from the group consisting of phosphates, carboxylates, sulfates, succinates, sulfosuccinates, sulfonates and disulfonates. For example, the anionic emulsifier may be selected from the group consisting of sodium alkyl sulfate, sodium polyoxyethylene sulfate, sodium lauryl ether sulfate, sodium polyoxyethylene lauryl ether sulfate, sodium lauryl sulfate, sodium alkyl sulfonate, sodium alkyl ether sulfonate, sodium alkyl benzene sulfonate, sodium linear alkyl benzene sulfonate, sodium alpha olefin sulfonate, sodium alcohol polyoxyethylene ether sulfonate, sodium dioctyl sulfosuccinate, sodium perfluorooctane sulfonate, sodium perfluorobutane sulfonate, alkyl diphenyloxide disulfonate, sodium dioctyl sulfosuccinate (DOSS), sodium alkyl-aryl phosphate, alkyl ether phosate, and sodium lauryl sarcosinate. However, the anionic emulsifier is not limited to these, and all known anionic emulsifiers may be included in the scope of the present invention.
[0052] The nonionic emulsifier may be of the ester type, ether type, ester-ether type, etc. For example, it may be polyoxyethylene glycol, polyoxyethylene glycol methyl ether, polyoxyethylene monoallyl ether, polyoxyethylene bisphenol-A ether, polypropylene glycol, polyoxyethylene alkenyl ether, etc. However, it is not limited thereto, and all known nonionic emulsifiers may be included in the scope of the present invention.
[0053] The conjugate diene copolymer may contain, based on the total weight, 20 to 45% by weight of the (a) conjugated diene monomer or conjugated diene polymer, 50 to 70% by weight of the (b) one or more monomers selected from the group consisting of acrylate monomers, vinyl monomers, and nitrile monomers, and 1 to 20% by weight of the (c) one or more monomers selected from the group consisting of unsaturated carboxylic acid monomers and hydroxyl group-containing monomers. The other components such as the emulsifier, buffer, and crosslinker may be optionally contained within the range of 0.1 to 10% by weight.
[0054] When the content ratio between the monomers constituting the conjugate diene copolymer falls within the above-mentioned range, Tg can be -10°C or more and 40°C or less.
[0055] When the content ratio between the monomers constituting the conjugate diene copolymer falls within the above-mentioned range, the flexibility, insulating properties, and electrolyte resistance of the insulating layer can be significantly improved.
[0056] In the experimental examples of the present invention, it was confirmed that when the content ratio between each monomer constituting the conjugate diene copolymer falls within the above-mentioned range, the initial adhesion, brittleness, and insulating properties are all excellent.
[0057] On the other hand, the average particle size of the copolymer may be 50 nm to 500 nm or less. Here, if the average particle size is less than 50 nm or exceeds 500 nm, it is not preferable because the dispersion stability may decrease.
[0058] Meanwhile, when the copolymer particles in the composition according to the present invention exist as an independent phase, the effect of improving the adhesive strength is enhanced, so it is very important to prevent the occurrence of agglomeration between the particles. Therefore, the composition according to the present invention includes a dispersion solvent for dispersing the copolymer particles. In the present invention, a non-aqueous organic solvent is used as the dispersion solvent.
[0059] The non-aqueous organic solvent may be at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol.
[0060] Preferably, the non-aqueous organic solvent may be N-methyl-pyrrolidone (NMP), but is not limited thereto.
[0061] The moisture content of the insulating layer composition for a lithium secondary battery according to an embodiment of the present invention may be 10,000 ppm or less, preferably 5,000 ppm or less, and more preferably 3,000 ppm or less. When the moisture content is within the above range, the insulating layer composition is coated separately from the electrode mixture layer, and thus the physical properties of the electrode are not deteriorated.
[0062] <Method of manufacturing positive electrode for lithium secondary battery>
[0063] Another example of the present invention is a method for manufacturing a positive electrode for a lithium secondary battery, the method including the steps of preparing a water-dispersed conjugated diene latex, adding a non-aqueous organic solvent to the water-dispersed conjugated diene latex, and heating and reducing pressure to prepare a slurry for an insulating coating layer, applying a slurry for a positive electrode mixture layer, the slurry including a positive electrode active material, a conductive material, and a non-aqueous binder, to one or both sides of a positive electrode current collector, applying the slurry for the insulating coating layer from a portion of an uncoated portion of the positive electrode current collector to cover a portion of the slurry for the positive electrode mixture layer applied to the current collector, and drying the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer applied to the positive electrode current collector.
[0064] The step of preparing a slurry for the insulating coating layer may include replacing water, which is a dispersion medium for conjugated dienes latex particles, with a non-aqueous organic solvent.
[0065] In one embodiment of the present invention, the step of preparing a slurry for the insulating coating layer may be a step of adding a non-aqueous organic solvent to the water-dispersible conjugated dienes latex, heating to a temperature of 40°C to 100°C, and reducing the pressure to less than 200 torr for 1 hour to 20 hours.
[0066] In one embodiment of the present invention, the conjugate diene latex can be styrene-butadiene latex particles, and the non-aqueous organic solvent can be NMP (N-methyl-pyrrolidone).
[0067] A non-aqueous organic solvent is added to the water-dispersed conjugated diene latex, and the mixture is heated and depressurized to replace the water, which is the dispersion medium for the conjugated diene latex particles, with the non-aqueous organic solvent.
[0068] In a preferred embodiment, the water-based styrene-butadiene latex (SBL) and NMP (N-methyl-pyrrolidone) are mixed, heated to a set temperature of 40°C to 100°C, and then the pressure is reduced to less than 200 torr to replace the solvent of the water-based styrene-butadiene latex (SBL) with NMP (N-methyl-pyrrolidone).
[0069] The conjugate diene latex particles in which the dispersion solvent water is replaced with a non-aqueous organic solvent maintain their particle shape even after being replaced with a non-aqueous organic solvent. The maintenance of the particle shape can be confirmed by particle size measurement. The particle size can be confirmed by, but is not limited to, a DLS particle size analyzer, a laser diffraction particle size analyzer, or an electron transmission microscope.
[0070] The positive electrode current collector may be one that does not induce chemical changes in the battery and has high conductivity. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. may be used, and in the case of aluminum or stainless steel, those that are surface-treated with carbon, nickel, titanium, silver, etc. may be used. For example, the current collector may be aluminum.
[0071] In addition, in the slurry for the positive electrode mixture layer, the positive electrode active material can be any positive electrode active material that is usually used in a positive electrode, and may be, but is not limited to, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or a lithium composite oxide that is a combination of these.
[0072] The non-aqueous binder contained in the positive electrode active material slurry may include one or more resins selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, and copolymers thereof. As an example, the binder may include polyvinylidene fluoride.
[0073] In this case, the conductive material is used to improve the performance of the positive electrode, such as electrical conductivity, and may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber. For example, the conductive material may include acetylene black.
[0074] Further, the solvent used in the slurry for the positive electrode mixture layer is a non-aqueous organic solvent, and may be N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol. The solvent may be one or more selected from the group consisting of N-methyl-2-pyrrolidone (NMP), for example.
[0075] In the step of applying the slurry for the insulating coating layer to the current collector, the slurry for the insulating layer may be applied while the slurry for the positive electrode mixture layer is still wet, or the slurry for the positive electrode mixture layer and the slurry for the insulating layer may be applied simultaneously.
[0076] The step of drying the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer may be performed by completely drying the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer using a drying method commonly known in the art to remove the solvent. In a specific example, the drying may be performed by changing a hot air method, a direct heating method, an induction heating method, or the like at a temperature at which the solvent is completely evaporated, but is not limited thereto. For example, the step of drying the insulating coating liquid may be performed by a hot air method.
[0077] At this time, the drying temperature may be in the range of 50° C. to 300° C., or may be 60 to 200° C. or 70 to 150° C. Meanwhile, if the drying temperature of the insulating coating liquid is less than 50° C., the temperature may be too low to completely dry the insulating coating liquid, and if it exceeds 300° C., the drying temperature may be too high to cause deformation of the electrodes.
[0078] A positive electrode mixture layer and an insulating coating layer are formed on the current collector, and the current collector is rolled to manufacture a positive electrode for a lithium secondary battery.
[0079] <Positive electrodes for lithium secondary batteries>
[0080] Another example of the present invention is a positive electrode for a lithium secondary battery, comprising a positive electrode current collector, a positive electrode tab protruding from the positive electrode current collector, and an insulating layer formed by coating an insulating material on the positive electrode tab, wherein the insulating material includes the insulating layer composition for a lithium secondary battery according to the present invention.
[0081] According to an embodiment of the present invention, the positive electrode including the insulating layer on the positive electrode tab can significantly shorten the manufacturing process of the battery, ultimately reducing the manufacturing cost of the battery, and can further improve the safety of the battery by widening the insulating area. In addition, it has an effect of not increasing the thickness of the electrode assembly, which is a problem that may occur when using a conventional insulating film or tape, that is, a very low possibility of detachment when bending the positive electrode tab for attachment to the area. In addition, it can solve the problem of reduced wet adhesion when a non-aqueous binder (such as PVDF) is used, and the problem of gelation of PVDF, an organic binder used as a positive electrode binder, when simultaneously coating with a slurry for a positive electrode mixture layer, when a water-based styrene butadiene copolymer (SBL) binder is used, which makes it impossible to simultaneously coat the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer.
[0082] <Lithium secondary battery>
[0083] Another example of the present invention is a lithium secondary battery including the positive electrode for lithium secondary batteries.
[0084] In addition to the electrodes, the lithium secondary battery generally further comprises a separator and a non-aqueous electrolyte containing a lithium salt.
[0085] The separation membrane is interposed between the positive electrode and the negative electrode, and is a thin insulating membrane having high ion permeability and mechanical strength. The pore size of the separation membrane is generally 0.01 to 10 μm, and the thickness is generally 5 to 300 μm. As such a separation membrane, for example, a sheet or nonwoven fabric made of an olefin polymer such as polypropylene, which is chemically resistant and hydrophobic, glass fiber, or polyethylene, etc. is used. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte can also serve as the separation membrane.
[0086] The lithium-containing non-aqueous electrolyte solution comprises a non-aqueous electrolyte solution and a lithium salt.
[0087] As the non-aqueous electrolyte, for example, non-quantum organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydroxyfuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate may be used.
[0088] The lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte solution, and examples of the lithium salt include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylates, lithium 4-phenylborate, imides, etc. are used.
[0089] In some cases, an organic solid electrolyte, an inorganic solid electrolyte, or the like may be used.
[0090] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymers containing ionic dissociation groups.
[0091] As the inorganic solid electrolyte, for example, nitrides, halides, sulfates, etc. of Li, such as LiN, LiI, LiNI, LiN-LiI-LiOH, LiSiO, LiSiO-LiI-LiOH, LiSiS, LiSiO, LiSiO-LiI-LiOH, LiPO-LiS-SiS2, etc., may be used.
[0092] In addition, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. may be added to the non-aqueous electrolyte solution in order to improve charge / discharge characteristics, flame retardancy, etc. In some cases, a halogen-containing solvent such as carbon tetrachloride or trifluoroethylene may be further added to impart non-flammability, carbon dioxide may be further added to improve high-temperature storage characteristics, and FEC (Fluoro-Ethylene carbonate), PRS (Propenesultone), etc. may be further added.
[0093] The secondary battery according to the present invention is not only used as a battery cell used as a power source for small devices, but is also preferably used as a unit battery for medium- to large-sized battery modules containing a large number of battery cells used as a power source for medium- to large-sized devices.
[0094] Preferred examples of the medium- to large-sized devices include, but are not limited to, power tools that are driven by a battery motor, electric vehicles including electric vehicles (EV), hybrid electric vehicles (HEV), plug-in hybrid electric vehicles (PHEV), etc., electric bicycles (E-bikes) and electric scooters (E-scooters), electric golf carts, and energy storage systems.
[0095] The present invention will be described in detail below with reference to examples. However, the following examples are merely illustrative of the present invention and are not intended to limit the present invention.
[0096] [Example 1]
[0097] 5 parts by weight of styrene-butadiene seed latex with a particle size of 55 nm was placed in a reactor and heated to 80°C, after which 38 g of 1,3-butadiene as a monomer, 59 g of styrene, 3 g of acrylic acid, 30.5 g of NaHCO3 as a buffer, 1 g of alkyldiphenyloxide disulfonate as an emulsifier, 1 g of dodecyl mercaptan as a molecular weight regulator, and 1 g of potassium persulfate as a polymerization initiator were added to the reactor for 4 hours, and the mixture was reacted for another 4 hours at 80°C to produce a styrene-butadiene copolymer latex with a solid content of 50%. At this time, the pH was adjusted to neutral (7) using sodium hydroxide. After polymerization, the size of the copolymer particles was analyzed using a Submicron particle sizer (Nicomp TM 380), and the average particle size of the polymerized copolymer particles was 150 nm.
[0098] 100g of the prepared styrene-butadiene copolymer latex was placed in a reactor, 600g of NMP (N-methyl-pyrrolidone) was added, mixed, and heated to 90°C, and the pressure was reduced to 15 torr within 1 to 4 hours to replace the water, which is the dispersion solvent of the styrene-butadiene copolymer particles, with NMP to prepare a composition containing a styrene-butadiene copolymer dispersed in NMP. At this time, the final moisture content was set to 10,000ppm or less, and the NMP was further corrected to a final solid content of 8%. The moisture content of the final product was measured with a Karl Fischer moisture meter.
[0099] [Example 2]
[0100] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that 30 g of 1,3-butadiene, 60 g of styrene, 5 g of methyl methacrylate, 2 g of acrylonitrile, 1 g of hydroxyacrylate, and 3 g of itaconic acid were used as monomers.
[0101] [Example 3]
[0102] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that 45 g of 1,3-butadiene, 50 g of styrene, 5 g of acrylic acid, and 0.2 g of dodecyl mercaptan as a molecular weight regulator were used as monomers.
[0103] [Example 4]
[0104] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that 22 g of 1,3-butadiene, 68 g of styrene, 5 g of methyl methacrylate, 2 g of hydroxyacrylate, and 3 g of itaconic acid were used as monomers.
[0105] [Comparative Example 1]
[0106] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that 48 g of 1,3-butadiene, 47 g of styrene, 1 g of methyl methacrylate, 2 g of hydroxyacrylate, and 2 g of acrylic acid were used as monomers.
[0107] [Comparative Example 2]
[0108] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that 20 g of 1,3-butadiene, 75 g of styrene, 2 g of methyl methacrylate, and 3 g of acrylic acid were used as monomers.
[0109] [Comparative Example 3]
[0110] A styrene-butadiene copolymer latex having a solid content of 50% was produced in the same manner as in Example 2.
[0111] 100g of the prepared styrene butadiene copolymer latex was placed in a reactor, 530g of NMP (N-methyl-pyrrolidone) was added, mixed, and heated to 85°C. The pressure was then reduced to 180 torr within 1 hour to replace the water, which is the dispersion solvent for the styrene butadiene copolymer particles, with NMP, to prepare a composition containing a styrene butadiene copolymer dispersed in NMP. NMP was added so that the final solid content was 8%, and the final moisture content was 50,010ppm. The moisture content of the final product was measured using a Karl Fischer moisture meter.
[0112] [Comparative Example 4]
[0113] A styrene-butadiene copolymer latex having a solid content of 50% was produced in the same manner as in Example 2.
[0114] 100g of the prepared styrene-butadiene copolymer latex was placed in a reactor, 530g of NMP (N-methyl-pyrrolidone) was added, mixed, and heated to 90°C. The pressure was then reduced to 100 torr within 7 hours to replace the water, which is the dispersion solvent for the styrene-butadiene copolymer particles, with NMP, to prepare a composition containing a styrene-butadiene copolymer dispersed in NMP. At this time, NMP was added so that the final solid content was 8%, and the final moisture content was 12,201 ppm. The moisture content of the final product was measured using a Karl Fischer moisture meter.
[0115] [Comparative Example 5] Preparation of compositions containing styrene butadiene latex without replacing dispersion solvent
[0116] To compare with a composition containing styrene-butadiene latex without solvent replacement, the styrene-butadiene latex prepared in Example 4 was mixed with carboxymethyl cellulose in a weight ratio of 9:1 without solvent replacement to prepare a composition. Carboxymethyl cellulose is used as a thickener to improve the coatability of styrene-butadiene latex without solvent replacement.
[0117] The types and amounts of monomers used in Examples 1 to 4 and Comparative Examples 1 to 5 are summarized in the following Table 1. The amounts used are expressed as % by weight based on the total weight of the monomers.
[0118] [Table 1]
[0119] For the compositions containing styrene-butadiene copolymers dispersed in NMP prepared in Examples 1 to 4 and Comparative Examples 1 to 5, the water content, viscosity, and Tg were measured and evaluated according to the methods described in Experimental Examples 1, 2, and 5 below, and the results are shown in Table 2 below.
[0120] In order to confirm the excellent physical properties of the compositions containing styrene butadiene copolymer dispersed in NMP prepared in Examples 1 to 4, the compositions containing styrene butadiene copolymer dispersed in NMP prepared in Comparative Examples 1 to 2, the composition containing PVDF (Comparative Example 6), the composition in which hydrogenated nitrile rubber was dissolved in NMP (Comparative Example 7), and the composition in which styrene butadiene rubber was dissolved in NMP (Comparative Example 8) were subjected to initial tackiness and brittleness evaluation according to the methods described in Experimental Examples 3 and 4 below, and the results are shown in Table 2 below. In the case of Comparative Example 8, the styrene butadiene rubber was not completely dissolved in NMP, but was partially dissolved, and gelled at 8% solid content. In the following experimental examples, the gelled part was removed and only the melted part was obtained to show the results of the experiment.
[0121] The compositions containing styrene-butadiene copolymer dispersed in NMP and the composition containing PVDF (Comparative Example 6) prepared in Examples 1 to 4 and Comparative Examples 1 to 2 were subjected to an insulation property evaluation and a moisture influence evaluation by the methods described in Experimental Examples 6 and 7 below, and the results are shown in Table 2 below. The compositions prepared in Comparative Examples 3 and 4 had the same composition as Example 2 except for the moisture content, so only the moisture influence evaluation, which may be influenced by the moisture content, was carried out. In order to compare the properties of a state in which the dispersion solvent of styrene-butadiene latex was not replaced with a non-aqueous organic solvent and a state in which it was replaced, the composition containing styrene-butadiene latex without replacement of the dispersion solvent prepared in Comparative Example 8 was subjected to a brittleness and moisture influence evaluation.
[0122] [Experimental Example 1] Moisture content
[0123] For the compositions prepared in Examples 1 to 4 and Comparative Examples 1 to 8, a Metrohm 899 Coulometer connected to an 860KF Thermoprep oven was used to set the oven temperature to 220°C, and 0.1 to 0.4 g of samples were weighed to measure the moisture content. In the case of Comparative Example 5, the product was prepared in an aqueous solution without replacing the dispersion solvent, and the moisture content was so high that it was impossible to measure using an instrument, so the solid content was measured and the remaining content was calculated and expressed as moisture.
[0124] [Experimental Example 2] Tg measurement
[0125] The compositions prepared in Examples 1 to 4 and Comparative Examples 1 to 8 were subjected to two cycles from -80°C to 80°C at 5°C / min using DSC, and the glass transition temperature was calculated as the intermediate value of the transition range in the second cycle. Using a TA Instruments DSC25, 3 to 20 mg of samples were weighed to measure Tg, and the results are shown in Table 2 below.
[0126] [Experimental Example 3] Initial Tackiness Evaluation
[0127] The compositions prepared in Examples 1 to 4, Comparative Examples 1 to 2, and Comparative Examples 5 to 8 were coated on aluminum metal foil and dried at 130° C. to prepare metal samples having an insulating coating layer of about 10 μm in thickness. The metal samples were cut to a size of 2 cm×12 cm and laminated on SUS plates (SUS plates), and the 90° adhesive strength was measured, and the results are shown in Table 2 below.
[0128] [Experimental Example 4] Brittleness measurement
[0129] The compositions prepared in Examples 1 to 4, Comparative Examples 1 to 2, and Comparative Examples 5 to 8 were coated on substrates to a final thickness of 20 μm, dried at 130° C., cut into 2 cm widths, and measured for brittleness. The samples were folded in half at room temperature, pressed once with a 1 kg roller, and then unfolded. The coating film was checked for cracks or the presence or absence of cracks with the naked eye, and the results are shown in Table 2 below.
[0130] [Experimental Example 5] Viscosity measurement
[0131] The viscosity of the compositions prepared in Examples 1 to 4 and Comparative Examples 1 to 8 was measured. The viscosity was measured at 25° C. using a Brookfield LV viscometer with a No. 63 spindle, rotated at 12 rpm, and then measured 1 minute later. When the viscosity was outside the measurement range, the rpm was lowered and the measurement was performed, and the results are shown in Table 2 below. In Table 2 below, 8% viscosity means the viscosity at a solid content of 8%.
[0132] [Experimental Example 6] Insulation characteristic measurement
[0133] LiNi as the positive electrode active material 0.8 Co 0.2 Mn 0.2 96 parts by weight of O2, 2 parts by weight of PVdF as a binder, and 2 parts by weight of carbon black as a conductive material were weighed and mixed in N-methylpyrrolidone (NMP) solvent to prepare a slurry for a positive electrode mixture layer. The slurry for the mixture layer was applied to an aluminum foil, dried, and then rolled to prepare a positive electrode having a positive electrode mixture layer with a thickness of 60 μm.
[0134] Thereafter, an insulating liquid which is a composition containing the styrene-butadiene copolymer produced in Examples 1 to 4, an insulating liquid which is a composition containing the styrene-butadiene copolymer produced in Comparative Examples 1 and 2, and an insulating liquid containing PVDF (Comparative Example 6) were applied onto the positive electrode mixture layer, and then dried to form a positive electrode insulating layer having a thickness of 10 μm.
[0135] A coin-type half cell was manufactured using the above positive electrode, lithium foil as the negative electrode, and an electrolyte containing 1M LiPF4 in a solvent of EC:EMC=3:7. The coin-type half cell was stored in an oven at 60°C for 15 days, and then the discharge capacity of the half cell was measured to confirm the insulating effect of the insulating layer. For comparison, a half cell was manufactured using a positive electrode without an insulating coin layer, and the 0.1C discharge capacity was set as 100. The discharge capacity ratio of the positive electrode having an insulating coating layer formed with the insulating liquid of Examples 1 to 4, Comparative Examples 1 and 2, and Comparative Example 6 was calculated, and the results are shown in Table 2 below.
[0136] [Table 2]
[0137] As shown in Table 2 above, in the cases of Examples 1 to 4, the initial adhesive strength, brittleness, and insulating properties were all excellent.
[0138] On the other hand, in the case of Comparative Example 1, Comparative Example 7, and Comparative Example 8, in which the Tg is less than -10°C, the initial adhesion is high, so that the electrodes adhere to each other after coating, and the electrodes adhere to each other during the winding process, making it difficult to carry out the process.
[0139] Also, as shown in Figure 1, in the case of Comparative Example 2, where the Tg exceeds 40°C, cracking occurred even though the initial adhesive strength was low. In the case of Comparative Example 5, cracking also occurred because the addition of a small amount of carboxymethyl cellulose, a thickener, caused high brittleness and affected the insulating liquid. For the same reason, even when styrene butadiene latex is coated separately without simultaneous coating, the insulating layer may crack or come off during the winding and slitting process.
[0140] In the case of Comparative Example 6 using PVDF, the initial adhesive strength was low, but the high-temperature discharge capacity ratio was high.
[0141] In particular, the positive electrodes in which the insulating coating layer was formed using the insulating liquids of Comparative Examples 1, 2, and 6 to 8 showed higher discharge rates than the positive electrodes in which the insulating coating layer was formed using the insulating liquids of Examples 1 to 4. If the wet adhesive strength in the electrolyte is low, the insulating liquid may be removed and swelled during high-temperature storage, resulting in the capacity of the positive electrode being expressed, and it appears that the higher the high-temperature discharge capacity ratio, the lower the insulating effect. It can be seen that the insulating liquids of Comparative Examples 1, 2, and 6 to 8 have low wet adhesive strength in the electrolyte, and the insulating liquid is removed and swelled during high-temperature storage, resulting in the capacity of the positive electrode being expressed.
[0142] [Experimental Example 7] Moisture Impact Assessment
[0143] LiNi as the positive electrode active material 0.8 Co 0.2 Mn 0.2 96 parts by weight of O2, 2 parts by weight of PVdF as a binder, and 2 parts by weight of carbon black as a conductive material were weighed and mixed in an N-methylpyrrolidone (NMP) solvent to prepare a slurry for a positive electrode mixture layer.
[0144] The slurry for the positive electrode mixture layer and the slurry for the insulating coating layer prepared in each of Examples 1 to 4 and Comparative Examples 3 to 5 were simultaneously applied to the current collector using a doctor blade so as to be overlaid, and the results were compared immediately after application and 1 minute after application, and the results are shown in Table 2 and FIG. 2. As shown in FIG. 2, in Examples 1 to 4, the initial coated state was maintained without penetration of the overlay portion both immediately after application and 1 minute after application, but in Comparative Examples 3 to 5, which have a moisture content of 10,000 ppm or more, the electrode slurry penetrated into the insulating layer and the coating boundary could not be reliably maintained. In particular, in the case of Comparative Example 5, in which the dispersion solvent was not replaced, the contact portion between the positive electrode slurry and the insulating liquid was coagulated by moisture immediately after application, so that it was confirmed that the aqueous insulating liquid without solvent replacement could not be coated simultaneously with the positive electrode slurry.
[0145] The higher the moisture content of the positive electrode insulating coating layer slurry, the more difficult it is for the positive electrode mixture layer slurry to permeate into the positive electrode insulating coating layer slurry when the positive electrode mixture layer slurry and the insulating layer slurry are coated simultaneously, making it difficult to achieve the expected insulating effect.
Claims
1. A conjugated diene copolymer as a binder polymer; A non-aqueous organic solvent is included as a dispersion solvent, The insulating layer composition for a lithium secondary battery, wherein the conjugate diene copolymer has a Tg of -10°C or more and 40°C or less.
2. Conjugated dienes copolymer particles having an average particle size of 50 nm to 500 nm are present as a separate phase; The insulating layer composition for a lithium secondary battery according to claim 1 .
3. The conjugate diene copolymer comprises: (a) a conjugated diene monomer or a conjugated diene polymer; (b) at least one monomer selected from the group consisting of an acrylate monomer, a vinyl monomer, and a nitrile monomer; and (c) a polymer of at least one monomer selected from the group consisting of an unsaturated carboxylic acid monomer and a hydroxyl group-containing monomer. The insulating layer composition for a lithium secondary battery according to claim 1 .
4. the conjugated diene monomer is one monomer selected from the group consisting of 1,3-butadiene, isoprene, chloroprene, and piperylene; The conjugated diene polymer is a polymer of two or more monomers selected from the group consisting of 1,3-butadiene, isoprene, chloroprene and piperylene, a styrene-butadiene copolymer, an acrylonitrile-butadiene copolymer, a styrene-isoprene copolymer, an acrylate-butadiene rubber, an acrylonitrile-butadiene-styrene rubber, an ethylene-propylene-diene polymer, a partially epoxidized or brominated polymer of these polymers, or a mixture thereof. The insulating layer composition for a lithium secondary battery according to claim 3 .
5. The acrylate monomer is at least one monomer selected from the group consisting of methyl ethacrylate, methacryloxyethyl ethylene urea, β-carboxyethyl acrylate, aliphatic monoacrylate, dipropylene diacrylate, ditrimethylolpropane tetraacrylate, dipentaerythriol hexaacrylate, pentaerythriol triacrylate, pentaerythriol tetraacrylate, and glycidyl methacrylate. The insulating layer composition for a lithium secondary battery according to claim 3 .
6. The vinyl monomer is at least one monomer selected from the group consisting of styrene, α-methylstyrene, β-methylstyrene, pt-butylstyrene, and divinylbenzene. The insulating layer composition for a lithium secondary battery according to claim 3 .
7. The nitrile monomer is one or more monomers selected from the group consisting of acrylonitrile, methacrylonitrile, and allyl cyanide. The insulating layer composition for a lithium secondary battery according to claim 3 .
8. The unsaturated carboxylic acid monomer is at least one monomer selected from the group consisting of maleic acid, fumaric acid, methacrylic acid, acrylic acid, glutaric acid, itaconic acid, tetrahydrophthalic acid, crotonic acid, isocrotonic acid, and nadic acid. The insulating layer composition for a lithium secondary battery according to claim 3 .
9. The hydroxy group-containing monomer is one or more monomers selected from the group consisting of hydroxyacrylate, hydroxyethyl acrylate, hydroxybutyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate. The insulating layer composition for a lithium secondary battery according to claim 3 .
10. The conjugate diene copolymer comprises, based on the total weight, 20 to 45% by weight of (a) a conjugated diene monomer or a conjugated diene polymer, 50 to 70% by weight of (b) at least one monomer selected from the group consisting of an acrylate monomer, a vinyl monomer, and a nitrile monomer, and 1 to 20% by weight of (c) a polymer of one or more monomers selected from the group consisting of an unsaturated carboxylic acid monomer and a hydroxyl group-containing monomer. The insulating layer composition for a lithium secondary battery according to claim 1 .
11. The non-aqueous organic solvent is at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol; The insulating layer composition for a lithium secondary battery according to claim 1 .
12. the conjugate diene copolymer is a styrene-butadiene copolymer; The non-aqueous organic solvent is NMP (N-methyl-pyrrolidone); The insulating layer composition for a lithium secondary battery according to claim 1 .
13. The moisture content is 10,000 ppm or less. The insulating layer composition for a lithium secondary battery according to claim 1 .
14. preparing a water-dispersed conjugated dienes latex; adding a non-aqueous organic solvent to the water-dispersed conjugated dienes latex, and heating and reducing pressure to prepare a slurry for an insulating coating layer; applying a slurry for a positive electrode mixture layer, the slurry including a positive electrode active material, a conductive material, and a non-aqueous binder, to one or both surfaces of a positive electrode current collector; applying the slurry for the insulating coating layer to a portion of an uncoated portion of the positive electrode current collector so as to cover a portion of the slurry for the positive electrode mixture layer applied to the current collector; and drying the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer applied to the positive electrode current collector. A method for producing a positive electrode for a lithium secondary battery.
15. The step of preparing a slurry for the insulating coating layer includes replacing water, which is a dispersion medium for the conjugate diene latex particles, with a non-aqueous organic solvent; The method for producing a positive electrode for a lithium secondary battery according to claim 14.
16. The conjugate diene latex particles maintain their particle shape even after the dispersion solvent is replaced with a non-aqueous organic solvent. The method for producing a positive electrode for a lithium secondary battery according to claim 15.
17. the conjugated diene latex is a styrene-butadiene latex particle; The non-aqueous organic solvent is NMP (N-methyl-pyrrolidone); The method for producing a positive electrode for a lithium secondary battery according to claim 14.
18. A positive electrode current collector; a positive electrode tab protruding from the positive electrode current collector; an insulating layer coated with an insulating material on the positive electrode tab; The insulating material comprises the composition of claim 1. Positive electrode for lithium secondary batteries.
19. The positive electrode for a lithium secondary battery according to claim 18, Lithium secondary battery.
Citation Information
Patent Citations
Electrode for nonaqueous electrolyte secondary battery or nonaqueous electrolyte capacitor
JP1999086874A
Nonaqueous secondary battery, and its manufacturing method thereof
JP2009163942A
Method for forming protective layer and power storage device
JP2015153638A
Binder composition for power storage device, slurry for power storage device electrode, power storage device electrode and power storage device
JP2016134241A
Composition for insulator layer formation, electrode body for electrochemical device, and electrochemical device
JP2019175736A