METHOD FOR MANUFACTURING ELECTRODE ASSEMBLY, ... AND LITHIUM SECONDARY BATTERY INCLUDING THE SAME
By transferring a lithium metal layer onto a separator within a transfer laminate, the method addresses the challenges of non-uniform pre-lithiation and safety in silicon-based electrodes, improving the initial charging capacity and cycle stability of lithium secondary batteries.
Patent Information
- Application Number
- JP2024529670
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-05-06
- Filing Date
- 2023-05-04
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2043-05-04
AI Technical Summary
Existing methods for pre-lithiating silicon-based negative electrodes in lithium secondary batteries face challenges such as high production costs, safety risks, and non-uniform lithium transfer, leading to increased initial irreversible capacity and reduced cycle stability due to volume changes and surface reactions.
A method involving a transfer laminate with a base layer, surface protective layer, and lithium metal layer is used to pre-lithiate the electrode by transferring the lithium metal layer onto a separator instead of directly onto the electrode, allowing for controlled pre-lithiation without additional layers, thereby preventing exposure to air and ensuring uniform lithium distribution.
This approach enhances the initial charging capacity and cycle stability of lithium secondary batteries by uniformly pre-lithiating the electrodes, reducing the need for additional layers and minimizing safety risks, while maintaining economic efficiency.
Smart Images

Figure 2024540561000001_ABST
Abstract
Description
[Technical field]
[0001] The present application relates to a method for manufacturing an electrode assembly, the electrode assembly, and a lithium secondary battery including the electrode assembly.
[0002] This application claims the benefit of the filing date of Korean Patent Application No. 10-2022-0055965, filed with the Korean Intellectual Property Office on May 6, 2022, the entire contents of which are incorporated herein by reference. [Background technology]
[0003] The rapid increase in the use of fossil fuels has led to an increased demand for alternative and clean energy, and one of the most actively researched fields in this area is the field of power generation and storage using electrochemical reactions.
[0004] At present, a representative example of an electrochemical element that uses such electrochemical energy is a secondary battery, and the range of its use is expanding more and more.
[0005] With the development of technology and increasing demand for mobile devices, the demand for secondary batteries as energy sources is rapidly increasing. Among such secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and widely used. In addition, research on methods for manufacturing high-density electrodes with higher energy density per unit volume as electrodes for such high-capacity lithium secondary batteries is being actively conducted.
[0006] In general, a secondary battery is composed of a positive electrode, a negative electrode, an electrolyte, and a separator. The negative electrode includes a negative electrode active material that inserts and removes lithium ions from the positive electrode, and the negative electrode active material may be silicon-based particles having a large discharge capacity.
[0007] Generally, carbon materials such as graphite are used for the negative electrode of lithium secondary batteries, but the theoretical capacity density of carbon is 372 mAh / g (833 mAh / cm 3). Therefore, in order to improve the energy density of the negative electrode, silicon (Si), tin (Sn), and their oxides and alloys, which are alloyed with lithium, are being considered as negative electrode materials. Among them, silicon-based materials have attracted attention due to their low cost and high capacity (4200mAh / g).
[0008] However, silicon has a problem in that the mechanical stability is reduced due to volume change (shrinkage or expansion) during the process of lithium ion insertion / extraction, which results in impaired cycle characteristics. Therefore, there is a need to develop a material that has structural stability and can ensure excellent stability and cycle characteristics when used as an active material for electrochemical devices.
[0009] In addition, when a silicon-based negative electrode active material is used, a problem occurs in that the initial irreversible capacity is large. In the charge / discharge reaction of a lithium secondary battery, lithium released from the positive electrode is inserted into the negative electrode during charging, and is removed from the negative electrode during discharging and returns to the positive electrode. However, in the case of a silicon-based negative electrode active material, the volume change and surface side reaction are significant, and most of the lithium inserted into the negative electrode during initial charging cannot return to the positive electrode. Therefore, a problem occurs in that the initial irreversible capacity is large. When the initial irreversible capacity is large, a problem occurs in that the battery capacity and cycle are rapidly reduced.
[0010] In order to solve the above problems, a method of prelithiating a silicon negative electrode containing a silicon-based negative electrode active material is known. Known prelithiating methods include a method of preparing an electrode after lithiating the negative electrode by a physical / chemical method such as electrolytic plating, lithium metal transfer, or lithium metal deposition, and a method of electrochemically prelithiating the negative electrode.
[0011] Conventional physicochemical methods have the risk of fire and explosion due to environmental factors such as the need to carry out the methods at high temperatures, and conventional electrochemical methods have the problem of being unable to uniformly control the initial irreversible capacity, which increases production costs.
[0012] In particular, in the lithium metal transfer process, it is difficult to transfer lithium metal safely and easily, and even if transferred, the highly reactive lithium metal starts to react directly with the negative electrode active material, causing problems such as particle cracking on the surface of the negative electrode active material layer.
[0013] To solve this problem, research has been conducted into adjusting the prelithiation rate of the lithium metal layer by pretreating the negative electrode active material layer before transferring the lithium metal layer or by including a diffusion rate control layer on the negative electrode active material layer. However, when such a process is performed, problems arise in that the battery manufacturing cost increases and the cell resistance increases.
[0014] Therefore, there is a need to study a process and materials for prelithiation of a negative electrode that is safer and more efficient and that can uniformly prelithiate lithium within the negative electrode active material layer. [Prior art documents] [Patent documents]
[0015] [Patent Document 1] JP 2009-080971 A Summary of the Invention [Problem to be solved by the invention]
[0016] The present application relates to a method for manufacturing an electrode assembly, the electrode assembly, and a lithium secondary battery including the electrode assembly. [Means for solving the problem]
[0017] One embodiment of the present specification includes a step of preparing a transfer laminate in which a substrate layer, a surface protective layer, and a lithium metal layer are laminated in this order; transferring the surface protective layer and the lithium metal layer to a separator such that the lithium metal layer is in contact with the separator; and forming an electrode assembly by positioning a separator between a negative electrode and a positive electrode such that the surface protective layer faces one of the negative electrode and the positive electrode; Including, In the step of transferring the surface protective layer and the lithium metal layer to the separator, the lithium metal layer has a thickness of 1 μm to 10 μm.
[0018] In yet another embodiment, an electrode assembly manufactured by the method of the present application is provided.
[0019] Finally, the present application provides a lithium secondary battery including a battery casing, an electrode assembly according to the present application provided inside the battery casing, and an electrolyte. Effect of the Invention
[0020] A main object of a method for manufacturing an electrode assembly according to an embodiment of the present invention is to enable uniform lithium transfer in a process of transferring a lithium metal layer onto an anode or cathode active material layer and prelithiating the lithium metal layer without providing an additional laminate structure such as a buffer layer on the anode or cathode active material layer.
[0021] That is, the method for manufacturing an electrode assembly according to the present application is characterized in that, unlike the conventional method in which a lithium metal layer is directly transferred onto an upper portion of an anode or cathode active material layer, a lithium metal layer is transferred onto one side of a separator, and then, during the manufacture of a battery assembly, the lithium metal layer is brought into contact with the separator in the process of laminating the anode or cathode, thereby performing pre-lithiation, or, after a cell assembly is manufactured and an electrolyte is injected, the anode or cathode is pre-lithiated.
[0022] In particular, by transferring the surface protective layer and the lithium metal layer to the separator at the same time, it is possible to prevent the lithium metal layer from being exposed to air. In addition, when the lithium metal layer is transferred to the separator together with the surface protective layer and then pre-lithiation is performed, a structure is formed in which the negative or positive active material layer is in contact with the surface protective layer, which is characterized in that a process of installing a separate layer for adjusting the pre-lithiation rate on the top of the negative or positive active material layer is not required.
[0023] As a result, the pre-lithiation rate in the negative or positive electrode active material layer can be easily adjusted, and it is economical because it is not necessary to provide a separate layer such as a buffer layer. In addition, the method according to the present application has the characteristic of being able to solve the problem of increased electrode resistance that occurs when a separate layer is provided. [Brief description of the drawings]
[0024] [Figure 1] 1A to 1C are diagrams illustrating a method for manufacturing an electrode assembly according to an embodiment of the present application. [Diagram 2] This is a diagram showing lithium metal transferred to a separator (5 cm x 5 cm). [Diagram 3] FIG. 1 is a diagram showing initial charge / discharge curves of an NCMA / Li cell (Example 1 of the present invention and Comparative Example 1). [Figure 4] FIG. 2 is a diagram showing initial charge / discharge curves of a Si / Li cell (Example 2 of the present invention and Comparative Example 2). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] Before describing the present invention, some terms will first be defined.
[0026] In this specification, when a part is said to "comprise" a certain component, this means that it may further include other components, rather than excluding other components, unless specifically stated to the contrary.
[0027] In this specification, "p to q" means a range of "not less than p and not more than q."
[0028] In this specification, the "specific surface area" is measured by the BET method, and specifically, is calculated from the amount of nitrogen gas adsorption at liquid nitrogen temperature (77K) using a BELSORP-miniII manufactured by BEL Japan Co., Ltd. That is, in this application, the BET specific surface area can mean the specific surface area measured by the above-mentioned measurement method.
[0029] In this specification, "Dn" means the average particle size, which means the particle size at the n% point of the cumulative particle number distribution by particle size. That is, D50 is the particle size at the 50% point of the cumulative particle number distribution by particle size, D90 is the particle size at the 90% point of the cumulative particle number distribution by particle size, and D10 is the particle size at the 10% point of the cumulative particle number distribution by particle size. Meanwhile, the average particle size may be measured using a laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and when the particles pass through a laser beam, the difference in the diffraction pattern according to the particle size is measured to calculate the particle size distribution.
[0030] In the present specification, when a polymer contains a certain monomer as a monomer unit, it means that the monomer participates in a polymerization reaction and is contained as a repeating unit in the polymer. In the present specification, when a polymer contains a monomer, this is interpreted as the same as when a polymer contains a monomer as a monomer unit.
[0031] In this specification, the term "polymer" is understood to be used in a broad sense including copolymers, unless specifically referred to as a "homopolymer."
[0032] In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) are polystyrene-equivalent molecular weights measured by gel permeation chromatography (GPC) using monodisperse polystyrene polymers (standard samples) of various degrees of polymerization commercially available for molecular weight measurement as standard substances. In this specification, the molecular weight means the weight average molecular weight unless otherwise specified.
[0033] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings in order to enable those skilled in the art to easily practice the present invention. However, the present invention may be embodied in many different forms and should not be construed as limited to the disclosed embodiments.
[0034] One embodiment of the present specification includes the steps of: preparing a transfer laminate in which a base layer, a surface protective layer, and a lithium metal layer are sequentially laminated; transferring the surface protective layer and the lithium metal layer to a separator such that the lithium metal layer is in contact with the separator; and positioning the separator between a negative electrode and a positive electrode such that the surface protective layer faces one electrode selected from the negative electrode and the positive electrode, thereby forming an electrode assembly; In the step of transferring the surface protective layer and the lithium metal layer to the separator, the lithium metal layer has a thickness of 1 μm to 10 μm.
[0035] The method for manufacturing an electrode assembly according to the present application is characterized in that, unlike the conventional method in which a lithium metal layer is directly transferred onto an upper portion of an anode or cathode active material layer, a lithium metal layer is transferred onto one side of a separator, and then, during the manufacture of an electrode assembly, the lithium metal layer is brought into contact with the separator in the process of laminating the anode or cathode, thereby allowing pre-lithiation to proceed, or, after a cell assembly is manufactured and an electrolyte is injected, pre-lithiation of the anode or cathode is performed.
[0036] In particular, by transferring the surface protective layer and the lithium metal layer to the separator at the same time, it is possible to prevent the lithium metal layer from being exposed to air. In addition, when the lithium metal layer is transferred to the separator together with the surface protective layer and subsequently pre-lithiation is performed, a structure is formed in which the surface protective layer contacts the negative or positive electrode active material layer, which is characterized by the fact that a process of installing a separate layer for adjusting the pre-lithiation rate on the top of the negative electrode active material layer is not required.
[0037] The manufacturing method of the electrode assembly of the present application will be described in detail below.
[0038] A method for manufacturing an electrode assembly according to one embodiment of the present application includes the step of preparing a transfer laminate in which a substrate layer, a surface protective layer, and a lithium metal layer are laminated in that order.
[0039] Said steps correspond to the steps of preparing a transfer laminate for transferring a lithium metal layer onto a separator.
[0040] In one embodiment of the present application, the substrate layer may be any layer that can withstand process conditions such as high temperatures during the deposition of the lithium metal layer, and that can prevent a reverse peeling problem in which the lithium metal layer is transferred onto the substrate layer during a winding process for transferring the deposited lithium metal layer.
[0041] Specifically, in one embodiment of the present application, the base layer may be one or more selected from the group consisting of polyethylene terephthalate (PET), polyimide (PI), poly(methylmethacrylate) (PMMA), polypropylene, polyethylene, and polycarbonate.
[0042] In one embodiment of the present application, the thickness of the base layer may be in the range of 1 μm or more and 300 μm or less, 5 μm or more and 200 μm or less, or 10 μm or more and 30 μm or less.
[0043] In one embodiment of the present application, the thickness of the lithium metal layer transferred to the separator may be 1 μm or more and 10 μm or less, and preferably, may satisfy the range of 2 μm or more and 10 μm or less.
[0044] When the thicknesses of the substrate layer and the lithium metal layer satisfy the above ranges, the lithium metal layer can be efficiently transferred to the negative electrode or positive electrode active material layer side, and reverse transfer can be prevented.
[0045] In addition, if the thickness of the lithium metal layer transferred to the separator is less than 2 μm, there are problems in that the initial irreversible capacity compensation of the negative electrode is insufficient, limiting the improvement of the initial efficiency of the battery, and the compensation of lithium loss during cycle charging and discharging is insufficient, limiting the improvement of the cycle life performance of the battery. If the thickness exceeds 10 μm, lithium is supplied to the battery more than necessary, increasing the manufacturing cost of the battery, and there is a risk of non-uniformity in the pre-lithiation quality of the electrode and overcharging occurring during the initial charging after manufacturing the battery.
[0046] On the other hand, in one embodiment of the present application, the lithium metal layer may have a 10-time average surface roughness of 0.02 μm or more and 0.2 μm or less, and preferably satisfies the range of 0.02 μm or more and 0.1 μm or less.
[0047] When the surface roughness of the lithium metal layer satisfies the above range, the lithium metal layer can be efficiently transferred to the separator and reverse transfer can be prevented. In particular, when the surface roughness of the lithium metal layer exceeds 0.2 μm, the lithium metal layer can be non-uniformly transferred to the separator, which can lead to high non-uniformity in the pre-lithiation quality of the electrode.
[0048] In this application, the surface roughness is expressed as Sa (the arithmetic mean height of a surface), which is a concept that extends Ra (the arithmetic mean height of a line) to a surface, and is calculated by the following formula: The height of the peaks (parts higher than the arithmetic mean surface) or the depth of the valleys (parts lower than the arithmetic mean surface) on the arithmetic mean surface is calculated as an absolute value, and then integrated with respect to the xy area for which the surface roughness is to be calculated, and this value is divided by the xy area A.
[0049]
number
[0050] When transferring a lithium metal layer using SLMP powder to a separator, the SLMP powder must be rolled and then formed into a sheet, which is then transferred to the separator, but since general SLMP powder has a large average particle size of about 30 μm, it is difficult to adjust the thickness to the range of the lithium metal layer of the present application, and even if it is formed into a sheet, the size of the SLMP particles is not uniform, and some SLMP powder remains in a particulate form, resulting in a surface roughness that is higher than that of the lithium metal layer of the present application. As a result, it is difficult to precisely control the degree of prelithiation, and there is a problem in that the non-uniformity of the prelithiation quality of the electrode increases.
[0051] In one embodiment of the present application, in order to improve the peelability of the lithium metal layer and ensure transferability to the separator, the transfer laminate further includes a surface protective layer on the surface where the base layer and the lithium metal layer are in contact.
[0052] That is, the substrate layer may have a surface protective layer formed on at least one side thereof, or may have a surface protective layer formed on both sides thereof. The surface protective layer can prevent a reverse peeling problem in which the lithium metal layer is transferred onto the substrate layer in a process for transferring the deposited lithium metal layer onto a separator, and can easily separate the substrate layer after the lithium metal layer is transferred onto the separator.
[0053] In one embodiment of the present application, there is provided a method for producing an electrode assembly, wherein the surface protective layer includes one or more selected from the group consisting of a polymer, a conductive material, and inorganic particles.
[0054] In one embodiment of the present application, the polymer may include one or more selected from the group consisting of an acrylic polymer, a fluorine-based polymer, and a silicon-based polymer.
[0055] In one embodiment of the present application, the conductive material may be the same as the negative electrode conductive material described later.
[0056] In one embodiment of the present application, the inorganic particles can be used without limitation as long as they are inorganic particles such as alumina or silica particles.
[0057] In particular, the surface protective layer is transferred to the separator together with the lithium metal layer when the lithium metal layer is transferred to the separator. As a result, the surface protective layer serves as a protective film to prevent the highly reactive lithium metal layer from being exposed to air, and is also transferred to the top of the negative or positive electrode active material layer in the pre-lithiation process described below. As a result, the surface protective layer is characterized in that it is possible to control the pre-lithiation speed by preventing direct contact between the negative or positive electrode active material layer and the lithium metal layer, thereby enabling uniform pre-lithiation and preventing lithium loss.
[0058] In one embodiment of the present application, the surface protective layer may be formed by a coating method, for example, the coating method may be a method selected from the group consisting of dip coating, spray coating, spin coating, die coating, gravure coating, micro-gravure coating, comma coating, and roll coating, but is not limited thereto, and various coating methods available in the art for forming a coating layer may be used.
[0059] In one embodiment of the present application, the thickness of the surface protective layer may be in the range of 100 nm or more and 1 μm or less.
[0060] In another embodiment, the thickness of the surface protective layer may be in the range of 100 nm or more and 1 μm or less, preferably 200 nm or more and 1 μm or less.
[0061] The surface protective layer may be completely dissolved in the electrolyte after the pre-lithiation process described below, or may not be dissolved and may remain on the negative electrode or positive electrode for the lithium secondary battery. In this case, the thickness of the surface protective layer satisfies the above range, and is characterized in that it does not cause problems in electrode resistance.
[0062] In one embodiment of the present application, the method for manufacturing the electrode assembly may include a step of transferring the surface protective layer and the lithium metal layer to a separator such that the lithium metal layer is in contact with the separator.
[0063] The step may refer to a step of transferring a lithium metal layer onto a separator to be transferred, instead of directly transferring the lithium metal layer onto the negative or positive active material layer.
[0064] In one embodiment of the present application, there is provided a method for manufacturing an electrode assembly, wherein the step of transferring a surface protective layer and a lithium metal layer to a separator so that the lithium metal layer is in contact with the separator includes the steps of: laminating the lithium metal layer of the transfer laminate onto one side of the separator; and removing the substrate layer.
[0065] In this regard, in one embodiment of the present application, there is provided a method for manufacturing an electrode assembly, wherein the step of transferring the surface protective layer and the lithium metal layer to the separator so that the lithium metal layer is in contact with the separator includes the steps of: pretreating the separator; and transferring the surface protective layer and the lithium metal layer onto the pretreated separator; and the pretreatment includes corona treatment or plasma treatment.
[0066] In one embodiment of the present application, the plasma treatment may refer to a process of applying a voltage of 15 kV to a plasma generating section of the separator, flowing N2 (800 slm) and CDA (5 slm) to generate plasma, and passing the separator at a speed of 5 lpm to treat the surface of the separator.
[0067] Specifically, in one embodiment of the present application, the pre-treating step may be an indirect plasma type.
[0068] As described above, before the lithium metal layer is transferred to the separator, the surface of the separator can be pretreated to improve the interfacial adhesion with the lithium metal layer later, thereby providing the characteristic that the substrate layer can be easily peeled off.
[0069] In addition, in one embodiment of the present application, there is provided a method for manufacturing an electrode assembly, wherein the step of transferring the surface protective layer and the lithium metal layer to the separator such that the lithium metal layer contacts the separator includes a dry-on-dry process.
[0070] That is, the transfer process according to the present application is characterized by including a dry on dry process, which has the advantage that the lithium metal layer can be transferred to the separator without using a solvent, and therefore no solvent washing or drying process is required.
[0071] In addition, by transferring the lithium metal layer to the separator using the dry-on-dry process as described above, the deposition thickness of the lithium metal layer can be accurately controlled within a desired range, which has the advantage that the pre-lithiation dosage of the subsequent negative electrode or positive electrode can be very accurately controlled.
[0072] Meanwhile, when the lithium metal layer is applied by a wet on dry process rather than a dry on dry process, specifically, stabilized lithium metal powder (SLMP) may be included in a solvent and coated on the separator.
[0073] As described above, when forming a lithium metal layer on a separator using a wet on dry process, a solvent is usually included, and therefore a solvent washing or drying process is required, resulting in a problem of low process economics. In addition, when using a wet on dry process, the coating weight per unit area must be controlled during coating, and in this case, there is a limit to reducing the pre-lithiation dosage, and if the dosage is increased, a pressurized condition is required, which may cause deformation of the separator.
[0074] In addition, when the wet-on-dry process is used as described above, the coating composition may penetrate into the pores of the non-uniform separator, causing problems such as clogging of the pores. In addition, even when the pre-lithiation is completed, a significant amount of unreacted lithium may remain on the surface of the electrode.
[0075] However, the transfer process according to the present application includes a dry-on-dry process, which can solve the above problems. In particular, the deposition thickness of the lithium metal layer can be accurately controlled within a desired range, and the pre-lithiation dosage of the subsequent anode or cathode can be very accurately controlled so that almost no lithium metal layer remains on the anode or cathode.
[0076] In one embodiment of the present application, a method for manufacturing the electrode assembly includes a step of forming an electrode assembly by positioning a separator between a negative electrode and a positive electrode such that the surface protective layer faces one electrode selected from the negative electrode and the positive electrode.
[0077] That is, through the above steps, the negative electrode active material layer on the negative electrode or the positive electrode active material layer on the positive electrode is assembled to face the lithium metal layer.
[0078] In one embodiment of the present application, the step of forming an electrode assembly by positioning a separator between the negative electrode and the positive electrode such that one electrode selected from the negative electrode and the positive electrode and the surface protective layer face each other may include the steps of forming a negative electrode current collector layer or a positive electrode current collector layer and a negative electrode active material layer or a positive electrode active material layer provided on one or both sides of the negative electrode current collector layer or the positive electrode current collector layer; and forming an electrode assembly by laminating, press laminating, or winding one side of the negative electrode active material layer or the positive electrode active material layer and one side of the surface protective layer of the electrode assembly.
[0079] In one embodiment of the present application, the lamination method refers to a method of manufacturing an electrode assembly by stacking an electrode and a separator without applying pressure, and the pressure lamination method refers to a method of laminating a separator and an electrode under pressure, or a method of laminating a separator and an electrode and then pressurizing the electrode assembly, etc. The winding method refers to a method of winding into a roll, and is not limited to a specific method.
[0080] In one embodiment of the present application, the prelithiation of the electrodes may be performed from the step of forming an assembly by positioning a separator between the negative electrode and the positive electrode so that the surface protective layer faces one electrode selected from the negative electrode and the positive electrode, or the prelithiation may be performed after injecting an electrolyte in the battery assembly step. That is, in one embodiment of the present application, the prelithiation may be performed on either the negative electrode or the positive electrode, and may be performed as dry prelithiation or wet prelithiation after injecting an electrolyte.
[0081] During the pre-lithiation of a negative electrode according to one embodiment of the present application, the initial charge capacity of the negative electrode is reduced due to the lithium introduced into the negative electrode, and the initial irreversible capacity of the negative electrode is reduced, and during the pre-lithiation of a positive electrode according to one embodiment of the present application, as the amount of lithium contained in the positive electrode increases, the initial charge capacity of the positive electrode is increased to compensate for the irreversible capacity of the negative electrode, and thus the energy density or life performance of the battery is improved depending on the degree of pre-lithiation, which means that the performance of the battery is superior to that of a battery using a negative electrode or a positive electrode that has not been pre-lithiated.
[0082] In one embodiment of the present application, the method may include forming a negative electrode including a negative electrode current collector layer and a negative electrode active material layer on one or both sides of the negative electrode current collector layer.
[0083] The step of laminating a negative electrode for a lithium secondary battery includes forming a negative electrode current collector layer and a negative electrode active material layer on one or both sides of the negative electrode current collector layer, the step of coating one or both sides of the negative electrode current collector layer with a negative electrode slurry including a negative electrode active material layer composition, and the negative electrode active material layer composition may include one or more selected from the group consisting of a negative electrode active material, a negative electrode conductive material, and a negative electrode binder.
[0084] In one embodiment of the present application, the negative electrode current collector layer generally has a thickness of 1 μm to 100 μm. Such a negative electrode current collector layer is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, plastic carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. In addition, fine irregularities may be formed on the surface to strengthen the binding force of the negative electrode active material, and may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0085] In one embodiment of the present application, the negative electrode current collector layer may have a thickness of 1 μm or more and 100 μm or less, and the negative electrode active material layer may have a thickness of 20 μm or more and 500 μm or less.
[0086] However, the thickness may vary depending on the type and application of the negative electrode used, and is not limited thereto.
[0087] In one embodiment of the present application, the negative electrode slurry may include a negative electrode active material layer composition and a slurry solvent.
[0088] In one embodiment of the present application, the solid content of the negative electrode slurry may be 5% or more and 40% or less.
[0089] In another embodiment, the solid content of the negative electrode slurry may be in the range of 5% to 40%, preferably 7% to 35%, and more preferably 10% to 30%.
[0090] The solid content of the negative electrode slurry may refer to the content of the negative electrode active material layer composition contained in the negative electrode slurry, or may refer to the content of the negative electrode active material layer composition based on 100 parts by weight of the negative electrode slurry.
[0091] When the solid content of the negative electrode slurry satisfies the above range, during the formation of the negative electrode active material layer, it has the characteristic that the viscosity is appropriate, the caking phenomenon of the particles of the negative electrode active material layer composition is minimized, and the negative electrode active material layer can be efficiently formed.
[0092] In one embodiment of the present application, the slurry solvent is not limited as long as it can dissolve the negative electrode active material layer composition. Specifically, distilled water may be used.
[0093] The negative electrode according to one embodiment of the present application may be formed by coating and drying the negative electrode slurry on the negative electrode current collector layer.
[0094] By the drying step, the slurry solvent in the negative electrode slurry can be dried.
[0095] In one embodiment of the present application, the negative electrode active material layer composition may include one or more selected from the group consisting of a negative electrode active material, a negative electrode conductive material, and a negative electrode binder.
[0096] In one embodiment of the present application, the negative electrode active material may include one or more selected from the group consisting of graphite, soft carbon, hard carbon, Si particles (SiO x (x = 0)), SiO x (0 < x < 2), Si / C, and Si alloys.
[0097] In the charge and discharge reaction of a lithium secondary battery, during charging, lithium released from the positive electrode is inserted into the negative electrode, and during discharging, it desorbs from the negative electrode and returns to the positive electrode again. However, in the case of a silicon-based negative electrode active material, volume change and surface side reactions are serious, and during the initial charging, most of the lithium inserted into the negative electrode cannot return to the positive electrode again. Therefore, the problem of a large initial irreversible capacity occurs. When the initial irreversible capacity increases, problems such as a sharp decrease in battery capacity and cycles occur.
[0098] In the present invention, in order to solve the above problems, the negative electrode of the lithium secondary battery is prelithiated to solve the initial irreversible capacity problem. Specifically, in the prelithiation process, when a lithium transfer process is performed, a transfer target is formed on the separator, so that the lithium can be easily transferred to the negative electrode, and the lithium in the negative electrode active material layer can be uniformly prelithiated.
[0099] In addition, in the case of the present invention, in order to improve capacity performance, a silicon-based active material is used as a negative active material, but in order to solve the problems of maintaining a conductive path due to volume expansion and maintaining the bond between the conductive material, binder, and active material, a binder that meets specific conditions and a conductive material composite bound to the binder are used to solve the conventional problems.
[0100] Meanwhile, the average particle size (D50) of the silicon-based active material of the present invention may be 5 μm to 10 μm, specifically 5.5 μm to 8 μm, and more specifically 6 μm to 7 μm. When the average particle size is within the above range, the specific surface area of the particles is within a suitable range, and the viscosity of the negative electrode slurry is formed within a suitable range. This allows smooth dispersion of the particles constituting the negative electrode slurry. In addition, when the size of the silicon-based active material is equal to or greater than the lower limit of the above range, the contact area between the silicon particles and the conductive material is excellent due to the composite of the conductive material and the binder in the negative electrode slurry, and the conductive network is more likely to be maintained, thereby increasing the capacity retention rate. Meanwhile, when the average particle size satisfies the above range, silicon particles that are too large are excluded, and the surface of the negative electrode is formed smoothly, thereby preventing non-uniformity of current density during charging and discharging.
[0101] In one embodiment of the present application, the silicon-based active material typically has a characteristic BET surface area. The BET surface area of the silicon-based active material is preferably less than 0.01 m 2 / g~150.0m 2 / g, more preferably 0.1m 2 / g~100.0m 2 / g, particularly preferably 0.2m 2 / g~80.0m2 / g, most preferably 0.2m 2 / g~18.0m 2 / g. The BET surface area is determined in accordance with DIN 66131 (with nitrogen).
[0102] In one embodiment of the present application, the silicon-based active material may be present, for example, in crystalline or amorphous form, and is preferably not porous.The silicon particles are preferably spherical or shard particles.Alternatively, the silicon particles may have a fibrous structure or may be present in the form of a silicon-containing thin film or coating, but less preferably.
[0103] The negative electrode composition according to the present application is characterized in that, even when a silicon-based active material having a remarkably high capacity is used within the above range, the performance of the negative electrode is not deteriorated and the output characteristics during charging and discharging are excellent, by using a specific conductive material and binder that can control the volume expansion rate during charging and discharging.
[0104] In one embodiment of the present application, the silicon-based active material may have a non-spherical shape, and the sphericity is, for example, 0.9 or less, for example, 0.7 to 0.9, for example, 0.8 to 0.9, for example, 0.85 to 0.9.
[0105] In this application, the circularity is determined by the following formula 1, where A is the area and P is the perimeter.
[0106] [Formula 1] 4πA / P 2
[0107] In the past, it was common to use only graphite-based compounds as negative electrode active materials, but recently, as the demand for high-capacity batteries has increased, attempts to mix and use silicon-based active materials to increase capacity have been increasing. However, silicon-based active materials have the limitation that their volume expands rapidly during the charge / discharge process, damaging the conductive path formed in the negative electrode active material layer and reducing the performance of the battery, so the type of negative electrode conductive material used together with the silicon-based active material is important.
[0108] In one embodiment of the present application, the negative electrode conductive material may include one or more selected from the group consisting of a dot-like conductive material, a sheet-like conductive material, and a linear conductive material.
[0109] In one embodiment of the present application, the dot-shaped conductive material can be used to improve the conductivity of the negative electrode, and is preferably conductive without inducing chemical changes. Specifically, the conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, conductive fiber, fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and may preferably include carbon black in terms of realizing high conductivity and excellent dispersibility.
[0110] In one embodiment of the present application, the point-like conductive material has a BET specific surface area of 40 m 2 / g or more 70m 2 / g or less, preferably 45m 2 / g or more 65m 2 / g or less, more preferably 50m 2 / g or more 60m 2 / g or less.
[0111] In one embodiment of the present application, the particle size of the dotted conductive material may be 10 nm to 100 nm, preferably 20 nm to 90 nm, and more preferably 40 nm to 60 nm.
[0112] In one embodiment of the present application, the negative electrode conductive material may include a sheet conductive material.
[0113] The planar conductive material can improve conductivity by increasing surface contact between silicon particles in the negative electrode, and at the same time, can suppress the disconnection of the conductive path due to volume expansion, and is used in a concept including a bulk type conductive material or a plate type conductive material.
[0114] In one embodiment of the present application, the sheet conductive material may include at least one selected from the group consisting of platelet graphite, graphene, graphene oxide, and graphite flakes, and may preferably be platelet graphite.
[0115] In one embodiment of the present application, the average particle size (D50) of the sheet conductive material may be 2 μm to 7 μm, specifically, 3 μm to 6 μm, and more specifically, 4 μm to 5 μm. If the above range is satisfied, the particle size is sufficient, so that the viscosity of the negative electrode slurry does not increase too much, and dispersion is easy. Therefore, when dispersing using the same equipment and time, the dispersion effect is excellent.
[0116] In one embodiment of the present application, there is provided a negative electrode composition, wherein the sheet conductive material has a D10 of 0.5 μm or more and 1.5 μm or less, a D50 of 2.5 μm or more and 3.5 μm or less, and a D90 of 7.0 μm or more and 15.0 μm or less.
[0117] In one embodiment of the present application, the sheet conductive material may be a sheet conductive material having a high BET specific surface area; or a sheet conductive material having a low specific surface area.
[0118] In one embodiment of the present application, the sheet conductive material may be a sheet conductive material with a high specific surface area or a sheet conductive material with a low specific surface area without any restrictions. In particular, the sheet conductive material of the present application may be affected to some extent by dispersion in terms of electrode performance, and it is particularly preferable to use a sheet conductive material with a low specific surface area in which dispersion problems do not occur.
[0119] In one embodiment of the present application, the sheet conductive material has a BET specific surface area of 1 m 2 / g or more.
[0120] In another embodiment, the sheet conductive material has a BET specific surface area of 1 m 2 / g or more 500m 2 / g or less, preferably 5m 2 / g or more 300m 2 / g or less, more preferably 5m 2 / g or more 250m 2 / g or less.
[0121] In another embodiment, the sheet conductive material is a sheet conductive material having a high specific surface area and a BET specific surface area of 50 m 2 / g or more 500m 2 / g or less, preferably 80m 2 / g or more 300m 2 / g or less, more preferably 100m 2 / g or more 300m 2 / g or less.
[0122] In another embodiment, the sheet conductive material is a sheet conductive material having a low specific surface area and a BET specific surface area of 1 m 2 / g or more 40m 2 / g or less, preferably 5m 2 / g or more 30m 2 / g or less, more preferably 5m 2 / g or more 25m 2 / g or less.
[0123] Alternatively, the conductive material may be a linear conductive material such as a carbon nanotube. The carbon nanotube may be a bundle-type carbon nanotube. The bundle-type carbon nanotube may include a plurality of carbon nanotube units. Specifically, unless otherwise specified, the term "bundle type" refers to a secondary shape in which a plurality of carbon nanotube units are arranged in parallel with the longitudinal axis of the carbon nanotube units being substantially aligned in the same direction or twisted into a bundle or rope. The carbon nanotube unit has a graphite sheet having a nano-sized cylindrical shape and an sp2 bond structure. In this case, the graphite sheet may exhibit conductive or semiconductive properties depending on the angle and structure at which it is wound. The bundle-type carbon nanotube may be uniformly dispersed during the manufacture of the negative electrode compared to an entangled type carbon nanotube, and may smoothly form a conductive network in the negative electrode, thereby improving the conductivity of the negative electrode.
[0124] In one embodiment of the present application, the linear conductive material may be SWCNT.
[0125] In one embodiment of the present application, there is provided a negative electrode for a lithium secondary battery, wherein the negative electrode conductive material includes a sheet conductive material and a linear conductive material.
[0126] When the above-mentioned dot-shaped conductive materials are not used, the output characteristics of the secondary battery of the present invention can be improved by including linear and sheet-shaped conductive materials as the negative electrode conductive material.
[0127] In one embodiment of the present application, the negative electrode conductive material may be 10 parts by weight or more and 40 parts by weight or less based on 100 parts by weight of the negative electrode active material layer composition.
[0128] In another embodiment, the negative electrode conductive material may be included in an amount of 10 parts by weight or more and 40 parts by weight or less, preferably 10 parts by weight or more and 30 parts by weight or less, and more preferably 15 parts by weight or more and 25 parts by weight or less, based on 100 parts by weight of the negative electrode active material layer composition.
[0129] In one embodiment of the present application, the sheet conductive material may be 90 parts by weight or more and 99.9 parts by weight or less, and the linear conductive material may be 0.1 parts by weight or more and 10 parts by weight or less, based on 100 parts by weight of the negative electrode conductive material.
[0130] In still another embodiment, the sheet conductive material may be included in an amount of 90 parts by weight to 99.9 parts by weight, preferably 93 parts by weight to 99.9 parts by weight, and more preferably 95 parts by weight to 99.9 parts by weight, based on 100 parts by weight of the negative electrode conductive material.
[0131] In still another embodiment, the linear conductive material may be included in an amount of 0.1 to 10 parts by weight, preferably 0.1 to 7 parts by weight, and more preferably 0.1 to 5 parts by weight, based on 100 parts by weight of the negative electrode conductive material.
[0132] In one embodiment of the present application, the negative electrode conductive material may include a linear conductive material and a sheet conductive material, and the ratio of the linear conductive material:sheet conductive material may satisfy 0.01:1 to 0.1:1.
[0133] In one embodiment of the present application, the ratio of the linear conductive material to the planar conductive material may satisfy 0.1:1.
[0134] In one embodiment of the present application, the negative electrode conductive material includes a linear conductive material and a planar conductive material, and by satisfying the above-mentioned composition and ratio, the battery does not significantly affect the life characteristics of conventional lithium secondary batteries, and has the characteristics of having many points at which charging and discharging are possible and excellent output characteristics at a high C-rate.
[0135] The negative electrode conductive material according to the present application has a completely different structure from the positive electrode conductive material applied to the positive electrode. That is, the negative electrode conductive material according to the present application plays a role of controlling the contact between the silicon-based active material, which has a very large volume expansion of the electrode due to charging and discharging, and the positive electrode conductive material plays a role of providing some conductivity while acting as a buffer for a shock-absorbing effect when rolled, and has a completely different structure and role from the negative electrode conductive material of the present invention.
[0136] In addition, the negative electrode conductive material according to the present application is applied to a silicon-based active material, and has a completely different structure from a conductive material applied to a graphite-based active material. That is, a conductive material used in an electrode having a graphite-based active material has particles that are simply smaller than the active material, and therefore has the properties of improving output characteristics and imparting some electrical conductivity, and has a completely different structure and role from a negative electrode conductive material applied together with a silicon-based active material as in the present invention.
[0137] In one embodiment of the present application, the negative electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and substances in which hydrogen is substituted with Li, Na, Ca, or the like, or may include various copolymers thereof.
[0138] The negative electrode binder according to one embodiment of the present application plays a role in controlling the negative electrode active material and the negative electrode conductive material in order to prevent twisting and deformation of the negative electrode structure during volume expansion and relaxation of the silicon-based active material. In the case where the above role is fulfilled, any conventional binder may be applied, specifically, a water-based binder may be used, and more specifically, a PAM-based binder may be used.
[0139] In one embodiment of the present application, the negative electrode binder may be contained in an amount of 30 parts by weight or less, preferably 25 parts by weight or less, more preferably 20 parts by weight or less, or may be contained in an amount of 5 parts by weight or more and 10 parts by weight or more, based on 100 parts by weight of the negative electrode active material layer composition.
[0140] In one embodiment of the present application, the method may further include pretreating the negative electrode active material layer.
[0141] At this time, the negative electrode active material layer may be pretreated in the same manner as the separator.
[0142] In one embodiment of the present application, the method may include forming a positive electrode comprising a positive electrode current collector layer and a positive electrode active material layer on one or both sides of the positive electrode current collector.
[0143] The step of laminating a positive electrode for a lithium secondary battery may include forming a positive electrode current collector layer and a positive electrode active material layer on one or both sides of the positive electrode current collector layer, and coating one or both sides of the positive electrode current collector layer with a positive electrode slurry including a positive electrode active material layer composition.
[0144] In the positive electrode, the positive electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, plastic carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may usually have a thickness of 3 μm to 500 μm, and fine irregularities may be formed on the surface of the positive electrode current collector to increase the adhesive force of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0145] The positive electrode active material layer composition may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; a lithium iron oxide such as LiFe3O4; 1+c1 Mn 2-c1 O4 (0≦c1≦0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-c2 M c2 Lithium nickel oxide with Ni site represented by the chemical formula LiMnO2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and satisfies 0.01≦c2≦0.3); 2-c3 M c3 O2 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≦c3≦0.1), chemical formula LiM 1-c4 M' c4Examples of the lithium manganese composite oxide include, but are not limited to, lithium manganese oxide represented by Li2Mn3MO8 (wherein M is a transition metal, M' is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≦c4≦0.1) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); and LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion. The positive electrode may be Li metal.
[0146] In one embodiment of the present application, the positive electrode active material layer composition is LiNi x Co y Mn z O2(x+y+z=1);LiNi a Co b Mn c Al d O2(a+b+c+d=1);LiMn2O4;LiNi 0.5 Mn 1.5 O2; and LiM x Fe y It may contain one or more selected from the group consisting of PO4 (M: transition metal, x+y=1).
[0147] The positive electrode active material layer may contain a positive electrode conductive material and a positive electrode binder in addition to the above-mentioned positive electrode active material layer composition.
[0148] In this case, the positive electrode conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing chemical changes in the battery that is constructed.Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like, and one or more of these may be used alone or in mixture.
[0149] In addition, the positive electrode binder plays a role of improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector.Specific examples include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination.
[0150] In one embodiment of the present application, the separator separates the negative electrode and the positive electrode to provide a path for lithium ions to move, and any separator that is generally used in secondary batteries may be used without any particular limitation, and in particular, a separator that has low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption ability is preferred. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, or the like, may be used. In addition, a coated separator containing a ceramic component or a polymeric substance may be used to ensure heat resistance or mechanical strength, and may be selectively used in a single layer or multilayer structure.
[0151] In one embodiment of the present application, the method for manufacturing the electrode assembly may include a step of pressurizing the assembly to prelithiate the negative electrode or the positive electrode.
[0152] The step may refer to a process of prelithiating the negative electrode or the positive electrode. In one embodiment of the present application, the step of prelithiating the negative electrode or the positive electrode is performed under a temperature condition of 60° C. to 80° C. with a pressure of 20 kgf / cm 2 ~60kgf / cm 2 The present invention provides a method for manufacturing an electrode assembly, comprising the steps of:
[0153] In one embodiment of the present application, there is provided an electrode assembly manufactured by the manufacturing method of the present application.
[0154] The present application also provides a lithium secondary battery including a battery exterior material, an electrode assembly according to the present application provided inside the battery exterior material, and an electrolyte.
[0155] Examples of the electrolyte include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries, but are not limited to these.
[0156] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.
[0157] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0158] In particular, among the carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are highly viscous organic solvents having a high dielectric constant and capable of dissociating lithium salts, and therefore can be preferably used. When such a cyclic carbonate is mixed with a linear carbonate having a low viscosity and a low dielectric constant, such as dimethyl carbonate and diethyl carbonate, in an appropriate ratio, an electrolyte having high electrical conductivity can be produced, and therefore such a cyclic carbonate can be more preferably used.
[0159] The metal salt may be a lithium salt, and the lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte solution. For example, the anion of the lithium salt is F - , Cl - , I - , NO3- , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more selected from the group consisting of may be used.
[0160] In addition to the constituents of the electrolyte, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, and aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing a decrease in the capacity of the battery, and improving the discharge capacity of the battery.
[0161] According to an embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same. The battery module and the battery pack include the secondary battery having high capacity, high rate characteristics, and high cycle characteristics, and therefore may be used as a power source for a medium- to large-sized device selected from the group consisting of an electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, and a power storage system. EXAMPLES
[0162] Below, preferred embodiments are presented to aid in understanding the present invention. However, these embodiments are merely illustrative of the present description, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical ideas of the present description. Naturally, such changes and modifications fall within the scope of the claims.
[0163] Manufacturing Example Manufacturing of transfer laminate A laminate was prepared by coating a 1 μm thick acrylic resin as a surface protective layer on a polyethylene terephthalate substrate layer, and a lithium metal layer was deposited on the surface protective layer of the laminate by thermal evaporation to form a 6 μm thick lithium metal layer, producing a transfer laminate.
[0164] Lithium transfer onto separator A PE separator coated on both sides with a ceramic layer (19μm, PE separator base: 9μm, single-sided ceramic coating layer thickness: 5μm) was laminated with a 6.2μm-thick evaporated Li / PET film, and roll-laminated with a load of 400kgf to transfer the lithium on the PET substrate to the ceramic-coated separator. The roll lamination was carried out at room temperature. The PET substrate was removed immediately after lamination to obtain a separator with the Li transferred (see figure).
[0165] Manufacturing of positive or negative electrodes The positive electrode slurry was prepared by adjusting the ratio of the positive electrode material (NCMA): conductive material (MWCNT): binder (PVDF-HFP) solids to 96wt%:2wt%:2wt% and using NMP as a solvent. The solids content in the slurry was adjusted to 65wt%. The capacity per single-sided coating standard area was 4.2mAh / cm. 2 The electrode slurry was coated on both sides of an aluminum current collector (thickness: 15 μm) so that the electrode slurry became 100%. The electrode was then dried in a vacuum oven at 130° C. for 12 hours and roll pressed to prepare an electrode having electrode active material layers coated on both sides.
[0166] The negative electrode slurry was prepared by adjusting the ratio of the negative electrode material (Micron Silicon, D50: 3.5 μm): conductive material (Denka Black): binder (polyacrylic acid binder) solids to 80 wt%: 10 wt%: 10 wt% and using distilled water as a solvent. The solids content in the slurry was adjusted to 25 wt%. The capacity per single-sided coating standard area was 11.9 mAh / cm. 2 The electrode slurry was coated on both sides of a copper current collector (thickness: 8 μm) so that the electrode slurry became 100%. The electrode was then dried in a vacuum oven at 130° C. for 12 hours and roll pressed to prepare a negative electrode having an electrode active material layer coated on both sides.
[0167] Example 1 A positive electrode was disposed so that the surface protective layer of the prepared positive electrode and the separator to which the lithium metal layer composed of a surface protective layer / lithium metal layer / separator was transferred was in contact with the positive electrode active material layer, and a coin half cell was fabricated by using a lithium foil having a thickness of 150 μm as a counter electrode on the opposite side of the separator.
[0168] The electrolyte used was ethylene carbonate (FEC) / ethyl methyl carbonate (EMC) = 3 / 7 (volume ratio) with 1M LiPF6 dissolved in it. When measuring the initial charge / discharge capacity, the C-rate was set to 0.1C, charging was performed with an upper limit voltage of 4.25V under CCCV conditions and a cut-off current of 0.005C, and discharging was performed with a lower limit voltage of 3.0V under CC conditions.
[0169] Example 2 The negative electrode was arranged so that the surface protective layer and the negative active material layer were in contact with each other among the prepared negative electrode and the separator to which the lithium metal layer composed of the surface protective layer / lithium metal layer / separator was transferred, and a coin half cell was manufactured by using a lithium foil having a thickness of 150 μm as a counter electrode on the opposite side of the separator. As the electrolyte, ethylene carbonate (FEC) / ethyl methyl carbonate (EMC)=3 / 7 (volume ratio) in which 1M LiPF6 was dissolved was used as in Example 1. When measuring the initial charge / discharge capacity, the C-rate was set to 0.1C, charging was performed under CCCV conditions with a lower limit voltage of 0.005V and a cut-off current of 0.005C, and discharging was performed under CC conditions with an upper limit voltage of 1.5V.
[0170] Comparative Example 1 A coin half-cell was produced using a ceramic-coated separator instead of transferring the transfer laminate to the separator in Example 1. The positive electrode, lithium counter electrode, and electrolyte were the same materials as in Example 1, and the coin half-cell evaluation conditions were also the same as in Example 1.
[0171] Comparative Example 2 A coin half cell was fabricated using a ceramic-coated separator instead of transferring the transfer laminate to the separator in Example 2. The negative electrode, lithium counter electrode, and electrolyte were the same materials as in Example 2, and the coin half cell evaluation conditions were also the same as in Example 2.
[0172] The coin half-cells according to Example 1 and Comparative Example 1 were used to evaluate the initial charge / discharge capacity, and the results are shown in Table 1 and FIG. 3 below. The coin half-cells according to Example 2 and Comparative Example 2 were used to evaluate the initial charge / discharge capacity, and the results are shown in Table 2 and FIG. 4 below.
[0173] [Table 1]
[0174] [Table 2]
[0175] As can be seen from Tables 1 and 2, the coin half-cell of Example 1 manufactured by the manufacturing method of the present application was confirmed to have a higher initial charge capacity than the coin half-cell of Comparative Example 1 which was not pre-lithiated, and the coin half-cell of Example 2 was confirmed to have a lower initial charge capacity than the coin half-cell of Comparative Example 2 which was not pre-lithiated.
[0176] This is because the surface protective layer and the lithium metal layer are simultaneously transferred to the separator, which prevents the highly reactive lithium metal layer from being exposed to air, prevents direct contact between the negative electrode or positive electrode active material layer and the lithium metal layer, and controls the pre-lithiation rate, thereby demonstrating good initial charge capacity.
[0177] As can be seen in Examples 1 and 2, in the method for producing an electrode assembly according to the present application, a lithium metal layer is transferred to one side of a separator, rather than being directly transferred onto the top of an anode or cathode active material layer as in the conventional method. Thereafter, during the production of a battery assembly, the lithium metal layer comes into contact with the separator in the process of laminating it with an anode or cathode, and during the production of a cell, pre-lithiation is performed after an electrolyte is injected.
[0178] In particular, by transferring the surface protective layer and the lithium metal layer to the separator at the same time, it is possible to prevent the lithium metal layer from being exposed to air, and also, when the lithium metal layer is transferred to the separator together with the surface protective layer and subsequently pre-lithiation is performed, a structure is formed in which the surface protective layer contacts the negative or positive active material layer, making it unnecessary to install a separate layer on the negative or positive active material layer for adjusting the pre-lithiation rate. As a result, it is possible to easily adjust the pre-lithiation rate in the negative or active material layer as in the conventional method, it is economical because it is not necessary to install a separate layer such as a buffer layer, and it is possible to reduce the risk of fire because pre-lithiation may be performed after injecting the electrolyte. [Explanation of symbols]
[0179] 10. Separator 20 Lithium metal layer 30...Surface protective layer 40...Base material layer 50...Negative electrode active material layer 60 Negative electrode current collector layer 200 ···Transfer laminate 300 ···Negative electrode for lithium secondary battery
Claims
1. A step of preparing a transfer laminate in which a substrate layer, a surface protective layer, and a lithium metal layer are laminated in this order; transferring the surface protective layer and the lithium metal layer to a separator such that the lithium metal layer is in contact with the separator; and forming an electrode assembly by positioning a separator between a negative electrode and a positive electrode such that the surface protective layer faces one of the negative electrode and the positive electrode; Including, In the step of transferring the surface protective layer and the lithium metal layer to the separator, the lithium metal layer has a thickness of 1 μm to 10 μm.
2. 2 . The method of claim 1 , wherein the lithium metal layer transferred to the separator in the step of transferring the surface protective layer and the lithium metal layer has a thickness of 2 μm to 10 μm.
3. 2 . The method of claim 1 , wherein the surface roughness of the lithium metal layer transferred to the separator in the step of transferring the surface protection layer and the lithium metal layer to the separator is 0.02 μm to 0.2 μm.
4. 2. The method of claim 1, wherein the step of forming an electrode assembly by positioning a separator between the negative electrode and the positive electrode such that the surface protective layer faces one of the negative electrode and the positive electrode comprises forming the electrode assembly by one of lamination, pressure lamination, and winding.
5. 2. The method of claim 1, wherein the step of transferring the surface protective layer and the lithium metal layer to the separator such that the lithium metal layer contacts the separator comprises a dry on dry process.
6. The step of transferring the surface protective layer and the lithium metal layer to the separator so that the lithium metal layer is in contact with the separator includes laminating the lithium metal layer of the transfer laminate onto one surface of the separator; and removing the substrate layer; The method for manufacturing the electrode assembly of claim 1 , comprising:
7. the negative electrode includes a negative electrode current collector layer and a negative electrode active material layer on one or both sides of the negative electrode current collector layer, The negative electrode active material layer includes a negative electrode active material layer composition, The method of claim 1 , wherein the negative electrode active material layer composition comprises at least one selected from the group consisting of a negative electrode active material, a negative electrode conductive material, and a negative electrode binder.
8. the positive electrode includes a positive electrode current collector layer and a positive electrode active material layer on one or both sides of the positive electrode current collector layer; The positive electrode active material layer includes a positive electrode active material layer composition, The positive electrode active material layer composition is LiNi x Co y Mn z O 2 (x+y+z=1);LiNi a Co b Mn c A d O 2 (a+b+c+d=1);LiMn 2 O 4 ;LiNi 0.5 Mn 1.5 O 2 and LiM x Fe y P.O. 4 The method for manufacturing an electrode assembly according to claim 1 , further comprising at least one selected from the group consisting of: (M: transition metal, x+y=1).
9. The step of transferring the surface protective layer and the lithium metal layer to the separator such that the lithium metal layer is in contact with the separator includes the steps of pretreating the separator; and transferring a surface protective layer and a lithium metal layer onto the pretreated separator; Including, The method for manufacturing an electrode assembly according to claim 1 , wherein the pretreatment comprises a corona treatment or a plasma treatment.
10. forming an electrode assembly by disposing a separator between the negative electrode and the positive electrode such that one electrode selected from the negative electrode and the positive electrode faces the surface protective layer, the step of pretreating the surface protective layer, The method for manufacturing an electrode assembly according to claim 1 , wherein the pretreatment comprises a corona treatment or a plasma treatment.
11. The negative electrode active material is graphite, soft carbon, hard carbon, SiO x (x=0), SiO x The method for manufacturing an electrode assembly according to claim 7 , comprising one or more selected from the group consisting of (0<x<2), Si / C, and Si alloy.
12. The method of claim 1 , wherein the surface protection layer comprises at least one selected from the group consisting of a polymer, a conductive material, and inorganic particles.
13. An electrode assembly manufactured by the method according to any one of claims 1 to 12.
14. Battery casing materials; The electrode assembly according to claim 13 provided inside the battery exterior material; and Electrolyte; A lithium secondary battery comprising:
Citation Information
Patent Citations
Lithium metal coating on battery separator
JP2018506149A
Lithium electrode manufacturing method
JP2020501313A
Lithium electrode and lithium secondary battery including the same
JP2021517729A
Anode for lithium ion battery