Battery cell, battery module, and method for manufacturing battery cell

The integration of a gel electrolyte around electrode tabs and a concentration gradient in the liquid electrolyte addresses tab disconnection issues, enhancing battery durability and performance by maintaining electrolyte contact and replenishing lithium salts.

JP2024540380AActive Publication Date: 2024-10-31LG ENERGY SOLUTION LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024526909
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-03-02
Filing Date
2023-02-28
Publication Date
2024-10-31
Estimated Expiration
2043-02-28

AI Technical Summary

Technical Problem

Lithium secondary battery cells experience frequent disconnection of electrode tabs due to mechanical rigidity issues, corrosion, and external impacts, leading to reduced performance and lifespan, especially in vehicles subjected to vibrations.

Method used

A battery cell design incorporating a gel electrolyte with low fluidity surrounding the electrode tabs and a liquid electrolyte with a lower molar concentration between the electrodes, forming a concentration gradient to maintain electrolyte wettability and prevent tab disconnection.

Benefits of technology

The design minimizes tab deformation and disconnection, improving battery durability and cycle characteristics by maintaining electrolyte contact and replenishing lithium salts, thus extending the battery's service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540380000001_ABST
    Figure 2024540380000001_ABST
Patent Text Reader

Abstract

The present invention relates to a battery cell having improved durability and lifespan, a manufacturing method of the battery cell, and a battery module including the battery cell. Specifically, the battery cell includes a cell case having an accommodation space, an electrode assembly accommodated in the accommodation space and including a plurality of electrodes, electrode tabs formed on at least one side of each of the plurality of electrodes, and a separator interposed between the plurality of electrodes, a gel electrolyte containing a first lithium salt of a first molar concentration and accommodated in the accommodation space surrounding the electrode tabs, and a liquid electrolyte containing a second lithium salt of a second molar concentration lower than the first molar concentration and accommodated between the plurality of electrodes.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2022-0027003 filed on March 2, 2022, and Korean Patent Application No. 10-2022-0027007 filed on March 2, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated as part of this specification.

[0002] The present invention relates to a battery cell, a battery module, and a method for manufacturing a battery cell, which improves the durability and life of the battery. [Background technology]

[0003] Currently commercially available secondary batteries include nickel-cadmium batteries, nickel-metal hydride batteries, nickel-zinc batteries, and lithium secondary batteries. Among them, lithium secondary batteries have almost no memory effect compared to nickel-based secondary batteries, so they can be charged and discharged freely. In addition, lithium secondary batteries have attracted attention due to their advantages of a very low self-discharge rate and high energy density.

[0004] Lithium secondary batteries mainly use lithium-based oxides and carbon materials as the positive and negative active materials, respectively. The lithium secondary battery includes an electrode assembly in which a positive electrode plate and a negative electrode plate, each coated with a positive electrode active material and a negative electrode active material, are disposed with a separator interposed therebetween, and an exterior material that hermetically houses the electrode assembly together with an electrolyte.

[0005] Generally, lithium secondary batteries can be classified into can-type secondary batteries and pouch-type secondary batteries according to the type of exterior material. In the can-type secondary battery, the electrode assembly is built into a metal can. In the pouch-type secondary battery, the electrode assembly is built into a pouch made of an aluminum laminate sheet.

[0006] In recent years, secondary batteries have been widely used not only in small devices such as portable electronic devices, but also in medium- and large-sized devices such as power storage devices in automobiles and power plants. When used in such medium- and large-sized devices, many battery cells are electrically connected to increase capacity and output. In particular, pouch-type battery cells, which are easy to stack, are often used in such medium- and large-sized devices. Here, a pouch-type battery cell refers to a battery cell in which an electrode assembly is housed in a pouch-type case made of a soft polymer material that does not have a uniform shape.

[0007] Meanwhile, the pouch sheet, which is the case of the pouch-type battery cell, is made of a soft material and includes a protruding portion on one side that is formed with an accommodation space for accommodating the electrode assembly, and a liquid injection portion formed on the other side that is open to inject the electrolyte.

[0008] The electrode assembly may include a positive electrode in which a positive electrode active material layer is formed on a positive electrode current collector, a negative electrode in which a negative electrode active material layer is formed on a negative electrode current collector, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.

[0009] Meanwhile, an electrode tab is formed on at least one side of the metal foil used for the positive electrode current collector and the negative electrode current collector. The electrode tab has a folded shape during a welding process with the electrode lead. However, since such an electrode tab is very thin and has relatively low mechanical rigidity, the folded shape of the electrode tab may be repeatedly folded and unfolded finely or the electrode tab may be easily broken due to an external impact or the like. Furthermore, the electrode tab may be corroded by some lithium salt contained in the electrolyte during charging and discharging, and if such corrosion continues to progress, the electrode tab may be broken.

[0010] Such disconnection of the electrode tab leads to inactivation of the electrode connected to the electrode tab, which causes the sudden death of the battery cell, significantly deteriorating the charge / discharge performance and life characteristics. In particular, in the case of a secondary battery installed in an automobile pack, since it is exposed to frequent vibrations and impacts, disconnection of the electrode tab may occur more frequently, which causes a problem of rapidly shortening the life of the battery cell.

[0011] In recent years, as the thickness of the current collector is made thinner to increase the energy density of the battery cell, the mechanical rigidity of the electrode tab is also reduced, and breakage frequently occurs at a folded portion of the electrode tab or at a connection portion between the electrode tab and the electrode. In addition, as the battery cell becomes smaller, the width of the electrode tab becomes narrower and the length of the tab becomes shorter, which increases the likelihood of breakage of the electrode tab when the battery cell is subjected to an external impact. Therefore, there is a need to develop a method for preventing breakage of the electrode tabs due to external impacts or electrolytes, and for improving the performance and service life of the battery cell. Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention has been made to solve the above problems, and aims to provide a battery cell that improves the durability and lifespan of the battery by disposing a gel electrolyte with low fluidity around the electrode tabs to prevent disconnection due to flow and deformation of the electrode tabs, and disposing a liquid electrolyte with high wettability around the electrode assembly excluding the periphery of the electrode tabs to increase the wettability of the electrolyte to the electrode assembly.

[0013] Another object of the present invention is to provide a battery module including the battery cell. Another object of the present invention is to provide a method for manufacturing the battery cell. [Means for solving the problem]

[0014] According to one embodiment, the present invention provides a cell case having a storage space, an electrode assembly accommodated in the accommodating space, the electrode assembly including a plurality of electrodes, electrode tabs formed on at least one side of each of the plurality of electrodes, and separators interposed between the plurality of electrodes; a gel electrolyte containing a first lithium salt having a first molar concentration and surrounding the electrode tab and contained in the containing space; a liquid electrolyte contained between the plurality of electrodes, the liquid electrolyte including a second lithium salt at a second molar concentration lower than the first molar concentration.

[0015] The battery cell may include a passivation film formed at an interface between the electrode tab and the gel electrolyte by combining a first lithium salt with a cation of the electrode tab. The passivation film may include at least one of AlF3 and LiF.

[0016] Meanwhile, the first lithium salt and the second lithium salt may be the same or different. The first lithium salt may include at least one of LiPF6 (Lithium hexafluorophosphate) and LiBF4 (Lithium tetrafluoroborate), and the second lithium salt may include at least one of LiPF6, LiFSI (Lithium bis(fluorosulfonyl)imide), LiTFSI (Lithium bis(trifluoromethanesulfonyl)imide), and LiBOB (Lithium bis(oxalato)borate).

[0017] On the other hand, the second molar concentration of the second lithium salt is lower than the first molar concentration of the first lithium salt by 0.1 M or more, and specifically, the ratio of the second molar concentration of the second lithium salt to the first molar concentration of the first lithium salt may be 1:1.3 to 1:5.

[0018] Meanwhile, the gel electrolyte may be located only on one side of the electrode assembly where the electrode tabs are formed in the accommodation space in order to prevent movement and deformation of the electrode tabs inside the battery cell due to an external impact, and the liquid electrolyte may be configured to surround the other side of the electrode assembly where the gel electrolyte is not formed.

[0019] According to another embodiment, the present invention provides a battery module including at least one battery cell of the present invention.

[0020] According to another embodiment, the present invention provides a method for manufacturing a semiconductor device, comprising the steps of: preparing an electrode assembly including a plurality of electrodes, an electrode tab formed on at least one side of each of the plurality of electrodes, and a separator interposed between the plurality of electrodes; disposing the electrode assembly in an accommodating space of a cell case; Injecting a gel electrolyte composition into the receiving space, the gel electrolyte composition including a first lithium salt having a first molar concentration and a curable compound, and then disposing the gel electrolyte composition around the electrode tab; curing the gel electrolyte composition to form a gel electrolyte surrounding the electrode tabs; and injecting a liquid electrolyte comprising a second lithium salt at a second molar concentration so as to be contained between the plurality of electrodes.

[0021] Meanwhile, the method may further include the step of forming a barrier between the receiving space of the cell case and the injection space for the gel electrolyte composition before injecting the gel electrolyte composition. Effect of the Invention

[0022] In the battery cell according to the present invention, a gel electrolyte having low fluidity is disposed around the electrode tabs, so that when an external impact is applied to the battery cell, the semi-solid gel electrolyte formed around the electrode tabs can minimize the flow and deformation of the electrode tabs. As a result, when the battery cell according to the present invention is mounted in an automobile, even if continuous impacts and vibrations occurring during travel are transmitted to the battery cell, damage to the electrode tabs can be minimized and disconnection of the electrode tabs can be prevented, thereby effectively improving the performance and lifespan of the battery cell.

[0023] In addition, the battery cell according to the present invention uses a liquid electrolyte in addition to a gel electrolyte, thereby improving wettability to the electrode assembly, and effectively reducing manufacturing time and costs.

[0024] Furthermore, the battery cell according to the present invention allows the first lithium salt in the gel electrolyte to move to the liquid electrolyte due to a molar concentration gradient between the first lithium salt in the gel electrolyte and the second lithium salt in the liquid electrolyte, and replenishes the lithium salt in the liquid electrolyte that is reduced due to lithium precipitation or the like during charging and discharging, thereby making it possible to provide a lithium secondary battery and a battery module with effectively improved cycle characteristics. [Brief description of the drawings]

[0025] [Figure 1] FIG. 2 is a plan view showing a battery cell according to one embodiment of the present invention. [Diagram 2] 1 is an exploded perspective view showing a pouch and an electrode assembly of a battery cell according to an embodiment of the present invention; [Diagram 3] FIG. 2 is an exploded perspective view showing a separator and an electrode according to an embodiment of the present invention. [Figure 4] 1 is a vertical cross-sectional view showing the interior of a battery cell according to one embodiment of the present invention. [Diagram 5] FIG. 2 is a plan view showing the interior of a battery cell according to one embodiment of the present invention. [Figure 6]1 is a front view showing a state in which multiple electrodes are inserted into the storage space of a pouch in a manufacturing method of a battery cell according to one embodiment of the present invention. FIG. [Figure 7] FIG. 2 is a front view showing the state inside the pouch in which a gel electrolyte composition is being injected into the storage space in a battery cell manufacturing method according to one embodiment of the present invention. [Figure 8] FIG. 2 is a front view showing the state inside the pouch in which the gel electrolyte composition is thermally cured in the storage space in the battery cell manufacturing method according to the embodiment of the present invention. [Figure 9] FIG. 2 is a side view showing a state before the battery cell is fixed using a fixing jig while the gel electrolyte composition is hardening in a battery cell manufacturing method according to one embodiment of the present invention. [Figure 10] FIG. 2 is a side view showing a state in which a battery cell is fixed using a fixing jig while a gel electrolyte composition is hardening in a battery cell manufacturing method according to an embodiment of the present invention. [Figure 11] 1 is a perspective view showing the state inside a pouch in which liquid electrolyte is being injected into the storage space in a method for manufacturing a battery cell according to one embodiment of the present invention; FIG. [Figure 12] 13 is a front view showing a state in which one side of the storage space of the pouch is further sealed in a method for manufacturing a battery cell according to one embodiment of the present invention. FIG. [Figure 13] 10 is a front view showing a state in which an injection space in the pouch has been removed in a battery cell manufacturing method according to one embodiment of the present invention. FIG. [Figure 14] 1 is a perspective view showing a battery module according to an embodiment of the present invention; [Figure 15] 5 is a partial enlarged view that illustrates a schematic enlargement of region A of the battery cell in FIG. 4. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The present invention will be described in detail below with reference to the drawings. In describing the present invention, if it is determined that a specific description of related known functions or configurations may unnecessarily obscure the gist of the present invention, the detailed description thereof will be omitted. Note that the following embodiments may be modified into various different forms, and the scope of the technical idea of ​​the present invention is not limited to the following embodiments. These embodiments are provided to make the present invention more complete and complete, and to fully convey the technical idea of ​​the present invention to those skilled in the art.

[0027] It should be understood that the technology described in the present invention is not limited to the particular embodiments, but includes various modifications, equivalents, and / or alternatives of the embodiments of the present invention.

[0028] In connection with the description of the drawings, like reference numbers may be used for like components. In the present invention, expressions such as "have," "can have," "include," or "can include" refer to the presence of a given feature (e.g., a value, a function, an operation, or a component such as a part) and do not exclude the presence of additional features.

[0029] In the present invention, expressions such as "A or B," "at least one of A or / and B," or "one or more of A or / and B" can include all possible combinations of the items listed together. For example, "A or B," "at least one of A and B," or "at least one of A or B" can refer to all of the following: (1) at least one A, (2) at least one B, or (3) both at least one A and at least one B.

[0030] The inventors conducted extensive research to develop a battery cell that prevents breakage due to flow and deformation of the electrode tabs and has excellent performance and lifespan, and discovered that by arranging a gel electrolyte with low fluidity around the electrode tabs so as to surround the electrode tabs and arranging a liquid electrolyte with excellent wettability around the electrode assembly where no gel electrolyte is formed, it is possible to significantly prevent breakage of the electrode tabs and improve cycle characteristics, leading to the completion of the present invention. Furthermore, the inventors discovered that the lifespan and performance of a battery can be effectively improved by injecting a liquid electrolyte with a low lithium salt concentration and low viscosity to improve the impregnation of the electrode assembly with the electrolyte, and by using a gel electrolyte containing a relatively high molar concentration of lithium salt in combination to replenish the lithium salt in the liquid electrolyte that is lost during charging and discharging, leading to the completion of the present invention.

[0031] Specifically, the battery cell 100 according to the present invention includes a cell case 110 , an electrode assembly 120 , electrode tabs 121 , a gel electrolyte 150 surrounding the periphery of the electrode tabs, and a liquid electrolyte 160 . The configuration of the battery cell of the present invention will be specifically described below.

[0032] Battery Cell FIG. 1 shows a plan view of a battery cell 100 according to an embodiment of the present invention. FIG. 2 shows an exploded perspective view of a pouch and electrode assembly 120 of the battery cell 100 according to an embodiment of the present invention. FIG. 3 shows an exploded perspective view of a separator 170 and electrodes 122p, 122n according to an embodiment of the present invention. FIG. 4 shows a vertical cross-sectional view showing the inside of the battery cell 100 according to an embodiment of the present invention. FIG. 5 shows a plan view showing the inside of the battery cell 100 according to an embodiment of the present invention. For reference, for convenience of explanation of the drawings, the gel electrolyte 150 and the liquid electrolyte 160 are omitted in FIG. 2, and the first cell sheet 114T of the battery cell 100 is removed in FIG. 5.

[0033] First, referring to Figures 1 and 2, a battery cell 100 of the present invention includes a cell case 110, a seal portion 111 heat-sealed to the outer periphery, and an electrode lead portion 130 including a positive electrode lead 130a and a negative electrode lead 130b protruding to the outside of the cell case, and a portion of the cell case may have a portion (P) protruding outwardly in a convex manner so as to accommodate an electrode assembly (not shown).

[0034] The cell case 110 may be a pouch-type case made of a soft material. Specifically, the cell case 110 may include a first cell sheet 114T covering an upper portion of the electrode assembly 120, and a second cell sheet 114P coupled to a portion of the lower surface of the first cell sheet 114T and covering a lower portion of the electrode assembly 120, as shown in FIG. 2. In this case, each of the first cell sheet 114T and the second cell sheet 114P may be a laminate sheet. Specifically, the laminate sheet may have a structure in which a thin metal film (e.g., an Al film) is laminated between a water-resistant polymer film (nylon) and a thermal adhesive polymer film (e.g., cast polypropylene). The structure of the laminate sheet and the materials constituting each layer are well known in the technical field to which the present invention belongs, and therefore detailed description thereof will be omitted.

[0035] The cell case 110 can be sealed by heat-sealing a portion of each of the first cell sheet 114T and the second cell sheet 114P to each other. The heat-sealing method can include a step of pressing at least a portion of the outer periphery of each of the first cell sheet 114T and the second cell sheet 114P facing each other with a high-temperature tool (e.g., a hot press) in a stacked state. At this time, the heat-sealing temperature may be 110 degrees Celsius to 150 degrees Celsius. By such heat-sealing, the cell case 110 can have a seal portion 111 heat-sealed to the outer periphery as shown in FIG. 1.

[0036] 2 to 5, the cell case 110 may include an accommodating space 110p1 that accommodates the electrode assembly 120, the electrode tab 121, the gel electrolyte 150, and the liquid electrolyte 160. The accommodating space 110p1 may be a portion in which at least one of the two cell sheets 114T and 114P is deformed into a cup shape by pressing the part of the cell sheet 114T and the cell sheet 114P with a high temperature hot press. The accommodating space 110p1 may be a portion (P) in which a part of each of the cell sheets 114T and 114P protrudes outward. The accommodating space 110p1 of the cell case 110 may be large enough to accommodate all of the electrodes 122, the separator 170, the gel electrolyte 150, and the liquid electrolyte 160. For example, as shown in FIG. 2, the storage space 110p1 of the cell case 110 can be formed by combining a portion (P) of the first cell sheet 114T that protrudes convexly toward the upper side and a portion (R) of the second cell sheet 114P that is concavely formed toward the lower side.

[0037] Meanwhile, the electrode assembly 120 is an electrode assembly having a structure in which a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode are sequentially stacked. FIG. 2 shows a structure in which the pouch and electrode assembly 120 of the battery cell 100 according to the present invention are separated, and FIG. 3 shows a structure in which the separator 170 and electrode 122 of the electrode assembly 120 according to the present invention, i.e., the positive electrode 122p and the negative electrode 122n, are separated.

[0038] As shown in FIG. 3, the electrodes 122 can include at least one positive electrode 122p and at least one negative electrode 122n, depending on the electrical polarity. The positive electrode 122p has a structure in which a positive electrode active material layer is formed on a current collector (not shown). In this case, the positive electrode active material layer may include a positive electrode active material, and optionally a conductive material and a binder. For example, the positive electrode 122p may be formed by applying a mixture of a positive electrode active material, a conductive material, and a binder to a current collector made of an aluminum alloy foil material.

[0039] The negative electrode 122n has a structure in which a negative electrode active material layer is formed on a current collector (not shown). In this case, the negative electrode active material layer may include a negative electrode active material, and optionally a conductive material and a binder. For example, the negative electrode 122n may be formed by applying a mixture of a negative electrode active material, a conductive material, and a binder to a current collector made of a copper alloy foil material.

[0040] The positive electrode active material, the negative electrode active material, the binder, and the conductive material may be any of the known materials used in lithium secondary batteries. A separator 170 may be interposed between the positive electrode 122p and the negative electrode 122n. The separator 170 may serve to block an internal short circuit between the positive electrode 122p and the negative electrode 122n and to impregnate the electrolyte. The separator 170 of the present invention may be any separator material that is commonly used in secondary batteries. For example, the separator 170 may include at least one material selected from the group consisting of polyethylene and polypropylene. The positive electrode 122p, the separator 170, and the negative electrode 122n may be stacked in order to form an electrode assembly 120 as shown in FIG. 2.

[0041] Meanwhile, an electrode tab 121 may be attached to the electrode collector as a path through which electrons can move. The mixture of the electrode active material, conductive material, and binder may not be applied to the electrode tab 121. That is, the electrode tab 121 may be formed by cutting an uncoated portion of an electrode collector that is not coated with an electrode active material, or may be formed separately by connecting another conductive member to the uncoated portion of the electrode collector by ultrasonic welding or the like.

[0042] At least one electrode tab 121 may be provided for each of the positive and negative electrodes. For example, as shown in FIG. 3, the positive electrode 122p and the negative electrode 122n may be provided with a positive electrode tab 121a and a negative electrode tab 121b protruding from the first side 122n1, respectively. However, the present invention is not necessarily limited to such a form. For example, the positive electrode tab 121a and the negative electrode tab 121b may be formed on at least one of the first side, the second side, the third side, and the fourth side in each of the front, rear, left, and right directions of the electrode 122. For example, when the positive electrode 122p has a quadrangle shape on a plane, the positive electrode tab 121a may be formed on at least one of the first side 122p1, the second side 122p2, the third side 122p3, and the fourth side 122p4. When the negative electrode 122n has a rectangular shape in a plan view, the negative electrode tab 121b may be formed on at least one of the first side 122n1, the second side 122n2, the third side 122n3, and the fourth side 122n4.

[0043] Meanwhile, the battery cell 100 according to an embodiment of the present invention may further include an electrode lead 130 coupled to a portion of the electrode tab 121 as shown in FIG. 2. The electrode lead 130 may be a conductive metal. Referring to FIG. 2, the electrode lead 130 may include a positive electrode lead 130a connected to the positive electrode tab 121a and a negative electrode lead 130b connected to the negative electrode tab 121b. The electrode lead 130 may be connected to one or more electrode tabs 121 in various ways, such as by welding. A portion of the electrode lead 130 may be disposed so as to be exposed to the outside of the cell case 110. That is, the electrode lead 130 serves as an electrode terminal of the battery cell 100. For example, the positive electrode lead 130a may serve as a positive electrode terminal of the battery cell 100, and the negative electrode lead 130b may serve as a negative electrode terminal of the battery cell 100. The battery cell 100 may include an insulating film 140 configured to surround a portion of an outer surface of the electrode lead 130. The insulating film 140 provides electrical insulation between the cell casing 110 and the electrode lead 130, and may be configured to be heat-sealed to the cell casing 110.

[0044] Meanwhile, referring to FIGS. 4 and 5, in the battery cell of the present invention, a gel electrolyte 150 having low fluidity may be disposed around the electrode tabs 121 including the positive electrode tab 121a and the negative electrode tab 121b so as to surround the electrode tabs 121.

[0045] The gel electrolyte 150 refers to an electrolyte having a gel phase. Here, the gel phase can be phenomenologically defined as a soft semi-solid material containing at least one liquid, and since it has high viscosity, it has no fluidity in a steady state and maintains a certain shape.

[0046] The gel electrolyte 150 may include a curable compound that can be cured to such an extent that the electrolyte exhibits a gel phase, and may further include an organic solvent and a first lithium salt.

[0047] The gel electrolyte 150 is mostly liquid by weight and may contain some solid material. For example, the gel electrolyte 150 may be manufactured by thermally curing or UV curing a curable compound mixed in a liquid electrolyte to change the phase of the liquid electrolyte into a gel electrolyte.

[0048] The gel electrolyte 150 may be located on one side of the electrode assembly 120 where the electrode tab 121 is located in the receiving space 110p1 so as to prevent the electrode tab 121 from moving due to an external impact on the battery cell 100. That is, the gel electrolyte 150 may surround the outer surface of the electrode tab 121 so as to suppress the movement and deformation of the electrode tab 121.

[0049] For example, as shown in FIG. 4, the gel electrolyte 150 may be located between the inner surface of the receiving space 110p1 and the first side 120a of the electrode assembly 120 where the electrode tab 121 is located. In this case, the gel electrolyte 150 may surround the outer surfaces of the positive electrode tab 121a and the negative electrode tab 121b so as to prevent the positive electrode tab 121a and the negative electrode tab 121b from flowing. However, the present invention is not necessarily limited to this form. For example, when the electrode tab 121 is located on at least one of the first side 120a, the second side 120b, the third side 120c, and the fourth side 120d of the electrode assembly 120, the gel electrolyte 150 may be located on at least one of the first side 120a, the second side 120b, the third side 120c, and the fourth side 120d of the electrode assembly 120 where the electrode tab 121 is located. The gel electrolyte 150 can also be configured to surround an outer surface of the electrode tab 121. In particular, the gel electrolyte 150 can be configured to surround the interface between the electrode tab 121 and the electrode lead 130.

[0050] Meanwhile, the gel electrolyte 150 is not necessarily located only on one side where the electrode tab 121 is formed, but the gel electrolyte 150 may also be located on the other side of the electrode assembly 120 where the electrode tab 121 is not located. For example, in the case of Fig. 5, the gel electrolyte 150 may be located in a part of the space between the electrode assembly 120 and the cell case 110 on each of the second side 120b and the fourth side 120d of the electrode assembly 120 where the electrode tab 121 is not located.

[0051] According to this configuration of the present invention, in comparison with the battery cell 100 of the conventional technology in which the liquid electrolyte 160 surrounds the electrode tab 121, when the battery cell 100 is subjected to an external impact, the gel electrolyte 150 surrounds the electrode tab 121, and the gel electrolyte 150 prevents the electrode tab 121 from moving, thereby preventing the connection portion between the electrode tab 121 and the electrode 122 or the bent portion of the electrode tab 121 from being broken due to frequent movement of the electrode tab 121.

[0052] In other words, when the battery cell 100 of the present invention is mounted in an automobile, even if frequent shocks and vibrations occurring during travel are transmitted to the battery cell 100, the semi-solid gel electrolyte 150 can minimize the flow and deformation of the electrode tab 121, thereby preventing breakage of the electrode tab 121. As a result, inactivation of the charge and discharge of the electrode 122 can be prevented, thereby effectively increasing the lifespan of the battery cell 100.

[0053] As shown in FIG. 4, the battery cell 100 of the present invention can also include a liquid electrolyte 160. The liquid electrolyte 160 may be accommodated adjacent to the inside of the cell case 110 so as to be in contact with the gel electrolyte 150. In this case, an interface (X) may be formed between the gel electrolyte 150 and the liquid electrolyte 160. The battery cell 100 of the present invention may be configured so that the first lithium salt of the gel electrolyte 150 can move to the liquid electrolyte 160 through the interface (X) between the gel electrolyte 150 and the liquid electrolyte 160. That is, the battery cell 100 of the present invention is configured so that the first lithium salt of the gel electrolyte 150 having a relatively high concentration can move to the liquid electrolyte 160 through the interface (X) between the gel electrolyte 150 and the liquid electrolyte 160. Therefore, even if the battery cell 100 is charged and discharged several times, it is possible to prevent the depletion of the lithium salt in the liquid electrolyte 160 containing the lithium salt having a relatively low molar concentration, and therefore the life of the battery cell 100 can be effectively increased.

[0054] 4 and 5, the liquid electrolyte 160 may be accommodated in the accommodation space 110p1 to surround at least one other side of the electrode assembly 120 where the gel electrolyte 150 is not formed, for example, where the electrode tab 121 is not located. When the electrode tab 121 is located on the first side 120a of the electrode assembly 120, the liquid electrolyte 160 may be located on any one of the remaining second side 120b, third side 120c, and fourth side 120d of the electrode assembly 120 where the electrode tab 121 is not formed. It is preferable that the liquid electrolyte 160 is located on the side where the amount of the liquid electrolyte 160 that can be replenished is as large as possible in preparation for consumption of the liquid electrolyte 160, thereby effectively preventing a decrease in the life of the battery cell 100. For example, as shown in FIG. 5, when the electrode tab 121 is located on the first side 120a of the electrode assembly 120, the liquid electrolyte 160 can be located to surround the remaining second side 120b, third side 120c, and fourth side 120d of the electrode assembly 120.

[0055] According to this configuration of the present invention, when the liquid electrolyte 160 located between the electrodes 122 is consumed during charging and discharging of the battery cell 100, the liquid electrolyte 160 located on at least one other side of the electrodes 122 on which the electrode tabs 121 are not formed can move between the electrodes 122 to replenish the liquid electrolyte 160. Therefore, even if the liquid electrolyte 160 between the electrodes 122 is consumed after multiple charging and discharging of the battery cell 100, the reduction in the lifespan of the battery cell 100 can be suppressed.

[0056] 15, an insoluble passivation film 123 formed by a reaction between anions of a lithium salt contained in a gel electrolyte 150 and cations of the electrode tab 121 may be formed on the metal surface of the electrode tab 121. The passivation film 123 may prevent corrosion by suppressing a reduction reaction on the surface of the electrode tab, and may minimize damage to the electrode tab 121 due to an external impact, thereby effectively suppressing breakage of the electrode tab 121.

[0057] In addition, the battery cell 100 according to an embodiment of the present invention can be charged and discharged by ion exchange between the positive electrode 122p and the negative electrode 122n via the liquid electrolyte 160. The liquid electrolyte 160 can be located between the positive electrode 122p and the negative electrode 122n so that ions can move between the positive electrode 122p and the negative electrode 122n. The liquid electrolyte 160 can be absorbed into each of the positive electrode 122p and the negative electrode 122n. The liquid electrolyte 160 can be located on the surface and in the pores of the separator 170. For example, in the case of a lithium secondary battery, the battery cell 100 can generally use a nonaqueous electrolyte. Next, each component of the gel electrolyte 150 and liquid electrolyte 160 contained in the battery cell of the present invention will be described in more detail.

[0058] (1) Gel electrolyte The gel electrolyte 150 of the present invention can be formed by injecting a gel electrolyte composition 155 containing a curable compound, a first lithium salt, an organic solvent, and a polymerization initiator into the accommodation space 110p1, followed by thermal polymerization.

[0059] In this case, the curable compound is not particularly limited as long as it has a polymerizable functional group selected from the group consisting of a vinyl group, an epoxy group, an allyl group, and a (meth)acrylic group in which a polymerization reaction can occur in the structure, forms a crosslinked bond by a polymerization reaction applied to the production of a general gel electrolyte, and can be changed into a gel phase.

[0060] Specifically, the curable compound may be at least one selected from a polymerizable monomer, an oligomer, and a copolymer. The polymerizable monomer may include a thermally polymerizable monomer or an ultraviolet light curable acrylate monomer.

[0061] Representative examples of the thermally polymerizable monomer include tetraethylene glycol diacrylate, polyethylene glycol diacrylate (molecular weight: 50 to 20,000), 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, trimethylolpropane ethoxylate triacrylate, trimethylolpropane propoxylate triacrylate, ditrimethylolpropane tetraacrylate, pentaerythritol tetraacrylate, pentaerythritol ethoxylate tetraacrylate, and the like. tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, poly(ethylene glycol) diglycidylether, 1,5-hexadiene diepoxide, glycerol propoxylate triglycidyl ether, vinylcyclohexene dioxide, 1,2,7,8-diepoxyoctane (1,2,7,The monomer may be at least one of 8-diepoxyoctane, 4-vinylcyclohexene dioxide, butyl glycidyl ether, diglycidyl 1,2-cyclohexanedicarboxylate, ethylene glycol diglycidyl ether, glycerol triglycidyl ether, and glycidyl methacrylate, and these monomers may be used alone or in combination of two or more.

[0062] In addition, the UV-curable acrylate monomer may include at least one of ODA (octyl / decyl acrylate), IDA (isodecyl acrylate), LA (lauryl acrylate), SA (stearyl acrylate), PEA (phenoxyethyl acrylate), MNPEOA (nonylphenol ethoxylate monoacrylate), tetrahydrofurfuryl acrylate, cyclohexyl acrylate, 4-butylcyclohexyl acrylate, dicyclopentenyl acrylate, dicyclopentenyloxyethyl acrylate, 4-HBA (4-hydroxybutyl acrylate), and phenoxyethyl acrylate. In addition, the oligomer may include at least one selected from the group consisting of a fluorine-based oligomer, a polyether-based oligomer, a polycarbonate-based oligomer, an acrylate-based oligomer, a polysiloxane-based oligomer, a phosphazene-based oligomer, a polyethylene-based oligomer, a urethane-based oligomer, an epoxy-based oligomer, polyethylene oxide, a polyester sulfide, polyvinyl alcohol, and polyvinylidene fluoride, and specifically, may include at least one selected from among a fluorine-based oligomer, a polycarbonate-based oligomer, and a polysiloxane-based oligomer. The copolymer can include at least one selected from the group consisting of allyl 1,1,2,2-tetrafluoroethyl ether (TFE)-(2,2,2-trifluoroethyl acrylate) copolymer, TFE-vinyl acetate copolymer, TFE-(2-vinyl-1,3-dioxolane) copolymer, TFE-vinyl methacrylate copolymer, TFE-methyl acrylate copolymer, TFE-methyl methacrylate (MMA) copolymer, and TFE-2,2,2-trifluoroethyl acrylate copolymer.

[0063] The curable compound may be contained in an amount of about 3 wt% to 30 wt%, preferably about 3 wt% to 25 wt%, more preferably about 3 wt% to 10 wt%, specifically 5 wt% to 7 wt%, based on the total weight of the gel electrolyte composition.

[0064] When the content of the curable compound is less than 3 wt % with respect to the total weight of the gel electrolyte composition 155, even if the curable compound is cured, the electrolyte is unlikely to form a gel phase. In addition, when the content of the curable compound is more than 30 wt % with respect to the total weight of the gel electrolyte composition 155, the viscosity of the gel electrolyte composition 155 increases, and the fluidity of the gel electrolyte composition 155 decreases when the gel electrolyte composition 155 is injected into the storage space of the battery cell 100. The gel electrolyte composition 155 remaining between the electrodes 122 may not be easily moved to the storage space 110p1 around the electrode tab 121, and a part of the gel electrolyte composition 155 may remain between the electrodes 122 during the movement. The gel electrolyte composition 155 remaining between the electrodes 122 has a higher ion conduction resistance than the liquid electrolyte 160, and may adversely affect the performance of the battery cell 100 (for example, an increase in the internal resistance of the battery). Therefore, when the content of the curable compound in the gel electrolyte composition 155 satisfies the above range, a viscosity that makes it easy to inject the gel electrolyte composition into the storage space can be secured.

[0065] Meanwhile, the first lithium salt is not particularly limited as long as it contains an anion that can form an insoluble passivation film on the metal surface of the electrode tab and suppress the induction of a reduction reaction on the surface of the electrode tab. Specifically, the first lithium salt is LiPF6, LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 , LiAlCl4, LiAlO4, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, and LiCH3SO3, and preferably, any one of LiPF6 and LiBF4.

[0066] Specifically, when the first lithium salt is one of LiPF6 and LiBF4, the first anion is F - and the first anion (F - ) and the cation (Al 3+15, an aluminum native oxide film (Al2O3) 124 is formed on the surface of the electrode tab 121 containing aluminum, and a passivation film 123 may be formed on the aluminum native oxide film. The passivation film 123 may include at least one of AlF3 and LiF.

[0067] On the other hand, when LiFSI (Lithium bis(fluorosulfonyl)imide) or LiTFSI (Lithium bis(trifluoromethanesulfonyl)imide) is used as the first lithium salt, it reacts with the aluminum metal surface of the electrode tab to generate Al(FSI)3 (Al((FSO2)2N)3) on the surface of the electrode tab, and since this reactant is soluble in the electrolyte solvent, it may dissolve in the electrolyte solvent and cause corrosion of the electrode tab. Therefore, the present invention uses LiPF6 and LiBF4 as the first lithium salt to generate AlF3, LiF, etc. that are less soluble (or insoluble) in the electrolyte solvent before Al(FSI)3, and forms a passivation film 123 on the aluminum metal surface of the electrode tab, thereby suppressing the corrosion reaction of the aluminum metal of the electrode tab.

[0068] However, LiPF6 and LiBF4 have the disadvantage of being low in ionic conductivity and thermal stability compared to LiFSI (Lithium bis(fluorosulfonyl)imide), LiTFSI (Lithium bis(trifluoromethanesulfonyl)imide), or LiBOB (Lithium bis(oxalato)borate). However, the battery cell 100 of the present invention can improve the disadvantages of LiPF6, LiBF4, etc., such as low ionic conductivity and thermal stability, by using a liquid electrolyte 160 with high ionic conductivity and thermal stability in combination, as described below.

[0069] Meanwhile, the first lithium salt may have a first molar concentration of 0.6M to 5.0M. Here, the first molar concentration means the amount of solute dissolved in 1 L of solution, expressed in moles. When the molar concentration of the first lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, and therefore can exhibit excellent electrolyte performance, and lithium ions can move effectively.

[0070] On the other hand, when the first molar concentration of the first lithium salt of the gel electrolyte 150 is less than 0.2 M, the excessively low concentration of the first lithium salt makes it impossible to effectively increase the life of the battery cell 100. Also, when the first molar concentration of the first lithium salt of the gel electrolyte 150 exceeds 5.0 M, the use of an excessive amount of lithium salt increases the viscosity of the gel electrolyte composition, thereby worsening the fluidity of the gel electrolyte composition, and the gel electrolyte composition is not easily moved to the storage space around the electrode tab. As a result, the gel electrolyte does not fill the entire space of the tab, and the liquid electrolyte penetrates, which may cause breakage of the tab and a decrease in life performance. Specifically, the first lithium salt may have a first molar concentration of 0.9M to 4.0M, specifically 1.0M to 3.0M.

[0071] On the other hand, the organic solvent is not particularly limited as long as it is an organic solvent used in electrolytes for secondary batteries, and specifically, it may be one or more selected from the group consisting of propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), vinylene carbonate (VC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), and γ-butyrolactone. However, the organic solvent is not necessarily limited to only the configurations listed above, and the same effect can be achieved even if a known configuration or its equivalent is applied. On the other hand, the remainder except for the curable compound, lithium salt, and polymerization initiator in the gel electrolyte composition of the present invention may be an organic solvent unless otherwise specified.

[0072] As the polymerization initiator, a typical thermal polymerization initiator or photopolymerization initiator well known in the art can be used depending on the type of the curable compound. Specifically, when a thermally polymerizable monomer is used as the curable compound, a thermal polymerization initiator can be used as the polymerization initiator, and when an ultraviolet-curable acrylate monomer is used as the curable compound, a photopolymerization initiator can be used as the polymerization initiator.

[0073] The thermal polymerization initiator is decomposed by heat to form radicals, which react with the polymerizable monomer, oligomer, or copolymer through free radical polymerization to gel the gel electrolyte composition. Specifically, non-limiting examples of the thermal polymerization initiator include benzoyl peroxide, acetyl peroxide, dilauryl peroxide, di-tert-butyl peroxide, t-butyl peroxy-2-ethyl-hexanoate, cumyl hydroperoxide, hydrogen peroxide, and the like. peroxide), and azo compounds such as 2,2'-azobis(2-cyanobutane), 2,2'-azobis(methylbutyronitrile), 2,2'-azobis(iso-butyronitrile) (AIBN), and 2,2'-azobisdimethylvaleronitrile (AMVN).

[0074] The thermal polymerization initiator is decomposed by heat, for example at 30° C. to 100° C., or at room temperature (5° C. to 30° C.) in the battery to form radicals, and the polymerizable monomer reacts with the acrylate compound through free radical polymerization to form the gel electrolyte 150.

[0075] The photopolymerization initiator can be decomposed by light to form radicals and react with the polymerizable monomer, oligomer, or copolymer through free radical polymerization to gel the gel electrolyte composition. Specifically, non-limiting examples of the photopolymerization initiator can include at least one of ethyl benzoin ether, isopropyl benzoin ether, α-methyl benzoin ethyl ether, benzoin phenyl ether, α-acyl oxime ester, 1,1-dichloroacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, anthraquinone, 2-anthraquinone, 2-chloroanthraquinone, thioxanthone, isopropyl thioxanthone, chlorothioxanthone, benzophenone, benzyl benzoate, and benzoyl benzoate.

[0076] The polymerization initiator may be included in an amount of 0.01 to 20 parts by weight, specifically 0.1 to 10 parts by weight, based on 100 parts by weight of the curable compound. When the polymerization initiator is included in an amount within the range of 0.01 to 20 parts by weight, the conversion rate of the curable compound can be increased, thereby ensuring the properties of the gel electrolyte 150.

[0077] On the other hand, the gel electrolyte composition before the formation of the gel electrolyte 150 preferably has a viscosity of about 3 cP to 100 cP, specifically 6 cP to 10 cP, and more specifically 6 cP to 7 cP, so as to be easily injected into the accommodation space 110p1.

[0078] If the viscosity of the gel electrolyte composition 155 is less than 3 cP, the electrode tabs 121 may flow, resulting in disconnection of the electrode tabs 121. Conversely, if the viscosity of the gel electrolyte composition 155 is more than 100 cP, the fluidity of the gel electrolyte composition 155 may decrease, making it difficult to move the gel electrolyte composition into the storage space around the electrode tabs. In addition, the amount of the curable compound and the first lithium salt used may increase, resulting in an increase in the manufacturing cost of the battery cell 100.

[0079] Furthermore, the viscosity of the hardened gel electrolyte after the formation of the gel electrolyte 150 is about 10,000 cP to 30,000 cP, specifically 20,000 cP, and the gel electrolyte may have a viscosity that is almost non-fluid.

[0080] In the present invention, when the viscosity of the gel electrolyte 150 satisfies the above range, even if frequent impacts and vibrations occurring during transportation are transmitted to the battery cell 100, the electrolyte 150 having a higher viscosity than the liquid electrolyte 160 can minimize the flow and deformation of the electrode tab 121.

[0081] In this manner, the present invention can control the viscosity of the gel electrolyte 150 to have a suitable viscosity that can prevent the movement and deformation of the electrode tab 121 by adjusting the content of each of the first lithium salt having a first molar concentration and the hardened polymer. This can reduce the deformation of the electrode tab 121 even when an external impact is applied to the battery cell 100. Therefore, when the battery cell 100 of the present invention is mounted in an automobile, even if frequent impacts and vibrations that occur during travel are transmitted to the battery cell 100, the electrolyte 150 having a higher viscosity than the liquid electrolyte 160 can minimize the movement and deformation of the electrode tab 121.

[0082] (2)Liquid electrolyte In the present invention, the liquid electrolyte comprises a second lithium salt and an organic solvent, and may optionally further comprise an additive.

[0083] The molar concentration of the second lithium salt in the liquid electrolyte may be about 0.5M to 2.0M. Meanwhile, when the second molar concentration of the second lithium salt of the liquid electrolyte 160 is less than 0.5 M, the lithium ion conductivity decreases, and the internal resistance of the battery cell increases, which may impair the life of the battery cell 100. Furthermore, when the second molar concentration of the second lithium salt exceeds 2.0 M, the amount of the second lithium salt used increases more than necessary, which increases the viscosity of the liquid electrolyte 160 and may reduce the wettability of the liquid electrolyte 160 to the electrode assembly 120, which may increase the manufacturing cost of the battery cell. The molar concentration of the second lithium salt in the liquid electrolyte may be about 0.75M to 1.8M, specifically about 0.8M to 1.5M.

[0084] In particular, in the present invention, the liquid electrolyte preferably contains a second lithium salt having a second molar concentration lower than the first molar concentration of the first lithium salt in the gel electrolyte so as to form a concentration gradient. Specifically, the second molar concentration of the second lithium salt is preferably at least 0.1 M lower than the first molar concentration of the first lithium salt.

[0085] In the present invention, by setting the second molar concentration of the second lithium salt in the liquid electrolyte 160 to be 0.1 M or more lower than the first molar concentration of the first lithium salt in the gel electrolyte 150, a suitable concentration gradient of the lithium salts in the gel electrolyte 150 and the liquid electrolyte 160 can be formed, and the first lithium salt in the gel electrolyte 150 can migrate to the liquid electrolyte 160 through the interface (X) between the gel electrolyte 150 and the liquid electrolyte 160. On the other hand, when the second molar concentration of the two lithium salts in the liquid electrolyte 160 is less than 0.1 M higher than the first molar concentration of the first lithium salt in the gel electrolyte 150, the amount of the first lithium salt in the gel electrolyte 150 that migrates to the liquid electrolyte 160 is small, and the effect of improving the life of the battery cell 100 may be insignificant.

[0086] Specifically, in the battery cell 100 according to an embodiment of the present invention, the first molar concentration of the first lithium salt in the gel electrolyte 150 is 0.6M to 5.0M, and the second molar concentration of the second lithium salt in the liquid electrolyte 160 is 0.5M to 2.0M. In this case, the second molar concentration of the second lithium salt may be lower than the first molar concentration of the first lithium salt by 0.1M or more. Preferably, the second molar concentration of the second lithium salt in the liquid electrolyte 160 may be 0.75M to 1.8M, and more preferably, 0.8M to 1.5M. In this way, by setting the second molar concentration of the second lithium salt to be lower than the first molar concentration of the first lithium salt by 0.1M or more, it is possible to form an appropriate concentration gradient of the lithium salts in the gel electrolyte 150 and the liquid electrolyte 160, and therefore the first lithium salt in the gel electrolyte 150 can move to the liquid electrolyte 160.

[0087] In the battery cell 100 according to one embodiment of the present invention, the ratio of the second molar concentration of the second lithium salt to the molar concentration of the first lithium salt may be 1:1.3 to 1:5. Preferably, the ratio of the second molar concentration of the second lithium salt to the molar concentration of the first lithium salt may be 1:1.3 to 1:5. More preferably, the ratio of the second molar concentration of the second lithium salt to the molar concentration of the first lithium salt may be 1:1.4 to 1:5.

[0088] In the present invention, since the ratio of the second molar concentration of the second lithium salt to the molar concentration of the first lithium salt falls within the above range, an appropriate concentration gradient of the lithium salts in gel electrolyte 150 and liquid electrolyte 160 can be formed, and the first lithium salt in gel electrolyte 150 can migrate to liquid electrolyte 160 via interface (X).

[0089] On the other hand, when the ratio of the second molar concentration of the second lithium salt to the molar concentration of the first lithium salt is less than 1:1.3, it is difficult to have an appropriate concentration gradient, and the amount of the first lithium salt in the gel electrolyte 150 that migrates to the liquid electrolyte 160 is small, so that the effect of increasing the life of the battery cell 100 may be insignificant. Also, when the ratio of the second molar concentration of the second lithium salt to the molar concentration of the first lithium salt is greater than 1:5, the amount of the first lithium salt used in the gel electrolyte 150 increases unnecessarily, making it difficult to inject the gel electrolyte composition and increasing the manufacturing cost of the battery cell 100.

[0090] On the other hand, typical examples of second lithium salts are LiPF6, LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10, LiAlCl4, LiAlO4, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiFSI (Lithium bis(fluorosulfonyl)imide, LiN(SO2F)2), LiTFSI (Lithium(bis)trifluoromethanesulfonimide, LiN(SO2CF3)2), LiBOB (Lithium bis(oxalato)borate, LiB(C2O4)2), and LiBETI (Lithium bisperfluoroethanesulfonimide, LiN(SO2CF2CF3)2), and may include a lithium salt that is the same as or different from the first lithium salt. More specifically, the second lithium salt may include at least one of LiPF6, LiFSI, LiTFSI, LiBOB2, and LiBETI. Preferably, the second lithium salt has a relatively high metal oxidation power compared to the first lithium salt, but has a relatively high ionic conductivity, can reduce internal electrical resistance, and can be used in combination with LiPF6 and at least one of LiFSI, LiTFSI, LiBOB2, and LiBETI, which are different from the first lithium salt, so that the thermal stability can be increased when the battery cell is exposed to a high-temperature environment.

[0091] On the other hand, when at least one of LiFSI, LiTFSI, LiBOB2, and LiBETI is used in combination with LiPF6 as the second lithium salt, the molar concentration ratio of LiPF6 to the other lithium salts other than LiPF6 may be 1:1 to 1:6.7, specifically 1:1 to 1:4. That is, when the molar concentration of LiPF6 is higher than the molar concentration of the lithium salts other than LiPF6, the ionic conductivity of the liquid electrolyte 160 decreases, and the internal resistance of the battery cell 100 may relatively decrease. On the other hand, when the molar concentration ratio of the other lithium salts other than LiPF6 to LiPF6 exceeds 6.7 times, the manufacturing cost of the battery cell may increase. Therefore, the battery cell 100 according to the present invention has an advantage that the amount of LiPF6 used, which is relatively inexpensive, can be increased while suppressing the increase in the internal electrical resistance of the battery cell 100, and the manufacturing cost of the battery cell 100 can be reduced by configuring the molar concentration ratio of the second lithium salt to the third lithium salt to be 1:1 to 1:6.7.

[0092] The organic solvent contained in the liquid electrolyte may be the same as or different from the organic solvent used in the gel electrolyte, and may be one or more selected from the group consisting of propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), vinylene carbonate (VC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), and γ-butyrolactone. The organic solvent is not necessarily limited to the above-listed configurations, and the same effect can be achieved by applying known configurations and their equivalents.

[0093] In addition, the liquid electrolyte may further contain additives as necessary to further improve the high-rate discharge characteristics, high-temperature stability, overcharge prevention, and battery expansion suppression effects of the battery.

[0094] Examples of such additives include at least one selected from the group consisting of non-fluorine-substituted cyclic carbonate compounds, sultone compounds, sulfate compounds, benzene compounds, amine compounds, and silane compounds.

[0095] Examples of the cyclic carbonate compound not substituted with fluorine include vinylene carbonate (VC) and vinyl ethylene carbonate (VEC).

[0096] Specific examples of the sultone-based compound include at least one selected from the group consisting of 1,3-propane sultone (PS), 1,4-butane sultone, ethene sultone, 1,3-propene sultone (PRS), 1,4-butene sultone, and 1-methyl-1,3-propene sultone.

[0097] Specific examples of the sulfate-based compound include ethylene sulfate (Esa), trimethylene sulfate (TMS), and methyl trimethylene sulfate (MTMS).

[0098] The benzene-based compound may be fluorobenzene, and the amine-based compound may be triethanolamine or ethylenediamine. The silane-based compound may be tetravinylsilane or the like.

[0099] The additive may be used in a mixture of two or more compounds, and may be included in an amount of 0.01 to 20% by weight, specifically 0.05 to 5% by weight, based on the total weight of the liquid electrolyte. If the content of the additive exceeds 20% by weight, excessive side reactions may occur during charging and discharging of the battery due to the excess additive.

[0100] Meanwhile, the viscosity of the liquid electrolyte 160 may be 2 cP to 20 cP. When the viscosity is within the above range, the electrolyte 160 can have an appropriate viscosity to uniformly and well permeate the electrodes 122, thereby improving the initial charge / discharge efficiency of the battery cell 100, shortening the manufacturing time of the battery cell 100, and effectively reducing the manufacturing cost.

[0101] In contrast, if the viscosity of the liquid electrolyte 160 is less than 2 cP, the capacity and lifespan of the battery cell 100 may decrease, and conversely, if the viscosity of the liquid electrolyte 160 is more than 20 cP, the wettability of the liquid electrolyte 150 may decrease, the manufacturing time may increase, and the manufacturing cost of the battery cell 100 may increase.

[0102] Meanwhile, in the battery cell 100 of the present invention, as the charge and discharge of the battery cell 100 is repeated, the effective lithium salt participating in the charge and discharge of the liquid electrolyte 160 is gradually decreased due to lithium precipitation, etc., but due to the concentration gradient of the lithium salt between the gel electrolyte 150 and the liquid electrolyte 160, the first lithium salt of the gel electrolyte 150, which is a solute, moves to the liquid electrolyte 160, and the liquid electrolyte 160 can be replenished with the lithium salt that is insufficient. As a result, although the battery cell 100 of the present invention is manufactured using the liquid electrolyte 160 with a relatively low concentration, the effective lithium salt participating in the charge and discharge of the liquid electrolyte 160 can be prevented from being depleted even if the battery cell 100 is charged and discharged multiple times, so that the life of the battery cell 100 can be effectively increased. In this regard, the present application proves the effect by the experimental example described below. Meanwhile, the method for manufacturing a battery cell of the present invention will be described in more detail below.

[0103] Battery cell manufacturing method According to one embodiment of the present invention, the method for manufacturing a battery cell of the present invention includes: preparing an electrode assembly including a plurality of electrodes, electrode tabs formed on at least one side of each of the plurality of electrodes, and separators interposed between the plurality of electrodes; disposing the electrode assembly in an accommodating space of a cell case; Injecting a gel electrolyte composition into the receiving space, the gel electrolyte composition including a first lithium salt having a first molar concentration and a curable compound, and then disposing the gel electrolyte composition around the electrode tab; curing the gel electrolyte composition to form a gel electrolyte surrounding the electrode tabs; and injecting a liquid electrolyte comprising a second lithium salt at a second molar concentration so as to be contained between the plurality of electrodes.

[0104] First, based on FIGS. 1, 4, and 5, FIGS. 6 to 11 show a manufacturing method for manufacturing a battery cell 100 of the present invention. First, a method for manufacturing a battery cell 100 according to an embodiment of the present invention may include the steps of: preparing an electrode assembly including a plurality of electrodes 122p, 122n, electrode tabs 121 formed on at least one side of each of the plurality of electrodes 122p, 122n, and a separator interposed between the plurality of electrodes 122p, 122n; disposing the electrode assembly 120 in an accommodation space 110p1 of a cell case 110; injecting a gel electrolyte composition including a first lithium salt with a first molar concentration and a curable compound into the accommodation space 110p1 so as to surround the electrode tabs; curing the gel electrolyte composition to prevent the electrode tabs 121 from flowing, and disposing a gel electrolyte around the electrode tabs; and injecting a liquid electrolyte 160 including a second lithium salt with a second molar concentration to be accommodated between the plurality of electrodes 122p, 122n.

[0105] In this case, the step of preparing the electrode assembly 120 may include a step of sequentially stacking a positive electrode 122p having a positive electrode tab 121a formed on one side, a separator 170, and a negative electrode 122n having a negative electrode tab 121b formed on one side to form the electrode assembly 120. In this case, the electrodes 122p and 122n may have an electrode tab 121 formed on at least one side.

[0106] In one embodiment, the step of disposing the electrode assembly 120 in the receiving space 110p1 of the pouch 114 includes disposing the electrode assembly 120 including the electrodes 122 with the electrode tabs 121 formed on at least one side and the separator 170 interposed between the electrodes 122 in the receiving space 110p1 of the pouch 114. Here, the pouch 114 can be said to be a configuration in a stage prior to manufacturing the cell case 110 in which the receiving space 110p1 is completely sealed. The pouch 114 may be formed by bonding the outer peripheries of the first cell sheet 114T and the second cell sheet 114P to each other. The pouch 114 may be formed with a receiving space 110p1 capable of containing the electrode tabs 121, the electrode assembly 120, the gel electrolyte composition 155, and the liquid electrolyte 160.

[0107] For example, the electrode tab 121 may be located on the first side 120a of the electrode assembly 120. However, the present invention is not limited to this embodiment, and in a battery cell (not shown) manufactured by a manufacturing method according to another embodiment, the electrode tab 121 may be located on each of the first side 120a and the third side 120c of the electrode assembly 120. In this case, the gel electrolyte 150 may be disposed on each of the first side 120a and the third side 120c of the electrode assembly 120 in the accommodation space 110p1 of the pouch 114. In this case, the liquid electrolyte 160 may be located between the electrode 122 and the separator 170, between the electrodes 122, and on the second side 120b and the fourth side 120d of the electrode assembly 120 in the accommodation space 110p1.

[0108] Therefore, according to this configuration of the present invention, compared to the conventional battery cell 100 in which the liquid electrolyte 160 surrounds the electrode tab 121, the manufacturing method of the present invention makes it possible to manufacture a battery cell 100 in which the connection portion between the electrode tab 121 and the electrode 122 or the folded portion of the electrode tab 121 can be effectively prevented from being broken by preventing the electrode tab 121 from flowing using the gel electrolyte 150 surrounding the electrode tab 121.

[0109] In addition, the manufacturing method of the present invention allows the manufactured battery cell 100 to form a passivation film 123 on the surface of the electrode tab 121, thereby preventing the electrode tab 121 from being broken due to corrosion of the electrode tab 121 caused by the lithium salt contained in the electrolyte of a conventional battery cell, thereby effectively improving the durability of the battery cell 100.

[0110] Specifically, FIG. 6 shows a front view illustrating a state in which multiple electrodes 122p, 122n are inserted into the accommodation space 110p1 of the pouch 114 in a manufacturing method for a battery cell 100 according to another embodiment of the present invention.

[0111] 7 is a front view showing the state inside the pouch in which the above-mentioned gel electrolyte composition 155 is injected into the housing space 110p1 in a manufacturing method of a battery cell 100 according to another embodiment of the present invention. For reference, in FIG. 7, for convenience of explanation of the drawings, the pouch 114 is shown transparently so that the state inside the pouch 114 can be seen from the outside.

[0112] 6, after the step of inserting an electrode assembly (not shown) into the storage space 110p1 of the cell sheet, the first cell sheet 114T and the second cell sheet 114P are laminated to form the pouch 114, and the first outer periphery 114a, the third outer periphery 114c, and the fourth outer periphery 114d are heat-sealed to each other except for a part of the outer periphery, for example, the second outer periphery 114b, to form the seal portion 111. In addition, the gel electrolyte composition 155 or the liquid electrolyte 160 is configured to flow into the storage space 110p1 through the gap between the second outer periphery 114b, which is spaced apart from the first cell sheet 114T and the second cell sheet 114P, without being heat-sealed.

[0113] 2, 5, and 7, an injection space 110p2 may be formed in the second outer periphery 114b region by the heat fusion process of the outer periphery. The injection space 110p2 may be a space located on one side (upper side) of the receiving space 110p1 in which the electrode 122 is received, among the internal spaces formed between the first cell sheet 114T and the second cell sheet 114P. For example, the region from the opened second outer periphery 114b of the pouch 114 to the front of the receiving space 110p1 may be set as the injection space 110p2. The injection space 110p2 may be configured to communicate with the receiving space 110p1. The injection space 110p2 may serve as a passageway for the gel electrolyte composition 155 or the liquid electrolyte 160 to move to the receiving space 110p1.

[0114] Referring to FIG. 7, the manufacturing method of the battery cell 100 of the present invention may further include a step of heat-sealing a portion between the injection space 110p2 and the storage space 110p1 of the pouch 114 to form a blocking portion 113 before injecting the gel electrolyte composition.

[0115] The blocking portion 113 may be formed by heat sealing from the first outer periphery 114a to the third outer periphery 114c of the pouch 114. Such a blocking portion can prevent the gel electrolyte composition injected into the accommodation space from migrating back to the injection space before the gel electrolyte composition is cured. This makes it easy to maintain the gel electrolyte composition arranged to surround the electrode tab until the gel electrolyte composition is cured, and therefore the efficiency of the manufacturing process can be significantly improved.

[0116] Referring to FIG. 7 together with FIG. 3, a gel electrolyte composition 155 containing the first lithium salt having the above-mentioned first molar concentration and a curable compound is injected into the inside of the accommodation space 110p1 through the injection space 110p2 so as to surround the electrode tab 121.

[0117] The gel electrolyte composition 155 may be configured to be a liquid electrolyte before curing, and to change from the liquid electrolyte to a gel phase electrolyte by curing the curable compound in a subsequent step. In addition, the gel electrolyte composition 155 may be disposed in the receiving space 110p1 so as to surround the outer surfaces of the electrode tabs 121 or to fill the spaces between the electrode tabs 121 after injection.

[0118] 8 is a front view showing the state inside the pouch where the gel electrolyte composition 155 is thermally cured in the containing space 110p1 in the manufacturing method of the battery cell 100 of the present invention. For reference, in FIG. 8, for convenience of explanation of the drawing, the pouch 114 is shown transparently so that the state inside the pouch 114 can be seen from the outside.

[0119] 8, the step of changing the gel electrolyte composition 155 into the gel electrolyte 150 in the gel phase so as to prevent the electrode tab 121 from flowing includes the step of injecting the gel electrolyte composition 155 into the receiving space 110p1 so as to surround the electrode tab 121, and then rotating the pouch 114 so that the electrode tab 121 faces downward. That is, the gel electrolyte composition 155 can move by gravity so as to surround the electrode tab 121.

[0120] In one embodiment, the curing step may include a step of curing the gel electrolyte composition 155 arranged in the accommodation space 110p1 so as to surround the electrode tab 121 into a gel phase. For example, when the gel electrolyte composition 155 contains a thermosetting compound, the gel electrolyte composition 155 can be thermally cured by storing the gel electrolyte composition 155 in a thermostatic chamber set at a predetermined temperature for a predetermined time or more. The thermosetting compound is heated to form crosslinks through a thermal polymerization reaction, and the gel electrolyte composition 155 in a liquid state can be converted into a gel state. For example, when the pouch 114 is stored in a thermostatic chamber, the pouch 114 can be stored in a thermostatic chamber at 60 degrees Celsius for 5 to 24 hours to convert the gel electrolyte composition 155 into a gel state.

[0121] Therefore, according to this configuration of the present invention, the manufacturing method of the battery cell 100 can manufacture a battery cell 100 in which the gel electrolyte 150 prevents the electrode tabs 121 from flowing and reduces deformation when an external impact is applied to the battery cell 100, compared to the conventional battery cell 100 in which the liquid electrolyte 160 surrounds the electrode tabs 121. As a result, the manufacturing method of the battery cell 100 of the present invention can effectively improve the durability of the battery cell 100.

[0122] Fig. 9 is a side view showing a state before the battery cell 100 is fixed using the fixing jig 210 while the gel electrolyte composition 155 is curing in the battery cell manufacturing method according to the present invention. Fig. 10 is a side view showing a state after the battery cell 100 has been fixed using the fixing jig 210 while the gel electrolyte composition 155 is curing in the battery cell manufacturing method according to the present invention. For convenience of explanation, electrode tabs 121 and the like are not shown in Figs. 9 and 10.

[0123] 9 and 10, in the step of injecting the gel electrolyte composition 155 containing the curable compound into the accommodation space 110p1 so as to surround the electrode tab 121, when the gel electrolyte composition 155 is injected into the pouch 114, a portion of the accommodation space 110p1 of the pouch 114 in which the gel electrolyte composition 155 is accommodated may be deformed in a convex shape toward the outside due to the fluidity of the gel electrolyte composition 155. When the gel electrolyte composition 155 is cured in such a way that a portion of the accommodation space 110p1 of the pouch 114 is deformed in a convex shape, the shape of the deformation may differ for each product, making it difficult to ensure consistent quality of the product, and the appearance of the pouch 114 may not be smooth, resulting in defects.

[0124] Thus, the step of changing the gel electrolyte composition 155 into the gel electrolyte 150 in the gel phase so as to prevent the electrode tab 121 from flowing in the manufacturing method of the present invention may include a step of pressurizing and fixing the pouch 114 while the gel electrolyte composition 155 is hardening. In this case, the pouch 114 may be fixed by applying pressure to both outer sides using a fixing jig 210. Specifically, the fixing jig 210 may include a first jig plate 212 and a second jig plate 213. Each of the first jig plate 212 and the second jig plate 213 may have a size corresponding to or larger than one side of the pouch 114. That is, each of the first jig plate 212 and the second jig plate 213 may have a size capable of covering the pouch 114. The pouch 114 and the electrode assembly 120 accommodated inside the pouch 114 may be interposed between the first jig plate 212 and the second jig plate 213. Then, a portion of the accommodation space 110p1 of the pouch 114 that has been deformed into a convex shape can be pressurized by the first jig plate 212 and the second jig plate 213.

[0125] The fixture 210 may further include a receiving base 211, a first support 214, and a second support 215. The first support 214 and the second support 215 may be located on both sides (Y-axis direction) of the pouch 114. The receiving base 211 may be configured to be mounted on the ground so that the fixture 210 can be stably positioned on the ground. The receiving base 211 may have a plate shape extending parallel to the ground. For example, as shown in FIG. 12, the first support 214 may include a column portion 214a extending from the upper surface of the receiving base 211 in the upward direction (Z-axis direction) and a connecting portion 214b extending horizontally from the column portion 214a and connected to the side portion of the first fixture plate 212 in the positive direction of the Y-axis. In addition, the second support 215 may include a pillar portion 215a extending upward from the upper surface of the receiving base 211, and a connecting portion 215b extending horizontally from the pillar portion 215a and connected to the side portion of the second jig plate 213 in the negative direction of the Y axis.

[0126] Furthermore, the first support 214 and the second support 215 can be configured to be movable in a direction approaching each other or in a direction away from each other on the receiving stand 211. For example, when the first support 214 and the second support 215 move in a direction approaching each other, the first jig plate 212 and the second jig plate 213 connected to the first support 214 and the second support 215, respectively, can move to approach each other. At this time, the pouch 114 and the electrode assembly 120 housed in the pouch 114 can be fixed by applying pressure to both outsides of the pouch 114 located between the first jig plate 212 and the second jig plate 213. For example, when the hardening of the gel electrolyte composition 155 is completed, the first support 214 and the second support 215 can be moved in a direction away from each other to release the fixed state of the pouch 114. For example, as shown in Fig. 9, the pouch 114 may have a shape in which a portion of the storage space 110p1 of the pouch 114 protrudes in a convex shape due to the gel electrolyte composition 155. However, as shown in Fig. 10, when the first support 214 and the second support 215 move toward the pouch 114, the pouch 114 is pressurized by the first jig plate 212 and the second jig plate 213, and such pressurization can guide the storage space 110p1, which has become convex due to the gel electrolyte composition 155, to deform into an inward shape.

[0127] Therefore, according to this configuration of the present invention, the manufacturing method of the present invention includes a step of pressurizing and fixing the pouch 114 while the gel electrolyte composition 155 is hardening so as to prevent the electrode tab 121 from flowing, thereby making it possible to stably fix the electrode assembly 120 accommodated inside the pouch 114 and to prevent the gel electrolyte composition 155 from solidifying in a state in which a portion of the accommodation space 110p1 of the pouch 114 is deformed into an outwardly convex shape due to the gel electrolyte composition 155. As a result, the manufacturing method of the present invention can effectively reduce the defective rate of the manufactured battery cells 100.

[0128] 11 is a perspective view showing the state inside pouch 114 in which liquid electrolyte 160 is being injected into accommodation space 110p1 in a battery cell manufacturing method according to the present invention. For reference, in FIG. 11, for the convenience of illustrating the drawing, pouch 114 is shown as transparent so that the inside can be seen from the outside.

[0129] 2, 4, 8, and 11 again, the method of manufacturing a battery cell according to the present invention may further include a step of rotating the electrode assembly 120 so that the electrode tab 121 is located in the X-axis direction before the step of injecting the liquid electrolyte 160. In this case, the pouch 114 may be in a form that is upright in the vertical direction (Z-axis direction) based on the ground so that the receiving space 110p1 is seen from the front based on the ground in FIG. 11. In this case, since the gel electrolyte composition 155 has already changed into a gel phase to form the gel electrolyte 150, even when the pouch 114 is rotated and disposed so that the electrode tab 121 is located at the side (X-axis direction) of the electrode assembly 120, the gel electrolyte 150 does not move to another position in the receiving space 110p1. The liquid electrolyte 160 may be filled in the remaining space of the receiving space 110p1 where the gel electrolyte 150 is not located.

[0130] Specifically, the step of injecting the liquid electrolyte 160 may include a step of injecting the liquid electrolyte 160 through the injection space 110p2 via the open second outer periphery 114b of the first cell sheet 114T and the second cell sheet 114P into the receiving space 110p1. In this case, the liquid electrolyte 160 may be positioned between the electrodes 122 and to surround the other side of the electrode 122 where the electrode tab 121 is not positioned. For example, the liquid electrolyte 160 may be positioned between the electrodes 122 and on the outermost side of the electrode 122. Also, as shown in FIG. 11, the liquid electrolyte 160 may be positioned to surround the second side 120b, the third side 120c, and the fourth side 120d of the electrode assembly 120.

[0131] In addition, in the battery cell manufacturing method of the present invention, by injecting highly fluid liquid electrolyte 160 containing a second lithium salt having a second molar concentration lower than that of gel electrolyte 150, the time required for absorption into the electrodes of electrode assembly 120 is shortened and the wettability of the electrodes is improved, thereby improving the initial charge / discharge efficiency, shortening the manufacturing time of battery cell 100, and effectively reducing manufacturing costs.

[0132] Fig. 12 is a front view showing one side of the containing space 110p1 of the pouch 114 being further sealed in the battery cell manufacturing method according to the present invention. Fig. 13 is a front view showing the injection space 110p2 of the pouch 114 being removed in the battery cell manufacturing method according to the present invention.

[0133] 12 and 13 together with FIG. 4, the manufacturing method of the battery cell 100 according to the present invention may further include a step of sealing the accommodation space 110p1 of the pouch 114 and a step of cutting the region of the injection space 110p2. Specifically, the step of sealing the accommodation space 110p1 of the pouch 114 may include heat sealing the entire boundary portion between the accommodation space 110p1 of the pouch 114 and the injection space 110p2. For example, as shown in FIG. 12, the first outer periphery 114a to the third outer periphery 114c of the pouch 114 may be heat sealed along the boundary between the accommodation space 110p1 of the pouch 114 and the injection space 110p2 of the pouch 114 to form the seal portion 111. For example, in the manufacturing method of the battery cell 100 of Figure 7 described above, when a portion between the injection space 110p2 and the storage space 110p1 of the pouch 114 is heat-sealed to form the blocking portion 113, the blocking portion 113 can be heat-sealed to the third outer peripheral portion 114c of the pouch 114 to further form the sealing portion 111.

[0134] Also, a cutting line (L) can be set on the outside of the seal portion 111. Then, as shown in FIG. 13, the region of the injection space 110p2 of the pouch 114 can be removed by cutting along the cutting line (L).

[0135] Furthermore, in the manufacturing method according to another embodiment of the present invention, a battery activation process may be performed before the step of sealing the accommodation space 110p1 of the pouch 114 performed in FIG. 12. Here, the battery activation process is a process of performing a charge / discharge operation for the first time in the battery cell 100. A large amount of gas is generated during the charge / discharge operation of the battery cell 100. The gas thus generated moves from the accommodation space 110p1 to the injection space 110p2 and can be discharged to the outside through the opened second outer periphery 114b of the pouch 114. In such a battery activation process, the magnitude of the charging current and the charging / discharging time may vary depending on the materials of the positive electrode 122p and the negative electrode 122n.

[0136] In addition, the manufacturing method according to the present invention may perform a battery aging process after the step of sealing the receiving space 110p1 of the pouch 114. At this time, the temperature may be, for example, 45 to 70 degrees Celsius, and the aging time may be 1 to 3 days.

[0137] The battery cell 100 manufactured by the manufacturing method of the present invention as described above has the gel electrolyte 150 with low fluidity arranged in a form surrounding the electrode tab 121, thereby preventing the electrode tab 121 from flowing and deforming due to an external impact, compared to a battery cell 100 in which the conventional liquid electrolyte 160 surrounds the electrode tab 121. Therefore, when the battery cell 100 of the present invention is applied to an automobile, even if the battery cell 100 is subjected to frequent impacts and vibrations that occur during travel, the gel electrolyte 150 can minimize the flow of the electrode tab 121 to prevent disconnection, thereby increasing the lifespan, and also preventing inactivation of the electrode 122 and improving reduction in battery capacity.

[0138] The battery cell 100 manufactured by the manufacturing method of the present invention as described above maximizes the amount of fluid liquid electrolyte 160 in the space between the accommodation space 110p1 and the electrode assembly 120, and includes a gel electrolyte 150 containing a first lithium salt at a first molar concentration higher than the second concentration of the second lithium salt in the liquid electrolyte 160. Therefore, even if the second lithium salt in the liquid electrolyte 160 decreases due to repeated charging and discharging, the first lithium salt moves from the gel electrolyte 150, which is a solute, to the liquid electrolyte 160 due to the concentration gradient of the lithium salt with the gel electrolyte 150, and replenishes the deficient lithium salt in the liquid electrolyte 160. This prevents the lithium salt in the liquid electrolyte 160 from being depleted, and effectively increases the life of the battery cell 100.

[0139] Meanwhile, FIG. 14 is a perspective view that diagrammatically illustrates a battery module 1000 according to one embodiment of the present invention. 14 together with FIG. 1, the present invention may provide a battery module 1000 including at least one battery cell 100. The battery module 1000 may include a module housing 1100 that accommodates at least one battery cell 100 therein, an external output terminal 1200 provided at a front end of the module housing 1100, and a control unit 1300 that controls charging and discharging of the battery cell 100. In addition, when two or more battery cells 100 are provided, the battery module 1000 may further include a bus bar (not shown) that electrically connects the two or more battery cells 100. The bus bar may be electrically connected to the electrode lead 130 of each of the battery cells 100. The battery module 1000 of the present invention may apply a known configuration to essential configurations other than the battery cell 100, and therefore a description of such configurations will be omitted.

[0140] The present invention will be described in detail below with reference to examples. However, the examples of the present invention may be modified in various different forms, and the scope of the present invention should not be construed as being limited to the examples described below. The examples of the present invention are provided to more completely explain the present invention to those having ordinary skill in the art.

[0141] Working Example Example 1 (Production of liquid electrolytes) LiPF6 was dissolved at a concentration of 0.75M in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (EMC) was mixed at a volume ratio of 30:70, and then vinylene carbonate (VC) was added at 1 wt% as an additive to prepare a liquid electrolyte. The viscosity of the liquid electrolyte was 2.5 cP.

[0142] (Production of gel electrolyte composition) LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (DMC) was mixed in a volume ratio of 30:70 so that the molar concentration was 2.0M, and then 5wt% of trimethylolpropane triacrylate was added as a curable polymer, 1wt% of AIBN (2,2'-azobis (iso-butyronitrile)) was added as a polymerization initiator, and 1wt% of vinylene carbonate (VC) was added to produce a gel electrolyte composition. At this time, the viscosity of the gel electrolyte composition was 8.0cP.

[0143] (Manufacturing of electrode assemblies) Cathode active material (Li(Ni) 0.8 Co 0.1 Mn 0.1A cathode active material slurry (solid content: 48% by weight) was prepared by adding a cathode active material (carbon powder), a binder (styrene-butadiene rubber, SBR), sodium carboxymethyl cellulose (CMC), and a conductive material (carbon black) in a weight ratio of 96:2:1:1 to water as a solvent. A cathode active material slurry (solid content: 70% by weight) was prepared by adding a cathode active material (carbon powder), a binder (styrene-butadiene rubber, SBR), sodium carboxymethyl cellulose (CMC), and a conductive material (carbon black) in a weight ratio of 96:2:1:1 to water as a solvent. The negative electrode active material slurry was applied to a negative electrode current collector (Cu thin film) with a thickness of 10 μm, dried, and then roll-pressed to prepare a negative electrode. The positive electrode, a separator made of three layers of polypropylene / polyethylene / polypropylene (PP / PE / PP), and the negative electrode were stacked to prepare an electrode assembly.

[0144] (Battery cell manufacturing) After preparing the electrode assembly manufactured by the above method, it was housed in a pouch, and the gel electrolyte composition manufactured as above was poured into the storage space so as to surround the electrode tab, and then the pouch was stored at a high temperature of 60°C for 5 hours in a thermostatic chamber to thermally harden the gel electrolyte composition into a gel electrolyte. Next, the liquid electrolyte manufactured as above was poured into the storage space of the pouch so that the electrode assembly was impregnated, and the pouch was sealed to manufacture a battery cell. At this time, the volume ratio of the liquid electrolyte and the gel electrolyte composition poured into the pouch was about 100:25.

[0145] Example 2 (Production of liquid electrolytes) LiPF6 and LiN(SO2F)2 (LiFSI) were dissolved in a non-aqueous organic solvent, ethylene carbonate (EC): ethyl methyl carbonate (EMC) mixed at a volume ratio of 30:70, to make the concentrations 0.3M and 0.7M, respectively. Then, 1wt% vinylene carbonate (VC) was added to produce a liquid electrolyte. At this time, the viscosity of the liquid electrolyte was 3.4cP.

[0146] (Production of gel electrolyte composition) LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (DMC) was mixed in a volume ratio of 30:70 so that the molar concentration was 2.0M. Then, 5wt% of trimethylolpropane triacrylate was added as a curable polymer, and 1wt% of AIBN (2,2'-azobis (iso-butyronitrile)) and 1wt% of vinylene carbonate (VC) were added as polymerization initiators to produce a gel electrolyte composition. At this time, the viscosity of the gel electrolyte was 8.0cP.

[0147] (Battery cell manufacturing) The electrode assembly prepared in Example 1 was housed in a pouch, and the gel electrolyte composition prepared above was poured into the housing space so as to surround the electrode tabs. The pouch was then stored in a thermostatic chamber at a high temperature of 60° C. for 5 hours, whereby the gel electrolyte composition was thermally cured into a gel electrolyte.

[0148] Next, the liquid electrolyte prepared above was injected into the receiving space of the pouch so as to impregnate the electrode assembly, and the pouch was then sealed to manufacture a battery cell. At this time, the volume ratio of the liquid electrolyte and the gel electrolyte composition injected into the pouch was about 100:25.

[0149] Example 3 (Production of liquid electrolytes) LiPF6 and LiN(SO2F)2 (LiFSI) were dissolved in a non-aqueous organic solvent, ethylene carbonate (EC): ethyl methyl carbonate (EMC) mixed at a volume ratio of 30:70, to 0.7M and 0.7M, respectively. Then, 1wt% vinylene carbonate (VC) was added to produce a liquid electrolyte. At this time, the viscosity of the liquid electrolyte was 3.4cP.

[0150] (Battery cell manufacturing) A battery cell was manufactured in the same manner as in Example 2, except that the liquid electrolyte prepared above was poured into the storage space of the pouch. At this time, the volume ratio of the liquid electrolyte and the gel electrolyte composition poured into the pouch was about 100:25.

[0151] (Battery cell manufacturing) The electrode assembly prepared in Example 1 was housed in a pouch, and the gel electrolyte composition prepared above was poured into the housing space so as to surround the electrode tabs. The pouch was then stored in a thermostatic chamber at a high temperature of 60° C. for 5 hours, whereby the gel electrolyte composition was thermally cured into a gel electrolyte.

[0152] Next, the liquid electrolyte prepared above was injected into the receiving space of the pouch so as to impregnate the electrode assembly, and the pouch was then sealed to manufacture a battery cell. At this time, the volume ratio of the liquid electrolyte and the gel electrolyte composition injected into the pouch was about 100:25.

[0153] Example 4 (Production of liquid electrolytes) LiPF6 and LiN(SO2F)2 (LiFSI) were dissolved in a non-aqueous organic solvent, ethylene carbonate (EC): ethyl methyl carbonate (EMC) mixed at a volume ratio of 30:70, to make the concentrations 0.3M and 0.7M, respectively. Then, 1wt% vinylene carbonate (VC) was added to produce a liquid electrolyte. At this time, the viscosity of the liquid electrolyte was 3.4cP.

[0154] (Production of gel electrolyte composition) LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (DMC) was mixed in a volume ratio of 30:70 so that the molar concentration was 5.0M. Then, 5 wt% of trimethylolpropane triacrylate was added as a curable polymer, and 1 wt% of AIBN (2,2'-azobis (iso-butyronitrile)) and 1 wt% of vinylene carbonate (VC) were added as polymerization initiators to produce a gel electrolyte composition. At this time, the viscosity of the gel electrolyte was 34.0 cP.

[0155] (Battery cell manufacturing) The electrode assembly prepared in Example 1 was housed in a pouch, and the gel electrolyte composition prepared above was poured into the housing space so as to surround the electrode tabs. The pouch was then stored in a thermostatic chamber at a high temperature of 60° C. for 5 hours, whereby the gel electrolyte composition was thermally cured into a gel electrolyte.

[0156] Next, the liquid electrolyte prepared above was injected into the receiving space of the pouch so as to impregnate the electrode assembly, and the pouch was then sealed to manufacture a battery cell. At this time, the volume ratio of the liquid electrolyte and the gel electrolyte composition injected into the pouch was about 100:25.

[0157] Example 5 (Production of liquid electrolytes) LiPF6 and LiN(SO2F)2 (LiFSI) were dissolved in a non-aqueous organic solvent, ethylene carbonate (EC): ethyl methyl carbonate (EMC) mixed at a volume ratio of 30:70, to make the concentrations 0.3M and 0.7M, respectively. Then, 1wt% vinylene carbonate (VC) was added to produce a liquid electrolyte. At this time, the viscosity of the liquid electrolyte was 3.4cP.

[0158] (Production of gel electrolyte composition) LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (DMC) was mixed in a volume ratio of 30:70 so that the molar concentration was 6.0M. Then, 5 wt% of trimethylolpropane triacrylate was added as a curable polymer, and 1 wt% of AIBN (2,2'-azobis (iso-butyronitrile)) and 1 wt% of vinylene carbonate (VC) were added as polymerization initiators to produce a gel electrolyte composition. At this time, the viscosity of the gel electrolyte was 62.0 cP.

[0159] (Battery cell manufacturing) The electrode assembly prepared in Example 1 was housed in a pouch, and the gel electrolyte composition prepared above was poured into the housing space so as to surround the electrode tabs. The pouch was then stored in a thermostatic chamber at a high temperature of 60° C. for 5 hours, whereby the gel electrolyte composition was thermally cured into a gel electrolyte.

[0160] Next, the liquid electrolyte prepared above was injected into the receiving space of the pouch so as to impregnate the electrode assembly, and the pouch was then sealed to manufacture a battery cell. At this time, the volume ratio of the liquid electrolyte and the gel electrolyte composition injected into the pouch was about 100:25.

[0161] Comparative Example 1 (Production of liquid electrolytes) LiPF6 was dissolved at a concentration of 1.0M in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (EMC) was mixed at a volume ratio of 30:70, and then vinylene carbonate (VC) was added at 1 wt% as an additive to prepare a liquid electrolyte. The viscosity of the liquid electrolyte was 3.3 cP.

[0162] (Production of gel electrolyte composition) LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (DMC) was mixed in a volume ratio of 30:70 so that the molar concentration was 1.0M, and then 5wt% of trimethylolpropane triacrylate was added as a curable polymer, 1wt% of AIBN (2,2'-azobis (iso-butyronitrile)) was added as a polymerization initiator, and 1wt% of vinylene carbonate (VC) was added to produce a gel electrolyte composition. At this time, the viscosity of the gel electrolyte composition was 4.7cP.

[0163] (Battery cell manufacturing) The electrode assembly prepared in Example 1 was housed in a pouch, and the gel electrolyte composition prepared above was poured into the housing space so as to surround the electrode tabs. The pouch was then stored in a thermostatic chamber at a high temperature of 60° C. for 5 hours, whereby the gel electrolyte composition was thermally cured into a gel electrolyte.

[0164] Next, the liquid electrolyte prepared above was injected into the receiving space of the pouch so as to impregnate the electrode assembly, and the pouch was then sealed to manufacture a battery cell. At this time, the volume ratio of the liquid electrolyte and the gel electrolyte composition injected into the pouch was about 100:25.

[0165] Comparative Example 2 (Production of liquid electrolytes) LiPF6 was dissolved at a concentration of 0.5M in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (EMC) was mixed at a volume ratio of 30:70, and then vinylene carbonate (VC) was added at 1 wt% as an additive to prepare a liquid electrolyte. The viscosity of the liquid electrolyte was 1.7 cP.

[0166] (Production of gel electrolyte composition) LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (DMC) was mixed in a volume ratio of 30:70 so that the molar concentration was 0.5M, and then 5wt% of trimethylolpropane triacrylate was added as a curable polymer, 1wt% of AIBN (2,2'-azobis (iso-butyronitrile)) was added as a polymerization initiator, and 1wt% of vinylene carbonate (VC) was added to produce a gel electrolyte composition. At this time, the viscosity of the gel electrolyte composition was 2.0cP.

[0167] (Battery cell manufacturing) The electrode assembly prepared in Example 1 was housed in a pouch, and the gel electrolyte composition prepared above was poured into the housing space so as to surround the electrode tabs. The pouch was then stored in a thermostatic chamber at a high temperature of 60° C. for 5 hours, whereby the gel electrolyte composition was thermally cured into a gel electrolyte.

[0168] Next, the liquid electrolyte prepared above was injected into the receiving space of the pouch so as to impregnate the electrode assembly, and the pouch was then sealed to manufacture a battery cell. At this time, the volume ratio of the liquid electrolyte and the gel electrolyte composition injected into the pouch was about 100:25.

[0169] Comparative Example 3 (Production of liquid electrolytes) LiPF6 was dissolved at a concentration of 2.0M in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (EMC) was mixed at a volume ratio of 30:70, and then vinylene carbonate (VC) was added at 1 wt% as an additive to prepare a liquid electrolyte. The viscosity of the liquid electrolyte was 6.7 cP.

[0170] (Production of gel electrolyte composition) LiPF6 was dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (DMC) was mixed in a volume ratio of 30:70 so that the molar concentration was 2.0M, and then 5wt% of trimethylolpropane triacrylate was added as a curable polymer, 1wt% of AIBN (2,2'-azobis (iso-butyronitrile)) was added as a polymerization initiator, and 1wt% of vinylene carbonate (VC) was added to produce a gel electrolyte composition. At this time, the viscosity of the gel electrolyte composition was 8.0cP.

[0171] (Battery cell manufacturing) The electrode assembly prepared in Example 1 was housed in a pouch, and the gel electrolyte composition prepared above was poured into the housing space so as to surround the electrode tabs. The pouch was then stored in a thermostatic chamber at a high temperature of 60° C. for 5 hours, whereby the gel electrolyte composition was thermally cured into a gel electrolyte.

[0172] Next, the liquid electrolyte prepared above was injected into the receiving space of the pouch so as to impregnate the electrode assembly, and the pouch was then sealed to manufacture a battery cell. At this time, the volume ratio of the liquid electrolyte and the gel electrolyte composition injected into the pouch was about 100:25.

[0173] Comparative Example 4 (Production of liquid electrolytes) A liquid electrolyte was prepared by dissolving LiN(SO2F)2 at a concentration of 1.0M in a non-aqueous organic solvent in which ethylene carbonate (EC):ethyl methyl carbonate (EMC) was mixed at a volume ratio of 30:70, and then adding 1wt% vinylene carbonate (VC) as an additive. The viscosity of the liquid electrolyte was 3.5cP.

[0174] (Production of gel electrolyte composition) LiN(SO2F)2 was dissolved to 1.0M in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (DMC) was mixed in a volume ratio of 30:70, and then 5wt% of trimethylolpropane triacrylate was added as a curable polymer, 1wt% of AIBN (2,2'-azobis (iso-butyronitrile)) was added as a polymerization initiator, and 1wt% of vinylene carbonate (VC) was added to produce a gel electrolyte composition. At this time, the viscosity of the gel electrolyte was 5.0cP.

[0175] (Battery cell manufacturing) Except for injecting the liquid electrolyte and gel electrolyte compositions prepared above, a battery cell was manufactured in the same manner as in Example 1. At this time, the volume ratio of the liquid electrolyte and the gel electrolyte composition injected into the pouch was about 100:25.

[0176] Comparative Example 5 (Production of liquid electrolytes) LiPF6 and LiN(SO2F)2 were dissolved in a non-aqueous organic solvent, which was a mixture of ethylene carbonate (EC): ethyl methyl carbonate (EMC) in a volume ratio of 30:70, to give concentrations of 0.7M and 0.3M, respectively, and then vinylene carbonate (VC) was added at 1wt% as an additive to produce a liquid electrolyte. The viscosity of the liquid electrolyte was 3.4cP.

[0177] (Production of gel electrolyte composition) LiPF6 and LiN(SO2F)2 were dissolved in a non-aqueous organic solvent in which ethylene carbonate (EC): ethyl methyl carbonate (DMC) was mixed in a volume ratio of 30:70 to make 0.7M and 0.3M, respectively, and then 5wt% of trimethylolpropane triacrylate was added as a curable polymer, 1wt% of AIBN (2,2'-azobis (iso-butyronitrile)) was added as a polymerization initiator, and 1wt% of vinylene carbonate (VC) was added to produce a gel electrolyte composition. At this time, the viscosity of the gel electrolyte was 4.8cP.

[0178] (Battery cell manufacturing) The electrode assembly prepared in Example 1 was housed in a pouch, and the gel electrolyte composition prepared above was poured into the housing space so as to surround the electrode tabs. The pouch was then stored in a thermostatic chamber at a high temperature of 60° C. for 5 hours, whereby the gel electrolyte composition was thermally cured into a gel electrolyte.

[0179] Next, the liquid electrolyte prepared above was injected into the receiving space of the pouch so as to impregnate the electrode assembly, and the pouch was then sealed to manufacture a battery cell. At this time, the volume ratio of the liquid electrolyte and the gel electrolyte composition injected into the pouch was about 100:25.

[0180] Experimental Example Experimental example 1: Evaluation of wettability of liquid electrolyte The time from when 1 ml of the liquid electrolyte applied to each of Example 1, Comparative Example 1, and Comparative Examples 3 to 5 was dropped onto the surface of the negative electrode using a dropper until the liquid electrolyte was completely absorbed by the negative electrode was measured, and the results are shown in the following Table 1. It can be evaluated that the shorter the measured time, the better the relative wettability.

[0181] [Table 1]

[0182] Referring to Table 1, it can be seen that the liquid electrolyte of Example 1 of the present invention has a low concentration of the second lithium salt and a low viscosity, and therefore has relatively better electrode wettability than the liquid electrolytes of Comparative Example 1 and Comparative Examples 3 to 5.

[0183] Experimental example 2: Evaluation of internal resistance Five battery cells each of Example 2 to Example 5 and Comparative Example 1 to Comparative Example 5 were prepared, and then a current of 2.5 C was applied to each electrode lead for 10 seconds while measuring the voltage drop. The internal resistance was then calculated using the following formula (1). Here, "internal resistance" refers to output resistance in electrochemical evaluation. Next, the average rate of change in the internal resistance of each battery cell was expressed as a percentage (%) based on the average internal resistance value of the battery cell of Comparative Example 1, and is shown in Table 2 below. Equation (1): R=V / I, where R is resistance, V is potential, and I is current.

[0184] [Table 2]

[0185] Referring to Table 2, it can be seen that the battery cells of Examples 2 to 5 of the present invention and the battery cell of Comparative Example 3 have a higher total lithium salt concentration in the electrolyte than the battery cell of Comparative Example 1, and therefore the internal resistance is reduced compared to the battery cell of Comparative Example 1. In particular, it can be seen that the rate of change in internal resistance of the battery cell of Example 5, which has the highest total lithium salt concentration, is the lowest.

[0186] On the other hand, it can be seen that the battery cell of Comparative Example 5 uses LiPF6, which has high resistance, and LiFSI, which has low resistance, in combination as the lithium salt in the electrolyte, and thus the internal resistance is reduced compared to the battery cell of Comparative Example 1. Also, in the case of the battery cell of Comparative Example 4, it can be seen that the internal resistance is reduced compared to Comparative Example 1 by excluding the use of LiPF6, which has high resistance, as the lithium salt in the electrolyte.

[0187] In contrast, in the battery cell of Comparative Example 2, the mobility of lithium ions decreased due to a decrease in the concentration of all lithium salts contained in the entire electrolyte, and the internal resistance increased significantly compared to the battery cell of Comparative Example 1.

[0188] Experimental example 3: Evaluation of battery cell life characteristics In order to evaluate the life characteristics of the battery cells manufactured in Examples 1 to 5 and the battery cells manufactured in Comparative Examples 2 to 5, each battery cell was fixed using a fixing jig, and 300 charge / discharge cycles were performed in a temperature atmosphere of 45° C. within a driving voltage range of 2.5 V to 4.2 V, with a charge current (0.33 C, charge cut-off current (cut-off): 1 / 20 C) and a discharge current (0.33 C). At this time, the difference between the charge capacity and discharge capacity of the first charge / discharge cycle of the battery cell was shown as charge / discharge efficiency (%) in Table 3 below. The charge / discharge cycle efficiency of each battery cell after 100 charge / discharge cycles and after 300 charge / discharge cycles was measured and shown in Table 3 below.

[0189] [Table 3]

[0190] Referring to Table 3, the battery cells of Examples 1 to 4 of the present invention have a cycle efficiency of about 98.3% or more for 100 charge / discharge cycles and about 94.7% or more for 300 charge / discharge cycles. That is, the first lithium salt of the gel electrolyte migrates to the liquid electrolyte through the interface between the gel electrolyte and the liquid electrolyte during charging / discharging, and can replenish the lithium salt consumed in the liquid electrolyte, which is considered to provide excellent long-term and short-term life characteristics.

[0191] On the other hand, in the case of the battery cell of Example 5, the gel electrolyte composition contains a slightly large amount of lithium salt, and the viscosity of the gel electrolyte composition increases, which reduces the fluidity of the gel electrolyte composition and makes it difficult to move the gel electrolyte composition to the storage space around the electrode tab. As a result, the liquid electrolyte permeates into the storage space where the tab is formed, causing disconnection of the tab, and the cycle characteristics are slightly deteriorated.

[0192] In the case of the battery cell of Comparative Example 2, the impregnation of the liquid electrolyte and the gel electrolyte is excellent due to the low concentration of lithium salt, so that the initial charge-discharge cycle is superior to that of the Examples. However, as the charge-discharge cycle progresses, the depletion of the lithium salt progresses, and the charge-discharge cycle efficiency decreases.

[0193] In the case of the battery cell of Comparative Example 3, it can be seen that the charge-discharge cycle efficiency is lower than that of the Examples because LiPF6, which is a lithium salt with high resistance, is used alone at a relatively high content.

[0194] In the case of the battery cells of Comparative Example 4 and Comparative Example 5, the initial performance was excellent because the lithium salt for the gel electrolyte contained LiN(SO2F)2, which can cause corrosion of the electrode tabs. However, as the charge / discharge cycles progressed, breakage of the electrode tabs occurred, and the life evaluation was terminated after 100 cycles. In particular, it can be confirmed that in the battery cell of Comparative Example 4, which contains a higher content of LiN(SO2F)2 in the electrolyte, breakage of the tabs occurred more quickly than in the battery cell of Comparative Example 5.

[0195] Experimental example 4: Evaluation of high temperature stability (hot box test) The battery cells manufactured in Examples 1 to 5 and the battery cells manufactured in Comparative Examples 1 to 5 were fully charged to a SOC (State Of Charge) of 100%, and the fully charged battery cells were stored inside a box, and the temperature inside the box was raised from room temperature to 150°C in increments of 2°C, and then the cells were stored at 150°C for 120 minutes. After checking whether the battery cells had ignited during storage, the number of battery cells that had ignited out of the five cells is shown in Table 4 below.

[0196] Experimental Example 5: Evaluation of the durability of electrode tabs The battery cells manufactured in Examples 1 to 5 and the battery cells manufactured in Comparative Examples 1 to 5 were fully charged to a SOC (State Of Charge) of 100%, and the fully charged battery cells were stored in a hot box at 60°C for two weeks, after which the battery cells were disassembled to check whether the positive electrode tabs (aluminum thin film) were broken. At this time, if even one of the positive electrode tabs of the battery cell was broken, it was classified as a battery cell in which the positive electrode tab was broken. The experimental results are shown in Table 4 below.

[0197] [Table 4]

[0198] Referring to Table 4, it was confirmed that in the battery cells of Examples 2 to 4 of the present invention, no battery cells caught fire during the evaluation of high temperature stability, and no breakage of the electrode tabs occurred.

[0199] Meanwhile, in the case of the battery cell of Example 1, it can be confirmed that the absence of LiN(SO2F)2 that can improve high temperature stability caused some ignitions, and in the case of the battery cell of Example 5, it can be confirmed that the liquid electrolyte penetrated into the tab area, causing some disconnection of the tab.

[0200] On the other hand, in the case of the battery cells of Comparative Examples 1 to 3, since the gel electrolyte does not contain LiN(SO2F)2 that induces corrosion of the electrode tabs, disconnection of the electrode tabs does not occur. However, it can be confirmed that the absence of LiN(SO2F)2 that can improve high temperature stability causes fires in most cases.

[0201] In the case of the battery cells of Comparative Example 4 and Comparative Example 5, it can be confirmed that the gel electrolyte contains LiN(SO2F)2, which induces corrosion of the electrode tabs, and therefore breakage of the electrode tabs occurs in most cases.

[0202] Although the embodiments have been described above with limited drawings, those having ordinary skill in the art may apply various technical modifications and variations based on the above. For example, the described techniques may be performed in a different order than described, and / or the components of the described systems, structures, devices, circuits, etc. may be combined or combined in a different manner than described, or may be substituted or replaced by other components or equivalents to achieve suitable results. Accordingly, other embodiments, examples, and equivalents of the claims are within the scope of the following claims. [Explanation of symbols]

[0203] 100: Battery cell 1000: Battery module 110: Cell case 110p1, 110p2: storage space, injection space 113: Cut-off section 114, 114T, 114P: Pouch, 1st cell sheet, 2nd cell sheet 114a, 114b, 114c, 114d: first outer circumference, second outer circumference, third outer circumference, fourth outer circumference 120, 122, 122p, 122n, 170: electrode assembly, electrode, positive electrode, negative electrode, separator 120a, 120b, 120c, 120d: first side, second side, third side, fourth side 121, 121a, 121b: electrode tab, positive electrode tab, negative electrode tab 130, 130a, 130b: electrode lead, positive electrode lead, negative electrode lead 140: Insulating film 111: Seal part 150: Gel electrolyte 155: Gel electrolyte composition 160:Liquid electrolyte 210: Fixture 211, 212, 213: Support, first jig plate, second jig plate 214, 214a, 214b: First support, column, connection part 215, 215a, 215b: Second support, column, connection part X: Interface 123: Passivation film 124:Natural oxide film

Claims

1. a cell case having a storage space; an electrode assembly accommodated in the accommodating space, the electrode assembly including a plurality of electrodes, electrode tabs formed on at least one side of each of the plurality of electrodes, and separators interposed between the plurality of electrodes; a gel electrolyte containing a first lithium salt having a first molar concentration and surrounding the electrode tab and accommodated in the accommodation space; a liquid electrolyte contained between the plurality of electrodes, the liquid electrolyte including a second lithium salt having a second molar concentration lower than the first molar concentration; Including a battery cell.

2. The battery cell according to claim 1 , further comprising a passivation film formed at an interface between the electrode tab and the gel electrolyte by combining a first lithium salt with a cation of the electrode tab.

3. The passivation film is made of AlF 3 3. The battery cell of claim 2 comprising at least one of: LiF; and LiF.

4. The battery cell of claim 1 , wherein the first lithium salt and the second lithium salt are the same or different.

5. The first lithium salt is LiPF 6 and LiBF 4 At least one of The second lithium salt is LiPF 6 13. The battery cell of claim 1 comprising at least one of LiFSI, LiTFSI, and LiBOB.

6. The second lithium salt is at least one of LiFSI, LiTFSI, and LiBOB, and LiPF 6 The battery cell of claim 5 .

7. 2. The battery cell of claim 1, wherein the second molar concentration of the second lithium salt is at least 0.1 M lower than the first molar concentration of the first lithium salt.

8. a first molar concentration of the first lithium salt is between 0.6 M and 5.0 M; 2. The battery cell of claim 1, wherein the second molar concentration of the second lithium salt is between 0.5M and 2.0M.

9. 2. The battery cell of claim 1, wherein a concentration ratio of the second molar concentration of the second lithium salt to the first molar concentration of the first lithium salt is 1:1.3 to 1:

5.

10. 2. The battery cell according to claim 1, wherein the gel electrolyte and the liquid electrolyte are arranged to be in contact with each other, and a first lithium salt contained in the gel electrolyte is configured to be movable to the liquid electrolyte through an interface between the gel electrolyte and the liquid electrolyte.

11. 2. The battery cell of claim 1, wherein the gel electrolyte is located only on one side of the electrode assembly on which the electrode tabs are formed in the receiving space to prevent movement and deformation of the electrode tabs inside the battery cell due to an external impact.

12. The battery cell according to claim 1 , wherein the liquid electrolyte is configured to surround the other side of the electrode assembly on which the gel electrolyte is not formed.

13. A battery module comprising at least one battery cell according to any one of claims 1 to 12.

14. preparing an electrode assembly including a plurality of electrodes, electrode tabs formed on at least one side of each of the plurality of electrodes, and separators interposed between the plurality of electrodes; disposing the electrode assembly in an accommodating space of a cell case; Injecting a gel electrolyte composition into the receiving space, the gel electrolyte composition including a first lithium salt having a first molar concentration and a curable compound, and then disposing the gel electrolyte composition around the electrode tab; curing the gel electrolyte composition to form a gel electrolyte surrounding the electrode tabs; injecting a liquid electrolyte containing a second lithium salt at a second molar concentration so as to be contained between the plurality of electrodes; A method for manufacturing a battery cell, comprising:

15. The method for manufacturing a battery cell according to claim 14, further comprising the step of forming a blocking portion between the receiving space of the cell case and the injection space of the gel electrolyte composition before injecting the gel electrolyte composition.

16. The first lithium salt is LiPF 6 and LiBF 4 At least one of The second lithium salt is LiPF 6 15. The method of claim 14, wherein the lithium ion implantation material comprises at least one of LiFSI, LiTFSI, and LiBOB.

17. The method of claim 14 , wherein the second molar concentration of the second lithium salt is at least 0.1 M lower than the first molar concentration of the first lithium salt.

18. 15. The method of claim 14, wherein a concentration ratio of the second molar concentration of the second lithium salt to the first molar concentration of the first lithium salt is 1:1.3 to 1:5.

Citation Information

Patent Citations

  • Non-aqueous electrolyte battery and its manufacturing method

    JP2003109557A

  • Secondary battery and method for manufacturing the same

    JP2015519703A

  • Gel polymer electrolyte and lithium secondary battery containing the same

    JP2015537352A

  • A battery cell containing a gelled electrolyte component in the pores of a separator membrane constituting an electrode assembly

    JP2018521483A